Method for storing ether group-containing polyvalent unsaturated compound composition, ether group-containing polyvalent unsaturated compound composition, monomer composition, tetrahydropyran ring polymer, photosensitive resin composition, cured product, member for display device, and method for producing same
The method of dissolving ether group-containing polyunsaturated compounds in non-aqueous solvents with temperature control and a polymerization inhibitor addresses storage stability issues, preventing filter clogging and ensuring efficient industrial-scale production by maintaining stability across temperature variations.
Patent Information
- Application Number
- PCT/JP2024/011307
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Ether group-containing polyunsaturated compounds have low storage stability, leading to the formation of insoluble foreign substances that cause filter clogging during storage, especially at varying temperatures, which hampers industrial-scale production efficiency.
A method involving dissolving ether group-containing polyunsaturated compounds in non-aqueous solvents with specific temperature control and the inclusion of a polymerization inhibitor to prevent the formation of microscopic insoluble foreign substances, ensuring stable storage and preventing filter clogging.
The method effectively suppresses filter clogging and maintains storage stability across temperature fluctuations, enabling efficient handling and production of ether group-containing polyunsaturated compounds on an industrial scale.
Smart Images

Figure JP2024011307_03102024_PF_FP_ABST
Abstract
Description
Method for storing ether group-containing polyunsaturated compound composition, ether group-containing polyunsaturated compound composition, monomer composition, tetrahydropyran ring polymer, photosensitive resin composition, cured product, member for display device, and method for manufacturing the same
[0001] The present invention relates to a method for storing an ether group-containing polyunsaturated compound composition, an ether group-containing polyunsaturated compound composition, a monomer composition, a tetrahydropyran ring polymer, a photosensitive resin composition, a cured product, a member for a display device, and a method for producing the same.
[0002] It has been known that compounds having a structure in which α-hydroxymethylacrylic acid or its ester is ether-dimerized (hereinafter also referred to as ether dimer) undergo cyclopolymerization via radical polymerization to form polymers containing a tetrahydropyran ring in the main chain. Such polymers have excellent transparency and heat resistance, and are used in various applications such as resist materials and coating materials.
[0003] Various resin compositions using such ether dimers are known. For example, Patent Document 1 describes a curable resin composition that contains a polymer obtained by polymerizing a monomer component containing an ether dimer and a curing component made of a polyfunctional (meth)acrylate and / or a compound having an epoxy group, and that can form a coating film that is excellent in both heat resistance and transparency.
[0004] On the other hand, although ether dimers have high radical polymerizability, they have a problem of low storage stability, and ether dimers with excellent storage stability have been investigated (Patent Document 2).
[0005] JP 2004-300204 A JP 2014-148610 A
[0006] Polymerizable compounds having unsaturated groups symmetrically arranged around an ether bond, such as ether dimers (hereinafter referred to as "ether group-containing polyunsaturated compounds"), are stored in a solution containing a stabilizer such as a polymerization inhibitor, as described in Patent Document 2. However, when a solution of the ether group-containing polyunsaturated compound is stored at temperatures below about 10°C in winter, crystals of the ether group-containing polyunsaturated compound precipitate and accumulate at the bottom of the container. When a solution containing precipitated crystals is stored at temperatures of about 30 to 40°C in summer, some of the ether group-containing polyunsaturated compound crosslinks, generating a large amount of minute insoluble foreign matter in the solution. When a monomer mixture containing such minute insoluble foreign matter is introduced into a reaction vessel, the filter in the introduction line clogs, causing a problem of blockage.
[0007] Therefore, when handling ether group-containing polyunsaturated compounds in a factory, it is preferable to keep the storage period as short as possible and quickly polymerize them to convert them into tetrahydropyran ring polymers, etc. In this case, it is not possible to produce a large amount of ether group-containing polyunsaturated compounds at once, resulting in poor production efficiency, particularly when producing them on an industrial production scale (e.g., 50 liters to 50 m 3 However, there is still room for further improvement in the method for storing ether group-containing polyunsaturated compounds in the above-mentioned storage tank.
[0008] In view of the above-mentioned current situation, the present invention aims to provide a method for storing a composition containing an ether group-containing polyunsaturated compound, which can suppress filter clogging caused by the generation of minute insoluble foreign matter.
[0009] In order to solve the above-mentioned problems, the present inventors have conducted various studies on methods for storing ether group-containing polyunsaturated compound compositions, and have found that by containing a specific range of amounts of an ether group-containing polyunsaturated compound, a polymerization inhibitor, and a non-aqueous solvent, and dissolving the precipitated ether group-containing polyunsaturated compound under specific temperature conditions, it is possible to prevent clogging of the filter caused by the generation of minute insoluble foreign matter, even when the composition is stored in the summer, and have completed the present invention.
[0010] That is, the present invention includes the following aspects: [1] A method for storing an ether group-containing polyunsaturated compound composition, the composition comprising an ether group-containing polyunsaturated compound (A) represented by the following general formula (1), a polymerization inhibitor (B), and a non-aqueous solvent (C), the content of the compound (A) being 5 to 50 mass% relative to 100 mass% of the composition, and the method comprising a dissolving step of dissolving the compound (A) precipitated in the composition at a temperature at least 5°C higher than the precipitation temperature of the compound (A):
[0011]
[0012] (In formula (1), R 1 and R 2each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms, which may have a substituent.) [2] The method for storing an ether group-containing polyunsaturated compound composition according to [1] above, wherein the dissolving step is a step of dissolving the precipitated ether group-containing polyunsaturated compound (A) by stirring the ether group-containing polyunsaturated compound composition. [3] The method for storing an ether group-containing polyunsaturated compound composition according to [1] or [2] above, wherein the storage method is a method for storing 50 liters or more of the ether group-containing polyunsaturated compound composition. [4] The method for storing an ether group-containing polyunsaturated compound composition according to any one of [1] to [3] above, wherein the amount of the precipitated ether group-containing polyunsaturated compound (A) is 3 parts by mass or more per 100 parts by mass of the total amount of the compound (A) in the ether group-containing polyunsaturated compound composition. [5] An ether group-containing polyunsaturated compound composition obtained by the method for storing an ether group-containing polyunsaturated compound composition according to any one of [1] to [4] above. [6] An ether group-containing polyunsaturated compound composition comprising an ether group-containing polyunsaturated compound (A) represented by the following general formula (1), a polymerization inhibitor (B), and a non-aqueous solvent (C), wherein the content of the compound (A) is 5 to 50 mass% relative to 100 mass% of the composition, and the number of foreign matter particles having a particle diameter of 2 to 5 μm per 10 mL of the composition is 500 to 5,000.
[0013]
[0014] (In formula (1), R 1 and R 2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms which may have a substituent.) [7] The ether group-containing polyunsaturated compound composition according to the above item [6], characterized in that it is the ether group-containing polyunsaturated compound composition of 50 liters or more. [8] A monomer composition characterized in that it contains the ether group-containing polyunsaturated compound composition according to any one of the above items [5] to [7], and an unsaturated monomer other than the ether group-containing polyunsaturated compound (A) represented by the following general formula (1):
[0015]
[0016] (In formula (1), R 1 and R 2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms which may have a substituent.) [9] A method for producing a monomer composition, comprising a step of mixing the ether group-containing polyunsaturated compound composition according to any one of the above items [5] to [7], and an unsaturated monomer other than the ether group-containing polyunsaturated compound (A) represented by the following general formula (1):
[0017]
[0018] (In formula (1), R 1 and R 2each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms, which may have a substituent.)
[10] A method for producing the monomer composition according to [9] above, comprising a step of filtering the ether group-containing polyunsaturated compound composition or a mixture of the ether group-containing polyunsaturated compound composition and an unsaturated monomer other than the ether group-containing polyunsaturated compound (A) represented by general formula (1).
[11] A tetrahydropyran ring-containing polymer obtained by polymerizing the monomer composition according to [8] above.
[12] A method for producing a tetrahydropyran ring-containing polymer, comprising a step of polymerizing the monomer composition according to [8] above.
[13] A photosensitive resin composition comprising the tetrahydropyran ring-containing polymer according to
[11] above and a photopolymerization initiator.
