Laminated glass and method for manufacturing same

The laminated glass design addresses foaming issues in high-temperature environments by using a P-polarized light reflecting coating and a wedge-shaped interlayer film with specific wedge angles, ensuring proper alignment and reducing bubble formation, thereby improving durability and visibility.

WO2024204369A1PCT designated stage expired Publication Date: 2024-10-03AGC INC

Patent Information

Application Number
PCT/JP2024/012280
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Laminated glass with a coating film that reflects P-polarized light is prone to foaming in the interlayer film, especially when exposed to high-temperature environments, due to differences in curvature between the inside and outside glass sheets, which can lead to mismatched bending behavior and subsequent foaming, particularly in designs with a wedge-shaped interlayer film.

Method used

The laminated glass design includes a coating film with a visible light reflectance of 10% or more for P-polarized light at an incident angle of 65 degrees, and an interlayer film with a wedge-shaped cross-section where the thickness increases from the lower side to the upper side, with local wedge angles α and β configured such that (β−α)>0.05 [mrad], to minimize foaming by ensuring the glass plates are pressed together nearly parallel at the lower edge, reducing the likelihood of bubble formation.

Benefits of technology

This configuration effectively reduces the occurrence of foaming in the interlayer film, even under harsh temperature conditions, while maintaining the visibility of the HUD image by minimizing double images and ensuring the glass plates are properly aligned, thus enhancing the durability and performance of the laminated glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012280_03102024_PF_FP_ABST
    Figure JP2024012280_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is laminated glass, comprising a curved first glass sheet, a curved second glass sheet, and an intermediate film located between the first glass sheet and the second glass sheet and bonding the first glass sheet and the second glass sheet together, wherein: a coating film is provided that has a visible light reflectance of at least 10% with respect to P-polarized visible light incident at an angle of incidence of 65 degrees; the intermediate film comprises a region with a wedge-shaped cross-section having a thickness that gradually increases from the lower side to the upper side in a state in which the laminated glass has been attached to a vehicle; and, on a straight line that passes through a first point that divides the upper side in two and a second point that divides the lower side in two in plan view, a local wedge angle α at a position 100 mm from the second point and a local wedge angle β at a position 500 mm from the second point satisfy the formula (β − α) > 0.05 [mrad].
Need to check novelty before this filing date? Find Prior Art

Description

Laminated glass and its manufacturing method

[0001] The present invention relates to laminated glass and a method for producing the same.

[0002] In head-up displays (hereinafter also referred to as HUDs), one technology is to apply a coating film that reflects P-polarized light to laminated glass to improve the brightness of the image and ensure visibility even when wearing polarized sunglasses. Another technology also reduces double images by combining such a coating film with an interlayer film that has a wedge-shaped cross section.

[0003] International Publication No. 2022 / 207004

[0004] In laminated glass having a coating film that reflects P-polarized light, for example, when left in a high-temperature environment for a long period of time, bubbles may form in the interlayer film, mainly near the bottom edge of the laminated glass. This bubbles occur because the coating film provided on one of the interior and exterior glass sheets that make up the laminated glass causes the glass sheets to behave differently when bent according to the vehicle design, resulting in different shapes, specifically, different curved shapes, at the periphery of each glass sheet. Bubbling in the interlayer film occurs particularly noticeably near the bottom edge of laminated glass in laminated glass having an interlayer film with a wedge-shaped cross section that thickens from the bottom edge to the top edge.

[0005] The present invention has been made in view of the above points, and has an object to make it difficult for bubbles to form in an interlayer film in a laminated glass having a coating film and an interlayer film with a wedge-shaped cross section.

[0006] A laminated glass according to one embodiment of the disclosure is a laminated glass comprising a curved first glass plate, a curved second glass plate, and an interlayer film positioned between the first glass plate and the second glass plate and bonding the first glass plate to the second glass plate, wherein the first glass plate has a fourth surface and a third surface, and the second glass plate has a first surface and a second surface, the fourth surface being a surface of the first glass plate opposite to the interlayer film, the third surface being a surface of the first glass plate facing the interlayer film, the second surface being a surface of the second glass plate facing the interlayer film, and the first surface being a surface of the second glass plate opposite to the interlayer film. a coating film is provided on the second surface, the third surface, or the fourth surface, and the coating film is configured to have a visible light reflectance of 10% or more for P-polarized visible light incident at an incident angle of 65°; the interlayer film has a region with a wedge-shaped cross section whose thickness gradually increases from the lower edge to the upper edge when the laminated glass is installed in a vehicle; and on a line passing through a first point that bisects the upper edge and a second point that bisects the lower edge in a plan view, a local wedge angle α at a position 100 mm away from the second point and a local wedge angle β at a position 500 mm away from the second point satisfy the equation: (β - α) > 0.05 mrad.

[0007] According to one embodiment of the disclosure, in a laminated glass having a coating film and an interlayer film with a wedge-shaped cross section, bubbles are less likely to occur in the interlayer film.

[0008] FIG. 2A is a schematic diagram illustrating a HUD system according to the first embodiment. FIG. 2A and FIG. 2B are diagrams illustrating laminated glass according to the first embodiment. FIG. 2B is a diagram (part 1) illustrating a local wedge angle. FIG. 2C is a diagram (part 2) illustrating a local wedge angle. FIG. 5A to FIG. 5C are diagrams (part 1) illustrating a method for manufacturing laminated glass. FIG. 6A and FIG. 6B are diagrams (part 2) illustrating a method for manufacturing laminated glass. FIG. 6A is a partial cross-sectional view illustrating laminated glass according to Modification 1 of the first embodiment. FIG. 6B is a cross-sectional view illustrating laminated glass according to Modification 2 of the first embodiment. FIG. 10A and FIG. 10B are cross-sectional views illustrating laminated glass according to Modification 4 of the first embodiment. FIG. 10C are diagrams illustrating examples and comparative examples.

[0009] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. In each drawing, the same components are designated by the same reference numerals, and duplicate explanations may be omitted. In each drawing, the size or shape may be partially exaggerated to make the contents of the present invention easier to understand.

[0010] In the following description, the term "vehicle" refers to any moving body capable of mounting laminated glass, including, but not limited to, automobiles, trains, ships, and aircraft.

[0011] Furthermore, in the following description, a planar view refers to viewing an object from the direction of a normal line passing through the center of gravity of the main surface of the object, and the shape seen in this way is referred to as a planar shape.

[0012] In addition, the terms "top" and "bottom" used in the following description refer to the top and bottom when the laminated glass is installed in a vehicle.

[0013] In the following description, the outermost edge of a given member is referred to as the "periphery," and an area of ​​the given member having a width that is inscribed in the "periphery" is referred to as the "periphery portion."

[0014] First Embodiment [HUD System] Fig. 1 is a schematic diagram illustrating a HUD system according to a first embodiment. The HUD system 1 shown in Fig. 1 includes a laminated glass 10, a light source 50, a first optical system 60, an image display element 70, a second optical system 80, and a concave mirror 90. The HUD system 1 is a head-up display system for a vehicle that displays a virtual image on the vehicle exterior side of the laminated glass 10. Note that in the HUD system 1, the first optical system 60 and the second optical system 80 may be provided as needed.

[0015] The laminated glass 10 is, for example, a windshield for a vehicle, and P-polarized visible light is incident on the laminated glass 10 from the inside of the vehicle. The laminated glass 10 is provided with a coating film 15 in an area where the P-polarized visible light reflected by the concave mirror 90 is incident. The coating film 15 may be formed on the entire surface of the laminated glass 10, or may be formed on only a portion of the laminated glass 10. It is sufficient that the coating film 15 is formed on at least an area where P-polarized light from the light source 50 is irradiated. The edge of the coating film 15 may be formed near the outer periphery of the laminated glass 10 or on or near the shielding layer to make the edge less noticeable.

[0016] The light source 50 is a light source that emits P-polarized visible light, and is, for example, a light-emitting diode or a laser. The light source 50 may include optical components such as a polarizing plate or a lens that converts S-polarized light into P-polarized light. The light source 50 is configured with, for example, three light sources: a red light source, a green light source, and a blue light source.

[0017] The first optical system 60 is composed of, for example, a prism or a lens that combines light emitted from multiple light sources. The image display element 70 is an element that generates an intermediate image, such as a liquid crystal display element or an organic light-emitting element. The second optical system 80 is composed of, for example, a lens or a reflecting mirror. The concave mirror 90 is an optical component that reflects the intermediate image with a reflective surface having a predetermined curvature, and is located closest to the laminated glass 10 among the optical components located on the optical path between the light source 50 and the laminated glass 10.

[0018] In the HUD system 1, light emitted from the light source 50 passes through a first optical system 60 and reaches an image display element 70, where an intermediate image is formed. The intermediate image formed by the image display element 70 is magnified by passing through a second optical system 80 and a concave mirror 90, and is then projected onto a coating film 15 on a laminated glass 10. The intermediate image projected onto the coating film 15 is mainly reflected by the coating film 15 and directed to a viewpoint I of a vehicle occupant, who then recognizes the intermediate image as a virtual image V (HUD image) in front of the laminated glass 10. The occupant may be, for example, the driver of the vehicle.

[0019] 1, θ is the angle of incidence when P-polarized visible light emitted from light source 50 is incident on coating film 15 via the predetermined optical system. The angle of incidence θ may be 57° (Brewster's angle), or may be greater than 57°, or may be less than 57°.

[0020] The HUD system 1 may have any configuration as long as it includes at least the laminated glass 10 and the light source 50. The HUD system 1 may be, for example, a laser scanning system in which a laser beam is scanned by an optical scanning unit formed of a microelectromechanical system (MEMS) or the like.

[0021] [Laminated Glass] Figures 2A and 2B are diagrams illustrating laminated glass according to the first embodiment. Figure 2A is a schematic diagram showing the laminated glass as viewed from inside the vehicle toward the outside of the vehicle, and Figure 2B is a cross-sectional view taken along line A-A in Figure 2A.

