Chloroprene-based latex composition, method for producing chloroprene-based latex composition, and aqueous adhesive
The chloroprene-based latex composition, formulated with controlled chloroprene dimers and vinyl monomers, addresses stability and odor issues in chloroprene-based latexes, resulting in a stable and odor-free adhesive with improved performance.
Patent Information
- Application Number
- PCT/JP2024/012046
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Chloroprene-based latex compositions produced with polyvinyl alcohol as an emulsifier have lower storage stability and mechanical stability, and often exhibit an odor due to chloroprene dimers formed during polymerization, making them challenging to produce effectively.
A chloroprene-based latex composition with a specific formulation containing chloroprene dimers (a, b, and c) and vinyl monomers with carboxyl groups, along with polyvinyl alcohol, is developed to achieve low odor and enhanced stability, where the total content of these components is carefully controlled within a specific range to optimize properties.
The resulting chloroprene-based latex composition exhibits improved storage stability, mechanical stability, and reduced odor, enabling the production of high-quality water-based adhesives with enhanced adhesive properties.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Chloroprene-based latex composition, method for producing chloroprene-based latex composition, and water-based adhesive
[0001] The present invention relates to a chloroprene-based latex composition, a method for producing the chloroprene-based latex composition, and a water-based adhesive.
[0002] Chloroprene latex is used in a variety of fields, including as a water-based adhesive used in the production of civil engineering and construction, plywood, furniture, shoes, and wetsuits; as a material for dip-molded products such as work gloves, laboratory gloves, and medical gloves; as rubber thread and balloons; and as a material for waterproof coatings in the civil engineering and construction fields.
[0003] Patent Document 1 discloses a polychloroprene latex composition obtained by emulsion polymerization of chloroprene and an ethylenically unsaturated carboxylic acid in the presence of a water-soluble polymer having a protective colloid effect. Patent Document 2 discloses a polychloroprene-based latex composition obtained by emulsion polymerization of chloroprene alone, or chloroprene and a monomer copolymerizable with chloroprene, in the presence of a polyoxyethylene alkyl ether having an HLB value of 14 to 19 and polyvinyl alcohol.
[0004] Japanese Patent No. 3294910 Japanese Patent Application Laid-Open No. 2005-008859
[0005] Chloroprene-based latex compositions produced using polyvinyl alcohol as an emulsifier have excellent adhesive properties and are therefore used, for example, as aqueous adhesives. However, chloroprene-based latex compositions produced using polyvinyl alcohol as an emulsifier tend to have lower storage stability and mechanical stability than chloroprene-based latexes produced using emulsifiers other than polyvinyl alcohol. In particular, when subjected to vibration during transportation or mechanical shear force from a stirrer or pump, aggregates may be formed. Furthermore, chloroprene-based latex compositions may have an odor due to chloroprene dimers and the like produced during chloroprene polymer polymerization. Therefore, it has been difficult to obtain a chloroprene-based latex composition that has little odor and excellent storage stability and mechanical stability.
[0006] The present invention has been made in view of the above circumstances, and provides a chloroprene-based latex composition that has little odor and is excellent in storage stability and mechanical stability, a method for producing the chloroprene-based latex composition, and an aqueous adhesive containing the chloroprene-based latex composition.
[0007] According to the present invention, there is provided a chloroprene latex composition containing a chloroprene polymer and water, wherein the chloroprene latex composition contains at least one chloroprene dimer selected from the group consisting of chloroprene dimer (a) represented by Formula (a), chloroprene dimer (b) represented by Formula (b), and chloroprene dimer (c) represented by Formula (c), and when the amount of the water is adjusted to obtain a chloroprene latex composition having a solid content of 50% by mass, the total content of the chloroprene dimer (a), the chloroprene dimer (b), and the chloroprene dimer (c) in the chloroprene latex composition having a solid content of 50% by mass is 0.0400 to 0.1500 parts by mass per 100 parts by mass of the chloroprene latex composition having a solid content of 50% by mass.
[0008]
[0009]
[0010]
[0011] As a result of intensive studies, the present inventors have found that, in a chloroprene latex composition containing a chloroprene polymer and water, by highly adjusting the production conditions thereof, the chloroprene latex composition contains at least one chloroprene dimer selected from the group consisting of chloroprene dimer (a) represented by formula (a), chloroprene dimer (b) represented by formula (b), and chloroprene dimer (c) represented by formula (c), and by controlling the total content thereof within a specific numerical range, a chloroprene latex composition having little odor and excellent storage stability and mechanical stability can be obtained, leading to the completion of the present invention.
[0012]
[0023] Various embodiments of the present invention are exemplified below. The embodiments shown below can be combined with each other. [1] A chloroprene-based latex composition containing a chloroprene polymer and water, wherein the chloroprene-based latex composition contains at least one chloroprene dimer selected from the group consisting of chloroprene dimer (a) represented by formula (a), chloroprene dimer (b) represented by formula (b), and chloroprene dimer (c) represented by formula (c), and when the amount of the water is adjusted to obtain a chloroprene-based latex composition having a solid content of 50% by mass, the total content of the chloroprene dimer (a), the chloroprene dimer (b), and the chloroprene dimer (c) in the chloroprene-based latex composition having a solid content of 50% by mass is 0.0400 to 0.1500 parts by mass per 100 parts by mass of the chloroprene latex composition having a solid content of 50% by mass.
[0013]
[0014]
[0015] [2] The chloroprene latex composition according to [1], wherein the content of the chloroprene dimer (a) in the chloroprene latex composition having a solid content of 50% by mass is 0.0050 to 0.0500 parts by mass relative to 100 parts by mass of the chloroprene latex composition having a solid content of 50% by mass, the content of the chloroprene dimer (b) in the chloroprene latex composition having a solid content of 50% by mass is 0.0100 to 0.1000 parts by mass relative to 100 parts by mass of the chloroprene latex composition having a solid content of 50% by mass, and the content of the chloroprene dimer (c) in the chloroprene latex composition having a solid content of 50% by mass is 0 to 0.0500 parts by mass relative to 100 parts by mass of the chloroprene latex composition having a solid content of 50% by mass. [3] The chloroprene-based latex composition according to [1] or [2], wherein the chloroprene polymer contains monomer units derived from chloroprene and monomer units derived from a vinyl monomer having a carboxyl group. [4] The chloroprene-based latex composition according to any one of [1] to [3], wherein the chloroprene polymer contains 0.01 to 5.00 parts by mass of monomer units derived from the vinyl monomer having a carboxyl group, relative to 100 parts by mass of the monomer units derived from chloroprene. [5] The chloroprene-based latex composition according to any one of [3] or [4], wherein the vinyl monomer having a carboxyl group contains an α,β-unsaturated carboxylic acid. [6] The chloroprene-based latex composition according to any one of [1] to [5], wherein the chloroprene polymer contains 0.01 to 5.00 parts by mass of monomer units derived from the vinyl monomer having a carboxyl group, relative to 100 parts by mass of the monomer units derived from chloroprene. [7] The chloroprene latex composition according to any one of [3] to [5], wherein the chloroprene polymer comprises a graft polymer containing monomer units derived from the chloroprene, monomer units derived from the carboxyl group-containing vinyl monomer, and a structure derived from polyvinyl alcohol. [8] The chloroprene latex composition according to any one of [7], wherein the chloroprene polymer comprises 0.30 to 5.00 parts by mass of the structure derived from polyvinyl alcohol per 100 parts by mass of the chloroprene polymer.[9] A method for producing a chloroprene-based latex composition, the method comprising: a polymerization step of polymerizing raw material monomers including a chloroprene monomer until a polymerization termination conversion rate is reached; the polymerization step comprises a raw material monomer divisional addition step, in which, when the raw material monomers used in the polymerization are taken as 100 mass%, the initial addition rate of the raw material monomers at the start of the polymerization is 10.0 to 70.0 mass%, and in the raw material monomer divisional addition step, the remaining raw material monomers are added in divisions after the start of the polymerization, the divisional addition starts before 25 mass% of the raw material monomers used in the polymerization are converted, and the divisional addition is carried out over a period of 20 minutes or more, when the polymerization time from the start of the polymerization until the polymerization termination conversion rate is taken as 100.
[10] A water-based adhesive containing the chloroprene-based latex composition according to any one of [1] to [8].
[0016] According to the present invention, there are provided a chloroprene-based latex composition that has little odor and is excellent in storage stability and mechanical stability, a method for producing the chloroprene-based latex composition, and an aqueous adhesive containing the chloroprene-based latex composition.
