Gelling agent, liquid composition, and hydrogel

The combination of cellulose oligomers and polysaccharides in an alkaline solution, gelled by acid neutralization, creates stable, temperature-responsive hydrogels for advanced applications in cell culture and drug delivery, addressing the limitations of existing technologies.

WO2024203856A1PCT designated stage expired Publication Date: 2024-10-03INSTITUTE OF SCIENCE TOKYO +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011311
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing gelling agents and hydrogel compositions do not effectively utilize cellulose oligomers to form hydrogels with polysaccharides, particularly in alkaline environments, limiting their application in cell culture and drug delivery systems.

Method used

A novel gelling agent and liquid composition using cellulose oligomers with an average degree of polymerization between 5 and 20, combined with polysaccharides like hyaluronic acid, which can be gelled by neutralizing an alkaline aqueous solution with an acid, forming a hydrogel through self-assembly and crosslinking of cellulose oligomer aggregates.

Benefits of technology

The solution enables the formation of stable, temperature-responsive hydrogels that can be used as scaffolds for cell culture and drug delivery, with controlled gelation and long-term stability, enhancing the functionality of hydrogel-based systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011311_03102024_PF_FP_ABST
    Figure JP2024011311_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a novel gelling agent and a gellable novel liquid composition and hydrogel using the same. A gelling agent according to an embodiment that is for gelling a polysaccharide such as hyaluronic acid contains a cellulose oligomer having an average degree of polymerization of 5-20 inclusive. A gellable liquid composition according to an embodiment contains a cellulose oligomer having an average degree of polymerization of 5-20 inclusive, a polysaccharide, and water.
Need to check novelty before this filing date? Find Prior Art

Description

Gelling agent, liquid composition and hydrogel

[0001] The present invention relates to a gelling agent, a gellable liquid composition, and a hydrogel obtained by gelling the liquid composition.

[0002] A gel formed by a composition containing cellulose or its derivative and a polysaccharide such as hyaluronic acid is known. For example, Patent Document 1 discloses that an aqueous solution containing hyaluronic acid and carboxymethylcellulose and having a pH of 3.5 or less is frozen and then thawed to produce a co-crosslinked gel composition consisting of hyaluronic acid and carboxymethylcellulose.

[0003] On the other hand, Patent Document 2 discloses the use of a cellulose oligomer having an average degree of polymerization of 5 to 20 as a medium additive added to a medium for culturing cells. The cellulose oligomer is an oligosaccharide having a structure in which glucose units are linked by β-1,4-glycosidic bonds. Patent Document 2 discloses that the cellulose oligomer is added to suspend cells in the medium, and does not disclose gelation by combining the cellulose oligomer with a polysaccharide.

[0004] JP 2003-019194 A JP 2021-069339 A

[0005] While investigating new uses for the above-mentioned cellulose oligomer, the present inventors discovered that cellulose oligomers form hydrogels through interactions with polysaccharides such as hyaluronic acid.

[0006] Embodiments of the present invention are based on the above findings, and have an object to provide a novel gelling agent capable of gelling polysaccharides, a gellable liquid composition containing a polysaccharide, and a hydrogel formed by gelling the liquid composition.

[0007] The present invention includes the following embodiments. [1] A gelling agent for gelling a polysaccharide, the gelling agent comprising a cellulose oligomer having an average degree of polymerization of 5 to 20. [2] A gellable liquid composition comprising a cellulose oligomer having an average degree of polymerization of 5 to 20, a polysaccharide, and water. [3] The liquid composition according to [2], which is an alkaline aqueous solution containing the cellulose oligomer and the polysaccharide and can be gelled by neutralizing with an acid. [4] The liquid composition according to [2], which is obtained by precipitating the cellulose oligomer by neutralizing with an acid an alkaline aqueous solution containing the cellulose oligomer and the polysaccharide. [5] The liquid composition according to [2] or [3], wherein the polysaccharide is a non-cellulosic polysaccharide. [6] The liquid composition according to [2] or [3], wherein the polysaccharide is at least one selected from the group consisting of glycosaminoglycans and water-soluble polysaccharides composed only of glucose and / or glucose derivatives polymerized through α-1,4-glycosidic bonds and α-1,6-glycosidic bonds. [7] The liquid composition according to any one of [2] to [6], wherein the cellulose oligomer is contained in an amount of 0.5 to 100 parts by mass per 100 parts by mass of the polysaccharide. [8] A hydrogel obtained by gelling the liquid composition according to any one of [2] to [7].