[0022] As shown in Fig. 2B, the laminated glass 10 is a laminated glass for a vehicle that includes a first glass plate 11, a second glass plate 12, an interlayer film 13, shielding layers 14A and 14B, and a coating film 15. The laminated glass 10 can be used, for example, as a windshield of a vehicle.

[0023] The first glass sheet 11 and the second glass sheet 12 are bonded together via an interlayer film 13. The first glass sheet 11 is disposed on a first side that faces the interior side of the vehicle when the laminated glass 10 is installed in the vehicle, and the second glass sheet 12 is disposed on a second side that faces the exterior side of the vehicle when the laminated glass 10 is installed in the vehicle. The shielding layers 14A and 14B are provided as needed.

[0024] The laminated glass 10 has, for example, a complex curved shape that is curved in both the vertical and horizontal directions when installed in a vehicle. However, the complex curved shape is not limited to a shape that is curved in both the vertical and horizontal directions when installed in a vehicle, but includes a shape that is curved in any two or more different directions. Alternatively, the laminated glass 10 may have a single curved shape that is curved in only one of the vertical or horizontal directions when installed in a vehicle. However, the single curved shape is not limited to a shape that is curved in only the vertical or horizontal direction when installed in a vehicle, but includes a shape that is curved in only one of the directions.

[0025] The laminated glass 10 is preferably curved so as to be convex toward the exterior of the vehicle. That is, the second glass sheet 12 is preferably curved so as to be convex toward the side opposite the interlayer film 13, and the first glass sheet 11 is preferably curved so as to be convex toward the interlayer film 13.

[0026] The first glass sheet 11 is an interior glass sheet that faces the interior side (first side) of the vehicle when the laminated glass 10 is installed in the vehicle. The first glass sheet 11 is curved. The first glass sheet 11 has a fourth surface 11 located on the opposite side from the interlayer film 13. 4 , and a third surface 11 facing the intermediate film 13 3 In the plan view shown in Fig. 2A, reference numeral 11t denotes an upper edge that is positioned on the upper side when the laminated glass 10 is installed in a vehicle. Reference numeral 11b denotes a lower edge that is positioned on the lower side when the laminated glass 10 is installed in a vehicle. The first glass sheet 11 includes an upper edge 11t, a lower edge 11b, and two side edges that connect the upper edge 11t and the lower edge 11b.

[0027] The second glass sheet 12 is an exterior glass sheet that faces the exterior side (second side) of the vehicle when the laminated glass 10 is installed in the vehicle. The second glass sheet 12 is curved. The second surface 12 of the second glass sheet 12 faces the interlayer film 13. 2 , and a first surface 12 located on the opposite side to the intermediate film 13 1 Similar to the first glass plate 11, the second glass plate 12 has, in plan view, an upper side, a lower side, and two side sides connecting the upper side and the lower side.

[0028] In the laminated glass 10, the minimum value of the radius of curvature is preferably 500 mm or more and 100,000 mm or less. The radii of curvature of the first glass sheet 11 and the second glass sheet 12 may be the same or different. When the radii of curvature of the first glass sheet 11 and the second glass sheet 12 are different, it is preferable that the radius of curvature of the first glass sheet 11 is smaller than the radius of curvature of the second glass sheet 12.

[0029] The first glass plate 11 and the second glass plate 12 are a pair of glass plates facing each other, and the interlayer film 13 is located between the pair of glass plates. The first glass plate 11 and the second glass plate 12 are fixed together with the interlayer film 13 sandwiched therebetween. The interlayer film 13 is a film that bonds the first glass plate 11 and the second glass plate 12 together.

[0030] The outer peripheral side surface of the interlayer film 13 is preferably edge-treated. That is, the outer peripheral side surface of the interlayer film 13 is preferably treated so as not to protrude significantly from the outer peripheral side surfaces of the first glass plate 11 and the second glass plate 12. From the viewpoint of not impairing the appearance, it is preferable that the amount by which the outer peripheral side surface of the interlayer film 13 protrudes from the outer peripheral side surfaces of the first glass plate 11 and the second glass plate 12 is 150 μm or less. Details of the first glass plate 11, the second glass plate 12, and the interlayer film 13 will be described later.

[0031] The shielding layers 14A and 14B are opaque layers and are provided, for example, in the form of strips along the peripheral edge of the laminated glass 10. The shielding layers 14A and 14B are, for example, opaque colored ceramic layers and may be any color, but dark colors such as black, brown, gray, and dark blue are preferred, with black being more preferred. The shielding layers 14A and 14B may be a colored interlayer or film with light-blocking properties, a combination of a colored interlayer and a colored ceramic layer, or a layer with a light-adjusting function. The colored film may be integrated with an infrared reflective film or the like.

[0032] The width of the shielding layers 14A and 14B in a plan view is, for example, approximately 10 mm to 250 mm, preferably 20 mm to 220 mm, and more preferably 30 mm to 200 mm. The width of the shielding layers 14A and 14B may be the same or different. The presence of the opaque shielding layers 14A and 14B in the laminated glass 10 suppresses ultraviolet degradation of the adhesive made of a resin such as urethane that holds the peripheral edge of the laminated glass 10 to the vehicle body, and also improves the appearance by making the adhesive invisible from outside the vehicle.

[0033] The shielding layers 14A and 14B can be formed, for example, by applying a ceramic color paste containing a fusible glass frit containing a black pigment onto a glass plate by screen printing or the like, and then firing the paste. The method for forming the shielding layers 14A and 14B is not limited to this. The shielding layers 14A and 14B may also be formed, for example, by applying an organic ink containing a black or dark color pigment onto a glass plate by screen printing or the like, and then drying the ink.

[0034] The shielding layer 14A is, for example, a fourth surface 11 of the first glass plate 11. 4 The shielding layer 14A can be provided on the peripheral edge of the fourth surface 11 of the first glass plate 11 via the coating film 15. 4 The shielding layer 14A may be provided on the peripheral portion of the fourth surface 11 of the first glass plate 11. 4 In the example of FIG. 2 , the shielding layer 14A may be provided on the entire peripheral portion of the fourth surface 11 of the first glass plate 11 in a plan view, or may be provided on a part of the peripheral portion. 42A and 2B, the fourth surface 11 of the first glass plate 11 is provided only on the outer edge portions of the upper side 11t and the two side sides. 4 The shielding layer 14A is not provided on the outer edge portion close to the lower side 11b.

[0035] The shielding layer 14B is, for example, a second surface 12 2 The shielding layer 14B may be provided on the peripheral edge of the second surface 12 of the second glass plate 12. 2 The shielding layer 14B may be provided on a part of the peripheral edge of the second surface 12 of the second glass plate 12. 2 2A and 2B, the shielding layer 14B may be provided on the entire peripheral portion of the second surface 12 of the second glass plate 12, or on a part of the peripheral portion. 2 It is to be noted that only one of the shielding layers 14A and 14B may be provided.

[0036] The laminated glass 10 may have an information transmission / reception area 16. The information transmission / reception area 16 is provided within an opening in the shielding layer 14A and / or 14B of the laminated glass 10. That is, if the laminated glass 10 has only the shielding layer 14A, the information transmission / reception area 16 is provided within the opening in the shielding layer 14A. If the laminated glass 10 has only the shielding layer 14B, the information transmission / reception area 16 is provided within the opening in the shielding layer 14B. If the laminated glass 10 has both the shielding layers 14A and 14B, the information transmission / reception area 16 is provided at a position where the opening in the shielding layer 14A overlaps with the opening in the shielding layer 14B.

[0037] The information transmission / reception area 16 is provided, for example, at the upper peripheral edge of the laminated glass 10. The information transmission / reception area 16 is an area where, for example, an information device that handles visible light, such as a visible light camera or an illuminance sensor, or an information device that handles infrared light, such as a LiDAR (Light Detection and Ranging) sensor, transmits and / or receives information. In other words, when the laminated glass 10 is installed in a vehicle, the information device can be placed on the interior side of the information transmission / reception area 16.

[0038] A HUD display area R used for a head-up display is defined in a part of the laminated glass 10. The HUD display area R is an area that allows P-polarized light to be incident from the first glass plate 11. The HUD display area R is not limited to one location, and may be, for example, divided into multiple locations in the vertical direction or multiple locations in the horizontal direction within the laminated glass 10 in a plan view.

[0039] The HUD display area R reflects a projected image from inside the vehicle and displays information. The HUD display area R is the range in the eye box based on SAE J1757-2 (2018) where light from the light source 50 is irradiated onto the laminated glass 10 when the HUD display position is moved. The HUD display area R is, for example, the fourth surface 11 of the first glass plate 11. 4 is located near the bottom side 11b.

[0040] In the HUD display area R and its surrounding area, the fourth surface 11 of the first glass plate 11 4 A coating film 15 is disposed on the entire laminated glass 10. The coating film 15 may be disposed over the entire HUD display region R, as long as it is disposed so as to include the entire HUD display region R. In the example of Figures 2A and 2B, the coating film 15 is disposed over the entire laminated glass 10. Disposing the coating film 15 over the entire laminated glass 10 is advantageous in that the boundary between the region where the coating film 15 is disposed and the surrounding region is not visible.

[0041] The coating film 15 is a film that reflects P-polarized visible light incident from the concave mirror 90 toward the inside of the vehicle. 4The coating film 15 is transparent to visible light. The thickness of the coating film 15 is, for example, 50 nm or more and 500 nm or less. The coating film 15 is configured so that the visible light reflectance Rva is 10% or more when P-polarized visible light is incident at an incident angle of 65 degrees. The visible light reflectance Rva is measured by measuring the spectral reflectance specified in ISO 9050:2003 using P-polarized light in visible wavelengths as incident light at an incident angle θ = 65 degrees, and then calculating the visible light reflectance Rva based on this measurement in accordance with the calculation method for visible light reflectance specified in ISO 9050:2003.

