Metallized film, production method for same, and film capacitor
By employing hydrocarbon oils with specific evaporation temperature ranges for masking and after-oil applications in the metallized film manufacturing process, the issues of defects and moisture absorption in film capacitors are addressed, resulting in reliable and environmentally friendly film capacitors with enhanced performance.
Patent Information
- Application Number
- PCT/JP2024/010098
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-03
AI Technical Summary
Existing metallized films face issues with defects such as unevenness and moisture absorption due to the use of fluorine and hydrocarbon-based masking oils, which affect the reliability and environmental sustainability of film capacitors.
The use of hydrocarbon oils with specific evaporation temperature ranges (10% evaporation temperature of 237°C or higher and 90% evaporation temperature of 337°C or lower) as masking or after-oils, ensuring stable adhesion and reduced moisture absorption, thereby improving the manufacturing process and performance of metallized films for film capacitors.
This approach minimizes defects and environmental impact, achieving reliable and cost-effective film capacitors with improved moisture resistance and dimensional accuracy, comparable to those using fluorine oils, while reducing the risk of metal deterioration.
Smart Images

Figure JP2024010098_03102024_PF_FP_ABST
Abstract
Description
Metallized film, its manufacturing method, and film capacitor
[0001] The present invention relates to a metallized film, a method for manufacturing the same, and a film capacitor using the metallized film.
[0002] When manufacturing a metallized film having a vapor deposition pattern consisting of vapor-deposited and non-vapor-deposited areas, the portions of the surface of the dielectric film that will become the non-vapor-deposited areas are masked in advance, and then metal is vapor-deposited to form the desired vapor deposition pattern on the surface of the dielectric film.
[0003] One masking method is the oil masking method, which uses oil as a masking material. Because metal does not deposit on areas where the masking oil is attached, a deposition pattern corresponding to the shape of the applied (attached) masking oil is formed on the surface of the dielectric film.
[0004] Incidentally, Patent Documents 1 and 2 use fluorinated oil (e.g., perfluoropolyether) as the masking oil. Fluorinated oil has good wettability to films, so defects caused by insufficient oil adhesion to areas to be masked (missing spots: defects in which metal is deposited in areas where metal should not be deposited) can be suppressed. Furthermore, fluorinated oil has high thermal stability and is less likely to decompose or otherwise change when heated, so evaporation is stable. This makes it less likely for oil to evaporate and scatter into unintended areas during metal deposition, masking areas where metal should be deposited (unevenness: defects in which metal is not deposited in areas where metal should be deposited, or the amount of deposition is extremely small).
[0005] However, fluorine oil is decomposed by the electron beam irradiated during metal deposition to improve adhesion between the dielectric film and the cooling roller, generating fluorine ions, which accelerate the deterioration of the deposited metal and reduce the reliability of the capacitor.Furthermore, fluorine oil is made from fluorocarbons, which are of concern for their environmental impact, so it is one of the substances whose use should be avoided.
[0006] Hydrocarbon oils are sometimes used as masking oils, but they have the drawback of being unstable in evaporation, which means that the amount of oil adhering to the dielectric film varies, resulting in frequent occurrence of unevenness and gaps.
[0007] Furthermore, vapor-deposited metal deteriorates due to moisture absorption, so silicone oil is sometimes applied to the vapor-deposited surface as an after-oil to form a protective film.
[0008] However, silicone oil has the property of easily allowing water vapor to pass through, so it was not possible to sufficiently suppress moisture absorption by the vapor-deposited metal.
[0009] Japanese Patent Application Laid-Open No. 63-7363 International Publication No. 2017 / 068758
[0010] The present invention is directed to improvements in metallized films.
[0011] The metallized film is characterized by using a hydrocarbon oil having a 10% evaporation temperature of 237°C or higher and a 90% evaporation temperature of 337°C or lower as a masking oil or after-oil.
[0012] In the metallized film, the contact angle of the hydrocarbon oil with respect to the dielectric film is preferably 17.9 to 22.8°, or the contact angle of the hydrocarbon oil with respect to the polypropylene film is preferably 17.9 to 22.8°.
[0013] The film capacitor of the present invention is characterized by using any one of the above metallized films.
[0014] The method for producing a metallized film of the present invention is characterized by including a step of evaporating and adhering a hydrocarbon oil.
[0015] When a hydrocarbon oil with a 10% evaporation temperature of 237°C or higher and a 90% evaporation temperature of 337°C or lower is used as a masking oil, the impact on the deterioration of the vapor-deposited metal and the environmental load are small. In addition, a metallized film with reduced unevenness and voids can be obtained.