[0017] The present invention will be described in detail below by illustrating embodiments of the present invention. The present invention is not limited by these descriptions. The features of the embodiments of the present invention described below can be combined with each other. Furthermore, each feature can be an invention independently.
[0018] 1. Chloroprene-Based Latex Composition The chloroprene-based latex composition according to the present invention contains a chloroprene polymer and water. The chloroprene-based latex composition according to the present invention also contains at least one chloroprene dimer selected from the group consisting of chloroprene dimer (a) represented by formula (a), chloroprene dimer (b) represented by formula (b), and chloroprene dimer (c) represented by formula (c). When the amount of water is adjusted to obtain a chloroprene-based latex composition having a solid content of 50% by mass, the total content of the chloroprene dimer (a), the chloroprene dimer (b), and the chloroprene dimer (c) in the chloroprene-based latex composition having a solid content of 50% by mass is 0.0400 to 0.1500 parts by mass per 100 parts by mass of the chloroprene-based latex composition having a solid content of 50% by mass. Each component will be described in detail below.
[0019] 1.1 Chloroprene-Based Polymer In the present invention, a chloroprene-based polymer refers to a polymer containing monomer units derived from 2-chloro-1,3-butadiene (hereinafter referred to as chloroprene). Examples of chloroprene-based polymers include chloroprene homopolymers and chloroprene copolymers (copolymers of chloroprene and monomers copolymerizable with chloroprene). A chloroprene-based polymer according to one embodiment of the present invention can be a copolymer containing monomer units derived from a monomer other than a chloroprene monomer. As described below, a chloroprene-based polymer according to one embodiment of the present invention can contain monomer units derived from a vinyl monomer containing a carboxyl group. Furthermore, a chloroprene-based polymer according to the present invention may contain a structure derived from polyvinyl alcohol.
[0020] A chloroprene-based polymer according to one embodiment of the present invention may contain a monomer unit derived from chloroprene and a monomer unit derived from a vinyl monomer containing a carboxyl group. The vinyl monomer containing a carboxyl group may contain an α,β-unsaturated carboxylic acid. Examples of the α,β-unsaturated carboxylic acid include unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, and 3-butenoic acid; unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid; monoesters of unsaturated dicarboxylic acids such as monomethyl maleate, monomethyl fumarate, and monomethyl itaconate; unsaturated polycarboxylic acids; and esters of unsaturated polycarboxylic acids. The polymer preferably contains (meth)acrylic acid and its esters, and more preferably contains methacrylic acid.
[0021] A chloroprene-based polymer according to one embodiment of the present invention may comprise a graft polymer comprising chloroprene-derived monomer units, carboxyl-containing vinyl monomer-derived monomer units, and a polyvinyl alcohol-derived structure. The chloroprene-based polymer according to one embodiment of the present invention is formed by graft copolymerization of polyvinyl alcohol with a polymer comprising chloroprene-derived monomer units and carboxyl-containing vinyl monomer-derived monomer units. The presence of a polyvinyl alcohol structure around the chloroprene monomer units is believed to result in more stable dispersion in water and improved storage stability and mechanical stability. The graft polymer according to one embodiment of the present invention is believed to comprise branch chains comprising chloroprene-derived monomer units and carboxyl-containing vinyl monomer-derived monomer units, and a backbone chain comprising a polyvinyl alcohol-derived structure.
[0022] As described above, the chloroprene polymer according to the present invention refers to a polymer containing monomer units derived from chloroprene, and includes polymers containing monomer units derived from chloroprene and monomer units derived from a vinyl monomer containing a carboxyl group. The chloroprene polymer according to the present invention also includes both a graft polymer graft-copolymerized with polyvinyl alcohol and a polymer not graft-copolymerized with polyvinyl alcohol (a polymer not having a polyvinyl alcohol structure).
[0023] The chloroprene polymer according to the present invention may also contain a structure derived from a compound (e.g., a monomer) other than chloroprene, a vinyl monomer containing a carboxyl group, and polyvinyl alcohol. Examples of such other monomers include 2,3-dichloro-1,3-butadiene, 1-chloro-1,3-butadiene, butadiene, isoprene, styrene, ethylene, unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile), and sulfur. These may be used alone or in combination of two or more. For example, commercially available chloroprene may contain a small amount of 1-chloro-1,3-butadiene as an impurity. 2-chloro-1,3-butadiene containing such a small amount of 1-chloro-1,3-butadiene may also be used as the chloroprene according to the present invention.
[0024] A chloroprene polymer according to one embodiment of the present invention may contain 30% by mass or less of monomer units and structures derived from compounds other than chloroprene, the carboxyl-containing vinyl monomer, and polyvinyl alcohol, relative to a total of 100% by mass of monomer units derived from chloroprene and the carboxyl-containing vinyl monomer in the chloroprene polymer. The content of structures derived from other compounds may be, for example, 0, 5, 10, 15, 20, 25, or 30% by mass, and may be within a range between any two of the values exemplified here. By ensuring that the content falls within the above range, the resulting chloroprene polymer can exhibit the effects of copolymerizing other monomers without impairing the properties derived from chloroprene, etc.
[0025] The chloroprene-based polymer according to one embodiment of the present invention may be a non-graft polymer composed of chloroprene monomer units and carboxyl group-containing vinyl monomer units, or a graft polymer composed of chloroprene monomer units, carboxyl group-containing vinyl monomer units, and a structure derived from polyvinyl alcohol.
[0026] The chloroprene polymer according to one embodiment of the present invention preferably contains 95 to 99.97 parts by mass of chloroprene-derived monomer units per 100 parts by mass of the chloroprene polymer. The content of the chloroprene-derived monomer units is, for example, 95, 96, 97, 98, 99, 99.9, or 99.97 parts by mass, and may be within a range between any two of the values exemplified here.
[0027] The chloroprene polymer according to one embodiment of the present invention preferably contains 0.01 to 5.00 parts by mass of monomer units derived from a vinyl monomer having a carboxyl group, relative to 100 parts by mass of monomer units derived from chloroprene contained in the chloroprene latex composition. The content of the monomer units derived from a vinyl monomer having a carboxyl group is, for example, 0.01, 0.02, 0.05, 0.10, 0.20, 0.50, 1.00, 2.00, 3.00, 4.00, or 5.00 parts by mass, and may be within a range between any two of the values exemplified here.
[0028] The chloroprene latex composition according to one embodiment of the present invention may contain a part of the added carboxyl-containing vinyl monomer in a state that is not contained in the chloroprene polymer, i.e., in a free state. The free carboxyl-containing vinyl monomer will be described later.
[0029] The chloroprene polymer according to one embodiment of the present invention preferably contains 0.30 to 5.00 parts by mass of a structure derived from polyvinyl alcohol (i.e., a polyvinyl alcohol structure in the graft polymer) relative to 100 parts by mass of the chloroprene polymer. The content of the structure derived from polyvinyl alcohol is, for example, 0.30, 0.50, 1.00, 1.50, 2.00, 2.50, 3.00, 3.50, 4.00, 4.50, or 5.00 parts by mass, and may be within a range between any two of the values exemplified here.
[0030] The chloroprene latex composition according to one embodiment of the present invention may contain a part of the added polyvinyl alcohol in a state that is not graft-copolymerized with the chloroprene polymer, i.e., in a free state. The free polyvinyl alcohol will be described later.
[0031] A chloroprene polymer according to one embodiment of the present invention contains the above-mentioned amounts of monomer units derived from chloroprene and a vinyl monomer containing a carboxyl group, and a structure derived from polyvinyl alcohol, and further contains a part of the vinyl monomer containing a carboxyl group and a part of the polyvinyl alcohol in a free state, thereby providing a chloroprene latex composition that can give an adhesive having excellent storage stability and mechanical stability as well as excellent adhesive properties such as initial peel strength, normal peel strength, water resistance, and softening point.
[0032] 1.2 Carboxyl Group-Containing Vinyl Monomer The chloroprene latex composition according to one embodiment of the present invention may contain a part of the added carboxyl group-containing vinyl monomer in a state that is not contained in the chloroprene polymer, i.e., in a free state (monomer state).
