Optical waveguide element, and optical modulation device and optical transmission apparatus using same

The use of a protective film and adhesive layers on the composite substrate of optical waveguide devices addresses peeling and cracking issues during cutting, enhancing the effective chip area and cutting efficiency for optical waveguide elements and transmitters.

WO2024201864A1PCT designated stage expired Publication Date: 2024-10-03SUMITOMO OSAKA CEMENT CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/013083
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Optical waveguide devices face issues with peeling and cracking of thin plates and intermediate layers during cutting, leading to reduced effective chip area and increased cutting time, especially when using materials like alpha quartz single crystal or sapphire as holding substrates.

Method used

A composite substrate with a protective film covering the first side surface of the thin plate, an adhesive layer at the interface, and grooves or irregularities on the surface to prevent peeling and cracking, along with an inclined first side surface to facilitate efficient cutting and maintain chip area.

Benefits of technology

The solution effectively suppresses peeling and cracking, reduces cutting time, and secures a wider effective area within the chip, enabling the production of high-quality optical waveguide elements for optical modulation devices and transmitters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023013083_03102024_PF_FP_ABST
    Figure JP2023013083_03102024_PF_FP_ABST
Patent Text Reader

Abstract

An optical waveguide element according to the present invention has a composite substrate provided with: a thin plate (1) in which an optical waveguide (10) is formed; and a holding substrate (4) to which the thin plate (1) is joined with an intermediate layer (2) therebetween. The optical waveguide element is characterized in that: a level difference is formed at a portion of side surfaces of the composite substrate; at the level difference, the position of a first side surface (B1) including the thin plate (1) is retreated inward of the composite substrate from the position of a second side surface (B2) including a holding substrate (3); and a protective film (PC) is disposed on the first side surface (B1).
Need to check novelty before this filing date? Find Prior Art

Description

Optical waveguide element, optical modulation device using the same, and optical transmitter

[0001] The present invention relates to an optical waveguide element, an optical modulation device using the same, and an optical transmission device, and in particular to an optical waveguide element having a composite substrate including a thin plate on which an optical waveguide is formed and a holding substrate to which the thin plate is bonded via an intermediate layer.

[0002] In the fields of optical communication and optical measurement, optical waveguide elements such as optical modulators are widely used. The optical waveguide is formed on a substrate having an electro-optic effect, such as lithium niobate (LN), and the optical modulator is provided with a modulation electrode that modulates the light wave propagating through the optical waveguide.

[0003] In driver-integrated modulators such as HB-CDMs (High Bandwidth Coherent Driver Modulators), there is a demand for incorporating the driver circuit that drives the optical waveguide element into the housing together with the optical waveguide element, and for further miniaturization of the overall package. To achieve this, the optical waveguide element itself is also being miniaturized, and a thin plate with a rib-type optical waveguide having a width and height of approximately 1 μm is being used. To increase the mechanical strength of the thin plate forming the optical waveguide, a holding substrate is used to hold the thin plate, and further, a composite substrate with an intermediate layer is used to improve adhesion between the thin plate and the holding substrate. Furthermore, functional layers such as electrodes are formed on the thin plate, and then the wafer is cut into individual optical waveguide element chips.

[0004] Specifically, the thin plate is a substrate with an electro-optic effect, such as LN, with a thickness of 1 μm or less, and the holding substrate is made of silicon (Si) or alpha quartz single crystal with a thickness of 0.2 to 1.0 mm to reinforce the mechanical strength. The intermediate layer is made of a material with a thickness of 10 μm or less that can increase the bonding strength, such as a Si oxide film, which is suitable for bonding an LN thin plate to a Si substrate.

[0005] By using silicon, a material widely used in the semiconductor industry, for the support substrate, the cutting conditions have been established, enabling high-quality cutting using a peripheral blade. Meanwhile, for broadband modulators, the use of low-dielectric-constant glass materials, alpha quartz single crystal, quartz, sapphire, and other materials for the support substrate is also being considered to improve dielectric properties. These materials generally tend to have lower machinability (ease of cutting) than silicon, making it difficult to maintain the quality of the cut surfaces of thin plates and intermediate layers using a single blade.

