Method for producing semiconductor substrate and composition for forming resist underlayer film

A polymer-based resist underlayer film composition with halogen atoms addresses the challenges of solvent resistance and pattern rectangularity in semiconductor manufacturing, enhancing the efficiency of semiconductor substrate production.

WO2024203160A1PCT designated stage expired Publication Date: 2024-10-03JSR CORPORATION

Patent Information

Application Number
PCT/JP2024/009011
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-08
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

In the manufacturing of semiconductor devices, existing resist underlayer films struggle to provide sufficient solvent resistance and pattern rectangularity, especially with the trend towards shorter exposure wavelengths, leading to issues with pattern skirting and rectangularity in highly integrated semiconductor substrates.

Method used

A composition comprising a polymer with a specific repeating unit and a solvent is used to form a resist underlayer film, which includes halogen atoms for enhanced secondary electron generation and crosslinking, promoting solvent resistance and pattern rectangularity when exposed to extreme ultraviolet rays.

Benefits of technology

The solution effectively forms a resist underlayer film with excellent solvent resistance and pattern rectangularity, enabling efficient manufacturing of semiconductor substrates with improved pattern shape and rectangularity, suitable for advanced semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009011_03102024_PF_FP_ABST
    Figure JP2024009011_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides: a composition for forming a resist underlayer film, the composition being capable of forming a resist underlayer film that is excellent in terms of solvent resistance and pattern rectangularity; and a method for producing a semiconductor substrate. This composition for forming a resist underlayer film contains a polymer that has a repeating unit represented by formula (1), and a solvent. (In formula (1), R1 represents a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. L1 represents a single bond or a divalent linking group. Ar1 represents a monovalent group having an aromatic ring having 6 to 20 ring members. The hydrogen atom of the aromatic ring is substituted by at least one halogen atom. Ar1 has at least one group that is selected from the group consisting of groups represented by formulae (2-1) to (2-8).) (In formulae (2-1) to (2-8), * represents a bond with an atom constituting Ar1, and R7 represents a divalent organic group having 1 to 20 carbon atoms, or a single bond. In formula (2-1) and formula (2-7), R8, R9 and R10 each independently represent a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. In formula (2-2), ** represents a bond with an atom constituting Cy. Cy represents a ring structure constituted together with two carbon atoms in the formula and having 3 to 20 ring members. R11 represents a hydrogen atom, a monovalent organic group having 1 to 20 carbon atoms, or a bond with **. R12 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. In formula (2-3), R13 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.)
Need to check novelty before this filing date? Find Prior Art

Description

Semiconductor substrate manufacturing method and composition for forming resist underlayer film

[0001] The present invention relates to a method for producing a semiconductor substrate and a composition for forming a resist underlayer film.

[0002] In the manufacture of semiconductor devices, for example, a multilayer resist process is used in which a resist pattern is formed by exposing and developing a resist film laminated on a substrate via a resist underlayer film such as an organic underlayer film or a silicon-containing film. In this process, the resist underlayer film is etched using the resist pattern as a mask, and the substrate is further etched using the resulting resist underlayer film pattern as a mask, thereby forming a desired pattern on the semiconductor substrate.

[0003] In recent years, semiconductor devices have become increasingly highly integrated, and the wavelength of the exposure light used has tended to be shortened from KrF excimer lasers (248 nm) and ArF excimer lasers (193 nm) to extreme ultraviolet light (13.5 nm, hereinafter also referred to as "EUV"). Various studies have been conducted on compositions for forming resist underlayer films (see International Publication No. 2013 / 141015).

[0004] International Publication No. 2013 / 141015

[0005] The resist underlayer film is required to have solvent resistance to the solvent in the resist composition, and pattern rectangularity that prevents pattern footing at the bottom of the resist film and ensures rectangularity of the resist pattern.

[0006] The present invention has been made in light of the above circumstances, and an object of the present invention is to provide a composition for forming a resist underlayer film, which is capable of forming a resist underlayer film that is excellent in solvent resistance and pattern rectangularity, and a method for producing a semiconductor substrate.

[0007] In one embodiment, the present invention relates to a composition for forming a resist underlayer film, comprising: a polymer having a repeating unit represented by the following formula (1) (hereinafter also referred to as “polymer [A]”); and a solvent (hereinafter also referred to as “solvent [B]”). (In formula (1), R 1is a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. 1 is a single bond or a divalent linking group. 1 is a monovalent group having an aromatic ring with 6 to 20 ring members. The aromatic ring is substituted with at least one halogen atom. 1 has at least one group (hereinafter also referred to as "specific group") selected from the group consisting of a group represented by the following formula (2-1), a group represented by the following formula (2-2), a group represented by the following formula (2-3), a group represented by the following formula (2-4), a group represented by the following formula (2-5), a group represented by the following formula (2-6), a group represented by the following formula (2-7), and a group represented by the following formula (2-8). (In formulas (2-1) to (2-8), * represents Ar 1 is a bond to the atom constituting R 7 is a divalent organic group having 1 to 20 carbon atoms or a single bond. 8 , R 9 and R 10 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. In formula (2-2), ** is a bond to an atom constituting Cy. Cy is a ring structure having 3 to 20 ring members formed together with the two carbon atoms in the formula. R 11 is a hydrogen atom, a monovalent organic group having 1 to 20 carbon atoms, or a bond to **. 12 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 13 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.

[0008] In another embodiment, the present invention relates to a method for producing a semiconductor substrate, comprising: a step of applying a composition for forming a resist underlayer film directly or indirectly to a substrate; a step of applying a composition for forming a resist film to the resist underlayer film formed in the step of applying the composition for forming a resist film; a step of exposing the resist film formed in the step of applying the composition for forming a resist film to radiation; and a step of developing at least the exposed resist film, wherein the composition for forming a resist underlayer film contains: a polymer having a repeating unit represented by the following formula (1); and a solvent. (In formula (1), R 1 is a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. 1 is a single bond or a divalent linking group. 1 is a monovalent group having an aromatic ring with 6 to 20 ring members. The aromatic ring is substituted with at least one halogen atom. 1 has at least one group selected from the group consisting of a group represented by the following formula (2-1), a group represented by the following formula (2-2), a group represented by the following formula (2-3), a group represented by the following formula (2-4), a group represented by the following formula (2-5), a group represented by the following formula (2-6), a group represented by the following formula (2-7), and a group represented by the following formula (2-8). (In formulas (2-1) to (2-8), * represents Ar 1 is a bond to the atom constituting R 7 is a divalent organic group having 1 to 20 carbon atoms or a single bond. 8 , R 9 and R 10 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. In formula (2-2), ** is a bond to an atom constituting Cy. Cy is a ring structure having 3 to 20 ring members formed together with the two carbon atoms in the formula. R 11 is a hydrogen atom, a monovalent organic group having 1 to 20 carbon atoms, or a bond to **. 12 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 13is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.

[0009] The composition for forming a resist underlayer film can form a film having excellent solvent resistance and pattern rectangularity. The method for producing a semiconductor substrate uses a composition for forming a resist underlayer film that can form a resist underlayer film having excellent solvent resistance and pattern rectangularity, so that a semiconductor substrate can be produced efficiently. Therefore, these compositions can be suitably used in the production of semiconductor devices, etc.

[0010] The composition for forming a resist underlayer film and the method for producing a semiconductor substrate according to each embodiment of the present invention will be described in detail below. Combinations of preferred aspects in the embodiments are also preferred.

[0011] <<Composition for forming a resist underlayer film>> The composition for forming a resist underlayer film (hereinafter also referred to as the “composition”) contains a polymer (A) and a solvent (B). The composition may contain optional components as long as the effects of the present invention are not impaired.

[0012] This composition is suitable as a composition for forming an underlayer film of a resist film to be exposed to extreme ultraviolet radiation. Examples of resist film-forming compositions include positive- or negative-type chemically amplified resist compositions containing a radiation-sensitive acid generator, positive-type resist compositions containing an alkali-soluble resin and a quinone diazide photosensitizer, negative-type resist compositions containing an alkali-soluble resin and a crosslinker, and metal-containing resist compositions containing metals such as tin, zirconium, and hafnium. The underlayer film formed using this composition contains halogen atoms derived from the polymer [A], thereby increasing the efficiency of secondary electron generation due to absorption of extreme ultraviolet radiation. As a result, upon exposure to extreme ultraviolet radiation, a sufficient difference in solubility occurs in the interface region of the organic resist film on the underlayer film side, and the insolubilization of the metal-containing resist film is promoted, thereby suppressing pattern tailing at the bottom of the resist film and ensuring rectangularity of the resist pattern. Furthermore, since the polymer [A] contains specific groups, a crosslinked structure is formed in the resulting resist underlayer film, reducing its solubility in organic solvents. The lower limit of the content of the metal or metal compound in the components other than the solvent in the metal-containing resist composition is preferably 50 mass %, more preferably 70 mass %, even more preferably 80 mass %, and particularly preferably 85 mass %. The upper limit of the content is, for example, 100 mass % or 95 mass %.

