Fumed silica for rubber composition and method for compressing fumed silica
Fumed silica with increased tap density and a controlled pore structure, combined with specific dispersion methods and silane coupling agents, addresses the wear and heat aging challenges in rubber tire compositions, enhancing performance and efficiency while reducing blending complexity.
Patent Information
- Application Number
- PCT/JP2024/012335
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-08-24
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Existing rubber tire compositions face challenges in achieving long tire lifespan due to inferior wear resistance and heat aging resistance when using wet silica as a reinforcing filler, leading to the need for increased carbon black content, which reduces fuel efficiency and productivity issues with bulky dry silica blending.
The development of fumed silica with increased tap density and a predetermined pore structure, allowing for sufficient dispersion in rubber components with reduced blending times, using methods like ball milling, vibrating milling, and uniaxial compression pressing, along with the use of a silane coupling agent to enhance dispersion and prevent agglomeration.
This approach enables fumed silica to be effectively dispersed in rubber compositions, improving wear resistance and heat aging resistance while maintaining fuel efficiency, reducing the need for carbon black and enhancing productivity by minimizing the number of blending divisions.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Fumed silica for rubber compositions and method for compressing fumed silica
[0001] The present invention relates to a fumed silica for use in a rubber composition and a method for compressing the fumed silica, and more particularly to a fumed silica that is easily and sufficiently dispersed in a rubber component and a method for compressing the fumed silica.
[0002] Automobile tires are required to have not only low fuel consumption but also a long life. To achieve a long life, it is necessary to improve the abrasion resistance and heat aging resistance of tires. To improve abrasion resistance, carbon black has been compounded as a reinforcing filler into rubber compositions for tires.
[0003] On the other hand, it is known that wet silica is effective in improving fuel economy, but the abrasion resistance when wet silica is blended is inferior to the abrasion resistance when carbon black is blended. Therefore, when wet silica is used as a reinforcing filler, part of the carbon black blended amount is replaced by wet silica, and the amount of carbon black blended is relatively reduced, so it is known that a decrease in the abrasion resistance of the tire rubber material is unavoidable.
[0004] Patent Document 1 proposes replacing a portion of wet silica with dry silica, and describes that dry silica can improve fuel economy and suppress a decrease in rubber hardness more than wet silica.
[0005] JP 2016-104840 A
[0006] However, in Patent Document 1, it is believed that the dry silica is compounded in a bulky state. When such bulky (low tap density) dry silica is compounded using a Banbury mixer, which is a common kneading device for rubber compositions, there is a problem that the dry silica does not get mixed into the rubber component and flows out. Therefore, it is necessary to compound the planned amount of dry silica in portions. However, there is a problem that the productivity decreases as the number of portions increases.
[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide fumed silica that can be sufficiently dispersed in a rubber component even with a small number of divided blending steps, and a method for compressing the fumed silica.
[0008] The present inventors have found that simply using fumed silica with a high tap density can result in the generation of aggregated particles of several tens of micrometers in unvulcanized or vulcanized rubber. Based on this finding, the present inventors have discovered that by not only increasing the tap density but also by providing a specific pore structure on the surface of the fumed silica, the fumed silica can be sufficiently dispersed even with fewer times of distribution and compounding in the rubber component, and have thus completed the present invention.
[0009] From the above, the aspects of the present invention are as follows.
[0010] [1] A fumed silica for a rubber composition having a tap density of 200 g / L or more, a pore peak radius of 22 nm or more obtained by applying the BJH method to an adsorption isotherm by nitrogen adsorption, and a pore volume of 1.6 mL / g or more. [2] The fumed silica for a rubber composition has a BET specific surface area of 180 m 2 / g or more 500m 2 [3] The fumed silica for a rubber composition according to [1] or [2], wherein the fumed silica for a rubber composition is untreated fumed silica for a rubber composition.
[0011] [4] A method for compressing fumed silica, in which fumed silica having a tap density of less than 200 g / L is subjected to uniaxial compression pressing to obtain compressed fumed silica having a tap density of 200 g / L or more.
[0012] According to the present invention, it is possible to provide fumed silica that can be sufficiently dispersed in a rubber component even with a small number of divided blending steps, and a method for compressing the fumed silica.
[0013] The present invention will be described in detail below based on specific embodiments in the following order: 1. Fumed silica for rubber compositions 2. Method for compressing fumed silica 2.1. Using a ball mill 2.2. Using a vibration mill 2.3. Using a uniaxial opposed compression press 3. Rubber composition 3.1. Diene rubber 3.2. Silane coupling agent 3.3. Amount of each component 3.4. Other components 4. Method for producing rubber composition
[0014] (1. Fumed Silica for Rubber Composition) The fumed silica for rubber composition according to this embodiment is fumed silica used to be compounded into a rubber composition, and is particularly preferably used in a rubber composition for tires. Fumed silica is fine particle silicon dioxide produced by high-temperature hydrolysis of silicon tetrachloride in an oxyhydrogen flame. Therefore, fumed silica is produced by a different method from wet silica produced by wet methods such as precipitation and gelation, and is also called dry silica. Among wet silicas, precipitated silica, which is generally used as a reinforcing material for rubber, has a specific surface area of 200 m 2 / g, while 400m 2 Fumed silica with a specific surface area of about 1 / g is used as a reinforcing material for silicone rubber, etc. Therefore, the primary particle size of the primary aggregates (smallest constituents) of fumed silica is smaller than that of precipitated silica due to its high specific surface area. The particles of fumed silica are aggregated and fused together in a beaded shape, forming bulky aggregates.
