Electrode
The electrode structure with a metal or semimetal first base layer and a metal second base layer, combined with a conductive carbon layer, addresses the challenge of maintaining low resistance and reliability by suppressing outgassing and oxidation, ensuring accurate and sensitive electrochemical measurements.
Patent Information
- Application Number
- PCT/JP2024/008518
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-28
- Filing Date
- 2024-03-06
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional carbon electrodes face challenges in maintaining low absolute resistance values and high reliability due to outgassing from film base materials, which can lead to increased resistance over time, and oxidation issues affecting measurement accuracy.
The electrode structure comprises a base film, a first base layer with a metal or semimetal layer, and a second base layer with a metal layer, where the resistivity of the first base layer is 10 times or more than the second base layer, and a conductive carbon layer with sp² and sp³ bonds, ensuring low absolute resistance and high reliability by suppressing outgassing and oxidation.
This configuration results in an electrode with a low absolute resistance value and high reliability, maintaining measurement sensitivity and accuracy over time by effectively managing outgassing and oxidation effects.
Smart Images

Figure JP2024008518_03102024_PF_FP_ABST
Abstract
Description
electrode
[0001] The present invention relates to an electrode.
[0002] Conventionally, carbon electrodes have been known as electrodes (working electrodes) used in electrochemical measurements.
[0003] As such a carbon electrode, for example, an electrode has been proposed which includes a film substrate, a titanium thin film, and a carbon thin film in that order in the thickness direction (see, for example, Patent Document 1 listed below).
[0004] As such a carbon electrode, for example, an electrode has been proposed which includes a film substrate, a silicon oxide thin film, a titanium thin film, and a carbon thin film in that order in the thickness direction (see, for example, Patent Document 2 listed below).
[0005] International Publication No. 2019 / 117112 Brochure International Publication No. 2022 / 019299 Brochure
[0006] On the other hand, electrodes used in electrochemical measurements must have a low absolute resistance value to improve measurement sensitivity, and must also be highly reliable to ensure measurement accuracy.
[0007] In the carbon electrode of Patent Document 1, the titanium thin film can reduce the absolute resistance value, but the absolute resistance value may change over time due to outgassing from the film substrate, and therefore even higher reliability is desired.
[0008] In the electrode of Patent Document 2, the silicon oxide thin film suppresses outgassing from the film substrate and ensures high reliability. However, the silicon oxide thin film oxidizes the titanium thin film during film formation, which can increase the absolute resistance value of the entire electrode. Therefore, it is desirable to further reduce the absolute resistance value of the entire electrode.
[0009] The present invention aims to provide an electrode having a low absolute resistance value and high reliability.
[0010] The present invention [1] includes an electrode comprising a base film, a first underlayer, a second underlayer, and a conductive carbon layer in that order toward one side in a thickness direction, wherein the first underlayer is a metal layer or a semi-metal layer, the second underlayer is a metal layer, and the resistivity of the first underlayer is 10 times or more the resistivity of the second underlayer.
[0011] The present invention [2] is a method for manufacturing a conductive carbon layer comprising: 2 Bonds and sp 3 The electrode according to [1] has a bond.
[0012] The present invention [3] includes the electrode according to [1] or [2], wherein the second underlayer contains titanium.
[0013] The present invention [4] is characterized in that the resistivity of the second underlayer is 3.0×10 -4 The electrode according to any one of [1] to [3] has a resistance of Ω·cm or less.
[0014] The present invention [5] includes the electrode according to any one of [1] to [4], wherein the first underlayer is a semi-metal layer and contains silicon.
[0015] The present invention [6] includes the electrode according to any one of [1] to [5], wherein the thickness of the first underlayer is 3 nm or more.
[0016] The present invention [7] includes the electrode according to any one of [1] to [6], which is an electrode for electrochemical measurements.
[0017] The electrode of the present invention has a low absolute resistance value and is highly reliable.
[0018] FIG. 1 is a cross-sectional view of one embodiment of the electrode of the present invention.
[0019] <One embodiment> One embodiment of the electrode film of the present invention will be described with reference to Fig. 1. In Fig. 1, the up-down direction on the paper surface is the up-down direction (thickness direction, first direction), the upper side of the paper surface is the upper side (one side in the thickness direction, one side in the first direction), and the lower side of the paper surface is the lower side (the other side in the thickness direction, the other side in the first direction). Furthermore, the left-right direction and the depth direction on the paper surface are surface directions perpendicular to the up-down direction. Specifically, they conform to the directional arrows in each figure.
