Method for producing positive electrode composition and method for producing positive electrode
The method of optimizing carbon black and carbon nanotube distribution in the positive electrode composition of lithium ion batteries addresses conductivity issues, resulting in batteries with low internal resistance and superior discharge rate characteristics.
Patent Information
- Application Number
- PCT/JP2024/001445
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-01-19
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium ion secondary batteries face challenges in achieving low internal resistance and excellent discharge rate characteristics due to poor conductivity of the positive electrode active material, which leads to reduced discharge capacity and shortened battery life, despite the use of conductive materials like carbon black and carbon nanotubes.
A method for manufacturing a positive electrode composition involving a slurry with carbon black and carbon nanotubes, where the particle size distribution of carbon black is optimized to enhance conductivity, and the carbon black and carbon nanotubes are efficiently mixed with a binder and active material to form a conductive path, ensuring low internal resistance and improved discharge rate.
The optimized positive electrode composition results in batteries with reduced internal resistance and enhanced discharge rate characteristics, leading to improved performance and extended battery life.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Method for producing positive electrode composition and method for producing positive electrode
[0001] The present invention relates to a method for producing a positive electrode composition and a method for producing a positive electrode.
[0002] In response to growing environmental and energy issues, there has been active development of technologies aimed at realizing a low-carbon society that reduces dependence on fossil fuels. Such technological development is wide-ranging, and includes the development of low-pollution vehicles such as hybrid electric vehicles and electric vehicles, natural energy generation and storage systems such as solar and wind power generation, and next-generation power transmission networks that supply electricity efficiently and reduce transmission losses.
[0003] Batteries are one of the key devices required for these technologies, and they are required to have high energy density to enable system miniaturization. They also need high output characteristics to enable stable power supply regardless of the ambient temperature. They also need good cycle characteristics to withstand long-term use. Therefore, conventional lead-acid batteries, nickel-cadmium batteries, and nickel-metal hydride batteries are rapidly being replaced by lithium-ion secondary batteries, which have higher energy density, output characteristics, and cycle characteristics.
[0004] Conventionally, the positive electrode of a lithium-ion secondary battery is manufactured by coating a current collector with a positive electrode paste containing a positive electrode active material, a conductive material, and a binder. Lithium-containing composite oxides such as lithium cobalt oxide and lithium manganese oxide have been used as the positive electrode active material. Furthermore, because the positive electrode active material has poor electrical conductivity, a conductive material such as carbon black has been added to the positive electrode paste to impart electrical conductivity (see, for example, Patent Document 1).
[0005] JP 2008-227481 A
[0006] In recent years, there has been a demand for further improvements in the performance of lithium-ion secondary batteries.
[0007] The present invention aims to provide a positive electrode composition and a method for producing the same that can realize a battery having low internal resistance and excellent discharge rate characteristics. Another object of the present invention is to provide a positive electrode and a method for producing the same that can realize a battery having low internal resistance and excellent discharge rate characteristics.
[0008] The present invention relates to, for example, the following [1] to [7]. [1] A positive electrode composition comprising: a preparation step of preparing a first slurry containing carbon black and a first liquid medium; and a mixing step of mixing the first slurry with a binder, carbon nanotubes, and an active material to obtain a positive electrode composition, wherein a particle group including secondary particles of the carbon black and tertiary particles formed by aggregation of the secondary particles in the first slurry has a volume-based particle size distribution of D 50 is 0.3 μm or more and 0.9 μm or less, and D 10 and D 90 D for the difference 50 The ratio (D 50 / (D 90 -D 10 )) is 0.2 or more and 0.8 or less. [2] The manufacturing method according to [1], wherein the mixing step includes: a first step of mixing the first slurry, a binder solution containing the binder and a second liquid medium, and a second slurry containing the carbon nanotubes and a third liquid medium to obtain a mixed solution; and a second step of mixing the mixed solution with an active material to obtain the positive electrode composition. [3] The manufacturing method according to [1], wherein the mixing step includes: a first step of mixing the first slurry with a binder solution containing the binder and a second liquid medium to obtain a first mixed solution; a second step of mixing the first mixed solution with a second slurry containing the carbon nanotubes and a third liquid medium to obtain a second mixed solution; and a third step of mixing the second mixed solution with the active material to obtain the positive electrode composition. [4] The manufacturing method according to [1], wherein the carbon black is 2 / g or more 400m 2[5] The manufacturing method according to any one of [1] to [3], wherein the carbon black in the positive electrode composition has a BET specific surface area of 1 / g or less and an average primary particle diameter of 17 nm or more and 30 nm or less. [6] The manufacturing method according to any one of [1] to [4], wherein the content of the carbon black in the positive electrode composition is 40 to 90 mass% based on the total amount of the carbon black and the carbon nanotubes. [7] The manufacturing method according to any one of [1] to [4], wherein the content of the carbon black in the positive electrode composition is 40 to 90 mass% based on the total amount of the carbon black and the carbon nanotubes. [8] The manufacturing method according to any one of [1] to [4], wherein the content of the carbon black in the positive electrode composition is 40 to 90 mass% based on the total amount of the carbon black and the carbon nanotubes. [9] The manufacturing method according to any one of [1] to [4], wherein the content of the carbon black in the positive electrode composition is 40 to 90 mass% based on the total amount of the carbon black and the carbon nanotubes.
[10] The manufacturing method according to any one of [1] to [4], wherein the content of the carbon black in the positive electrode composition is 40 to 90 mass% based on the total amount of the carbon black and the carbon nanotubes.
[11] The manufacturing method according to any one of [1] to [4], wherein the content of the carbon black in the positive electrode composition is 40 to 90 mass% based on the total amount of the carbon black and the carbon nanotubes.
[12] The manufacturing method according to any one of [1] to [4], wherein the content of the carbon black in the positive electrode composition is 40 to 90 mass% based on the total amount of the carbon black and the carbon nanotubes.
[13] The manufacturing method according to any one of [1] to [4], wherein the content of the carbon black in the positive electrode composition is 40 to 90 mass% based on the total 10 is 0.15 μm or more and 0.42 μm or less, and D 90 [7] A method for producing a positive electrode, comprising a step of applying the positive electrode composition produced by the method for producing a positive electrode according to any one of [1] to [6] onto a current collector to form a composite layer containing the carbon black, the carbon nanotubes, the binder, and the active material on the current collector.
[0009] According to the present invention, a positive electrode composition capable of realizing a battery having low internal resistance and excellent discharge rate characteristics, and a method for producing the same are provided. Also, according to the present invention, a positive electrode capable of realizing a battery having low internal resistance and excellent discharge rate characteristics, and a method for producing the same are provided.
[0010] Preferred embodiments of the present invention will be described in detail below.
[0011] [Method for Producing Positive Electrode Composition] The method for producing the positive electrode composition of the present embodiment includes a preparation step of preparing a first slurry containing carbon black and a first liquid medium, and a mixing step of mixing the first slurry, a binder, carbon nanotubes, and an active material to obtain the positive electrode composition.
[0012] In this embodiment, the particle size distribution of the particle group including the secondary particles of carbon black in the first slurry and the tertiary particles formed by aggregation of the secondary particles is D 50 In addition, in the particle size distribution, D 10 and D 90 D for the difference 50 The ratio (D50 / (D 90 -D 10 )) is 0.2 or more and 0.8 or less.
[0013] According to the method for producing a positive electrode composition of this embodiment, a positive electrode composition can be obtained that can realize a battery having low internal resistance and excellent discharge rate characteristics.
[0014] In this embodiment, carbon black and carbon nanotubes function as conductive materials. The basic role of a conductive material is to impart conductivity to a positive electrode active material that has poor conductivity. In addition, in lithium-ion secondary batteries, the positive electrode active material expands and contracts with repeated charge and discharge, gradually losing contact between the positive electrode active materials. The conductive material also plays a role in connecting the positive electrode active materials that have lost contact.
[0015] If the dispersibility of the conductive material in the positive electrode active material is poor, the positive electrode active material and the conductive material cannot be in sufficient contact, making it difficult to form a conductive path, resulting in a problem of not being able to fully utilize the performance of the active material. As a result, areas with poor conductivity appear locally in the positive electrode, which is thought to result in insufficient utilization of the active material, a decrease in discharge capacity, and a shortened battery life. While increasing the content of the conductive material is considered to ensure a conductive path, from the perspective of improving battery characteristics, it is desirable to reduce the content of the conductive material in the positive electrode that does not contribute to charge / discharge capacity and increase the content of the positive electrode active material.
[0016] In the method for producing a positive electrode composition of this embodiment, the carbon black in the first slurry is D 50 and the ratio (D 50 / (D 90 -D 10 )) form particle groups within the above range, the carbon black is efficiently distributed between the active materials and on the surfaces of the active materials, which is thought to more efficiently form conductive paths between the active materials through the cooperation of the carbon black and the carbon nanotubes, thereby achieving both low internal resistance and excellent discharge rate characteristics.
[0017] Each step of the method for producing the positive electrode composition of this embodiment will be described in detail below.
[0018] (Preparation Step) The preparation step is a step of preparing a first slurry containing carbon black and a first liquid medium. 50 and ratio (D 50 / (D 90 -D 10 )) may be mixed so that the total amount of the components falls within the above range to obtain a first slurry.
[0019] <Carbon Black> The carbon black may be any carbon black commonly used as a conductive material for batteries, such as acetylene black, furnace black, channel black, etc. From the viewpoint of excellent purity and ease of obtaining excellent battery characteristics, acetylene black is preferred.
[0020] Carbon black: 100m 2 / g or more 400m 2 Carbon black having a BET specific surface area of 1 / g or less and an average primary particle diameter of 17 nm or more and 30 nm or less is preferred.
[0021] The BET specific surface area of carbon black is, for example, 100 m 2 / g or more, and 2 / g or more, 140m 2 / g or more, or 160m 2 When the BET specific surface area of carbon black is large, the number of electrical contacts with the active material and the conductive material increases, and the conductivity improves, which tends to make it easier to obtain better battery characteristics.
