Optical member and method for manufacturing optical member

The optical member with a silicon oxide film and water-repellent coating on a smooth substrate addresses the issues of reflectance and water adhesion, enhancing image quality and durability by using a fine uneven structure and intermediate layer to reduce reflectance and improve water repellency.

WO2024203250A1PCT designated stage expired Publication Date: 2024-10-03FUJIFILM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009419
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-11
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Optical members used in cameras and similar devices face challenges with high reflectance and water droplet adhesion, leading to image quality issues, particularly when exposed to the outdoors where raindrops can cause reflections and image deterioration.

Method used

An optical member with a smooth substrate and a silicon oxide film featuring a fine uneven structure, coated with a water-repellent film containing a fluorine compound, which has a low adhesion energy and a sliding angle of 10° or less, combined with an intermediate layer to reduce reflectance and enhance water repellency.

Benefits of technology

The solution effectively suppresses water droplet adhesion and reflection, achieving high water repellency and low reflectance, thereby improving image quality and durability against environmental factors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009419_03102024_PF_FP_ABST
    Figure JP2024009419_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: an optical member comprising an optical substrate that has a smooth surface and a silicon oxide film that is provided on the optical substrate, wherein the silicon oxide film has a fine uneven structure on a surface thereof and is provided with a fluorine compound-containing water-repellent film on a surface of the fine uneven structure, and the surface of the water-repellent film has an adhesion energy of 0.2 mN / m-6 mN / m; and a method for manufacturing the optical member.
Need to check novelty before this filing date? Find Prior Art

Description

Optical member and method for manufacturing the same

[0001] The present disclosure relates to optical members and methods for manufacturing optical members.

[0002] Optical components used in cameras and the like are desired to have low reflectivity for incident light. Furthermore, for optical components provided on surfaces exposed to the outside, there is a demand to prevent water droplets such as raindrops from adhering to the optical components in order to prevent raindrops from appearing in images.

[0003] Japanese Patent Application Laid-Open No. 2020-56866 discloses a glass laminate comprising an anti-reflection layer made of a multilayer film including a silicon oxide film on the irregular surface of a glass substrate having a textured surface on which fine irregularities are formed, and an anti-fouling layer on the surface of the anti-reflection layer.

[0004] Japanese Patent Application Laid-Open No. 2018-198050 discloses a transparent substrate with an antifouling film, which includes an antiglare layer having an uneven surface formed by applying a binder containing silicon oxide as a main component onto the transparent substrate and firing the applied binder, and an antifouling layer formed on the antiglare layer.

[0005] Japanese Patent Application Laid-Open No. 2015-59977 discloses a method for forming fine irregularities on the surface of a transparent substrate.

[0006] An object of the present disclosure is to provide an optical member that is highly water-repellent and can suppress adhesion of water droplets, and a method for manufacturing the optical member.

[0007] The optical member of the present disclosure comprises an optical substrate having a smooth surface and a silicon oxide film provided on the optical substrate, the silicon oxide film having a fine uneven structure on the surface thereof, and a water-repellent film containing a fluorine compound on the surface of the fine uneven structure, the adhesion energy of the surface of the water-repellent film being 0.2 mN / m to 6 mN / m.

[0008] Fluorine compounds are -(OCF 2 CF 2 ) n - group, n is an integer of 1 or more, and -(OCF 2 ) m It is preferred that the aryl group does not contain a - group, where m is an integer of 1 or more.

[0009] It is preferable that the sliding angle of a 5 μL water droplet on the surface of the water-repellent film is 10° or less.

[0010] The silicon oxide film preferably has an aluminum content of 0.25 wt. % or less, a calcium content of 2.0 wt. % or less, a boron content of 2.0 wt. % or less, and a carbon content of 6 wt. % or less.

[0011] The silicon oxide film is preferably a sputtered film or a vapor-deposited film.

[0012] When the composition of silicon oxide contained in the silicon oxide film is expressed as SiOx, it is preferable that 1.90≦x≦2.00.

[0013] It is preferable that the average height from the bottom of the recesses to the top of the protrusions of the fine uneven structure is 150 nm to 600 nm, and the average period is 150 nm to 450 nm.

[0014] In the optical member of the present disclosure, the water-repellent film preferably has a contact angle of water of 140° or more on the surface thereof.

[0015] The optical member of the present disclosure preferably has a haze of 2.5% or less.

[0016] The optical member of the present disclosure preferably has an average reflectance of 1% or less when light having a wavelength of 400 nm to 700 nm is incident perpendicularly on the surface.

[0017] The optical member of the present disclosure preferably has a transmission wavefront aberration of λ / 5 or less for light with a wavelength of λ nm.

[0018] The optical member of the present disclosure preferably includes an intermediate layer between the optical substrate and the silicon oxide film, the intermediate layer having a refractive index different from that of the silicon oxide film, for reducing the reflectance of incident light.

[0019] The method for manufacturing an optical element of the present disclosure includes a film-forming step of forming a silicon oxide film on one surface of an optical substrate by a vapor-phase film-forming method, a mask-forming step of forming an etching mask on the silicon oxide film, an etching step of etching the silicon oxide film through the etching mask by a vapor-phase etching method to form a fine uneven structure on the surface of the silicon oxide film, and a coating step of forming a water-repellent film containing a fluorine compound on the surface of the fine uneven structure, and in the etching step, etching is carried out until the distance from the surface of the silicon oxide film facing the optical substrate to the apex of the maximum convexity of the fine uneven structure becomes smaller than the film thickness of the silicon oxide film immediately after film formation.

[0020] According to the optical member and the method for manufacturing the optical member of the present disclosure, an optical member that is highly water-repellent and can suppress the adhesion of water droplets can be obtained.

[0021] 12A is a cross-sectional schematic diagram of an optical member according to an embodiment; FIG. 12B is a cross-sectional schematic diagram of an optical member according to a modified example; FIG. 13A is a diagram illustrating a manufacturing process of an optical member according to an embodiment; FIG. 13B is a diagram illustrating details of a mask formation process; FIG. 13C is a diagram illustrating details of an etching process; FIG. 13D is a cross-sectional SEM image illustrating a change in the surface shape of a silicon oxide film over time due to chemical etching; FIG. 13E is a diagram illustrating a method for measuring the sliding angle of water; FIG. 13F is an image of a water droplet when the stage is tilted at 0° and 3.4°; FIG. 13G is a diagram illustrating a method for calculating the adhesion energy of the surface of an optical member; FIG. 13H is a diagram illustrating a method for deriving the average height of the unevenness of a fine uneven structure (part 1); FIG. 13I is a diagram illustrating a method for evaluating the sliding property; FIG. 13J is a diagram illustrating the relationship between etching time and adhesion energy; FIG. 13J is a diagram illustrating the contact angle of water at each position on the X-axis; FIG. 13J is a diagram illustrating a method for evaluating the sliding property of a fine uneven structure ... a contact angle of water at each position on the X-axis; FIG. 13J is a diagram illustrating a method for evaluating the sliding property of a fine uneven structure; 2 FIG. 16B is a schematic diagram for explaining the area ratio of the target and the optical glass piece. 217A is a schematic diagram showing a state in which an optical glass piece is placed on a target. FIG. 17A is an image taken when measuring the transmitted wavefront aberration of sample 6-1, FIG. 17B is an image taken when measuring the transmitted wavefront aberration of sample 6-2, FIG. 17C is an image taken when measuring the transmitted wavefront aberration of sample 6-3, and FIG. 17D is an image taken when measuring the transmitted wavefront aberration of sample 6-4. FIG. 17B is an image taken when measuring the transmitted wavefront aberration of sample 6-4. FIG. 17C is an image taken when measuring the transmitted wavefront aberration of sample 6-3, and FIG. 17D is an image taken when measuring the transmitted wavefront aberration of sample 6-4. FIG. 17D is an image taken when measuring the transmitted wavefront aberration of sample 6-4. FIG. 17D is an image taken when measuring the transmitted wavefront aberration of sample 6-4. FIG. 17D is an image taken when measuring the transmitted wavefront aberration of sample 6-4. FIG. 17D is an image taken when measuring the transmitted wavefront aberration of sample 6-3 ...

[0022] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. For ease of visualization, the thicknesses and ratios of each layer have been appropriately modified and do not necessarily reflect the actual thicknesses and ratios. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0023] 1 shows a cross-sectional view of an optical member according to one embodiment. The optical member 1 comprises an optical substrate 10 having a smooth surface, a silicon oxide film 20 provided on the optical substrate 10, and a water-repellent film 30 provided on the surface of the silicon oxide film 20. The adhesion energy of the surface of the water-repellent film 30 of the optical member 1 is 0.2 mN / m to 6 mN / m. The adhesion energy is preferably 5.62 mN / m or less, more preferably 2.85 mN / m or less, and even more preferably 0.29 mN / m to 1.29 mN / m.

[0024] The shape of the optical substrate 10 is not particularly limited, and may be a transparent substrate that is mainly used in optical devices, such as a flat plate, a concave lens, or a convex lens, and may be a substrate composed of a combination of a curved surface having a positive or negative curvature and a flat surface.

[0025] The silicon oxide film 20 has a fine uneven structure 22 on its surface. In the silicon oxide film 20, the aluminum content is 0.25 wt. % or less, the calcium content is 2.0 wt. % or less, the boron content is 2.0 wt. % or less, and the carbon content is 6.0 wt. % or less. The aluminum content is preferably 0.1 wt. % or less, the calcium content is preferably 1.0 wt. % or less, the boron content is preferably 1.0 wt. % or less, and the carbon content is preferably 4.0 wt. % or less. The contents of the components contained in the silicon oxide film 20 can be measured by X-ray photoelectron spectroscopy (XPS).

