Nanostructure-dispersion-liquid-containing container, storage repository for accommodating same, and method for storing nanostructure dispersion liquid
By filling a container with a nanostructure dispersion liquid at a high volume ratio and using specific resins for the inner surface, stored at 25°C or lower, the challenges of maintaining dispersion stability are addressed, ensuring effective storage and handling of nanostructures like carbon nanotubes.
Patent Information
- Application Number
- PCT/JP2024/007875
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-01
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for storing nanostructure dispersions, such as those containing carbon nanotubes, face challenges in maintaining dispersion stability due to environmental changes and handling issues, leading to decreased dispersibility and aggregation.
A container filled with a nanostructure dispersion liquid at a 90% or higher volume ratio, using a resin such as high-density polyethylene or fluororesin for the inner surface, and stored at 25°C or lower, effectively maintains dispersion stability by minimizing environmental impacts and aggregation.
This approach ensures excellent dispersion stability of nanostructures, preventing aggregation and maintaining dispersibility over time, even during storage and transportation.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Container containing nanostructure dispersion, storage cabinet for storing the same, and method for storing nanostructure dispersion
[0001] The present invention relates to a container containing a nanostructure dispersion, a storage cabinet for storing the container, and a method for storing a nanostructure dispersion.
[0002] In recent years, various nanostructures such as nanocarbons, nanofibers, and nanowires have attracted attention as materials with various excellent properties such as mechanical properties. Among these, nanocarbons, particularly fibrous carbon nanostructures such as carbon nanotubes (hereinafter sometimes referred to as "CNTs"), have attracted attention as materials with excellent electrical conductivity, thermal conductivity, and mechanical properties.
[0003] However, nanostructures such as CNTs are minute structures with nanometer-sized diameters, making them difficult to handle and process when used alone. Therefore, nanostructures are used for various applications after forming an assembly by assembling multiple nanostructures into, for example, a film, or after combining them with a polymeric material such as resin or rubber or a metal to form a composite material. A method for forming an assembly of nanostructures has been proposed, in which the dispersion medium is removed from a nanostructure dispersion in which nanostructures are dispersed. Another method for forming a composite material containing nanostructures has been proposed, in which the composite material is precipitated or sedimented from a composite material composition formed by mixing a matrix material such as a polymeric material with a nanostructure dispersion.
[0004] Here, from the viewpoint of enabling nanostructure aggregates and composite materials to exhibit excellent properties, a nanostructure dispersion liquid in which nanostructures are well dispersed in a dispersion medium is required as the nanostructure dispersion liquid used to form the aggregates and composite materials. For example, Patent Document 1 discloses the finding that by filling a sealed container used for storing or transporting the nanostructure dispersion liquid with a predetermined amount or more of the nanostructure dispersion liquid, it is possible to reduce the effects of environmental changes during storage and vibrations during transport, and to prevent a decrease in the dispersibility of the nanostructures.
[0005] International Publication No. 2017 / 115707
[0006] According to the technology disclosed in Patent Document 1, it is possible to provide a container containing a nanostructure dispersion liquid that can prevent the dispersibility of the nanostructures contained in the nanostructure dispersion liquid in the container from decreasing even when the container is stored or transported.
[0007] The technology disclosed in Patent Document 1 leaves room for further improvement in the dispersibility of nanostructures in the nanostructure dispersion. Therefore, an object of the present invention is to provide a nanostructure dispersion having excellent dispersion stability.
[0008] The present inventors have conducted extensive research to solve the above-mentioned problems. They have discovered that a nanostructure dispersion having excellent dispersion stability can be provided by satisfying the following conditions in a nanostructure dispersion container comprising a storage cabinet containing nanostructures having functional groups and a dispersion medium, and a sealed container for containing the nanostructure dispersion: The conditions are that the nanostructure dispersion fills the sealed container at a rate of 90.0% by volume or more, that at least the inner surface of the sealed container is formed from a resin containing at least one selected from high-density polyethylene, low-density polyethylene, polystyrene, polypropylene, and a fluororesin, and that the storage temperature of the storage cabinet is 25°C or less.
[0009] The present invention aims to advantageously solve the above-mentioned problems. [1] The nanostructure dispersion container of the present invention is a nanostructure dispersion container contained in a storage cabinet. The nanostructure dispersion container comprises a nanostructure dispersion containing nanostructures and a dispersion medium, and a sealed container containing the nanostructure dispersion. The nanostructures are fibrous carbon nanostructures having functional groups. The nanostructure dispersion is filled at a filling rate of 90.0% by volume or more in the sealed container. At least the inner surface of the sealed container that comes into contact with the nanostructure dispersion is formed of a resin, the resin including at least one selected from high-density polyethylene, low-density polyethylene, polystyrene, polypropylene, and a fluororesin. The storage cabinet is equipped with a control unit that can set the storage temperature of the nanostructure dispersion container to 25°C or less. Storing such a predetermined nanostructure dispersion container in a storage cabinet set to 25°C or less can provide a nanostructure dispersion with excellent dispersion stability. Furthermore, in this specification, "fibrous" refers to an aspect ratio of 10 or more. In this specification, "high density polyethylene" refers to polyethylene having a density of 942 kg / m 3 "Low density polyethylene" means polyethylene having a density of 910 kg / m or more. 3 More than 930kg / m 3 This means polyethylene of less than
[0010] [2] Here, in the container containing the nanostructure dispersion of the present invention, it is preferable that the nanostructures include carbon nanotubes.
[0011] [3] In the container containing the nanostructure dispersion liquid of [2] above, the carbon nanotubes preferably include single-walled carbon nanotubes.
[0012] [4] In the nanostructure dispersion container according to [2] or [3] above, it is preferable that the carbon nanotubes exhibit an upwardly convex t-plot obtained from an adsorption isotherm.
[0013] [5] Furthermore, the storage cabinet of the present invention, which can advantageously solve the above problem, is a storage cabinet for storing a container containing a nanostructure dispersion liquid according to any one of [1] to [4] above.