[0042] Examples of the coating film 15 include a film having a laminated structure of a high refractive index film / a low refractive index film, an infrared reflective film having a laminated structure of a metal film such as silver and a dielectric film, and a low-e film made of a transparent conductive film such as ITO. Among these, a film having a laminated structure of a high refractive index film / a low refractive index film is preferred in terms of maintaining a high P-polarized light reflectance. When the high refractive index film / a low refractive index film has a two-layer structure, for example, the fourth surface 11 of the first glass plate 11 is preferably coated with the high refractive index film / a low refractive index film. 4 When the high refractive index film / low refractive index film has a three-layer structure or more, the fourth surface 11 of the first glass plate 11 is laminated with the high refractive index film and the low refractive index film in this order. 4 High refractive index films and low refractive index films are alternately laminated in any order on the substrate.

[0043] The refractive index of the high-refractive-index film is preferably 1.8 or more, 1.9 or more, 2.0 or more, or 2.1 or more, and preferably 2.5 or less, at a wavelength of 550 nm. The refractive index of the low-refractive-index film is typically less than 1.8, 1.7 or less, or 1.6 or less, and preferably 1.2 or more, at a wavelength of 550 nm.

[0044] Specifically, the high-refractive-index film preferably contains at least one of the following: oxides of Zr, Nb, or Sn; mixed oxides containing at least two of Ti, Zr, Nb, Si, Sb, Sn, Zn, and In; nitrides of Si and Zr; and mixed nitrides of Si or Zr. The low-refractive-index film preferably contains at least one of silicon oxide, silicon oxynitride, silicon oxycarbide, and mixed oxides. Examples of mixed oxides include mixed oxides of silicon and aluminum, and mixed oxides of silicon and zirconium.

[0045] The first layer of the high refractive index film is optionally made up of one or more sublayers. The thickness (geometric film thickness) of the first layer of the high refractive index film is preferably 50 nm or more and 100 nm or less, particularly 60 nm or more and 80 nm or less. The first layer of the low refractive index film is optionally made up of one or more sublayers. The thickness (geometric film thickness) of the first layer of the low refractive index film is preferably 70 nm or more and 160 nm or less, particularly 100 nm or more and 140 nm or less.

[0046] Generally, in a HUD system having a coating film 15, a light source or an optical system is installed so that the angle of incidence of P-polarized light incident on the coating film 15 is approximately 57 degrees. However, in a HUD system having a coating film 15, there are limitations on the position in the vehicle where the light source or optical system can be installed, and therefore the angle of incidence θ may deviate from 57 degrees.

[0047] In the HUD system 1, the closer the HUD display region R is to the bottom edge of the laminated glass 10, the larger the incident angle θ tends to be. For example, when the incident angle θ is 67 degrees or 72 degrees, more light passes through the coating film 15. Therefore, unless some countermeasures are taken, more light is reflected from surfaces of the laminated glass 10 that are closer to the exterior of the vehicle than the coating film 15. As a result, when P-polarized visible light is incident on the laminated glass 10, a virtual image may appear as a split image. This split image is a double image, and the appearance of a double image reduces the visibility of the HUD image.

[0048] Therefore, in the HUD display region R, the intermediate film 13 is disposed on the fourth surface 11 of the first glass plate 11 when the laminated glass 10 is installed in the vehicle.4 The interlayer film 13 has a wedge-shaped cross-sectional area whose thickness gradually increases from the bottom edge to the top edge. By irradiating P-polarized light onto the wedge-shaped cross-sectional area of ​​the interlayer film 13, the distance between the main image and the double image can be reduced so that the main image and the double image nearly overlap, even when the incident angle θ deviates from 57 degrees, making the double image less noticeable.

[0049] As shown in FIG. 3 , in the laminated glass 10 , the fourth surface 11 of the first glass plate 11 is 4 An imaginary line passing through a first point Pt that bisects the upper side 11t of the glass plate 11 and a second point Pb that bisects the lower side 11b is defined as a straight line S1. 4 3 indicates a position at a distance L1 of 100 mm from the second point Pb when measured along the line S1. 4 1 indicates a position at a distance L2 of 500 mm from the second point Pb when measured along the line .

[0050] 4 is a partial cross-sectional view taken along the line S1 in FIG. 3. In FIG. 4, the symbol N1 indicates a line passing through the point P1 on the fourth surface 11 of the first glass plate 11. 4 The normal line N2 of the fourth surface 11 of the first glass plate 11 passes through the point P2. 4 As shown in Fig. 4, the local wedge angle α at point P1 located 100 mm away from the second point Pb is larger than the local wedge angle β at point P2 located 500 mm away from the second point Pb.

[0051] Here, the local wedge angle at a certain point P is defined as a value obtained by dividing the change in thickness of the interlayer film 13 within a range of ±40 mm from the point P on the line S1 by the distance therebetween, 80 mm. 4 The measurement shall be taken along the normal to the

[0052] That is, the local wedge angle α at the position of point P1 is equal to ((thickness of the intermediate film 13 at 100 mm + 40 mm) - (thickness of the intermediate film 13 at 100 mm - 40 mm)) / 80 mm. Also, the local wedge angle β at the position of point P2 is equal to ((thickness of the intermediate film 13 at 500 mm + 40 mm) - (thickness of the intermediate film 13 at 500 mm - 40 mm)) / 80 mm.

[0053] The conspicuousness of the secondary image also varies depending on the projection distance of the HUD image. The projection distance of the HUD image is preferably 2 m or more, more preferably 3 m or more, even more preferably 5 m or more, and particularly preferably 10 m or more. Here, the projection distance of the HUD image is the distance from the center of the eyebox to the focal position of the virtual image V based on SAE J1757-2 (2018). The method for measuring the focal length of the HUD is based on SAE J1757-2 (2018). As the projection distance of the HUD image increases, the secondary image becomes darker and the amount of separation of the secondary image from the main image is reduced, making the secondary image less noticeable. Furthermore, as the projection distance of the HUD image increases, the HUD image approaches the focal distance of the driver while driving, improving the visibility of the HUD image.

[0054] Here, the first glass plate 11, the second glass plate 12, and the interlayer film 13 will be described in detail.

[0055] [Glass Plates] The first glass plate 11 and the second glass plate 12 may be inorganic glass or organic glass. Examples of inorganic glass include soda-lime glass, aluminosilicate glass, borosilicate glass, alkali-free glass, and quartz glass, without any particular limitations. The second glass plate 12, which is on the vehicle exterior side of the laminated glass 10, is preferably inorganic glass from the viewpoint of scratch resistance, and soda-lime glass from the viewpoint of formability. When the first glass plate 11 and the second glass plate 12 are soda-lime glass, clear glass, green glass containing a predetermined amount or more of iron, and dark green glass are preferably used. Glass that absorbs ultraviolet or infrared light may also be used. Transparent glass is preferred, but colored glass may also be used to the extent that transparency is not impaired.

[0056] The inorganic glass may be either untempered glass or tempered glass. Untempered glass is produced by forming molten glass into a flat plate and slowly cooling it. Tempered glass is produced by forming a compressive stress layer on the surface of untempered glass. Tempered glass can reduce residual stress by isotropically distributing stress.

[0057] The tempered glass may be either physically tempered glass such as air-cooled tempered glass or chemically tempered glass. Physically tempered glass can be tempered by generating a compressive stress layer on the glass surface due to the temperature difference between the glass surface and the interior of the glass through an operation other than gradual cooling, such as rapidly cooling a uniformly heated glass sheet from a temperature near its softening point during bending.

[0058] For example, chemically strengthened glass can be strengthened by bending and then applying compressive stress to the glass surface by an ion exchange method or the like.

[0059] Examples of materials for the organic glass include polycarbonate, acrylic resins such as polymethyl methacrylate, polyvinyl chloride, and transparent resins such as polystyrene.

[0060] The first glass sheet 11 and the second glass sheet 12 are not limited to a trapezoidal or rectangular shape, and may be processed into various shapes and curvatures. The first glass sheet 11 and the second glass sheet 12 may be bent using a gravity forming method, a press forming method, a roller forming method, or the like. The forming method for the first glass sheet 11 and the second glass sheet 12 is also not particularly limited. For example, the inorganic glass is preferably a glass sheet formed by a float method or the like.

[0061] The thickness of the second glass sheet 12 at its thinnest portion is preferably 1.1 mm or more and 3 mm or less. When the thickness of the second glass sheet 12 is 1.1 mm or more, the strength, such as resistance to flying stones, is sufficient. When the thickness of the second glass sheet 12 is 3 mm or less, the mass of the laminated glass 10 does not become too large, which is preferable in terms of vehicle fuel efficiency. The thickness of the second glass sheet 12 at its thinnest portion is more preferably 1.8 mm or more and 2.8 mm or less, even more preferably 1.8 mm or more and 2.6 mm or less, even more preferably 1.8 mm or more and 2.2 mm or less, and even more preferably 1.8 mm or more and 2.1 mm or less.

[0062] The thickness of the first glass plate 11 is preferably 0.3 mm or more and 2.3 mm or less. When the thickness of the first glass plate 11 is 0.3 mm or more, the handleability is good. When the thickness of the first glass plate 11 is 2.3 mm or less, the mass does not become too large.

[0063] Furthermore, if the thickness of the first glass sheet 11 is not appropriate, when two sheets of glass with particularly deep curvatures are used as the first glass sheet 11 and the second glass sheet 12 to form laminated glass, a mismatch will occur between the shapes of the two sheets, which will have a significant impact on the quality of the glass, such as residual stress after crimping.