[0026] The silicon oxide film 20 is preferably a film formed by a vapor phase film deposition method. Specifically, the silicon oxide film 20 is preferably a sputtered film formed by a sputtering method, or a vapor deposition film formed by a vapor deposition method.

[0027] When the composition of silicon oxide contained in the silicon oxide film 20 is expressed as SiOx, it is preferable that 1.90≦x≦2.00, and more preferably 1.95≦x≦2.00.

[0028] The fine uneven structure 22 formed on the surface of the silicon oxide film 20 preferably has an average height from the bottom of the recesses to the top of the protrusions of 150 nm to 600 nm, and an average period of the unevenness of 150 nm to 450 nm. The average height is more preferably 150 nm to 450 nm, and even more preferably 200 nm to 350 nm. The average period is more preferably 150 nm to 400 nm, and even more preferably 150 nm to 350 nm.

[0029] The method for measuring the average height and average period of the irregularities will be explained in the examples below.

[0030] The water-repellent film 30 is provided on the surface of the fine uneven structure 22 of the silicon oxide film 20. The water-repellent film 30 constitutes the outermost surface of the optical member 1. The water-repellent film 30 contains a fluorine compound. Examples of fluoride compounds include Surf Clear (manufactured by Canon Optron), Optool (HD-1100TH: manufactured by Daikin Corporation), Fluorosurf (NL-1: manufactured by Fluorosurf Corporation), KY1091 (manufactured by Shin-Etsu Chemical Co., Ltd.), and NB05 (manufactured by Katsurayama Technology Co., Ltd.). Examples of fluorine compounds that constitute the water-repellent film 30 include -(OCF 2 CF 2 ) n - group (where n is an integer of 1 or more), and -(OCF 2 ) m It is more preferable that the fluorine compound does not contain a - group (where m is an integer of 1 or more). As will be shown in the examples below, the fluorine compound does not contain a -(OCF 2 ) m (OCF 2 CF 2 ) n -functional group rather than -(OCF 2 ) m does not contain a - group, -(OCF 2 CF 2 ) n Fluorine compounds consisting of only - functional groups provide higher durability (see Table 11 below).

[0031] In the optical member 1, it is preferable that the sliding angle of a 5 μL water droplet on the surface of the water-repellent film 30 is 10° or less.

[0032] The sliding angle is a value measured by the following method: The optical element 1 is placed on a flat stage, and a water droplet with a volume of 5 μL is dropped onto the surface of the water-repellent film 30. In this state, the stage is gradually tilted at a rate of 0.2° / second. The angle at which the edge of the water droplet begins to move is taken as the sliding angle.

[0033] The optical member 1 preferably has a water contact angle of 140° or more on the surface of the water-repellent film 30. The water contact angle can be measured using a commercially available contact angle meter. In this specification, the water contact angle refers to a static contact angle measured with a 2 mL water droplet.

[0034] The optical member 1 preferably has a haze of 2.5% or less. A smaller haze is more preferable. The smaller the haze of the optical member 1, the less scattering there is within the optical member and the higher the quality, so the smaller the haze is, the more preferable it is. The haze can be measured using a commercially available haze meter.

[0035] The optical member 1 preferably has an average reflectance of 1% or less when light having a wavelength of 400 nm to 700 nm is incident perpendicularly to the substrate surface. The average reflectance means the average value of the reflectance at each wavelength between 400 nm and 700 nm. It is preferable that the average reflectance is 1% or less at all wavelengths between 400 nm and 700 nm. The lower the reflectance, the higher the anti-reflection performance.

[0036] The reflectance for each wavelength is measured by irradiating light at an incident angle of 0° onto the optical member 1. The wavelength dependency of the reflectance can be measured using a commercially available spectrometer.

[0037] The optical member 1 preferably has a transmission wavefront aberration of λ / 5 or less for light with a wavelength of λ nm. The transmission wavefront aberration can be measured using a commercially available laser interferometer.

[0038] As described above, the optical element 1 of this embodiment includes an optical substrate 10 having a smooth surface and a silicon oxide film 20 disposed on the optical substrate 10. The silicon oxide film 20 has a microrelief structure 22 on its surface, and a water-repellent film 30 containing a fluorine compound is disposed on the surface of the microrelief structure 22. By providing the water-repellent film 30 on the surface of the microrelief structure 22 formed on the silicon oxide film 20, a significantly higher water repellency can be achieved compared to when the water-repellent film 30 is disposed on a flat surface. By providing the water-repellent film 30 on the surface of the microrelief structure, the surface area of ​​the water-repellent film can be increased. As a result, the difference between the surface free energy of water and the surface free energy of the optical element increases. The greater the difference between the surface free energy of water and the surface free energy of the optical element, the higher the water repellency. When a water-repellent film made of a typical fluorine compound is applied to a flat substrate, the water contact angle on the surface is approximately 110°. With this optical element 1, a water contact angle of more than 120°, or even 140° or more, can be achieved.

[0039] Furthermore, because the adhesion energy of the surface of the water-repellent film 30 is 0.2 mN / m to 6 mN / m, water droplets are less likely to remain on the surface of the optical member 1, providing a lotus effect of high water sliding off. The excellent water sliding off property can prevent water droplets from adhering to the surface. Therefore, the optical member 1 is suitable as a lens filter to be provided on the externally exposed surface of a camera or the like.

[0040] The above configuration makes it possible to realize an optical element in which the sliding angle of a 5 μL water droplet on the surface of the water-repellent film 30 is 10° or less. If the sliding angle of the water droplet is 10° or less, it can be said that the water droplet has very good sliding properties, and adhesion of water droplets to the surface can be further effectively prevented.

[0041] In the optical member 1 of this embodiment, the silicon oxide film 20 has an aluminum content of 0.25 wt. % or less, a calcium content of 2.0 wt. % or less, a boron content of 2.0 wt. % or less, and a carbon content of 6 wt. % or less. With this configuration, when fabricating the optical member 1, the generation of compounds that react with the etching gas and inhibit etching can be suppressed during vapor-phase etching of the silicon oxide film 20 (see Test 2 described below). Therefore, the fine concave-convex structure 22 can be easily formed.

[0042] In addition, when the silicon oxide film 20 is a film produced by a vapor phase film formation method, for example, a sputtered film or a vapor deposition film produced by a sputtering method or a vapor deposition method, it is possible to make the impurity concentration of the film sufficiently reduced.

[0043] When the composition of silicon oxide (SiOx) contained in the silicon oxide film 20 satisfies 1.90≦x≦2.00, the difference between the maximum and minimum values ​​in the in-plane distribution of water contact angles on the surface of the optical element 1, i.e., the surface of the water-repellent film 30, can be suppressed to approximately 10% of the maximum value (see Test 3 described below).

[0044] When the average height from the bottom of the recesses to the top of the protrusions of the fine uneven structure formed on the surface of the silicon oxide film 20 of the optical element 1 is 150 nm to 600 nm and the average period is 150 nm to 450 nm, the water repellency is higher and the adhesion of water droplets can be more effectively suppressed.

[0045] If the contact angle of water on the surface of the optical member 1 provided with the water-repellent film 30 is 140° or more, very high water repellency can be obtained.

[0046] (Modification) Fig. 2 shows a cross-sectional view of a modification of the optical element 2. In Fig. 2, the same components as those in Fig. 1 are denoted by the same reference numerals. The optical element 2 includes an intermediate layer 12 between the optical substrate 10 and the silicon oxide film 20, the intermediate layer 12 having a refractive index different from that of the silicon oxide film 20, for reducing the reflectance of incident light. In this specification, the term "intermediate layer" refers to a layer provided between the optical substrate 10 and the silicon oxide film 20.

[0047] The intermediate layer 12 may be a single layer or a multilayer film. When the intermediate layer 12 is a single layer, by using a single-layer dielectric film having a refractive index between that of the optical substrate 10 and that of the silicon oxide film 20, an optical element 1 having a reflectance of 1% or less for light in the 400 nm to 700 nm range can be realized. When the intermediate layer 12 is a multilayer film, as shown in FIG. 2(a), it is preferable that high-refractive index layers 12a having a relatively high refractive index and low-refractive index layers 12b having a relatively low refractive index are alternately stacked. In FIG. 2(a), six low-refractive index layers 12b and high-refractive index layers 12a are alternately stacked in this order from the optical substrate 10 side, but the stacking order of the high-refractive index layers 12a and low-refractive index layers 12b may be reversed. There is no particular limitation on the number of layers in the multilayer film, and the intermediate layer 12 may have a three-layer structure, as shown in FIG. 2(b).

[0048] The high refractive index layer 12a has a higher refractive index than the low refractive index layer 12b, and the low refractive index layer 12b has a lower refractive index than the high refractive index layer 12a. However, it is more preferable that the refractive index of the high refractive index layer 12a is higher than the refractive index of the optical substrate 10, and the refractive index of the low refractive index layer 12b is lower than the refractive index of the optical substrate 10.

[0049] The high refractive index layers 12a and the low refractive index layers 12b do not have to have the same refractive index, but it is preferable to use the same material and have the same refractive index in order to reduce material costs, film formation costs, and the like.

[0050] The high refractive index layer 12a is made of niobium pentoxide (Nb 2 O 5 ), titanium oxide (TiO 2 ), zirconium oxide (ZrO 2 ), tantalum pentoxide (Ta 2 O 5 ), silicon oxynitride (SiON), silicon nitride (Si 3 N 4 ) and silicon niobium oxide (SiNbO).