[0013] Each component contained in the composition will be described below.

[0014] <Polymer [A]> The polymer [A] has a repeating unit represented by the following formula (1) (hereinafter also referred to as "repeating unit (1)"). The polymer [A] can contain one or two or more types of repeating unit (1). The polymer [A] may have a repeating unit other than the repeating unit (1). The composition can contain one or two or more types of polymer [A]. (In formula (1), R 1 is a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. 1 is a single bond or a divalent linking group. 1is a monovalent group having an aromatic ring with 6 to 20 ring members. The aromatic ring is substituted with at least one halogen atom. 1 has at least one group selected from the group consisting of a group represented by the following formula (2-1), a group represented by the following formula (2-2), a group represented by the following formula (2-3), a group represented by the following formula (2-4), a group represented by the following formula (2-5), a group represented by the following formula (2-6), a group represented by the following formula (2-7), and a group represented by the following formula (2-8). (In formulas (2-1) to (2-8), * represents Ar 1 is a bond to the atom constituting R 7 is a divalent organic group having 1 to 20 carbon atoms or a single bond. 8 , R 9 and R 10 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. In formula (2-2), ** is a bond to an atom constituting Cy. Cy is a ring structure having 3 to 20 ring members formed together with the two carbon atoms in the formula. R 11 is a hydrogen atom, a monovalent organic group having 1 to 20 carbon atoms, or a bond to **. 12 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 13 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.

[0015] In the above formula (1), R 1 The monovalent hydrocarbon group having 1 to 20 carbon atoms represented by the formula (I) is not particularly limited, and examples thereof include a monovalent chain hydrocarbon group having 1 to 20 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms, and combinations thereof.

[0016] Examples of the monovalent chain hydrocarbon group having 1 to 20 carbon atoms include alkyl groups such as methyl, ethyl, n-propyl, i-propyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, and neopentyl; alkenyl groups such as ethenyl, propenyl, and butenyl; and alkynyl groups such as ethynyl, propynyl, and butynyl.

[0017] Examples of the monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms include cycloalkyl groups such as a cyclopentyl group and a cyclohexyl group; cycloalkenyl groups such as a cyclopropenyl group, a cyclopentenyl group and a cyclohexenyl group; bridged ring saturated hydrocarbon groups such as a norbornyl group, an adamantyl group and a tricyclodecyl group; and bridged ring unsaturated hydrocarbon groups such as a norbornenyl group and a tricyclodecenyl group.

[0018] Examples of the monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms include a phenyl group, a tolyl group, a naphthyl group, an anthracenyl group, a pyrenyl group, a fluorenyl group, and a 9-methylidenefluorenyl group.

[0019] R 1 When has a substituent, examples of the substituent include a monovalent chain hydrocarbon group having 1 to 10 carbon atoms, a halogen atom such as a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom, an alkoxy group such as a methoxy group, an ethoxy group, or a propoxy group, an alkoxycarbonyl group such as a methoxycarbonyl group or an ethoxycarbonyl group, an alkoxycarbonyloxy group such as a methoxycarbonyloxy group or an ethoxycarbonyloxy group, an acyl group such as a formyl group, an acetyl group, a propionyl group, or a butyryl group, a cyano group, and a nitro group.

[0020] Among them, R 1 In terms of copolymerizability of the monomer that gives the repeating unit (1), a hydrogen atom or a methyl group is preferred.

[0021] In the above formula (1), L 1 Examples of the divalent linking group represented by the formula (I) include a divalent hydrocarbon group having 1 to 20 carbon atoms, a divalent heteroatom-containing group, a group having the divalent heteroatom-containing group between carbon atoms in the divalent hydrocarbon group having 1 to 20 carbon atoms, a group in which some or all of the hydrogen atoms in the hydrocarbon group have been substituted with monovalent heteroatom-containing groups, and combinations thereof.

[0022] The divalent hydrocarbon group having 1 to 20 carbon atoms includes the above-mentioned R 1A group in which one hydrogen atom has been removed from a monovalent hydrocarbon group having 1 to 20 carbon atoms, represented by the following formula (I) can be suitably used, and a group in which one hydrogen atom has been removed from a phenyl group or a group in which one hydrogen atom has been removed from a 9-methylidenefluorenyl group is preferred.

[0023] Examples of heteroatoms constituting the divalent or monovalent heteroatom-containing group include oxygen atoms, nitrogen atoms, sulfur atoms, phosphorus atoms, silicon atoms, halogen atoms, etc. Examples of halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms.

[0024] Examples of the divalent heteroatom-containing group include —CO—, —CS—, —NR′—, —O—, —S—, and —SO 2 - or a group combining these. R' is a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms. Preferred divalent hetero atom-containing groups are -CO-O-, -CO-NH-, and -O-.

[0025] Examples of the monovalent heteroatom-containing group include a hydroxy group, a sulfanyl group, a cyano group, a nitro group, a carboxy group, an amino group, and a halogen atom.

[0026] In the above formula (1), Ar 1 Examples of the aromatic ring having 6 to 20 ring members in Ar include aromatic hydrocarbon rings such as a benzene ring, a naphthalene ring, an anthracene ring, an indene ring, and a pyrene ring, aromatic heterocyclic rings such as a pyridine ring, a pyrazine ring, a pyrimidine ring, a pyridazine ring, and a triazine ring, and combinations thereof. 1 The aromatic ring is preferably a benzene ring, a naphthalene ring, an anthracene ring or a pyrene ring, more preferably a benzene ring or a naphthalene ring, and even more preferably a benzene ring.

[0027] The aromatic ring is substituted with at least one halogen atom. Preferably, the aromatic ring is substituted with at least two halogen atoms. In this case, the multiple halogen atoms may be the same or different. Examples of halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms. Preferably, the halogen atom is an iodine atom.

[0028] In the above formulas (2-1) to (2-8), R 7 The divalent organic group having 1 to 20 carbon atoms represented by the formula (1) is L 1 A divalent linking group represented by the following formula can be preferably used.

[0029] R 7 As the alkyl group, a combination of a divalent hydrocarbon group having 1 to 10 carbon atoms and a divalent heteroatom-containing group is preferred, and a combination of a methanediyl group, an ethanediyl group, a propanediyl group, a benzenediyl group, or a combination thereof with —O—, —CO—, or a combination thereof is more preferred.

[0030] In the above formulas (2-1) to (2-3) and (2-7), R 8 , R 9 , R 10 , R 11 , R 12 and R 13 (Hereinafter referred to as “R 8 ~R 13 "). Examples of the monovalent organic group having 1 to 20 carbon atoms and represented by the formula (I) include a monovalent hydrocarbon group having 1 to 20 carbon atoms, a group having a divalent heteroatom-containing group between carbon atoms of the hydrocarbon group or at the end of the hydrocarbon group, a group in which some or all of the hydrogen atoms of the hydrocarbon group have been substituted with a monovalent heteroatom-containing group, or a combination thereof. The "organic group" is a group having at least one carbon atom.

[0031] R 8 ~R 13 The monovalent hydrocarbon group having 1 to 20 carbon atoms in the formula (1) is R 1 A monovalent hydrocarbon group having 1 to 20 carbon atoms and represented by the following formula can be suitably used.

[0032] R 8 ~R 13 The divalent heteroatom-containing group and the monovalent heteroatom-containing group in the formula (1) are 1 A divalent heteroatom-containing group and a monovalent heteroatom-containing group in the above formula can be suitably employed.

[0033] R 8 ~R13 are preferably all hydrogen atoms.

[0034] In the formula (2-2), examples of the ring structure having 3 to 20 ring members formed together with the two carbon atoms in the formula represented by Cy include R 1 Preferably, Cy is a cycloalkane ring having 5 to 10 carbon atoms, more preferably a cyclopentane ring, a cyclohexane ring, or a cycloheptane ring.

[0035] Specific examples of the group represented by the above formula (2-1) include structures represented by the following formulas (2-1-1) to (2-1-10).

[0036] Specific examples of the group represented by the above formula (2-2) include structures represented by the following formulas (2-2-1) to (2-2-6).

[0037] Specific examples of the group represented by the above formula (2-3) include structures represented by the following formulas (2-3-1) to (2-3-6).

[0038] Specific examples of the group represented by the above formula (2-4) include structures represented by the following formulas (2-4-1) to (2-4-6).

