Composite material and molded body

The composite material of fluororesin and oxidized carbon nanotubes addresses the issue of metal elution in semiconductor manufacturing by controlling impurities and resistivity, ensuring effective conductivity and reduced contamination.

WO2024204272A1PCT designated stage expired Publication Date: 2024-10-03ZEON CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012088
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional composite materials containing fluororesin and carbon nanotubes face challenges in reducing metal elution while maintaining electrical conductivity, particularly in semiconductor manufacturing equipment, where electrostatic discharge and metal contamination are concerns.

Method used

A composite material comprising fluororesin and oxidized carbon nanotubes with controlled impurity content below 10 ppm, optimized volume resistivity, and specific carbon nanotube content and ash levels, which reduces metal elution while ensuring conductivity, is developed.

Benefits of technology

The composite material achieves reduced metal elution and enhanced conductivity, making it suitable for semiconductor manufacturing equipment, such as chemical nozzles and tubes, by using oxidized carbon nanotubes with precise composition and processing methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

Disclosed is a composite material which contains a fluororesin and carbon oxide nanotubes, and which has an impurity content of less than 10 ppm. Also disclosed is a molded body which is obtained by molding the composite material. It is preferable that the composite material has a volume resistivity of 1 × 103 Ω∙cm to 1 × 108 Ω∙cm (inclusive). It is also preferable that the content ratio of the carbon oxide nanotubes in the composite material is 0.005% by mass to 0.2% by mass (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Composite materials and moldings

[0001] The present invention relates to a composite material and a molded article, and more particularly to a composite material containing a fluororesin and oxidized carbon nanotubes, and a molded article using the composite material.

[0002] Carbon nanotubes (hereinafter sometimes referred to as "CNTs") have excellent electrical conductivity, thermal conductivity, sliding properties, mechanical properties, etc., and therefore their application in a wide range of applications is being considered. In recent years, therefore, progress has been made in developing a technology that takes advantage of the excellent properties of carbon nanotubes and combines them with resins to provide resin materials that combine the properties of resins, such as processability and strength, with the properties of carbon nanotubes, such as electrical conductivity.

[0003] Specifically, for example, Patent Documents 1 and 2 disclose particulate composite materials containing fluororesin and carbon nanotubes.

[0004] International Publication No. WO 2018 / 066433 International Publication No. WO 2012 / 107991

[0005] Here, composite materials containing fluororesin and carbon nanotubes have excellent chemical resistance and conductivity, and are therefore used as molding materials for parts of semiconductor manufacturing equipment, such as chemical nozzles and tubes used in semiconductor manufacturing.

[0006] However, the above-mentioned conventional composite materials have room for improvement in terms of further reducing the amount of metal elution while ensuring electrical conductivity from the viewpoints of suppressing the occurrence of electrostatic discharge and preventing metal contamination.

[0007] Therefore, an object of the present invention is to provide a composite material and a molded article that are electrically conductive and have a small amount of metal elution.

[0008] The present invention aims to advantageously solve the above-mentioned problems, and [1] the composite material of the present invention is characterized by including a fluororesin and oxidized carbon nanotubes, and having an impurity content of less than 10 ppm. In this way, by including oxidized carbon nanotubes and keeping the impurity content less than 10 ppm, it is possible to reduce the amount of metal elution while ensuring electrical conductivity. Here, in the present invention, the impurity content of the composite material can be measured by the method described in the examples.

[0009] [2] The composite material described in [1] above has a volume resistivity of 1×10 3 Ω・cm or more 1×10 8 It is preferable that the volume resistivity is 1×10 Ω·cm or less. 3 Ω・cm or more 1×10 8 If the resistivity is Ω·cm or less, better conductivity can be exhibited. In the present invention, the volume resistivity of the composite material can be measured by the method described in the examples.

[0010] Furthermore, [3] in the composite material described in [1] or [2] above, it is preferable that the content of the oxidized carbon nanotubes is 0.005 mass % or more and 0.2 mass % or less. If the content of the oxidized carbon nanotubes is within the above range, the electrical conductivity can be further increased while the amount of metal elution can be further reduced.

