Plated steel sheet and method for manufacturing same

The production of a plated steel sheet with a specific composition and metal structure using controlled hot rolling and oxidation-reduction treatments addresses the complexity of conventional methods, achieving high strength and workability with improved manufacturing efficiency.

WO2024203604A1PCT designated stage expired Publication Date: 2024-10-03KOBE STEEL LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010714
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-02-19
Filing Date
2024-03-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional methods for manufacturing plated steel sheets with high strength and workability are complex and may not ensure stable production, limiting their strength and workability improvements.

Method used

A plated steel sheet with a specific composition (C: 0.150-0.250%, Si: 0.80-2.20%, Mn: 1.50-2.80%, Cr: 0.15-1.50%, Ti: 0.012-0.100%, B: 0.0015-0.0100%, P: 0.100% or less, S: 0.050% or less, Al: 0.005-1.000%, N: 0.0100% or less) and a metal structure (total bainite and tempered martensite of 95% or less, retained austenite of 5% or more, and minimal polygonal ferrite and bainitic ferrite) is produced using a simplified process involving hot rolling, controlled cooling, and oxidation-reduction treatments.

Benefits of technology

The method results in a plated steel sheet with tensile strength of 1150 MPa or more, yield stress of 850 MPa or more, elongation of 14% or more, and hole expansion rate of 30% or more, enhancing both strength and workability while simplifying the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Disclosed is a plated steel sheet which comprises a steel sheet and a plating layer that is disposed on the surface of the steel sheet, and which has a tensile strength of 1,150 MPa or more. The steel sheet in the plated steel sheet has a specific component composition, and has a metal structure wherein: the total amount of bainite and tempered martensite is 95% by area or less; the amount of residual austenite is 5% by volume or more; the total amount of polygonal ferrite and bainitic ferrite is 5% by area or less; and the amount of other structures is 5% by area or less.
Need to check novelty before this filing date? Find Prior Art

Description

Coated steel sheet and its manufacturing method

[0001] The present disclosure relates to plated steel sheets and methods for producing the same.

[0002] There has been a demand for improved occupant safety in vehicles, and for this purpose, the strength of vehicle body materials has been improved. On the other hand, against the backdrop of worsening issues such as global warming, there has been an accelerating movement to improve automobile fuel efficiency. It is known that reducing the weight of vehicle bodies is an effective way to improve fuel efficiency.

[0003] Plated steel sheets used in automobile bodies are required to have high strength (e.g., tensile strength of 1150 MPa or more) to achieve weight reduction of the vehicle body. Furthermore, because plated steel sheets need to be processed into part shapes, plated steel sheets are required to have high formability (high elongation EL, high hole expansion ratio λ, etc.).

[0004] Patent Documents 1 and 2 disclose plated steel sheets that contain C, Si, and Mn as essential components and have a predetermined metal structure, thereby exhibiting high ductility and high strength. Patent Document 3 discloses a plated steel sheet that contains C, Si, Mn, Al, and at least one selected from V, Mo, Ti, and Nb as essential components and has a predetermined metal structure, thereby exhibiting high ductility and high workability (high λ, etc.).

[0005] International Publication No. WO2020 / 080402 International Publication No. WO2020 / 080401 International Publication No. WO2019 / 159771

[0006] In Patent Documents 1 to 3, the manufacturing method, particularly the cooling after reheating after hot rolling (and cold rolling), is strictly controlled in order to obtain the desired performance. For example, in Patent Document 1, the cooling rate must be controlled or maintained in at least six temperature ranges (810 to 700°C, 700 to 490°C, 490 to 405°C, 405 to 310°C, 315 to 255°C, and 255°C to the cooling stop temperature (254 to 220°C)). In Patent Document 2, the cooling rate must be controlled or maintained in at least five temperature ranges (810 to 650°C, 650 to 505°C, 505 to 405°C, 405 to 315°C, and 315 to the cooling stop temperature (310 to 255°C)). In Patent Document 3, the cooling rate must be controlled or maintained in at least four temperature ranges (830 to 550°C or less, Ac1+60°C to 550°C, 550 to 400°C, and 375 to 150°C). As described above, the plated steel sheets disclosed in Patent Documents 1 to 3 require complicated manufacturing methods for achieving high strength and high formability, and there is a risk that they cannot be produced stably, for example. Furthermore, there is room for improvement in strength and formability.

[0007] The present disclosure has been made in view of the above circumstances, and one of its objectives is to provide a plated steel sheet that can be more easily manufactured, has high strength, can contribute to weight reduction of a vehicle body, and exhibits high formability, and a manufacturing method thereof.

[0008] A first aspect of the present invention is a plated steel sheet comprising a steel sheet and a plating layer disposed on a surface of the steel sheet, the plated steel sheet having a tensile strength of 1150 MPa or more, wherein the steel sheet contained in the plated steel sheet has a component composition consisting of: C: 0.150 to 0.250 mass%, Si: 0.80 to 2.20 mass%, Mn: 1.50 to 2.80 mass%, Cr: 0.15 to 1.50 mass%, Ti: 0.012 to 0.100 mass%, B: 0.0015 to 0.0100 mass%, P: 0.100 mass% or less (including 0 mass%), S: 0.050 mass% or less (including 0 mass%), Al: 0.005 to 1.000 mass%, N: 0.0100 mass% or less (including 0 mass%), and the balance: iron and inevitable impurities; and The plated steel sheet has a metallographic structure in which the total of bainite and tempered martensite is 95% by area or less, retained austenite is 5% by volume or more, the total of polygonal ferrite and bainitic ferrite is 5% by area or less, and the remaining structure is 5% by area or less.

[0009] A second aspect of the present invention is the plated steel sheet according to the first aspect, wherein, in the sheet thickness direction, a position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is in a region that is 0.2% or more of the sheet thickness from the surface of the steel sheet.

[0010] A third aspect of the present invention is the plated steel sheet according to the first or second aspect, wherein the maximum carbon concentration (mass %) in a region extending from the surface of the steel sheet to 20 μm in the sheet thickness direction is less than 70% of the bulk carbon concentration.

[0011] A fourth aspect of the present invention is the plated steel sheet according to any one of the first to third aspects, wherein the retained austenite includes 10 to 50 volume % of first retained austenite having a solute C content of 0.9 mass % or less, and 10 to 50 volume % of second retained austenite having a solute C content of more than 0.9 mass % and 1.1 mass % or less.

[0012] Aspect 5 of the present invention is a method for producing a plated steel sheet according to any one of Aspects 1 to 4, comprising: hot rolling a steel having the chemical composition according to Aspect 1 to obtain a rolled sheet; heating the rolled sheet to a first heating temperature of 850°C or higher; after the heating step, holding the rolled sheet at the first heating temperature for 50 seconds or more; after the holding step, cooling the rolled sheet to a cooling stop temperature of 200 to 350°C, wherein an average cooling rate from the first heating temperature to 550°C is 5°C / second or higher and an average cooling rate from 550°C to the cooling stop temperature is 1°C / second or higher; after the cooling step, heating the steel to a second heating temperature of 300°C to 450°C and holding the temperature for 50 to 1000 seconds to obtain a steel sheet; and forming a coating layer on the steel sheet.

[0013] A sixth aspect of the present invention is the production method according to the fifth aspect, further comprising, after the step of obtaining the rolled plate, performing an oxidation treatment under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750°C, and the holding step includes reduction treatments in which a first reduction treatment is performed at a dew point of -35 to -15°C, and then a second reduction treatment is performed at a dew point of -25 to 0°C, which is higher than the dew point of the first reduction treatment.

[0014] A seventh aspect of the present invention is the manufacturing method according to the fifth or sixth aspect, wherein the cooling step is performed at an average cooling rate of 400° C. to the cooling stop temperature of 40° C. / second or less.

[0015] According to the embodiments of the present invention, it is possible to provide a plated steel sheet that can be more easily manufactured, has high strength, contributes to weight reduction of a vehicle body, and exhibits high formability, and a method for manufacturing the same.

