Thermally expandable refractory material composition, thermally expandable refractory material, and method for producing thermally expandable refractory material

The thermally expandable refractory material composition, featuring a polymer with moisture-curable functional groups and a curing catalyst, addresses the slow curing issue of conventional materials by achieving rapid curing at 50°C and 13% RH, enhancing productivity and efficiency in the application process.

WO2024204161A1PCT designated stage expired Publication Date: 2024-10-03SEKISUI CHEMICAL CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011887
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional thermally expandable refractory materials with moisture-curable compositions take a long time to cure, hindering productivity due to the need for extensive shelf space and prolonged curing times, especially for thicker applications.

Method used

A thermally expandable refractory material composition incorporating a polymer with moisture-curable functional groups, a thermally expandable compound, and a curing catalyst, which can cure within 60 minutes at 50°C and 13% RH, utilizing crosslinkable silyl group-containing polyoxyalkylene polymers and silylated urethanes to accelerate the curing process.

Benefits of technology

The composition allows for rapid curing of the thermally expandable refractory material, significantly reducing deep curing time and improving productivity by enabling quick hardening even in deep sections, thus enhancing operational efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

A thermally expandable refractory material composition containing a polymer having a moisture-curing functional group, a thermally expandable compound, and a curing catalyst, wherein a deep-portion curing time of a coating film, which is obtained by applying the thermally expandable refractory material composition so as to have a thickness of 2 mm, is 60 min or less in an environment of 50°C and 13% RH.
Need to check novelty before this filing date? Find Prior Art

Description

Thermally expandable fire-resistant material composition, thermally expandable fire-resistant material, and method for producing thermally expandable fire-resistant material

[0001] The present invention relates to a thermally expandable fire-resistant composition, a thermally expandable fire-resistant material formed from the thermally expandable fire-resistant composition, and a method for making the thermally expandable fire-resistant material.

[0002] Conventionally, thermally expandable fire-resistant materials that expand when heated have been widely used in buildings and the like. The thermally expandable fire-resistant materials expand when heated, and the resulting expansion residue forms a fire-resistant insulating layer, thereby exhibiting fire-resistant insulating performance, thereby preventing the occurrence of fires and the spread of fire when a fire occurs. As described in Patent Document 1, for example, a thermally expandable fire-resistant material containing a resin and a thermally expandable compound such as expandable graphite is widely used. The thermally expandable fire-resistant material is generally fixed to a building or the like via an adhesive layer laminated on the thermally expandable fire-resistant material.

[0003] In recent years, for the purpose of improving workability, attempts have been made to form a thermally expandable fireproof material on a workpiece by applying a thermally expandable fireproof material composition that is liquid at room temperature to the workpiece, such as a building fixture, and then curing the composition. In this case, it is known that the thermally expandable fireproof material composition contains, for example, a moisture-curing polymer, and the thermally expandable fireproof material composition is cured by being left in a room temperature environment (see, for example, Patent Documents 2 and 3).

[0004] JP 2020-45390 A International Publication No. 2022 / 097740 Patent No. 6825618 A

[0005] As described above, when a thermally expandable fireproof material is formed using a moisture-curable thermally expandable fireproof material composition, the thermally expandable fireproof material has a certain thickness, and therefore, it often takes a long time for the interior to harden. Therefore, after application, the thermally expandable fireproof material composition requires a long curing time, and a shelf for curing is required, which results in a problem of inefficient production.

[0006] Therefore, an object of the present invention is to provide a thermally expandable fire-resistant composition that can be cured to the inside in a short time, even if it is a moisture-curing type thermally expandable fire-resistant composition, thereby improving productivity, and a method for producing a thermally expandable fire-resistant material using the thermally expandable fire-resistant composition.

[0007] The gist of the present invention is as follows: [1] A thermally expandable fireproof composition containing a polymer having a moisture-curable functional group, a thermally expandable compound, and a curing catalyst, wherein the thermally expandable fireproof composition is applied to a thickness of 2 mm, and the resulting coating film has a deep curing time of 60 minutes or less under an environment of 50°C and 13% RH. [2] A thermally expandable fireproof composition containing a polymer having a moisture-curable functional group, a thermally expandable compound, and a curing catalyst, wherein the polymer comprises at least one polymer selected from the group consisting of a crosslinkable silyl group-containing polyoxyalkylene polymer having a branched structure and a silylated urethane. [3] A thermally expandable fireproof composition containing a polymer having a moisture-curable functional group, a thermally expandable compound, and a curing catalyst, further comprising an inorganic hydrate. [4] A thermally expandable fireproof composition containing a polymer having a moisture-curable functional group, a thermally expandable compound, and a curing catalyst, the thermally expandable fireproof composition comprising a first part containing the polymer and the curing catalyst, and a second part containing the polymer and water. [5] The thermally expandable fireproof composition according to any one of [1] to [4] above, wherein the polymer is a crosslinkable silyl group-containing polymer. [6] The thermally expandable fireproof composition according to any one of [1] and [3] to [5] above, wherein the polymer comprises at least one polymer selected from the group consisting of a crosslinkable silyl group-containing polyoxyalkylene polymer having a branched structure and a silylated urethane. [7] The thermally expandable fireproof composition according to any one of [1], [2], and [4] to [6] above, further comprising an inorganic hydrate. [8] The thermally expandable fireproof composition according to any one of [1] to [7] above, wherein the thermally expandable compound comprises thermally expandable graphite. [9] The thermally expandable fire-resistant composition according to the above item [8], wherein the thermally expandable compound further contains a foamable flame retardant.

[10] The thermally expandable fire-resistant composition according to any one of the above items [1] to [3] and [5] to [9], which comprises a combination of a first part containing the polymer and the curing catalyst and a second part containing the polymer and water.

[11] The thermally expandable fire-resistant composition according to any one of the above items [1] to

[10] , which has fluidity at room temperature.

[12] A thermally expandable fireproof material obtained by curing the thermally expandable fireproof material composition described in any one of [1] to

[11] above.

[13] A method for producing a thermally expandable fireproof material, comprising the steps of: applying or filling an article to be treated with the thermally expandable fireproof material composition described in any one of [1] to

[12] above; and moisture-curing the thermally expandable fireproof material composition applied to or filled on the article to be treated.

[14] A method for producing a thermally expandable fireproof material, comprising the steps of applying or filling an article to be treated with a thermally expandable fireproof material composition containing a polymer having a moisture-curable functional group, a thermally expandable compound, and a curing catalyst; and leaving the thermally expandable fireproof material composition applied to or filled on the article to be treated in an environment at a temperature of 50°C or higher and a humidity of 10% RH or higher to moisture-cure the thermally expandable fireproof material composition.

[0008] According to the present invention, it is possible to provide a thermally expandable fire-resistant composition that can be cured to the inside in a short time even if it is a moisture-curing type thermally expandable fire-resistant composition, thereby improving productivity, and a method for producing a thermally expandable fire-resistant material using the thermally expandable fire-resistant composition.

[0009] The present invention will be described in detail below using embodiments. <Thermal Expandable Fireproof Material Composition> A thermal expandable fireproof material composition according to one embodiment of the present invention contains a polymer having a moisture-curable functional group (hereinafter, sometimes simply referred to as "polymer (X)"), a thermal expandable compound, and a curing catalyst. Each component used in the thermal expandable fireproof material composition will be described in detail below.

[0010] <Polymer component having moisture-curable functional group> The thermally expandable fireproof material composition contains a polymer (X) having a moisture-curable functional group. By containing the polymer (X), the thermally expandable fireproof material composition can be imparted with moisture-curing properties. The polymer (X) is an adhesive component for exhibiting adhesiveness to an object to be applied. Examples of the moisture-curable functional group include a crosslinkable silyl group and an isocyanate group. Examples of the polymer (X) include a crosslinkable silyl group-containing polymer and an isocyanate group-containing polymer. The polymer (X) may be used alone or in combination of two or more types.

[0011] Among the above, a crosslinkable silyl group-containing polymer is preferred as the polymer (X). The crosslinkable silyl group in the crosslinkable silyl group-containing polymer is a moisture-curable functional group, specifically a functional group represented by the following formula (1). In the crosslinkable silyl group-containing polymer, the number of crosslinkable silyl groups per molecule is not particularly limited as long as there is one or more, but for example, about 1 to 5 crosslinkable silyl groups are preferred, and about 2 to 4 crosslinkable silyl groups are more preferred.

