Exhaust gas purification catalyst

The specific composition of the Ce-Zr-Al composite oxide in the catalyst layer addresses the challenge of maintaining oxygen storage and Rh's purification performance at high temperatures, ensuring effective exhaust gas purification by balancing Ce and Al content.

WO2024204075A1PCT designated stage expired Publication Date: 2024-10-03MITSUI MINING & SMELTING CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011722
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Exhaust gas purification catalysts face challenges in maintaining the oxygen storage capacity and purification performance of Rh-based catalysts, especially when exposed to high temperatures, due to excessive Ce in Ce-Zr-Al composite oxides, which leads to oxidation of Rh and decreased performance.

Method used

The catalyst layer contains a Ce-Zr-Al composite oxide with a specific composition where Ce is 70% or more by mass, and the Ce to Zr mass ratio is between 0.03 and 0.50, along with an Al to Ce+Zr mass ratio of 0.10 to 10, to enhance oxygen storage capacity and prevent deterioration of Rh's purification performance at high temperatures.

Benefits of technology

This composition effectively improves the oxygen storage capacity of the Ce-Zr-Al composite oxide and maintains the exhaust gas purification performance of Rh, even after exposure to high temperatures, by optimizing the Ce and Al content in the catalyst layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011722_03102024_PF_FP_ABST
    Figure JP2024011722_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide an exhaust gas purification catalyst that comprises a catalyst layer containing Rh and a Ce-Zr-Al-based composite oxide and can improve the oxygen storage capacity of the Ce-Zr-Al-based composite oxide and prevent deterioration of the exhaust gas purification performance of the Rh. Provided is an exhaust gas purification catalyst (1) comprising a base material (10) and a first catalyst layer (20) provided on the base material (10), wherein: the first catalyst layer (20) contains Rh and a composite oxide containing Ce, Zr and Al; the amount of the composite oxide is 70 mass% or greater based on the total mass of all components of the first catalyst layer (20) other than Rh; and the ratio of the amount of Ce in the composite oxide in terms of metal to the amount of Zr in the composite oxide in terms of metal is from 0.03 to 0.50 as a mass ratio.
Need to check novelty before this filing date? Find Prior Art

Description

Exhaust gas purification catalyst

[0001] The present invention relates to a catalyst for purifying exhaust gases.

[0002] Exhaust gases emitted from internal combustion engines of automobiles, motorcycles, and the like contain harmful components such as hydrocarbons (HC), carbon monoxide (CO), and nitrogen oxides (NOx). Catalysts containing precious metal elements such as Pt, Pd, and Rh are used to purify and neutralize these harmful components. Pt and Pd are primarily involved in the oxidation purification of HC and CO, while Rh is primarily involved in the reduction purification of NOx.

[0003] Exhaust gas purification catalysts use a carrier that supports catalytically active components (e.g., precious metal elements such as Pt, Pd, and Rh). Examples of the carrier include composite oxides containing Ce, Zr, and Al (hereinafter sometimes referred to as "Ce-Zr-Al composite oxides") (see, for example, Patent Documents 1 and 2).

[0004] Patent Document 1 describes the use of a Ce-Zr-Al composite oxide in which the molar ratio of the amount of Ce to the amount of Zr (Ce / Zr) is 1 / 3 to 3 / 1 and the molar ratio of the amount of Al to the total amount of Ce and Zr (Al / (Ce+Zr)) is 2 to 10 as a support for supporting a precious metal element.

[0005] In Patent Document 2, Al 2 O 3 -CeO 2 -ZrO 2 Ternary composite oxide / (Al 2 O 3 -CeO 2 -ZrO 2 Ternary complex oxide + Al 2 O 3 -ZrO 2 The mass ratio of Al (binary composite oxide) is in the range of 0.33 to 0.5. 2 O 3 -CeO 2 -ZrO 2 Ternary composite oxide and Al 2 O 3 -ZrO 2It is described that a binary composite oxide is used as a support for supporting Rh.

[0006] Japanese Patent Application Laid-Open No. 10-202102 Japanese Patent Application Laid-Open No. 2017-189745

[0007] It is desirable to control the air / fuel ratio (air-fuel ratio) supplied to an internal combustion engine to be close to the theoretical air-fuel ratio (stoichiometry). However, the actual air-fuel ratio fluctuates from stoichiometry to the rich (excess fuel atmosphere) or lean (lean fuel atmosphere) side, depending on the vehicle's running conditions, etc., and the air-fuel ratio of exhaust gas also fluctuates to the rich or lean side. Ce-Zr-Al-based composite oxides have oxygen storage capacity (OSC). Therefore, by using Ce-Zr-Al-based composite oxides, it is possible to alleviate fluctuations in the oxygen concentration in exhaust gas and expand the operating window of catalytically active components.

[0008] Ce contributes to oxygen storage capacity. Therefore, in a catalytic layer containing Rh and Ce—Zr—Al-based composite oxide, as the amount of Ce in the Ce—Zr—Al-based composite oxide increases, the oxygen storage capacity of the Ce—Zr—Al-based composite oxide improves, and the exhaust gas purification performance of Rh improves. However, Ce promotes the oxidation of Rh. Here, Pt and Pd have the property of easily exhibiting exhaust gas purification performance when moderately oxidized, while Rh has the property of easily decreasing exhaust gas purification performance when oxidized. Therefore, if the amount of Ce in the Ce—Zr—Al-based composite oxide is excessive, the oxidation of Rh is promoted, and the exhaust gas purification performance of Rh decreases. Therefore, when a Ce—Zr—Al-based composite oxide is used as a support, it is particularly difficult to achieve both oxygen storage capacity and exhaust gas purification performance when Rh is used as the catalytic active component, compared to when Pt and / or Pd are used as the catalytic active component. Furthermore, if the Ce content in the Ce-Zr-Al composite oxide is excessive, the heat resistance of the Ce-Zr-Al composite oxide will be insufficient, and therefore, in a high-temperature environment, aggregation of the Ce-Zr-Al composite oxide will occur, the pores of the Ce-Zr-Al composite oxide will disappear (i.e., the specific surface area will decrease), and the like will occur, which will lead to the burial of Rh, sintering of Rh, and the exhaust gas purification performance of Rh after exposure to a high-temperature environment will decrease. In this specification, "high temperature" means a temperature of preferably 800°C or higher, more preferably 850°C or higher, and even more preferably 900°C or higher.

[0009] On the other hand, if the proportion of components other than the Ce-Zr-Al composite oxide among all components other than Rh in the catalytic layer increases, the difference in the degree of thermal expansion and thermal contraction between the Ce-Zr-Al composite oxide and the components other than the Ce-Zr-Al composite oxide in a high-temperature environment will cause Rh to be buried or sintered, resulting in a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment.

[0010] Therefore, in an exhaust gas purification catalyst having a catalytic layer containing Rh and a Ce-Zr-Al-based composite oxide, it is desired to improve the oxygen storage capacity of the Ce-Zr-Al-based composite oxide and to prevent a decrease in the exhaust gas purification performance of Rh (in particular, to prevent a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment).

[0011] Therefore, an object of the present invention is to provide an exhaust gas purification catalyst that includes a catalytic layer containing Rh and a Ce-Zr-Al-based composite oxide, and that can improve the oxygen storage capacity of the Ce-Zr-Al-based composite oxide and prevent a decrease in the exhaust gas purification performance of Rh (in particular, prevent a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment).

[0012] The present inventors have discovered that in an exhaust gas purification catalyst having a catalytic layer containing Rh and a Ce—Zr—Al-based composite oxide, by setting the amount of Ce—Zr—Al-based composite oxide to 70 mass % or more, based on the total mass of all components other than Rh in the catalytic layer, and by setting the ratio of the amount of Ce in the Ce—Zr—Al-based composite oxide, converted into metal, to the amount of Zr in the Ce—Zr—Al-based composite oxide, converted into metal, to a mass ratio of 0.03 to 0.50, the oxygen storage capacity of the Ce—Zr—Al-based composite oxide can be improved and a decrease in the exhaust gas purification performance of Rh can be prevented (in particular, a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment can be prevented), and this has led to the completion of the present invention.

[0013] The present invention encompasses the following: [1] A catalyst for purifying exhaust gases, comprising a substrate and a first catalytic layer provided on the substrate, wherein the first catalytic layer contains a composite oxide containing Rh and Ce, Zr, and Al, the amount of the composite oxide being 70 mass% or more based on the total mass of all components of the first catalytic layer other than Rh, and the ratio of the amount of Ce in the composite oxide, calculated on a metal basis, to the amount of Zr in the composite oxide, calculated on a metal basis, is 0.03 to 0.50, in mass ratio. [2] The catalyst for purifying exhaust gases according to [1], wherein the ratio of the amount of Al in the composite oxide, calculated on a metal basis, to the total amount of Ce and Zr in the composite oxide, calculated on a metal basis, is 0.10 to 10, in mass ratio. [3] The catalyst for purifying exhaust gases according to [1] or [2], wherein the total amount of Ce, Zr, and Al in the composite oxide, calculated on an oxide basis, is 75 mass% or more based on the mass of the composite oxide. [4] The catalyst for purifying exhaust gas according to any one of [1] to [3], wherein the amount of rare earth elements other than Ce in the composite oxide, calculated as oxides, is 25 mass % or less based on the mass of the composite oxide. [5] The catalyst for purifying exhaust gas according to [4], wherein the rare earth elements other than Ce are selected from La, Y, Pr, and Nd. [6] The catalyst for purifying exhaust gas according to any one of [1] to [5], wherein the first catalyst layer contains an Al-based oxide. [7] The catalyst for purifying exhaust gas according to any one of [1] to [6], wherein the first catalyst layer contains a binder. [8] The catalyst for purifying exhaust gas according to [7], wherein the binder is an inorganic oxide other than a Ce-Zr-Al-based composite oxide. [9] The exhaust gas purifying catalyst according to any one of [1] to [8], wherein the exhaust gas purifying catalyst comprises a second catalyst layer provided on the substrate, the first catalyst layer is provided on the upper side of the second catalyst layer, and the second catalyst layer contains one of Pd or Pt, or both Pd and Pt.

[0014] According to the present invention, there is provided an exhaust gas purification catalyst having a catalytic layer containing Rh and a Ce-Zr-Al-based composite oxide, which can improve the oxygen storage capacity of the Ce-Zr-Al-based composite oxide and prevent a decrease in the exhaust gas purification performance of Rh (in particular, prevent a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment).

[0015] Fig. 1 is a partial end view showing a state in which an exhaust gas purification catalyst according to one embodiment of the present invention is arranged in an exhaust path of an internal combustion engine. Fig. 2 is an end view taken along line A-A in Fig. 1. Fig. 3 is an enlarged view of the area indicated by the symbol R in Fig. 2. Fig. 4 is an end view taken along line B-B in Fig. 1.

[0016] <Explanation of Terms> The terms used in this specification will be explained below.

[0017] <Rare Earth Elements> Examples of rare earth elements include Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu.