[0016] Fig. 1 is a graph showing the relationship between the dew point at the center of the soaking zone during the second reduction treatment and R / t. Fig. 2 is a schematic diagram of an X-ray diffraction pattern. Fig. 3 is a diagram showing an example of a carbon concentration profile obtained in an example. Fig. 4 is a graph showing the relationship between R / t and the position at which the carbon concentration (mass%) in the sheet thickness direction is 50% of the bulk carbon concentration. Fig. 5 is a graph showing the relationship between R / t and the ratio of the maximum carbon concentration (mass%) in a region from the steel sheet surface to 20 µm deep, relative to the bulk carbon concentration.

[0017] The present inventors conducted extensive research to develop a plated steel sheet that can be more easily manufactured and exhibits high strength (tensile strength TS of 1150 MPa or more, yield stress YS of 850 MPa or more) and high formability (elongation EL of 14% or more, hole expansion ratio λ of 30% or more). As a result, they were able to develop a plated steel sheet that exhibits high strength and high formability by using a steel sheet containing a predetermined chemical composition, particularly Cr, Ti, and B in predetermined amounts as essential elements, and further having a predetermined metallographic structure. They also discovered that the plated steel sheet can be manufactured using an easier manufacturing method, in which the cooling rate during reheating after hot rolling (and cold rolling) is controlled within two fewer temperature ranges (first heating temperature to 550°C, 550°C to cooling stop temperature) than in conventional techniques. Details of each requirement specified in the embodiments of the present invention are provided below.

[0018] <1. Plated Steel Sheet> A plated steel sheet according to an embodiment of the present invention includes a steel sheet and a plating layer disposed on the surface of the steel sheet. The plating layer may be a zinc-based plating layer such as a hot-dip galvanized layer, a galvannealed hot-dip galvanized layer, or an electrogalvanized layer, or an aluminum plating layer such as a hot-dip aluminum plating layer. The zinc-based plating layer may be a zinc-based alloy plating layer such as zinc-Ni, zinc-Fe, or zinc-Al. The plating layer may be formed on at least one surface (e.g., the rolled surface) of the steel sheet, or may be formed on both opposing surfaces, or may be formed on the entire surface of the steel sheet. Specific examples of plated steel sheets including the zinc-based plating layer include hot-dip galvanized steel sheets (GI), galvannealed hot-dip galvanized steel sheets (GA), and electrogalvanized steel sheets (EG).

[0019] 2. Chemical Composition of Steel Sheet Included in Plated Steel Sheet> The steel sheet included in the plated steel sheet according to an embodiment of the present invention (which may be, for example, the portion of the plated steel sheet excluding the plating layer) preferably contains 0.150 to 0.250 mass% C, 0.80 to 2.20 mass% Si, 1.50 to 2.80 mass% Mn, 0.15 to 1.50 mass% Cr, 0.012 to 0.100 mass% Ti, 0.0015 to 0.0100 mass% B, 0.100 mass% or less (including 0 mass%) of P, 0.050 mass% or less (including 0 mass%) of S, 0.005 to 1.000 mass% of Al, and 0.0100 mass% or less (including 0 mass%) of N, with the balance being iron and inevitable impurities. Each of the components is described in detail below.

[0020] (C: 0.150 to 0.250 mass%) C is an important element for improving the strength of steel. C is also an important element for stabilizing austenite and ensuring residual γ. Furthermore, C also has the effect of suppressing the formation of polygonal ferrite during cooling from high temperatures. In order to exert this effect, the C content is set to 0.150 mass% or more, preferably 0.170 mass% or more, and more preferably 0.190 mass% or more. On the other hand, since an excessive C content deteriorates weldability, the C content is set to 0.250 mass% or less, preferably 0.240 mass% or less, and more preferably 0.230 mass% or less.

[0021] (Si: 0.80 to 2.20 mass%) Si is a solid-solution strengthening element that contributes to increasing the strength of steel. Si also has the effect of improving temper softening resistance and suppressing the softening of martensite during tempering. Si also has the effect of suppressing the formation of carbides, condensing and stabilizing C in austenite, and is an important element for ensuring retained γ. To achieve this effect, the Si content is 0.80 mass% or more, preferably 1.00 mass% or more, and more preferably 1.20 mass% or more. On the other hand, excessive Si content causes a large amount of scale to form on the steel sheet surface during hot rolling, deteriorating the surface condition, such as causing scale marks. Therefore, the Si content is 2.20 mass% or less, preferably 2.00 mass% or less, and more preferably 1.80 mass% or less.

[0022] (Mn: 1.50 to 2.80 mass%) Mn is an important element that not only increases the strength of steel but also directly contributes to the stabilization of austenite. It is also an element that improves hardenability and has the effect of suppressing the formation of polygonal ferrite. In order to exert this effect, the Mn content is set to 1.50 mass% or more, preferably 1.70 mass% or more, and more preferably 1.90 mass% or more. On the other hand, an excessive Mn content causes adverse effects such as the occurrence of cracks in the cast slab, so the Mn content is set to 2.80 mass% or less, preferably 2.70 mass% or less, more preferably 2.60 mass% or less, and even more preferably 2.20 mass% or less.

[0023] (Cr: 0.15 to 1.50 mass%) Cr is an element that suppresses the formation of polygonal ferrite and vetic ferrite during cooling from high temperatures. Furthermore, Cr is one of the important elements because it improves tempering softening resistance and also has the effect of suppressing the softening of martensite during tempering and the decomposition of residual γ during alloying treatment. In order to exert the above-mentioned effects, the Cr content is 0.15 mass% or more, preferably 0.17 mass% or more, and more preferably 0.20 mass% or more. On the other hand, if Cr is contained in excess, not only will the effect saturate but formability will also deteriorate, so the Cr content is 1.50 mass% or less, preferably 1.20 mass% or less, and more preferably 1.00 mass% or less.

[0024] (Ti: 0.012 to 0.100 mass%) Ti refines the metal structure and contributes to improving the strength and toughness of the steel sheet. Furthermore, it is one of the important elements that binds with solute N to prevent the formation of BN. In order to exert the above-mentioned effects, the Ti content is set to 0.012 mass% or more, preferably 0.014 mass% or more, and more preferably 0.016 mass% or more. On the other hand, if Ti is contained in excess, not only will the above-mentioned effects saturate, but the yield ratio will increase and shape fixability will deteriorate, so the Ti content is set to 0.100 mass% or less, preferably 0.080 mass% or less, and more preferably 0.060 mass% or less.

[0025] (B: 0.0015 to 0.0100 mass%) B is one of the important elements that suppresses the formation of polygonal ferrite and vetic ferrite during cooling from high temperatures. To achieve the above-mentioned effect, the B content is set to 0.0015 mass% or more, preferably 0.0017 mass% or more, and more preferably 0.0020 mass% or more. On the other hand, if B is contained in excess, not only will the effect saturate but formability will also deteriorate, so the B content is set to 0.0100 mass% or less, preferably 0.0080 mass% or less, and more preferably 0.0060 mass% or less.

[0026] (P: 0.100% by mass or less (including 0% by mass)) P is an element that is inevitably present as an impurity element. P is an element that promotes grain boundary embrittlement due to grain boundary segregation and deteriorates formability. Therefore, the less P there is, the better, and the P content is 0.100% by mass or less, preferably 0.080% by mass or less, and more preferably 0.050% by mass or less. In this specification, "including 0% by mass" means that it includes embodiments in which it is not intentionally added, that is, cases in which the content is below the unavoidable impurity level (it does not exclude cases in which it is intentionally added).

[0027] (S: 0.050% by mass or less (including 0% by mass)) S is an element that is inevitably present as an impurity element. S is an element that forms sulfide-based inclusions such as MnS, which become crack initiation sites and deteriorate formability. Therefore, the lower the S content, the better, and the S content is 0.050% by mass or less, preferably 0.030% by mass or less, and more preferably 0.020% by mass or less.

