Composite oxide particles
Polycrystalline composite oxide particles with a low thermal expansion coefficient and specific properties are produced to address the issue of particle adhesion and thermal expansion in semiconductor packaging, ensuring stability and visibility in semiconductor substrates.
Patent Information
- Application Number
- PCT/JP2024/004493
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-02-09
- Publication Date
- 2024-10-03
AI Technical Summary
Existing composite oxide particles with a cordierite component have a low softening point, causing them to stick together and lose their spherical structure, making them unsuitable for use as a powdered inorganic filler in semiconductor packaging due to high thermal expansion coefficients.
Development of polycrystalline composite oxide particles with a main crystal phase of cordierite or indialite, having a thermal expansion coefficient of 1.5 ppm or less, spherical shape, and a specific particle size distribution, which are produced by mixing cordierite particles with nanoparticles and heating them within a specific temperature range to maintain their crystallinity and shape.
The resulting particles are highly crystalline, spherical, and have a low thermal expansion coefficient, allowing them to prevent warping in semiconductor substrates and remain colorless for easier defect identification, while maintaining their spherical shape and high crystallinity.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
composite oxide particles
[0001] The present invention relates to composite oxide particles.
[0002] In recent years, various next-generation semiconductor packaging materials have been studied. For example, Patent Document 1 describes a crystallized glass containing at least one crystal of cordierite and its polymorph, indialite. The crystallized glass described in Patent Document 1 is described as being useful, for example, as a component of a high-frequency electronic device on a high-frequency substrate.
[0003] The softening point of the composite oxide containing the cordierite component is relatively low, at around 900°C. Therefore, when the indialite phase, a crystalline polymorph of cordierite, begins to form, the particles adhere to each other and form clumps, making it impossible to maintain a particulate (spherical) structure. Therefore, the crystallized glass described in Patent Document 1 cannot be used in a powdery, spherical form like an inorganic filler.
[0004] International Publication No. 2022 / 059724
[0005] An object of the present invention is to provide composite oxide particles that are spherical, highly crystalline, whitish, and have a low coefficient of thermal expansion.
[0006] The present inventors have conducted extensive research to solve the above problems, and as a result have found the following solutions, which have led to the completion of the present invention. (1) Composite oxide particles that are polycrystalline and contain at least one of cordierite and indialite as a main crystalline phase, and have a thermal expansion coefficient of 1.5 ppm or less as measured by a TMA method. (2) Composite oxide particles according to (1) above, having a particle diameter of 0.1 μm or more and 500.0 μm or less. (3) Composite oxide particles according to (1) or (2) above, which have a crystallinity of 40 or more as calculated by the following formula (I) when measured by X-ray diffraction at a diffraction angle 2θ in the range of 15 to 40°. Crystallinity = crystalline peak area / (crystalline peak area + amorphous peak area) (I) (4) The composite oxide particles according to any one of (1) to (3) above, wherein in a particle size distribution measured by a laser diffraction method, the difference D90 - D10 between the particle size D90, which is the 90% cumulative diameter, and the particle size D10, which is the 10% cumulative diameter, is 1000.0 μm or less. (5) The composite oxide particles according to any one of (1) to (4) above, wherein the circularity is 0.70 or more. (6) The composite oxide particles according to any one of (1) to (5) above, wherein the half-width of the main crystalline peak in the diffraction angle 2θ range of 27.5 to 29.5°, as measured by an X-ray diffraction method, is 0.20° or less. (7) The composite oxide particles according to any one of (1) to (6) above, wherein the nanoparticles are contained in an amount of 0.1% by mass or more and 30% by mass or less. (8) Composite oxide particles according to any one of (1) to (7) above, wherein L* in the L*a*b* color space is 91.00 or more and 100.00 or less, a* is -10.00 or more and 3.00 or less, and b* is -10.00 or more and 5.00 or less. (9) A method for producing composite oxide particles, comprising the steps of mixing cordierite particles and nanoparticles to obtain mixed particles, and heating the mixed particles. (10) The production method according to (9) above, wherein the heating step is carried out at 1000°C or more and 1400°C or less.