[0018] <Oxide> The oxide of Al is Al 2 O 3 , Zr oxide is ZrO 2 , and the oxide of Si is SiO 2 , the oxide of B is B 2 O 3 , Cr oxide is Cr 2 O 3 , Mg oxide is MgO, Ca oxide is CaO, Sr oxide is SrO, Ba oxide is BaO, Fe oxide is Fe 3 O 4 , Mn oxide is Mn 3 O 4 , Ni oxide is NiO, Ti oxide is TiO 2 The oxides of rare earth elements are sesquioxides (Ln) except for oxides of Ce, Pr and Tb. 2 O 3 , Ln represents a rare earth element other than Ce, Pr, and Tb), and the oxide of Ce is CeO 2 , Pr oxide is Pr 6 O 11 , the oxide of Tb is Tb 4 O 7 means.

[0019] <Al-based oxide> The Al-based oxide refers to an oxide containing Al. The Al-based oxide preferably refers to an oxide containing Al, in which, among elements other than O constituting the oxide, Al is the element with the largest content by mass. Among the Al-containing oxides, those that fall under the Ce—Zr—Al-based composite oxide of the present invention are not considered to fall under the Al-based oxide. The Ce—Zr—Al-based composite oxide of the present invention will be described later.

[0020] The Al-based oxide is, for example, in the form of particles. The Al-based oxide is used as a support for a catalytically active component. From the viewpoint of improving the supportability of the catalytically active component, the Al-based oxide is preferably porous. The Al-based oxide is distinguished from alumina used as a binder. In this specification, alumina used as a binder may be referred to as an "alumina binder," and alumina used as a support may be referred to as an "alumina material."

[0021] The Al-based oxide may contain one or more elements (hereinafter, sometimes referred to as "other elements") other than Al and O. The other elements can be selected from, for example, rare earth elements (e.g., Ce, Y, Pr, La, Nd, Sm, Eu, Gd, etc.), alkaline earth metal elements (e.g., Mg, Ca, Sr, Ba, etc.), B, Si, Zr, Cr, etc.

[0022] Examples of Al-based oxides include alumina (oxide composed of Al and O), oxides obtained by modifying the surface of alumina with other elements, oxides obtained by dissolving other elements in alumina, etc. Examples of Al-based oxides containing other elements include alumina-silica, alumina-silicate, alumina-zirconia, alumina-chromia, alumina-ceria, and alumina-lanthana.

[0023] In the Al-based oxide, other elements are in the form of a solid solution phase (e.g., Al 2 O 3 The crystalline or amorphous phase may be formed as a single phase (e.g., a solid solution phase of the crystalline or amorphous oxide of the other element), or may be formed as both a solid solution phase and a single phase (e.g., a phase of an oxide of the other element).

[0024] From the viewpoint of improving the heat resistance of the Al-based oxide, the amount of Al in the Al-based oxide, calculated as Al oxide, is preferably 20% by mass or more, more preferably 25% by mass or more, even more preferably 30% by mass or more, still more preferably 35% by mass or more, and still more preferably 40% by mass or more, based on the mass of the Al-based oxide, with the upper limit being 100% by mass.

[0025] In one embodiment, the Al-based oxide contains Zr. This can improve the heat resistance of the Al-based oxide. In this specification, an Al-based oxide containing Zr may be referred to as an "Al-Zr-based oxide." From the viewpoint of improving the heat resistance of the Al-based oxide, the amount of Zr in the Al-based oxide, calculated as oxide, based on the mass of the Al-based oxide, is preferably 10 mass% or more and 80 mass% or less, more preferably 15 mass% or more and 70 mass% or less, even more preferably 20 mass% or more and 60 mass% or less, still more preferably 25 mass% or more and 55 mass% or less, and even more preferably 30 mass% or more and 50 mass% or less.

[0026] In another embodiment, the Al-based oxide contains one or more rare earth elements. This can improve the heat resistance of the Al-based oxide. From the viewpoint of improving the heat resistance of the Al-based oxide, the one or more rare earth elements are preferably selected from Y, Pr, Sc, La, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. From the viewpoint of improving the heat resistance of the Al-based oxide, the amount of rare earth elements in the Al-based oxide, calculated as oxide, is preferably 1% by mass or more and 15% by mass or less, more preferably 3% by mass or more and 10% by mass or less, and even more preferably 5% by mass or more and 7% by mass or less, based on the mass of the Al-based oxide. The term "amount of rare earth elements in the Al-based oxide, calculated as oxide," when the Al-based oxide contains one rare earth element, refers to the amount of the one rare earth element calculated as oxide. When the Al-based oxide contains two or more rare earth elements, it refers to the total amount of the two or more rare earth elements calculated as oxide.

[0027] In yet another embodiment, the Al-based oxide contains Zr and one or more rare earth elements, thereby improving the heat resistance of the Al-based oxide. The above description of the embodiment in which the Al-based oxide contains Zr and the above description of the embodiment in which the Al-based oxide contains one or more rare earth elements also apply to this embodiment.

[0028] When the composition of the Al-based oxide is known, the amount of each element in the Al-based oxide calculated as an oxide can be determined from the composition of the Al-based oxide.

[0029] When the composition of the Al-based oxide is unknown, the amount of each element in the Al-based oxide in terms of oxide can be measured by analyzing the sample by energy dispersive X-ray spectroscopy (EDX) and then performing EDX elemental analysis of the specified particles based on the obtained element mapping. Specifically, the Al-based oxide particles and other particles (e.g., Ce—Zr—Al-based composite oxide particles, etc.) are qualitatively identified (color-coded) by elemental mapping, and the specified particles are subjected to composition analysis (elemental analysis), thereby measuring the amount of each element in the specified particles in terms of oxide.

[0030] <Ce-based oxide> The Ce-based oxide refers to an oxide containing Ce, in which Ce is the element with the highest content by mass of elements other than O constituting the oxide. Among Ce-containing oxides, those that fall under the Ce-Zr-Al-based composite oxide of the present invention are not considered to fall under the Ce-based oxide. The Ce-Zr-Al-based composite oxide of the present invention will be described later.

[0031] The Ce-based oxide is, for example, in the form of particles. The Ce-based oxide is used as a support for a catalytically active component. From the viewpoint of improving the supportability of the catalytically active component, the Ce-based oxide is preferably porous. The Ce-based oxide is distinguished from ceria used as a binder. In this specification, ceria used as a binder may be referred to as a "ceria binder."

[0032] The Ce-based oxide may contain one or more elements (hereinafter sometimes referred to as "other elements") other than Ce and O. The other elements can be selected from, for example, rare earth elements other than Ce, alkaline earth metal elements (e.g., Mg, Ca, Sr, Ba, etc.), Fe, Mn, Ni, Zr, Al, etc.

[0033] Examples of Ce-based oxides include ceria (an oxide composed of Ce and O), oxides obtained by modifying the surface of ceria with other elements, and oxides obtained by dissolving other elements in ceria.

[0034] In Ce-based oxides, other elements are present in the solid solution phase (e.g., CeO 2 The crystalline or amorphous phase may be formed as a single phase (e.g., a solid solution phase of the crystalline or amorphous oxide of the other element), or may be formed as both a solid solution phase and a single phase (e.g., a phase of an oxide of the other element).

[0035] The amount of Ce in the Ce-based oxide, calculated as Ce oxide, is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 99% by mass or more, based on the mass of the Ce-based oxide, with the upper limit being 100% by mass.

[0036] The amount of Zr in the Ce-based oxide, calculated as Zr oxide, is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 3% by mass or less, and even more preferably 1% by mass or less, based on the mass of the Ce-based oxide. The lower limit is zero. The amount of Zr in the Ce-based oxide, calculated as Zr oxide, is smaller than the amount of Zr in the Ce-Zr-based composite oxide, and from this point of view, the Ce-based oxide is distinguished from the Ce-Zr-based composite oxide.

[0037] The amount of each element in the Ce-based oxide calculated as an oxide can be measured in the same manner as the amount of each element in the Al-based oxide calculated as an oxide.

[0038] <Ce—Zr-based composite oxide> The Ce—Zr-based composite oxide refers to a composite oxide containing Ce and Zr, in which the Ce oxide-equivalent content in the composite oxide is 5 mass% to 95 mass% based on the mass of the composite oxide, the Zr oxide-equivalent content in the composite oxide is 5 mass% to 95 mass% based on the mass of the composite oxide, and the Al oxide-equivalent content in the composite oxide is less than 5 mass% based on the mass of the composite oxide. Among composite oxides containing Ce and Zr, those that fall under the Ce—Zr—Al-based composite oxide of the present invention do not fall under the Ce—Zr-based composite oxide. The Ce—Zr—Al-based composite oxide of the present invention will be described later.

[0039] The Ce—Zr-based composite oxide is, for example, in the form of particles. The Ce—Zr-based composite oxide is used as a support for a catalytically active component. From the viewpoint of improving the supportability of the catalytically active component, the Ce—Zr-based composite oxide is preferably porous.

[0040] In the Ce-Zr based composite oxide, Ce exists in a solid solution phase (e.g., CeO 2 and ZrO 2 or a single phase that is a crystalline phase or an amorphous phase (e.g., a solid solution phase with CeO 2 Although Ce may form a solid solution phase or both a solid solution phase and a single phase, it is preferable that at least a part of Ce forms a solid solution phase.

[0041] In the Ce-Zr composite oxide, Zr exists in a solid solution phase (e.g., CeO 2 and ZrO 2 or a single phase that is a crystalline phase or an amorphous phase (e.g., ZrO 2 Although Zr may form a solid solution phase or both a solid solution phase and a single phase, it is preferable that at least a part of Zr forms a solid solution phase.

[0042] From the viewpoint of improving the heat resistance and oxygen storage capacity of the Ce—Zr-based composite oxide, the total amount of Ce and Zr in the Ce—Zr-based composite oxide, calculated as oxides, is preferably 70% by mass or more, more preferably 75% by mass or more, even more preferably 80% by mass or more, and even more preferably 85% by mass or more, based on the mass of the Ce—Zr-based composite oxide, with the upper limit being 100% by mass.

[0043] From the viewpoint of improving the oxygen storage capacity of the Ce—Zr-based composite oxide, the amount of Ce in the Ce—Zr-based composite oxide, calculated as Ce oxide, is preferably 5% by mass or more and 95% by mass or less, more preferably 5% by mass or more and 90% by mass or less, even more preferably 7% by mass or more and 90% by mass or less, and still more preferably 10% by mass or more and 85% by mass or less, based on the mass of the Ce—Zr-based composite oxide.

[0044] From the viewpoint of improving the heat resistance of the Ce—Zr-based composite oxide, the amount of Zr in the Ce—Zr-based composite oxide, calculated as Zr oxide, based on the mass of the Ce—Zr-based composite oxide, is preferably 5 mass % or more and 95 mass % or less, more preferably 5 mass % or more and 90 mass % or less, even more preferably 7 mass % or more and 90 mass % or less, and even more preferably 10 mass % or more and 85 mass % or less.

[0045] The Ce—Zr-based composite oxide may contain one or more elements (hereinafter sometimes referred to as “other elements”) other than Ce, Zr, and O. The other elements can be selected from, for example, rare earth elements other than Ce, alkaline earth metal elements (e.g., Mg, Ca, Sr, Ba, etc.), Fe, Mn, Ni, Al, etc.