[0016] When a hydrocarbon oil having a 10% evaporation temperature of 237° C. or higher and a 90% evaporation temperature of 337° C. or lower is used as the after-oil, moisture absorption by the vapor-deposited metal can be suppressed.
[0017] It is a figure which shows the vapor deposition pattern of the film capacitor based on one embodiment of this invention. It is a cross-sectional view of the main part of the metallized film. It is a cross-sectional view of the main part of the metallized film which applied after oil. It is a graph which shows the result of the humidity load test.
[0018] A film capacitor according to one embodiment of the present invention will be described below. The film capacitor uses a metallized film 1 shown in Figures 1 and 2. The metallized film 1 has a vapor deposition pattern consisting of vapor-deposited areas 3 and non-vapor-deposited areas 4 on the surface of a dielectric film 2. The vapor-deposited areas 3 refer to areas where a metal such as aluminum or zinc is vapor-deposited. The non-vapor-deposited areas 4 refer to areas where no metal is vapor-deposited. The non-vapor-deposited areas 4 are, for example, margin areas that separate the vapor-deposited areas. The vapor-deposited areas 3 separated by the margin areas become, for example, segmented electrodes 5. The segmented electrodes are connected to each other by fuse portions 6. Figure 1 shows a cut-out portion of the metallized film 1, which is actually continuous in the film feed direction.
[0019] The dielectric film is a synthetic resin film. For example, it is a film made of any of polypropylene, polyethylene terephthalate, polyethylene naphthalate, polyphenylene sulfide, polyvinylidene fluoride, and cycloolefin polymer. Polypropylene film is particularly preferred, and biaxially oriented polypropylene film is more preferred. It is also preferred that the surface is subjected to corona treatment. The thickness of the film is not particularly limited, but is, for example, 2.5 μm.
[0020] The non-vapor-deposited portion is formed by an oil masking method. The masking oil used in the oil masking method is a hydrocarbon oil that satisfies at least the following condition 1. It is more preferable that the masking oil is a hydrocarbon oil that satisfies both conditions 1 and 2. Furthermore, among the hydrocarbon oils that satisfy both conditions 1 and 2, it is even more preferable that the masking oil is paraffin oil.
[0021] [Condition 1] 10% evaporation temperature is 237°C or higher, and 90% evaporation temperature is 337°C or lower
[0022] If the 10% evaporation temperature is lower than 237°C, the masking oil will evaporate easily, causing unevenness. If the 90% evaporation temperature is higher than 337°C, voids will easily occur.
[0023] The evaporation temperature is a value measured by thermogravimetry based on JIS K0129 (2005). Specifically, a sample of masking oil was placed in an aluminum container (without a lid) of a simultaneous thermogravimetry-differential thermal analyzer (DTG-60H: manufactured by Shimadzu Corporation), and the temperature was raised from room temperature to 600°C at a rate of 10°C per minute, and the temperatures when the mass was reduced by 10% and when the mass was reduced by 90% were measured.
[0024] [Condition 2] Contact angle to dielectric film is 17.9 to 22.8°
[0025] The "contact angle" is preferably the contact angle with respect to a polypropylene film, more preferably the contact angle with respect to a biaxially oriented polypropylene film, and even more preferably the contact angle with respect to the corona-treated surface of a biaxially oriented polypropylene film.
[0026] If the contact angle is smaller than 17.9°, the masking oil tends to spread beyond the intended range, resulting in unevenness.If the contact angle is larger than 22.8°, it becomes difficult to adhere the masking oil to the dielectric film, resulting in voids.
[0027] The contact angle is a value measured by the sessile drop method based on JIS R3257 (1999). Specifically, at an ambient temperature of 25°C and humidity of 50%, 3±0.5 μL of liquid is dropped onto a sample using a microsyringe, and the sample is allowed to stand. After 1.5±0.1 seconds, the droplet is photographed. The radius r and height h of the droplet are determined and substituted into the following equation to determine the contact angle θ.