[0020] As shown in Fig. 1 , the electrode 1 has a predetermined thickness. The electrode 1 has a film shape (including a sheet shape). The electrode 1 includes, in order toward one side in the thickness direction, a base film 2, a first base layer 3, a second base layer 4, and a conductive carbon layer 5. Specifically, the electrode 1 includes only the base film 2, the first base layer 3, the second base layer 4, and the conductive carbon layer 5.
[0021] [Substrate Film] The substrate film 2 is a substrate that supports the first underlayer 3, the second underlayer 4, and the conductive carbon layer 5. The substrate film 2 is the bottom layer of the electrode 1 and has a film shape.
[0022] The base film 2 has a predetermined thickness. Examples of materials for the base film 2 include organic materials.
[0023] An example of the organic material is a resin material.
[0024] Examples of resin materials include polyester resin, acetate resin, polyethersulfone resin, polycarbonate resin, polyamide resin, polyimide resin, polyolefin resin, acrylic resin, polyvinyl chloride resin, polyvinylidene chloride resin, polystyrene resin, polyvinyl alcohol resin, polyarylate resin, and polyphenylene sulfide resin, and preferably polyester resin.
[0025] Examples of polyester resins include polyethylene terephthalate and polyethylene naphthalate, and preferably polyethylene terephthalate.
[0026] The materials for the base film 2 can be used alone or in combination.
[0027] There are no particular limitations on the thickness of the base film 2. The thickness of the base film 2 is, for example, 2 μm or more, preferably 20 μm or more, more preferably 50 μm or more, and even more preferably 100 μm or more, and for example, 1000 μm or less, preferably 500 μm or less, and more preferably 300 μm or less.
[0028] <First Undercoat Layer> The first undercoat layer 3 is a layer that suppresses the influence of the base film 2 on the second undercoat layer 4. The first undercoat layer 3 is disposed on one surface in the thickness direction of the base film 2. Specifically, the first undercoat layer 3 is in contact with the entire one surface in the thickness direction of the base film 2. The first undercoat layer 3 has a predetermined thickness.
[0029] The first underlayer 3 may be a metal layer or a semi-metal layer. It is preferable that the first underlayer 3 is not a metal oxide layer or a semi-metal oxide layer.
[0030] If the first underlayer 3 is not a metal oxide layer or a semi-metal oxide layer, oxidation can be suppressed when forming the second underlayer 4 described later, and the absolute resistance value of the electrode 1 can be reduced.
[0031] The metal layer serving as the first underlayer 3 is made of a metal.
[0032] Examples of metals that can be used as materials for the first underlayer 3 include platinum, tin, tantalum, chromium, palladium, niobium, rhenium, strontium, vanadium, ytterbium, gallium, hafnium, zirconium, titanium, germanium, scandium, lutetium, yttrium, lanthanum, neodymium, thulium, praseodymium, holmium, cerium, erbium, europium, dysprosium, samarium, radium, bismuth, terbium, gadolinium, manganese, and alloys thereof.
[0033] The metals used as the material for the first underlayer 3 can be used alone or in combination.
[0034] The semi-metal layer as the first underlayer 3 is made of a semi-metal. The semi-metal is not limited.
[0035] An example of a semimetal that can be used as the material for the first underlayer 3 is silicon.
[0036] The semi-metals as the material of the first underlayer 3 can be used alone or in combination.
[0037] The first underlayer 3 is preferably a semi-metal layer.
[0038] The resistivity (measured value in a thin film) of the first underlayer 3 is, for example, 10×10-6 Ω cm or more, preferably 4.0 × 10 -5 Ω cm or more, more preferably 10 × 10 -5 Ω cm or more, more preferably 5.0 × 10 -4 Ω cm or more, particularly preferably 10 × 10 -4 Ω cm or more, for example, 1.0 × 10 3 It is Ω·cm or less.
[0039] The resistivity (thin film measured value) of the first underlayer 3 can be determined by multiplying the absolute resistance value (Ω / □) of the single layer of the first underlayer 3 (the state in which the first underlayer 3 is formed on the base film 2) by the thickness of the first underlayer 3. Specifically, it is measured as described in the examples below.
[0040] If the resistivity of the first underlayer 3 is equal to or higher than the lower limit described above, even if the first underlayer 3 is oxidized due to outgassing from the substrate film 2, the effect on the absolute resistance value of the electrode 1 is small, and therefore the absolute resistance value of the electrode 1 can be reduced.