[0039] Specific examples of the group represented by the above formula (2-5) include structures represented by the following formulas (2-5-1) to (2-5-6).

[0040] Specific examples of the group represented by the above formula (2-6) include structures represented by the following formulas (2-6-1) to (2-6-3).

[0041] Specific examples of the group represented by the above formula (2-7) include structures represented by the following formulas (2-7-1) to (2-7-2).

[0042] Specific examples of the group represented by the above formula (2-8) include structures represented by the following formulas (2-8-1) to (2-8-2).

[0043] Specific examples of the repeating unit (1) include repeating units represented by the following formulas (1-1) to (1-15).

[0044]

[0045]

[0046] In the above formulas (1-1) to (1-15), R 1 is synonymous with the above formula (1).

[0047] The lower limit of the content of repeating unit (1) in all repeating units constituting polymer [A] (the total content when multiple types are present) is preferably 10 mol%, more preferably 30 mol%, and even more preferably 75 mol%. The upper limit of the content may be 100 mol%, i.e., polymer [A] may be a homopolymer of repeating unit (1). When polymer [A] is a copolymer, the upper limit of the content of repeating unit (1) may be 99 mol% or 95 mol%.

[0048] The polymer [A] may further have a repeating unit represented by the following formula (3) (excluding the case of the above formula (1)) (hereinafter also referred to as "repeating unit (2)"). The polymer [A] may have one or more types of repeating unit (2).

[0049] In the above formula (3), R 31 is a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. 31 is a single bond or a divalent linking group. 41 is a monovalent organic group having 1 to 20 carbon atoms.

[0050] R 31 The monovalent hydrocarbon group having 1 to 20 carbon atoms represented by the formula (1) is 1A monovalent hydrocarbon group having 1 to 20 carbon atoms represented by the following formula can be preferably used. 31 When R has a substituent, R in the above formula (1) 1 The substituents that may be possessed by the group may be suitably employed.

[0051] L 31 The divalent linking group represented by the formula (1) L 1 A divalent linking group represented by the following formula can be preferably used. 31 is preferably a single bond.

[0052] R 41 The monovalent organic group having 1 to 20 carbon atoms represented by the formula (2-1), (2-2) and (2-3) above includes R 8 ~R 13 A monovalent organic group having 1 to 20 carbon atoms and represented by the following formula can be preferably used. A substituted or unsubstituted monovalent heterocyclic group is also suitable as this monovalent organic group.

[0053] Examples of the heterocyclic group include a group in which one hydrogen atom has been removed from an aromatic heterocyclic structure and a group in which one hydrogen atom has been removed from an aliphatic heterocyclic structure. Five-membered aromatic structures that have aromaticity due to the introduction of heteroatoms are also included in the heterocyclic structure. Examples of heteroatoms include oxygen atoms, nitrogen atoms, and sulfur atoms.

[0054] Examples of the aromatic heterocyclic structure include: oxygen atom-containing aromatic heterocyclic structures such as furan, pyran, benzofuran, and benzopyran; nitrogen atom-containing aromatic heterocyclic structures such as pyrrole, imidazole, pyridine, pyrimidine, pyrazine, indole, quinoline, isoquinoline, acridine, phenazine, and carbazole; sulfur atom-containing aromatic heterocyclic structures such as thiophene; and aromatic heterocyclic structures containing multiple heteroatoms such as thiazole, benzothiazole, thiazine, and oxazine.

[0055] Examples of the aliphatic heterocyclic structure include oxygen atom-containing aliphatic heterocyclic structures such as oxirane, oxetane, tetrahydrofuran, tetrahydropyran, dioxolane, and dioxane; nitrogen atom-containing aliphatic heterocyclic structures such as aziridine, pyrrolidine, pyrazolidine, piperidine, and piperazine; sulfur atom-containing aliphatic heterocyclic structures such as thietane, thiolane, and thiane; aliphatic heterocyclic structures containing multiple heteroatoms such as oxazoline, morpholine, oxathiolane, oxazine, and thiomorpholine; and structures in which an aliphatic heterocyclic structure and an aromatic ring structure are combined, such as benzoxazine.

[0056] The cyclic structure also includes a lactone structure, a cyclic carbonate structure, a sultone structure, and a structure containing a cyclic acetal.

[0057] Specific examples of the repeating unit (2) include repeating units represented by the following formulas (3-1) to (3-20).

[0058]

[0059]

[0060] In the above formulas (3-1) to (3-20), R 31 is the same as the above formula (3).

[0061] When the polymer [A] contains the repeating unit (2), the content of the repeating unit (2) in all repeating units constituting the polymer [A] (when a plurality of repeating units are present, the total content) is preferably 5 mol %, more preferably 10 mol %, and even more preferably 15 mol %. The upper limit of the content is preferably 90 mol %, more preferably 85 mol %, and even more preferably 80 mol %.

[0062] The polymer [A] may contain, as other repeating units, repeating units containing a sulfonate ester structure, repeating units derived from maleic acid, maleic anhydride, maleimide derivatives, etc., or repeating units containing a structure that generates acid upon exposure, such as a sulfonimide salt structure, a sulfonamide salt structure, or an imide salt structure. When the polymer [A] contains other repeating units, the lower limit of the content of the other repeating units (the total content when multiple types are present) relative to all repeating units constituting the polymer [A] is preferably 1 mol%, more preferably 5 mol%, and even more preferably 10 mol%. The upper limit of the content is preferably 90 mol%, more preferably 85 mol%, and even more preferably 80 mol%.

[0063] The lower limit of the weight-average molecular weight of the polymer (A) is preferably 1,000, more preferably 1,500, even more preferably 2,000, and particularly preferably 2,500. The upper limit of the molecular weight is preferably 10,000, more preferably 8,000, even more preferably 6,000, and particularly preferably 5,000. The method for measuring the weight-average molecular weight is as described in the Examples.

[0064] The lower limit of the content of the polymer [A] in the composition for forming a resist underlayer film is preferably 0.05 mass %, more preferably 0.1 mass %, even more preferably 0.15 mass %, and particularly preferably 0.2 mass %, based on the total mass of the polymer [A] and the solvent [B]. The upper limit of the content is preferably 1 mass %, more preferably 0.8 mass %, even more preferably 0.6 mass %, and particularly preferably 0.4 mass %, based on the total mass of the polymer [A] and the solvent [B].

[0065] The lower limit of the content of the polymer (A) in the components other than the solvent (B) in the composition for forming a resist underlayer film is preferably 10% by mass, more preferably 20% by mass, and even more preferably 30% by mass. The upper limit of the content is preferably 100% by mass, but may also be 90% by mass or 85% by mass.

[0066] [Method for Synthesizing Polymer [A]] The polymer [A] can be synthesized by radical polymerization, ionic polymerization, polycondensation, polyaddition, addition condensation, etc., depending on the type of monomer. For example, when the polymer [A] is synthesized by radical polymerization, the polymer can be synthesized by polymerizing monomers that provide each structural unit in an appropriate solvent using a radical polymerization initiator, etc.

[0067] Examples of the radical polymerization initiator include azo radical initiators such as azobisisobutyronitrile (AIBN), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2-cyclopropylpropionitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), dimethyl 2,2'-azobisisobutyrate, and dimethyl-2,2'-azobis(2-methylpropionate); and peroxide radical initiators such as benzoyl peroxide, t-butyl hydroperoxide, and cumene hydroperoxide. These radical initiators can be used alone or in combination of two or more.

[0068] As the solvent used in the polymerization, the solvent [B] described below can be suitably used. These solvents used in the polymerization may be used alone or in combination of two or more kinds.

[0069] The reaction temperature in the polymerization is usually 40° C. to 150° C., preferably 50° C. to 120° C. The reaction time is usually 1 hour to 48 hours, preferably 1 hour to 24 hours.

[0070] <Solvent (B)> The solvent (B) is not particularly limited as long as it can dissolve or disperse the polymer (A) and any optional components contained as needed.

[0071] Examples of the solvent (B) include hydrocarbon solvents, ester solvents, alcohol solvents, ketone solvents, ether solvents, nitrogen-containing solvents, water, etc. The solvent (B) can be used alone or in combination of two or more.

[0072] Examples of hydrocarbon solvents include aliphatic hydrocarbon solvents such as n-pentane, n-hexane, and cyclohexane, and aromatic hydrocarbon solvents such as benzene, toluene, and xylene.