[0046] When the Ce—Zr-based composite oxide contains other elements, the other elements may be present in a solid solution phase (e.g., CeO 2 and oxides of other elements, ZrO 2 and oxides of other elements, CeO 2 and ZrO 2The other element may form a solid solution phase (e.g., a solid solution phase of the other element and an oxide thereof), or may form a single phase that is a crystalline phase or an amorphous phase (e.g., a single phase of an oxide of the other element), or may form both a solid solution phase and a single phase, but it is preferable that at least a part of the other element forms a solid solution phase.

[0047] Examples of Ce-Zr based composite oxides include CeO 2 -ZrO 2 solid solution, CeO 2 -ZrO 2 Oxides obtained by modifying the surface of solid solutions with other elements, such as CeO 2 -ZrO 2 Examples include oxides obtained by dissolving other elements in a solid solution.

[0048] In one embodiment, the Ce—Zr-based composite oxide contains one or more rare earth elements other than Ce. This can improve the heat resistance of the Ce—Zr-based composite oxide. From the viewpoint of improving the heat resistance of the Ce—Zr-based composite oxide, the one or more rare earth elements are preferably selected from Y, Pr, Sc, La, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu.

[0049] The amount of each element in the Ce-Zr based composite oxide calculated as an oxide can be measured in the same manner as the amount of each element in the Al based oxide calculated as an oxide.

[0050] <Catalyst for Purifying Exhaust Gas> Hereinafter, an exhaust gas purifying catalyst 1 (hereinafter sometimes referred to as "catalyst 1") according to one embodiment of the present invention will be described with reference to FIGS.

[0051] As shown in Figure 1, a catalyst 1 is disposed in an exhaust passage in an exhaust pipe P of an internal combustion engine. The internal combustion engine is, for example, a gasoline engine. Exhaust gas emitted from the internal combustion engine flows through the exhaust passage in the exhaust pipe P from one end to the other end of the exhaust pipe P and is purified by the catalyst 1 provided in the exhaust pipe P. In the drawing, the exhaust gas flow direction is indicated by the symbol X. In this specification, the upstream side of the exhaust gas flow direction X may be referred to as the "exhaust gas inflow side" or "upstream side," and the downstream side of the exhaust gas flow direction X may be referred to as the "exhaust gas outflow side" or "downstream side."

[0052] In the exhaust passage in the exhaust pipe P, other exhaust gas purifying catalysts may be arranged upstream and / or downstream of the catalyst 1 .

[0053] As shown in FIGS. 2 to 4, the catalyst 1 includes a substrate 10 and a first catalyst layer 20 provided on the substrate 10 .

[0054] The catalyst 1 may include a catalyst layer other than the first catalyst layer 20 at one or more positions selected from below, above, downstream, and upstream of the first catalyst layer 20. For example, as shown in FIGS. 2 to 4 , the catalyst 1 may include a second catalyst layer 30 provided on the substrate 10. The second catalyst layer 30 is a layer that is provided as needed, and embodiments in which the second catalyst layer 30 is omitted are also encompassed by the present invention. However, from the viewpoint of improving exhaust gas purification performance, it is preferable that the catalyst 1 include the second catalyst layer 30.

[0055] <Substrate> The substrate 10 will be described below.

[0056] The material constituting the substrate 10 can be appropriately selected from known materials. Examples of materials constituting the substrate 10 include ceramic materials and metal materials, with ceramic materials being preferred. Examples of ceramic materials include carbide ceramics such as silicon carbide, titanium carbide, tantalum carbide, and tungsten carbide; nitride ceramics such as aluminum nitride, silicon nitride, boron nitride, and titanium nitride; and oxide ceramics such as alumina, zirconia, cordierite, mullite, zircon, aluminum titanate, and magnesium titanate. Examples of metal materials include alloys such as stainless steel.

[0057] 2 to 4, the substrate 10 has a cylindrical portion 11, partition walls 12 provided in the cylindrical portion 11, and cells 13 separated by the partition walls 12. The substrate 10 is preferably a honeycomb structure.

[0058] As shown in Fig. 2, the tubular portion 11 defines the outer shape of the substrate 10, and the axial direction of the tubular portion 11 coincides with the axial direction of the substrate 10. As shown in Fig. 2, the shape of the tubular portion 11 is cylindrical, but it may be other shapes such as an elliptical cylinder or a polygonal cylinder.

[0059] 2 to 4 , partition walls 12 are present between adjacent cells 13, and the adjacent cells 13 are separated by the partition walls 12. The partition walls 12 may have a porous structure that allows exhaust gas to pass through. The thickness of the partition walls 12 is, for example, 20 μm or more and 1500 μm or less.

[0060] As shown in FIG. 4, the cell 13 extends in the exhaust gas flow direction X, and has an end on the exhaust gas inlet side and an end on the exhaust gas outlet side.

[0061] As shown in Fig. 4, both the end on the exhaust gas inlet side and the end on the exhaust gas outlet side of the cell 13 are open. Therefore, the exhaust gas that flows in from the end (opening) on ​​the exhaust gas inlet side of the cell 13 flows out from the end (opening) on ​​the exhaust gas outlet side of the cell 13. This type of configuration is called a flow-through type.

[0062] 2 and 3, the end (opening) of the cell 13 on the exhaust gas inlet side has a rectangular shape in plan view, but may have other shapes such as a hexagon, an octagon, etc. The end (opening) of the cell 13 on the exhaust gas outlet side also has a similar shape in plan view.

[0063] The cell density per square inch of the substrate 10 is, for example, 100 cells or more and 1000 cells or less. The cell density per square inch of the substrate 10 means the total number of cells 13 per square inch in a cross section obtained by cutting the substrate 10 along a plane perpendicular to the exhaust gas flow direction X.

[0064] The volume of the substrate 10 is, for example, 0.1 L or more and 20 L or less. The volume of the substrate 10 means the apparent volume of the substrate 10. For example, when the substrate 10 is cylindrical, the outer diameter of the substrate 10 is 2r, and the length of the substrate 10 is L. 10 Then, the volume of the substrate 10 is calculated by the formula: Volume of the substrate 10 = π × r 2 ×L 10 It is expressed as:

[0065] The substrate 10 may be provided with a first sealing portion that seals the exhaust gas outlet end of some of the cells 13, and a second sealing portion that seals the exhaust gas inlet end of the remaining cells 13. As a result, some of the cells 13 become inlet-side cells whose exhaust gas inlet end is open and whose exhaust gas outlet end is blocked with a first sealing portion, while the remaining cells 13 become outlet-side cells whose exhaust gas inlet end is blocked with a second sealing portion and whose exhaust gas outlet end is open. A plurality (e.g., four) outlet-side cells are arranged around one inlet-side cell, and the inlet-side cell and the outlet-side cells arranged around the inlet-side cell are separated by a porous partition wall 12. Exhaust gas flowing in from the exhaust gas inlet end (opening) of the inlet-side cell passes through the porous partition wall 12 and flows out from the exhaust gas outlet end (opening) of the outlet-side cell. This type of configuration is called a wall-flow type. When exhaust gas that has flowed in from the exhaust gas inlet-side end (opening) of the inlet-side cell passes through the porous partition wall portion 12, particulate matter (PM) in the exhaust gas is captured in the pores of the partition wall portion 12. Therefore, when the substrate 10 is of the wall-flow type, the catalyst 1 is useful as a particulate filter for a gasoline engine or a particulate filter for a diesel engine.

[0066] <First catalytic layer> The first catalytic layer 20 will now be described.

[0067] As shown in FIGS. 3 and 4, the first catalyst layer 20 is provided above the second catalyst layer 30 .

[0068] The phrase "the first catalytic layer 20 is provided above the second catalytic layer 30" means that part or all of the first catalytic layer 20 is present on one of the two main surfaces of the second catalytic layer 30 opposite the main surface on the partition wall section 12 side. The "main surface of the second catalytic layer 30" means the outer surface of the second catalytic layer 30 extending in the exhaust gas flow direction X. The first catalytic layer 20 may be provided directly on the main surface of the second catalytic layer 30 or may be provided via another layer, but is usually provided directly on the main surface of the second catalytic layer 30. The first catalytic layer 20 may be provided so as to cover part of the main surface of the second catalytic layer 30 or so as to cover the entire main surface of the second catalytic layer 30. The "first catalytic layer 20 provided on the substrate 10" includes both an embodiment in which the first catalytic layer 20 is provided directly on the main surface of the second catalytic layer 30, and an embodiment in which the first catalytic layer 20 is provided on the main surface of the second catalytic layer 30 via another layer.

[0069] When the second catalytic layer 30 is omitted, the first catalytic layer 20 is provided on the cell 13-side surface of the partition wall section 12. The "cell 13-side surface of the partition wall section 12" means the outer surface of the partition wall section 12 extending in the exhaust gas flow direction X. The first catalytic layer 20 may be provided directly on the cell 13-side surface of the partition wall section 12 or may be provided via another layer, but is usually provided directly on the cell 13-side surface of the partition wall section 12.

[0070] When the first catalytic layer 20 is provided directly on the cell 13-side surface of the partition wall section 12, the first catalytic layer 20 may be composed of a portion that protrudes from the cell 13-side surface of the partition wall section 12 toward the cells 13 (hereinafter referred to as a "protruding portion"), or may be composed of a portion that exists inside the partition wall section 12 (hereinafter referred to as an "internal portion"), or may have both a protruding portion and an internal portion. The "first catalytic layer 20 provided on the substrate 10" includes any of an embodiment in which the first catalytic layer 20 is composed of a protruding portion, an embodiment in which the first catalytic layer 20 is composed of an internal portion, and an embodiment in which the first catalytic layer 20 has both a protruding portion and an internal portion.

[0071] 4 , the first catalytic layer 20 extends along the exhaust gas flow direction X from the end of the partition wall 12 on the exhaust gas inlet side to the end of the partition wall 12 on the exhaust gas outlet side. The first catalytic layer 20 may extend along the exhaust gas flow direction X from the end of the partition wall 12 on the exhaust gas inlet side so as not to reach the end of the partition wall 12 on the exhaust gas outlet side, or may extend in the direction opposite to the exhaust gas flow direction X from the end of the partition wall 12 on the exhaust gas outlet side so as not to reach the end of the partition wall 12 on the exhaust gas inlet side.

[0072] From the viewpoint of achieving a good balance between exhaust gas purification performance and cost, the mass of the first catalytic layer 20 per unit volume of the portion of the substrate 10 on which the first catalytic layer 20 is formed (mass after calcination) is preferably 20 g / L or more and 200 g / L or less, more preferably 30 g / L or more and 150 g / L or less, even more preferably 40 g / L or more and 120 g / L or less, and even more preferably 50 g / L or more and 100 g / L or less. The mass of the first catalytic layer 20 per unit volume of the portion of the substrate 10 on which the first catalytic layer 20 is formed is calculated by the formula: (mass of the first catalytic layer 20) / ((volume of the substrate 10)×(average length L of the first catalytic layer 20) 20 / Length L of the substrate 10 10 In this specification, the term "length" refers to the dimension of the substrate 10 in the axial direction, unless otherwise specified.