[0041] There are no particular limitations on the thickness of the first underlayer 3. The thickness of the first underlayer 3 is, for example, 1 nm or more, preferably 3 nm or more, and for example, 50 nm or less, preferably 25 nm or less, more preferably 10 nm or less.
[0042] When the thickness of the first underlayer 3 is equal to or greater than the above-mentioned lower limit, the first underlayer 3 has excellent uniformity across the surface. In addition, the permeation of outgassing from the substrate film 2 can be suppressed, and the change over time in the absolute value of the resistance of the second underlayer 4 (described later) can be suppressed, resulting in excellent reliability of the electrode 1.
[0043] <Second Underlayer> The second underlayer 4 is disposed on one thickness-wise surface of the first underlayer 3. Specifically, the second underlayer 4 is in contact with the entire one thickness-wise surface of the first underlayer 3. The second underlayer 4 has a predetermined thickness.
[0044] The second underlayer 4 may be a metal layer.
[0045] The metal layer serving as the second underlayer 4 is made of a metal.
[0046] As the metal material for the second underlayer 4, a metal capable of forming a carbide together with the carbon of the conductive carbon layer 5, which will be described next, is preferred.
[0047] From the viewpoint of ensuring the chemical stability of the conductive carbon layer 5, examples of metals that can be used as the material for the second underlayer 4 include silver, copper, gold, aluminum, magnesium, rhodium, tungsten, iridium, cobalt, nickel, ruthenium, indium, osmium, iron, platinum, tin, tantalum, chromium, palladium, niobium, rhenium, strontium, vanadium, ytterbium, gallium, hafnium, zirconium, titanium, germanium, scandium, lutetium, yttrium, lanthanum, neodymium, thulium, praseodymium, holmium, cerium, erbium, europium, dysprosium, samarium, radium, bismuth, terbium, gadolinium, molybdenum, and manganese, and preferably titanium and niobium.
[0048] The metals used as the material for the second underlayer 4 can be used alone or in combination.
[0049] The resistivity (measured value in thin film) of the second underlayer 4 is, for example, 10×10 -4 Ω cm or less, preferably 5.0 × 10 -4 Ω cm or less, more preferably 3.0 × 10 -4 Ω cm or less, more preferably 2.0 × 10 -4 Ω cm or less, particularly preferably 1.5 × 10 -4 Ω cm or less, for example, 1.0 × 10 -7 It is Ω·cm or more.
[0050] The resistivity (thin film measured value) of the second underlayer 4 can be determined by multiplying the absolute resistance value (Ω / □) of the electrode (electrode including the base film 2, the second underlayer 4, and the conductive carbon layer 5) by the thickness of the second underlayer 4. As with the first underlayer 3, the absolute resistance value (Ω / □) of the second underlayer 4 as a single layer may be used. However, since the resistivity of the second underlayer 4 is sufficiently lower than the resistivity of the conductive carbon layer 5, the influence of the absolute resistance value (Ω / □) of the conductive carbon layer 5 on the electrode can be ignored, and therefore the absolute resistance value (Ω / □) of the electrode described above can be used. Specifically, it is measured as described in the examples below.
[0051] If the resistivity of the second underlayer 4 is equal to or less than the upper limit, the absolute value of the resistance of the electrode 1 can be reduced.
[0052] There are no particular limitations on the thickness of the second underlayer 4. The thickness of the second underlayer 4 is, for example, 1 nm or more, preferably 3 nm or more, more preferably 5 nm or more, and for example, 50 nm or less, preferably 30 nm or less.
[0053] If the thickness of the second underlayer 4 is equal to or greater than the above-mentioned lower limit, the second underlayer 4 has excellent uniformity across the surface.
[0054] On the other hand, if the thickness of the second underlayer 4 is equal to or less than the above upper limit, the second underlayer 4 also has excellent conductivity.
[0055] The resistivity of the first underlayer 3 is 10 times or more, preferably 100 times or more, more preferably 1×10 times or more, than the resistivity of the second underlayer 4. 3 times or more, more preferably 1×10 4 times or more, for example, 1×10 20 It is less than double.
[0056] If the resistivity of the first underlayer 3 is a multiple of or greater than the above-mentioned lower limit of the resistivity of the second underlayer 4, even if the first underlayer 3 is oxidized by outgassing from the substrate film 2, the impact on the absolute resistance value of the entire electrode 1 can be suppressed, and resistance changes can be suppressed.