[0014] [6] Furthermore, a method for storing a nanostructure dispersion liquid of the present invention, which can advantageously solve the above-mentioned problems, comprises storing the nanostructure dispersion liquid in a sealed container filled with a nanostructure dispersion liquid containing nanostructures and a dispersion medium, wherein the nanostructures are fibrous carbon nanostructures having functional groups, the nanostructure dispersion liquid has a filling rate of 90.0% by volume or more, at least the inner surface of the sealed container that comes into contact with the nanostructure dispersion liquid is formed from a resin, and the resin includes at least one selected from high-density polyethylene, low-density polyethylene, polystyrene, polypropylene, and a fluororesin, and the container containing the nanostructure dispersion liquid is stored at a temperature below 25° C. This storage method can provide a nanostructure dispersion liquid with excellent dispersion stability.
[0015] According to the present invention, it is possible to provide a nanostructure dispersion liquid having excellent dispersion stability.
[0016] The nanostructure dispersion liquid stored in the container containing the nanostructure dispersion liquid of the present invention can be subjected to a treatment such as purification as necessary and then used for a desired purpose.
[0017] (Container containing nanostructure dispersion) The nanostructure dispersion container of the present invention is a container containing nanostructure dispersion contained in a storage cabinet. This nanostructure dispersion container comprises a nanostructure dispersion containing nanostructures and a dispersion medium, and a sealed container containing the nanostructure dispersion. The nanostructures are fibrous carbon nanostructures having functional groups, and the nanostructure dispersion fills the sealed container at a rate of 90.0% by volume or more. At least the inner surface of the sealed container that comes into contact with the nanostructure dispersion is formed from a resin, and the resin includes at least one selected from high-density polyethylene, low-density polyethylene, polystyrene, polypropylene, and fluororesin. The storage cabinet containing the nanostructure dispersion container is equipped with a control unit that can set the storage temperature of the nanostructure dispersion container to 25°C or below. The control unit is not particularly limited, but may include an operating unit (cooling / heating device) that heats and cools the interior of the storage cabinet, and a temperature control device that sends operating signals to the operating unit to control the heating and cooling of the interior of the storage cabinet. Specifically, the storage cabinet may be, for example, a constant temperature and humidity chamber.
[0018] Furthermore, at least the inner surface of the sealed container that comes into contact with the nanostructure dispersion is formed from a predetermined resin. Here, the predetermined resin includes at least one selected from high-density polyethylene, low-density polyethylene, polystyrene, polypropylene, and fluororesin. Furthermore, "at least the inner surface of the sealed container is made of at least one of the predetermined resins" refers not only to the case where the entire sealed container is made of the predetermined resin, but also to the case where the inner surface of the sealed container is lined with the predetermined resin. In this case, the material constituting the sealed container body (e.g., the exterior) is not particularly limited and may be glass or metal. By storing such a container containing the predetermined nanostructure dispersion at 25°C or below, the dispersion stability of the nanostructure dispersion can be improved. The shape of the sealed container is not particularly limited, and may be any sealed container with a filling port, for example, that can be sealed after filling with the nanostructure dispersion. Specifically, the sealed container may be, for example, a bottle with a lid.
[0019] Here, when the stored nanostructure dispersion is used for a desired purpose, an ion exchange process may be carried out, if necessary, to remove impurities such as metals from the nanostructure dispersion. In this ion exchange process, the nanostructure dispersion may be brought into contact with a strongly acidic ion exchange resin. In such an ion exchange process, the strongly acidic ion exchange resin may be brought into contact with the nanostructure dispersion. If the nanostructure dispersion to be subjected to the ion exchange process has excellent dispersion stability, aggregation of the nanostructures and clogging of the ion exchange resin by the nanostructures during the ion exchange process can be effectively suppressed.
[0020] The nanostructure dispersion comprises nanostructures and a dispersion medium, and may optionally further contain additives such as dispersants, molecular additives, and ionic particles.
[0021] <Nanostructures> Examples of nanostructures include, but are not limited to, nanocarbons such as fullerenes, graphene, and fibrous carbon nanostructures; nanofibers such as cellulose nanofibers; nanowires such as silver nanowires; and boron nitride nanotubes. These may be used alone or in combination of two or more.
[0022] Among the above, nanocarbons are preferred as the nanostructures, and fibrous carbon nanostructures are more preferred. The fibrous carbon nanostructures are not particularly limited, and examples thereof include carbon nanotubes, carbon nanofibers, carbon nanohorns, and vapor-grown carbon fibers. These may be used alone or in combination of two or more. Of these, it is more preferred to use carbon nanotubes as the fibrous carbon nanostructures. This is because carbon nanotubes have excellent electrical conductivity, thermal conductivity, and mechanical properties.
[0023] Here, carbon nanotubes that can be suitably used as nanostructures may consist solely of carbon nanotubes, or may be a mixture of carbon nanotubes and fibrous carbon nanostructures other than carbon nanotubes. The carbon nanotubes are not particularly limited, and single-walled carbon nanotubes and / or multi-walled carbon nanotubes can be used. However, single-walled to five-walled carbon nanotubes are preferred, and single-walled carbon nanotubes are more preferred. This is because single-walled carbon nanotubes have superior electrical conductivity, thermal conductivity, and mechanical properties compared to multi-walled carbon nanotubes.
[0024] Furthermore, it is preferable to use, as the fibrous carbon nanostructure, a carbon nanostructure having a ratio (3σ / Av) of the standard deviation (σ) of the diameter multiplied by 3 (3σ) to the average diameter (Av) of more than 0.20 and less than 0.60, more preferably a carbon nanostructure having a 3σ / Av of more than 0.25, and even more preferably a carbon nanostructure having a 3σ / Av of more than 0.50. This is because fibrous carbon nanostructures having a 3σ / Av of more than 0.20 and less than 0.60 have excellent electrical conductivity, thermal conductivity, and mechanical properties. The "average diameter (Av) of fibrous carbon nanostructures" and the "standard deviation of the diameters of fibrous carbon nanostructures (σ: sample standard deviation)" can each be determined by measuring the diameters (outer diameters) of 100 randomly selected fibrous carbon nanostructures using a transmission electron microscope. The average diameter (Av) and standard deviation (σ) of the fibrous carbon nanostructures may be adjusted by changing the manufacturing method or manufacturing conditions of the fibrous carbon nanostructures, or by combining multiple types of fibrous carbon nanostructures obtained by different manufacturing methods.
