Sputtering target, method for producing sputtering target, oxide thin film, thin film transistor, and electronic device

The development of a sputtering target with a carefully controlled oxide sintered body composition addresses nodule formation issues, enabling the formation of suitable oxide semiconductor thin films and extending target life for stable sputtering operations.

WO2024203953A1PCT designated stage expired Publication Date: 2024-10-03IDEMITSU KOSAN CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011486
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Sputtering targets with oxide sintered bodies containing indium oxide face issues with nodule generation during continuous sputtering, leading to abnormal discharge and reduced target life, which complicates the formation of oxide semiconductor thin films suitable for transistor applications.

Method used

A sputtering target with an oxide sintered body having a specific density, average crystal grain size, and pore distribution, along with controlled impurity levels, particularly low carbon content and limited positive tetravalent metal oxide content, is developed to suppress nodule formation and enhance target longevity.

Benefits of technology

The approach allows for the formation of oxide thin films suitable for oxide semiconductor applications with reduced nodule generation and extended target life, ensuring stable and long-lasting sputtering performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011486_03102024_PF_FP_ABST
    Figure JP2024011486_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This sputtering target comprises an oxide-sintered body containing indium oxide as the main component. The oxide-sintered body has a density of at least 6.9 g / cm3 as measured by the Archimedean method. The average crystal grain size of crystal grains of indium oxide contained in the oxide-sintered body is 5-25 μm. In a field of view when the surface of the oxide-sintered body is observed at a magnification factor of 500 times, the area proportion of pores surrounded by at least three adjacent crystal grains to the area of the field of view is at most 3%.
Need to check novelty before this filing date? Find Prior Art

Description

Sputtering target, sputtering target manufacturing method, oxide thin film, thin film transistor, and electronic device

[0001] The present invention relates to a sputtering target, a method for manufacturing a sputtering target, an oxide thin film, a thin film transistor, and an electronic device.

[0002] 2. Description of the Related Art In recent years, research has been conducted into the application of oxide semiconductor thin films as channel layers of thin film transistors (hereinafter sometimes referred to as TFTs).

[0003] Oxide semiconductor thin films are generally formed by physical vapor deposition methods such as sputtering. In particular, oxide semiconductor thin films are often formed by magnetron sputtering because of their large-area uniformity and thin-film stability. Specifically, for example, in order to apply an oxide semiconductor thin film to a channel layer of a TFT, a sputtering target having a sintered body with the same atomic composition as the oxide semiconductor thin film is sputtered.

[0004] Recently, for example, Non-Patent Document 1 has reported that indium oxide (In 2 O 3 ) target, hydrogen gas was introduced during the deposition of the oxide semiconductor thin film, and hydrogenated polycrystalline In was formed. 2 O 3 (In 2 O 3 :H) thin film and high mobility In applied to TFT 2 O 3 :H TFTs have been reported.

[0005] Furthermore, as disclosed in Patent Documents 1 to 6, for example, it is known to use indium oxide doped with an element as a sputtering target to form a transparent electrode film.

[0006] For example, Patent Document 1 discloses an In alloy containing tin as an additive element. 2 O 3It is disclosed that the sintered body can be used as a sputtering target. The sintered body described in Patent Document 1 has a ratio of the number of tin atoms to the total number of atoms of all metal elements in the sintered body of 0.01% to 0.2%, and a relative density of 98% or more.

[0007] Patent Document 2 discloses a sputtering target made of an oxide sintered body containing indium oxide as a main component. In the sputtering target, the Archimedes density AD (g / cm) of the oxide sintered body is 3 ) and the theoretical density TD (g / cm) calculated from the lattice constant obtained by X-ray diffraction 3 ) and have a relationship of AD / TD>0.995.

[0008] Patent Document 3 discloses a sputtering target for forming a transparent electrode film, which contains 0.1 mass % to 5 mass % of zirconium oxide in indium oxide, and the zirconium oxide is dissolved in the indium oxide.

[0009] Patent Document 4 discloses a sputtering target using a sintered body composed of In, Sn, O, and unavoidable impurities. The sintered body described in Patent Document 4 contains Sn such that the atomic ratio Sn / (In+Sn) is 1.8% or more and 3.7% or less (excluding 3.7%), the average crystal grain size of the sintered body is in the range of 1.0 μm to 5.0 μm, and the area ratio of voids with a major axis diameter of 0.1 to 1.0 μm is 0.5% or less. The sintered body described in Patent Document 4 is composed of two phases: an indium oxide phase and a tin oxide-rich phase, with the area ratio of the tin oxide-rich phase being 0.1% to 1.0%, and 95% or more of the tin oxide-rich phase being present at the grain boundary triple junctions.

[0010] Patent Document 5 describes a sputtering target made of an oxide sintered body, in which the arithmetic mean roughness (Ra) and maximum height roughness (Rz) of the sputtering region and the crystal grain size (d) of the oxide sintered body satisfy at least one of the following formulas: (1) (0.05 μm≦Ra (μm)≦d (μm)×0.2) and (2) (0.4 μm≦Rz (μm)≦d (μm)×1.8).

[0011] Patent Document 6 describes a method for manufacturing a steel sheet having a Sn content of SnO2 In terms of the amount, it is 2.5 mass % to 10.0 mass %. 2 O 3 The parent phase and the In 2 O 3 In present in the grain boundaries of the parent phase 4 Sn 3 O 12 The ITO sintered body described in Patent Document 6 has a relative density of 98.0% or more, and the In phase is a sputtering target having an ITO sintered body. 2 O 3 The average grain size of the parent phase is 17 μm or less, and the In 4 Sn 3 O 12 The area ratio of the phase is 0.4% or more.

[0012] JP 2017-141155 A JP 2005-060798 A JP 2015-129348 A WO 2016 / 072441 JP 2009-221589 A WO 2015 / 125588

[0013] Magari, Y., Kataoka, T., Yeh, W., & Furuta, M. (2022). High-mobility hydrogenated polycrystalline In2O3(In2O3: H) thin-film transistors. Nature Communications, 13(1), 1-8.

[0014] When sputtering targets including an oxide sintered body containing indium oxide as a main component are continuously sputtered, black products called nodules may form on the surface of the sputtering target. The formation of nodules may cause abnormal discharge and may be a source of particle generation, resulting in a shortened target life and a decrease in productivity of oxide thin films.

[0015] In conventional techniques, the problem has been solved by adding a tetravalent element to a target including an oxide sintered body containing indium oxide as the main component in order to reduce nodules generated during sputtering. However, when a tetravalent element is added to indium oxide, the carrier concentration of the oxide thin film formed from the target increases. For this reason, thin films formed using a target including an oxide sintered body of indium oxide to which a tetravalent element has been added have been used as conductive films, but are not suitable for the application of oxide semiconductor thin films.

[0016] An object of the present invention is to provide a sputtering target including an oxide sintered body containing indium oxide as a main component, which is capable of forming an oxide thin film applicable as an oxide semiconductor thin film, which suppresses nodule generation during sputtering, and which has a long life. Furthermore, an object of the present invention is to provide a method for manufacturing the sputtering target, an oxide thin film using the sputtering target, a thin-film transistor including the oxide thin film, and an electronic device including the thin-film transistor.

[0017] [1] A sputtering target comprising an oxide sintered body containing indium oxide as a main component, wherein the oxide sintered body has a density of 6.9 g / cm as measured by Archimedes' method. 3 or more, wherein the average crystal grain size of the indium oxide crystal grains contained in the oxide sintered body is 5 μm or more and 25 μm or less, and in a field of view when the surface of the oxide sintered body is observed at a magnification of 500 times, the area ratio of voids surrounded by three or more adjacent crystal grains to the area of ​​the field of view is 3% or less.

[0018] [2] The sputtering target according to [1], wherein the indium oxide has an average crystal grain size of 5.4 μm or more and 23 μm or less.

[0019] [3] The sputtering target according to [1] or [2], wherein the area ratio of the voids is 2.6% or less.

[0020] [4] The sputtering target according to any one of [1] to [3], wherein the oxide sintered body contains 100 ppm or less of C (carbon) element as an impurity by mass.

[0021] [5] The sputtering target according to any one of [1] to [4], wherein the oxide sintered body contains an oxide of a metal element exhibiting a positive tetravalent valence, and the content of the oxide of the metal element exhibiting a positive tetravalent valence in the oxide sintered body is 2 atomic % or less with respect to the indium oxide in the oxide sintered body.

[0022] [6] The sputtering target according to [5], wherein the metal element exhibiting a positive tetravalent valence is one or more elements selected from the group consisting of Sn (tin), Ti (titanium), Ce (cerium), and Zr (zirconium).

[0023] [7] The sputtering target according to any one of [1] to [6], wherein the indium oxide is contained in an amount of 50 atomic % or more relative to the entire oxide sintered body.

[0024] [8] The sputtering target according to any one of [1] to [7], wherein the indium oxide is contained in an amount of 98 atomic % or more relative to the entire oxide sintered body.

[0025] [9] The sputtering target according to any one of [1] to [8], wherein, in a particle size distribution of indium oxide crystal grains contained in the oxide sintered body, a proportion of the indium oxide crystal grains having a particle size of 5 μm or more and 40 μm or less is 90% or more in terms of number ratio.

[0026]

[10] The sputtering target according to any one of [1] to [9], wherein, in a particle size distribution of indium oxide crystal grains contained in the oxide sintered body, a proportion of the indium oxide crystal grains having a particle size of 5 μm or more and 40 μm or less is 94% or more in terms of the number proportion.

[0027]

[11] The sputtering target according to any one of [1] to

[10] , wherein the area ratio of the voids is determined by observing the surface of the oxide sintered body with a scanning electron microscope or an electron beam microanalyzer.

[0028]

[12] A method for producing the sputtering target according to any one of [1] to

[11] , comprising: a step of producing a molded body by using a raw material powder containing an indium compound as a main component and adjusting a concentration of impurities so that the C (carbon) element contained in the oxide sintered body is 100 ppm or less by mass; and a step of firing the molded body so that the average crystal grain size of the indium oxide crystal grains contained in the oxide sintered body is 5 μm or more and 25 μm or less.

[0029]

[13] A method for manufacturing a sputtering target, comprising: a step of producing a molded body using a raw material powder containing as a main component an indium compound having an average particle size of 0.1 μm or more and 2 μm or less; and a step of firing the molded body by controlling at least the sintering temperature and the sintering time so that the average crystal particle size of the indium oxide crystal grains contained in the oxide sintered body is 5 μm or more and 25 μm or less, and the area ratio of voids surrounded by three or more adjacent crystal grains on the sputtering surface of the oxide sintered body to the total area of ​​the sputtering surface is 3% or less.

[0030]

[14] The method for producing a sputtering target according to

[13] , wherein in the step of producing the compact, a raw material powder mainly composed of an indium compound is crushed by a crusher and then molded.

[0031]

[15] An oxide thin film formed by using the sputtering target according to any one of [1] to

[11] .

[0032]

[16] A thin film transistor comprising the oxide thin film according to

[15] .

[0033]

[17] An electronic device comprising the thin film transistor according to

[16] .

[0034] According to one aspect of the present invention, a sputtering target including an oxide sintered body containing indium oxide as a main component can be provided, which can form an oxide thin film that can be used as an oxide semiconductor thin film, can suppress nodule generation during sputtering, and has a long life. Furthermore, the present invention can provide a method for manufacturing the sputtering target, an oxide thin film using the sputtering target, a thin film transistor including the oxide thin film, and an electronic device including the thin film transistor.

[0035] 1 is a perspective view showing the shape of a target according to one embodiment of the present invention; FIG. 2 is a perspective view showing the shape of a target according to one embodiment of the present invention; FIG. 3 is a perspective view showing the shape of a target according to one embodiment of the present invention; FIG. 4 is a longitudinal cross-sectional view showing a thin film transistor according to one embodiment of the present invention; FIG. 5 is a longitudinal cross-sectional view showing a thin film transistor according to one embodiment of the present invention; FIG. 6 is a longitudinal cross-sectional view showing a thin film transistor according to one embodiment of the present invention; FIG. 7 is a longitudinal cross-sectional view showing a quantum tunnel field effect transistor according to one embodiment of the present invention; FIG. 8 is a longitudinal cross-sectional view showing another embodiment of a quantum tunnel field effect transistor; FIG. 9 is a longitudinal cross-sectional view showing a manufacturing procedure for a quantum tunnel field effect transistor; FIG. 10 is a longitudinal cross-sectional view showing a manufacturing procedure for a quantum tunnel field effect transistor; FIG. 11 is a longitudinal cross-sectional view showing a manufacturing procedure for a quantum tunnel field effect transistor; FIG. 12 is a longitudinal cross-sectional view showing a manufacturing procedure for a quantum tunnel field effect transistor; FIG. 13 is a top view showing a display device using a thin film transistor according to one embodiment of the present invention; FIG. 14 is a diagram showing a circuit of a pixel portion that can be applied to pixels of a VA-mode liquid crystal display device; FIG. 15 is a diagram showing a circuit of a pixel portion of a display device using an organic EL element; FIG. 16 is a diagram showing a circuit of a pixel portion of a solid-state imaging device using a thin film transistor according to one embodiment of the present invention; FIG. 17 is an optical microscope image of a sputtering target according to one embodiment of the present invention; FIG. 18 is an optical microscope image of a sputtering target according to an aspect of a comparative example.