[0073] Examples of ester-based solvents include carbonate-based solvents such as diethyl carbonate and propylene carbonate, acetate monoester-based solvents such as methyl acetate and ethyl acetate, acetate diester-based solvents such as 1,6-diacetoxyhexane, lactone-based solvents such as γ-butyrolactone, polyhydric alcohol partial ether carboxylate-based solvents such as diethylene glycol monomethyl ether acetate and propylene glycol monomethyl ether acetate, and lactate-based solvents such as methyl lactate and ethyl lactate.

[0074] Examples of alcohol solvents include monoalcohol solvents such as methanol, ethanol, n-propanol, 4-methyl-2-pentanol, and 2,2-dimethyl-1-propanol, and polyalcohol solvents such as ethylene glycol and 1,2-propylene glycol.

[0075] Examples of the ketone solvent include chain ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, and 2-heptanone, and cyclic ketone solvents such as cyclohexanone.

[0076] Examples of the ether solvent include chain ether solvents such as n-butyl ether, polyhydric alcohol ether solvents such as cyclic ether solvents such as tetrahydrofuran, and polyhydric alcohol partial ether solvents such as diethylene glycol monomethyl ether and propylene glycol monomethyl ether.

[0077] Examples of nitrogen-containing solvents include chain nitrogen-containing solvents such as N,N-dimethylacetamide, and cyclic nitrogen-containing solvents such as N-methylpyrrolidone.

[0078] The solvent (B) is preferably a ketone solvent, an ether solvent, or an ester solvent, more preferably a cyclic ketone solvent, a polyhydric alcohol partial ether solvent, or a polyhydric alcohol partial ether carboxylate solvent, and still more preferably cyclohexanone, propylene glycol monomethyl ether, or propylene glycol monomethyl ether acetate.

[0079] [Optional Components] The composition for forming a resist underlayer film may contain optional components within a range that does not impair the effects of the present invention. Examples of optional components include a crosslinking agent, an acid generator, a dehydrating agent, an acid diffusion controller, a surfactant, etc. The optional components may be used alone or in combination of two or more. The content of the optional components relative to the total mass of the polymer [A] and the optional components is preferably 30 mass% or less, and more preferably 20 mass% or less.

[0080] [Method for preparing a composition for forming a resist underlayer film] The composition for forming a resist underlayer film can be prepared by mixing the polymer [A], the solvent [B], and, if necessary, any optional components in a predetermined ratio, and preferably filtering the resulting mixture through a membrane filter or the like having a pore size of 0.5 μm or less.

[0081] <<Method for Manufacturing Semiconductor Substrate>> The method for manufacturing a semiconductor substrate includes a step of applying a composition for forming a resist underlayer film directly or indirectly to a substrate (hereinafter also referred to as a “coating step (I)”), a step of applying a composition for forming a resist film to the resist underlayer film formed in the above-mentioned coating step of the composition for forming a resist film (hereinafter also referred to as a “coating step (II)”), a step of exposing the resist film formed in the above-mentioned coating step of the composition for forming a resist film to radiation (hereinafter also referred to as an “exposure step”), and a step of developing at least the exposed resist film (hereinafter also referred to as a “development step”).

[0082] According to the method for producing a semiconductor substrate, by using a predetermined composition for forming a resist underlayer film in the coating step (I), a resist underlayer film having excellent solvent resistance and pattern rectangularity can be formed, and therefore a semiconductor substrate having a good pattern shape can be produced.

[0083] It is preferable that the method for producing a semiconductor substrate further includes, before the coating step (II), a step of heating the resist underlayer film formed in the resist underlayer film-forming composition coating step at 200°C or higher (hereinafter also referred to as a "heating step").

[0084] The method for producing a semiconductor substrate may further include, as necessary, a step of forming a silicon-containing film directly or indirectly on the substrate (hereinafter also referred to as a "silicon-containing film-forming step") prior to the coating step (I).

[0085] Hereinafter, each step in the case where the heating step, which is a preferred step, and the silicon-containing film forming step, which is an optional step, are included will be described.

[0086] [Silicon-containing film forming step] In this step, which is carried out before the coating step (I), a silicon-containing film is formed directly or indirectly on a substrate.

[0087] Examples of the substrate include metal or semimetal substrates such as silicon substrates, aluminum substrates, nickel substrates, chromium substrates, molybdenum substrates, tungsten substrates, copper substrates, tantalum substrates, and titanium substrates, among which silicon substrates are preferred.The substrate may also be a substrate on which a silicon nitride film, an alumina film, a silicon dioxide film, a tantalum nitride film, a titanium nitride film, or the like is formed.

[0088] The silicon-containing film can be formed by coating a silicon-containing film-forming composition, chemical vapor deposition (CVD), atomic layer deposition (ALD), or the like. Examples of methods for forming a silicon-containing film by coating a silicon-containing film-forming composition include a method in which the silicon-containing film-forming composition is directly or indirectly applied to a substrate, and the resulting coating film is then cured by exposure and / or heating. Examples of commercially available silicon-containing film-forming compositions include "NFC SOG01," "NFC SOG04," and "NFC SOG080" (all from JSR Corporation). Silicon oxide films, silicon nitride films, silicon oxynitride films, and amorphous silicon films can be formed by chemical vapor deposition (CVD) or atomic layer deposition (ALD).

[0089] Examples of radiation used for the exposure include electromagnetic waves such as visible light, ultraviolet light, far ultraviolet light, X-rays and gamma rays, and particle beams such as electron beams, molecular beams and ion beams.

[0090] The lower limit of the temperature when heating the coating film is preferably 90° C., more preferably 150° C., and still more preferably 200° C. The upper limit of the temperature is preferably 550° C., more preferably 450° C., and still more preferably 300° C.

[0091] The lower limit of the average thickness of the silicon-containing film is preferably 1 nm, more preferably 10 nm, and even more preferably 15 nm. The upper limit is preferably 20,000 nm, more preferably 1,000 nm, and even more preferably 100 nm. The average thickness of the silicon-containing film can be measured in the same manner as the average thickness of the resist underlayer film.

[0092] Examples of cases in which a silicon-containing film is formed indirectly on a substrate include cases in which a silicon-containing film is formed on a low dielectric insulating film or an organic underlayer film formed on a substrate.

[0093] [Coating step (I)] In this step, the resist underlayer film-forming composition is coated on the silicon-containing film formed on the substrate.The coating method of the resist underlayer film-forming composition is not particularly limited, and can be carried out by any suitable method such as spin coating, casting coating, roll coating, etc.This forms a coating film, and the resist underlayer film is formed by the evaporation of the solvent [B].

[0094] The lower limit of the average thickness of the resist underlayer film formed is preferably 0.5 nm, more preferably 1 nm, and even more preferably 2 nm. The upper limit of the average thickness is preferably 50 nm, more preferably 20 nm, even more preferably 10 nm, and particularly preferably 7 nm. The average thickness is measured according to the method described in the Examples.

[0095] When the composition for forming a resist underlayer film is applied directly to the substrate, the silicon-containing film forming step may be omitted.

[0096] [Heating Step] Next, the resist underlayer film formed in the coating step (I) is heated. Heating the resist underlayer film promotes the formation of a crosslinked structure by the specific group in the polymer (A). This step is carried out before the coating step (II).

[0097] The coating film may be heated in an air atmosphere or a nitrogen atmosphere. The lower limit of the heating temperature is 180°C, but is preferably 200°C, more preferably 210°C, and even more preferably 220°C. The upper limit of the heating temperature is preferably 400°C, more preferably 350°C, and even more preferably 280°C. The lower limit of the heating time is preferably 15 seconds, more preferably 30 seconds. The upper limit of the time is preferably 800 seconds, more preferably 400 seconds, and even more preferably 200 seconds.

[0098] [Coating Step (II)] In this step, a resist film-forming composition is coated onto the resist underlayer film formed in the resist underlayer film-forming composition coating step. The method for coating the resist film-forming composition is not particularly limited, and examples thereof include a rotary coating method.

[0099] To explain this step in more detail, for example, a resist composition is applied so that the resist film to be formed has a predetermined thickness, and then the applied resist film is pre-baked (hereinafter also referred to as "PB") to volatilize the solvent in the applied film, thereby forming the resist film.

[0100] The PB temperature and PB time can be appropriately determined depending on the type of the resist film-forming composition used, etc. The lower limit of the PB temperature is preferably 30°C, more preferably 50°C. The upper limit of the PB temperature is preferably 200°C, more preferably 150°C. The lower limit of the PB time is preferably 10 seconds, more preferably 30 seconds. The upper limit of the PB time is preferably 600 seconds, more preferably 300 seconds.

[0101] The resist film-forming composition used in this step is preferably a composition that is subjected to exposure to extreme ultraviolet rays, and examples thereof include positive or negative chemically amplified resist compositions that contain a radiation-sensitive acid generator, and metal-containing resist compositions that contain a metal such as tin, zirconium, or hafnium.