[0012] -SR 1 a X 3-a (1) In formula (1), R 1 is a hydrocarbon group, preferably an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, more preferably an alkyl group having 1 to 4 carbon atoms. X represents a reactive group, and the reactive group represented by X is a group selected from a halogen atom, a hydrogen atom, a hydroxyl group, an alkoxy group, an acyloxy group, a ketoximate group, an amide group, an acid amide group, a mercapto group, a ketoxime group, an alkenyloxy group, and an aminooxy group, and when there are multiple Xs, they may be the same group or different groups. Of these, X is preferably an alkoxy group or a ketoxime group, more preferably an alkoxy group. a is an integer of 0, 1, or 2, more preferably 0 or 1. The alkoxy group is preferably an alkoxy group having 1 to 4 carbon atoms, and specific examples thereof include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, a sec-butoxy group, and a tert-butoxy group. Of these, a methoxy group and an ethoxy group are preferred, and a methoxy group is most preferred.

[0013] Examples of crosslinkable silyl group-containing polymers include crosslinkable silyl group-containing polyoxyalkylene polymers, crosslinkable silyl group-containing acrylic polymers, crosslinkable silyl group-containing acrylic-modified polyoxyalkylene polymers, silylated urethanes, and crosslinkable silyl group-containing silicone resins. By using these polymers as polymer (X), the residual hardness and expansion ratio can be increased in a well-balanced manner. Furthermore, the weather resistance and other properties are good, making them suitable for outdoor use. Furthermore, the adhesive strength to various substrates is likely to be good.

[0014] The crosslinkable silyl group-containing polyoxyalkylene polymer is preferably a polymer containing a crosslinkable silyl group in the molecule and having a polyoxyalkylene in the main chain skeleton, and more preferably a polymer having a polyoxyalkylene in the main chain skeleton and having a crosslinkable silyl group at the end of the main chain. Here, examples of polyoxyalkylene include polyoxyethylene, polyoxypropylene, polyoxybutylene, polyoxytetramethylene, polyoxyethylene-polyoxypropylene copolymer, and polyoxypropylene-polyoxybutylene copolymer. Of these, polyoxypropylene is preferred.

[0015] The crosslinkable silyl group-containing polyoxyalkylene polymer may be linear or may have a branched structure. In the case of a linear structure, a polymer containing crosslinkable silyl groups at both ends of the main chain is more preferred. Furthermore, in the case of a branched structure, it is preferable to impart a branched structure to the polyoxyalkylene. Specifically, the polyoxyalkylene may be obtained by ring-opening polymerization of an alkylene oxide using a low-molecular-weight active hydrogen compound having three or more active hydrogens, such as a trihydric or higher polyhydric alcohol, as an initiator. The low-molecular-weight active hydrogen compound having three or more active hydrogens is not particularly limited, but triols such as glycerin and trimethylolpropane may be used. Even when the crosslinkable silyl group-containing polyoxyalkylene polymer has a branched structure, it is preferable that the crosslinkable silyl group be present at the molecular chain terminal. However, the branched structure of the polymer increases the number of molecular chain terminals, thereby increasing the number of crosslinkable silyl groups. Therefore, the crosslinkable silyl group-containing polyoxyalkylene polymer can have a branched structure, thereby increasing the curing rate.

[0016] The silylated urethane has a urethane bond (-NHCOO-) or a urea bond (-NHCONH-) in the molecule. The silylated urethane has a urethane bond or a urea bond, which improves the curing property and can improve the curing rate of the thermally expandable fireproof material composition. The silylated urethane contains a crosslinkable silyl group, and it is preferable that the crosslinkable silyl group is present, for example, at a terminal. The silylated urethane may have a polyoxyalkylene in its main chain skeleton. Specific examples of polyoxyalkylene are as described above, with polyoxypropylene being preferred. The silylated urethane may also have a urethane structure in its main chain skeleton formed by reacting an oxyalkylene glycol, such as oxypropylene glycol, with an isocyanate.

[0017] The crosslinkable silyl group-containing acrylic-modified polyoxyalkylene polymer is preferably a polymer containing a crosslinkable silyl group in the molecule and having a (meth)acrylic-modified polyoxyalkylene in the main chain skeleton, more preferably a polymer having a (meth)acrylic-modified polyoxyalkylene in the main chain skeleton and having a crosslinkable silyl group at the main chain terminal. The (meth)acrylic-modified polyoxyalkylene is preferably a (meth)acrylic-modified polyoxypropylene.

[0018] Examples of crosslinkable silyl group-containing acrylic polymers include polymers having an acrylic polymer in the main chain skeleton and one or more crosslinkable silyl groups in the molecule. Conventional acrylic polymers can be used here, and are not particularly limited as long as they are acrylic polymers obtained by polymerizing or copolymerizing one or more acrylic monomers selected from (meth)acrylic acid, (meth)acrylic acid esters, (meth)acrylonitrile, (meth)acrylamide, and the like. The acrylic polymer is preferably one whose main component is a (meth)acrylic acid ester monomer (e.g., 50% by mass or more, preferably 70% by mass or more of the polymer), and examples of the (meth)acrylic acid ester include those having approximately 4 to 20 carbon atoms. Furthermore, in addition to the above acrylic monomers, it is also possible to copolymerize the acrylic polymer with a monomer copolymerizable therewith. Examples of copolymerizable monomers include vinyl monomers such as fluoroolefins, α-olefins, vinyl esters, and vinyl ethers. The crosslinkable silyl group-containing acrylic polymer may have a crosslinkable silyl group at the terminal, or in a side chain, or may have a crosslinkable silyl group at both ends.

[0019] The crosslinkable silyl group-containing silicone resin is preferably a polymer having polyorganosiloxane in the main chain and having crosslinkable silyl groups at the terminals.

[0020] The number average molecular weight of polymer (X) is not particularly limited, but is, for example, 3,000 to 100,000, preferably 5,000 to 50,000, and more preferably 7,000 to 40,000. When the number average molecular weight of polymer (X) is a certain value or more, it is easy to improve the mechanical strength, etc. of the heat-expandable fireproof material composition after curing. On the other hand, when it is a certain value or less, it is easy to improve the fluidity, etc. of the heat-expandable fireproof material composition. The number average molecular weight is a value measured by GPC (gel permeation chromatography) using polystyrene equivalents. The same applies to the plasticizers described below.

[0021] Commercially available products can be used as the polymer (X). For example, crosslinkable silyl group-containing polyoxyalkylene polymers such as "MS Polymer S203" and "MS Polymer S303" manufactured by Kaneka Corporation can be used. Furthermore, crosslinkable silyl group-containing polyoxyalkylene polymers having a branched structure such as "Excestar S6250" manufactured by AGC can be used. Furthermore, silylated urethanes such as "SPUR3030" manufactured by Mentive Performance Materials Japan can be used. Furthermore, crosslinkable silyl group-containing acrylic polymers such as "US-6150" manufactured by Toagosei Co., Ltd. can be used. Furthermore, crosslinkable silyl group-containing silicone resins such as "Sekisui Silicone Sealant" manufactured by Sekisui Fuller Co., Ltd. can be used.

[0022] Among the above, the polymer (X) preferably contains at least one polymer (hereinafter sometimes referred to as polymer (X1)) selected from the group consisting of crosslinkable silyl group-containing polyoxyalkylene polymers having a branched structure and silylated urethanes. In the present invention, the use of polymer (X1) can increase the curing rate of the thermally expandable fireproof material composition, allowing rapid curing even in deep portions. The content of polymer (X1) in the thermally expandable fireproof material composition is, for example, 20 to 100 parts by mass, preferably 30 to 80 parts by mass, and more preferably 40 to 70 parts by mass, per 100 parts by mass of polymer (X). When the content of polymer (X1) is a certain amount or more, the composition becomes fast-curing, allowing rapid curing even in deep portions.

[0023] Furthermore, as the polymer (X), the polymer (X1) may be used alone, or a polymer other than the polymer (X1) (hereinafter, sometimes referred to as polymer (X2)) may be used in addition to the polymer (X1). The polymer (X2) is not particularly limited, but examples thereof include a crosslinkable silyl group-containing acrylic polymer and a linear crosslinkable silyl group-containing polyoxyalkylene polymer. The use of a crosslinkable silyl group-containing polyoxyalkylene polymer can impart greater flexibility, enabling it to follow the expansion and contraction of components due to temperature differences. Furthermore, the use of a crosslinkable silyl group-containing acrylic polymer can provide high weather resistance and reduce deterioration when used in locations exposed to ultraviolet light. The content of polymer (X2) in the thermally expandable fireproof material composition is, for example, 0 to 80 parts by mass, preferably 20 to 70 parts by mass, and more preferably 30 to 60 parts by mass per 100 parts by mass of polymer (X).

[0024] The content of polymer (X) is preferably 10 to 70% by mass, based on the total solid content of the thermally expandable fireproof material composition. By making the content of polymer (X) 10% by mass or more, the thermally expandable fireproof material obtained by curing the thermally expandable fireproof material composition can have good adhesion to the substrate. Furthermore, by making the content 70% by mass or less, it is possible to contain a certain amount or more of components other than polymer (X), such as a thermally expandable compound, and various performances such as fire resistance can be improved. From these viewpoints, the content of polymer (X) in the thermally expandable fireproof material composition is more preferably 15 to 50% by mass or more, and even more preferably 20 to 40% by mass or more.

