Composite substrate

By creating voids within the intermediate SiO2 layer at a specific area ratio, the composite substrate prevents void formation at the bonding interface during annealing, ensuring strong bonding and stability of the functional substrate to the supporting substrate.

WO2024203566A1PCT designated stage expired Publication Date: 2024-10-03NGK INSULATORS LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010624
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The generation of voids at the bonding interface during annealing treatment in composite substrates leads to a decrease in bonding strength and the risk of the functional substrate peeling off from the supporting substrate, due to impurities like moisture and gas being trapped within the intermediate SiO2 layer.

Method used

Forming voids inside the intermediate SiO2 layer at a predetermined area ratio of 1 to 7% within the stretching direction, which allows trapped impurities to expand and be removed, thereby preventing void formation at the bonding interface during annealing.

Benefits of technology

This approach effectively suppresses the generation of voids at the bonding interface, maintaining bonding strength and preventing peeling of the functional substrate from the supporting substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010624_03102024_PF_FP_ABST
    Figure JP2024010624_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This composite substrate comprises: a functional substrate having a predetermined function; a support substrate supporting the functional substrate; and an intermediate layer provided between the support substrate and the functional substrate. The functional substrate and the support substrate are joined with the intermediate layer interposed therebetween. Within the intermediate layer, (a) void(s) is / are formed at a predetermined area ratio in the extension direction of the intermediate layer, the predetermined area ratio being 1-7%.
Need to check novelty before this filing date? Find Prior Art

Description

Composite PCB

[0001] The present invention relates to a composite substrate.

[0002] Conventionally, composite substrates formed by bonding multiple layers of substrates have been widely used as materials for various devices such as semiconductor elements. For example, a composite substrate that realizes a high-performance semiconductor element with excellent response speed and power consumption is made by bonding a support substrate and a Si substrate to a SiO 2 SOI (Silicon On Insulator) substrates are known, in which the substrate is bonded via a layer. Furthermore, to realize piezoelectric devices such as SAW (Surface Acoustic Wave) filters, LN (LiNbO 3 ) and LT (LiTaO 3 Composite substrates using piezoelectric material substrates such as .

[0003] The composite substrate described above is made up of a functional substrate having a predetermined function, such as a Si substrate or a piezoelectric material substrate, and a supporting substrate, and a SiO 2 This direct bonding requires a surface activation process to activate the bonding surfaces.

[0004] As a surface activation treatment for manufacturing a composite substrate, Patent Documents 1 and 2 disclose a method using plasma generated by oxygen gas, nitrogen gas, argon gas, etc. This method makes it possible to activate the bonding surface at a relatively low temperature (about 400°C).

[0005] Japanese Patent Application Publication No. 2016-225537 International Publication No. 2022 / 190465

[0006] SiO forming an intermediate layer between the functional substrate and the support substrate 2The composite substrate described above can be formed by depositing each layer, subjecting the bonding surface on the functional substrate side to a surface activation treatment, and then directly bonding the bonding surfaces on the support substrate side. To improve the bonding strength, an annealing treatment may be performed after bonding, in which the entire composite substrate is heated to a predetermined temperature. This annealing treatment forms covalent bonds via OH groups at the interface between the bonding surfaces (bonding interface), thereby improving the bonding strength.

[0007] On the other hand, if moisture or gases used in the process before bonding adhere to the bonding surface, they will turn into SiO after bonding. 2 These impurities may be mixed into the SiO 2 When the layers are heated, the impurities expand, which can cause voids to form at the bonding interface. The formation of voids at the bonding interface reduces the bonding strength, and as the voids grow, there is a risk that the functional substrate will peel off from the support substrate.

[0008] The present invention has been made in view of the above, and a main object of the present invention is to realize a composite substrate that can suppress the generation of voids at the bonding interface during annealing treatment.

[0009] The composite substrate according to the present invention comprises a functional substrate having a predetermined function, a support substrate that supports the functional substrate, and an intermediate layer provided between the support substrate and the functional substrate, wherein the functional substrate and the support substrate are bonded to each other via the intermediate layer, and voids are formed within the intermediate layer at a predetermined area ratio with respect to the extension direction of the intermediate layer, the area ratio being within the range of 1 to 7%.

[0010] According to the present invention, it is possible to realize a composite substrate that can suppress the generation of voids at the bonding interface during annealing treatment.