[0064] However, by setting the thickness of the first glass sheet 11 to 0.3 mm or more and 2.3 mm or less, glass quality such as residual stress can be maintained. Setting the thickness of the first glass sheet 11 to 0.3 mm or more and 2.3 mm or less is particularly effective in maintaining glass quality in glass with a deep curvature. The thickness of the first glass sheet 11 is more preferably 0.5 mm or more and 2.2 mm or less, and even more preferably 0.7 mm or more and 2.1 mm or less. If the thickness of the first glass sheet 11 is within these ranges, the above-mentioned effects become even more pronounced.

[0065] A coating having water repellency, ultraviolet or infrared blocking properties, or a coating having low reflectivity or low radiation properties may be provided on the outer side of the first glass plate 11 and / or the second glass plate 12. Furthermore, a coating having ultraviolet or infrared blocking properties, low radiation properties, visible light absorption properties, coloring, or the like may be provided on the side of the first glass plate 11 and / or the second glass plate 12 that contacts the interlayer film 13.

[0066] When the first glass sheet 11 and the second glass sheet 12 are curved inorganic glass sheets, the first glass sheet 11 and the second glass sheet 12 are bent after being formed by a float method or the like and before being bonded with the interlayer film 13. The bending is performed by heating the glass to soften it. The heating temperature of the glass during bending is preferably controlled within a range of approximately 550°C to 700°C.

[0067] [Interlayer Film] Thermoplastic resins are often used for the interlayer film 13, and examples thereof include thermoplastic resins that have conventionally been used for this type of application, such as plasticized polyvinyl acetal resins, plasticized polyvinyl chloride resins, saturated polyester resins, plasticized saturated polyester resins, polyurethane resins, plasticized polyurethane resins, ethylene-vinyl acetate copolymer resins, ethylene-ethyl acrylate copolymer resins, cycloolefin polymer resins, and ionomer resins. In addition, resin compositions containing modified hydrogenated block copolymers, as described in Japanese Patent No. 6,065,221, can also be suitably used.

[0068] Among these, plasticized polyvinyl acetal resins are preferably used because they have an excellent balance of properties such as transparency, weather resistance, strength, adhesive strength, penetration resistance, impact energy absorption, moisture resistance, heat insulation, and sound insulation. These thermoplastic resins may be used alone or in combination of two or more. The term "plasticized" in the plasticized polyvinyl acetal resin means that the resin has been plasticized by adding a plasticizer. The same applies to other plasticized resins.

[0069] However, when a specific substance is encapsulated in the interlayer film 13, the substance may be deteriorated by a specific plasticizer depending on the type of substance encapsulated. In such cases, it is preferable to use a resin that does not substantially contain that plasticizer. Examples of resins that do not contain plasticizers include ethylene-vinyl acetate copolymer (EVA) resins.

[0070] Examples of the polyvinyl acetal resin include polyvinyl formal resin obtained by reacting polyvinyl alcohol (PVA) with formaldehyde, polyvinyl acetal resin in the narrow sense obtained by reacting PVA with acetaldehyde, and polyvinyl butyral (PVB) resin obtained by reacting PVA with n-butylaldehyde. PVB is particularly preferred because it has an excellent balance of properties such as transparency, weather resistance, strength, adhesive strength, penetration resistance, impact energy absorbency, moisture resistance, heat insulation, and sound insulation. These polyvinyl acetal resins may be used alone or in combination of two or more.

[0071] However, the material forming the interlayer 13 is not limited to thermoplastic resin. The interlayer 13 may also contain functional particles such as infrared absorbers, ultraviolet absorbers, and luminescent agents. The interlayer 13 may also have a colored portion called a shade band. The color pigment used to form the colored portion is one that can be used for plastics, and the amount added may be adjusted so that the visible light transmittance of the colored portion is 40% or less. Examples of the color pigment include organic color pigments such as azo-based, phthalocyanine-based, quinacridone-based, perylene-based, perinone-based, dioxazine-based, anthraquinone-based, and isoindolino-based pigments, and inorganic color pigments such as oxides, hydroxides, sulfides, chromates, sulfates, carbonates, silicates, phosphates, arsenates, ferrocyanides, carbon, and metal powders. These color pigments may be used alone or in combination.

[0072] The intermediate film 13 may have multiple layers. For example, the intermediate film 13 may include three or more layers.

[0073] The thickness of the interlayer film 13 is preferably 0.5 mm or more at its thinnest part. When the interlayer film 13 has multiple layers, the thickness of the interlayer film 13 is the sum of the thicknesses of the individual layers. When the thickness of the interlayer film 13 at its thinnest part is 0.5 mm or more, the impact resistance required for laminated glass is sufficient. Furthermore, the thickness of the interlayer film 13 is preferably 3 mm or less at its thickest part. When the maximum thickness of the interlayer film 13 is 3 mm or less, the mass of the laminated glass does not become too large. The maximum thickness of the interlayer film 13 is more preferably 2.8 mm or less, and even more preferably 2.6 mm or less.

[0074] Furthermore, when the interlayer film 13 has multiple layers, it is desirable that each layer included in the interlayer film 13 be formed of the same material, but they may also be formed of different materials. However, from the viewpoint of adhesion to the first glass sheet 11 and the second glass sheet 12, or functional materials to be incorporated into the laminated glass 10, it is desirable that the above-mentioned materials be used for a portion that accounts for 50% or more of the film thickness of the interlayer film 13.

[0075] To produce the interlayer film 13, for example, an appropriate resin material for the interlayer film is selected from the above-mentioned materials and extruded in a heated, molten state using an extruder. The extrusion conditions, such as the extrusion speed, of the extruder are set to be uniform. The extruded resin film is then stretched as necessary to impart curvature to the upper and lower edges in accordance with the design of the laminated glass, thereby completing the interlayer film 13.

[0076] [Laminated Glass] The total thickness of the laminated glass 10 is preferably 2.8 mm or more and 10 mm or less. If the total thickness of the laminated glass 10 is 2.8 mm or more, sufficient rigidity can be ensured. Furthermore, if the total thickness of the laminated glass 10 is 10 mm or less, sufficient transmittance can be obtained and haze can be reduced. The total thickness of the laminated glass 10 is preferably 7 mm or less, more preferably 6 mm or less, and even more preferably 5 mm or less.

[0077] The plate misalignment between the first glass plate 11 and the second glass plate 12 is preferably 1.5 mm or less, and more preferably 1 mm or less, on at least one side of the laminated glass 10. Here, the plate misalignment between the first glass plate 11 and the second glass plate 12 refers to the amount of misalignment between the outer peripheral side surface of the first glass plate 11 and the outer peripheral side surface of the second glass plate 12 in a plan view.

[0078] It is preferable that the misalignment between the first glass sheet 11 and the second glass sheet 12 be 1.5 mm or less along at least one side of the laminated glass 10, since it does not impair the appearance. It is even more preferable that the misalignment between the first glass sheet 11 and the second glass sheet 12 be 1.0 mm or less along at least one side of the laminated glass 10, since it does not impair the appearance.

[0079] [Method for Manufacturing Laminated Glass] To manufacture the laminated glass 10, first, as shown in FIG. 5A, 3 and fourth surface 11 4 a first glass plate 11 having an intermediate film 13 and a first surface 12 1 and the second surface 12 2 The first glass plate 11 and the second glass plate 12 have a constant thickness. Here, the film thickness of the interlayer film 13 is assumed to be constant. Alternatively, the interlayer film 13 may have a wedge-shaped cross section.

[0080] Next, as shown in FIG. 5B, the fourth surface 11 of the first glass plate 11 4 The coating film 15 is formed on the fourth surface 11 of the first glass plate 11 by, for example, sputtering or CVD, etc., and has a visible light reflectance of 10% or more when P-polarized visible light is incident at an incident angle of 65 degrees. 4 In the example shown in FIG. 5B , the fourth surface 11 of the first glass plate 11 4 The coating film 15 is formed on the entire surface of the fourth surface 11 of the first glass plate 11. 4 In the example shown in FIG. 5B , the coating film 15 may be formed on a part of the fourth surface 11 of the first glass plate 11. 4As shown in FIGS. 10A and 10B, the coating film 15 is formed on the third surface 11 of the first glass plate 11. 3 or the second surface 12 of the second glass plate 12 2 Alternatively, the coating film 15 may be formed on a large piece of glass, and then the glass may be cut to prepare the first glass plate 11 on which the coating film 15 is formed.

[0081] Next, after the step of forming the coating film 15, the first glass sheet 11 and the second glass sheet 12 are bent as shown in FIG. 5C . The first glass sheet 11 and the second glass sheet 12 can be bent, for example, by press molding. Specifically, a mold with projections and recesses corresponding to the final shape of the laminated glass 10 is prepared, and the first glass sheet 11 and the second glass sheet 12 are each heated to a predetermined temperature to soften them, and then the mold is used to press the first glass sheet 11 and the second glass sheet 12 to bend them. The first glass sheet A and the second glass sheet B may also be bent by gravity molding, roller molding, or the like.

[0082] Next, in FIG. 6A , one of the two opposing sides of the interlayer film 13 and its vicinity are stretched along the one side in the direction indicated by the arrow in plan view. However, the stretching direction is not limited thereto. For example, the one side and its vicinity may be stretched entirely in the left-right direction, with the degree of stretching varying in the up-down direction. For example, a stretching machine may be used for stretching. For example, by stretching the one side and its vicinity of the rectangular interlayer film 13 in plan view in the direction indicated by the arrow, the interlayer film 13 becomes trapezoidal in plan view, and the extended side and its vicinity become wedge-shaped in cross section, as shown in FIG. 6B . When the interlayer film 13 is stretched strongly, there is an upper limit to the elongation of the one side and its vicinity, and the degree of stretching saturates, eliminating thickness deviation and resulting in thinning with no or almost no wedge angle. In contrast, a wedge angle is generated in a portion other than the vicinity of the one side, and a difference is created between the wedge angle in the vicinity of the one side and the wedge angle in the other portion. That is, an interlayer film 13 having local wedge angles α and β as shown in FIG. 4 can be formed.