[0025] <Thermal Expandable Compound> The thermal expandable compound is a compound that expands the thermal expandable fireproof material by expanding itself or by generating gas or the like when heated. When the thermal expandable fireproof material composition contains the thermal expandable compound, the thermal expandable fireproof material expands when heated to a temperature equal to or higher than the expansion initiation temperature of the thermal expandable compound, and the expansion residue forms a fire-resistant heat insulating layer. Examples of the thermal expandable compound include thermally expandable layered inorganic materials, foamable flame retardants, thermally expandable microcapsules, and thermal decomposition type foaming agents. The thermally expandable compounds may be used alone or in combination of two or more.

[0026] (Thermal Expandable Layered Inorganic Material) The thermal expandable layered inorganic material is a conventionally known material that expands upon heating, such as vermiculite and thermal expandable graphite, with thermal expandable graphite being preferred. The thermal expandable layered inorganic material may be used alone or in combination of two or more. The thermal expandable layered inorganic material may be in the form of particles or flakes. The thermal expandable layered inorganic material, particularly thermal expandable graphite, can increase the degree of expansion and form large-volume voids upon thermal expansion. Furthermore, the expansion initiation temperature can be adjusted to a temperature range suitable for a fire-resistant material. Furthermore, the residual hardness of the expansion residue can be easily increased, thereby improving the fire resistance and fire extinguishing performance of the fire-resistant material.

[0027] Thermally expandable graphite is a type of crystalline compound obtained by treating powders of natural flaky graphite, pyrolytic graphite, kish graphite, or the like with an inorganic acid and a strong oxidizing agent to produce a graphite intercalation compound, which maintains the layered structure of carbon. Examples of inorganic acids include concentrated sulfuric acid, nitric acid, and selenic acid. Examples of strong oxidizing agents include concentrated nitric acid, persulfates, perchloric acid, perchlorates, permanganates, dichromates, and hydrogen peroxide. The thermally expandable graphite obtained by the acid treatment described above may be further neutralized with ammonia, aliphatic lower amines, alkali metal compounds, alkaline earth metal compounds, or the like.

[0028] The particle size of the thermally expandable graphite is preferably 20 to 200 mesh. When the particle size of the thermally expandable graphite is within this range, it expands to easily create large-volume voids, thereby improving fire resistance. It also improves dispersibility in resins. The average aspect ratio of the thermally expandable graphite is preferably 2 or more, more preferably 5 or more, and even more preferably 10 or more. There is no particular upper limit to the average aspect ratio of the thermally expandable graphite, but from the viewpoint of preventing cracking of the thermally expandable graphite, it is preferably 1,000 or less. When the average aspect ratio of the thermally expandable graphite is 2 or more, it expands to easily create large-volume voids, thereby improving flame retardancy. The average aspect ratio of the thermally expandable graphite is determined by measuring the maximum dimension (major axis) and minimum dimension (minor axis) of each of 10 pieces of thermally expandable graphite, and then averaging the values ​​obtained by dividing the maximum dimension (major axis) by the minimum dimension (minor axis). The major axis and minor axis of the thermally expandable graphite can be measured using, for example, a field emission scanning electron microscope (FE-SEM).

[0029] (Intumescent flame retardant) Examples of intumescent flame retardants include phosphorus-containing compounds such as ammonium phosphate, ammonium polyphosphate, aluminum phosphite, and melamine polyphosphate. Intumescent flame retardants are flame retardants that can impart flame retardancy to thermally expandable fire-resistant materials, but also have the property of expanding themselves when heated. Intumescent flame retardants may be used alone or in combination of two or more. From the viewpoints of fire resistance and residue hardness, the intumescent flame retardant is preferably at least one selected from ammonium polyphosphate and aluminum phosphite.

[0030] (Thermal-Expandable Microcapsules) Thermally expandable microcapsules have a volatile substance, such as a low-boiling point solvent, encapsulated within a resin shell. When heated, the shell resin softens, causing the encapsulated volatile substance to volatilize or expand. The resulting pressure causes the shell to expand, increasing the particle size. The shell of the thermally expandable microcapsule is preferably formed from a thermoplastic resin. Examples of the thermoplastic resin include vinyl polymers such as ethylene, styrene, vinyl acetate, vinyl chloride, vinylidene chloride, acrylonitrile, butadiene, and chloroprene, copolymers thereof, polyamides such as nylon 6 and nylon 66, and polyesters such as polyethylene terephthalate. Among these, acrylonitrile copolymers are preferred because they are less permeable to the encapsulated volatile substance. The volatile substance encapsulated inside the thermally expandable microcapsules may be one or more low-boiling liquids selected from hydrocarbons having 3 to 7 carbon atoms, such as propane, propylene, butene, normal butane, isobutane, isopentane, neopentane, normal pentane, hexane, and heptane; methane halides, such as methyl chloride and methylene chloride; chlorofluorocarbons, such as CCl3F and CCl2F2; tetraalkylsilanes, such as tetramethylsilane and trimethylethylsilane; and petroleum ether. A suitable example of a thermally expandable microcapsule is a microcapsule having an outer shell resin made of a copolymer of acrylonitrile and vinylidene chloride, encapsulating a hydrocarbon having 3 to 7 carbon atoms, such as isobutane. The thermally expandable microcapsules may be used alone or in combination.

[0031] (Thermal Decomposition Type Foaming Agent) Examples of thermal decomposition foaming agents include compounds that foam upon heating and generate gas. The thermally expandable fireproof material composition is expanded by the generated gas. As the thermal decomposition foaming agent, organic or inorganic chemical foaming agents can be used. Examples of organic foaming agents include azo compounds such as azodicarbonamide, azodicarboxylic acid metal salts (e.g., barium azodicarboxylate), and azobisisobutyronitrile; nitroso compounds such as N,N'-dinitrosopentamethylenetetramine; hydrazine derivatives such as hydrazodicarbonamide, 4,4'-oxybis(benzenesulfonylhydrazide), and toluenesulfonylhydrazide; semicarbazide compounds such as toluenesulfonylsemicarbazide; melamine, dicyandiamide, and pentaerythritol. Examples of inorganic foaming agents include ammonium carbonate, sodium carbonate, ammonium bicarbonate, sodium bicarbonate, ammonium nitrite, sodium borohydride, and anhydrous monosodium citrate. Among these, from the viewpoints of obtaining fine bubbles and from the viewpoints of economy and safety, azo compounds and nitroso compounds are preferred, azodicarbonamide, azobisisobutyronitrile, and N,N'-dinitrosopentamethylenetetramine are more preferred, and azodicarbonamide is particularly preferred. The thermally decomposable foaming agents may be used alone or in combination of two or more. When thermally expandable microcapsules or a thermally decomposable foaming agent are used as the thermally expandable compound, it is preferable that the thermally expandable fire-resistant composition further contains at least one selected from an intumescent flame retardant and a flame retardant in order to impart appropriate fire resistance.

[0032] The expansion onset temperature of the thermally expandable compound is preferably 100 to 250°C. By setting the expansion onset temperature at or above the lower limit, it is possible to prevent the thermally expandable fire-resistant material from accidentally expanding except when a fire breaks out. Furthermore, by setting the temperature at or below 250°C, the material expands quickly when a fire breaks out, thereby improving fire resistance and fire extinguishing performance. From these perspectives, the expansion onset temperature is more preferably 125 to 200°C, even more preferably 150 to 195°C, and even more preferably 155 to 190°C. A preferred example of a thermally expandable compound having the above expansion onset temperature is thermally expandable graphite. Therefore, the expansion onset temperature of thermally expandable graphite is preferably 100 to 250°C, more preferably 125 to 200°C, even more preferably 150 to 195°C, and even more preferably 155 to 190°C.

[0033] When a thermally expandable fire-resistant composition contains two or more thermally expandable compounds, it is preferable that the expansion onset temperature of at least one of the thermally expandable compounds be within the above-mentioned range. It is preferable that the thermally expandable compound with the lowest expansion onset temperature be within the above-mentioned range. For example, when a thermally expandable compound contains thermally expandable graphite and an intumescent flame retardant, the expansion onset temperature of the thermally expandable graphite is lower than the expansion onset temperature of the intumescent flame retardant. Therefore, as described above, it is preferable that the expansion onset temperature of the thermally expandable graphite be within the above-mentioned range. As described below, the expansion onset temperature is determined by heating the thermally expandable compound using a rheometer and measuring the temperature at which a normal force rises. The measured temperature is used as the expansion onset temperature. While the expansion onset temperature of a thermally decomposable foaming agent is generally not detectable by the above-mentioned measurement method, it is preferable that the temperature at which the foaming agent decomposes and generates gas (decomposition temperature) be within the above-mentioned temperature range.

