Rail and method for manufacturing same
The steel rail composition and controlled cooling method address the issue of rail breakage by optimizing element content and cooling processes, reducing crack formation and propagation, thus enhancing the rail's durability and reducing replacement frequency.
Patent Information
- Application Number
- PCT/JP2024/001017
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-01-16
- Publication Date
- 2024-10-03
AI Technical Summary
Rail breakage from the bottom due to repeated tensile and compressive stresses, leading to increased frequency of rail replacements, as existing methods to control crack formation and propagation are insufficient.
A steel rail composition with specific element percentages (C, Si, Mn, Cr, Al, P, S, V, Cu, Ni, Nb, Mo, B, Ti, Mg, Ca, W, Sb, Sn, Co) and a manufacturing method involving controlled cooling rates after hot rolling to achieve desired 0.2% proof stress, longitudinal residual stress, and stress intensity factor range, thereby suppressing crack occurrence and propagation.
The solution effectively reduces the likelihood and propagation speed of cracks at the rail bottom, enhancing the rail's resistance to breakage and extending its service life by controlling the 0.2% proof stress, longitudinal residual stress, and fatigue crack propagation speed.
Smart Images

Figure JP2024001017_03102024_PF_FP_ABST
Abstract
Description
Rail and manufacturing method thereof
[0001] The present invention relates to a rail and a method for manufacturing the same.
[0002] Compared to other modes of transport, rail transport is highly efficient and environmentally friendly, and efforts are being made to increase transport capacity through measures such as increasing operating speeds, increasing freight car loads, and congested timetables. As a result, the number of wheels passing over rails is also increasing, and repeated tensile and compressive stresses are applied to the rails, causing them to break from the bottom, and the frequency of rail replacement is gradually increasing, becoming a problem. Therefore, there is a growing demand for rail steel that can reduce breakage from the bottom.
[0003] Therefore, various studies have been conducted with the aim of further improving the prevention of breakage from the rail bottom. For example, Patent Document 1 describes a steel rail with a pearlite structure containing 0.65 to 1.40% C, in which pearlite blocks with grain sizes of 1 to 15 μm are present in an area of 0.2 mm2 at least in a region extending from the bottom surface to a depth of 10 mm. 2 More than 200 rails have been disclosed.
[0004] Patent Document 2 discloses a rail in which, after rail rolling, the rail head is accelerated cooled from the austenite region, while the rail bottom surface is accelerated cooled between 800 and 450°C at a cooling rate of 1 to 5°C / sec, resulting in an average pearlite hardness at the rail bottom surface of HB 320 or more.
[0005] Patent Document 3 discloses a rail containing, by mass%, 0.65 to 1.20% C, 0.05 to 2.00% Si, and 0.05 to 2.00% Mn, with the remainder being Fe and unavoidable impurities, in which 97% or more of the head surface and bottom surface are pearlite structures, the surface hardness of the pearlite structure is in the range of Hv 320 to 500, the maximum surface roughness is 180 μm or less, and the ratio of the surface hardness to the maximum surface roughness is 3.5 or more.
[0006] JP 2006-57127 A JP 1-139724 A International Publication No. 2011 / 021582
[0007] According to the rails disclosed in Patent Documents 1 to 3, it is possible to control the structure of the rail bottom portion and increase the strength of the rail bottom portion, but this alone is not sufficient to prevent cracks from occurring in the rail bottom portion or to reduce the rate of crack propagation due to tensile stress, and there is a risk of breakage from the rail bottom portion.
[0008] To prevent rail breakage from the bottom, it is effective to prevent cracks from occurring at the rail bottom and, if a crack exists at the rail bottom, to prevent the crack from propagating when a mechanical load is applied. The present invention was made to solve this problem, and provides a rail that can prevent rail breakage from the bottom by controlling the chemical composition of the rail and by controlling the 0.2% proof stress at the center of the rail bottom, the longitudinal residual stress at the center of the rail bottom, and the crack propagation speed within predetermined ranges, along with a manufacturing method thereof.