[0025] The fibrous carbon nanostructures that are usually used are those that show a normal distribution when the diameter measured as described above is plotted on the horizontal axis and the frequency on the vertical axis and approximated by a Gaussian.
[0026] Furthermore, the fibrous carbon nanostructure preferably has a radial breathing mode (RBM) peak when evaluated by Raman spectroscopy. Note that the Raman spectrum of a fibrous carbon nanostructure consisting only of multi-walled carbon nanotubes with three or more walls does not include an RBM.
[0027] Furthermore, the fibrous carbon nanostructure preferably has a ratio of the G band peak intensity to the D band peak intensity in the Raman spectrum (G / D ratio) of 1 to 20. This is because a fibrous carbon nanostructure having a G / D ratio of 1 to 20 has excellent electrical conductivity, thermal conductivity, and mechanical properties.
[0028] Furthermore, the average diameter (Av) of the fibrous carbon nanostructures is preferably 0.5 nm or more, more preferably 1 nm or more, and preferably 15 nm or less, and even more preferably 10 nm or less. This is because, if the average diameter (Av) of the fibrous carbon nanostructures is 0.5 nm or more, aggregation of the fibrous carbon nanostructures can be suppressed and the dispersibility of the fibrous carbon nanostructures in the dispersion liquid can be improved. Also, this is because fibrous carbon nanostructures with an average diameter (Av) of 15 nm or less have excellent electrical conductivity, thermal conductivity, and mechanical properties.
[0029] Furthermore, the BET specific surface area of the fibrous carbon nanostructure is 400 m 2 / g or more, and 2 / g or more, and more preferably 2,500m 2 / g or less, and 2 / g or less. 2 This is because the fibrous carbon nanostructures with a BET specific surface area of 2,500 m / g or more are excellent in electrical conductivity, thermal conductivity and mechanical properties. 2 / g or less, the dispersibility of the fibrous carbon nanostructure in the dispersion liquid can be further improved. In the present invention, the "BET specific surface area" refers to the nitrogen adsorption specific surface area measured using the BET method.
[0030] Furthermore, the fibrous carbon nanostructure preferably has a plurality of micropores. The fibrous carbon nanostructure preferably has micropores with a pore diameter of less than 2 nm, and the amount of micropores present is preferably 0.40 mL / g or more, more preferably 0.43 mL / g or more, as determined by the following method, with the upper limit typically being about 0.65 mL / g. When the fibrous carbon nanostructure has micropores as described above, aggregation of the fibrous carbon nanostructures in the dispersion is suppressed, thereby further improving the dispersibility of the fibrous carbon nanostructures in the dispersion. The micropore volume can be adjusted, for example, by appropriately modifying the preparation method and preparation conditions of the fibrous carbon nanostructures. Here, the "micropore volume (Vp)" can be calculated by measuring the nitrogen adsorption isotherm of the fibrous carbon nanostructure at liquid nitrogen temperature (77 K) and using the nitrogen adsorption amount at a relative pressure P / P0 = 0.19, as V, according to the formula (I): Vp = (V / 22,414) × (M / ρ). where P is the measured pressure at adsorption equilibrium, P is the saturated vapor pressure of liquid nitrogen at the time of measurement, M is the molecular weight of the adsorbate (nitrogen) of 28.010, and ρ is the density of the adsorbate (nitrogen) at 77 K of 0.808 g / cm 3 The micropore volume can be determined using, for example, "BELSORP (registered trademark)-mini" (manufactured by BEL Japan Co., Ltd.).
[0031] Furthermore, it is preferable that the t-plot obtained from the adsorption isotherm of the fibrous carbon nanostructure exhibits an upwardly convex shape. It is particularly preferable that the fibrous carbon nanostructure is not subjected to an aperture treatment and exhibits an upwardly convex shape. This is because fibrous carbon nanostructures exhibiting an upwardly convex t-plot have excellent electrical conductivity, thermal conductivity, and mechanical properties. The "t-plot" can be obtained by converting the relative pressure into the average thickness t (nm) of the nitrogen gas adsorption layer in the adsorption isotherm of the fibrous carbon nanostructure measured by the nitrogen gas adsorption method. That is, the average thickness t of the nitrogen gas adsorption layer corresponding to the relative pressure is calculated from a known standard isotherm in which the average thickness t of the nitrogen gas adsorption layer is plotted against the relative pressure P / P0, and the above conversion is performed to obtain the t-plot of the fibrous carbon nanostructure (the t-plot method by de Boer et al.).
[0032] Here, in materials with pores on the surface, the growth of a nitrogen gas adsorption layer can be classified into the following processes (1) to (3). The slope of the t-plot changes depending on the following processes (1) to (3): (1) The process of forming a monomolecular adsorption layer of nitrogen molecules on the entire surface; (2) The process of forming a multimolecular adsorption layer and the accompanying capillary condensation filling process within the pores; and (3) The process of forming a multimolecular adsorption layer on an apparently non-porous surface where the pores are filled with nitrogen.
[0033] In the t-plot showing an upward convex shape, the plot is located on a straight line passing through the origin in the region where the average thickness t of the nitrogen gas adsorption layer is small, but as t increases, the plot shifts downward from the straight line. Fibrous carbon nanostructures having such a t-plot shape have a large ratio of the internal specific surface area to the total specific surface area of the fibrous carbon nanostructure, indicating that a large number of openings are formed in the carbon nanostructures that make up the fibrous carbon nanostructure.