[0008] According to embodiments of the present invention, it is possible to provide a novel gelling agent capable of gelling a polysaccharide, a gellable liquid composition containing a polysaccharide, and a hydrogel obtained by gelling the liquid composition.

[0009] Schematic diagram for explaining the assumed mechanism of gelation according to one embodiment. Photographs showing the state of Examples 1 to 3 and Comparative Examples 1 to 4 after 24 hours of inversion.

[0010] [Gelling Agent] The gelling agent according to the embodiment is a gelling agent for gelling polysaccharides, and contains a cellulose oligomer having an average degree of polymerization of 5 to 20.

[0011] Cellulose oligomers are oligosaccharides with a structure in which glucose units are linked by β-1,4-glycosidic bonds, and are also called cellooligosaccharides. Cellulose oligomers may have no substituents or may have a substituent at the anomeric position of the reducing end.

[0012] In this embodiment, the cellulose oligomer used has an average degree of polymerization (DP) (the average number of glucose units present in one molecule) of 5 to 20. From the viewpoint of forming a more uniform gel, the average degree of polymerization (DP) is preferably 5 to 18, more preferably 6 to 15, even more preferably 6 to 10, and even more preferably 7 to 9. The average degree of polymerization of the cellulose oligomer is a weighted average of the degrees of polymerization according to the mass ratio of the cellulose oligomer. The cellulose oligomer is usually a mixture of compounds with different degrees of polymerization, and may include, for example, one with a degree of polymerization of 4 to 20, one with a degree of polymerization of 5 to 18, or one with a degree of polymerization of 5 to 13.

[0013] As the cellulose oligomer, it is preferable to use a compound represented by the following general formula (1).

[0014] In formula (1), R represents a hydrogen atom or a substituent introduced in place of a hydrogen atom. The wavy line in the bond between the carbon at position 1 (anomeric carbon) of the reducing end and the OR group indicates that the OR group has an α-configuration, a β-configuration, or a mixture of α- and β-configurations. The OR group preferably has a β-configuration.

[0015] In formula (1), n ​​is the average degree of polymerization and represents a number of 5 to 20. n is preferably 5 to 18, more preferably 6 to 15, even more preferably 6 to 10, and still more preferably 7 to 9.

[0016] The method for synthesizing cellulose oligomers is not particularly limited. For example, a method can be used in which α-glucose-1-phosphate (hereinafter sometimes referred to as αG1P) and at least one primer selected from the group consisting of glucose, cellobiose, and derivatives thereof are reacted with cellodextrin phosphorylase (hereinafter sometimes referred to as CDP). This reaction is a synthesis method that utilizes the reverse reaction of CDP, in which αG1P is used as a glucose donor and at least one primer selected from the group consisting of glucose, cellobiose, and derivatives thereof (i.e., glucose acceptor) is reacted with CDP, thereby sequentially polymerizing αG1P as a monomer relative to the primer. Note that by replacing the hydrogen atom of the hydroxy group at the anomeric position in the primer with a substituent, cellulose oligomers with various substituents can be synthesized.

[0017] The cellulose oligomer may be synthesized using CDP as described above and used as it is, or may be dissolved in an alkaline aqueous solution and used, or may be self-assembled.

[0018] Self-assembled cellulose oligomers can be prepared as follows. Specifically, a cellulose oligomer is dissolved in an alkaline aqueous solution to prepare an aqueous solution, and the resulting aqueous solution is neutralized with an acid. This causes the cellulose oligomer to become insoluble and precipitate. The cellulose oligomer then self-assembles by incubating the solution while stirring, vibrating, or in a stationary state. That is, the cellulose oligomer molecules align to form a cellulose oligomer aggregate having a cellulose type II crystalline structure. In one embodiment, the cellulose oligomer may be a cellulose oligomer aggregate having a cellulose type II crystalline structure, the constituent of which is a compound represented by formula (1).

[0019] The cellulose oligomer assembly may have a sheet-like structure (cellulose nanosheet). Here, the sheet-like structure is a concept that also encompasses elongated ribbon-like structures (cellulose nanoribbons).

[0020] In one embodiment, the gelling agent may be an aqueous dispersion of the cellulose oligomer. That is, the gelling agent may be a dispersion in which the cellulose oligomer aggregate is dispersed in water. Alternatively, in one embodiment, the gelling agent may be an aqueous solution in which the cellulose oligomer is dissolved in an alkaline aqueous solution. Alternatively, in one embodiment, the gelling agent may be in the form of a powder obtained by drying the aqueous dispersion or solution of the cellulose oligomer by freeze-drying or the like.