[0009] The gist of the present invention is as follows: [1] In mass%, C: 0.60% or more and less than 0.90%, Si: 0.10% or more and 1.20% or less, Mn: 0.10% or more and 1.50% or less, Cr: 0.05% or more and 2.00% or less, Al: 0.0002% or more and 0.005% or less, P: 0% or more and 0.035% or less, S: 0% or more and 0.020% or less, V: 0% or more and 0.30% or less, Cu: 0% or more and 1.0% or less, Ni: 0% or more and 1.0% or less, Nb: 0% or more and 0.05% or less, Mo: 0% or more and 0.5% or less, B: 0% or more and 0.0050% or less, Ti: 0% or more and 0.01% or less, Mg: 0% or more and 0.01% or less, Ca: 0% or more and 0.02% or less, W: 0% or more and 0.10% or less. The steel has a chemical composition containing Sb: 0% or more and 0.05% or less, Sn: 0% or more and 0.05% or less, and Co: 0% or more and 1.0% or less, with the balance being Fe and unavoidable impurities, the 0.2% proof stress at the center of the rail bottom is more than 500 MPa and less than 1100 MPa, the longitudinal residual stress at the center of the rail bottom is less than 200 MPa, and the stress intensity factor range ΔK at the center of the rail bottom is 15 MPa m 1/2 The fatigue crack propagation rate is 5.0×10 -8m / cycle or less, rail. [2] The rail of [1], wherein the composition contains, in mass%, one or more elements selected from the group consisting of V: 0.001% to 0.30%, Cu: 0.001% to 1.0%, Ni: 0.001% to 1.0%, Nb: 0.001% to 0.05%, Mo: 0.001% to 0.5%, B: 0.0001% to 0.0050%, Ti: 0.001% to 0.01%, Mg: 0.0005% to 0.01%, Ca: 0.0005% to 0.02%, W: 0.001% to 0.10%, Sb: 0.001% to 0.05%, Sn: 0.001% to 0.05%, and Co: 0.001% to 1.0%. [3] A method for manufacturing a rail as set forth in [1] or [2], wherein, after hot rolling a steel bloom having the chemical composition as set forth in [1] or [2], the average cooling rate when cooling the center of the rail bottom from the cooling start point T1 to the cooling stop point T2 is set to be 0.4°C / sec or more and 6.0°C / sec or less, and the average cooling rate of the foot toes of both rail bottoms while cooling the center of the rail bottom from the cooling start point T1 to the cooling stop point T2 is equal to or less than the average cooling rate of the center of the rail bottom, wherein T1 is a temperature in the range of 650°C or more and 800°C or less, and T2 is a temperature in the range of 400°C or more and 600°C or less.
[0010] Here, the 0.2% proof stress at the center of the rail bottom, the longitudinal residual stress at the center of the rail bottom, and the stress intensity factor range ΔK at the center of the rail bottom are 15 MPa m 1/2 The fatigue crack propagation rate at each of the above conditions can be a value measured by the method described in the Examples.
[0011] According to the present invention, it is possible to provide a rail and a manufacturing method thereof that can suppress crack occurrence at the rail bottom, and, if a crack exists at the rail bottom, reduce the crack propagation speed when a mechanical load is applied, thereby suppressing breakage from the rail bottom.
[0012] FIG. 1 is a cross-sectional view of a rail; FIG. 2 is a diagram showing the cross-sectional area and thickness of the bottom of a rail; FIG. 3 is a schematic diagram of an example of accelerated cooling in a manufacturing method for a rail; FIG. 4 is a schematic diagram of another example of accelerated cooling in a manufacturing method for a rail; FIG. 5 is a diagram showing the extraction position of a tensile test specimen; FIG. 6 is a diagram showing the dimensions of a tensile test specimen; FIG. 7 is a diagram showing the extraction position of a fatigue crack propagation test specimen; FIG. 8 is a diagram showing the dimensions of a fatigue crack propagation test specimen; FIG. 9 is a diagram showing a method for measuring residual stress by a strain gauge cutting method.
[0013] <Rail Parts> The designations of each rail part in the present invention will be explained with reference to the rail cross-sectional view in Figure 1. In the rail 1 shown in Figure 1, 11 is the head, 12 is the web, and 13 is the bottom (foot). If the width of the rail bottom surface is W, the center of the rail bottom (bottom center) is the center of the width direction of the back surface of the bottom, located 0.5 x W from each end. Furthermore, the rail bottom foot (bottom foot) is located 0.15 x W from each end in the width direction of the back surface of the bottom.
[0014] <Composition of Rail> The composition of the steel rail of the present invention will be described below. In the following description, "%" represents "mass %" unless otherwise specified.
[0015] C: 0.60% or more but less than 0.90% C is an essential element for forming cementite in pearlite structures and ensuring 0.2% yield strength. The 0.2% yield strength improves with increasing C content. If the C content is less than 0.60%, it is difficult to obtain excellent 0.2% yield strength and fracture toughness. Therefore, the C content is set to 0.60% or more, preferably 0.63% or more, and more preferably 0.70% or more. Furthermore, if the C content is 0.90% or more, pro-eutectoid cementite forms at austenite grain boundaries during transformation after hot rolling, and cracks tend to propagate along the formed pro-eutectoid cementite, significantly increasing the crack propagation rate. Therefore, the C content is set to less than 0.90%, preferably 0.89% or less, and more preferably 0.85% or less.
[0016] Si: 0.10% or more and 1.20% or less Si is a deoxidizing agent and a strengthening element for the pearlite structure, and 0.10% or more is required to fully obtain this effect. The Si content is preferably 0.15% or more, more preferably 0.20% or more. If the Si content exceeds 1.20%, martensite structure tends to form, which in turn increases the 0.2% proof stress and the amount of Si oxides increases, significantly increasing the crack propagation rate. Therefore, the Si content is set to 1.20% or less, preferably 1.10% or less, and more preferably 1.00% or less.