[0028] (Al: 0.005 to 1.000 mass%) Al is an element that acts as a deoxidizer, and in order to exert this effect, the Al content is set to 0.005 mass% or more, preferably 0.010 mass% or more, more preferably 0.020 mass% or more, and even more preferably 0.030 mass% or more. On the other hand, if Al is contained in excess, a large amount of inclusions such as alumina is generated in the steel sheet, deteriorating formability, so the Al content is set to 1.000 mass% or less, preferably 0.800 mass% or less, and more preferably 0.500 mass% or less.

[0029] (N: 0.0100% by mass or less (including 0% by mass)) N is an element that is inevitably present as an impurity element. N is an element that forms nitrides, and these nitrides become the starting points for cracks, deteriorating formability. Therefore, the lower the N content, the better, and the N content is 0.0100% by mass or less, preferably 0.0080% by mass or less, and more preferably 0.0060% by mass or less.

[0030] The steel sheet included in the plated steel sheet according to the embodiment of the present invention preferably has the above-described chemical composition, with the balance being iron and inevitable impurities in one embodiment of the present invention. Elements introduced due to the conditions of raw materials, materials, manufacturing facilities, etc. are permitted as inevitable impurities. Note that, for example, P, S, and N, which are typically present in smaller amounts, are considered inevitable impurities, but their composition ranges are separately specified as described above. Therefore, in this specification, the term "unavoidable impurities" constituting the balance is used to refer to elements excluding those whose composition ranges are separately specified.

[0031] 3. Metallographic Structure of Steel Sheet Included in Plated Steel Sheet> The metallographic structure of the steel sheet included in the plated steel sheet according to an embodiment of the present invention has a total of 95 area % or less of bainite and tempered martensite, 5 volume % or more of retained austenite, 5 area % or less of polygonal ferrite and bainitic ferrite, and 5 area % or less of the remaining structure. Each structure will be described below.

[0032] (Total of bainite and tempered martensite is 95 area% or less) Bainite and tempered martensite are metal structures necessary for ensuring strength. However, if these metal structures are contained in excess, workability such as elongation decreases, so the total of bainite and tempered martensite is set to 95 area% or less, preferably 92 area% or less, and more preferably 90 area% or less. The lower limit of the total of these structures is preferably 50 area% or more, more preferably 60 area% or more, and even more preferably 70 area% or more.

[0033] (Residual Austenite of 5% by Volume or More) Retained austenite (hereinafter also referred to as "residual γ") is mainly present between laths in the metal structure, but may also exist in the form of clumps in aggregates of lath-shaped structures (e.g., blocks or packets) and on the grain boundaries of prior γ. This retained γ exhibits high workability, such as high elongation, by transforming into martensite when the steel sheet is deformed under strain. In other words, the presence of retained γ promotes hardening of the portion that is deformed under strain and prevents strain concentration. These effects are generally referred to as the TRIP effect, and contribute to achieving a balance between high strength and high workability. To exhibit the TRIP effect, the retained γ is set to 5% by volume or more, preferably 6% by volume or more, and more preferably 7% by volume or more, of the entire metal structure. The upper limit of the retained γ is not particularly limited, but may be 40% by area or less, 30% by area or less, or 20% by area or less.

[0034] The amount of solute carbon in the residual γ can be an indicator that affects the stability of martensitic transformation of the residual γ during deformation. By including both a predetermined amount of residual γ with a relatively low amount of solute carbon and a predetermined amount of residual γ with a relatively high amount of solute carbon, it becomes easier to achieve the desired elongation. According to one embodiment of the present invention, the residual γ preferably includes 10 to 50 volume % of residual γ with a solute carbon content of 0.9 mass % or less (hereinafter also referred to as "first residual γ") and 10 to 50 volume % of residual γ with a solute carbon content of more than 0.9 mass % and 1.1 mass % or less (hereinafter also referred to as "second residual γ"). More preferably, the residual γ includes 15 to 50 volume % of both the first residual γ and the second residual γ.

[0035] (Total of polygonal ferrite and bainitic ferrite is 5 area% or less) Polygonal ferrite and bainitic ferrite are soft structures that can reduce strength and, in some cases, can also reduce the hole expansion ratio λ. Therefore, the total of these structures is set to 5 area% or less, preferably 3 area% or less, and more preferably 1 area% or less, of the entire metal structure. The lower limit of the total of these structures is not particularly limited, and may be 0 area%.

[0036] (Remaining structure is 5% by area or less) In order to ensure high strength and high workability, the remaining structure such as fresh martensite and pearlite must be 5% by area or less in total. The lower limit of the remaining structure is not particularly limited, and may be 0% by area.

[0037] The area ratio (or volume ratio) of the metallographic structure is measured by the method described in the Examples below.

[0038] <4. Mechanical Properties of Plated Steel Sheet> The plated steel sheet according to this embodiment can exhibit high strength (high tensile strength, high yield stress) and high formability (high elongation, high hole expansion ratio). In this specification, a high-strength plated steel sheet is one having a tensile strength TS of 1150 MPa or more and a yield stress YS of 850 MPa or more. Also, in this specification, a high-formability plated steel sheet is one having an elongation EL of 14% or more and a hole expansion ratio λ of 30% or more. The tensile strength is preferably 1180 MPa or more. The yield stress is preferably 900 MPa or more. The elongation EL is preferably 15% or more. The hole expansion ratio λ is preferably 35% or more.

[0039] The thickness of the steel sheet included in the plated steel sheet according to this embodiment is not particularly limited. The thickness of the steel sheet included in the plated steel sheet according to this embodiment may be, for example, 0.8 mm or more and 2.3 mm or less. The coating weight of the plated steel sheet according to this embodiment is not particularly limited, and may be, for example, 10 to 100 g / m per side. 2 Examples include the degree of

[0040] <5. Decarburized Layer in the Surface of Steel Sheet Contained in Plated Steel Sheet> In the plated steel sheet according to this embodiment, (I) in the sheet thickness direction, the position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is preferably located in a region of 0.2% or more of the sheet thickness from the surface of the steel sheet. This position relates to the thickness of the decarburized layer that contributes to bendability. By ensuring that this position is located in a region of 0.2% or more of the sheet thickness from the surface of the steel sheet and that the decarburized layer that contributes to bendability has a certain thickness or more, it is possible to reliably exhibit excellent bendability in bending. The position where the carbon concentration (mass %) is 50% of the bulk carbon concentration may be located in a region of 0.5% or more, or even 1.0% or more of the sheet thickness from the surface of the steel sheet.

[0041] The steel sheet included in the plated steel sheet according to this embodiment preferably has the following characteristics: (II) the maximum carbon concentration (mass %) in the region from the surface of the steel sheet to 20 μm in the thickness direction is less than 70% of the bulk carbon concentration. The inventors examined steel sheets included in conventional plated steel sheets and first found that a region with a significantly high carbon concentration exists in the surface layer of the steel sheet, and that this is the cause of deterioration in bendability. Then, as described below, they investigated the manufacturing conditions of the steel sheet and found that excellent bendability can be obtained by promoting decarburization in the surface layer of the steel sheet to suppress the carbon concentration in the surface layer of the steel sheet. Specifically, they found that excellent bendability can be obtained by suppressing the maximum carbon concentration (mass %) in the region from the surface of the steel sheet to 20 μm in the thickness direction to less than 70% of the bulk carbon concentration. The maximum carbon concentration is preferably 65% ​​or less of the bulk carbon concentration, and more preferably 60% or less of the bulk carbon concentration.

[0042] From the viewpoint of exhibiting excellent bendability, the plated steel sheet according to the present embodiment preferably satisfies at least one of the above (I) and (II), and more preferably satisfies both of the above (I) and (II).

[0043] The "surface of the steel sheet" refers to the position of the interface between the plating layer and the steel sheet. In the case of a zinc-based plating, for example, the position of the interface between the plating layer and the steel sheet refers to the point at which Zn constituting the plating layer is no longer detected (the Zn analysis value is 0) when Zn is analyzed from the surface of the plating layer in the thickness direction of the plating layer by GD-OES, as measured in the examples described later, and this point is defined as the starting point of the distance (depth) from the steel sheet surface.

