Aldehyde hydrogenation catalyst
The catalyst with nickel, molybdenum, and sulfur, specifically controlled in composition and cation distribution, addresses the issue of low alcohol selectivity in aldehyde hydrogenation, achieving high selectivity and efficiency by suppressing side reactions in the hydrogenation of aldehydes to alcohols.
Patent Information
- Application Number
- PCT/JP2024/011640
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional catalysts for hydrogenating aldehydes to synthesize alcohols suffer from low alcohol selectivity due to side reactions, which are promoted by acid in the catalyst and result in the formation of ethers and acetals.
A catalyst comprising nickel, molybdenum, and sulfur, with controlled molybdenum cation levels and low standard deviation, is developed to suppress side reactions and enhance alcohol selectivity, where nickel content is 5-40% by mass, molybdenum content is 0.05-5% by mass, and sulfur content is 0.01-1% by mass, with molybdenum cations limited to 2 or less and a standard deviation of 0.7 or less.
The catalyst achieves high alcohol selectivity by effectively suppressing side reactions, leading to improved performance and increased alcohol production efficiency.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Aldehyde hydrogenation catalyst
[0001] The present invention relates to a catalyst for the hydrogenation of aldehydes to synthesize alcohols.
[0002] Catalysts for hydrogenating aldehydes to synthesize alcohols have been known for a long time. For example, Patent Document 1 discloses a reduced nickel catalyst containing one or more metals selected from magnesium, calcium, barium, strontium, and zirconium in an amount of 3 to 15% relative to the nickel content of the nickel diatomaceous earth catalyst. This document also discloses a method for hydrogenating saturated or unsaturated aldehydes using this reduced nickel catalyst to produce the corresponding alcohol. Furthermore, this document describes a major problem in the hydrogenation reaction of aldehydes using a nickel catalyst, which involves side reactions that produce ethers and acetals. Furthermore, noting that these side reactions are promoted by the acid present in the catalyst, it describes how the inclusion of a basic metal salt in the catalyst significantly suppresses these side reactions. Furthermore, Patent Document 2 describes how the side reactions are suppressed and the alcohol selectivity is increased by highly dispersing silica with an alkali metal component fixed on its surface in the catalyst.
[0003] Methods that do not use basic metal components are also known. For example, Patent Document 3 describes that the selectivity to alcohols is improved by using a catalyst in which catalytically active components are supported with a gentle concentration gradient from the surface to the center.
[0004] Thus, in the reaction of hydrogenating aldehydes to synthesize alcohols, it has been known that the selectivity of alcohols can be increased by changing the acidity of the catalyst used or the state of supporting the active metal.
[0005] Japanese Patent Publication No. 44-17127 Japanese Patent Application Laid-Open No. 2020-163334 Japanese Patent Application Laid-Open No. 2005-279587
[0006] The present invention solves the problem that in the reaction of hydrogenating an aldehyde to synthesize an alcohol, side reactions occur when using conventional catalysts, resulting in low alcohol selectivity.
[0007] The present inventors have focused on catalysts containing nickel, molybdenum, and sulfur, and have found that by controlling the number of molybdenum cations to a certain level or less and reducing the variation in this number of cations, it is possible to obtain a catalyst that suppresses side reactions in the reaction of hydrogenating aldehyde to synthesize alcohol, thereby achieving high selectivity for alcohol.
[0008] More specifically, by hydrogenating an aldehyde using a catalyst containing nickel, molybdenum, and sulfur, the nickel content is 5% by mass or more and 40% by mass or less, calculated as NiO, the molybdenum content is 0.05% by mass or more and 5% by mass or less, calculated as MoO, the sulfur content is 0.01% by mass or more and 1% by mass or less, calculated as SO, and the number of molybdenum cations is 2 or less and the standard deviation of the number of cations is 0.7 or less, the selectivity of alcohol can be increased.
[0009] According to the present invention, a catalyst can be provided that has high selectivity for alcohol in a reaction for synthesizing alcohol by hydrogenating aldehyde.
[0010] The present invention includes an invention relating to a catalyst used in a reaction for synthesizing an alcohol by hydrogenating an aldehyde (hereinafter also referred to as "the catalyst of the present invention"). The catalyst of the present invention will be described in detail below.