[0006] For example, as shown in Fig. 1(a), a composite substrate of a thin plate 1, an intermediate layer 2, and a holding substrate 3 is cut using a blade C1. In this case, frictional heat generated during processing, wear and falling off of the blade abrasive grains, and the influence of cutting fluid used to suppress these, can cause peeling, chipping, or chipping of the thin plate or intermediate layer, which can then develop into cracks, as shown in Fig. 1(b).

[0007] Furthermore, with optical waveguide elements, there is a growing demand for miniaturization in addition to faster communication speeds, and this has led to the formation of dense waveguides, electrodes, and other functional layers on chips. To form these, it is necessary to secure as large a chip surface area as possible, but if designs take into account peeling of thin plates, etc., the effective area will be narrower for the same chip size.

[0008] Figure 2 shows a method known as a bevel cut or step cut, in which two types of blades (C2, C3) are used for cutting. Compared to cutting in a single cutting step as shown in Figure 1, the first cut (see Figure 2(a)) in Figure 2 can be made shallower. Therefore, by using a cutting blade appropriate for each layer, peeling and cracking of the thin plate and intermediate layer can be suppressed. However, increasing the number of cuts poses the problem of increased time required for cutting.

[0009] Patent Document 1 also proposes a method of forming a groove 4 on the upper surface of the inside of the cut surface of the chip, as shown in Figure 3. The groove 4 acts as a breakwater, and when cut, it can prevent peeling of the thin plate or intermediate layer and the progression of cracks into the substrate, as shown in Figure 3(b). However, there is a problem in that the effective area of ​​the chip is narrowed by the width of the groove 4.

[0010] Patent Document 2 discloses a method in which the upper part of a composite substrate is removed in advance by dry etching (see FIG. 4(a)) and wet etching (see FIG. 4(b)), and then the substrate is divided along the removed part by laser irradiation or by a crystal cleavage plane (see FIG. 4(c)). Compared to blade cutting, this cutting method produces a higher quality processed surface and a narrower cutting width, ensuring a wider effective area within the chip. However, as shown in FIG. 4(b), peeling of thin plates and intermediate layers and under- (over-) etching can occur during wet etching.

[0011] JP 2007-48995 A JP 2002-277661 A

[0012] The present invention aims to solve the above-mentioned problems by providing an optical waveguide element that can suppress peeling and cracking of thin plates and intermediate layers in a composite substrate, suppress an increase in the time required for cutting, and ensure a large effective area within the chip, and also to provide an optical modulation device and an optical transmission device using this optical waveguide element.

[0013] In order to solve the above problems, the optical waveguide element, optical modulation device, and optical transmitter of the present invention have the following technical features: (1) An optical waveguide element having a composite substrate including a thin plate on which an optical waveguide is formed and a holding substrate to which the thin plate is bonded via an intermediate layer, characterized in that a step is formed on a part of a side surface of the composite substrate, and in the step, the position of a first side surface including the thin plate is receded toward the inside of the composite substrate from the position of a second side surface including the holding substrate, and a protective film is disposed on the first side surface.

[0014] (2) In the optical waveguide element described in (1) above, the protective film is formed so as to cover from the first side surface to a part of the upper surface of the thin plate.

[0015] (3) The optical waveguide element according to (1) above is characterized in that an adhesive layer is disposed on a part of the interface between the protective film and the composite substrate.

[0016] (4) The optical waveguide element according to (1) above, wherein a groove is formed in the composite substrate at a position further inward of the first side surface of the composite substrate.

[0017] (5) The optical waveguide element according to (1) above is characterized in that the surface of the first side surface is formed with irregularities.

