Interlayer film for laminated glass, and laminated glass
The interlayer film configuration addresses the issue of reduced vibration damping in high frequency regions by maintaining consistent thickness ratios and glass transition temperatures, enhancing sound insulation and mechanical strength while minimizing scrap generation.
Patent Information
- Application Number
- PCT/JP2024/012452
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Laminated glass manufactured using interlayer films produced by extrusion molding often experiences reduced vibration damping performance in high frequency regions due to unintended changes in layer thickness at the end portions, leading to suboptimal performance in scattering glass fragments upon impact.
The interlayer film is designed with specific configurations, such as varying glass transition temperatures and layer structures, to maintain consistent thickness ratios and improve vibration damping properties across the end portions, enhancing sound insulation and mechanical strength while reducing scrap generation.
The improved interlayer film configuration enhances vibration damping in high frequency regions, maintaining sound insulation and mechanical strength, and reduces scrap generation during manufacturing, effectively addressing the limitations of existing extrusion molding methods.
Smart Images

Figure JP2024012452_03102024_PF_FP_ABST
Abstract
Description
Interlayer film for laminated glass and laminated glass
[0001] The present invention relates to an interlayer film for laminated glass used to obtain laminated glass. The present invention also relates to laminated glass using the interlayer film for laminated glass.
[0002] Laminated glass is excellent in safety because it generates only a small amount of glass fragments even when broken by external impact. For this reason, laminated glass is widely used in automobiles, railway vehicles, aircraft, ships, buildings, etc. Laminated glass is manufactured by sandwiching an interlayer film between a pair of glass sheets.
[0003] Patent Document 1 below discloses a viscoelastic plastic interlayer (interlayer film) intended to be incorporated between two glass panes to form a laminated glazing with vibration and sound damping properties, the interlayer including at least one layer made of a viscoelastic plastic with vibration and sound damping properties and having a specific resonant frequency and a specific loss factor.
[0004] WO2013 / 175101A1
[0005] Interlayer films are generally produced by extrusion molding. The present inventors have found that laminated glass produced using an interlayer film produced by extrusion molding may not be able to improve vibration damping in the high frequency range at edge portions of the laminated glass that correspond to the edge portions of the interlayer film.
[0006] An object of the present invention is to provide an interlayer film for laminated glass that can improve vibration damping in the high frequency range at the edge portion of the laminated glass that corresponds to the edge portion of the interlayer film. Another object of the present invention is to provide laminated glass that can improve vibration damping in the high frequency range at the edge portion of the laminated glass.
[0007] This specification discloses the following interlayer film for laminated glass and laminated glass.
[0008] Item 1. An interlayer film for laminated glass, the interlayer film having a first end and a second end opposite the first end, wherein when laminated glass P is obtained by disposing a portion of the interlayer film from the first end toward the second end between two sheets of green glass each having a thickness of 2.0 mm, laminated glass Q is obtained by disposing a portion of the interlayer film from the first end toward the second end between two sheets of green glass each having a thickness of 2.0 mm, laminated glass R is obtained by disposing a portion of the interlayer film from the second end toward the first end between two sheets of green glass each having a thickness of 0 mm and a thickness of 25 mm, and laminated glass S is obtained by disposing a portion of the interlayer film from the second end toward the first end between two sheets of green glass each having a thickness of 2.0 mm.
[0009] Configuration A: The rate of change A1 represented by the following formula (A1) is less than 10%, and the rate of change A2 represented by the following formula (A2) is less than 10%.
[0010] Rate of change A1 (%) = (|P A -Q A | / Q A )×100...(A1)
[0011] P A : Secondary loss coefficient of the laminated glass P Q A : Secondary loss coefficient of the laminated glass Q
[0012] Rate of change A2 (%) = (|R A -S A | / S A )×100...(A2)
[0013] R A : Secondary loss coefficient of the laminated glass R S A : Secondary loss coefficient of the laminated glass S
[0014] Configuration B: The rate of change B1 represented by the following formula (B1) is less than 10%, and the rate of change B2 represented by the following formula (B2) is less than 10%.
[0015] Change rate B1 (%) = (|P B -Q B | / Q B )×100...(B1) P B : Secondary resonance frequency Q of the laminated glass P B : Secondary resonance frequency of the laminated glass Q
[0016] Rate of change B2 (%) = (|R B -S B | / S B )×100...(B2)
[0017] R B : Secondary resonance frequency S of the laminated glass R B : Secondary resonance frequency of the laminated glass S
[0018] Item 2. The interlayer film for laminated glass according to Item 1, which satisfies the above-mentioned configuration A.
[0019] Item 3. The interlayer film for laminated glass according to Item 1, wherein the configuration B is satisfied.
[0020] Item 4. The interlayer film for laminated glass according to Item 1, wherein the configuration A and the configuration B are satisfied.
[0021] Item 5. The interlayer film for laminated glass according to any one of Items 1 to 4, comprising a first layer containing a resin and a second layer containing a resin, the second layer being disposed on the first surface side of the first layer.
[0022] Item 6. The interlayer film for laminated glass according to Item 5, wherein the resin in the first layer is a thermoplastic resin, and the resin in the second layer is a thermoplastic resin.