[0057] <Conductive Carbon Layer> The conductive carbon layer 5 has electrode properties and serves as an electrode. The conductive carbon layer 5 is disposed on one surface in the thickness direction of the second underlayer 4. Specifically, the conductive carbon layer 5 is in contact with the entire one surface in the thickness direction of the second underlayer 4. The conductive carbon layer 5 is the uppermost layer of the electrode 1 and has a predetermined thickness.
[0058] The material of the conductive carbon layer 5 is carbon, preferably sp 2 Bonds and sp 3 It is a carbon with a sp bond. 2 Bonds and sp 3 Carbon with sp bonds has a graphite-type structure and a diamond structure. 3 Number of bonded atoms and sp 2 sp for the sum of the number of atoms bonded 3 The ratio of the number of bonded atoms (sp 3 / sp 3 +sp 2 ) is not particularly limited. 3 / sp 3 +sp 2 ) is, for example, 0.1 or more, preferably 0.2 or more, and for example, 0.9 or less, preferably 0.5 or less. 3 / sp 3 +sp 2 ) is a spectrum obtained by measuring one surface in the thickness direction of the conductive carbon layer 5 by X-ray photoelectron spectroscopy. 2 Bond peak intensity and sp 3 Calculations are based on peak binding intensities.
[0059] There are no particular limitations on the thickness of the conductive carbon layer 5. The thickness of the conductive carbon layer 5 is, for example, 5 nm or more, preferably 8 nm or more, and for example, 200 nm or less, preferably 100 nm or less, more preferably 50 nm or less. The thickness of the conductive carbon layer 5 can be calculated by measuring X-ray reflectivity.
[0060] In addition, a carbide layer (not shown) is preferably formed at the interface between the conductive carbon layer 5 and the second underlayer 4. The carbide layer is made of carbide, which is a compound of the metal of the second underlayer 4 and the carbon of the conductive carbon layer 5. The carbide layer improves the adhesion between the conductive carbon layer 5 and the second underlayer 4. In this case, the electrode 1 includes, in order toward one side in the thickness direction, the base film 2, the first underlayer 3, the second underlayer 4, a carbide layer (not shown), and the conductive carbon layer 5.
[0061] The conductive carbon layer 5 may contain other elements in addition to carbon.
[0062] <Method for Manufacturing Electrode> Next, a method for manufacturing the electrode 1 will be described. First, a base film 2 is prepared. Next, a first base layer 3, a second base layer 4, and a conductive carbon layer 5 are formed in this order on one side of the base film 2 in the thickness direction.
[0063] Examples of methods for forming the first underlayer 3 include dry methods and wet methods. Preferably, the dry method is used. Examples of dry methods include PVD (physical vapor deposition) and CVD (chemical vapor deposition). Preferably, the dry method is used. Examples of PVD methods include sputtering, vacuum deposition, laser deposition, and ion plating (arc deposition). Preferably, the PVD method is used sputtering. The sputtering method is not particularly limited. Examples of sputtering methods include unbalanced magnetron sputtering (UBM sputtering), high-power pulse sputtering, electron cyclotron resonance sputtering, RF sputtering, DC sputtering (DC magnetron sputtering), DC pulse sputtering, and ion beam sputtering.
[0064] In the sputtering method, for example, a sputtering gas containing an inert gas and an inorganic target are used, and the sputtering gas preferably does not contain oxygen.
[0065] If the sputtering gas does not contain oxygen, oxidation of the metal or semimetal used as the material for the first underlayer 3 can be suppressed.
[0066] An example of the inert gas is argon.
[0067] Examples of materials for the first underlayer 3 include the above-mentioned metals and semimetals, and preferably semimetals.
[0068] The second underlayer 4 may be formed by the same method as the above-described method for forming the first underlayer 3 .
[0069] From the viewpoint of ensuring the chemical stability of the conductive carbon layer 5, the material of the second underlayer 4 may be, for example, the metals mentioned above, and preferably titanium and niobium.
[0070] The conductive carbon layer 5 can be formed by the same method as the above-described method for forming the first underlayer 3. When the conductive carbon layer 5 is formed by a sputtering method, for example, carbon, preferably sintered carbon, is used as the target material.
[0071] As a result, the electrode 1 is obtained.