[0022] The BET specific surface area of carbon black is, for example, 500 m 2 / g or less, and 2 / g or less, 400m 2 / g or less, or 350m 2 / g or less. When the BET specific surface area of carbon black is small, the interaction between the liquid medium and the conductive material and the interaction between the conductive materials are small, which makes it easier to mix the active material uniformly, makes it easier to form a strong conductive path, and tends to make it easier to obtain better battery characteristics. That is, the BET specific surface area of carbon black is, for example, 100 m 2 / g or more 500m 2 / g or less, 100m 2 / g or more 450m 2 / g or less, 100m 2 / g or more 400m 2 / g or less, 100m 2 / g or more 350m 2 / g or less, 120m 2 / g or more 500m 2 / g or less, 120m 2 / g or more 450m 2 / g or less, 120m 2 / g or more 400m 2 / g or less, 120m 2 / g or more 350m 2 / g or less, 140m 2 / g or more 500m 2 / g or less, 140m 2 / g or more 450m 2 / g or less, 140m 2 / g or more 400m 2 / g or less, 140m 2 / g or more 350m 2 / g or less, 160m 2 / g or more 500m 2 / g or less, 160m 2 / g or more 450m 2 / g or less, 160m 2 / g or more 400m 2 / g or less, or 160m 2 / g or more 350m 2 / g or less.
[0023] The BET specific surface area of carbon black can be measured by the static volume method in accordance with JIS Z8830 using nitrogen as an adsorbate.
[0024] The average primary particle size of the carbon black may be, for example, 17 nm or more, or 18 nm or more. It is believed that a large average primary particle size of the carbon black reduces the interaction between the liquid medium and the conductive material, and the interaction between the conductive materials, making it easier to mix uniformly with the active material and form a strong conductive path, thereby making it easier to obtain excellent battery characteristics.
[0025] The average primary particle diameter of the carbon black may be, for example, 30 nm or less, or may be 29 nm or less, 27 nm or less, 25 nm or less, 23 nm or less, or 21 nm or less. It is believed that a small average primary particle diameter of the carbon black increases the number of electrical contacts with the active material and the conductive material, improving conductivity and making it easier to obtain excellent battery characteristics. That is, the average primary particle diameter of the carbon black may be, for example, 17 nm or more and 30 nm or less, 17 nm or more and 29 nm or less, 17 nm or more and 27 nm or less, 17 nm or more and 25 nm or less, 17 nm or more and 23 nm or less, 17 nm or more and 21 nm or less.
[0026] The average primary particle diameter of carbon black refers to the average value of circle-equivalent diameters measured based on images of carbon black observed with a transmission electron microscope (TEM). Specifically, the average primary particle diameter of carbon black is obtained by taking 10 images of carbon black at a magnification of 100,000 using a transmission electron microscope JEM-2000FX (manufactured by JEOL Ltd.), measuring the circle-equivalent diameters of 200 primary particles of carbon black randomly sampled from the obtained images by image analysis, and calculating the arithmetic mean.
[0027] From the viewpoint of excellent conductivity, the volume resistivity of the carbon black may be 0.30 Ω·cm or less or 0.25 Ω·cm or less. The volume resistivity of the carbon black is measured, for example, in a compressed state under a load of 7.5 MPa.
[0028] The ash content and moisture content of the carbon black are not particularly limited. The ash content of the carbon black may be, for example, 0.04% by mass or less, and the moisture content of the carbon black may be, for example, 0.10% by mass or less.
[0029] The method for producing carbon black is not particularly limited. For example, the carbon black may be produced by a production method including a synthesis step of treating a raw material gas containing hydrocarbons in a cylindrical cracking furnace to obtain carbon black, and a purification step of removing magnetic foreign matter from the carbon black obtained in the synthesis step using a magnet.
[0030] In the synthesis step, the raw material gas is treated in a cylindrical cracking furnace. The cylindrical cracking furnace may include, for example, a pyrolysis section for carrying out a pyrolysis reaction of hydrocarbons and an aging section for modifying the pyrolysis reaction product. The cylindrical cracking furnace may further include a supply port for supplying the raw material gas to the pyrolysis section and a recovery port for recovering the carbon black produced from the aging section.
[0031] In the thermal decomposition section, the supplied raw material gas preferably remains at a temperature of 1900°C or higher for 30 to 150 seconds. A raw material gas residence time of 30 seconds or longer ensures the completion of the thermal decomposition reaction and the development of a chain structure to form a carbon aerosol. Furthermore, a raw material gas residence time of 150 seconds or shorter suppresses the agglomeration of the carbon aerosol, making it easier to remove magnetic foreign matter in the purification step and to obtain high-purity carbon black.
[0032] In the aging section, the pyrolysis reaction product supplied from the pyrolysis section preferably resides at a temperature of 1700°C or higher for 20 to 90 seconds. A residence time of the pyrolysis reaction product of 20 seconds or more modifies the carbon aerosol and promotes the growth of aggregates, making it easier to obtain higher quality carbon black. Furthermore, a residence time of the pyrolysis reaction product of 90 seconds or less suppresses the agglomeration of the carbon aerosol, making it easier to remove magnetic foreign matter in the purification step and making it easier to obtain high-purity carbon black.
[0033] The residence times in the thermal decomposition section and the aging section can be adjusted appropriately by adjusting the linear velocity of the gas flowing through them. The residence time in the aging section is preferably shorter than the residence time in the thermal decomposition section. That is, the linear velocity of the gas in the aging section is preferably higher than the linear velocity of the gas in the thermal decomposition section.
[0034] In this embodiment, the source gas preferably contains acetylene as a carbon source. The content of the carbon source (e.g., acetylene) in the source gas is, for example, 10% by volume or more, preferably 20% by volume or more, more preferably 30% by volume or more, and may be 100% by volume. The content of each component in the source gas is expressed as a volume ratio based on the volume at 100°C and 1 atmosphere.
[0035] The feed gas may further contain hydrocarbons other than the carbon source (e.g., acetylene). Examples of other hydrocarbons include methane, ethane, propane, ethylene, propylene, butadiene, benzene, toluene, xylene, gasoline, kerosene, light oil, and heavy oil. The addition of these other hydrocarbons can change the reaction temperature and increase or decrease the specific surface area of the carbon black. The other hydrocarbons are preferably selected from the group consisting of aromatic hydrocarbons such as benzene and toluene, and unsaturated hydrocarbons such as ethylene and propylene.
[0036] When the raw material gas contains acetylene and other hydrocarbons, the content of the other hydrocarbons is, for example, 0.1 to 99 parts by volume, preferably 0.2 to 50 parts by volume, and more preferably 0.3 to 30 parts by volume, relative to 100 parts by volume of acetylene.
[0037] The raw material gas may further contain water vapor, oxygen, hydrogen, carbon dioxide, etc. It is preferable to use a high-purity gas with a purity of 99.9% by volume or more. The use of such a high-purity gas tends to facilitate the production of carbon black with a low content of magnetic foreign matter and a stable BET specific surface area.
[0038] The content of the water vapor gas may be, for example, 0 to 80 parts by volume, preferably 0.1 to 70 parts by volume, more preferably 1 to 60 parts by volume, and even more preferably 3 to 55 parts by volume, relative to 100 parts by volume of the carbon source (e.g., acetylene) in the raw material gas. When the content of the water vapor gas is within the above range, the BET specific surface area of the carbon black tends to be larger.
[0039] In the synthesis process, it is preferable to supply oxygen gas to the pyrolysis section together with the raw material gas, and it is more preferable to supply oxygen gas to the pyrolysis section by spraying it from around the supply port through which the raw material gas is supplied to the pyrolysis section.
[0040] The cylindrical cracking furnace preferably has an oxygen gas injection port near the raw material gas supply port, and more preferably has a plurality of injection ports provided at equal intervals so as to surround the supply port. The number of injection ports is preferably 3 or more, more preferably 3 to 8.
[0041] The cylindrical cracking furnace may also be equipped with a nozzle having a multi-tube structure (e.g., a double-tube structure, a triple-tube structure, etc.) having a raw material gas supply port and an injection port for injecting oxygen gas from around the port. In the case of a double-tube structure, for example, the raw material gas may be injected from a gap on the inner tube side, and the oxygen gas may be injected from a gap on the outer tube side. In the case of a triple-tube structure consisting of an inner tube, a middle tube, and an outer tube, for example, the oxygen gas may be injected from a gap formed by the outer wall of the middle tube and the inner wall of the outer tube, and the raw material gas may be injected from the remaining gap.
[0042] The amount of oxygen gas injected is not particularly limited as long as the production yield of carbon black is not taken into consideration. Carbon black can be produced even if more oxygen gas than necessary is injected. The amount of oxygen gas injected may be, for example, 0 to 300 parts by volume, 0 to 250 parts by volume, 0 to 220 parts by volume, or 0 to 200 parts by volume, relative to 100 parts by volume of the carbon source (e.g., acetylene) in the raw material gas, and is preferably 0.1 to 190 parts by volume, more preferably 0.5 to 180 parts by volume, and even more preferably 1 to 160 parts by volume. Increasing the amount of oxygen gas injected tends to increase the BET specific surface area of the carbon black, while decreasing the amount of oxygen gas injected tends to increase the primary particle size of the carbon black.
[0043] In the synthesis step, the primary particle size, BET specific surface area, and crystallite size (Lc) of the resulting carbon black can be adjusted by adjusting, for example, the addition rate of hydrocarbons other than acetylene, the amount of oxygen gas to be injected, etc.
[0044] The purification step is a step of removing magnetic foreign matter from the carbon black obtained in the synthesis step using a magnet. The purification step may be, for example, a step of removing magnetic foreign matter from the carbon black obtained in the synthesis step by bringing the carbon black into contact with a magnet or placing it in the vicinity of a magnet (e.g., by passing it near a magnet).
[0045] The maximum surface magnetic flux density of the magnet is not particularly limited, but may be, for example, 700 mT or more, preferably 1000 mT or more, and more preferably 1200 mT or more. This allows fine magnetic foreign matter adhering to the carbon black to be more strongly adsorbed, making it easier to obtain carbon black with a lower nickel content. The upper limit of the maximum surface magnetic flux density of the magnet is not particularly limited, and may be, for example, 1400 mT or less. That is, the maximum surface magnetic flux density of the magnet may be, for example, 700 mT or more and 1400 mT or less, 1000 mT or more and 1400 mT or less, or 1200 mT or more and 1400 mT or less.