[0034] The bending point of the t-plot of the fibrous carbon nanostructure is preferably in a range satisfying 0.2≦t(nm)≦1.5, more preferably in a range of 0.45≦t(nm)≦1.5, and even more preferably in a range of 0.55≦t(nm)≦1.0. The "position of the bending point" is the intersection of the approximate straight line A in the above-mentioned process (1) and the approximate straight line B in the above-mentioned process (3).
[0035] Furthermore, the fibrous carbon nanostructure preferably has a ratio (S2 / S1) of the internal specific surface area S2 to the total specific surface area S1 obtained from the t-plot of 0.05 to 0.30. The total specific surface area S1 and the internal specific surface area S2 of the fibrous carbon nanostructure are not particularly limited, but individually, S1 is preferably 400 m 2 / g or more 2,500m 2 / g or less, and 2 / g or more 1,200m 2 On the other hand, S2 is preferably 30m / g or less. 2 / g or more 540m 2 / g or less. Here, the total specific surface area S1 and the internal specific surface area S2 of the fibrous carbon nanostructure can be determined from the t-plot. Specifically, first, the total specific surface area S1 can be determined from the slope of the approximation line in step (1), and the external specific surface area S3 can be determined from the slope of the approximation line in step (3). Then, the internal specific surface area S2 can be calculated by subtracting the external specific surface area S3 from the total specific surface area S1.
[0036] Incidentally, the measurement of the adsorption isotherm of the fibrous carbon nanostructure, the creation of the t-plot, and the calculation of the total specific surface area S1 and the internal specific surface area S2 based on the analysis of the t-plot can be performed using, for example, a commercially available measuring device, "BELSORP (registered trademark)-mini" (manufactured by BEL Japan Co., Ltd.).
[0037] Furthermore, fibrous carbon nanostructures having functional groups can be efficiently produced by, for example, acid treatment of fibrous carbon nanostructures produced by a method known as the "super-growth method" disclosed in International Publication No. 2006 / 011655. The above-described preferred attributes of the fibrous carbon nanostructures, particularly the number of CNT layers, 3σ / Av, the plot shape obtained by Gaussian approximation of a plot of diameter on the horizontal axis and frequency on the vertical axis, the peak position and G / D ratio of the Raman spectrum, the average diameter (Av), the BET specific surface area, and the micropore volume, also apply to fibrous carbon nanostructures having functional groups. In the super-growth method, raw material compounds and a carrier gas are supplied to a substrate having a catalyst layer for carbon nanotube production on its surface to synthesize CNTs by chemical vapor deposition (CVD), and the catalytic activity of the catalyst layer is dramatically improved by the presence of a trace amount of an oxidizing agent (catalytic activator) in the system. Hereinafter, the carbon nanotubes as the fibrous carbon nanostructures obtained by the super-growth method may be referred to as "SGCNTs."
[0038] The fibrous carbon nanostructure may be composed of only SGCNTs, or may be composed of SGCNTs and non-cylindrical carbon nanostructures. Specifically, the fibrous carbon nanostructure may include a single-layer or multi-layer flat cylindrical carbon nanostructure (sometimes referred to as a "graphene nanotape (GNT)") having tape-like portions along its entire length, with the inner walls being close to or bonded together.
[0039] The functional group of the fibrous carbon nanostructure having a functional group can be selected from the group consisting of a hydroxyl group, an aldehyde group, a carbonyl group, and a carboxyl group. The method for introducing these functional groups into the fibrous carbon nanostructure is not particularly limited, and any method can be used. For example, the fibrous carbon nanostructure can be oxidized with an oxidizing acid such as nitric acid to form the above-mentioned functional group on the fibrous carbon nanostructure. If the fibrous carbon nanostructure has a functional group, its dispersibility in the dispersion can be improved. Whether the fibrous carbon nanostructure has a functional group can be determined by subjecting the dispersion to solid-liquid separation and then quantitatively analyzing the amount of oxygen element in the solid content using X-ray photoelectron spectroscopy (XPS).
[0040] For example, the method for oxidizing the fibrous carbon nanostructures with nitric acid is not particularly limited, but examples include a method in which an oxidizing acid such as nitric acid is mixed with the fibrous carbon nanostructures to obtain a mixture, and the resulting mixture is allowed to react with stirring for 1 to 13 hours at a temperature of 83°C to 120°C. Subsequently, it is preferable to optionally add water or the like to reduce the acid concentration, and then carry out a step (purification step) of removing impurities by filtration such as cross-flow filtration while adjusting the pH to around 7.0. The temperature during the purification step is not particularly limited, but can be 20°C to 35°C.
[0041] The above-mentioned purification step can remove metal impurities that are inevitably mixed in during the production of nanostructures. Examples of metal impurities include metal catalysts used during the production of nanostructures, such as alkali metals, alkaline earth metals, metal elements belonging to groups 3 to 13, and the lanthanoid group, as well as metal elements such as Si, Sb, As, Pb, Sn, and Bi, and metal compounds containing these. More specifically, examples include metal elements such as Al, Sb, As, Ba, Be, Bi, B, Cd, Ca, Cr, Co, Cu, Ga, Ge, Fe, Pb, Li, Mg, Mn, Mo, Ni, K, Na, Sr, Sn, Ti, W, V, Zn, and Zr, as well as metal compounds containing these. The concentration of metal impurities in the fibrous carbon nanostructures having functional groups is preferably 1×10 to further enhance the dispersion stability of the dispersion. 18 atoms / cm 3 Preferably, it is less than 15×10 10 atoms / cm 3 The concentration of metal impurities can be measured, for example, by a transmission electron microscope (TEM), a scanning electron microscope (SEM), an energy dispersive X-ray analyzer (EDAX), a vapor phase decomposition apparatus, or an inductively coupled plasma (ICP) mass analyzer (VPD, ICP / MS), but is usually measured using ICP mass analyzer (ICP / MS) because it can provide high accuracy.