[0051] The low refractive index layer 12b is made of a material such as silicon oxide (SiO 2 ), silicon oxynitride (SiON), gallium oxide (Ga 2 O 3 ), aluminum oxide (Al 2 O 3 ), lanthanum oxide (La 2 O 3 ), lanthanum fluoride (LaF 3 ), magnesium fluoride (MgF 2 ), sodium aluminum fluoride (Na 3 AlF 6 ) etc.

[0052] The refractive index of any compound can be changed to some extent by forming a film by controlling the ratio of constituent elements so as to deviate from the stoichiometric composition ratio or by controlling the film formation density.

[0053] (Manufacturing Method) A manufacturing method for the optical member 1 of one embodiment will be described.

[0054] 3, the method for manufacturing the optical element 1 includes steps A to D. Step A is a film formation step in which a silicon oxide film 20 is formed on the optical substrate 10. Step B is a mask formation step in which a mask 40 is formed on the silicon oxide film 20. Step C is an etching step in which the mask 40 is used to vapor-etch the silicon oxide film 20 with an etching gas G. Step D is a coating step in which a water-repellent film 30 is formed on the surface of the etched silicon oxide film 20. Arrow F schematically indicates the coating process.

[0055] In the film formation step (step A), a silicon oxide film 20 is formed on one surface of the optical substrate 10 by a vapor phase film formation method. Examples of vapor phase film formation methods include sputtering, vacuum deposition, and chemical vapor deposition, with sputtering being particularly preferred. By using a vapor phase film formation method, it is possible to prevent impurities from being mixed into the silicon oxide film 20. In other words, a sputtered film formed by a sputtering method or a vapor deposition film formed by a vacuum deposition method can be said to be a film in which the mixing of elements other than the target (i.e., impurities) is sufficiently prevented.

[0056] For example, when the silicon oxide film 20 is formed by sputtering, SiO 2 By using a target and introducing oxygen into the film-forming chamber and adjusting the flow rate of the oxygen, the x in silicon oxide (SiOx) can be adjusted as desired.

[0057] The silicon oxide film 20 has a thickness of, for example, 500 nm to 1500 nm.

[0058] The details of the mask formation step (step B) are shown in Fig. 4. As an example, the mask formation step includes, as shown in Fig. 4, step B-1: an Al-containing thin film formation step of forming a thin film 42 containing aluminum (hereinafter referred to as the Al-containing thin film 42) on the silicon oxide film 20, and step B-2: a hot water treatment step of treating the Al-containing thin film 42 with hot water.

[0059] In the Al-containing thin film forming step (step B-1), the Al-containing thin film 42 is formed by a vapor phase deposition method. Examples of the vapor phase deposition method include sputtering, vacuum deposition, and chemical vapor deposition, with sputtering being particularly preferred. When the silicon oxide film 20 is formed by sputtering, it is preferable to form the Al-containing thin film 42 continuously in the same chamber.

[0060] Examples of the Al-containing thin film 42 include an aluminum film, an aluminum oxide film, and an aluminum nitride film. The thickness of the Al-containing thin film 42 is preferably 0.5 to 60 nm, more preferably 2 to 40 nm, and even more preferably 5 to 20 nm.

[0061] The hot water treatment in the hot water treatment step (step B-2) refers to a treatment in which the laminate is exposed to hot water of 60°C or higher for at least 1 minute. Examples of hot water treatment include a method of immersing the laminate on which the Al-containing thin film 42 has been formed in room temperature water (pure water is particularly preferred) and then boiling the water, a method of immersing the laminate in hot water maintained at a high temperature, or a method of exposing the Al-containing thin film 42 to high-temperature steam. In this embodiment, the pure water 6 contained in the water tank 5 is heated, and the laminate consisting of the optical substrate 10, the silicon oxide film 20, and the Al-containing thin film 42 is immersed in the heated pure water 6 to perform the hot water treatment. The boiling or immersion time is particularly preferably 3 minutes or more and 15 minutes or less. The temperature of the hot water is preferably higher than 90°C. The higher the temperature, the shorter the treatment time tends to be.

[0062] The hot water treatment transforms the Al-containing thin film 42 into a concave-convex structure layer whose main component is alumina hydrate, as shown in step B-3. The concave-convex structure layer corresponds to the mask 40. Hereinafter, the term "convex-convex structure layer 40" is synonymous with the mask 40. The alumina hydrate that constitutes the concave-convex structure layer 40 includes boehmite (expressed as Al2O3.H2O or AlOOH), which is alumina monohydrate, and bayerite (expressed as Al2O3.3H2O or Al(OH)3), which is alumina trihydrate (aluminum hydroxide).

[0063] The concave-convex structure layer 40 has a randomly shaped concave-convex structure, and the size (size of the apex angle) and direction of the convex portions vary, but the concave-convex structure layer 40 has a generally sawtooth cross section.

[0064] The details of the etching step (step C) are shown in Fig. 5. As an example, the etching step includes step C-1: a physical etching step in which the concave-convex structure layer 40 is physically etched according to its shape, and step C-2: a reactive etching (chemical etching) step in which the silicon oxide film 20 exposed in the recesses of the concave-convex structure layer 40 is selectively etched, as shown in Fig. 5.

[0065] In the physical etching step (step C-1), the concave-convex structure layer 40 made of alumina hydrate is etched to expose the silicon oxide film 20 in the recesses of the concave-convex structure layer 40. Here, the etching gas G1 is, for example, a mixture of argon (Ar) and CHF 3 A mixed gas of fluorine (fluorine), methyl fluoride (trifluoromethane), and methyl fluoride (trifluoromethane) is used. The ratio of the physical etching time t1 to the time t2 of the subsequent chemical etching step (t1 / t2) × 100 is preferably 0.56 to 2.22. Specifically, t1 is preferably about 15 to 60 seconds, and more preferably 30 to 45 seconds (see Test 6 below).

[0066] In the chemical etching step (step C-2), the silicon oxide film 20 exposed in the recess is etched. The etching gas G2 is, for example, SF 6 (sulfur hexafluoride) and CHF 3 In this case, a mixed gas of SF6, which is a reactive gas, is used. 6 SiO 2 and reacting with SiF 4 is generated and vaporized to produce SiO 2 is chemically etched. In this chemical etching step, etching is carried out until the distance d2 from the surface of the silicon oxide film 20 facing the optical substrate 10 to the apex of the largest convexity of the fine concave-convex structure becomes smaller than the film thickness d1 of the silicon oxide film 20 immediately after film formation. The chemical etching time t2 is preferably 600 to 3600 seconds (10 to 60 minutes), more preferably 900 to 3000 seconds (15 to 50 minutes), and particularly preferably 1800 to 2700 seconds (30 to 45 minutes) (see Test 1 described below).

[0067] After the chemical etching step, a cleaning step (step C-3) is carried out to remove the uneven structure layer 40 remaining on the surface of the silicon oxide film 20.

[0068] In the cleaning process (process C-3), SH 3 O 3 The concave-convex structure layer 40 is removed using a mixed solution of sulfuric acid and hydrogen peroxide, and after drying, ultraviolet (UV) irradiation is performed.

[0069] In the coating step (step D), a water-repellent film 30 containing a fluorine compound is formed on the surface of the etched silicon oxide film 20. The coating method may be dry coating or wet coating. Examples of fluorine compounds for dry coating include Surf Clear (manufactured by Canon Optron), and examples of fluorine compounds for wet coating include Optool (HD-1100TH: manufactured by Daikin Corporation), Fluorosurf (NL-1: manufactured by Fluorosurf), KY1091 (manufactured by Shin-Etsu Chemical Co., Ltd.), and NB05 (manufactured by Katsurayama Technology Co., Ltd.).

[0070] Through the above steps, the optical member 1 can be manufactured.

[0071] When fabricating an optical element 2 including an intermediate layer 12, the intermediate layer 12 is formed before forming the silicon oxide film 20 on the optical substrate 10. It is also preferable to use a vapor phase deposition method for forming the intermediate layer 12. Vapor phase deposition makes it possible to easily form layered structures with a variety of refractive indices and layer thicknesses.

[0072] FIG. 6 shows cross-sectional SEM images showing the change in the surface shape of a silicon oxide film over time due to chemical etching. (1) to (5) show the results of a silicon oxide film (SiO in FIG. 6) with a thickness of 1000 nm formed on a substrate. 2The cross-sections of samples with different chemical etching times are shown after a 45-second physical etching process using the above manufacturing process. Samples (1) to (5) are arranged in order of etching time, with sample (1) being the sample with the shortest etching time and sample (5) being the sample with the longest etching time. At relatively short etching times like samples (1) and (2), recesses are formed only in parts of the surface, and it cannot be said that the entire surface is uneven. As the etching time increases, the number of recesses gradually increases, and in sample (3), recesses are formed over almost the entire surface of the silicon oxide film. After the entire surface is uneven, etching proceeds so that the entire surface is removed while maintaining the uneven shape. In sample (4), almost no flat areas are observed on the surface of the silicon oxide film. Furthermore, in sample (5), which has the longest etching time, etching has progressed until the distance from the surface of the silicon oxide film 20 facing the optical substrate 10 to the apex of the maximum convexity of the fine unevenness structure is smaller than the thickness of the silicon oxide film 20 immediately after deposition. In (5), the distance from the surface of the silicon oxide film on the optical substrate 10 side to the apex of the maximum convexity of the fine concave-convex structure is approximately 500 nm, which is approximately half the original film thickness of 1000 nm.

