Functional film and method for manufacturing same, and image display device
The functional film with a carbon and metal-rich primer layer addresses the issue of light-induced adhesion loss in image display devices, ensuring excellent durability and optical performance by enhancing adhesion between the resin film base and the functional inorganic layer.
Patent Information
- Application Number
- PCT/JP2023/044402
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2023-12-12
- Publication Date
- 2024-10-03
AI Technical Summary
Existing functional films used in image display devices, such as liquid crystal displays and organic EL displays, face challenges in maintaining adhesion between the resin film base material and the functional inorganic layer after exposure to light, particularly ultraviolet rays, which affects their durability and performance.
A functional film with a primer layer containing carbon, oxygen, and metal elements, where the carbon content is 10 atomic % or more and the metal element content is also 10 atomic % or more, interposed between the resin film base material and the functional inorganic layer, enhances light-resistant adhesion. The primer layer is preferably a sputtered layer with specific metal elements like Ti, Si, Mo, and Ta, and has a thickness of 20 nm or less, ensuring excellent adhesion and optical functionality.
The functional film achieves excellent light-resistant adhesion, maintaining the integrity of the film even after light exposure, thereby improving the durability and image quality of image display devices by reducing light scattering and enhancing the optical functions such as antireflection.
Smart Images

Figure JP2023044402_03102024_PF_FP_ABST
Abstract
Description
Functional film, its manufacturing method, and image display device
[0001] The present invention relates to a functional film having a functional inorganic layer, a method for producing the same, and an image display device.
[0002] In image display devices such as liquid crystal displays and organic EL displays, functional films having a functional inorganic layer made of an inorganic material are used. Examples of the functional inorganic layer include an antireflection layer, a gas barrier layer, and a transparent conductive layer. For example, an antireflection film having an antireflection layer is disposed on the viewing side of the image display device for the purposes of preventing deterioration of image quality due to reflection of external light and improving contrast.
[0003] Patent Document 1 discloses a method for forming a SiO primer layer on a hard coat film, and a niobium oxide (Nb 2 O 5 ) layer as a low refractive index layer and silicon oxide (SiO 2 ) layers and an anti-reflection film comprising an anti-reflection layer consisting of an alternating laminate of the layers.
[0004] JP 2009-47876 A
[0005] As in the antireflection film described in Patent Document 1, a primer layer is usually provided between the resin film substrate and the functional inorganic layer to ensure adhesion between them. However, it is difficult to obtain a functional film that has excellent adhesion after irradiation with light such as ultraviolet light (hereinafter, this may be referred to as "light-resistant adhesion") using only the technology described in Patent Document 1.
[0006] In view of the above, an object of the present invention is to provide a functional film having excellent light-resistant adhesion, a method for producing the same, and an image display device using the functional film.
[0007] <Aspects of the Present Invention> The present invention includes the following aspects.
[0008] [1] A functional film having a resin film substrate, a functional inorganic layer, and a primer layer interposed between the resin film substrate and the functional inorganic layer, wherein the primer layer contains carbon, oxygen, and a metal element as constituent elements, the carbon content in the primer layer is 10 atomic % or more relative to a total of 100 atomic % of carbon, oxygen, and the metal element, and the metal element content in the primer layer is 10 atomic % or more relative to a total of 100 atomic % of carbon, oxygen, and the metal element.
[0009] [2] The functional film according to [1], wherein the metal element is one or more metal elements selected from the group consisting of Group 4 elements, Group 5 elements, Group 6 elements, and Group 14 elements other than carbon in the periodic table.
[0010] [3] The functional film according to [2], wherein the metal element is one or more metal elements selected from the group consisting of Ti, Si, Mo, Nb, and Ta.
[0011] [4] The functional film according to any one of [1] to [3], wherein the thickness of the primer layer is 20 nm or less.
[0012] [5] The functional film according to any one of [1] to [4], wherein the outermost layer on the primer layer side of the resin film substrate is a hard coat layer containing a resin as a main component.
[0013] [6] The functional film according to [5], wherein the amount of particles having a number average primary particle diameter of less than 1.0 μm in the hard coat layer is 10 parts by weight or less relative to 100 parts by weight of the resin in the hard coat layer.
[0014] [7] The functional film according to any one of [1] to [6], wherein the oxygen content in the primer layer is 35 atomic % or less, relative to a total of 100 atomic % of carbon, oxygen, and the metal element.
[0015] [8] The functional film according to any one of [1] to [7], wherein the arithmetic mean height Sa of the main surface of the resin film substrate on the primer layer side is 4.0 nm or less.
[0016] [9] A functional film having a resin film substrate, a functional inorganic layer, and a primer layer interposed between the resin film substrate and the functional inorganic layer, wherein the primer layer is a sputtered layer and contains carbon, oxygen, and a metal element as constituent elements.
[0017]
[10] The functional film according to any one of [1] to [9], wherein the functional inorganic layer is an anti-reflection layer.
[0018]
[11] The method for producing a functional film according to [9] above, comprising the step of forming the primer layer on one main surface of the resin film substrate by a sputtering method.
[0019]
[12] An image display device comprising: an image display panel; and the functional film according to
[10] , which is arranged on the viewing side of the image display panel.
[0020] According to the present invention, it is possible to provide a functional film having excellent light-resistant adhesion, a method for producing the same, and an image display device using the functional film.
[0021] 1 is a cross-sectional view showing an example of a functional film according to the present invention, a cross-sectional view showing another example of a functional film according to the present invention, and a cross-sectional view showing an example of an image display device according to the present invention.
[0022] Preferred embodiments of the present invention are described below. First, the terms used in this specification are explained. "Metal element" includes silicon (Si), which is generally classified as a semimetal element. Unless otherwise specified, "refractive index" refers to the refractive index for light with a wavelength of 550 nm in an atmosphere at 23°C. The "main surface" of a layered material (more specifically, a resin film substrate, a resin film, a hard coat layer, a primer layer, a functional inorganic layer, an anti-reflection layer, etc.) refers to the surface perpendicular to the thickness direction of the layered material. Unless otherwise specified, the "thickness (film thickness)" of each layer constituting the functional film is the arithmetic average of 10 measurements obtained by randomly selecting 10 measurement points from an image of a cross section cut through the layer in the thickness direction and measuring the thickness of the selected 10 measurement points. "Solid content" refers to non-volatile components in the composition, such as components other than the solvent.