[0072] The total thickness of the obtained electrode 1 is, for example, 2 μm or more, preferably 20 μm or more, more preferably 50 μm or more, and even more preferably 100 μm or more, and for example, 1000 μm or less, preferably 500 μm or less, and more preferably 300 μm or less.
[0073] The absolute resistance value of the electrode 1 is, for example, 1.0×10 3 Ω / □ or less, preferably 5.0×10 2 Ω / □ or less, more preferably 3.0×10 2 The absolute resistance value is Ω / □ or less. The absolute resistance value can be measured by the method described below.
[0074] The rate of change in the absolute resistance value (reliability) of the electrode 1 is, for example, 50% or less, preferably 10% or less, more preferably 5% or less, even more preferably 3% or less, and particularly preferably 1% or less. The rate of change in the absolute resistance value (reliability) can be measured by the method described below.
[0075] <Effects> This electrode 1 comprises, in order toward one side in the thickness direction, a base film 2, a first underlayer 3, a second underlayer 4, and a conductive carbon layer 5. The first underlayer 3 is a metal layer or a semi-metal layer, and the second underlayer 4 is a metal layer. The resistivity of the first underlayer 3 is at least 10 times that of the second underlayer 4, so that the absolute value of resistance is low and the electrode has high reliability.
[0076] More specifically, since the first underlayer 3 is provided on one side of the substrate film 2 in the thickness direction, permeation of outgassing from the substrate film 2 can be suppressed, and oxidation of the second underlayer 4 can be suppressed.
[0077] Even if the first underlayer 3 is oxidized by outgassing from the base film 2 and the absolute resistance value of the first underlayer 3 increases, the resistivity of the first underlayer 3 is more than 10 times that of the second underlayer 4, so the effect on the absolute resistance value of the entire electrode 1 can be suppressed and the absolute resistance value of the electrode 1 can be reduced.
[0078] Furthermore, the first underlayer 3 can suppress permeation of outgassing from the substrate film 2 and can suppress oxidation of the second underlayer 4, so that the electrode 1 has excellent reliability.
[0079] Furthermore, since the first underlayer 3 is a metal or semimetal, oxidation of the second underlayer 4 can be suppressed, and the absolute resistance value of the electrode 1 can be reduced.
[0080] <Use> There is no particular limitation on the use of the electrode 1. For example, the electrode 1 may be used as an electrode for electrochemical measurement. Specifically, the electrode 1 is provided in an electrochemical measurement system that includes the electrode 1 as a working electrode.
[0081] The present invention will be described in more detail below with reference to examples and comparative examples. It should be noted that the present invention is in no way limited to these examples and comparative examples. The specific numerical values of the blending ratios (content ratios), physical property values, parameters, etc. used in the following description can be replaced with the upper limit (a numerical value defined as "equal to or less than") or lower limit (a numerical value defined as "equal to or more than") of the corresponding blending ratios (content ratios), physical property values, parameters, etc. described in the "Description of the Invention" above.
[0082] Example 1 A substrate film 2 made of polyethylene terephthalate and having a thickness of 188 μm was prepared.
[0083] Next, a semi-metal layer (first underlayer 3) made of silicon was formed by magnetron sputtering on one surface in the thickness direction of the substrate film 2. The conditions for the magnetron sputtering were as follows.
[0084] Target material: silicon Target power: 1.1 W / cm 2 Sputtering gas: argon Pressure in sputtering chamber: 0.2 Pa
[0085] The thickness of the semi-metal layer was 5 nm.
[0086] Next, a metal layer (second underlayer 4) made of titanium was formed on one surface in the thickness direction of the semi-metal layer (first underlayer 3) by magnetron sputtering under the following conditions:
[0087] Target material: titanium Target power: 0.4 W / cm 2 Sputtering gas: argon Pressure in sputtering chamber: 0.2 Pa
[0088] The thickness of the second underlayer 4 was 8 nm.
[0089] Next, a conductive carbon layer 5 was formed by DC pulse sputtering on one surface in the thickness direction of the second underlayer 4. The conditions for the DC pulse sputtering were as follows.
[0090] Target material: sintered carbon Target power: 3.0 W / cm 2 Sputtering gas: argon Pressure in sputtering chamber: 0.2 Pa
[0091] The thickness of the conductive carbon layer 5 was 10 nm.
[0092] In this way, an electrode 1 was manufactured which was provided with the substrate film 2, the semi-metal layer (first underlayer 3), the second underlayer 4, and the conductive carbon layer 5 in this order toward one side in the thickness direction.