[0042] The Z-average particle size of the nanostructures measured by dynamic light scattering is preferably 45.0 nm or more and 70.0 nm or less, more preferably 45.1 nm or more and 69.5 nm or less, and even more preferably 45.2 nm or more and 69.0 nm or less. If the Z-average particle size of the nanostructures measured by dynamic light scattering is within the above range, the generation of aggregates in the dispersion can be effectively suppressed, resulting in excellent dispersion stability. The Z-average particle size of the nanostructures measured by dynamic light scattering can be measured by the method described in the Examples of this specification.
[0043] <Dispersion medium> The dispersion medium for dispersing the nanostructure is not particularly limited, and examples thereof include water; alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, t-butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol, amyl alcohol, methoxypropanol, propylene glycol, and ethylene glycol; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; ethyl acetate, butyl acetate, ethyl lactate, esters of α-hydroxycarboxylic acids, and benzyl benzoate. Examples of suitable solvents include esters such as benzoic acid (benzyl benzoate); ethers such as diethyl ether, dioxane, tetrahydrofuran, and monomethyl ether; amide-based polar organic solvents such as N,N-dimethylformamide, dimethyl sulfoxide, dimethylacetamide, and N-methylpyrrolidone; aromatic hydrocarbons such as toluene, xylene, chlorobenzene, ortho-dichlorobenzene, and para-dichlorobenzene; salicylaldehyde, dimethyl sulfoxide, 4-methyl-2-pentanone, N-methylpyrrolidone, γ-butyrolactone, and tetramethylammonium hydroxide. Among these, water and dimethylacetamide are preferred, and water is more preferred, from the viewpoint of achieving particularly excellent dispersibility of nanostructures. These solvents may be used alone or in combination of two or more.
[0044] <Additives> Additives that can be optionally incorporated into the nanostructure dispersion include, but are not limited to, dispersants, molecular additives, and pH adjusters. Examples of dispersants and molecular additives include, but are not limited to, those disclosed in International Publication No. 2017 / 115707. Examples of pH adjusters include, but are not limited to, aqueous ammonia and aqueous ammonium nitrate. From the perspective of improving the properties (particularly, conductivity, etc.) of electronic devices formed using the nanostructure dispersion, the concentration of additives contained in the nanostructure dispersion is preferably 1% by mass or less.
[0045] <pH of Nanostructure Dispersion> The pH of the nanostructure dispersion is preferably 5.5 or higher, preferably 8.0 or lower, and more preferably 7.5 or lower. If the pH of the nanostructure dispersion is 5.5 or higher, the dispersion stability of the nanostructures can be improved. As a result, when an electronic device is manufactured using the nanostructure dispersion, the quality of the resulting electronic device can be improved. Furthermore, if the pH of the nanostructure dispersion is 7.5 or lower even during the manufacturing stage, for example, elution of metal components from ceramic filtration membranes used in the process of manufacturing the nanostructure dispersion can be suppressed, thereby reducing the amount of metal impurities contained in the nanostructure dispersion. As a result, the quality of the resulting electronic device can be improved.
[0046] <Method for Preparing Nanostructure Dispersion> The nanostructure dispersion can be prepared through a step (dispersion step) of dispersing a mixture containing fibrous carbon nanostructures having functional groups as nanostructures, a dispersion medium, and optional additives to obtain a dispersion. Furthermore, the dispersion obtained through the dispersion step is filled into a sealed container as needed (filling step). The dispersion filled into the sealed container is then subjected to a dispersion treatment as needed (container-filled dispersion dispersion step). Here, the dispersion filled into the sealed container can be stored in this state for a predetermined period of time (storage step). As described above, the filling step, container-filled dispersion dispersion step, and storage step are optional steps. Of these, the filling step, container-filled dispersion dispersion step, and storage step may be performed alone or in combination. When both the container-filled dispersion dispersion step and the storage step are performed, the order of their execution is not particularly limited. (i) The container-filled dispersion dispersion step may be performed immediately after the filling step, and then the storage step may be performed, or (ii) the container-filled dispersion dispersion step may be performed after the storage step. Furthermore, in the case of (i) above, a step of dispersing the container-containing dispersion may be carried out after the storage step.
[0047] In the dispersion step, a mixture containing fibrous carbon nanostructures having functional groups, a dispersion medium, and optional additives is subjected to a dispersion treatment to obtain a dispersion liquid. The dispersion method is not particularly limited, and any dispersion method can be used, but it is preferable to use a dispersion method using ultrasonic treatment. The dispersion temperature can be, for example, 5°C or higher and 35°C or lower. The dispersion time is preferably 0.5 hours or higher and 4 hours or lower. By setting the dispersion time within the above range, the Z-average particle size of the nanostructures based on dynamic light scattering can be appropriately controlled.
[0048] In the filling step, the dispersion obtained through the dispersing step is filled into a sealed container as needed. It is preferable to use a sealed container whose inner surface, at least the portion of which comes into contact with the dispersion, is made of a resin. Such a resin preferably contains at least one selected from high-density polyethylene, low-density polyethylene, polystyrene, polypropylene, and a fluorine-based resin. Among these, fluorine-based resins such as polytetrafluoroethylene (PTFE), fluorinated ethylene propylene (FEP), perfluoroalkoxyalkane (PFA), ethylene tetrafluoroethylene (ETFE), chlorotrifluoroethylene (CTFE), and polyvinylidene fluoride (PVDF) are more preferable, with ETFE and PVDF being particularly preferable. By storing the dispersion in a sealed container whose inner surface is made of at least one of the above resins, aggregation of the fibrous carbon nanostructures having functional groups can be effectively suppressed, thereby further improving the dispersion stability of the dispersion.
[0049] The reason why the above-mentioned various resins are suitable as materials for forming the sealed container is thought to be that they have low gas permeability. If the resin used as the material for forming the sealed container has low gas permeability, it is possible to effectively prevent gas from entering the sealed container. As a result, gases such as CO 2The reaction of the functional groups on the surface of the fibrous carbon nanostructure with the carbon nanoparticles, etc., can be effectively suppressed, which would promote aggregation. Furthermore, if the resin constituting the sealed container has low gas permeability, leakage of gas from inside the sealed container to the outside of the container can be suppressed, and from this perspective, detachment of the functional groups on the surface of the fibrous carbon nanostructure can be suppressed, thereby improving dispersion stability.