[0036] Hereinafter, embodiments will be described with reference to the drawings, etc. However, it will be readily understood by those skilled in the art that the embodiments can be implemented in many different ways and that various changes in form and details can be made without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the following description of the embodiments.

[0037] In the drawings, sizes, layer thicknesses, regions, etc. may be exaggerated for clarity. Therefore, the present invention is not limited to the illustrated sizes, layer thicknesses, regions, etc. Note that the drawings are schematic illustrations of ideal examples, and the present invention is not limited to the shapes, values, etc. shown in the drawings.

[0038] The ordinal numbers "first," "second," and "third" used in this specification are used to avoid confusion between components, and components that are not specified numerically are not limited in number.

[0039] In this specification and the like, the terms "film" or "thin film" and "layer" can be used interchangeably in some cases.

[0040] In the sintered body and oxide thin film of this specification and the like, the terms "compound" and "crystalline phase" can be interchangeable in some cases.

[0041] In this specification, the “oxide sintered body” may be simply referred to as the “sintered body.” In this specification, the “sputtering target” may be simply referred to as the “target.”

[0042] In this specification, "electrically connected" includes connection via "something that has some kind of electrical function." Here, "something that has some kind of electrical function" is not particularly limited as long as it allows electrical signals to be transmitted and received between the connected objects. For example, "something that has some kind of electrical function" includes electrodes, wiring, switching elements (such as transistors), resistive elements, inductors, capacitors, and other elements with various functions.

[0043] In this specification, the functions of the source and drain of a transistor may be interchanged when transistors of different polarities are used or when the direction of current flow changes during circuit operation, etc. Therefore, in this specification, the terms source and drain may be used interchangeably.

[0044] In this specification, a numerical range expressed using "to" means a range that includes the numerical value before "to" as the lower limit and the numerical value after "to" as the upper limit.

[0045] The present inventors have invented the present invention based on the following findings. The inventors investigated the suppression of nodules formed on the surface of a sputtering target including an oxide sintered body containing indium oxide as a main component when sputtering is performed continuously using the target. The inventors also investigated the application of an oxide thin film formed using a sputtering target including an oxide sintered body containing indium oxide as a main component as an oxide semiconductor thin film. As a result, the inventors discovered that, in an oxide sintered body containing indium oxide as a main component, the generation of nodules on the surface of the target during sputtering can be suppressed by examining the average crystal grain size of indium oxide crystal grains contained in the oxide sintered body and the amount of vacancies present in a region surrounded by three or more adjacent indium oxide crystal grains. Specifically, by setting the average crystal grain size of indium oxide crystal grains contained in the oxide sintered body within a specific range, it is possible to reduce the amount of vacancies present in a region surrounded by three or more adjacent indium oxide crystal grains while maintaining the flexural strength, thereby suppressing the generation of nodules. Furthermore, the inventors have found that by examining the density of the sintered body, it is possible to obtain a target having a long life in which nodule generation and cracking are suppressed. Furthermore, the inventors have found that, even when a metal element exhibiting a positive tetravalent valence is not intentionally contained or, even when a metal element exhibiting a positive tetravalent valence is intentionally contained, by examining the content of the metal element exhibiting a positive tetravalent valence, the carrier concentration can be kept low and the target can be used as an oxide semiconductor thin film.

[0046] [Sputtering Target] The sputtering target according to this embodiment uses an oxide sintered body. The oxide sintered body is used as a film raw material when forming a film by sputtering. That is, the sintered body provided in the target according to this embodiment is an oxide sintered body containing indium oxide as a main component. The oxide sintered body has a density of 6.9 g / cm as measured by Archimedes' method. 3 or more, the average crystal grain size of the indium oxide crystal grains contained in the oxide sintered body is 5 μm or more and 25 μm or less, and in a field of view when the surface of the oxide sintered body is observed at a magnification of 500 times, the area ratio of voids surrounded by three or more adjacent crystal grains to the area of ​​the field of view is 3% or less.

[0047] The sintered body used as the material of the target according to this embodiment contains indium oxide as a main component, and (i) the density of the oxide sintered body measured by Archimedes' method is 6.9 g / cm 3 By satisfying all of the above conditions (i) to (iii), namely, (ii) the average crystal grain size of the indium oxide crystal grains in the oxide sintered body is 5 μm or more and 25 μm or less, and (iii) the area ratio of voids surrounded by three or more adjacent crystal grains to the area of ​​the field of view when the surface of the oxide sintered body is observed at a magnification of 500 times, to the area of ​​the field of view, is 3% or less, nodule generation during sputtering is suppressed and the target has a long life. Furthermore, an oxide thin film formed using the target according to this embodiment is applicable as an oxide semiconductor thin film. That is, the target according to this embodiment is useful as a sputtering target for forming an oxide semiconductor thin film.

[0048] In the sintered body provided in the target according to this embodiment, the sintered body preferably contains indium oxide as a main component and, in one aspect, does not contain an oxide of a metal element exhibiting a positive tetravalent valence as an additional element. In this case, the sintered body may consist essentially of indium oxide alone. In the sintered body provided in the target according to this embodiment, the sintered body preferably contains indium oxide as a main component and, in one aspect, also preferably contains an oxide of a metal element exhibiting a positive tetravalent valence as an additional element. In this case, the content of the oxide of the metal element exhibiting a positive tetravalent valence in the sintered body is preferably 2 atomic % or less relative to the indium oxide in the oxide sintered body. Note that in this specification, atomic % may be expressed as at % in some cases.

[0049] That is, in one aspect, the target according to this embodiment includes a sintered body containing indium oxide as a main component, and the sintered body either contains an oxide of a metal element exhibiting a positive tetravalent valence or does not contain an oxide of a metal element exhibiting a positive tetravalent valence, and preferably satisfies all of the conditions (i) to (iii) above.

[0050] The sintered body preferably contains indium oxide in an amount of 50 atomic % or more, more preferably 98 atomic % or more, even more preferably 99 atomic % or more, still more preferably 99.1 atomic % or more, and even more preferably 99.9 atomic % or more, based on the entire sintered body.

[0051] In one embodiment, the sintered body may consist essentially of In (indium) and O (oxygen). In one embodiment, the sintered body may consist essentially of In (indium), O (oxygen), and a metal element exhibiting a positive tetravalent valence as an intentionally added additional element. Here, "substantially" means that the sintered body according to this embodiment may contain other components within the range in which the effects of the present invention resulting from the combination of the In element and the O element are achieved, and within the range in which the effects of the present invention resulting from the combination of the In element, the O element, and the metal element exhibiting a positive tetravalent valence are achieved. In this case, the sintered body provided in the target according to this embodiment may contain elements that are impurities.

[0052] Impurities refer to elements that are not intentionally added, but are mixed in during raw materials, manufacturing processes, etc. In other words, impurities are inevitable impurities that are inevitably included. The same applies to the following explanation. Examples of impurities include at least one element selected from the group consisting of alkali metal elements (elements such as Li (lithium), Na (sodium), K (potassium), and Rb (rubidium)), alkaline earth metal elements (elements such as Mg (magnesium), Ca (calcium), Sr (strontium), and Ba (barium)), B element (boron element), C element (carbon element), N element (nitrogen element), F element (fluorine element), Si element (silicon element), Zr element (zirconium element), Fe element (iron element), Zn element (zinc element), Sn element (tin element), Al element (aluminum element), and Cl element (chlorine element).

[0053] When the sintered body provided in the target according to this embodiment contains C (carbon) element as an impurity, the sintered body preferably contains C (carbon) element as an impurity at 100 ppm or less by mass, more preferably less than 100 ppm, even more preferably 90 ppm or less, even more preferably 80 ppm or less, and even more preferably 60 ppm or less. If the content of C (carbon) element as an impurity in the sintered body is 100 ppm or less, it is easy to suppress nodule generation during sputtering. Furthermore, if the C (carbon) element as an impurity is 100 ppm (mass ratio) or less, all of the conditions (i) to (iii) above can be satisfied with respect to indium oxide in the oxide sintered body.

[0054] The content (atomic %) of each metal element in the sintered body can be determined by measuring the amount of each element present by ICP (Inductive Coupled Plasma) measurement or XRF (X-ray Fluorescence) measurement. An inductively coupled plasma optical emission spectrometer can be used for ICP measurement. A thin film X-ray fluorescence analyzer can be used for XRF measurement. Furthermore, the mass-based content of C (carbon) element as an impurity in the sintered body can be measured by a carbon mass analyzer.

[0055] When the sintered body provided with the target according to this embodiment contains an oxide of a metal element exhibiting a positive tetravalent valence as an additive element, as described above, the content of the oxide of the metal element exhibiting a positive tetravalent valence in the sintered body is preferably 2 atomic % or less relative to the indium oxide in the oxide sintered body. The content of the oxide of the metal element exhibiting a positive tetravalent valence in the sintered body is preferably 1.7 atomic % or less, more preferably 1.5 atomic % or less, even more preferably 1 atomic % or less, even more preferably 0.9 atomic % or less, even more preferably 0.8 atomic % or less, and even more preferably 0.7 atomic % or less. If the content of the oxide of the metal element exhibiting a positive tetravalent valence in the sintered body is 2 atomic % or less (preferably 1.7 atomic % or less) relative to the indium oxide in the oxide sintered body, the oxide thin film formed using the target according to this embodiment can be easily used as an oxide semiconductor thin film. Furthermore, if the content of the oxide of the metal element exhibiting a positive tetravalent valence in the sintered body is 2 atomic % or less, all of the conditions (i) to (iii) can be satisfied for indium oxide in the oxide sintered body.

[0056] The metal element exhibiting a positive tetravalent atomic valence as the additive element is preferably one or more elements selected from the group consisting of Sn (tin), Ti (titanium), Ce (cerium), and Zr (zirconium), from the viewpoint of facilitating application as an oxide semiconductor thin film.

[0057] The content of the oxide of the metal element exhibiting a positive tetravalent valence in the sintered body can be determined by measuring the amount of each element present by ICP (Inductive Coupled Plasma) measurement or XRF (X-ray Fluorescence) measurement. An inductively coupled plasma optical emission spectrometer can be used for the ICP measurement. A thin film X-ray fluorescence analyzer can be used for the XRF measurement.

[0058] The sintered body provided in the target according to this embodiment has a density of an oxide sintered body (hereinafter sometimes referred to as the density of the sintered body) measured by Archimedes' method of 6.9 g / cm 3The density of the oxide sintered body measured by Archimedes' method is 6.9 g / cm 3 If the density is equal to or greater than this, it is possible to suppress cracking of the target and abnormal discharge during film formation. 3 The following levels are included:

[0059] The density of the sintered body measured by the Archimedes method is the actually measured density. Note that, for the density of indium oxide, the value of the specific gravity of oxides listed in "Chemical Handbook, Basics I, Revised 2nd Edition, edited by the Chemical Society of Japan (Maruzen Co., Ltd.)" can be used, since the density and specific gravity are almost equivalent.

[0060] In the sintered body provided in the target according to this embodiment, the average crystal grain size of the indium oxide crystal grains contained in the sintered body is 5 μm or more and 25 μm or less. From the viewpoint of further suppressing the generation of nodules during sputtering, the average crystal grain size of the indium oxide crystal grains contained in the sintered body is preferably 5.2 μm or more, and more preferably 5.4 μm or more. The average crystal grain size of the indium oxide crystal grains contained in the sintered body is preferably 24 μm or less, and more preferably 23 μm or less. From the same viewpoint, the average crystal grain size of the indium oxide crystal grains contained in the sintered body may be, for example, 5.2 μm or more and 24 μm or less, or 5.4 μm or more and 23 μm or less.

[0061] In the sintered body provided in the target according to this embodiment, in the particle size distribution of the indium oxide crystal grains contained in the sintered body, the proportion of the indium oxide crystal grains having a particle size of 5 μm or more and 40 μm or less is preferably 90% or more by number. If the proportion of the indium oxide crystal grains having a particle size of 5 μm or more and 40 μm or less is 90% or more by number, it is easier to suppress the generation of nodules during sputtering. If the proportion of the indium oxide crystal grains having a particle size of 5 μm or more and 40 μm or less is more preferably 92% or more by number, even more preferably 94% or more, and even more preferably 95% or more by number. If the proportion of the indium oxide crystal grains having a particle size of 5 μm or more and 40 μm or less is 90% or more by number, abnormal grain growth is suppressed, and cracking of the target is more easily suppressed.