[0093] Example 2 An electrode of Example 2 was manufactured in the same manner as the electrode of Example 1, except for the following: The thickness of the semi-metallic layer was set to 3 nm, and a metal layer made of niobium and having a thickness of 15 nm was formed on one thickness-wise surface of the semi-metallic layer (first underlayer 3) as the second underlayer 4. The magnetron sputtering conditions for forming the second underlayer 4 were as follows:
[0094] Target material: niobium Target power: 0.4 W / cm 2 Sputtering gas: argon Pressure in sputtering chamber: 0.2 Pa
[0095] Examples 3 and 4 Electrodes of Examples 3 and 4 were produced in the same manner as the electrode of Example 2, except that the thickness of the metal layer (second underlayer 4) made of niobium was changed as shown in Table 1.
[0096] Comparative Example 1 The electrode 1 was treated in the same manner as in Example 1, except that the first underlayer 3 was not formed. That is, the electrode 1 was provided with the base film 2, the second underlayer 4, and the conductive carbon layer 5 in this order toward one side in the thickness direction.
[0097] Comparative Example 2 The same process as in Example 1 was carried out except that a semi-metal oxide layer was formed instead of the semi-metal layer. That is, a semi-metal oxide layer made of silicon oxide was formed by magnetron sputtering on one surface in the thickness direction of the base film 2. The conditions for the magnetron sputtering were as follows:
[0098] Target material: silicon Target power: 3.3 W / cm 2Sputtering gas: argon and oxygen (flow ratio 9:1) Sputtering pressure: 0.2 Pa
[0099] The thickness of the semi-metal oxide layer was 5 nm.
[0100] In this way, an electrode 1 was produced which was provided with the substrate film 2, the semi-metal oxide layer, the second underlayer 4, and the conductive carbon layer 5 in this order toward one side in the thickness direction.
[0101] Comparative Examples 3 to 5 were treated in the same manner as in Examples 2 to 4, except that the first underlayer 3 was not formed. That is, the electrodes 1 in Comparative Examples 3 to 5 were provided with a base film 2, a second underlayer 4, and a conductive carbon layer 5 in this order toward one side in the thickness direction.
[0102] [Specific Resistivity of First Underlayer (Actual Thin Film Measurement Value)] Sample 1 was prepared by forming a semi-metallic layer (first underlayer 3) made of silicon on one thickness-wise surface of a 188 μm-thick polyethylene terephthalate substrate film 2 using a magnetron sputtering method. The conditions for the magnetron sputtering method when forming the first underlayer 3 were the same as those in Example 1. The thickness of the semi-metallic layer was 5 nm.
[0103] The absolute resistance value of the prepared sample 1 was measured by the same method as that described in the evaluation below. The absolute resistance value (Ω / □) of sample 1 was measured at the upper limit of measurement of the measuring device (1.0 × 10 7 The resistivity of the silicon thin film with a thickness of 5 nm exceeded 50,000×10 -4 The resistivity of Sample 1 was greater than Ω·cm. The resistivity of Sample 1 corresponds to the resistivity of the first underlayer of Example 1 (measured thin film value).
[0104] Sample 2 was prepared in the same manner as Sample 1, except that a semi-metallic layer (first underlayer 3) made of silicon with a thickness of 3 nm was formed, and the absolute resistance value was measured. The absolute resistance value of Sample 2 was also measured within the upper limit of measurement of the measurement device (1.0 × 10 7 The resistivity of the silicon thin film with a thickness of 3 nm exceeded 30,000×10 -4The resistivity of Sample 2 corresponds to the resistivity of the first underlayer of Examples 2 to 4 (measured thin film value).
[0105] Sample 3 was prepared in the same manner as Sample 1, except that the magnetron sputtering conditions were the same as those of Comparative Example 2. That is, Sample 3 had a first underlayer 3 made of a semi-metal oxide layer with a thickness of 5 nm on one surface in the thickness direction of a substrate film 2. The absolute resistance value of Sample 3 was also measured. The absolute resistance value of Sample 3 was also measured within the upper measurement limit of the measurement device (1.0 × 10 7 The resistivity of the semi-metal oxide layer with a thickness of 5 nm exceeded 50,000×10 -4 The resistivity of Sample 3 was greater than Ω·cm. The resistivity of Sample 3 corresponds to the resistivity of the first underlayer of Comparative Example 2 (measured thin film value).