[0073] The "mass of the first catalytic layer 20" refers to the sum of the mass of precious metal elements in metal equivalents and the mass of metal elements other than precious metal elements in oxide equivalents, among all metal elements contained in the first catalytic layer 20. That is, the "mass of the first catalytic layer 20" refers to the calculated mass obtained by summing the mass of precious metal elements contained in the first catalytic layer 20 in metal equivalents and the mass of metal elements other than precious metal elements contained in the first catalytic layer 20 in oxide equivalents. "Metal elements" also include metalloid elements such as Si and B. "Noble metal elements" include Au, Ag, Pt, Pd, Rh, Ru, Ir, and Os. The meaning of "oxide" is as described in the "Terminology" section above.

[0074] Average length L of the first catalyst layer 20 20An example of the measurement method is as follows.

[0075] Extending from the catalyst 1 in the axial direction of the substrate 10, the length L of the substrate 10 10 A sample having the same length as the sample is cut out. The sample is, for example, cylindrical with a diameter of 25.4 mm. The diameter of the sample can be changed as needed. When the first catalyst layer 20 extends from the end of the partition wall 12 on the exhaust gas inlet side along the exhaust gas flow direction X, the sample is cut at 5 mm intervals along a plane perpendicular to the axial direction of the substrate 10, and a first cut piece, a second cut piece, ..., an n-th cut piece is obtained in order from the end of the sample on the exhaust gas inlet side. When the first catalyst layer 20 extends from the end of the partition wall 12 on the exhaust gas outlet side along the direction opposite to the exhaust gas flow direction X, the sample is cut at 5 mm intervals along a plane perpendicular to the axial direction of the substrate 10, and a first cut piece, a second cut piece, ..., an n-th cut piece is obtained in order from the end of the sample on the exhaust gas outlet side. In either case, the length of the cut pieces is 5 mm. The composition of the cut pieces is analyzed using an X-ray fluorescence analyzer (XRF) (for example, an energy dispersive X-ray analyzer (EDX), a wavelength dispersive X-ray analyzer (WDX), etc.), an inductively coupled plasma atomic emission spectrometer (ICP-AES), a scanning electron microscope-energy dispersive X-ray analysis method (SEM-EDX), etc., and it is confirmed based on the composition of the cut pieces whether or not the cut pieces contain a part of the first catalyst layer 20.

[0076] It is not necessary to perform composition analysis on a cut piece that is clearly containing a portion of the first catalytic layer 20. For example, the cut surface can be observed using a scanning electron microscope (SEM), an electron probe microanalyzer (EPMA), or the like to confirm whether the cut piece contains a portion of the first catalytic layer 20. When observing the cut surface, elemental mapping of the cut surface may be performed.

[0077] After confirming whether the cut pieces include a part of the first catalytic layer 20, the length of the first catalytic layer 20 included in the sample is calculated based on the following formula: Length of the first catalytic layer 20 included in the sample = 5 mm × (number of cut pieces including a part of the first catalytic layer 20)

[0078] For example, if the first to kth cut pieces include a portion of the first catalytic layer 20, but the (k+1)th to nth cut pieces do not include a portion of the first catalytic layer 20, the length of the first catalytic layer 20 included in the sample is (5×k) mm.

[0079] An example of a more detailed method for measuring the length of the first catalytic layer 20 included in a sample is as follows. A k-th piece (a piece obtained from the exhaust gas outlet side of the sample among the cut pieces including a part of the first catalytic layer 20 when the first catalytic layer 20 extends from the end of the partition wall 12 on the exhaust gas inlet side along the exhaust gas flow direction X, or a piece obtained from the exhaust gas inlet side of the sample among the cut pieces including a part of the first catalytic layer 20 when the first catalytic layer 20 extends from the end of the partition wall 12 on the exhaust gas outlet side along the direction opposite to the exhaust gas flow direction X) is cut in the axial direction of the substrate 10, and the part of the first catalytic layer 20 present on the cut surface is observed using an SEM, an EPMA, or the like, thereby measuring the length of the part of the first catalytic layer 20 in the k-th piece. Then, the length of the part of the first catalytic layer 20 included in the sample is calculated based on the following formula: Length of the first catalytic layer 20 included in the sample = (5 mm × (k - 1)) + (length of the part of the first catalytic layer 20 included in the k-th piece)

[0080] For 8 to 16 samples arbitrarily cut out from the catalyst 1, the length of the first catalyst layer 20 included in each sample was measured, and the average value thereof was taken as the average length L of the first catalyst layer 20. 20 Let's say.

[0081] From the viewpoint of achieving a good balance between exhaust gas purification performance and cost, the total mass of all components other than Rh in the first catalytic layer 20 per unit volume of the portion of the substrate 10 on which the first catalytic layer 20 is formed is preferably 20 g / L or more and 200 g / L or less, more preferably 30 g / L or more and 150 g / L or less, even more preferably 40 g / L or more and 120 g / L or less, and still more preferably 50 g / L or more and 100 g / L or less.

[0082] The "total mass of all components other than Rh in the first catalytic layer 20" refers to the sum of the masses, in metal equivalent, of the precious metal elements other than Rh and the masses, in oxide equivalent, of the metal elements other than the precious metal elements, of all the metal elements other than Rh contained in the first catalytic layer 20. In other words, the "total mass of all components other than Rh in the first catalytic layer 20" refers to the calculated mass obtained by summing the masses, in metal equivalent, of the precious metal elements other than Rh contained in the first catalytic layer 20 and the masses, in oxide equivalent, of the metal elements other than the precious metal elements contained in the first catalytic layer 20. The meanings of "metal element," "precious metal element," and "oxide" are as described above.

[0083] The first catalytic layer 20 contains a composite oxide containing Rh, Ce, Zr, and Al (hereinafter, may be referred to as a "Ce-Zr-Al based composite oxide").

[0084] Rh is contained in the first catalytic layer 20 in a form that can function as a catalytically active component, for example, in the form of a catalytically active component containing Rh, such as metallic Rh, an alloy containing Rh, or a compound containing Rh (e.g., an oxide of Rh). From the viewpoint of improving exhaust gas purification performance, the catalytically active component containing Rh is preferably in a particulate form.

[0085] From the viewpoint of achieving a good balance between exhaust gas purification performance and cost, the amount of Rh in the first catalytic layer 20 in terms of metal, based on the mass of the first catalytic layer 20, is preferably 0.05 mass % or more and 5 mass % or less, more preferably 0.1 mass % or more and 3 mass % or less, and even more preferably 0.2 mass % or more and 1.5 mass % or less.

[0086] The first catalytic layer 20 may contain one or more precious metal elements other than Rh. Examples of precious metal elements other than Rh include Au, Ag, Pt, Pd, Ir, Ru, and Os. The precious metal elements other than Rh are contained in the first catalytic layer 20 in a form that can function as a catalytically active component, such as a metal, an alloy containing the precious metal element, or a compound containing the precious metal element (e.g., an oxide of the precious metal element). From the viewpoint of improving exhaust gas purification performance, the catalytically active component containing the precious metal element other than Rh is preferably in a particulate form.

[0087] If the first catalytic layer 20 contains Rh and a precious metal element other than Rh, the Rh and the precious metal element other than Rh may form an alloy, which may reduce the active sites of Rh that contribute to the exhaust gas purification performance. Therefore, it is preferable that the first catalytic layer 20 does not substantially contain any precious metal element other than Rh.

[0088] The phrase "the first catalytic layer 20 is substantially free of precious metal elements other than Rh" means that the mass percentage of the metal-equivalent mass of precious metal elements other than Rh in the first catalytic layer 20 based on the metal-equivalent mass of Rh in the first catalytic layer 20 is preferably 1.0 mass% or less, more preferably 0.5 mass% or less, and even more preferably 0.1 mass% or less. The lower limit is zero. The phrase "the metal-equivalent mass of precious metal elements other than Rh in the first catalytic layer 20" means, when the first catalytic layer 20 contains one kind of precious metal element other than Rh, the metal-equivalent mass of that one kind of precious metal element, or, when the first catalytic layer 20 contains two or more kinds of precious metal elements other than Rh, the metal-equivalent mass of the two or more kinds of precious metal elements.

[0089] When the composition of the raw materials used to form the first catalytic layer 20 is known, the amount of each metal element in the first catalytic layer 20 in terms of metal or oxide can be determined from the composition of the raw materials used to form the first catalytic layer 20.

[0090] When the composition of the raw materials used to form the first catalytic layer 20 is unknown, the amount of each metal element in the first catalytic layer 20 in terms of metal or oxide can be measured using a common method such as scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX), electron probe microanalyzer (EPMA), X-ray fluorescence spectroscopy (XRF), inductively coupled plasma atomic emission spectroscopy (ICP-AES), etc. Specifically, the method is as follows.

[0091] First, a test piece cut out from catalyst 1 is pulverized and then analyzed by XRF or ICP-AES to identify the 20 metal elements with the largest molar amounts. The test piece may contain a portion derived from substrate 10 and / or a portion derived from second catalyst layer 30, as long as it contains a portion derived from first catalyst layer 20.

[0092] Next, the portion of the test piece derived from the first catalytic layer 20 is analyzed by SEM-EDX or EPMA. In SEM-EDX or EPMA, the 20 metal elements identified above are analyzed, and the total mol % of the 20 metal elements is set to 100 mol %, and the mol % of each metal element is analyzed for each of 10 SEM fields. The average mol % of each metal element in the 10 fields is taken as the mol % of each metal element in the first catalytic layer 20. From the mol % of each metal element in the first catalytic layer 20, the mass % of each precious metal element in the first catalytic layer 20 in terms of metal, and the mass % of each metal element other than the precious metal elements in the first catalytic layer 20 in terms of oxide are calculated. The mass % of each precious metal element in the first catalytic layer 20 in terms of metal is calculated from the formula: (mass of each precious metal element in terms of metal calculated from mol %) / ((mass of precious metal elements in terms of metal calculated from mol %)+(mass of metal elements other than precious metal elements in terms of oxide calculated from mol %))×100. The mass % of each metal element other than precious metal elements in the first catalytic layer 20 in terms of oxide is calculated from the formula: (mass of each metal element other than precious metal elements in terms of oxide calculated from mol %) / ((mass of precious metal elements in terms of metal calculated from mol %)+(mass of metal elements other than precious metal elements in terms of oxide calculated from mol %))×100.

[0093] It is desirable to control the air / fuel ratio (air-fuel ratio) supplied to an internal combustion engine to be close to the theoretical air-fuel ratio (stoichiometry). However, the actual air-fuel ratio fluctuates from stoichiometry to the rich (excess fuel atmosphere) or lean (lean fuel atmosphere) side, depending on the vehicle's running conditions, etc., and the air-fuel ratio of the exhaust gas also fluctuates to the rich or lean side. Because Ce-Zr-Al-based composite oxides have oxygen storage capacity, the use of Ce-Zr-Al-based composite oxides can alleviate fluctuations in the oxygen concentration in exhaust gases and expand the operating window of the catalyst.