[0062] In the sintered body provided in the target according to this embodiment, in a field of view when the surface of the sintered body is observed at a magnification of 500 times, the area ratio of voids surrounded by three or more adjacent indium oxide crystal grains to the area of ​​the field of view is 3% or less. The area ratio of the voids is preferably less than 3%, more preferably 2.6% or less, and even more preferably 2.5% or less. If the area ratio of the voids is 3% or less, it is easier to suppress the generation of nodules during sputtering. Note that if the area ratio of voids surrounded by three or more adjacent indium oxide crystal grains is 3% or less, it can be determined that the area ratio of voids surrounded by three or more adjacent crystal grains on the sputtering surface of the oxide sintered body is 3% or less to the total area of ​​the sputtering surface.

[0063] The area ratio of vacancies surrounded by three or more adjacent indium oxide crystal grains means the ratio of vacancies present in a region surrounded by three or more adjacent indium oxide crystal grains, expressed as an area ratio. In this specification, a region surrounded by three or more adjacent indium oxide crystal grains may be referred to as a grain boundary multiple point. Examples of grain boundary multiple points include a grain boundary triple junction, which is a region surrounded by three adjacent indium oxide crystal grains, a grain boundary quadruple junction, which is a region surrounded by four adjacent indium oxide crystal grains, and a grain boundary quintuple junction, which is a region surrounded by five adjacent indium oxide crystal grains.

[0064] The average crystal grain size and particle size distribution of indium oxide contained in the sintered body, as well as the area ratio of voids, can be observed using a scanning electron microscope (SEM) or an electron probe X-ray microanalyzer (EPMA). The average crystal grain size and particle size distribution of indium oxide contained in the sintered body can be measured as follows. Specifically, first, when the shape of the sputtering target is circular, a square inscribed in the circle is divided into 16 equal areas, and a sintered body sample is prepared at the center of each square. When the shape of the sputtering target is rectangular or cylindrical, it is divided into 16 equal areas, and a sintered body sample is prepared at the center of each rectangle (16 in total). Here, the sintered body sample is a measurement sample. Sintered body samples were prepared by cutting the sintered body into pieces less than 1 cm (1 cm x 1 cm in size), and then embedding the sintered body samples in a 1-inch diameter epoxy-based room-temperature curing resin. The embedded sintered body samples were then polished sequentially using abrasive paper #400, #600, #800, 3 μm diamond suspension water, and 50 nm colloidal silica (for final finishing). The polished surface was then observed at an arbitrary magnification using an SEM or EPMA at an accelerating voltage of 10 kV, to the extent that 100 or more crystal grains could be observed. From the observation results of each sintered body sample, the crystal grains were measured as circle-equivalent diameters according to JIS R 1670, and the average crystal grain size and particle size distribution were calculated. The average crystal grain size of the crystalline phase contained in the sintered body was the average crystal grain size of the crystalline phase having a bixbyite structure composed mainly of In and O elements.

[0065] The area ratio of voids surrounded by three or more adjacent indium oxide crystal grains is observed by SEM or EPMA at a magnification of 500x using the same method as for the average crystal grain size and grain size distribution of indium oxide contained in the sintered body. Then, the contrast and brightness are adjusted using image processing software so that voids can be distinguished, and a binarization threshold is set to perform binarization. After binarization, the area ratio of voids is calculated.

[0066] In the sintered body used as the material for the target according to this embodiment, the flexural strength of the sintered body is preferably 170 MPa or more. The flexural strength of the sintered body is more preferably 175 MPa or more, and even more preferably 180 MPa or more. The upper limit of the flexural strength of the sintered body is not particularly limited. If the flexural strength of the sintered body is 170 MPa or more, for example, sputtering becomes easier while cracking of the target is suppressed. The flexural strength of the sintered body is determined based on JIS R 1601:2008 by placing a rectangular columnar test piece on two supports spaced 30 mm apart, applying a load to the presser with the presser in contact with the center, and calculating the average load (three-point bending strength) of 10 test pieces at which the test pieces break.

[0067] In one aspect, the sputtering target according to this embodiment preferably includes the above-described oxide sintered body and a backing plate. In one aspect, the sputtering target according to this embodiment may be a target consisting only of the oxide sintered body. The shape of the sputtering target is not particularly limited. The sputtering target may be, for example, a plate-like shape as shown by reference numeral 1 in FIG. 1A or a cylindrical shape as shown by reference numeral 1A in FIG. 1B. In the case of a plate-like shape, the planar shape may be a rectangle as shown by reference numeral 1 in FIG. 1A or a circle as shown by reference numeral 1B in FIG. 1C. The oxide sintered body may be integrally molded, or may be a multi-division type in which a plurality of divided oxide sintered bodies (reference numeral 1C) are each fixed to a backing plate 3 as shown in FIG. 1D.

[0068] <Method for manufacturing sputtering target> A preferred method for manufacturing the target according to this embodiment will be described. The method for manufacturing the sputtering target according to this embodiment is a method for manufacturing a sputtering target including an oxide sintered body containing indium oxide as a main component.

[0069] In one aspect, the manufacturing method includes the steps of: producing a molded body by adjusting the concentrations of raw material powder containing an indium compound as a main component and impurities so that the C (carbon) element contained in the oxide sintered body is 100 ppm or less by mass; and firing the molded body so that the average crystal grain size of the indium oxide crystal grains contained in the oxide sintered body is 5 μm or more and 25 μm or less.

[0070] In another aspect, the manufacturing method includes the steps of: producing a molded body using a raw material powder containing as a main component an indium compound having an average particle size of 0.1 μm or more and 2 μm or less; and firing the molded body by controlling at least the sintering temperature and sintering time so that the average crystal particle size of the indium oxide crystal grains contained in the oxide sintered body is 5 μm or more and 25 μm or less, and the area ratio of voids surrounded by three or more adjacent crystal grains on the sputtering surface of the oxide sintered body to the total area of ​​the sputtering surface is 3% or less.

[0071] In the step of producing a compact in the production method, it is preferable to crush raw material powder containing an indium compound as a main component using a crusher and then mold the powder.

[0072] In a preferred method for manufacturing the target according to this embodiment, the process for producing a molded body (hereinafter, this may be referred to as the molding process) may include a process for preparing a sintered body raw material containing a raw material powder mainly composed of an indium compound (hereinafter, this may be referred to as the sintered body raw material preparation process), a process for calcining the sintered body raw material obtained in the raw material preparation process (hereinafter, this may be referred to as the calcination process), which is a process that is provided as needed, and a molded body production process.

[0073] A preferred manufacturing method of the target according to this embodiment may further include, after a step of firing the molded body (hereinafter sometimes referred to as the firing step), at least one of a step of grinding the sintered body (hereinafter sometimes referred to as the grinding step), a step of cleaning the ground sintered body (hereinafter sometimes referred to as the cleaning step), and a step of bonding the sintered body to a backing plate (hereinafter sometimes referred to as the bonding step).

[0074] (Sintered body raw material preparation process) The sintered body raw material preparation process is a process of preparing a sintered body raw material containing an indium compound. In the sintered body raw material preparation process, first, a raw material powder of an indium compound to be used as a raw material for the sintered body included in the sputtering target according to this embodiment is prepared. Examples of the indium compound include at least one of an oxide of indium and a hydroxide of indium. From the viewpoint of ease of sintering and suppression of remaining by-products, the indium compound is preferably an oxide of indium (i.e., indium oxide).

[0075] The purity of the raw material powder of the indium compound is preferably 2N (99% by mass) or more, more preferably 3N (99.9% by mass) or more, and even more preferably 4N (99.99% by mass) or more. Furthermore, the content of hydrocarbon compounds in the raw material powder of the indium compound is preferably 0.6% by mass or less, more preferably 0.3% by mass or less, even more preferably 0.2% by mass or less, even more preferably 0.1% by mass or less, even more preferably 0.05% by mass or less, and even more preferably 0.01% by mass or less. It is particularly preferable that the raw material powder of the indium compound does not contain hydrocarbon compounds. By adjusting the purity of the indium compound and the content of the hydrocarbon compound, the impurity concentration of the sintered body can be reduced. Specifically, by adjusting the purity of the indium compound and the content of the hydrocarbon compound, the C (carbon) element as an impurity contained in the oxide sintered body can be easily reduced to 100 ppm or less by mass. Furthermore, by adjusting the purity of the indium compound and the content of the hydrocarbon compound, for example, in a TFT including an oxide thin film, the occurrence of electron scattering caused by impurities can be suppressed, thereby achieving high performance characteristics.

[0076] In the sintered body raw material preparation step, a raw material powder containing an indium compound as a main component is prepared. Therefore, in the sintered body raw material preparation step, in addition to the raw material powder of the indium compound, a raw material powder of a metal element compound exhibiting a positive tetravalent valence to be used as an additive element may be prepared. However, when the raw material powder of the metal element compound exhibiting a positive tetravalent valence is used as the amount contained in the sintered body, it is preferable to limit the content of the raw material powder of the metal element compound exhibiting a positive tetravalent valence to 2 atomic % or less (preferably 1.7 atomic % or less) relative to the indium oxide in the oxide sintered body. When using a raw material powder of a metal element compound exhibiting a positive tetravalent valence, limiting its content to 2 atomic % or less (preferably 1.7 atomic % or less) facilitates the formation of a thin film having a carrier concentration suitable for the semiconductor film of a TFT. The raw material powder of the metal element compound exhibiting a positive tetravalent valence preferably has the same purity as the raw material powder of the indium compound. The raw material powder of the metal element compound exhibiting a positive tetravalent valence is preferably adjusted in terms of the content of hydrocarbon compounds, as with the raw material powder of the indium compound. A single raw material powder of an indium compound and a mixed raw material powder of a raw material powder of an indium compound and a raw material powder of a compound of a metal element exhibiting a positive tetravalent valence may be collectively referred to simply as raw material powder.

[0077] The average particle size of the raw material powder is preferably 0.1 μm or more and 2 μm or less, and more preferably 0.5 μm or more and 1.5 μm or less. By controlling the particle size of the raw material powder, it is possible to easily suppress the occurrence of cracks and abnormal grain growth due to localized heating during sintering. Furthermore, by controlling the average particle size of the raw material powder within the range of 0.1 μm or more and 2 μm or less, crystallization in the sintering process is facilitated, the particle size distribution of the crystal grains contained in the sintered body becomes uniform, and the density of the sintered body is easily increased. The average particle size of the raw material powder can be measured using a laser diffraction particle size analyzer or the like.

[0078] The raw material powder may be prepared having an average particle size of, for example, 0.1 μm or more and 2 μm or less. Alternatively, the raw material powder may be prepared by, for example, crushing raw material powder having an average particle size larger than 2 μm using a crusher to adjust the average particle size of the raw material powder to be in the range of 0.1 μm or more and 2 μm or less. In this case, it is preferable to use raw material powder having an average particle size larger than 2 μm and mix and crush it using a crusher to adjust the average particle size of the raw material powder to be in the range of 0.1 μm or more and 2 μm or less.

[0079] The prepared raw material powders (single raw material powder of an indium compound, or a mixed raw material powder of an indium compound and a compound of a metal element exhibiting a positive tetravalent valence) are mixed and crushed to obtain a raw material mixture. The obtained raw material mixture may be used as a sintered body raw material. When the raw material powders are mixed and crushed, a binder may be added to the raw material powders. When a hydrocarbon compound is used as the binder, by using the minimum amount necessary as the binder, it becomes easier to reduce the C (carbon) element as an impurity contained in the oxide sintered body to 100 ppm or less by mass.

[0080] The mixing and crushing of the raw material powders can be performed using known crushers, such as a ball mill, bead mill, jet mill, or ultrasonic device. Among these methods, if hydrocarbon impurities are mixed in from at least one of the container and the crushing media, the hydrocarbon impurities will remain in the sintered body during sintering. Therefore, it is preferable to use a dry crushing and mixing method using a ceramic container and ceramic media, or a wet crushing and mixing method. From the perspective of suppressing the incorporation of hydrocarbon impurities, it is preferable to adopt a wet type mixing method for the mixing and crushing of the raw material powders. By suppressing the incorporation of hydrocarbon impurities, the C (carbon) element as an impurity contained in the oxide sintered body can be easily reduced to 100 ppm or less by mass. The mixing and crushing conditions can be adjusted as appropriate. The mixing and crushing time varies depending on the size of the equipment and the amount of raw material mixture to be processed. The processing time can be adjusted, for example, so that the particle size distribution of the raw material mixture is nearly uniform, with all particles being 2 μm or less (preferably all being 1 μm or less). Examples of crushing media (beads) used in a bead mill include zirconia, alumina, quartz, silicon nitride, stainless steel, mullite, glass, and silicon carbide (SiC). In this specification, the terms "crushing" and "pulverization" can be interchangeable in some cases.

[0081] The raw material mixture after mixing and crushing may be rapidly dried and granulated by a spray drying method. A raw material granulated powder is obtained by granulating the raw material mixture. Specifically, a spray dryer is used to granulate the raw material mixture after mixing and crushing. The specific drying conditions using a spray dryer are determined by various conditions such as the concentration of the raw material mixture to be dried, the hot air temperature used for drying, the rotation speed of the spray dryer, and the air volume. When performing the spray drying method, it is advisable to determine the optimal conditions in advance. The shape of the raw material granulated powder obtained by granulating the raw material mixture is not particularly limited, but a spherical shape is preferable. The obtained raw material granulated powder may be used as a sintered body raw material.