[0011] [Catalyst of the Present Invention] The catalyst of the present invention contains nickel, molybdenum, and sulfur. Nickel acts as an active component in the reaction of hydrogenating aldehyde to synthesize alcohol. Molybdenum and sulfur are thought to have the effect of increasing the selectivity of alcohol.
[0012] The nickel contained in the catalyst of the present invention may be either metal, nickel oxide, or a mixture thereof. Metallic nickel is active in aldehyde hydrogenation reactions, but metallic nickel is easily oxidized in air to form nickel oxide. Therefore, the nickel contained in the nickel catalyst exists partially or entirely in the form of nickel oxide, and is reduced to metallic nickel with hydrogen or the like before the hydrogenation reaction before use. Furthermore, by forming an oxide film on the surface of metallic nickel or by adsorbing carbon dioxide or the like, the nickel can be handled stably even in air.
[0013] The nickel content of the catalyst of the present invention is 5% by mass or more and 40% by mass or less, calculated as NiO. The nickel content in the present invention is calculated using the following formula: Nickel content [% by mass] = (mass of Ni converted to NiO / total mass of catalyst) × 100. This nickel content is preferably 5% by mass or more and 30% by mass or less, and more preferably 5% by mass or more and 20% by mass or less. The catalyst of the present invention having a nickel content within the above range tends to have a high alcohol selectivity.
[0014] The molybdenum contained in the catalyst of the present invention may be any of metal, molybdenum oxide, or a mixture thereof. It is believed that molybdenum, when partially or entirely present in a state coexisting with sulfur, serves to increase the alcohol selectivity. Furthermore, the molybdenum present in a state coexisting with sulfur may exist alone or in the form of a compound.
[0015] The molybdenum content of the catalyst of the present invention is 0.05% by mass or more and 5% by mass or less, calculated as MoO3. The molybdenum content in the present invention is calculated using the following formula: Molybdenum content [mass %] = (mass of molybdenum converted to MoO3 / total mass of catalyst) × 100. This molybdenum content is preferably 0.05% by mass or more and 4% by mass or less, and more preferably 0.1% by mass or more and 3% by mass or less. The catalyst of the present invention having a molybdenum content within the above range tends to have high alcohol selectivity.
[0016] The sulfur contained in the catalyst of the present invention may be any of molybdenum sulfide, sulfur oxide, or a mixture thereof. Generally, sulfur is known to poison nickel-containing catalysts. However, in the catalyst of the present invention, sulfur is present in part or in whole in a state coexisting with molybdenum, which is thought to enhance the alcohol selectivity.
[0017] The sulfur content of the catalyst of the present invention is 0.01% by mass or more and 1% by mass or less, calculated as SO3. The sulfur content in the present invention is calculated using the following formula: Sulfur content [mass%] = (mass of sulfur converted to SO3 / total mass of catalyst) × 100 This sulfur content is preferably 0.01% by mass or more and 0.5% by mass or less, and more preferably 0.01% by mass or more and less than 0.1% by mass. The catalyst of the present invention having a sulfur content within the above range tends to have high alcohol selectivity.
[0018] The catalyst of the present invention has a molybdenum cation number of 2 or less. In the present invention, the molybdenum cation number is an index representing the valence of molybdenum. The molybdenum cation number varies depending on the state of molybdenum and the state of sulfur bonding to the molybdenum surface. The molybdenum cation number can be measured by energy dispersive X-ray analysis (EDS). The molybdenum cation number in the present invention is determined by observing the catalyst surface using a scanning electron microscope / energy dispersive X-ray analyzer (SEM-EDS), detecting multiple spots where molybdenum is detected, and calculating the average number of molybdenum cations at 15 points. In the catalyst of the present invention, molybdenum and sulfur coexist, resulting in a molybdenum cation number of 2 or less. In the catalyst of the present invention, the molybdenum cation number is preferably 1.75 or less, more preferably 1.5 or less. The lower limit of the molybdenum cation number is not particularly limited, but may be 0 or more, or 0.1 or more. In the catalyst of the present invention in which the number of cations is within the above range, molybdenum and sulfur coexist in large amounts, and therefore alcohol selectivity tends to be high.