[0021] When the gelling agent is the above-mentioned aqueous dispersion, the content (concentration) of the cellulose oligomer is not particularly limited, and is, for example, preferably 0.10 to 15% (w / v), more preferably 0.12 to 5.0% (w / v), and even more preferably 0.12 to 1.0% (w / v).

[0022] When the gelling agent is the above-mentioned aqueous solution, the content (concentration) of the cellulose oligomer is not particularly limited, and is preferably, for example, 0.12 to 1.3% (w / v), more preferably 0.14 to 0.70% (w / v).

[0023] In this specification, "% (w / v)" means a mass volume percent concentration, which is the mass (g) of the target substance contained in a volume of 100 mL.

[0024] The gelling agent may contain a cellulose oligomer and water as a dispersion medium or solvent, as well as various additives such as an alkali agent, a buffer, and an inorganic salt.

[0025] Examples of alkaline agents include sodium hydroxide, potassium hydroxide, and lithium hydroxide.

[0026] Examples of the buffer include phosphate buffered saline (PBS), 2-morpholinoethanesulfonic acid (MES) buffer, trishydroxymethylaminomethane (Tris) buffer, 3-morpholinopropanesulfonic acid (MOPS) buffer, and 4-(2-hydroxyethyl)-1-piperazineethanesulfonic acid (HEPES) buffer.

[0027] Examples of inorganic salts include sodium chloride, potassium chloride, and lithium chloride.

[0028] The gelling agent is used to gel polysaccharides. Non-cellulosic polysaccharides are preferably used as polysaccharides. More preferably, the polysaccharides include (A) glycosaminoglycans and (B) water-soluble polysaccharides composed solely of glucose and / or glucose derivatives polymerized via α-1,4-glycosidic bonds and α-1,6-glycosidic bonds, and any one of these may be used alone or in combination of two or more. Many of these are constituent polysaccharides of the extracellular matrix, and are preferably used in this embodiment.

[0029] The glycosaminoglycan (A) is a polysaccharide having an amino sugar structure in which a hydroxy group of the sugar is substituted with an amino group. Examples of glycosaminoglycans include hyaluronic acid, chondroitin sulfate, heparin, keratan sulfate, and heparan sulfate.

[0030] The water-soluble polysaccharide (B) is a polysaccharide having a structure in which glucose and / or glucose derivatives are polymerized via α-1,4-glycosidic bonds and α-1,6-glycosidic bonds, and examples thereof include dextran and its derivatives (e.g., carboxymethyldextran (CM-Dex)), pullulan, etc.

[0031] In this specification, the above polysaccharides are a concept that encompasses salts thereof such as sodium salts when they have anionic groups.

[0032] In one embodiment, the polysaccharide is preferably at least one selected from the group consisting of hyaluronic acid, chondroitin sulfate, heparin, carboxymethyl dextran, and pullulan.

[0033] [Liquid Composition] The liquid composition according to the embodiment contains the gelling agent, and is therefore a gellable liquid composition containing a cellulose oligomer having an average degree of polymerization of 5 or more and 20 or less, a polysaccharide, and water.

[0034] In the liquid composition, the cellulose oligomer and polysaccharide are as described above, and therefore further explanation will be omitted.

[0035] In the liquid composition, the content of the cellulose oligomer is preferably 0.5 to 100 parts by mass per 100 parts by mass of the polysaccharide. Because the cellulose oligomer is used as a gelling agent to gel an aqueous solution of the polysaccharide, the content of the cellulose oligomer is preferably equal to or less than the content of the polysaccharide. The content of the cellulose oligomer is preferably 1 to 80 parts by mass, more preferably 2 to 70 parts by mass, even more preferably 3 to 60 parts by mass, and even more preferably 4 to 50 parts by mass per 100 parts by mass of the polysaccharide.

[0036] In one embodiment, when hyaluronic acid is used as the polysaccharide, the content of the cellulose oligomer is preferably 5 to 100 parts by mass, more preferably 8 to 80 parts by mass, even more preferably 10 to 60 parts by mass, and even more preferably 15 to 40 parts by mass, per 100 parts by mass of hyaluronic acid.