[0007] The composite oxide particles according to the present invention are spherical, highly crystalline, whitish, and have a low coefficient of thermal expansion. Therefore, the composite oxide particles according to the present invention can be dispersed in a substrate to efficiently prevent thermal warping of, for example, a semiconductor package substrate. Furthermore, because the composite oxide particles according to the present invention are whitish, they do not become discolored even when used in a semiconductor package substrate. As a result, defects and stains occurring on the semiconductor package substrate can be easily optically identified.
[0008] The composite oxide particles according to the present invention are polycrystalline and contain at least one of cordierite and indialite as a main crystalline phase, i.e., contain a plurality of fine single crystals (crystal grains) of at least one of cordierite and indialite.
[0009] Cordierite and indialite are compounds having a composition of 2MgO.2Al2O3.5SiO2 and have different crystal structures. Whether the main crystalline phase mainly contains cordierite or indialite is presumably dependent on, for example, the heating temperature (firing temperature) during production of the composite oxide particles according to the present invention. Specifically, heating at approximately 1000°C or higher and 1200°C or lower tends to produce composite oxide particles having the indialite phase as the main crystalline phase. On the other hand, heating at approximately 1200°C or higher and 1400°C or lower tends to produce composite oxide particles having the cordierite phase as the main crystalline phase.
[0010] The composite oxide particles according to the present invention have a thermal expansion coefficient of 1.5 ppm or less as measured by the TMA method. Because the thermal expansion coefficient is 1.5 ppm or less, when the composite oxide particles according to the present invention are dispersed in a semiconductor package substrate, for example, the substrate can be efficiently prevented from warping due to heat. The thermal expansion coefficient of the composite oxide particles according to the present invention as measured by the TMA method is preferably less than 0.0 ppm.
[0011] Thermomechanical analysis (TMA) is a method for measuring the thermal expansion of a test sample by measuring the difference in the amount of thermal expansion between a standard sample and a test sample when the sample is heated at a constant rate. Quartz glass, alumina, etc. are used as the standard sample.
[0012] The composite oxide particles according to the present invention may contain other crystalline phases or amorphous phases, as long as at least one of cordierite and indialite constitutes the main crystalline phase. The other crystalline phases and amorphous phases may remain as impurities (e.g., unavoidable impurities) at the grain boundaries of the main crystalline phase, or may be intentionally added to the extent that they do not impair the effects of the present invention. The other crystalline phases and amorphous phases are not limited, and examples thereof include a protenstenite phase, a forestenite phase, a mullite phase, and a cristobalite phase.
[0013] The composite oxide particles according to the present invention may further contain nanoparticles. The nanoparticles are fine particles having a particle diameter of 1.0 nm or more and 600.0 nm or less, preferably 50.0 nm or more and 500.0 nm or less. The nanoparticles are used when producing the composite oxide particles according to the present invention and do not adversely affect the effects of the present invention. Therefore, it is acceptable for the nanoparticles to remain in the composite oxide particles according to the present invention. The addition of nanoparticles can adjust surface properties such as wettability, making them easier to add to resin substrates, for example.
[0014] The nanoparticles are not limited, and examples thereof include nano-sized silica particles, nano-sized titania particles, nano-sized magnesia particles, and nano-sized alumina particles. Nano-sized silica particles are preferred. Nano-sized magnesia and alumina particles, which are components of cordierite, are also preferred. The composite oxide particles according to the present invention contain nanoparticles in a proportion of, for example, 0.1% by mass or more and 30% by mass or less of the total of the nano-sized silica particles (nanoparticles) and the composite oxide particles.