[0019] The catalyst of the present invention has a standard deviation of the number of molybdenum cations of 0.7 or less. This standard deviation of the number of molybdenum cations is an index showing the variation in the number of molybdenum cations, with a smaller value indicating a smaller variation. The catalyst of the present invention has a small variation in the number of molybdenum cations, resulting in a high alcohol selectivity. Furthermore, the catalyst of the present invention preferably has a number of molybdenum cations of 0.6 or less, more preferably 0.5 or less.
[0020] The specific surface area of the catalyst of the present invention is 50 m 2 / g or more, 250m 2 / g or less, and 2 / g or more, 225m 2 / g or less is more preferable, and 100m 2 / g or more, 200m 2 In the catalyst of the present invention having a specific surface area within the above range, molybdenum and sulfur tend to coexist, and the selectivity for alcohols tends to be higher.
[0021] When the catalyst of the present invention contains metallic nickel, the nickel crystallite size is preferably 10 nm or less, more preferably 2 nm or more and 9 nm or less, and particularly preferably 3 nm or more and 8 nm or less. The catalyst of the present invention having a nickel crystallite size in the above-mentioned range is likely to have a higher alcohol selectivity and is less likely to experience a decrease in catalytic activity when used continuously.
[0022] The catalyst of the present invention preferably contains a carrier. The catalyst of the present invention, in which nickel, molybdenum, and sulfur are dispersed and supported on a carrier, tends to have a higher alcohol selectivity. The carrier contained in the catalyst of the present invention is preferably at least one or more selected from silica, alumina, silica-alumina, and diatomaceous earth.
[0023] The catalyst of the present invention is preferably a molded body. The catalyst of the present invention can be used in powder form in the method for producing alcohol by hydrogenating aldehyde, but a molded body is preferred because it is easier to separate and recover after the reaction. The shape of the molded body may be any conventionally known shape. For example, it may be spherical, cylindrical, or similar. The shape of the catalyst of the present invention is preferably a cylindrical shape or a similar shape. This cylindrical shape also includes cylindrical, trilobal, and four-leaf shapes. The shape of the nickel catalyst of the present invention is preferably a cylindrical shape, with a diameter in the range of 0.5 mm to 7 mm and a length in the range of 1 mm to 10 mm.
[0024] [Method for Producing the Catalyst of the Present Invention] The catalyst of the present invention can be produced, for example, by a production method comprising the following steps (1) to (4): (1) a mother liquor preparation step of preparing a mother liquor in which nickel and sulfur are dissolved in water; (2) a precipitation step of adding a precipitant to the mother liquor to form a precipitate containing nickel and sulfur; (3) a molybdenum loading step of mixing the precipitate with a molybdenum impregnation solution in which molybdenum is dissolved to prepare a catalyst precursor containing nickel, molybdenum, and sulfur; and (4) a catalysis step of calcining the catalyst precursor to obtain a catalyst. The method for producing the catalyst of the present invention will be described in detail using this production method as an example. However, the method for producing the catalyst of the present invention is not limited to this production method.
[0025] [Mother Liquor Preparation Step] This step involves preparing a mother liquor in which nickel and sulfur are dissolved in water. This can be prepared by a conventional method, such as dissolving nickel sulfate in water or dissolving nickel in sulfuric acid. The nickel content of this mother liquor, calculated as NiO, is preferably 1% by mass or more and 20% by mass or less, more preferably 3% by mass or more and 15% by mass or less, and particularly preferably 5% by mass or more and 10% by mass or less, based on the total mass of the mother liquor. The sulfur content of this mother liquor, calculated as SO3, is preferably 1% by mass or more and 20% by mass or less, more preferably 3% by mass or more and 15% by mass or less, and particularly preferably 5% by mass or more and 10% by mass or less, based on the total mass of the mother liquor.