[0015] In this embodiment, the tap density of the fumed silica for a rubber composition is 200 g / L or more. As described above, fumed silica is bulky, and therefore, the tap density of fumed silica is usually lower than 200 g / L in many cases. Therefore, when the tap density of the fumed silica is low (when the fumed silica is bulky), the fumed silica for a rubber composition according to this embodiment is preferably fumed silica (compressed fumed silica) in which the tap density is increased by compressing the fumed silica.
[0016] Since the tap density of the fumed silica for rubber compositions is 200 g / L or more, the fumed silica for rubber compositions can be sufficiently dispersed in a rubber composition for tires even when the fumed silica for rubber compositions is blended with a rubber component and kneaded. Furthermore, even when a Banbury mixer, which is difficult to knead with bulky components, is used, the bulkiness is suppressed, so the fumed silica can be sufficiently kneaded with other components.
[0017] The tap density of the fumed silica for rubber compositions is preferably 250 g / L or more, more preferably 300 g / L or more. The upper limit of the tap density is not particularly limited, but from the viewpoint of production, it is, for example, 320 g / L or less.
[0018] In this embodiment, the bulkiness of the fumed silica for a rubber composition may be evaluated by a parameter other than the tap density. For example, it may be evaluated by the apparent density measured by the tamp method specified in JIS K5101-12-2.
[0019] The apparent density of the fumed silica for a rubber composition measured by the tamp method is preferably 150 g / L or more and 250 g / L or less, and more preferably 170 g / L or more and less than 200 g / L. A detailed method for measuring the apparent density by the tamp method will be described in the examples.
[0020] Although the method for compressing fumed silica will be described in detail later, examples of the method for compressing fumed silica include a method using a ball mill and a method using a vibration mill. In these methods, the fumed silica is compressed between balls or between balls and a mill container. When compression is performed using such hard materials with a small contact area, a mechanochemical reaction may occur, resulting in the generation of agglomerated particles with low dispersibility (e.g., particles with a particle size of 20 μm or more). As a result, agglomerated particles due to poor dispersion of the fumed silica may occur in the rubber composition, even though the tap density of the fumed silica is high and the number of divided blends is small.
[0021] The inventors speculate that such low dispersibility is due to the fact that compression improves the wettability of the rubber component and the fumed silica on the surface of the fumed silica, forming pores of a size that make it difficult for the silane coupling agent responsible for cross-linking to penetrate, slowing the rate at which the silane coupling agent penetrates into the fumed silica aggregates, and as a result, the coupling agent is unable to react sufficiently uniformly.
[0022] Therefore, the fumed silica for rubber compositions according to this embodiment has a pore peak radius of 22 nm or more, obtained by applying the BJH method to an adsorption isotherm by nitrogen adsorption, and a pore volume of 1.6 mL / g or more. Fumed silica for rubber compositions, in which the pores on the surface of the fumed silica are controlled as described above, can sufficiently react with a silane coupling agent, even if it has a high tap density, and can suppress the generation of agglomerated particles.
[0023] The pore peak radius is preferably 30 nm or more, more preferably 50 nm or more. On the other hand, the upper limit of the pore peak radius is not particularly limited, but is, for example, 85 nm.
[0024] The pore volume is preferably 2 mL / g or more, more preferably 4 mL / g, and the upper limit of the pore volume is not particularly limited, but is, for example, 6 mL / g.
[0025] The pore peak radius and pore volume are physical property values obtained by applying the BJH method to an adsorption isotherm by nitrogen adsorption. The adsorption isotherm by nitrogen adsorption can be obtained by measurement and analysis under conditions in which a sample degassed to a pressure of 1 Pa or less at 150°C is allowed to adsorb nitrogen at liquid nitrogen temperature.
[0026] In this embodiment, the BET specific surface area of the fumed silica for rubber compositions is 180 m 2 / g or more, and 2 / g or more is more preferable, and 250m 2When the BET specific surface area of the fumed silica for a rubber composition is within the above range, the number of silanol groups that serve as reaction sites with the diene rubber or the silane coupling agent can be sufficiently secured in the fumed silica for a rubber composition.
[0027] The upper limit of the BET specific surface area of the fumed silica for rubber compositions is not particularly limited, but for example, it is 500 m 2 / g. If the BET specific surface area of the fumed silica for rubber compositions is too small, the flame temperature during production of the fumed silica must be increased, which causes the structure unique to fumed silica to be lost and tends to make it difficult to produce fumed silica stably. If the BET specific surface area of the fumed silica for rubber compositions is too large, it tends to make it difficult to produce fumed silica stably. The above BET specific surface area is a specific surface area measured by the nitrogen adsorption BET method.
[0028] Fumed silica has siloxane bonds, but on its surface, in addition to siloxane groups, silanol groups, in which hydroxy groups are bonded to silicon atoms, are present. The density of silanol groups on the surface of fumed silica (surface silanol group density) is lower than that of wet silica due to differences in the manufacturing method. In this embodiment, the surface silanol group density of the fumed silica for rubber compositions is 3 groups / nm 2 By keeping the surface silanol group density within the above range, the amount of silanol groups, which are reaction sites with the coupling agent, is maintained while preventing a decrease in wettability with rubber due to moisture adsorption on the silica surface, thereby enabling the expectation of even finer dispersibility. Furthermore, although the cohesion of powders with a large amount of adsorbed moisture increases during the compression process, it is expected that silica aggregation during this compression process will be prevented.
[0029] The surface silanol group density may be measured by, for example, the Karl Fischer method, the Igros method, or active hydrogen titration using a Grignard reagent.