[0083] In this step, as shown in FIGS. 3 and 4, the intermediate film 13 is attached to the fourth surface 11 of the laminated glass 10 after the laminated glass 10 is installed in the vehicle. 4 The interlayer film 11 has a shape including a wedge-shaped cross-section region whose thickness gradually increases from the lower edge 11b toward the upper edge 11t. Furthermore, on a line S1 passing through a first point Pt that bisects the upper edge 11t and a second point Pb that bisects the lower edge 11b in a plan view, the local wedge angle α at a position 100 mm from the second point Pb and the local wedge angle β at a position 500 mm from the second point Pb are extended so as to satisfy the formula (β-α)>0.05 [mrad]. The same procedure can be used when preparing an interlayer film 13 having a wedge-shaped cross-section without a constant film thickness.

[0084] When the intermediate film 13 includes a plurality of layers, a laminate of the plurality of layers is prepared, and then the entire laminate is stretched.

[0085] 6A and 6B, the unhatched views on the left are plan views, and the hatched views on the right are cross-sectional views. In the cross-sectional views on the right in Figures 6A and 6B, the thickness direction of the interlayer film 13 is emphasized more than in the cross-sectional view of the interlayer film 13 shown in Figure 5A. The steps shown in Figures 6A and 6B and the steps shown in Figures 5B and 5C may be performed in either order, or may be performed in parallel.

[0086] Next, the third surface 11 of the first glass plate 11 3 and the second surface 12 of the second glass plate 12 2 The stretched interlayer film 13 is placed between the first glass plate 11 and the second glass plate 12 and pressure-bonded. For example, the interlayer film 13 is sandwiched between the first glass plate 11 and the second glass plate 12 with the coating film 15 facing outward to form a laminate. Then, for example, this laminate is placed in a rubber bag, a rubber chamber, a resin bag, or the like, and bonded at a temperature controlled in the range of approximately 70°C to 110°C in a vacuum with a gauge pressure controlled in the range of 100 kPa to -65 kPa. The heating conditions, temperature conditions, and lamination method are selected as appropriate.

[0087] Furthermore, a laminated glass 10 with even greater durability can be obtained by performing a heating and pressing process under controlled conditions, for example, at a temperature of 100°C to 150°C and an absolute pressure of 0.6 MPa to 1.5 MPa. However, in some cases, this heating and pressing process may not be performed in order to simplify the process or in consideration of the properties of the material to be sealed in the laminated glass 10. The laminated glass 10 is completed through the above processes.

[0088] Alternatively, a so-called cold bending method may be used in which the second glass sheet 12 is bent in advance, and the first glass sheet, which is in a flat state sandwiched between the second glass sheet 12 and the interlayer film 13, is curved to match the shape of the second glass sheet 12 and bonded to produce the laminated glass 10.

[0089] In addition to the interlayer film 13, a film or device having a function such as heating, infrared reflection, light emission, power generation, light control, touch panel, visible light reflection, scattering, decoration, or absorption may be provided between the first glass sheet 11 and the second glass sheet 12, as long as the effects of the present invention are not impaired. Furthermore, the surface of the laminated glass 10 may have a film having a function such as anti-fogging, water repellency, heat shielding, or low reflection. Furthermore, a film having a function such as heat shielding or heat generation may be provided on the inner main surface of the first glass sheet 11 or the inner main surface of the second glass sheet 12.

[0090] As described above, in the laminated glass 10, the first glass sheet 11 is provided with a coating film 15, but the second glass sheet 12 is not. In such a case, when the first glass sheet 11 and the second glass sheet 12 are bent during the manufacturing process of the laminated glass 10, the bending behavior of each glass sheet differs. As a result, mismatching may occur after bending. The mismatching refers to a state in which the peripheral shapes of each glass sheet differ.

[0091] The mismatch can be a factor in the generation of bubbles in the interlayer film 13. In particular, when the curvature of the glass at the periphery of the first glass sheet 11, which is the glass sheet on the vehicle interior side, is larger than the curvature of the glass at the periphery of the second glass sheet 12, which is the glass sheet on the vehicle exterior side, the third surface 11 of the first glass sheet 11 may be larger than the curvature of the glass at the periphery of the second glass sheet 12, which is the glass sheet on the vehicle exterior side. 3A gap called an opening occurs between the lower edge of the glass and the interlayer film 13, which can easily lead to bubbling of the interlayer film 13 after the vehicle is released onto the market. Furthermore, bubbling of the interlayer film 13 occurs particularly remarkably near the lower edge of laminated glass having an interlayer film with a wedge-shaped cross section.

[0092] To address this issue, the laminated glass 10 is designed so that the local wedge angle α and the local wedge angle β satisfy the formula (β-α)>0.05 [mrad], thereby making it difficult for bubbles to form in the interlayer 13. 4 The local wedge angle α near the bottom edge 11b of the laminated glass is small. Therefore, when the interlayer film 13 is disposed between the first glass sheet 11 and the second glass sheet 12 and then pressed together, the first glass sheet 11 and the second glass sheet 12 are pressed together in a nearly parallel manner near the bottom edge 11b. As a result, even if the laminated glass is left in a harsh environment such as a high-temperature environment for a long period of time, the third surface 11 of the first glass sheet 11 can be easily secured. 3 This reduces the risk of a gap occurring between the lower side or its vicinity and the interlayer 13, and thus reduces the likelihood of bubbles occurring in the interlayer 13. It is preferable that (β-α) satisfies 0.30.

[0093] The laminated glass 10 is preferably configured to satisfy the formula α<0.35 mrad, and more preferably α<0.10 mrad. The smaller the local wedge angle α, the more closely parallel the first glass sheet 11 and the second glass sheet 12 are compressed together at and near the lower edge 11b, making it less likely that bubbles will form in the interlayer film 13. It is also preferable that the formula (α+0.05 mrad)<β<0.30 mrad be satisfied. A value of β within this range is sufficient to reduce ghost images, and not increasing β more than necessary can also contribute to reducing mismatch between the first and second glass sheets.

[0094] 3, the average thickness of the interlayer film 13 in the range from 70 mm to 130 mm from the bottom edge 11b may be 0.80 mm or less, or may be 0.70 mm or less. The thinner the interlayer film 13, the more likely it is that bubbles will form. However, because the laminated glass 10 is configured to satisfy the formula (β-α)>0.05 mrad, even a thin interlayer film 13 can be made less susceptible to bubbles.

[0095] For example, the first glass plate 11 has a weight ratio of Fe 2 O 3 The sum of the total iron content converted into iron by weight may be lower than that of the second glass sheet 12. The second glass sheet 12 has a weight ratio of Fe 2 O 3 The sum of the total iron content, converted into mrad, may be 0.1% or more. For example, the first glass sheet 11 may be clear glass, and the second glass sheet 12 may be green glass. When the compositions of the first glass sheet 11 and the second glass sheet 12 are different in this way, their behavior during bending differs, making bubbles more likely to form in the interlayer film 13. To prevent this, it is effective to satisfy the formula (β - α) > 0.05 [mrad].

[0096] 2A and 2B, when viewed from above, the second surface 12 2 A shielding layer 14B is provided on the lower side and the outer edge of the vicinity thereof, and the fourth surface 11 of the first glass plate 11 4 If a shielding layer is not provided on the lower side 11b and the outer edge portion in the vicinity thereof, the behavior during bending will be significantly different, and bubbles will be more likely to occur in the interlayer film 13. Therefore, as a countermeasure, it is effective to make sure that the formula (β-α)>0.05 [mrad] is satisfied.

[0097] In the laminated glass 10, the difference in thickness between the first glass sheet 11 and the second glass sheet 12 is preferably 0.3 mm or less, and more preferably less than 0.2 mm. The smaller the difference in thickness between the first glass sheet 11 and the second glass sheet 12, the less difference in behavior during bending, making it more difficult for bubbles to form in the interlayer film 13.

[0098] <Modification> FIG. 7 is a partial cross-sectional view illustrating a laminated glass according to Modification 1 of the first embodiment, and shows a cross section corresponding to FIG. 4 .

[0099] The laminated glass 10A shown in Figure 7 differs from the laminated glass 10 in that the interlayer film 13 is replaced with an interlayer film 13A. The interlayer film 13A has a three-layer structure. Specifically, the interlayer film 13A has an interlayer film 131 bonded to the first glass plate 11, an interlayer film 132 bonded to the second glass plate 12, and an interlayer film 133 sandwiched between the interlayer film 131 and the interlayer film 132.

[0100] For example, the intermediate film 133 is a core layer and has a smaller shear storage modulus than the intermediate films 131 and 132. The intermediate films 131 and 132 are skin layers and have a larger shear storage modulus than the intermediate film 133. The shear storage modulus of the intermediate film 131 and the shear storage modulus of the intermediate film 132 may be the same or different. The shear storage modulus can be changed, for example, by adjusting the amount of plasticizer added to the resin. The shear storage modulus in the present invention is a value measured by a general dynamic viscoelasticity measurement method under measurement conditions of a temperature of 20°C, a frequency of 1 Hz, and a strain of 0.05%.

[0101] The thickness of the intermediate film 133 is preferably 0.05 mm or more and 0.3 mm or less, and more preferably 0.07 mm or more and 0.2 mm or less. The thickness of the intermediate films 131 and 132 is preferably 0.1 mm or more and 2.0 mm or less, and more preferably 0.1 mm or more and 1.0 mm or less. The thickness of the intermediate film 133 may be thinner than the thickness of the intermediate films 131 and 132.

[0102] In this way, sandwiching a core layer with a low shear storage modulus between skin layers with a high shear storage modulus can improve the sound insulation of laminated glass 10A. Note that even if the interlayer film has four or more layers and the shear storage modulus of any layer other than both outermost layers is made smaller than the shear storage modulus of both outermost layers, the sound insulation of laminated glass 10A can be improved in the same way as above.