[0026] The mother liquor obtained in this step preferably contains a carrier in addition to nickel and sulfur. The inclusion of a carrier in the mother liquor is preferred because nickel and sulfur are dispersed and supported on the surface of the carrier in the precipitation step described below. The carrier that can be used in this step is preferably at least one or more selected from silica, alumina, silica-alumina, and diatomaceous earth. The carrier content in this mother liquor, calculated as the mass of the carrier when added to the mother liquor relative to the total mass of the mother liquor, is preferably 1% by mass or more and 20% by mass or less, more preferably 1% by mass or more and 10% by mass or less, and particularly preferably 1% by mass or more and 5% by mass or less. Adjusting the carrier content within the above-mentioned range allows the mother liquor to be easily handled, which is preferred from the viewpoint of productivity.
[0027] The mother liquor obtained in this step is preferably acidic, with a pH of preferably not more than 6. By making the mother liquor acidic, nickel and sulfur can be stably present in a dissolved state in the mother liquor.
[0028] [Precipitation Step] This step is a step of forming a precipitate containing nickel and sulfur by adding a precipitant to the mother liquor obtained in the previous step. In this step, by adding the precipitant to the mother liquor, a precipitate containing nickel and sulfur is formed in the mother liquor. The mother liquor in which this precipitate has been formed is also called a precipitation slurry.
[0029] The precipitant added to the mother liquor in this step can be appropriately selected from among common precipitants depending on the pH of the mother liquor. When the mother liquor is acidic, a basic compound such as sodium carbonate, sodium hydroxide, potassium carbonate, sodium hydroxide, or ammonia, or an aqueous solution of such a compound, can be used as the precipitant. In this step, the precipitant is preferably added to the mother liquor until the pH of the precipitation slurry obtained by adding the precipitant to the mother liquor becomes 8.0 or more and 10.5 or less, more preferably 8.5 or more and 10.0 or less.
[0030] In this step, the temperature of the mother liquor is preferably adjusted to a range of 50° C. to 90° C., more preferably 60° C. to 85° C. If the temperature of the mother liquor is adjusted to the above range and the precipitating agent is added, a precipitate in which nickel and sulfur are more dispersed can be formed.
[0031] In this step, it is preferable to age the precipitation slurry. Specifically, based on the pH immediately after adding the entire amount of the precipitant to the mother liquor, it is preferable to age the mother liquor until the pH becomes −0.20 or less, more preferably until the pH becomes −0.20 or less and −0.50 or more, and particularly preferably until the pH becomes −0.20 or less and −0.40 or more. This aging can reduce unreacted nickel and sulfur. Furthermore, it is preferable to adjust the temperature of the precipitation slurry to a range of 50° C. or more and 90° C. or less, and more preferably to a range of 60° C. or more and 85° C. or less. When the temperature of the precipitation slurry is adjusted to the above-mentioned range and aged, the pore volume and specific surface area of the finally obtained catalyst tend to increase.
[0032] In this step, it is preferable to remove the solvent contained in the precipitation slurry to separate the precipitate. When separating the precipitate from the precipitation slurry, the separation conditions are adjusted so as not to remove too much sulfur. For example, the solvent can be removed by evaporation to dryness or spray drying to separate the precipitate, or when the precipitate is separated by filtration, the washing conditions are adjusted so as not to remove too much sulfur. Sulfur is known to be a poisonous substance for nickel-containing catalysts. Therefore, in general, in methods for producing nickel-containing catalysts, thorough washing is performed to remove sulfur. However, in this production method, sulfur remains in the precipitate. If sulfur is removed by separation or washing, it is preferable to support sulfur on the precipitate using an aqueous solution containing a sulfate such as sulfuric acid or ammonium sulfate.
[0033] [Molybdenum Supporting Step] This step is a step of preparing a catalyst precursor containing nickel, molybdenum, and sulfur by mixing the precipitate obtained in the above-mentioned precipitation step with a molybdenum impregnation solution in which molybdenum has been dissolved.
[0034] In this step, it is preferable to prepare a molybdenum impregnation solution by dissolving a molybdenum compound in water. For example, the molybdenum impregnation solution can be prepared by dissolving a soluble molybdenum compound such as ammonium molybdate or sodium molybdate in water, or by dissolving a sparingly soluble molybdenum compound such as molybdenum oxide with an acid. The molybdenum content of the molybdenum impregnation solution, calculated as MoO mass, based on the total amount of the molybdenum impregnation solution, is preferably 0.1 mass% or more and 15.0 mass% or less, more preferably 0.5 mass% or more and 10.0 mass% or less, and particularly preferably 1.0 mass% or more and 5.0 mass% or less.