[0034] The content of the thermally expandable compound is preferably 10 to 80% by mass, based on the total solid content of the thermally expandable fireproof material composition. By incorporating the thermally expandable compound at or above the lower limit, the expansion ratio during combustion is sufficiently high, resulting in good fire resistance of the thermally expandable fireproof material. Furthermore, by incorporating the thermally expandable compound at or below the upper limit, it becomes possible to incorporate a certain amount of polymer (X) into the thermally expandable fireproof material composition, which facilitates the development of good adhesive properties. Furthermore, since the thermally expandable compound is more likely to be properly retained by the polymer (X) after curing, the mechanical strength of the thermally expandable fireproof material is also improved. The content of the thermally expandable compound in the thermally expandable fireproof material composition is more preferably 15 to 70% by mass, even more preferably 20 to 60% by mass, and even more preferably 25 to 55% by mass.

[0035] Among the above-mentioned thermally expandable compounds, it is preferable to use at least one of thermally expandable graphite and a foamable flame retardant. By using these, the thermally expandable compound imparts flame retardancy to the thermally expandable fire-resistant material, making it easier to improve fire resistance. Furthermore, it is more preferable to use at least thermally expandable graphite as the thermally expandable compound. By using thermally expandable graphite, it becomes easier to adjust the expansion start temperature to within the above range, and also to increase the expansion ratio and residual hardness.

[0036] The content of thermally expandable graphite is preferably 5 to 60 mass% based on the total solid content of the thermally expandable fireproof material composition. By incorporating thermally expandable graphite at or above the lower limit, the expansion ratio and residual hardness are likely to be increased, and the fire resistance performance of the thermally expandable fireproof material is improved. Furthermore, by incorporating the content at or below the upper limit, it becomes possible to incorporate a certain amount of components other than thermally expandable graphite, such as polymer (X) and a foamable flame retardant, into the thermally expandable fireproof material composition, making it easier to improve various performances. The content of thermally expandable graphite in the thermally expandable fireproof material composition is more preferably 7 to 50 mass%, even more preferably 10 to 40 mass%, and even more preferably 15 to 30 mass%, based on the total solid content.

[0037] Furthermore, from the viewpoint of fire resistance, it is also preferable to use a combination of thermally expandable graphite and an intumescent flame retardant as the thermally expandable compound. The content of the thermally expandable graphite when these are used in combination is as described above. On the other hand, the content of the intumescent flame retardant is preferably 3 to 70 mass% based on the total solid content of the thermally expandable fire-resistant material composition. By incorporating an intumescent flame retardant at or above the lower limit, it becomes easier to increase the expansion ratio and residual hardness, thereby improving the fire resistance performance of the thermally expandable fire-resistant material. Furthermore, by incorporating an intumescent flame retardant at or below the upper limit, it becomes possible to incorporate a certain amount of components other than the intumescent flame retardant, such as polymer (X) and thermally expandable graphite, into the thermally expandable fire-resistant material composition, thereby improving various performances. The content of the intumescent flame retardant is more preferably 5 to 50 mass%, even more preferably 8 to 40 mass%, and even more preferably 10 to 30 mass%.

[0038] When thermally expandable graphite and an intumescent flame retardant are used in combination, the mass ratio of the content of the intumescent flame retardant to the thermally expandable graphite in the thermally expandable fire-resistant material composition (intumescent flame retardant / thermally expandable graphite) is preferably 0.1 to 10. By setting the content ratio within the above range, it becomes easier to increase the expansion ratio and residual hardness, and the fire resistance performance of the thermally expandable fire-resistant material becomes good. From these viewpoints, the content ratio is more preferably 0.2 to 5, even more preferably 0.4 to 3, and even more preferably 0.5 to 2.

[0039] <Curing Catalyst> The thermally expandable fireproof material composition of the present invention further contains a curing catalyst. By including a curing catalyst in the thermally expandable fireproof material composition of the present invention, the curing reaction can be accelerated and the curing rate can be increased. Examples of the curing catalyst that can be used include titanium-based catalysts, tin-based catalysts, zirconium-based catalysts, aluminum-based catalysts, and bismuth-based catalysts, with tin-based catalysts being preferred among these. The content of the curing catalyst in the thermally expandable fireproof material composition is not particularly limited, but is, for example, 0.1 to 15 parts by mass, preferably 0.5 to 10 parts by mass, and more preferably 1 to 6 parts by mass per 100 parts by mass of the polymer (X).

[0040] (Inorganic Hydrate) The thermally expandable fireproof material composition of the present invention may contain an inorganic hydrate. Examples of inorganic hydrates include gypsum dihydrate and montmorillonite. When heated, the inorganic hydrate releases the water contained therein, and the released water causes the polymer (X) to react. Therefore, when the thermally expandable fireproof material composition contains an inorganic hydrate, moisture curing can be promoted by heating. As the inorganic hydrate, gypsum dihydrate is preferred because it easily releases water and is inexpensive.

[0041] The content of the inorganic hydrate in the thermally expandable fireproof material composition is, for example, 1 to 50 parts by mass relative to 100 parts by mass of the polymer (X). By setting the content of the inorganic hydrate to 1 part by mass, the curing-accelerating effect of the inorganic hydrate can be sufficiently obtained. Furthermore, by setting the content to 50 parts by mass or less, an effect commensurate with the content can be obtained. The content of the inorganic hydrate is preferably 5 to 40 parts by mass, more preferably 10 to 30 parts by mass.

[0042] (Inorganic Filler) The thermally expandable refractory composition of the present invention may contain an inorganic filler other than the thermally expandable compound and inorganic hydrate described above. When heated to form an expandable insulating layer, the inorganic filler increases the heat capacity, suppresses heat transfer, and acts as an aggregate to improve the strength of the expansion residue. The inorganic filler that can be used in the present invention is not particularly limited, and examples thereof include metal oxides such as alumina, zinc oxide, titanium oxide, calcium oxide, magnesium oxide, iron oxide, tin oxide, antimony oxide, and ferrite; metal carbonates such as calcium carbonate, zinc carbonate, strontium carbonate, and barium carbonate; metal hydroxides such as calcium hydroxide, magnesium hydroxide, aluminum hydroxide, and hydrotalcite; calcium sulfate, gypsum fiber, calcium salts such as calcium silicate; silica, diatomaceous earth, dawsonite, barium sulfate, talc, clay, mica, bentonite, activated clay, and sepiolite. Examples of inorganic fillers include imogolite, sericite, glass fibers, glass beads, silica-based balloons, aluminum nitride, boron nitride, silicon nitride, carbon black, graphite, carbon fibers, carbon balloons, various metal powders, potassium titanate, magnesium sulfate, lead zirconate titanate, aluminum borate, molybdenum sulfide, silicon carbide, stainless steel fibers, zinc borate, various magnetic powders, slag fibers, fly ash, metal phosphates such as sodium phosphate, potassium phosphate, magnesium phosphate, and aluminum phosphate, metal orthophosphates, metal metaphosphates, and metal tripolyphosphates. The inorganic fillers may be used alone or in combination of two or more. Among these, calcium carbonate, barium sulfate, aluminum hydroxide, and the like are preferred from the viewpoint of improving the fire resistance of the thermally expandable refractory material, and calcium carbonate is more preferred. The inorganic fillers may be used alone or in combination of two or more. When the thermally expandable fireproof material composition contains an inorganic filler, the content thereof is preferably 1 to 50 mass %, more preferably 5 to 45 mass %, and even more preferably 10 to 40 mass %, based on the total solid content of the thermally expandable fireproof material composition.

[0043] (Thermoplastic Resin) The thermally expandable fireproof material composition may contain a thermoplastic resin. By containing a thermoplastic resin, the thermally expandable fireproof material composition is likely to have increased mechanical strength after combustion and high residue hardness. In addition, it is possible to improve adhesion to the substrate, and it is likely to maintain good adhesion to the substrate even after combustion. As the thermoplastic resin, ethylene-vinyl acetate copolymer resin (EVA) and ethylene-(meth)acrylic acid ester copolymer resin can be preferably used. The thermoplastic resin may be used alone or in combination of two or more types. Of these, ethylene-vinyl acetate copolymer resin (EVA) is more preferred as the thermoplastic resin.

[0044] The ethylene-vinyl acetate copolymer resin (EVA) is not particularly limited as long as it is a resin obtained by copolymerizing ethylene and vinyl acetate. The vinyl acetate content of the ethylene-vinyl acetate copolymer resin is not particularly limited, but from the viewpoint of improving adhesiveness, residual hardness, etc., it is preferably 15 to 45 mass%, more preferably 20 to 40 mass%, and even more preferably 25 to 35 mass%. The vinyl acetate content is measured in accordance with JIS K 6924-1:1997.