[0011] [4] In the composite material according to any one of [1] to [3] above, the oxidized carbon nanotubes preferably have an ash content of less than 3 mass%. Using oxidized carbon nanotubes with an ash content of less than 3 mass% can further reduce the amount of metal elution. In the present invention, the ash content of the oxidized carbon nanotubes can be measured by the method described in the Examples.

[0012] Furthermore, [5] in the composite material according to any one of [1] to [4] above, it is preferable that the G / D ratio of the oxidized carbon nanotubes is 0.5 or more. If the G / D ratio of the oxidized carbon nanotubes is 0.5 or more, better electrical conductivity can be exhibited. In the present invention, the G / D ratio of the oxidized carbon nanotubes can be measured by the method described in the Examples.

[0013] [6] In the composite material according to any one of the above [1] to [5], the fluororesin is preferably at least one selected from the group consisting of polytetrafluoroethylene, polychlorotrifluoroethylene, and a copolymer of tetrafluoroethylene and perfluoroalkoxyethylene. Use of these resins can further improve chemical resistance.

[0014] Another object of the present invention is to advantageously solve the above-mentioned problems, and the present invention provides a molded article [7] characterized by being obtained by molding the composite material according to any one of the above [1] to [6]. In this way, by using the above-mentioned composite material, a molded article can be obtained that has a reduced amount of metal elution while maintaining electrical conductivity.

[0015] According to the present invention, it is possible to obtain a composite material and a molded article that are electrically conductive and have a small amount of metal elution.

[0016] The present invention will be described in detail below. Here, the composite material of the present invention can be suitably used as a molding material for the molded article of the present invention. The molded article of the present invention can be suitably used as a part of a semiconductor manufacturing device, such as a chemical nozzle or tube used in semiconductor manufacturing, without any particular limitation.

[0017] (Composite Material) The composite material of the present invention contains a fluororesin and oxidized carbon nanotubes, and is required to have an impurity content of less than 10 ppm. The composite material of the present invention may optionally further contain one or more other components selected from the group consisting of resins other than fluororesin, carbon nanotubes other than oxidized carbon nanotubes, and additives such as antioxidants and plasticizers. However, the content of other components in the composite material of the present invention is preferably 5% by mass or less, more preferably 1% by mass or less, even more preferably 0.1% by mass or less, and particularly preferably 0% by mass (i.e., the composite material consists only of the fluororesin, the oxidized carbon nanotubes, and impurities inevitably mixed in during the preparation of the composite material).

[0018] The composite material of the present invention contains oxidized CNTs, ensuring sufficient electrical conductivity. Furthermore, the composite material of the present invention has an impurity content of less than 10 ppm, resulting in a low amount of metal elution.

[0019] <Fluorine resin> As the fluororesin, there is no particular limitation, for example, polytetrafluoroethylene (PTFE), copolymer of tetrafluoroethylene and perfluoroalkoxyethylene (PFA), copolymer of tetrafluoroethylene and hexafluoropropylene (FEP), copolymer of tetrafluoroethylene and ethylene (ETFE), polychlorotrifluoroethylene (PCTFE), copolymer of chlorotrifluoroethylene and ethylene (ECTFE), polyvinylidene fluoride (PVDF) and polyvinyl fluoride (PVF) etc. From the viewpoint of chemical resistance, preferred fluororesin is at least one selected from the group consisting of polytetrafluoroethylene, polychlorotrifluoroethylene and copolymer of tetrafluoroethylene and perfluoroalkoxyethylene.In addition, the above-mentioned fluororesin may be used alone, or two or more may be used in combination.

[0020] The composite material preferably has a fluororesin content of 90% by mass or more, more preferably 95% by mass or more, even more preferably 99% by mass or more, and particularly preferably 99.9% by mass or more.

[0021] <Oxidized CNT> The oxidized CNT contained in the composite material can be obtained by oxidizing single-walled carbon nanotubes and / or multi-walled carbon nanotubes. Among them, the oxidized CNT is preferably obtained by oxidizing single-walled to five-walled carbon nanotubes, and more preferably obtained by oxidizing single-walled carbon nanotubes. The use of oxidized CNT obtained by oxidizing single-walled carbon nanotubes can further increase the conductivity of the composite material.