[0017] Mn: 0.10% or more and 1.50% or less Mn is an element that strengthens the pearlite structure, and 0.10% or more is required to fully obtain this effect. The Mn content is preferably 0.20% or more, and more preferably 0.30% or more. If the Mn content exceeds 1.50%, the high hardenability of Mn makes it easier for martensite to form, which in turn increases the 0.2% proof stress and significantly increases the rate of crack propagation. Therefore, the Mn content is set to 1.50% or less, preferably 1.40% or less, and more preferably 1.30% or less.
[0018] P: 0% or more and 0.035% or less If P is contained in an amount exceeding 0.035%, the ductility, which is a characteristic of the rail itself, deteriorates. Therefore, the P content is set to 0.035% or less, and preferably 0.020% or less. The lower limit of the P content is not particularly limited and may be 0%, but setting it to less than 0.001% would inevitably increase the steelmaking cost, so the P content can be set to 0.001% or more.
[0019] S: 0% or more and 0.020% or less S is an element that exists in steel mainly in the form of A-type inclusions. If the S content exceeds 0.020%, the amount of these inclusions increases significantly, and at the same time, coarse inclusions are formed, which deteriorates the cleanliness of the rail steel and significantly increases the crack propagation rate of the rail. Therefore, the S content is set to 0.020% or less, preferably 0.015% or less, and more preferably 0.010% or less. The lower limit of the S content is not particularly limited and may be 0%, but if it is less than 0.0005%, steelmaking costs will inevitably increase, so the S content can be set to 0.0005% or more.
[0020] Cr: 0.05% or more and 2.00% or less. Cr increases the pearlite equilibrium transformation temperature and contributes to refinement of lamellar spacing. At the same time, the inclusion of Cr further increases the 0.2% yield strength through solid solution strengthening. Since a Cr content of less than 0.05% does not provide sufficient 0.2% yield strength, the Cr content is set to 0.05% or more, preferably 0.10% or more, and more preferably 0.15% or more. If the Cr content exceeds 2.00%, the hardenability increases and martensite structure is more likely to form, resulting in an increase in 0.2% yield strength and a significant increase in the rate of crack propagation. Therefore, the Cr content is set to 2.00% or less, preferably 1.60% or less, and more preferably 1.40% or less.
[0021] Al: 0.0002% to 0.005% Al is a deoxidizing agent and a strengthening element for pearlite structures, and 0.0002% or more is required to fully obtain this effect. If the Al content exceeds 0.005%, the 0.2% yield strength increases and the amount of Al oxide increases, significantly increasing the speed of crack propagation. Therefore, the Al content is set to 0.0002% to 0.005%.
[0022] In addition to the basic components described above, the chemical composition of the rail of the present invention may optionally contain one or more elements selected from the following: V: 0% to 0.30%, Cu: 0% to 1.0%, Ni: 0% to 1.0%, Nb: 0% to 0.05%, Mo: 0% to 0.5%, B: 0% to 0.0050%, Ti: 0% to 0.01%, Mg: 0% to 0.01%, Ca: 0% to 0.02%, W: 0% to 0.10%, Sb: 0% to 0.05%, Sn: 0% to 0.05%, and Co: 0% to 1.0%. These are optional elements and do not necessarily need to be included, so their lower limits are 0%. However, if these elements are included, their preferred contents are as follows:
[0023] V: 0.001% or more and 0.30% or less V forms carbonitrides in steel, disperses and precipitates in the matrix, and improves fracture toughness by improving 0.2% proof stress. This effect is exhibited when the V content is 0.001% or more. Therefore, when V is added, the V content is preferably 0.001% or more, and more preferably 0.005% or more. On the other hand, when the V content exceeds 0.30%, the 0.2% proof stress increases, and the fracture toughness decreases. Furthermore, the alloy cost increases, which increases the cost of the rail steel. Therefore, when V is added, the V content is preferably 0.30% or less, and more preferably 0.29% or less.
[0024] Cu: 0.001% or more and 1.0% or less Like Cr, Cu is an element that can further increase strength through solid solution strengthening. If the Cu content is less than 0.001%, the effect is small, while if it exceeds 1.0%, Cu cracking is likely to occur. Therefore, if Cu is contained, the Cu content is preferably 0.001% or more and 1.0% or less.
[0025] Ni: 0.001% to 1.0% Ni is an element that can increase strength without degrading ductility. Furthermore, adding Ni in combination with Cu suppresses Cu cracking, so it is desirable to add Ni when Cu is added. A Ni content of less than 0.001% results in little effect, while a Ni content of more than 1.0% increases hardenability, martensite is formed, and the rate of crack propagation tends to increase significantly. Therefore, when Ni is added, the Ni content is preferably 0.001% to 1.0%.
[0026] Nb: 0.001% or more and 0.05% or less Nb is an element that combines with C in steel to precipitate as carbides during and after rolling, improving the 0.2% proof stress and thereby improving fracture toughness. However, if the Nb content is less than 0.001%, the effect is small, and if it is contained in excess of 0.05%, no effect commensurate with the content can be obtained. Therefore, when Nb is contained, the Nb content is preferably 0.001% or more and 0.05% or less.
