Writing-feel-improving sheet
The writing quality improving sheet enhances the touch panel experience by incorporating a plasticizer and porous fine particles to achieve a dynamic friction coefficient that mimics paper-like writing and absorbs sebum-based fingerprints, addressing the issues of poor writing quality and fingerprint visibility on touch panels.
Patent Information
- Application Number
- PCT/JP2024/003795
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-02-06
- Publication Date
- 2024-10-03
AI Technical Summary
Touch panels used for both display and input, such as those with touch pens, suffer from poor writing quality due to their hard surface, and fingerprints from finger oils further degrade the writing experience and appearance, requiring frequent cleaning.
A writing quality improving sheet with a base material and a writing quality improving layer containing a plasticizer and porous fine particles, which provides a dynamic friction coefficient of 0.12 or more, enhancing the writing feel and absorbing sebum-based fingerprints over time, thus maintaining performance without the need for cleaning.
The sheet provides a writing experience similar to writing on paper with a pencil, offering resistance and vibration feelings, and maintains writing quality even with sebum-based fingerprints, improving the appearance and durability of the touch panel surface.
Smart Images

Figure JP2024003795_03102024_PF_FP_ABST
Abstract
Description
Writing feel improvement sheet
[0001] The present invention relates to a fingerprint-resistant sheet for improving writing feel.
[0002] In recent years, image display devices (touch panels) with position detection functions that combine display and input functions have become increasingly popular in various electronic devices. In addition to touch panels that allow input with fingers, some also allow input with a touch pen, which allows for more precise and accurate input than with a finger. However, the display module of a touch panel is typically hard. Therefore, the writing experience with a touch pen is different from the writing experience when writing on paper with a writing implement, and is difficult to describe as satisfactory.
[0003] In order to solve the problem of the writing feel when using a touch pen on a touch panel, it has been considered to attach a film that improves the writing feel (hereinafter, sometimes referred to as a "writing feel improving film" or "writing feel improving sheet") to the outermost surface of the touch panel. For example, Patent Document 1 discloses an example of such a writing feel improving film, which includes a transparent substrate film and linear convex portions that form a mesh structure on at least one surface of the transparent substrate film, the mesh structure having a plurality of regularly arranged compartments, and the linear convex portions occupying 5 to 80% of the area of the entire surface of the touch film.
[0004] JP 2015-054417 A
[0005] However, even when the input method for a touch panel is a touch pen, the touch panel is often touched with the hand, and fingerprints from finger oils are usually left on the surface of the touch panel. When fingerprints are left on the writing feel improving film as described above, the writing feel with the touch pen deteriorates. Furthermore, the fingerprints become conspicuous, which not only deteriorates the appearance but also makes it difficult to see the displayed image.
[0006] To provide a sheet for improving writing feel that provides a good writing feel with a touch pen, does not require wiping off fingerprints caused by sebum even when the sheet is adhered to the touch pen, and is unlikely to deteriorate the writing feel.
[0007] In order to achieve the above-mentioned object, first, the present invention provides a writing feel improvement sheet comprising a substrate and a writing feel improvement layer with which a touch pen comes into contact, wherein the writing feel improvement layer contains at least one of a plasticizer and porous microparticles, and wherein the writing feel improvement sheet is characterized in that the coefficient of dynamic friction measured by bringing the tip of a touch pen having a tip diameter of 0.5 mm into contact with the surface of the writing feel improvement layer with which the touch pen comes into contact, applying a load of 200 g to the touch pen, and sliding the touch pen linearly at a speed of 1.6 mm / sec while maintaining the angle between the touch pen and the surface of the writing feel improvement layer at 45°, is 0.12 or more (Invention 1).
[0008] In the writing experience improving sheet according to the above invention (Invention 1), the above-mentioned coefficient of dynamic friction imparts a favorable sense of resistance and vibration to the writing experience with a touch pen. These sensations combine to create an excellent writing experience similar to that of writing with a pencil on paper. Furthermore, because the writing experience improving layer contains at least one of a plasticizer and porous microparticles, their sebum-absorbing properties allow the writing experience layer to absorb sebum over time, even if fingerprints are left on the surface of the writing experience improving layer. Therefore, even if fingerprints are not wiped off, the appearance improves over time, and writing experience is less likely to deteriorate.
[0009] In the above invention (Invention 1), it is preferable that a diluted solution of oleic acid is applied to the surface of the writing feel improving layer that comes into contact with the touch pen, and the solution is allowed to dry naturally, and the dynamic friction coefficient measured using the measurement method 24 hours after the application is 0.12 or more (Invention 2).
[0010] In the above inventions (Inventions 1 and 2), when the kinetic friction coefficient is defined as the kinetic friction coefficient before application, a diluted solution of oleic acid is applied to the surface of the writing feel improving layer that comes into contact with the touch pen, the solution is allowed to dry naturally, and the kinetic friction coefficient measured by the measurement method 24 hours after application is defined as the kinetic friction coefficient after application, it is preferable that the ratio of the kinetic friction coefficient after application to the kinetic friction coefficient before application is 0.85 or more (Invention 3).
[0011] In the above inventions (Inventions 1 to 3), it is preferable that the writing feel improving layer is a layer formed by curing a coating composition containing a curable component, at least one of the plasticizer and porous microparticles, and a filler (excluding the porous microparticles) (Invention 4).
[0012] In the above inventions (Inventions 1 to 3), it is preferable that the writing feel improving layer is a layer formed by curing a coating composition containing a curable component, the plasticizer, and the porous microparticles (Invention 5).
[0013] In the above inventions (Inventions 1 to 5), the surface of the writing feel improving layer is subjected to a 125 g / cm 2 application of #0000 steel wool. 2 It is preferable that the number of scratches generated when the surface is rubbed five times back and forth over a distance of 10 cm under a load of 1000 kJ / cm is 10 or less (Invention 6).
[0014] The writing feel improving sheet according to the present invention provides a good writing feel, and even if fingerprints caused by sebum are left on the sheet, there is no need to wipe off the fingerprints, and the writing feel is unlikely to deteriorate.
[0015] 1 is a cross-sectional view of a writing feel improving sheet according to one embodiment of the present invention.
[0016] Hereinafter, an embodiment of the present invention will be described. A writing feel improving sheet according to one embodiment of the present invention is a sheet that constitutes the outermost layer of a touch panel on which a touch pen is used, and includes a substrate and a writing feel improving layer that comes into contact with the touch pen. Preferably, as shown in Figure 1, the writing feel improving sheet 1 according to this embodiment includes a substrate 11 and a writing feel improving layer 12 provided on one side of the substrate 11. The writing feel improving layer 12 contains at least one of a plasticizer and porous microparticles.