[0046] The purification step may be a step of removing magnetic foreign matter from the carbon black so that the nickel content is 50 ppb or less (preferably 40 ppb or less, more preferably 30 ppb or less, and even more preferably 20 ppb or less). There is no particular lower limit for the nickel content, but the nickel content in the carbon black may be, for example, 1 ppb or more, and from the viewpoints of cost and productivity, it may be 10 ppb or more, or 15 ppb or more. That is, the nickel content in the carbon black may be, for example, from 1 ppb to 50 ppb, from 1 ppb to 40 ppb, from 1 ppb to 30 ppb, from 1 ppb to 20 ppb, from 10 ppb to 50 ppb, from 10 ppb to 40 ppb, from 10 ppb to 30 ppb, from 10 ppb to 20 ppb, from 15 ppb to 50 ppb, from 15 ppb to 40 ppb, from 15 ppb to 30 ppb, or from 15 ppb to 20 ppb.
[0047] <First Liquid Medium> The first liquid medium is not particularly limited as long as it is a dispersion medium capable of finely dispersing carbon black. Examples of the first liquid medium include water, N-methyl-2-pyrrolidone, cyclohexane, methyl ethyl ketone, and methyl isobutyl ketone. Of these, N-methyl-2-pyrrolidone is preferred from the viewpoint of easy dispersibility of carbon black. In this specification, N-methyl-2-pyrrolidone may be abbreviated as "NMP."
[0048] The content of carbon black in the first slurry may be, for example, 1% by mass or more, 3% by mass or more, 5% by mass or more, 7% by mass or more, 9% by mass or more, or 10% by mass or more. A high content of carbon black tends to make it easier to prepare a positive electrode composition with a high solids concentration.
[0049] The carbon black content in the first slurry may be, for example, 30% by mass or less, 25% by mass or less, 20% by mass or less, or 15% by mass or less. A low carbon black content makes it easier to obtain a low-viscosity positive electrode composition. A low viscosity positive electrode composition makes it easier to obtain a uniform electrode when the positive electrode composition is applied. That is, the carbon black content in the first slurry may be, for example, 1% by mass or more and 30% by mass or less, 1% by mass or more and 25% by mass or less, 1% by mass or more and 20% by mass or less, 1% by mass or more and 15% by mass or less, 3% by mass or more and 30% by mass or less, 3% by mass or more and 25% by mass or less, 3% by mass or more and 20% by mass or less, 3% by mass or more and 15% by mass or less, 5% by mass or more and 30% by mass or less, 5% by mass or more and 25% by mass or less, 5% by mass or more and 20% by mass or less, or 5% by mass or less. Upper 15% by mass or less, 7% by mass or more and 30% by mass or less, 7% by mass or more and 25% by mass or less, 7% by mass or more and 20% by mass or less, 7% by mass or more and 15% by mass or less, 9% by mass or more and 30% by mass or less, 9% by mass or more and 25% by mass or less, 9 qualities % or more and 20% by mass or less, 9% by mass or more and 15% by mass or less, 10% by mass or more and 30% by mass or less, 10% by mass or more and 25% by mass or less, 10% by mass or more and 20% by mass or less, or 10% by mass or more and 15% by mass or less.
[0050] <Dispersant> The first slurry may further contain a dispersant, which may be any component that has the function of assisting dispersion of carbon black in the first liquid medium.
[0051] Examples of dispersants include polymeric dispersants and low molecular weight dispersants, and from the viewpoint of long-term dispersion stability of carbon black, polymeric dispersants are preferred.
[0052] The dispersant may be, for example, a dispersant selected from the group consisting of polyvinyl alcohol, polyvinylpyrrolidone, polyvinyl butyral, carboxymethyl cellulose and its salts, polyvinyl acetal, polyvinyl acetate, polyvinylamine, and polyvinyl formal.
[0053] The content of the dispersant in the first slurry may be, for example, 1 part by mass or more, 3 parts by mass or more, 5 parts by mass or more, or 7 parts by mass or more, relative to 100 parts by mass of carbon black. A high content of the dispersant tends to make it easier to disperse the conductive material more uniformly, and to obtain better battery characteristics. The content of the dispersant in the first slurry may be, for example, 50 parts by mass or less, 30 parts by mass or less, 20 parts by mass or less, or 15 parts by mass or less, relative to 100 parts by mass of carbon black. A low content of the dispersant tends to reduce the insulating component in the positive electrode composition, reducing the resistance of the electrode and making it easier to obtain better battery characteristics. That is, the content of the dispersant in the first slurry may be, for example, 1 part by mass or more and 50 parts by mass or less, 1 part by mass or more and 30 parts by mass or less, 1 part by mass or more and 20 parts by mass or less, 1 part by mass or more and 15 parts by mass or less, 3 parts by mass or more and 50 parts by mass or less, 3 parts by mass or more and 30 parts by mass or less, 3 parts by mass or more and 20 parts by mass or less, 3 parts by mass or more and 15 parts by mass or less, 5 parts by mass or more and 50 parts by mass or less, 5 parts by mass or more and 30 parts by mass or less, 5 parts by mass or more and 20 parts by mass or less, 5 parts by mass or more and 15 parts by mass or less, 7 parts by mass or more and 50 parts by mass or less, 7 parts by mass or more and 30 parts by mass or less, 7 parts by mass or more and 20 parts by mass or less, or 7 parts by mass or more and 15 parts by mass or less.
[0054] <Particle Size Distribution of Carbon Black Particle Groups in First Slurry> The volume-based particle size distribution of the particle group, which includes the secondary particles of carbon black in the first slurry and the tertiary particles formed by agglomeration of the secondary particles, is measured by a laser diffraction / scattering method. Specifically, the measurement is performed under the following conditions. Measuring instrument: Laser diffraction / scattering particle size distribution measuring device (Microtrac MT3300EXII, manufactured by Microtrac Bell Corporation). Measurement conditions: Measurement range: 0.02 to 2000 μm, particle permeability / absorption, particle shape / non-spherical, solvent: NMP, circulation output: 5. Sample input amount: Slurry is added and adjusted so that the transmittance (TR) displayed upon sample input is 0.85 to 0.9. Note that secondary particles of carbon black are particles generally called aggregates in the classification of carbon black structures, which are formed by chemically bonding primary particles of carbon black. Tertiary particles of carbon black are particles generally called agglomerates.
[0055] In this specification, D 10 means the particle size (10% diameter) (μm) at an integrated value of 10% in the particle size distribution, and D 50 means the particle size (50% diameter) (μm) at an integrated value of 50% in the particle size distribution, and D 90 means the particle size (90% diameter) (μm) at 90% cumulative value in the particle size distribution.
[0056] D in the above particle size distribution 50 is 0.3 μm or more and 0.9 μm or less. 10 and D 90 D for the difference 50 The ratio (D 50 / (D 90 -D 10 )) is 0.2 or more and 0.8 or less.
[0057] D 50 may be 0.35 μm or more, 0.4 μm or more, or 0.5 μm or more. 50 may be 0.85 μm or less. 50may be, for example, 0.3 μm or more and 0.9 μm or less, 0.3 μm or more and 0.85 μm or less, 0.35 μm or more and 0.9 μm or less, 0.35 μm or more and 0.85 μm or less, 0.4 μm or more and 0.9 μm or less, 0.4 μm or more and 0.85 μm or less, 0.5 μm or more and 0.9 μm or less, or 0.5 μm or more and 0.85 μm or less.
[0058] Ratio (D 50 / (D 90 -D 10 )) may be 0.25 or more, 0.3 or more, or 0.35 or more. 50 / (D 90 -D 10 )) may be 0.7 or less, 0.6 or less, 0.5 or less, or 0.45 or less. 50 / (D 90 -D 10 )) may be, for example, 0.2 or more and 0.8 or less, 0.2 or more and 0.7 or less, 0.2 or more and 0.6 or less, 0.2 or more and 0.5 or less, 0.2 or more and 0.45 or less, 0.25 or more and 0.8 or less, 0.25 or more and 0.7 or less, 0.25 or more and 0.6 or less, 0.25 or more and 0.5 or less, 0.25 or more and 0.45 or less, 0.3 or more and 0.8 or less, 0.3 or more and 0.7 or less, 0.35 or more and 0.6 or less, 0.35 or more and 0.5 or less, or 0.35 or more and 0.45 or less.
[0059] D 10 may be 0.15 μm or more, 0.20 μm or more, or 0.25 μm or more. 10 may be 0.42 μm or less, 0.40 μm or less, or 0.38 μm or less. 10 may be, for example, 0.15 μm or more and 0.42 μm or less, 0.15 μm or more and 0.40 μm or less, 0.15 μm or more and 0.38 μm or less, 0.20 μm or more and 0.42 μm or less, 0.20 μm or more and 0.40 μm or less, 0.20 μm or more and 0.38 μm or less, 0.25 μm or more and 0.42 μm or less, 0.25 μm or more and 0.40 μm or less, or 0.25 μm or more and 0.38 μm or less. 90may be 0.9 μm or more, 1.5 μm or more, or 2.0 μm or more. 90 may be 4.0 μm or less, 3.0 μm or less, or 2.6 μm or less. 90 may be, for example, 0.9 μm or more and 4.0 μm or less, 0.9 μm or more and 3.0 μm or less, 0.9 μm or more and 2.6 μm or less, 1.5 μm or more and 4.0 μm or less, 1.5 μm or more and 3.0 μm or less, 1.5 μm or more and 2.6 μm or less, 2.0 μm or more and 4.0 μm or less, 2.0 μm or more and 3.0 μm or less, or 2.0 μm or more and 2.6 μm or less.
[0060] The carbon black in the first slurry is D 10 and D 90 By forming particle groups with a particle diameter within the above range, the carbon black is more efficiently arranged between the active materials and on the surfaces of the active materials, which is believed to result in more efficient formation of conductive paths between the active materials through the cooperation of the carbon black and the carbon nanotubes, thereby achieving both low internal resistance and excellent discharge rate characteristics at a higher level.
[0061] In this embodiment, D 10 , D 50 , D 90 and ratio (D 50 / (D 90 -D 10 ) can be adjusted by appropriately selecting the mixing method (e.g., stirring means, stirring time, etc.) when forming the slurry.
[0062] <Viscosity of First Slurry> The viscosity of the first slurry at 25° C. and a shear rate of 10 (1 / sec) is desirably 100 to 1300 mPa·sec, for example, from the viewpoint of increasing the solids concentration of the positive electrode composition and facilitating the production of a uniform positive electrode.
[0063] <Method for Producing First Slurry> The first slurry can be produced by mixing carbon black, a first liquid medium, and, if necessary, a dispersant so that the carbon black has the above-mentioned particle size distribution.
[0064] The mixing method is not particularly limited, and may be carried out by a known method (for example, stirring and mixing using a bead mill, ball mill, sand mill, twin-screw kneader, planetary mixer, disper mixer, etc.). These methods and devices may also be used in appropriate combination.