[0015] The composite oxide particles according to the present invention are not limited in size as long as they are spherical. For example, the composite oxide particles according to the present invention preferably have an average particle diameter (D50) of 0.1 μm or more and 500.0 μm or less in terms of the cumulative 50% volume average particle diameter (D50). When the composite oxide particles according to the present invention have an average particle diameter (D50) of 0.1 μm or more and 500.0 μm or less, the film thickness when kneaded into a resin can be reduced to 1 mm or less. The composite oxide particles according to the present invention more preferably have a particle diameter of 1.0 μm or more and 250.0 μm or less.
[0016] The particle size is measured, for example, as follows. First, the composite oxide particles are dispersed in an aqueous solution of sodium hexametaphosphate. Next, the particle size distribution is measured by a laser diffraction method using a laser diffraction particle size distribution analyzer. An example of a laser diffraction particle size distribution analyzer is the "Microtrac: MT-3300EXII" manufactured by Nikkiso Co., Ltd.
[0017] Depending on the application, the composite oxide particles according to the present invention are desirably those with a relatively small variation in particle size. For example, in the composite oxide particles according to the present invention, the difference D90 - D10 between the particle size D90, which is the cumulative 90% diameter, and the particle size D10, which is the cumulative 10% diameter, in the particle size distribution measured by laser diffraction is preferably 1000.0 μm or less. When D90 - D10 is 1000.0 μm or less, the composite oxide particles according to the present invention are easily filled into resin. D90 - D10 is more preferably 800.0 μm or less. D10 and D90 are calculated from a volume-based cumulative frequency distribution curve.
[0018] The composite oxide particles according to the present invention are not limited in shape as long as they are spherical. Depending on the application, composite oxide particles according to the present invention are preferably close to perfect spheres. For example, the composite oxide particles according to the present invention preferably have a circularity of 0.70 or more. When the composite oxide particles according to the present invention have a circularity of 0.70 or more, the loading amount of the composite oxide particles according to the present invention can be easily increased when the composite oxide particles according to the present invention are mixed with a resin to prepare a resin composite. The composite oxide particles according to the present invention more preferably have a circularity of 0.80, and even more preferably 0.85 or more.
[0019] Circularity is measured, for example, by an apparatus based on the principle of dynamic image analysis in accordance with ISO 13322-2. An example of such an apparatus is the "CAMSIZER X2" manufactured by Verder Scientific. Circularity is specifically measured as follows: First, a predetermined amount of composite oxide particles is weighed. Next, the composite oxide particles are sequentially placed into the apparatus, and while agglomerated particles are dispersed with dry air at 50 kPa, particles passing in front of the camera are measured. The measurement is performed in a dry state. This measurement is repeated three times, and the circularity is analyzed from the integrated average of the measurement results.
[0020] The particle size is taken as the circle-equivalent particle size. The circle-equivalent particle size means the particle size of a perfect circle that has the same area as the projected particle image. The particle size is based on volume. Circularity is analyzed in accordance with ISO 9276-6. Circularity is calculated by 4πA / P2. A represents the measured area of the projected particle image, and P represents the measured perimeter of the projected particle image.
[0021] Although particles have a three-dimensional shape, the particles passing in front of the camera are measured in a two-dimensional manner. Therefore, in this specification, "circularity" is used, and the closer the circularity is to 1.00, the closer the particle is to being a perfect sphere.
[0022] Whether a compound has crystallinity or amorphousness can be determined, for example, by X-ray diffraction spectroscopy. If the compound has amorphousness, a halo peak is observed in the X-ray diffraction spectrum. The composite oxide particles according to the present invention may contain an amorphous phase as long as they are crystalline. The degree of crystallinity, which is a measure of crystallinity, of the composite oxide particles according to the present invention is not limited. The composite oxide particles according to the present invention preferably have a degree of crystallinity of 40 or more. When the composite oxide particles have a degree of crystallinity of 40 or more, the composite oxide particles according to the present invention have the advantage of being less affected by amorphous portions. The composite oxide particles according to the present invention more preferably have a degree of crystallinity of 80 or more, and even more preferably 90 or more.