[0035] In this step, it is preferable to mix a molding aid together with the molybdenum impregnation liquid. Conventionally known molding aids can be used in this step. For example, inorganic compound binders such as diatomaceous earth, powdered silica, alumina, etc., and sols in which these are dispersed can be used. Organic binders such as polyvinyl alcohol, cellulose, and acrylic can also be used. The type and amount of binder added can be appropriately adjusted to suit the conditions of various molding methods. The product can then be molded using a conventionally known molding method. For example, it is preferable to mold the product into an optimal shape for use as a catalyst using methods such as extrusion molding and compression molding.
[0036] [Catalyzation Step] This step involves calcining the catalyst precursor obtained in the previous step to obtain a catalyst. In this step, the nickel compound contained in the catalyst precursor is decomposed by calcination to produce nickel oxide. The calcination temperature required for the decomposition of the nickel compound varies depending on the type of nickel compound. However, nickel oxide is generally obtained by calcining at a temperature of 300°C or higher and 450°C or lower. However, if the calcination is performed at a temperature that is too high, nickel oxide will aggregate and grow. A catalyst with such aggregated nickel oxide will have reduced catalytic activity in the reaction of hydrogenating aldehyde to synthesize alcohol. In this step, the catalyst precursor is preferably calcined at a temperature in the range of 350°C or higher and 400°C or lower. Furthermore, the calcination time is preferably in the range of approximately 1 hour to 24 hours.
[0037] In this process, a reduction stabilization treatment may be further performed after the calcination. This reduction stabilization treatment refers to a method of reducing nickel oxide contained in the catalyst to metallic nickel and then covering the surface with an oxide film. Using such a method, even catalysts containing metallic nickel can be safely handled in air. It also facilitates pretreatment prior to the reaction of hydrogenating aldehyde to synthesize alcohol. One method for reducing nickel oxide to metallic nickel is, for example, to heat the catalyst in a reducing gas flow until the nickel oxide is reduced. However, excessive heating can cause the metallic nickel to aggregate and grow, increasing the crystallite size of the metallic nickel. Therefore, such a reduction treatment is preferably performed at a temperature range of 350°C or higher and 500°C or lower, and more preferably at a temperature range of 380°C or higher and 450°C or lower. The time required for the reduction treatment varies depending on the amount of catalyst charged. The completion of the reduction treatment can be determined by analyzing the water content of the gas after the reaction. As the reduction treatment approaches completion, the amount of water produced by reduction decreases.
[0038] Because the catalyst contains metallic nickel after reduction treatment, it will oxidize rapidly if exposed to air. In some cases, the heat of oxidation may cause it to catch fire. Therefore, it is preferable to slowly oxidize the surface of the catalyst after reduction treatment in an inert gas with a very small amount of oxygen. This type of treatment is also called stabilization treatment. This treatment allows the catalyst containing metallic nickel to be handled safely even in air.
[0039] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. [Measurement and Evaluation Methods] Various measurements and evaluations were carried out as follows.
[0040] [pH Measurement] The pH was measured at a liquid temperature of 40°C using a pH meter (manufactured by Yamagata Toa DKK Co., Ltd., "MM43-X") and a pH electrode (manufactured by Yamagata Toa DKK Co., Ltd., "GST-5841C").
[0041] [Composition Analysis] (Ni, Mo, and S) A sample was dissolved in acid and diluted with water to an appropriate concentration, and then the Ni and Mo contents were measured using an ICP optical emission spectrometer (Agilent Technologies, 730ICP-OES, inductively coupled plasma optical emission spectroscopy). S was measured by a combustion method. The respective contents were calculated based on the total amount of catalyst, with Ni converted to NiO, Mo converted to MoO3, and S converted to SO3.