[0027] Mo: 0.001% to 0.5% Mo is an element that can further increase strength through solid solution strengthening, but at less than 0.001%, this effect is minimal, while at more than 0.5%, hardenability increases, martensite begins to form, and the rate of crack propagation tends to increase significantly. Therefore, when Mo is added, the Mo content is preferably 0.001% to 0.5%.
[0028] B: 0.0001% or more and 0.0050% or less B is an element that precipitates as a nitride and can further increase the strength of a rail through precipitation strengthening. If the B content is 0.0001% or more and less, this effect is small, while if it exceeds 0.0050%, the alloy cost increases. Therefore, if B is added, the B content is preferably 0.0001% or more and 0.0050% or less.
[0029] Ti: 0.001% or more and 0.01% or less Ti is an element that precipitates as carbide, nitride, or carbonitride, and can further increase the strength of rails through precipitation strengthening. If the Ti content is less than 0.001%, the effect is small, while if it exceeds 0.01%, the alloy cost increases. Therefore, if Ti is added, the Ti content is preferably 0.001% or more and 0.01% or less.
[0030] Mg: 0.0005% or more and 0.01% or less Mg is an element that combines with oxygen to precipitate MgO, thereby further increasing strength. If the Mg content is less than 0.0005%, this effect is small, while if it exceeds 0.01%, the increase in MgO tends to significantly increase the speed of crack propagation. Therefore, if Mg is added, the Mg content is preferably 0.0005% or more and 0.01% or less.
[0031] Ca: 0.0005% or more and 0.02% or less Ca is an element that combines with oxygen to precipitate CaO, thereby further increasing strength. If the Ca content is less than 0.0005%, the effect is small, while if it exceeds 0.02%, the increase in CaO tends to significantly increase the speed of crack propagation. Therefore, if Ca is added, the Ca content is preferably 0.0005% or more and 0.02% or less.
[0032] W: 0.001% or more and 0.10% or less W is an element that precipitates as carbide and can further increase the strength of rails through precipitation strengthening. If the W content is less than 0.001%, this effect is small, while if it exceeds 0.10%, the alloy cost increases. Therefore, if W is added, the W content is preferably 0.001% or more and 0.10% or less.
[0033] Sb: 0.001% or more and 0.05% or less Sb has a significant effect of preventing decarburization of steel during reheating of rail billets in a heating furnace before hot rolling. If the Sb content exceeds 0.05%, it has a negative effect on the ductility and toughness of the steel. Therefore, if Sb is contained, the Sb content is preferably 0.05% or less. On the other hand, if Sb is contained, the Sb content is preferably 0.001% or more in order to exert the effect of reducing the decarburized layer.
[0034] Sn: 0.001% or more and 0.05% or less Sn is an element that has a significant effect of preventing decarburization of steel during reheating of rail billets in a heating furnace before hot rolling. If the Sn content exceeds 0.05%, it has a negative effect on the ductility and toughness of the steel. Therefore, if Sn is contained, the Sn content is preferably 0.05% or less. On the other hand, if Sn is contained, the Sn content is preferably 0.001% or more in order to exert the effect of reducing the decarburized layer.
[0035] Co: 0.001% or more and 1.0% or less Co is an element that can further increase the strength of steel by increasing the pearlite equilibrium transformation temperature and reducing lamellar spacing. Co also has the effect of suppressing the precipitation of proeutectoid cementite. If the Co content exceeds 1.0%, martensite will form in the steel, resulting in a decrease in ductility. For these reasons, if the composition contains Co, the Co content is preferably 1.0% or less. There is no particular lower limit for the Co content, but for high strength, it is preferably 0.001% or more. A more preferred range of Co content is 0.001 to 0.5%.
[0036] The chemical composition of the steel for rails of the present invention, other than the above-mentioned essential and optional elements, consists of Fe and unavoidable impurities. Examples of unavoidable impurities include N and O, with N content up to 0.008% and O content up to 0.004%. Depending on the raw materials, materials, and manufacturing equipment, impurities other than N and O may be unavoidably mixed into the steel. Examples of raw materials include iron ore, reduced iron, and scrap. The above impurities are also acceptable within the scope of the present invention, provided they do not impair the objectives of the present invention. Examples of impurities other than N and O include Pb, Zr, Bi, Zn, Se, As, Te, Tl, Cd, Hf, Ag, Hg, Ga, Ge, and REM.
[0037] <Rail Microstructure> In the microstructure of the rail of the present invention, pearlite accounts for 95% or more of the area of the rail bottom. The remaining structure other than pearlite is permissible as long as its total area ratio is 5% or less, as this does not significantly affect the properties of the present invention. Examples of the remaining structure include ferrite and bainite. The microstructure can be identified by the method described in the Examples.
[0038] <0.2% yield strength at the center of the rail bottom is more than 500 MPa and less than 1100 MPa> The rail of the present invention has a 0.2% yield strength at the center of the rail bottom that is more than 500 MPa and less than 1100 MPa. If the 0.2% yield strength is 500 MPa or less, resistance to crack initiation when a wheel passes over it is weak, making cracks more likely to occur at the rail bottom due to stress generated within the rail. On the other hand, if the 0.2% yield strength is 1100 MPa or more, the strength of the rail bottom becomes too high, which in turn increases susceptibility to crack growth after initiation and makes the rail more susceptible to breakage. Therefore, the 0.2% yield strength at the center of the rail bottom is set to more than 500 MPa, preferably 550 MPa or more. Furthermore, the 0.2% yield strength at the center of the rail bottom is set to less than 1100 MPa, preferably 1000 MPa or less.