[0018] (6) In the optical waveguide element described in (1) above, the first side surface is inclined so that the surface faces upward.

[0019] (7) An optical modulation device comprising the optical waveguide element according to any one of (1) to (6) above, a housing for accommodating the optical waveguide element, and an optical fiber for inputting and outputting light waves to and from the optical waveguide element.

[0020] (8) The optical modulation device according to (7) above is characterized in that a modulation electrode for modulating the light wave propagating through the optical waveguide is provided on the substrate, and an electronic circuit for amplifying the modulation signal input to the modulation electrode is provided inside or outside the housing.

[0021] (9) An optical transmitter comprising the optical modulation device according to (8) above and an electronic circuit for outputting a modulation signal that causes the optical modulation device to perform a modulation operation.

[0022] According to the present invention, an optical waveguide element includes a composite substrate including a thin plate having an optical waveguide formed thereon and a holding substrate to which the thin plate is bonded via an intermediate layer. A step is formed on a portion of the side of the composite substrate, and at the step, the position of a first side including the thin plate is recessed inward from the position of a second side including the holding substrate. A protective film is disposed on the first side, protecting the first side with the protective film, effectively preventing damage to the first side when cutting along the second side. Cutting the portion including the thin plate, such as the thin plate or intermediate layer, employs a technique that prevents peeling and cracking of the thin plate, and then covers the first side with a protective film. This allows for an efficient cutting technique to be used when cutting the portion including the holding substrate, thereby minimizing the increase in cutting time. Furthermore, because damage to the first side is suppressed, an optical waveguide element can be provided that ensures a large effective area within the chip. It is also possible to provide an optical modulation device and an optical transmission device using an optical waveguide element that achieves this excellent effect.

[0023] 1A and 1B are diagrams illustrating an example of conventional cutting in a single cutting step, where (a) shows the state of cutting with a blade, and (b) shows the state of the chip after cutting. FIG. 1C is a diagram illustrating an example of conventional cutting in two cutting steps, where (a) shows the first cutting step, (b) shows the second cutting step, and (c) shows the state of the chip after cutting. FIG. 1D is a diagram illustrating an example of arranging a groove near the cut portion disclosed in Patent Document 1, where (a) shows the state of cutting with a blade, and (b) shows the state of the chip after cutting. FIG. 1E is a diagram illustrating a cutting method disclosed in Patent Document 2, where (a) shows the state after dry etching, (b) shows the state after wet etching, and (c) shows the state after cutting with a laser or the like. FIG. 1F is a plan view showing an example of an optical waveguide element of the present invention. FIG. 1G is a cross-sectional view taken along the dashed dotted line A-A' in FIG. 5. FIG. 1G is a diagram illustrating an example of a method for forming an optical waveguide element of the present invention, showing each step in the order of (a) to (d). FIG. 1H is a cross-sectional view showing an application example of FIG. 6. FIG. 1I is a diagram illustrating an example of arranging a groove 4 near the first side surface B1. 1 is a diagram showing an example of forming unevenness on the surface of a first side surface B1. FIG. 2 is a diagram showing an example of configuring the first side surface B1 as an inclined surface. FIG. 3 is a plan view showing an optical modulation device and an optical transmission device according to the present invention.

[0024] 5 and 6, the present invention provides an optical waveguide element having a composite substrate including a thin plate 1 having an optical waveguide 10 formed thereon and a holding substrate 4 to which the thin plate is bonded via an intermediate layer 2, the composite substrate having a step formed in a portion of its side surface, the step positioning a first side surface B1 including the thin plate 1 toward the inside of the composite substrate from the position of a second side surface B2 including the holding substrate 3, and a protective film PC disposed on the first side surface B1.

[0025] As the substrate 1, substrates having an electro-optic effect such as LN, lithium tantalate, lead lanthanum zirconate titanate (PLZT), vapor-deposited films made from these materials, and various other materials such as semiconductor materials and organic materials can be used.