[0082] When a raw material mixture as a sintered body raw material that has not been subjected to a calcination treatment in the calcination step described below is used and the raw material mixture is granulated by a spray drying method, the raw material mixture after mixing and crushing may be used as is to prepare the raw material granulated powder. When a raw material mixture as a sintered body raw material that has been subjected to a calcination treatment in the calcination step described below is used and the raw material mixture is granulated by a spray drying method, the raw material mixture that has been subjected to the calcination treatment may be used again as a crushed raw material mixture. In the raw material mixture that has been subjected to the calcination treatment, particles are bonded to each other, so when a granulation treatment is performed, it is preferable to perform a crushing treatment before the granulation treatment.

[0083] The granulated raw granulated powder may be classified to adjust the particle size of the raw granulated powder. The raw granulated powder with the adjusted particle size may be used as a sintered raw material. Examples of classification methods include sieving the raw granulated powder that has been subjected to a granulation process to select particles belonging to a desired particle size range. The sieve used in this method is preferably a sieve having openings large enough to allow raw granulated powder of a desired particle size to pass through. The sieves used in this method are preferably a first sieve for selecting the raw granulated powder based on the lower limit of the particle size range and a second sieve for selecting the raw granulated powder based on the upper limit of the particle size range. For example, when controlling the particle size of the raw granulated powder to a range of 150 μm or less, a sieve having openings large enough to allow raw granulated powder of 150 μm or less to pass through but not raw granulated powder exceeding 150 μm is used to select raw granulated powder within the range of 150 μm or less. Furthermore, when the particle size of the raw granulated powder is controlled to, for example, a range of 25 μm or more and 150 μm or less, first, a sieve (first sieve) having openings large enough to allow raw granulated powder less than 25 μm to pass through but not allow raw granulated powder of 25 μm or more to pass through is used to select raw granulated powder having a particle size of 25 μm or more. Next, the raw granulated powder after this selection is sorted using a sieve (second sieve) having openings large enough to allow raw granulated powder of 150 μm or less to pass through but not allow raw granulated powder of more than 150 μm to pass through, to select raw granulated powder having a particle size of 25 μm or more and 150 μm or less. The second sieve may be used first, followed by the first sieve.

[0084] (Calking Step) The target manufacturing method according to this embodiment may include a step of calcining the sintered raw material obtained in the raw material preparation step (this step is referred to as the calcining step). In the calcining step, the sintered raw material as a raw material mixture obtained after mixing and crushing the raw material powder may be calcined. In the calcining step, after obtaining the sintered raw material as a raw material mixture that will be the raw material of the sputtering target material, this raw material mixture (i.e., the sintered raw material) is calcined. The calcining step is a step that is provided as needed.

[0085] Since calcination makes it easy to increase the density of the sintered body obtained, the method for manufacturing a target according to this embodiment preferably includes a calcination step. On the other hand, from the viewpoint of suppressing an increase in costs, it is more preferable to increase the density of the sintered body without providing a calcination step.

[0086] In the calcination, the sintered body raw material is preferably heat-treated at a temperature ranging from 500°C to 1200°C for a treatment time ranging from 1 hour to 100 hours. The calcination is preferably carried out at a temperature ranging from 800°C to 1200°C for a treatment time ranging from 2 hours to 50 hours. By setting the heat treatment conditions to 500°C or higher and 1 hour or longer, the thermal decomposition of the indium compound is sufficient. On the other hand, by setting the heat treatment conditions to 1200°C or lower and 100 hours or shorter, particle coarsening can be suppressed. The calcined product obtained in the calcination step is preferably crushed before the molding step and firing step described below.

[0087] (Molded body preparation process) The molded body preparation process of the molding process is included in the process of producing a molded body using a raw material powder mainly composed of an indium compound. Specifically, the molded body preparation process is a process of pressurizing and molding the above-mentioned sintered body raw material (or the calcined product as the sintered body raw material if the calcination process is provided) to form a molded body. This process forms the molded body into a shape suitable for a target. If the calcination process is provided, the obtained fine powder of the calcined product can be granulated and then press-molded into a desired shape.

[0088] The average thickness of the molded body is preferably 5.5 mm or more, more preferably 6 mm or more, even more preferably 8 mm or more, and particularly preferably 12 mm or more. When the average thickness of the molded body is 5.5 mm or more, the temperature gradient in the thickness direction of the molded body is reduced, and it is expected that the combination of crystal types on the surface and in the depths is less likely to change.

[0089] Examples of molding processes that can be used in the molding step include press molding (uniaxial pressing), mold molding, slip casting, and injection molding. In order to obtain a sintered body (target) with high sintering density, molding is preferably performed by cold isostatic pressing (CIP) or the like. Furthermore, two or more molding steps may be performed, such as by cold isostatic pressing (CIP) and hot isostatic pressing (HIP) after press molding (uniaxial pressing).

[0090] When using a cold isostatic or hydrostatic pressure device, the surface pressure is 78.5 MPa (800 kgf / cm 2 converted to SI units) or more, 392.4 MPa (4000 kgf / cm 2 It is preferable to hold the sintered compact at a pressure of 196.2 MPa or more and 294.3 MPa or less for 0.5 minutes or more and 60 minutes or less. It is more preferable to hold the sintered compact at a pressure of 196.2 MPa or more and 294.3 MPa or less for 2 minutes or more and 30 minutes or less. Within the above range, it is expected that compositional irregularities inside the compact will be reduced and made uniform. By setting the sintered compact at a pressure of 78.5 MPa or more, the resistance of the sintered compact after sintering can be reduced. By setting the sintered compact at a pressure of 392.4 MPa or less, molding can be performed without increasing the size of the equipment. A holding time of 0.5 minutes or more can prevent the resistance after sintering from becoming high. A holding time of 60 minutes or less can prevent the process from taking too long and becoming uneconomical.

[0091] In the molding process, a molding aid is preferably used to reduce the proportion of voids in the sintered body. The use of a molding aid facilitates control of the crystal grain size of the oxide sintered body, making it easier to control the area ratio of voids surrounded by three or more adjacent crystal grains to 3% or less. The molding aid can be an inorganic molding aid primarily composed of alumina or silica, which does not contain hydrocarbon compounds. Alternatively, organic molding aids such as polyvinyl alcohol, methyl cellulose, polywax, and oleic acid may be used. However, when using a molding aid, it is preferable to use the minimum amount of molding aid required for slurrying. Too little molding aid can make it difficult to control the particle size of the raw granulated powder, resulting in a decrease in the density of the sintered body. Furthermore, too much molding aid can cause unintended metal elements to be mixed into the oxide sintered body or can cause the carbon (C) element to exceed 100 ppm by mass, which tends to increase the area ratio of voids surrounded by three or more adjacent crystal grains. The minimum required amount of molding aid varies depending on the amount of raw material powder, the type of molding aid, and the molding conditions of the raw material powder, and is adjusted appropriately depending on the production conditions. By using the minimum required amount of molding aid, it is possible to prevent unintended contamination of metal elements contained in the oxide sintered body, and also to reduce the C (carbon) element as an impurity contained in the oxide sintered body to 100 ppm or less by mass.

[0092] By the molding process described above (including the sintered body raw material preparation process, the calcination process, and the molded body production process), the impurity concentration of the molded body using a raw material powder mainly composed of an indium compound (for example, a raw material powder mainly composed of indium oxide powder) is adjusted so that the C (carbon) element contained in the oxide sintered body is 100 ppm or less by mass. Furthermore, by using a raw material powder mainly composed of an indium compound and adjusting the impurity concentration to produce a molded body so that the C (carbon) element contained in the oxide sintered body is 100 ppm or less by mass, atomic diffusion of indium oxide proceeds uniformly in the subsequent firing process, abnormal grain growth can be suppressed, and voids in the sintered body can be reduced. Specifically, the above advantages can be obtained by using a raw material powder containing an indium compound as the main component, in which the purity of the indium compound and the content of the hydrocarbon compound have been adjusted, and producing a molded body by adjusting the concentration of impurities; or, in the case of using a compound of a metal element exhibiting a positive tetravalent valence, using a raw material powder in which the purity of the indium compound and the compound of the metal element exhibiting a positive tetravalent valence and the content of the hydrocarbon compound have been adjusted, and producing a molded body by adjusting the concentration of impurities.

[0093] (Firing Step) The firing step is a step of firing the molded body produced in the molding step. In this specification and the like, the terms "firing" and "sintering" can be interchangeable in some cases. In the firing step, a sintered body is obtained by sintering the molded body obtained in the molding step. In the firing step, a commonly used sintering method such as atmospheric sintering, hot press sintering, or hot isostatic pressing (HIP) sintering can be used. The obtained sintered body becomes a sputtering target material.

[0094] The sintering temperature is preferably higher than 1400°C and not higher than 1700°C. The sintering temperature is more preferably 1410°C or higher, even more preferably 1420°C or higher, even more preferably 1470°C or higher, and even more preferably 1500°C or higher. The sintering temperature is preferably 1680°C or lower, more preferably 1660°C or lower, and even more preferably 1650°C or lower. The sintering time is preferably 10 hours or longer and 50 hours or shorter, more preferably 12 hours or longer and 40 hours or shorter, and even more preferably 13 hours or longer and 30 hours or shorter.

[0095] When the sintering temperature is higher than 1400°C and the sintering time is 10 hours or longer, the density of the sintered body can be improved, and the average crystal grain size of the crystal grains contained in the sintered body can be controlled to a range of 5 μm to 25 μm, making it difficult for abnormal discharge of the target to occur.When the sintering temperature is 1700°C or lower and the sintering time is 50 hours or shorter, it is possible to suppress an increase in the average crystal grain size due to significant crystal grain growth and the occurrence of coarse voids, making it difficult for a decrease in the strength of the sintered body and abnormal discharge of the target to occur.

[0096] In one aspect of the firing step, by controlling at least the sintering temperature and sintering time within the above ranges, a sintered body can be obtained in which the average crystal grain size of the indium oxide crystal grains contained in the oxide sintered body is 5 μm or more and 25 μm or less, and the area ratio of voids surrounded by three or more adjacent crystal grains to the total area of ​​the sputtering surface of the oxide sintered body is 3% or less. The sputtering surface of the oxide sintered body may be a flat surface or a curved surface. Both the flat surface and the curved surface may include irregularities. The total area of ​​the sputtering surface is the surface of the sputtering surface of the oxide sintered body. For example, if the sputtering surface is a curved surface including irregularities, the total area of ​​the sputtering surface represents the surface area of ​​the curved surface including the irregularities. The area ratio of voids surrounded by three or more adjacent indium oxide crystal grains to the total area of ​​the sputtering surface being 3% or less can be achieved by satisfying that, in a field of view when the surface of the sintered body is observed at a magnification of 500 times, the area ratio of voids surrounded by three or more adjacent indium oxide crystal grains to the area of ​​the field of view is 3% or less. This area ratio can be measured by the measurement method described above.

[0097] In the atmospheric sintering method, the compact is sintered in an air atmosphere or an oxygen gas atmosphere. The oxygen gas atmosphere preferably has an oxygen concentration of, for example, 10% by volume or more and 50% by volume or less. By performing the temperature rise process in an air atmosphere, the density of the sintered body can be increased.

[0098] In order to more easily control the particle size distribution of indium oxide crystal grains in the oxide sintered body so that the proportion of particles with particle sizes of 5 μm or more and 40 μm or less is 90% or more by number, for example, it is preferable to control the temperature distribution in the sintering furnace as the atmosphere in the sintering process to ±50°C or less from the set sintering temperature within a range of more than 1400°C and less than 1700°C. The temperature distribution in the sintering furnace is more preferably ±40°C or less from the set sintering temperature, even more preferably ±30°C or less from the set sintering temperature, and even more preferably ±20°C or less from the set sintering temperature. By controlling the temperature distribution in the sintering furnace to ±50°C or less from the set temperature, the particle size growth of indium oxide is more easily uniform, and nodule generation during sputtering is more easily suppressed. Here, ±50°C or less from the set sintering temperature means a range of -50°C or more from the set sintering temperature to +50°C or less from the set sintering temperature.

[0099] The heating rate during sintering is preferably 0.1°C / min or more and 2°C / min or less when increasing the temperature from 800°C to the sintering temperature. In the sintered body according to this embodiment, the temperature range of 800°C or more is the temperature range in which sintering proceeds most rapidly. If the heating rate within this temperature range is 0.1°C / min or more, the C (carbon) element contained in the dispersion aid can be efficiently reduced, and excessive grain growth can be suppressed, thereby reducing voids in the oxide sintered body and achieving high density. Furthermore, if the heating rate is 2°C / min or less, temperature distribution in the molded body can be suppressed, and warping or cracking of the sintered body can be suppressed. When increasing the temperature from 800°C to the sintering temperature, the heating rate is preferably 0.5°C / min or more and 2.0°C / min or less, and more preferably 1.0°C / min or more and 1.8°C / min or less.