[0039] <Stress intensity factor range ΔK at the center of the rail bottom is 15 MPa m 1/2 The fatigue crack propagation rate is 5.0×10 -8 m / cycle or less> The rail of the present invention has a stress intensity factor range ΔK of 15 MPa m 1/2The fatigue crack propagation rate is 5.0×10 -8 m / cycle or less. The stress intensity factor range ΔK is 15 MPa m 1/2 The fatigue crack propagation rate (hereinafter referred to as the fatigue crack propagation rate) is 5.0 × 10 -8 If the fatigue crack propagation rate exceeds 5.0×10 m / cycle, the crack propagation rate at the rail base is too fast, increasing the possibility of the rail breaking before regular inspection or replacement. -8 m / cycle or less, preferably 4.8 × 10 -8 The lower limit of the fatigue crack propagation rate at the center of the rail bottom is not particularly limited, but from the viewpoint of the lamellar spacing that can be industrially refined, it is set to 1.0 × 10 -8 m / cycle or more.
[0040] <Longitudinal residual stress at the center of the rail bottom of less than 200 MPa> The rail of the present invention has a longitudinal residual stress at the center of the rail bottom of less than 200 MPa. If the residual stress at the center of the rail bottom is less than 200 MPa, it becomes easier to avoid situations in which a large tensile residual stress acts on the rail bottom, accelerating the rate of fatigue crack growth and leading to rail breakage. The residual stress at the center of the rail bottom is more preferably 150 MPa or less. On the other hand, while strong compressive residual stress can be obtained by cooling the rail bottom to a lower temperature, this actually reduces production efficiency, so the residual stress at the center of the rail bottom of -100 MPa or more is preferred.
[0041] <Rail Shape> The shape of the rail in the present invention is not particularly limited, and may be any of the rail shapes described in JIS E 1101:2001, BS EN13674-1:2011, American Railway Engineering and Maintenance-of-Way Association (AREMA), etc.
[0042] <Rail Manufacturing Method> The rail manufacturing method of the present invention will be described. The rail of the present invention is prepared by hot-rolling a bloom having the above-described chemical composition, followed by cooling the rail bottom center from the cooling start point T1 to the cooling stop point T2 at an average cooling rate of 0.4°C / sec to 6.0°C / sec. The average cooling rate at the foot toes of both rail bottoms during cooling the rail bottom center from the cooling start point T1 to the cooling stop point T2 is equal to or less than the average cooling rate at the rail bottom center. Here, the cooling start point T1 is a temperature in the range of 650°C to 800°C. The cooling start point T1 and the cooling stop point T2 are surface temperatures at the rail bottom center measured with a radiation thermometer. The average cooling rate at the rail bottom center is the difference between the cooling start point T1 and the cooling stop point T2 at the rail bottom center divided by the time required for cooling. The average cooling rate of the rail bottom base toes is calculated by dividing the difference in surface temperature at each rail bottom base toe measured with a radiation thermometer at the points corresponding to the cooling start point T1 and the cooling stop point T2 at the rail bottom center by the time required to cool the rail bottom center to the cooling start point T1 and the cooling stop point T2. The two rail bottom toes are usually cooled so that their thermal histories are the same. The temperatures of the rail bottom toes corresponding to the cooling start point T1 and the cooling stop point T2 at the rail bottom center are usually the same, and the average cooling rate of each rail bottom toe is also usually the same.
[0043] (Hot Rolling) The steel blooms used as rail materials have the above-mentioned rail composition and can be produced by any method. They can be produced by casting, particularly continuous casting. For example, steel can be melted in a converter or electric furnace, and if necessary, subjected to secondary refining such as degassing to adjust the steel composition to the above-mentioned ranges. The melted steel can then be continuously cast into a cast steel.
[0044] It is preferable to heat the slab before subjecting it to hot rolling. For example, the slab can be heated to 1200°C or higher and 1350°C or lower in a heating furnace and then hot rolled. In the hot rolling process, hot rolling can be performed using a breakdown rolling mill, a roughing rolling mill, or a finishing rolling mill. In this hot rolling process, the austenite grains that have become coarse due to heating can be refined by rolling and recrystallization in the recrystallization temperature range, or by introducing strain in the non-recrystallization temperature range, thereby refining the structure after pearlite transformation.
[0045] In order to refine the structure after pearlite transformation, the rolling end temperature of the bottom (foot) portion in hot rolling is preferably set to 800°C or higher and 1000°C or lower.