[0102] [Exposure Step] In this step, the resist film formed in the resist film-forming composition application step is exposed to radiation. This step causes a difference in solubility between the exposed and unexposed areas of the resist film in a basic liquid developer or an organic solvent. More specifically, the solubility of the exposed areas of the resist film in a basic liquid increases, or the solubility of the exposed areas in an organic solvent decreases.

[0103] The radiation used for exposure can be appropriately selected depending on the type of the resist film-forming composition used, etc. Examples include visible light, ultraviolet light, far ultraviolet light, electromagnetic waves such as X-rays and gamma rays, and particle beams such as electron beams, molecular beams, and ion beams. Among these, far ultraviolet light is preferred, and KrF excimer laser light (wavelength 248 nm), ArF excimer laser light (wavelength 193 nm), F 2 Excimer laser light (wavelength 157 nm), Kr 2 Excimer laser light (wavelength 147 nm), ArKr excimer laser light (wavelength 134 nm), or extreme ultraviolet light (wavelength 13.5 nm, etc., also referred to as "EUV") is more preferred, and ArF excimer laser light or EUV is even more preferred. The exposure conditions can be appropriately determined depending on the type of resist film-forming composition used, etc.

[0104] Furthermore, in this process, after the exposure, post-exposure baking (hereinafter also referred to as "PEB") can be performed to improve the performance of the resist film, such as resolution, pattern profile, and developability. The PEB temperature and PEB time can be appropriately determined depending on the type of resist film-forming composition used, etc. The lower limit of the PEB temperature is preferably 50°C, more preferably 70°C. The upper limit of the PEB temperature is preferably 200°C, more preferably 150°C. The lower limit of the PEB time is preferably 10 seconds, more preferably 30 seconds. The upper limit of the PEB time is preferably 600 seconds, more preferably 300 seconds.

[0105] [Development Step] In this step, the exposed resist film is developed. At this time, a part of the resist underlayer film may also be developed. Examples of the developer used in this development include an alkaline aqueous solution (alkaline developer), a liquid containing an organic solvent (organic solvent developer), etc.

[0106] The basic liquid for alkaline development is not particularly limited, and known basic liquids can be used. Examples of basic liquids for alkaline development include aqueous alkaline solutions containing at least one alkaline compound dissolved therein, such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, aqueous ammonia, ethylamine, n-propylamine, diethylamine, di-n-propylamine, triethylamine, methyldiethylamine, ethyldimethylamine, triethanolamine, tetramethylammonium hydroxide (TMAH), pyrrole, piperidine, choline, 1,8-diazabicyclo-[5.4.0]-7-undecene, and 1,5-diazabicyclo-[4.3.0]-5-nonene. Among these, aqueous TMAH solutions are preferred, and 2.38% by mass aqueous TMAH solutions are more preferred.

[0107] Examples of organic solvent developers for use in organic solvent development include those exemplified above as the solvent [B]. As the organic solvent developer, an ester solvent, an ether solvent, an alcohol solvent, a ketone solvent, and / or a hydrocarbon solvent is preferred, a ketone solvent is more preferred, and 2-heptanone is particularly preferred.

[0108] In this step, washing and / or drying may be carried out after the development.

[0109] [Etching Step] In this step, etching is performed using the resist pattern (and resist underlayer film pattern) as a mask. The etching may be performed once or multiple times, i.e., etching may be performed sequentially using the pattern obtained by etching as a mask. From the viewpoint of obtaining a pattern with a better shape, multiple times is preferred. When etching is performed multiple times, for example, etching is performed sequentially in the order of the silicon-containing film and the substrate. Examples of etching methods include dry etching and wet etching. From the viewpoint of obtaining a better pattern shape on the substrate, dry etching is preferred. For this dry etching, for example, a gas plasma such as oxygen plasma is used. By the above etching, a semiconductor substrate having a predetermined pattern is obtained.

[0110] Dry etching can be performed using, for example, a known dry etching apparatus. The etching gas used for dry etching can be appropriately selected depending on the mask pattern, the elemental composition of the film to be etched, etc., and can be, for example, CHF 3 , C.F. 4 , C 2 F 6 , C 3 F 8 , SF 6 Fluorine-based gases such as Cl 2 , BCl 3 Chlorine gases such as O 2 , O 3 , H 2 Oxygen-based gases such as O, H 2 , N.H. 3 , CO, CO 2 , C.H. 4 , C2 H 2 , C 2 H 4 , C 2 H 6 , C 3 H 4 , C 3 H 6 , C 3 H 8 , HF, HI, HBr, HCl, NO, BCl 3 reducing gases such as He, N 2 and inert gases such as Ar. These gases may be used in combination. When etching a substrate using the pattern of the resist underlayer film as a mask, a fluorine-based gas is usually used.

[0111] After the substrate pattern is formed, if the silicon-containing film remains on the substrate, the silicon-containing film can be removed by carrying out a removal step.

[0112] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples.

[0113] [Weight-average molecular weight (Mw), number-average molecular weight (Mn), polydispersity index (PDI: Mw / Mn)] The Mw and Mn of the polymer were measured by gel permeation chromatography (detector: differential refractometer) using Tosoh Corporation's GPC columns (two "G2000HXL" columns and one "G3000HXL" column) under the following analytical conditions: flow rate: 1.0 mL / min, elution solvent: tetrahydrofuran, column temperature: 40°C, with monodisperse polystyrene as the standard. The PDI was calculated from the determined Mw and Mn.

[0114] [Average Film Thickness] The average film thickness was determined by measuring the film thickness at 9 arbitrary positions at 5 cm intervals, including the center of the resist underlayer film formed on a silicon wafer (substrate), using a spectroscopic ellipsometer (J.A. WOOLLAM's "M2000D"), and calculating the average of these film thicknesses.

[0115] <Synthesis of Polymer [A]> Each polymer [A] was synthesized according to the procedure shown below. In the formulas shown in the synthesis examples below, the number attached to each repeating unit indicates the content (mol %) of that repeating unit. When no number is attached to a repeating unit, the content of that repeating unit is 100 mol %. The composition ratio is 13 This was confirmed by C-NMR.

[0116]

[0117]

[0118]

[0119]

[0120]

[0121]

[0122]

[0123]

[0124] <Synthesis of Monomers> The following compounds (a-1) to (a-56) were used as monomers in the synthesis of polymer (A).

[0125]

[0126]

[0127]

[0128]

[0129] As raw materials for synthesizing the above monomers, the following compounds (c-1) to (c-14) and the following compounds (d-1) to (d-21) were used.

[0130]

[0131]

[0132] d-1: Epichlorohydrin d-2: 3,4-Epoxycyclohexylmethanol d-3: 3-Oxetanemethanol d-4: Propargyl bromide d-5: 4-Ethynylbenzoyl chloride d-6: Propargyl alcohol d-7: Propiolic acid d-8: Ultrapure water d-9: 2-(chloromethyl)-1,2-epoxypropane d-10: 4-Chloromethyl-1,3-dioxiran-2-one d-11: (2-chloroethoxy)ethene d-12: 4-Chloromethylbenzocyclobutene

[0133]

[0134] Synthesis Example 1-1 (Synthesis of Compound (a-1)) 100 mL of dimethylformamide, 10 g of compound (c-1) (3,5-diiodo-4-hydroxystyrene), and 3.71 g of potassium carbonate were placed in a reaction vessel and stirred at room temperature for 5 minutes. 3.73 g of compound (d-1) (epichlorohydrin) and 0.45 g of potassium iodide were added, and the mixture was stirred at 70°C for 5 hours. 200 mL of ethyl acetate and 200 mL of water were added, followed by washing with water three times. The organic layer was concentrated to obtain compound (a-1) as a white solid.

[0135] Synthesis Example 1-2 (Synthesis of Compound (a-2)) 100 mL of tetrahydrofuran, 10 g of Compound (c-1), 4.48 g of Compound (d-2) (3,4-epoxycyclohexylmethanol), 9.17 g of triphenylphosphine, and 6.09 g of diethyl diazodicarboxylate were placed in a reaction vessel and stirred at room temperature for 4 hours. 200 mL of a 5% aqueous oxalic acid solution and 200 mL of ethyl acetate were added, and the aqueous layer was removed. 200 mL of water was added to the organic layer, and the mixture was washed three times with water. The organic layer was concentrated to obtain Compound (a-2) as a white solid.