[0030] In addition, silanol groups tend to adsorb water. Therefore, surface treatments are sometimes performed to reduce the reactivity of silanol groups with water by reacting them with other substances. Surface-treated fumed silica is called surface-treated fumed silica, while untreated fumed silica is called untreated fumed silica.
[0031] In this embodiment, surface-treated fumed silica and untreated fumed silica are distinguished by the degree of modification hydrophobicity (M value) shown below. The degree of modification hydrophobicity (M value) is a value obtained by a measurement method utilizing the fact that surface-treated fumed silica floats in water but is completely suspended in methanol. The method described in the examples of WO 2004 / 099075 can be used to measure the M value. When surface-treated fumed silica and untreated fumed silica are represented by the M value, the M value of surface-treated fumed silica is 1 or more, and the M value of untreated fumed silica is less than 1.
[0032] In this embodiment, from the viewpoint that the silane coupling agent has a bulky molecular structure and can react in sufficient amounts with the silica surface, the fumed silica for rubber compositions is preferably untreated fumed silica for rubber compositions that contains little moisture that induces self-condensation of the coupling agent and has a sufficient number of silanol groups, which serve as reaction sites.
[0033] (2. Method for compressing fumed silica) The fumed silica for a rubber composition according to this embodiment has a tap density of 200 g / L or more. However, due to its manufacturing method, fumed silica is bulky and has a low tap density. Therefore, fumed silica for a rubber composition having a tap density of 200 g / L or more is generally obtained by compressing fumed silica.
[0034] As described above, examples of methods for compressing fumed silica include a method of compressing using a ball mill, a method of compressing using a vibration mill, etc. However, with ordinary compression methods, the pores on the surface of the fumed silica become too small due to compression, and it is thought that the small pores slow the rate at which the silane coupling agent penetrates and diffuses into the silica agglomerated particles.
[0035] Therefore, the surface of the fumed silica may be partially coated before compression so that the pore peak radius and pore volume after compression can easily satisfy the above-mentioned ranges. For example, a surfactant, wax, or the like can be used for the coating. Nonionic surfactants are preferred as surfactants. Examples of nonionic surfactants include fatty acid surfactants such as coconut oil fatty acid N-methylethanolamide, and alkylamine ether surfactants such as alkyldiamine EO adducts of N,N',N'-tris(2-hydroxyethyl)-N-alkyl(C14-C18))1,3-diaminopropane. Furthermore, hydrocarbon waxes are preferred as waxes, such as paraffin wax. Examples of paraffin waxes include general paraffin waxes with a melting point of approximately 60 to 80°C, and paraffin waxes commonly used as tire antioxidants. Examples of coating methods include a method in which molten wax is sprayed from a one-fluid or two-fluid nozzle into a mixer in which fumed silica has been mixed and stirred, and a method in which fumed silica and finely powdered wax particles are mixed together and then heated to a temperature equal to or higher than the melting point of the wax to melt the wax and diffuse it onto the silica surface.
[0036] When a uniaxial opposed compression press, a ball mill, or a vibration mill is used to compress the fumed silica, it is preferable to employ the following compression treatment conditions.
[0037] (2.1. When a ball mill is used) When the ball diameter is small, the curvature is small, so the compressive force from the balls tends to be a point load, whereas when the ball diameter is large, the compressive force tends to be a surface load. Therefore, the ball diameter in the ball mill is preferably 27 to 60 mm, and more preferably 32 to 45 mm. If the ball diameter is too small, the impact force caused by the concentrated load during crushing and compression is too strong, changing the pore structure on the surface of the fumed silica, and the above-mentioned range tends to not be satisfied. If the ball diameter is too large, the number of balls packed for the same volume is reduced, so the frequency of collisions is low, which increases the crushing time and may increase the production cost.
[0038] The rotation speed of the ball mill is preferably 50 to 600 rpm, more preferably 200 to 400 rpm. If the rotation speed is too low, the balls will not fall but will simply roll on the wall of the pot, which may result in insufficient impact force during grinding and may prevent the tap density of the fumed silica from increasing. Furthermore, if the rotation speed is too low, it will be necessary to extend the grinding time to achieve a tap density of 200 g / L or more, which may reduce productivity and increase production costs. If the rotation speed is too high, there is a risk of reduced grinding efficiency.
[0039] The ball filling rate in the ball mill is preferably 10 to 80%, more preferably 20 to 50%. If the ball filling rate is too low, the tap density of the fumed silica may not be high due to insufficient grinding efficiency. Furthermore, if the ball filling rate is too low, the grinding time must be extended to achieve a tap density of 200 g / L or more of the fumed silica, which may reduce productivity and increase production costs. If the ball filling rate is too high, the amount of material filled may decrease, which may reduce grinding efficiency.
[0040] (2.2. When a Vibration Mill is Used) The ball diameter or rod diameter in the vibration mill is preferably 27 mm or more, and more preferably 32 to 60 mm. If the ball diameter or rod diameter is too small, the impact during grinding will be too strong, changing the pore structure on the surface of the fumed silica, and the above-mentioned ranges will tend not to be satisfied. If the ball diameter is too large, the gaps between the balls will be large and the collision frequency will be low, which will lengthen the grinding time and may increase the production cost.
[0041] The vibration frequency in the vibration mill is preferably 600 to 2000 CPM, more preferably 800 to 1500 CPM. If the vibration frequency is too low, the impact force during pulverization may be insufficient, and the tap density of the fumed silica may not be high. Furthermore, if the vibration frequency is too low, it is necessary to extend the pulverization time to achieve a tap density of 200 g / L or more, which may reduce productivity and increase production costs. If the vibration frequency is too high, the impact force may be too large, and stable pulverization may not be possible.