[0023] The "arithmetic mean height Sa (surface roughness Sa)" is a parameter of the surface shape measured in accordance with ISO 25178. The specific method for measuring the arithmetic mean height Sa is the same as or a similar method to that described in the examples below.
[0024] Unless otherwise specified, the number average primary particle diameter of particles is the number average value of the circle equivalent diameters (Heywood diameter: diameter of a circle having the same area as the projected area of a primary particle) of 100 primary particles measured using a scanning electron microscope and image processing software (for example, "ImageJ" manufactured by the National Institutes of Health, USA).
[0025] "Periodic Table" refers to the long-period periodic table of elements based on the provisions of IUPAC (International Union of Pure and Applied Chemistry).
[0026] Unless otherwise specified, the "major component" of a material means the component that is contained in the largest amount in that material by weight.
[0027] Hereinafter, the compound and its derivatives may be collectively referred to by adding "based" after the compound name. Furthermore, when the compound name is followed by "based" to represent the name of a polymer, it means that the repeating unit of the polymer is derived from the compound or its derivative. Unless otherwise specified, the components, functional groups, etc. exemplified in this specification may be used alone or in combination of two or more types.
[0028] The drawings referred to in the following description mainly show each component in a schematic manner for ease of understanding, and the size, number, shape, etc. of each component shown may differ from the actual size, number, shape, etc. of each component due to the convenience of creating the drawings. Furthermore, for convenience of explanation, in drawings described later, the same components as those in previously described drawings may be assigned the same reference numerals, and their explanation may be omitted.
[0029] <First embodiment: functional film> The functional film according to the first embodiment of the present invention (hereinafter sometimes referred to as "functional film F1") is a laminate having a resin film substrate, a functional inorganic layer, and a primer layer interposed between the resin film substrate and the functional inorganic layer. The primer layer contains carbon, oxygen, and metal elements as constituent elements. The carbon content in the primer layer is 10 atomic % or more relative to a total of 100 atomic % of carbon, oxygen, and metal elements. The metal element content in the primer layer is 10 atomic % or more relative to a total of 100 atomic % of carbon, oxygen, and metal elements.
[0030] Hereinafter, the content of carbon in the primer layer relative to the total of 100 atomic % of carbon, oxygen, and metal elements in the primer layer may be simply referred to as the "carbon content." Furthermore, the content of metal elements in the primer layer relative to the total of 100 atomic % of carbon, oxygen, and metal elements in the primer layer may be simply referred to as the "metal element content."
[0031] The carbon content and metal element content can both be calculated from the elemental composition at the center of the primer layer in the thickness direction by analyzing the composition in the thickness direction by X-ray photoelectron spectroscopy. Hereinafter, X-ray photoelectron spectroscopy may be referred to as "XPS." The method for analyzing the composition in the thickness direction of the primer layer by XPS is the same as or a similar method to that described in the examples below. Unless otherwise specified, the carbon content and metal element content are both values calculated from the elemental composition at the center of the primer layer in the thickness direction (when half of the total etching time has elapsed). The "total etching time" refers to the time from the start to the end of etching the primer layer.
[0032] The functional film F1 has excellent light-resistant adhesion. The reason for this is presumed to be as follows. In the following, unless otherwise specified, "light-resistant adhesion" refers to the light-resistant adhesion between the resin film substrate and the functional inorganic layer.
[0033] In the functional film F1, a primer layer containing carbon and metal elements in specific ranges is interposed between the resin film substrate and the functional inorganic layer. Carbon tends to have a high affinity with the resin film substrate, and metal elements tend to have a high affinity with the functional inorganic layer. Therefore, in the functional film F1, the adhesion between the resin film substrate and the functional inorganic layer can be maintained well even after light irradiation. Therefore, the functional film F1 has excellent light-resistant adhesion.
[0034] In the first embodiment, in order to obtain a functional film having superior light-resistant adhesion between the resin film substrate and the primer layer, the carbon content is preferably 20 atomic % or more, more preferably 30 atomic % or more, even more preferably 40 atomic % or more, and even more preferably 45 atomic % or more.
[0035] In the first embodiment, in order to obtain a functional film having superior light-resistant adhesion between the functional inorganic layer and the primer layer, the carbon content is preferably 70 atomic % or less, more preferably 65 atomic % or less, even more preferably 60 atomic % or less, and even more preferably 55 atomic % or less.
[0036] In the first embodiment, in order to obtain a functional film having superior light-resistant adhesion between the functional inorganic layer and the primer layer, the metal element content is preferably 12 atomic % or more, and more preferably 15 atomic % or more.
[0037] In the first embodiment, in order to obtain a functional film having superior light-resistant adhesion between the resin film substrate and the primer layer, the metal element content is preferably 50 atomic % or less, more preferably 45 atomic % or less, even more preferably 40 atomic % or less, even more preferably 35 atomic % or less, and particularly preferably 30 atomic % or less.
[0038] In the first embodiment, in order to obtain a functional film having superior light-resistant adhesion, the total content of carbon and metal elements in the primer layer is preferably 50 atomic % or more and 90 atomic % or less, more preferably 55 atomic % or more and 85 atomic % or less, even more preferably 60 atomic % or more and 80 atomic % or less, and even more preferably 65 atomic % or more and 80 atomic % or less, relative to 100 atomic % of the total of carbon, oxygen, and metal elements.
[0039] In the first embodiment, in order to obtain a functional film having excellent light-resistant adhesion, the oxygen content in the primer layer is preferably 35 atomic % or less relative to 100 atomic % of the total of carbon, oxygen, and metal elements.
[0040] In the first embodiment, in order to stably maintain the primer layer, the oxygen content in the primer layer is preferably 10 atomic % or more, more preferably 15 atomic % or more, and even more preferably 20 atomic % or more, relative to 100 atomic % in total of carbon, oxygen, and metal elements.
[0041] The configuration of a functional film F1 according to a first embodiment will be described below with reference to the drawings. FIG. 1 is a cross-sectional view showing an example of a functional film F1. The functional film 10 shown in FIG. 1 has a resin film substrate 11, a functional inorganic layer 12, and a primer layer 13 interposed between the resin film substrate 11 and the functional inorganic layer 12. The primer layer 13 is in contact with both the resin film substrate 11 and the functional inorganic layer 12. The primer layer 13 contains carbon, oxygen, and metal elements as constituent elements. In the primer layer 13, the carbon content and the metal element content are both 10 atomic % or more.