[0022] Here, the average diameter of the oxidized CNTs is preferably 0.5 nm or more, more preferably 1 nm or more, and preferably 15 nm or less, and even more preferably 10 nm or less. If the average diameter of the oxidized CNTs is 0.5 nm or more and 15 nm or less, the conductivity of the composite material can be further increased. The average diameter of the oxidized CNTs can be determined by measuring the diameter (outer diameter) of 100 randomly selected oxidized CNTs using a transmission electron microscope.

[0023] In addition, the oxidized CNT has a BET specific surface area of ​​200 m 2 / g or more, and 2 / g or more is more preferable, and 2,000m 2 / g or less, and 2 / g or less is more preferable. If the BET specific surface area is within the above range, the electrical conductivity of the composite material can be further increased. Here, the "BET specific surface area" means the nitrogen adsorption specific surface area measured according to the BET method.

[0024] Furthermore, the oxidized CNTs preferably have an ash content of less than 3 mass%, more preferably 1 mass% or less, even more preferably 0.5 mass% or less, and particularly preferably 0.15 mass% or less. If the ash content is within this range, the electrical conductivity of the composite material can be further increased while the amount of metal elution can be further reduced.

[0025] Furthermore, the oxidized CNT preferably has a G / D ratio of 0.5 or more, more preferably 1.0 or more, and even more preferably 2.5 or more, and preferably 150 or less, more preferably 50 or less, and even more preferably 10 or less. If the G / D ratio is within the above range, the electrical conductivity of the composite material can be further increased while the amount of metal elution can be further reduced.

[0026] Furthermore, the surface oxygen atomic concentration of the oxidized CNT is preferably 1.0 at% or more, more preferably 1.5 at% or more, preferably 6.0 at% or less, more preferably 5.0 at% or less, even more preferably 3.5 at% or less, even more preferably 3.0 at% or less, and particularly preferably 2.0 at% or less. If the surface oxygen atomic concentration is within the above range, it is possible to further reduce the amount of metal elution while suppressing a decrease in the conductivity of the composite material caused by the introduction of a large number of defects into the oxidized CNT due to excessive oxidation treatment of the carbon nanotubes. The "surface oxygen atomic concentration" can be measured using X-ray photoelectron spectroscopy (XPS).

[0027] The composite material preferably has an oxidized CNT content of 0.005% by mass or more, more preferably 0.01% by mass or more, and preferably 0.5% by mass or less, more preferably 0.2% by mass or less, and even more preferably 0.1% by mass or less. If the oxidized CNT content is equal to or greater than the lower limit, the electrical conductivity of the composite material can be further increased. If the oxidized CNT content is equal to or less than the upper limit, the amount of metal elution can be further reduced.

[0028] <Properties of Composite Material> The composite material containing the above-described fluororesin and oxidized CNT must have an impurity content of less than 10 ppm, and preferably has the following properties.

[0029] [Impurity Content] The impurity content of the composite material is less than 10 ppm, preferably 8 ppm or less, more preferably 5 ppm or less, even more preferably less than 3 ppm, and particularly preferably below the detection limit. If the impurity content is within the above range, the amount of metal elution from the composite material can be sufficiently reduced.

[0030] Impurities contained in the composite material include metals (residual metal impurities) derived from the metal catalyst used in producing the CNTs used as raw materials for the oxidized CNTs. The impurity content in the composite material can be controlled, for example, by adjusting the oxidation treatment conditions when oxidizing CNTs to obtain oxidized CNTs or the blending amount of oxidized CNTs. The impurity content in the composite material can also be adjusted using known metal removal methods, such as filtration using a magnetic filter.

[0031] [Volume Resistivity] The composite material has a volume resistivity of 1×10 3 Ω・cm or more 1×10 8 It is preferably Ω cm or less, and 1×10 3 Ω・cm or more 1×10 5 It is more preferable that the resistance is Ω cm or less, and 1×10 3 Ω・cm or more 5×10 4 It is more preferable that the volume resistivity is Ω·cm or less. If the volume resistivity is within the above range, the electrical conductivity of the composite material can be sufficiently increased.