[0100] By the firing process described above, the average crystal grain size of the indium oxide crystal grains contained in the sintered body can be controlled to 5 μm or more and 25 μm or less. Also, the average crystal grain size of the indium oxide crystal grains contained in the sintered body can be controlled to 5 μm or more and 25 μm or less, and the area ratio of vacancies present at multi-point grain boundaries can be controlled to 3% or less. Furthermore, the average crystal grain size of the indium oxide crystal grains contained in the sintered body can be controlled to 5 μm or more and 25 μm or less, and the density can be controlled to 6.9 g / cm. 3 As a result, a sintered body can be obtained in which the area ratio of voids present at multiple grain boundaries is 3% or less.

[0101] (Grinding process) The grinding process is a process of cutting the sintered body into a shape suitable for installation in a sputtering device. The surface of the sintered body often has at least one of the following phenomena: the presence of a highly oxidized sintered portion, or the surface is uneven. The sintered body is then cut to a specified size.

[0102] In the grinding step, the surface of the sintered body is preferably ground off by 0.3 mm or more, more preferably by 0.5 mm or more, and even more preferably by 2 mm or more. By grinding off the surface of the sintered body by 0.3 mm or more, it is possible to remove portions of the crystal structure near the surface that have changed.

[0103] The oxide sintered body is preferably ground, for example, by a surface grinder to obtain a material having an average surface roughness Ra of 5 μm or less. Furthermore, the sputtering surface of the sputtering target is subjected to mirror finishing to obtain a material having an average surface roughness Ra of 1000×10 -10 The polishing method may be 1 / 2 m or less. This mirror finish (polishing) can be performed using known polishing techniques such as mechanical polishing, chemical polishing, mechanochemical polishing (a combination of mechanical polishing and chemical polishing), etc. For example, polishing to #2000 or higher may be performed using a fixed abrasive polisher (using water as the polishing liquid), or lapping may be performed using a free abrasive lap (using SiC paste or the like as the abrasive), and then the abrasive may be replaced with diamond paste for lapping. The polishing method is not limited to these methods. Examples of the abrasive include #200, #400, or #800 abrasives.

[0104] (Cleaning step) After the grinding step, the oxide sintered body is preferably cleaned by cleaning means such as air blowing and running water washing. When removing foreign matter by air blowing, removal can be made more effective by using a dust collector to suck air from the opposite side of the nozzle. Note that there are limitations to air blowing and running water washing, so ultrasonic cleaning or the like can also be performed. An effective ultrasonic cleaning method is to use multiple oscillations at a frequency between 25 kHz and 300 kHz. For example, it is recommended to perform ultrasonic cleaning by multiple oscillations at 12 different frequencies in 25 kHz increments between 25 kHz and 300 kHz.

[0105] (Bonding Step) The bonding step is a step of bonding the sintered body after the processing step to a backing plate with a low melting point metal (for example, metallic indium, metallic gallium, etc.).

[0106] In order to maintain cooling efficiency during sputtering, the bonding rate is preferably 90% or more, more preferably 95% or more, and even more preferably 98% or more. The bonding rate here refers to the ratio of the area of ​​the surface where the target material and the target support material are bonded via the bonding layer to the area of ​​the overlapping surfaces of the target material and the target support.

[0107] [Oxide Thin Film] The oxide thin film according to this embodiment is an oxide thin film formed using the sputtering target according to this embodiment. The oxide thin film according to this embodiment is obtained by film formation using the sputtering target according to this embodiment. The oxide thin film according to this embodiment is an oxide semiconductor thin film. The oxide thin film according to this embodiment is preferably obtained by a production method including, for example, a step of forming an oxide thin film by sputtering using the sputtering target according to this embodiment (hereinafter, sometimes referred to as an oxide thin film formation step), and a step of subjecting the oxide thin film to a heat treatment (hereinafter, sometimes referred to as a heat treatment step).

[0108] The oxide thin film according to this embodiment is an amorphous oxide thin film after sputtering deposition and before heat treatment (annealing treatment), and the heat treatment after sputtering deposition improves crystallization, turning it into a crystalline oxide thin film. In other words, a crystalline oxide thin film can be obtained by the method for producing an oxide thin film according to this embodiment. In this embodiment, a crystalline oxide thin film may also be referred to as a "crystalline oxide thin film."

[0109] Whether an oxide thin film is amorphous or crystalline can be confirmed by X-ray diffraction (XRD) measurement of each oxide thin film. When no peak is observed in XRD measurement of an oxide thin film, the oxide thin film is determined to be amorphous, and when a peak is observed, the oxide thin film is determined to be crystalline. Note that when XRD measurement of an oxide thin film is performed, if a broad pattern is observed instead of a clear peak, the oxide thin film is determined to be nanocrystalline. On the other hand, even when XRD measurement of an oxide thin film indicates that the oxide thin film is amorphous, when residues (patterning residues) generated during patterning processing in fabricating TFTs are confirmed, the residues may be present. For this reason, even when XRD measurement of an oxide thin film indicates that the oxide thin film is amorphous, it is difficult to determine whether the oxide thin film is uniformly amorphized.

[0110] In the oxide thin film formation process, it is preferable to use a gas that is substantially free of impurity gases. Specifically, in the oxide thin film formation process, it is preferable to use one or more gases selected from the group consisting of argon, hydrogen, water vapor, and oxygen, which are substantially free of impurity gases, as the sputtering gas. Among these, the sputtering gas is preferably a mixed gas of argon, hydrogen, water vapor, and oxygen that is substantially free of impurity gases, and more preferably a mixed gas of argon, hydrogen, and oxygen that is substantially free of impurity gases. The phrase "substantially free of impurity gases" means that impurity gases other than argon, hydrogen, water vapor, and oxygen are not actively introduced, except for adsorbed water brought in due to gas insertion, chamber leaks, and gases that cannot be eliminated (unavoidable impurity gases), such as adsorbed gases. In this embodiment, the sputtering gas may be, for example, a commercially available mixed gas of high-purity argon and high-purity oxygen, a mixed gas of high-purity hydrogen and high-purity argon, or a mixed gas of high-purity hydrogen, high-purity oxygen, and high-purity argon. The sputtering gas is preferably a mixture of high-purity hydrogen, high-purity oxygen, and high-purity argon, and impurity gases are preferably excluded from the sputtering gas, if possible.

[0111] The proportion of impurity gas in the sputtering gas is preferably 0.1 vol% or less, more preferably 0.05 vol% or less. If the proportion of impurity gas is 0.1 vol% or less, crystallization of the oxide thin film proceeds without problems by annealing treatment after film formation. When a mixed gas of high-purity hydrogen, high-purity oxygen, and high-purity argon is used, the purity of each of the high-purity argon, high-purity hydrogen, and high-purity oxygen is preferably 99 vol% or more, more preferably 99.9 vol% or more, and even more preferably 99.99 vol% or more.

[0112] When a mixed gas of high-purity hydrogen, high-purity oxygen, and high-purity argon is used as the sputtering gas, the oxygen partial pressure in the mixed gas of argon, hydrogen, and oxygen, which is the sputtering gas, is [O 2 ] / ([Ar]+[H 2 ]+[O 2]). The oxygen partial pressure is preferably in the range of 0% to 20%. If the oxygen partial pressure is in the above range, the film is easily crystallized and becomes a semiconductor by annealing after film formation. By changing the oxygen partial pressure, the degree of oxidation of the resulting thin film, i.e., the degree of crystallization, can be adjusted. The oxygen partial pressure can be selected appropriately as needed.

[0113] When a mixed gas of high-purity hydrogen, high-purity oxygen, and high-purity argon is used as the sputtering gas, the hydrogen partial pressure in the mixed gas of argon, hydrogen, and oxygen, which is the sputtering gas, is [H 2 ] / ([Ar]+[H 2 ]+[O 2 ]). The hydrogen partial pressure is preferably in the range of 0% to 10%, more preferably in the range of 0% to 5%. By changing the hydrogen partial pressure, the hydrogen content of the semiconductor thin film can be adjusted, and the degree of crystallization immediately after film formation can be controlled. The hydrogen partial pressure can be selected appropriately as needed.

[0114] In the heat treatment step, the heat treatment temperature for crystallizing the amorphous thin film after film formation is preferably in the range of 200°C to 500°C, and more preferably in the range of 250°C to 470°C. If the heat treatment temperature is 200°C or higher, the oxide thin film is easily crystallized. If the heat treatment temperature is 500°C or lower, abnormal crystal growth and enlargement of crystal grains can be suppressed, and hydrogen is less likely to be desorbed from the crystal grains, suppressing the generation of defect level density. Therefore, when applied to TFTs, electrical characteristics with good mobility and reliability can be obtained.

[0115] In the heat treatment step, the heat treatment time for crystallizing the amorphous thin film after film formation is preferably 0.1 to 5 hours, more preferably 0.3 to 3 hours, and even more preferably 0.5 to 2 hours. If the heat treatment time is 0.1 hours or more, the oxide thin film is likely to crystallize without failing to crystallize. If the heat treatment time is 5 hours or less, it is economically advantageous.

[0116] The carrier concentration of the oxide thin film according to this embodiment is 1×10 19 / cm3 Preferably, it is 1×10 or less. 18 / cm 3 The carrier concentration of the oxide thin film according to this embodiment is more preferably 1×10 13 / cm 3 The oxide thin film according to this embodiment may have a carrier concentration of 1×10 or more. 19 / cm 3 or less (preferably 1 × 10 18 / cm 3 When the oxide thin film has a carrier concentration of 0.01 to 0.10, the oxide thin film is likely to exhibit oxide semiconductor properties. The carrier concentration can be measured by Hall effect measurement.

[0117] The oxide thin film according to this embodiment can be applied to various integrated circuits such as logic circuits, memory circuits, and differential amplifier circuits, and can be applied to electronic devices, etc. The oxide thin film according to this embodiment can also be applied as a part of a layer in a solar cell, and a part of a layer in a display device such as a liquid crystal device, an organic electroluminescence device, an inorganic electroluminescence device, a micro organic EL display, a micro LED (Light Emitting Diode) display, and a mini LED display. Furthermore, the oxide thin film according to this embodiment can be applied as a part of a layer in a solid-state imaging device, an X-ray sensor, a power semiconductor device, a touch panel, an LSI (Large Scale Integrated Circuit), a resistance change type memory, a DRAM (Dynamic Random Access Memory), a ferroelectric memory, a BEOL (Back End of Line), and a microprocessor. The oxide thin film according to this embodiment can also be used as a semiconductor layer of a field-effect transistor, a static induction transistor, a quantum tunnel field-effect transistor, a Schottky barrier transistor, a Schottky diode, a PN diode, and a resistor element, or as a part of any of these layers.

[0118] [Thin Film Transistor and Electronic Device] The thin film transistor according to this embodiment includes a thin film transistor including the oxide thin film according to this embodiment. The oxide thin film according to this embodiment is preferably an oxide semiconductor thin film.

[0119] It is preferable to use the oxide thin film according to this embodiment as the channel layer of a thin film transistor.

[0120] When the thin film transistor according to this embodiment has the oxide thin film according to this embodiment as a channel layer, other element configurations in the thin film transistor are not particularly limited, and known element configurations can be adopted.

[0121] The thin film transistor according to this embodiment can be suitably used in electronic devices. Specifically, the thin film transistor according to this embodiment can be suitably used in display devices such as liquid crystal displays and organic EL displays.

[0122] The thickness of the channel layer in the thin film transistor according to this embodiment is usually 10 nm or more and 300 nm or less, and preferably 20 nm or more and 250 nm or less.

[0123] The channel layer in the thin film transistor according to this embodiment is usually used in an N-type region, but can also be used in various semiconductor devices such as a PN junction transistor in combination with various P-type semiconductors, such as a P-type Si-based semiconductor, a P-type oxide semiconductor, and a P-type organic semiconductor.

[0124] The thin film transistor according to this embodiment can be applied to various integrated circuits such as field-effect transistors, logic circuits, memory circuits, and differential amplifier circuits. Furthermore, in addition to field-effect transistors, the thin film transistor can also be applied to static induction transistors, Schottky barrier transistors, Schottky diodes, and resistor elements. That is, the thin film transistor according to this embodiment can be applied to the applications exemplified in the "Applications of Thin Film Transistors" section described later.

[0125] The shape of the thin film transistor according to this embodiment is not particularly limited, and is preferably a back channel etch type transistor, an etch stopper type transistor, a top gate type transistor, a double gate type transistor, etc. Each transistor may have a self-aligned structure.

[0126] Specific examples of thin film transistors are shown in Figures 2, 3, 4, and 5. As shown in Figure 2, a thin film transistor 100 includes a silicon wafer 20, a gate insulating film 30, an oxide thin film 40, a source electrode 50, a drain electrode 60, and interlayer insulating films 70 and 70A.