[0017] In the writing feel improving sheet 1 according to this embodiment, the kinetic friction coefficient measured by bringing the tip of a touch pen having a 0.5 mm diameter into contact with the surface of the writing feel improving layer 12 that the touch pen comes into contact with, and then applying a load of 200 g to the touch pen and sliding the touch pen linearly at a speed of 1.6 mm / sec while maintaining an angle of 45° between the touch pen and the surface of the writing feel improving layer 12, is preferably 0.12 or more. Note that a specific method for measuring the kinetic friction coefficient is as shown in the test examples described later.
[0018] The writing feel improving sheet 1 according to this embodiment has the above-mentioned coefficient of dynamic friction, which imparts a desirable sense of resistance and vibration to the writing feel with a touch pen. The combination of these sensations makes the writing feel with the touch pen closer to the sensation of writing with a pencil on paper (particularly the sensation of writing with a B pencil on five sheets of paper), resulting in an excellent writing feel.
[0019] Furthermore, in the writing feel improving sheet 1 according to this embodiment, the writing feel improving layer 12 contains at least one of a plasticizer and porous microparticles, so that even if fingerprint marks caused by sebum are left on the surface of the writing feel improving layer 12, the sebum is absorbed into the writing feel improving layer 12 over time. Therefore, even if the fingerprint marks caused by sebum are not wiped off, the appearance improves over time and the writing feel is less likely to deteriorate. This effect is sometimes referred to as "fingerprint resistance."
[0020] As the touch pen, for example, a touch pen with a hard felt tip and a pen tip diameter of 0.1 to 5 mm, or a touch pen with a polyacetal tip, etc. can be used, and the above-mentioned effect can be obtained regardless of the type of touch pen used.
[0021] From the viewpoint of the writing feel with the touch pen, the dynamic friction coefficient is preferably 0.14 to 0.8, more preferably 0.16 to 0.6, particularly preferably 0.18 to 0.4, and even more preferably 0.19 to 0.3.
[0022] 1. Elements 1-1. Substrate The substrate 11 may be appropriately selected from those suitable for touch panels in which a touch pen is used, and is preferably a plastic film that has good affinity with the writing feel improving layer 12. However, the substrate 11 may also be a glass plate or glass film.
[0023] Examples of such plastic films include polyester films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, polyolefin films such as polyethylene and polypropylene, cellophane, diacetyl cellulose film, triacetyl cellulose film, acetyl cellulose butyrate film, polyvinyl chloride film, polyvinylidene chloride film, polyvinyl alcohol film, ethylene-vinyl acetate copolymer film, polystyrene film, polycarbonate film, polymethylpentene film, polysulfone film, polyether ether ketone film, polyether sulfone film, polyetherimide film, fluororesin film, polyamide film, acrylic resin film, polyurethane resin film, norbornene polymer film, cyclic olefin polymer film, cyclic conjugated diene polymer film, and vinyl alicyclic hydrocarbon polymer film, or laminate films thereof. Among these, polyethylene terephthalate film, polycarbonate film, and norbornene polymer film are preferred, as they can maintain the writing feel of the touch pen well in combination with the writing feel improving layer 12 described above, and polyethylene terephthalate film is particularly preferred. From the perspective of the SDGs, the material that constitutes the plastic film may be a material with a high biomass content, a material that can be recycled or reused, or a recycled or reused material.
[0024] Furthermore, in order to improve adhesion to layers (such as the writing feel improving layer 12 and the adhesive layer described below) provided on the surface of the substrate 11, one or both sides may be subjected to a surface treatment such as a primer treatment, an oxidation method, or a roughening method, as desired. Examples of oxidation methods include corona discharge treatment, chromic acid treatment, flame treatment, hot air treatment, and ozone / ultraviolet treatment, while examples of roughening methods include sandblasting and solvent treatment. These surface treatment methods are appropriately selected depending on the type of substrate 11. As an example, a plastic film, particularly a polyethylene terephthalate film, on which an easy-adhesion layer has been formed by a primer treatment is preferably used.
[0025] The thickness of the substrate 11 is not particularly limited, but considering the use in a touch panel, it is preferably 25 to 500 μm, more preferably 38 to 400 μm, and even more preferably 50 to 300 μm.
[0026] 1-2. Writing Experience Improving Layer (1) Material of Writing Experience Improving Layer The writing experience improving layer 12 of the writing experience improving sheet 1 in this embodiment may be formed from any material as long as it contains at least one of a plasticizer and porous microparticles and satisfies the aforementioned dynamic friction coefficient, but is preferably formed by curing a coating composition C described below. Coating composition C makes it easy to form a writing experience improving layer 12 that satisfies the aforementioned dynamic friction coefficient and is fingerprint-resistant. Note that, from the perspective of the SDGs, the material constituting the writing experience improving layer 12 may be a material with a high biomass content, a material that can be recycled or reused, or a recycled or reused material.
[0027] The coating composition C in this embodiment preferably contains a curable component, at least one of a plasticizer and porous microparticles, and a filler (excluding the porous microparticles), or a curable component, a plasticizer, and porous microparticles, and more preferably a curable component, a plasticizer, and a filler, which makes it easier to form a writing feel improving layer 12 that satisfies the aforementioned dynamic friction coefficient and can exhibit better fingerprint resistance.
[0028] (1-1) Curable Component The curable component is a component that is cured by a trigger such as active energy rays or heat, and examples thereof include an active energy ray-curable component, a thermosetting component, etc. In the present embodiment, it is preferable to use an active energy ray-curable component from the viewpoints of the hardness of the writing feel improving layer 12 to be formed, the heat resistance of the substrate 11 (plastic film), etc.
[0029] The active energy ray-curable component is preferably one that cures upon irradiation with active energy rays and does not inhibit the sebum absorption function of the plasticizer or porous fine particles.
[0030] Specific examples of the active energy ray-curable component include polyfunctional (meth)acrylate monomers, (meth)acrylate prepolymers, and active energy ray-curable polymers. Among these, polyfunctional (meth)acrylate monomers or (meth)acrylate prepolymers are more preferred. The polyfunctional (meth)acrylate monomers and (meth)acrylate prepolymers may be used alone or in combination. In this specification, the term "(meth)acrylate" refers to both acrylate and methacrylate. The same applies to other similar terms.
[0031] Examples of polyfunctional (meth)acrylate monomers include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified phosphate di(meth)acrylate, allylated cyclohexyl di(meth)acrylate, isocyanurate di(meth)acrylate, and trimethylolpropane tri(meth)acrylate. Examples of the polyfunctional (meth)acrylate include polyfunctional (meth)acrylates such as acrylate, dipentaerythritol tri(meth)acrylate, propionic acid-modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, tris(acryloxyethyl)isocyanurate, propionic acid-modified dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ethylene oxide-modified dipentaerythritol hexa(meth)acrylate, and caprolactone-modified dipentaerythritol hexa(meth)acrylate. These may be used alone or in combination of two or more.
[0032] Examples of the (meth)acrylate prepolymer include polyester acrylate, epoxy acrylate, urethane acrylate, and polyol acrylate prepolymers.