[0103] When a film includes a soft layer with a low shear storage modulus, such as the interlayer film 13A, bubbles tend to form at the interface between the layer with the low shear storage modulus and the layer with the high shear storage modulus. Therefore, as a countermeasure against this, it is effective to satisfy the formula (β - α) > 0.05 [mrad].

[0104] FIG. 8 is a cross-sectional view illustrating a laminated glass according to Modification 2 of the first embodiment, showing a cross section corresponding to FIG. 2B.

[0105] The laminated glass 10B shown in FIG. 8 has a fourth surface 11 4 The laminated glass 10 differs from the laminated glass 10 in that a molding 17 is disposed on the outer edge of the fourth surface 11 of the first glass sheet 11. 4 A shielding layer 14A is provided on the lower side and its vicinity. A molding 17 is fixed to the interior side of this shielding layer 14A. The molding 17 can be fixed to the shielding layer 14A by, for example, adhering a resin member formed by extrusion molding to the shielding layer 14A of the first glass plate 11. The molding 17 is fixed to the fourth surface 11 of the first glass plate 11. 4 Since the intermediate film 13 is disposed only on the outer edge of the lower side 11 b , the end of the intermediate film 13 is exposed from the molding 17 at the lower side 11 b and its vicinity.

[0106] In laminated glass having molding covering the edges of the interlayer film 13, the edges of the interlayer film 13 are protected by the molding, making it difficult for bubbles to form in the interlayer film 13. In contrast, in laminated glass 10B, the edges of the interlayer film 13 are exposed from the molding 17 and are not protected by the molding 17, which makes bubbles more likely to form in the interlayer film 13. Therefore, as a countermeasure, it is effective to satisfy the formula (β - α) > 0.05 [mrad].

[0107] Fig. 9 is a plan view illustrating a laminated glass according to Modification 3 of the first embodiment, and is a diagram schematically illustrating the laminated glass as viewed from inside the vehicle to outside the vehicle. In Fig. 9, L1 = 100 mm, and L2 = 500 mm.

[0108] The laminated glass 10C shown in Figure 9 differs from the laminated glass 10 in that the HUD display region R is located so as to overlap the shielding layer 14B in a planar view. At least the region defining the local wedge angles α and β is located so as to overlap the shielding layer 14B in a planar view. Specifically, the shielding layer 14B is provided in a region including a range that is 60 mm or more and 540 mm or less from the second point Pb on the line S1. Note that instead of or in addition to the shielding layer 14B, the shielding layer 14A may be provided in a region including a range that is 60 mm or more and 540 mm or less from the second point Pb on the line S1.

[0109] When the HUD display region R is located at a position overlapping with the shielding layer 14B in a plan view, it is less susceptible to the influence of external light and the contrast of the HUD image is less likely to decrease, improving the visibility of the HUD image. As a result, if bubbles occur in the interlayer 13, the bubbles also become more visible, so as a countermeasure, it is effective to satisfy the formula (β-α)>0.05 [mrad].

[0110] 10A and 10B are cross-sectional views illustrating a laminated glass according to Modification 4 of the first embodiment, and show a cross section corresponding to FIG. 2B.

[0111] In the laminated glass 10 shown in FIGS. 2A and 2B, the coating film 15 is formed on the fourth surface 11 of the first glass plate 11. 4 However, the laminated glass according to the present disclosure is not limited to the embodiment shown in Figures 2A and 2B. For example, as in laminated glass 10D shown in Figure 10A, a coating film 15 is provided on the third surface 11 of the first glass sheet 11. 3 Alternatively, as in the laminated glass 10E shown in FIG. 10B , the coating film 15 may be provided on the second surface 12 of the second glass sheet 12. 2 In this way, in the laminated glass according to the present disclosure, the second surface 12 of the second glass plate 12 2 , the third surface 11 of the first glass plate 11 3 , or the fourth surface 11 of the first glass plate 11 4 The coating film 15 may be provided on the surface of the substrate 10.

[0112] Furthermore, when two types of coating films are provided on a laminated glass, for example, when the coating films provided on the first glass sheet 11 and the second glass sheet 12 are of different types, mismatch may occur after the two glass sheets are bent. To address this issue, it is effective to satisfy the formula (β-α)>0.05 [mrad].

[0113] In the case of the laminated glasses 10D and 10E, as with the laminated glass 10, mismatches may occur during the manufacturing process of the laminated glasses 10D and 10E when the first glass sheet 11 and the second glass sheet 12 are bent because the glass sheets behave differently. Therefore, as with the laminated glass 10, the laminated glasses 10D and 10Eh can be designed so that the local wedge angles α and β satisfy the formula (β-α)>0.05 mrad, thereby making it difficult for bubbles to form in the interlayer film 13.

[0114] As in the case of the laminated glass 10, the coating film 15 is formed on the fourth surface 11 of the first glass plate 11. 4 This is preferable in that the main reflective surface becomes the surface of the coating film 15 that contacts the first glass plate 11, limiting the number of sub-images to one and making the sub-image less noticeable.

[0115] Examples and Comparative Examples The following describes examples and comparative examples, but the present invention is not limited to these examples. Examples 1 and 4 are examples, and Examples 2, 3, 5, and 6 are comparative examples.

[0116] [Example 1] A clear glass (Fe) manufactured by AGC was used as a flat first glass sheet A that would become the inner sheet (glass sheet on the vehicle interior side) when laminated. 2 O 3 The total iron content converted to iron was 0.08%. A green glass (Fe, 2 O 3A first glass sheet A and a second glass sheet B were prepared, each having a size of 1,560 mm x 966 mm x 1.8 mm thickness. Neither the first glass sheet A nor the second glass sheet B was wedge-shaped in cross section, but had a uniform thickness. In addition, a non-wedge sound-insulating film having a uniform thickness and consisting of three layers of PVB film was prepared as interlayer film C. In interlayer film C, the thicknesses of the PVB films on both sides were 0.33 mm, and the thickness of the middle PVB film was 0.1 mm.

[0117] Next, a coating film (TiZrO 2 / SiO 2 The geometric film thickness was 73.9 nm / 99.5 nm.

[0118] Next, a mold with concave and convex shapes corresponding to the final shape of the laminated glass was prepared, and the first glass sheet A and the second glass sheet B were each heated to 600°C to soften them, and then the mold was used to press the first glass sheet A and the second glass sheet B to bend them.

[0119] Next, a plastic film stretching machine D was used to stretch one of the opposing sides of the interlayer film C and the surrounding area to form a wedge-shaped cross section. The stretching machine D used was the one shown in U.S. Pat. No. 2,933,759. The stretching machine D stretches the interlayer film C by heating it and aligning it with an umbrella-shaped cylinder. The degree of stretching can be selected by the opening angle (radius R) of the umbrella-shaped cylinder. In Example 1, R was set to 1,800 mm, and the interlayer film C was strongly stretched. As a result of strongly stretching the interlayer film C, there was no thickness deviation near the one side because there was an upper limit to elongation, and the film was thinned with no or almost no wedge angle. In contrast, a wedge angle was formed in areas other than the vicinity of the one side, resulting in a difference between the wedge angle near the one side and the wedge angle in the other areas.

[0120] Next, a laminate was prepared by sandwiching the stretched interlayer film C between a curved first glass plate A provided with a coating film and a curved second glass plate B, and the first glass plate A and the second glass plate B and the interlayer film C were bonded together in a vacuum controlled at a gauge pressure of 100 kPa to -65 kPa and a temperature controlled at a range of approximately 70°C to 110°C. A heat-pressure bonding process was then carried out under conditions controlled at a temperature of 100°C to 150°C and an absolute pressure of 0.6 MPa to 1.5 MPa, to prepare a Type A laminated glass. The Type A laminated glass was designed for use with an incident angle of 62 degrees for P-polarized light and a HUD projection distance of 6.2 m.

[0121] Example 2 A type A laminated glass was produced in the same manner as in Example 1, except that the interlayer film C (non-wedge sound-insulating film) was not stretched at all.

[0122] [Example 3] A type A laminated glass was produced in the same manner as in Example 1, except that the stretching machine D was set to R = 3000 mm and the interlayer film C (non-wedge sound-insulating film) was weakly stretched. In Example 3, as a result of weakly stretching the interlayer film C, a substantially constant wedge angle was formed from one side to the other.

[0123] Example 4 A type B laminated glass was produced in the same manner as in Example 1, except that the first glass sheet A was clear glass manufactured by AGC with dimensions of 1580 mm x 811 mm x 1.8 mm thickness, the second glass sheet B was green glass manufactured by AGC with dimensions of 1580 mm x 811 mm x 2.0 mm thickness, and a wedge sound-insulating film with a predetermined wedge angle formed in advance was used as the interlayer film C. Note that the type B laminated glass was designed for use with an incident angle of P-polarized light of 67 degrees and an HUD projection distance of 2.5 m. In Example 4, as a result of strongly stretching the interlayer film C, an additional wedge angle was generated in addition to the wedge angle before stretching. A larger additional wedge angle was generated in areas other than the vicinity of one side than in the vicinity of one side.

[0124] Example 5 A type B laminated glass was produced in the same manner as in Example 1, except that a first glass plate A and a second glass plate B similar to those in Example 4 were prepared, an interlayer film C (non-wedge sound-insulating film) similar to that in Example 1 was prepared, and the interlayer film C was not stretched at all.

[0125] [Example 6] A type B laminated glass was produced in the same manner as in Example 1, except that the same first glass sheet A, second glass sheet B, and interlayer film C (wedge sound-insulating film) as in Example 4 were prepared, and the stretcher D was set to R = 3000 mm to weakly stretch the interlayer film C. In Example 6, as a result of weakly stretching the interlayer film C, an additional wedge angle was generated in addition to the wedge angle before stretching. Approximately the same additional wedge angle was generated near one side and on the other side opposite the one side. [Example 7] A type B laminated glass was produced in the same manner as in Example 1, except that the same first glass sheet A, second glass sheet B, and interlayer film C (wedge sound-insulating film) as in Example 4 were prepared, and the stretcher D was set to R = 3000 mm to weakly stretch the interlayer film C. In Example 7, as a result of weakly stretching the interlayer film C, an additional wedge angle was generated in addition to the wedge angle before stretching. Near one side and on the other side opposite the one side, approximately the same additional wedge angle was created.