[14] A method for producing a photosensitive resin composition, comprising a step of mixing the tetrahydropyran ring-containing polymer according to
[11] above with a photopolymerization initiator.
[15] A cured product obtained by curing the photosensitive resin composition according to
[13] above.
[16] A method for producing a cured film, comprising a step of curing the photosensitive resin composition described in
[13] above.
[17] A member for a display device, comprising a cured product described in
[15] above on a substrate.
[18] A method for producing a member for a display device, comprising a step of curing the photosensitive resin composition described in
[13] above on a substrate to form a cured film.
[19] A method for producing a tetrahydropyran ring-containing polymer, comprising a step of storing an ether group-containing polyunsaturated compound composition by the method for storing an ether group-containing polyunsaturated compound composition described in any one of [1] to [4] above, and a step of polymerizing the stored ether group-containing polyunsaturated compound composition and a monomer composition containing an unsaturated monomer other than the ether group-containing polyunsaturated compound (A) represented by the following general formula (1):
[0019] (In formula (1), R 1 and R 2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms which may have a substituent.
[0020] According to the method for storing an ether group-containing polyunsaturated compound composition of the present invention, filter clogging caused by the generation of minute insoluble foreign matter can be suppressed, and a monomer composition, a tetrahydropyran ring-containing polymer, a photosensitive resin composition, a cured product, etc., using the composition can be efficiently obtained.
[0021] The present invention is described in detail below. Note that a combination of two or more of the individual preferred embodiments of the present invention described below is also a preferred embodiment of the present invention. Furthermore, in this specification, "(meth)acrylic acid" means "acrylic acid and / or methacrylic acid," and "(meth)acrylate" means "acrylate and / or methacrylate." Furthermore, in this specification, a numerical range "(minimum value) to (maximum value)" means "(minimum value) or more and (maximum value) or less." For example, when it is written as "5 to 10," it means "5 or more and 10 or less."
[0022] 1. Method for storing an ether group-containing polyunsaturated compound composition The present invention relates to a method for storing an ether group-containing polyunsaturated compound composition, the composition comprising an ether group-containing polyunsaturated compound (A) represented by the following general formula (1), a polymerization inhibitor (B), and a non-aqueous solvent (C), wherein the content of compound (A) is 5 to 50 mass% relative to 100 mass% of the composition, and the method includes a dissolving step of dissolving compound (A) precipitated in the composition at a temperature at least 5°C higher than the precipitation temperature of compound (A):
[0023] (In formula (1), R 1 and R 2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms which may have a substituent.
[0024] The storage method for an ether group-containing polyunsaturated compound composition of the present invention (hereinafter also referred to as the "storage method of the present invention") can suppress filter clogging caused by the generation of insoluble particles. The storage method of the present invention can suppress filter clogging because, when the ether group-containing polyunsaturated compound (A) represented by the general formula (1) (hereinafter also referred to as "compound (A)") precipitates at low storage temperatures in winter, the polymerization inhibitor is incorporated into the precipitate, making the polymerization inhibitor in the composition less effective. If left untreated, compound (A) will gel and generate insoluble particles due to seasonal temperature increases. However, by dissolving the precipitate once a certain amount of compound (A) has precipitated and storing it, the polymerization inhibitor can be appropriately present in the composition, thereby suppressing the generation of insoluble particles even when the storage temperature rises in summer. The phenomenon of the generation of insoluble particles is particularly pronounced when a large amount of ether group-containing polyunsaturated compound composition is stored.
[0025] For example, in the case of color filters for CMOS sensors used in smartphones, the size of each pixel is approximately 1 μm x 1 μm. The smaller the pixel size, the greater the adverse effect that foreign matter (raw material impurities, pigment clumps, etc.) has on image quality. To prevent this from affecting the pixels, the amount of foreign matter in the resin composition used in the color filter must be reduced, and the amount of foreign matter in the polymer solution used in the resin composition must also be reduced by removing it using a filter or other means. The storage method of the present invention can suppress the generation of such minute insoluble foreign matter.
[0026] The method for storing a composition of the present invention (hereinafter also referred to as the “storage method of the present invention”) includes a dissolving step of dissolving the compound (A) precipitated in a composition containing the compound (A), a polymerization inhibitor (B), and a non-aqueous solvent (C) at a temperature that is 5° C. or more higher than the precipitation temperature of the compound (A).
[0027] Compound (A) is usually dissolved in the ether group-containing polyunsaturated compound composition immediately after production, but precipitates in the composition when the temperature drops below the precipitation temperature. When compound (A) precipitates in the composition, white crystals can be visually confirmed. The temperature of the composition when such white crystals can be observed is below the precipitation temperature of compound (A). The precipitation temperature of compound (A) can be determined by the following method. That is, 10 g of the ether group-containing polyunsaturated compound composition is placed in a sample bottle and placed in a refrigerator adjusted to a predetermined temperature. After 24 hours, the sample bottle is removed and checked for precipitation of crystals. If precipitation has occurred, the crystals are again dissolved by heating and placed in a refrigerator adjusted to a temperature 1°C higher than the previous time, and it is similarly checked for precipitation of crystals. In this way, the temperature is changed by 1°C increments, and the temperature at which crystals precipitate is repeated. The highest temperature at which crystals precipitate is taken as the precipitation temperature.
[0028] The method for storing a composition of the present invention is preferably used for a composition containing a compound that precipitates as crystals during the autumn to winter temperature drop and dissolves during the spring to summer temperature rise, and in such cases, the technical significance of the present invention can be realized. The method for storing a composition of the present invention is preferably used for a composition containing a compound represented by formula (1) with a precipitation temperature of 25°C or less. More preferably, the method is used for a composition containing a compound represented by formula (1) with a precipitation temperature of 20°C or less, and even more preferably, for a composition containing a compound represented by formula (1) with a precipitation temperature of 15°C or less. The precipitation temperature of compound (A) is preferably 0°C to 25°C, more preferably 0°C to 20°C, and even more preferably 5°C to 15°C.
[0029] In the present invention, the dissolving step is preferably carried out when the amount of the precipitated compound (A) is 3 parts by mass or more relative to 100 parts by mass of the total content of the compound (A) in the ether group-containing polyunsaturated compound composition. By carrying out the dissolving step when the compound (A) is precipitated at such a ratio, the technical significance of the present invention is more fully realized. More preferably, the dissolving step is carried out when the amount of the precipitated compound (A) is 5 to 80 parts by mass, and even more preferably 5 to 60 parts by mass, relative to 100 parts by mass of the total content of the compound (A) in the composition.
[0030] In the storage method of the present invention, the precipitated compound (A) may be dissolved at a temperature that is 5°C or more higher than the precipitation temperature of compound (A). However, in consideration of sufficient dissolution of compound (A) and heating costs, the precipitated compound (A) is preferably dissolved at a temperature that is 10 to 50°C higher, more preferably 10 to 40°C higher, and even more preferably 10 to 30°C higher than the precipitation temperature of compound (A).
[0031] The time for maintaining the temperature 5°C or more higher than the precipitation temperature of compound (A) is preferably 1 to 12 hours, more preferably 2 to 10 hours, and even more preferably 2 to 6 hours, in consideration of sufficient dissolution and costs.
[0032] To dissolve the precipitated compound (A) at a temperature 5°C or higher than the precipitation temperature of compound (A), a method of heating the ether group-containing polyunsaturated compound composition to a predetermined temperature or placing it in an environment at a predetermined temperature to dissolve compound (A) can be mentioned. In this case, the composition can be left to stand or stirred, but stirring is preferred in terms of efficient dissolution. Examples of the stirring include a method of shaking or rotating a container containing the composition, or a method using a stirring bar or stirring blade, and in consideration of handling and workability, a method of shaking or rotating a container containing the composition is preferred.
[0033] The stirring time is not particularly limited, but in consideration of sufficient dissolution and costs, it is preferably 0.5 to 24 hours, more preferably 1 to 12 hours, even more preferably 2 to 10 hours, and even more preferably 2 to 6 hours.
[0034] The specific temperature in the dissolving step is preferably 18 to 60°C, more preferably 20 to 50°C, and even more preferably 30 to 45°C.
[0035] The storage method of the present invention preferably further comprises a step of leaving the composition after the dissolving step at a temperature higher than the temperature at which compound (A) precipitates for one day or more.