[0023] The composite oxide particles according to the present invention are measured by X-ray diffraction, and the crystallinity is calculated by the following formula (I) within the diffraction angle 2θ range of 15 to 40°: Crystallinity = crystalline peak area / (crystalline peak area + amorphous peak area) (I).
[0024] In the composite oxide particles according to the present invention, the half-width of the main peak of the crystals measured by X-ray diffraction in the diffraction angle 2θ range of 27.5 to 29.5° is preferably 0.20° or less. When this half-width is 0.20° or less, the composite oxide particles according to the present invention can be said to have high crystallinity of the crystal plane of the main peak that characterizes the composite oxide. The composite oxide particles according to the present invention more preferably have a half-width of 0.18° or less.
[0025] The composite oxide particles according to the present invention have a whitish color. Therefore, the composite oxide particles according to the present invention do not color a substrate, such as a semiconductor package substrate, when dispersed therein, making it easier to optically detect defects and contamination on the substrate. Furthermore, because the composite oxide particles according to the present invention have a whitish color, they are also preferable for use as a filler to be mixed when preparing a composite. Specifically, the composite oxide particles according to the present invention preferably have an L* in the L*a*b* color space of 91.00 or more and 100.00 or less, more preferably 92.50 or more and 100.00 or less, an a* of −10.00 or more and 3.00 or less, more preferably −5.00 or more and less than 1.50, and even more preferably −2.00 or more and less than 1.00, and an b* of −10.00 or more and 5.00 or less, more preferably −5.00 or more and 3.50 or less, and even more preferably −1.50 or more and less than 3.00. When L*, a*, and b* are within such ranges, the composite oxide particles according to the present invention can be judged to have a stronger whiteness.
[0026] The method for producing the composite oxide particles according to the present invention is not limited, and includes, for example, a step of mixing cordierite particles and nanoparticles to obtain mixed particles, and a step of heating the mixed particles.
[0027] In the step of mixing cordierite particles and nanoparticles to obtain mixed particles, the cordierite particles and nanoparticles as raw materials are mixed. The cordierite particles may be used as they are, or may be flame-melted and solidified into granules. Specifically, cordierite particles may be flame-melted at 1200°C or higher and 1500°C or lower, dropped, and solidified into granules by cooling during dropping.
[0028] As described above, examples of nanoparticles include nanosilica. Details of nanoparticles are as described above, and a detailed description will be omitted. In mixed particles containing cordierite particles and nanoparticles, the mixing ratio of cordierite particles to nanoparticles is not limited. For example, the nanoparticles are preferably contained in a ratio of 0.1% by mass or more and 30% by mass or less. By using nanoparticles in such a ratio, the spherical shape can be maintained.
[0029] In the step of heating the mixed particles, the obtained mixed particles are heated. The heating temperature is not limited, but is preferably 1000° C. or higher and 1400° C. or lower. By heating at such a temperature, polycrystalline composite oxide particles having a main crystalline phase containing at least one of cordierite and indialite can be produced more efficiently, and amorphous composite oxide particles are less likely to be obtained.
[0030] In order to efficiently obtain composite oxide particles containing indialite as the main crystalline phase, it is preferable to heat the mixture at a temperature of 1000° C. to 1200° C. On the other hand, in order to obtain composite oxide particles containing cordierite as the main crystalline phase, it is preferable to heat the mixture at a temperature of 1200° C. to 1400° C.
[0031] Heating may be performed in air or in an inert gas atmosphere. The inert gas is not limited, and examples thereof include nitrogen gas and argon gas. The heating time is not limited, and is, for example, from 1 hour to 24 hours.