[0042] The resin film substrate 11 is a laminate of a resin film 14 and a hard coat layer 15 containing a resin as a main component. In the example shown in Fig. 1 , the outermost layer on the primer layer 13 side of the resin film substrate 11 is the hard coat layer 15. That is, the functional film 10 has the resin film 14, the hard coat layer 15, the primer layer 13, and the functional inorganic layer 12 in this order.
[0043] In order to suppress light scattering due to unevenness on the principal surface of the resin film substrate 11 on the primer layer 13 side (in the case of FIG. 1, the principal surface 15a of the hard coat layer 15 on the primer layer 13 side), the arithmetic mean height Sa of the principal surface is preferably 4.0 nm or less, more preferably 3.0 nm or less, even more preferably 2.0 nm or less, and even more preferably 1.0 nm or less. In particular, when the functional inorganic layer 12 is an optically functional layer that suppresses light scattering, such as an antireflection layer described below, the optical function can be improved by setting the arithmetic mean height Sa of the principal surface of the resin film substrate 11 on the primer layer 13 side within the above-mentioned preferred range. The lower limit of the arithmetic mean height Sa of the principal surface of the resin film substrate 11 on the primer layer 13 side is not particularly limited, but is, for example, 0.1 nm.
[0044] The functional film F1 may have a layer structure different from that of the functional film 10 shown in Fig. 1. For example, the functional film F1 may be a functional film 20 including a multilayered functional inorganic layer 21 as shown in Fig. 2. An example of the functional inorganic layer 21 is an anti-reflection layer having a multilayered structure.
[0045] When the functional inorganic layer 21 is an antireflection layer with a multilayer structure, the functional inorganic layer 21 has four layers, namely, a high refractive index layer 22, a low refractive index layer 23, a high refractive index layer 24, and a low refractive index layer 25, in this order from the primer layer 13 side. Details of the high refractive index layer and the low refractive index layer will be described later. The antireflection layer of the functional film is not limited to the four-layer structure as shown in FIG. 2 , and may have a two-layer structure, a three-layer structure, a five-layer structure, or a laminated structure of six or more layers. The antireflection layer of the functional film may also have a single-layer structure. Examples of antireflection layers with a single-layer structure include an antireflection layer made of a niobium oxide layer and an antireflection layer made of a silicon oxide layer.
[0046] The configuration of the functional film F1 according to the first embodiment has been described above, but the configuration of the functional film F1 is not limited to the above example. For example, the functional film F1 may have a primer layer and a functional inorganic layer provided in this order on both main surfaces of a resin film substrate. Furthermore, the hard coat layer is not an essential component of the functional film F1. When the hard coat layer is not provided in the functional film F1, for example, a resin film is used alone as the resin film substrate. Furthermore, the functional film F1 may have layers different from the layers included in the above configuration (resin film, hard coat layer, primer layer, and functional inorganic layer).
[0047] Next, the elements of the functional film F1 according to the first embodiment will be described.
[0048] [Resin Film] The resin film is, for example, a flexible resin film. Furthermore, when the functional film F1 is an optically functional film such as an anti-reflection film, a transparent resin film is preferable. Examples of materials constituting the resin film include polyester resin, polyolefin resin, polystyrene resin, acrylic resin, polycarbonate resin, polyethersulfone resin, polysulfone resin, polyamide resin, polyimide resin, cellulose resin, norbornene resin, polyarylate resin, and polyvinyl alcohol resin. Examples of polyester resins include polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate. Examples of polyolefin resins include polyethylene, polypropylene, and cycloolefin polymer (COP). Examples of cellulose resins include triacetyl cellulose (TAC). These materials may be used alone or in combination. From the viewpoints of transparency and strength, the material of the resin film is preferably one selected from the group consisting of polyester resin, polyolefin resin, and cellulose resin, more preferably one selected from the group consisting of PET, COP, and TAC, and even more preferably TAC. That is, the resin film is preferably one film selected from the group consisting of polyester resin film, polyolefin resin film, and cellulose resin film, more preferably one film selected from the group consisting of PET film, COP film, and TAC film, and even more preferably TAC film.
[0049] From the viewpoint of strength, the thickness of the resin film is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more. From the viewpoint of handleability, the thickness of the resin film is preferably 300 μm or less, and more preferably 200 μm or less.
[0050] One or both main surfaces of the resin film may be subjected to a surface modification treatment, such as a corona treatment, a plasma treatment, an ozone treatment, a primer treatment, a glow treatment, or a coupling agent treatment.
[0051] The total light transmittance (JIS K 7375-2008) of the resin film is preferably 80% or more, more preferably 90% or more, and even more preferably 95% or more and 100% or less, from the viewpoint of improving the transparency of the functional film.
[0052] [Hard Coat Layer] The hard coat layer is a layer that enhances the mechanical properties of the functional film, such as hardness and elastic modulus, and is primarily composed of a resin. The hard coat layer is made of, for example, a cured product of a curable resin composition (a composition for forming a hard coat layer). Examples of the curable resin contained in the curable resin composition include polyester resin, acrylic resin, urethane resin, urethane acrylate resin, amide resin, silicone resin, epoxy resin, and melamine resin. These curable resins may be used alone or in combination of two or more. From the viewpoint of increasing the hardness of the hard coat layer, the curable resin is preferably one or more selected from the group consisting of acrylic resin and urethane acrylate resin, and more preferably a urethane acrylate resin.
[0053] Furthermore, examples of the curable resin composition include an ultraviolet-curable resin composition and a thermosetting resin composition. From the viewpoint of improving the productivity of functional films, the curable resin composition is preferably an ultraviolet-curable resin composition. The ultraviolet-curable resin composition contains one or more selected from the group consisting of an ultraviolet-curable monomer, an ultraviolet-curable oligomer, and an ultraviolet-curable polymer. A specific example of the ultraviolet-curable resin composition is a composition for forming a hard coat layer described in JP 2016-179686 A.
[0054] The curable resin composition may also contain particles having a number average primary particle diameter of less than 1.0 μm (hereinafter, may be referred to as "nanoparticles"). When the hard coat layer is made of a cured product of the curable resin composition containing nanoparticles, fine irregularities are formed on the surface of the hard coat layer, which tends to improve adhesion between the hard coat layer and layers formed thereon.
[0055] From the viewpoint of forming a fine uneven shape that contributes to improving adhesion, the number average primary particle diameter of the nanoparticles is preferably 20 nm or more and 80 nm or less, and more preferably 25 nm or more and 70 nm or less.