[0036] The step of leaving the composition standing is not particularly limited, and can be carried out by a known method such as placing the composition in a container or the like and leaving it standing at a predetermined temperature.
[0037] The temperature at which the compound (A) precipitates is as described above. The temperature at which the composition is allowed to stand may be any temperature at which the compound (A) does not precipitate again, and is preferably equal to or higher than the temperature at which the compound (A) precipitates. In consideration of preventing precipitation of the compound (A) and the heating cost, the temperature at which the composition is allowed to stand is preferably 5 to 40°C higher than the precipitation temperature of the compound (A), more preferably 5 to 25°C higher, and even more preferably 5 to 10°C higher.
[0038] The standing period in the standing step is preferably 1 day or more, and is preferably 1 to 100 days, more preferably 1 to 50 days, and even more preferably 1 to 10 days.
[0039] In order to further prevent filter clogging caused by the generation of minute insoluble foreign matter from the ether group-containing polyunsaturated compound composition, it is preferable that the composition be left standing at the above-mentioned temperature until the start of use of the composition.
[0040] The storage method of the present invention enables good storage of an ether group-containing polyunsaturated compound composition containing compound (A), and is particularly suitable for storing a large amount of the ether group-containing polyunsaturated compound composition. The amount of the composition to be stored is not particularly limited, but is preferably 50 liters or more, more preferably 100 liters or more. The upper limit of the amount of the composition is not particularly limited, but from the viewpoints of workability and handling, 200 liters or less is preferred. The amount of the composition to be stored is preferably 50 to 200 liters, more preferably 100 to 200 liters.
[0041] The storage method of the present invention may further include other steps, such as a purification step and a concentration step of the composition. These steps may be carried out by known methods.
[0042] Each component contained in the ether group-containing polyunsaturated compound composition will be described below. <Ether group-containing polyunsaturated compound (A)> The ether group-containing polyunsaturated compound (A) used in the present invention is a compound represented by the general formula (1) above. In the general formula (1), R 1 and R 2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms which may have a substituent. The hydrocarbon group preferably has 1 to 12 carbon atoms, and more preferably has 1 to 8 carbon atoms.
[0043] The hydrocarbon group having 1 to 25 carbon atoms, which may have a substituent, is not particularly limited, and examples thereof include linear or branched alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, t-butyl, t-amyl, stearyl, lauryl, and 2-ethylhexyl; aryl groups such as phenyl; alicyclic groups such as cyclohexyl, t-butylcyclohexyl, dicyclopentadienyl, tricyclodecanyl, isobornyl, adamantyl, and 2-methyl-2-adamantyl; alkyl groups substituted with alkoxy such as 1-methoxyethyl and 1-ethoxyethyl; and alkyl groups substituted with aryl groups such as benzyl. Among these, hydrocarbon groups having primary or secondary carbon atoms that are difficult to eliminate by acid or heat, such as methyl, ethyl, cyclohexyl, and benzyl, are particularly preferred in terms of further improving the heat resistance of the resulting polymer, and methyl is most preferred.
[0044] R 1 and R 2 may be the same or different. R 1 and R 2 are the same, that is, compound (A) is preferably a symmetric compound. However, from the viewpoint of storage stability of compound (A), 1 and R 2 are different, that is, the compound (A) may be an asymmetric compound.
[0045] Preferably, compound (A) is a symmetrical ether dimer, ie, 2,2'-[oxybis(methylene)]bisacrylic acid or dialkyl 2,2'-[oxybis(methylene)]bis-2-propenoate.
[0046] Specific examples of the symmetrical ether dimer include 2,2'-[oxybis(methylene)]bisacrylic acid, dimethyl-2,2'-[oxybis(methylene)]bis-2-propenoate, diethyl-2,2'-[oxybis(methylene)]bis-2-propenoate, di(n-propyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(isopropyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, and di(n-butyl)-2,2'-[oxybis(methylene)]bis-2-propenoate. di(isobutyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(t-butyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(t-amyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(stearyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(lauryl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(2-ethylhexyl)-2,2'-[oxybis(methylene)]bis-2- propenoate, di(1-methoxyethyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(1-ethoxyethyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, dibenzyl-2,2'-[oxybis(methylene)]bis-2-propenoate, diphenyl-2,2'-[oxybis(methylene)]bis-2-propenoate, dicyclohexyl-2,2'-[oxybis(methylene)]bis-2-propenoate, di(t-butylcyclohexyl)-2,2'-[oxybis(methylene)]bis-2-propenoate di(dicyclopentadienyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(tricyclodecanyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(isobornyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, diadamantyl-2,2'-[oxybis(methylene)]bis-2-propenoate, di(2-methyl-2-adamantyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, and the like.Among these, dimethyl-2,2'-[oxybis(methylene)]bis-2-propenoate, diethyl-2,2'-[oxybis(methylene)]bis-2-propenoate, dicyclohexyl-2,2'-[oxybis(methylene)]bis-2-propenoate, and dibenzyl-2,2'-[oxybis(methylene)]bis-2-propenoate are particularly preferred, and dimethyl-2,2'-[oxybis(methylene)]bis-2-propenoate is most preferred. Only one type of compound (A) may be used, or two or more types may be used.
[0047] The method for producing compound (A) is not particularly limited, and compound (A) may be produced by a known method, for example, the method described in JP-A-2014-148610.
[0048] The content of compound (A) in the composition is 5 to 50% by mass relative to 100% by mass of the composition, preferably 5 to 40% by mass, more preferably 10 to 40% by mass, and even more preferably 20 to 40% by mass, relative to 100% by mass of the composition.
[0049] <Polymerization Inhibitor (B)> Examples of the polymerization inhibitor in the present invention include phenolic compounds, organic acid copper salts, phenothiazines, phosphites, thioethers, hindered amine compounds, ascorbic acids, thiocyanates, thiourea derivatives, nitrites, sulfites, thiosulfates, hydroxylamine derivatives, N-oxyl compounds, etc. Among these, in terms of coloration, compatibility, etc., hydroxy group-containing compounds having a ring structure, particularly phenolic compounds, are preferred, and specific examples thereof include hydroquinone, methylhydroquinone, trimethylhydroquinone, t-butylhydroquinone, methoquinone, 6-t-butyl-2,4-xylenol, 2,6-di-t-butylphenol, 2,6-di-t-butyl-4-methoxyphenol, and 2,2'-methylenebis(4-methyl-6-t-butylphenol). N-oxyl compounds are also preferred, and specific examples thereof include derivatives of 2,2,6,6-tetramethylpiperidine-1-oxyl, particularly 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl. These may be used alone or in combination of two or more.
[0050] The content of the polymerization inhibitor is not particularly limited, but from the viewpoint of storage stability, it is preferably 0.0006 to 1% by mass, more preferably 0.001 to 0.1% by mass, and even more preferably 0.003 to 0.05% by mass, relative to 100% by mass of the composition.
[0051] <Non-aqueous solvent (C)> The non-aqueous solvent in the present invention is not particularly limited as long as it is an organic solvent that can uniformly dissolve the compound (A) and the polymerization inhibitor. However, at least one solvent selected from the group consisting of alcohol-based solvents, ether-based solvents, ester-based solvents, ketone-based solvents, aromatic solvents, amide-based solvents, nitrile-based solvents, and sulfoxide-based solvents is preferred.
[0052] Examples of the alcohol solvent include monoalcohols such as methanol, ethanol, isopropanol, n-butanol, and s-butanol; glycols such as ethylene glycol and propylene glycol; and polyhydric alcohols such as glycerin.
[0053] Examples of the ether solvent include cyclic ethers such as tetrahydrofuran and dioxane; glycol monoethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, and 3-methoxybutanol; and glycol ethers such as ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol ethyl methyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl methyl ether, propylene glycol dimethyl ether, and propylene glycol diethyl ether.
[0054] Examples of the ester solvents include ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monobutyl ether acetate, dipropylene glycol monomethyl ether acetate, Examples of the alkyl ester include glycol monoether esters such as dipropylene glycol monoethyl ether acetate, dipropylene glycol monobutyl ether acetate, and 3-methoxybutyl acetate; and alkyl esters such as methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, butyl acetate, methyl propionate, ethyl propionate, butyl propionate, methyl lactate, ethyl lactate, butyl lactate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, methyl acetoacetate, and ethyl acetoacetate.