[0032] The volume resistivity of the composite material can be controlled by adjusting the amount of oxidized CNTs added, for example; increasing the amount of oxidized CNTs added can reduce the volume resistivity.

[0033] [Metal elution amount] The composite material preferably has a metal elution amount of 1.5 ppb or less, more preferably 1.0 ppb or less, even more preferably 0.6 ppb or less, and particularly preferably 0.3 ppb or less. The metal elution amount of the composite material can be measured by the method described in the examples.

[0034] <Method for producing composite material> The composite material of the present invention is not particularly limited, and can be obtained, for example, by carrying out an oxidation treatment step of CNT to obtain oxidized CNT, and then carrying out a compounding step of compounding the oxidized CNT with a fluororesin.

[0035] [Oxidation Treatment Step] In the oxidation treatment step, raw CNTs are oxidized to obtain oxidized CNTs. In this oxidation treatment step, the CNTs are oxidized and residual metal impurities in the CNTs can also be removed.

[0036] Here, the CNTs used as the raw material are not particularly limited, and known CNTs such as commercially available CNTs can be used.

[0037] The oxidation of CNTs can be carried out using, for example, a gas phase oxidation method or a liquid phase oxidation method. Specifically, in the gas phase oxidation method, air, ozone, Cl 2 , HCl, SF 6 and H 2 CNTs can be oxidized by contacting them with a gaseous oxidizing agent such as S. Furthermore, in the liquid-phase oxidation method, CNTs can be oxidized by contacting them with an oxidizing agent in a dispersion medium such as water. The oxidizing agent used in the liquid-phase oxidation method can be any oxidizing agent that can oxidize CNTs and dissolves in the dispersion medium. Among these, it is preferable to use at least one selected from the group consisting of nitric acid, sulfuric acid, hydrochloric acid, hydrogen peroxide, ammonium persulfate, and sodium hypochlorite.

[0038] Among these, the oxidation of CNT is preferably carried out using a liquid-phase oxidation method, and from the viewpoint of reducing the impurity content in the composite material, the liquid-phase oxidation method is more preferably carried out using nitric acid, sulfuric acid, or hydrochloric acid as the oxidizing agent. The oxidation of CNT by the liquid-phase oxidation method is preferably carried out by refluxing a mixture containing CNT, an oxidizing agent, and a dispersion medium under predetermined temperature conditions. The temperature condition when refluxing the mixture is preferably 100°C or higher and 180°C or lower, and the reflux time is preferably 3 hours or higher and 20 hours or lower.

[0039] The obtained oxidized CNTs can be recovered by optionally performing solid-liquid separation such as filtration, washing, and then drying.

[0040] [Compositing Step] The composite of the oxidized CNT and the fluororesin in the composite step is not particularly limited and can be carried out using any known composite method. Among them, the composite is preferably carried out by mixing and dispersing the fluororesin and the oxidized CNT in a dispersion medium such as an organic solvent, and then removing the dispersion medium from the resulting slurry.

[0041] The organic solvent is not particularly limited, and examples thereof include isopropyl alcohol, tetrahydrofuran, methyl ethyl ketone, cyclohexane, toluene, and fluorine-based solvents. Of these, cyclohexane is preferred.

[0042] The mixing and dispersion of the fluororesin and oxidized CNTs can be carried out using, without particular limitation, a homogenizer, an ultrasonic disperser, a jet mill, a ball mill, or the like.

[0043] The dispersion medium can be removed from the slurry by solid-liquid separation such as centrifugation or drying such as vacuum drying. Among these, the dispersion medium is preferably removed by centrifuging the slurry to remove the supernatant, followed by vacuum drying.

[0044] (Molded Article) The molded article of the present invention can be obtained by molding the composite material described above using a molding machine, such as an extruder, injection molding machine, compressor, or roller, depending on the desired shape of the molded article. The molded article may optionally be subjected to a crosslinking treatment. The molded article preferably has the same volume resistivity and metal elution amount as those described above for the composite material.

[0045] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples. In the following description, "%" representing amounts is based on mass unless otherwise specified. In the examples and comparative examples, the ash content, G / D ratio, and surface oxygen atom concentration of carbon nanotubes, as well as the impurity content, volume resistivity, and amount of eluted metal of composite materials were measured or evaluated using the following methods.