[0056] As the material for the nanoparticles, inorganic oxides are preferred. Examples of inorganic oxides include oxides of metals (or semi-metals) such as silicon oxide (silica), titanium oxide, aluminum oxide, zirconium oxide, niobium oxide, zinc oxide, tin oxide, cerium oxide, and magnesium oxide. The inorganic oxide may also be a composite oxide of multiple (semi-)metals. Among the exemplified inorganic oxides, silicon oxide is preferred because of its high adhesion-improving effect. In other words, silicon oxide particles (silica particles) are preferred as nanoparticles. Functional groups such as acrylic groups and epoxy groups may be introduced onto the surfaces of inorganic oxide particles as nanoparticles in order to improve adhesion and affinity with resins.
[0057] The arithmetic mean height Sa of the principal surface of the resin film substrate on the primer layer side can be adjusted, for example, by changing the amount of nanoparticles in the hard coat layer. In order to suppress light scattering due to unevenness on the surface of the hard coat layer, the amount of nanoparticles in the hard coat layer is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, and even more preferably 1 part by weight or less, per 100 parts by weight of the resin. In the first embodiment, even if the hard coat layer does not contain nanoparticles, adhesion between the hard coat layer and the primer layer can be ensured. Therefore, in order to further suppress light scattering due to unevenness on the surface of the hard coat layer, it is preferable that the hard coat layer does not substantially contain nanoparticles.
[0058] The curable resin composition (hard coat layer-forming composition) contains, for example, the above-mentioned curable resin and a polymerization initiator (e.g., a photopolymerization initiator), and optionally a solvent capable of dissolving or dispersing these components. In addition to the above components, the curable resin composition (hard coat layer-forming composition) may contain additives such as particles (microparticles) having a number-average primary particle diameter of 1.0 μm or more, nanoparticles, leveling agents, viscosity modifiers (thixotropic agents, thickeners, etc.), antistatic agents, antiblocking agents, dispersants, dispersion stabilizers, antioxidants, ultraviolet absorbers, antifoaming agents, surfactants, and lubricants.
[0059] The thickness of the hard coat layer is preferably 1 μm or more, more preferably 2 μm or more, from the viewpoint of increasing the hardness of the hard coat layer, and is preferably 50 μm or less, more preferably 40 μm or less, even more preferably 35 μm or less, and still more preferably 30 μm or less, from the viewpoint of ensuring the flexibility of the functional film.
[0060] [Primer Layer] The primer layer is provided to enhance adhesion between the resin film substrate and the functional inorganic layer. The primer layer contains carbon, oxygen, and metal elements as constituent elements. The carbon content in the primer layer is 10 atomic % or more relative to 100 atomic % of the total of carbon, oxygen, and metal elements. The metal element content in the primer layer is 10 atomic % or more relative to 100 atomic % of the total of carbon, oxygen, and metal elements.
[0061] In order to obtain a functional film having excellent light-resistant adhesion, the metal element in the primer layer is preferably one or more metal elements selected from the group consisting of Group 4 elements, Group 5 elements, Group 6 elements, and Group 14 elements other than carbon in the periodic table, and more preferably one or more metal elements selected from the group consisting of Group 5 elements and Group 14 elements other than carbon.
[0062] In order to obtain a functional film with even better light-resistant adhesion, the metal element in the primer layer is preferably one or more metal elements selected from the group consisting of Ti, Si, Mo, Nb, and Ta, and more preferably one or more metal elements selected from the group consisting of Si, Nb, and Ta.
[0063] The primer layer may contain small amounts of elements such as hydrogen, nitrogen, and argon that are taken in from the raw materials used during film formation, the resin film, and the external environment. In the primer layer, the content of elements other than carbon, oxygen, and metal elements is preferably 3 atomic % or less, more preferably 1 atomic % or less, and even more preferably 0.5 atomic % or less. The total content of carbon, oxygen, and metal elements among the elements constituting the primer layer is preferably 90 atomic % or more, more preferably 95 atomic % or more, and even more preferably 97 atomic % or more, and may be 99 atomic % or more, 99.5 atomic % or more, or 99.9 atomic % or more.
[0064] In order to obtain a functional film having excellent light-resistant adhesion, the thickness of the primer layer is preferably 0.1 nm or more, more preferably 0.5 nm or more, and even more preferably 1.0 nm or more. In order to fully exhibit the functions of the functional inorganic layer, the thickness of the primer layer is preferably 20 nm or less, and more preferably 15 nm or less.
[0065] The method for forming the primer layer is not particularly limited, and may be a dry coating method or a wet coating method, but dry coating methods such as vacuum deposition, CVD, and sputtering are preferred because they can form a thin film with a uniform thickness. Furthermore, in order to obtain a functional film with superior light-resistant adhesion, the primer layer is preferably formed by a sputtering method. That is, in order to obtain a functional film with superior light-resistant adhesion, the primer layer is preferably a sputtered layer.
[0066] [Functional Inorganic Layer] Examples of the functional inorganic layer include an anti-reflection layer, a gas barrier layer, and a transparent conductive layer. The elemental composition of the functional inorganic layer is not particularly limited and can be adjusted appropriately depending on the application. The thickness of the functional inorganic layer is also not particularly limited and can be adjusted appropriately depending on the application. Hereinafter, a detailed description will be given using an example in which the functional inorganic layer is an anti-reflection layer.
[0067] (Antireflection Layer) The antireflection layer is preferably composed of two or more thin films with different refractive indices. Generally, the optical film thickness (product of refractive index and thickness) of the thin films of the antireflection layer is adjusted so that the reversed phases of incident light and reflected light cancel each other out. By making the antireflection layer a multilayer laminate of two or more thin films with different refractive indices, the reflectance can be reduced over a wide wavelength range of visible light.
[0068] Examples of materials for the thin film constituting the antireflection layer include metal (or semimetal) oxides, nitrides, fluorides, etc. The antireflection layer is preferably an alternate laminate of high refractive index layers and low refractive index layers.