[0050] Here, when filling the sealed container with the nanostructure dispersion, the filling rate of the container containing the dispersion is preferably 90.0 vol% or more, more preferably 94.0 vol% or more, and preferably less than 98.0 vol%, and more preferably 97.0 vol% or less. If the filling rate of the container containing the dispersion is equal to or greater than the above-mentioned lower limit, a decrease in the dispersibility of the nanostructures contained in the nanostructure dispersion in the container can be effectively suppressed. On the other hand, if the filling rate is equal to or less than the above-mentioned upper limit, the possibility of the nanostructure dispersion spilling out of the container or the container bursting during use of the nanostructure dispersion can be effectively suppressed. Note that the nanostructure dispersion is preferably filled into the sealed container in a nitrogen gas atmosphere or argon gas atmosphere (i.e., an inert gas atmosphere), or in a clean environment of Class 10 or higher.
[0051] In the container-filled dispersion process, the dispersion filled in the sealed container is subjected to a dispersion treatment as necessary. Ultrasonic treatment can be used as a dispersion method for such dispersion treatment. The ultrasonic treatment conditions can be 5°C or higher and 35°C or lower, and 0.5 hours or longer and 120 minutes or shorter. The longer the dispersion time, the smaller the Z-average particle size of the nanostructures measured by dynamic light scattering. The shorter the dispersion time, the larger the Z-average particle size of the nanostructures measured by dynamic light scattering. Therefore, by appropriately controlling the dispersion time, the Z-average particle size of the nanostructures measured by dynamic light scattering can be appropriately controlled.
[0052] In the storage step, the dispersion liquid filled in the sealed container is left standing in that state and stored for a predetermined period of time. At this time, the sealed container is placed in a storage cabinet. The storage temperature in the storage cabinet needs to be 25°C or less from the viewpoint of dispersion stability, and is preferably above 0°C from the viewpoint of avoiding freezing. It is presumed that if the storage temperature is 25°C or less, Brownian motion in the dispersion liquid can be suppressed, and aggregation of nanostructures can be effectively suppressed. The upper and lower limits of the temperature range of the storage temperature can be 20°C, 15°C, 10°C, or 5°C.
[0053] The storage period is not particularly limited, but since long-term storage may increase the Z-average particle size of the nanostructures as determined by dynamic light scattering, i.e., may impair dispersibility, it is preferable that the storage period be such that the Z-average particle size is 70 nm or less, and specifically, 370 days or less.
[0054] Furthermore, the pressure of the atmosphere in which the sealed container is stored during the storage step (hereinafter also referred to as "storage pressure") is preferably 0 kPa or more and 100 kPa or less in gauge pressure. A storage pressure of 0 kPa or more can prevent a decrease in the pH of the nanostructure dispersion itself. This is presumably because the storage pressure is 0 kPa or more in gauge pressure, in other words, the storage pressure is not a reduced pressure condition, and therefore the compounds derived from the functional groups of the nanostructures and the compounds derived from any additives contained in the nanostructure dispersion can be prevented from evaporating. As a result of preventing a decrease in the pH of the nanostructure dispersion itself, aggregation of the nanostructures can be prevented, and ultimately, the uniformity of electronic devices manufactured using the nanostructure dispersion can be improved. Furthermore, a storage pressure of 100 kPa or less can prevent the nanostructure dispersion from thickening due to pressure. As a result, when manufacturing electronic devices using the nanostructure dispersion, for example, when a coating process is performed, the occurrence of coating spots can be effectively prevented. Furthermore, if the storage pressure is 100 kPa or less, when a gas barrier bag is used to increase the storage pressure, the bag can be prevented from breaking. The use of a gas barrier bag is not only effective as a tool for increasing the storage pressure, but can also be effective from the viewpoint of inhibiting the flow of gas between the inside and outside of the sealed container. The material of such a gas barrier bag is not particularly limited, but examples thereof include those listed above as resins that constitute the inner surface of the sealed container that comes into contact with the dispersion.
[0055] The nanostructure dispersion of the present invention can be removed from the sealed container and used to produce a nanostructure assembly by (1) removing the dispersion medium, or (2) mixing with a matrix material to form a composite material composition, which can be used to produce a composite material in any manner. In this case, an ion exchange step may be carried out, if necessary, to remove impurities such as metals from the nanostructure dispersion prior to removing the dispersion medium or mixing with the matrix material. As described above, the nanostructure dispersion of the present invention has excellent dispersion stability, which effectively prevents aggregation of the nanostructures and clogging of the ion exchange resin by the nanostructures during the ion exchange step.
[0056] (Method for storing nanostructure dispersion) The method for storing nanostructure dispersion of the present invention is a method for storing nanostructure dispersion in a sealed container filled with nanostructure dispersion containing nanostructures and a dispersion medium. Essential requirements here are that the nanostructures are fibrous carbon nanostructures having functional groups, and that the nanostructure dispersion has a filling rate of 90.0% by volume or more. Furthermore, at least the inner surface of the sealed container that comes into contact with the nanostructure dispersion must be formed from a resin, and the resin must include at least one selected from high-density polyethylene, low-density polyethylene, polystyrene, polypropylene, and fluororesin. Furthermore, the method for storing nanostructure dispersion of the present invention requires that the container containing the nanostructure dispersion be stored at a temperature below 25°C. This method for storing nanostructure dispersion ensures good dispersion stability of the nanostructure dispersion contained in the sealed container, thereby providing a nanostructure dispersion with excellent dispersion stability.
[0057] As the container for containing the nanostructure dispersion liquid, the above-mentioned container for containing the nanostructure dispersion liquid of the present invention can be suitably used.
[0058] When storing such a container containing a nanostructure dispersion liquid, it is possible to suitably use a storage cabinet equipped with a control unit that can set the storage temperature of the container containing the nanostructure dispersion liquid to 25°C or below.