[0136] Synthesis Example 1-3 (Synthesis of Compound (a-3)) 100 mL of tetrahydrofuran, 10 g of Compound (c-1), 3.08 g of Compound (d-3) (3-oxetanemethanol), 9.17 g of triphenylphosphine, and 6.09 g of diethyl diazodicarboxylate were added to a reaction vessel and stirred at room temperature for 4 hours. 200 mL of a 5% aqueous oxalic acid solution and 200 mL of ethyl acetate were added, and the aqueous layer was removed. 200 mL of water was added to the organic layer, and the mixture was washed three times with water. The organic layer was concentrated to obtain Compound (a-3) as a white solid.

[0137] Synthesis Example 1-4 Synthesis of Compound (a-4) 100 mL of tetrahydrofuran, 10 g of compound (c-1), 3.84 g of compound (d-4) (propargyl bromide), 1.7 g of tetrabutylammonium bromide, and 20.0 g of a 25% aqueous solution of tetramethylammonium hydroxide were added to a reaction vessel and stirred at 60°C for 4 hours. 200 mL of a 5% aqueous solution of oxalic acid and 200 mL of ethyl acetate were added, and the aqueous layer was removed. 200 mL of water was added to the organic layer, and the mixture was washed three times with water. The organic layer was concentrated to obtain compound (a-4) as a white solid.

[0138] Synthesis Example 1-6 (Synthesis of Compound (a-6)) 100 mL of tetrahydrofuran, 10 g of Compound (c-1), 4.43 g of Compound (d-5) (4-ethynylbenzoyl chloride), 1.7 g of tetrabutylammonium bromide, and 20.0 g of a 25% aqueous solution of tetramethylammonium hydroxide were added to a reaction vessel and stirred at 60°C for 4 hours. 200 mL of a 5% aqueous solution of oxalic acid and 200 mL of ethyl acetate were added, and the aqueous layer was removed. 200 mL of water was added to the organic layer, and the mixture was washed three times with water. The organic layer was concentrated to obtain Compound (a-6) as a white solid.

[0139] Synthesis Example 1-7 Synthesis of Compound (a-7) 100 mL of tetrahydrofuran, 10 g of Compound (a-1), 1.6 g of Compound (d-6) (propargyl alcohol), and 1.3 g of potassium hydroxide were placed in a reaction vessel and stirred at 80°C for 5 hours. 200 mL of a 5% aqueous oxalic acid solution and 200 mL of ethyl acetate were added, and the aqueous layer was removed. 200 mL of water was added to the organic layer, which was then washed three times with water. The organic layer was concentrated to obtain Compound (a-7) as a white solid.

[0140] Synthesis Example 1-9 (Synthesis of Compound (a-9)) 50 mL of dimethylacetamide, 10 g of Compound (a-1), and 1.64 g of Compound (d-7) (propiolic acid) were placed in a reaction vessel and stirred at 80°C for 4 hours. 200 mL of ethyl acetate was added, and the mixture was washed with water three times. The organic layer was concentrated to obtain Compound (a-9) as a white solid.

[0141] Synthesis Example 1-10 Synthesis of Compound (a-10) 50 mL of dimethylacetamide, 20 mL of compound (d-8) (ultrapure water), and 10 g of compound (a-1) were placed in a reaction vessel and stirred at 100°C for 8 hours. 200 mL of ethyl acetate was added, and the mixture was washed with water three times. The organic layer was concentrated to obtain compound (a-10) as a white solid.

[0142] Synthesis Example 1-12 Synthesis of Compound (a-12) 100 mL of dimethylformamide, 10 g of compound (c-3) (4-hydroxy-2,6-diiodophenylacrylate), and 3.71 g of potassium carbonate were placed in a reaction vessel and stirred at room temperature for 5 minutes. 7.68 g of compound (d-9) (2-(chloromethyl)-1,2-epoxypropane) and 0.45 g of potassium iodide were added, and the mixture was stirred at 70°C for 5 hours. 200 mL of ethyl acetate and 200 mL of water were added, and the mixture was washed with water three times. The organic layer was concentrated to obtain compound (a-12) as a white solid.

[0143] Synthesis Example 1-16 Synthesis of Compound (a-16) 50 mL of dimethylacetamide, 3.28 g of compound (d-10), 10.00 g of compound (c-3), and 16.6 g of potassium carbonate were placed in a reaction vessel and stirred at 60°C for 4 hours. The reaction solution was filtered to remove insoluble matter. The organic layer was washed three times with water and then concentrated to obtain compound (a-16) as a white solid.

[0144] Synthesis Example 1-17 Synthesis of Compound (a-17) 50 mL of dimethylacetamide, 5.12 g of compound (d-11), 10.00 g of compound (c-3), 6.65 g of potassium carbonate, and 0.64 g of 18-crown-6 were placed in a reaction vessel and stirred for 4 hours at 110° C. 100 mL of ethyl acetate was added to the reaction solution, and the organic layer was washed with water three times and then concentrated to obtain compound (a-17) as a white solid.

[0145] Synthesis Example 1-18 Synthesis of Compound (a-18) 100 mL of dimethylformamide, 10 g of compound (c-3), and 3.32 g of potassium carbonate were placed in a reaction vessel and stirred at room temperature for 5 minutes. 3.70 g of compound (d-12) was added and stirred at 70°C for 5 hours. 200 mL of ethyl acetate and 200 mL of water were added, followed by washing with water three times. The organic layer was concentrated to obtain compound (a-18) as a white solid.

[0146] Synthesis Example 1-33 Synthesis of Compound (a-33) A reaction vessel was charged with 100 mL of tetrahydrofuran, 10.0 g of compound (c-6) (vinylfluorene), 22.33 g of compound (d-13), 75.9 g of a 25% aqueous solution of tetramethylammonium hydride, and 1.67 g of tetrabutylammonium bromide, and the mixture was stirred at 40°C for 5 hours. 200 mL of ethyl acetate and 200 mL of water were added, and the mixture was washed three times with water. The organic layer was concentrated to obtain compound (a-33) as a white solid.

[0147] [Synthesis Examples 1-5, 1-8, 1-11, 1-13 to 1-15, 1-19 to 1-32, 1-34 to 1-56] (Synthesis of compounds (a-5), (a-8), (a-11), (a-13) to (a-15), (a-19) to (a-32), and (a-34) to (a-56))] Compounds (a-11), (a-19), and (a-41) were synthesized in the same manner as compound (a-1), compounds (a-14), (a-22), (a-44), and compounds (a-50) to (a-56) were synthesized in the same manner as compound (a-2), compounds (a-13), (a-21), and (a-43) were synthesized in the same manner as compound (a-3), compounds (a-5), (a-8), (a-15), (a-23), and (a-45) were synthesized in the same manner as compound (a-4), and compounds (a-9) were synthesized in the same manner as compound (a-9). Compound (a-49) was synthesized using the above procedure, compound (a-20), compound (a-29), and compound (a-42) were synthesized in the same manner as compound (a-12), compound (a-24), compound (a-27), compound (a-30), and compound (a-46) were synthesized in the same manner as compound (a-16), compound (a-25), compound (a-31), and compound (a-47) were synthesized in the same manner as compound (a-17), compound (a-26), compound (a-28), compound (a-32), and compound (a-48) were synthesized in the same manner as compound (a-18), and compound (a-34) to compound (a-40) were synthesized in the same manner as compound (a-33). The yields (%) of the obtained [a] compounds are also shown in Table 1-1 and Table 1-2.

[0148]

[0149]

[0150] The following compounds (e-1) to (e-6) were used as monomers in the synthesis of polymer (A).

[0151]

[0152] Synthesis Example 2-1 Synthesis of Polymer (A-1) 3 g of dimethylacetamide was placed in a reaction vessel and kept at 80°C, and a mixed solution of 3.00 g of compound (a-1), 0.32 g of dimethyl-2,2-azobis(2-methylpropionate), and 6.00 g of dimethylacetamide was added dropwise from a feeder over 3 hours. After completion of the dropwise addition, the mixture was stirred at 80°C for 3 hours. The obtained polymerization solution was purified by precipitation with a 10-fold amount of methanol, and 2.80 g of polymer (A-1) was obtained as a white solid.

[0153] Synthesis Example 2-10 Synthesis of Polymer (A-10) 3 g of dimethylacetamide was placed in a reaction vessel and kept at 80°C, and a mixed solution of 3.00 g of compound (a-4), 0.45 g of compound (e-1) (styrenesulfonic acid neopentyl ester), 0.42 g of dimethyl-2,2-azobis(2-methylpropionate), and 6 g of dimethylacetamide was added dropwise over 3 hours. After completion of the dropwise addition, the mixture was stirred at 80°C for 3 hours. The obtained polymerization solution was purified by precipitation with a 10-fold amount of methanol, to obtain a white solid polymer (A-10).