[0028] The metallized film is manufactured as follows. First, masking oil is applied to the surface of the dielectric film, for example, by flexographic printing. Specifically, a relief plate with convex portions having substantially the same shape as the non-vapor-deposited portions is prepared, and masking oil is applied to the relief plate. For example, masking oil stored in an oil tank is first heated using a heat source such as a heater to evaporate it. Next, the evaporated masking oil is applied to a roll (deposition process). The roll is then pressed against the relief plate. The relief plate is then pressed against the surface of the dielectric film, and the masking oil is transferred (deposited). During this process, the masking oil adhering to the convex portions of the relief plate is transferred, and a masking oil layer 7 is formed on the dielectric film (see Figure 2). On the other hand, the masking oil adhering to the concave portions of the relief plate is not transferred. Therefore, the shape of the transferred masking oil layer 7 is substantially the same as the convex portions of the relief plate. As a method for applying the masking oil, in addition to flexographic printing, screen printing, gravure printing, offset printing, spraying, die coating, etc. may also be used.
[0029] Next, metal is vapor-deposited onto the surface of the dielectric film onto which the masking oil has been transferred. For example, this is done by vacuum vapor deposition. Specifically, the dielectric film is placed in a vacuum vapor deposition machine, and metal is vapor-deposited onto the surface that has been subjected to corona discharge treatment so that the film resistance value reaches a predetermined value. The metal is heated, for example, by resistance heating. The metal is vapor-deposited on the areas where the masking oil is not attached, forming vapor-deposited areas. On the other hand, the metal is not vapor-deposited on the areas where the masking oil is attached, forming non-vapor-deposited areas. In essence, a vapor-deposited pattern is formed that corresponds to the recessed shape of the relief plate.
[0030] The film capacitor of the present invention is manufactured by winding the metallized film having the above-described structure and forming metallikon electrodes on both axial ends thereof by, for example, spraying a metal. Note that stacking may be used instead of winding.
[0031] Next, the results of comparative testing of metallized films produced using different masking oils will be described.
[0032] Example 1 A metallized film using, as the masking oil, a hydrocarbon oil (paraffin oil) having a 10% evaporation temperature of 237°C, a 90% evaporation temperature of 317°C, and a contact angle of 17.9°.
[0033] Example 2 A metallized film using, as the masking oil, a hydrocarbon oil (paraffin oil) having a 10% evaporation temperature of 265°C, a 90% evaporation temperature of 337°C, and a contact angle of 22.8°.
[0034] Comparative Example 1 A metallized film using, as the masking oil, a hydrocarbon oil (paraffin oil) having a 10% evaporation temperature of 215°C, a 90% evaporation temperature of 295°C, and a contact angle of 14.3°.
[0035] Comparative Example 2 A metallized film using, as the masking oil, a hydrocarbon oil (paraffin oil) having a 10% evaporation temperature of 253°C, a 90% evaporation temperature of 358°C, and a contact angle of 27.4°.
[0036] In each example and comparative example, metallized films were manufactured under the same conditions except for the masking oil. Specifically, a biaxially oriented polypropylene film 8000 m long and 2.5 μm thick was used as the dielectric film. The surface was corona-treated, and then masking oil was applied to the corona-treated surface by flexographic printing. Aluminum was then vapor-deposited to form a predetermined vapor-deposited pattern. As shown in Figure 1, the vapor-deposited pattern had a lattice-like margin (non-vapor-deposited area 4), and adjacent segmented electrodes 5 were connected to each other by fuses 6.
[0037] As one of the inspection items, the presence or absence of unevenness (a defect in which metal is not deposited or the amount of deposition is extremely small in areas where metal should be deposited) and gaps (a defect in which metal is deposited in areas where metal should not be deposited) were confirmed. Regarding unevenness, the presence or absence of unevenness was confirmed visually at a position 1500 m from the initial stage, magnified 20 times with a microscope. Regarding gaps, samples were sampled from the initial, middle, and final stages (N = 30 each), and the presence or absence of gaps was confirmed by comparing them with a limit sample at 40 times magnification with a microscope.
[0038] As other inspection items, the width dimension A of the margin portion extending in a direction perpendicular to the film feed direction, the width dimension B of the margin portion extending in a direction parallel to the film feed direction, and the width dimension C of the fuse portion provided between the margin portions extending in a direction parallel to the film feed direction were measured. Regarding dimensional accuracy, samples (N=30 for each) were sampled from the initial, middle, and final stages, and the dimensions were measured using a microscope at 40x magnification to check whether the average value and standard deviation σ of each dimension were within the reference values in Table 1. The reference values refer to the dimensional accuracy obtained when a fluorine oil with a 10% evaporation temperature of 235°C or higher, a 90% evaporation temperature of 335°C, and a contact angle of 17.9 to 22.8° was used as the masking oil (other conditions were the same as in each Example and Comparative Example).