[0042] [Crystallite size measurement] X-ray diffraction measurements were performed on the samples using an X-ray diffractometer (Rigaku MultiFlex) manufactured by Rigaku Corporation. First, the sample to be measured was pulverized and packed into a sample plate. X-ray diffraction (Cu-Kα radiation source) measurements were performed under the following conditions: tube voltage 40 kV, tube current 20 mA, scanning range 10-70°, divergence slit 1.0 mm, scattering slit 1.0 mm, receiving slit 0.3 mm, scan speed 4° / min. The Ni crystallite size was determined by detecting a diffraction peak with a peak top near 2θ = 44° in the X-ray diffraction measurement, and calculated using the Scherrer formula using analysis software (JADE Version 5.0).
[0043] [Specific Surface Area Measurement] The specific surface area was calculated by the nitrogen adsorption method (BET method). Specifically, using a specific surface area measurement device (Macsorb 1220, manufactured by Mountech), approximately 0.1 g of sample was placed in a measurement cell and degassed in a nitrogen gas flow at 250°C for 40 minutes. After that, the sample was kept at liquid nitrogen temperature in a mixed gas flow of 30% by volume of nitrogen and 70% by volume of helium, allowing nitrogen to adsorb to the sample at equilibrium. The temperature of the sample was then gradually raised to room temperature while the mixed gas was flowing. The amount of nitrogen desorbed during this period was measured, and the specific surface area of the sample was calculated by dividing the amount by the sample weight after measurement.
[0044] <Measurement of Molybdenum Cation Number> SEM measurements were performed using a JEOL JSM6010LA microscope, with W as the X-ray source. The catalysts obtained in the examples were crushed into powder and attached to carbon tape without overlapping. The catalyst surface was measured. The acceleration voltage was adjusted to 20 kV-15 kV, and the SS was set to 4 nm. Subsequently, EDS analysis was performed at 2,500-10,000x magnification, and the analysis position was probe-tracked to allow tracing of the measurement position. Then, composition conversion was performed using the ZAF method. The Mo particle size was calculated from the resulting peak. After adjusting the beam diameter to this particle size, the microscope was magnified at 500-10,000x magnification, and the analysis position was probe-tracked to allow tracing of the measurement position. Point analysis of S and Mo was performed at 30 points. <Calculation Method> Fifteen points where Mo was detected were randomly extracted from the obtained data, and the number of Mo cations was calculated for each. These values were used to calculate the average and standard deviation. Here, the number of cations is calculated assuming that the number of oxygen atoms in a fully oxidized state (MoO3 in the case of Mo) is 24, and is 0 in the case of a fully oxidized state.
[0045] [Activity Evaluation: Aldehyde Hydrogenation Reaction] <Pretreatment> 12.0 g of sample was placed in a glass tube, which was then maintained at 150°C for 60 minutes under a hydrogen flow. The atmosphere inside the glass tube was then replaced with nitrogen and cooled to room temperature. The sample was then placed in an autoclave in a nitrogen atmosphere. <Hydrogenation Test> 50 g of n-butyl aldehyde and 50 g of n-butyl alcohol were injected into the autoclave. After injection, the temperature was raised to 100°C while stirring at 400 rpm. After heating, hydrogen was injected until the pressure inside the autoclave reached 5 MPa, and the autoclave was maintained at a pressure of 5 MPa. The amount of hydrogen absorption was checked every 5 minutes during the maintenance period, and the reaction was terminated when no hydrogen absorption was confirmed for 5 minutes. After the maintenance period, the autoclave was cooled to room temperature to obtain a reaction liquid. <Analysis> The resulting reaction solution was analyzed using a gas chromatograph (Shimadzu Corporation, GC-14B) to measure the contents of n-butylaldehyde (NBD) and n-butanol (NBA). Then, the NBA selectivity was calculated using the following formula. [NBA selectivity] NBA selectivity (%) = (number of moles of NBA after reaction - number of moles of NBA before reaction) / (number of moles of NBD after reaction - number of moles of NBD before reaction) x 100
[0046] Example 1 Mother Liquor Preparation Step 900 g of nickel sulfate hydrate (NiSO4·6H2O, Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 3,200 g of tap water. Next, 110 g of diatomaceous earth was dispersed therein to prepare a mother liquor. The temperature of this mother liquor was adjusted to 72.5°C. The nickel content of this mother liquor was 6.1% by mass, the sulfur content was 6.5% by mass, and the diatomaceous earth content was 2.6% by mass. The pH of the mother liquor was 5.3.