[0045] The melt flow rate (MFR) of the thermoplastic resin is not particularly limited, but from the viewpoint of coatability, adhesiveness, etc., it is, for example, 1 to 3,000 g / 10 min, preferably 5 to 2,500 g / 10 min, more preferably 10 to 1,500 g / 10 min, even more preferably 100 to 1,000 g / 10 min, and even more preferably 150 to 1,000 g / min. The melt flow rate is measured under conditions of 190°C and a load of 21.2 N, and for ethylene-vinyl acetate copolymer resins, it is preferably measured in accordance with JIS K 6924-1:1997. For thermoplastic resins other than ethylene-vinyl acetate copolymer resins, such as ethylene-(meth)acrylic acid ester copolymer resins, it is preferably measured in accordance with JIS K 7210:1999.

[0046] (Plasticizer) The thermally expandable fireproof material composition may contain a plasticizer. Use of a plasticizer tends to improve the fluidity of the thermally expandable fireproof material composition. Examples of plasticizers include phthalate esters such as dimethyl phthalate, diethyl phthalate, dibutyl phthalate, diisobutyl phthalate, dihexyl phthalate, bis(2-ethylhexyl) phthalate, dioctyl phthalate, diisononyl phthalate, dinonyl phthalate, diisodecyl phthalate, diisoundecyl phthalate, and bisbutylbenzyl phthalate; and polyalkylene glycols such as diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, and polypropylene glycol. Among these, polyalkylene glycols are preferred, and polypropylene glycol is more preferred. The plasticizer is preferably a component that is liquid at room temperature.

[0047] When the plasticizer is a polyalkylene glycol, its number-average molecular weight is preferably 1,000 to 10,000, more preferably 1,500 to 5,000, and even more preferably 2,000 to 4,000. When the number-average molecular weight of the polyalkylene glycol used as the plasticizer is within the above range, the flowability and coatability of the thermally expandable fireproof material composition are ensured, while the mechanical properties after curing are also likely to be good. The content of the plasticizer in the thermally expandable fireproof material composition is preferably 5 to 100 parts by mass, more preferably 20 to 80 parts by mass, even more preferably 35 to 75 parts by mass, and even more preferably 45 to 70 parts by mass, per 100 parts by mass of the polymer (X).

[0048] (Dehydrating Agent) The thermally expandable fireproof material composition may further contain a dehydrating agent. By containing a dehydrating agent, the thermally expandable fireproof material composition can be prevented from hardening due to moisture contained in the air or the like during storage. Examples of dehydrating agents include silane compounds such as vinyltrimethoxysilane, dimethyldimethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, tetramethoxysilane, phenyltrimethoxysilane, and diphenyldimethoxysilane, and ester compounds such as methyl orthoformate, ethyl orthoformate, methyl orthoacetate, and ethyl orthoacetate. These dehydrating agents may be used alone or in combination of two or more. Of these, vinyltrimethoxysilane is preferred. The content of the dehydrating agent is preferably 0.2 to 15 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 1 to 8 parts by mass, per 100 parts by mass of polymer (X).

[0049] (Coupling Agent) The thermally expandable fireproof material composition of the present invention may contain a coupling agent. By containing a coupling agent, the adhesive strength of the thermally expandable fireproof material composition to the substrate can be easily increased. Examples of the coupling agent include silane coupling agents and titanium coupling agents, with silane coupling agents being preferred. As the silane coupling agent, any known agent can be used without particular limitation, with aminosilane coupling agents being preferred. The aminosilane coupling agent contains a silicon atom to which an alkoxy group is bonded and a functional group containing a nitrogen atom in one molecule. By using an aminosilane coupling agent, the adhesive strength of the thermally expandable fireproof material composition can be easily improved. Specific examples of aminosilane coupling agents include 3-aminopropyltrimethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N,N'-bis-[3-(trimethoxysilyl)propyl]ethylenediamine, N,N'-bis-[3-(triethoxysilyl)propyl]ethylenediamine, N,N'-bis-[3-(methyldimethoxysilyl)propyl]ethylenediamine, N,N'-bis-[3-(trimethoxysilyl)propyl]hexamethylenediamine, and N,N'-bis-[3-(triethoxysilyl)propyl]hexamethylenediamine. The silane coupling agents may be used alone or in combination of two or more. The content of the silane coupling agent is preferably from 0.2 to 15 parts by mass, more preferably from 0.5 to 10 parts by mass, and even more preferably from 1 to 8 parts by mass, relative to 100 parts by mass of the polymer (X).

[0050] (Flame Retardant) The thermally expandable fire-resistant material composition of the present invention may contain a flame retardant other than the intumescent flame retardant described above. Examples of such a flame retardant include a phosphate ester compound. Examples of the phosphate ester compound include trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, octyl diphenyl phosphate, tributoxyethyl phosphate, trichloroethyl phosphate, tris(2-chloropropyl)phosphate, tris(2,3-dichloropropyl)phosphate, tris(2,3-dibromopropyl)phosphate, tris(bromochloropropyl)phosphate, bis(2,3-dibromopropyl)-2,3-dichloropropyl phosphate, bis(chloropropyl)monoctyl phosphate, tris(2-ethylhexyl)phosphate, triphenyl phosphate, tricresyl phosphate (TCP), trixylenyl phosphate, cresyl diphenyl phosphate, and xylenyl diphenyl phosphate.

[0051] The thermally expandable fireproof material composition of the present invention may contain additives other than those described above, as necessary, within the scope of not impairing the object of the present invention. Examples of such additives include lubricants, anti-shrinkage agents, crystal nucleating agents, colorants (pigments, dyes, etc.), ultraviolet absorbers, antioxidants, antiaging agents, flame retardant aids, antistatic agents, surfactants, vulcanizing agents, dispersants, and surface treatment agents. The additives may be used alone or in combination of two or more.

[0052] (Method for producing the thermally expandable fireproof composition) The thermally expandable fireproof composition of the present invention can be obtained by mixing the polymer (X), the thermally expandable compound, the curing catalyst, and other additives, such as inorganic hydrates, inorganic fillers, thermoplastic resins, plasticizers, dehydrating agents, coupling agents, flame retardants, and other additives, which are added as needed. The components may be mixed in a sealed mixer under reduced pressure until the mixture is homogeneous.

[0053] The thermally expandable fireproof composition of the present invention may be a one-component type or a two-component type. When it is a one-component type, the thermally expandable fireproof composition obtained by mixing the above components is preferably stored in a sealed container or the like to prevent contact with moisture. When used, it is preferably taken out of the sealed container and applied to or filled into an object to be treated.

[0054] (Two-component type) In the case of a two-component type, the thermally expandable fireproof composition is preferably divided into a first component and a second component, and the first component and the second component are mixed at the time of use to obtain the thermally expandable fireproof composition. In a two-component type thermally expandable fireproof composition, the mass ratio of the first component to the second component (second component / first component) is preferably 1 or close to 1, preferably 0.8 to 1.2, more preferably 0.9 to 1.1, and even more preferably 0.95 to 1.05. In this way, by setting the mass ratio of the first component to the second component to a value close to 1, the preparation of the thermally expandable fireproof composition becomes easier.

[0055] In a two-component thermally expandable fireproof composition, it is preferable to include a curing catalyst in the first component and water in the second component. This prevents the first and second components from reacting before mixing, but after mixing, the presence of both water and the curing catalyst in the thermally expandable fireproof composition allows the reaction of polymer (X) to proceed immediately. This allows the thermally expandable fireproof composition to cure at a rapid curing rate. The amount of water in the thermally expandable fireproof composition is, for example, 0.1 to 8 parts by mass, preferably 0.2 to 5 parts by mass, and more preferably 0.4 to 3 parts by mass, per 100 parts by mass of polymer (X) contained in the entire thermally expandable fireproof composition. By limiting the water content to 0.1 parts by mass, the water can adequately promote the curing reaction when the first and second components are mixed. Furthermore, by limiting the amount of water to 8 parts by mass or less, it is possible to prevent unnecessary side reactions caused by water.

[0056] In a two-component thermally expandable fireproof material composition, it is preferable that the first component contains a polymer (X) in addition to the curing catalyst, and the second component contains a polymer (X) in addition to water. By containing the polymer (X) in both the first and second components, both the first and second components can be made to flow at room temperature. However, it is preferable that the first component does not contain water and the second component does not contain a curing catalyst. This configuration prevents the coexistence of the polymer (X), water, and curing catalyst in both the first and second components, and prevents curing before mixing.

[0057] Furthermore, each component other than the polymer (X), water, and curing catalyst may be appropriately contained in each of the first and second agents, but it is preferable that both the first and second agents contain a thermally expandable compound. Furthermore, when an inorganic filler is used, it is also preferable that both the first and second agents contain the inorganic filler. Similarly, when a plasticizer is used, it is also preferable that both the first and second agents contain the plasticizer. Furthermore, when a thermoplastic resin is used, it is also preferable that both the first and second agents contain the thermoplastic resin. By separately blending each component into the first and second agents, it becomes easier to achieve a mixing ratio close to 1 when mixing the first and second agents.