[0044] The plated steel sheet according to this embodiment has high tensile strength (1150 MPa or more), high yield stress (850 MPa or more), high elongation (14% or more), and high hole expansion ratio (30% or more), and further, when subjected to a bending test shown in the examples described later, can exhibit excellent bendability with an R / t of less than 2.5.

[0045] 6. Method for manufacturing plated steel sheet A method for manufacturing a plated steel sheet according to an embodiment of the present invention includes the following steps: (A) hot-rolling a steel having the above-described chemical composition to obtain a rolled sheet; (B) heating the rolled sheet to a first heating temperature of 850°C or higher; (C) holding the rolled sheet at the first heating temperature for 50 seconds or more; (D) cooling the rolled sheet after the holding step to a cooling stop temperature of 200 to 350°C, wherein the average cooling rate from the first heating temperature to 550°C is 5°C / second or higher and the average cooling rate from 550°C to the cooling stop temperature is 1°C / second or higher; (E) after the cooling step, heating the steel to a second heating temperature of 300 to 450°C and holding the temperature for 50 to 1000 seconds to obtain a steel sheet; and (F) forming a coating layer on the steel sheet. Each step is described in detail below.

[0046] (A) Step of Obtaining Rolled Plate Steel having the above-described composition is melted and cast by a conventional method, and the steel (steel slab) is subjected to a conventional hot rolling process to obtain a rolled plate. As an example, a steel (steel slab) having the above-described composition cast by a continuous casting method, an ingot method, a thin slab casting method, or the like may be reheated to about 1150 to 1300°C, hot rolled to a finish rolling temperature of about 850 to 950°C, and then coiled at about 500 to 700°C to obtain a rolled plate.

[0047] If necessary, the rolled plate may be pickled by a conventional method to remove surface scale, and if necessary, the rolled plate may be further subjected to cold rolling by a conventional method.

[0048] (B) Step of heating the rolled sheet to a first heating temperature: The rolled sheet is heated to a first heating temperature of 850°C or higher. By setting the first heating temperature to 850°C or higher, recrystallization can be promoted and the metal structure can be made uniform. The upper limit of the first heating temperature is not particularly limited, but may be, for example, 1000°C or lower.

[0049] (C) Step of holding at first heating temperature The rolled sheet is held at the first heating temperature for 50 seconds or more. By holding at the first heating temperature for 50 seconds or more, recrystallization can be promoted and the metal structure can be homogenized. The upper limit of the holding time is not particularly limited, and from the viewpoint of productivity, it may be, for example, 30 minutes or less.

[0050] After step (A), an oxidation treatment is preferably performed under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750°C (hereinafter also referred to as "step (B1)"). Step (C) preferably includes a first reduction treatment in which the dew point is -35 to -15°C, followed by a second reduction treatment in which the dew point is -25 to 0°C, which is higher than the dew point of the first reduction treatment (hereinafter also referred to as "step (C1)"). For example, the oxidation treatment in step (B1) may be performed after step (A) and before step (B), or may be performed during the temperature increase to the first heating temperature in step (B) (i.e., step (B) may include the oxidation treatment in step (B1)). The reduction treatment in step (C1) may be performed during the holding at the first heating temperature in step (C).

[0051] By subjecting the surface of a steel sheet to an oxidation treatment in step (B1), an Fe oxide layer can be formed on the surface of the steel sheet. Subsequently, by performing a reduction treatment in step (C1) in a reducing atmosphere, a decarburized layer can be formed on the surface of the steel sheet, while a reduced Fe layer capable of favorably forming, for example, a coating layer can be formed. The inventors have conducted studies and found that by performing the oxidation treatment as described above and, in the reduction treatment, defining the dew point ranges of the first and second reduction treatments and setting the dew point of the second reduction treatment higher than that of the first reduction treatment, it is possible to easily ensure the carbon concentration in the surface layer of the steel sheet described above, which enables the steel sheet to achieve high tensile strength, high yield stress, high elongation, high hole expansion ratio, and excellent bendability. Each step of the oxidation treatment and the reduction treatment will be described below.

[0052] (B1) Oxidation Treatment The oxidation treatment is preferably carried out under conditions of an oxygen concentration of 0.1 to 2%. From the viewpoint of obtaining an excellent coating appearance, the oxygen concentration is preferably 0.1% or more, more preferably 0.15% or more, and even more preferably 0.2% or more. On the other hand, if the oxygen concentration is too high, excessive oxidation can easily cause oxide scale to adhere to the rolls in the furnace, resulting in the occurrence of indentation marks on the steel sheet, a defect known as pickup. From the viewpoint of suppressing the occurrence of such defects, the oxygen concentration is preferably 2% or less, more preferably 1.7% or less, and even more preferably 1.5% or less. The concentrations of elements other than oxygen are not particularly limited. For example, CO 2 , N 2 , H 2 For example, the oxidation treatment is carried out in a direct fired furnace (DFF) type annealing furnace or the like, in a combustion gas such as coke oven gas (COG) or liquefied petroleum gas (LPG), to remove unburned O and other unavoidable impurities. 2 The treatment can be carried out in a gas atmosphere with a controlled concentration.

[0053] The oxidation treatment is preferably carried out under the condition of an ultimate temperature of 650 to 750°C. For example, heating may be carried out in an oxidation heating zone in a DFF type annealing furnace to an ultimate temperature range of 650 to 750°C. By achieving an ultimate temperature of 750°C or less, the SiO 2 on the surface of the steel sheet in the vicinity of the edge in the sheet width direction can be reduced. 2 This can suppress the reaction between the FeO and the steel sheet caused by the oxidation treatment, thereby improving the adhesion between the steel sheet and the plating layer.

[0054] In this specification, the "ultimate temperature" during heating in the oxidation treatment step means the maximum ultimate sheet temperature of the rolled sheet that is heated and controlled in the oxidation heating zone.

[0055] The temperature reached in the oxidation treatment is more preferably 730°C or lower, even more preferably 720°C or lower, and even more preferably 700°C or lower. On the other hand, from the viewpoint of forming an Fe oxide layer in the gas atmosphere, the steel sheet temperature in the oxidation treatment is preferably 650°C or higher. The steel sheet temperature in the oxidation treatment is more preferably 670°C or higher.

[0056] The temperature rise time in the oxidation treatment is not particularly limited, and may be adjusted so as not to form a fayalite layer, which would adversely affect platability, if the oxidation treatment is too long. Specifically, the temperature rise time in the oxidation treatment may be appropriately adjusted taking into consideration the hot rolling conditions (particularly the coiling temperature), the annealing conditions before pickling, the pickling conditions, and the steel sheet temperature during heating in the oxidation treatment. For example, the temperature rise time in the oxidation treatment is preferably 10 seconds or more, more preferably 15 seconds or more. Furthermore, for example, the temperature rise time in the oxidation treatment is preferably 120 seconds or less, more preferably 90 seconds or less. Note that, although the above description has been given of the case where the oxidation treatment is performed while the temperature is being raised, the mode of the oxidation treatment is not limited thereto, and the oxidation treatment may be performed by, for example, raising the temperature to the target temperature and maintaining the target temperature.

[0057] (C1) Reduction Treatment In the reduction treatment, a decarburized layer is formed on the surface layer of the steel sheet, while a reduced Fe layer that can favorably form a plating layer is formed. In the manufacturing method according to this embodiment, the reduction treatment preferably includes a first reduction treatment in which the dew point is −35 to −15° C., followed by a second reduction treatment in which the dew point is −25 to 0° C., which is higher than the dew point in the first reduction treatment. The first reduction treatment and the second reduction treatment will be described below.