[0073] According to the inventors' investigations, samples (3), (4), and (5) can achieve sufficient anti-reflection effects, and by forming a water-repellent film on the surface, they exhibit super-water-repellency. However, while sample (5) achieves a surface with high sliding properties, preventing water droplets from adhering to the surface due to the lotus effect, samples (3) and (4) exhibit low sliding properties, due to the petal effect, allowing water droplets to adhere to the surface. This means that the surface adhesion energy of the uneven structures of samples (3) and (4) does not satisfy the range of 0.2 mN / m to 6 mN / m.

[0074] By carrying out etching until the distance from the surface of the silicon oxide film 20 facing the optical substrate 10 to the apex of the maximum convexity of the fine concave-convex structure becomes smaller than the film thickness of the silicon oxide film 20 immediately after film formation, a fine concave-convex structure having a cross-sectional structure as shown in (5) can be obtained. In other words, an optical member having a surface adhesion energy of 0.2 mN / m to 6 mN / m can be realized.

[0075] When carrying out the above-mentioned chemical etching, if the silicon oxide film 20 contains impurity elements that react with the etching gas to generate compounds that are difficult to gasify, the SiO 2 There is a possibility that the reaction between SiO and reactive gases may be inhibited. 2 If the reaction between SF and the reactive gas is inhibited, problems such as a slow etching rate, an unstable etching rate, or etching not proceeding properly may occur. 6 Impurity elements that react with SiO to produce fluorine compounds that are difficult to gasify include aluminum, calcium, boron, and carbon. 2 If the silicon oxide film 20 is formed by a vapor phase film formation method such as sputtering using a target, the incorporation of these impurity elements can be sufficiently suppressed compared to when the film is formed by a liquid phase film formation method such as sol-gel, and the problem of etching inhibition in the chemical etching process does not occur.

[0076] Furthermore, optical substrates used in cover glasses, lenses, etc. may contain metals other than Si (e.g., Al, Ca) for purposes such as lowering the softening point or adjusting the refractive index. Therefore, if an attempt is made to form a concave-convex structure directly on the surface of an optical element by etching the surface of the optical substrate, the above-mentioned problems may arise in the chemical etching step of step C-2, which may result in a long time required to form the concave-convex structure or may make it impossible to form a concave-convex structure of sufficient depth. In the manufacturing method of the present optical element 1, a silicon oxide film 20 is formed on the optical substrate 10, so there is no problem even if impurity elements are mixed into the optical substrate 10, and the method can be applied regardless of the material of the optical substrate 10.

[0077] In addition, an optical element having a silicon oxide film 20 on an optical substrate 10, a microrelief structure 22 on the surface of the silicon oxide film 20, and no water-repellent film 30, exhibits superhydrophilic properties on the surface of the microrelief structure 22. In the case of an optical element having a superhydrophilic microrelief structure 22, water spreads on the surface, suppressing adhesion of water to the surface, thereby preventing adhesion of raindrops and the like. However, in a camera equipped with an optical element having such a superhydrophilic film as a lens filter, when water spreads on the lens filter during shooting, it does not dry uniformly, resulting in wet and dry areas, which can degrade the image. By providing a water-repellent film 30, as in the optical element 1, it is possible to repel raindrops and the like, thereby preventing contamination compared to when water spreads. Even when used as a camera lens filter, it does not cause the above-mentioned image degradation, making it highly practical.

[0078] Samples of examples and comparative examples of optical members were prepared and various tests were carried out to verify the optical members of the present disclosure. The results will be described below.

[0079] In preparing the samples used in each test, an RF magnetron sputtering device BMS-800II (Shinron Co., Ltd.) was used as the film deposition device. The film deposition conditions for each film will be described later.

[0080] The properties of each sample were measured by the following methods.

[0081] (Reflectance) The reflectance was measured using a microspectrophotometer (USPM-PU: Olympus Optical Co., Ltd.) The reflectance for each wavelength was measured when the incident angle on the optical member was 0° (vertical incidence).

[0082] (Contact Angle of Water) The contact angle of water was measured using a contact angle meter (DM300: Kyowa Interface Science Co., Ltd.) Here, the static contact angle was measured using a water droplet of 2 μL.

[0083] (Water Sliding Angle) A method for measuring the water sliding angle will be described with reference to FIG. 7 . An optical element 1 is placed on a flat stage (not shown), and a 5 μL water droplet 50 is dropped onto the surface 1a (surface of the water-repellent film) of the optical element 1. In this state, the stage is gradually tilted at a rate of 0.2° / second to gradually lift one end of the optical element 1 (the left side in the figure) and tilt the optical element 1. The tilt angle is indicated by θ in FIG. 7 . The tilt angle θ is gradually increased, and the angle at which the end 50e of the water droplet 50 begins to move is taken as the sliding angle. Image 52 in FIG. 8 is an image of the water droplet 50 on the optical element 1 when the stage plane is horizontal, i.e., when the tilt angle θ = 0°. Image 54 in FIG. 8 is an image of the water droplet 50 on the optical element 1 when the stage plane is tilted at a tilt angle θ = 3.4°. Here, the optical element 1 is tilted so that the right side of the page in FIG. 8 is downward and the left side is upward. As shown by the dashed line, there is a discrepancy between the position of the water droplet 50 at θ = 0° and the position of the water droplet 50 at θ = 3.4°. The change in position of the right side of the water droplet 50, i.e., the downwardly tilted end, was measured. Figure 9 shows an example of measuring the relationship between the stage tilt angle [°] and the position of the end 50e of the water droplet 50 (droplet position). As shown in Figure 9, the angle at which the droplet position changed significantly was defined as the sliding angle. In the example shown in Figure 9, the sliding angle changed significantly between the tilt angle of 3.4° where the significant change occurred and the tilt angle of 3.0° immediately preceding that change, so the angle 3.2°, midway between those measurement points, was defined as the sliding angle. Note that the sliding angle was measured 10 times for each optical element, and the average of the 10 measurements was defined as the sliding angle of that optical element.

[0084] (Adhesion Energy) The adhesion energy was calculated from the sliding angle of the water using the following formula (1). As shown in FIG. 7 , assuming that the surface 1a of the optical element 1 is flat and the contact surface of the water droplet 50 in contact with the surface 1a of the optical element is circular, the radius of the contact surface is r. The sliding angle obtained by the above procedure is α. The component of gravity acting downward on the slope on the water droplet 50 at the moment of sliding is expressed as mg sin α = Vρg sin α, where m is the weight of the water droplet 50, V is the volume of the water droplet 50, and ρ is the density of the water droplet 50. If the adhesion energy of the surface 1a of the optical element 1 is E, the force with which the surface 1a of the optical element 1 supports the water droplet 50 is 2πrE. At the moment the droplet slides down, this component of gravity and the force supporting the water droplet are balanced. That is, there is the relationship Vρg sin α = 2πrE. Therefore, the adhesion energy E is expressed by formula (1). E=Vρg·sin α / 2πr (1) In this example, the adhesion energy E was calculated using the sliding angle α measured using a water droplet with a volume V of 5 μL. However, the sliding angle α is a value that changes depending on the volume V of the water droplet 50, and the adhesion energy E does not depend on the volume V of the water droplet 50.

[0085] (Haze) Haze was measured using a haze meter (NDH5000: Nippon Denshoku). Haze [%] = (amount of diffuse transmitted light / (amount of perpendicular transmitted light+amount of diffuse transmitted light)) × 100. A larger haze means a larger amount of diffuse transmitted light.

[0086] (Average Height of Concave and Convex Surfaces) The average height of the concave and convex surfaces is the average height from the bottom of the concave portions to the top of the convex portions of the fine concave and convex surface structure formed on the surface of a silicon oxide film. This was calculated as follows. This will be explained with reference to FIG. 10 . First, a cross section of the optical component was imaged at 50,000 times magnification using a scanning electron microscope (SEM) to obtain an SEM image (213 × 320 pixels) (S1). This corresponds to an area of ​​1.7 μm in height and 2.56 μm in width. In FIG. 10 , the vertical and horizontal axes in each image indicate the number of pixels. The SEM image was binarized to detect the edges of the concave and convex surface structure (S2), a fill process was performed to fill in the concave and convex surfaces (S3), noise was removed (S4), and the boundary between the air on the concave and convex surface and the concave and convex surfaces was determined (S5). Through these steps S1 to S5, for example, the boundary line of the concave and convex surfaces, with the deepest position being zero in height, as shown in FIG. 11 , was obtained. As shown in Fig. 11, the height of the irregularities was random, with the apex of the maximum convexity being approximately 310 nm, but when the irregularity heights were integrated and averaged, the average height of the irregularities in the example shown in Fig. 11 was 168 nm, as indicated by the dashed line. Note that Fig. 11 shows data for Sample 1-4 of Test 1, which will be described later.

[0087] (Average Period of Irregularities) The average period was calculated by obtaining the spatial frequency spectrum, determining the spatial frequency value at which the maximum intensity was obtained, and then calculating the period from this spatial frequency value. Specifically, a SEM image (see FIG. 12A) of the planar micro-irregularity structure was obtained at a magnification of 10,000 times using a scanning electron microscope, and a 1000 x 680 pixel range was cut out from the SEM image and subjected to a two-dimensional Fourier transform. In the image of FIG. 12A, one pixel corresponds to 10 nm. The squared intensity spectrum of the obtained two-dimensional spatial frequency was integrated in the azimuthal direction, and the spectral intensity corresponding to the magnitude of the spatial frequency was calculated to calculate the relationship between the one-dimensional spatial frequency and the spectral intensity. Then, the spatial frequency value at which the maximum intensity (peak) was obtained was determined by fitting the vicinity of the vertex with a Gaussian function (see FIG. 12B). For example, if the spatial frequency value showing the maximum intensity was 5 μm, -1 , the period [μm] is 1 / 5=0.2 and the average period is 200 nm.