[0055] Examples of the ketone solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone.
[0056] Examples of the aromatic solvent include benzene, toluene, xylene, and ethylbenzene.
[0057] Examples of the amide solvent include dimethylformamide, dimethylacetamide, and N-methylpyrrolidone.
[0058] Examples of the nitrile solvent include acetonitrile, propionitrile, and benzonitrile.
[0059] Examples of the sulfoxide solvent include dimethyl sulfoxide.
[0060] In particular, in terms of further suppressing clogging of the filter, it is preferable that the non-aqueous solvent contains at least an ester-based solvent or an alcohol-based solvent, and it is preferable that the ester-based solvent contains at least propylene glycol monomethyl ether acetate, and the alcohol-based solvent contains at least isopropanol.
[0061] The content of the non-aqueous solvent is not particularly limited, but from the viewpoint of easily dissolving compound (A), it is preferably 40 to 94 mass%, more preferably 50 to 90 mass%, and even more preferably 50 to 85 mass%, relative to 100 mass% of the composition.
[0062] The composition may contain other components in addition to the above-mentioned components. Examples of the other components include water. It is preferable that the composition does not contain any polymerizable compound such as an unsaturated monomer other than the compound (A).
[0063] When the composition contains water, the content of water is preferably 0.3 to 10% by mass, more preferably 0.5 to 7% by mass, and even more preferably 1 to 5% by mass, relative to 100% by mass of the composition.
[0064] The content of the other components may be appropriately selected depending on the purpose and use of the composition, but is, for example, preferably 0.3 to 10% by mass, more preferably 0.5 to 7% by mass, and even more preferably 0.5 to 5% by mass, relative to 100% by mass of the composition.
[0065] The method for producing the composition is not particularly limited, and the components may be mixed uniformly in a predetermined ratio and liquefied.
[0066] As described above, the storage method of the present invention can suppress filter clogging caused by minute insoluble foreign matter in the composition even when the composition is stored for a long period of time. An ether group-containing polyunsaturated compound composition obtained by such a storage method of the present invention also constitutes one aspect of the present invention.
[0067] 2. Ether Group-Containing Polyunsaturated Compound Composition The present invention also relates to an ether group-containing polyunsaturated compound composition containing an ether group-containing polyunsaturated compound (A) represented by the following general formula (1), a polymerization inhibitor (B), and a non-aqueous solvent (C), wherein the content of the compound (A) is 5 to 50% by mass relative to 100% by mass of the composition, and the number of foreign matter particles having a particle size of 2 to 5 μm is 500 to 5,000 per 10 mL of the composition:
[0068] (In formula (1), R 1 and R 2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms which may have a substituent.
[0069] The ether group-containing polyunsaturated compound composition of the present invention (hereinafter also simply referred to as "the composition of the present invention") has a number of foreign matter particles having a particle diameter of 2 to 5 μm per 10 mL of the composition of 500 to 5,000. Therefore, by using a resin composition containing the composition of the present invention, which has a small number of foreign matter particles, a cured product having desired properties can be obtained satisfactorily without causing filter clogging.
[0070] In the composition of the present invention, the number of foreign particles having a particle diameter of 2 to 5 μm per 10 mL of the composition is preferably 500 to 4,900, more preferably 500 to 4,800, and even more preferably 500 to 4,700, in order to prevent filter clogging. The number of foreign particles having a particle diameter of 2 to 5 μm can be measured using a liquid particle counter (SVSS-C-16, manufactured by PAMAS). Foreign particle shapes include spherical, ellipsoidal, cubic, rectangular, pyramidal, needle-like, columnar, rod-like, cylindrical, scale-like, plate-like, and thin flake-like shapes. The PAMAS particle counter employs a light-blocking sensor as its measurement principle. Specifically, a sample passes through a measurement channel and is irradiated with a laser beam emitted from a light source. Foreign particles in the sample block the laser beam as they pass, casting a shadow on the detector beyond the beam, thereby measuring the size (particle diameter) and number of foreign particles. The number of foreign particles having a particle diameter of 2 to 5 μm is measured using such a liquid particle counter of the light blocking type.
[0071] In the composition of the present invention, the compound (A), the polymerization inhibitor (B), and the non-aqueous solvent (C) may be the same as those described above. The contents of each of them are also as described above.
[0072] The composition of the present invention is preferably 50 liters or more of the composition, more preferably 70 liters or more of the composition, and even more preferably 90 liters or more of the composition.
[0073] The composition of the present invention can be obtained by the above-mentioned storage method, and therefore contains a small amount of foreign matter. A resin composition containing the composition can suitably give a cured product having desired properties.
[0074] 3. Monomer Composition The present invention also relates to a monomer composition comprising the above-described ether group-containing polyunsaturated compound composition and an unsaturated monomer other than the ether group-containing polyunsaturated compound (A) represented by the above general formula (1).
[0075] The unsaturated monomer other than compound (A) is not particularly limited, and can be appropriately selected according to the use of the polymer obtained by polymerizing the monomer composition, as long as it is a monomer having a radical polymerizable unsaturated bond (hereinafter also referred to as copolymerizable group) copolymerizable with compound (A).The unsaturated monomer may be a compound having only one copolymerizable group in the same molecule (hereinafter also referred to as monofunctional monomer), or a compound having two or more copolymerizable groups (hereinafter also referred to as polyfunctional monomer), but from the viewpoint of obtaining a soluble polymer, a monofunctional monomer is preferred.
[0076] Examples of the monofunctional monomer include (meth)acrylic acid esters such as cyclohexyl (meth)acrylate, α-allyloxymethyl acrylic acid esters, (meth)acrylamide, unsaturated monocarboxylic acids such as (meth)acrylic acid, unsaturated polycarboxylic acids, unsaturated monocarboxylic acids in which the unsaturated group and the carboxyl group are chain-extended, unsaturated acid anhydrides, aromatic vinyls, N-substituted maleimides, α-olefins, vinyl halides, conjugated dienes, vinyl esters, vinyl ethers, N-vinyl compounds, unsaturated isocyanates, and acetylene. Specific examples of these monofunctional monomers include the monofunctional monomers described in JP 2015-148610 A. The monofunctional monomers may be used alone or in combination of two or more.
[0077] The content of the unsaturated monomer other than the compound (A) may be appropriately selected depending on the application of the polymer obtained by polymerizing the monomer composition, and is not particularly limited. However, the content is preferably 40 to 99 mass%, more preferably 50 to 99 mass%, and even more preferably 60 to 98 mass%, relative to 100 mass% of all monomer components contained in the monomer composition.
[0078] In the monomer composition of the present invention, the content of the compound (A) is preferably 1 to 60 mass%, more preferably 1 to 50 mass%, and even more preferably 2 to 40 mass%, based on 100 mass% of all monomer components contained in the monomer composition.
[0079] In the monomer composition of the present invention, the total content of the unsaturated monomer and the compound (A) is preferably 5 to 99 mass%, more preferably 50 to 99 mass%, even more preferably 55 to 97 mass%, and still more preferably 60 to 95 mass%, based on 100 mass% of the monomer composition.
[0080] In the monomer composition of the present invention, the content of the polymerization inhibitor (B) is preferably 0.0006 to 1 mass%, more preferably 0.001 to 0.1 mass%, and even more preferably 0.003 to 0.05 mass%, based on 100 mass% of the monomer composition.
[0081] In the monomer composition of the present invention, the content of the non-aqueous solvent (C) is preferably 0.5 to 94 mass%, more preferably 40 to 94 mass%, even more preferably 50 to 90 mass%, and still more preferably 50 to 85 mass%, based on 100 mass% of the monomer composition.
[0082] The number of foreign particles having a particle diameter of 2 to 5 μm per 10 mL of the monomer composition is preferably 500 or more and 5,000 or less, more preferably 500 or more and 4,900 or less, and even more preferably 500 or more and 4,800 or less. The number of foreign particles can be measured by the method described above.
[0083] The method for producing the monomer composition includes a method comprising a step of mixing the above-mentioned ether group-containing polyunsaturated compound composition with an unsaturated monomer other than the compound (A). The present invention also includes a method for producing a monomer composition, comprising a step of mixing the above-mentioned ether group-containing polyunsaturated compound composition with an unsaturated monomer other than the ether group-containing polyunsaturated compound (A) represented by the above general formula (1).