[0127] The silicon wafer 20 is a gate electrode. The gate insulating film 30 is an insulating film that blocks electrical conduction between the gate electrode and the oxide thin film 40, and is provided on the silicon wafer 20. The oxide thin film 40 is a channel layer and is provided on the gate insulating film 30. The oxide thin film 40 is made of the oxide thin film according to this embodiment.

[0128] The source electrode 50 and the drain electrode 60 are conductive terminals for passing source current and drain current through the oxide thin film 40, and are provided so as to be in contact with the vicinity of both ends of the oxide thin film 40. The interlayer insulating film 70 is an insulating film that blocks conduction between the source electrode 50 and the drain electrode 60 and the oxide thin film 40 except at the contact portions between the source electrode 50 and the drain electrode 60 and the oxide thin film 40. The interlayer insulating film 70A is an insulating film that blocks conduction between the source electrode 50 and the drain electrode 60 and the oxide thin film 40 except at the contact portions between the source electrode 50 and the drain electrode 60 and the oxide thin film 40. The interlayer insulating film 70A is also an insulating film that blocks conduction between the source electrode 50 and the drain electrode 60. The interlayer insulating film 70A also functions as a channel layer protective layer.

[0129] 3, the structure of the thin-film transistor 100A is similar to that of the thin-film transistor 100, except that the source electrode 50 and the drain electrode 60 are provided so as to be in contact with both the gate insulating film 30 and the oxide thin film 40. Another difference is that an interlayer insulating film 70B is provided integrally so as to cover the gate insulating film 30, the oxide thin film 40, the source electrode 50, and the drain electrode 60.

[0130] There are no particular limitations on the materials forming the drain electrode 60, the source electrode 50, and the gate electrode, and any commonly used material can be selected. In the examples shown in Figures 2 and 3, a silicon wafer is used as the substrate, and the silicon wafer also functions as the electrode, but the electrode material is not limited to silicon. For example, indium tin oxide (ITO), indium zinc oxide (IZO), ZnO, and SnO 2 2, 3, 4, and 5, a gate electrode may be formed on a substrate such as glass.

[0131] There is no particular limitation on the material for forming the interlayer insulating films 70, 70A, and 70B, and any commonly used material can be selected. x , M.N. x , and M.N. x O y (where M is a metal element, and x and y are real numbers greater than 0. The same applies to x and y in the compounds exemplified below.) Specific examples of the material include SiO 2 , SiO x , SiN x , and SiN x O y Furthermore, the material can be, for example, Al 2 O 3 , Ta 2 O 5 , TiO 2 , MgO, ZrO 2 , CeO 2 , K. 2 O, Li 2 O, Na 2 O, Rb 2 O, Sc 2 O 3 , Y 2 O 3 , HfO 2 , CaHfO 3 , PbTiO 3,BaTa 2 O 6 , SrTiO 3 , Sm 2 O 3 Compounds such as AlN can also be used. The valence of the anions (oxygen anions and nitrogen anions) in these oxide compounds and nitride compounds is not particularly limited as long as it is a real number greater than 0.

[0132] When the thin film transistor according to this embodiment is a back channel etch type (bottom gate type), it is preferable to provide a protective film on the drain electrode, the source electrode, and the channel layer. By providing a protective film, the durability of the TFT is likely to be improved even when the TFT is driven for a long time. In the case of a top gate type TFT, for example, a gate insulating film is formed on the channel layer.

[0133] When the thin-film transistor according to this embodiment is a top-gate TFT, for example, it has a structure in which an interlayer insulating film is formed as a buffer layer on a substrate and a gate insulating film is formed on a channel layer. As shown in FIG. 4, the thin-film transistor 100B includes a substrate 21, a buffer layer 22, a channel layer (crystalline oxide thin film) 11, a first low-resistance region 11A-1, a second low-resistance region 11A-2 (crystalline oxide thin film), a semiconductor region 11B (crystalline oxide thin film), a gate insulating film 24, a gate electrode 25, an interlayer insulating film 26, a source electrode 27, a drain electrode 28, and a protective film 29. In the thin-film transistor 100B, the first low-resistance region 11A-1 and the second low-resistance region 11A-2 are formed, for example, by dry processes such as ion implantation and plasma treatment. An electrode layer may also be provided between the substrate 21 and the buffer layer 22 as a write shield layer.

[0134] 5, in the case where the thin-film transistor according to the present embodiment is a top-gate TFT, a thin-film transistor 100C has a similar configuration to the thin-film transistor 100B except that the interlayer insulating film 26 has a two-layer structure (a first interlayer insulating film 26-1 and a second interlayer insulating film 26-2). In the thin-film transistor 100C, the first low-resistance region 11A-1 and the second low-resistance region 11A-2 are formed by, for example, ion implantation.

[0135] The protective film or insulating film can be formed by, for example, CVD, which may require high-temperature processes. Furthermore, the protective film or insulating film often contains impurity gases immediately after deposition, so it is preferable to subject it to a heat treatment (annealing treatment). Removing the impurity gases through the heat treatment results in a stable protective film or insulating film, which facilitates the formation of highly durable TFT elements.

[0136] By using the oxide thin film according to this embodiment, the film is less susceptible to the effects of temperature in the CVD process and subsequent heat treatment, and therefore the stability of the TFT characteristics can be improved even when a protective film or an insulating film is formed.

[0137] In the characteristics of the thin film transistor according to this embodiment, the On / Off ratio is 10 6 That's it, 10 12 The following is preferred: 7 That's it, 10 11 More preferably, 10 or less 8 That's it, 10 10 More preferably, the On / Off ratio is 10 or less. 6 An On / Off ratio of 10 or more is preferable for driving liquid crystal and OLED displays. 12 If the On / Off ratio is 10 or less, an organic EL display with high contrast can be driven. 12 If the off-state current is 10 -11 A or less, and when the thin film transistor is used as a transfer transistor or reset transistor in a CMOS image sensor, it is possible to extend the image retention time and improve the sensitivity. The On / Off ratio can be calculated by determining the ratio [On current value / Off current value], where the value of Id when Vg = -10 V is the Off current value and the value of Id when Vg = 20 V is the On current value.

[0138] In the characteristics of the thin film transistor according to this embodiment, the threshold voltage (Vth) is preferably −3.0 V or more and 3.0 V or less, more preferably −2.0 V or more and 2.0 V or less, and even more preferably −1.0 V or more and 1.0 V or less. When the threshold voltage (Vth) is −3.0 V or more and 3.0 V or less, by incorporating a Vth correction circuit into the TFT, correction to Vth = 0 V becomes possible. When the TFT obtained in this way is incorporated into a panel, it is possible to drive a display without uneven brightness or burn-in. From the transfer characteristic graph, the threshold voltage (Vth) is determined by the current value Id between the source and drain = 10 -9 It can be defined as the gate voltage Vg at A.

[0139] <Quantum Tunnel Field Effect Transistor> The oxide thin film according to this embodiment can also be used in a quantum tunnel field effect transistor (FET), which may also be referred to as a quantum tunnel field effect transistor.

[0140] 6 is a schematic diagram (longitudinal cross-sectional view) of a quantum tunnel field effect transistor (FET) according to one embodiment. The quantum tunnel field effect transistor 501 includes a p-type semiconductor layer 503, an n-type semiconductor layer 507, a gate insulating film 509, a gate electrode 511, a source electrode 513, and a drain electrode 515.

[0141] A p-type semiconductor layer 503, an n-type semiconductor layer 507, a gate insulating film 509, and a gate electrode 511 are stacked in this order. A source electrode 513 is provided on the p-type semiconductor layer 503. A drain electrode 515 is provided on the n-type semiconductor layer 507. The p-type semiconductor layer 503 is a p-type Group IV semiconductor layer, and in this case is a p-type silicon layer. In this case, the n-type semiconductor layer 507 is an n-type oxide thin film according to the above embodiment. The source electrode 513 and the drain electrode 515 are conductive films.

[0142] Although not shown in Fig. 6, an insulating layer may be formed on the p-type semiconductor layer 503. In this case, the p-type semiconductor layer 503 and the n-type semiconductor layer 507 are connected via a contact hole, which is a region where the insulating layer is partially opened. Although not shown in Fig. 6, the quantum tunnel field effect transistor 501 may also have an interlayer insulating film covering its upper surface.

[0143] The quantum tunnel field effect transistor 501 is a quantum tunnel field effect transistor (FET) that switches current by controlling the current tunneling through the energy barrier formed by the p-type semiconductor layer 503 and the n-type semiconductor layer 507 using the voltage of the gate electrode 511. In this structure, the band gap of the oxide thin film that constitutes the n-type semiconductor layer 507 is large, making it possible to reduce the off-current.

[0144] FIG. 7 is a schematic diagram (longitudinal cross-sectional view) of a quantum tunnel field-effect transistor 501A according to another embodiment. The quantum tunnel field-effect transistor 501A has the same configuration as the quantum tunnel field-effect transistor 501, except that a silicon oxide layer 505 is formed between a p-type semiconductor layer 503 and an n-type semiconductor layer 507. The presence of the silicon oxide layer reduces the off-state current. The thickness of the silicon oxide layer 505 is preferably 10 nm or less. By making the thickness of the silicon oxide layer 505 10 nm or less, it is possible to prevent tunneling current from flowing, the formation of an energy barrier from being difficult, and changes in barrier height, thereby preventing a decrease or change in the tunneling current. The thickness of the silicon oxide layer 505 is preferably 8 nm or less, more preferably 5 nm or less, even more preferably 3 nm or less, and even more preferably 1 nm or less.

[0145] In the quantum tunnel field effect transistors 501 and 501A, the n-type semiconductor layer 507 is also an n-type oxide semiconductor.

[0146] The oxide thin film constituting the n-type semiconductor layer 507 may be amorphous. When the oxide thin film constituting the n-type semiconductor layer 507 is amorphous, it can be etched with an organic acid such as oxalic acid, the difference in etching rate with other layers becomes large, and etching can be performed satisfactorily without affecting metal layers such as wiring.

[0147] The oxide thin film constituting the n-type semiconductor layer 507 may be crystalline. When the oxide thin film constituting the n-type semiconductor layer 507 is crystalline, the band gap becomes larger than in the case of an amorphous material, and the off-current can be reduced. Since the work function can also be increased, it becomes easier to control the current tunneling through the energy barrier formed by the p-type Group IV semiconductor material and the n-type semiconductor layer 507.

[0148] The method for manufacturing the quantum tunnel field effect transistor 501 is not particularly limited, but the following method can be exemplified. First, as shown in Fig. 8A, an insulating film 505A is formed on a p-type semiconductor layer 503, and a part of the insulating film 505A is opened by etching or the like to form a contact hole 505B. Next, as shown in Fig. 8B, an n-type semiconductor layer 507 is formed on the p-type semiconductor layer 503 and the insulating film 505A. At this time, the p-type semiconductor layer 503 and the n-type semiconductor layer 507 are connected via the contact hole 505B.

[0149] 8C, a gate insulating film 509 and a gate electrode 511 are formed in this order on the n-type semiconductor layer 507. Next, as shown in FIG. 8D, an interlayer insulating film 519 is provided so as to cover the insulating film 505A, the n-type semiconductor layer 507, the gate insulating film 509, and the gate electrode 511.

[0150] Next, as shown in Fig. 8E, a contact hole 519A is formed by opening a portion of the insulating film 505A and interlayer insulating film 519 on the p-type semiconductor layer 503, and a source electrode 513 is provided in the contact hole 519A. Furthermore, as shown in Fig. 8E, a contact hole 519B is formed by opening a portion of the gate insulating film 509 and interlayer insulating film 519 on the n-type semiconductor layer 507, and a drain electrode 515 is formed in the contact hole 519B. Through the above procedure, the quantum tunnel field effect transistor 501 can be manufactured.

[0151] After forming n-type semiconductor layer 507 on p-type semiconductor layer 503, heat treatment is performed at a temperature of 150° C. or higher and 600° C. or lower, thereby forming silicon oxide layer 505 between p-type semiconductor layer 503 and n-type semiconductor layer 507. By adding this step, quantum tunnel field effect transistor 501A can be manufactured.

[0152] The thin film transistor according to this embodiment is preferably a channel-doped thin film transistor, which is a transistor in which carriers in the channel are appropriately controlled by n-type doping rather than by oxygen deficiency, which is susceptible to fluctuations in response to external stimuli such as atmosphere and temperature, and which has the effect of achieving both high mobility and high reliability.

[0153] <Applications of Thin Film Transistor> The thin film transistor according to this embodiment can be suitably used in solar cells, display elements (liquid crystal elements, organic electroluminescence elements, inorganic electroluminescence elements, etc.), and power semiconductor elements. The thin film transistor according to this embodiment can be suitably used as a transistor in active matrix devices such as display devices (liquid crystal displays, organic electroluminescence (EL) displays, micro organic EL displays, micro light-emitting diode (LED) displays, mini LED displays, etc.), solid-state imaging elements, and touch panels. The thin film transistor according to this embodiment can also be applied to various integrated circuits such as field-effect transistors, logic circuits, memory circuits, and differential amplifier circuits, which can be applied to electronic devices, etc. The electronic device according to this embodiment preferably includes a thin film transistor. Furthermore, the thin film transistor according to this embodiment can be applied to static induction transistors and Schottky barrier transistors in addition to field-effect transistors. The thin film transistor according to this embodiment can also be applied as a transistor for sensors such as image sensors, X-ray sensors, and biosensors.