[0033] The polyester acrylate prepolymer can be obtained, for example, by esterifying the hydroxyl groups of a polyester oligomer having hydroxyl groups at both ends, which is obtained by condensation of a polycarboxylic acid and a polyhydric alcohol, with (meth)acrylic acid, or by esterifying the terminal hydroxyl groups of an oligomer obtained by adding an alkylene oxide to a polycarboxylic acid, with (meth)acrylic acid.
[0034] Epoxy acrylate prepolymers can be obtained, for example, by reacting (meth)acrylic acid with the oxirane ring of a relatively low molecular weight bisphenol epoxy resin or novolac epoxy resin to esterify it.
[0035] The urethane acrylate prepolymer can be obtained, for example, by esterifying a polyurethane oligomer obtained by reacting a polyether polyol or polyester polyol with a polyisocyanate with (meth)acrylic acid.
[0036] The polyol acrylate prepolymer can be obtained, for example, by esterifying the hydroxyl groups of a polyether polyol with (meth)acrylic acid.
[0037] The above prepolymers may be used singly or in combination of two or more.
[0038] (1-2) Plasticizer A plasticizer is usually a material that softens resin, but in this embodiment, by having a plasticizer present in the writing feel improving layer 12, it can absorb sebum adhering to the surface of the writing feel improving layer 12.
[0039] Examples of the plasticizer include citric acid-based plasticizers such as acetyl tributyl citrate and acetyl triethyl citrate; phthalate ester-based plasticizers such as dimethyl phthalate, diethyl phthalate, dibutyl phthalate, dioctyl phthalate, di-n-octyl phthalate, and dicyclohexyl phthalate; trimellitate ester-based plasticizers such as trioctyl trimellitate, triisononyl trimellitate, and triisodecyl trimellitate; adipic acid-based plasticizers such as dioctyl adipate, diisononyl adipate, and diisodecyl adipate; polyester-based plasticizers such as phthalic acid-based polyesters; and triclay phosphate plasticizers. Examples of suitable plasticizers include phosphate ester plasticizers such as dimethylsilyl, trioctyl phosphate, and triphenyl phosphate; epoxy plasticizers such as epoxidized linseed oil and epoxidized butyl stearate; saturated alkanediol ester plasticizers such as 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate and 2,2,4-trimethyl-1,3-pentanediol diisobutyrate; liquid polybutene, mineral oil, lanolin, wax, liquid polyisoprene, liquid polyacrylate, triethanolamine, alkylamine, amine alkylene oxide adduct, glycerin, diglycerin, and silicone oil. These may be used alone or in combination of two or more.
[0040] Among the above, from the viewpoint of exhibiting sebum absorbency while maintaining good strength of the uneven shape for improving writing feel, citric acid-based plasticizers or saturated alkanediol ester-based plasticizers are preferred, and acetyl tributyl citrate or 2,2,4-trimethyl-1,3-pentanediol diisobutyrate are particularly preferred.
[0041] When coating composition C in this embodiment contains a plasticizer, the content thereof is preferably 0.1 to 100 parts by mass, more preferably 1 to 75 parts by mass, particularly preferably 3 to 50 parts by mass, even more preferably 5 to 30 parts by mass, and even more preferably 6 to 20 parts by mass, relative to 100 parts by mass of the curable component. This allows the coating composition C to effectively exhibit sebum absorbency while maintaining good strength of the uneven shape for improving the writing feel.
[0042] (1-3) Porous Microparticles By containing porous microparticles, the coating composition C can absorb sebum adhering to the surface of the writing feel improving layer 12. Furthermore, depending on the particle size, shape, amount of the porous microparticles, etc., the porous microparticles can also satisfy the above-mentioned dynamic friction coefficient. Note that the porous microparticles can also be used in combination with a plasticizer or a filler (excluding the porous microparticles).
[0043] The porous microparticles may have a pore structure that exhibits the desired sebum absorbency, and examples of such structures include micropores with a diameter of 2 nm or less, mesopores with a diameter of 2 to 50 nm, and macropores with a diameter of 50 to 100 nm, depending on the properties of the porous material used. The pore structure can be confirmed, for example, by observing the surface of the microparticles using an electron microscope or the like.
[0044] Examples of porous microparticles having sebum-absorbing properties include microparticles made of porous materials such as carbon materials such as activated carbon, silica gel, zeolite, porous coordination polymers (PCPs), covalent organic frameworks (COFs), and metal organic frameworks (MOFs). These may be used alone or in combination of two or more.
[0045] The shape of the porous microparticles may be either regular or irregular, but when the porous microparticles are used to improve the writing feel (particularly when no filler is contained), regular shapes are preferred, and spherical shapes are particularly preferred.
[0046] When coating composition C contains a filler (excluding the porous microparticles) and the filler is used to improve the writing feel, the average particle size of the porous microparticles is preferably 0.01 to 20 μm, and particularly preferably 0.1 to 16 μm, from the viewpoint of preventing the filler from impairing the effect. This allows sebum absorbency to be effectively exhibited. Furthermore, when the porous microparticles are used to improve the writing feel (particularly when no filler is contained), the average particle size is preferably 1 to 12 μm, more particularly preferably 2 to 8 μm, and particularly preferably 3 to 5 μm. This makes it easier to satisfy the aforementioned dynamic friction coefficient while effectively exhibiting sebum absorbency.
[0047] The specific surface area of the porous particles is 100 to 10,000 m 2 / g, and particularly 500 to 8000m 2 / g, which allows the material to exhibit excellent sebum absorbency.
[0048] The pore volume of the porous microparticles is preferably 0.01 to 10 ml / g, and more preferably 0.1 to 5 ml / g, which allows the microparticles to exhibit excellent sebum absorption.
[0049] When coating composition C contains a filler (excluding the porous microparticles) and the filler is used to improve the writing feel, the content of the porous microparticles in coating composition C is preferably 0.01 to 50 parts by mass, and particularly preferably 0.1 to 30 parts by mass, relative to 100 parts by mass of the curable component. This allows sebum absorbency to be effectively exhibited. Furthermore, when the porous microparticles are used to improve the writing feel (particularly when no filler is contained), the content of the porous microparticles is preferably 1 to 50 parts by mass, more preferably 2 to 40 parts by mass, particularly preferably 3 to 30 parts by mass, and even more preferably 4 to 20 parts by mass, and of these, preferably 5 to 10 parts by mass, relative to 100 parts by mass of the curable component. This makes it easier to satisfy the aforementioned dynamic friction coefficient while effectively exhibiting sebum absorbency.
[0050] (1-4) Filler The coating composition C also preferably contains a filler (other than the porous fine particles). This makes it easier to satisfy the dynamic friction coefficient described above and provides the writing feel improving layer 12 with anti-glare properties.