[0037] In the liquid composition, the content (concentration) of the cellulose oligomer is not particularly limited, and is, for example, preferably 0.10 to 1.0% (w / v), more preferably 0.12 to 0.50% (w / v), even more preferably 0.15 to 0.40% (w / v), even more preferably 0.18 to 0.35% (w / v), and even more preferably 0.20 to 0.30% (w / v).

[0038] The content (concentration) of the polysaccharide in the liquid composition is not particularly limited and may be, for example, 0.30 to 10.0% (w / v), 0.50 to 8.0% (w / v), 0.60 to 6.0% (w / v), or 0.80 to 5.0% (w / v). In one embodiment, when hyaluronic acid is used as the polysaccharide, the content (concentration) of hyaluronic acid in the liquid composition is not particularly limited, but is preferably 0.50 to 1.5% (w / v), more preferably 0.60 to 1.3% (w / v), and even more preferably 0.80 to 1.2% (w / v).

[0039] In the liquid composition, the cellulose oligomer may be contained in a state in which it is dissolved in an alkaline aqueous solution, or in a state in which it is dispersed in water as a cellulose oligomer aggregate.

[0040] For example, in one embodiment, the liquid composition may be an alkaline aqueous solution containing cellulose oligomers and polysaccharides, which can be gelled by neutralizing with an acid.

[0041] In one embodiment, the liquid composition may contain a cellulose oligomer aggregate dispersed in water and a polysaccharide dissolved in water. In this case, the gellable liquid composition is obtained by precipitating the cellulose oligomer by neutralizing an alkaline aqueous solution containing the cellulose oligomer and the polysaccharide with an acid.

[0042] The liquid composition may contain, in addition to the cellulose oligomer, polysaccharide, and water, various additives such as alkaline agents, buffering agents, inorganic salts, low-molecular-weight organic compounds, proteins, etc. The alkaline agents, buffering agents, and inorganic salts are as described above, and therefore further description will be omitted.

[0043] [Hydrogel] The liquid composition can form a hydrogel by gelation. Therefore, the hydrogel according to the embodiment is obtained by gelling the liquid composition. Therefore, the hydrogel contains the cellulose oligomer, the polysaccharide, and water, and may further contain various additives contained in the liquid composition. The contents of the cellulose oligomer and polysaccharide in the hydrogel and the ratio of the two are as described above for the liquid composition, and therefore further explanation is omitted.

[0044] Here, the term "hydrogel" refers to a dispersion in which water is the dispersion medium and has lost its fluidity and solidified. Specifically, in the gelation evaluation test described below, if the vial is inverted and, after 10 minutes, the dispersion is not at all dripping down to the bottom of the vial but is entirely retained at the top of the vial, it is determined that gelation has occurred (i.e., a hydrogel has been formed).

[0045] The liquid composition has temperature-responsive gelling ability, i.e., the liquid composition gels (or can be made to gel faster than in a low-temperature environment) upon heating, and can maintain its gel state even after subsequent cooling.

[0046] The hydrogel is formed by the interaction between the cellulose oligomer and the polysaccharide, forming a complex between them. Specifically, the cellulose oligomer is contained in the hydrogel as a self-assembled cellulose oligomer aggregate, and the aggregation of the cellulose oligomer aggregate is thought to function as a crosslinking agent (physical crosslink) that connects the molecular chains of the polysaccharide.

[0047] For example, a hydrogel can be formed by first self-assembling cellulose oligomers to form an aqueous dispersion of cellulose oligomer aggregates, and then mixing the aqueous dispersion with a polysaccharide or an aqueous solution thereof. However, a more preferred method is to precipitate the cellulose oligomers by neutralizing an alkaline aqueous solution containing the cellulose oligomers and polysaccharides with an acid. This allows for the formation of a more uniform hydrogel.

[0048] FIG. 1 is a conceptual diagram illustrating a possible gelation mechanism according to one embodiment. Here, a hydrogel is formed by neutralizing an alkaline aqueous solution. An acid is added to an alkaline aqueous solution containing dissolved cellulose oligomers and polysaccharides to neutralize the solution (to a neutral pH). A buffer may be added to the acid. When the neutralized aqueous solution is placed in a high-temperature environment (e.g., 37°C) for a predetermined time (e.g., 24 hours), the fluidity of the aqueous solution is lost, forming a hydrogel. In contrast, when the neutralized aqueous solution is placed in a low-temperature environment (e.g., 4°C) for a predetermined time (e.g., 24 hours), the fluidity of the aqueous solution is maintained, forming a sol. When the sol is then placed in a high-temperature environment (e.g., 37°C) for a predetermined time (e.g., 24 hours), the fluidity is lost, forming a hydrogel.