[0032] The composite oxide particles according to the present invention are obtained by such a process. Immediately after heating, the composite oxide particles may solidify, for example, in the shape of the container. Even in such solidified state, they can be easily broken up by hand or a mallet after cooling, and smooth composite oxide particles are obtained. The obtained composite oxide particles are spherical, crystalline, and whitish, and the main crystalline phase contains at least one of cordierite and indialite. Due to such a structure, the composite oxide particles according to the present invention have a thermal expansion coefficient measured by the TMA method of 1.5 ppm or less, preferably less than 0.0 ppm.
[0033] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0034] Preparation Example First, irregular cordierite particles (manufactured by Marusu Yuyaku Co., Ltd., product number: SS400) were flame-melted at 1500°C, and the flame-molten material was dropped. The material was cooled during dropping and solidified into granules, thereby preparing raw material particles.
[0035] Example 1 The raw material particles obtained in Preparation Example 1 and nanosilica (SO-E1 manufactured by Admatechs Co., Ltd.) were mixed in a mortar at a ratio of 95% by mass and 5% by mass, and the mixture was mixed for 10 minutes.
[0036] Next, the raw material particles were placed in an alumina crucible and fired at 1200°C for 10 hours to obtain spherical composite oxide particles. XRD measurement was performed on the obtained spherical composite oxide particles. The obtained spectrum did not contain a broad halo peak, confirming that the obtained spherical composite oxide particles had high crystallinity. Furthermore, from the firing temperature and the XRD spectrum, it was confirmed that the obtained spherical composite oxide particles contained at least one of an indialite phase and a cordierite phase.
[0037] Example 2 Spherical composite oxide particles were obtained using the same procedure as in Example 1, except that the particles were fired at 1,400°C for 10 hours. XRD measurement of the obtained spherical composite oxide particles yielded a spectrum lacking a broad halo peak. This spectrum confirmed that the obtained spherical composite oxide particles had high crystallinity. Furthermore, the firing temperature and the XRD spectrum confirmed that the obtained spherical composite oxide particles contained at least one of an indialite phase and a cordierite phase.
[0038] Example 3 Spherical composite oxide particles were obtained using the same procedure as in Example 2, except that the raw material particles obtained in Preparation Example and nanosilica were used in a ratio of 70% by mass and 30% by mass, respectively. XRD measurement of the obtained spherical composite oxide particles resulted in a spectrum lacking a broad halo peak. This spectrum confirmed that the obtained spherical composite oxide particles had high crystallinity. Furthermore, the firing temperature and XRD spectrum confirmed that the obtained spherical composite oxide particles contained at least one of an indialite phase and a cordierite phase.
[0039] Example 4 Spherical composite oxide particles were obtained using the same procedure as in Example 1, except that the raw material particles obtained in Preparation Example and nanosilica were used in a ratio of 99% by mass and 1% by mass, respectively. XRD measurement of the obtained spherical composite oxide particles resulted in a spectrum lacking a broad halo peak. This spectrum confirmed that the obtained spherical composite oxide particles had high crystallinity. Furthermore, the firing temperature and XRD spectrum confirmed that the obtained spherical composite oxide particles contained at least one of an indialite phase and a cordierite phase.
[0040] Comparative Example 1 The raw material particles obtained in Preparation Example were placed in an alumina crucible and fired at 850°C for 10 hours to obtain spherical composite oxide particles. The obtained spherical composite oxide particles were subjected to XRD measurement. The obtained spectrum showed a broad halo peak, confirming that the obtained spherical composite oxide particles contained an amorphous phase and a crystalline phase.
[0041] Comparative Example 2 An attempt was made to obtain spherical composite oxide particles using the same procedure as in Comparative Example 1, except that the firing was performed at 1,400° C. for 10 hours. However, a clumped composite oxide was obtained, and spherical particles were not obtained.
[0042] The spherical composite oxide particles obtained in Examples 1 to 4 and Comparative Example 1 were examined for particle size, specific surface area, roundness, thermal expansion coefficient, crystallinity, and color.