[0058] Among the above, the thermally expandable fireproof material composition according to one embodiment of the present invention is preferably any one of the following aspects (1) to (3) from the viewpoint of being able to increase the curing rate and cure to the interior in a short time, even though it is a moisture-curable thermally expandable fireproof material composition. (1) The polymer having a moisture-curable functional group (polymer (X)) contains at least one polymer selected from the group consisting of a crosslinkable silyl group-containing polyoxyalkylene polymer having a branched structure and a silylated urethane. (2) The thermally expandable fireproof material composition further contains an inorganic hydrate. (3) The thermally expandable fireproof material composition is composed of a combination of a first part containing polymer (X) and a curing catalyst and a second part containing polymer (X) and water.

[0059] <Curability> In a thermally expandable fireproof composition according to one embodiment of the present invention, a coating film obtained by applying the thermally expandable fireproof composition to a thickness of 2 mm has a deep curing time of 60 minutes or less under an environment of 50°C and 13% RH. A deep curing time of 60 minutes or less allows the thermally expandable fireproof composition to be sufficiently cured to the interior in a short time when applied to or filled on an object and then cured to form a thermally expandable fireproof material. Therefore, subsequent work can be carried out promptly after application or filling, thereby improving productivity. The deep curing time is preferably 55 minutes or less, more preferably 50 minutes or less, even more preferably 45 minutes or less, and even more preferably 40 minutes or less. The shorter the deep curing time, the better; for example, 5 minutes or more is sufficient, but 10 minutes or more is also acceptable from the viewpoint of ensuring a certain usable time. As shown in the Examples below, the deep curing time is determined by placing a specific weight on a 2 mm thick coating film for 5 seconds every 5 minutes, and judging whether or not curing has progressed deep into the coating based on whether or not a mark of the weight remains when the weight is removed. The deep curing time is the first time when no mark of the weight remains.

[0060] In the present invention, the deep curing time can be shortened as described above by appropriately adjusting the components blended into the thermally expandable refractory composition. Specifically, by using polymer (X1) as polymer (X), the thermally expandable refractory composition can be fast-cured and cured to a deep portion in a short curing time. Furthermore, by adjusting the content of polymer (X1) to a certain amount or more as described above, the deep curing time can be further shortened. Furthermore, by adding an inorganic hydrate, particularly gypsum dihydrate, to the thermally expandable refractory composition, the thermally expandable refractory composition can be fast-cured and cured to a deep portion in a short curing time. In this case, too, by adjusting the content of inorganic hydrate, particularly gypsum dihydrate, to a certain amount or more as described above, the deep curing time can be further shortened. Furthermore, by making the thermally expandable refractory composition a two-component type and adding water to the second part, the thermally expandable refractory composition can be fast-cured and cured to a deep portion in a short curing time. In this case as well, by setting the water content to a certain amount or more as described above, it becomes easier to further shorten the deep curing time.

[0061] Furthermore, the thermally expandable fireproof composition of the present invention preferably has a surface curing time of 40 minutes or less, more preferably 30 minutes or less, even more preferably 25 minutes or less, and even more preferably 20 minutes or less, under an environment of 23°C and 50% RH for a coating film obtained by applying the thermally expandable fireproof composition to a thickness of 2 mm. By shortening the surface curing time as well as the deep curing time, productivity can be further improved. The shorter the surface curing time, the better, for example, 5 minutes or more is sufficient, but from the viewpoint of ensuring a certain usable time, it may also be 10 minutes or more. As shown in the examples described below, the surface curing time is determined by touching the surface of a formed 2 mm thick coating film with a spatula every 5 minutes and determining whether the thermally expandable fireproof composition adheres to the spatula, and the shortest time at which the thermally expandable fireproof composition does not adhere to the spatula is defined as the surface curing time.

[0062] <Flowability> The thermally expandable fireproof material composition preferably has flowability at room temperature (23°C). Since the thermally expandable fireproof material composition has flowability at room temperature (23°C), it can be easily applied to an object to be applied, such as a building, by coating, filling, etc. On the other hand, after curing, the thermally expandable fireproof material composition can be adhered to an object to be applied with good adhesiveness by being applied by coating or the like and then cured.

[0063] The viscosity of the thermally expandable fireproof material composition at 23°C is preferably 1,000,000 mPa·s or less, more preferably 750,000 mPa·s or less, and even more preferably 500,000 mPa·s or less. When the viscosity at 23°C is below these upper limit values, the thermally expandable fireproof material composition can be applied to the substrate with good applicability, thereby improving workability. Furthermore, the viscosity of the thermally expandable fireproof material composition at 23°C is not particularly limited, but from the viewpoint of preventing dripping when applying the composition, it is, for example, 400 mPa·s or more, preferably 4,000 mPa·s or more, more preferably 10,000 mPa·s or more, and even more preferably 50,000 mPa·s or more.

[0064] <Thermal-Expandable Fireproof Material> The thermally expandable fireproof material of the present invention is obtained by curing the thermally expandable fireproof material composition described above. The thermally expandable fireproof material of the present invention is preferably obtained by applying the thermally expandable fireproof material composition described above to an object to be treated and then curing the composition, and is preferably formed into a film on the object to be treated. The thermally expandable fireproof material may also be obtained by filling gaps in the object to be treated and curing the filled thermally expandable fireproof material composition. Examples of the object to be treated include components having a hollow portion therein, such as square pipes and sash frames, and the thermally expandable fireproof material composition may be filled into the hollow portion. The size of the thermally expandable fireproof material filled into the gaps in the object to be treated is not particularly limited, and it is preferably a size appropriate for the gap.

[0065] The thickness of the thermally expandable fireproof material formed on the object to be treated by coating or filling is, for example, 0.1 to 50 mm, preferably 0.5 to 30 mm, more preferably 1 to 20 mm, and even more preferably 2 to 10 mm. Furthermore, among the above, the thickness of the thermally expandable fireproof material formed in the form of a film on the object to be treated by coating is relatively thin and is not particularly limited, but is, for example, 0.1 to 20 mm, preferably 0.5 to 15 mm, more preferably 1 to 10 mm, and even more preferably 1.5 to 5 mm.

[0066] The thermally expandable fireproof material of the present invention has a volume expansion ratio of 10 times or more when heated at 600°C for 10 minutes, and a residual hardness of 0.1 kgf / cm 2 It is preferable that the thermally expandable fireproof material has a volume expansion ratio and residual hardness that are equal to or greater than the above lower limit values, thereby enabling the material to have good fire resistance. The volume expansion ratio is more preferably 20 times or greater, and even more preferably 30 times or greater. The upper limit of the volume expansion ratio is not particularly limited, but is, for example, 150 times, preferably 100 times, from the viewpoint of ensuring that the expansion residual hardness is at least a certain value. The residual hardness is more preferably 0.15 kgf / cm 2 More preferably, 0.25 kgf / cm 2 More preferably, it is 0.3 kgf / cm 2 The upper limit of the residual hardness is not particularly limited, but is, for example, 1.5 kgf / cm 2The volume expansion ratio and residual hardness can be measured by the measurement methods described in the examples below.

[0067] <Method for producing a thermally expandable fireproof material> A method for producing a thermally expandable fireproof material according to one embodiment of the present invention includes the following steps A and B. Step A: applying or filling a thermally expandable fireproof material composition onto an object to be treated, and Step B: moisture-curing the thermally expandable fireproof material composition applied to or filled onto the object to be treated. Each step will be described below.

[0068] (Step A) In step A, the method for applying the thermally expandable refractory composition to the workpiece is not particularly limited, and examples include a method of applying the thermally expandable refractory composition to the workpiece using a caulking gun or a known coating device, and a method of applying the thermally expandable refractory composition to the workpiece by spraying. Furthermore, in step A, if the workpiece has gaps or other gaps that can be filled with the thermally expandable refractory composition, the workpiece may be filled with the thermally expandable refractory composition. In the present invention, as described above, the thermally expandable refractory composition has fluidity at room temperature, so that the thermally expandable refractory composition can be easily applied to or filled into the workpiece at a temperature near room temperature (e.g., about 5 to 40°C). However, the thermally expandable refractory composition may be applied or filled after being appropriately heated.

[0069] (Step B) Step B is a step of curing the heat-expandable fireproof composition applied to or filled on an object to be treated. The curing method is not particularly limited as long as the heat-expandable fireproof composition is moisture-curable. For example, the heat-expandable fireproof composition (i.e., the object to be treated to which the heat-expandable fireproof composition has been applied or filled) can be left in an environment of around room temperature (e.g., about 5 to 40°C) in the atmosphere to moisture-cure the heat-expandable fireproof composition. The time for which the heat-expandable fireproof composition is left is not particularly limited, but is, for example, about 10 to 1,440 minutes, preferably 20 to 720 minutes, and more preferably about 30 to 360 minutes.