[0049] The mechanism of this gelation is presumed to be as follows: By neutralizing the alkaline aqueous solution, the cellulose oligomers become insoluble and precipitate, and then self-assemble to form cellulose oligomer aggregates. Because polysaccharides are present in the aqueous solution, an interaction occurs between the self-assembly of the cellulose oligomers and the polysaccharide molecular chains, as shown in Figure 1. Furthermore, the cellulose oligomer aggregates aggregate under high temperature conditions, and these aggregates act as cross-linking agents connecting the polysaccharide molecular chains. Therefore, a hydrogel with a three-dimensional network is formed by the polysaccharide molecular chains and the aggregates.

[0050] On the other hand, in a low-temperature environment, although interactions occur between the cellulose oligomer aggregates and the polysaccharide molecular chains, aggregation of the cellulose oligomer aggregates does not occur (or the aggregation rate is so slow that aggregation to the extent that fluidity is lost does not occur within a specified time), and it is thought that a fluid sol is formed. When the sol is placed in a high-temperature environment, aggregation of the cellulose oligomer aggregates is promoted, forming a crosslinked structure that connects the polysaccharide molecular chains, and forming a hydrogel with a three-dimensional network.

[0051] The temperature at which the liquid composition is gelled is not particularly limited, and may be, for example, 15° C. or higher, 20° C. or higher, or 25° C. or higher. The upper limit of the gelling temperature is also not particularly limited, and may be, for example, 60° C. or lower, or 50° C. or lower. The time period over which the liquid composition is gelled is not particularly limited, and may be 10 hours or longer, 15 hours or longer, or 18 hours or longer.

[0052] [Uses] The uses of the hydrogel according to the embodiment are not particularly limited, and examples thereof include a scaffold for cell culture, and a drug delivery system for incorporating drugs or useful proteins into the hydrogel to control their distribution in the body.

[0053] The present invention will be further explained below with reference to examples, but is not limited to these.

[0054] [Synthesis of Cellulose Oligomer] According to the method described in T. Serizawa et al., Polym. J., 2016, 48, 539-544 (using D-glucose as a primer), a cellulose oligomer (derived from glucose) having an average degree of polymerization of 9 (n = 9) represented by the following formula was synthesized. Also, according to the method described in T. Serizawa et al., Langmuir, 2017, 33, 13415-13422 (using cellobiose as a primer), a cellulose oligomer (derived from cellobiose) having an average degree of polymerization of 7 (n = 7) represented by the following formula was synthesized.

[0055] Specifically, 200 mmol / L of αG1P, 50 mmol / L of D-glucose or cellobiose, and 0.2 U / mL of cellodextrin phosphorylase (CDP) were mixed in 500 mmol / L of 2-[4-(2-hydroxyethyl)-1-piperazinyl]ethanesulfonic acid (HEPES) buffer (pH 7.5) and incubated for 3 days at 60°C. The reaction solution containing the product was centrifuged (15,000 rpm, 10 minutes or more, 4°C), the supernatant was removed, and then ultrapure water was added to redisperse the product. This centrifugation (under the same conditions) was repeated until the supernatant replacement rate reached 99.999% or more, yielding a cellulose oligomer.

[0056] The average degree of polymerization of the product was measured using a proton nuclear magnetic resonance (NMR) spectrometer. The sample was prepared by dissolving 12 mg or more of the lyophilized product in 600 μL of a 4% by weight sodium deuterium hydroxide deuterium oxide solution. The NMR spectrometer used was an ADVANCE III HD500 (Bruker Biospin, magnetic field strength: 500 MHz, 16 accumulations). The average degree of polymerization was calculated based on the integral values ​​of the protons at the anomeric positions (δ ~ 5.1, 4.5) of the reducing end of the cellulose oligomer and the other anomeric positions (δ ~ 4.3).

[0057] [Polysaccharides] The polysaccharides used in the examples are as follows: Hyaluronic acid: manufactured by Nacalai Tesque, Inc. CM-Dex: manufactured by Tokyo Chemical Industry Co., Ltd. Chondroitin sulfate C sodium: manufactured by Nacalai Tesque, Inc. Heparin sodium: manufactured by Nacalai Tesque, Inc.