[0011] FIG. 1 is a schematic cross-sectional view showing a general configuration of a composite substrate according to one embodiment of the present invention. FIG. 2 is a view showing an example of a manufacturing process for a composite substrate according to one embodiment of the present invention. FIG. 3 is a view showing an example of a manufacturing process for a composite substrate according to one embodiment of the present invention. FIG. 4 is a view showing an example of a manufacturing process for a composite substrate according to one embodiment of the present invention. FIG. 5 is a view showing an AFM image and an enhanced image at the bonding interface of Example 1. FIG. 6 is a view showing an AFM image and an enhanced image at the bonding interface of Example 2. FIG. 7 is a view showing an AFM image and an enhanced image at the bonding interface of Comparative Example 2. FIG. 8 is a view showing an AFM image and an enhanced image at the bonding interface of Comparative Example 4. FIG. 9 is a graph summarizing the relationship between the area ratio of void portions and the number of voids at the bonding interface.

[0012] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments. In addition, in order to clarify the description, the drawings may show the width, thickness, shape, etc. of each part more schematically than in the embodiments, but these are merely examples and do not limit the interpretation of the present invention.

[0013] 1 is a schematic cross-sectional view showing the overall configuration of a composite substrate according to one embodiment of the present invention. The composite substrate 100 in this embodiment has a structure in which a functional substrate 10 having a predetermined function is bonded to a support substrate 30 via an intermediate layer 20.

[0014] The functional substrate 10 has functions for realizing various devices, and is made of materials according to the functions. For example, in the composite substrate 100 used for a SAW filter or an optical waveguide, a piezoelectric material substrate can be made, for example, LN (LiNbO 3 : lithium niobate) and LT (LiTaO 3 Examples of piezoelectric materials include piezoelectric materials such as silicon dioxide (SiO2), silicon nitride (SiO2), and lithium tantalate (LTC). In the composite substrate 100 used as an SOI substrate, the functional substrate 10 is made of a silicon substrate, which is a semiconductor. In addition to these, various materials can be used as the functional substrate 10 depending on the application of the composite substrate 100.

[0015] In the following, an example in which the functional substrate 10 is made of an LT material will be described, but the same applies to cases in which other materials are used.

[0016] The intermediate layer 20 is provided on the support substrate 30 and is disposed between the functional substrate 10 and the support substrate 30. The material of the intermediate layer 20 is, for example, SiO 2 is.

[0017] The intermediate layer 20 can be formed by any suitable method, such as sputtering, vacuum deposition, physical vapor deposition such as ion beam assisted deposition (IAD), chemical vapor deposition, or atomic layer deposition (ALD). The intermediate layer 20 can be formed at a temperature of, for example, room temperature (25° C.) to 300° C.

[0018] The support substrate 30 supports the functional substrate 10. Any appropriate substrate can be used as the support substrate 30. The support substrate 30 may be made of a single crystal or a polycrystalline material. It may also be made of a metal. The functional substrate 10 and the support substrate 30 are bonded to each other via an intermediate layer 20.

[0019] The material constituting the support substrate 30 is preferably silicon, sialon, sapphire, cordierite, mullite, glass, quartz, crystal, alumina, SUS, iron-nickel alloy (42 alloy), MgF 2 , CaF 2 and brass. The support substrate 30 may have any suitable thickness.

[0020] The silicon may be single crystal silicon, polycrystalline silicon, or high-resistivity silicon.

[0021] Typically, the sialon is a ceramic obtained by sintering a mixture of silicon nitride and alumina, and for example, Si 6 -wAlwOwN 8 Sialon has a composition represented by -w. Specifically, sialon has a composition in which alumina is mixed into silicon nitride, and w in the formula represents the mixing ratio of alumina. w is preferably 0.5 or more and 4.0 or less.

[0022] Typically, the sapphire is Al 2 O 3 The alumina is a single crystal having a composition of Al 2 O 3 The alumina is preferably a translucent alumina.

[0023] Typically, the cordierite is 2MgO.2Al 2 O 3 5SiO 2 The mullite is a ceramic having a composition of 3Al 2 O 3 2SiO 2 ~2Al 2 O 3 SiO 2 It is a ceramic having a composition in the range of

[0024] Although not shown, the composite substrate 100 may further include any layer. The type, function, number, combination, arrangement, etc. of such layers may be appropriately set depending on the purpose.