[0059] The preferred ranges for the storage temperature, storage period, and pressure of the storage atmosphere are the same as those for the preferred ranges for the storage period and pressure in the storage process described in the section <Method for preparing nanostructure dispersion liquid>.
[0060] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples. The carbon nanotubes used in the examples and comparative examples were synthesized by the following method. Various evaluations in the examples and comparative examples were also performed using the following methods.
[0061] (Synthesis of Carbon Nanotubes) CNTs (SGCNT-1) were prepared by the super-growth method according to the description in International Publication No. 2006 / 011655. During the preparation of SGCNT-1, a catalyst layer was formed on the substrate surface by a wet process, and a raw material gas containing acetylene as the main component was used. The obtained SGCNT-1 had a BET specific surface area of 1,050 m. 2 / g (unopened), the micropore volume was 0.44 mL / g, and the Raman spectrophotometer measurement showed a pore size of 100 to 300 cm, which is characteristic of single-walled CNTs. -1 A radial breathing mode (RBM) spectrum was observed in the low wavenumber region. Furthermore, using a transmission electron microscope, the diameter and length of 100 randomly selected SGCNT-1 were measured, resulting in an average diameter (Av) of 3.3 nm, a standard deviation of the diameter (σ) multiplied by 3 (3σ) of 1.9 nm, a ratio of these (3σ / Av) of 0.58, and an average length of 500 μm. Furthermore, an adsorption isotherm of SGCNT-1 was measured using a fully automated specific surface area measuring device (manufactured by Mountec Co., Ltd., product name "Macsorb (registered trademark) HM model-1210"), and a t-plot was created by converting the relative pressure in the resulting adsorption isotherm to the average thickness t (nm) of the nitrogen gas adsorption layer. The t-plot showed an upwardly convex shape.
[0062] (Z-average particle size) 0.085 g of carbon nanotube dispersion (solid content concentration 0.3%) was diluted with 15 g of ultrapure water in a polypropylene container and then stirred for 5 seconds using a vortex mixer (manufactured by AS ONE Corporation, product name: Vortex Mixer GHW-3000). Thereafter, the Z-average particle size was measured using dynamic light scattering (DLS) (manufactured by Malvern Panalytical, product name: Zetasizer Nano ZS) according to the following procedure to obtain the Z-average particle size. The Z-average particle size was measured over time, and the amount of change (increase (%) calculated by dividing the value after time by the initial value minus the initial value) was obtained. A smaller amount of change indicates better dispersion stability. (1) Pretreatment before measurement 0.085 g of carbon nanotube dispersion (solid concentration 0.3%) was diluted with 15 g of ultrapure water in a PP container, and then stirred for 5 seconds in a vortex mixer (manufactured by AS ONE Corporation, product name: Vortex Mixer GHW-3000). (2) Measurement The carbon nanotube dispersion obtained above was added to a polystyrene cell (manufactured by Malvern Panalytical, product name: 12 mm square polystyrene cell DTS0012), and DLS measurement was performed under sample conditions (refractive index: 1.12, absorptivity: 39.2, dispersion medium: water, measurement temperature: 25.0 ° C, equilibration time: 240 seconds) and measurement conditions (measurement angle: 173 ° backscattering) to measure the Z-average particle size.
[0063] Example 1: Nanostructured SGCNT-1 (80 g) was stirred in 12 L of 10.4 M nitric acid for 2 hours, then diluted with ultrapure water to a 9.1 M nitric acid concentration, and purified by refluxing at 120°C for 12.5 hours. The mixture was then diluted with ultrapure water to a 1.7 M nitric acid concentration, and cross-flow filtered using a 0.01 μm ceramic membrane until the pH reached 6.5. The liquid that passed through the ceramic membrane was discarded as permeate, and the liquid that did not pass through the filter pores was collected as retentate. Subsequently, ammonia water and ammonium nitrate water were added to the retentate to adjust the pH of the retentate to 7.9 and the nitrate ion concentration to 100 ppm. Then, ultrasonic treatment was performed for 3 hours using an ultrasonic irradiation machine (Tokyo Ultrasonics Giken Co., Ltd., product name: PUC-1415). Carbon nanotube dispersion 1 was thus obtained. DLS measurement was performed on the obtained carbon nanotube dispersion 1 as described above, and the Z-average particle size was measured. A 4 L (actual capacity: 4.20 L) polyethylene sealed container (manufactured by Aicello, product name: Clean Barrier Bottle SGL (G) PR, made of high-density polyethylene) was filled with carbon nanotube dispersion 1 (4.00 L) in a class 100 clean booth. The filling rate of the CNT dispersion in the sealed container was 95.2% by volume. The container filled with the CNT dispersion was then placed in a constant temperature and humidity chamber (manufactured by ESPEC, product name: SH-241) set at 25 ° C. as a storage cabinet. 90 days later, starting from the day of placement, the CNT dispersion-filled container was removed, and the CNT dispersion in the container was allowed to stand for 2 hours to return to room temperature, after which it was subjected to DLS measurement. As a result, the Z-average particle size increase rate was 21.6%.
[0064] Example 2 The same operation as in Example 1 was carried out, except that a thermo-hygrostat set at 5° C. was used as the storage cabinet. As a result, the Z-average particle size increase rate was 7.5%.
[0065] (Example 3) The same operation as in Example 1 was carried out, except that 4.7 L of carbon nanotube dispersion 1 was filled into a 5 L volume ETFE container (manufactured by Sanplatec Co., Ltd., product name: ETFE narrow-mouth large rotational molding container) as a sealed container. As a result, the Z-average particle size increase rate was 18.3%. The filling rate of the CNT dispersion in the sealed container was 94.0 vol%.
[0066] Example 4 The same operation as in Example 3 was carried out, except that a thermo-hygrostat set at 5° C. was used as the storage cabinet. As a result, the Z-average particle size increase rate was 7.1%.