[0033] The chloroprene-based latex composition according to one embodiment of the present invention may contain 0.01 to 5.00 parts by mass of a free carboxyl group-containing vinyl monomer relative to 100 parts by mass of chloroprene-derived monomer units contained in the chloroprene-based latex composition. The content of the carboxyl group-containing vinyl monomer is, for example, 0.01, 0.02, 0.05, 0.10, 0.20, 0.50, 1.00, 2.00, 3.00, 4.00, or 5.00 parts by mass, and may be within a range between any two of the values exemplified here.
[0034] The chloroprene-based latex composition according to one embodiment of the present invention may contain 35 to 75 parts by weight of the added vinyl monomer having a carboxyl group in a free state, based on 100 parts by weight of the vinyl monomer having a carboxyl group. The amount of the vinyl monomer having a free carboxyl group is, for example, 35, 40, 45, 50, 55, 60, 65, 70, or 75 parts by weight, and may be within a range between any two of the values exemplified here.
[0035] 1.3 Polyvinyl Alcohol The chloroprene latex composition according to the present invention may contain a part of the added polyvinyl alcohol in a state not contained in the chloroprene polymer (graft polymer), i.e., in a free state.
[0036] <Polymerization degree of polyvinyl alcohol> The polyvinyl alcohol according to one embodiment of the present invention preferably has a polymerization degree of 250 to 1000. The polymerization degree of polyvinyl alcohol is, for example, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, or 1000, and may be within a range between any two of the numerical values exemplified here.
[0037] <Saponification degree of polyvinyl alcohol> The polyvinyl alcohol according to one embodiment of the present invention preferably has a saponification degree of 76 to 95 mol%. The saponification degree is, for example, 76, 78, 80, 82, 84, 86, 88, 90, 91, 92, 93, 94, or 95 mol%, and may be within a range between any two of the values exemplified here. By setting the polymerization degree and saponification degree of polyvinyl alcohol within the above numerical ranges, it becomes easier to adjust the viscosity and dispersibility of the polymerization solution to appropriate ranges during the polymerization step of the chloroprene polymer, and stable polymerization can be performed.
[0038] In one embodiment of the present invention, the polyvinyl alcohol may include polyvinyl alcohol L. The polyvinyl alcohol L according to one embodiment of the present invention may have a degree of polymerization of less than 450. The degree of polymerization of polyvinyl alcohol L may be, for example, 100, 125, 150, 175, 200, 225, 250, 275, 300, 325, 350, 375, 400, 410, 420, 430, 440, or 445, or may be within a range between any two of the values exemplified here.
[0039] The polyvinyl alcohol L according to the present invention may have a degree of saponification of 76 to 90 mol %. The degree of saponification of the polyvinyl alcohol L is, for example, 76, 78, 80, 82, 84, 86, 88, or 90 mol %, and may be within a range between any two of the values exemplified here.
[0040] The chloroprene-based latex composition according to one embodiment of the present invention uses polyvinyl alcohol L having a degree of polymerization of less than 450, which can activate colloidal coalescence and redispersion in the early stages of polymerization, thereby providing a chloroprene-based latex composition with better controlled properties such as particle size, particle dispersion, and viscosity, and with better storage stability. Furthermore, according to one embodiment of the present invention, the use of polyvinyl alcohol L provides a chloroprene-based latex composition that can provide an adhesive with better storage stability and mechanical stability, as well as with better adhesive properties such as initial peel strength, normal peel strength, water resistance, and softening point.
[0041] The chloroprene-based latex composition according to one embodiment of the present invention may contain a polyvinyl alcohol other than the polyvinyl alcohol L.
[0042] In one embodiment of the present invention, the total amount of polyvinyl alcohol (free polyvinyl alcohol) and the polyvinyl alcohol-derived structure contained in the graft polymer in the chloroprene latex composition is preferably 0.30 to 5.00 parts by mass, relative to 100 parts by mass of the chloroprene latex composition. The total amount of (free) polyvinyl alcohol and the polyvinyl alcohol-derived structure contained in the graft polymer in the chloroprene latex composition may be 0.30, 0.50, 1.00, 1.50, 2.00, 2.50, 3.00, 3.50, 4.00, 4.50, or 5.00 parts by mass, and may be within a range between any two of the values exemplified here.
[0043] The chloroprene latex composition according to one embodiment of the present invention preferably contains 0.30 to 5.00 parts by mass of free polyvinyl alcohol that is not graft copolymerized, relative to 100 parts by mass of the chloroprene polymer. The content of the free polyvinyl alcohol is, for example, 0.30, 0.50, 1.00, 1.50, 2.00, 2.50, 3.00, 3.50, 4.00, 4.50, or 5.00 parts by mass, and may be within a range between any two of the values exemplified here.
[0044] 1.4 Chloroprene Dimer The chloroprene latex composition according to the present invention contains at least one chloroprene dimer selected from the group consisting of chloroprene dimer (a) represented by formula (a), chloroprene dimer (b) represented by formula (b), and chloroprene dimer (c) represented by formula (c).
[0045]
[0046]
[0047]
[0048] The chloroprene-based latex composition according to one embodiment of the present invention preferably contains chloroprene dimer (b). The chloroprene-based latex composition according to one embodiment of the present invention preferably contains chloroprene dimer (b) and chloroprene dimer (a). The chloroprene-based latex composition according to one embodiment of the present invention may also contain chloroprene dimer (a), chloroprene dimer (b), and chloroprene dimer (c). The chloroprene-based latex composition according to one embodiment of the present invention may also contain chloroprene dimers other than chloroprene dimer (a), chloroprene dimer (b), and chloroprene dimer (c).
[0049] When the chloroprene latex composition according to the present invention is prepared into a chloroprene latex composition having a solid content of 50% by mass by adjusting the amount of water, the total content of the chloroprene dimer (a), the chloroprene dimer (b), and the chloroprene dimer (c) in the chloroprene latex composition having a solid content of 50% by mass is 0.0400 to 0.1500 parts by mass relative to 100 parts by mass of the chloroprene latex composition having a solid content of 50% by mass. The total content of the chloroprene dimer (a), the chloroprene dimer (b), and the chloroprene dimer (c) is, for example, 0.0400, 0.0500, 0.0600, 0.0700, 0.0800, 0.0900, 0.1000, 0.1100, 0.1200, 0.1300, 0.1400, or 0.1500 parts by mass, and may be within a range between any two of the numerical values exemplified here.
[0050] The contents of chloroprene dimer (a), chloroprene dimer (b), and chloroprene dimer (c) in the chloroprene-based latex composition can be controlled by precisely adjusting the production conditions of the chloroprene-based latex composition, for example, the type and amount of each component used in the polymerization step, the timing of addition, and the polymerization time. By setting the contents of chloroprene dimer (a), chloroprene dimer (b), and chloroprene dimer (c) within the above-mentioned numerical ranges, the chloroprene-based latex composition according to the present invention becomes a chloroprene-based latex composition that has little odor and excellent storage stability and mechanical stability. The contents of each chloroprene dimer in the chloroprene-based latex composition can be measured by the method described in the Examples.
[0051] In the chloroprene latex composition according to one embodiment of the present invention, the content of the chloroprene dimer (a) relative to 100 parts by mass of the chloroprene latex composition having a solid content of 50% by mass in the chloroprene latex composition having a solid content of 50% by mass can be 0.0050 to 0.0500 parts by mass, for example, 0.0050, 0.0100, 0.0150, 0.0200, 0.0250, 0.0300, 0.0350, 0.0400, 0.0450, or 0.0500 parts by mass, and may be within a range between any two of the values exemplified here.
[0052] In the chloroprene latex composition according to one embodiment of the present invention, the content of the chloroprene dimer (b) relative to 100 parts by mass of the chloroprene latex composition having a solid content of 50% by mass may be 0.0100 to 0.1000 parts by mass, for example, 0.0100, 0.0150, 0.0200, 0.0250, 0.0300, 0.0350, 0.0400, 0.0450, 0.0500, 0.0600, 0.0700, 0.0800, 0.0900, or 0.1000 parts by mass, or may be within a range between any two of the values exemplified here.
[0053] In the chloroprene latex composition according to one embodiment of the present invention, the content of the chloroprene dimer (c) relative to 100 parts by mass of the chloroprene latex composition having a solid content of 50% by mass in the chloroprene latex composition having a solid content of 50% by mass can be 0 to 0.0500 parts by mass, for example, 0, 0.0010, 0.0050, 0.0100, 0.0150, 0.0200, 0.0250, 0.0300, 0.0350, 0.0400, 0.0450, or 0.0500 parts by mass, and may be within a range between any two of the values exemplified here.