[0051] Examples of fillers include inorganic fine particles such as silica, calcium carbonate, aluminum hydroxide, magnesium hydroxide, clay, talc, and titanium dioxide; organic fine particles such as acrylic resin, polystyrene resin, polyethylene resin, and epoxy resin; and fine particles made of silicon-containing compounds having an intermediate structure between inorganic and organic (for example, the Tospearl series, which are silicone resin fine particles manufactured by Momentive Performance Materials Japan, Inc.). These fillers may be used alone or in combination of two or more.
[0052] Examples of the fine particles made of the acrylic resin include those made of a homopolymer of methyl methacrylate and copolymers of methyl methacrylate with monomers such as vinyl acetate, styrene, methyl acrylate, and ethyl (meth)acrylate.
[0053] The shape of the filler may be a regular shape such as a sphere, or may be an unspecified shape. However, from the viewpoint of making it easier to satisfy the above-mentioned dynamic friction coefficient, a regular shape is preferable, and a spherical shape is particularly preferable.
[0054] As a specific filler, it is preferable to use regular-shaped fine particles (e.g., silicone resin fine particles) made of a silicon-containing compound having an intermediate structure between inorganic and organic, and it is particularly preferable to use spherical silicone resin fine particles, which makes it easier to satisfy the above-mentioned dynamic friction coefficient.
[0055] The refractive index of the filler is preferably 1.2 to 3, more preferably 1.3 to 2, particularly preferably 1.35 to 1.6, and even more preferably 1.4 to 1.5, which makes it easier to achieve the desired optical properties.
[0056] The average particle size of the filler is preferably 0.1 to 20 μm, more preferably 1 to 12 μm, particularly preferably 2 to 8 μm, and even more preferably 3 to 5 μm. This makes it easier to meet the aforementioned dynamic friction coefficient and provides good anti-glare properties. It also prevents the plasticizer and porous microparticles from interfering with the sebum absorption function. The average particle size of the filler is measured by centrifugal sedimentation light transmission method.
[0057] The filler is preferably silica nanoparticles. The use of silica nanoparticles makes it easier to satisfy the above-mentioned dynamic friction coefficient. The average particle size of the silica nanoparticles is preferably 1 to 200 nm, more preferably 5 to 100 nm, and even more preferably 10 to 50 nm. The average particle size of the silica nanoparticles is measured by dynamic light scattering.
[0058] The silica nanoparticles may be modified with an organic substance to improve dispersibility. The silica nanoparticles are also preferably in the form of an organosol (colloidal). The organosol improves the dispersibility of the silica nanoparticles, improving the uniformity and light transmittance of the resulting writing feel improving layer 12.
[0059] The modification with an organic substance can be carried out by a conventional method. For example, CH 2 =C(CH 3 ) COO(CH 2 ) 3 Si(OCH 3 ) 3 The surface of the silica particles can be modified by adding a silane coupling agent having the above structure to an organosol of silica nanoparticles, heating the mixture to about 50° C., and stirring for several hours. The structure and amount of the silane coupling agent to be used are appropriately selected depending on the required degree of dispersibility of the silica nanoparticles.
[0060] As the dispersion solvent for the organosol, methyl ethyl ketone, methyl isobutyl ketone, etc., which have excellent compatibility with the polyfunctional (meth)acrylate and the leveling agent and excellent volatility when the writing feel improving layer 12 is formed, are preferred.
[0061] As the silica nanoparticles, commercially available products can be used, and among them, organosilica sol MEK-ST, MIBK-ST, etc. manufactured by Nissan Chemical Industries, Ltd. are preferably used.
[0062] When coating composition C contains a filler (including silica nanoparticles), the content thereof is preferably 1 to 50 parts by mass, more preferably 2 to 40 parts by mass, particularly preferably 3 to 30 parts by mass, even more preferably 4 to 20 parts by mass, and most preferably 5 to 10 parts by mass, per 100 parts by mass of the curable component. This makes it easier to satisfy the dynamic friction coefficient described above and provides good anti-glare properties. Furthermore, the sebum absorption effect of the plasticizer and porous microparticles is prevented from being hindered.
[0063] (1-5) Photopolymerization Initiator When ultraviolet light is used to cure the active energy ray-curable component, the coating composition C preferably contains a photopolymerization initiator. By containing a photopolymerization initiator, the active energy ray-curable component can be polymerized efficiently, and the polymerization and curing time and the ultraviolet irradiation dose can be reduced.
[0064] Examples of such photopolymerization initiators include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)ketone, benzophenone, Examples of suitable benzoxanthone include benzophenone, p-phenylbenzophenone, 4,4'-diethylaminobenzophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyl dimethyl ketal, acetophenone dimethyl ketal, p-dimethylaminobenzoic acid ester, oligo[2-hydroxy-2-methyl-1[4-(1-methylvinyl)phenyl]propanone], 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, etc. These may be used alone or in combination of two or more.
[0065] When the coating composition C contains a photopolymerization initiator, the content thereof is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, and even more preferably 1 to 10 parts by mass, relative to 100 parts by mass of the active energy ray-curable component, which makes it easier for the resulting writing feel-improving layer to have the desired hardness.
[0066] (1-6) Antifouling Agent The coating composition C according to this embodiment preferably contains an antifouling agent. This makes the writing feel improving layer 12 formed excellent in antifouling properties, making it difficult for fingerprints and dirt to adhere to it.
[0067] Examples of the antifouling agent include a silicone-based antifouling agent, a fluorine-based antifouling agent, and an acrylic-based antifouling agent. Among these, it is preferable to use a fluorine-based antifouling agent from the viewpoint of making it difficult for fingerprints and stains to adhere. As the fluorine-based antifouling agent, a fluorine-based resin having a (meth)acrylate group polymerizable with the polyfunctional (meth)acrylate monomer or (meth)acrylate prepolymer as the curable component described above is preferred.
[0068] When coating composition C contains an antifouling agent, the content thereof is preferably 0.01 to 30 parts by mass, more preferably 0.05 to 20 parts by mass, particularly preferably 0.1 to 10 parts by mass, even more preferably 0.3 to 5 parts by mass, and of these, preferably 0.5 to 2 parts by mass, relative to 100 parts by mass of the curable component. This makes it difficult for fingerprints and dirt to adhere, allowing the surface to maintain good condition and preventing deterioration of the writing feel and finger smoothness due to dirt.
[0069] (1-7) Leveling Agent The coating composition C according to this embodiment preferably contains a leveling agent. This allows the writing feel improving layer 12 to have a uniform thickness without streak-like defects or unevenness, and to exhibit excellent optical properties and appearance.
[0070] Examples of the leveling agent include silicone-based leveling agents, fluorine-based leveling agents, acrylic-based leveling agents, and vinyl-based leveling agents. Among these, silicone-based leveling agents and fluorine-based leveling agents are preferred from the viewpoints of leveling properties and compatibility with other components. The leveling agents may be used alone or in combination of two or more.
[0071] The leveling agent may be modified or unmodified, and may have a reactive group or may not have a reactive group.