[0069] The high refractive index layer has a refractive index of, for example, 1.9 or more, preferably 2.0 or more. Examples of materials for the high refractive index layer include titanium oxide and niobium oxide (Nb 2 O 5 Examples of the material for the low refractive index layer include silicon oxide (SiO ), zirconium oxide, tantalum oxide, zinc oxide, indium oxide, indium tin oxide (ITO), antimony-doped tin oxide (ATO), etc. Among these, one or more materials selected from the group consisting of titanium oxide and niobium oxide are preferred. The refractive index of the low refractive index layer is, for example, 1.6 or less, and preferably 1.5 or less. Examples of the material for the low refractive index layer include silicon oxide (SiO 2 Examples of such a thin film include titanium nitride, magnesium fluoride, barium fluoride, calcium fluoride, hafnium fluoride, and lanthanum fluoride. Among these, silicon oxide is preferred. In particular, it is preferred to alternately stack niobium oxide thin films as high-refractive index layers and silicon oxide thin films as low-refractive index layers. In addition to the low-refractive index layer and the high-refractive index layer, a medium-refractive index layer having a refractive index of more than 1.6 and less than 1.9 may be provided.
[0070] The thickness of each of the high refractive index layer and the low refractive index layer is preferably 5 nm or more and 200 nm or less, and more preferably 10 nm or more and 150 nm or less. The thickness of each layer may be designed so that the reflectance of visible light is reduced depending on the refractive index, the layer structure, etc. For example, the layer structure of the high refractive index layer and the low refractive index layer may be a four-layer structure consisting of, from the primer layer side, a high refractive index layer with an optical thickness of 20 nm or more and 55 nm or less, a low refractive index layer with an optical thickness of 25 nm or more and 55 nm or less, a high refractive index layer with an optical thickness of 80 nm or more and 250 nm or less, and a low refractive index layer with an optical thickness of 100 nm or more and 150 nm or less.
[0071] When the antireflection layer is a four-layer alternating laminate in which niobium oxide thin films as high refractive index layers and silicon oxide thin films as low refractive index layers are alternately laminated, the antireflection layer may be configured to include, from the primer layer side, a niobium oxide thin film having a thickness of 5 nm to 20 nm, a silicon oxide thin film having a thickness of 10 nm to 40 nm, a niobium oxide thin film having a thickness of 65 nm to 120 nm, and a silicon oxide thin film having a thickness of 60 nm to 100 nm, in this order.
[0072] In order to obtain a functional film having excellent flex resistance, the thickness of the antireflection layer is preferably 140 nm or more and 280 nm or less, more preferably 170 nm or more and 280 nm or less, even more preferably 180 nm or more and 260 nm or less, and even more preferably 190 nm or more and 250 nm or less. In this specification, the "thickness of the antireflection layer" refers to the sum of the thicknesses of the layers constituting the antireflection layer (total thickness).
[0073] [Preferred Embodiments of Functional Film] In order to obtain a functional film with even better light-resistant adhesion, the functional film F1 preferably satisfies the following condition 1, more preferably satisfies the following condition 2, and even more preferably satisfies the following condition 3. Condition 1: The carbon content in the primer layer is 20 atomic % or more and 70 atomic % or less, and the metal element content in the primer layer is 12 atomic % or more and 50 atomic % or less. Condition 2: The above condition 1 is satisfied, and the total content of carbon and metal elements in the primer layer is 50 atomic % or more and 90 atomic % or less, relative to 100 atomic % of the total of carbon, oxygen, and metal elements. Condition 3: The above condition 2 is satisfied, and the oxygen content in the primer layer is 35 atomic % or less, relative to 100 atomic % of the total of carbon, oxygen, and metal elements.
[0074] Second Embodiment: Functional Film Next, a functional film according to a second embodiment of the present invention (hereinafter, sometimes referred to as "functional film F2") will be described. In the following description, the description of the same content as in the first embodiment may be omitted. The following description will focus on the differences from the first embodiment (functional film F1).
[0075] The functional film F2 is a laminate having a resin film substrate, a functional inorganic layer, and a primer layer interposed between the resin film substrate and the functional inorganic layer. The primer layer of the functional film F2 is a sputtered layer and contains carbon, oxygen, and metal elements as constituent elements. By having the above-mentioned configuration, the functional film F2 has excellent light-resistant adhesion.
[0076] The functional film F2 is not particularly limited as long as it satisfies the above-described configuration. However, in the second embodiment, in order to obtain a functional film having better light-resistant adhesion, it is preferable that the carbon content and the metal element content in the primer layer are both 10 atomic % or more.
[0077] Other aspects of the second embodiment are the same as those described above in the section <First embodiment: functional film>.
[0078] <Third embodiment: manufacturing method of functional film> Next, a manufacturing method of a functional film according to a third embodiment of the present invention will be described. The manufacturing method of a functional film according to the third embodiment is a suitable manufacturing method for the functional film F2 according to the second embodiment described above. In the following description, the description of the same content as in the first and second embodiments may be omitted.
[0079] The method for producing a functional film according to the third embodiment includes a step of forming a primer layer on one main surface of a resin film substrate by sputtering (primer layer forming step).
[0080] The method for producing a functional film according to the third embodiment may include other steps (other steps) in addition to the primer layer forming step, such as a hard coat layer forming step and a functional inorganic layer forming step, which will be described later.
[0081] Hereinafter, each step included in an example of the method for producing a functional film according to the third embodiment will be described.
[0082] [Hard Coat Layer Forming Step] The hard coat layer forming step is a step of forming a hard coat layer on one main surface of a resin film. For example, a curable resin composition (hard coat layer forming composition) is applied to the resin film, and the solvent is removed and the resin is cured as needed, thereby forming a hard coat layer. The hard coat layer forming composition contains, for example, the above-mentioned curable resin and a polymerization initiator (e.g., a photopolymerization initiator), and, as needed, a solvent capable of dissolving or dispersing these components.
[0083] In addition to the above components, the composition for forming a hard coat layer may contain additives such as microparticles, nanoparticles, leveling agents, viscosity modifiers (thixotropic agents, thickeners, etc.), antistatic agents, antiblocking agents, dispersants, dispersion stabilizers, antioxidants, ultraviolet absorbers, antifoaming agents, surfactants, and lubricants.
[0084] The hard coat layer-forming composition can be applied by any suitable method, such as bar coating, roll coating, gravure coating, rod coating, slot orifice coating, curtain coating, fountain coating, or comma coating. The drying temperature of the applied coating film may be set appropriately depending on the composition of the hard coat layer-forming composition, and is, for example, 50°C or higher and 150°C or lower. When the resin component in the hard coat layer-forming composition is a thermosetting resin, the coating film is cured by heating. When the resin component in the hard coat layer-forming composition is a photocurable resin, the coating film is cured by irradiating it with active energy rays such as ultraviolet light. The integrated light intensity of the irradiated light is preferably 100 mJ / cm. 2 More than 500mJ / cm 2 The following is the result.