[0042] The ball filling rate in the vibration mill is preferably 30 to 90%, more preferably 30 to 50%. If the ball filling rate is too low, the tap density of the fumed silica may not be high due to insufficient grinding efficiency. Furthermore, if the ball filling rate is too low, the grinding time must be extended to achieve a tap density of 200 g / L or more of the fumed silica, which may reduce productivity and increase production costs. If the ball filling rate is too high, the grinding efficiency may be reduced.
[0043] (2.3. Using a Uniaxial Opposed Compression Press) A uniaxial opposed compression press is a device that compresses powder by forcing it between opposing pressure rolls using a degassing screw or similar device. If the clearance between the rolls is kept sufficiently small, a uniform uniaxial compression force is continuously applied to the powder. On the other hand, in ball mill compression, the compression force tends to be a single point load, and there is a possibility that the same agglomerated powder may be repeatedly compressed. Therefore, using a uniaxial opposed compression press results in a smaller distribution of apparent density in the compressed powder compared to devices such as vibration mills and ball mills. It also prevents the increase of silanol groups due to mechanochemical effects. The degree of powder compression can be adjusted by adjusting the powder supply rate via the degassing screw, the pressure applied between the rolls, and the roll rotation speed to adjust the bulk density. Generally, a high bulk density product is obtained by slowing the roll rotation speed, increasing the inter-roll pressure, and slowing the roll rotation speed. If a low bulk density product is required, the opposite conditions can be selected.
[0044] (3. Rubber Composition) In this embodiment, the rubber composition contains the above-mentioned fumed silica for rubber compositions, a diene rubber, and a silane coupling agent. The rubber composition preferably further contains a diol. The rubber composition is preferably a rubber composition for tires.
[0045] (3.1. Diene Rubber) The diene rubber contained in the rubber composition is preferably at least one selected from natural rubber, isoprene rubber, butadiene rubber, styrene-butadiene rubber, acrylonitrile-butadiene rubber, butyl rubber, ethylene-propylene-diene rubber, and chloroprene rubber. The content of each of the above rubbers constituting the diene rubber may be determined appropriately depending on the application, etc. Among these, at least one selected from natural rubber and styrene-butadiene rubber is preferred.
[0046] Examples of natural rubber include natural rubber (NR) and modified natural rubbers such as epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), deproteinized natural rubber (DPNR), and high-purity natural rubber (HPNR). These natural rubbers may be used alone or in combination of two or more. In this embodiment, NR is preferred as the natural rubber.
[0047] Examples of styrene-butadiene rubber (SBR) include unmodified solution-polymerized SBR (S-SBR), unmodified emulsion-polymerized SBR (E-SBR), and modified SBRs thereof (modified S-SBR, modified E-SBR).
[0048] (3.2. Silane Coupling Agent) Hydrophobic diene rubber and the fumed silica for rubber compositions, which has hydrophilic silanol groups, have low affinity, making them difficult to mix during kneading. Therefore, by incorporating a silane coupling agent, a crosslinked structure between the diene rubber and the fumed silica for rubber compositions is easily formed via the silane coupling agent, making it easier for the fumed silica for rubber compositions to be uniformly dispersed in the diene rubber. As a result, the presence of coarse fumed silica that is not dispersed in the rubber component in the rubber composition can be suppressed.
[0049] The silane coupling agent is not particularly limited as long as it is one that is commonly used in rubber compositions. In this embodiment, a sulfur-containing silane coupling agent is preferred. Examples of sulfur-containing silane coupling agents include sulfide-based silane coupling agents, mercapto-based silane coupling agents, and thioester-based silane coupling agents. Examples of sulfide-based silane coupling agents include bis-(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)disulfide, and 3-trimethoxysilylpropylbenzothiazole tetrasulfide. Examples of mercapto-based silane coupling agents include γ-mercaptopropyltriethoxysilane and mercapto-thiocarboxylate oligomer. Examples of thioester-based silane coupling agents include 3-octanoylthiopropyltriethoxysilane.
[0050] (3.3. Diol) A diol is a dihydric alcohol, a hydrocarbon having two hydroxy groups. By incorporating a diol, the Mooney viscosity of the tire rubber composition is reduced, but the A hardness of the tire rubber material is increased, allowing the amount of fumed silica to be reduced. As a result, the fuel economy and abrasion resistance of the tire rubber material are improved. Furthermore, by incorporating a diol together with the above-mentioned silane coupling agent, a tire rubber material with good heat aging resistance can be obtained. Note that the above effects tend not to be obtained with monohydric alcohols and trihydric or higher alcohols.
[0051] In this embodiment, preferred examples of the diol include propylene glycol, 1,3-propanediol, dipropylene glycol, diethylene glycol, and polyethylene glycol having a degree of polymerization of about 200 to 1000, and propylene glycol, 1,3-propanediol, dipropylene glycol, diethylene glycol, and polyethylene glycol having a degree of polymerization of 300 to 500 are more preferred.
[0052] (3.4. Amount of Each Component) The amount of fumed silica for a rubber composition according to this embodiment is preferably 10 parts by mass or more and 70 parts by mass or less per 100 parts by mass of diene rubber. When the amount of fumed silica for a rubber composition is within the above range, a rubber composition in which the fumed silica for a rubber composition is sufficiently dispersed can be obtained. If the amount of fumed silica for a rubber composition is too large, the fumed silica will not be sufficiently dispersed in the rubber component, and a good kneaded product will not tend to be obtained.