[0126] [Evaluation 1 (Measurement of Mismatch)] In Examples 1 to 7, after the first glass sheet A and the second glass sheet B were bent and formed, and before preparing a laminated glass, the second glass sheet B was superimposed on the first glass sheet A. Then, the maximum value of the gap between the first glass sheet A and the second glass sheet B was measured at a position that would become the bottom side when the laminated glass was completed and mounted on a vehicle, and this value was taken as the mismatch.

[0127] [Evaluation 2 (Measurement of local wedge angle, etc.)] The local wedge angles α and β were measured based on the method described above. The value of (β-α) was also calculated. When the laminated glass was completed and installed in a vehicle, the average film thickness of the interlayer film C was measured in an area from 60 mm to 140 mm from the second point on the line shown in Figure 4. The film thickness of the interlayer film C was measured using a multilayer film thickness measuring device, Optigauge, manufactured by Lumetrics.

[0128] [Evaluation 3 (Measurement of Ghost Image Distance)] For the laminated glasses of Examples 1 to 7, the ghost image distance defined in 4.1.7 of SAE J1757-2 (2018) was measured based on the method specified in the standard. The standard recommends measurement at three viewpoints: upper, middle, and lower (UE2, CE2, LE2), but here, evaluation was performed using only the central viewpoint (CE2). Taking into account the visibility of the HUD image, a ghost image distance of 1.0 mm or less was rated "good" (indicated by a circle), and a ghost image distance of more than 1.0 mm was rated "poor" (indicated by an x).

[0129] [Evaluation 4 (Temperature at which bubbles occur)] The laminated glasses of Examples 1 to 7 were left in an oven at 100°C for 15 hours, and then visually observed from a position 30 cm away from the second glass plate B to check for the presence or absence of bubbles in the interlayer film C. If no bubbles were found, the temperature was set to 110°C and left for 1 hour, and the presence or absence of bubbles was similarly checked. If no bubbles were found, the temperature was set to 120°C and left for 1 hour, and the presence or absence of bubbles was similarly checked. If no bubbles were found, the temperature was set to 130°C and left for 1 hour, and the presence or absence of bubbles was similarly checked. If no bubbles were found, the temperature was set to 140°C and left for 1 hour, and the presence or absence of bubbles was similarly checked. If no bubbles occurred even at 140°C, the glass was rated as "excellent (indicated by a ◎ mark)," if bubbles first occurred at 140°C, the glass was rated as "good (indicated by a ○ mark)," and if bubbles occurred even slightly at 130°C or below, the glass was rated as "poor (indicated by an × mark)."

[0130] [Evaluation 5 (Overall Evaluation)] An overall evaluation was made based on the results of Evaluation 3 (measurement of the distance to the double image) and Evaluation 4 (temperature at which foaming occurs). For the overall evaluation, if at least one of Evaluation 3 (measurement of the distance to the double image) and Evaluation 4 (temperature at which foaming occurs) was "poor (indicated by an x ​​mark)", the evaluation was deemed "poor (indicated by an x ​​mark)". Furthermore, if both Evaluation 3 (measurement of the distance to the double image) and Evaluation 4 (temperature at which foaming occurs) were "good (indicated by an o mark)", the evaluation was deemed "good (indicated by an o mark)". Furthermore, if Evaluation 3 (measurement of the distance to the double image) was "good (indicated by an o mark)" and Evaluation 4 (temperature at which foaming occurs) was "excellent (indicated by a ◎ mark)", the evaluation was deemed "excellent (indicated by an ◎ mark)".

[0131] Table 1 summarizes the results for Types A and B, and FIG. 11 summarizes the results for Examples 1 to 7.

[0132] Comparing Example 1 and Example 2 in Figure 11, in Example 1, because the interlayer film C was stretched strongly, the difference (β - α) between the local wedge angle β in the HUD display area and the local wedge angle α below the HUD display area was 0.07 mrad. Because the local wedge angle β in the HUD display area was a moderate value, the distance of the double image was short and the visibility of the HUD image was good. Therefore, the evaluation of the distance of the double image was good. Furthermore, because the local wedge angle α was small and the first glass sheet A and the second glass sheet B were pressed in a nearly parallel manner near the bottom edge of the laminated glass, no bubbles were generated in the interlayer film C even at 140°C. Therefore, the evaluation of bubbles was excellent. As a result, the overall evaluation was excellent.

[0133] In contrast, in Example 2, the wedge angle of the interlayer film C was essentially zero because it was not stretched, resulting in a long double image distance and poor visibility of the HUD image. Therefore, the double image distance was rated as poor. Meanwhile, the wedge angle was essentially zero, and the first glass sheet A and the second glass sheet B were pressed together in a nearly parallel manner at the bottom edge of the laminated glass and its vicinity, so no bubbles were generated in the interlayer film C even at 140°C. Therefore, the bubble evaluation was excellent. As a result, the overall evaluation was poor.

[0134] In Example 3, because the interlayer film C was stretched weakly, the difference (β - α) between the local wedge angle β in the HUD display area and the local wedge angle α below the HUD display area was 0.02 mrad. Because the local wedge angle β in the HUD display area was an appropriate value, the distance of the double image was short and the visibility of the HUD image was good. Therefore, the evaluation of the distance of the double image was Good. However, because the stretching was insufficient, the local wedge angle α was not small enough, and the first glass sheet A and the second glass sheet B were not pressed together in a nearly parallel manner at the bottom edge of the laminated glass and its vicinity, which resulted in the generation of bubbles in the interlayer film C at 130°C. Therefore, the evaluation of bubbles was Poor. As a result, the overall evaluation was Poor.

[0135] Comparing Example 4 and Example 5 in Figure 11, in Example 4, the interlayer film C, which had a predetermined wedge angle formed in advance, was strongly stretched, so the difference (β - α) between the local wedge angle β in the HUD display area and the local wedge angle α at the edge below the HUD display area and its vicinity was 0.09 mrad. Because the local wedge angle β in the HUD display area was a moderate value, the distance of the double image was short and the visibility of the HUD image was good. Therefore, the evaluation of the distance of the double image was Good. On the other hand, because the wedge angle was originally formed, the local wedge angle α was not sufficiently small, and the first glass sheet A and the second glass sheet B were not pressed together in a nearly parallel manner at the bottom edge and its vicinity of the laminated glass. Therefore, bubbles occurred in the interlayer film C at 140°C. Therefore, the evaluation of bubbles was Good. As a result, the overall evaluation was Good.

[0136] In contrast, in Example 5, the wedge angle of the interlayer film C was essentially zero because it was not stretched, resulting in a long double image distance and poor visibility of the HUD image. Therefore, the double image distance was rated as x. Meanwhile, the wedge angle was essentially zero, and the first glass sheet A and the second glass sheet B should have been pressed together in a nearly parallel manner near the bottom edge of the laminated glass, but bubbles formed in the interlayer film C at 140°C. Therefore, the bubble evaluation was rated as good. As a result, the overall evaluation was poor.

[0137] In Example 6, because the interlayer film C was stretched weakly, the difference (β - α) between the local wedge angle β in the HUD display area and the local wedge angle α at the edge below the HUD display area and in its vicinity was 0.02 mrad. Because the local wedge angle β in the HUD display area was an appropriate value, the distance of the double image was short, and the visibility of the HUD image was good. Therefore, the evaluation of the distance of the double image was Good. However, because the stretching was insufficient, the local wedge angle α was not small enough, and the first glass sheet A and the second glass sheet B were not pressure-bonded in a nearly parallel manner at the bottom edge of the laminated glass and in its vicinity, so bubbles occurred in the interlayer film C at 120°C. Therefore, the evaluation of bubbles was Poor. As a result, the overall evaluation was Poor.

[0138] Although both Example 4 and Example 6 had relatively large α values, Example 4 received a good evaluation of bubbling, while Example 6 received a poor evaluation of bubbling. This is thought to be because Example 4 had a larger (β-α) value than Example 6, which caused the first glass sheet and the second outer glass sheet to approach each other closer at the bottom edge of the laminated glass and in its vicinity, thereby suppressing the generation of bubbling. The above was also confirmed by comparing Example 4 with Example 7.

[0139] From the above results, it can be said that if the formula (β-α)>0.05 [mrad] is satisfied, the distance of the double image is short, the visibility of the HUD image is good, and bubbling is unlikely to occur. It can also be said that it is preferable to satisfy the formula α<0.10 [mrad].

[0140] Although the preferred embodiments have been described in detail above, the present invention is not limited to the above-described embodiments, and various modifications and substitutions can be made to the above-described embodiments without departing from the scope of the claims.