[0154] Hereinafter, the case where the thin film transistor according to this embodiment is used in a display device and a solid-state image sensor will be described.

[0155] First, a case where the thin film transistor according to this embodiment is used in a display device will be described with reference to Figures 9A to 9C. Figure 9A is a top view of the display device according to this embodiment. Figure 9B is a circuit diagram for explaining the circuit of the pixel portion when a liquid crystal element is applied to the pixel portion of the display device according to this embodiment. Also, Figure 9C is a circuit diagram for explaining the circuit of the pixel portion when an organic EL element is applied to the pixel portion of the display device according to this embodiment.

[0156] The thin film transistor according to this embodiment can be used as a transistor disposed in a pixel portion. Since the thin film transistor according to this embodiment can be easily made into an n-channel type, part of a driver circuit that can be configured with an n-channel transistor is formed over the same substrate as the transistor in the pixel portion. By using the thin film transistor described in this embodiment for the pixel portion or the driver circuit, a highly reliable display device can be provided.

[0157] 9A shows an example of a top view of an active matrix display device. A pixel portion 301, a first scanning line driver circuit 302, a second scanning line driver circuit 303, and a signal line driver circuit 304 are formed on a substrate 300 of the display device. A plurality of signal lines are arranged in the pixel portion 301, extending from the signal line driver circuit 304, and a plurality of scanning lines are arranged in the pixel portion 301, extending from the first scanning line driver circuit 302 and the second scanning line driver circuit 303. Pixels each having a display element are arranged in a matrix at the intersections of the scanning lines and the signal lines. The substrate 300 of the display device is connected to a timing control circuit (also referred to as a controller or a control IC) via a connection portion such as an FPC (Flexible Printed Circuit).

[0158] 9A , the first scanning line driver circuit 302, the second scanning line driver circuit 303, and the signal line driver circuit 304 are formed on the same substrate 300 as the pixel portion 301. This reduces the number of components, such as driver circuits, that are provided externally, thereby reducing costs. Furthermore, if the driver circuits are provided externally to the substrate 300, it becomes necessary to extend the wiring, which increases the number of connections between the wiring. If the driver circuits are provided on the same substrate 300, the number of connections between the wiring can be reduced, thereby improving reliability and yield.

[0159] 9B shows an example of a pixel circuit configuration, which is applicable to the pixel portion of a VA-type liquid crystal display device.

[0160] This pixel circuit can be applied to a configuration in which one pixel has multiple pixel electrodes. Each pixel electrode is connected to a different transistor, and each transistor is configured to be driven by a different gate signal. This allows the signals applied to each pixel electrode of a multi-domain pixel to be controlled independently.

[0161] The gate wiring 312 of the transistor 316 and the gate wiring 313 of the transistor 317 are separated so as to receive different gate signals. On the other hand, the source or drain electrode 314 functioning as a data line is used in common by the transistors 316 and 317. The thin film transistors according to this embodiment can be used for the transistors 316 and 317. This makes it possible to provide a highly reliable liquid crystal display device.

[0162] The transistor 316 is electrically connected to a first pixel electrode, and the transistor 317 is electrically connected to a second pixel electrode. The first pixel electrode and the second pixel electrode are separated from each other. The shapes of the first pixel electrode and the second pixel electrode are not particularly limited. For example, the first pixel electrode may be V-shaped.

[0163] The gate electrode of the transistor 316 is connected to the gate wiring 312, and the gate electrode of the transistor 317 is connected to the gate wiring 313. By applying different gate signals to the gate wiring 312 and the gate wiring 313, the operation timing of the transistors 316 and 317 can be made different, thereby controlling the alignment of the liquid crystal.

[0164] Furthermore, a storage capacitor may be formed by the capacitor wiring 310, a gate insulating film that functions as a dielectric, and a capacitor electrode that is electrically connected to the first pixel electrode or the second pixel electrode.

[0165] The multi-domain structure has one pixel having a first liquid crystal element 318 and a second liquid crystal element 319. The first liquid crystal element 318 is composed of a first pixel electrode, a counter electrode, and a liquid crystal layer therebetween, and the second liquid crystal element 319 is composed of a second pixel electrode, a counter electrode, and a liquid crystal layer therebetween.

[0166] The pixel portion is not limited to the configuration shown in Fig. 9B, and may include a switch, a resistor, a capacitor, a transistor, a sensor, or a logic circuit.

[0167] Another example of the circuit configuration of a pixel is shown in Fig. 9C, which shows the structure of a pixel portion of a display device using organic EL elements.

[0168] 9C is a diagram showing an example of an applicable circuit for the pixel portion 320. Here, an example is shown in which two n-channel transistors are used in one pixel. The oxide thin film according to this embodiment can be used in the channel formation region of the n-channel transistor. Digital time grayscale driving can be applied to the circuit for the pixel portion.

[0169] The thin film transistor according to this embodiment can be used for the switching transistor 321 and the driving transistor 322. This makes it possible to provide a highly reliable organic EL display device.

[0170] The configuration of the circuit in the pixel portion is not limited to the configuration shown in Fig. 9C. A switch, a resistor, a capacitor, a sensor, a transistor, or a logic circuit may be added to the circuit in the pixel portion shown in Fig. 9C. The above is a description of the case where the thin film transistor according to this embodiment is used in a display device.

[0171] Next, a case where the thin film transistor according to this embodiment is used in a solid-state imaging device will be described with reference to FIG.

[0172] A CMOS (Complementary Metal Oxide Semiconductor) image sensor is a solid-state imaging device that holds a potential in a signal charge storage section and outputs that potential to a vertical output line via an amplification transistor. If a leak current occurs in the reset transistor and / or transfer transistor included in the CMOS image sensor, the leak current causes charging or discharging, changing the potential of the signal charge storage section. When the potential of the signal charge storage section changes, the potential of the amplification transistor also changes, resulting in a value that deviates from the original potential, degrading the captured image.

[0173] The operational effect when the thin film transistor according to this embodiment is applied to the reset transistor and transfer transistor of a CMOS image sensor will be described. Either a thin film transistor or a bulk transistor may be applied to the amplifying transistor.

[0174] 10 is a diagram showing an example of the pixel configuration of a CMOS image sensor. A pixel is composed of a photodiode 3002, which is a photoelectric conversion element, a transfer transistor 3004, a reset transistor 3006, an amplifier transistor 3008, and various wirings, and a plurality of pixels are arranged in a matrix to form a sensor. A selection transistor electrically connected to the amplifier transistor 3008 may be provided. The transistor symbols "OS" and "Si" represent oxide semiconductor and silicon, respectively, and represent materials that are preferable for use in the respective transistors. This also applies to the subsequent drawings.

[0175] The photodiode 3002 is connected to the source side of the transfer transistor 3004, and a signal charge storage region 3010 (also called FD: floating diffusion) is formed on the drain side of the transfer transistor 3004. The source of the reset transistor 3006 and the gate of the amplification transistor 3008 are connected to the signal charge storage region 3010. As an alternative configuration, the reset power supply line 3110 can be eliminated. For example, the drain of the reset transistor 3006 can be connected to the power supply line 3100 or the vertical output line 3120 instead of the reset power supply line 3110. Note that the oxide thin film according to this embodiment may be used for the photodiode 3002, and the same material as the oxide thin films used for the transfer transistor 3004 and the reset transistor 3006 may be used.

[0176] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples.

[0177] [1] Preparation of a sputtering target A sputtering target having an oxide sintered body containing indium oxide as a main component was prepared by the following specific procedure.

[0178] (Examples 1 to 6) First, an indium oxide powder having an average particle size of 4 μm or less and a purity of 99.99% by mass was prepared as a raw material powder. The average particle size of the indium oxide powder was measured using a laser diffraction particle size analyzer (SALD-300V, manufactured by Shimadzu Corporation), and the median diameter D50 was used.

[0179] Next, the prepared indium oxide powder, polyvinyl alcohol, zirconia balls with a diameter of 2 mm, and water were placed in an alumina pot for crushing, and mixed and crushed for two hours using a planetary ball mill to prepare a raw material mixture. The average particle size of the prepared raw material mixture was 2 μm or less. The average particle size of the indium oxide powder in the raw material mixture was 2 μm or less (in Table 1, the average particle size of the indium oxide powder in the raw material mixture is referred to as the average particle size of the raw material powder). For polyvinyl alcohol, an amount was weighed so that the concentration of C (carbon) element as an impurity in the sintered body was 100 ppm or less by mass. The mixed and crushed mixture was then fed to a spray dryer and granulated at a rotation speed of 12,000 rpm and a hot air temperature of 150°C to obtain a raw material granulated powder. Next, the raw granulated powder was passed through a 90 mesh sieve to remove raw granulated powder with a particle size exceeding 150 μm, and the raw granulated powder was classified into particle sizes of 150 μm or less to obtain raw granulated powder with an adjusted particle size. The obtained raw granulated powder had a spherical shape. This raw granulated powder with an adjusted particle size was used as a sintered body raw material. Next, this sintered body raw material was placed in a mold and subjected to a pressure of 300 kg / cm. 2 This press-molded body was subjected to a pressure of 2600 kg / cm. 2 The mixture was densified by CIP at a pressure of 1000 kJ / cm 2 to obtain a compact.

[0180] The obtained molded body was heated in a sintering furnace in an air atmosphere up to the maximum sintering temperature shown in Table 1, and then maintained at this sintering temperature for 20 hours to obtain a sintered body.

[0181] The obtained sintered body was subjected to surface grinding. After polishing, the surface that had been subjected to surface grinding was used as the sputtering surface, and the surface opposite to the sputtering surface was used as the bonding surface. The bonding surface side of the sintered body was bonded to a backing plate. By bonding to the backing plate, a sputtering target was obtained.

[0182] (Examples 7 to 12) First, as raw material powder, indium oxide powder with an average particle size of 4 μm or less and a purity of 99.99% by mass was prepared. Furthermore, raw material powders of compounds of metal elements showing a positive tetravalent valence shown in Table 2 with an average particle size of 4 μm or less were prepared. The raw material powders of compounds of metal elements showing a positive tetravalent valence prepared are as follows. The average particle size of each raw material powder was measured using a laser diffraction particle size distribution device (SALD-300V, manufactured by Shimadzu Corporation), and the median diameter D50 was used. Tin oxide (SnO 2 ) powder. Titanium oxide (TiO) with a purity of 99.99% by mass 2 ) powder. Zirconium oxide (ZrO) with a purity of 99.99% by mass 2 ) powder. Cerium oxide (CeO) with a purity of 99.99% by mass 2 ) powder.

[0183] Next, the oxides of metal elements exhibiting a positive tetravalent valence were weighed out so that the content (atomic %) of the oxides in the sintered body was the value shown in Table 2. The prepared indium oxide powder, polyvinyl alcohol, zirconia balls with a diameter of 2 mm, and water were mixed and crushed in a planetary ball mill for two hours to prepare a raw material mixture such that the average particle size of each raw material powder in the raw material mixture was 2 μm or less. The average particle size of the raw material powders of the indium oxide powder and the compound of metal elements exhibiting a positive tetravalent valence in the raw material mixture was 2 μm or less (in Table 2, the average particle size of the raw material powders of the indium oxide powder and the compound of metal elements exhibiting a positive tetravalent valence in the raw material mixture is referred to as the average raw material powder particle size). As in Example 1, the polyvinyl alcohol was weighed out in an amount such that the concentration of C (carbon) element as an impurity in the sintered body was 100 ppm or less by mass. A sintered body was obtained in the same manner as in Example 1, except for the above. The obtained sintered body was then ground and bonded in the same manner as in Example 1 to obtain a sputtering target.

[0184] (Comparative Examples 1 to 6) Sputtering targets were obtained in the same manner as in Example 1, except that sintered bodies were obtained by changing the average particle size of the indium oxide powder in the raw material mixture and the sintering temperature to the conditions shown in Table 3. In Comparative Example 6, an indium oxide powder containing 0.8 mass % of carbon impurities was used.