[0046] <Ash content> Carbon nanotubes (CNT or oxidized CNT) to be measured were heated from room temperature to 800°C at a heating rate of 5°C / min in an air atmosphere using a thermogravimetric analyzer (manufactured by TA Instruments, product name "TGA5500"), and the proportion of residues when heated was taken as the ash content in the CNT (= (residue / carbon nanotubes) x 100%). <G / D ratio> A microscopic Raman spectrophotometer (manufactured by Bruker, product name "SENTERRA") was used to measure the Raman spectrum of the carbon nanotubes to be measured. The Raman spectrum obtained was analyzed using a Raman microscope (manufactured by Bruker, product name "SENTERRA") at 1590 cm -1 The intensity of the G-band peak observed near 1340 cm -1The intensity of the D band peak observed in the vicinity was determined, and the G / D ratio was calculated. <Surface oxygen atom concentration> The carbon nanotubes (CNT or oxidized CNT) to be measured were each analyzed using an X-ray photoelectron spectrometer (manufactured by ULVAC-PHI, product name "PHI5000 VersaProve II"). Then, for the carbon nanotubes to be measured, the O1s peak area and the total detected peak area were determined, and based on these, the ratio (at%) of the amount of oxygen atoms (O) present to the total atomic weight constituting the surface was calculated (= O atom abundance / total atomic weight × 100), and the obtained value was taken as the surface oxygen atomic concentration (at%). <Impurity content> The composite material was compression-molded into a tablet with a diameter of 40 mm to obtain a measurement sample. The obtained measurement sample was measured using an X-ray fluorescence analyzer (manufactured by Rigaku Corporation, product name "ZSX Primus IV") under the following conditions. X-ray tube: Rh, 4 kW; Analyzed elements: 5B to 92U; Measurement time: 15 minutes; Analysis diameter: 30 mm; Detection limit: 3 ppm. The total amount of the measured elements, 11Na to 92U, was calculated as the impurity amount (ppm) in the composite material. <Volume Resistivity> Using a low resistivity meter (manufactured by Mitsubishi Chemical Analytech Co., Ltd., product name "Loresta-GX MCP-T700", probe: LSP), the volume resistivity of the obtained molded body was measured at five different measurement points, and the average value of the five measurements was calculated. This average value was used as the volume resistivity. A lower volume resistivity value indicates better conductivity. <Metal Leaching Amount> The molded body was washed with ultrapure water to obtain a test specimen. The obtained test specimen was immersed in 100 mL of 3.6% hydrochloric acid (manufactured by Kanto Chemical Co., Ltd., EL-UM grade) and stored at room temperature for 168 hours. The immersion liquid after storage was collected as a test liquid, and the metal content was measured using inductively coupled plasma mass spectrometry ICP-MS (manufactured by PerkinElmer, product name "ELAN DRC II"). The total metal content of six elements, Al, Fe, Co, Mo, Cr, and Ni, which are derived from residual metal impurities in the CNT, was calculated as the amount of metal elution. The smaller the value of the amount of metal elution, the better the cleanliness.