[0154] Synthesis Example 2-16 Synthesis of Polymer (A-16) 3 g of dimethylacetamide was placed in a reaction vessel and kept at 80°C, and a mixed solution of 3.00 g of compound (a-1), 0.28 g of compound (e-6) (glycerol methacrylate), 0.42 g of dimethyl-2,2-azobis(2-methylpropionate), and 6 g of dimethylacetamide was added dropwise over 3 hours. After completion of the dropwise addition, the mixture was stirred at 80°C for 3 hours. The obtained polymerization liquid was purified by precipitation with a 10-fold amount of methanol, to obtain a white solid polymer (A-16).

[0155] Synthesis Example 2-34 Synthesis of Polymer (A-34) 3 g of ethyl acetate, 3 g of compound (a-27), 14 mg of 1-isobutoxyethyl acetate, and 5 mL of toluene were placed in an argon-purged reaction vessel and cooled to -10°C. 0.55 g of a 25% toluene solution of ethylaluminum dichloride was added and stirred for 6 hours, and then 1 mL of a 1% methanol solution of sodium methoxide was added. The resulting polymerization liquid was precipitated and purified with a 10-fold amount of methanol, yielding 2.20 g of polymer (A-34) as a white solid.

[0156] [Synthesis Examples 2-2 to 2-9, 2-11 to 2-15, 2-17 to 2-33, 2-35 to 2-55] (Synthesis of Polymers (A-2) to (A-9), (A-11) to (A-15), (A-17) to (A-33), and (A-35) to (A-62)) Except for using Monomer 1 and Monomer 2 shown in Tables 2-1 and 2-2, polymers (A-2) to (A-9), polymers (A-18) to (A-33), and polymers (A-36) to (A-62) were synthesized in the same manner as for polymer (A-1). Polymers (A-11) to (A-15) were synthesized in the same manner as for polymer (A-10). Polymer (A-17) was synthesized in the same manner as for polymer (A-16). Polymer (A-35) was synthesized in the same manner as for polymer (A-34). The Mw, Mn and PDI of the obtained polymer [A] are shown in Tables 2-1 and 2-2.

[0157] Comparative Synthesis Example 1 Synthesis of Polymer (x-1) 3 g of dimethylacetamide was placed in a reaction vessel and maintained at 80°C, and a mixed solution of 3.00 g of 2-(4-ethynylphenoxymethyl)oxirane, 0.78 g of dimethyl-2,2-azobis(2-methylpropionate), and 6.00 g of dimethylacetamide was added dropwise from a feeder over 3 hours. After completion of the dropwise addition, the mixture was stirred at 80°C for 3 hours. The resulting polymerization solution was purified by precipitation with a 10-fold amount of methanol, yielding 2.80 g (yield: 74%) of polymer (x-1) represented by the following formula as a white solid. The resulting polymer (x-1) had Mw: 4500, Mn: 2800, and PDI: 1.6.

[0158]

[0159] Comparative Synthesis Example 2 Synthesis of Polymer (x-2) 3 g of dimethylacetamide was placed in a reaction vessel and maintained at 80°C, and a mixed solution of 3.00 g of 4-hydroxystyrene, 0.31 g of dimethyl-2,2-azobis(2-methylpropionate), and 6.00 g of dimethylacetamide was added dropwise from a feeder over 3 hours. After completion of the dropwise addition, the mixture was stirred at 80°C for 3 hours. The resulting polymer solution was purified by precipitation with a 10-fold amount of methanol, yielding 2.50 g (yield: 75%) of polymer (x-2) represented by the following formula as a white solid. The resulting polymer (x-2) had Mw: 4500, Mn: 2800, and PDI: 1.6.

[0160]

[0161]

[0162]

[0163] <Preparation of Composition> The polymer [A], comparative polymer [E], polymer [B] solvent [C] acid generator and crosslinking agent [D] used in the preparation of the composition are shown below.

[0164] [[A] Polymer] A-1 to A-55: Polymers (A-1) to (A-62) synthesized above

[0165] [Comparative Polymers] x-1 to x-2: Polymers (x-1) to (x-2) synthesized above

[0166] [E] Polymer E-1: Compound represented by the following formula (E-1) E-2: Compound represented by the following formula (E-2)

[0167] [B] Solvent: B-1: Propylene glycol monomethyl ether acetate B-2: Cyclohexanone

[0168] [[C] Acid Generator] C-1: Compound represented by the following formula (C-1) C-2: Compound represented by the following formula (C-2) C-3: Compound represented by the following formula (C-3)

[0169] [[D] Crosslinking Agent] D-1: A compound represented by the following formula (D-1):

[0170] [Example 1-1] 25 parts by mass of (A-1) as the polymer [A] was dissolved in 7,900 parts by mass of (B-1) and 2,000 parts by mass of (B-2) as the solvent [B]. The resulting solution was filtered through a polytetrafluoroethylene (PTFE) membrane filter with a pore size of 0.45 μm to prepare composition (J-1).

[0171] Examples 1-2 to 1-65 and Comparative Examples 1-1 to 1-2 Compositions (J-2) to (J-58) and (CJ-1) to (CJ-2) were prepared in the same manner as in Example 1, except that the types and amounts of each component were used as shown in Table 1 below. In Table 3, "-" indicates that the corresponding component was not used.

[0172]

[0173] <Evaluation> Using the compositions prepared above, the solvent resistance and the rectangularity of the resist pattern formed by EUV exposure were evaluated by the following methods. The evaluation results are shown in Table 4 below.

[0174] [Solvent Resistance] The composition prepared above was applied to a 12-inch silicon wafer by spin coating using a spin coater (Tokyo Electron Limited's "CLEAN TRACK ACT12"). Next, the wafer was heated at 250°C for 60 seconds in an air atmosphere, and then cooled at 23°C for 60 seconds to form a resist underlayer film with an average thickness of 5 nm, thereby obtaining a substrate with a resist underlayer film formed on the substrate. The obtained substrate with a resist underlayer film was immersed in cyclohexanone (23°C) for 1 minute. The average film thicknesses before and after immersion were measured. The absolute value of the value obtained by {(X-X0) / X0} x 100 was calculated, where X0 is the average thickness of the resist underlayer film before immersion and X is the average thickness of the resist underlayer film after immersion, and this was used as the film thickness change rate (%). The solvent resistance was evaluated as "A" (good) when the film thickness change rate was less than 1%, as "B" (fairly good) when it was 1% or more but less than 10%, and as "C" (poor) when it was 10% or more.

[0175] <Preparation of Resist Composition> Resist composition (R-1) was obtained by mixing 100 parts by mass of a polymer having a structural unit (1) derived from 4-hydroxystyrene, a structural unit (2) derived from styrene, and a structural unit (3) derived from 4-t-butoxystyrene (the proportions of the structural units were (1) / (2) / (3)=65 / 5 / 30 (mol %)), 1.0 part by mass of triphenylsulfonium trifluoromethanesulfonate as a radiation-sensitive acid generator, and 4,400 parts by mass of ethyl lactate and 1,900 parts by mass of propylene glycol monomethyl ether acetate as solvents, and filtering the resulting solution through a filter with a pore size of 0.2 μm.

[0176] [Pattern Rectangularity (EUV Exposure)] An organic underlayer film forming material (JSR Corporation's "HM8006") was applied to a 12-inch silicon wafer by a spin coating method using a spin coater (Tokyo Electron Limited's "CLEAN TRACK ACT12"), and then heated at 250°C for 60 seconds to form an organic underlayer film with an average thickness of 100 nm. A silicon-containing film-forming composition (JSR Corporation's "NFC SOG080") was applied to this organic underlayer film, heated at 220°C for 60 seconds, and then cooled at 23°C for 30 seconds to form a silicon-containing film with an average thickness of 20 nm. The composition prepared above was applied to the silicon-containing film formed above to form a resist underlayer film. The resist underlayer film formed above was heated at 250°C for 90 seconds, and then cooled at 23°C for 30 seconds to obtain a resist underlayer film with an average thickness of 5 nm. Resist composition (R-1) was applied onto the resist underlayer film formed above, heated at 130° C. for 60 seconds, and then cooled at 23° C. for 30 seconds to form a resist film with an average thickness of 50 nm. Next, the resist film was irradiated with extreme ultraviolet rays using an EUV scanner (ASML's "TWINSCAN NXE:3300B" (NA 0.3, sigma 0.9, quadrupole illumination, 1:1 line and space mask with a line width on the wafer of 16 nm). After irradiation with extreme ultraviolet rays, the substrate was heated at 110°C for 60 seconds and then cooled at 23°C for 60 seconds. Thereafter, the substrate was developed by the puddle method using a 2.38 mass% aqueous solution of tetramethylammonium hydroxide (20°C to 25°C), washed with water, and dried to obtain an evaluation substrate on which a resist pattern was formed. A scanning electron microscope (Hitachi High-Technologies Corporation's "SU8220") was used to measure and observe the resist pattern of the evaluation substrate. The pattern rectangularity was evaluated as "A" (good) when the cross-sectional shape of the pattern was rectangular, and as "B" (poor) when there was a footing on the cross-section of the pattern.