[0185] [A] Evaluation of Sintered Body [A-1] Average Crystal Grain Size and Particle Size Distribution The average crystal grain size and particle size distribution of the sintered body, which was the material for the sputtering target obtained in each of the above Examples and Comparative Examples, were observed using an electron probe microanalyzer (EPMA) JXA-8621MX (manufactured by JEOL Ltd.). First, the square inscribed in the circle of the circular sputtering target was divided into 16 equal-area pieces, and sintered body samples were prepared at 16 center points of each square. The sintered body samples were prepared by cutting the sintered body into pieces less than 1 cm (1 cm x 1 cm in size), and these sintered body samples were embedded in a 1-inch diameter (1-inch diameter) epoxy-based room-temperature curing resin. The embedded sintered body samples were then polished using abrasive paper #400, #600, #800, 3 μm diamond suspension in water, and 50 nm colloidal silica (for final finishing), in that order. The polished surface was then observed at 500x magnification under an acceleration voltage of 10 kV, and the crystal grains of each of the 16 sintered body samples were measured as equivalent circle diameters based on JIS R 1670 to observe the average crystal grain size and particle size distribution. The average crystal grain size of the crystalline phase contained in the sintered body was taken as the average crystal grain size of the crystalline phase having a bixbyite structure composed of In and O elements. The particle size distribution is expressed as a number ratio.

[0186] [A-2] Area ratio of voids For the oxide sintered bodies that are the materials for the sputtering targets obtained in each of the above Examples and Comparative Examples, voids surrounded by three or more adjacent crystal grains were observed using the same method as for the average crystal grain size and particle size distribution described above, and the visual field magnification was set to 500x. The contrast and brightness were adjusted using image processing software (ImageJ) so that the voids could be distinguished, a binarization threshold was set, and grayscale binarization processing was performed. After the binarization processing, the area ratio of voids surrounded by three or more adjacent crystal grains was calculated.

[0187] [A-3] Density Measurement For the oxide sintered bodies used as the materials for the sputtering targets obtained in each of the above Examples and Comparative Examples, sintered body samples for measurement were taken, and the actual densities of the sintered bodies measured by the Archimedes method were measured. Specifically, measurements were performed using water at room temperature. Note that, for the density of indium oxide, since density and specific gravity are almost equivalent, the value of the specific gravity of the oxide listed in Chemistry Handbook, Basics I, edited by the Chemical Society of Japan, Revised 2nd Edition (Maruzen Co., Ltd.) was used.

[0188] [A-4] Measurement of flexural strength The flexural strength of the sintered body, which was the material for the sputtering target obtained in each of the above Examples and Comparative Examples, was measured by the following procedure. First, ten test pieces in the shape of a rectangular prism, measuring 3 mm thick x 4 mm wide x 36 mm long, were cut out from the obtained sintered body. Next, based on JIS R1601:2008, the three-point bending strength was measured using a materials testing machine (Shimadzu Corporation, EZ Graph), and the average value of the three-point bending strength measurements of the ten test pieces was taken as the flexural strength.

[0189] [A-5] Concentration of Impurity (C) Element The concentration of C (carbon) element as an impurity in the sintered body, which is the material of the sputtering target obtained in each of the above Examples and Comparative Examples, was measured by cutting the obtained sintered body into a 1 cm (size of 1 cm × 1 cm) piece using a carbon content analyzer (CSLS600, manufactured by LECO Corporation).

[0190] [A-6] Content of oxide of metal element exhibiting positive tetravalent atomic valence The content (atomic %) of oxide of metal element exhibiting positive tetravalent atomic valence in the sintered body, which is the material of the sputtering target obtained in each of the above examples and comparative examples, was measured by an inert gas dissolution method using an inductively coupled plasma optical emission spectrometer (ICP-AES, manufactured by Shimadzu Corporation).

[0191] [A-7] Number of Arcing Occurrences The number of arcing occurrences for the sputtering targets obtained in the above examples and comparative examples was 1.23 W / cm 2The number of arcing events was measured using a micro-arc counter attached to a pulsed DC power supply (Pinnacle Plus+, manufactured by ADVANCED ENERGY).

[0192] [A-8] Nodule Coverage The nodule coverage of the sputtering targets obtained in each of the above Examples and Comparative Examples was measured as follows: After discharging a circular sputtering target for 12 hours, the circular target was photographed from above the sputtering surface with a digital camera, and portions of the photograph other than the sintered body were deleted using image processing software (ImageJ).The contrast and brightness were then adjusted so that the nodules could be distinguished, a binarization threshold was set, and grayscale binarization processing was performed. The area ratio of the nodules was calculated to obtain the nodule coverage.

[0193] [2] Preparation of Oxide Thin Films (Examples 1 to 12, Comparative Examples 1 to 6) Using the sputtering targets obtained in each of the above Examples and Comparative Examples, oxide thin films (oxide semiconductor thin film layers) with a thickness of 30 nm were formed by sputtering on glass substrates (EAGLE XG (registered trademark), manufactured by CORNING). A mixed gas of high-purity argon, high-purity oxygen, and high-purity hydrogen (specifically, a mixed gas containing the three gases (i) to (iii) of high-purity argon, (ii) high-purity oxygen, and (iii) a gas in which high-purity argon is mixed with 5% by volume of high-purity hydrogen (impurity gas concentration: 0.01% by volume)) was used as the sputtering gas. The film formation conditions were as follows:

[0194] <Film formation conditions> Substrate temperature: 25°C Ultimate pressure: 3×10 -4 Pa or less Atmospheric gas: Ar + O 2 +H 2 (O 2 Flow rate ratio 2% - Hydrogen flow rate ratio 3%) Sputtering pressure (total pressure): 0.5 Pa Input voltage: DC 400 W Magnetic flux density: 600 G (Gauss) Distance between S (substrate) and T (target): 70 mm

[0195] [B] Evaluation of Oxide Thin Film [B-1] Carrier Concentration The carrier concentration of the oxide thin film (oxide semiconductor thin film layer) obtained in each Example and Comparative Example was measured by the Hall effect. The oxide thin film formed above was heated in air at 300°C for 1 hour, cut into a 10 mm square, and the Hall effect was evaluated at 25°C using a resistivity / Hall measurement system (ResiTest 8400, manufactured by Toyo Corporation).

[0196]

[0197]

[0198]

[0199] From the results shown in Tables 1 to 3, the sintered bodies according to Examples 1 to 12 have a density measured by the Archimedes method of 6.9 g / cm 3 or more, the average crystal grain size is 5 μm or more and 25 μm or less, and the area ratio of voids surrounded by three or more adjacent crystal grains is 3% or less. Therefore, it can be seen that the sintered bodies according to Examples 1 to 12 suppress nodule generation during sputtering while maintaining a flexural strength of 180 MPa or more, and sputtering targets with long lifespans are obtained. Furthermore, as shown in FIG. 11 , it was confirmed that the sintered body used in the sputtering target according to an embodiment of the present invention has a larger crystal grain size and fewer voids at grain boundary multiple points than the sintered body used in the sputtering target according to an embodiment of the present invention shown in FIG. 12 . Furthermore, it was confirmed that the sputtering target according to an embodiment of the present invention experienced fewer arcing events and had a smaller nodule coverage than the sputtering target according to an embodiment of the present invention. Furthermore, from the results shown in Tables 1 to 3, it can be seen that the oxide thin films according to Examples 1 to 12 have a carrier concentration of 1×10 19 / cm 3 Therefore, it is found that the oxide thin films according to Examples 1 to 12 can be used as oxide semiconductor thin films. In particular, the oxide thin films according to Examples 1 to 10 have a carrier concentration of 1×10 18 / cm 3This shows that the film is more easily applicable to oxide semiconductor thin films.

[0200] 1, 1A, 1B: oxide sintered body (sputtering target), 1C: oxide sintered body, 3: backing plate, 20: silicon wafer, 30: gate insulating film, 40: oxide thin film, 50: source electrode, 60: drain electrode, 70: interlayer insulating film, 70A: interlayer insulating film, 70B: interlayer insulating film, 100: thin film transistor, 100A: thin film transistor, 11: channel layer (crystalline oxide thin film), 11A-1: first low resistance region, 11B : semiconductor region, 11A-2: second low resistance region, 21: substrate, 22: buffer layer, 24: gate insulating film, 25: gate electrode, 26: interlayer insulating film, 27: source electrode, 28: drain electrode, 29: protective film, 100B: thin film transistor, 100C: thin film transistor, 300: substrate, 301: pixel section, 302: first scanning line driving circuit, 303: second scanning line driving circuit, 304: signal line driving circuit, 310: capacitance wiring, 312: gate Wiring, 313: gate wiring, 314: drain electrode, 316: transistor, 317: transistor, 318: first liquid crystal element, 319: second liquid crystal element, 320: pixel portion, 321: switching transistor, 322: driving transistor, 3002: photodiode, 3004: transfer transistor, 3006: reset transistor, 3008: amplification transistor, 3010: signal charge storage portion, 3100: power supply line, 31 10: reset power supply line, 3120: vertical output line, 501: quantum tunnel field effect transistor, 501A: quantum tunnel field effect transistor, 503: p-type semiconductor layer, 505: silicon oxide layer, 505A: insulating layer, 505B: contact hole, 507: n-type semiconductor layer, 509: gate insulating film, 511: gate electrode, 513: source electrode, 515: drain electrode, 519: interlayer insulating film, 519A, 519B: contact holes.

Claims

1. A sputtering target comprising an oxide sintered body mainly composed of indium oxide, wherein the oxide sintered body has a density of 6.9 g / cm3 as measured by Archimedes' method. 3 or more, wherein an average crystal grain size of indium oxide crystal grains contained in the oxide sintered body is 5 μm or more and 25 μm or less, and in a field of view when a surface of the oxide sintered body is observed at a magnification of 500 times, an area ratio of voids surrounded by three or more adjacent crystal grains to the area of ​​the field of view is 3% or less.

2. The sputtering target according to claim 1, wherein the indium oxide has an average crystal grain size of 5.4 μm or more and 23 μm or less.

3. A sputtering target according to claim 1 or 2, wherein the area ratio of the voids is 2.6% or less.

4. The sputtering target according to any one of claims 1 to 3, wherein the oxide sintered body contains C (carbon) element as an impurity in an amount of 100 ppm or less by mass.

5. A sputtering target according to any one of claims 1 to 4, wherein the oxide sintered body contains an oxide of a metal element exhibiting a positive tetravalent atomic valence, and the content of the oxide of the metal element exhibiting a positive tetravalent atomic valence in the oxide sintered body is 2 atomic % or less relative to the indium oxide in the oxide sintered body.

6. The sputtering target according to claim 5, wherein the metal element exhibiting a positive tetravalent atomic valence is one or more elements selected from the group consisting of Sn (tin), Ti (titanium), Ce (cerium), and Zr (zirconium).

7. The sputtering target according to any one of claims 1 to 6, wherein the indium oxide is contained in an amount of 50 atomic % or more based on the entire oxide sintered body.

8. The sputtering target according to any one of claims 1 to 7, wherein the indium oxide is contained in an amount of 98 atomic % or more based on the entire oxide sintered body.

9. A sputtering target according to any one of claims 1 to 8, wherein in the particle size distribution of indium oxide crystal grains contained in the oxide sintered body, the proportion of crystal grains of the indium oxide having a particle size of 5 μm or more and 40 μm or less is 90% or more in terms of number ratio.

10. A sputtering target according to any one of claims 1 to 9, wherein in the particle size distribution of indium oxide crystal grains contained in the oxide sintered body, the proportion of crystal grains of the indium oxide having a particle size of 5 μm or more and 40 μm or less is 94% or more in terms of number ratio.

11. The sputtering target according to any one of claims 1 to 10, wherein the area ratio of the voids is determined by observing the surface of the oxide sintered body with a scanning electron microscope or an electron beam microanalyzer.

12. A method for producing a sputtering target according to any one of claims 1 to 11, comprising the steps of: producing a molded body using a raw material powder mainly composed of an indium compound and adjusting the concentration of impurities so that the C (carbon) element contained in the oxide sintered body is 100 ppm or less by mass; and sintering the molded body so that the average crystal grain size of the indium oxide crystal grains contained in the oxide sintered body is 5 μm or more and 25 μm or less.

13. A method for manufacturing a sputtering target, comprising: a step of producing a molded body using a raw material powder containing as its main component an indium compound having an average grain size of 0.1 μm or more and 2 μm or less; and a step of sintering the molded body by controlling at least the sintering temperature and sintering time so that the average grain size of the indium oxide crystal grains contained in the oxide sintered body is 5 μm or more and 25 μm or less, and the area ratio of voids surrounded by three or more adjacent crystal grains on the sputtering surface of the oxide sintered body is 3% or less relative to the total area of ​​the sputtering surface.

14. The method for producing a sputtering target according to claim 13, wherein in the step of producing the molded body, a raw material powder mainly composed of an indium compound is crushed by a grinder and then molded.

15. An oxide thin film formed by using the sputtering target according to any one of claims 1 to 11.

16. A thin film transistor comprising the oxide thin film of claim 15.

17. An electronic device comprising the thin film transistor according to claim 16.

Citation Information

Patent Citations

  • ITO sputtering target and manufacturing method thereof

    JP2012126937A

  • ITO sputtering target, method for manufacturing the same, ITO transparent conductive film and method for manufacturing the same

    JP2020164930A

  • ITO sputtering target material and method for producing same

    WO2015125588A1

  • ITO sputtering target and method for manufacturing same, ITO transparent electroconductive film, and method for manufacturing ITO transparent electroconductive film