[0065] The various conditions for mixing are: 50 and ratio (D 50 / (D 90 -D 10 )) may be appropriately adjusted so that it falls within the above range. For example, by increasing the stirring time, 50 tends to be small, and the ratio (D 50 / (D 90 -D 10 )) tends to become larger. Also, by shortening the stirring time, D 50 tends to be large, and the ratio (D 50 / (D 90 -D 10 ) tends to be smaller.
[0066] (Mixing Step) The mixing step is a step of mixing the first slurry, the binder, the carbon nanotubes, and the active material to obtain a positive electrode composition.
[0067] The mixing step may be, for example, the first or second embodiment described below.
[0068] A first aspect of the mixing step includes a first step of mixing a first slurry, a binder solution containing a binder and a second liquid medium, and a second slurry containing carbon nanotubes and a third liquid medium to obtain a mixed solution, and a second step of mixing the mixed solution with an active material to obtain a positive electrode composition.
[0069] According to the first aspect, a positive electrode composition can be obtained that can achieve lower internal resistance and better discharge rate characteristics compared to a case in which carbon black, carbon nanotubes, a binder, and an active material are mixed simultaneously.
[0070] In the first step of the first embodiment, the method for mixing the first slurry, the binder solution, and the second slurry is not particularly limited, and may be performed by a known method (e.g., stirring and mixing using a ball mill, a sand mill, a twin-screw kneader, a planetary mixer, a disper mixer, etc.) The first step of the first embodiment may be, for example, a step of charging the first slurry, the binder solution, and the second slurry into a mixing vessel and then stirring to obtain a mixed solution.
[0071] The second step in the first embodiment is a step of mixing the mixed solution obtained in the first step with an active material to obtain a positive electrode composition.
[0072] In the second step of the first embodiment, the method for mixing the mixed solution and the active material is not particularly limited, and may be performed by a known method (e.g., stirring and mixing using a ball mill, sand mill, twin-screw kneader, planetary mixer, disperser mixer, etc.) The second step of the first embodiment may be, for example, a step of adding the active material to a mixing vessel containing the mixed solution and then stirring to obtain a positive electrode composition.
[0073] A second aspect of the mixing step includes a first step of mixing a first slurry with a binder solution containing a binder and a second liquid medium to obtain a first mixed solution, a second step of mixing the first mixed solution with a second slurry containing carbon nanotubes and a third liquid medium to obtain a second mixed solution, and a third step of mixing the second mixed solution with an active material to obtain a positive electrode composition.
[0074] According to the second aspect, a positive electrode composition can be obtained that can achieve lower internal resistance and better discharge rate characteristics compared to a case in which carbon black, carbon nanotubes, a binder, and an active material are mixed simultaneously.
[0075] In the first step of the second embodiment, the method for mixing the first slurry and the binder solution is not particularly limited, and may be performed by a known method (e.g., stirring and mixing using a ball mill, sand mill, twin-screw kneader, planetary mixer, disper mixer, etc.) The first step of the second embodiment may be, for example, a step of charging the first slurry and the binder solution into a mixing vessel and then stirring to obtain a first mixed solution.
[0076] In the second step of the first embodiment, the method for mixing the first mixed liquid and the second slurry is not particularly limited, and may be performed by a known method (e.g., stirring and mixing using a ball mill, sand mill, twin-screw kneader, planetary mixer, disper mixer, etc.) The second step of the second embodiment may be, for example, a step of adding the second slurry to a mixing vessel containing the first mixed liquid, followed by stirring to obtain the second mixed liquid.
[0077] In the third step of the second embodiment, the method for mixing the second mixed solution and the active material is not particularly limited, and may be performed by a known method (e.g., stirring and mixing using a ball mill, sand mill, twin-screw kneader, planetary mixer, disperser mixer, etc.). The third step of the second embodiment may be, for example, a step of adding the active material to a mixing vessel containing the second mixed solution and then stirring to obtain a positive electrode composition.
[0078] One reason why the first and second aspects achieve the above-mentioned effects is thought to be that in the first step, the interaction between the binder and the carbon black creates a dispersed state in which the carbon black is less likely to aggregate and is less likely to become entangled with the carbon nanotubes, thereby suppressing the non-uniformity of the electrode structure caused by the aggregation of the carbon black or the entanglement of the carbon black with the carbon nanotubes.
[0079] <First Slurry> The first slurry is prepared in the above-described preparation step.
[0080] The amount of the first slurry used and the content of carbon black in the first slurry may be appropriately changed so that the content of carbon black in the positive electrode composition falls within a desired range.
[0081] <Binder Solution> The binder solution contains a binder and a second liquid medium.
[0082] Examples of binders include polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene copolymer, and (meth)acrylic acid ester copolymer. The polymer structure of the binder may be, for example, a random copolymer, an alternating copolymer, a graft copolymer, or a block copolymer. As the binder, polyvinylidene fluoride is preferred from the viewpoint of excellent voltage resistance.
[0083] The amount of binder solution used and the content of the binder in the binder are not particularly limited, and may be appropriately changed so that the content of the binder in the positive electrode composition falls within a desired range.
[0084] The second liquid medium may be any liquid medium capable of dissolving the binder, and may be compatible with the first and third liquid media. Examples of the second liquid medium include water, N-methyl-2-pyrrolidone, cyclohexane, methyl ethyl ketone, and methyl isobutyl ketone. Of these, N-methyl-2-pyrrolidone is preferred from the viewpoint of solubility. The second liquid medium may be the same as or different from the first liquid medium, but is preferably the same as the first liquid medium.
[0085] The content of the second liquid medium in the binder solution is not particularly limited as long as it is within a range in which the binder can be dissolved, and may be changed appropriately so that the solids concentration of the positive electrode composition falls within a desired range.
[0086] The solids concentration of the binder solution is not particularly limited and may be, for example, 1% by mass or more, 2% by mass or more, 3% by mass or more, or 4% by mass or more. The solids concentration of the binder solution may be, for example, 11% by mass or less, 10% by mass or less, or 9% by mass or less. That is, the solids concentration of the binder solution may be, for example, 1% by mass or more to 11% by mass or less, 1% by mass or more to 10% by mass or less, 1% by mass or more to 9% by mass or less, 2% by mass or more to 11% by mass or less, 2% by mass or more to 10% by mass or less, 2% by mass or more to 9% by mass or less, 3% by mass or more to 11% by mass or less, 3% by mass or more to 10% by mass or less, 3% by mass or more to 9% by mass or less, 4% by mass or more to 11% by mass or less, 4% by mass or more to 10% by mass or less, or 4% by mass or more to 9% by mass or less.
[0087] The binder solution may further contain components other than the binder and the second liquid medium. Examples of other components in the binder solution include a conductive material, a thickener, a surfactant, etc. The binder solution may further contain, for example, polyvinylpyrrolidone, polyvinylimidazole, polyethylene glycol, polyvinyl alcohol, polyvinyl butyral, carboxymethyl cellulose, acetyl cellulose, or a carboxylic acid-modified (meth)acrylic acid ester copolymer, etc.
[0088] <Second Slurry> The second slurry contains carbon nanotubes and a third liquid medium.
[0089] The average diameter of the carbon nanotubes is preferably 5 nm or more. When the average diameter of the carbon nanotubes is 5 nm or more, the interaction between the liquid medium and the conductive material and the interaction between the conductive materials are reduced, making it easier for the carbon nanotubes to be dispersed more uniformly in the active material. This makes it easier to form conductive paths and to obtain better battery characteristics. The average diameter of the carbon nanotubes may be 6 nm or more.
[0090] Furthermore, the average diameter of the carbon nanotubes is preferably 15 nm or less. When the average diameter of the carbon nanotubes is 15 nm or less, the number of electrical contacts between the active material and the conductive material increases, the effect of imparting conductivity is improved, and better battery characteristics are more easily obtained. From the viewpoint of further reducing internal resistance and improving discharge rate characteristics, the average diameter of the carbon nanotubes is preferably 12 nm or less, more preferably 10 nm or less, and may be 9 nm or less, 8 nm or less, or 7 nm or less. That is, the average diameter of the carbon nanotubes may be, for example, 5 nm or more and 15 nm or less, 5 nm or more and 12 nm or less, 5 nm or more and 10 nm or less, 5 nm or more and 9 nm or less, 5 nm or more and 8 nm or less, 5 nm or more and 7 nm or less, 6 nm or more and 15 nm or less, 6 nm or more and 12 nm or less, 6 nm or more and 10 nm or less, 6 nm or more and 9 nm or less, 6 nm or more and 8 nm or less, or 6 nm or more and 7 nm or less.
[0091] The average diameter of carbon nanotubes refers to the average value of diameters measured based on images of carbon nanotubes observed with a transmission electron microscope (TEM). Specifically, a transmission electron microscope JEM-2000FX (manufactured by JEOL Ltd.) is used to take 10 images of carbon nanotubes at a magnification of 200,000, and the diameters of 100 carbon nanotubes randomly selected from the obtained images are measured by image analysis, and the arithmetic mean is calculated.
[0092] The BET specific surface area of carbon nanotubes is 170 to 320 m 2 / g. The BET specific surface area of the carbon nanotubes is preferably 170 m 2 When the BET specific surface area of the carbon nanotubes is 320 m / g or more, the number of electrical contact points with the active material and the conductive material increases, and the effect of imparting conductivity is improved, making it easier to obtain excellent battery characteristics. 2 / g or less, the interaction between the liquid medium and the conductive material and the interaction between the conductive materials are reduced, and the conductive material is more easily dispersed in the active material, which makes it easier to form conductive paths and to obtain better battery characteristics.
[0093] In this specification, the BET specific surface area of the carbon nanotubes is measured by the static capacitance method in accordance with JIS Z8830 using nitrogen as an adsorbate.
[0094] The BET specific surface area of the carbon nanotube is 180 m from the viewpoint of reducing the internal resistance and improving the discharge rate characteristics and cycle characteristics. 2 / g or more, 200m 2 / g or more, 230m 2 / g or more, 250m 2 / g or more or 280m 2 The BET specific surface area of the carbon nanotubes may be 310 m / g or more from the viewpoint of further reducing the internal resistance and further improving the discharge rate characteristics. 2 That is, the BET specific surface area of the carbon nanotube may be, for example, 170 m 2 / g or more 320m 2 / g or less, 180m 2 / g or more 320m 2 / g or less, 200m 2 / g or more 320m 2 / g or less, 230m 2 / g or more 320m 2 / g or less, 250m 2 / g or more 320m 2 / g or less, 280m 2 / g or more 320m 2 / g or less, 170m 2 / g or more 310m 2 / g or less, 180m 2 / g or more 310m 2 / g or less, 200m 2 / g or more 310m 2 / g or less, 230m 2 / g or more 310m 2 / g or less, 250m 2 / g or more 310m 2 / g or less, or 280m 2 / g or more 310m 2 / g or less.