[0046] Furthermore, hot rolling is preferably performed so that the area reduction rate of the bottom portion when rolling at 1050°C or below is 11% or more, more preferably 13% or more. The area reduction rate can be 20% or less, preferably 18% or less. Here, the area reduction rate at 1050°C or below is a value calculated by the equation area reduction rate (%) = {(S0 - S1) / S0} × 100, where S0 is the cross-sectional area of the bottom portion when the temperature drops to 1050°C or below, and S1 is the cross-sectional area of the bottom portion after finish rolling. In the final rolling pass, the thickness reduction rate (thickness reduction rate) of the bottom portion is preferably the same as or greater than the area reduction rate of that pass. For example, if the area reduction rate in finish rolling is 11%, the thickness reduction rate at the center of the bottom portion during finish rolling can be 15% or more. This allows for the introduction of large strain into the bottom portion, further promoting the refinement of the structure after pearlite transformation, and effectively increasing the fatigue strength of the back surface of the bottom portion. By designing the groove so that the width dimension of the bottom portion is widened in this finish rolling, rolling can be stably performed in which the thickness reduction rate in finish rolling is relatively large compared to the area reduction rate in finish rolling. The difference between the thickness reduction rate and the area reduction rate in finish rolling (thickness reduction rate - area reduction rate) is preferably 4% to 8%, more preferably 5% to 7%. Here, the thickness reduction rate in finish rolling is a value calculated by the following equation: thickness reduction rate (%) = {(H0 - H1) / H0} × 100, where H0 is the thickness of the bottom portion before finish rolling and H1 is the cross-sectional area of the bottom portion after finish rolling. Note that the finish rolling referred to here refers to one pass of final rolling performed using the final rolling groove of one final rolling mill. By performing finish rolling under these conditions, the 0.2% proof stress of the bottom portion is more than 500 MPa and less than 1100 MPa, and the stress intensity factor range ΔK of the rail bottom portion is 15 MPa m 1 / 2 The fatigue crack propagation rate is 5.0×10 -8This condition is also effective in achieving a longitudinal residual stress of less than 200 MPa at the width center of the rail bottom surface. Here, the cross-sectional area of the rail bottom is the area of the shaded area marked S in the rail cross-sectional view in Figure 2, and the thickness of the rail bottom is the height marked H in the same figure.
[0047] Other hot rolling conditions are not particularly limited.
[0048] (Accelerated Cooling) In the manufacturing method of the present invention, accelerated cooling is performed after hot rolling at the center of the rail bottom and the foot toes of the rail bottom so as to achieve a predetermined average cooling rate.
[0049] The cooling start point T1 of accelerated cooling is a temperature in the range of 650°C to 800°C. If the cooling start temperature is below 650°C, the pearlite transformation temperature will increase and the 0.2% proof stress will decrease. On the other hand, if cooling is performed from above 800°C, martensite is more likely to form at the bottom of the rail, which will increase the 0.2% proof stress and tend to accelerate the crack propagation rate. For this reason, the cooling start temperature is set to 650°C to 800°C.
[0050] The cooling stop point T2 is a temperature in the range of 400°C to 600°C. If the cooling stop temperature is below 400°C, cooling will continue even after pearlite transformation is complete, increasing the cooling time and reducing productivity. On the other hand, if the cooling stop temperature is above 600°C, cooling will be stopped before pearlite transformation is complete, resulting in a decrease in 0.2% yield strength. Therefore, the cooling stop temperature is set to 400°C to 600°C.
[0051] The average cooling rate from the cooling start point T1 to the cooling end point T2 is 0.4°C / s or more and 6.0°C / s or less. If the average cooling rate is less than 0.4°C / s, the 0.2% proof stress of the rail base decreases, the tensile residual stress increases, and the fatigue crack growth rate increases. On the other hand, if the average cooling rate exceeds 6.0°C / s, the 0.2% proof stress of the rail base increases, and the fatigue crack growth rate increases. Therefore, the average cooling rate during accelerated cooling is preferably 0.4°C / s or more and 6.0°C / s or less, and more preferably 0.4°C / s or more and 2.9°C / s or less.
[0052] The rail bottom center is thicker than the other parts of the rail, making it more susceptible to heat accumulation. This means that when cooling is completed and the temperature returns to room temperature, large longitudinal tensile residual stresses tend to develop in the rail bottom center, potentially increasing the rate of fatigue crack propagation in the rail bottom. To prevent this, the manufacturing method of the present invention effectively cools the rail bottom center more intensely than the thinner base toe parts of the rail bottom, thereby ensuring that the average cooling rate at the rail bottom center is equal to or greater than the corresponding average cooling rate at each base toe. From this perspective, the average cooling rates at both base toes of the rail from the cooling start point T1 to the cooling stop point T2 at the rail bottom center are set to be equal to or less than the cooling rate at the rail bottom center. The average cooling rate at each base toe of the rail is preferably between 0.4°C / s and 2.5°C / s. It is preferable that the average cooling rate at the center of the rail bottom is V1, and the average cooling rate at the toe of each rail bottom is (V1-0)°C / sec to (V1-1.5) / sec°C.
[0053] The accelerated cooling method is not particularly limited, and may be, for example, a cooling method using online heat treatment equipment. The cooling medium is not particularly limited, and may be one or more selected from air, spray water, mist, etc., but air is preferably used.