[0088] "Test 1" Samples 1-1 to 1-10 of optical components were prepared, each having a silicon oxide film on an optical substrate, a fine uneven structure on the surface of the silicon oxide film, and a water-repellent film on the fine uneven structure, and various evaluations were performed.

[0089] (Sample Preparation Method) Samples 1-1 to 1-10 were prepared as follows. A white plate substrate (B270i: manufactured by SCHOTT) with a diameter of 80 mm and a thickness of 2.5 mm was used as the optical substrate. A silicon oxide film of 1000 nm was formed on this white plate substrate by sputtering, and an aluminum film of 10 nm was further formed by sputtering. Next, the white plate substrate on which the silicon oxide film and aluminum film were laminated was subjected to a hot water treatment in which it was immersed in hot water at 100°C for 3 minutes. This converted the aluminum film into a fine concave-convex layer made of alumina hydrate.

[0090] To form a silicon oxide film, SiO 2 The sputtering conditions were as follows:

[0091] -Sputtering conditions for silicon oxide film- Target input power: 500 W Vacuum degree: 0.2 Pa, Ar / O 2 Mixed atmosphere (O 2 Flow rate: 200 sccm) No substrate heating

[0092] -Sputtering conditions for aluminum film- Target input power: 600 W Vacuum degree: 0.2 Pa, Ar atmosphere (Ar flow rate: 200 sccm) No substrate heating

[0093] Thereafter, an etching process was carried out using the fine concave-convex layer as a mask. First, physical etching was carried out, followed by chemical etching. The concave portions of the fine concave-convex layer were penetrated by physical etching to expose the silicon oxide film. Then, the silicon oxide film exposed in the concave portions of the fine concave-convex layer was etched by chemical etching. The conditions for physical etching and chemical etching were as follows:

[0094] Physical Etching Conditions: ICP (Inductively Coupled Plasma) power: 300 W, bias power: 120 W, etching pressure: 3 Pa, etching gas: Ar (100 sccm), CHF 3 (10 sccm) Substrate temperature: 10° C. Etching time: 45 sec.

[0095] Chemical Etching Conditions: ICP power: 500 W, bias power: 15 W, etching pressure: 0.6 Pa, etching gas: SF 6 (40sccm), CHF 3 (40 sccm) Substrate temperature: 10° C. Etching time: 5 minutes to 70 minutes (varies depending on the sample). The etching times for each of Samples 1-1 to 1-10 are shown in Table 1 below.

[0096] A water-repellent film was formed by dip-coating a fluorine coating (product surface Fluorosurf NL-1, manufactured by Fluoro Technology Co., Ltd.) on the uneven structure formed on the surface of the silicon oxide film by etching.

[0097] For Samples 1-1 to 1-10 prepared as described above, the calculated adhesion energy and the evaluation results of the water sliding property on the surface of each sample are shown in Table 1.

[0098] (Evaluation of Water Slippage) The method for evaluating water slippage is described below. First, the number of remaining water droplets was measured using the following procedure: 1) Pure water was poured into an empty spray bottle of a commercially available Fujifilm Hydro Ag alcohol spray. 2) As shown in FIG. 13A, sample S (samples 1-1 to 1-10) was held vertically using a jig (not shown), and the spray bottle 56 was positioned so that the distance from the surface of sample S to the center of the bottom of the spray bottle 56 was 150 mm. 3) In this state, the spray lever was pressed three times to spray pure water onto the surface of sample S. 4) After that, sample S was placed horizontally, and the number of water droplets remaining on the surface was counted. The surface of sample S was observed using a stereomicroscope at 5x magnification. As shown in FIG. 13B , a 40 × 40 mm area centered on the center O of the sample S was divided into four parts, and the water droplets were counted in each of the following areas: a 20 × 20 mm area in the first quadrant, a 20 × 20 mm area in the second quadrant, a 20 × 20 mm area in the third quadrant, and a 20 × 20 mm area in the fourth quadrant. The average number of water droplets in the four areas was taken as the number of residual water droplets.

[0099] The number of remaining water droplets was evaluated for each of Samples 1-1 to 1-10 according to the following criteria. The evaluation results for water sliding are shown in Table 1. A: 2 or less remaining water droplets B: 3 to 5 remaining water droplets C: 6 to 10 remaining water droplets D: More than 10 remaining water droplets

[0100]

[0101] Samples 1-2 to 1-9, which satisfied the adhesion energy of 0.2 mN / m to 6 mN / m, achieved a sliding property rating of C or higher. Conversely, Samples 1-1 and 1-10, which did not satisfy the adhesion energy of 0.2 mN / m to 6 mN / m, achieved a sliding property rating of D. Samples 1-2 to 1-9 correspond to examples of the optical member of the present disclosure, and Samples 1-1 and 1-10 correspond to comparative examples. Good sliding property was achieved when the adhesion energy was 5.62 mN / m or less, even better sliding property was achieved when the adhesion energy was 2.85 mN / m or less, and very good sliding property was achieved when the adhesion energy was 0.29 mN / m to 1.29 mN / m.

[0102] Figure 14 shows the etching time dependence of adhesion energy based on Table 1. In Test 1, the chemical etching time required to achieve good sliding properties was 10 to 60 minutes. Furthermore, by setting the chemical etching time to 15 to 50 minutes, better sliding properties were obtained, and by setting it to 30 to 45 minutes, very good sliding properties were obtained. In Figure 14, the range indicated by the double arrows is the range in which good sliding properties were obtained. If the etching time is less than 5 minutes, it is thought that etching is insufficient and the uneven structure is not sufficiently formed, and if it exceeds 60 minutes, it is thought that etching proceeds too far and the uneven structure that was once formed is destroyed.

[0103] Here, for Samples 1-1 to 1-7, the water contact angle β, water sliding angle α, reflectance R, and haze H were evaluated. The evaluation criteria are shown in Table 2, and the evaluation results are shown in Table 3. Table 3 also shows the evaluation of sliding properties and adhesion energy shown in Table 1.

[0104]

[0105] The evaluation criteria shown in Table 2 were the same for Test 2 and onwards.

[0106]

[0107] As shown in Table 3, the evaluation of water sliding property and the evaluation of water sliding angle were consistent. In the adhesion energy range of 0.29 mN / m to 1.29 mN / m, all evaluations were B or higher.

[0108] "Test 2" Samples 2-1 to 2-7 of optical members having a microrelief structure on the surface of an optical substrate and a water-repellent film on the microrelief structure were prepared and subjected to various evaluations. Samples 2-1 to 2-7 are all comparative examples of the optical member of the present disclosure in that they do not have a silicon oxide film.

[0109] (Sample Preparation Method) Samples 2-1 to 2-7 were prepared as follows. A white plate substrate (B270i: manufactured by SCHOTT) with a diameter of 80 mm and a thickness of 2.5 mm was used as the optical substrate. An aluminum film was formed to a thickness of 10 nm on this white plate substrate by sputtering. Next, the white plate substrate on which the aluminum film was laminated was subjected to a hot water treatment in which it was immersed in hot water at 100°C for 3 minutes. This converted the aluminum film into a fine concave-convex layer made of alumina hydrate.

[0110] An Al target was used to form the aluminum film, and the sputtering conditions were the same as in Test 1.

[0111] Thereafter, an etching process was carried out using the fine concave-convex layer as a mask. First, physical etching was carried out, followed by chemical etching. The concave portions of the fine concave-convex layer were penetrated by physical etching to expose the surface of the white board substrate. Then, the white board substrate exposed in the concave portions of the fine concave-convex layer was etched by chemical etching. The physical etching and chemical etching conditions were the same as in Test 1. The chemical etching time varied depending on the sample, ranging from 5 to 45 minutes. The chemical etching time for each sample is shown in Table 4.

[0112] The uneven structure formed on the surface of the white board substrate by etching was dip-coated with a fluorine coating (product surface Fluorosurf NL-1: manufactured by Fluoro Technology Co., Ltd.) to form a water-repellent film.

[0113] For Samples 2-1 to 2-7 prepared as described above, the water contact angle β, water sliding angle α, reflectance R, and haze H were evaluated according to the evaluation criteria shown in Table 2. Table 4 shows the evaluation results.

[0114]

[0115] All of Samples 2-1 to 2-7 showed low sliding properties. Surface analysis of the samples (photoelectron spectroscopy: XPS) detected Al and F on the surface. The results of this surface analysis indicate that Al in the white board substrate reacted with the etching gas to form AlF, which has a low vapor pressure. 3 It is presumed that this formed a residue on the surface and inhibited etching.

[0116] "Test 3" The composition dependency of the SiOx film on the etching distribution was investigated.

[0117] (Sample Preparation Method) A white plate substrate (B270i: manufactured by SCHOTT) having a diameter of 80 mm and a thickness of 2.5 mm was used as the optical substrate. A silicon oxide film (SiO x A 1000 nm thick silicon oxide film was formed on the white plate, and then a 10 nm thick aluminum film was formed by sputtering. The conditions for forming the silicon oxide film will be described later. The conditions for forming the aluminum film were the same as those in Test 1. Next, the white plate substrate on which the silicon oxide film and aluminum film were laminated was subjected to a hot water treatment by immersing it in hot water at 100°C for 3 minutes. This converted the aluminum film into a fine concave-convex layer made of alumina hydrate.

[0118] Thereafter, an etching process was carried out using the fine concave-convex layer as a mask. First, physical etching was carried out, followed by chemical etching. The concave portions of the fine concave-convex layer were penetrated by physical etching to expose the silicon oxide film. Then, the silicon oxide film exposed in the concave portions of the fine concave-convex layer was etched by chemical etching. The physical etching and chemical etching conditions were the same as those in Test 1, except that the chemical etching time for all samples was 30 minutes.