[0094] Ce contributes to oxygen storage capacity. Therefore, in a catalytic layer containing Rh and Ce—Zr—Al-based composite oxide, as the amount of Ce in the Ce—Zr—Al-based composite oxide increases, the oxygen storage capacity of the Ce—Zr—Al-based composite oxide improves, and the exhaust gas purification performance of Rh improves. However, Ce promotes the oxidation of Rh. Here, Pt and Pd have the property of easily exhibiting exhaust gas purification performance when moderately oxidized, while Rh has the property of easily decreasing exhaust gas purification performance when oxidized. Therefore, if the amount of Ce in the Ce—Zr—Al-based composite oxide is excessive, the oxidation of Rh is promoted, and the exhaust gas purification performance of Rh decreases. Therefore, when a Ce—Zr—Al-based composite oxide is used as a support, it is particularly difficult to achieve both oxygen storage capacity and exhaust gas purification performance when Rh is used as the catalytic active component, compared to when Pt and / or Pd are used as the catalytic active component. Furthermore, if the Ce content in the Ce-Zr-Al composite oxide is excessive, the heat resistance of the Ce-Zr-Al composite oxide will be insufficient, and therefore, in a high-temperature environment, aggregation of the Ce-Zr-Al composite oxide will occur, the pores of the Ce-Zr-Al composite oxide will disappear (i.e., the specific surface area will decrease), and the like will occur, which will lead to the burial of Rh, sintering of Rh, and the exhaust gas purification performance of Rh after exposure to a high-temperature environment will decrease. In this specification, "high temperature" means a temperature of preferably 800°C or higher, more preferably 850°C or higher, and even more preferably 900°C or higher.

[0095] Therefore, in the present invention, in order to improve the oxygen storage capacity of the Ce—Zr—Al-based composite oxide and prevent a decrease in the exhaust gas purification performance of Rh (particularly, to prevent a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment), the ratio of the amount of Ce in the Ce—Zr—Al-based composite oxide (in terms of metal) to the amount of Zr in the Ce—Zr—Al-based composite oxide (in terms of metal) is adjusted. Specifically, the ratio of the amount of Ce in the Ce—Zr—Al-based composite oxide (in terms of metal) to the amount of Zr in the Ce—Zr—Al-based composite oxide (in terms of metal) is preferably 0.03 to 0.50, more preferably 0.07 to 0.50, even more preferably 0.07 to 0.42, and even more preferably 0.10 to 0.42, in mass ratio. In this specification, a Ce—Zr—Al-based composite oxide in which the above ratio is 0.03 or more and 0.50 or less in mass ratio may be referred to as the “Ce—Zr—Al-based composite oxide of the present invention.”

[0096] From the viewpoint of more effectively improving the oxygen storage capacity of the Ce—Zr—Al-based composite oxide and preventing a decrease in the exhaust gas purification performance of Rh (particularly, preventing a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment), the ratio of the amount of Al in the Ce—Zr—Al-based composite oxide of the present invention, calculated as metal, to the total amount of Ce and Zr in the Ce—Zr—Al-based composite oxide of the present invention, calculated as metal, is preferably 0.10 or more and 10 or less, more preferably 0.22 or more and 10 or less, even more preferably 0.26 or more and 8 or less, and even more preferably 0.41 or more and 6 or less, in mass ratio.

[0097] From the viewpoint of more effectively improving the oxygen storage capacity of the Ce—Zr—Al-based composite oxide and preventing a decrease in the exhaust gas purification performance of Rh (particularly, preventing a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment), the total amount of Ce, Zr, and Al in the Ce—Zr—Al-based composite oxide of the present invention, calculated as oxides, is preferably 75 mass % or more, more preferably 85 mass % or more, even more preferably 90 mass % or more, and even more preferably 95 mass % or more, based on the mass of the Ce—Zr—Al-based composite oxide of the present invention, the upper limit being 100 mass %.

[0098] From the viewpoint of more effectively improving the oxygen storage capacity of the Ce—Zr—Al-based composite oxide and preventing a decrease in the exhaust gas purification performance of Rh (particularly, preventing a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment), the amount of Ce in the Ce—Zr—Al-based composite oxide of the present invention, calculated as Ce oxide, is from 1% by mass to 30% by mass, more preferably from 2% by mass to 25% by mass, based on the mass of the Ce—Zr—Al-based composite oxide of the present invention.

[0099] From the viewpoint of more effectively improving the oxygen storage capacity of the Ce—Zr—Al-based composite oxide and preventing a decrease in the exhaust gas purification performance of Rh (particularly, preventing a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment), the total amount of Ce and Zr in the Ce—Zr—Al-based composite oxide of the present invention, calculated as oxides, is preferably 10% by mass or more and 90% by mass or less, more preferably 15% by mass or more and 85% by mass or less, and even more preferably 20% by mass or more and 80% by mass or less, based on the mass of the Ce—Zr—Al-based composite oxide of the present invention.

[0100] The Ce—Zr—Al-based composite oxide of the present invention may contain one or more elements other than Ce, Zr, Al, and O (hereinafter, sometimes referred to as “other elements”). The other elements may be selected, for example, from rare earth elements other than Ce. The rare earth elements other than Ce may be selected, for example, from Y, Pr, Sc, La, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, etc. However, from the viewpoint of more effectively improving the oxygen storage capacity of the Ce—Zr—Al-based composite oxide and preventing a decrease in the exhaust gas purification performance of Rh (particularly, preventing a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment), it is preferable to select the other elements from La, Y, Pr, and Nd.

[0101] From the viewpoint of more effectively improving the oxygen storage capacity of the Ce—Zr—Al-based composite oxide and preventing a decrease in the exhaust gas purification performance of Rh (particularly, preventing a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment), the amount of rare earth elements other than Ce in the Ce—Zr—Al-based composite oxide of the present invention, calculated as oxides, is preferably 25 mass % or less, more preferably 20 mass % or less, even more preferably 15 mass % or less, and even more preferably 10 mass % or less, based on the mass of the Ce—Zr—Al-based composite oxide of the present invention. The lower limit is zero. The "amount of rare earth elements other than Ce in the Ce—Zr—Al-based composite oxide of the present invention, calculated as oxides," when the Ce—Zr—Al-based composite oxide of the present invention contains one rare earth element other than Ce, means the amount of the one rare earth element calculated as oxide. When the Ce—Zr—Al-based composite oxide of the present invention contains two or more rare earth elements other than Ce, it means the total amount of the two or more rare earth elements calculated as oxides.

[0102] When the Ce—Zr—Al-based composite oxide of the present invention contains a rare earth element other than Ce, from the viewpoint of more effectively improving the oxygen storage capacity of the Ce—Zr—Al-based composite oxide and preventing a decrease in the exhaust gas purification performance of Rh (particularly, preventing a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment), the amount of the rare earth element other than Ce in the Ce—Zr—Al-based composite oxide of the present invention, calculated as an oxide, is preferably 5 mass % or more, more preferably 7 mass % or more, and even more preferably 10 mass % or more, based on the mass of the Ce—Zr—Al-based composite oxide of the present invention. Each of these lower limits may be combined with any of the above-mentioned upper limits.

[0103] The amount of each element in the Ce-Zr-Al based composite oxide calculated as metal or oxide can be measured in the same manner as the amount of each element in the Al based oxide calculated as oxide.

[0104] In the Ce—Zr—Al based composite oxide of the present invention, Ce exists in a solid solution phase (e.g., CeO 2 and ZrO 2 Solid solution phase with CeO 2 and ZrO 2 and Al 2 O 3or a single phase that is a crystalline phase or an amorphous phase (e.g., a solid solution phase with CeO 2 Although Ce may form a solid solution phase or both a solid solution phase and a single phase, it is preferable that at least a part of Ce forms a solid solution phase.

[0105] In the Ce—Zr—Al based composite oxide of the present invention, Zr exists in a solid solution phase (e.g., CeO 2 and ZrO 2 Solid solution phase with CeO 2 and ZrO 2 and Al 2 O 3 or a single phase that is a crystalline phase or an amorphous phase (e.g., ZrO 2 Although Zr may form a solid solution phase or both a solid solution phase and a single phase, it is preferable that at least a part of Zr forms a solid solution phase.

[0106] In the Ce—Zr—Al based composite oxide of the present invention, Al exists in a solid solution phase (e.g., CeO 2 and Al 2 O 3 Solid solution phase with ZrO 2 and Al 2 O 3 Solid solution phase with CeO 2 and ZrO 2 and Al 2 O 3 A solid solution phase with Al may be formed, or a single phase (such as a crystalline phase or an amorphous phase) may be formed. 2 O 3 Although Al may form a solid solution phase, it is preferable that at least a part of Al forms a solid solution phase.

[0107] In the Ce—Zr—Al based composite oxide of the present invention, rare earth elements other than Ce are present in a solid solution phase (e.g., CeO 2 and a solid solution phase of an oxide of a rare earth element other than Ce, ZrO 2 and a solid solution phase of an oxide of a rare earth element other than Ce, CeO 2 and ZrO 2 and a solid solution phase of oxides of rare earth elements other than Ce, Al 2 O 3The rare earth element other than Ce may form a solid solution phase (e.g., a solid solution phase of Ce and an oxide of a rare earth element other than Ce), or may form a single phase that is a crystalline phase or an amorphous phase (a single phase of an oxide of a rare earth element other than Ce), but it is preferable that at least a part of the rare earth element other than Ce forms a solid solution phase.

[0108] The Ce—Zr—Al-based composite oxide of the present invention is, for example, in the form of particles. The Ce—Zr—Al-based composite oxide of the present invention is used as a support for a catalytically active component (e.g., Rh). From the viewpoint of improving the supportability of the catalytically active component, the Ce—Zr—Al-based composite oxide of the present invention is preferably porous.

[0109] From the viewpoint of improving the exhaust gas purification performance of the catalytically active component (e.g., Rh), it is preferable that at least a portion of the catalytically active component (e.g., Rh) is supported on the Ce—Zr—Al-based composite oxide of the present invention. "At least a portion of the catalytically active component is supported on a support" means that at least a portion of the catalytically active component is physically and / or chemically adsorbed or retained on the outer surface and / or the inner surface of the pores of the support. The fact that at least a portion of the catalytically active component is supported on the support can be confirmed, for example, by analyzing the first catalyst layer 20 using scanning electron microscope-energy dispersive X-ray analysis (SEM-EDX) and finding that at least a portion of the catalytically active component and the support are present in the same region.

[0110] The first catalytic layer 20 may contain one or more components other than Rh and the Ce-Zr-Al-based composite oxide of the present invention (hereinafter, these may be referred to as "other components"). However, if the proportion of components other than the Ce-Zr-Al-based composite oxide among all components other than Rh in the first catalytic layer 20 increases, the difference in the degree of thermal expansion and thermal contraction between the Ce-Zr-Al-based composite oxide and the components other than the Ce-Zr-Al-based composite oxide in a high-temperature environment will cause the Rh to be buried or sintered, resulting in a decrease in the exhaust gas purification performance of the Rh after exposure to a high-temperature environment.