[0141] In addition to the above embodiments, the following supplementary note is further disclosed: (Supplementary note 1) A laminated glass including a curved first glass sheet, a curved second glass sheet, and an interlayer film positioned between the first glass sheet and the second glass sheet and bonding the first glass sheet to the second glass sheet, wherein a fourth surface is a surface of the first glass sheet opposite to the interlayer film, a third surface is a surface of the first glass sheet facing the interlayer film, a second surface is a surface of the second glass sheet facing the interlayer film, and a first surface is a surface of the second glass sheet opposite to the interlayer film, and a coating film is provided on the second surface, the third surface, or the fourth surface, and the coating film has a visible light reflectance of 10% or more when P-polarized visible light is incident at an incident angle of 65 degrees, and the interlayer film has a region with a wedge-shaped cross section whose thickness gradually increases from a lower edge side to an upper edge side when the laminated glass is installed in a vehicle. Laminated glass, in which, in a plan view, on a line passing through a first point dividing the upper side in half and a second point dividing the lower side in half, a local wedge angle α at a position 100 mm from the second point and a local wedge angle β at a position 500 mm from the second point satisfy the formula: (β - α) > 0.05 [mrad], where: local wedge angle α = ((interlayer film thickness at 100 mm + 40 mm from the second point) - (interlayer film thickness at 100 mm - 40 mm from the second point)) / 80 mm local wedge angle β = ((interlayer film thickness at 500 mm + 40 mm from the second point) - (interlayer film thickness at 500 mm - 40 mm from the second point)) / 80 mm (Appendix 2) Laminated glass according to Appendix 1, wherein the formula: α < 0.10 [mrad] is satisfied. (Appendix 3) The laminated glass according to Appendices 1 or 2, wherein the formula β<0.30 [mrad] is satisfied. (Appendix 4) The laminated glass according to any one of Appendices 1 to 3, wherein the interlayer film includes three or more layers. (Appendix 5) The laminated glass according to Appendices 4, wherein the shear storage modulus of any layer in the interlayer film other than both outermost layers is lower than the shear storage modulus of both outermost layers.(Appendix 6) The laminated glass according to any one of Appendices 1 to 5, wherein the average thickness of the interlayer film in an area on the straight line that is 60 mm to 140 mm from the second point is 0.80 mm or less. (Appendix 7) The laminated glass according to any one of Appendices 1 to 6, wherein a molding is arranged on an outer edge of the fourth surface, and an end of the interlayer film on the lower side is exposed from the molding. (Appendix 8) The first glass sheet contains, by weight, Fe. 2 O 3 The sum of the total iron content converted into Fe is lower than that of the second glass sheet, and the second glass sheet has a weight ratio of Fe 2 O 3The laminated glass according to any one of Appendices 1 to 7, wherein the sum of the total iron content converted into ρ is 0.1% or more. (Appendix 9) The laminated glass according to any one of Appendices 1 to 8, wherein, in a plan view, a shielding layer is provided on an outer edge portion of the lower side of the second surface, and wherein, in a plan view, no shielding layer is provided on an outer edge portion of the lower side of the fourth surface. (Appendix 10) The laminated glass according to any one of Appendices 1 to 9, wherein a shielding layer is provided on the second surface and / or the fourth surface, and an information transmitting / receiving area is provided in an opening of the shielding layer. (Appendix 11) The laminated glass according to any one of Appendices 1 to 10, wherein the difference in plate thickness between the first glass plate and the second glass plate is less than 0.2 mm. (Appendix 12) The laminated glass according to any one of Appendices 1 to 11, wherein a shielding layer is provided on the second surface and / or the fourth surface in a region including a range from 60 mm to 540 mm from the second point on the straight line.(Supplementary Note 13) A method for manufacturing laminated glass including a curved first glass sheet, a curved second glass sheet, and an interlayer film located between the first glass sheet and the second glass sheet and bonding the first glass sheet and the second glass sheet, the method comprising the steps of: preparing the first glass sheet having a third side and a fourth side, the interlayer film, and the second glass sheet having a first side and a second side; forming a coating film on the second side, the third side, or the fourth side, the coating film having a visible light reflectance of 10% or more when P-polarized visible light is incident at an incident angle of 65 degrees; bending the first glass sheet and the second glass sheet after the step of forming the coating film; and extending at least one side and a portion thereof adjacent to the one side of two opposing sides of the interlayer film along the one side in a plan view. and placing the stretched interlayer film between the third surface of the first glass sheet and the second surface of the second glass sheet and pressing them together, wherein in the stretching step, the interlayer film has a region with a wedge shape in cross section that gradually increases in thickness from the lower edge toward the upper edge of the fourth surface when the laminated glass is attached to a vehicle, and the interlayer film is stretched so that, on a line that passes through a first point that bisects the upper edge and a second point that bisects the lower edge in plan view, a local wedge angle α at a position 100 mm from the second point and a local wedge angle β at a position 500 mm from the second point satisfy the equation: (β - α) > 0.05 mrad.

[0142] 1 HUD system 10, 10A, 10B, 10C, 10D, 10E Laminated glass 11 First glass plate 11 3 3rd page 11 4 Fourth surface 11t Upper edge 11b Lower edge 12 Second glass plate 12 1 1st page 12 2Second surface 13, 13A, 131, 132, 133 Intermediate film 14A, 14B Shielding layer 15 Coating film 16 Information transmission / reception area 17 Molding 50 Light source 60 First optical system 70 Image display element 80 Second optical system 90 Concave mirror The entire contents of the specification, claims, drawings and abstract of Japanese Patent Application No. 2023-052990, filed on March 29, 2023, are hereby incorporated by reference as the disclosure of the specification of the present invention.

Claims

1. A laminated glass comprising a curved first glass plate, a curved second glass plate, and an intermediate film located between the first glass plate and the second glass plate and bonding the first glass plate and the second glass plate, wherein the first glass plate has a third surface and a fourth surface, and the second glass plate has a first surface and a second surface, the fourth surface is a surface of the first glass plate opposite to the intermediate film, the third surface is a surface of the first glass plate facing the intermediate film, the second surface is a surface of the second glass plate facing the intermediate film, and the first surface is a surface of the second glass plate opposite to the intermediate film, and a coating film is provided on the second surface, the third surface, or the fourth surface, and the coating film is configured to have a visible light reflectance of 10% or more for P-polarized visible light incident at an incident angle of 65 degrees, The interlayer film has a region of a wedge shape in cross section whose thickness gradually increases from the lower side to the upper side when the laminated glass is attached to a vehicle, and on a line passing through a first point dividing the upper side in half and a second point dividing the lower side in half in a plan view, a local wedge angle α at a position 100 mm away from the second point and a local wedge angle β at a position 500 mm away from the second point satisfy the formula: (β-α)>0.05 [mrad], where: local wedge angle α=((thickness of the interlayer film at 100 mm+40 mm from the second point)-(thickness of the interlayer film at 100 mm-40 mm from the second point)) / 80 mm local wedge angle β=((thickness of the interlayer film at 500 mm+40 mm from the second point)-(thickness of the interlayer film at 500 mm-40 mm from the second point)) / 80 mm 2. The laminated glass according to claim 1, wherein the formula α<0.10 [mrad] is satisfied.

3. The laminated glass according to claim 1 or 2, wherein the formula β<0.30 [mrad] is satisfied.

4. The laminated glass according to claim 1 or 2, wherein the interlayer film comprises three or more layers.

5. The laminated glass according to claim 4, wherein the shear storage modulus of any layer other than both outermost layers in the interlayer film is smaller than the shear storage modulus of both outermost layers.

6. The laminated glass according to claim 1 or 2, wherein the average thickness of the interlayer film in an area on the straight line that is 60 mm or more and 140 mm or less from the second point is 0.80 mm or less.

7. The laminated glass according to claim 1 or 2, wherein a molding is disposed on the outer edge of said fourth surface, and an end of said interlayer film is exposed from said molding at and near said lower edge.

8. The first glass plate is composed of Fe in a weight ratio. 2 O 3 The sum of the total iron content converted into Fe is lower than that of the second glass sheet, and the second glass sheet has a weight ratio of Fe 2 O 3 3. The laminated glass according to claim 1, wherein the sum of the total iron content calculated as iron content is 0.1% or more.

9. The laminated glass according to claim 1 or 2, wherein, in plan view, a shielding layer is provided on the outer edge of the lower side and its vicinity of the second surface, and no shielding layer is provided on the outer edge of the lower side of the fourth surface.

10. The laminated glass according to claim 1 or 2, wherein a shielding layer is provided on the second surface and / or the fourth surface, and an information transmitting / receiving area is provided within an opening in the shielding layer.

11. The laminated glass according to claim 1 or 2, wherein the difference in thickness between the first glass sheet and the second glass sheet is less than 0.2 mm.

12. The laminated glass according to claim 1 or 2, wherein a shielding layer is provided on the second surface and / or the fourth surface in an area including a range that is 60 mm or more and 540 mm or less from the second point on the straight line.

13. A method for manufacturing laminated glass comprising a curved first glass sheet, a curved second glass sheet, and an intermediate film located between the first glass sheet and the second glass sheet and bonding the first glass sheet and the second glass sheet, comprising the steps of: preparing the first glass sheet having a third side and a fourth side, the intermediate film, and the second glass sheet having a first side and a second side; forming a coating film on the second side, the third side, or the fourth side, the coating film being configured to have a visible light reflectance of 10% or more for P-polarized visible light incident at an incident angle of 65 degrees; bending the first glass sheet and the second glass sheet after the step of forming the coating film; and extending at least one side of two opposing sides of the intermediate film along the one side in a plan view. and placing the stretched interlayer film between the third surface of the first glass sheet and the second surface of the second glass sheet and pressing the stretched interlayer film, wherein in the stretching step, the interlayer film has a region that has a wedge-shaped cross section whose thickness gradually increases from a lower edge to an upper edge of the fourth surface in a state in which the laminated glass is attached to a vehicle, and the interlayer film is stretched such that, on a line that passes through a first point that bisects the upper edge and a second point that bisects the lower edge in a plan view, a local wedge angle α at a position 100 mm away from the second point and a local wedge angle β at a position 500 mm away from the second point satisfy the formula: (β - α) > 0.05 [mrad].

Citation Information

Patent Citations

  • gaming machines

    JP2023052990A

  • laminated glass plate

    JP6065221B2

  • Apparatus for stretching plastic

    US2933759A

  • Transparent laminate with resin molding, window material of vehicle or building, and method for manufacturing transparent laminate with resin molding

    JP2013163627A

  • Curved vehicle windshield made from laminated glass

    JP2014024752A

Cited By

  • Automobile window glass

    WO2026115937A1