[0053] The amount of the fumed silica for a rubber composition is more preferably 20 parts by mass or more, and even more preferably 32 parts by mass or more, per 100 parts by mass of the diene rubber, while the amount of the fumed silica for a rubber composition is more preferably 60 parts by mass or less, and even more preferably 50 parts by mass or less, per 100 parts by mass of the diene rubber.
[0054] From the viewpoint of increasing the wettability of the fumed silica surface to rubber and increasing the dispersibility of the fumed silica, the amount of the silane coupling agent (the content of the silane coupling agent in the rubber composition for tires) is set to 0.50 μmol / m relative to the BET specific surface area per 1 g of the fumed silica. 2 3.9 μmol / m or more 2 It is preferable that:
[0055] By using a silane coupling agent in an amount within the above range, the diene rubber and the fumed silica for rubber compositions are sufficiently dispersed, and a rubber composition can be obtained in which the fumed silica for rubber compositions is sufficiently dispersed in the rubber component. If the amount of silane coupling agent is too large, the coupling agent acts as a plasticizer, causing the viscosity of the rubber composition to become too low, resulting in insufficient dispersion of the fumed silica in the rubber component and an inability to obtain a good kneaded product. In addition, the hardness of the rubber after vulcanization tends to decrease, so the amount of filler required to achieve the same hardness tends to increase, resulting in poor fuel economy.
[0056] The amount of the silane coupling agent to be blended is 0.7 μmol / m relative to the specific surface area of the fumed silica. 2More preferably, it is equal to or greater than this.
[0057] The amount of the diol to be added may be determined according to the specific surface area of the fumed silica, similarly to the silane coupling agent, in order to reduce the viscosity of the kneaded rubber. The amount of the diol to be added (the content of the diol in the rubber composition) is 3 μmol / m relative to the BET specific surface area per 1 g of the fumed silica. 2 14 μmol / m or more 2 The following is the result.
[0058] The blending amount is 3.4 μmol / m 2 It is preferable that the concentration is 6.8 μmol / m or more. 2 On the other hand, the blending amount is more preferably 11 μmol / m or more. 2 It is preferable that:
[0059] (3.5. Other Components) In this embodiment, the rubber composition may contain components to be blended into rubber compositions in addition to the above-described components (diene rubber, fumed silica for rubber compositions, and silane coupling agent). An example of such a component is a lubricant. Blending a lubricant improves the kneadability of each component, making it easier to obtain a rubber composition in which each component is well dispersed.
[0060] Examples of lubricants include stearic acid and process oil. A lubricant may be used alone, or two or more types may be used in combination. Examples of process oils include aromatic oils made from mineral oils, synthetic oils, paraffin oils, naphthenic oils, etc. These may be used alone, or two or more types may be used in combination.
[0061] The amount of lubricant (the amount of lubricant in the rubber composition) is not limited. For example, the amount of lubricant is preferably 2 parts by mass or more and 60 parts by mass or less per 100 parts by mass of diene rubber. Furthermore, the amount of lubricant is more preferably 4 parts by mass or more and even more preferably 30 parts by mass or less per 100 parts by mass of diene rubber.
[0062] If the amount of lubricant is too small, the viscosity becomes high and kneading becomes poor, which may prevent the fumed silica for rubber compositions from being sufficiently dispersed in the diene rubber, whereas if the amount of lubricant is too large, shearing is not applied during kneading, which may prevent the fumed silica for rubber compositions from being sufficiently dispersed in the diene rubber.
[0063] Furthermore, the rubber composition may contain a reinforcing filler other than the fumed silica for rubber compositions. Examples of reinforcing fillers include carbon black, wet silica, clay, mica, talc, calcium carbonate, aluminum hydroxide, aluminum oxide, and titanium oxide. When a reinforcing filler is compounded, an appropriate amount of a filler coupling agent may also be compounded. The amount of the reinforcing filler to be compounded is not limited as long as the effects of the present invention can be obtained, and a general compounding amount may be used.
[0064] Furthermore, the rubber composition may contain various additives such as zinc oxide, antioxidants, plasticizers, processing aids, liquid polymers, thermosetting resins, etc. The amounts of these additives to be added are not limited as long as the effects of the present invention can be obtained, and may be general amounts.
[0065] (4. Method for Producing Rubber Composition) The rubber composition is obtained by kneading the diene rubber, the fumed silica for rubber compositions, the silane coupling agent, and, if necessary, other components.
[0066] In this embodiment, the rubber composition may be produced by kneading predetermined components to prepare a master batch, and then blending and kneading the remaining components into the master batch, or by kneading all of the components together.
[0067] When preparing the masterbatch, it is preferable to prepare the masterbatch by kneading the above-mentioned diene rubber, the above-mentioned fumed silica for rubber compositions, the above-mentioned silane coupling agent, and, if necessary, other components.
[0068] After the masterbatch is prepared, other components are blended into the masterbatch and kneaded to obtain a rubber composition. In this embodiment, since fumed silica for rubber compositions having a tap density of 200 g / L or more is blended, a rubber composition in which the fumed silica is sufficiently dispersed in the rubber components can be obtained even when kneading is performed using, for example, a Banbury mixer.
[0069] The kneading conditions may be set so that the components are thoroughly kneaded.
[0070] The rubber composition described above is suitable as a rubber composition for tires. By using the rubber composition according to this embodiment as a rubber composition for tires, a rubber material for tires excellent in fuel economy, abrasion resistance, and heat aging resistance can be obtained. The rubber material for tires is a material obtained by vulcanizing the rubber composition for tires.
[0071] Such rubber material for tires can be suitably used for tires for passenger cars, trucks, buses, etc. It can be suitably used for various tire components, particularly for treads, base treads, sidewalls, clinches, etc.