[0047] Example 1 Oxidation Treatment of CNTs 20 mL of 17% by mass hydrochloric acid was added to 0.1 g of single-walled carbon nanotubes (manufactured by Zeon Corporation, product name "ZEONANO (registered trademark) SG101") and oxidized by heating under reflux with stirring in an oil bath at 150°C for 6 hours. After cooling to room temperature, the mixture was filtered using a PTFE membrane filter with a pore size of 0.1 μm. The filtrate was then washed with ultrapure water until the pH was neutral. The resulting solid was collected and vacuum-dried overnight at 120°C using a vacuum dryer to obtain oxidized carbon nanotubes. The G / D ratio and ash content of the resulting oxidized carbon nanotubes were measured. The results are shown in Table 1. <Preparation of Composite Material> In a 1 L glass bottle, 400 g of cyclohexane as a dispersion medium, 99.95 g of PTFE (polytetrafluoroethylene) fluororesin particles (manufactured by AGC, product name "Fluon PTFE G163", average particle size: 25 μm, specific gravity: 2.15 g / mL), and 0.05 g of the oxidized carbon nanotubes obtained above were mixed, and the mixture was stirred at 20°C and 12,000 rpm for 15 minutes using a homogenizer (manufactured by Primix Corporation, product names "Labo-Lution" (registered trademark), Neokaiser (registered trademark)) to obtain a slurry containing the fluororesin particles and the oxidized carbon nanotubes. The slurry was then centrifuged using a centrifuge (manufactured by Thinky Corporation, product name "Awatori Rentaro ARE-310"). The supernatant dispersion medium was then removed. The mixture was then dried in a vacuum dryer (manufactured by Yamato Scientific Co., Ltd.) at 125°C for 2 hours to obtain a composite (composite material) of fluororesin and oxidized carbon nanotubes. The resulting composite material was then evaluated for impurity content. The results are shown in Table 1. <Preparation of Molded Product> The resulting composite material was then pulverized in a mill mixer. The resulting composite material particles were placed in a mold and preformed using a compression molding machine (manufactured by Dumbbell, product name "SDOP-13021V-2HC-AT") at 20°C, 9 MPa, and a pressure holding time of 5 minutes to obtain a sheet-like preform measuring 130 mm long, 80 mm wide, and 2 mm thick. The preform was then demolded and baked in a hot air circulating oven under nitrogen at 370°C for 6 hours to obtain a molded product. The volume resistivity and metal elution amount of the resulting molded product were then measured.The results are shown in Table 1.

[0048] Example 2 Oxidized carbon nanotubes, a composite material, and a molded product were obtained in the same manner as in Example 1, except that carbon nanotubes (manufactured by OCSiAl Corporation, product name "TUBALL") were used instead of single-walled carbon nanotubes (manufactured by Zeon Corporation, product name "ZEONANO (registered trademark) SG101"), and the blending ratios of the fluororesin particles and the oxidized carbon nanotubes were changed as shown in Table 1. Then, various measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0049] (Example 3) Oxidized carbon nanotubes, a composite material, and a molded product were obtained in the same manner as in Example 1, except that carbon nanotubes (manufactured by JEIO Corporation, product name "JC142") were used instead of single-walled carbon nanotubes (manufactured by Zeon Corporation, product name "ZEONANO (registered trademark) SG101"), and the blending ratios of the fluororesin particles and the oxidized carbon nanotubes were changed as shown in Table 1. Then, various measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0050] Example 4 Oxidized carbon nanotubes, a composite material, and a molded article were obtained in the same manner as in Example 1, except that PTFE fluororesin particles (manufactured by AGC, product name "Fluon PTFE G163," average particle size: 25 μm, specific gravity: 2.15 g / mL) were replaced with PCTFE (polychlorotrifluoroethylene) fluororesin particles (manufactured by Daikin Industries, Ltd., product name "Neoflon PCTFE M-400H," which were immersed in liquid nitrogen in a freeze-pulverizer and then freeze-pulverized three times at a pulverization temperature of -90°C, with a median particle size of 100 μm). The blending ratios of the fluororesin particles and oxidized carbon nanotubes were changed as shown in Table 1. Various measurements were then performed in the same manner as in Example 1. The results are shown in Table 1.

[0051] Example 5 Oxidized carbon nanotubes, a composite material, and a molded article were obtained in the same manner as in Example 1, except that PTFE fluororesin particles (manufactured by AGC, product name "Fluon PTFE G163," average particle size: 25 μm, specific gravity: 2.15 g / mL) were replaced with fluororesin particles made of PFA (a copolymer of tetrafluoroethylene and perfluoroalkoxyethylene) (manufactured by AGC, product name "Fluon PFA P-36P," cotton-like particles with a median particle size of 150 μm obtained by immersing the particles in liquid nitrogen in a freeze-pulverizer and then freeze-pulverizing them three times at a grinding temperature of -90°C), and the blending ratio of the fluororesin particles and oxidized carbon nanotubes was changed as shown in Table 1. Various measurements were then performed in the same manner as in Example 1. The results are shown in Table 1.