[0095] The ratio of the average diameter to the BET specific surface area of the carbon nanotubes (average diameter / BET specific surface area) is 0.01 to 0.068 nm / (m 2 The ratio (average diameter / BET specific surface area) is a value obtained by dividing the average diameter of the carbon nanotubes by the BET specific surface area of the carbon nanotubes. 2 / g) or more, the carbon nanotubes are less likely to be entangled with each other and are more likely to be dispersed uniformly in the active material. This makes it easier to form conductive paths, resulting in better battery characteristics. 2 / g) or less, the number of carbon nanotubes per unit weight increases, allowing electricity to flow more efficiently throughout the active material, resulting in better battery characteristics.
[0096] The method for producing the carbon nanotubes is not particularly limited, and the carbon nanotubes may be produced by, for example, a conventionally known method for producing carbon nanotubes.
[0097] Carbon nanotubes can be produced, for example, by placing a powdered catalyst of iron supported on magnesia (magnesium oxide) across the entire horizontal cross section of a vertical reactor, flowing methane vertically through the reactor, bringing the methane into contact with the catalyst at 500 to 1200° C., and then oxidizing the resulting product (unoxidized carbon nanotubes).This method of producing carbon nanotubes makes it easy to obtain carbon nanotubes consisting of several graphene layers.
[0098] The oxidation treatment of the product may be, for example, a calcination treatment. The temperature of the calcination treatment is not particularly limited and may be, for example, 300 to 1000°C. The temperature of the calcination treatment is affected by the atmospheric gas, and therefore, it is preferable to perform the calcination treatment at a relatively low temperature when the oxygen concentration is high and at a relatively high temperature when the oxygen concentration is low. Specifically, the calcination treatment of the product may be performed in the atmosphere within a range of ±50°C of the combustion peak temperature of the carbon nanotubes before the oxidation treatment. However, when the oxygen concentration is higher than that of the atmosphere, calcination is performed at a temperature range lower than the calcination peak temperature, and when the oxygen concentration is lower than that of the atmosphere, a temperature range higher than the calcination peak temperature is selected. In particular, when performing the calcination treatment of the carbon nanotubes before the oxidation treatment in the atmosphere, it is preferable to perform the calcination treatment within a range of ±15°C of the combustion peak temperature of the carbon nanotubes before the oxidation treatment.
[0099] The oxidation treatment of the above product may be a treatment with hydrogen peroxide, mixed acid, nitric acid, or the like. Examples of methods for treating the above product with hydrogen peroxide include mixing the above product with 34.5% aqueous hydrogen peroxide to a concentration of 0.01 to 10% by mass and reacting at a temperature of 0 to 100°C for 0.5 to 48 hours. Examples of methods for treating the above product with mixed acid include mixing the above product with a mixed solution of concentrated sulfuric acid and concentrated nitric acid (concentrated sulfuric acid:concentrated nitric acid=3:1) to a concentration of 0.01 to 10% by mass and reacting at a temperature of 0 to 100°C for 0.5 to 48 hours. The mixing ratio of the mixed acid (concentrated sulfuric acid:concentrated nitric acid) can be adjusted within a range of 1:10 to 10:1 depending on the amount of single-walled carbon nanotubes in the above product. As a method for treating the above product with nitric acid, for example, a method can be mentioned in which the above product is mixed with nitric acid having a concentration of 40 to 80 mass % so as to have a concentration of 0.01 to 10 mass %, and the mixture is reacted at a temperature of 60 to 150°C for 0.5 to 48 hours.
[0100] By subjecting the above-mentioned product to an oxidation treatment, impurities such as amorphous carbon and single-walled carbon nanotubes with low heat resistance can be selectively removed from the product, thereby improving the purity of several-layer graphene, particularly 2- to 5-layer carbon nanotubes. At the same time, by subjecting the product to an oxidation treatment, functional groups are added to the surface of the carbon nanotubes, improving their affinity with the dispersion medium and additives and improving dispersibility. Among the above-mentioned oxidation treatments, a treatment using nitric acid is preferred.
[0101] The oxidation treatment may be carried out immediately after obtaining the carbon nanotubes before the oxidation treatment, or after another purification treatment. For example, when iron / magnesia is used as a catalyst, the oxidation treatment may be carried out after a purification treatment with an acid such as hydrochloric acid to remove the catalyst before the oxidation treatment, or after the oxidation treatment, a purification treatment to remove the catalyst may be carried out.
[0102] The amount of the second slurry used and the content of carbon nanotubes in the second slurry are not particularly limited, and may be changed as appropriate so that the content of carbon nanotubes in the positive electrode composition falls within a desired range.
[0103] The third liquid medium may be any liquid medium capable of dispersing carbon nanotubes and compatible with the first and second liquid media. Examples of the third liquid medium include water, N-methyl-2-pyrrolidone, cyclohexane, methyl ethyl ketone, and methyl isobutyl ketone. Among these, N-methyl-2-pyrrolidone is preferred from the viewpoint of easy dispersibility of carbon nanotubes. The third liquid medium may be the same as or different from the first liquid medium, but is preferably the same as the first liquid medium.
[0104] The content of the third liquid medium in the second slurry is not particularly limited as long as it is within a range in which the carbon nanotubes can be dispersed, and may be appropriately changed so that the solids concentration of the positive electrode composition falls within a desired range.
[0105] The solid content concentration of the second slurry is not particularly limited and may be, for example, 0.2 mass% or more, 0.8 mass% or more, 1.5 mass% or more, or 2.5 mass% or more. The solid content concentration of the second slurry may be, for example, 15 mass% or less, 12.5 mass% or less, 10 mass% or less, or 7.5 mass% or less. That is, the solid content concentration of the second slurry is, for example, 0.2 mass% or more and 15 mass% or less, 0.2 mass% or more and 12.5 mass% or less, 0.2 mass% or more and 10 mass% or less, 0.2 mass% or more and 7.5 mass% or less, 0.8 mass% or more and 15 mass% or less, 0.8 mass% or more and 12.5 mass% or less, 0.8 mass% or more and 10 mass% or less, 0.8 mass% or more and 7. 5 mass% or less, 1.5 mass% or more and 15 mass% or less, 1.5 mass% or more and 12.5 mass% or less, 1.5 mass% or more and 10 mass% or less, 1.5 mass% or more and 7.5 mass% or less, 2.5 mass% or more and 15 mass% or less, 2.5 mass% or more and 12.5 mass% or less, 2.5 mass% or more and 10 mass% or less, or 2.5 mass% or more and 7.5 mass% or less.
[0106] The second slurry may further contain components other than the carbon nanotubes and the third liquid medium, such as polyvinylpyrrolidone, polyvinylimidazole, polyethylene glycol, polyvinyl alcohol, polyvinyl butyral, carboxymethyl cellulose, acetyl cellulose, or a carboxylic acid-modified (meth)acrylic acid ester copolymer.
[0107] <Active Material> The active material may be any material that can reversibly store and release cations. 4 The lithium-containing composite oxide may be a lithium-containing composite oxide containing manganese having a resistivity of Ω cm or more, or a lithium-containing polyanion compound. Examples of the lithium-containing composite oxide containing manganese include LiMnO 2 , LiMnO 3 , LiMn 2 O 3 , Li 1+x Mn 2-x O 4 Lithium manganate such as LiMn (where x = 0 to 0.33); x Ni yCo z O 2 (However, x+y+z=1, 0≦y<1, 0≦z<1, 0≦x<1), Li 1+x Mn 2-x-y M y O 4 (where x = 0 to 0.33, y = 0 to 1.0, 2-x-y > 0), LiMn 2-x M x O 2 (where x = 0.01 to 0.1), Li 2 Mn 3 MO 8 Examples of lithium-containing polyanion compounds include composite oxides containing one or more transition metal elements such as LiFePO 4 , LiMnPO 4 , Li 2 MPO 4 Examples of suitable anionic compounds include polyanionic compounds such as F (wherein M is at least one metal selected from Co, Ni, Fe, Cr, and Zn), in which M in each composition formula is at least one metal selected from the group consisting of Fe, Co, Ni, Al, Cu, Mg, Cr, Zn, and Ta.
[0108] The average particle diameter of the active material (D 50 ) may be 20 μm or less or 10 μm or less from the viewpoint that the binding property between the conductive material and the binder is sufficiently excellent and a battery having more excellent cycle characteristics can be easily obtained. 50 ) can be measured by laser light scattering.
[0109] The amount of the active material used may be appropriately changed so that the content of the active material in the positive electrode composition falls within a desired range.
[0110] The positive electrode composition obtained by the manufacturing method of this embodiment contains carbon black, carbon nanotubes, a binder, and an active material. The positive electrode composition may further contain a dispersant.