[0111] Therefore, in the present invention, in order to prevent a decrease in the exhaust gas purification performance of Rh (particularly, to prevent a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment), the amount of the Ce—Zr—Al-based composite oxide in the first catalytic layer 20 is adjusted. Specifically, the amount of the Ce—Zr—Al-based composite oxide of the present invention in the first catalytic layer 20 is preferably 70 mass % or more, more preferably 75 mass % or more, even more preferably 80 mass % or more, and even more preferably 90 mass % or more, based on the total mass of all components other than Rh in the first catalytic layer 20. The upper limit is 100 mass %.

[0112] When the composition of the raw materials used to form the first catalytic layer 20 is known, the amount of the Ce-Zr-Al-based composite oxide of the present invention in the first catalytic layer 20 can be determined from the composition of the raw materials used to form the first catalytic layer 20.

[0113] When the composition of the raw materials used to form the first catalytic layer 20 is unknown, the amount of the Ce—Zr—Al-based composite oxide of the present invention in the first catalytic layer 20 can be measured by a conventional method such as inductively coupled plasma optical emission spectroscopy (ICP), X-ray fluorescence spectroscopy (XRF), or scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX). Specifically, the method is as follows.

[0114] (A) Elemental analysis is performed on the sample obtained from the first catalytic layer 20 using a standard method such as ICP, XRF, or SEM-EDX to identify the types of constituent elements of the entire sample and determine the content (mass%) of each identified element. (B) Elemental mapping is performed on the sample obtained from the first catalytic layer 20 using a standard method such as SEM-EDX to identify the types of particles contained in the sample (e.g., Ce-Zr-Al composite oxide particles, Al-based oxide particles, etc.). (C) For each type of particle, elemental analysis is performed on a number of arbitrarily selected particles (e.g., 50 particles) using SEM-EDX to identify the types of constituent elements of the particles and determine the content (mass%) of each identified element. The average content (mass%) of each element is determined for each type of particle. (D) An equation is created and solved to represent the relationship between the content (mass%) of each element in the sample, the content (mass%) of each element in each type of particle, and the content (mass%) of each type of particle in the sample, thereby calculating the content (mass%) of each type of particle in the sample, and this is set as the content (mass%) of each type of particle in the first catalyst layer 20.

[0115] The first catalytic layer 20 may contain one or more binders. This can prevent peeling of the first catalytic layer 20. The binder is not particularly limited as long as it is an inorganic oxide other than a Ce—Zr—Al-based composite oxide. The binder can be selected from inorganic binders such as alumina, zirconia, titania, silica, ceria, and yttria. When the first catalytic layer 20 contains a binder, from the viewpoint of more effectively preventing a decrease in the exhaust gas purification performance of Rh (particularly, preventing a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment) and preventing peeling of the first catalytic layer 20, the amount of the binder in the first catalytic layer 20 is preferably 0.5% by mass or more and 10% by mass or less, more preferably 1% by mass or more and 8% by mass or less, based on the total mass of all components of the first catalytic layer 20 other than Rh. The "amount of binder in the first catalytic layer 20" means the amount of one type of binder when the first catalytic layer 20 contains one type of binder, and means the total amount of the two or more types of binders when the first catalytic layer 20 contains two or more types of binders.

[0116] The first catalytic layer 20 may contain one or more supports (hereinafter, sometimes referred to as "other supports") other than the Ce-Zr-Al-based composite oxide of the present invention. When the first catalytic layer 20 contains the other supports, at least a part of the catalytically active component (e.g., Rh) may be supported on the other supports.

[0117] From the viewpoint of effectively preventing a decrease in the exhaust gas purification performance of Rh (particularly, preventing a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment), the amount of the other carrier in the first catalytic layer 20 is preferably 28 mass% or less, more preferably 25 mass% or less, even more preferably 20 mass% or less, and even more preferably 10 mass% or less, based on the total mass of all components other than Rh in the first catalytic layer 20. The lower limit is zero. The smaller the amount of the other carrier in the first catalytic layer 20, the more preferable it is. When the first catalytic layer 20 contains one other type of carrier, the term "amount of the other carrier in the first catalytic layer 20" refers to the amount of that one type of carrier, and when the first catalytic layer 20 contains two or more other types of carriers, the term refers to the total amount of the two or more types of carriers.

[0118] The amount of the other carrier in the first catalytic layer 20 may be, for example, 1 mass % or more, 3 mass % or more, or 5 mass % or more, based on the total mass of all components other than Rh in the first catalytic layer 20. Each of these lower limits may be combined with any of the above-mentioned upper limits.

[0119] The method for measuring the amount of other carriers in the first catalytic layer 20 is the same as the method for measuring the amount of the Ce—Zr—Al-based composite oxide of the present invention in the first catalytic layer 20 .

[0120] The other carrier can be selected from inorganic oxides. The inorganic oxide is, for example, particulate. From the viewpoint of easily supporting the catalytically active component, the inorganic oxide is preferably porous. The inorganic oxide may or may not have oxygen storage capacity. In this specification, an inorganic oxide having oxygen storage capacity may be referred to as an "OSC material."

[0121] Examples of inorganic oxides include Al-based oxides, Ce-based oxides, Ce—Zr-based composite oxides, Ce—Zr—Al-based composite oxides other than the Ce—Zr—Al-based composite oxide of the present invention, and oxides of rare earth elements other than Ce (for example, Y 2 O 3 etc.), oxides of alkaline earth metal elements (e.g., MgO, CaO, SrO, BaO etc.), ZrO 2 , SiO 2 , TiO 2 , NiO, etc.

[0122] In one embodiment, the first catalytic layer 20 contains an Al-based oxide in addition to the Ce—Zr—Al-based composite oxide of the present invention.

[0123] In one embodiment, the Al-based oxide includes Zr. In another embodiment, the Al-based oxide includes one or more rare earth elements. In yet another embodiment, the Al-based oxide includes Zr and one or more rare earth elements. The description of these embodiments is as above.

[0124] <Second catalytic layer> The second catalytic layer 30 will now be described.

[0125] 3 and 4 , the second catalytic layer 30 is provided on the cell 13 side surface of the partition wall section 12. The "cell 13 side surface of the partition wall section 12" means the outer surface of the partition wall section 12 extending in the exhaust gas flow direction X. The second catalytic layer 30 may be provided directly on the cell 13 side surface of the partition wall section 12 or via another layer, but is usually provided directly on the cell 13 side surface of the partition wall section 12.

[0126] The second catalytic layer 30 may be composed of a portion that protrudes from the cell 13-side surface of the partition wall section 12 toward the cell 13 (hereinafter referred to as a "protruding portion"), or may be composed of a portion that exists inside the partition wall section 12 (hereinafter referred to as an "internal portion"), or may have both a protruding portion and an internal portion. The "second catalytic layer 30 provided on the substrate 10" includes any of an embodiment in which the second catalytic layer 30 is composed of a protruding portion, an embodiment in which the second catalytic layer 30 is composed of an internal portion, and an embodiment in which the second catalytic layer 30 has both a protruding portion and an internal portion.

[0127] 4 , the second catalytic layer 30 extends along the exhaust gas flow direction X from the end of the partition wall 12 on the exhaust gas inlet side to the end of the partition wall 12 on the exhaust gas outlet side. The second catalytic layer 30 may extend along the exhaust gas flow direction X from the end of the partition wall 12 on the exhaust gas inlet side so as not to reach the end of the partition wall 12 on the exhaust gas outlet side, or may extend in the direction opposite to the exhaust gas flow direction X from the end of the partition wall 12 on the exhaust gas outlet side so as not to reach the end of the partition wall 12 on the exhaust gas inlet side.

[0128] From the viewpoint of achieving a good balance between exhaust gas purification performance and cost, the mass of the second catalytic layer 30 per unit volume of the portion of the substrate 10 on which the second catalytic layer 30 is formed (mass after calcination) is preferably 20 g / L or more and 200 g / L or less, more preferably 30 g / L or more and 150 g / L or less, even more preferably 40 g / L or more and 120 g / L or less, and even more preferably 50 g / L or more and 100 g / L or less. The mass of the second catalytic layer 30 per unit volume of the portion of the substrate 10 on which the second catalytic layer 30 is formed is calculated by the formula: (mass of the second catalytic layer 30) / ((volume of the substrate 10)×(average length L of the second catalytic layer 30) 30 / Length L of the substrate 10 10 In this specification, the term "length" refers to the dimension of the substrate 10 in the axial direction, unless otherwise specified.

[0129] The above description regarding the mass of the first catalytic layer 20 also applies to the mass of the second catalytic layer 30. When applied, the "first catalytic layer 20" is read as the "second catalytic layer 30."

[0130] Average length L of the first catalyst layer 20 20 The above description of the method for measuring the average length L of the second catalyst layer 30 30 When applying this method, the "first catalyst layer 20" is referred to as the "second catalyst layer 30" and the "average length L 20 " is "average length L 30 " can be read as ".

[0131] From the viewpoint of improving exhaust gas purification performance, it is preferable that the second catalytic layer 30 contains either Pd or Pt, or both Pd and Pt. By providing the first catalytic layer 20 on the upper side of the second catalytic layer 30, it is possible to prevent phosphorus poisoning of either Pd or Pt, or both Pd and Pt, contained in the second catalytic layer 30.

[0132] Pd is contained in the second catalytic layer 30 in a form capable of functioning as a catalytically active component, such as metallic Pd, an alloy containing Pd, or a compound containing Pd (e.g., an oxide of Pd). Pt is contained in the second catalytic layer 30 in a form capable of functioning as a catalytically active component, such as metallic Pt, an alloy containing Pt, or a compound containing Pt (e.g., an oxide of Pt). The catalytically active component containing Pd and the catalytically active component containing Pt are each, for example, in the form of particles.

[0133] From the viewpoint of achieving a good balance between exhaust gas purification performance and cost, the amount of either Pd or Pt, or both Pd and Pt, in the second catalytic layer 30, in terms of metal is preferably 0.07 mass % or more and 10 mass % or less, more preferably 0.3 mass % or more and 6 mass % or less, and even more preferably 0.7 mass % or more and 4 mass % or less, based on the mass of the second catalytic layer 30. The phrase "the amount of either Pd or Pt, or both Pd and Pt, in terms of metal, in the second catalytic layer 30" means the amount of either Pd or Pt in terms of metal when the second catalytic layer 30 contains one of Pd or Pt, or means the total amount of both Pd and Pt in terms of metal when the second catalytic layer 30 contains both Pd and Pt.

[0134] The amounts of Pd and Pt in the second catalytic layer 30 in terms of metal can be measured in the same manner as the amounts of the respective metal elements in the first catalytic layer 20 described above in terms of metal.

[0135] From the viewpoint of improving the exhaust gas purification performance, it is preferable that the second catalyst layer 30 contains one or more types of carriers, and at least a part of the catalytically active component is supported on one or more types of carriers. The meaning of "at least a part of the catalytically active component is supported on a carrier" and the method for confirming this are the same as those described above.

[0136] The one or more supports can be selected from, for example, inorganic oxides. The inorganic oxide is, for example, particulate. From the viewpoint of easily supporting the catalytically active component, the inorganic oxide is preferably porous. The inorganic oxide may or may not have oxygen storage capacity.