[0072] When coating composition C contains a leveling agent, the content thereof is preferably 0.01 to 5.0 parts by mass, more preferably 0.05 to 3.0 parts by mass, particularly preferably 0.1 to 1.0 part by mass, and even more preferably 0.2 to 0.5 parts by mass, relative to 100 parts by mass of the curable component. This makes it possible to form a good surface condition that easily satisfies the above-mentioned physical properties, and achieves both excellent fingerprint resistance and a smooth writing feel.
[0073] (1-8) Other Components In addition to the above components, the coating composition C of the present embodiment may contain various additives. Examples of the various additives include dispersants, ultraviolet absorbers, infrared absorbers, antioxidants, light stabilizers, antistatic agents, silane coupling agents, antiaging agents, thermal polymerization inhibitors, colorants, refractive index modifiers, surfactants, storage stabilizers, plasticizers, lubricants, and antifoaming agents.
[0074] (2) Thickness The thickness of the writing feel improving layer 12 is preferably 0.5 to 50 μm, more preferably 1.0 to 30 μm, particularly preferably 1.5 to 20 μm, even more preferably 2.0 to 12 μm, and even more preferably 2.5 to 9.0 μm, most preferably 3.0 to 6.0 μm. This makes it easier to satisfy the dynamic friction coefficient described above and also improves fingerprint resistance.
[0075] When the thickness of the writing feel improving layer 12 is α (μm) and the average particle size of the filler is β (μm), the value of β / α preferably satisfies 0.001 to 100, more preferably satisfies 0.01 to 50, particularly preferably satisfies 0.1 to 10, even more preferably satisfies 0.5 to 5, more preferably satisfies 0.8 to 2, and most preferably satisfies 0.9 to 1.1. This makes it easier to satisfy the dynamic friction coefficient described above and to adjust optical properties such as haze value to desired values.
[0076] 1-3. Other Configurations The writing feel improving sheet 1 according to this embodiment may include an adhesive layer on the surface of the substrate 11 opposite the writing feel improving layer 12. The adhesive that constitutes the adhesive layer is not particularly limited, and known adhesives such as acrylic adhesives, rubber adhesives, and silicone adhesives can be used, and it is preferable to use an adhesive having a predetermined transparency.
[0077] When the writing feel improving sheet 1 according to the present embodiment includes the above-described adhesive layer, the writing feel improving sheet 1 according to the present embodiment may have a release film laminated on the surface of the adhesive layer opposite to the substrate 11. The release film is not particularly limited as long as it has the desired releasability on its release surface (the surface in contact with the adhesive layer), and any known release film, such as a resin film having one surface subjected to a release treatment with a release agent, can be used.
[0078] 2. Manufacturing Method of Writing Feel Improving Sheet The writing feel improving sheet 1 according to this embodiment can be manufactured by applying a coating liquid containing a coating composition for the writing feel improving layer 12, preferably coating composition C, and optionally a solvent, to the substrate 11 and curing it to form the writing feel improving layer 12.
[0079] The solvent can be used to improve coatability, adjust viscosity, adjust solid content concentration, etc., and any solvent can be used without particular limitation as long as it dissolves or disperses each component. Specific examples of the solvent include alcohols such as methanol, ethanol, isopropanol, butanol, and octanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; esters such as ethyl acetate, butyl acetate, ethyl lactate, and γ-butyrolactone; ethers such as ethylene glycol monomethyl ether (methyl cellosolve), ethylene glycol monoethyl ether (ethyl cellosolve), diethylene glycol monobutyl ether (butyl cellosolve), and propylene glycol monomethyl ether; aromatic hydrocarbons such as benzene, toluene, and xylene; and amides such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone.
[0080] The coating composition may be applied by a conventional method, such as bar coating, knife coating, roll coating, blade coating, die coating, or gravure coating. After the coating composition is applied, the resulting film is preferably dried at 40 to 120°C for about 30 seconds to 5 minutes.
[0081] Here, when the coating composition contains a leveling agent, the coating film applied with the coating composition will be free of streak-like defects and unevenness, and therefore a writing feel improving layer 12 with a uniform film thickness and excellent appearance can be formed.
[0082] When the coating composition is active energy ray-curable, such as coating composition C, the coating composition is cured by irradiating the coating film of the coating composition with active energy rays such as ultraviolet rays or electron beams. The ultraviolet irradiation can be carried out using a high-pressure mercury lamp, a Heraeus H lamp, a xenon lamp, or the like, and the irradiation dose of the ultraviolet rays is an illuminance of 50 to 1000 mW / cm. 2 , light intensity 50-1000mJ / cm 2 On the other hand, electron beam irradiation can be carried out using an electron beam accelerator or the like, and the dose of electron beam irradiation is preferably about 10 to 1000 krad.
[0083] The coating film of the coating composition can be irradiated with active energy rays in an air atmosphere or an inert gas atmosphere. Depending on the type of active energy ray-curable component, the coating composition can be cured well without being inhibited by oxygen by irradiating with active energy rays in an inert gas atmosphere.
[0084] Examples of inert gases include nitrogen, argon, and helium, with nitrogen and argon being preferred, and nitrogen being particularly preferred. The oxygen concentration in the inert gas atmosphere is preferably 5% or less, more preferably 3% or less, and particularly preferably 2% or less.
[0085] 3. Physical Properties of the Writing Experience Improving Sheet (1) Dynamic Friction Coefficient When a 0.2% by mass ethanol solution of oleic acid (artificial sebum liquid) is applied to the surface of the writing experience improving layer 12 of the writing experience improving sheet 1 according to this embodiment, which comes into contact with a touch pen, using a wire bar #2 and allowed to dry naturally, the dynamic friction coefficient (post-application dynamic friction coefficient) measured 24 hours after application of the artificial sebum liquid using the same measurement method as described above is preferably 0.12 or more, more preferably 0.14 to 0.80, particularly preferably 0.16 to 0.60, and even more preferably 0.18 to 0.40, and most preferably 0.19 to 0.30. As a result, even after application of the artificial sebum liquid, an excellent writing experience improvement effect can be obtained 24 hours later. In other words, with this writing experience improving sheet 1, even if fingerprints caused by sebum are left behind, there is no need to wipe off the fingerprints, and writing experience is less likely to deteriorate.
[0086] Furthermore, the ratio of the kinetic friction coefficient after application to the kinetic friction coefficient before application of the artificial sebum liquid (kinetic friction coefficient before application; the kinetic friction coefficient described above) (kinetic friction coefficient ratio; kinetic friction coefficient after application / kinetic friction coefficient before application) is preferably 0.85 or more, more preferably 0.90 or more, particularly preferably 0.95 or more, and even more preferably 0.98 or more. Such a large kinetic friction coefficient ratio results in small changes in the kinetic friction coefficient, and it can be said that the artificial sebum liquid is absorbed into the writing feel improving layer 12 over time. Therefore, in such a writing feel improving sheet 1, even if fingerprints caused by sebum are left, there is no need to wipe off the fingerprints, and the writing feel is unlikely to deteriorate. Note that the upper limit of the kinetic friction coefficient ratio is not particularly limited, but from the viewpoint of realizing a writing feel equivalent to that before sebum is attached, it is preferably 1.5 or less, more preferably 1.3 or less, particularly preferably 1.1 or less, and even more preferably 1.05 or less.