[0054] 1.5 Surfactant The chloroprene-based latex composition according to one embodiment of the present invention may contain a surfactant. The chloroprene-based latex composition according to one embodiment of the present invention may contain a surfactant having an HLB value of 3 to 10.
[0055] The HLB value of the surfactant is, for example, 3, 4, 5, 6, 7, 8, 9, or 10, and may be within a range between any two of the values exemplified here. In the present invention, the HLB (Hydrophile-Lipophile Balance) value means the HLB value according to Davies' theory, and is expressed as HLB value = Σ (number of hydrophilic group groups) - Σ (number of lipophilic group groups) + 7.
[0056] The chloroprene-based latex composition according to one embodiment of the present invention may contain 0 to 0.36 parts by mass of a surfactant relative to 100 parts by mass of the chloroprene-based latex composition. The content of the surfactant is, for example, 0, 0.04, 0.06, 0.08, 0.10, 0.15, 0.20, 0.25, 0.30, 0.32, 0.34, or 0.36 parts by mass, and may be within a range between any two of the values exemplified here.
[0057] The surfactant is not particularly limited, and known anionic, nonionic, and cationic surfactants can be used, but a nonionic surfactant is preferred. The nonionic surfactant preferably contains at least one of a fatty acid alkanolamide and a fatty acid ester. Specific examples include sorbitan fatty acid esters such as sorbitan monostearate, sorbitan monolaurate, and sorbitan monopalmitate; glycerol fatty acid esters such as glycerol monostearate; and fatty acid alkanolamides such as lauric acid diethanolamide, myristic acid diethanolamide, and palmitic acid diethanolamide. These surfactants may be used alone or in combination of two or more.
[0058] The amounts of each component contained in the chloroprene-based latex composition, such as the amount of monomer units derived from chloroprene monomers, the amount of monomer units derived from carboxyl group-containing vinyl monomers, the structure derived from polyvinyl alcohol, the amount of free carboxyl group-containing vinyl monomers, and the amount of free polyvinyl alcohol, can be controlled by adjusting the production conditions during production of the chloroprene-based latex composition, specifically, the amount of each raw material charged, the polymerization conditions, etc. Furthermore, each content can be calculated from the analytical values and charged amounts by the methods described in the Examples.
[0059] 1.5 Physical Properties of Chloroprene Latex Composition <Storage Stability> When 235 g of the chloroprene latex composition according to one embodiment of the present invention is placed in a glass container having a body diameter of 19.5 cm and a volume of 225 ml and stored at 40°C, the period until the chloroprene latex composition precipitates to a thickness of 2 mm or more at the bottom of the container, or until the coagulate remaining on a wire netting is dried at 125°C for 1 hour and the coagulate accounts for 0.005% or more of the solids content of the chloroprene latex composition is preferably 6 weeks or more, more preferably 8 weeks or more. Specifically, the storage stability can be evaluated by the method described in the examples.
[0060] <Mechanical Stability> The chloroprene-based latex composition according to one embodiment of the present invention preferably has a mechanical stability of 0.100% or less. The mechanical stability may be, for example, 0.010, 0.020, 0.030, 0.040, 0.050, 0.060, 0.070, 0.080, 0.090, or 0.100%, or may be within a range between any two of the values exemplified here. The mechanical stability can be evaluated by the method described in the examples.
[0061] The storage stability and mechanical stability of the chloroprene latex composition according to the present invention can be adjusted by appropriately controlling the polymerization step, for example, by adjusting the type, amount, addition timing, and polymerization time of each component used in the polymerization step, and by appropriately controlling the particle size and viscosity of the polymerization solution.
[0062] The chloroprene-based latex composition according to one embodiment of the present invention preferably has little odor, particularly a pungent odor. Specifically, when 100 mL of the chloroprene-based latex composition is placed in a 250 mL plastic bottle, the bottle is sealed with a lid, and the bottle is stored at 40°C for 24 hours. After the lid is opened, the headspace gas is subjected to olfactory measurement by an olfactory panel. Preferably, the composition has no pungent odor or a slight pungent odor, and is not a strong or overpowering pungent odor. The odor of the chloroprene-based latex composition can be controlled by adjusting the type and amount of chloroprene dimer contained in the chloroprene-based latex composition.
[0063] 2. Method for Producing Chloroprene-Based Latex Composition The method for producing the chloroprene-based latex composition according to the present invention is not particularly limited, and the composition can be produced, for example, by the following method. The method for producing the chloroprene-based latex composition according to the present invention includes a polymerization step of polymerizing raw material monomers including a chloroprene monomer until a polymerization termination conversion is reached. The polymerization step also includes a raw material monomer divided addition step. In the polymerization step, when the raw material monomers used in the polymerization are taken as 100% by mass, the initial addition rate of the raw material monomers at the start of polymerization is 10.0 to 70.0% by mass. In the raw material monomer divided addition step, the remaining raw material monomers are added in divided portions after the start of polymerization. The divided addition starts before 25% by mass of the raw material monomers used in the polymerization are converted, and the divided addition is carried out over a period of 20 minutes or more, when the polymerization time from the start of polymerization until the polymerization termination conversion is taken as 100 minutes.
[0064] 2.1 Polymerization Step In the polymerization step according to the present invention, raw material monomers including a chloroprene monomer are polymerized until a polymerization termination conversion is reached. The raw material monomer according to the present invention includes a chloroprene monomer and may also include a chloroprene monomer and a vinyl monomer having a carboxyl group. The raw material monomer according to the present invention may further include another monomer other than chloroprene and a vinyl monomer having a carboxyl group. Examples of the other monomers include the monomers listed above.
[0065] <Raw Material Monomer> (Initial Addition) The polymerization process according to one embodiment of the present invention may include an initial addition step of charging at least a portion of the raw material monomers to be used in the polymerization process into a polymerization vessel before the start of polymerization, and may particularly include an initial addition step of charging at least a portion of chloroprene into a polymerization vessel. When the raw material monomers used in the polymerization are taken as 100% by mass, the initial addition rate of the raw material monomers at the start of polymerization is 10.0 to 70.0% by mass. Furthermore, when the chloroprene monomer used as a raw material is taken as 100% by mass, the initial addition rate of the chloroprene monomer at the start of polymerization is preferably 10.0 to 70.0% by mass. The initial addition rate of the raw material monomer, particularly the chloroprene monomer, at the start of polymerization is, for example, 10.0, 15.0, 20.0, 25.0, 30.0, 35.0, 40.0, 45.0, 50.0, 55.0, 65.0, or 70.0 mass%, and may be within a range between any two of the numerical values exemplified here.
[0066] In the polymerization step according to one embodiment of the present invention, a portion of the monomers other than chloroprene to be used in the polymerization step may be charged into the polymerization vessel before the start of polymerization, and a portion of the monomers other than chloroprene to be used in the polymerization step may be added after the start of polymerization. For example, in one embodiment of the present invention, all of the monomers other than chloroprene to be used in the polymerization step may be charged into the polymerization vessel before the start of polymerization, and all of the vinyl monomers having a carboxyl group to be used in the polymerization step may be charged into the polymerization vessel before the start of polymerization.
[0067] The amount of the carboxyl group-containing vinyl monomer added is preferably adjusted so that the resulting chloroprene polymer has the above-described composition and the amount of the free carboxyl group-containing vinyl monomer in the resulting chloroprene latex composition is within the above-described range. Specifically, it is preferable to add 1.0 to 5.0 parts by mass per 100 parts by mass of the raw material monomers used in the polymerization step. The amount of the carboxyl group-containing vinyl monomer added is, for example, 1.0, 2.0, 3.0, 4.0, or 5.0 parts by mass, and may be within a range between any two of the values exemplified here.
[0068] (Divided Addition) The polymerization process according to the present invention includes a raw material monomer divided addition step. In the raw material monomer divided addition step, the remaining raw material monomer, particularly chloroprene, is added in divided additions after the initiation of polymerization. In the raw material monomer divided addition step, a monomer other than chloroprene may be further added in divided additions after the initiation of polymerization. Divided addition means adding the remaining raw material monomer, particularly chloroprene, in at least two or more installments. The number of divided additions can be at least two or more installments, preferably at least five or more installments, and more preferably ten or more installments. Divided addition includes continuous addition in which the remaining raw material monomer, particularly chloroprene, is continuously added at a constant flow rate, and divided addition is preferably continuous addition.