[0025] The composite substrate 100 can be manufactured in any suitable shape. In one embodiment, the composite substrate 100 can be manufactured in the form of a so-called wafer. The size of the composite substrate 100 can be appropriately set depending on the purpose, for example, with a wafer (substrate) diameter of 50 mm to 200 mm.

[0026] 2 to 5 are diagrams showing an example of a manufacturing process for a composite substrate according to an embodiment of the present invention.

[0027] 2A shows a preparation step in the manufacturing process of the composite substrate 100. In this step, a support substrate 30 is prepared. For example, a high-resistivity Si substrate (resistivity of 2 kΩ·cm or more) having a thickness of 0.23 mm is used as the support substrate 30.

[0028] 2(b) shows the blasting process in the manufacturing process of the composite substrate 100. In this process, an abrasive having an average particle size of, for example, about 2 μm is sprayed by a blast gun onto the surface of the support substrate 30 prepared in the preparation process of FIG. 2(a), thereby blasting the support substrate 30. It is preferable to use powder of, for example, SiC, glass, alumina, or the like as the abrasive.

[0029] Here, if the distance between the support substrate 30 and the blast gun during blasting is too short (for example, less than 10 mm), the abrasive sprayed first from the blast gun bounces off the surface of the support substrate 30, collides with the abrasive sprayed later, and does not reach the support substrate 30, resulting in little progress in the blasting process. On the other hand, if this distance is too long (for example, 100 mm or more), the speed at which the abrasive sprayed from the blast gun reaches the surface of the support substrate 30 is too low, and the kinetic energy required for the blasting process cannot be obtained. Therefore, it is preferable that the distance between the support substrate 30 and the blast gun during blasting be within the range of approximately 10 to 100 mm.

[0030] Fig. 2(c) shows an enlarged view of a portion of the cross section of the support substrate 30 after blasting. In the blasting process shown in Fig. 2(b), the surface of the support substrate 30 is unevenly scraped by the abrasive, resulting in the uneven shape shown in Fig. 2(c). This uneven surface of the support substrate 30 is partially dug deeper than other portions, forming holes 31.

[0031] 3D shows a film-forming step for the support substrate 30 in the manufacturing process of the composite substrate 100. In this step, a film of, for example, SiO 2 is formed to a predetermined thickness on the surface of the support substrate 30 that has been processed to have an uneven shape by the blasting process shown in FIG. 2 By depositing the amorphous material, a first intermediate film 20A for constituting the intermediate layer 20 is formed.

[0032] Fig. 3(e) shows an enlarged view of a portion of the cross section of the support substrate 30 after film formation. In the film formation step of Fig. 3(d), the first intermediate film 20A is formed along the surface of the support substrate 30 that has been processed to have an uneven shape.

[0033] 3(f) shows a step of planarizing the bonding surface in the manufacturing process of the composite substrate 100. In this step, the surface of the first intermediate film 20A formed on the support substrate 30 in the film formation step of FIG. 3(d) is polished to planarize the bonding surface of the support substrate 30 (first intermediate film 20A).

[0034] Fig. 3(g) shows an enlarged view of a portion of the cross section of the support substrate 30 after planarization. In the planarization step of Fig. 3(f), the surface of the first intermediate film 20A is polished, thereby entirely planarizing the irregularities formed along the surface of the support substrate 30. However, the partially deep holes 31 remain without being completely planarized.

[0035] 4(h) shows the activation step in the manufacturing process of the composite substrate 100. In this step, first, an LT substrate 10A made of an LT material with a predetermined thickness and a mirror-polished surface is prepared, and then, by carrying out the film-forming step and planarization step similar to those shown in FIGS. 3(d) and 3(f), a second intermediate film 20B is formed on the LT substrate 10A and its surface is planarized. Next, N is applied to the surface of the first intermediate film 20A on the support substrate 30 and the surface of the second intermediate film 20B on the LT substrate 10A, which have been planarized by the planarization step shown in FIG. 2 The surfaces are activated by irradiating them with plasma.

[0036] Fig. 4(i) shows the bonding step in the manufacturing process of the composite substrate 100. In this step, the surface of the first intermediate film 20A on the support substrate 30 side and the surface of the second intermediate film 20B on the LT substrate 10A side, which have been activated in the activation step of Fig. 4(h), are directly bonded together to form a bonded body of the support substrate 30 and the LT substrate 10A, with these surfaces serving as bonding surfaces.