[0106] <Evaluation> [Absolute Resistance Value] The electrodes of each Example and Comparative Example were cut to a size of 210 x 297 mm, and the absolute resistance value was measured by eddy current measurement using a NAPSON NC-80LINE. A non-contact measurement probe unit was swept along the long side, and the average of the sheet resistance values excluding data from 10 mm at both ends was used as the absolute resistance value. The results of the absolute resistance values are shown in Table 1. The absolute resistance values of the electrodes of Comparative Examples 1 and 3 to 5 were also multiplied by the thickness of the second underlayer 4 to calculate the resistivity of the second underlayer 4 (measured thin film value). As described above, because the resistivity of the second underlayer 4 was sufficiently lower than the resistivity of the conductive carbon layer 5, the influence of the absolute resistance value (Ω / □) of the conductive carbon layer 5 on the electrode was negligible. The results are shown in Table 1. The resistivity (thin film measured value) of each of the second underlayers 4 in Comparative Example 1 and Comparative Examples 3 to 5 corresponds to the resistivity (thin film measured value) of the second underlayers 4 in Examples 1 to 4.
[0107] [Reliability] In each example and comparative example, the reliability of the electrode was evaluated by the following method. That is, the electrodes of Example 1 and each comparative example were cut to a size of 210 x 297 mm and stored at room temperature under atmospheric conditions for one month. The absolute resistance values before and after storage were measured by the above method. The rate of change in absolute resistance value (reliability) was calculated from the absolute resistance values before and after storage according to the following formula. The results regarding reliability are shown in Table 1. Rate of change in absolute resistance value (%) = (| absolute resistance value before storage - absolute resistance value after storage |) / absolute resistance value before storage x 100
[0108]
[0109] The resistivity (thin film measured value) of the first underlayer used in each example was 10 times or more the resistivity (thin film measured value) of the second underlayer. Note that, when measuring the absolute resistance values used for the resistivity (thin film measured value) of the first underlayer and the resistivity (thin film measured value) of the second underlayer, both measurements were taken with the substrate film attached. However, when comparing the resistivity magnifications, the influences of these two measurements cancel each other out and can be ignored.
[0110] In each example, the first underlayer was a metal layer or a semi-metal layer, and the resistivity (measured thin film value) of the first underlayer was 10 times or more the resistivity (measured thin film value) of the second underlayer, resulting in excellent absolute resistance and reliability of the electrode. On the other hand, Comparative Example 1 and Comparative Examples 3 to 5 did not have a first underlayer and therefore were inferior in reliability. Furthermore, Comparative Example 2 had a poor absolute resistance value because the first underlayer was a semi-metal oxide layer.
[0111] The above invention is provided as an exemplary embodiment of the present invention, but this is merely an example and should not be interpreted as limiting. Modifications of the present invention that are obvious to those skilled in the art are intended to be included in the scope of the following claims.
[0112] The electrode of the present invention is suitably used as an electrode (working electrode) for electrochemical measurements.
[0113] REFERENCE SIGNS LIST 1 Electrode 2 Base film 3 First underlayer 4 Second underlayer 5 Conductive carbon layer
Claims
1. An electrode comprising, in order toward one side in a thickness direction, a base film, a first underlayer, a second underlayer, and a conductive carbon layer, wherein the first underlayer is a metal layer or a semi-metal layer, the second underlayer is a metal layer, and the resistivity of the first underlayer is 10 times or more the resistivity of the second underlayer.
2. The conductive carbon layer is sp 2 Bonds and sp 3 The electrode of claim 1 having a bond.
3. The electrode of claim 1, wherein said second underlayer comprises titanium or niobium.
4. The resistivity of the second underlayer is 3.0×10 -4 2. The electrode of claim 1, having a resistivity of less than or equal to Ω·cm.
5. The electrode of claim 1, wherein the first underlayer is a semi-metal layer and comprises silicon.
6. The electrode according to claim 1, wherein the first underlayer has a thickness of 3 nm or more.
7. The electrode according to any one of claims 1 to 6, which is an electrode for electrochemical measurements.
Citation Information
Patent Citations
Electrode
WO2022019299A1
Thin film-laminated film
WO2016013478A1
Electrode film and electrochemical measurement system
WO2019117112A1
Electrode and electrode chip
WO2021192248A1
Electrode
WO2022202715A1
Cited By
Electrode and biosensor
WO2026186281A1