[0087] (2) Haze Value The haze value of the writing feel improving sheet 1 according to this embodiment is preferably 0 to 50%, more preferably 0.1 to 30%, particularly preferably 0.5 to 20%, and even more preferably 1 to 15%. This makes it particularly suitable for optical applications. The haze value in this specification is a value measured in accordance with JIS K7136:2000.
[0088] (3) Haze Value Change When a 0.2% by mass ethanol solution of oleic acid (artificial sebum liquid) is applied to the surface of the writing feel improving layer 12 of the writing feel improving sheet 1 according to this embodiment, which is in contact with a touch pen, using a wire bar #2 and allowed to dry naturally, the haze value change (points) obtained by subtracting the haze value (%) before application from the haze value (%) 24 hours after application of the artificial sebum liquid is preferably 1.5 points or less as an upper limit, more preferably 1.2 points or less, particularly preferably 0.9 points or less, and even more preferably 0.6 points or less, and most preferably 0.3 points or less, with a lower limit of 0.0 points being the most preferable. Because the haze value change is as small as described above, it can be said that the artificial sebum liquid is absorbed into the writing feel improving layer 12 over time, and therefore, even if fingerprints are left on the surface of the writing feel improving sheet 1 (writing feel improving layer 12), the fingerprints become invisible over time.
[0089] (4) Evaluation of Scratch Resistance The surface of the writing feel improving layer 12 of the writing feel improving sheet 1 according to this embodiment was scratched with #0000 steel wool at 125 g / cm 2 The number of scratches that occur when rubbing 10 cm back and forth five times under a load of 10 ...
[0090] (5) Contact Angle The oleic acid contact angle on the surface of the writing feel improving layer 12 of the writing feel sheet 1 according to this embodiment is preferably 30° to 100°, more preferably 40° to 90°, particularly preferably 50° to 80°, even more preferably 60° to 70°, and even more preferably 62° to 67°. This facilitates good finger slippage when operating a touch panel with a finger, resulting in excellent touch panel operability. In particular, in combination with the aforementioned dynamic friction coefficient, it is possible to achieve both a good writing feel with a touch pen and ease of use with a finger. The oleic acid contact angle refers to the angle on the side including the droplet, when a droplet of oleic acid is placed on the surface of the writing feel improving layer, between the tangent of the droplet at the contact portion of the writing feel improving layer surface and the surface of the writing feel improving layer.
[0091] The water contact angle on the surface of the writing feel improving layer 12 of the writing feel improving sheet 1 according to this embodiment is preferably 60° to 120°, more preferably 70° to 110°, particularly preferably 80° to 106°, even more preferably 90° to 102°, and most preferably 92° to 99°. This facilitates good finger slippage when operating the touch panel with a finger, making the touch panel more operable. In particular, in combination with the aforementioned dynamic friction coefficient, it is possible to achieve both a good writing feel with a touch pen and operability with a finger. The detailed method for measuring the contact angle is as shown in the test examples described below.
[0092] (6) Surface Free Energy The surface free energy of the surface of the writing feel improving layer 12 of the writing feel improving sheet 1 according to this embodiment is 15 to 50 mJ / m 2 is preferably 18 to 40 mJ / m 2 More preferably, it is 20 to 30 mJ / m 2 It is preferable that the luminance is 21 to 25 mJ / m 2It is preferable that the surface of the surface is such that the surface of ...
[0093] 4. Use of the Writing Experience Improving Sheet The writing experience improving sheet 1 according to this embodiment can be used as a sheet constituting the outermost layer of a touch panel (image display device with position detection function) in which a touch pen is used. Specifically, it is preferably used by being laminated on a cover material in a touch panel having a display module such as a liquid crystal (LCD) module, a light-emitting diode (LED) module, or an organic electroluminescence (organic EL) module, or a touch sensor. The writing experience improving sheet 1 is preferably laminated on the cover material by being attached via the aforementioned adhesive layer.
[0094] The touch pen used with the writing feel improving sheet 1 according to this embodiment is not particularly limited, and conventionally known touch pens can be used. For example, touch pens with polyacetal nibs, hard felt nibs, elastomer nibs, etc. can be used. The shape of the touch pen nib is also not particularly limited, and can be appropriately selected from disk-shaped, circular, polygonal, etc., but a circular nib is preferred from the perspective of providing a sense of resistance and vibration when writing with a pencil. When the touch pen nib is circular, the diameter of the nib is preferably 0.1 to 5 mm, more preferably 0.2 to 2 mm, and even more preferably 0.3 to 1 mm.
[0095] 5. Touch Panel with Writing Experience Improvement Sheet By laminating the writing experience improvement sheet according to the embodiment described above on a touch panel, a touch panel with a writing experience improvement sheet (including the concept of a display body with a touch panel component) can be obtained. Specifically, the touch panel with writing experience improvement sheet comprises a writing experience improvement sheet having a touch pen contact surface that comes into contact with a touch pen, and a touch panel, with the side of the writing experience improvement sheet opposite the touch pen contact surface laminated on the display surface side of the touch panel. The writing experience improvement sheet may be laminated directly on the display surface of the touch panel, or may be laminated on the display surface side of the touch panel via another member or layer.
[0096] The type and type of the touch panel are not particularly limited, and for example, capacitive, electromagnetic induction, resistive, surface acoustic wave (ultrasonic), infrared, and other touch panels can be used. Among these, capacitive touch panels are preferred from the viewpoint of easily reproducing an excellent writing feel, and capacitive touch panels that also incorporate electromagnetic induction are particularly preferred when taking into account the reproducibility of characters and the like written with a touch pen. The specific configurations of the capacitive and electromagnetic induction touch panels are not particularly limited, and conventionally known touch panels can be used.
[0097] The above-described embodiments have been described to facilitate understanding of the present invention, and are not intended to limit the present invention. Therefore, each element disclosed in the above embodiments is intended to include all design modifications and equivalents that fall within the technical scope of the present invention.
[0098] For example, another layer may be interposed between the substrate 11 and the writing feel improving layer 12 in the writing feel improving sheet 1. Furthermore, another layer, such as a hard coat layer, may be provided on the surface of the substrate 11 opposite the writing feel improving layer 12.
[0099] In this specification, when it is stated that "X to Y" (X and Y are any numbers), it means "X or more and Y or less" unless otherwise specified, and also means "preferably greater than X" or "preferably smaller than Y". Furthermore, when it is stated that "X or more" (X is any number), it means "preferably greater than X" unless otherwise specified, and when it is stated that "Y or less" (Y is any number), it also means "preferably smaller than Y" unless otherwise specified.