[0026] As a method for forming an optical waveguide, a rib-type optical waveguide can be used, in which the portion of the substrate corresponding to the optical waveguide is convex, for example, by etching the surface of the substrate other than the optical waveguide and forming grooves on both sides of the optical waveguide. Bending loss can be reduced by using a horizontal slot waveguide, in which a slot waveguide structure is formed in the thickness direction by thinning the substrate. An optical waveguide can also be formed by forming a high refractive index portion on the substrate surface using a thermal diffusion method or a proton exchange method using titanium (Ti) or the like. A composite optical waveguide can also be formed by diffusing a high refractive index material into the rib-type optical waveguide portion. In particular, when miniaturizing the optical waveguide element itself or using a bent optical waveguide, a convex waveguide with a width or height of approximately 1 μm, which has strong optical confinement, is used.

[0027] To achieve velocity matching between the microwaves and light waves of the modulation signal, the substrate on which the optical waveguide is formed is thinned by grinding and polishing to a thickness of 10 μm or less, more preferably 5 μm or less, and even more preferably less than 1 μm (the lower limit of the thickness is preferably 0.3 μm or more), or by the Smart Cut method (a method of thinning by ion implantation delamination). The height of the rib-type optical waveguide is preferably set to 1 μm or less. It is also possible to form a vapor-deposited film on another substrate to a thickness approximately equal to that of the substrate described above, and then process the film into the shape of the optical waveguide described above.

[0028] A substrate (thin plate, thin film) 1 on which an optical waveguide is formed is adhesively fixed to a holding substrate 3 via an intermediate layer 2 to enhance mechanical strength. In the present invention, a substrate integrating the thin plate 1, intermediate layer 2, and holding substrate 3 is referred to as a "composite substrate." The holding substrate 3 can be made of silicon (Si), a glass material with a low dielectric constant, alpha quartz single crystal, quartz, sapphire, or the like, with a thickness of 0.2 to 1.0 mm. Furthermore, a material with a lower refractive index than the thin plate 1 is used for the intermediate layer to achieve velocity matching between light waves and electrical signals (microwaves). Furthermore, to prevent thermal stress from being applied to the thin plate 1, a material with a thermal expansion coefficient close to that of the thin plate 1 is preferred. Examples of usable materials include silicon dioxide, silicon nitride, aluminum oxide, magnesium fluoride, lanthanum oxide, zinc oxide, magnesium oxide, calcium fluoride, and yttrium oxide. Furthermore, to maintain adhesive strength, the holding substrate 3 is preferably thicker than the optical waveguide substrate, 10 μm or less.

[0029] A feature of the optical waveguide element of the present invention is that, as shown in Figures 5 and 6, a protective film PC is formed on the first side surface B1 including the thin plate 1. Figure 5 is a plan view of the optical waveguide element, and for ease of viewing the drawing, the optical waveguide is not shown, but as shown in Figure 6, a rib-type optical waveguide 10 is disposed between the signal electrode ES and the ground electrodes (EG1, EG2).

[0030] 6 is an example of a cross-sectional view taken along dashed line A-A' in FIG. 5, in which a protective film PC is disposed on the first side surface B1 including the thin plate 1 on which the optical waveguide 10 is formed. The thin plate 1 and intermediate layer 2 in the portion to be cut are removed in advance by dry etching, and a protective film PC having a thickness of 1 μm or more is formed so as to cover the removed side surface B1 and not to be caught by the blade used during cutting. The lower end of the protective film PC can also be positioned midway through the intermediate layer 2 or inside the holding substrate 3.

[0031] The material used for the protective film PC can be a material used only for the protective film, but since functional layers such as electrodes and spot size converters are formed on the thin plate 1, it is also possible to use the material used for these functional layers. Furthermore, organic dielectrics such as resist-like resins with a small Young's modulus and easy patterning are preferred, and materials such as polyamide resins, melamine resins, phenolic resins, amino resins, and epoxy resins can be used. Forming the protective film simultaneously with the formation of these functional layers also helps prevent the production process from becoming too complicated.