[0069] The divided addition is initiated before 25% by mass of the raw material monomers used in the polymerization is converted. That is, the divided addition is initiated when the polymerization conversion rate is less than 25%, assuming that the raw material monomers used in the polymerization are 100% by mass. The polymerization conversion rate (mass%) can be calculated by [(mass of polymer / total mass of monomers used in polymerization) × 100]. Hereinafter, the polymerization conversion rate may also be simply referred to as the conversion rate. The divided addition can be initiated when the conversion rate is 0% by mass or more but less than 25%. The conversion rate at the start of the divided addition is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, or 24% by mass, and may be within a range between any two of the values exemplified here. Furthermore, the divided addition is preferably initiated before all of the raw material monomers, particularly chloroprene, in the polymerization system are consumed.
[0070] In the production method of the present invention, the divided addition is carried out over a period of 20 or more times, where the polymerization time from the start of polymerization to reaching the polymerization termination conversion is taken as 100. Here, the divided addition can be considered to start with the first divided addition made after the start of polymerization and end with the last divided addition when all of the monomers have been added. The divided addition can be 20 to 70 times, where the polymerization time is taken as 100, and is, for example, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, or 70 times, or may be within a range between any two of the values exemplified here.
[0071] According to the production method of the present invention, by initially adding a specific portion of the chloroprene monomer to be used in polymerization and then adding the remainder in portions at a specific timing over a specific period of time, it is possible to control the type and amount of chloroprene dimers to be produced and also to appropriately control the particle size and viscosity of the polymerization solution, and it is presumed that this makes it possible to obtain a chloroprene latex composition that has little odor and is excellent in storage stability and mechanical stability.
[0072] <Emulsifier> In the polymerization step according to the present invention, at least one of polyvinyl alcohol and a surfactant may be added. The polyvinyl alcohol and the surfactant function as an emulsifier. The polyvinyl alcohol and the surfactant are preferably the polyvinyl alcohol and the surfactant of the above-described embodiment.
[0073] The amount of polyvinyl alcohol added is preferably adjusted so that the resulting chloroprene polymer has the above-described composition and the amount of free polyvinyl alcohol in the resulting chloroprene latex composition is within the above-described range. Specifically, 1.0 to 5.0 parts by mass is preferably added per 100 parts by mass of the raw material monomers used in the polymerization step. The amount of polyvinyl alcohol added is, for example, 1.0, 2.0, 3.0, 4.0, or 5.0 parts by mass, and may be within a range between any two of the values exemplified here.
[0074] In the polymerization step according to one embodiment of the present invention, a surfactant may be further added. The amount of surfactant added may be 0 to 0.60 parts by mass relative to 100 parts by mass of the raw material monomers used in the polymerization step. The amount of surfactant added may be, for example, 0, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, or 0.60 parts by mass, or may be within a range between any two of the values exemplified here.
[0075] In the polymerization step according to one embodiment of the present invention, all of the emulsifier to be used in the polymerization step can be charged into the polymerization vessel before the start of polymerization. Alternatively, in the polymerization step according to one embodiment of the present invention, at least a portion of the emulsifier to be used in the polymerization step can be added in portions after the start of polymerization.
[0076] <pH Adjuster> In the polymerization step according to one embodiment of the present invention, a pH adjuster may be added. Examples of the pH adjuster include potassium hydroxide, sodium hydroxide, diethanolamine, diisopropanolamine, and triisopropanolamine. Two or more pH adjusters may be used in combination.
[0077] <Reducing Agent> In the polymerization step according to one embodiment of the present invention, a reducing agent can be added. Examples of the reducing agent include potassium pyrosulfite, potassium sulfite, potassium hydrogen sulfite, potassium phosphate, potassium hydrogen phosphate, sodium hydrogen sulfite, and sodium sulfite. The amount of the reducing agent added can be 0.01 to 3.0 parts by mass per 100 parts by mass of the raw material monomers used in the polymerization step.
[0078] In the polymerization step according to one embodiment of the present invention, a polymerization initiator can be used. Examples of the polymerization initiator that can be used include inorganic peroxides such as potassium persulfate, ammonium persulfate, sodium persulfate, and hydrogen peroxide; and organic peroxides such as benzoyl peroxide. These polymerization initiators can be used alone or in combination of two or more. The amount of the polymerization initiator used is preferably 0.01 to 10 parts by mass relative to 100 parts by mass of the raw material monomers used in the polymerization step.
[0079] <Chain Transfer Agent> A chain transfer agent can be used in the polymerization step according to one embodiment of the present invention. The chain transfer agent is not particularly limited, and known chain transfer agents such as long-chain alkyl mercaptans such as n-dodecyl mercaptan, tert-dodecyl mercaptan, and n-octyl mercaptan, dialkyl xanthogen disulfides such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide, and iodoform can be used. These may be used alone, or two or more types may be used in combination. The amount of chain transfer agent added can be 0.001 to 10 parts by mass relative to 100 parts by mass of the raw material monomers used in the polymerization step.
[0080] In a polymerization process according to one embodiment of the present invention, all of the chain transfer agent used in the polymerization process can be charged into the polymerization vessel before the initiation of polymerization. Alternatively, in a polymerization process according to one embodiment of the present invention, a portion of the chain transfer agent used in the polymerization process can be charged into the polymerization vessel before the initiation of polymerization, and at least a portion of the chain transfer agent can be added after the initiation of polymerization. For example, the divided addition of the chain transfer agent can be initiated simultaneously with the divided addition of the monomer. When at least a portion of the chain transfer agent is added before the initiation of polymerization and the remaining chain transfer agent is added after the initiation of polymerization, the remaining chain transfer agent can be added in one or more divided additions, or can be added continuously at a constant flow rate. For example, the divided addition of the chain transfer agent can be continuous, and can be carried out over a period of time similar to the divided addition of the chloroprene monomer. When at least a portion of the chain transfer agent is added after the initiation of polymerization, 70 parts by mass or less of 100 parts by mass of the chain transfer agent used in the polymerization process can be added after the initiation of polymerization. In this case, the amount of chain transfer agent added after the initiation of polymerization can be, for example, 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, or 70 parts by mass, or may be within a range between any two of the values exemplified here.
[0081] <Polymerization Temperature> The polymerization temperature is preferably in the range of 0 to 55° C. from the viewpoint of ease of reaction control, etc. From the viewpoint of carrying out the polymerization reaction more smoothly and safely, it is preferable that the lower limit of the polymerization temperature is 10° C. or more and the upper limit is 55° C. or less.
[0082] <Polymerization Termination Conversion Rate> In the polymerization step according to the present invention, after the desired polymerization conversion rate is reached, the polymerization reaction can be terminated by adding a polymerization terminator, and the conversion rate at the end of the polymerization is defined as the polymerization termination conversion rate. The polymerization termination conversion rate can be in the range of 50 to 99.9% by mass. The polymerization termination conversion rate is, for example, 50, 60, 70, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 99.5, or 99.9% by mass, and may be within a range between any two of the values exemplified here.
[0083] <Polymerization Terminator> Examples of the polymerization terminator include diethylhydroxyamine, thiodiphenylamine, 4-tert-butylcatechol, 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), etc. The amount added can be 0.02 to 0.1 parts by mass relative to 100 parts by mass of all the monomers used in the polymerization step.
[0084] 2.2 Step of Removing Unreacted Monomer The production method according to one embodiment of the present invention may include a step of removing unreacted monomer. In the step of removing unreacted monomer, unreacted monomer after the completion of polymerization is removed from the polymerization solution after the completion of polymerization by a conventional method such as steam stripping or vacuum heating evaporation, thereby obtaining a chloroprene-based latex composition.
[0085] The solids concentration of the chloroprene-based latex composition in the polymerization solution at the end of the polymerization can be, for example, 20, 25, 30, 35, 40, 45, 50, 55, or 60 mass %, and may be within a range between any two of the numerical values exemplified here.
[0086] 3. Adhesive (Water-Based Adhesive) An adhesive according to one embodiment of the present invention includes the above-described chloroprene-based latex composition. The adhesive may also be a water-based adhesive. An adhesive according to one embodiment of the present invention may include the above-described chloroprene-based latex composition, a tackifier resin, and a metal oxide.
[0087] <Tackifying Resin> Examples of tackifying resins include rosin resins, polymerized rosin resins, α-pinene resins, β-pinene resins, terpene phenol resins, C5 fraction petroleum resins, C9 fraction petroleum resins, C5 / C9 fraction petroleum resins, DCPD petroleum resins, alkylphenol resins, xylene resins, coumarone resins, coumarone-indene resins, etc. These may be used alone or in combination of two or more.