[0100] The present invention will be explained in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.
[0101] Example 1 A mixture of 100 parts by mass of a polyfunctional urethane acrylate (manufactured by Arakawa Chemical Industries, Ltd., product name "Opstar Z7530") as an active energy ray-curable component (urethane acrylate-based prepolymer), 7.2 parts by mass of acetyl tributyl citrate as a plasticizer, and fine particles (manufactured by Momentive Performance Materials Japan, product name "Tospearl 145L", average particle size: 4.5 μm, refractive index: 1) made of a silicone resin (a silicon-containing compound having an intermediate structure between inorganic and organic) as a filler was used. .43) 6.8 parts by mass (expressed as a solid content equivalent; the same applies to other components), 3 parts by mass of 1-hydroxycyclohexyl phenyl ketone as a photopolymerization initiator, 0.7 parts by mass of a fluorine-based resin (manufactured by DIC Corporation, product name "Megafac RS-90") as an antifouling agent, and 0.2 parts by mass of polydimethylsiloxane (manufactured by Dow-Toray Industries, product name "SH28") as a silicone-based leveling agent were mixed in propylene glycol monomethyl ether to obtain a coating liquid of the coating composition.
[0102] The coating liquid of the coating composition obtained above was applied to the surface of the easy-adhesion layer side of a polyester film with an easy-adhesion layer (manufactured by Toray Industries, Inc., product name "Lumirror U40", thickness: 125 μm) as a substrate, and dried at 70° C. for 1 minute.
[0103] Next, under a nitrogen atmosphere, ultraviolet light was irradiated using an ultraviolet irradiation device (manufactured by Eye Graphics, product name "Eigrantage ECS-401GX type") under the following conditions to form a writing feel improving layer having a thickness of 4.5 μm on the substrate, thereby obtaining a writing feel improving sheet. [Ultraviolet light irradiation conditions] Light source: high-pressure mercury lamp Lamp power: 2 kW Conveyor speed: 4.23 m / min Illuminance: 300 mW / cm 2 ・Light intensity: 250mJ / cm 2
[0104] Examples 2 to 4, Comparative Examples 1 to 3 Writing feel improving sheets were produced in the same manner as in Example 1, except that the blend amount of plasticizer and the thickness of the writing feel improving layer were changed as shown in Table 1.
[0105] [Test Example 1] (Quantitative evaluation of fingerprint resistance) A 0.2% by mass ethanol solution of oleic acid as a pseudo-sebum liquid was applied to the surface of the writing feel improving layer of each of the writing feel improving sheets manufactured in the Examples and Comparative Examples using a wire bar #2, and then allowed to dry naturally. Note that the oleic acid used was oleic acid manufactured by Tokyo Chemical Industry Co., Ltd.
[0106] For the above-mentioned writing feel improving sheet, before application of the artificial sebum liquid, immediately after application, and after 24 hours of application, the haze value (%) is measured according to JIS K7136:2000 using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "NDH5000").In addition, the haze value change (point) is calculated by subtracting the haze value (%) before application from the haze value (%) immediately after application of the artificial sebum liquid, and the haze value change (point; quantitative evaluation of fingerprint resistance) is calculated by subtracting the haze value (%) before application from the haze value (%) after 24 hours of application of the artificial sebum liquid.The respective results are shown in Table 2.
[0107] Test Example 2 (Sensory Evaluation of Fingerprint Resistance) Fingerprints made from finger sebum were left on the surface of the writing feel improving layer of the writing feel improving sheets produced in the Examples and Comparative Examples. 24 hours later, the surface of the writing feel improving layer of the writing feel improving sheet was visually inspected under a three-wavelength fluorescent lamp, and the fingerprint resistance was evaluated sensorily according to the following criteria. The results are shown in Table 1. ⊚: Fingerprints were barely visible. ◯: Fingerprints were inconspicuous. Δ: Fingerprints were slightly noticeable. ×: Fingerprints were clearly visible.
[0108] [Test Example 3] (Measurement of dynamic friction coefficient) The substrate side of the writing feel improving sheet produced in the examples and comparative examples was attached to one side of a glass plate (thickness: 1.2 mm) via a double-sided adhesive sheet, and this was used as a measurement sample.
[0109] The measurement sample was placed on a measurement cart of a static and dynamic friction tester (manufactured by Trinity Lab, product name "Tribomaster TL201Ts") with the writing feel improving layer side (touch pen contact surface) facing up. Note that the measurement cart moves linearly back and forth in a predetermined direction while maintaining the horizontality of the installation surface of the measurement sample when the static and dynamic friction tester is used.
[0110] Next, the touch pen was fixed to the static and dynamic friction measuring device so that the pen tip was in contact with the touch pen contact surface. At this time, the touch pen was fixed at an angle so that the angle between the touch pen and the touch pen contact surface was 45°. At this time, the rear end side of the touch pen was inclined toward the traveling direction of the measurement dolly, and the direction of inclination in a plan view was parallel to the traveling direction. As the touch pen, a touch pen with a hard felt tip (manufactured by Wacom Co., Ltd., product name "ACK-20003", pen tip diameter: 0.5 mm) was used.
[0111] Next, with a load of 200 g applied to the touch pen, the measurement cart was moved at a speed of 1.6 mm / sec to slide the touch pen on the touch pen contact surface (sliding distance: 100 mm), and the dynamic friction coefficient (dynamic friction coefficient before application) was calculated based on the friction force measured at that time. The results are shown in Table 2.
[0112] Next, a 0.2% by mass ethanol solution of oleic acid as a pseudo-sebum liquid was applied to the surface of the writing feel improving layer of each of the writing feel improving sheets produced in the Examples and Comparative Examples using a wire bar #2, and then allowed to dry naturally. Note that the oleic acid used was that manufactured by Tokyo Chemical Industry Co., Ltd.
[0113] Twenty-four hours after application of oleic acid, the dynamic friction coefficient (dynamic friction coefficient after application) was calculated in the same manner as above. The ratio of the dynamic friction coefficient after application to the dynamic friction coefficient before application (dynamic friction coefficient ratio; dynamic friction coefficient after application / dynamic friction coefficient before application) was also calculated. The results are shown in Table 2.
[0114] Test Example 4 (Evaluation of Finger Smoothness) A finger was slid over the surface of the writing feel improving layer of the writing feel improving sheets produced in the Examples and Comparative Examples, and finger smoothness was evaluated according to the following criteria. The easier it was for the finger to slide, the easier it was for the touch panel to be operable with the finger. The results are shown in Table 2. ⊚: Finger slid very easily. ◯: Finger slid. Δ: Finger did not slide easily. ×: Finger did not slide at all.