[0058] (C1a) First Reduction Treatment In the first reduction treatment, the dew point is preferably set in the range of -35 to -15°C. If the dew point exceeds -15°C, decarburization is likely to proceed more than necessary, which may result in a decrease in strength. In addition, the reduction treatment becomes difficult to proceed, and a defect called pickup is likely to occur, in which iron oxide produced in the oxidation treatment adheres to the rolls and causes pressure scratches on the steel sheet. Therefore, the dew point is preferably set to -15°C or lower. A dew point of -20°C or lower is more preferable. On the other hand, from the viewpoint of suppressing the need for additional equipment and costs, the dew point in the first reduction treatment is preferably set to -35°C or higher. A dew point of -30°C or higher is more preferable.

[0059] The dew point may be within the above range in the atmosphere at the center of the front stage of the reduction zone where the first reduction treatment is performed. The dew point in the first reduction treatment and the second reduction treatment described below can be controlled, for example, by introducing water vapor gas and mixing it with the atmospheric gas in the furnace, or by bubbling the atmospheric gas to mix water vapor therein.

[0060] The atmosphere of the first reduction treatment satisfies the above dew point and contains N 2 , H 2 , CO, H 2 O, O 2 and other unavoidable impurities. In the first reduction treatment, after the steel sheet reaches a temperature of 800°C in the atmosphere, the steel sheet is heated in a temperature range of 850 to 920°C for, for example, 60 to 240 seconds. The "holding" mentioned above includes not only a constant temperature but also a case where the temperature fluctuates within the temperature range.

[0061] (C1b) Second Reduction Treatment Next, the dew point in the second reduction treatment will be described. FIG. 1 is a graph created using a reference example described later, showing the relationship between the dew point at the center of the soaking zone during the second reduction treatment and R / t. From FIG. 1, it can be seen that in order to achieve excellent bendability with an R / t of less than 2.5, the dew point in the second reduction treatment needs to be −25° C. or higher. On the other hand, the upper limit of the dew point in the second reduction treatment is preferably 0° C. or lower in order to exhibit higher strength. The dew point in the second reduction treatment is more preferably −15° C. or lower.

[0062] The atmosphere of the second reduction treatment satisfies the above dew point and contains N 2 , H 2 , CO, H 2 O, O 2 and other unavoidable impurities. In the second reduction treatment, the steel sheet is heated in the above atmosphere in a temperature range in which the steel sheet reaches a temperature of 850 to 920°C for, for example, 60 to 240 seconds. The "holding" mentioned above includes not only a constant temperature but also a case in which the temperature fluctuates within the above temperature range.

[0063] The first reduction treatment and the second reduction treatment may be performed in separate atmospheres having different dew points as described above, and the specific embodiment is not limited thereto. For example, a reduction furnace for performing each of the first reduction treatment and the second reduction treatment may be provided. In addition, when the steel sheet is a plated steel sheet, a partition wall having an opening area ratio of 20% or less may be provided midway in the reduction zone of the continuous hot-dip galvanizing line to separate the first reduction treatment from the second reduction treatment.

[0064] Between the first reduction treatment and the second reduction treatment, for example, a holding step for maintaining at least one of the conditions (dew point, etc.) of the first reduction treatment may be inserted, as long as it does not adversely affect the securing of the decarburized state of the steel sheet according to this embodiment. Preferably, the second reduction treatment is performed subsequent to the first reduction treatment.

[0065] The oxidation treatment and reduction treatment may be carried out using any known single or multiple pieces of equipment. Preferably, from the viewpoints of production efficiency, cost, and quality maintenance, a continuous hot-dip galvanizing line (CGL) is used. By using a continuous hot-dip galvanizing line, oxidation treatment and reduction treatment by an oxidation-reduction method, and hot-dip galvanizing treatment and alloying treatment when producing, for example, a galvanized steel sheet as a steel sheet, can be carried out continuously in a single production line. More specifically, oxidation treatment and reduction treatment by an oxidation-reduction method can be carried out, for example, using an annealing furnace in a DFF-type continuous hot-dip galvanizing line. The oxidation treatment can be carried out, for example, in the heating zone of a DFF-type annealing furnace, as described above. The reduction treatment can be carried out, for example, in the soaking zone of a DFF-type annealing furnace.

[0066] (D) Step of cooling to a cooling stop temperature after step (C): After step (C), the material is cooled at a predetermined cooling rate to a cooling stop temperature of 200 to 350°C. First, the average cooling rate from the first heating temperature to 550°C (hereinafter also referred to as the "first average cooling rate") is 5°C / second or more. If the first average cooling rate is less than 5°C / second, there is a risk of excessive formation of polygonal ferrite. The first average cooling rate is preferably 7°C / second or more. There is no particular upper limit to the first average cooling rate, but from the viewpoint of ease of control, it may be, for example, 100°C / second or less.

[0067] Next, the average cooling rate from 550°C to the cooling stop temperature (200 to 350°C) (hereinafter also referred to as the "second average cooling rate") is 1°C / second or more. If the second average cooling rate is less than 1°C / second, there is a risk of excessive bainitic ferrite being generated. The second average cooling rate is preferably 2°C / second or more. There is no particular upper limit to the second average cooling rate, but from the viewpoint of ease of control, it may be, for example, 100°C / second or less. Furthermore, if the cooling stop temperature is less than 200°C, the amount of martensite becomes excessive and there is a risk that the amount of retained austenite cannot be sufficiently secured. If it exceeds 350°C, there is a risk that the amount of martensite cannot be sufficiently secured and that residual structures such as fresh martensite and pearlite become excessive.

[0068] Furthermore, the average cooling rate from 400°C to the cooling stop temperature (hereinafter also referred to as the "third average cooling rate") is preferably 40°C / sec or less, which promotes C enrichment in untransformed austenite due to bainite transformation, stabilizes the residual γ, and makes it easier to ensure a predetermined amount of the first residual γ, which has a relatively low amount of solute C.

[0069] (E) After step (D), the steel sheet is heated to a second heating temperature to obtain the steel sheet. After step (D), the steel sheet is heated (reheated) to a second heating temperature of 300°C to 450°C and held for 50 to 1000 seconds to obtain the steel sheet used in the plated steel sheet according to the embodiment of the present invention. This step promotes bainite transformation and C enrichment in untransformed austenite, thereby ensuring a sufficient amount of retained austenite and further facilitating the securing of a predetermined amount of second retained γ with a relatively stable high amount of solute C. If the second heating temperature is outside the above temperature range or the holding time is less than 50 seconds, the amount of retained austenite may not be sufficient. On the other hand, if the holding time is too long, the above effects saturate, so it is preferable to set the holding time to 1000 seconds or less. The metal structure specified in the embodiment of the present invention is obtained mainly through steps (D) and (E).

[0070] (F) Step of forming a plating layer on the steel sheet The above-mentioned plating layer is formed on the surface of the steel sheet. The conditions for forming the plating layer are not particularly limited, and a conventional plating process can be used. For example, when forming a hot-dip galvanized layer, the hot-dip galvanizing process may be performed by immersing the steel sheet in a hot-dip galvanizing bath at a temperature of 300°C or higher and 550°C or lower. The plating time may be adjusted as appropriate to ensure the desired coating weight, and is preferably set to, for example, 1 to 10 seconds.

[0071] For alloying hot-dip galvanizing, an alloying treatment may be performed after the above-mentioned hot-dip galvanizing. The alloying treatment temperature is not particularly limited, but if the alloying treatment temperature is too low, alloying does not proceed sufficiently, so it is preferably 450°C or higher, more preferably 460°C or higher, and even more preferably 480°C or higher. However, if the alloying treatment temperature is too high, alloying proceeds excessively, resulting in an excessive Fe concentration in the coating layer and deterioration of coating adhesion. From this perspective, the alloying treatment temperature is preferably 550°C or lower, more preferably 540°C or lower, and even more preferably 530°C or lower. The alloying treatment time is not particularly limited, and may be adjusted so that the hot-dip galvanizing is alloyed. The alloying treatment time is, for example, 10 to 60 seconds.

[0072] The method for manufacturing a plated steel sheet according to an embodiment of the present invention may include other steps within the scope of the present disclosure.

[0073] The following examples are provided to more specifically describe the embodiments of the present invention. The embodiments of the present invention are not limited to the following examples, and may be modified as appropriate within the scope of the above-described and below-described aims, and all such modifications are within the technical scope of the embodiments of the present invention.