[0067] (Example 5) The same operation as in Example 1 was carried out, except that 0.94 L of the carbon nanotube dispersion 1 was filled into a 1 L volume PFA container (manufactured by Flon Industries Co., Ltd., product name: F-1004) as a sealed container. As a result, the Z-average particle size increase rate was 18.8%. The filling rate of the CNT dispersion in the sealed container was 94.0 vol%.
[0068] Example 6 A polyethylene sealed container (manufactured by Aicello, product name: Clean Barrier Bottle SGL(G)PR) with a volume of 4 L (actual capacity: 4.20 L) was used as the sealed container, and carbon nanotube dispersion liquid 1 (4.00 L) was filled in a class 100 clean booth. The filling rate of the CNT dispersion liquid in the sealed container was 95.2 volume %. Next, the container containing carbon nanotube dispersion liquid 1 was placed in a gas barrier bag (manufactured by Asahi Kasei Pax, product name: Corpac Sta St3550a), and the opening of the bag was then set in a vacuum gas filling sealer (manufactured by Fuji Impulse, product name: V-610G). N2 was then pressurized to 100 kPa, and the opening was heat-sealed and hermetically sealed. Thereafter, the container filled with the CNT dispersion liquid was placed in a constant temperature and humidity chamber (manufactured by ESPEC, product name: SH-241) set to 25°C. After 90 days from the day of addition, the container filled with the CNT dispersion was removed, and the CNT dispersion in the container was allowed to stand for 2 hours to return to room temperature, after which it was used for DLS measurement. As a result, the Z-average particle size increase rate was 13.1%.
[0069] Comparative Example 1 The same operation as in Example 1 was carried out, except that a thermo-hygrostat set at 35° C. was used. As a result, the Z-average particle size increase rate was 33.0%.
[0070] Comparative Example 2 The same operation as in Example 1 was carried out, except that 1.88 L of carbon nanotube dispersion 1 was filled into a 2 L vinyl chloride container (manufactured by Tokyo Glass Kikai Co., Ltd., product name: PVC wide-mouth bottle CE-2000) as a sealed container. As a result, the Z-average particle size increase rate was 27.2%. The filling rate of the CNT dispersion in the sealed container was 94.0% by volume.
[0071] Comparative Example 3 Carbon nanotube dispersion liquid 1 (4.00 L) was filled into a polyethylene airtight container (manufactured by Aicello, product name: Clean Barrier Bottle SGL(G)PR) with a volume of 4 L (actual capacity: 4.20 L) in a class 100 clean booth. The filling rate of the CNT dispersion liquid in the airtight container was 95.2% by volume. Thereafter, the container containing carbon nanotube dispersion liquid 1 was placed in a gas barrier bag (manufactured by Asahi Kasei Pax, product name: Corpac Sta St3550a), and the opening of the bag was then set in a vacuum sealer (manufactured by Fuji Impulse, product name: V-460-10) set to a vacuum setting of -100 kPa. After degassing to -87 kPa, the opening was heat-sealed and hermetically sealed. Thereafter, the container was placed in a constant temperature and humidity chamber (manufactured by ESPEC, product name: SH-241) set to 35°C. After 90 days from the day of addition, the container filled with the CNT dispersion was removed, and the CNT dispersion in the container was allowed to stand for 2 hours to return to room temperature, after which it was subjected to DLS measurement. As a result, the Z-average particle size increase rate was 36.5%.
[0072] According to the present invention, it is possible to provide a nanostructure dispersion liquid having excellent dispersion stability.
Claims
1. A container containing a nanostructure dispersion liquid stored in a storage facility, the container containing the nanostructure dispersion liquid comprising a nanostructure dispersion liquid containing nanostructures and a dispersion medium, and a sealed container for containing the nanostructure dispersion liquid, the nanostructures being fibrous carbon nanostructures having functional groups, the filling rate of the nanostructure dispersion liquid in the sealed container being 90.0 volume % or more, at least the inner surface portion of the sealed container that comes into contact with the nanostructure dispersion liquid being formed from a resin, the resin comprising at least one type selected from high density polyethylene, low density polyethylene, polystyrene, polypropylene, and fluorine-based resin, and the storage facility being equipped with a control unit capable of setting the storage temperature of the container containing the nanostructure dispersion liquid to 25°C or below.
2. A container containing a nanostructure dispersion liquid according to claim 1, wherein the nanostructure is a carbon nanotube.
3. The container containing the nanostructure dispersion liquid according to claim 2, wherein the carbon nanotubes include single-walled carbon nanotubes.
4. A container containing a nanostructure dispersion liquid according to claim 2, wherein the carbon nanotubes have an upwardly convex t-plot obtained from an adsorption isotherm.
5. A storage unit for storing a container containing the nanostructure dispersion liquid according to any one of claims 1 to 4.
6. A method for storing a nanostructure dispersion liquid, comprising storing the nanostructure dispersion liquid in a state in which the nanostructure dispersion liquid containing nanostructures and a dispersion medium is filled in a sealed container, wherein the nanostructures are fibrous carbon nanostructures having functional groups, the filling rate of the nanostructure dispersion liquid is 90.0 volume % or more, the sealed container is a container in which at least the inner surface portion that comes into contact with the nanostructure dispersion liquid is formed from a resin, the resin comprises at least one type selected from high density polyethylene, low density polyethylene, polystyrene, polypropylene, and a fluororesin, and the container containing the nanostructure dispersion liquid is stored at a temperature condition of less than 25°C.
Citation Information
Patent Citations
Reduction of aggregates in nanowire suspensions stored in containers
JP2015527259A
Production method of transparent conductive film and transparent conductive film
JP2020119707A
Carbon nanotube dispersion and utilization thereof
JP2020189770A
Nanotube solution treated with molecular additive, nanotube film having enhanced adhesion property, and methods for forming the nanotube solution and the nanotube film
US20130224934A1
Container holding nanostructure liquid dispersion, method for storing and method for transporting nanostructure liquid dispersion, and method for producing aggregate and composition for composite material using nanostructure liquid dispersion
WO2017115707A1