[0088] The method for adding the tackifier resin is not particularly limited, but it is preferable to add it as an aqueous emulsion in order to disperse the resin uniformly in the adhesive. To prepare an aqueous emulsion of the tackifier resin, there are several methods, such as dissolving the resin in an organic solvent such as toluene, emulsifying / dispersing it in water using an emulsifier, and then removing the organic solvent by heating under reduced pressure, or pulverizing the resin into fine particles and emulsifying / dispersing them.
[0089] The amount of tackifier resin added (in terms of solid content) can be 10 to 50 parts by mass relative to 100 parts by mass of the adhesive. The amount of tackifier resin added (in terms of solid content) can be, for example, 10, 15, 20, 25, 30, 35, 40, 45, or 50 parts by mass, and may be within a range between any two of the values exemplified here.
[0090] <Metal Oxide> Examples of metal oxides include zinc oxide, titanium oxide, iron oxide, etc. These may be used alone or in combination of two or more.
[0091] The amount of metal oxide added (in terms of solid content) can be 0.1 to 5.0 parts by mass relative to 100 parts by mass of the adhesive, and the amount of metal oxide added (in terms of solid content) can be, for example, 0.1, 0.2, 0.5, 1.0, 2.0, 3.0, 4.0, or 5.0 parts by mass, or can be within a range between any two of the values exemplified here.
[0092] In addition to the above components, the adhesive according to one embodiment of the present invention may contain, as appropriate, a pH adjuster, a plasticizer, a filler, an antioxidant, a pigment, a colorant, a wetting agent, an antifoaming agent, a thickener, other resin emulsions (latex), and the like.
[0093] An adhesive prepared using the chloroprene-based latex composition of the present invention can be used for bonding the same types of adherends, such as paper, wood, cloth, leather, rubber, plastic, plastic foam, pottery, glass, ceramic, and metal, or for bonding different types of adherends.
[0094] The chloroprene-based latex composition according to one embodiment of the present invention can be prepared, for example, by the following method.
[0095] <Preparation of Adhesive> 50 parts by mass of a tackifier resin (Tamanol E-100 manufactured by Arakawa Chemical Industries, Ltd.) and 1 part by mass of a metal oxide (zinc oxide: AZ-SW manufactured by Osaki Kogyo Co., Ltd.) are added to 100 parts by mass (solid content equivalent) of a chloroprene-based latex composition, and the mixture is stirred using a Three-One motor. A thickener (RM-8W manufactured by Rohm and Haas Co.) is added so that the viscosity of the solution becomes 3000 to 4000 mPa s at 25°C x 30 rpm, to obtain an adhesive.
[0096] The adhesive according to the present invention preferably has the following properties when an adhesive sample is prepared as follows: <Preparation of Adhesive Sample> The obtained adhesive is applied to two pieces of canvas (25 x 150 mm) at a rate of 300 g (solid content) / m 2 The adhesive is applied with a brush so that the adhesive becomes 100% by weight, and the applied surfaces are dried in an atmosphere of 80°C for 9 minutes, and then allowed to stand at room temperature for 1 minute, and then the applied surfaces are laminated together and pressed with a hand roller to obtain an adhesive sample. The obtained adhesive sample is evaluated as follows.
[0097] <Initial Peel Strength> The aqueous adhesive according to one embodiment of the present invention preferably has an initial peel strength of 3.0 N / mm or more in a T-peel test (initial peel strength) measured using a tensile tester at a tensile speed of 200 mm / min when the adhesive sample is roller-pressed and then left at room temperature for 10 minutes. The initial peel strength is, for example, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, or 6.0 N / mm, and may be within a range between any two of the values exemplified here.
[0098] <Normal Peel Strength> The aqueous adhesive according to one embodiment of the present invention preferably has a normal peel strength of 4.0 N / mm or more in a T-peel test (normal peel strength) measured using a tensile tester at a tensile speed of 200 mm / min after leaving the adhesive sample at room temperature for 5 days. The normal peel strength may be, for example, 4.0, 4.5, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, or 6.0 N / mm, or may be within a range between any two of the values exemplified here.
[0099] <Water Resistance Strength> The water-based adhesive according to one embodiment of the present invention preferably has a water resistance of 2.2 N / mm or more in a T-peel test (water resistance) measured using a tensile tester at a tensile speed of 200 mm / min after leaving the adhesive sample at room temperature for 5 days and then immersing it in water at 23° C. for 2 days. The water resistance is, for example, 2.2, 2.4, 2.6, 2.8, 3.0, 3.2, 3.4, 3.6, 3.8, or 4.0 N / mm, and may be within a range between any two of the values exemplified here.
[0100] <Softening Point> The aqueous adhesive according to one embodiment of the present invention can have a softening point of 40 to 80° C., as determined by applying the resulting adhesive to two pieces of canvas (25×150 mm) with a brush to a thickness of 0.5 mm, bonding the pieces together, and then heating the pieces at a rate of 2° C. / 5 minutes while applying a load of 500 g using a T-peeler. The softening point is the temperature at which the pieces are peeled off. The softening point may be, for example, 40, 45, 50, 55, 60, 65, 70, 75, or 80° C., and may be within a range between any two of the values exemplified here.
[0101] The chloroprene-based latex composition according to one embodiment of the present invention preferably has the above-described properties when used as an adhesive with the above-described formulation, specifically the formulation described in the Examples.
[0102] The present invention will be described in more detail below based on examples, but the present invention should not be construed as being limited to these examples.
[0103] <Production of Chloroprene-Based Latex Composition> (Example 1) 94 parts by mass of water, 1.8 parts by mass of polyvinyl alcohol (a), 1.3 parts by mass of polyvinyl alcohol (b), and 0.8 parts by mass of polyvinyl alcohol (c) were charged into a 10-liter reactor under a nitrogen stream and dissolved. While stirring the resulting mixture, 29.1 parts by mass of chloroprene, 3.0 parts by mass of methacrylic acid, and 0.09 parts by mass of octyl mercaptan were added and stirred at 30°C for 10 minutes (initial addition (hereinafter also referred to as initial addition)). 0.1 parts by mass of sodium sulfite was added as a reducing agent, and polymerization was initiated at 35°C using potassium persulfate as an initiator under a nitrogen atmosphere. At the start of polymerization, i.e., when the polymerization rate relative to the total monomers used during polymerization was 0%, the divided addition process was started, and 67.9 parts by mass of chloroprene and 0.21 parts by mass of octyl mercaptan were continuously added at 13.4 g / min over 4.5 hours (continuous addition (hereinafter also referred to as continuous addition)). Thereafter, when the conversion rate reached 98.1%, an emulsion of phenothiazine was added to terminate the polymerization. The pH of the polymerization solution was adjusted to 7.2 using a 45% aqueous diethanolamine solution, and unreacted monomer was removed under reduced pressure to obtain a chloroprene-based latex composition. Water was further added to adjust the solids content of the chloroprene-based latex composition to 50% by mass.
[0104] (Examples 2 to 6, Comparative Examples 1 to 5) Chloroprene-based latex compositions with a solid content concentration of 50% by mass were produced in the same manner as in Example 1, except that the polymerization recipe and polymerization conditions were as shown in Table 2. The polymerization degrees and saponification degrees of polyvinyl alcohol (a), polyvinyl alcohol (b), and polyvinyl alcohol (c) are shown below. Polyvinyl alcohol (a): polymerization degree 300, saponification degree 88.0 Polyvinyl alcohol (b): polymerization degree 300, saponification degree 80.0 Polyvinyl alcohol (c): polymerization degree 500, saponification degree 87.8
[0105] <Evaluation of Chloroprene-Based Latex Composition> (Amount of Chloroprene Dimer in 100 Parts by Mass of Chloroprene-Based Latex Composition) The amount of chloroprene dimer in the obtained chloroprene-based latex composition having a solids concentration of 50% by mass was calculated by the following method. 20 mL of acetone and 0.05 mL of acetic acid were added to a 30 mL screw bottle, the screw cap was closed, and the mass of the container and solvent was weighed. Approximately 2 g of the chloroprene-based latex composition was then dropped therein, and the mass was accurately weighed again to accurately calculate the mass of the chloroprene-based latex composition. Subsequently, the screw bottle was shaken and stirred for 1 hour to extract the chloroprene dimer in the chloroprene-based latex composition into acetone. Thereafter, 5 mL of a 100 mg / L acetone solution of chlorobenzene (internal standard) was added, and the amount of chloroprene dimer was quantified by GC by comparing with the internal standard. GC conditions: Apparatus: GC-MS; Column: DB-WAX 60 m x 0.25 mm (film thickness: 0.25 μm); Column temperature: 50°C (keep for 10 min) → 5°C / min → 150°C (keep for 20 min) → 30°C / min → 220°C (keep for 60 min); Injection port temperature: 170°C; Detection temperature: 250°C (FID); Sample injection volume: 2 μL (autosampler).