[0047] <Precipitation Step> A precipitant was prepared by dissolving 717 g of sodium carbonate (Na2CO3, Kanto Chemical Co., Inc.) in 2,780 g of tap water. The temperature of this precipitant was adjusted to 72.5°C. This precipitant was added to the mother liquor obtained in the previous step at a constant rate over 80 minutes to obtain a precipitated slurry. At this time, the pH of the precipitated slurry was 9.5. The temperature of this precipitated slurry was then maintained at 72.5°C and stirred for 120 minutes for aging. At this time, the pH of the precipitated slurry was 9.2. The aged precipitated slurry was filtered under reduced pressure using a Nutsche filter to obtain a cake-like precipitate. The entire amount of the obtained cake-like precipitate was poured into 7 L of warm water adjusted to 40°C to form a slurry, followed by suspension washing and filtration. The same step was repeated, and the sulfur content of the precipitate was adjusted to 0.10 mass% in terms of SO3, based on the mass of the precipitate after drying at 120°C. The precipitate was then dried in a tray dryer for 12 hours at 120° C. After drying, the precipitate was crushed using a hammer crusher mill.
[0048] <Molybdenum Supporting Step> 22.5 g of ammonium molybdate tetrahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 800 ml of ion-exchanged water to obtain a molybdenum impregnation solution. 341 g of the precipitate obtained in the previous step, the entire amount of the molybdenum impregnation solution, 1,500 g of silica sol (primary particle size 5 nm, pH 10, SiO2 content 20.5%, stabilized with sodium hydroxide) as a molding aid, and 1,020 g of powdered silica were mixed and kneaded using a double-arm kneader. 10 g of carboxymethyl cellulose was then added as a molding aid and further kneaded. The resulting clay was molded into a 5.0 mm diameter cylinder using a twin-screw auger extruder. This was dried at 120 ° C to obtain a catalyst precursor.
[0049] <Catalyst Formation Step> 500 g of the catalyst precursor obtained in the previous step was calcined in a muffle furnace at 380°C for 4.5 hours to obtain a catalyst. 250 g of this catalyst was reduced in a hydrogen atmosphere at 430°C for 10 hours and then subjected to stabilization treatment at 80°C to obtain a catalyst. This catalyst was used as a sample to carry out the above-mentioned measurements and evaluations. The results are shown in Table 1.
[0050] [Example 2] A catalyst was obtained in the same manner as in Example 1, except that the amount of ammonium molybdate tetrahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) used in the molybdenum loading step was 11.2 g. The obtained catalyst was subjected to the above-described measurements and evaluations. The results are shown in Table 1.
[0051] [Example 3] A catalyst was obtained in the same manner as in Example 1, except that the amount of ammonium molybdate tetrahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was changed to 45.1 g in the molybdenum supporting step. The obtained catalyst was subjected to the above-described measurements and evaluations. The results are shown in Table 1.
[0052] Example 4 A catalyst was obtained in the same manner as in Example 1, except that in the molybdenum loading step, the amount of silica sol added was 1,190 g, the amount of precipitate added was 682 g, the amount of powdered silica added was 801 g, and the amount of ammonium molybdate tetrahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was 45.1 g. The obtained catalyst was subjected to the above-described measurements and evaluations. The results are shown in Table 1.
[0053] Comparative Example 1: No Molybdenum A catalyst was obtained in the same manner as in Example 1, except that the molybdenum impregnation solution was not added in the molybdenum supporting step. The obtained catalyst was subjected to the above-described measurements and evaluations. The results are shown in Table 1.
[0054] Comparative Example 2: High Nickel Content, High Molybdenum Content A catalyst was obtained in the same manner as in Example 1, except that in the molybdenum loading step, the amount of silica sol added was 540 g, the amount of precipitate added was 1,370 g, the amount of powdered silica added was 364 g, and the amount of ammonium molybdate tetrahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was 180.7 g. The obtained catalyst was subjected to the above-described measurements and evaluations. The results are shown in Table 1.