[0084] The mixing method is not particularly limited as long as it can uniformly mix the components, and can be carried out by a method using a known mixer or disperser.
[0085] The method for producing the monomer composition preferably includes a step of filtering the composition or the mixture of the composition and the unsaturated monomer obtained in the mixing step, which can reduce the number of foreign matters to a desired range.
[0086] The filtration method is not particularly limited and may be appropriately selected from known methods such as natural filtration, reduced pressure filtration, pressure filtration, centrifugal filtration, etc. The filtration can be carried out using filter paper, a glass fiber filter, a membrane filter, a cartridge filter, etc.
[0087] The method for producing the monomer composition may further include other steps, such as a purification step. These steps can be carried out by known methods.
[0088] 4. Tetrahydropyran Ring-Containing Polymer The present invention also relates to a tetrahydropyran ring-containing polymer obtained by polymerizing the above-described monomer composition. The monomer composition contains the above-described compound (A). By polymerizing the monomer composition, compound (A) undergoes polymerization while undergoing cyclization, thereby obtaining a polymer having a tetrahydropyran ring-containing structural unit represented by the following formula (2):
[0089]
[0090] (In the formula, R 1 and R 2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms which may have a substituent. 1 and R 2 is R in the above formula (1). 1 and R 2 are the same as
[0091] The content of the structural unit represented by formula (2) in the tetrahydropyran ring-containing polymer can be appropriately set depending on the application and purpose of the polymer, but is preferably 1 to 60% by mass, more preferably 1 to 50% by mass, and even more preferably 2 to 40% by mass, relative to 100% by mass of all structural units. Furthermore, from the viewpoint of improving heat resistance and developability, it is preferably 0.5 to 5% by mass, more preferably 0.5 to 4% by mass, and even more preferably 0.5 to 2% by mass. Even when the content of the structural unit represented by formula (2) is low, the polymer can be used as a display device component.
[0092] The tetrahydropyran ring-containing polymer may also have a structural unit derived from an unsaturated monomer other than the compound (A). The content thereof can be appropriately set depending on the application and purpose of the polymer, but is preferably 40 to 99% by mass, more preferably 50 to 99% by mass, and even more preferably 60 to 98% by mass, relative to 100% by mass of all structural units.
[0093] The weight-average molecular weight of the tetrahydropyran ring-containing polymer is not particularly limited and may be appropriately selected depending on the purpose and application, but is, for example, preferably 2,000 to 200,000, more preferably 5,000 to 100,000, and even more preferably 5,000 to 50,000. The weight-average molecular weight is a value obtained by measurement by gel permeation chromatography (GPC).
[0094] The acid value of the tetrahydropyran ring-containing polymer is not particularly limited and may be appropriately selected depending on the purpose and application, but is, for example, preferably 3 to 350 mgKOH / g, more preferably 5 to 350 mgKOH / g, and even more preferably 40 to 300 mgKOH / g. The acid value is a value obtained by measurement by neutralization titration using a potassium hydroxide (KOH) solution, and is the acid value per 1 g of polymer solid content.
[0095] The tetrahydropyran ring-containing polymer may further contain a polymerizable double bond in the side chain. By having a polymerizable double bond in the side chain, the polymer can be cured by heat or light. Therefore, when the polymer is made into a photosensitive resin composition, the sensitivity to light is improved, the polymer can be cured with a smaller amount of light, and the mechanical strength after curing is also increased.
[0096] A method for introducing a polymerizable double bond into a side chain includes adding a compound containing at least one selected from the group consisting of an epoxy group, an oxazoline group, and a hydroxyl group and a polymerizable unsaturated double bond to a polymer. In terms of the reactivity of the resulting polymer, the polymerizable unsaturated double bond is preferably a double bond possessed by a (meth)acryloyl group.
[0097] Examples of the compound containing a polymerizable unsaturated double bond and at least one selected from the group consisting of an epoxy group, an oxazoline group, and a hydroxyl group include compounds having a hydroxyl group and a double bond, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and allyl alcohol; compounds having an epoxy group and a double bond, such as glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and allyl glycidyl ether; and compounds having an oxazoline group and a double bond, such as vinyloxazoline and isopropenyloxazoline. Among these, glycidyl (meth)acrylate and 3,4-epoxycyclohexylmethyl (meth)acrylate are preferred because they are highly reactive, allow easy reaction control, are easily available, and can introduce not only a radically polymerizable double bond but also a hydroxyl group at the same time.
[0098] The amount of the compound containing at least one selected from the group consisting of an epoxy group, an oxazoline group, and a hydroxyl group and a polymerizable unsaturated double bond added is preferably 5 to 120 parts by mass, more preferably 10 to 80 parts by mass, per 100 parts by mass of the polymer. If the amount is too small, the curability will be insufficient and the strength after curing will be insufficient, while if the amount is too large, the storage stability of the polymer having a polymerizable double bond in its side chain may decrease.
[0099] As reaction conditions for adding at least one selected from the group consisting of an epoxy group, an oxazoline group, and a hydroxyl group to a compound containing a polymerizable unsaturated double bond, the temperature is preferably 50°C to 150°C, more preferably 80°C to 140°C, and most preferably 90°C to 120°C. If the temperature is lower than the above range, the addition reaction may not proceed sufficiently, while if the temperature is higher than the above range, gelation is likely to occur during the addition reaction. The reaction time is preferably 0.5 to 24 hours, more preferably 1 to 15 hours.
[0100] A known catalyst can be used in the addition reaction as needed. For example, when the compound to be added has an epoxy group, a tertiary amine such as triethylamine is preferred as the catalyst. The amount of catalyst used is preferably 0.01 to 30% by mass, more preferably 0.05 to 5% by mass, and most preferably 0.1 to 2% by mass, relative to the polymer. If the amount of catalyst used is below the above range, the addition reaction may not proceed sufficiently. On the other hand, if the amount used exceeds the above range, the resulting polymer may be discolored, or the catalyst may not dissolve and precipitate.
[0101] Furthermore, during the addition reaction, a gas having an inhibiting effect may be introduced into the reaction system or an inhibitor may be added. By introducing a gas having an inhibiting effect into the reaction system or adding an inhibitor, gelation during the addition reaction can be prevented.
[0102] The method for polymerizing the above-mentioned monomer composition to obtain a tetrahydropyran ring-containing polymer is not particularly limited, but a radical polymerization mechanism is preferred in terms of being advantageous for industrial production. The polymerization method includes known polymerization methods such as bulk polymerization, precipitation polymerization, solution polymerization, and suspension polymerization, and may be appropriately selected depending on the purpose and application, but a solution polymerization method is preferred in terms of reaction control and improving the cyclopolymerization rate.
[0103] The polymerization may be carried out by a known method by appropriately adding a polymerization initiator, a chain transfer agent, a polymerization solvent, etc. Examples of the polymerization initiator used in the polymerization include known polymerization initiators such as organic peroxides such as t-butylperoxy-2-ethylhexanoate, and azo compounds such as 2,2'-azobis(isobutyronitrile). Examples of the chain transfer agent include known chain transfer agents such as mercaptan chain transfer agents and α-methylstyrene dimer. The amounts used can be appropriately selected using known methods. For details of the polymerization conditions, etc., see, for example, the description in JP 2014-148610 A.
[0104] Such a method for producing a tetrahydropyran ring-containing polymer, which comprises a step of polymerizing the above-mentioned monomer composition, also constitutes one aspect of the present invention.
[0105] The method for producing the tetrahydropyran ring-containing polymer may include other steps in addition to the polymerization step. Examples of the other steps include an aging step, a drying step, a purification step, a dilution step, and a concentration step. These steps can be carried out by known methods.
[0106] As described above, the monomer composition is preferably an ether group-containing polyunsaturated compound composition stored by the method for storing an ether group-containing polyunsaturated compound composition of the present invention. This method for producing a tetrahydropyran ring-containing polymer also includes a step of storing an ether group-containing polyunsaturated compound composition by the method for storing an ether group-containing polyunsaturated compound composition, and a step of polymerizing the stored ether group-containing polyunsaturated compound composition and a monomer composition containing an unsaturated monomer other than the compound (A) represented by the general formula (1).