[0072] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments and may be modified in various ways within the scope of the present invention.
[0073] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0074] (Experiment 1) (Preparation of Rubber Composition for Tires) In Experiment 1, the diene rubber was SBR rubber. The following components (A) to (D) and (E-1) to (E-4) were charged into a 0.6 L Banbury mixer-type plastomill (Model BB600, manufactured by Toyo Seiki Seisaku-sho, Ltd.) so that the compounding amounts per 100 parts by mass of SBR rubber were as shown in Table 1. After charging, the rotor rotation speed was adjusted within a range of 20 to 100 rpm so that the temperature of the kneaded mixture was within a range of 140 to 150°C, and the mixture was kneaded for 5 minutes after the temperature was reached. The air cylinder pressure was 0.5 MPa. After kneading was completed, the mixture was cooled to room temperature and removed to obtain a kneaded mixture.
[0075] The amounts of diene rubber and other additives were calculated so that the fill factor after kneading would be 70%, and the components were added to the Plastomill and kneaded. The filler was added twice. (A) Diene rubber (A-1) SBR (S-SBR E-581 manufactured by Asahi Kasei Corporation) (A-2) BR (BR01 manufactured by ENEOS Materials Corporation) (B) Filler (B-1) Carbon black (S-SBR 6 manufactured by Tokai Carbon, nitrogen adsorption BET specific surface area: 120 m 2 / g, tap density: 400 g / L) (B-2) Wet silica (manufactured by Tosoh Silica, Nipsil AQ, nitrogen adsorption BET specific surface area: 200 m 2 / g, tap density: 300 g / L, silanol group density: 6 / nm 2 , Pycnometer method true density: 2.1 g / cm 3 (B-3) Hydrophilic fumed silica (manufactured by Tokuyama, Reolosil QS-40, nitrogen adsorption BET specific surface area: 380 m 2 / g, tap density 50 g / L, silanol group density 2.3 / nm 2 , Pycnometer method true density: 2.2 g / cm 3 (B-4) Hydrophilic fumed silica (manufactured by Tokuyama, Reolosil QS-30C, nitrogen adsorption BET specific surface area: 300 m 2 / g, tap density: 100 g / L, silanol group density: 2.1 / nm 2 , Pycnometer method true density: 2.2 g / cm 3 ) (BM-1) to (BM-3) Fumed silica compressed using a ball mill (BC-1) to (BC-4) Fumed silica compressed using a uniaxial opposed compression press (C) Silane coupling agent (C-1) Polysulfide coupling agent (Si69, manufactured by EVONIK) (D) Diol (D-1) 1,3-propanediol (E) Other components (E-1) Lubricant (stearic acid, NOF Corp., Beads Stearic Acid YR) (E-2) Lubricant (zinc oxide, Seido Chemical Co., Ltd., zinc oxide type 2) (E-3) Antioxidant (Ozonone 6C, manufactured by Seiko Chemical Co., Ltd.) (E-4) Process oil (Aromax 3 (TDAE Oil) manufactured by Fuji Industries Co., Ltd.)
[0076] [Preparation of Ball Mill-Compressed Fumed Silica] Fumed silica compressed by ball milling was prepared as follows. Approximately 200 g of the fumed silica (B-4) was placed in a 7-L alumina ball mill (filling ratio of alumina balls with a ball diameter of 32 mm, 30%) and milled at room temperature at 300 rpm for approximately 3 hours to obtain compressed fumed silica (BM-1) with a tap density of 200 g / L. By extending the ball milling time to 5 and 8 hours, respectively, compressed fumed silica (BM-2) with a tap density of 250 g / L and compressed fumed silica (BM-3) with a tap density of 320 g / L were obtained.
[0077] [Preparation of Uniaxially Opposed Compressed Fumed Silica] Fumed silica compressed using a uniaxial opposed compression press was prepared as follows. Specifically, the fumed silica (B-4) was compressed using a Freund Turbo WP-230x80 compactor as a uniaxial opposed compression press. The roller clearance was fixed at 0.5 mm, the roller rotation speed at 10 rpm, and the compression pressure applied to the roll at 0.3 T / cm. The degree of vacuum of the screw feeder feeding the powder to the roller was varied from -10 kPa to -45 kPa to obtain compressed fumed silica with different tap densities. The tap densities of the obtained compressed fumed silica were 200 g / L (BC-1), 250 g / L (BC-2), 320 g / L (BC-3), and 385 g / L (BC-4), respectively.
[0078] The tap density of the filler was measured as follows. First, a 1 L resin graduated cylinder was placed on an electronic balance, tared, and filled with approximately 1 L of filler, and the weight M1 (g) was recorded. After that, the cylinder was manually tapped 30 times from a height of approximately 10 cm, and the volume V1 (ml) was measured, and the tap density ρ1 was calculated using the following formula. The results are shown in Table 1. Tap density ρ1 = 1000 × M1 / V1 (g / L)
[0079] The apparent density of the filler by the tamp method was measured as follows. Each filler was passed through a sieve with 500 μm openings, dried at 105°C for 2 hours, and then cooled in a desiccator. 200±10 mL of filler was filled into the measuring cylinder of the tamp volume meter, and the weight of the filler, M2 (g), was recorded. After that, the measuring cylinder was rotated 1250 times using the cam of the tamp volume meter, and the volume V2 (mL) was measured, and the apparent density ρ2 by the tamp method was calculated using the following formula. Other measurement conditions were in accordance with JIS 5101-12-2. The results are shown in Table 1. Apparent density by the tamp method ρ2 = 1000 × M2 / V2 (g / L)
[0080] The nitrogen adsorption BET specific surface area of each filler was measured by the nitrogen adsorption BET method using a BELSOP MINI X manufactured by Microtrac Co., Ltd. The results are shown in Table 1.