[0111] The content of carbon black in the positive electrode composition may be, for example, 0.01% by mass or more, based on the total mass of the solid content, and from the viewpoint of further reducing internal resistance and further improving discharge rate characteristics, it may be 0.05% by mass or more, 0.1% by mass or more, 0.2% by mass or more, 0.3% by mass or more, 0.4% by mass or more, or 0.5% by mass or more. The content of carbon black in the positive electrode composition may be, for example, 10% by mass or less, 7% by mass or less, 5% by mass or less, 4% by mass or less, 3% by mass or less, or 2% by mass or less, based on the total mass of the solid content in the positive electrode composition. That is, the content of carbon black in the positive electrode composition is, for example, 0.01% by mass or more and 10% by mass or less, 0.01% by mass or more and 7% by mass or less, 0.01% by mass or more and 5% by mass or less, 0.01% by mass or more and 4% by mass or less, 0.01% by mass or more and 3% by mass or less, 0.01% by mass or more and 2% by mass or less, 0.05% by mass or more and 10% by mass or less, 0.05% by mass or more and 7% by mass or less, 0.05% by mass or more and 10 ... .. 05% to 5% by mass, 0.05% to 4% by mass, 0.05% to 3% by mass, 0.05% to 2% by mass, 0.1% to 10% by mass, 0.1% by mass to 7 Mass% or less, 0.1 mass% or more and 5 mass% or less, 0.1 mass% or more and 4 mass% or less, 0.1 mass% or more and 3 mass% or less, 0.1 mass% or more and 2 mass% or less, 0.2 mass% or more and 10 mass% or less, 0.2 mass% 7 mass% or less, 0.2 mass% or more and 5 mass% or less, 0.2 mass% or more and 4 mass% or less, 0.2 mass% or more and 3 mass% or less, 0.2 mass% or more and 2 mass% or less, 0.3 mass% or more and 10 mass% or less, 0.3 0.3% to 5% by mass, 0.3% to 4% by mass, 0.3% to 3% by mass, 0.3% to 2% by mass, 0.4% to 10% by mass, 0.4 mass% or more and 7 mass% or less, 0.4 mass% or more and 5 mass% or less, 0.4 mass% or more and 4 mass% or less, 0.4 mass% or more and 3 mass% or less, 0.4 mass% or more and 2 mass% or less, 0.5 mass% or more and 10 mass% Hereinafter, it may be 0.5 mass% or more and 7 mass% or less, 0.5 mass% or more and 5 mass% or less, 0.5 mass% or more and 4 mass% or less, 0.5 mass% or more and 3 mass% or less, or 0.5 mass% or more and 2 mass% or less.
[0112] The content of carbon nanotubes in the positive electrode composition may be, for example, 0.01% by mass or more, based on the total mass of the solid content, and from the viewpoint of further reducing internal resistance and improving discharge rate characteristics, it may be 0.03% by mass or more, 0.05% by mass or more, 0.07% by mass or more, 0.1% by mass or more, or 0.2% by mass or more. Furthermore, the content of carbon nanotubes in the positive electrode composition may be, for example, 5% by mass or less, 3% by mass or less, 2% by mass or less, 1% by mass or less, 0.9% by mass or less, 0.8% by mass or less, or 0.7% by mass or less, based on the total mass of the solid content in the positive electrode composition.That is, the content of carbon nanotubes in the positive electrode composition is, for example, 0.01% by mass or more and 5% by mass or less, 0.01% by mass or more and 3% by mass or less, 0.01% by mass or more and 2% by mass or less, 0.01% by mass or more and 1% by mass or less, 0.01% by mass or more and 0.9% by mass or less, 0.01% by mass or more and 0.8% by mass or less, 0.01% by mass or more and 0.7% by mass or less, 0.03% by mass or more and 5% by mass or less, 0.03% by mass or more, based on the total mass of the solid content. 3 mass% or less, 0.03 mass% or more and 1 mass% or less, 0.03 mass% or more and 0.9 mass% or less, 0.03 mass% or more and 0.8 mass% or less, 0.03 mass% or more and 0.7 mass% or less , 0.05 mass% to 5 mass%, 0.05 mass% to 3 mass%, 0.05 mass% to 2 mass%, 0.05 mass% to 1 mass%, 0.05 mass% to 0.9 mass%, 0.05 mass% to 0. 8 mass% or less, 0.05 mass% or more and 0.7 mass% or less, 0.07 mass% or more and 5 mass% or less, 0.07 mass% or more and 3 mass% or less, 0.07 mass% or more and 2 mass% or less, 0.07 mass% or more and 1 mass% or less, 0.07 Mass% or more and 0.9 mass% or less, 0.07 mass% or more and 0.8 mass% or less, 0.07 mass% or more and 0.7 mass% or less, 0.1 mass% or more and 5 mass% or less, 0.1 mass% or more and 3 mass% or less, 0.1 mass% or more and 2 mass% or less , 0.1 mass% or more and 1 mass% or less, 0.1 mass% or more and 0.9 mass% or less, 0.1 mass% or more and 0.8 mass% or less, 0.1 mass% or more and 0.7 mass% or less, 0.2 mass% or more and 5 mass% or less, 0.2 mass% or more and 3 mass% Hereinafter, it may be 0.2 mass% or more and 2 mass% or less, 0.2 mass% or more and 1 mass% or less, 0.2 mass% or more and 0.9 mass% or less, 0.2 mass% or more and 0.8 mass% or less, or 0.2 mass% or more and 0.7 mass% or less.
[0113] The content of carbon black in the positive electrode composition (C 1 ) the carbon nanotube content (C 2 ) ratio (C 2 / C 1 ) (mass ratio) may be, for example, 0.1 or more, and from the viewpoint of further reducing the internal resistance and further improving the discharge rate characteristics, it may be 0.2 or more, 0.3 or more, or 0.4 or more. 2 / C 1) may be, for example, 1 or less, and from the viewpoint of further reducing the internal resistance and further improving the discharge rate characteristics, it may be 0.95 or less, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, or 0.5 or less. That is, the ratio (C 2 / C 1 ) is, for example, 0.1 or more and 1 or less, 0.1 or more and 0.95 or less, 0.1 or more and 0.9 or less, 0.1 or more and 0.8 or less, 0.1 or more and 0.7 or less, 0.1 or more and 0.6 or less, 0.1 or more and 0.5 or less, 0.2 or more and 1 or less, 0.2 or more and 0.95 or less, 0.2 or more and 0.9 or less, 0.2 or more and 0.8 or less, 0.2 or more and 0.7 or less, 0.2 or more and 0.6 or less, 0.2 or more and 0.5 or less, 0.3 or more and 1 or less, 0.3 or more and 0.95 or less, 0.3 or more and 0.9 or less, 0.3 or more and 0.8 or less, 0.3 or more and 0.7 or less, 0.3 or more and 0.6 or less, 0.3 or more and 0.5 or less, 0.4 or more and 1 or less, 0.4 or more and 0.95 or less, 0.4 or more and 0.9 or less, 0.4 or more and 0.8 or less, 0.4 or more and 0.7 or less, 0.4 or more and 0.6 or less, or 0.4 or more and 0.5 or less.
[0114] The content of the binder in the positive electrode composition may be, for example, 0.3% by mass or more based on the total mass of the solids in the positive electrode composition, and from the viewpoint of further improving the binding property of the composite layer and more excellent cycle characteristics, it may be 0.5% by mass or more, 0.7% by mass or more, or 1% by mass or more. Furthermore, the content of the binder in the positive electrode composition may be, for example, 5% by mass or less based on the total mass of the solids in the positive electrode composition, and from the viewpoint of further reducing the resistance of the composite layer and more improving the discharge rate characteristics, it may be 4% by mass or less, 3% by mass or less, or 2% by mass or less. That is, the content of the binder in the positive electrode composition may be, for example, 0.3% by mass to 5% by mass, 0.3% by mass to 4% by mass, 0.3% by mass to 3% by mass, 0.3% by mass to 2% by mass, 0.5% by mass to 5% by mass, 0.5% by mass to 4% by mass, 0.5% by mass to 3% by mass, 0.5% by mass to 2% by mass, 0.7% by mass to 5% by mass, 0.7% by mass to 4% by mass, 0.7% by mass to 3% by mass, 0.7% by mass to 2% by mass, 1% by mass to 5% by mass, 1% by mass to 4% by mass, 1% by mass to 3% by mass, or 1% by mass to 2% by mass.
[0115] The content of the active material in the positive electrode composition may be, for example, 80% by mass or more, based on the total mass of the solid content in the positive electrode composition, and from the viewpoint of further improving battery characteristics, it is preferably 85% by mass or more, and may be 87% by mass or more, 89% by mass or more, 91% by mass or more, 93% by mass or more, or 95% by mass. Furthermore, the content of the active material in the positive electrode composition may be, for example, 99.5% by mass or less, 99% by mass or less, 98.5% by mass or less, or 98% by mass or less, based on the total mass of the solid content in the positive electrode composition. That is, the content of the active material in the positive electrode composition is, for example, 80% by mass or more and 99.5% by mass or less, 80% by mass or more and 99% by mass or less, 80% by mass or more and 98.5% by mass or less, 80% by mass or more and 98% by mass or less, 85% by mass or more and 99.5% by mass or less, 85% by mass or more and 99% by mass or less, 85% by mass or more and 98.5% by mass or less, 85% by mass or more and 98% by mass or less, 87% by mass or more and 99.5% by mass or less, 87% by mass or more and 99% by mass or less, 87% by mass or more and 98.5% by mass or less, 87% by mass or more and 98% by mass or less, 89% by mass or more and 99.5% by mass or less, based on the total mass of the solid content in the positive electrode composition. 89 mass% or more and 99 mass% or less, 89 mass% or more and 98.5 mass% or less, 91 mass% or more and 99.5 mass% or less, 91 mass% or more and 99 mass% or less, 91 mass% or more and 98.5 mass% or less, 91 mass% or more and 98 mass% or less, 93 mass% or more and 99.5 mass% % by mass or less, 93 mass% or more and 99 mass% or less, 93 mass% or more and 98.5 mass% or less, 93 mass% or more and 98 mass% or less, 95 mass% or more and 99.5 mass% or less, 95 mass% or more and 99 mass% or less, 95 mass% or more and 98.5 mass% or less, or 95 mass% or more and 98 mass% or less.
[0116] The solids concentration of the positive electrode composition is not particularly limited and may be, for example, 50% by mass or more, preferably 55% by mass or more, more preferably 60% by mass or more, or may be 65% by mass or more or 70% by mass or more. The solids concentration of the positive electrode composition may be, for example, 90% by mass or less, and from the viewpoint of further reducing the viscosity of the positive electrode composition, may be preferably 86% by mass or less, more preferably 82% by mass or less, or may be 78% by mass or less or 74% by mass or less. That is, the solid content concentration of the positive electrode composition is, for example, 50 mass% or more and 90 mass% or less, 50 mass% or more and 86 mass% or less, 50 mass% or more and 82 mass% or less, 50 mass% or more and 78 mass% or less, 50 mass% or more and 74 mass% or less, and 55 mass%. % to 90 mass%, 55 mass% to 86 mass%, 55 mass% to 82 mass%, 55 mass% to 78 mass%, 55 mass% to 74 mass%, 60 mass% to 90 mass%, 60 mass% to 86 mass%, 6 0 mass% to 82 mass%, 60 mass% to 78 mass%, 60 mass% to 74 mass%, 65 mass% to 90 mass%, 65 mass% to 86 mass%, 65 mass% to 82 mass%, 65 mass% to 78 mass% Below, it may be 65 mass% or more and 74 mass% or less, 70 mass% or more and 90 mass% or less, 70 mass% or more and 86 mass% or less, 70 mass% or more and 82 mass% or less, 70 mass% or more and 78 mass% or less, or 70 mass% or more and 74 mass% or less.