[0085] [Primer layer forming process] The primer layer forming process is a process of forming (depositing) a primer layer on a resin film substrate by a dry process. Sputtering is preferred as the dry process. When using sputtering, for example, sputtering may be performed while rotating a film-forming plate in a batch process for small-lot production. Alternatively, a drum roll may be used instead of the film-forming plate, and a film may be formed while transporting the resin film substrate by a roll-to-roll method (roll-to-roll sputtering method). In the sputtering method, film formation is performed while introducing an inert gas such as argon, and optionally a reactive gas such as oxygen, into the film-forming chamber. Note that, in the subsequent functional inorganic layer forming process, when the functional inorganic layer is formed by reactive sputtering while introducing oxygen, oxygen is incorporated into the primer layer in the functional inorganic layer forming process, even if oxygen is not introduced into the film-forming chamber in the primer layer forming process. Therefore, even if oxygen is not introduced into the film formation chamber in the primer layer formation process, the oxygen content in the primer layer can be adjusted by changing the reactive sputtering conditions (target, amount of oxygen introduced, discharge power, etc.) in the functional inorganic layer formation process.
[0086] Furthermore, as a sputtering method, a method using a mixed target containing carbon and a metal element may be adopted, or a dual sputtering method may be adopted in which a first target (e.g., a carbon target) and a second target (e.g., a metal element target) are placed in a film formation chamber at a distance from each other and a film is formed.
[0087] Examples of power sources for performing the sputtering method include DC power sources, AC power sources, RF power sources, and MFAC power sources (AC power sources with a frequency band of several kHz to several MHz). The substrate temperature when performing the sputtering method is not particularly limited as long as it is within a range in which the substrate is durable, but is, for example, −30° C. or higher and 150° C. or lower. The pressure in the film formation chamber when performing the sputtering method can be appropriately set depending on the type of target and the target film thickness of the primer layer, but is, for example, 0.1 Pa or higher and 1.0 Pa or lower.
[0088] The discharge power when employing the dual sputtering method can be set appropriately depending on the type of target and the target film thickness and target composition ratio of the primer layer, and for example, the discharge power applied to the carbon target is 1 W or more and 5000 W or less, and the discharge power applied to the metal element target is 1 W or more and 5000 W or less. The carbon content and metal element content in the primer layer can be adjusted, for example, by changing at least one of the discharge power applied to the carbon target and the metal element target when forming the film by the dual sputtering method and the type of power source.
[0089] [Functional Inorganic Layer Formation Step] In the functional inorganic layer formation step, a functional inorganic layer is formed on the surface of the primer layer. The method for forming the functional inorganic layer is not particularly limited, and may be either a wet coating method or a dry coating method. Dry coating methods such as vacuum deposition, CVD, and sputtering are preferred because they can form thin films with a uniform thickness, and sputtering is more preferred. The sputtering method may be a batch sputtering method or a roll-to-roll sputtering method. When forming an oxide layer as the functional inorganic layer, the oxide layer can be formed by sputtering using either an oxide target or reactive sputtering using a metal (or semimetal) target. When performing sputtering in the functional inorganic layer formation step, the discharge power applied to the target is, for example, 50 W or more and 3000 W or less. Other conditions for performing sputtering in the functional inorganic layer formation step can be appropriately set, for example, among the conditions described above in the [Primer Layer Formation Step].
[0090] Through the above steps, the functional film F2 is obtained. In the third embodiment, the film formation conditions for the primer layer and the functional inorganic layer are appropriately changed, and the carbon content and the metal element content in the primer layer are adjusted to 10 atomic % or more, respectively, to produce the functional film F1.
[0091] <Fourth embodiment: Image display device> Next, an image display device according to a fourth embodiment of the present invention will be described. The image display device according to the fourth embodiment includes an image display panel and a functional film having an anti-reflection layer as a functional inorganic layer, which is arranged on the viewing side of the image display panel. The functional film arranged on the viewing side of the image display panel is functional film F1 or F2 having an anti-reflection layer as a functional inorganic layer. Hereinafter, descriptions of content that overlaps with the first and second embodiments may be omitted.
[0092] Fig. 3 is a cross-sectional view showing an example of an image display device according to a fourth embodiment. The image display device 100 shown in Fig. 3 includes an image display panel 101 and a functional film 20, which is an example of the functional film F1 according to the first embodiment, arranged on the viewing side (upper side in Fig. 3) of the image display panel 101. The functional film 20 includes a multilayer anti-reflection layer as a functional inorganic layer 21. Thus, the functional film 20 in Fig. 3 is an anti-reflection film. Furthermore, in the image display device 100, the resin film 14 of the functional film 20 and the image display panel 101 are bonded together via an adhesive layer 102.
[0093] The adhesive constituting the adhesive layer 102 is not particularly limited, and can be appropriately selected and used from transparent adhesives whose base polymer is, for example, an acrylic polymer, a silicone polymer, polyester, polyurethane, polyamide, polyvinyl ether, a vinyl acetate-vinyl chloride copolymer, a modified polyolefin, an epoxy resin, a fluorine-based resin, natural rubber, synthetic rubber, etc. The thickness of the adhesive layer 102 is not particularly limited, but is preferably 5 μm or more and 100 μm or less from the viewpoint of achieving both a thin layer and adhesiveness.
[0094] The image display panel 101 may be, for example, an image display panel including an image display cell such as a liquid crystal cell or an organic EL cell.
[0095] The image display device according to the fourth embodiment has an anti-reflection film disposed on the viewing side of the image display panel, thereby reducing reflection of external light and providing excellent visibility. In addition, the image display device according to the fourth embodiment has a functional film F1 or F2, providing excellent light resistance.