[0043] <Particle size> The obtained spherical composite oxide particles were dispersed in an aqueous sodium hexametaphosphate solution. The particle size distribution was then measured by laser diffraction using a laser diffraction particle size distribution analyzer (Microtrac: MT-3300EXII, manufactured by Nikkiso Co., Ltd.). D10, D50, and D90 were calculated from the volume-based cumulative frequency distribution curve. The D50 value and the difference between D90 and D10 (D90 - D10) are shown in Table 1.
[0044] <Specific Surface Area> The specific surface area of the obtained spherical composite oxide particles was measured in accordance with the specific surface area measurement method for powders (solids) by gas adsorption (JIS Z 8830:2013). Specifically, nitrogen was used as the adsorption gas, and 1 g of the spherical composite oxide particles was placed in a sample tube to obtain an adsorption / desorption isotherm. The specific surface area (m2 / g) was calculated using the multipoint plot method. The results are shown in Table 1.
[0045] <Circularity> The circularity of the obtained spherical composite oxide particles was measured using an apparatus based on the principle of dynamic image analysis in accordance with ISO 13322-2 (CAMSIZER X2 (manufactured by Verder Scientific)). Specifically, 3 g of spherical composite oxide particles was weighed. Next, the composite oxide particles were sequentially placed into the apparatus, and while agglomerated particles were dispersed with dry air at 50 kPa, particles passing in front of the camera were measured. The measurement was carried out in a dry state. This measurement was repeated three times, and the circularity was analyzed from the integrated average of the measurement results. The circularity was calculated by 4πA / P2. A represents the measured value of the area of the projected particle image, and P represents the measured value of the circumferential length of the projected particle image. The results are shown in Table 1.
[0046] <Thermal expansion coefficient> The raw materials (raw material particles and, if necessary, nanosilica) for the obtained spherical composite oxide particles were used to obtain rectangular sintered bodies (20 mm x 4 mm x 4 mm) by firing at the same temperatures as in Examples 1 to 4 and Comparative Examples 1 and 2. The linear expansion coefficients of the obtained sintered bodies (samples) were measured using a TD5020SE (manufactured by NETZSCH). Specifically, the linear expansion coefficients of the obtained samples were measured in the air at temperatures ranging from 30 to 300°C in accordance with thermomechanical analysis (JIS R1618). Sapphire was used as the standard sample. This linear expansion coefficient was taken as the thermal expansion coefficient. The results are shown in Table 1.
[0047] <Crystallinity> The crystallinity of the obtained spherical composite oxide particles was measured by X-ray diffraction. Specifically, measurements were performed using a powder X-ray diffractometer X'PertPROMPD (manufactured by Spectris Co., Ltd.) to obtain a diffraction spectrum. The measurement conditions were a CuKα X-ray source, an X-ray output of 45 kV and 40 mA, and a scanning speed of 0.2 deg / s. If a clear, sharp peak was observed, the sample was judged to be crystalline, and if a broad halo peak was observed, the sample was judged to be amorphous. From the results of the built-in software HighScorePlus, the crystallinity was calculated using the above-mentioned formula (I) (crystallinity = crystalline peak area / (crystalline peak area + amorphous peak area)). The results are shown in Table 1.
[0048] <Color> The color of the obtained spherical composite oxide particles was determined based on the L*a*b* color space. Specifically, the obtained spherical composite oxide particles were placed on a glass plate in a 1.5 cm x 1.5 cm square shape so that there were no gaps, and a cover glass was placed on top to fix the sample, thereby obtaining a sample piece. The obtained sample piece was subjected to black correction and white correction using a spectrophotometer CM-3700A (manufactured by Konica Minolta, Inc.), and then subjected to SCI reflectance measurement in accordance with JIS Z8722 condition c, with diffuse illumination received at an 8° angle, to obtain lightness L* and chromaticity a* and b*. L* = 0.00 indicates black, L* = 100.00 indicates white, and the following relationships apply: 0.00≦L*≦100.00, -100.00≦a*≦100.00, and -100.00≦b*≦100.00. A sample was judged to be white when it satisfied the conditions of L*>91.00, a*<3.00, and b*<5.00. The results are shown in Table 1.