[0058] [Test Example 1: Examples 1-3, Comparative Examples 1-4] 1 mL mighty vials were used as containers. A 1 mol / L NaOH aqueous solution containing dissolved cellulose oligomer and hyaluronic acid was neutralized with a 1 mol / L HCl aqueous solution to prepare a 300 μL aqueous solution. At this time, a phosphate buffer component was added to the HCl aqueous solution so that the aqueous solution after neutralization became phosphate buffered saline (PBS, [NaCl] 137 mmol / L). The concentrations of cellulose oligomer and hyaluronic acid in the aqueous solution after neutralization were as shown in Table 1 below. The types of cellulose oligomers are as shown in Table 1. The resulting aqueous solution was allowed to stand in an atmosphere of 25°C for 24 hours, and then gelation evaluation was performed.

[0059] The gelation evaluation was carried out by inverting the vial after standing, and 10 minutes after inversion, if none of the aqueous solution (dispersion system) had flowed down to the bottom of the vial and was entirely retained at the top of the vial, it was judged that gelation had occurred. In Table 1, gelled samples are indicated as "gels" and non-gelled samples are indicated as "sols."

[0060]

[0061] The results are shown in Table 1. No gelation occurred in Comparative Example 1, which did not contain a cellulose oligomer. No gelation occurred in Comparative Examples 2, 3, or 4, which did not contain hyaluronic acid. In contrast, gelation occurred in Examples 1 to 3, which used a combination of cellulose oligomer and hyaluronic acid, and a hydrogel was obtained in which the cellulose oligomer and hyaluronic acid were combined due to the interaction between them.

[0062] 2 is a photograph showing the state 24 hours after inversion, and the gel state was maintained without flowing even after 24 hours in Examples 1 to 3. When comparing the types of cellulose oligomer, Examples 1 and 2, which used a cellobiose-derived cellulose oligomer, formed a more transparent and uniform gel than Example 3, which used a glucose-derived cellulose oligomer.

[0063] [Test Example 2: Comparative Examples 5 and 6] In a 1mL mighty vial, prepare 300μL aqueous solution by dissolving sodium carboxymethylcellulose (manufactured by Nacalai Tesque) and hyaluronic acid.At this time, the concentration of sodium carboxymethylcellulose in this aqueous solution is 0.20% (w / v) in Comparative Example 5, and 0.30% (w / v) in Comparative Example 6.In addition, the concentration of hyaluronic acid is 1.0% (w / v) in both Comparative Examples 5 and 6.After the obtained aqueous solution is left standing in the atmosphere of 25 ℃ for 24 hours, gelation evaluation is carried out in the same manner as in Test Example 1.

[0064] As a result, in Comparative Examples 5 and 6, in which sodium carboxymethylcellulose was used instead of cellulose oligomer, the aqueous solution was observed to flow down 10 minutes after the vials were inverted after standing, and no gelation occurred.

[0065] [Test Example 3: Examples 4 to 6] The concentration of hyaluronic acid in the aqueous solution after neutralization is set to 0.40% (w / v) in Example 4, 0.60% (w / v) in Example 5, and 0.80% (w / v) in Example 6, and other conditions are the same as in Example 1 to obtain the aqueous solution after neutralization, and then stand in the atmosphere of 25 ℃ for 24 hours, and then carry out gelation evaluation.As a result, in Examples 4 to 6, after standing, the vial is inverted and turned upside down, and the aqueous solution does not flow down after 10 minutes, and gelation occurs.In addition, in Examples 4 to 6, even after 24 hours have passed since being inverted and turned upside down, the gel state is maintained.

[0066] [Test Example 4: Examples 7-9, Comparative Examples 7-12: Temperature Dependence of Static Storage] In a 1mL mighty vial, 1mol / L NaOH aqueous solution in which cellulose oligomer and hyaluronic acid are dissolved is neutralized with 1mol / L HCl aqueous solution containing phosphate buffer components, and the neutralized aqueous solution is phosphate buffered saline (PBS, [NaCl] 137mmol / L) to prepare 300μL aqueous solution.At this time, the concentration of cellulose oligomer (derived from cellobiose) in the neutralized aqueous solution is 0.20% (w / v), and the concentration of hyaluronic acid is 1.0% (w / v).The obtained aqueous solution is left standing for 24 hours in an atmosphere of 4 ℃ in Example 7, in an atmosphere of 25 ℃ in Example 8, and in an atmosphere of 37 ℃ in Example 9, and then the same gelation evaluation as in Test Example 1 is carried out.