[0117] The viscosity of the positive electrode composition at 25°C and a shear rate of 10 (1 / sec) may be, for example, 6000 mPa·s or less, preferably 5000 mPa·s or less, more preferably 4000 mPa·s or less, or even 3000 mPa·s or less. The viscosity of the positive electrode composition at 25°C and a shear rate of 10 (1 / sec) may be, for example, 500 mPa·s or more, preferably 600 mPa·s or more, more preferably 700 mPa·s or more, or even 800 mPa·s or more. That is, the viscosity of the positive electrode composition at 25°C and a shear rate of 10 (1 / sec) is, for example, 500 mPa·s or more and 6000 mPa·s or less, 500 mPa·s or more and 5000 mPa·s or less, 500 mPa·s or more and 4000 mPa·s or less, 500 mPa·s or more and 3000 mPa·s or less, 600 mPa·s or more and 6000 mPa·s or less, 600 mPa·s or more and 5000 mPa·s or less, 600 mPa·s or more and 4000 mPa·s or less, 600 mPa·s or more and 600 mPa·s or less The viscosity may be from 700 mPa·s to 3000 mPa·s, from 700 mPa·s to 6000 mPa·s, from 700 mPa·s to 5000 mPa·s, from 700 mPa·s to 4000 mPa·s, from 700 mPa·s to 3000 mPa·s, from 800 mPa·s to 6000 mPa·s, from 800 mPa·s to 5000 mPa·s, from 800 mPa·s to 4000 mPa·s, or from 800 mPa·s to 3000 mPa·s.
[0118] [Method for Manufacturing Positive Electrode] The method for manufacturing a positive electrode of this embodiment includes a step of applying the positive electrode composition manufactured by the above-described manufacturing method onto a current collector to form a composite layer containing carbon black, carbon nanotubes, a binder, and an active material on the current collector. The composite layer is a layer containing the solid content of the positive electrode composition (at least carbon black, carbon nanotubes, a binder, and an active material), and may be a layer obtained by removing at least a portion of the liquid medium from the positive electrode composition.
[0119] The current collector is not particularly limited, and known current collectors can be used without any particular limitation. For example, metal foils (metals such as gold, silver, copper, platinum, aluminum, iron, nickel, chromium, manganese, lead, tungsten, and titanium, and alloys containing any one of these as the main component) are used as current collectors. Among these, it is preferable to use aluminum for the positive electrode and copper for the negative electrode. Current collectors are generally provided in the form of foils, but are not limited thereto, and perforated foil and mesh-shaped current collectors can also be used.
[0120] The method for applying the positive electrode composition onto the current collector is not particularly limited, and may be, for example, a die coating method, a dip coating method, a roll coating method, a doctor coating method, a knife coating method, a spray coating method, a gravure coating method, a screen printing method, or an electrostatic coating method.
[0121] The amount of the positive electrode composition to be applied is not particularly limited, and may be adjusted appropriately so that the thickness of the composite layer falls within a desired range.
[0122] The composite layer may be formed by removing at least a portion of the liquid medium from a coating film of the positive electrode composition formed on the current collector. The method for removing the liquid medium is not particularly limited, and examples of methods for removing at least a portion of the liquid medium by vaporizing it by heating and / or reducing pressure include leaving it to dry, using a blower dryer, a hot air dryer, an infrared heater, and a far-infrared heater.
[0123] The method for producing a positive electrode according to this embodiment may further include a pressurizing step of pressing the mixture layer and the current collector in the stacking direction. The pressurizing step can bring the mixture layer and the current collector into close contact with each other.
[0124] The pressing method in the pressing step is not particularly limited, and may be, for example, a roll press, a mold press, a calendar press, or the like.
[0125] The thickness of the composite layer in the positive electrode is not particularly limited and may be, for example, 50 μm or more, and from the viewpoint of increasing the capacity of the battery, it is preferably 55 μm or more, more preferably 60 μm or more, and may be 65 μm or more or 70 μm or more. Furthermore, the thickness of the composite layer in the positive electrode may be, for example, 150 μm or less, and from the viewpoint of further improving the discharge rate characteristics, it is preferably 140 μm or less, more preferably 130 μm or less, and may be 120 μm or less or 110 μm or less. That is, the thickness of the composite layer in the positive electrode is, for example, 50 μm or more and 150 μm or less, 50 μm or more and 140 μm or less, 50 μm or more and 130 μm or less, 50 μm or more and 120 μm or less, 50 μm or more and 110 μm or less, 55 μm or more and 150 μm or less, 55 μm or more and 140 μm or less, 55 μm or more and 130 μm or less, 55 μm or more and 120 μm or less, 55 μm or more and 110 μm or less, 60 μm or more and 150 μm or less, 60 μm or more and 14 ...10 μm or less, The thickness may be 0 μm or more and 130 μm or less, 60 μm or more and 120 μm or less, 60 μm or more and 110 μm or less, 65 μm or more and 150 μm or less, 65 μm or more and 140 μm or less, 65 μm or more and 130 μm or less, 65 μm or more and 120 μm or less, 65 μm or more and 110 μm or less, 70 μm or more and 150 μm or less, 70 μm or more and 140 μm or less, 70 μm or more and 130 μm or less, 70 μm or more and 120 μm or less, or 70 μm or more and 110 μm or less.
[0126] The positive electrode of this embodiment can be suitably used as a positive electrode for a battery, particularly a secondary battery (lithium ion secondary battery).
[0127] The battery (preferably a secondary battery, more preferably a lithium ion secondary battery) of this embodiment includes a positive electrode manufactured by the above-described manufacturing method. The configuration of the battery of this embodiment, other than the positive electrode, may be the same as that of a known battery.
[0128] The use of the battery in this embodiment is not particularly limited, and the battery can be used in a wide range of fields, for example, portable AV devices such as digital cameras, video cameras, portable audio players, and portable LCD televisions, portable information terminals such as notebook personal computers, smartphones, and mobile PCs, as well as portable game devices, power tools, electric bicycles, hybrid vehicles, electric vehicles, and power storage systems.
[0129] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0130] [Example 1] (Carbon Black) A carbon black reactor (furnace length 6 m, furnace diameter 0.65 m) was equipped with a nozzle installed upstream of which acetylene was injected at a rate of 12 Nm. 3 / h, toluene 32 kg / h, oxygen 20 Nm 3 / h to produce carbon black, which was then collected in a bag filter installed downstream of the reactor. The carbon black was then passed through a dry cyclone device and an iron-removing magnet and collected in a tank. The acetylene, toluene, and oxygen were heated to 115°C before being supplied to the reactor, yielding carbon black A. The resulting carbon black A had a BET specific surface area of 301 m. 2 / g, the average primary particle diameter was 19 nm, and the crystallite size (Lc) was 16 Å.
[0131] (Preparation of First Slurry) Carbon black A, N-methyl-2-pyrrolidone (referred to as NMP) as a dispersion medium, and polyvinyl alcohol (Poval B05, manufactured by Denka Co., Ltd.) as a dispersant were prepared. 1.0% by mass of polyvinyl alcohol and 11.0% by mass of carbon black A were added to 89.0% by mass of NMP, and the mixture was stirred for 120 minutes using a planetary mixer (Hivis Dispermix 3D-5, manufactured by Primix Corporation) to prepare a slurry containing carbon black A. The resulting slurry was placed in a bead mill (Mugen Flow MGF2-ZA, manufactured by Ashizawa Finetech Co., Ltd.) equipped with zirconia beads (diameter 0.5 mm), and a dispersion treatment was carried out for 30 minutes. After the dispersion treatment, the zirconia beads were removed by filtration, and a slurry of carbon black A (first slurry) was prepared. The particle size distribution of carbon black A was as shown in Table 1.
[0132] (Preparation of Positive Electrode Composition) LB-108 (manufactured by Cnano Corporation) was prepared as a multi-walled carbon nanotube slurry. The BET specific surface area of the multi-walled carbon nanotubes was 300 m 2 The average diameter of the multi-walled carbon nanotubes was 7 nm. 50 A 10 μm diameter lithium nickel manganese cobalt oxide (manufactured by Beijing Dangsheng Co., Ltd., "ME6E"), an NMP solution of polyvinylidene fluoride as a binder, and NMP as a dispersion medium were prepared. The first slurry, the NMP solution containing the binder, and the multi-walled carbon nanotube slurry were mixed using a planetary centrifugal mixer (Thinky Corporation, Awatori Rentaro ARV-310) to obtain a mixed solution. Next, the mixed solution and the active material were mixed, and NMP was added thereto until a coatable viscosity was achieved. The mixture was then mixed using the planetary centrifugal mixer until uniform, obtaining a positive electrode composition. The positive electrode composition was prepared so that, in terms of solid ratio, the active material was 97.7% by mass, carbon black was 0.7% by mass, multi-walled carbon nanotubes were 0.3% by mass, and the binder was 1.3% by mass.
[0133] (Production of Positive Electrode) The positive electrode composition was applied to one side of a 15 μm thick aluminum foil (manufactured by UACJ Corporation) using an applicator to form a laminate, which was then placed in a dryer for pre-drying at 105° C. for 1 hour to completely remove the NMP. The laminate was then pressed and cut to obtain a positive electrode including a current collector and a composite layer.
[0134] (Production of negative electrode) Pure water (manufactured by Kanto Chemical Co., Ltd.) as a solvent, artificial graphite (manufactured by Hitachi Chemical Co., Ltd., "MAG-D") as a negative electrode active material, styrene butadiene rubber (manufactured by Nippon Zeon Co., Ltd., "BM-400B", hereinafter referred to as SBR) as a binder, carboxymethyl cellulose (manufactured by Daicel Corporation, "D2200", hereinafter referred to as CMC) as a dispersant, and carbon black (manufactured by Denka Co., Ltd., "Li-400") as a conductive material were prepared. Next, CMC was weighed and mixed so that it was 1% by mass in solid content, carbon black was 1% by mass, and artificial graphite was 96% by mass in solid content, and pure water was added to this mixture. The mixture was mixed until uniform using a planetary centrifugal mixer (manufactured by Thinky Corporation, Awatori Rentaro ARV-310) to obtain a mixture. Next, SBR was weighed out so that the solid content was 2% by mass, added to the resulting mixture, and mixed until uniform using a planetary centrifugal mixer (Thinky Corporation, Awatori Rentaro ARV-310). A coating liquid for forming a negative electrode was obtained. The coating liquid for forming a negative electrode was then applied to a 10 μm thick copper foil (manufactured by UACJ Corporation) using an applicator to form a laminate, which was then placed in a dryer and pre-dried at 60 ° C. for 1 hour. The laminate was then pressed with a linear pressure of 50 kg / cm using a roll press to prepare a total thickness of 60 μm. The resulting mixture was then vacuum dried at 120 ° C. for 3 hours to completely remove residual moisture, resulting in a negative electrode comprising a current collector and a composite layer.