[0096] Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0097] <Method for measuring arithmetic mean height Sa> First, a method for measuring the arithmetic mean height Sa of the main surface on the primer layer side of the resin film substrate used will be described. Using a resin film substrate before the primer layer was formed as a sample, the three-dimensional surface shape of the surface of the resin film substrate before the primer layer was formed (the surface on which the primer layer was formed) was measured using an atomic force microscope (AFM) under the following conditions, and the arithmetic mean height Sa was obtained in accordance with ISO 25178. Apparatus: "Dimension 3100" manufactured by Bruker Corporation Controller: Nanoscope V Measurement mode: Tapping mode Cantilever: Si single crystal Measurement field of view: 1 μm × 1 μm
[0098] <Preparation of Functional Film of Example 1> [Hard Coat Layer Formation Step] A photopolymerization initiator (IGM Resins' Omnirad 907) and a leveling agent (DIC's GRANDIC PC4100) were added to a butyl acetate solution of UV-curable urethane acrylate (DIC's Luxidia 17-806, solids concentration: 80 wt%). The amounts of the photopolymerization initiator and leveling agent added were 5 parts by weight and 0.03 parts by weight, respectively, per 100 parts by weight of the solids in the butyl acetate solution of urethane acrylate. Butyl acetate was added to the resulting mixture to obtain a resin composition with a solids concentration of 75 wt%. Next, cyclopentanone was added to the resulting resin composition to obtain a hard coat layer-forming composition H1 with a solids concentration of 50 wt%. Next, the hard coat layer-forming composition H1 was applied to one main surface of a TAC film (thickness: 40 μm) to form a coating film. Next, the coating film was dried by heating at a temperature of 100°C for 60 seconds, and then cured by ultraviolet irradiation. When irradiating ultraviolet light, a high-pressure mercury lamp was used as the light source, ultraviolet light with a wavelength of 365 nm was used, and the cumulative light amount was 300 mJ / cm. 2 This resulted in a resin film substrate including a TAC film and a hard coat layer (thickness: 5 μm). The arithmetic mean height Sa of the hard coat layer surface (primer layer-formed surface) of the obtained resin film substrate was 0.5 nm.
[0099] [Primer Layer Formation Step] The resin film substrate obtained by the above procedure was set in a sputtering deposition apparatus, and the deposition chamber was filled with 5.0 × 10 -4 The pressure was reduced to 100 Pa or less. Next, a carbon target was used as the first target, a Si target was used as the second target, and argon gas was used as the film-forming gas, and a primer layer was formed on one main surface of the hard coat layer by a dual-target sputtering method. When forming the film by the dual-target sputtering method, the pressure in the film-forming chamber was maintained at 0.3 Pa at room temperature, and a discharge power of 188 W was applied to the first target from an RF power supply, and a discharge power of 22 W was applied to the second target from a DC power supply.
[0100] [Functional Inorganic Layer Forming Step] Following the primer layer forming step, a functional inorganic layer forming step was carried out. Specifically, a Nb target was used as the target, and argon gas and oxygen gas (introduced volume ratio: Ar / O) were used as the film forming gas. 2 A functional inorganic layer (niobium oxide layer) was formed on the primer layer obtained in the primer layer formation step by a reactive sputtering method using a niobium oxide (NbO) alloy (NbO 2 ) having a molecular weight of 14000 (m / s) and a molecular weight of 14000 (m / s). During the film formation by the reactive sputtering method, a discharge power of 120 W was applied to the Nb target from an RF power supply at room temperature while the pressure in the film formation chamber was maintained at 0.3 Pa.
[0101] Through the above steps, a functional film having a primer layer (thickness: 10 nm) and a functional inorganic layer (thickness: 20 nm) on a resin film substrate was obtained as the functional film of Example 1.
[0102] <Preparation of Functional Films of Example 2, Example 3, and Comparative Examples 1 to 4> The functional films of Example 2, Example 3, and Comparative Examples 1 to 4 were obtained by the same preparation method as Example 1, except that the film-forming conditions for the primer layer and the functional inorganic layer were as shown in Table 1 below. Note that, for Example 3 and Comparative Examples 1 to 4, in which a Si target was used when forming the functional inorganic layer, the volume ratio of argon gas and oxygen gas introduced (Ar / O 2 ) was set to 13 / 5.5.
[0103] <Preparation of Functional Films of Example 4, Example 5, and Comparative Example 6> The functional films of Example 4, Example 5, and Comparative Example 6 were each obtained by the same preparation method as in Example 3, except that the hard coat layer formation step was not performed, a PET film (thickness: 50 μm) was used as the resin film substrate, and the film formation conditions for the primer layer were as shown in Table 1 described below.
[0104] <Preparation of functional film of comparative example 5> A functional film of comparative example 5 was obtained by the same preparation method as in example 3, except that composition H2 for forming a hard coat layer prepared by the following procedure was used instead of composition H1 for forming a hard coat layer, a primer layer was not formed, and the film formation conditions for the functional inorganic layer were as shown in the below-described Table 1. The arithmetic mean height Sa of the hard coat layer surface (primer layer-forming surface) of the resin film substrate used in comparative example 5 was 4.4 nm.
[0105] [Method for preparing hard coat layer-forming composition H2] A methyl ethyl ketone dispersion (Shin-Etsu Silicones Co., Ltd.'s "QSG-30", solids concentration: 30 wt%) of silica particles having a number average primary particle diameter of 30 nm (refractive index at a wavelength of 405 nm: 1.47) was added to and mixed with an ultraviolet-curable acrylic resin composition (DIC Corporation's "GRANDIC PC-1070", refractive index at a wavelength of 405 nm: 1.55) to prepare hard coat layer-forming composition H2. The amount of silica particles added was adjusted so that the amount of silica particles relative to the total solids content of the hard coat layer (total of resin and particles) was 45 wt%.
[0106] <Composition analysis of primer layer> Using an X-ray photoelectron spectrometer equipped with an Ar ion gun ("Quantera SXM" manufactured by ULVAC-PHI, Inc.), composition analysis in the thickness direction of the primer layer was performed by XPS while etching from the functional inorganic layer side of the functional film under the conditions below, and the content of each element (C, O, and metal elements) in the center part in the thickness direction of the primer layer (when half of the total etching time had elapsed) was calculated. The content of each element was calculated using the peak corresponding to the binding energy of each element obtained from the wide scan spectrum.