[0074] A steel (steel slab) having the chemical composition shown in Table 1 was heated at 1250°C for 30 minutes, then hot-rolled to a reduction of approximately 90% and a finish rolling temperature of 920°C. The slab was then cooled to 660°C, coiled, and then cooled to room temperature to obtain a rolled plate having a thickness of 1.8 to 2.6 mm. The obtained rolled plate was pickled to remove surface scale, and then cold-rolled to a thickness of 1.0 to 1.6 mm. In Table 1, "-" indicates that the element was not intentionally added. In the following tables, values ​​marked with * indicate that the element is outside the range of the embodiment of the present invention.

[0075]

[0076] The above-described step (B1) and steps (B) to (F) were performed on the rolled sheet to obtain plated steel sheets of Test Nos. 1 to 17. The conditions for each step are shown in Table 2. Although not shown in Table 2, in Test Nos. 11 to 14, step (B1) was performed during the temperature increase to the first heating temperature in step (B), with an oxygen concentration of 0.1 to 2%, an ultimate temperature of 650 to 750°C, and a temperature increase time in the oxidation treatment of 10 to 120 seconds. Step (C) included a reduction step (C1) in which a first reduction treatment (C1a) with a dew point of −35 to −15°C was performed, followed by a second reduction treatment (C1b) with a dew point higher than that of the first reduction treatment. The heating times (holding times) for the first reduction treatment and the second reduction treatment were each 60 seconds or longer. Although not shown in Table 2, in Test Nos. 11 to 14, step (B1) was performed during the temperature increase to the first heating temperature in step (B), with an oxygen concentration of 0.1 to 2%, an ultimate temperature of 650 to 750°C, and a temperature increase time in the oxidation treatment of 10 to 120 seconds. In Nos. 1 to 17, in step (F), a galvannealed layer was formed by a known method. Specifically, in step (F), the steel sheet was immersed in a galvannealing bath at a temperature of 300°C or higher and 550°C or lower to perform galvannealing treatment (galvanizing time: 1 to 10 seconds), and then subjected to alloying treatment, with the alloying treatment temperature being 480 to 500°C and the alloying treatment time being 20 to 25 seconds.

[0077]

[0078] The steel sheets of Test Nos. 1 to 17 described above were evaluated as follows.

[0079] <Metal structure evaluation> A test specimen was taken from the center of the steel sheet in the direction perpendicular to the rolling direction and thickness direction (sheet width direction), and a cross section parallel to the rolling direction and sheet width direction, located ¼ of the sheet thickness from the steel sheet surface, was exposed by electrolytic polishing or the like. The cross section was observed using an SEM, and the area fractions of polygonal ferrite, bainitic ferrite, MA, and pearlite were measured. The sum of the area fraction of bainite and the area fraction of tempered martensite was calculated by subtracting the sum of the area fractions of polygonal ferrite, bainitic ferrite, MA, and pearlite from 100 area %.

[0080] The volume fraction of retained γ in the metal structure constituting the steel sheet was measured by X-ray diffraction. Specifically, an X-ray diffraction pattern was obtained from the cross section using an X-ray source: Co-Kα, and the volume fraction of retained γ relative to the entire metal structure was measured based on a known method (ISIJ Int. Vol. 33. (1993), No. 7, p. 776).

[0081] The area fraction of fresh martensite in the remaining structure was calculated by subtracting the volume fraction (≒area fraction) of the retained γ from the area fraction of MA, assuming that the volume fraction of the retained γ is the area fraction. The proportions of the first retained γ and the second retained γ to the total retained γ were calculated as follows.

[0082] First, the carbon concentration distribution of the residual γ was determined using the three diffraction peaks of (200)γ, (220)γ, and (311)γ measured with the above-mentioned X-ray diffractometer. Figure 2 is a schematic diagram of an X-ray diffraction pattern. As shown in Figure 2, for the three diffraction peaks of (200)γ, (220)γ, and (311)γ, the 2θ (2θ avg (hkl)) and its half width Δ2θ(hkl) were determined. Here, (hkl) means (200), (220), or (311) (the same applies below).

[0083] Next, the above 2θ avg From (hkl), d(hkl) was calculated from the following formula (1) using the Bragg condition: λ = 2d sin θ (d: lattice spacing, λ: wavelength of Co-Kα radiation). avg(hkl) / 2)} ...(1)

[0084] The lattice constants a0(hkl) were calculated using the following formula (2), and the arithmetic average of the lattice constants a0 was calculated. a0(hkl)=d(hkl)√(h 2 +k 2 +l 2 ) ... (2)

[0085] The carbon concentration % C is calculated using the following formula (3): avg (unit: mass%) was calculated. avg =(1 / 0.033)×(a0-3.572)...(3)

[0086] Next, the half-value width Δ%C of the carbon concentration distribution of the residual γ was determined by the following procedure.

[0087] First, the diffraction angles at the upper and lower limits of the half-width Δ2θ(hkl) of the diffraction angle 2θ(hkl) of each peak were calculated using the following formulas (4) and (5) (see FIG. 2): 2θL(hkl)=2θ avg (hkl) - Δ2θ (hkl) / 2 ... (4) 2θH (hkl) = 2θ avg (hkl)+Δ2θ(hkl) / 2...(5)

[0088] Using the above 2θL(hkl) and 2θH(hkl), the upper and lower limits of the half-width of the carbon concentration distribution, %CL and %CH, were determined using the Bragg conditions and the above formulas (1) to (3) in the same manner as above. The half-width of the carbon concentration distribution, Δ%C, was then determined using the following formula (6): Δ%C=%CH-%CL (6)

[0089] Assuming that the carbon concentration distribution is a normal distribution, the standard deviation σ %C was calculated from the half-width Δ%C as follows. That is, the probability density function f(x) of the normal distribution is expressed by the following formula (7) using the mean value u and the standard deviation σ. f(x) = {1 / √(2πσ 2 )}×exp{-(xu) 2 / (2σ 2 ) ... (7)

[0090] The probability f(u) at the average value was calculated by substituting x=u into the above formula (7) using the following formula (8): f(u)=1 / √(2πσ2 ) ... (8)

[0091] Average value u = % C avg The probability density f(%C) at a value (%C ±Δ%C / 2) shifted up or down by 1 / 2 of the half-width Δ%C from avg ±Δ%C / 2) is the average value u = %C avg Probability f(u) = f(%C avg ), and therefore, from the above formulas (7) and (8), the relationship of the following formula (9) is obtained: {1 / √(2πσ%C 2 )}×exp{-(Δ%C / 2) 2 / (2σ%C 2 )}=1 / {2 √(2πσ%C 2 ) ... (9)

[0092] By transforming the above formula (9), the following formula (10) is derived as a formula for calculating the standard deviation σ%C from the half-height width Δ%C, and the standard deviation σ%C was calculated by substituting the half-height width Δ%C into this formula (10). σ%C = √{(Δ%C / 2) 2 / (2ln2)} ...(10)

[0093] The average value %C of the carbon concentration distribution in the residual γ obtained as described above avg Using the cumulative distribution function g(x) shown in the following formula (11) and the standard deviation σ%C, the following formula (12) was derived as a formula for finding the volume fraction VγR(C≦1.0%) of residual γ with a carbon concentration of 1.0 mass% or less relative to the entire metal structure, and VγR(C≦1.0%) was calculated using this formula (12): g(x)=(½)×[1+erf{(x−u) / √(2σ 2 )}]...(11) VγR(C≦1.0%)=VγR×g(1.0)=VγR×(1 / 2)×[1+erf{(1.0-%C avg ) / √(2σ%C 2 )] ... (12)

[0094] The average value %C of the carbon concentration distribution in the residual γ obtained as described above avgUsing the cumulative distribution function g(x) shown in the above formula (11) and the standard deviation σ%C, the following formulas (13) and (14) were derived to calculate the volume fractions VγR(C≦0.9%) and VγR(0.9%<C≦1.1%) of residual γ with carbon concentrations of 0.9 mass% or less and more than 0.9 mass% and 1.1 mass% or less relative to the entire metal structure, respectively. After calculating VγR(C≦0.9%) using these formulas (13) and (14), the proportions of each of these to the total residual γ volume fraction were determined. VγR(C≦0.9%) = VγR×g(0.9) = VγR×(½)×[1+erf{(0.9−%C avg ) / √(2σ%C 2 )}]...(13) VγR (0.9%<C≦1.1%)=VγR×g(1.2)−VγR(C≦0.9%)=VγR×(1 / 2)×[1+erf{(1.1−%C avg ) / √(2σ%C 2 )}]-VγR×(1 / 2)×[1+erf{(0.9-%C avg ) / √(2σ%C 2 )] ... (14)

[0095] In addition, no structure other than fresh martensite and pearlite was observed in the remaining structure.