[0039] The average value is in mm
[0040] Table 2 shows the inspection results. As can be seen from the table, in Examples 1 and 2, unevenness, missing parts, and dimensional accuracy are all equivalent to the standards. On the other hand, in Comparative Example 1, unevenness is below the standards, and in Comparative Example 2, missing parts and dimensional accuracy are below the standards.
[0041] 〇: Equivalent to the standard (using fluorine oil) ×: Below the standard
[0042] As shown above, hydrocarbon-based oils can produce results comparable to those obtained with fluorine-based oils by specifying the evaporation temperature and contact angle with the dielectric film. Fluorine-based oils, however, have problems such as being decomposed by the electron beam irradiated during metal deposition to improve adhesion between the dielectric film and the cooling roller, generating fluorine ions, which accelerate the deterioration of the deposited metal, and are expensive. On the other hand, hydrocarbon-based oils are less likely to cause such problems, making it possible to produce inexpensive, reliable film capacitors.
[0043] The applicant has separately confirmed that the lifespan (the rate of decrease in capacitance when a voltage of 600 VDC is applied in an environment of 105°C) of a film capacitor using fluorinated oil as masking oil is substantially the same as that of a film capacitor using the metallized film of Example 1 or Example 2.
[0044] Next, we will explain a metallized film using a hydrocarbon-based oil as an after-oil. After-oil is an oil applied to the deposition surface of the metallized film (the surface on which the deposition portion 3 is formed). The applied after-oil forms a protective film 8 on the deposition metal (deposition portion 3) (see Figure 3). The protective film 8 is formed, for example, by heating and evaporating after-oil filled in an oil tank using a heat source such as a heater, and then adhering the evaporated after-oil to the deposition surface. That is, after-oil is applied by evaporation, similar to the application of masking oil. However, after-oil is applied directly, whereas masking oil is applied indirectly via an intermediary such as a roll or relief plate. Note that Figure 3 depicts a boundary between the masking oil layer 7 and the after-oil layer 8, but the two layers may be mixed together, making the boundary unclear.
[0045] The hydrocarbon oil used as the after-lubricant satisfies the following condition 1.
[0046] [Condition 1] 10% evaporation temperature is 237°C or higher, and 90% evaporation temperature is 337°C or lower
[0047] If the 10% evaporation temperature is lower than 237°C, the after-oil will evaporate easily, and the protective film will not be formed stably. Also, if the 90% evaporation temperature is higher than 337°C, when the after-oil is heated to the evaporation temperature using a heat source such as a heater, the temperature difference between the position close to the heat source and the position far from the heat source will likely become large. As a result, the amount of evaporated oil will be unstable, and the protective film will not be formed stably.
[0048] The evaporation temperature is a value measured by thermogravimetry based on JIS K0129 (2005). Specifically, a sample of masking oil was placed in an aluminum container (without a lid) of a simultaneous thermogravimetry-differential thermal analyzer (DTG-60H: manufactured by Shimadzu Corporation), and the temperature was raised from room temperature to 600°C at a rate of 10°C per minute, and the temperatures when the mass was reduced by 10% and when the mass was reduced by 90% were measured.
[0049] The after-treatment oil is preferably a paraffin oil among hydrocarbon oils. The same oil as the masking oil may be used. That is, a hydrocarbon oil (paraffin oil) that satisfies conditions 1 and 2 may be used as the masking oil and after-treatment oil.
[0050] The method for applying the after-oil to the deposition surface may be the evaporation method described above, or may be a flexographic printing method, a screen printing method, a gravure printing method, an offset printing method, a spray method, a die coating method, or the like.
[0051] Next, the results of comparative testing of metallized films manufactured using different after-oils will be described.
[0052] Example 11 A metallized film using a hydrocarbon oil (paraffin oil) with a 10% evaporation temperature of 237°C and a 90% evaporation temperature of 317°C as an after-oil.
[0053] Example 12 A metallized film using a hydrocarbon oil (paraffin oil) with a 10% evaporation temperature of 265°C and a 90% evaporation temperature of 337°C as an after-oil.
[0054] Comparative Example 11 A metallized film using a hydrocarbon oil (paraffin oil) having a 10% evaporation temperature of 215°C and a 90% evaporation temperature of 295°C as the after-oil.
[0055] Comparative Example 12 A metallized film using a hydrocarbon oil (paraffin oil) having a 10% evaporation temperature of 253°C and a 90% evaporation temperature of 358°C as the after-oil.