[0054] To ensure that the average cooling rates of the rail bottom center and the rail bottom foot tips satisfy predetermined conditions, the rail bottom center can be cooled more aggressively than the rail bottom foot tips. For example, as shown in Figure 3, a nozzle 21 can be used to directly spray the coolant onto an area that is 1 / 5 of the rail bottom width W (0.2 times W) on either side of the rail bottom center, while other areas of the rail bottom, such as the rail bottom foot tips, are cooled by the coolant flowing along the bottom surface. In Figure 3, the area directly sprayed by the coolant is set to 1 / 5 of the rail bottom width W, but the range can be changed to approximately 0.1 to 0.5 times W by selecting the appropriate nozzle. Another effective method is to spray the coolant from the rail web side toward the rail bottom center using a nozzle 22, as shown in Figure 4.
[0055] The cooling of other portions of the rail (for example, the rail head) is not particularly limited, and may be allowed to cool naturally or may be subjected to accelerated cooling.
[0056] (Others) After cooling, the rail material may be subjected to known treatments, for example, cold roller straightening.
[0057] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0058] A billet having the chemical composition shown in Table 1 was heated to 1250°C and then hot-rolled into a rail shape at the finishing rolling temperature shown in Table 2. The rail shape was a 60 kg rail shape specified in JIS E 1101:2001. The area reduction ratio of the base during rolling at 1050°C or less was set to the value shown in Table 2. For the final rolling pass, the thickness reduction ratio (thickness reduction ratio) of the base was set to 15% or more, which was greater than the area reduction ratio of the corresponding pass, as described above. The rail was then transported to an online heat treatment facility, where the center of the rail base was cooled at the average cooling rate shown in Table 2. The rail was then transported to a cooling bed and allowed to cool to room temperature. The base was cooled by intensively spraying refrigerant from appropriately selected air nozzles over an area of 0.1 × W to 0.5 × W, with respect to the base width W, so as to sandwich the center of the rail base, as shown in Figure 3. However, in Test No. For Tests 31, 41, and 46, the coolant was sprayed over almost the entire surface of the rail base. For Tests 3, 4, 9, 10, 11, 20, 21, and 47, cooling was also performed from the rail bottom side, as shown in Figure 4. The cooling start and stop points in Table 2 refer to the surface temperatures measured using a two-dimensional radiation thermometer, which can measure the temperature distribution at the center of the rail base. The average cooling rate is the average cooling rate between these temperatures. The average cooling temperature at the rail base tip was calculated by measuring the temperature at one rail base tip (0.15 × W from one end) using a spot thermometer and dividing the temperature by the accelerated cooling time. Because the cooling conditions at the rail base were uniform across the rail center, the measured value at one rail base tip was used.
[0059]
[0060]
[0061] The rails obtained as described above were subjected to a tensile test, a fatigue crack propagation test, a residual stress test and a fatigue test in the following manner.
[0062] <Tensile test> As shown in Figure 5, tensile test specimens were taken from a position including the center of the rail bottom, and tensile tests were conducted in accordance with JIS Z2241. The shape of the test specimen is shown in Figure 6. After the tensile test, the 0.2% proof stress was determined.
[0063] <Fatigue crack propagation test> As shown in Figure 7, test specimens for fatigue crack propagation tests were taken from positions including the center of the rail bottom. The shape of the test specimen is shown in Figure 8. In Figure 8, the test specimen is, for example, a plate-like specimen with a width W = 20 mm, a length H = 100 mm, and a thickness B = 5 mm, and a notch is provided in the center (H / 2) of the length H, with a length L = 2 mm, a width C = 0.2 mm, and a curvature R = 0.1 mm at the end of the notch. Using this test specimen, a fatigue crack propagation test was carried out under the condition of a stress ratio R = 0.1, and ΔK = 15 MPa m 1 / 2 The fatigue crack propagation rate da / dN (m / cycle) was measured.
[0064] <Residual Stress Test> The residual stress of the rail was measured using the strain gauge cutting method. Specifically, a 2-m-long rail was sampled, and a strain gauge with a gauge length of 3 mm, a resistance of 120 Ω, and a gauge factor of 2 was attached to the width center of the bottom surface of the rail, as shown in Figure 9, at a position 1 m from the center in the longitudinal direction, to measure the initial strain. Next, the rail was sawed at the position shown in Figure 9, and the strain after sawing was measured. The residual stress in the longitudinal direction of the rail was calculated from the change in strain before and after sawing. If the residual stress in the longitudinal direction of the rail was less than 200 MPa, the residual stress was determined to be good.
[0065] <Fatigue Test> The fatigue test was evaluated as follows. The obtained rails were cut into 1500 mm lengths and subjected to repeated three-point bending tests using a Mayekawa Testing Machinery Mfg. Co., Ltd. "Pulsator 250PUS" in a head-up position, with the rail head facing up and the rail bottom facing down. Specifically, three-point bending was performed 3.5 million times under the following conditions: test load: 1000 kN, repetition rate: 600 rpm, and bending support interval: 1000 mm, and the presence or absence of fractures was confirmed visually. In addition, for rails that did not fracture (unfractured rails), the presence or absence of cracks at the rail bottom was confirmed visually after the fatigue test. Unfractured rails were judged to have good fatigue properties and were therefore rails that could suppress breakage from the rail bottom. In particular, rails without visible cracks were considered to have excellent properties.