[0177]

[0178] <Evaluation> Using the compositions prepared above, the rectangularity of resist patterns obtained by EUV exposure was evaluated by the following method. The evaluation results are shown in Table 5 below.

[0179] <Preparation of Resist Composition (R-2)> Compound (S-1) used in the preparation of resist composition (R-2) was synthesized according to the following procedure. In a reaction vessel, 6.5 parts by mass of isopropyltin trichloride was added to 150 mL of 0.5 N aqueous sodium hydroxide solution while stirring, and the mixture was stirred for 2 hours. The precipitate that formed was collected by filtration, washed twice with 50 parts by mass of water, and then dried to obtain compound (S-1). Compound (S-1) was an oxide hydroxide product (i-PrSnO) of the hydrolysis product of isopropyltin trichloride. (3/2-x/2) (OH) x (where 0<x<3 is the structural unit).

[0180] 2 parts by mass of the compound (S-1) synthesized above and 98 parts by mass of propylene glycol monoethyl ether were mixed, and the resulting mixture was passed through an activated 4 Å molecular sieve to remove residual water, followed by filtration through a filter with a pore size of 0.2 μm to prepare resist composition (R-2).

[0181] [Pattern Rectangularity (EUV Exposure)] An organic underlayer film-forming material ("HM8006" manufactured by JSR Corporation) was applied onto a 12-inch silicon wafer by spin coating using a spin coater ("CLEAN TRACK ACT12" manufactured by Tokyo Electron Limited), and then heated at 250°C for 60 seconds to form an organic underlayer film with an average thickness of 100 nm. The resist underlayer film-forming composition prepared above was applied onto this organic underlayer film, heated at 220°C for 60 seconds, and then cooled at 23°C for 30 seconds to form a resist underlayer film with an average thickness of 5 nm. Resist composition (R-2) was applied onto this resist underlayer film by spin coating using the spin coater, and after a predetermined time had elapsed, heated at 90°C for 60 seconds and then cooled at 23°C for 30 seconds to form a resist film with an average thickness of 35 nm. The resist film was exposed to light using an EUV scanner (ASML's "TWINSCAN NXE:3300B" (NA 0.3, sigma 0.9, quadrupole illumination, 1:1 line and space mask with on-wafer line width of 16 nm). After exposure, the substrate was heated at 110°C for 60 seconds and then cooled at 23°C for 60 seconds. Thereafter, the substrate was developed by a puddle method using 2-heptanone (20 to 25°C) and then dried to obtain an evaluation substrate on which a resist pattern was formed. A scanning electron microscope (Hitachi High-Tech's "CG-6300") was used to measure and observe the resist pattern of the evaluation substrate. The pattern rectangularity was evaluated as "A" (good) when the cross-sectional shape of the pattern was rectangular, and as "B" (poor) when there was a footing on the cross section of the pattern.

[0182]

[0183] As can be seen from the results in Tables 4 and 5, the resist underlayer films formed from the compositions of the Examples were superior in solvent resistance and pattern rectangularity compared to the resist underlayer films formed from the compositions of the Comparative Examples.

[0184] The composition for forming a resist underlayer film of the present invention can form a film having excellent solvent resistance and pattern rectangularity. The method for producing a semiconductor substrate of the present invention uses a composition for forming a resist underlayer film that can form a resist underlayer film having excellent solvent resistance and pattern rectangularity, so that semiconductor substrates can be produced efficiently. Therefore, these compositions can be suitably used in the production of semiconductor devices, etc.

Claims

1. A composition for forming a resist underlayer film, comprising: a polymer having a repeating unit represented by the following formula (1); and a solvent. (In formula (1), R 1 is a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. 1 is a single bond or a divalent linking group. 1 is a monovalent group having an aromatic ring having 6 to 20 ring members. The hydrogen atoms in the aromatic ring are substituted with at least one halogen atom. 1 has at least one group selected from the group consisting of a group represented by the following formula (2-1), a group represented by the following formula (2-2), a group represented by the following formula (2-3), a group represented by the following formula (2-4), a group represented by the following formula (2-5), a group represented by the following formula (2-6), a group represented by the following formula (2-7), and a group represented by the following formula (2-8). (In formula (2-1) to formula (2-8), * represents Ar 1 is a bond to the atom constituting R 7 is a divalent organic group having 1 to 20 carbon atoms or a single bond. 8 , R 9 and R 10 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. In formula (2-2), ** is a bond to an atom constituting Cy. Cy is a ring structure having 3 to 20 ring members formed together with the two carbon atoms in the formula. R 11 is a hydrogen atom, a monovalent organic group having 1 to 20 carbon atoms, or a bond to **. 12 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 13 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.

2. L 1 The composition for forming a resist underlayer film according to claim 1 , wherein is a single bond.

3. The composition for forming a resist underlayer film according to claim 1, wherein the hydrogen atoms on the aromatic ring are substituted with at least two halogen atoms.

4. The composition for forming a resist underlayer film according to any one of claims 1 to 3, wherein the halogen atom is an iodine atom.

5. The composition for forming a resist underlayer film according to any one of claims 1 to 3, wherein the content of the repeating unit represented by formula (1) in all repeating units constituting the polymer is 10 mol % or more.

6. The composition for forming a resist underlayer film according to any one of claims 1 to 3, which is a composition for forming an underlayer film of a resist film to be exposed to extreme ultraviolet rays.

7. The composition for forming a resist underlayer film according to any one of claims 1 to 3, wherein the resist underlayer film has a thickness of 20 nm or less.

8. The composition for forming a resist underlayer film according to claim 6, wherein the composition for forming a resist film contains a metal.

9. A method for producing a semiconductor substrate, comprising: a step of applying a composition for forming a resist underlayer film directly or indirectly to a substrate; a step of applying a composition for forming a resist film to the resist underlayer film formed in the step of applying the composition for forming a resist film; a step of exposing the resist film formed in the step of applying the composition for forming a resist film to radiation; and a step of developing at least the exposed resist film, wherein the composition for forming a resist underlayer film comprises a polymer having a repeating unit represented by the following formula (1) and a solvent. (In formula (1), R 1 is a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. 1 is a single bond or a divalent linking group. 1 is a monovalent group having an aromatic ring having 6 to 20 ring members. The hydrogen atoms in the aromatic ring are substituted with at least one halogen atom. 1 has at least one group selected from the group consisting of a group represented by the following formula (2-1), a group represented by the following formula (2-2), a group represented by the following formula (2-3), a group represented by the following formula (2-4), a group represented by the following formula (2-5), a group represented by the following formula (2-6), a group represented by the following formula (2-7), and a group represented by the following formula (2-8). (In formula (2-1) to formula (2-8), * represents Ar 1 is a bond to the atom constituting R 7 is a divalent organic group having 1 to 20 carbon atoms or a single bond. 8 , R 9 and R 10 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. In formula (2-2), ** is a bond to an atom constituting Cy. Cy is a ring structure having 3 to 20 ring members formed together with the two carbon atoms in the formula. R 11 is a hydrogen atom, a monovalent organic group having 1 to 20 carbon atoms, or a bond to **. 12 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 13 is a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.

10. The method for manufacturing a semiconductor substrate according to claim 9, wherein said radiation is extreme ultraviolet radiation.

11. The method for producing a semiconductor substrate according to claim 9 or 10, wherein the resist underlayer film has a thickness of 20 nm or less.

12. The method for producing a semiconductor substrate according to claim 9 or 10, wherein the resist film-forming composition contains a metal.

Citation Information

Patent Citations

  • Resist underlayer film material, resist underlayer film forming method and pattern forming method

    JP2012063653A

  • Resist composition, resist pattern forming method, and compound

    JP2023161653A

  • Actinic ray sensitive or radiation sensitive resin composition, resist film, pattern forming method, electronic device manufacturing method

    WO2022044706A1

  • Pattern forming method, electronic device manufacturing method, actinic ray-sensitive or radiation-sensitive resin composition, and resist film

    WO2023286764A1

Cited By

  • Compound, composition, resin composition, composition for forming film, composition for forming film for lithography, and composition for forming resist film

    WO2025079648A1

  • Epoxy compound and use thereof

    WO2025100238A1

  • Underlayer film-forming composition for metal-containing resist film and method for producing semiconductor substrate