[0081] The surface silanol group density of the fumed silica ((B-3), (B-4), (BM-1) to (BM-3), (BC-1) to (BC-4)) was measured using a coulometric titrator (MKC-610, manufactured by Kyoto Electronics Manufacturing Co., Ltd.) equipped with a moisture vaporizer (ADP-512, manufactured by Kyoto Electronics Manufacturing Co., Ltd.). That is, the temperature was raised to 130°C in the low-temperature furnace of the moisture vaporizer, and the moisture amount corresponding to the loss on drying of the silica was measured by coulometric titration using the MKC-610 model. Thereafter, the moisture amount corresponding to the loss on ignition was measured in the high-temperature furnace heated to 1000°C in the same manner by coulometric titration. The moisture amount corresponding to the loss on ignition generated between 130°C and 1000°C was converted to silanol group density using the following formula. The results are shown in Table 1. Silanol group density (number / nm 2 ) = 668.9 × H2O (%) / specific surface area (m 2 / g)
[0082] The pore peak radius and pore volume of the fumed silica ((B-3), (B-4), (BM-1) to (BM-3), (BC-1) to (BC-4)) were measured as follows. Using a BELSOP MINI X manufactured by Microtrac, an adsorption isotherm was obtained by adsorbing nitrogen at liquid nitrogen temperature onto a sample that had been degassed at 150°C to a pressure of 1 Pa or less. The pore peak radius and pore volume were calculated from the obtained adsorption isotherm based on the BJH theory using the analysis software provided with the BELSOP MINI X. The results are shown in Table 1.
[0083]
[0084] The kneaded product obtained above and the following components (E-5), (E-6), and (E-7) were added and mixed using a 6-inch roll tester to obtain a rubber composition for tires. The amount of sulfur added was set to the amount shown in Table 2, taking into account the amount of sulfur contained in the other added components. (E) Other Components (E-5) Sulfur (5% oil-containing fine sulfur powder manufactured by Tsurumi Chemical Industry Co., Ltd.) (E-6) Vulcanization accelerator (Sansera CM-G, N-cyclohexyl-2-benzothiazole sulfenamide (CBS) manufactured by Sanshin Chemical Industry Co., Ltd.) (E-7) Vulcanization accelerator (Sansera D-G, 1,3-diphenylguanidine (DPG) manufactured by Sanshin Chemical Industry Co., Ltd.)
[0085]
[0086] Test specimens were prepared from the resulting rubber compositions for tires to evaluate the following properties. The resulting test specimens were used to evaluate the following physical properties.
[0087] (Processability: Mooney Viscosity) For test pieces of the obtained rubber composition for tires, the Mooney viscosity at 100°C (ML1+4 100°C) was measured in accordance with JIS K6300-1 using a Mooney viscometer (VR-1132 manufactured by Ueshima Seisakusho). When the Mooney viscosity is low, the processability of the rubber composition for tires tends to be good. The results are shown in Table 2.
[0088] (Preparation of tire rubber material test pieces) Subsequently, the obtained tire rubber composition was press-vulcanized at 160°C for T90+1 minute to obtain a tire rubber material. Test pieces for the following evaluations were prepared from the obtained tire rubber material. The obtained test pieces were used to evaluate the following physical properties.
[0089] (A Hardness) The hardness (Shore A hardness) of the test pieces of the obtained rubber material for tires was measured using a durometer in accordance with JIS K6253 Type A. Since the target A hardness of the rubber material for tires is 65, it is preferable that the A hardness of the test pieces is also around 65. In Comparative Examples 3 to 5, the tap density of the filler was low, so the amount compounded per mixing (mixing volume) was large, and the filler was not kneaded into the other components in the mixer and instead flowed out of the mixer. Therefore, in Comparative Examples 3 to 5, only a smaller amount of filler than the planned amount could be compounded. As a result, the A hardness of the obtained rubber material was very low, making it unsuitable as a rubber material for tires. The results are shown in Table 2.