[0037] Fig. 5(j) shows a bonded body of the support substrate 30 and the LT substrate 10A. The first intermediate film 20A and the second intermediate film 20B are bonded and integrated by the bonding step of Fig. 4(i), thereby forming the intermediate layer 20. As a result, the support substrate 30 and the LT substrate 10A are bonded to each other via the intermediate layer 20, and a bonded body of the support substrate 30 and the LT substrate 10A as shown in Fig. 5(j) is formed.

[0038] Figure 5(k) shows an enlarged view of a portion of the cross section of the bonded body shown in Figure 5(j). In the bonding process shown in Figure 4(i), the opening of the hole 31 partially formed in the first intermediate film 20A is blocked by the second intermediate film 20B. As a result, voids 21 are partially formed in the intermediate layer 20, where the first intermediate film 20A and the second intermediate film 20B are integrated, at a predetermined area ratio relative to the extension direction of the intermediate layer 20. The predetermined area ratio is 1% or more and 7% or less. If the area ratio is less than 1%, voids are likely to occur, and if the area ratio is greater than 7%, the bonding strength is insufficient and the functional substrate is likely to peel off during thinning processing. More preferably, the area ratio is 1.4% or more and 6.6% or less.

[0039] 5(l) shows the annealing step in the manufacturing process of the composite substrate 100. In this step, the bonded assembly of the support substrate 30 and the LT substrate 10A formed in the bonding step of FIG. 4(i) is heated to a predetermined temperature. This forms covalent bonds via OH groups inside the intermediate layer 20, improving the bonding strength of the bonded assembly.

[0040] 5(l), impurities such as moisture and gas that adhere to the surfaces of the first intermediate film 20A and the second intermediate film 20B during the planarization and activation steps and are trapped within the intermediate layer 20 during the subsequent bonding step may expand due to heating. The expansion of such impurities causes voids to form at the bonding interface between the first intermediate film 20A and the second intermediate film 20B within the intermediate layer 20, leading to a decrease in bonding strength. If the voids continue to grow, there is a risk that the LT substrate 10A will peel off from the support substrate 30.

[0041] In this embodiment, as described above, by partially forming voids 21 within the intermediate layer 20, even if impurities such as moisture and gas trapped within the intermediate layer 20 expand due to heating, the impurities tend to remain within the voids 21. This suppresses the generation of voids at the bonding interface within the intermediate layer 20 during annealing, and suppresses a decrease in bonding strength and peeling of the LT substrate 10A.

[0042] 5( m) shows the thinning step in the manufacturing process of the composite substrate 100. In this step, the LT substrate 10A is polished to a predetermined thickness to thin the bonded body after the annealing treatment step shown in FIG. 5( l), thereby forming the functional substrate 10 made of the LT material. For example, the LT substrate 10A can be polished to thin the substrate using grinding, CMP (Chemical Mechanical Polishing), surface planarization using a gas cluster ion beam, or the like.

[0043] Through the above steps, the composite substrate 100 having the structure shown in FIG. 1 is manufactured.

[0044] Examples for verifying the structure of the composite substrate according to the present invention will be specifically described below. Unless otherwise specified, the following procedures were carried out at room temperature.

[0045] Example 1 A bonded body was produced according to the manufacturing process described with reference to Figures 2 to 5. Specifically, an LT substrate 10A having a thickness of 0.25 mm and a support substrate 30 made of a high-resistivity Si substrate having a thickness of 0.23 mm were used. A blast gun was then placed 40 mm away from the surface of the support substrate 30, and a powdered abrasive having an average particle size of 2 µm was sprayed at a pressure of 0.25 MPa for 4 minutes to perform blasting. After that, SiO was applied to the surface of the support substrate 30 and the surface of the LT substrate 10A after blasting. 2 The amorphous bodies were formed into films each having a thickness of 0.5 μm to form a first intermediate film 20A and a second intermediate film 20B, and the surfaces of the films were polished by CMP by about 0.1 μm each to be flattened.