[0096] <Means for Measuring Decarburization Behavior: Measurement of Carbon Profile by GD-OES> As described below, carbon profile was measured by GD-OES (Glow Discharge Optical Emission Spectrometry) to examine the decarburization behavior.

[0097] (Sample Preparation) Materials measuring 50 mm x 40 mm x thickness or 30 mm x 30 mm x thickness were collected. They were then degreased as per usual methods to prepare samples. Using these samples, the mass % concentration of each element was measured using GD-OES under the following conditions.

[0098] (Measurement conditions) Equipment used: Marcus-type radio frequency glow discharge optical emission surface analyzer (rf-GD-OES) GD-Profiler 2 manufactured by HORIBA, Ltd. Sputtering method: normal sputtering Measurement range: φ4 mm Type of gas: Ar Elements to be analyzed: B, C, O, Al, Si, Ti, Cr, Mn, Fe, Zn, P, S, N (In this example, the evaluation was performed on these elements, but if elements other than those mentioned above are contained in, for example, the plating layer and / or the steel sheet, the elements other than those mentioned above will also be analyzed.)

[0099] (Measurement Method) GD-OES measurements were carried out on the plated surface of the sample up to a depth of 150 μm in the thickness direction.

[0100] (Analysis Method) Since the sputtering rate of the above-mentioned device is almost constant, the sputtering crater depth of the sample was measured after the analysis was completed, and the value (sputtering depth) was plotted on the horizontal axis.

[0101] The details of the calibration curve method for converting the measured emission intensity of each element into a concentration are shown below.

[0102] Sputter weight W of element i per unit time i (g / sec) and luminescence intensity I i The relationship between W and W is expressed by the following formula (15) using the slope a and intercept b of the calibration curve. i = aI i + b (15) Sputter weight W of the element i per unit time i is the concentration C i (wt.%), density ρ (g / cm 3 ), and for a reference sample with a known sputtering rate Δd (cm / sec), the sputtering area S (cm 2 ) and is calculated by the following formula (16): i =C i ×ρ×Δd×S (16)

[0103] W i Using two or more reference samples with known emission intensities I iThe slope a and intercept b of the above formula (15) were determined, and a calibration curve was created with the horizontal axis representing the emission intensity and the vertical axis representing the spatter weight. The reference samples used are shown in Table 3 below. Using the created calibration curve, the spatter weight was determined from the emission intensity of each target element, and the weight ratio was used to convert it into a concentration. The calibration curve used to convert the O concentration was 2 Correction was performed using the formula so that the concentration ratio of Si to O became 1:2.

[0104]

[0105] The carbon analysis results were used to obtain carbon profiles, an example of which is shown in Figure 3. Figure 3 shows the carbon profiles of Test No. 12 and Test No. 14. It can be seen from Figure 3 that the carbon profiles of all materials have a carbon concentration peak within the surface layer of 20 µm (specifically, in the internal oxide layer), but that in Test No. 14 the carbon concentration is higher than the bulk carbon concentration, whereas in Test No. 12 the carbon concentration is kept sufficiently lower than the bulk carbon concentration.

[0106] From the obtained carbon concentration profile in the sheet thickness direction, the position where the carbon concentration (mass%) was 50% of the bulk carbon concentration and the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm were determined. Note that the bulk carbon concentration was corrected for analysis so that the carbon concentration at a sufficiently deep position (120 to 150 μm) measured by GD-OES was the value obtained by conventional steel analysis. For example, if the steel analysis value was 0.22% and the GD-OES analysis value was 0.25%, the GD-OES analysis value was multiplied by 0.22 / 0.25 and used for analysis.

[0107] <Evaluation of Tensile Strength, Yield Stress, and Elongation> JIS No. 5 test pieces (plate-shaped test pieces) were taken so that the longitudinal direction of the test piece was perpendicular to the rolling direction in a plane parallel to the cold-rolled rolling surface of the steel sheet. A tensile test was performed using the test piece to measure the tensile strength TS, yield stress YS, and elongation EL. Examples in which the tensile strength TS was 1150 MPa or more were evaluated as sufficient, and examples in which it was less than 1150 MPa were evaluated as insufficient. Examples in which the yield stress YS was 850 MPa or more were evaluated as sufficient, and examples in which it was less than 850 MPa were evaluated as insufficient. Examples in which the elongation EL was 14% or more were evaluated as sufficient, and examples in which it was less than 14% were evaluated as insufficient.

[0108] <Hole Expanding Ratio Evaluation> Test pieces measuring 90 mm x 90 mm x 100 mm were taken from each cold-rolled steel sheet. Using the test pieces, a hole expanding test was performed based on JIS Z 2256:2010 to measure the hole expanding ratio λ. Examples where the hole expanding ratio λ was 30% or more were evaluated as sufficient, and examples where the hole expanding ratio λ was less than 30% were evaluated as insufficient.

[0109] <Bendability (R / t) Evaluation> The bendability of the steel sheets was evaluated by the following procedure. Test pieces with a width of 40 mm and a length of 100 mm were prepared with the major axis taken perpendicular to the rolling direction, and a bending test was performed using the V-block method in accordance with JIS Z 2248:2014. The bending radius was varied from 0 to 7 mm to determine the minimum bending radius at which the material could be bent without breaking. This was taken as the bending radius R (mm), and the bending radius R (mm) / sheet thickness t (mm) was calculated. Examples where the bending radius R (mm) / sheet thickness t (mm) was less than 2.5 were evaluated as having excellent bendability (◯), and examples where it was 2.5 or more were evaluated as having poor bendability (×).

[0110] The results are shown in Table 4. In Table 4, "PF + BF" is the sum of the area fraction of polygonal ferrite and the area fraction of bainitic ferrite, "B + M" is the sum of the area fraction of bainite and the area fraction of tempered martensite, "residual γ" is the volume fraction of all retained austenite, "first residual γ / residual γ" is the ratio (volume %) of the first residual γ to all retained γ, "second residual γ / residual γ" is the ratio (volume %) of the second residual γ to all retained γ, "residual structure" is the area fraction of the residual structure, and "maximum surface layer carbon concentration" is the maximum carbon concentration (mass %) in the region from the surface of the steel sheet to 20 μm in the sheet thickness direction. The composition shown in Table 4 is a partial excerpt of the composition shown in Table 1 to clarify the differences between Test Nos. 1 to 17. The residual structure was fresh martensite and pearlite.

[0111]

[0112] The results in Table 4 can be considered as follows. Test Nos. 1 to 14 in Table 4 all satisfied the requirements specified in the embodiments of the present invention, were easier to manufacture, and exhibited high strength and high workability. Furthermore, when comparing Test Nos. 11 to 14, Test Nos. 11 to 13 satisfied the preferred requirements specified in the embodiments of the present invention and had excellent bendability. On the other hand, Test Nos. 15 to 17 in Table 4 all did not satisfy the requirements specified in the embodiments of the present invention and had insufficient strength and / or workability.

[0113] In Test No. 15, the Si content was less than 0.80 mass % and the residual γ was less than 5 volume %, so the tensile strength was less than 1150 MPa and the elongation was less than 14%.