[0090] (Fuel efficiency performance: tan δ at 60°C) Test pieces of the obtained rubber material for tires were measured in accordance with JIS K6394 using a dynamic viscoelasticity tester (VR-7130 manufactured by Ueshima Seisakusho) under the following conditions. Tan δ (60°C) was calculated from the measured value at 60°C. Measurement temperature: 60°C Static strain: 10% Dynamic strain: ±2% Frequency: 10 Hz
[0091] The rolling resistance index was calculated using the following formula, with the calculated tan δ (60°C) of Standard Example 1 (Comparative Example 1) set to 1.0. The higher the index, the better the rolling resistance. The results are shown in Table 2. (Rolling resistance index) = (tan δ (60°C) of Standard Example 1) / (tan δ (60°C) of Example)
[0092] (Wear resistance performance: FPS abrasion volume) For the test pieces of the obtained rubber material for tires, the FPS abrasion volume was measured using an FPS abrasion tester (AB-2012 manufactured by Ueshima Seisakusho) under conditions of a temperature of 35°C, a load of 40 N, a slip ratio of 10%, and a test time of 2 minutes. The volume loss was calculated from the FPS abrasion volume, and the abrasion index was calculated using the following formula, with the loss volume of Standard Example 1 (Comparative Example 1) being set at 1.0. The higher the index, the better the abrasion resistance performance. The results are shown in Table 2. (Wear index) = (loss volume of Standard Example 1) / (loss volume of Example)
[0093] (Heat Aging Resistance) The obtained rubber composition for tires was vulcanized in a 2 mm thick mold at 160°C for T90+1 minute, and the obtained vulcanized rubber sheet was punched out using a JIS No. 3 dumbbell to prepare a sample. The sample was heat aged for 5 days (120 hours) in a Geer oven set at 80°C, and then the strength at break (breaking strength) of the sample, together with an unaged sample, was measured using a tensile tester in accordance with JIS K6251. The ratio of the unaged breaking strength to the breaking strength after aging was taken as an index of heat aging resistance. The heat resistance index was calculated using the following formula. A heat resistance index of 1 or more indicates excellent heat aging resistance, while a heat resistance index of less than 1 indicates poor heat aging resistance due to a decrease in breaking strength caused by thermal degradation. The results are shown in Table 2. (Heat resistance index) = {(breaking strength after heat aging) / (breaking strength of unaged sample)}
[0094] Furthermore, for the samples before the heat aging test, the strength index was calculated using the following formula, with the breaking strength of Standard Example 1 (Comparative Example 1) set at 1.00. The higher the strength index, the better the strength. The results are shown in Table 2. (Strength index) = (Breaking strength of Example) / (Breaking strength of Standard Example 1)
[0095] From Table 2, it was confirmed that when the diene rubber is SBR rubber, by using fumed silica for rubber compositions having the above-mentioned physical properties as a filler, a rubber material for tires having good properties can be obtained while reducing the number of times the fumed silica for rubber compositions is compounded in installments. On the other hand, it was confirmed that when the number of times a filler with a low tap density is compounded is reduced, only an amount of the filler smaller than the planned amount can be compounded, and a rubber material having the desired hardness cannot be obtained.
[0096] (Experiment 2) In Experiment 2, natural rubber was used as the diene rubber. (A-3) shown below, and the above-mentioned (B) to (D), (E-1) to (E-4) were charged into a 0.6 L Banbury mixer-type plastomill (Model BB600, manufactured by Toyo Seiki Seisaku-sho) so that the compounding amounts per 100 parts by mass of natural rubber were as shown in Table 3. After charging, a kneaded product was prepared under the same conditions as in Experiment 1. The filler (B), silane coupling agent (C), diol (D), and other components (E-1) to (E-4) other than (A-3) were the same as those used in Experiment 1. Therefore, the physical properties of the fillers used in Experiment 2 are as shown in Table 1. (A) Diene rubber (A-3) Natural rubber made in Vietnam: SVR
[0097] The kneaded product obtained, (E-5) above, and (E-8) shown below were added and mixed using a 6-inch roll tester to obtain a rubber composition for tires. The amount of sulfur added was set to the amount shown in Table 3, taking into account the amount of sulfur contained in other added components. The other component (E-5) was the same as the component used in Experiment 1. (E) Other Components (E-8) Vulcanization accelerator (Suncerer NS-G N-(tert-butyl)-2-benzothiazole sulfenamide (TBBS) manufactured by Sanshin Chemical Industry Co., Ltd.)
[0098] Test specimens were prepared from the obtained rubber composition for tires by the same method as in Experiment 1, and the physical properties were evaluated by the same method and conditions as in Experiment 1. The results are shown in Table 3. Furthermore, the obtained rubber composition for tires was vulcanized under the same conditions as in Experiment 1 to obtain a rubber material for tires. Test specimens were prepared from the obtained rubber material for tires by the same method as in Experiment 1, and the physical properties were evaluated by the same method and conditions as in Experiment 1. The results are shown in Table 3.
[0099]
[0100] From Table 3, it was confirmed that even when the diene rubber is natural rubber, by using fumed silica for rubber compositions having the above-mentioned physical properties as a filler, it is possible to obtain a rubber material for tires having good properties while reducing the number of times the fumed silica for rubber compositions is mixed in. On the other hand, it was confirmed that when the number of times a filler with a low tap density is mixed is reduced, only an amount of the filler smaller than the planned amount can be mixed, and a rubber material having the desired hardness cannot be obtained.
[0101] The fumed silica of the present invention is obtained by compressing bulky fumed silica into a dust-free form. Therefore, by using the fumed silica of the present invention, not only can it be added to the above-mentioned rubber composition for tires, but also when it is added to silicone rubber, clear rubber for shoes, and paints other than tires, it can be expected to prevent dust generation and shorten processing time by being quickly incorporated into the medium.
Claims
1. A fumed silica for rubber compositions having a tap density of 200 g / L or more, a pore peak radius of 22 nm or more, as obtained by applying the BJH method to an adsorption isotherm by nitrogen adsorption, and a pore volume of 1.6 mL / g or more.
2. The BET specific surface area of the fumed silica for rubber compositions is 180 m 2 / g or more 500m 2 The fumed silica for a rubber composition according to claim 1, wherein the molecular weight of the fumed silica is 1 / g or less.
3. The fumed silica for rubber compositions according to claim 1 or 2, wherein the fumed silica for rubber compositions is an untreated fumed silica for rubber compositions.
4. A method for compressing fumed silica, comprising uniaxially compressing fumed silica having a tap density of less than 200 g / L to obtain compressed fumed silica having a tap density of 200 g / L or more.
Citation Information
Patent Citations
Tire rubber composition
JP2016104840A
Hydrophobic fumed silica
WO2004099075A1
Production of silicon nitride-silicon carbide composite sintered compact
JP1994116038A
Granule composed of silicon dioxide as base produced by pyrolysis method,its production, and catalyst carrier containing it
JP1996253309A
Dispersion liquid for producing sintered material
JP2004161611A