[0046] Next, the surface of the first intermediate film 20A on the support substrate 30 and the surface of the second intermediate film 20B on the LT substrate 10A are coated with N 2 After irradiating each with plasma to activate them, the surfaces of these films were placed together and pressed together at room temperature to directly bond them together, thereby integrating the first interlayer film 20A and the second interlayer film 20B to form the intermediate layer 20, and obtaining a bonded body in which the support substrate 30 and the LT substrate 10A were bonded together via the intermediate layer 20.

[0047] Next, the resulting bonded body was placed in a high-temperature furnace, heated from room temperature to 130° C., held there for about 4 hours, and then returned to room temperature, thereby carrying out an annealing treatment.

[0048] Next, the LT substrate 10A of the bonded body after the annealing treatment was ground and polished to reduce the thickness of the LT substrate 10A to 1 μm, thereby forming the functional substrate 10, thereby obtaining the composite substrate 100 having the structure shown in Fig. 1. In the composite substrate 100 of Example 1, no voids were observed at the bonding interface in the intermediate layer 20.

[0049] Example 2 In the manufacturing process of Example 1, the average particle size of the abrasive used in the blasting process was changed to 3 μm, and the other conditions were the same as in Example 1, and the other steps were also performed under the same conditions as in Example 1 to obtain composite substrate 100 having the structure shown in Figure 1. In composite substrate 100 of Example 2, no voids were observed at the bonding interface in intermediate layer 20.

[0050] Comparative Example 1 Composite substrate 100 having the structure shown in Fig. 1 was obtained by omitting the blasting process from the manufacturing process of Example 1 and performing the other processes under the same conditions as Example 1. In composite substrate 100 of Comparative Example 1, approximately 80 voids were generated at the bonding interface in intermediate layer 20.

[0051] Comparative Example 2 In the manufacturing process of Example 1, the average particle size of the abrasive used in the blasting process was changed to 1.2 μm, and the other conditions were the same as in Example 1, and the other steps were also performed under the same conditions as in Example 1 to obtain composite substrate 100 having the structure shown in Figure 1. In composite substrate 100 of Comparative Example 2, approximately 20 voids were generated at the bonding interface in intermediate layer 20.

[0052] Comparative Example 3 In the manufacturing process of Example 1, the average particle size of the abrasive used in the blasting process was changed to one larger than 3 μm, and the other conditions were the same as in Example 1, and the other steps were also the same as in Example 1. In this Comparative Example 3, the bonding strength of the bonded body after the annealing treatment was insufficient, and LT substrate 10A peeled off in the subsequent thin plate processing step, so composite substrate 100 having the structure shown in FIG.

[0053] (Comparative Example 4) In the manufacturing process of Example 1, the installation position of the blast gun in the blasting process was changed to a distance of 100 mm from the surface of the support substrate 30, and the other conditions were the same as in Example 1. In addition, the other processes were also performed under the same conditions as in Example 1, and a composite substrate 100 having the structure shown in Figure 1 was obtained.

[0054] (Confirmation of Bonding Interface) In order to confirm the bonding interface within the intermediate layer 20 for each of the composite substrates 100 produced in Examples 1 and 2 and Comparative Examples 2 and 4, the functional substrate 10 made of the 1 μm-thick LT substrate 10A was removed by polishing, and further, a portion of the intermediate layer 20 (a thickness of 0.5 μm) corresponding to the second intermediate film 20B before bonding was removed by polishing. Thereafter, the exposed surface (bonding interface) of each polished composite substrate 100 was observed with an AFM (Atomic Force Microscope) to obtain an AFM image, and predetermined image processing was performed on each obtained AFM image to obtain an enhanced image in which the void portion at the bonding interface was emphasized. 6(a) and (b) show an AFM image and an emphasized image at the bonded interface of Example 1, FIGS. 7(a) and (b) show an AFM image and an emphasized image at the bonded interface of Example 2, FIGS. 8(a) and (b) show an AFM image and an emphasized image at the bonded interface of Comparative Example 2, and FIGS. 9(a) and (b) show an AFM image and an emphasized image at the bonded interface of Comparative Example 4, respectively.

[0055] The area ratio of the void portion relative to the stretching direction of the intermediate layer 20 calculated from the enhanced image of Example 1 shown in Figure 6(b) was 1.4%. The area ratio of the void portion relative to the stretching direction of the intermediate layer 20 calculated from the enhanced image of Example 2 shown in Figure 7(b) was 6.6%. The area ratio of the void portion relative to the stretching direction of the intermediate layer 20 calculated from the enhanced image of Comparative Example 2 shown in Figure 8(b) was 0.3%. The area ratio of the void portion relative to the stretching direction of the intermediate layer 20 calculated from the enhanced image of Comparative Example 4 shown in Figure 9(b) was 0.19%.