[0107] [Analysis conditions] X-ray source: Monochrome AlKα X-ray focal spot size: 100 μmφ (15 kV, 25 W) Photoelectron take-off angle: 45° to the sample surface Charge neutralization conditions: Combined use of an electron neutralization gun and an Ar ion gun (neutralization mode) Bond energy correction: Correction of the peak derived from C—C bonds to 285.0 eV Acceleration voltage of Ar ion gun: 1 kV Raster size of Ar ion gun: 2 mm × 2 mm Etching rate of Ar ion gun: 1.2 nm / min (SiO 2 Conversion)
[0108] <Evaluation of Light-Resistant Adhesion> A glass plate was attached to the resin film substrate side of the functional film (the side on which the functional inorganic layer was not formed) via a transparent acrylic adhesive, and the adhesion was measured using a weathering tester (Iwasaki Electric Co., Ltd.'s "Eye Super UV Tester SUV-W161") at a temperature of 85°C, a relative humidity of 45%, and a radiation intensity (integrated illuminance of light with a wavelength of 290 to 450 nm) of 150 W / cm. 2 Under the conditions, the surface of the functional inorganic layer was irradiated with light from a metal halide lamp, and an accelerated light resistance test was performed for 32.5 hours. Next, cuts were made at 1 mm intervals on the surface of the functional inorganic layer of the sample after the accelerated light resistance test, forming a grid of 100 squares. Next, a polyester wiper ("Anticon Gold" manufactured by Sanplatec Co., Ltd.) fixed to a 20 mm square stainless steel jig was slid over the grid (load: 1.5 kg, 1000 reciprocations) while continuously dripping isopropyl alcohol to prevent the surface of the functional inorganic layer from drying. Then, the number of peeled squares was counted, and the light-resistant adhesion was evaluated according to the following criteria. "Peeling" is defined as 0.25 mm per square. 2 This means that peeling of 1 / 4 or more of the area of one square occurred. A: The number of peeled squares was 25 or less. B: The number of peeled squares was 26 or more and 50 or less. C: The number of peeled squares was 51 or more. D: Peeling had already occurred before the cuts were made (peeling occurred due to the accelerated light resistance test).
[0109] When the evaluation result was A or B, it was evaluated as "excellent in light-resistant adhesion." On the other hand, when the evaluation result was C or D, it was evaluated as "not excellent in light-resistant adhesion."
[0110] <Results> For Examples 1 to 5 and Comparative Examples 1 to 6, the film-forming conditions for the primer layer, the film-forming conditions for the functional inorganic layer, the composition of the primer layer, and the evaluation results of light-resistant adhesion are shown in Table 1. In Table 1, a "-" in the column for film-forming conditions for the primer layer means that the target in question was not used. In Table 1, a "-" in the column for composition of the primer layer means that no measurement was performed. In Table 1, the content of each element (C, O, and metal elements) in the column for composition of the primer layer was calculated assuming that the total of C, O, and metal elements is 100 atomic %.
[0111]
[0112] As shown in Table 1, in Examples 1 to 5, the carbon content in the primer layer was 10 atomic % or more, relative to 100 atomic % of the total of carbon, oxygen, and metal elements. In Examples 1 to 5, the metal element content in the primer layer was 10 atomic % or more, relative to 100 atomic % of the total of carbon, oxygen, and metal elements. The primer layers in Examples 1 to 5 were sputtered layers.
[0113] As shown in Table 1, the evaluation results for light-resistant adhesion in Examples 1 to 5 were A. Therefore, the functional films of Examples 1 to 5 were excellent in light-resistant adhesion.
[0114] As shown in Table 1, in Comparative Example 1, the content of metal elements in the primer layer was less than 10 atomic %, relative to 100 atomic % of the total of carbon, oxygen, and metal elements. In Comparative Examples 2 to 4 and 6, no carbon target was used as the material for the primer layer. In Comparative Example 5, no primer layer was formed.
[0115] As shown in Table 1, the evaluation results for light-resistant adhesion in Comparative Examples 1 to 6 were C or D. Therefore, the functional films of Comparative Examples 1 to 6 did not have excellent light-resistant adhesion.
[0116] The above results demonstrate that the present invention can provide a functional film with excellent light-resistant adhesion.
[0117] REFERENCE SIGNS LIST 10, 20 Functional film 11 Resin film substrate 12, 21 Functional inorganic layer 13 Primer layer 14 Resin film 15 Hard coat layer 100 Image display device 101 Image display panel
Claims
1. A functional film having a resin film substrate, a functional inorganic layer, and a primer layer interposed between the resin film substrate and the functional inorganic layer, wherein the primer layer contains carbon, oxygen, and metal elements as constituent elements, the carbon content in the primer layer is 10 atomic % or more relative to a total of 100 atomic % of carbon, oxygen, and the metal elements, and the metal element content in the primer layer is 10 atomic % or more relative to a total of 100 atomic % of carbon, oxygen, and the metal elements.
2. The functional film according to claim 1, wherein the metal element is one or more metal elements selected from the group consisting of Group 4 elements, Group 5 elements, Group 6 elements, and Group 14 elements other than carbon in the periodic table.
3. The functional film according to claim 2, wherein the metal element is one or more metal elements selected from the group consisting of Ti, Si, Mo, Nb and Ta.
4. The functional film according to claim 1, wherein the thickness of the primer layer is 20 nm or less.
5. The functional film according to claim 1, wherein the outermost layer of the resin film substrate on the side of the primer layer is a hard coat layer containing a resin as a main component.
6. The functional film according to claim 5, wherein the amount of particles having a number average primary particle diameter of less than 1.0 μm in the hard coat layer is 10 parts by weight or less per 100 parts by weight of the resin in the hard coat layer.
7. The functional film according to claim 1, wherein the oxygen content in the primer layer is 35 atomic % or less relative to a total of 100 atomic % of carbon, oxygen and the metal elements.
8. The functional film according to claim 1, wherein the arithmetic mean height Sa of the main surface of the resin film substrate facing the primer layer is 4.0 nm or less.
9. A functional film having a resin film substrate, a functional inorganic layer, and a primer layer interposed between the resin film substrate and the functional inorganic layer, wherein the primer layer is a sputtered layer and contains carbon, oxygen, and metal elements as constituent elements.
10. The functional film according to claim 1 or 9, wherein the functional inorganic layer is an anti-reflection layer.
11. A method for producing a functional film according to claim 9, comprising the step of forming the primer layer on one of the main surfaces of the resin film substrate by a sputtering method.
12. An image display device comprising: an image display panel; and the functional film according to claim 10, disposed on the viewing side of the image display panel.
Citation Information
Patent Citations
Method of manufacturing substrate with transparent electrode
JP2011183567A
Thermal spray coated reinforced polymer composites
JP2014111364A
Film deposition method
JP2018193581A
Manufacturing method of optical film
JP2021085760A
Optical laminate and picture display unit
JP2022156882A