[0070] However, the thermally expandable fireproof material composition applied to or filled on the object to be treated may be heated as necessary, for example, to a temperature of 40° C. or higher, or to a temperature of 50° C. or higher. The upper limit of the temperature is not particularly limited, but is, for example, 90° C., preferably 80° C. The polymer (X) can be cured more quickly and deeply by being cured by heating than by being cured at around room temperature.

[0071] Alternatively, the thermally expandable fireproof composition (i.e., an object to which the thermally expandable fireproof composition has been applied or filled) may be left in a humidity-controlled high-humidity environment to moisture-cure the thermally expandable fireproof composition. The polymer (X) can be cured more quickly to a deep portion by being placed in a high-humidity environment than by moisture-cure in the atmosphere. Specifically, the humidity may be adjusted to, for example, 10% RH or higher, 40% RH or higher, 50% RH or higher, or 60% RH or higher. The upper limit of the humidity is not particularly limited, but may be, for example, 90% RH or lower, and preferably 80% RH or lower.

[0072] (Preferred embodiment) A method for producing a thermally expandable fireproof material according to a preferred embodiment of the present invention comprises sequentially carrying out the following steps A1 and A2: A1: applying or filling a thermally expandable fireproof composition onto an object to be coated; and A2: leaving the thermally expandable fireproof composition applied or filled onto the object to be coated in an environment at a temperature of 50°C or higher and a humidity of 10% RH or higher to moisture-cure the thermally expandable fireproof composition.

[0073] In the manufacturing method according to this embodiment, step A1 is the same as step A described above, and in step A1, as in step A, the heat-expandable fireproof material composition may be applied to or filled into the object to be coated.

[0074] In step B2, the heat-expandable fireproof composition applied to or filled on the object to be treated is moisture-cured, as in step B described above, but in step B2, the heat-expandable fireproof composition is left to stand in an environment at a temperature of 50° C. or higher and a humidity of 10% RH or higher to perform moisture curing. As described above, in step B2, by moisture-curing the heat-expandable fireproof composition under high temperature and high humidity, the heat-expandable fireproof composition can be rapidly cured, and it becomes possible to cure the heat-expandable fireproof composition deep within in a short period of time.

[0075] The upper limit of the temperature is not particularly limited, but is, for example, 90°C, preferably 80°C, and more preferably 70°C. By setting the temperature in step B2 at or below these upper limits, rapid curing is possible without using extra energy and without causing deterioration of the workpiece due to heating or dripping of the thermally expandable fireproof composition. Furthermore, the humidity is preferably 13% RH or higher. The upper limit of the humidity is not particularly limited, but is, for example, 90% RH, preferably 80% RH, and more preferably 70% RH. By setting the humidity in step B2 at or below these upper limits, rapid curing is possible without using extra energy and without causing deterioration of the thermally expandable fireproof composition or the workpiece due to moisture. The time for which the thermally expandable fireproof composition is left at the above temperature and humidity is not particularly limited, but is, for example, about 10 to 180 minutes, preferably 20 to 120 minutes, and more preferably 25 to 80 minutes.

[0076] The heat-expandable fireproof composition used in the manufacturing method of this embodiment is as described above, and a detailed description thereof will be omitted. However, the deep curing time of the heat-expandable fireproof composition does not necessarily have to be 60 minutes or less and may be longer than 60 minutes. Even if the deep curing time is longer than 60 minutes, rapid curing of the heat-expandable fireproof composition is possible by moisture-curing the heat-expandable fireproof composition at high temperatures as described above, making it possible to cure the heat-expandable fireproof composition to its deep portions in a short time. Of course, in this embodiment, to achieve faster curing, the deep curing time of the heat-expandable fireproof composition may be 60 minutes or less, as described above, and may be preferably 55 minutes or less, more preferably 50 minutes or less, even more preferably 45 minutes or less, and even more preferably 40 minutes or less. It should be noted that the above manufacturing method can also be said to produce a fire-resistant object to be applied, comprising an object to be applied and a heat-expandable fireproof material formed on the object to be applied.

[0077] <Uses> The thermally expandable fireproof material composition and thermally expandable fireproof material of the present invention can be used in various buildings such as detached houses, apartment buildings, high-rise houses, skyscrapers, commercial facilities, public facilities, etc., various vehicles such as automobiles and trains, ships, aircraft, electronic devices, etc. For example, in buildings, the composition can be applied to fittings such as windows, shoji screens, doors, sliding doors, and sliding screens, as well as building materials other than fittings such as walls, beams, pillars, floors, bricks, roofs, boards, piping, and wiring. For example, in fittings, the thermally expandable fireproof material composition can be applied to a sash and cured to form a fire-resistant sash having the thermally expandable fireproof material.

[0078] In addition, in buildings, the composition can be used as a fire-resistant filler or a fire-resistant, watertight filler by filling gaps formed in walls, ceilings, floors, etc. More specifically, the composition can be used as a fire-resistant filler or a fire-resistant, watertight filler by filling gaps in penetrations (e.g., compartment penetrations) for inserting piping or wiring in walls, ceilings, floors, etc. Furthermore, the composition can be filled into the interior of a frame material such as a sash frame that constitutes a building fixture, or the interior of a square pipe that constitutes a pillar, beam, etc., and then cured to form a building fixture, pillar, beam, etc. having a heat-expandable fireproof material. Furthermore, the composition can be used as a fire-resistant joint material by applying it to the exterior wall of a building or filling gaps in the exterior wall.

[0079] The thermally expandable fire-resistant material composition of the present invention can be used in battery cases, electronic devices such as smartphones, etc. by applying it to the surface of a battery case for a lithium ion battery or the like, or to a cover material for the electronic device, or by filling gaps in the battery case, gaps inside the electronic device, etc. When used in electronic devices, the thermally expandable fire-resistant material composition of the present invention can prevent the occurrence of fires and the like even if a battery such as a lithium ion battery experiences thermal runaway.

[0080] The thermally expandable fireproof material composition of the present invention can also be used as an adhesive to bond various components in various buildings, various vehicles such as automobiles and trains, ships, aircraft, electronic devices, etc. It can also be used as a packing to seal between components in various buildings, various vehicles such as automobiles and trains, ships, aircraft, electronic devices, etc. In particular, when used as an adhesive or packing around batteries such as lithium ion batteries in electric vehicles or electronic devices such as smartphones, it is effective in suppressing fires that occur when batteries such as lithium ion batteries experience thermal runaway. Furthermore, in ships, it can be used as an adhesive or watertight material for fire-resistant and restricted areas of ships. Among the above, the thermally expandable fireproof material composition of the present invention is more preferably used for building materials.

[0081] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0082] The components used in the examples and comparative examples are as follows. <Polymer (X)> Si-containing PPG polymer: "MS Polymer S303", manufactured by Kaneka Corporation, a polyalkylene oxide having a main chain skeleton composed of polypropylene oxide and a propyldimethoxysilyl group at the end of the main chain, linear, number average molecular weight: 20,000 Si-containing acrylic polymer: an acrylic polymer having a trimethoxysilyl group at the end of the main chain skeleton or at a side chain, manufactured by Toagosei Co., Ltd., product name "US-6150", weight average molecular weight: 7,000 Branched Si-containing PPG polymer: manufactured by AGC, product name "Excestar S6250", a polyoxypropylene polymer having a main chain composed of polyoxypropylene and a branched structure in the main chain, a dimethoxysilyl group at the end of the main chain, number of dimethoxysilyl groups = 3, number average molecular weight: 8,000 Silylated urethane: "SPUR3030", manufactured by Mentive Performance Materials Japan, a silylated urethane with a polypropylene oxide main chain skeleton, a urethane bond or urea bond in the main chain skeleton, and trimethoxysilyl groups at both ends of the main chain. Number average molecular weight: 22,300

[0083] <Thermal expansion compounds> Thermal expansion graphite: "EXP42S160", manufactured by Fuji Graphite Co., Ltd., expansion start temperature 160°C Aluminum phosphite: "APA100", manufactured by Taihei Chemical Co., Ltd.

[0084] ・Dihydrate gypsum: "Calcium sulfate A", manufactured by Yoshino Gypsum Co., Ltd. ・Calcium carbonate: "BF300", manufactured by Bihoku Funka Co., Ltd. ・EVA: ethylene-vinyl acetate copolymer resin, hot melt adhesive base, "Ultrathene 726", manufactured by Tosoh Corporation, vinyl acetate content 33% by mass, melt flow rate 700 g / 10 min (190 ° C, load 21.2 N) ・Plasticizer: "Exenol 3020", polyether plasticizer (polypropylene glycol), manufactured by AGC, number average molecular weight 3200 ・Curing catalyst: dibutyltin compound, "Neostan U220H", manufactured by Nitto Kasei Co., Ltd. ・Dehydrating agent: "KBM-1003", manufactured by Shin-Etsu Chemical Co., Ltd., vinyltrimethoxysilane ・Coupling agent: "KBM-603", N-(2-aminoethyl)-3-aminopropyltrimethoxysilane ・Water

[0085] (Experimental Examples 1 to 5, Experimental Examples 7 to 9) Each component according to the formulation in Table 1 was mixed using a planetary mixer under vacuum for 60 minutes until uniform, thereby obtaining a one-component thermally expandable fire-resistant composition.