[0107] 5. Photosensitive Resin Composition The present invention also provides a photosensitive resin composition containing the above-mentioned tetrahydropyran ring-containing polymer and a photopolymerization initiator. The photosensitive resin composition of the present invention contains the above-mentioned tetrahydropyran ring-containing polymer and a photopolymerization initiator, and therefore has excellent curability and can provide a cured product having desired properties.
[0108] The content of the tetrahydropyran ring-containing polymer in the photosensitive resin composition is not particularly limited and can be appropriately selected depending on the purpose and application, but is preferably 5 to 90 mass%, more preferably 10 to 80 mass%, and even more preferably 15 to 70 mass%, relative to 100 mass% of the total solid content. In this specification, the term "total solid content" refers to the total amount of components that form a cured product (components excluding solvents and curing catalysts that volatilize during the formation of a cured product).
[0109] Examples of the photopolymerization initiator include 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one ("IRGACURE 907", manufactured by BASF); benzoin and its alkyl ethers such as benzoin; acetophenones; anthraquinones; thioxanthones such as 2,4-dimethylthioxanthone; ketals such as acetophenone dimethyl ketal and benzil dimethyl ketal; benzophenones such as benzophenone and 4,4'-bis-diethylaminobenzophenone; acylphosphine oxides, and and xanthones; α-aminoketone compounds; α-hydroxyketone compounds; oxime ester compounds such as 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime) ("OXE01", manufactured by BASF); benzoin compounds; thioxanthone compounds; halomethylated triazine compounds; halomethylated oxadiazole compounds; biimidazole compounds such as 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole; and the like. Specific examples of the photopolymerization initiator include the photopolymerization initiators described in JP-A-2014-148610. These may be used alone or in combination of two or more.
[0110] The content of the photopolymerization initiator is preferably 0.1 to 30% by mass, more preferably 0.2 to 25% by mass, and even more preferably 0.5 to 20% by mass, relative to 100% by mass of the total solid content of the photosensitive resin composition.
[0111] Furthermore, examples of photosensitizers and photoradical polymerization accelerators that may be used in combination with the photopolymerization initiator include mercaptan-based hydrogen donors such as 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, and 2-mercaptobenzimidazole.
[0112] The photosensitive resin composition may further contain a polymerizable compound, which is a low-molecular-weight compound having a polymerizable unsaturated bond (also referred to as a polymerizable unsaturated group) that can be polymerized by irradiation with active energy rays such as free radicals, electromagnetic waves (e.g., infrared rays, ultraviolet rays, X-rays, etc.), or electron beams, and examples thereof include monofunctional compounds having one polymerizable unsaturated group in the molecule and polyfunctional compounds having two or more polymerizable unsaturated groups.
[0113] Examples of the polymerizable compound include aromatic vinyl monomers such as styrene, α-methylstyrene, α-chlorostyrene, vinyltoluene, divinylbenzene, diallyl phthalate, and diallyl benzene phosphonate; vinyl ester monomers such as vinyl acetate and vinyl adipate; methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, β-hydroxyethyl (meth)acrylate, (2-oxo-1,3-dioxolan-4-yl)-methyl (meth)acrylate, (di)ethylene glycol di(meth)acrylate, and the like. Examples of the polymerizable compound include (meth)acrylic monomers such as tri(meth)acrylate, propylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and tris(hydroxyethyl)isocyanurate tri(meth)acrylate; triallyl cyanurate; unsaturated polyester; epoxy acrylate; urethane acrylate; polyester acrylate, etc. These polymerizable compounds may be used alone or in combination of two or more.
[0114] The content of the polymerizable compound is preferably 10 to 70% by mass, more preferably 15 to 70% by mass, and even more preferably 20 to 65% by mass, relative to 100% by mass of the total solid content of the photosensitive resin composition.
[0115] The photosensitive resin composition may contain other components in addition to the components described above. Examples of the other components include solvents; colorants (pigments, dyes); dispersants; heat resistance improvers; leveling agents; development aids; inorganic fine particles such as silica fine particles; silane-based, aluminum-based, titanium-based coupling agents; fillers; thermosetting resins; curing aids such as polyfunctional thiol compounds; plasticizers; polymerization inhibitors; ultraviolet absorbers; antioxidants; matting agents; antifoaming agents; antistatic agents; slip agents; surface modifiers; thixotropic agents; thixotropic aids; quinone diazide compounds; polyhydric phenol compounds; cationic polymerizable compounds; thermal acid generators; and the like. These may be used alone or in combination of two or more. These other components can be appropriately selected from known compounds and used, and the amount used can be appropriately determined.
[0116] The method for preparing the photosensitive resin composition is not particularly limited, and any known method may be used. For example, the photosensitive resin composition may be prepared by mixing and dispersing the above-described components using various mixers or dispersers. The method may further include other commonly performed steps. When the photosensitive resin composition contains a colorant, it is preferable to prepare the composition through a known colorant dispersion process.
[0117] A method for producing a photosensitive resin composition, which comprises a step of mixing such a tetrahydropyran ring-containing polymer with a photopolymerization initiator, also constitutes one aspect of the present invention.
[0118] 6. Cured Product The present invention also relates to a cured product obtained by curing the above-described photosensitive resin composition. The method for curing the photosensitive resin composition to obtain a cured product is not particularly limited, and known methods may be used. For example, the photosensitive resin composition is applied to a substrate by a known method, and the applied product is dried as needed to form a coating film. The coating film is then exposed to light through a photomask, and after exposure, the unexposed portion is dissolved in an alkaline aqueous solution and subjected to alkaline development. The coating is then washed as needed, followed by heating (post-curing), thereby obtaining a cured product. The coating, drying, exposure, alkaline development, and heating can be performed by known methods, such as the method described in JP 2014-148610 A.
[0119] A method for producing a cured product, which includes a step of curing the photosensitive resin composition, also constitutes one aspect of the present invention.
[0120] The photosensitive resin composition is preferably used in applications such as various optical members and electrical / electronic devices, including color filters, black matrices, photospacers, black column spacers, inks, printing plates, printed wiring boards, semiconductor elements, photoresists, insulating films, films, and organic protective films used in liquid crystal, organic EL, quantum dot, and micro LED liquid crystal displays, solid-state imaging elements, and touch panel display devices.
[0121] 7. Display Device Members A display device member having the above-described cured product on a substrate is also a preferred embodiment of the present invention. The cured product (cured film) formed from the above-described photosensitive resin composition is suitable as a transparent member and is also useful as a protective film or insulating film in various display devices. The substrate is not particularly limited and can be appropriately selected from known substrates depending on the purpose and application, and examples thereof include the substrates described in JP 2014-148610 A.
[0122] The present invention also includes a method for producing a member for a display device, which includes a step of curing the above-described photosensitive resin composition on a substrate to form a cured film.
[0123] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass."
[0124] The various evaluation methods used in the present examples are as follows. <Number of foreign particles> The number of foreign particles with a particle diameter of 2 μm to 5 μm per 10 ml of the ether dimer composition was measured using a liquid particle counter (manufactured by PAMAS, main body model: SVSS-C-16, sensor model: HCB-LD-50 / 50). The measurement was carried out in a clean room.
[0125] <Measurement of Molecular Weight> The weight average molecular weight (Mw) was determined in polystyrene equivalent terms using tetrahydrofuran (THF) as the mobile phase and a gel permeation chromatography (GPC) apparatus HLC-8320GPC manufactured by Tosoh Corporation and four TSKgel Super HZM-M (manufactured by Tosoh Corporation) columns.
[0126] <Polymer concentration in polymer solution> A solution obtained by adding 4 g of acetone to 1 g of the polymer solution and dissolving it was naturally dried at room temperature and further dried under reduced pressure (160°C / 5 mmHg) for 5 hours, then allowed to cool in a desiccator and its weight was measured. The non-volatile content of the polymer solution was calculated from the weight loss, and this was taken as the polymer concentration.