[0067] In Comparative Examples 7 to 9, no cellulose oligomer was added, and otherwise aqueous solutions were prepared in the same manner as in Examples 7 to 9. The resulting aqueous solutions were allowed to stand for 24 hours in an atmosphere of 4°C in Comparative Example 7, in an atmosphere of 25°C in Comparative Example 8, and in an atmosphere of 37°C in Comparative Example 9, and then gelation evaluation was performed in the same manner as in Test Example 1.

[0068] In Comparative Examples 10 to 12, hyaluronic acid was not added, and otherwise aqueous solutions were prepared in the same manner as in Examples 7 to 9. The obtained aqueous solutions were allowed to stand for 24 hours in an atmosphere of 4°C in Comparative Example 10, in an atmosphere of 25°C in Comparative Example 11, and in an atmosphere of 37°C in Comparative Example 12, and then gelation evaluation was performed in the same manner as in Test Example 1.

[0069] The results are shown in Table 2 below. Comparative Examples 7 to 9, which contained only hyaluronic acid without the addition of cellulose oligomer, did not gel when left standing at 4°C, 25°C, or 37°C. Similarly, Comparative Examples 10 to 12, which contained only cellulose oligomer without the addition of hyaluronic acid, did not gel when left standing at 4°C, 25°C, or 37°C. In contrast, when cellulose oligomer and hyaluronic acid were combined, Example 7, which was left standing at 4°C, did not gel, but Examples 8 and 9, which were left standing at 25°C and 37°C, maintained a gel state not only 10 minutes after inversion but also 24 hours after inversion. This demonstrates that gelation can be controlled by the standing temperature. Furthermore, the gel tended to become more opaque as the standing temperature increased. This suggests that aggregation of cellulose oligomer aggregates may contribute to gelation.

[0070] A vial containing the sol of Example 7 that had not gelled was placed upright and left to stand for 24 hours in a 37°C atmosphere, after which a similar gelation evaluation was performed. The sol gelled, and the gel state remained even 24 hours after inversion. Furthermore, when the vial in this gel state was placed upright, left to stand for 24 hours in a 4°C atmosphere, and then inverted, the gel state remained even 24 hours after inversion. Thus, it was found that the liquid product (sol) obtained by standing at 4°C gelled when left at 37°C. Furthermore, after gelation, it did not return to a liquid state even when returned to 4°C. In other words, it was found that the gel, once formed, was stable against temperature changes. This suggests that once aggregated, cellulose oligomer aggregates do not disperse even when the temperature is lowered.

[0071] [Test Example 5: Dependence on Standing Time] Neutralized aqueous solutions (hyaluronic acid concentration: 1.0% (w / v), cellulose oligomer (derived from cellobiose) concentration: 0.20% (w / v), NaCl concentration: 137 mmol / L (PBS conditions)) were prepared in the same manner as in Example 1. The obtained neutralized aqueous solutions were each left standing in an atmosphere of 25°C for the standing times shown in Table 3 below, and the same gelation evaluation as in Test Example 1 was carried out.

[0072] The results are shown in Table 3 below, and it was found that gelation occurred when the formulation of Example 1 was left standing for 18 hours or more. Since the time required for self-assembly of cellulose oligomers is thought to be shorter, this supports the possibility that aggregation of cellulose oligomer aggregates contributes to gelation.

[0073]

[0074] Test Example 6: Evaluation of Hydrogel Stability A neutralized aqueous solution (hyaluronic acid concentration: 1.0% (w / v), cellulose oligomer (derived from cellobiose) concentration: 0.20% (w / v), NaCl concentration: 137 mmol / L (PBS conditions)) was prepared in the same manner as in Example 1 above, and the resulting neutralized aqueous solution was allowed to stand for 24 hours in an atmosphere at 25°C to produce the hydrogel of Example 10. Furthermore, the hydrogel of Example 11 was prepared in the same manner as in Example 10, except that the cellulose oligomer concentration was set to 1.0% (w / v). Next, 600 μL of ultrapure water was poured into each vial of Examples 10 and 11 to form a layer of ultrapure water on each hydrogel. The vials were then allowed to stand in an atmosphere at 25°C, and the state of the hydrogel was observed from immediately after the start of standing for 60 days.

[0075] As a result, in both Examples 10 and 11, the hydrogels maintained a gel state for at least two months after the addition of ultrapure water. In Example 11, in which the cellulose oligomer concentration was 1.0% (w / v), the hydrogel was observed floating up in the vial approximately six days after the start of standing. This suggests that in Example 11, the salt inside was being released due to osmotic pressure. However, the shape of the hydrogel itself remained unchanged. This suggests that the hydrogels of Examples 10 and 11 are stable in ultrapure water and may have constructed a network structure strong enough to withstand immersion in ultrapure water.