[0106] The detection sensitivity ratio between chloroprene dimer and the internal standard (chlorobenzene) was set to 1 / 0.82. The content of each chloroprene dimer was calculated using the following formula, and measurements were performed with n = 3. Chloroprene dimer content [mass %] = (chloroprene dimer peak area) / (internal standard peak area) / relative sensitivity × amount of internal standard added / (sample mass [mg]) × 100 Relative sensitivity: 0.82
[0107] (Amount of each component in 100 parts by mass of chloroprene-based latex composition) The composition of each component shown below was calculated from the charged amount and analytical value. - Amount of polyvinyl alcohol structure (including free polyvinyl alcohol) per 100 parts by mass of chloroprene-based latex composition - Amount of polyvinyl alcohol structure in the graft polymer (in the chloroprene-based polymer) per 100 parts by mass of chloroprene-based polymer - Amount of free polyvinyl alcohol per 100 parts by mass of chloroprene-based polymer - Amount of vinyl monomer containing a carboxyl group in the chloroprene-based polymer per 100 parts by mass of chloroprene-derived monomer units in the chloroprene-based polymer - Amount of free vinyl monomer units containing a carboxyl group per 100 parts by mass of chloroprene-derived monomer units in the chloroprene-based polymer The results are shown in Tables 1 and 2.
[0108] (Amount of polyvinyl alcohol structure in graft polymer) The amount of polyvinyl alcohol structure in the graft polymer was calculated by the following method: First, the amount of free polyvinyl alcohol that was not graft copolymerized was quantified by the following method, and the amount of free polyvinyl alcohol was subtracted from the amount of polyvinyl alcohol charged to determine the amount of polyvinyl alcohol structure in the graft polymer.
[0109] Preparation of Reagents: 4 g of boric acid was dissolved in 96 mL of pure water to prepare a 4% boric acid solution. 2.5 g of potassium iodide was dissolved in approximately 70 mL of pure water to prepare a potassium iodide solution. 1.27 g of iodine was weighed and dissolved in the previously prepared potassium iodide solution, and pure water was added until the total volume reached 100 mL to prepare an iodine solution.
[0110] Preparation of PVA standard solution: 0.1 g of PVA was accurately weighed into a 100 mL measuring flask, 50-60 mL of pure water was added, and the solution was dissolved in a water bath (approximately 95°C). After cooling to room temperature, pure water was added up to the mark and mixed well. 10 mL of this solution was taken and placed in a 100 mL measuring flask, and pure water was added up to the mark and mixed well to prepare a standard solution with a PVA concentration of 0.1 mg / mL.
[0111] Preparation of a calibration curve: 1, 5, 10, 15, and 20 mL of the above standard solution were dispensed into 50 mL volumetric flasks, and 15 mL of 4% boric acid solution was added to each, followed by pure water to a total volume of 45 mL. To each was then added 3 mL of iodine solution, and pure water was added up to the mark. The mixture was mixed thoroughly to prepare solutions with PVA concentrations of 2, 10, 20, 30, and 40 mg / L. Using a blank solution prepared without iodine as a control, the absorbance was measured using a spectrophotometer at a wavelength of 650 nm and a cell glass of 10 mm, and a concentration-absorbance calibration curve was prepared.
[0112] Preparation of Measurement Samples: 9 g of the chloroprene-based latex composition of each Example and Comparative Example was weighed into a 200 mL beaker, and 171 g of pure water was added while stirring to dilute the composition 20 times by mass. 100 g of the diluted solution (2 x 50 g) was placed in a cell and centrifuged at 6,000 rpm for 30 minutes. 1 mL of the supernatant was taken into a 50 mL measuring flask, and 15 mL of 4% boric acid aqueous solution was added. Pure water was then added until the total volume reached 45 mL. 3 mL of iodine solution was then added, and pure water was added up to the mark, mixed well, and the resulting solution was used as a measurement sample.
[0113] Using a blank solution as a control, absorbance was measured using a spectrophotometer at a wavelength of 650 nm and a cell glass of 10 mm. The measurement was carried out after diluting the original chloroprene-based latex composition 1000 times (20 times dilution x 50 times dilution).
[0114] Calculation of PVA concentration, amount of free polyvinyl alcohol, and amount of polyvinyl alcohol structure in the graft polymer. The PVA concentration S of the measurement sample is calculated using the following formula: c was calculated. c = ABS x A S c : PVA concentration in the measuring flask [mg / L], ABS: absorbance, A: coefficient (calculated from the calibration curve using Lotus 1-2-3). Subsequently, the free polyvinyl alcohol concentration in the chloroprene-based latex composition was calculated using the following formula. c = S c ×C / BL c where B is the concentration of free polyvinyl alcohol in the chloroprene-based latex composition [g / kg], B is the amount of diluted solution [g], and C is the amount of supernatant solution [g].
[0115] Finally, the amount of free polyvinyl alcohol in the chloroprene-based latex composition and the amount of polyvinyl alcohol structure in the graft polymer were calculated using the following formulas: PVA F =L c ×L Q PVA F : Amount of free polyvinyl alcohol [g] L Q : Amount of chloroprene-based latex composition [kg] PVA G = PVA Q -PVA F PVA G : Amount of polyvinyl alcohol structure in the graft polymer [g] PVA Q : Amount of polyvinyl alcohol charged [g]
[0116] The obtained PVA G was divided by the amount of the chloroprene polymer in the chloroprene latex composition to calculate the amount of polyvinyl alcohol structure in the graft polymer relative to 100 parts by mass of the chloroprene polymer. The "amount of chloroprene polymer" was the sum of the amount of chloroprene monomer units, the amount of vinyl monomer units containing a carboxyl group (excluding vinyl monomers containing a free carboxyl group), and the amount of polyvinyl alcohol structure (excluding free polyvinyl alcohol) in the chloroprene latex composition.
[0117] (Amount of copolymerization of carboxyl group-containing vinyl monomer) The chloroprene-based polymers according to the examples and comparative examples have a large gel content, and the amount of methacrylic acid copolymerized is 1 Therefore, the methacrylic acid / chloroprene peak area ratio was calculated by PyGC / MS (SIM method), and standard samples (without gel content) with different amounts of methacrylic acid copolymerized were used. 1 H-NMR measurement is possible) 1 The amount of copolymerized methacrylic acid was calculated using the methacrylic acid / chloroprene peak area ratio (MAA copolymerization amount) by H-NMR vs. the methacrylic acid / chloroprene peak area ratio by PyGC / MS (SIM method).
[0118] Preparation of samples for PyGC / MS (SIM method) The samples were freeze-dried and extracted with an ethanol-toluene azeotropic mixture (ETA). The extracted residue after drying was measured by PyGC / MS (SIM method).
[0119] PyGC / MS (SIM method) Using methacrylic acid: m / z = 86 and chloroprene: m / z = 91, the methacrylic acid / chloroprene peak area ratio was calculated under the following measurement conditions. Apparatus: JEOL Jms-Q1050GC GC Column: DB-WAX 60 m * 0.25 mm (0.5 μm) Column temperature: 100 ° C (0 min) → 10 ° C / min → 240 ° C (11 min) Injection port temperature: 240 ° C Carrier: He 1.0 mL / min (Split 1:30) MS Interface temperature: 240 ° C Ion source temperature: 250 ° C Ionization current: 50 μ A Ionization voltage: 70 eV Detector voltage: -1200 V Ionization method: EI SIM (m / z: 86.91) Py Frontier Labs PY-3030D Pyrolysis temperature: 590 ° C Sample amount: 0.1 mg Interface temperature: 300 ° C
[0120] ・ 1 Preparation of sample used for H-NMR measurement The chloroprene-based latex composition was purified using methanol and xylene to obtain a sample. Approximately 30 mg of the sample was dissolved in approximately 1 mL of deuterated chloroform, and the measurement was performed.