[0056] Figure 10 is a graph summarizing the relationship between the area ratio of voids and the number of voids at the bonding interface in each composite substrate 100 of Examples 1 and 2 and Comparative Examples 1 to 3. In Figure 10, point 101 represents Example 1, point 102 represents Example 2, point 103 represents Comparative Example 1, point 104 represents Comparative Example 2, and point 105 represents Comparative Example 3. Note that in Comparative Example 1, blasting was omitted as described above, so the area ratio of voids was set to 0%. In Comparative Example 3, the average particle size of the abrasive was larger than that of Example 2 (average particle size 3 μm), and therefore the area ratio of voids was 7.5%, which was larger than the value calculated in Example 2 (6.6%).

[0057] 10, it can be seen that if the area ratio of the void portion is within the range of 1 to 7%, sufficient bonding strength can be obtained while suppressing the generation of voids to zero at the bonding interface within intermediate layer 20. In other words, in composite substrate 100 produced in each of the steps of Figures 2 to 5, by setting the conditions of the blasting process described above so that voids are formed within intermediate layer 20 at an area ratio within the range of 1 to 7% with respect to the extension direction of intermediate layer 20, it is possible to realize composite substrate 100 that can suppress the generation of voids at the bonding interface during annealing treatment.

[0058] According to the embodiment of the present invention described above, the following advantageous effects are achieved.

[0059] (1) The composite substrate 100 includes a functional substrate 10 having a predetermined function, a support substrate 30 that supports the functional substrate 10, and an intermediate layer 20 that is provided between the support substrate 30 and the functional substrate 10. The functional substrate 10 and the support substrate 30 are bonded to each other via the intermediate layer 20, and voids are formed within the intermediate layer 20 at a predetermined area ratio relative to the extension direction of the intermediate layer 20. This area ratio is within the range of 1 to 7%. This configuration makes it possible to realize a composite substrate 100 that can suppress the generation of voids at the bonding interface during annealing treatment.

[0060] (2) The intermediate layer 20 is made of SiO 2 In this way, it is possible to firmly bond the functional substrate 10 and the support substrate 30 via the intermediate layer 20.

[0061] (3) The functional substrate 10 is made of LN (LiNbO 3 ) or LT(LiTaO 3 The functional substrate 10 may be a piezoelectric material substrate made of a silicon (Si) material. The functional substrate 10 may also be a semiconductor substrate made of a silicon (Si) material. In this way, substrates having various functions can be used as the functional substrate 10 depending on the application of the composite substrate 100.

[0062] The present invention is not limited to the above-described embodiment, and can be implemented using any components without departing from the spirit of the present invention.

[0063] The above-described embodiments and modifications are merely examples, and the present invention is not limited to these details as long as the features of the invention are not impaired. Furthermore, although various embodiments and modifications have been described above, the present invention is not limited to these details. Other aspects that can be considered within the scope of the technical idea of ​​the present invention are also included within the scope of the present invention.

[0064] 10: Functional substrate 10A: LT substrate 20: Intermediate layer 20A: First intermediate film 20B: Second intermediate film 21: Gap 30: Support substrate 31: Hole 100: Composite substrate

Claims

1. A composite substrate comprising: a functional substrate having a predetermined function; a support substrate supporting the functional substrate; and an intermediate layer disposed between the support substrate and the functional substrate, wherein the functional substrate and the support substrate are bonded to each other via the intermediate layer, and within the intermediate layer, voids are formed at a predetermined area ratio in the extension direction of the intermediate layer, and the predetermined area ratio is 1% or more and 7% or less.

2. In the composite substrate according to claim 1, the intermediate layer is made of SiO 2 A composite substrate.

3. A composite substrate according to claim 1, wherein the functional substrate is a piezoelectric material substrate.

4. A composite substrate according to claim 1, wherein the functional substrate is a semiconductor substrate made of a silicon material.

Citation Information

Patent Citations

  • Composite substrate

    WO2013129572A1

  • Joined body of piezoelectric material substrate and support substrate

    WO2019220721A1

  • Joined body of piezoelectric material substrate and support substrate

    WO2019220724A1