[0076] [Test Example 7: Example 12: Long-term storage at low temperature] A neutralized aqueous solution (hyaluronic acid concentration: 1.0% (w / v), cellulose oligomer (derived from cellobiose) concentration: 0.20% (w / v), NaCl concentration: 137 mmol / L (PBS condition)) was prepared in the same manner as in Example 7 above, and the obtained neutralized aqueous solution was left to stand in an atmosphere of 4 ° C for 24 hours. When this was inverted and left to stand at 4 ° C for 24 hours, the aqueous solution flowed down and did not gel. After leaving it in an inverted state at 4 ° C for 24 hours, the aqueous solution accumulated in the mouth of the vial was dropped, and the vial was turned upright again and left to stand in an atmosphere of 4 ° C. Then, after a total of 2 weeks of standing after neutralization, it was observed to become cloudy. Therefore, this was inverted and gelation evaluation was performed, and after 10 minutes, it gelled without flowing down. When it was further left to stand in an inverted state at 25 ° C for 24 hours, the gel state was maintained even after 24 hours. This indicates that gelation occurs when the standing time is extended, even when the solution is left standing at 4°C. This is thought to be because it takes a long time for the cellulose oligomer aggregates to aggregate in a low-temperature environment of 4°C.

[0077] Test Example 8: Examples 13 to 17 and Comparative Examples 13 to 15 According to Table 4 below, instead of 1.0% (w / v) hyaluronic acid, CM-Dex, chondroitin sulfate C sodium, and heparin sodium were used at a concentration of 5.0% (w / v), and the concentration of cellulose oligomer (derived from cellobiose) was as shown in Table 4. Otherwise, neutralized aqueous solutions were prepared in the same manner as in Test Example 1, and the obtained aqueous solutions were allowed to stand in an atmosphere of 25°C for 24 hours, after which gelation evaluation was performed.

[0078] The results are shown in Table 4 below. When CM-Dex, chondroitin sulfate C sodium, or heparin sodium was used as the polysaccharide, gelation did not occur in Comparative Examples 13 to 15, which did not contain a cellulose oligomer. In contrast, in Examples 13 to 17, which contained a cellulose oligomer in addition to these polysaccharides, the aqueous solution did not flow off and gelation occurred 10 minutes after inversion.

[0079]

[0080] The various numerical ranges described in this specification can be arbitrarily combined with their respective upper and lower limit values, and all such combinations are considered to be preferred numerical ranges described in this specification. Furthermore, a numerical range described as "X to Y" means from X to Y.

[0081] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included within the scope and spirit of the invention, as well as within the scope of the invention described in the claims and their equivalents.

Claims

1. A gelling agent for gelling polysaccharides, comprising a cellulose oligomer having an average degree of polymerization of 5 or more and 20 or less.

2. A gellable liquid composition comprising a cellulose oligomer having an average degree of polymerization of 5 or more and 20 or less, a polysaccharide, and water.

3. The liquid composition according to claim 2, which is an alkaline aqueous solution containing said cellulose oligomer and said polysaccharide and can be gelled by neutralizing with an acid.

4. The liquid composition according to claim 2, wherein the cellulose oligomer is precipitated by neutralizing an alkaline aqueous solution containing the cellulose oligomer and the polysaccharide with an acid.

5. The liquid composition of claim 2, wherein the polysaccharide is a non-cellulosic polysaccharide.

6. The liquid composition according to claim 2, wherein the polysaccharide is at least one selected from the group consisting of glycosaminoglycans and water-soluble polysaccharides composed only of glucose and / or glucose derivatives polymerized through α-1,4-glycosidic bonds and α-1,6-glycosidic bonds.

7. The liquid composition according to claim 2, comprising 0.5 to 100 parts by mass of said cellulose oligomer per 100 parts by mass of said polysaccharide.

8. A hydrogel formed by gelling the liquid composition according to any one of claims 2 to 7.

Citation Information

Patent Citations

  • Co-crosslinked gel composition comprising hyaluronic acid and carboxymethyl cellulose

    JP2003019194A

  • Medium additive for suspension culture, medium composition and culture method

    JP2021069339A

  • Gellant

    JP2009185228A

  • cellulose produced by enzymes