[0127] <Acid value> 80 mL of acetone and 10 mL of water were added to 0.5 to 1 g of the polymer solution, and the mixture was stirred to dissolve uniformly. The acid value of the solution was measured by titration using an automatic titrator ("COM-555", manufactured by Hiranuma Sangyo Co., Ltd.) with a 0.1 mol / L aqueous KOH solution as a titrant. The acid value of the polymer was then calculated from the acid value of the solution and the polymer concentration.
[0128] (Preparation Example) Preparation of Ether Dimer Composition 1. Reaction A reactor equipped with a stirrer, a temperature sensor, and a cooling tube was charged with 450.0 parts of methyl α-hydroxymethylacrylate (RHMA-M), 13.5 parts of 1,4-diazabicyclo[2.2.2]octane (DABC), and 0.9 parts of p-methoxyphenol (MEHQ), and the mixture was heated to 90°C with stirring. After the internal temperature reached 85°C, the reaction was carried out for 9 hours while maintaining the temperature at 90±5°C under normal pressure inside the reactor.
[0129] 2. Dilution with Methanol After it was confirmed that the temperature of the reaction liquid had dropped to 40° C. or less, 355.0 parts of methanol (MeOH) was added for dilution (conditions: atmospheric pressure, 35±5° C.).
[0130] 3. Crystallization The MeOH diluted solution was added dropwise to a different reactor containing 1,485.0 parts of water to crystallize the RHMA ether dimer (conditions: atmospheric pressure, 30° C. or less).
[0131] 4. Filtration The slurry containing the RHMA ether dimer was filtered using a pressure filter (conditions: atmospheric pressure to 0.1 MPa, 15° C. or less).
[0132] 5. Cake Washing The RHMA ether dimer filter cake was washed with water (conditions: normal pressure to 0.1 MPa, normal temperature). Washing was repeated three times using 380.0 parts of water each time.
[0133] 6. Dissolution of Cake 184.0 parts of propylene glycol monomethyl ether acetate (PGMEA) was added to the RHMA ether dimer cake and dissolved (conditions: atmospheric pressure, 60°C).
[0134] 7. Oil-water separation The oil layer containing the RHMA ether dimer was separated from the aqueous layer, and the aqueous layer was removed (conditions: atmospheric pressure, 60°C). The oil layer was 412.5 parts, and the removed aqueous layer was 141.9 parts.
[0135] 8. Solution Preparation (Concentration Adjustment) To the oil phase (solution containing RHMA ether dimer and PGMEA), 180.0 parts of PGMEA, 340.0 parts of isopropanol (IPA), 0.049 parts of MEHQ, and 0.006 parts of 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl (4H-TEMPO) were added to obtain 932.5 parts of an ether dimer composition. A portion was sampled, and the number of foreign particles was measured using a liquid particle counter, which was found to be 325 particles. Each composition was analyzed using gas chromatography, a Karl Fischer moisture meter, and a spectrophotometer, and found to be 25.0% by mass of RHMA ether dimer (MD), 37.1% by mass of PGMEA, 36.8% by mass of IPA, and 1.1% by mass of water. The precipitation temperature of the RHMA ether dimer was 13°C.
[0136] Storage Stability of Ether Dimer Composition Example 1 160 kg (175 L) of the ether dimer composition obtained in the above Preparation Example was placed in a 200 L SUS drum, sealed, and stored in a refrigerator at 5°C. After one week, the lid of the drum was opened and the bottom of the container was examined to confirm the precipitation of white crystals of ether dimer. The amount of precipitation was approximately 53 parts by mass per 100 parts by mass of the total ether dimer content. The lid of the drum was then sealed and placed in a 40°C insulated cabinet. The drum was then rotated for four hours using a drum rotator to dissolve the precipitated ether dimer. After dissolution of the ether dimer, the drum was allowed to stand in the insulated cabinet at 40°C for three months. The lid of the drum was then opened, a portion was sampled, and the number of foreign particles was measured using a liquid-borne particle counter, which was found to be 2,611.
[0137] Example 2 80 kg (87 L) of the ether dimer composition obtained in the above Preparation Example was placed in a 100 L SUS drum, sealed, and stored in a refrigerator at 5°C. After one week, the lid of the drum was opened and the bottom of the container was examined to confirm the precipitation of white ether dimer crystals. The amount of precipitation was 53 parts by mass per 100 parts by mass of the total ether dimer content. The lid of the drum was then sealed and placed in a 40°C insulated cabinet. The drum was then rotated for four hours using a drum rotator to dissolve the precipitated ether dimer. After the ether dimer was dissolved, the drum was allowed to stand in the insulated cabinet at 50°C for three months. The lid of the drum was then opened, a portion was sampled, and the number of foreign particles was measured using a liquid particle counter, which was 4,528 particles.
[0138] Comparative Example 1 160 kg (175 L) of the ether dimer composition obtained in the above Preparation Example was placed in a 200 L SUS drum, sealed, and stored in a refrigerator at 5°C. After one week, the lid of the drum was opened and the bottom of the container was inspected to confirm the presence of ether dimer crystals. The amount of precipitated ether dimer was 53 parts by mass relative to 100 parts by mass of the total ether dimer content. The lid of the drum was then sealed and placed in a 40°C insulated cabinet. The drum was then left standing in the 40°C insulated cabinet for three months without dissolving the ether dimer. The lid of the drum was then opened and it was confirmed that ether dimer crystals were still present. The lid of the drum was then sealed and the drum was rotated for four hours using a drum rotator in a 40°C insulated cabinet to dissolve the precipitated ether dimer. The lid of the drum was then opened and a portion was sampled. The number of foreign particles was measured using a liquid particle counter, which was found to be 12,117.
[0139] From Examples 1 and 2 and Comparative Example 1, it was found that by dissolving the precipitated ether dimer, the number of foreign matters in the ether dimer composition after standing was significantly reduced.
[0140] <Synthesis of Tetrahydropyran Ring-Containing Copolymer: Binder Resin> (Example 3) A reaction vessel equipped with a condenser was prepared as the reaction vessel. A monomer dripping vessel was prepared by thoroughly stirring and mixing 120 parts by mass of the ether dimer composition obtained in Example 1, 34 parts by mass of methacrylic acid, 136 parts by mass of cyclohexyl methacrylate, and 5.2 parts by mass of t-butylperoxy-2-ethylhexanoate (NOF Corporation's "Perbutyl O"). A portion of the stirred mixture was sampled, and the number of foreign particles was measured using a liquid particle counter, resulting in 1,139 particles. A chain transfer agent dripping vessel was prepared by thoroughly stirring and mixing 14 parts by mass of n-dodecanethiol and 30 parts by mass of PGMEA. A drip pump was installed at the bottom of the monomer dripping vessel, allowing the monomer mixture in the monomer vessel to be dripped into the reaction vessel using the drip pump. A 1 μm pore size filter was also installed immediately before the reaction vessel.
[0141] 388 parts by mass of PGMEA was charged into the reaction vessel, and after purging with nitrogen, the reaction vessel was heated in an oil bath with stirring to raise the temperature to 90°C. After the temperature of the reaction vessel stabilized at 90°C, dripping was initiated from the monomer dripping vessel and the chain transfer agent dripping vessel. A portion of the solution from the monomer dripping vessel that had passed through the filter was sampled, and the number of foreign particles was measured using a liquid particle counter, revealing a reduced number of 118 particles. The dripping was carried out over 135 minutes while maintaining the temperature at 90°C. The dripping proceeded smoothly without clogging the filter. 60 minutes after the end of the dripping, the temperature was raised to 110°C, and the reaction vessel was maintained at 110°C for 3 hours. Next, IPA was removed at 110°C under reduced pressure, and then the mixture was cooled to room temperature. PGMEA was added to adjust the concentration, thereby obtaining a polymer solution (binder resin solution) of a copolymer containing a tetrahydropyran ring (weight average molecular weight: 8000, polymer concentration: 33.3 mass%, acid value: 71 mgKOH / g).