[0056] Metallized films were manufactured under the same conditions for each example and comparative example, except for the use of different after-treatment oils. Specifically, a biaxially oriented polypropylene film measuring 8000 m in length and 2.5 μm in thickness was used as the dielectric film. The surface was corona-treated, and then masking oil was applied to the corona-treated surface by flexographic printing. Aluminum was then vapor-deposited to form a predetermined vapor deposition pattern. As shown in Figure 1, the vapor deposition pattern had a lattice-like margin (non-vapor-deposited area 4), and adjacent segmented electrodes 5 were connected to each other by fuses 6. The after-treatment oil was applied directly to the entire vapor deposition surface by heating and evaporating after-treatment oil filled in an oil tank with a heater.
[0057] The test was conducted to check whether a stable protective film had been formed. Specifically, the metallized films of Examples 11 and 12 and Comparative Examples 11 and 12 were wound, and metallikon electrodes were formed on both axial ends by, for example, spraying metal, to produce film capacitors with a capacitance of 193 μF. Next, each film capacitor was placed in an environment of 115°C and a voltage of 600 VDC was applied for 2000 hours. After 2000 hours, each film capacitor was unwound, and 10 m of metallized film was removed from each film capacitor. The light transmittance of the vapor-deposited portion 3 in the film thickness direction of each metallized film was measured. The light transmittance was measured using a light emitter and a light receiver (Keyence Corporation, Fiber Sensor FS-V21, FU-77V).
[0058]
[0059] Table 3 shows the maximum and minimum values of the measured light transmittance. When the vapor-deposited metal (vapor-deposited portion 3) deteriorates due to moisture, it becomes colorless and the light transmittance increases. Therefore, the larger the difference between the maximum and minimum light transmittance, the more uneven the formation of the protective film. However, as shown in Table 3, in Examples 11 and 12, the difference between the maximum and minimum light transmittance is smaller than in Comparative Examples 11 and 12, and the protective film is formed with a substantially constant thickness. In other words, it can be seen that a stable protective film is formed.
[0060] Hydrocarbon oils have extremely low water vapor permeability, so when a stable protective film is formed, it is possible to prevent contact between the vapor deposition portion 3 and water vapor and suppress deterioration of the vapor deposition portion 3.
[0061] Figure 4 is a graph showing the results of a humidity load test. The test involved placing the film capacitors in an 85°C, 85% humidity environment, applying a voltage of 450 VDC, and examining the change in capacitance after a specified time. Note that "Example 11" in the figure refers to a film capacitor using the same metallized film as Example 11, "Comparative Example 13" refers to a film capacitor using the same metallized film as Example 11 except that silicone oil with a 10% evaporation temperature of 193°C and a 90% evaporation temperature of 264°C was used as the after-oil, and "Comparative Example 14" refers to a film capacitor using the same metallized film as Example 11 except that no after-oil was applied.
[0062] As shown in the figure, the capacitor capacitance after about 3,500 hours in Example 11 decreased by only about 0.7%, while it decreased by about 3.1% in Comparative Example 13. This shows that higher moisture resistance was obtained compared to when silicone oil was used as an after-oil.
[0063] REFERENCE SIGNS LIST 1 Metallized film 2 Dielectric film 3 Vapor-deposited portion 4 Non-vapor-deposited portion 5 Segmented electrode 6 Fuse portion 7 Masking oil layer 8 After-oil layer (protective film) A Width dimension of margin portion B Width dimension of margin portion C Width dimension of fuse portion
Claims
1. Metallized film using a hydrocarbon oil with a 10% evaporation temperature of 237°C or higher and a 90% evaporation temperature of 337°C or lower as a masking oil or after-oil.
2. The metallized film of claim 1, wherein the contact angle of the hydrocarbon oil with the dielectric film is from 17.9 to 22.8 degrees.
3. The metallized film of claim 1, wherein the contact angle of the hydrocarbon oil with the polypropylene film is 17.9 to 22.8 degrees.
4. A film capacitor using the metallized film according to any one of claims 1 to 3.
5. The method of claim 1, further comprising the step of depositing said hydrocarbon oil by evaporation.
Citation Information
Patent Citations
Vacuum evaporation method
JP1980079867A
Oil masking device and vacuum deposition device provided with it
JP2001279425A
Zinc-metallized base material for metallized capacitor and process for its production
WO1987003419A1
Cited By
Metallized film, film capacitor
WO2026203445A1