[0055] Comparative Example 3: No Use of Molybdenum Impregnation Solution A catalyst was obtained in the same manner as in Example 1, except that in the molybdenum supporting step, no molybdenum impregnation solution was added and 18.4 g of powdered molybdenum trioxide was added. The obtained catalyst was subjected to the above-described measurements and evaluations. The results are shown in Table 1.
[0056] Comparative Example 4: High Molybdenum Content A catalyst was obtained in the same manner as in Example 1, except that the amount of ammonium molybdate tetrahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was changed to 135.2 g in the molybdenum loading step. The obtained catalyst was subjected to the above-described measurements and evaluations. The results are shown in Table 1.
[0057] Comparative Example 5: No Sulfur A catalyst was obtained in the same manner as in Example 1, except that 1,000 g of nickel nitrate hydrate (Ni(NO)·6H O, Fujifilm Wako Pure Chemical Industries, Ltd.) was added instead of nickel sulfate hydrate (NiSO·6H O, Fujifilm Wako Pure Chemical Industries, Ltd.) in the mother liquor preparation step. The obtained catalyst was subjected to the above-described measurements and evaluations. The results are shown in Table 1.
[0058] Comparative Example 6: Medium Nickel Content, No Molybdenum A catalyst was obtained in the same manner as in Example 4, except that the amount of ammonium molybdate added in the molybdenum loading step was 0 g. The obtained catalyst was subjected to the above-described measurements and evaluations. The results are shown in Table 1.
[0059]
[0060] When comparing the catalyst of Comparative Example 1, which does not contain molybdenum, with the catalyst of Example 1, it was confirmed that the inclusion of molybdenum increases NBA selectivity. Furthermore, it was confirmed that the catalyst of Example 1 has a shorter reaction time and higher activity than the catalyst of Comparative Example 1. Furthermore, when comparing the catalyst of Example 4, which has a higher nickel content than the catalyst of Example 1, with the catalyst of Comparative Example 6, which has a similar nickel content, it was confirmed that the same trend was observed. When comparing the catalyst of Comparative Example 5, which does not contain sulfur, with the catalyst of Example 1, it was confirmed that the inclusion of sulfur increases NBA selectivity. Furthermore, it was confirmed that the catalyst of Example 1 has a shorter reaction time and higher activity than the catalyst of Comparative Example 5. When comparing the catalyst of Comparative Example 3, which has a standard deviation of molybdenum cations of 0.7 or more, with the catalyst of Example 1, it was confirmed that reducing this standard deviation increases NBA selectivity. Furthermore, it was confirmed that the catalyst of Example 1 has a shorter reaction time and higher activity than the catalyst of Comparative Example 3. When the catalyst of Comparative Example 4, which has a molybdenum content of more than 5 mass%, is compared with the catalyst of Example 1, it was confirmed that the number and standard deviation of molybdenum cations are reduced by lowering the molybdenum content, and the NBA selectivity is increased.
[0061] This application claims priority based on Japanese Patent Application No. 2023-52589, filed March 29, 2023, the disclosure of which is incorporated herein in its entirety by reference.
Claims
1. A catalyst for hydrogenating an aldehyde to synthesize an alcohol, comprising nickel, molybdenum, and sulfur, the nickel content being 5% by mass or more and 40% by mass or less, calculated as NiO, the molybdenum content being 0.05% by mass or more and 5% by mass or less, calculated as MoO3, the sulfur content being 0.01% by mass or more and 1% by mass or less, calculated as SO3, the number of molybdenum cations being 2 or less, and the standard deviation of the number of cations being 0.7 or less.
Citation Information
Patent Citations
Method for preparing alcohols by selectively hydrogenating aldehydes
CN102408304A
Catalyst suitable for preparing 2-ethylhexanal through hydrogenation of isooctenal as well as preparation method and application of catalyst
CN116237054A
JP1974082609A
Nickel catalyst and production method of the same
JP2020163334A
Hydrogenation of oxo aldehydes to oxo alcohols in the presence of a nickel-molybdenum catalyst
US20050065384A1