[0119] A water-repellent film was formed by dip-coating a fluorine coating (product surface Fluorosurf NL-1, manufactured by Fluoro Technology Co., Ltd.) on the uneven structure formed on the surface of the silicon oxide film by etching.

[0120] - Deposition of silicon oxide film - To deposit a silicon oxide film, SiO 2 Using a target, the target input power and oxygen gas O 2 By changing the flow rate, samples with SiOx films with different x were fabricated. The composition ratio x, target input power, and oxygen gas flow rate are shown in Table 5. The other conditions were the same as in Test 1.

[0121]

[0122] The composition ratio x was measured using a Rutherford Backscattering Spectroscopy (RBS) device manufactured by NEC Corporation (device body: 3SDH-R10, accelerator: 3SDH Pelletron) and data analysis software RBS-400 manufactured by CE&A.

[0123] The contact angle distribution within the substrate surface was measured for each sample. The center of the 80 mm diameter sample was used as the origin, and water contact angles were measured at 5 mm intervals on two orthogonal axes, the X axis and the Y axis. The measurement results are shown in Table 6. (1) indicates the water contact angle [°] at each position X on the X axis for each sample, and (2) indicates the water contact angle [°] at each position Y on the Y axis for each sample.

[0124]

[0125] In this example, the contact angle distribution had approximately the same symmetry in the X-axis and Y-axis directions. Figure 15 shows the relationship between position on the X-axis and contact angle. As shown in Figure 15, the contact angle decreases as you move outward from the center (position 0) of the substrate. In the range of 1.9≦x≦2.0, the difference in contact angle between the center position 0 and the ±35 mm positions can be approximately 10% of the contact angle at the center position 0 mm. In other words, if the range is 1.95≦x≦2.0, the difference in contact angle between the inside and outside can be made smaller, which is preferable.

[0126] It is a known phenomenon that the etching amount differs between the center and the edge of a substrate during vapor-phase etching. This phenomenon is thought to be caused by the fact that the distribution of plasma, in which the etching gas is separated into electrons and ions, is not uniform on the substrate but concentrates around the edges, resulting in a greater etching amount at the edges than at the center.

[0127] Furthermore, from the results in Table 6, SiO x It was revealed that the difference in the amount of etching between the center and edge of the substrate changes depending on the composition ratio x. When the oxygen composition in the silicon oxide film becomes small, the Si concentration becomes relatively large. The etching gas SF used in chemical etching 6 +CH 3The etching rate of F is Si>SiO x The silicon-rich film is more easily etched. This tendency, combined with the phenomenon that plasma tends to concentrate around the substrate, causes the etching amount distribution within the substrate surface to become smaller than that of SiO x It is thought that this varies depending on the composition ratio x.

[0128] For each sample, the height of the irregularities was measured at three locations on the X axis: the center of the substrate, the intermediate portion (half portion) between the center and the edge, and the edge of the substrate. The results are shown in Table 7. In Table 7, the irregularity height is shown as a value normalized by setting the highest irregularity height (the irregularity height at the center of the substrate of the sample with composition ratio x = 2) to 1.

[0129]

[0130] As shown in Table 7, the difference in unevenness height between the center and edge of the substrate, i.e., the difference in etching amount, becomes significant when the composition ratio x is 1.8 or less. Since there is a correlation between the in-plane distribution of unevenness height and the in-plane distribution of contact angle shown in Table 6, it is thought that the in-plane distribution of unevenness height is a factor in the in-plane distribution of contact angle.

[0131] "Test 4" In Test 2, a white board substrate (B270i: manufactured by SCHOTT) was used as the optical substrate, and when an attempt was made to form a fine uneven structure by etching its surface, the etching was inhibited and the uneven structure could not be formed. In Test 4, when a silicon oxide film was formed on the optical substrate, a sample to which impurities were added was prepared, and an experiment was conducted to determine the impurity concentration at which etching was not inhibited.

[0132] SF, an etching gas 6 The elements that can react with the silicon dioxide film to form a compound are boron (B), calcium (Ca), aluminum (Al), and carbon (C). Therefore, these elements (hereinafter collectively referred to as impurity elements) were investigated. When forming a silicon dioxide film, an optical glass piece containing any of Al, Ca, and B, or a custom-made carbon piece, was added to the SiO 2 A silicon oxide film containing an impurity element was produced by depositing the silicon oxide film on a target.

[0133] The concentration of impurity elements is SiO 2 The area of ​​the optical glass piece or carbon piece placed on the target was adjusted to change the thickness. The thickness of the optical glass piece and the carbon piece was 1 mm. Figure 16A shows a 6-inch SiO 2 15A is a schematic plan view of the target 60. As shown in FIG. 2 The area of ​​the target 60 is divided into 16 equal parts, and SiO 2 An optical glass piece 62 or a carbon piece is placed on the target 60 so that its area is SiO 2 The target 60 was placed at 1 / 16, 2 / 16, ..., n / 16 of the target 60. Figure 16B shows two optical glass pieces 62 placed on SiO 2 FIG. 10 is a schematic diagram showing the state where the target 60 is placed on the substrate.

[0134] (Sample Preparation Method) A white plate substrate having a diameter of 80 mm and a thickness of 2.5 mm was used as the optical substrate. A silicon oxide film was formed on the white plate substrate by sputtering to a thickness of 1000 nm, and an aluminum film was further formed by sputtering to a thickness of 10 nm. When forming the silicon oxide film, the optical glass piece 62 or the carbon piece was used as described above. 2 A plurality of samples with different impurity concentrations were prepared by placing them on the target 60. A hot water treatment was carried out under the same conditions as in Test 1, and an etching treatment was carried out under the same conditions as in Test 1. Finally, as in Test 1, a fluorine coating (product surface Fluorosurf NL-1: manufactured by Fluoro Technology Co., Ltd.) was dip coated onto the uneven structure formed on the surface of the white board substrate to form a water-repellent film.

[0135] The optical glass pieces 62 used were B270i (manufactured by SCHOTT), H-ZF52 (manufactured by Chengdu Guangming), or S-LHA58 (manufactured by Ohara). B270i contains Al, H-ZF52 contains Ca, and S-LHA58 contains B. Table 8 shows the area ratio of the pieces, the optical glass type, the impurity elements, and the impurity concentrations [wt%] for each sample. Each sample was subjected to composition analysis by XPS after the silicon oxide film was formed but before etching to determine the impurity concentrations.

[0136] (Evaluation) The etching state of each sample was evaluated. The etching state was evaluated based on the water contact angle measured at the center of the substrate. This is because a good etching state is considered to have high water repellency. In this example, the evaluation was performed using the following evaluation criteria: A: Contact angle of 140° or more B: Contact angle of 120° or more but less than 140° C: Contact angle of less than 120°

[0137] The evaluation results are shown in Table 8.

[0138]

[0139] As shown in Table 8, when the impurity contained in the silicon oxide film is aluminum, the impurity content is preferably 0.25 wt% or less, more preferably 0.10 wt% or less. When the impurity contained in the silicon oxide film is calcium, the impurity content is preferably 2.00 wt% or less, more preferably 1.00 wt% or less. When the impurity contained in the silicon oxide film is boron, the impurity content is preferably 2.00 wt% or less, more preferably 1.00 wt% or less. When the impurity contained in the silicon oxide film is carbon, the impurity content is preferably 6.0 wt% or less, more preferably 4.0 wt% or less.

[0140] When a fine uneven structure is formed directly on the surface of an optical substrate, as described above, the etching process may be hindered by the influence of elements contained in the optical substrate that bond with fluorine. In contrast, a silicon oxide film is formed on the optical substrate by vapor-phase deposition, which can suppress the inclusion of impurities, and a fine uneven structure is formed on the surface. Therefore, even if the optical substrate contains elements that bond with fluorine as components, the problem of the etching process being hindered does not occur, and various optical substrates can be used regardless of type.

[0141] "Test 5" A group of samples was prepared by changing the average height and average period of the uneven structure by changing the chemical etching conditions in the sample preparation method of Test 1, and the reflectance R, haze H, and water sliding property were evaluated. The results are shown in Table 9.

[0142] From the results in Table 9, the average height and average period of the irregularities can be in the range of 100 nm to 600 nm, and the average period can be in the range of 100 nm to 450 nm, depending on the combination of the two. The average height is preferably 150 nm to 600 nm, more preferably 150 nm to 450 nm, and particularly preferably 200 nm to 350 nm. The average period is preferably 150 nm to 450 nm, more preferably 150 nm to 400 nm, and particularly preferably 150 nm to 350 nm. As a combination, when the average height is 100 nm to 150 nm, the average period is preferably 300 nm to 450 nm. When the average height is 150 nm to 200 nm, the average period can be in the range of 100 nm to 450 nm, preferably 100 nm to 350 nm, and more preferably 100 nm to 200 nm. When the average height is 200 nm to 500 nm, the average period can be 100 nm to 450 nm, preferably 100 nm to 350 nm. An average height of 200 nm to 350 nm and an average period of 100 nm to 350 nm are particularly preferred. When the average height is 500 nm to 600 nm, the average period is preferably 100 nm to 350 nm, more preferably 100 nm to 200 nm.

[0143] "Test 6" The inventors discovered that in the manufacturing process of the optical member of the present disclosure, when a silicon oxide film having an uneven surface is formed on a flat optical substrate, the quality of the transmitted wavefront (contour interval) varies depending on the etching process conditions. In Test 6, the transmitted wavefront aberration required to obtain a good image was investigated.