[0049]
[0050] As described above, the composite oxide particles obtained in Examples 1 to 4 (corresponding to the composite oxide particles according to the present invention) contain at least one of a cordierite phase and an indialite phase. As shown in Table 1, the composite oxide particles obtained in Examples 1 to 4 all have a D50 of 0.1 μm or more and 500.0 μm or less, and the difference between D90 and D10, D90 - D10, is 1000.0 μm or less. The composite oxide particles obtained in Examples 1 to 4 are all white, spherical, and have a circularity of 0.7 or more, and a thermal expansion coefficient (linear expansion coefficient) of 0.0 ppm or less. Furthermore, the composite oxide particles obtained in Examples 1 to 4 are crystalline, have a degree of crystallinity of 40 or more within a diffraction angle 2θ range of 15 to 40°, and have a half-width of the main crystal peak of 0.20° or less within a diffraction angle 2θ range of 27.5 to 29.5°.
[0051] On the other hand, the composite oxide particles obtained in Comparative Example 1 were pink rather than white, and had a thermal expansion coefficient (linear expansion coefficient) of 4.0 ppm, exceeding 1.5 ppm, indicating the presence of amorphous portions. As shown in Table 1, the composite oxide particles obtained in Comparative Example 2 were lumpy after firing and could not be broken down with a wooden mallet, so they were crushed into particles with a hammer. The composite oxide particles obtained in Comparative Example 2 were crystalline and white, but had a thermal expansion coefficient (linear expansion coefficient) of 1.7 ppm, exceeding 1.5 ppm. In Comparative Example 3 listed in Table 1, the color of the raw material particles obtained in Preparation Example was determined based on the L*a*b* color space.
Claims
1. Composite oxide particles which are polycrystalline, the main crystal phase of which contains at least one of cordierite and indialite, and which have a thermal expansion coefficient of 1.5 ppm or less as measured by the TMA method.
2. The composite oxide particles according to claim 1, having an average particle diameter (D50) of 0.1 μm or more and 500.0 μm or less.
3. The composite oxide particles according to claim 1, which have a crystallinity of 40 or more when measured by an X-ray diffraction method and calculated by the following formula (I) in a diffraction angle 2θ range of 15 to 40°: Crystallinity = crystalline peak area / (crystalline peak area + amorphous peak area) ... (I) 4. The composite oxide particles according to claim 1, wherein in a particle size distribution measured by a laser diffraction method, the difference D90-D10 between a particle size D90 that is the 90% cumulative diameter and a particle size D10 that is the 10% cumulative diameter is 1000.0 μm or less.
5. The composite oxide particles according to claim 1, having a circularity of 0.70 or more.
6. The composite oxide particles according to claim 1, wherein the half-width of the main crystal peak in the diffraction angle 2θ range of 27.5 to 29.5°, as measured by X-ray diffraction, is 0.20° or less.
7. The composite oxide particles according to claim 1, wherein the nanoparticles are contained in an amount of 0.1% by mass or more and 30% by mass or less.
8. The composite oxide particles according to claim 1, wherein in the L*a*b* color space, L* is from 91.00 to 100.00, a* is from -10.00 to 3.00, and b* is from -10.00 to 5.
00.
9. A method for producing composite oxide particles, comprising: a step of mixing particulate cordierite and nanoparticles to obtain mixed particles; and a step of heating the mixed particles.
10. The method according to claim 9, wherein the heating step is carried out at a temperature of 1000°C or higher and 1400°C or lower.
Citation Information
Patent Citations
Production of low-thermal expansion cordierite
JP1990111659A
Production of cordierite powder and its ceramic
JP1994172023A
Cordierite filler, its production method, film material, and cured film
JP2009149487A
Grayed oxide ceramic sintered compact, and production method thereof
JP2016008163A
Cordierite sintered body
JP2016204198A