[0121] ・ 1 H-NMR Equipment configuration: Solution NMR (using 5 mm probe) Measurement conditions Analytical equipment: Superconducting nuclear magnetic resonance equipment ECX-400 manufactured by JEOL Observation nuclei: 1 H Measurement conditions: Single Pulse Sample tube rotation speed: 12 Hz Measurement temperature: 30°C Pulse width: 3.5 μsec (45° pulse) Repetition time: 7 seconds Number of integrations: 128 times
[0122] The amount of the carboxyl-containing vinyl monomer in the chloroprene polymer was calculated based on the methacrylic acid / chloroprene peak area ratio, relative to 100 parts by mass of the chloroprene-derived monomer units in the chloroprene polymer. The amount of the carboxyl-containing vinyl monomer released was calculated by subtracting the amount of methacrylic acid copolymerized from the charged amount.
[0123] (Storage Stability) Eight sealed glass containers each containing 235 g of the chloroprene latex composition were prepared. All of the containers were stored at 40°C, and one of the containers was removed every week, and the chloroprene latex was filtered through a 100-mesh wire mesh. The time required for the thickness of the chloroprene latex composition remaining at the bottom of the glass container to reach 2 mm or more was recorded, or the time required for the coagulated material remaining on the wire mesh to reach 0.005% or more of the solid content of the chloroprene latex composition after drying at 125°C for 1 hour was recorded. The evaluation results are shown in Tables 1 and 2.
[0124] (Mechanical Stability) Using a Marlon testing apparatus in accordance with JIS K 6828, a shear force of 10 kg load and 1,000 rpm was applied to 50 g of a chloroprene-based latex composition for 10 minutes, and the amount of coagulated material generated was evaluated. The coagulated material adhering to the rotor of the Marlon testing apparatus was collected on a SUS80 mesh wire screen, washed with pure water, dried under reduced pressure, and then the mass was measured. The evaluation results are shown in Tables 1 and 2. The values in the tables were calculated by the following formula after drying and weighing the coagulated material generated; a smaller value indicates better stability against shear force. Mechanical stability (%) = dry mass of coagulated material [g] / 50 [g] x 100
[0125] (Odor Evaluation) 100 mL of the chloroprene-based latex composition was placed in a 250 mL plastic bottle, the bottle was sealed with a lid, and stored at 40°C for 24 hours. After that, the lid was opened and an olfactory panel measured the headspace gas and evaluated the intensity of the irritating odor on a four-point scale according to the following criteria: 1: No irritating odor, 2: Slight irritating odor, 3: Strong irritating odor, 4: Extremely irritating odor
[0126] <Preparation of Adhesive> The chloroprene-based latex composition of each Example and Comparative Example, a tackifier resin (terpene phenol, manufactured by Arakawa Chemical Industries, Ltd., Tamanol E-100 (solids concentration 53%)), and a metal oxide (aqueous zinc oxide, manufactured by Osaki Kogyo Co., Ltd., AZ-SW (solids concentration 50%)) were mixed in the formulations shown in Tables 1 and 2 to prepare adhesives.
[0127] <Evaluation of adhesive> The obtained adhesive was applied to two pieces of canvas (25 x 150 mm) at 300 g (solid content) / m 2 The adhesive was applied with a brush so that the adhesive layer was coated with the adhesive, dried in an atmosphere of 80°C for 9 minutes, and left at room temperature for 1 minute. The coated surfaces were then laminated together and pressed with a hand roller to obtain an adhesive sample. The obtained adhesive sample was evaluated as follows. The evaluation results are shown in Tables 1 and 2.
[0128] (Initial Peel Strength) The obtained adhesive sample was pressed with a roller and then left at room temperature for 10 minutes, followed by a T-peel test at a pulling rate of 200 mm / min using a tensile tester.
[0129] (Normal Peel Strength) The obtained adhesive sample was left at room temperature for 5 days, and then subjected to a T-peel test at a pulling rate of 200 mm / min using a tensile tester.
[0130] (Water Resistance Strength) The obtained adhesive sample was left at room temperature for 5 days, and then further immersed in water at 23° C. for 2 days, and a T-peel test was performed using a tensile tester at a tensile speed of 200 mm / min.
[0131] (Softening point) The obtained adhesive was applied to two pieces of canvas (25 x 150 mm) with a brush to a thickness of 0.5 mm, and the pieces were bonded together. Using a T-peeler, the temperature was raised at 2°C / 5 minutes while a load of 500 g was applied, and the temperature at which the pieces were peeled off was recorded as the softening point.
[0132]
[0133]
Claims
1. A chloroprene-based latex composition comprising a chloroprene polymer and water, the chloroprene-based latex composition comprising at least one chloroprene dimer selected from the group consisting of a chloroprene dimer (a) represented by formula (a), a chloroprene dimer (b) represented by formula (b), and a chloroprene dimer (c) represented by formula (c), and when the amount of the water is adjusted to obtain a chloroprene-based latex composition having a solid content concentration of 50% by mass, the total content of the chloroprene dimer (a), the chloroprene dimer (b), and the chloroprene dimer (c) in the chloroprene latex composition having a solid content concentration of 50% by mass is 0.0400 to 0.1500 parts by mass per 100 parts by mass of the chloroprene latex composition having a solid content concentration of 50% by mass.
2. The chloroprene-based latex composition according to claim 1, wherein the content of the chloroprene dimer (a) in the chloroprene-based latex composition having a solid content concentration of 50% by mass is 0.0050 to 0.0500 parts by mass relative to 100 parts by mass of the chloroprene-based latex composition having a solid content concentration of 50% by mass, the content of the chloroprene dimer (b) in the chloroprene-based latex composition having a solid content concentration of 50% by mass is 0.0100 to 0.1000 parts by mass relative to 100 parts by mass of the chloroprene-based latex composition having a solid content concentration of 50% by mass, and the content of the chloroprene dimer (c) in the chloroprene-based latex composition having a solid content concentration of 50% by mass is 0 to 0.0500 parts by mass relative to 100 parts by mass of the chloroprene-based latex composition having a solid content concentration of 50% by mass.
3. The chloroprene latex composition according to claim 1 or 2, wherein the chloroprene polymer contains monomer units derived from chloroprene and monomer units derived from a vinyl monomer containing a carboxyl group.
4. The chloroprene latex composition according to claim 3, wherein the chloroprene polymer contains 0.01 to 5.00 parts by mass of monomer units derived from the carboxyl group-containing vinyl monomer, relative to 100 parts by mass of monomer units derived from the chloroprene.
5. The chloroprene-based latex composition according to claim 3, wherein the vinyl monomer containing a carboxyl group comprises an α,β-unsaturated carboxylic acid.
6. The chloroprene-based latex composition according to claim 1 or 2, which contains polyvinyl alcohol.
7. The chloroprene latex composition according to claim 3, wherein the chloroprene polymer comprises a graft polymer containing a monomer unit derived from the chloroprene, a monomer unit derived from the vinyl monomer containing a carboxyl group, and a structure derived from polyvinyl alcohol.
8. The chloroprene latex composition according to claim 7, wherein the chloroprene polymer contains 0.30 to 5.00 parts by mass of a structure derived from the polyvinyl alcohol per 100 parts by mass of the chloroprene polymer.
9. A method for producing a chloroprene-based latex composition, comprising: a polymerization step of polymerizing raw material monomers including a chloroprene monomer until a polymerization completion conversion rate is reached; the polymerization step comprises a raw material monomer split addition step; in the polymerization step, when the raw material monomers used in the polymerization are taken as 100 mass%, an initial addition rate of the raw material monomers at the start of polymerization is 10.0 to 70.0 mass%, and in the raw material monomer split addition step, the remaining raw material monomers are added in splits after the start of polymerization; the split addition starts before 25 mass% of the raw material monomers used in the polymerization are converted; and the split addition is carried out over a period of 20 or more hours, when the polymerization time from the start of polymerization to the time when the polymerization completion conversion rate is taken as 100.
10. A water-based adhesive comprising the chloroprene-based latex composition according to claim 1 or 2.
Citation Information
Patent Citations
Polychloroprene latex composition, adhesive, coating material and production method for the same composition
JP2005008859A
Polychloroprene latex composition
JP3294910B2
Process for the preparation of (co)polychloroprene in water emulsion
EP0728774A1
Removal of chloroprene dimer from polchloroprene
JP1991203609A
Polychloroprene latex composition and method for producing the same
JP2007063370A