[0052] (Comparative Example 1) A composite material and a molded article were obtained in the same manner as in Example 1, except that no oxidation treatment of the CNTs was performed and commercially available oxidized carbon nanotubes (manufactured by Sigma-Aldrich, product name "Multi-walled Carbon Nanotubes", outer diameter: 6 to 13 nm, length: 2.5 to 20 μm) were used, and the blending ratio of the fluororesin particles and the oxidized carbon nanotubes was changed as shown in Table 1. Then, various measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0053] Comparative Example 2: Without carrying out the oxidation treatment of CNT, carbon nanotubes (manufactured by Kumho Petrochemical Co., Ltd., product name "K-nanos 100P", BET specific surface area: 259 m) were used instead of oxidized carbon nanotubes. 2 A composite material and a molded article were obtained in the same manner as in Example 1, except that a fluororesin particle (100%) was used and the blending ratio of the fluororesin particles and the carbon nanotubes was changed as shown in Table 1. Various measurements were then carried out in the same manner as in Example 1. The results are shown in Table 1.

[0054] (Comparative Example 3) A composite material and a molded article were obtained in the same manner as in Example 1, except that no oxidation treatment of the CNTs was performed, carbon nanotubes (manufactured by Nanosil Co., Ltd., product name "Nanosil NC7000") were used instead of oxidized carbon nanotubes, and the blending ratio of the fluororesin particles and carbon nanotubes was changed as shown in Table 1. Then, various measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0055] (Comparative Example 4) A composite material and a molded article were obtained in the same manner as in Example 1, except that no oxidation treatment of the CNTs was performed, carbon nanotubes (manufactured by JEIO, product name "JC142") were used instead of oxidized carbon nanotubes, and the blending ratios of the fluororesin particles and carbon nanotubes were changed as shown in Table 1. Then, various measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0056] (Comparative Example 5) A composite material and a molded body were obtained in the same manner as in Example 1, except that no oxidation treatment of the CNTs was performed, carbon nanotubes (manufactured by OCSiAl Corporation, product name "TUBALL") were used instead of oxidized carbon nanotubes, and the blending ratios of the fluororesin particles and carbon nanotubes were changed as shown in Table 1. Then, various measurements were performed in the same manner as in Example 1. The results are shown in Table 1.

[0057]

[0058] From Table 1, in Examples 1 to 5, the volume resistivity was 1×10 3 ~1 x 10 8 It is clear that the amount of metal elution can be reduced while maintaining electrical conductivity of about Ω·cm.

[0059] According to the present invention, it is possible to obtain a composite material and a molded article that are electrically conductive and have a small amount of metal elution.

Claims

1. A composite material comprising a fluororesin and oxidized carbon nanotubes, the composite material having an impurity content of less than 10 ppm.

2. Volume resistivity is 1 x 10 3 Ω・cm or more 1×10 8 3. The composite material of claim 1, having a resistivity of Ω·cm or less.

3. The composite material according to claim 1, wherein the content of the oxidized carbon nanotubes is 0.005% by mass or more and 0.2% by mass or less.

4. The composite material of claim 1, wherein the oxidized carbon nanotubes have an ash content of less than 3% by mass.

5. The composite material of claim 1, wherein the oxidized carbon nanotubes have a G / D ratio of 0.5 or greater.

6. The composite material according to claim 1, wherein the fluororesin is at least one selected from the group consisting of polytetrafluoroethylene, polychlorotrifluoroethylene, and a copolymer of tetrafluoroethylene and perfluoroalkoxyethylene.

7. A molded article obtained by molding the composite material according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Valve device

    JP2018173170A

  • Member for conveying semiconductor substrate and manufacturing apparatus of semiconductor device having the same

    JP2020119923A

  • Resin composition for secondary battery electrode, method for manufacturing mixture slurry for secondary battery electrode, method for manufacturing electrode membrane, and method for manufacturing secondary battery

    JP2023012943A

  • Method For Manufacturing The Conductive Transparent And Superhydrophobic Film Using Carbon Nanotube

    KR1020120034370A

  • Fibrous carbon nanostructure dispersion and method for producing same, and fibrous carbon nanostructure

    WO2018180901A1