[0137] Examples of inorganic oxides include Al-based oxides, Ce-based oxides, Ce—Zr-based composite oxides, Ce—Zr—Al-based composite oxides, and oxides of rare earth elements other than Ce (for example, Y 2 O 3 etc.), oxides of alkaline earth metal elements (e.g., MgO, CaO, SrO, BaO etc.), ZrO 2 , SiO 2 , TiO 2 , NiO, etc.

[0138] The second catalyst layer 30 may contain a binder, which may be selected from inorganic binders such as alumina, zirconia, titania, silica, ceria, and yttria.

[0139] <Method for manufacturing exhaust gas purifying catalyst> The exhaust gas purifying catalyst 1 can be manufactured by forming the second catalyst layer 30 on the substrate 10, and then forming the first catalyst layer 20 on the upper side of the second catalyst layer 30.

[0140] The second catalytic layer 30 can be formed by mixing a source of a precious metal element (e.g., a Pd salt) and other components (e.g., an inorganic oxide, a binder, a solvent) to prepare a slurry for the second catalytic layer, applying the slurry for the second catalytic layer onto the partition wall portions 12 of the substrate 10, drying, and firing the slurry.

[0141] The first catalytic layer 20 can be formed by mixing a source of a precious metal element (e.g., an Rh salt) and other components (e.g., a Ce-Zr-Al composite oxide, and optionally other inorganic oxides, a binder, a solvent, etc.) to prepare a slurry for the first catalytic layer, applying the slurry for the first catalytic layer onto the second catalytic layer 30, drying, and firing.

[0142] The binder can be selected from metal oxide sols such as alumina sol, zirconia sol, titania sol, silica sol, ceria sol, yttria sol, etc. The solvent can be selected from water, organic solvents, etc.

[0143] The drying temperature is, for example, 60° C. or higher and 150° C. or lower, and the drying time is, for example, 0.1 hour or higher and 1 hour or lower. The firing temperature is, for example, 300° C. or higher and 700° C. or lower, and the firing time is, for example, 1 hour or higher and 10 hours or lower. The firing can be carried out, for example, in an air atmosphere.

[0144] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.

[0145] An Al—Zr-based oxide was prepared and used in Example 2 and Comparative Examples 1 to 3. Hereinafter, the Al—Zr-based oxide may be referred to as “AZ.”

[0146] The composition of the Al-Zr oxide is as follows: 2 O 3 Amount converted: 50 mass% ZrO 2 Amount converted into oxide: 40 mass% Amount converted into oxide of rare earth elements other than Ce: 10 mass%

[0147] Ce—Zr—Al-based composite oxides (I) to (V) were prepared. In Example 1, Example 2, Comparative Examples 1 and 2, Ce—Zr—Al-based composite oxide (II) was used, in Example 3, Ce—Zr—Al-based composite oxide (I) was used, in Example 4, Ce—Zr—Al-based composite oxide (III), in Example 5, Ce—Zr—Al-based composite oxide (IV), and in Comparative Example 4, Ce—Zr—Al-based composite oxide (V) was used. In Comparative Example 3, none of the Ce—Zr—Al-based composite oxides was used. Hereinafter, the Ce—Zr—Al-based composite oxide may be referred to as "CZA."

[0148] The composition of the Ce-Zr-Al composite oxide (I) is as follows: CeO 2 Amount converted: 3 mass% ZrO 2 Amount converted: 50 mass% Al of Al 2 O3 Amount converted to oxide: 42 mass% Amount converted to oxide of rare earth elements other than Ce: 5 mass%

[0149] The composition of the Ce-Zr-Al composite oxide (II) is as follows: CeO 2 Amount converted: 10 mass% ZrO 2 Amount converted: 50 mass% Al of Al 2 O 3 Amount converted into oxide: 35 mass% Amount converted into oxide of rare earth elements other than Ce: 5 mass%

[0150] The composition of the Ce-Zr-Al composite oxide (III) is as follows: CeO 2 Amount converted: 19 mass% ZrO 2 Amount converted: 50 mass% Al of Al 2 O 3 Amount converted to oxide: 26 mass% Amount converted to oxide of rare earth elements other than Ce: 5 mass%

[0151] The composition of the Ce-Zr-Al composite oxide (IV) is as follows: CeO 2 Amount converted: 22.5 mass% ZrO 2 Amount converted: 50 mass% Al of Al 2 O 3 Amount converted into oxide: 22.5 mass% Amount converted into oxide of rare earth elements other than Ce: 5 mass%

[0152] The composition of the Ce-Zr-Al composite oxide (V) is as follows: CeO 2 Amount converted: 38.5 mass% ZrO 2 Amount converted: 50 mass% Al of Al 2 O 3 Amount converted to oxide: 6.5 mass% Amount converted to oxide of rare earth elements other than Ce: 5 mass%

[0153] Table 1 shows the compositional characteristics of the Ce—Zr—Al based composite oxides (I) to (V).

[0154]

[0155] Example 1 (1) Formation of Lower Layer A palladium nitrate aqueous solution, an OSC material, an alumina material, barium sulfate, an alumina binder, and water were added to a mixing vessel, and the mixture was mixed and stirred to prepare a lower layer forming slurry. A flow-through type substrate was immersed in the lower layer forming slurry, and the flow-through type substrate coated with the lower layer forming slurry was dried in a dryer at 150°C for 0.5 hours, and then fired in an electric furnace at 500°C for 1 hour to form a lower layer on the flow-through type substrate.

[0156] The mass of the lower layer per unit volume of the portion of the flow-through substrate on which the lower layer was formed was 122 g / L. The mass of Pd in ​​the lower layer per unit volume of the portion of the flow-through substrate on which the lower layer was formed was 2 g / L. The total mass of all components other than Pd in ​​the lower layer per unit volume of the portion of the flow-through substrate on which the lower layer was formed was 120 g / L. The amounts of each component in the lower layer-forming slurry were adjusted so that the OSC material was 45 mass%, the alumina material was 45 mass%, the barium sulfate was 5 mass%, and the alumina binder was 5 mass%, based on the total mass of the components other than Pd in ​​the lower layer (100 mass%).

[0157] (2) Formation of Upper Layer A rhodium nitrate aqueous solution, Ce—Zr—Al composite oxide (II), alumina binder, and water were added to a mixing vessel, and the mixture was mixed and stirred to prepare an upper layer forming slurry. The flow-through type substrate on which the lower layer had been formed was immersed in the upper layer forming slurry, and the flow-through type substrate coated with the upper layer forming slurry was dried using a dryer at 150°C for 0.5 hours, and then fired using an electric furnace at 500°C for 1 hour to form an upper layer on the lower layer. In this way, the exhaust gas purification catalyst of Example 1 was obtained.

[0158] The total mass of all components other than Rh in the upper layer per unit volume of the flow-through substrate where the upper layer was formed was adjusted to 100 g / L. The mass of Rh in the upper layer per unit volume of the flow-through substrate where the upper layer was formed was adjusted to 0.5 g / L.

[0159] The amounts of each component in the upper layer-forming slurry were adjusted so that the Ce-Zr-Al composite oxide (II) in the upper layer was 95% by mass and the alumina binder in the upper layer was 5% by mass, with the total mass of all components other than Rh in the upper layer being taken as 100% by mass. Since the total mass of all components other than Rh in the upper layer per unit volume of the portion of the flow-through substrate on which the upper layer is formed is 100 g / L, the mass of the Ce-Zr-Al composite oxide (II) in the upper layer per unit volume of the portion of the flow-through substrate on which the upper layer is formed is 95 g / L, and the mass of the alumina binder in the upper layer per unit volume of the portion of the flow-through substrate on which the upper layer is formed is 5 g / L.

[0160] Example 2 (1) Formation of Lower Layer In the same manner as in Example 1, a lower layer was formed on a flow-through type substrate.

[0161] (2) Formation of Upper Layer A rhodium nitrate aqueous solution, Ce—Zr—Al composite oxide (II), Al—Zr oxide, alumina binder, and water were added to a mixing vessel, and the mixture was mixed and stirred to prepare an upper layer forming slurry. The flow-through type substrate on which the lower layer had been formed was immersed in the upper layer forming slurry, and the flow-through type substrate coated with the upper layer forming slurry was dried using a dryer at 150°C for 0.5 hours, and then fired using an electric furnace at 500°C for 1 hour to form an upper layer on the lower layer. In this way, the exhaust gas purification catalyst of Example 2 was obtained.

[0162] The total mass of all components other than Rh in the upper layer per unit volume of the flow-through substrate where the upper layer was formed was adjusted to 100 g / L. The mass of Rh in the upper layer per unit volume of the flow-through substrate where the upper layer was formed was adjusted to 0.5 g / L.

[0163] The amounts of each component in the upper layer-forming slurry were adjusted so that the Ce—Zr—Al-based composite oxide (II) in the upper layer was 70 mass%, the Al—Zr-based oxide in the upper layer was 25 mass%, and the alumina binder in the upper layer was 5 mass%, based on the total mass of all components other than Rh in the upper layer (100 mass%). Since the total mass of all components other than Rh in the upper layer per unit volume of the portion of the flow-through substrate on which the upper layer is formed is 100 g / L, the mass of the Ce—Zr—Al-based composite oxide (II) in the upper layer per unit volume of the portion of the flow-through substrate on which the upper layer is formed is 70 g / L, the mass of the Al—Zr-based oxide in the upper layer per unit volume of the portion of the flow-through substrate on which the upper layer is formed is 25 g / L, and the mass of the alumina binder in the upper layer per unit volume of the portion of the flow-through substrate on which the upper layer is formed is 5 g / L.

[0164] Example 3 (1) Formation of Lower Layer In the same manner as in Example 1, a lower layer was formed on a flow-through type substrate.

[0165] (2) Formation of Upper Layer An upper layer was formed on the lower layer in the same manner as in Example 1, except that the Ce—Zr—Al-based composite oxide (I) was used instead of the Ce—Zr—Al-based composite oxide (II), thereby obtaining a catalyst for purifying exhaust gases of Example 3.

[0166] Example 4 (1) Formation of Lower Layer In the same manner as in Example 1, a lower layer was formed on a flow-through type substrate.

[0167] (2) Formation of Upper Layer An upper layer was formed on the lower layer in the same manner as in Example 1, except that the Ce—Zr—Al-based composite oxide (III) was used instead of the Ce—Zr—Al-based composite oxide (II), thereby obtaining a catalyst for purifying exhaust gases of Example 4.

[0168] Example 5 (1) Formation of Lower Layer In the same manner as in Example 1, a lower layer was formed on a flow-through type substrate.

[0169] (2) Formation of Upper Layer An upper layer was formed on the lower layer in the same manner as in Example 1, except that the Ce—Zr—Al-based composite oxide (II) was replaced with the Ce—Zr—Al-based composite oxide (IV), to obtain a catalyst for purifying exhaust gases of Example 5.

[0170] Comparative Example 1 (1) Formation of Lower Layer In the same manner as in Example 1, a lower layer was formed on a flow-through type substrate.