[0142] Example 4 A reaction vessel equipped with a cooling tube was prepared as the reaction vessel. A monomer dropping vessel was prepared by thoroughly stirring and mixing 120 parts by mass of the ether dimer composition obtained in Example 2, 34 parts by mass of methacrylic acid, 136 parts by mass of cyclohexyl methacrylate, and 5.2 parts by mass of t-butylperoxy-2-ethylhexanoate (NOF Corporation's "Perbutyl O") in a monomer dropping vessel. A chain transfer agent dropping vessel was prepared by thoroughly stirring and mixing 14 parts by mass of n-dodecanethiol and 30 parts by mass of PGMEA. A dropping pump was installed at the bottom of the monomer dropping vessel, allowing the monomer mixture in the monomer tank to be dropped into the reaction vessel using the dropping pump. A 1 μm pore size filter was also installed immediately before the reaction vessel. 388 parts by mass of PGMEA was charged into the reaction vessel, and after purging with nitrogen, the reaction vessel was heated in an oil bath with stirring until the temperature of the reaction vessel reached 90°C. After the temperature of the reaction vessel was stabilized at 90° C., dropping was started from the monomer dropping vessel and the chain transfer agent dropping vessel. Dropping was carried out over 135 minutes for each vessel while maintaining the temperature at 90° C. The dropping proceeded smoothly without clogging the filters.
[0143] Comparative Example 2 Synthesis was carried out in the same manner as in Example 2, except that the ether dimer composition obtained in Comparative Example 1 was used. After the temperature of the reaction vessel was stabilized at 90° C., dropping was started from the monomer dropping vessel and the chain transfer agent dropping vessel. 20 minutes after the start of dropping, the filter immediately before the reaction vessel became clogged, making it impossible to drop the monomer.
[0144] <Preparation of Photosensitive Resin Composition and Evaluation of Color Filter Suitability> (Preparation of Pigment Dispersion) 7.24 parts of brominated zinc phthalocyanine as a green pigment, 2.54 parts of C.I. Pigment Yellow 150, 60.00 parts of PGMEA, 2 parts of a dispersant ("DISPERBYK-2000" manufactured by BYK-Chemie) in terms of solid content, 3.3 parts of the binder resin obtained in Example 2 in terms of solid content, and 225 parts of zirconia beads were filled into a stainless steel container and dispersed for 6 hours using a paint shaker to prepare a green pigment dispersion.
[0145] (Preparation of Photosensitive Resin Composition) 57.78 parts of green pigment dispersion, 23.40 parts of PGMEA, 8 parts of ethyl 3-ethoxypropionate, 5.47 parts of binder resin, 3.63 parts of dipentaerythritol hexaacrylate, 0.38 parts of 2,2'-bis (o-chlorophenyl) -4,4',5,5'-tetraphenyl-1,2'-biimidazole, 0.19 parts of 4,4'-bis - diethylaminobenzophenone, 0.38 parts of 2-mercaptobenzothiazole, 0.76 parts of 2-methyl-1 [4- (methylthio) phenyl] -2-morpholinopropan-1-one was thoroughly mixed to prepare a photosensitive resin composition containing a tetrahydropyran ring-containing copolymer and a photopolymerization initiator.
[0146] (Production of Color Filter) The photosensitive resin composition was applied to a glass substrate having a square of 50 mm and a thickness of 0.7 mm using a spin coater, and then dried at 80° C. for 3 minutes. Then, the composition was irradiated with 300 mJ / cm 2 using a 2 kW high-pressure mercury lamp. 2The entire surface was exposed to light at an exposure dose of 1000 kJ / cm 2 , and a colored coated substrate was formed on the glass substrate, forming a photosensitive resin composition. This was then subjected to a heat curing treatment at a temperature of 230°C for 30 minutes. The spectral transmittance of the resulting coated substrate was measured using a spectrophotometer (Hitachi, Ltd., "U-3310"), and the chromaticity (light source C) in the XYZ light system was calculated. The results were x 0.280, y 0.600, and Y 57.4.
[0147] As described above, a binder resin was synthesized and a photosensitive resin composition was prepared using an ether dimer composition with high storage stability as a raw material, and a good color filter was successfully produced.
Claims
1. A method for storing an ether group-containing polyunsaturated compound composition, comprising: an ether group-containing polyunsaturated compound (A) represented by the following general formula (1), a polymerization inhibitor (B), and a non-aqueous solvent (C), the content of compound (A) being 5 to 50% by mass relative to 100% by mass of the composition; and comprising a dissolving step of dissolving compound (A) precipitated in the composition at a temperature at least 5°C higher than the precipitation temperature of compound (A). (In formula (1), R 1 and R 2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms which may have a substituent.
2. A method for storing an ether group-containing polyunsaturated compound composition as described in claim 1, characterized in that the dissolving step is a step of dissolving the precipitated ether group-containing polyunsaturated compound (A) by stirring the ether group-containing polyunsaturated compound composition.
3. A method for storing an ether group-containing polyunsaturated compound composition according to claim 1 or 2, characterized in that the storage method is a method for storing 50 liters or more of the ether group-containing polyunsaturated compound composition.
4. A method for storing an ether group-containing polyunsaturated compound composition according to any one of claims 1 to 3, characterized in that the amount of the precipitated ether group-containing polyunsaturated compound (A) is 3 parts by mass or more per 100 parts by mass of the total content of the compound (A) in the ether group-containing polyunsaturated compound composition.
5. An ether group-containing polyunsaturated compound composition, characterized in that it is obtained by the method for storing an ether group-containing polyunsaturated compound composition according to any one of claims 1 to 4.
6. An ether group-containing polyunsaturated compound composition comprising an ether group-containing polyunsaturated compound (A) represented by the following general formula (1), a polymerization inhibitor (B), and a non-aqueous solvent (C), characterized in that the content of the compound (A) is 5 to 50% by mass relative to 100% by mass of the composition, and the number of foreign matter particles having a particle size of 2 to 5 μm per 10 mL of the composition is 500 to 5,000. (In formula (1), R 1 and R 2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms which may have a substituent.
7. The ether group-containing polyunsaturated compound composition according to claim 6, characterized in that the amount of said ether group-containing polyunsaturated compound composition is 50 liters or more.
8. A monomer composition comprising the ether group-containing polyunsaturated compound composition according to any one of claims 5 to 7, and an unsaturated monomer other than the ether group-containing polyunsaturated compound (A) represented by the following general formula (1): (In formula (1), R 1 and R 2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms which may have a substituent.
9. A method for producing a monomer composition, comprising a step of mixing the ether group-containing polyunsaturated compound composition according to any one of claims 5 to 7 with an unsaturated monomer other than the ether group-containing polyunsaturated compound (A) represented by the following general formula (1): (In formula (1), R 1 and R 2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms which may have a substituent.
10. A method for producing a monomer composition according to claim 9, characterized in that it comprises a step of filtering the ether group-containing polyunsaturated compound composition or a mixture of the ether group-containing polyunsaturated compound composition and an unsaturated monomer other than the ether group-containing polyunsaturated compound (A) represented by the general formula (1).
11. A tetrahydropyran ring-containing polymer obtained by polymerizing the monomer composition according to claim 8.
12. A method for producing a tetrahydropyran ring-containing polymer, comprising the step of polymerizing the monomer composition according to claim 8.
13. A photosensitive resin composition comprising the tetrahydropyran ring-containing polymer according to claim 11 and a photopolymerization initiator.
14. A method for producing a photosensitive resin composition, comprising the step of mixing the tetrahydropyran ring-containing polymer according to claim 11 with a photopolymerization initiator.
15. A cured product obtained by curing the photosensitive resin composition according to claim 13.
16. A method for producing a cured product, comprising the step of curing the photosensitive resin composition according to claim 13.
17. A member for a display device, comprising the cured product according to claim 15 on a substrate.
18. A method for producing a member for a display device, comprising the step of curing the photosensitive resin composition according to claim 13 on a substrate to form a cured product.
19. A method for producing a tetrahydropyran ring-containing polymer, comprising the steps of: storing an ether group-containing polyunsaturated compound composition by the method for storing an ether group-containing polyunsaturated compound composition according to any one of claims 1 to 4; and polymerizing a monomer composition containing the stored ether group-containing polyunsaturated compound composition and an unsaturated monomer other than the ether group-containing polyunsaturated compound (A) represented by the following general formula (1): (In formula (1), R 1 and R 2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms which may have a substituent.
Citation Information
Patent Citations
Ether dimer composition and polymer
JP2014148610A
Method of producing polymer using porous metal complex
JP2015172120A
Curable resin composition and color filter
JP2016035564A
Polymer and application of the same
JP2016065159A