[0135] (Production of Battery) The positive electrode, separator and negative electrode were stacked and then packed with an aluminum laminate film and pre-sealed. Subsequently, an electrolyte was injected, followed by battery formatting and vacuum sealing to produce a laminated secondary battery.
[0136] (Evaluation of Positive Electrode) (1) Internal Resistance The fabricated battery was charged at 25°C at a constant current and constant voltage of 4.3 V with a 0.2 C limit, and then discharged to 3.0 V at a constant current of 0.2 C. Next, five charge / discharge cycles were performed under the same conditions, and then charged to a charge depth of 50%. Then, impedance measurements were performed at a frequency range of 10 MHz to 0.001 Hz and an oscillating voltage of 5 mV to measure the internal resistance. The results are shown in Table 1. (2) Discharge Rate Characteristics (Rate Capacity Retention Ratio) The fabricated battery was charged at a constant current and constant voltage of 4.3 V with a 0.2 C limit at 25°C, and then discharged to 3.0 V at a constant current of 0.2 C. Next, it was again recovered charged at a constant current and constant voltage of 4.3 V with a 0.2 C limit, and then discharged to 3.0 V at a constant current of 0.2 C, and the discharge capacity was measured. Next, the recovery charge was performed under the condition of a constant current and constant voltage of 4.3 V with a limit of 0.2 C, while the discharge current was changed stepwise from 0.5 C to 1 C, 2 C, and 3 C. Recovery charge and discharge were repeated, and the discharge capacity for each discharge current was measured. As an index of the discharge rate characteristics of the battery, the capacity retention rate at 3 C discharge relative to that at 0.2 C discharge was calculated as the rate capacity retention rate. The results are shown in Table 1.
[0137] Example 2 A first slurry was prepared in the same manner as in Example 1, except that the time for dispersion treatment using a bead mill was changed to 20 minutes and the particle size distribution of carbon black A was changed as shown in Table 1. Using the obtained first slurry, a positive electrode composition was prepared, a positive electrode and a negative electrode were manufactured, a battery was manufactured, and the positive electrode was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0138] [Example 3] A first slurry was prepared in the same manner as in Example 1, except that the time for dispersion treatment using a bead mill was changed to 40 minutes and the particle size distribution of carbon black A was changed as shown in Table 1. Using the obtained first slurry, a positive electrode composition was prepared, a positive electrode and a negative electrode were manufactured, a battery was manufactured, and the positive electrode was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0139] [Example 4] (Preparation of first slurry) Carbon black was Li-435 (manufactured by Denka Co., Ltd., average primary particle diameter: 23 nm, BET specific surface area: 141 m 2 / g) (hereinafter, carbon black B), NMP as a dispersion medium, and polyvinyl alcohol (Poval B05, manufactured by Denka Co., Ltd.) as a dispersant were prepared. 0.95 mass% polyvinyl alcohol and 13.5 mass% Li-435 were added to 85.6 mass% NMP, and the mixture was stirred for 120 minutes using a planetary mixer (Hivis Dispermix 3D-5, manufactured by Primix Corporation). The resulting slurry was then placed in a bead mill (Mugen Flow MGF2-ZA, manufactured by Ashizawa Finetech Co., Ltd.) equipped with zirconia beads (diameter 0.5 mm), and subjected to a dispersion treatment for 20 minutes. After the dispersion treatment, the zirconia beads were removed by filtration to obtain a first slurry. The particle size distribution of carbon black B was as shown in Table 1. Using this first slurry, the preparation of a positive electrode composition, the manufacture of a positive electrode and a negative electrode, the manufacture of a battery, and the evaluation of the positive electrode were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0140] Example 5 A first slurry was prepared in the same manner as in Example 4, except that the time for dispersion treatment using a bead mill was changed to 10 minutes and the particle size distribution of carbon black B was changed as shown in Table 1. Using the obtained first slurry, a positive electrode composition was prepared, a positive electrode and a negative electrode were manufactured, a battery was manufactured, and the positive electrode was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0141] [Example 6] A first slurry was prepared in the same manner as in Example 4, except that the time for dispersion treatment using a bead mill was changed to 30 minutes and the particle size distribution of carbon black B was changed as shown in Table 1. Using the obtained first slurry, preparation of a positive electrode composition, production of a positive electrode and a negative electrode, production of a battery, and evaluation of the positive electrode were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0142] Comparative Example 1 (Preparation of Positive Electrode Composition) A positive electrode composition was prepared in the same manner as in Example 1, except that multi-walled carbon nanotubes were not blended and the blending amount of carbon black A was 1.0 mass%. Except for using the obtained positive electrode composition, the positive electrode and negative electrode were manufactured, a battery was manufactured, and the positive electrode was evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0143] Comparative Example 2 (Preparation of Positive Electrode Composition) A positive electrode composition was prepared in the same manner as in Example 1, except that carbon black was not added and the amount of multi-walled carbon nanotubes added was 1.0 mass%. Except for using the resulting positive electrode composition, the positive electrode and negative electrode were produced, a battery was produced, and the positive electrode was evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0144] Comparative Example 3 A positive electrode composition was prepared in the same manner as in Example 1, except that no multi-walled carbon nanotubes were added, the active material content was 96.0 mass%, the carbon black B content was 2.0 mass%, and the binder content was 2.0 mass%. Except for using the resulting positive electrode composition, the positive electrode and negative electrode were produced, a battery was produced, and the positive electrode was evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0145] Comparative Example 4 A first slurry was prepared in the same manner as in Example 1, except that the time for dispersion treatment using a bead mill was changed to 60 minutes and the particle size distribution of carbon black A was changed as shown in Table 2. Using the obtained first slurry, a positive electrode composition was prepared, a positive electrode and a negative electrode were manufactured, a battery was manufactured, and the positive electrode was evaluated in the same manner as in Example 1. The results are shown in Table 3.
[0146] Comparative Example 5 A first slurry was prepared in the same manner as in Example 1, except that the time for dispersion treatment using a bead mill was changed to 10 minutes and the particle size distribution of carbon black A was changed as shown in Table 2. Using the obtained first slurry, a positive electrode composition was prepared, a positive electrode and a negative electrode were manufactured, a battery was manufactured, and the positive electrode was evaluated in the same manner as in Example 1. The results are shown in Table 3.
[0147] Comparative Example 6 A first slurry was prepared in the same manner as in Example 4, except that the time for dispersion treatment using a bead mill was changed to 50 minutes and the particle size distribution of carbon black B was changed as shown in Table 2. Using the obtained first slurry, a positive electrode composition was prepared, a positive electrode and a negative electrode were manufactured, a battery was manufactured, and the positive electrode was evaluated in the same manner as in Example 4. The results are shown in Table 3.
[0148] Comparative Example 7 A first slurry was prepared in the same manner as in Example 4, except that the time for dispersion treatment using a bead mill was changed to 5 minutes and the particle size distribution of carbon black B was changed as shown in Table 2. Using the obtained first slurry, a positive electrode composition was prepared, a positive electrode and a negative electrode were manufactured, a battery was manufactured, and the positive electrode was evaluated in the same manner as in Example 4. The results are shown in Table 3.
[0149]
[0150]
[0151]
Claims
1. A method for producing a positive electrode composition comprising the steps of: preparing a first slurry containing carbon black and a first liquid medium; and mixing the first slurry with a binder, carbon nanotubes, and an active material to obtain a positive electrode composition, wherein a volume-based particle size distribution of a particle group including secondary particles of the carbon black and tertiary particles formed by agglomeration of the secondary particles in the first slurry is greater than or equal to D 50 is 0.3 μm or more and 0.9 μm or less, and D 10 and D. 90 D for the difference 50 The ratio (D 50 / (D 90 -D 10 ) is 0.2 or more and 0.8 or less.
2. The manufacturing method according to claim 1, wherein the mixing step includes: a first step of mixing the first slurry, a binder solution containing the binder and a second liquid medium, and a second slurry containing the carbon nanotubes and a third liquid medium to obtain a mixed solution; and a second step of mixing the mixed solution with an active material to obtain the positive electrode composition.
3. The manufacturing method according to claim 1, wherein the mixing step includes: a first step of mixing the first slurry with a binder solution containing the binder and a second liquid medium to obtain a first mixed liquid; a second step of mixing the first mixed liquid with a second slurry containing the carbon nanotubes and a third liquid medium to obtain a second mixed liquid; and a third step of mixing the second mixed liquid with the active material to obtain the positive electrode composition.
4. The carbon black is 100 m 2 / g or more 400m 2 The method according to claim 1 , wherein the sintered body has a BET specific surface area of 100 nm or less and an average primary particle size of 17 nm or more and 30 nm or less.
5. The method according to claim 1, wherein the content of the carbon black in the positive electrode composition is 40 to 90 mass % based on the total amount of the carbon black and the carbon nanotubes.
6. In the volume-based particle size distribution of the particle group including the secondary particles of the carbon black in the first slurry and the tertiary particles formed by agglomeration of the secondary particles, 10 is 0.15 μm or more and 0.42 μm or less, and D 90 The method according to claim 1 , wherein the thickness is 0.9 μm or more and 4.0 μm or less.
7. A method for producing a positive electrode, comprising the step of applying the positive electrode composition produced by the method according to any one of claims 1 to 6 onto a current collector, to form a composite layer on the current collector, the composite layer containing the carbon black, the carbon nanotubes, the binder and the active material.
Citation Information
Patent Citations
Conductive slurry, electrode slurry and electrode for electric double-layer capacitor using the slurry
JP2008227481A
Lithium secondary battery and method for manufacturing the same
JP2013089575A
Carbon black dispersion
KR1020160029715A
Slurry including carbon black, electrode paste, method for producing electrode, and method for producing secondary battery
WO2020218211A1
Method for producing positive electrode composition and method for producing positive electrode
WO2023026898A1