[0032] If the protective film is formed before forming functional layers such as electrodes, over-etching of the intermediate layer, which may occur in subsequent wet etching processes, can be suppressed. In this case, a material that can withstand the chemicals used in wet etching, such as tantalum, gold (Au), silver, aluminum, or Si, is selected.

[0033] If the protective film has low adhesion to the thin plate 1, the holding substrate 3, or the intermediate layer 2, an adhesion layer BL can be formed at a portion of the interface between the protective film PC and these substrates. This adhesion layer can be formed also on the bottom surface of the step between the first side surface B1 and the second side surface B2 to further enhance adhesion. The material used for the adhesion layer BL depends on the material used for the protective film PC. For example, if Au is used for the protective film PC, Ti, niobium (Nb), nickel, chromium, etc. can be used for the adhesion layer. In particular, using Ti, Nb, etc. not only improves adhesion to the protective film, but also provides excellent corrosion resistance to iodine, an etchant for Au.

[0034] FIG. 7 shows an example of cutting a chip using a protective film PC. As shown in FIG. 7(a), the thin plate 1 and intermediate layer 2 are removed by dry etching. Next, as shown in FIG. 7(b), a protective film PC is formed on the first side B1. An adhesion layer BL can also be formed in advance. As shown in FIG. 7(c), when cutting the holding substrate 3 with a blade C4, the blade C4 is positioned so as not to intersect with the protective film PC. This allows cutting in a single step, thereby preventing peeling and cracking of the thin plate 1, intermediate layer 2, and functional layers (not shown) formed on the thin plate. It also reduces processing time. As shown in FIG. 7(d), cutting can be performed close to the protective film PC, minimizing damage to the interior of the composite substrate, thereby ensuring a large effective chip area. While cutting is performed with a blade C4 in FIG. 7, a larger effective area can also be achieved by using a laser for cutting.

[0035] 6 and 7(d), the protective film PC can be formed so as to cover from the first side surface B1 to a part of the upper surface of the thin plate 1. This makes it possible to widen the area that can be protected by the protective film PC and also to increase the adhesion between the protective film PC and the thin plate 1, etc.

[0036] The protective film PC can be formed over the entire first side surface B1, including the thin plate 1, but it can also be formed continuously or discontinuously around the periphery of the chip. Forming the protective film PC continuously enhances the protective effect. However, for the surface where the optical waveguide end is formed, a protective layer need not be formed because the end surface is polished after cutting. For example, it is possible to provide a portion on the right side of the drawing in FIG. 5 where no protective film is formed. This is because, in an optical waveguide element having a pattern in which the optical waveguide is folded back, the side where light waves are input to or output from the optical waveguide is formed on this right side.

[0037] 8 is a cross-sectional view showing an application example of Fig. 6, in which the protective film PC is formed integrally with the electrode (particularly the ground electrode EG1). By forming the protective film from the same material as the electrode, for example, Au, and further electrically connecting the protective film PC and the ground electrode, the protective layer can function as the ground electrode, and a larger effective area can be secured within the chip.

[0038] 9 shows the formation of a groove 4 on the surface of the composite substrate (thin plate 1) near the first side B1 on which the protective film PC is formed. This groove can suppress the progression of damage to the inside of the thin plate in the unlikely event that the thin plate 1 peels off. Furthermore, by arranging the protective film so that the protective film PC fits into the groove 4, the bonding strength of the protective film to the thin plate can be increased due to the anchor effect.

[0039] 10, the surface of the first side surface B1 on which the protective film PC is disposed is uneven. By arranging the protective film PC in accordance with the unevenness, the contact area between the first side surface and the protective film is increased, and the bonding strength between them can be increased.