[0086] (Experimental Examples 6 and 10) The first and second parts were obtained by mixing the components according to the formulations in Table 1 under a vacuum atmosphere for 60 minutes using a planetary mixer until they were uniform. The first and second parts were mixed immediately before the measurement and evaluation of the physical properties to obtain thermally expandable fire-resistant compositions.

[0087] The measurement and evaluation methods for each physical property are as follows: [Evaluation Method] (Expansion Start Temperature of Thermally Expandable Graphite) 100 mg of thermally expandable graphite was taken as a sample, and the temperature was increased at a rate of 10°C / min using a rheometer ("Discovery HR2" manufactured by TA Instruments) to measure the temperature at which the force in the normal direction rose, and this was taken as the expansion start temperature.

[0088] (Viscosity) The viscosity of the thermally expandable fireproof material at 23° C. is a value measured in accordance with JIS K6833 using a B-type viscometer at a rotation speed of 10 rpm.

[0089] (Deep Cure Time) In an atmosphere of 23°C and 50% RH, a thermally expandable fireproof composition sealed in a paper cartridge was extruded from a caulking gun onto a metal plate (material: SUS) to a coating thickness of 2 mm. Immediately after application (1 second later), and also after application, the coating was left in an environment of 50°C and 13% RH. A cylindrical metal weight (weighing 500 g) with a diameter of 2 cm was placed on the coating for 5 seconds, and every 5 minutes after application. The deep cure time was determined as the first time that the weight left no trace of its shape when removed. The weight was placed in a different position each time.

[0090] (Surface curing time) Under the same conditions as for the deep curing time, the heat-expandable fireproof composition was applied to a thickness of 2 mm. Immediately after application (after 1 second) and after application, the coating was left in an environment of a temperature of 23°C and a humidity of 50% RH, and the surface of the coating film was touched with a metal spatula every 5 minutes after application, and the time until the heat-expandable fireproof composition no longer adhered to the spatula was measured as the surface curing time.

[0091] (Fire Resistance Test) The heat-expandable fireproof material composition obtained in each example was applied to a 98 mm square iron plate at 23°C in a 30 mm square area, and the heat-expandable fireproof material composition was left to harden in an environment of 23°C and 50% RH for 168 hours to form a heat-expandable fireproof material with a thickness of approximately 1.5 mm on the iron plate. The iron plate on which the heat-expandable fireproof material was formed was placed in an electric furnace preheated to 600°C, heated and burned for 10 minutes, and then removed. The expansion ratio was calculated using the following formula: Expansion ratio = Volume of expansion residue after combustion / Volume of heat-expandable fireproof material before combustion. Furthermore, using a compression tester (manufactured by Kato Tech Co., Ltd., "Finger Filling Tester"), compression was applied from the top surface of the expansion residue with a compression tool (a three-point indenter with a diameter of 1 mm) at a speed of 0.1 cm / sec, and the largest compression load was read at a compression depth of 0 to 8 mm, which was taken as the residue hardness.

[0092] (Adhesion Strength) Two SUS plates as specified in JIS G4303 were prepared. The SUS plates were rectangular in planar shape, measuring 100 mm in length, 20 mm in width, and 4.0 mm in thickness. A thermally expandable fireproof material composition was applied to the surface of one of the SUS plates, and the other SUS plate was placed on top of the surface coated with the thermally expandable fireproof material composition to prepare a laminate. The thermally expandable fireproof material composition was applied to an aluminum alloy plate at room temperature so that the coating width (vertical direction) was 20 mm, the coating length (horizontal direction) was 20 mm, and the coating thickness was 0.3 mm. The laminate was left in an environment of 23°C and 50% RH for 7 days, and the two SUS plates were bonded together with the thermally expandable fireproof material to prepare a test specimen. The obtained test specimen was subjected to a tensile test using a universal tensile testing machine (manufactured by Instron) by pulling in the shear direction at a rate of 1 mm / min, and the tensile shear strength at the time when the thermally expandable fireproof material constituting the test specimen broke was measured.

[0093]

[0094] In Experimental Examples 1 to 10, as shown by the deep curing time, when the heat-expandable fireproof material composition was left at high temperatures (50°C, 13% RH), it cured deeply within a short time of less than two hours. Therefore, it is understood that heat-expandable fireproof material compositions can be rapidly cured by curing at high temperatures, improving productivity. Furthermore, since the heat-expandable fireproof material compositions of Experimental Examples 1 to 6 and 10 had deep curing times of 60 minutes or less, they cured relatively quickly when applied to an iron plate or the like and left at room temperature. For example, even when pressed with a finger after two hours of room temperature curing, the coating did not deform, and a strong cured coating was formed in a short time. Furthermore, in Experimental Examples 1 to 6 and 10, heat-expandable fireproof materials were obtained that adhered to iron plates with high adhesive strength and had good fire resistance. In contrast, in Experimental Examples 7 to 9, the deep curing time was longer than 60 minutes, so when applied to an iron plate or the like and left at room temperature, the coating did not harden in a short time; for example, when the coating film was pressed with a finger after 2 hours, it deformed, and a strong cured coating could not be formed in a short time.

Claims

1. A heat-expandable fire-resistant composition comprising a polymer having a moisture-curable functional group, a heat-expandable compound, and a curing catalyst, wherein the heat-expandable fire-resistant composition is applied to a thickness of 2 mm to obtain a coating film, and the deep curing time of the coating film is 60 minutes or less under an environment of 50°C and 13% RH.

2. A heat-expandable fire-resistant composition comprising a polymer having a moisture-curable functional group, a heat-expandable compound, and a curing catalyst, wherein the polymer comprises at least one polymer selected from the group consisting of a crosslinkable silyl group-containing polyoxyalkylene polymer having a branched structure and a silylated urethane.

3. A thermally expandable fire-resistant composition comprising a polymer having a moisture-curable functional group, a thermally expandable compound, and a curing catalyst, the thermally expandable fire-resistant composition further comprising an inorganic hydrate.

4. A heat-expandable fire-resistant composition containing a polymer having a moisture-curable functional group, a heat-expandable compound, and a curing catalyst, the heat-expandable fire-resistant composition being a combination of a first part containing the polymer and the curing catalyst, and a second part containing the polymer and water.

5. The thermally expandable fire-resistant composition according to claim 1, wherein the polymer is a crosslinkable silyl group-containing polymer.

6. The thermally expandable fire-resistant composition according to claim 1, wherein the polymer comprises at least one polymer selected from the group consisting of a crosslinkable silyl group-containing polyoxyalkylene polymer having a branched structure and a silylated urethane.

7. The thermally expandable refractory composition of claim 1 further comprising an inorganic hydrate.

8. The thermally expandable refractory composition of claim 1, wherein said thermally expandable compound comprises thermally expandable graphite.

9. The thermally expandable fire-resistant composition according to claim 8, wherein said thermally expandable compound further comprises an intumescent flame retardant.

10. The thermally expandable fire-resistant composition according to claim 1, comprising a combination of a first part containing the polymer and the curing catalyst, and a second part containing the polymer and water.

11. The thermally expandable fireproof composition according to claim 1, which has fluidity at room temperature.

12. A thermally expandable fire-resistant material obtained by curing the thermally expandable fire-resistant material composition according to any one of claims 1 to 11.

13. A method for producing a heat-expandable fire-resistant material, comprising the steps of: applying or filling a heat-expandable fire-resistant composition according to any one of claims 1 to 11 onto or in a workpiece; and moisture-curing the heat-expandable fire-resistant composition applied to or filled onto the workpiece.

14. A method for producing a heat-expandable fire-resistant material, comprising the steps of: applying or filling a heat-expandable fire-resistant composition containing a polymer having a moisture-curable functional group, a heat-expandable compound, and a curing catalyst to an object to be treated; and leaving the heat-expandable fire-resistant composition applied or filled to the object to be treated in an environment at a temperature of 50°C or higher and a humidity of 10% RH or higher to moisture-cure the heat-expandable fire-resistant composition.

Citation Information

Patent Citations

  • Fire-resistant resin composition, and thermally expandable sheet

    JP2020045390A

  • Fireproof structure for structure, hardening composition, fireproof material, and fireproof structure formation method

    JP6825618B2

  • Thermoexpandable refractory material composition, thermoexpandable refractory material, and method for producing thermoexpandable refractory material

    WO2022097740A1

  • Thermally expanded fire-resistant resin composition

    JP2018035300A

  • Flame retardant adhesives and sealants with improved mechanical properties