[0114] In Test No. 16, the Cr content was less than 0.15% by mass and the total area of ​​polygonal ferrite and bainitic ferrite was more than 5%, so the tensile strength was less than 1150 MPa.

[0115] Test No. 17 did not contain B, and the total of polygonal ferrite and bainitic ferrite exceeded 5 area%, so the tensile strength was less than 1150 MPa, the yield stress was less than 850 MPa, and the hole expansion ratio λ was less than 30%.

[0116] [Reference Example] Hereinafter, a Reference Example will be described in which the relationship between the above requirements (I) and (II) and bendability was investigated in more detail. As a sample for annealing, a base sheet was prepared having a bulk carbon concentration, i.e., a C content of the steel sheet (base sheet) of 0.22 mass% (0.22 mass% C), a Si content of 1.7 mass%, a Mn content of 2.0 mass%, a Cr content of 0.5 mass%, an Al content of 0.04 mass%, and the balance being Fe and inevitable impurities (note that "unavoidable impurities" here can include P: more than 0 mass% but not more than 0.1 mass%, S: more than 0 mass% but not more than 0.05 mass%, and N: more than 0 mass% but not more than 0.01 mass%), a structure of ferrite and pearlite, and a strength of 700 to 800 MPa.

[0117] The annealing samples were subjected to oxidation treatment and reduction treatment using an actual machine. Specifically, the oxidation treatment was performed at the oxygen concentration and ultimate temperature shown in Table 5, and then the first reduction treatment (heating zone) and the second reduction treatment (soaking zone) shown in Table 5 were performed in this order under the conditions (ultimate temperature, dew point) shown in Table 5.

[0118] The steel sheet after the second reduction treatment was cooled to 460°C and then immersed in an Al-Zn plating bath containing 0.08 to 0.13 mass% of Al (Al is effective Al%, plating bath temperature is 460 to 480°C) to perform galvanization. The coating weight was 40 g / m by gas wiping. 2 90g / m or more 2 The conditions were controlled as follows, and then alloying treatment was carried out at 480 to 490°C for 20 to 30 seconds to obtain galvannealed steel sheets.

[0119]

[0120] The obtained plated steel sheets were subjected to carbon profile measurement using the GD-OES described above. From the obtained carbon concentration profile in the sheet thickness direction, the position where the carbon concentration (mass%) was 50% of the bulk carbon concentration and the maximum carbon concentration (mass%) in a region extending 20 μm from the steel sheet surface were determined. Note that the bulk carbon concentration was corrected for analysis so that the carbon concentration measured by GD-OES at a sufficiently deep position (120 to 150 μm) was the value obtained by conventional steel analysis. For example, if the steel analysis value was 0.22% and the GD-OES analysis value was 0.25%, the GD-OES analysis value was multiplied by 0.22 / 0.25 and used for analysis.

[0121] Furthermore, the resulting plated steel sheets were evaluated for limit bending strength (R / t) as described below.

[0122] [Evaluation of limit bending property (R / t)] The bendability of the steel sheet was evaluated by the following procedure. Test pieces with a width of 40 mm and a length of 100 mm, with the major axis perpendicular to the rolling direction, were prepared, and a bending test was performed using the V-block method in accordance with JIS Z 2248:2014. In the bending test, the bending radius was varied from 0 to 7 mm to determine the minimum bending radius at which the material could be bent without breaking. This was taken as the limit bending radius R (mm), and the ratio of limit bending radius R (mm) to sheet thickness t (mm) was calculated. A ratio of limit bending radius R (mm) to sheet thickness t (mm) of less than 2.5 was evaluated as having excellent bendability, and a ratio of 2.5 or more was evaluated as having poor bendability.

[0123]

[0124] Based on the results of Table 6 above, a graph showing the relationship between the position where the carbon concentration (mass %) in the sheet thickness direction is 50% of the bulk carbon concentration and R / t is shown in Figure 4. It can be seen from Figure 4 that in order to achieve excellent bendability with an R / t of less than 2.5, the position where the carbon concentration (mass %) in the sheet thickness direction is 50% of the bulk carbon concentration should be in a region that is 0.20% or more of the sheet thickness from the surface of the steel sheet.

[0125] Based on the results of Table 6 above, a graph showing the relationship between R / t and the ratio of the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm, relative to the bulk carbon concentration, is shown in Figure 5. From Figure 5, it can be seen that in order to achieve excellent bendability with an R / t of less than 2.5, it is best to set the ratio of the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm, relative to the bulk carbon concentration, to less than 70%.

[0126] This application claims priority from Japanese Patent Application No. 2023-056175, filed March 30, 2023, and Japanese Patent Application No. 2024-022773, filed February 19, 2024. Japanese Patent Application Nos. 2023-056175 and 2024-022773 are incorporated herein by reference.

Claims

1. A plated steel sheet comprising a steel sheet and a plating layer disposed on a surface of the steel sheet, the plated steel sheet having a tensile strength of 1150 MPa or more, the steel sheet contained in the plated steel sheet has a component composition consisting of: C: 0.150 to 0.250 mass%, Si: 0.80 to 2.20 mass%, Mn: 1.50 to 2.80 mass%, Cr: 0.15 to 1.50 mass%, Ti: 0.012 to 0.100 mass%, B: 0.0015 to 0.0100 mass%, P: 0.100 mass% or less (including 0 mass%), S: 0.050 mass% or less (including 0 mass%), Al: 0.005 to 1.000 mass%, N: 0.0100 mass% or less (including 0 mass%), and the balance: iron and inevitable impurities; and A plated steel sheet having a metal structure in which a total of bainite and tempered martensite is 95 area % or less, retained austenite is 5 volume % or more, a total of polygonal ferrite and bainitic ferrite is 5 area % or less, and a remaining structure is 5 area % or less.

2. The plated steel sheet according to claim 1, wherein in the sheet thickness direction, a position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is located in a region that is 0.2% or more of the sheet thickness from the surface of the steel sheet.

3. The plated steel sheet according to claim 1, wherein the maximum carbon concentration (mass%) in the region extending from the surface of the steel sheet to 20 μm in the sheet thickness direction is less than 70% of the bulk carbon concentration.

4. The plated steel sheet according to claim 1, wherein the retained austenite contains 10 to 50 volume % of first retained austenite having a solute C amount of 0.9 mass % or less, and 10 to 50 volume % of second retained austenite having a solute C amount of more than 0.9 mass % and 1.1 mass % or less.

5. A method for producing a plated steel sheet according to any one of claims 1 to 4, comprising the steps of: hot rolling a steel having the chemical composition according to claim 1 to obtain a rolled sheet; heating the rolled sheet to a first heating temperature of 850°C or more; after the heating step, holding the sheet at the first heating temperature for 50 seconds or more; after the holding step, cooling the sheet to a cooling stop temperature of 200 to 350°C, wherein an average cooling rate from the first heating temperature to 550°C is 5°C / second or more and an average cooling rate from 550°C to the cooling stop temperature is 1°C / second or more; after the cooling step, heating the sheet to a second heating temperature of 300°C to 450°C and holding the temperature for 50 to 1000 seconds to obtain a steel sheet; and forming a plating layer on the steel sheet.

6. The manufacturing method according to claim 5, further comprising, after the step of obtaining the rolled plate, performing an oxidation treatment under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750°C, and the holding step includes performing a first reduction treatment having a dew point of -35 to -15°C, followed by a second reduction treatment having a dew point of -25 to 0°C, which is higher than that of the first reduction treatment.

7. The manufacturing method according to claim 5, wherein the cooling step is performed at an average cooling rate of 40°C / sec or less from 400°C to the cooling stop temperature.

Citation Information

Patent Citations

  • Method for generating scan data and method for creating printed material

    JP2023056175A

  • Displacement detection method, displacement detection device and machine tool

    JP2024022773A

  • High-strength steel sheet and manufacturing method therefor

    WO2019159771A1

  • Steel sheet and manufacturing method therefor

    WO2020080401A1

  • Steel sheet and manufacturing method therefor

    WO2020080402A1