[0040] 11 shows the first side surface B1 tilted so that the surface faces upward. When forming the adhesion layer BL by sputtering, vapor deposition, or the like, the thickness of the adhesion layer can be increased by the amount of tilt, ensuring that the adhesion layer BL is also formed on the first side surface B1. Similarly, the protective film PC can be formed thicker, enhancing the protective function of the thin plate and intermediate layer.

[0041] As shown in Figure 12, a compact optical modulation device MD can be provided by housing the optical waveguide element (substrate 1) of the present invention in a housing CA made of metal or the like and connecting the outside of the housing to the optical waveguide element with an optical fiber F. Naturally, an optical fiber can be directly connected to the input or output portion of the optical waveguide of substrate 1, or optically connected via a spatial optical system. Note that reference numeral 5 denotes a reinforcing member superimposed on substrate 1 along the end face of substrate 1, and is used when directly joining an optical component such as an optical fiber to the end face of substrate 1.

[0042] A modulation signal S that causes the optical modulation device MD to perform a modulation operation 0An optical transmitter OTA can be configured by connecting an electronic circuit (digital signal processor DSP) that outputs a modulated signal S to an optical modulation device MD. Because the modulated signal S to be applied to the optical waveguide element needs to be amplified, a driver circuit DRV is used. The driver circuit DRV and digital signal processor DSP can be placed outside the housing CA, but they can also be placed inside the housing CA. In particular, placing the driver circuit DRV inside the housing further reduces the propagation loss of the modulated signal from the driver circuit, enabling a wider bandwidth.

[0043] As described above, according to the present invention, it is possible to provide an optical waveguide element that can suppress peeling and cracking of the thin plate and intermediate layer in the composite substrate, suppress an increase in the time required for cutting, and ensure a large effective area within the chip. Furthermore, it is possible to provide an optical modulation device and an optical transmission device that use the optical waveguide element having such excellent effects.

[0044] 1 Thin plate 2 Intermediate layer 3 Holding substrate 4 Groove PC Protective film BL Adhesion layer B1 First side surface B2 Second side surface

Claims

1. An optical waveguide element having a composite substrate comprising a thin plate having an optical waveguide formed thereon and a holding substrate to which the thin plate is bonded via an intermediate layer, wherein a step is formed on a portion of a side of the composite substrate, and in the step, the position of a first side including the thin plate is retreated toward the inside of the composite substrate from the position of a second side including the holding substrate, and a protective film is disposed on the first side.

2. An optical waveguide element according to claim 1, wherein the protective film is formed so as to cover from the first side surface to a part of the upper surface of the thin plate.

3. The optical waveguide element according to claim 1, wherein an adhesive layer is disposed on a portion of the interface between said protective film and said composite substrate.

4. An optical waveguide element according to claim 1, wherein said composite substrate has a groove formed at a position further inward of said first side surface.

5. An optical waveguide element according to claim 1, wherein the surface of said first side is formed with projections and recesses.

6. An optical waveguide element according to claim 1, wherein the first side surface is inclined so that the surface faces upward.

7. An optical modulation device comprising: an optical waveguide element according to any one of claims 1 to 6; a housing for accommodating said optical waveguide element; and an optical fiber for inputting and outputting optical waves to and from said optical waveguide element.

8. An optical modulation device according to claim 7, characterized in that a modulation electrode for modulating the light wave propagating through the optical waveguide is provided on the substrate, and an electronic circuit for amplifying the modulation signal input to the modulation electrode is provided inside or outside the housing.

9. An optical transmitter comprising: an optical modulation device according to claim 8; and an electronic circuit for outputting a modulation signal for causing said optical modulation device to perform a modulation operation.

Citation Information

Patent Citations

  • Optical waveguide

    JP2004295118A

  • Semiconductor device and method for manufacturing the same

    JP2008140829A

  • Optical waveguide device

    JP2021105658A

  • Optical device, optical communication apparatus, and optical device manufacturing method

    JP2022142650A