[0066] <Microstructure> Test specimens for microstructural observation were cut from a manufactured rail at a position including the center of the rail bottom, based on a depth of 1 mm from the surface. After mirror polishing, they were etched with 1% nitric acid alcohol (1% Nital) and microstructural observation was carried out using an optical microscope at 100x magnification (one field of view 1200 μm × 950 μm, 10 fields of view). If any structures other than pearlite were present, they were photographed. The structures other than pearlite were traced on the photographed structure, and the image analysis software Image-Pro (Nippon Roper Co., Ltd.) was used to calculate the fraction of structures other than pearlite according to the following formula: Fraction of structures other than pearlite = {(area other than pearlite) / (area of pearlite + area of structures other than pearlite)} × 100
[0067] As can be seen from Table 2, the rails of the invention examples all had a 0.2% proof stress at the center of the rail bottom of more than 500 MPa and less than 1100 MPa, a longitudinal residual stress at the center of the rail bottom of less than 200 MPa, and a stress intensity factor range ΔK at the center of the rail bottom of less than 15 MPa m 1 / 2 The fatigue crack propagation rate at this temperature was 5.0×10-8 m / cycle or less, indicating that the material has good properties.
[0068] According to the present invention, it is possible to provide a rail and a manufacturing method thereof that can suppress crack occurrence at the rail bottom, and, if a crack exists at the rail bottom, reduce the crack propagation speed when a mechanical load is applied, thereby suppressing breakage from the rail bottom.
[0069] REFERENCE SIGNS LIST 1 rail 11 head 12 abdomen 13 bottom (foot) 21 nozzle 22 nozzle P center Center of rail bottom P end Rail bottom foot
Claims
1. By mass, C: 0.60% or more but less than 0.90%, Si: 0.10% or more but less than 1.20%, Mn: 0.10% or more but less than 1.50%, Cr: 0.05% or more but less than 2.00%, Al: 0.0002% or more but less than 0.005%, P: 0% or more but less than 0.035%, S: 0% or more but less than 0.020%, V: 0% or more but less than 0.30%, Cu: 0% or more but less than 1.0%, Ni: 0% or more but less than 1.0%, Nb: 0% or more but less than 0.05%, Mo: 0% or more but less than 0.5%, B: 0% or more but less than 0.0050%, Ti: 0% or more but less than 0.01%, Mg: 0% or more but less than 0.01%, Ca: 0% or more but less than 0.02%, W: 0% or more but less than 0.10%, The steel has a chemical composition containing Sb: 0% or more and 0.05% or less, Sn: 0% or more and 0.05% or less, and Co: 0% or more and 1.0% or less, with the balance being Fe and unavoidable impurities, the 0.2% proof stress at the center of the rail bottom is more than 500 MPa and less than 1100 MPa, the longitudinal residual stress at the center of the rail bottom is less than 200 MPa, and the stress intensity factor range ΔK at the center of the rail bottom is less than 15 MPa m 1/2 The fatigue crack propagation rate at -8 m / cycle or less on rail.
2. A rail as claimed in claim 1, wherein the composition contains, by mass, one or more elements selected from the group consisting of V: 0.001% or more and 0.30% or less, Cu: 0.001% or more and 1.0% or less, Ni: 0.001% or more and 1.0% or less, Nb: 0.001% or more and 0.05% or less, Mo: 0.001% or more and 0.5% or less, B: 0.0001% or more and 0.0050% or less, Ti: 0.001% or more and 0.01% or less, Mg: 0.0005% or more and 0.01% or less, Ca: 0.0005% or more and 0.02% or less, W: 0.001% or more and 0.10% or less, Sb: 0.001% or more and 0.05% or less, Sn: 0.001% or more and 0.05% or less, and Co: 0.001% or more and 1.0% or less.
3. A method for manufacturing a rail as claimed in claim 1 or 2, comprising the steps of: hot rolling a steel slab having the chemical composition as claimed in claim 1 or 2; cooling the center of the rail bottom from the cooling start point T1 to the cooling stop point T2 at an average cooling rate of 0.4°C / sec or more and 6.0°C / sec or less; and the average cooling rate of both rail bottom toes during the cooling of the center of the rail bottom from the cooling start point T1 to the cooling stop point T2 is equal to or less than the average cooling rate of the center of the rail bottom, wherein T1 is a temperature in the range of 650°C to 800°C, and T2 is a temperature in the range of 400°C to 600°C.
Citation Information
Patent Citations
Heat treatment for steel rail excellent in falling load-resisting characteristic
JP1989139724A
Pearlitic rail having excellent drop fracture resistance
JP2006057127A
Pearlite rail
WO2011021582A1
High-ductility and alpine-cold railway steel rail and production method thereof
CN112239831A
Method for controlling high-performance steel rail bottom center residual stress
CN112676347A