[0144] Samples 6-1 to 6-4 were prepared by changing the time ratio of the physical etching time to the chemical etching time in the sample preparation method of Test 1. Samples 6-1 to 6-4 were prepared under other conditions in accordance with the sample preparation method of Test 1. Table 10 shows the physical etching time t1, chemical etching time t2, and the etching time ratio (t1 / t2) × 100 for each of Samples 6-1 to 6-4.

[0145] Each sample was evaluated for transmitted wavefront aberration, image evaluation, and water repellency, and the results are shown in Table 10. The evaluation methods were as follows.

[0146] (Method for measuring transmitted wavefront aberration) The transmitted wavefront aberration was measured using a laser interferometer (Fujifilm F601). The measurement light had a wavelength λ of 633 nm. The measurement was performed by irradiating the measurement light onto the surface of the optical element having the concave-convex structure. Table 10 also shows the PV value as the transmitted wavefront aberration. Figures 17A to 17D show images of the surface of the optical element when measuring the transmitted wavefront aberration for each of Samples 6-1 to 6-4. The part indicated by the black circle in the center is the optical element.

[0147] (Image Evaluation Method) Samples 6-1 to 6-4 were each attached as a lens filter to a general-purpose portable TV camera (body: Sony HDC-4300, lens: Fujinon UA18x7.6BERD), a subject was photographed, and the photographed image was displayed on a monitor. The photographed images were sensorily evaluated according to the following evaluation criteria. A: The subject was clearly recognizable. B: The photographed image was displayed, but the subject could not be distinguished. C: No photographed image was obtained.

[0148] (Evaluation of Water Slippage Property) For Samples 6-1 to 6-4, the water slippage property was evaluated in the same manner as in Test 1.

[0149]

[0150] As shown in Table 10, the transmitted wavefront aberration is preferably λ / 5 or less, and more preferably λ / 5 to λ / 8.

[0151] 18 shows the relationship between the physical etching time t1 and the wavefront aberration PV value. The dashed line represents the fitting curve y=0.0582e 0.0283x and R 2 The value is R 2 18, the wavefront aberration PV value tends to increase as the physical etching time t1 increases.

[0152] Sample 6-4, which showed poor results in the image evaluation and the slippage evaluation, was analyzed.

[0153] For SEM observation, a sample for SEM observation was prepared after physical etching and before chemical etching using the same manufacturing method as Sample 6-4, and cross-sectional SEM images were taken. As a result, there were areas where the recesses in the mask (alumina hydrate uneven structure layer) had penetrated and etched the underlying silicon oxide film, and areas where the uneven structure of the mask had been destroyed and disappeared.

[0154] For elemental analysis, analytical samples were prepared by the same manufacturing method as Samples 6-1 to 6-4, up to the chemical etching process, and then subjected to X-ray fluorescence analysis. As a result, the Ar concentration (wt%) in the silicon oxide film of Sample 6-4 was approximately 15 times higher than that of Samples 6-1 to 6-3.

[0155] Generally, the transmitted wavefront aberration correlates with the deformation of the substrate. During physical etching using Ar, accelerated Ar gets mixed into the silicon oxide film and distorts the SiO 2 The Si-O-Si network of the film is distorted, resulting in SiO 2 It is presumed that the film stress increased, the high stress deformed the substrate, and the transmitted wavefront deteriorated (the transmitted wavefront aberration increased).

[0156] Based on the above analysis results and the relationship between the physical etching time t1 and the wavefront aberration PV value shown in Figure 17, the physical etching time t1 is preferably 60 seconds or less, and more preferably 45 seconds or less. To improve water repellency, the physical etching time t1 is preferably 30 seconds or more. The etching time ratio (t1 / t2) x 100 of the physical etching time t1 to the chemical etching time t2 is preferably 2.22 or less, and more preferably 1.67 or less. The etching time ratio (t1 / t2) x 100 is particularly preferably 1.11 to 1.67.

[0157] "Test 7" As a constituent material of the water-repellent film, fluorine compounds, which are particularly preferable from the viewpoint of durability, were investigated.

[0158] (Sample Preparation Method) The same sample preparation method as in Test 3 was used, except that the silicon oxide film was replaced with SiO xThe etching process was carried out with x=2. In the process of forming the water-repellent film, different fluorine compounds were dip-coated to prepare samples 7-1 to 7-4. Sample 7-1 was made of -(OCF 2 CF 2 ) n Fluorine compounds containing - as functional groups. Sample 7-2 is -(OCF 2 CF 2 ) n Fluorine compounds containing - as functional groups. Sample 7-3 is -(OCF 2 ) m (OCF 2 CF 2 ) n Fluorine compounds containing - as functional groups. Sample 7-4 is -(OCF 2 ) m (OCF 2 CF 2 ) n Fluorine compounds containing - as a functional group were used.

[0159] Each sample was continuously irradiated with light from a 150 W xenon lamp (Super Bright 152S, manufactured by Kenko Tokina Co., Ltd.), and the water contact angle was measured periodically. The light-emitting surface of the xenon lamp and the surface of the sample were placed opposite each other, with a distance of 10 mm between them.

[0160] The number of days until the contact angle decreased to 3% and 5% of the initial value is summarized in Table 11. Four samples were prepared for each type. The contact angles and number of days in Table 11 are averages of the four samples.

[0161]

[0162] In Table 11, "not confirmed" means that the value did not decrease by 5% even after 150 days. In the table, n and m are both integers of 1 or more.

[0163] As shown in Table 11, the fluorine compound is -(OCF 2 CF 2 ) n - group, n is an integer of 1 or more, and -(OCF 2 ) mSamples 7-1 and 7-2, which do not contain the - group and m is an integer of 1 or more, took a very long time for the contact angle to decrease to 5% from the initial value, and were highly durable.

[0164] "Test 8" The effect of providing an intermediate layer between the optical substrate and the silicon oxide film was examined.

[0165] (Sample Preparation Method) ((Sample 8-1A)) Sample 8-1A was prepared as follows. A white board substrate (FDS90: manufactured by SCHOTT) with a diameter of 80 mm and a thickness of 2.5 mm was used as the optical substrate. FDS90 has a refractive index n of 1.839 for light with a wavelength of 633 nm. An intermediate layer was formed on this white board substrate by sputtering. Then, a silicon oxide film with a thickness of 1000 nm was formed on the intermediate layer by sputtering, and an aluminum film with a thickness of 10 nm was further formed by sputtering. Next, the white board substrate with the silicon oxide film and aluminum film laminated thereon was subjected to a hot water treatment in which it was immersed in hot water at 100°C for 3 minutes. This converted the aluminum film into a finely textured layer composed of alumina hydrate. The film formation conditions for the silicon oxide film and the aluminum film were the same as those for the sample preparation method of Test 1.

[0166] Thereafter, an etching treatment was carried out using the fine concave-convex layer as a mask under the same physical and chemical etching conditions as in the sample preparation method of Test 1, except that the chemical etching time was 45 minutes.

[0167] Furthermore, a water-repellent film was formed on the uneven structure formed on the surface of the silicon oxide film in the same manner as in Test 1.

[0168] The intermediate layer is a single-layer silicon oxynitride film (SiO x N y )

[0169] ((Sample 8-1B)) Sample 8-1B was produced, which had the same configuration as Sample 8-1A, but did not include an intermediate layer. Sample 8-1B was produced using the same production method as Sample 8-1A, except that the process of forming an intermediate layer was omitted and a silicon oxide film was formed directly on the surface of the white plate substrate.

[0170] ((Sample 8-2A)) A white board substrate (H-ZLAF90: manufactured by SCHOTT) with a diameter of 80 mm and a thickness of 2.5 mm was used as the optical substrate. H-ZLAF90 has a refractive index n of 1.9928 for light with a wavelength of 633 nm. As the intermediate layer, a multilayer film with a five-layer structure was formed by alternately laminating a dielectric film with a low refractive index and a dielectric film with a high refractive index. Sample 8-2A was produced by the same production method as Sample 8-1A, except that the type of optical substrate was changed, the intermediate layer was a multilayer film, and the chemical etching time was set to 30 minutes.

[0171] The intermediate layer is a silicon oxynitride film (SiO x N y ) as a high refractive index dielectric film, and niobium oxide (Nb 2 O 5-x The refractive index and film thickness of each film are as shown in Table 12 below. In Table 12, the intermediate layer closest to the silicon oxide film is shown as the first layer, and the intermediate layer closest to the substrate is shown as the fifth layer.

[0172]

[0173] ((Sample 8-2B)) Sample 8-2B was produced, which had the same configuration as Sample 8-2A, but did not include an intermediate layer. Sample 8-2B was produced using the same production method as Sample 8-2A, except that the process of forming an intermediate layer was omitted and a silicon oxide film was formed directly on the surface of the white plate substrate.

[0174] ((Sample 8-3A)) A white board substrate (BaFD7: manufactured by SCHOTT) with a diameter of 80 mm and a thickness of 2.5 mm was used as the optical substrate. BaFD7 has a refractive index n of 1.698 for light with a wavelength of 633 nm. As the intermediate layer, a multilayer film with a three-layer structure was formed by alternately laminating a dielectric film with a low refractive index and a dielectric film with a high refractive index. Sample 8-3A was produced by the same production method as Sample 8-1A, except that the type of optical substrate was changed, the intermediate layer was a multilayer film, and the chemical etching time was set to 50 minutes.

[0175] The intermediate layer is a silicon oxynitride film (SiO x N y ) as a high refractive index dielectric film, and niobium oxide (Nb 2 O 5-x The refractive index and film thickness of each film are as shown in Table 13 below. In Table 13, the intermediate layer closest to the silicon oxide film is shown as the first layer, and the intermediate layer closest to the substrate is shown as the third layer.