[0171] (2) Formation of Upper Layer An upper layer was formed on the lower layer in the same manner as in Example 2, except that the amounts of each component in the upper layer-forming slurry were adjusted so that the Ce-Zr-Al-based composite oxide (II) in the upper layer was 50 mass %, the Al-Zr-based oxide in the upper layer was 45 mass %, and the alumina binder in the upper layer was 5 mass %, relative to the total mass of all components other than Rh in the upper layer (100 mass %), to obtain a catalyst for purifying exhaust gas of Comparative Example 1.

[0172] The total mass of all components other than Rh in the upper layer per unit volume of the portion of the flow-through type substrate on which the upper layer is formed is 100 g / L, so the mass of the Ce-Zr-Al-based composite oxide (II) in the upper layer per unit volume of the portion of the flow-through type substrate on which the upper layer is formed is 50 g / L, the mass of the Al-Zr-based oxide in the upper layer per unit volume of the portion of the flow-through type substrate on which the upper layer is formed is 45 g / L, and the mass of the alumina binder in the upper layer per unit volume of the portion of the flow-through type substrate on which the upper layer is formed is 5 g / L.

[0173] Comparative Example 2 (1) Formation of Lower Layer In the same manner as in Example 1, a lower layer was formed on a flow-through type substrate.

[0174] (2) Formation of Upper Layer An upper layer was formed on the lower layer in the same manner as in Example 2, except that the amounts of each component in the upper layer-forming slurry were adjusted so that the Ce-Zr-Al-based composite oxide (II) in the upper layer was 25 mass %, the Al-Zr-based oxide in the upper layer was 70 mass %, and the alumina binder in the upper layer was 5 mass %, relative to the total mass of all components other than Rh in the upper layer (100 mass %). Thus, a catalyst for purifying exhaust gases of Comparative Example 2 was obtained.

[0175] The total mass of all components other than Rh in the upper layer per unit volume of the portion of the flow-through type substrate on which the upper layer is formed is 100 g / L, so the mass of the Ce-Zr-Al-based composite oxide (II) in the upper layer per unit volume of the portion of the flow-through type substrate on which the upper layer is formed is 25 g / L, the mass of the Al-Zr-based oxide in the upper layer per unit volume of the portion of the flow-through type substrate on which the upper layer is formed is 70 g / L, and the mass of the alumina binder in the upper layer per unit volume of the portion of the flow-through type substrate on which the upper layer is formed is 5 g / L.

[0176] Comparative Example 3 (1) Formation of Lower Layer In the same manner as in Example 1, a lower layer was formed on a flow-through type substrate.

[0177] (2) Formation of Upper Layer An upper layer was formed on the lower layer in the same manner as in Example 2, except that the amounts of each component in the slurry for forming the upper layer were adjusted so that the Al—Zr-based oxide in the upper layer was 95 mass % and the alumina binder in the upper layer was 5 mass %, relative to the total mass of all components other than Rh in the upper layer (100 mass %), to obtain a catalyst for purifying exhaust gases of Comparative Example 3. Note that in Comparative Example 3, no Ce—Zr—Al-based composite oxide was used.

[0178] The total mass of all components other than Rh in the upper layer per unit volume of the portion of the flow-through type substrate on which the upper layer is formed is 100 g / L, so the mass of the Al—Zr-based oxide in the upper layer per unit volume of the portion of the flow-through type substrate on which the upper layer is formed is 95 g / L, and the mass of the alumina binder in the upper layer per unit volume of the portion of the flow-through type substrate on which the upper layer is formed is 5 g / L.

[0179] Comparative Example 4 (1) Formation of Lower Layer In the same manner as in Example 1, a lower layer was formed on a flow-through type substrate.

[0180] (2) Formation of Upper Layer An upper layer was formed on the lower layer in the same manner as in Example 1, except that the Ce—Zr—Al-based composite oxide (V) was used instead of the Ce—Zr—Al-based composite oxide (II), thereby obtaining a catalyst for purifying exhaust gases of Comparative Example 4.

[0181] [Test Example 1] (1) Degradation Treatment The following durability conditions were imposed on each exhaust gas purification catalyst as a degradation treatment assuming a driving distance of 50,000 to 100,000 kilometers. Specifically, each exhaust gas purification catalyst was maintained at the following temperature for the following time in a state where it was in contact with exhaust gas emitted by operating an engine under the following conditions. (Durability Conditions) Durability engine: NA 2L passenger gasoline engine Gasoline used: Commercially available regular gasoline Temperature and time: 100 hours at 950°C

[0182] (2) Evaluation of OSC Using a temperature-programmed reduction treatment device (TPR device) manufactured by Henmi Slide Rule Co., Ltd., the OSC of each exhaust gas purification catalyst after the aging treatment was measured by a CO pulse method. In the OSC measurement, each exhaust gas purification catalyst after the aging treatment was pretreated by heating it to 800°C in a He flow and maintaining that temperature for 40 minutes, and then cooled to 300°C. Then, while maintaining at 300°C, O 2 After the gas was injected in four pulses to perform oxidation treatment, O 2 The gas was stopped, and the test gas containing CO was injected in 10 pulses. The OSC amount (μmol / g) of each exhaust gas purification catalyst at 300°C was measured from the total amount of consumed CO gas using an infrared gas concentration measuring device (Shimadzu Corporation, CGT-7000). The "OSC amount (μmol / g) of each exhaust gas purification catalyst at 300°C" refers to the OSC amount per unit mass of the catalyst layer (lower layer and upper layer) of each exhaust gas purification catalyst. The test gas was prepared by diluting CO gas by 25% by volume with He gas. The percentage of the OSC amount (μmol / g) of each exhaust gas purification catalyst relative to the OSC amount (μmol / g) of the exhaust gas purification catalyst of Example 1 was calculated, and this was used as the relative value of the OSC amount of each exhaust gas purification catalyst. The results are shown in Table 2.

[0183] The relative value of the OSC amount of the exhaust gas purification catalyst of Comparative Example 3 (because the upper layer of Comparative Example 3 does not contain an OSC such as a Ce-Zr-Al composite oxide, the OSC amount of Comparative Example 3 essentially corresponds to the OSC amount of the lower layer alone) was subtracted from the relative value of the OSC amount of each exhaust gas purification catalyst, and the resulting value was divided by the mass of the Ce-Zr-Al composite oxide in the upper layer per unit volume of the portion of the flow-through substrate on which the upper layer was formed, and the resulting value was used as an index representing the OSC per unit mass of the Ce-Zr-Al composite oxide. The results are shown in Table 2.

[0184] (3) Evaluation of exhaust gas purification performance Each of the exhaust gas purification catalysts after the degradation treatment was placed in the exhaust passage, and an exhaust model gas (CO: 0.50%, H 2 : 0.17%, O 2 : 0.50%, NO: 400ppm, C 3 H 6 :1180ppm, CO 2 : 14%, H 2 O: 10%, N 2 While the mixture (including the remaining part) was passed through the reactor at a space velocity of 100,000 / h, the temperature of the supplied gas was raised to 500°C at a rate of 20°C / min, and the purification rate of nitrogen oxides (NOx) in the discharged gas was continuously measured to determine the temperature (light-off temperature T50) (°C) at which the purification rate of nitrogen oxides (NOx) reached 50%. The light-off temperature T50 was determined during temperature rise. The results are shown in Table 2.

[0185]

[0186] As shown in Table 2, Examples 1 to 5, which satisfied the following conditions: [Condition 1] the amount of Ce—Zr—Al-based composite oxide is 70 mass % or more, based on the total mass of all components other than Rh in the upper layer; and [Condition 2] the ratio of the amount of Ce in the Ce—Zr—Al-based composite oxide, calculated on a metal basis, to the amount of Zr in the Ce—Zr—Al-based composite oxide, calculated on a metal basis, is 0.03 to 0.50, in mass ratio, were able to improve the oxygen storage capacity of the Ce—Zr—Al-based composite oxide and prevent a decrease in the exhaust gas purification performance of Rh (particularly, prevent a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment). In contrast, Comparative Examples 1 and 2, which satisfied Condition 2 but not Condition 1, were unable to improve the oxygen storage capacity of the Ce—Zr—Al-based composite oxide or prevent a decrease in the exhaust gas purification performance of Rh (particularly, prevent a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment). Furthermore, Comparative Example 4, which satisfied Condition 1 but not Condition 2, was able to improve the oxygen storage capacity of the Ce—Zr—Al-based composite oxide, but was unable to prevent a decrease in the exhaust gas purification performance of Rh (particularly, to prevent a decrease in the exhaust gas purification performance of Rh after exposure to a high-temperature environment). Furthermore, Comparative Example 3, which satisfied neither Condition 1 nor Condition 2, had an insufficient amount of OSC.

[0187] DESCRIPTION OF SYMBOLS 1... catalyst for purifying exhaust gas 10... substrate 11... cylindrical portion 12... partition portion 13... cell 20... first catalyst layer 30... second catalyst layer

Claims

1. A catalyst for purifying exhaust gas comprising a substrate and a first catalytic layer provided on the substrate, wherein the first catalytic layer contains a composite oxide containing Rh and Ce, Zr and Al, the amount of the composite oxide is 70 mass% or more based on the total mass of all components other than Rh of the first catalytic layer, and the ratio of the amount of Ce in the composite oxide in terms of metal to the amount of Zr in the composite oxide in terms of metal is 0.03 or more and 0.50 or less, in terms of mass.

2. The exhaust gas purification catalyst according to claim 1, wherein the ratio of the amount of Al in said composite oxide in terms of metal to the total amount of Ce and Zr in said composite oxide in terms of metal is 0.10 or more and 10 or less, in terms of mass.

3. The exhaust gas purifying catalyst according to claim 1, wherein the total amount of Ce, Zr and Al in the composite oxide calculated as oxides is 75 mass % or more based on the mass of the composite oxide.

4. The exhaust gas purifying catalyst according to claim 3, wherein the amount of rare earth elements other than Ce in said composite oxide calculated as oxides is 25 mass % or less based on the mass of said composite oxide.

5. The exhaust gas purifying catalyst according to claim 4, wherein the rare earth elements other than Ce are selected from the group consisting of La, Y, Pr and Nd.

6. The exhaust gas purifying catalyst according to claim 1, wherein the first catalyst layer contains an Al-based oxide.

7. The exhaust gas purifying catalyst according to claim 1, wherein the first catalyst layer contains a binder.

8. The exhaust gas purifying catalyst according to claim 7, wherein the binder is an inorganic oxide other than a Ce-Zr-Al based composite oxide.

9. The exhaust gas purifying catalyst according to claim 1, wherein the exhaust gas purifying catalyst comprises a second catalyst layer provided on the substrate, the first catalyst layer is provided on an upper side of the second catalyst layer, and the second catalyst layer contains one of Pd or Pt, or both Pd and Pt.

Citation Information

Patent Citations

  • Catalyst for purifying exhaust gas

    JP1998202102A

  • Catalyst converter

    JP2017189745A

  • Catalyst for cleaning exhaust gas

    JP2005224792A

  • Catalyst for cleaning exhaust

    JP2010005591A

  • Exhaust gas purifying catalyst

    JP2010227804A