[0115] Test Example 5 (Sensory Evaluation of Writing Feel) The writing feel improving sheets produced in the Examples and Comparative Examples were placed on a glass substrate with the writing feel improving layer side facing up. A panelist simulated a predetermined writing task on the surface of the writing feel improving layer of the writing feel improving sheet using a touch pen with a hard felt tip (manufactured by Wacom Co., Ltd., product name "ACK-20003", pen tip diameter: 0.5 mm) to evaluate the writing feel as follows (before application). The evaluation results based on the panelists' evaluations and the following criteria are shown in Table 2. The evaluation of each writing feel was based on the writing feel when writing on five sheets of paper (manufactured by Kokuyo S&T Co., Ltd., product name "Campus Notebook A Ruled No. 201A") using a pencil (manufactured by Mitsubishi Pencil Co., Ltd., product name "Mitsubishi Pencil Uni B") with a writing pressure of 200 g. The results are shown in Table 2.
[0116] (1) Resistance Resistance as a writing feel was evaluated according to the following criteria: A: There was a moderate resistance when writing, and the pen did not slide easily. F1: There was some resistance when writing, and the pen did not slide easily. F2: There was too little resistance when writing, and the pen slid easily.
[0117] (2) Vibration Sensation The vibration sensation as a writing experience was evaluated according to the following criteria: A: Moderate vibration was transmitted to the hand. F1: The vibration transmitted to the hand was too small. F2: The vibration transmitted to the hand was too large.
[0118] Next, a 0.2% by mass ethanol solution of oleic acid as a pseudo-sebum liquid was applied to the surface of the writing feel improving layer of the writing feel improving sheets produced in the Examples and Comparative Examples using a wire bar #2, followed by air drying. The oleic acid used was oleic acid manufactured by Tokyo Chemical Industry Co., Ltd. 24 hours after application of the oleic acid, the writing feel was evaluated in the same manner as above (after application). The results are shown in Table 2.
[0119] Test Example 6 (Evaluation of Scratch Resistance) The surface of the writing feel improving layer of each of the writing feel improving sheets produced in the Examples and Comparative Examples was scratched with #0000 steel wool at a rate of 125 g / cm. 2 The sheet was rubbed five times back and forth over a distance of 10 cm under a load of 0.5 g. The surface of the writing feel improving sheet was visually inspected under a three-wavelength fluorescent lamp, and the scratch resistance was evaluated according to the following criteria. The results are shown in Table 2. ⊚: No scratches were found. ◯: 1 to 3 scratches were found. △: 4 to 10 scratches were found. ×: 11 or more scratches were found.
[0120] Test Example 7 (Contact Angle Measurement) The contact angle of oleic acid on the surface of the writing feel improving layer of the writing feel improving sheets produced in the Examples and Comparative Examples was measured under the following conditions using a contact angle measuring meter (manufactured by Kyowa Interface Science Co., Ltd., product name "DM-701"). Note that oleic acid manufactured by Tokyo Chemical Industry Co., Ltd. was used as the oleic acid. The results are shown in Table 2. - Amount of oleic acid droplet: 2 μl - Measurement time: 3 seconds after dropping - Image analysis method: θ / 2 method
[0121] In the same manner as described above, the water contact angle on the surface of the writing feel improving layer of the writing feel improving sheets manufactured in the Examples and Comparative Examples was measured under the following conditions. The results are shown in Table 1. Water droplet volume: 2 μl Measurement time: 3 seconds after dropping Image analysis method: θ / 2 method
[0122] [Test Example 8] (Measurement of Surface Free Energy) The contact angles of various liquid droplets on the surface of the writing feel improving layer of the writing feel improving sheets produced in the Examples and Comparative Examples were measured, and the surface free energy (mJ / m) was calculated based on the measured values according to the Kitazaki-Hata theory. 2 ) was measured. The contact angle was measured using a contact angle meter (manufactured by Kyowa Interface Science Co., Ltd., product name "DM-701") by the sessile drop method in accordance with JIS R3257. For the droplets, diiodomethane was used as the "dispersion component" and 1-bromonaphthalene as the "dipole component" and distilled water as the "hydrogen bond component". The results are shown in Table 2.
[0123]
[0124]
[0125] As can be seen from Table 2, the quantitative evaluation of fingerprint resistance using oleic acid was consistent with the sensory evaluation of fingerprint resistance caused by actual sebum. Furthermore, the writing feel improving sheets produced in the examples provided a good writing feel with a touch pen, and even when fingerprints caused by sebum were left on the sheets, there was no need to wipe them off, and good writing feel performance was maintained over time.
[0126] The writing feel improving sheet of the present invention is suitably used as the outermost layer of a touch panel on which a touch pen is used.
[0127] 1... Writing feel improving sheet 11... Base material 12... Writing feel improving layer
Claims
1. A writing feel improving sheet comprising a substrate and a writing feel improving layer with which a touch pen comes into contact, the writing feel improving layer containing at least one of a plasticizer and a porous microparticle, the writing feel improving layer being characterized in that the tip of a touch pen having a diameter of 0.5 mm is brought into contact with the surface of the writing feel improving layer with which the touch pen comes into contact, and then a load of 200 g is applied to the touch pen while the touch pen is slid linearly at a speed of 1.6 mm / sec while maintaining the angle between the touch pen and the surface of the writing feel improving layer at 45°, and the dynamic friction coefficient measured is 0.12 or more.
2. The writing feel improving sheet according to claim 1, characterized in that a diluted solution of oleic acid is applied to the surface of the writing feel improving layer that comes into contact with the touch pen, the diluted solution is allowed to dry naturally, and the dynamic friction coefficient measured by the measuring method 24 hours after the application is 0.12 or more.
3. The writing feel improving sheet according to claim 1, characterized in that when the kinetic friction coefficient is the kinetic friction coefficient before application, a diluted solution of oleic acid is applied to the surface of the writing feel improving layer that comes into contact with a touch pen, the solution is allowed to dry naturally, and the kinetic friction coefficient measured 24 hours after application using the measurement method is taken as the kinetic friction coefficient after application, the ratio of the kinetic friction coefficient after application to the kinetic friction coefficient before application is 0.85 or more.
4. The writing feel improving sheet according to claim 1, characterized in that the writing feel improving layer is a layer formed by curing a coating composition containing a hardening component, at least one of the plasticizer and porous microparticles, and a filler (excluding the porous microparticles).
5. The writing feel improving sheet according to claim 1, characterized in that the writing feel improving layer is a layer formed by curing a coating composition containing a hardenable component, the plasticizer, and the porous microparticles.
6. The surface of the writing feel improving layer is subjected to a test with a thickness of 125 g / cm using #0000 steel wool. 2 2. The sheet for improving writing feel according to claim 1, characterized in that the number of scratches caused when rubbed 5 times back and forth over a distance of 10 cm under a load of 100 mm is 10 or less.
Citation Information
Patent Citations
Hard coat film and production method thereof
JP2014237250A
Writing feeling enhancement sheet
JP2020049917A
Writability improvement sheet
JP2022124137A
Surface material for pen input device
WO2020213156A1