[0176]

[0177] ((Sample 8-3B)) Sample 8-3B was produced, which had the same structure as Sample 8-3A, but did not include an intermediate layer. Sample 8-3B was produced by the same production method as Sample 8-3A, except that the step of forming an intermediate layer was omitted and a silicon oxide film was formed directly on the surface of the white plate substrate.

[0178] The wavelength dependence of reflectance was measured for Samples 8-1A and 8-1B and the results are shown in Figure 19. In Figure 19, the solid line shows the wavelength dependence of reflectance for Sample 8-1A with an intermediate layer, and the dashed line shows the wavelength dependence of reflectance for Sample 8-1B without an intermediate layer.

[0179] The average reflectance in the wavelength range of 400 nm to 700 nm was 0.1% for Sample 8-1A and 1.83% for Sample 8-1B. It is believed that Sample 8-1A was able to reduce the difference in refractive index between the layers by providing an intermediate layer with a refractive index between the refractive index of the optical substrate and the refractive index of the silicon oxide film (n = 1.46), thereby reducing the reflectance.

[0180] The wavelength dependence of reflectance was measured for Samples 8-2A and 8-2B and the results are shown in Figure 20. In Figure 20, the solid line shows the wavelength dependence of reflectance for Sample 8-2A with an intermediate layer, and the dashed line shows the wavelength dependence of reflectance for Sample 8-2B without an intermediate layer.

[0181] The average reflectance in the wavelength range of 400 nm to 700 nm was 0.1% for Sample 8-2A and 2.8% for Sample 8-2B. Sample 8-2A has an intermediate layer made of a multilayer film between the optical substrate and the silicon oxide film, and it is thought that the intermediate layer caused interference between reflected light beams at the boundaries of each film, which contributed to the reduction in reflectance.

[0182] The wavelength dependence of reflectance was measured for Samples 8-3A and 8-3B and the results are shown in Figure 21. In Figure 21, the solid line shows the wavelength dependence of reflectance for Sample 8-3A with an intermediate layer, and the dashed line shows the wavelength dependence of reflectance for Sample 8-3B without an intermediate layer.

[0183] The average reflectance in the wavelength range of 400 nm to 700 nm was 0.1% for Sample 8-3A and 2.8% for Sample 8-3B. Sample 8-3A has an intermediate layer made of a multilayer film between the optical substrate and the silicon oxide film, and it is thought that the intermediate layer caused interference between reflected light beams at the boundaries of each film, which contributed to the reduction in reflectance.

[0184] Test 8 revealed that providing an intermediate layer has the effect of significantly reducing reflectance.

[0185] The following supplementary notes are further disclosed in relation to the above-described embodiments. (Supplementary Note 1) An optical member comprising an optical substrate having a smooth surface and a silicon oxide film provided on the optical substrate, wherein the silicon oxide film has a fine uneven structure on the surface thereof, and wherein a water-repellent film containing a fluorine compound is provided on the surface of the fine uneven structure, and wherein the adhesion energy of the surface of the water-repellent film is 0.2 mN / m to 6 mN / m. (Supplementary Note 2) The fluorine compound is -(OCF 2 CF 2 ) n - group, n is an integer of 1 or more, and -(OCF 2 ) mThe optical member according to Appendix 1, wherein the water-repellent film has a sliding angle of 10° or less when a 5 μL water droplet slides on the surface of the water-repellent film. (Appendix 4) The optical member according to any one of Appendix 1 to Appendix 3, wherein the silicon oxide film has an aluminum content of 0.25 wt. % or less, a calcium content of 2.0 wt. % or less, a boron content of 2.0 wt. % or less, and a carbon content of 6 wt. % or less. (Appendix 5) The optical member according to any one of Appendix 1 to Appendix 4, wherein the silicon oxide film is a sputtered film or a vapor-deposited film. (Appendix 6) The optical member according to any one of Appendix 1 to Appendix 5, wherein, when the composition of silicon oxide contained in the silicon oxide film is expressed as SiOx, 1.90≦x≦2.00. (Appendix 7) The optical element according to any one of Appendices 1 to 6, wherein the microrelief structure has an average height from the bottom of the recesses to the top of the protrusions of 150 nm to 600 nm and an average period of 150 nm to 450 nm. (Appendix 8) The optical element according to any one of Appendices 1 to 7, wherein the contact angle of water on the surface of the water-repellent film is 140° or more. (Appendix 9) The optical element according to any one of Appendices 1 to 8, wherein the haze is 2.5% or less. (Appendix 10) The optical element according to any one of Appendices 1 to 9, wherein the average reflectance when light having a wavelength of 400 nm to 700 nm is perpendicularly incident on the surface is 1% or less. (Appendix 11) The optical element according to any one of Appendices 1 to 10, wherein the transmitted wavefront aberration for light having a wavelength of λ nm is λ / 5 or less. (Appendix 12) The optical element according to any one of Appendices 1 to 11, further comprising an intermediate layer between the optical substrate and the silicon oxide film, the intermediate layer having a refractive index different from that of the silicon oxide film, for reducing the reflectance of incident light.(Appendix 13) A method for manufacturing an optical component, comprising: a film-forming step of forming a silicon oxide film on one surface of an optical substrate by a vapor phase film-forming method; a mask-forming step of forming an etching mask on the silicon oxide film; an etching step of etching the silicon oxide film through the etching mask by a vapor phase etching method to form a fine uneven structure on the surface of the silicon oxide film; and a coating step of forming a water-repellent film containing a fluorine compound on the surface of the fine uneven structure, wherein in the etching step, etching is carried out until the distance from the surface of the silicon oxide film facing the optical substrate to the apex of the maximum convexity of the fine uneven structure becomes smaller than the film thickness of the silicon oxide film immediately after deposition.

[0186] The disclosure of Japanese Patent Application No. 2023-054253, filed on March 29, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually indicated to be incorporated by reference.

[0187] REFERENCE SIGNS LIST 1, 2 Optical member 1a Surface of optical member 5 Water tank 6 Pure water 10 Optical substrate 12 Intermediate layer 12a High refractive index layer 12b Low refractive index layer 20 Silicon oxide film 22 Fine concave-convex structure 30 Water-repellent film 40 Concave-convex structure layer (mask) 42 Al-containing thin film 50 Water droplet 50e Edge of water droplet 52, 54 Image of water droplet 60 SiO 2 Target 62 Optical Glass Piece

Claims

1. An optical component comprising an optical substrate having a smooth surface and a silicon oxide film provided on the optical substrate, the silicon oxide film having a fine uneven structure on its surface, and a water-repellent film containing a fluorine compound on the surface of the fine uneven structure, the adhesion energy of the water-repellent film being 0.2 mN / m to 6 mN / m.

2. The fluorine compound is -(OCF 2 CF 2 ) n - group, n being an integer of 1 or more, and -(OCF 2 ) m 2. The optical member according to claim 1, which does not include a - group, where m is an integer of 1 or more.

3. The optical element according to claim 1, wherein the sliding angle of a 5 μL water droplet on the surface of the water-repellent film is 10° or less.

4. The optical member according to claim 1, wherein the silicon oxide film has an aluminum content of 0.25 wt. % or less, a calcium content of 2.0 wt. % or less, a boron content of 2.0 wt. % or less, and a carbon content of 6 wt. % or less.

5. The optical element according to any one of claims 1 to 4, wherein the silicon oxide film is a sputtered film or a vapor deposition film.

6. The optical member according to any one of claims 1 to 4, wherein, when the composition of silicon oxide contained in the silicon oxide film is expressed as SiOx, 1.90≦x≦2.

00.

7. The optical member according to any one of claims 1 to 4, wherein the average height from the bottom of the recesses to the top of the protrusions of the fine uneven structure is 150 nm to 600 nm, and the average period is 150 nm to 450 nm.

8. The optical member according to claim 1, wherein the contact angle of water on the surface of said water-repellent film is 140° or more.

9. The optical member according to any one of claims 1 to 4, having a haze of 2.5% or less.

10. The optical member according to any one of claims 1 to 4, which has an average reflectance of 1% or less when light having a wavelength of 400 nm to 700 nm is perpendicularly incident on the surface.

11. The optical member according to any one of claims 1 to 4, which has a transmission wavefront aberration of λ / 5 or less for light having a wavelength of λ nm.

12. An optical component according to any one of claims 1 to 4, comprising an intermediate layer between the optical substrate and the silicon oxide film, the intermediate layer having a refractive index different from that of the silicon oxide film, for reducing the reflectance of incident light.

13. A method for manufacturing an optical component, comprising: a deposition step of depositing a silicon oxide film on one surface of an optical substrate by a vapor deposition method; a mask formation step of forming an etching mask on the silicon oxide film; an etching step of etching the silicon oxide film through the etching mask by a vapor etching method to form a fine uneven structure on a surface of the silicon oxide film; and a coating step of forming a water-repellent film containing a fluorine compound on the surface of the fine uneven structure, wherein in the etching step, etching is performed until the distance from the surface of the silicon oxide film facing the optical substrate to the top of the maximum convexity of the fine uneven structure becomes smaller than the film thickness of the silicon oxide film immediately after deposition.

Citation Information

Patent Citations

  • Antireflection film

    JP1997288202A

  • Optical element and optical apparatus

    JP2007328191A

  • Optical element and optical apparatus

    JP2007328192A

  • Water-repelling and oil-repelling antifouling glass, process of production thereof and glass window, solar energy utilization device, and optical equipment using the glass

    JP2010222199A

  • Water-repellent antireflection structure

    JP2020038311A