[0023] Item 7. The interlayer film for laminated glass according to Item 5 or 6, further comprising a third layer containing a resin, the third layer being disposed on a second surface side of the first layer opposite the first surface side.
[0024] Item 8. The interlayer film for laminated glass according to Item 7, wherein the resin in the third layer is a thermoplastic resin.
[0025] Item 9. The interlayer film for laminated glass according to any one of Items 5 to 8, wherein the first layer and the second layer have different glass transition temperatures.
[0026] Item 10. The interlayer film for laminated glass according to any one of Items 5 to 9, wherein the layer having the highest glass transition temperature has a glass transition temperature of 32°C or higher.
[0027] Item 11. The interlayer film for laminated glass according to Item 10, wherein the layer having the highest glass transition temperature has a glass transition temperature of 37°C or higher.
[0028] Item 12. The interlayer film for laminated glass according to any one of Items 5 to 11, wherein the second layer is a surface layer of the interlayer film and is the layer with the highest glass transition temperature.
[0029] Item 13. The interlayer film for laminated glass according to any one of Items 5 to 12, wherein the tan δ at the glass transition temperature of the layer with the lowest glass transition temperature is 1.2 or greater.
[0030] Item 14. The interlayer film for laminated glass according to Item 13, wherein the tan δ at the glass transition temperature of the layer with the lowest glass transition temperature is 1.4 or higher.
[0031] Item 15. The interlayer film for laminated glass according to any one of Items 5 to 14, wherein the first layer is the layer with the lowest glass transition temperature.
[0032] Item 16. The interlayer film for laminated glass according to any one of Items 5 to 15, wherein the end face of the first end portion has an end face of the layer with the lowest glass transition temperature, and the end face of the second end portion has an end face of the layer with the lowest glass transition temperature.
[0033] Item 17. The interlayer film for laminated glass according to any one of Items 5 to 16, which satisfies the following configuration C:
[0034] Configuration C: The rate of change C1 represented by the following formula (C1) is greater than 0% and not greater than 50%, and the rate of change C2 represented by the following formula (C2) is greater than 0% and not greater than 50%.
[0035] Rate of change C1 (%) = (|T P -T Q | / T Q)×100...(C1)
[0036] T P : The ratio of the thickness of the layer with the lowest glass transition temperature at a position 12.5 mm from the first end toward the second end to the thickness of the interlayer film at a position 12.5 mm from the first end toward the second end, T Q : The ratio of the thickness of the layer with the lowest glass transition temperature at a position 112.5 mm from the first end toward the second end to the thickness of the interlayer film at a position 112.5 mm from the first end toward the second end
[0037] Rate of change C2 (%) = (|T R -T S | / T S )×100...(C2)
[0038] T R : The ratio of the thickness of the layer with the lowest glass transition temperature at a position 12.5 mm from the second end toward the first end to the thickness of the interlayer film at a position 12.5 mm from the second end toward the first end, T S : The ratio of the thickness of the layer with the lowest glass transition temperature at a position 112.5 mm from the second end toward the first end to the thickness of the interlayer film at a position 112.5 mm from the second end toward the first end
[0039] Item 18. The interlayer film for laminated glass according to any one of Items 1 to 17, comprising a resin and a plasticizer, wherein the content of the plasticizer contained in the interlayer film is 36 parts by weight or less per 100 parts by weight of the resin contained in the interlayer film.
[0040] Item 19. The interlayer film for laminated glass according to any one of Items 1 to 18, wherein the cross-sectional shape of the interlayer film in the thickness direction is wedge-shaped.
[0041] Item 20. A laminated glass comprising a first laminated glass member, a second laminated glass member, and the interlayer film for laminated glass according to any one of Items 1 to 19, wherein the interlayer film for laminated glass is disposed between the first laminated glass member and the second laminated glass member.
[0042] Item 21. A laminated glass having a first end and a second end opposite the first end, wherein the following configuration A' or the following configuration B' is satisfied.
[0043] Configuration A': The rate of change A3 represented by the following formula (A3) is less than 10%, and the rate of change A4 represented by the following formula (A4) is less than 10%.
[0044] Rate of change A3 (%) = (|P A '-Q A '| / Q A ')×100...(A3)
[0045] P A Q′: Secondary loss coefficient of the laminated glass in the portion of the laminated glass from the position of 0 mm to the position of 25 mm from the first end toward the second end A ': Secondary loss coefficient of the laminated glass in a portion of the laminated glass from a position 100 mm to a position 125 mm from the first end toward the second end
[0046] Rate of change A4 (%) = (|R A '-S A '| / S A ')×100...(A4)
[0047] R A ': secondary loss coefficient S of the laminated glass in a portion of the laminated glass from the position of 0 mm to the position of 25 mm from the second end toward the first end A ': Secondary loss coefficient of the laminated glass in a portion of the laminated glass from a position 100 mm to a position 125 mm from the second end toward the first end
[0048] Configuration B': The rate of change B3 represented by the following formula (B3) is less than 10%, and the rate of change B4 represented by the following formula (B4) is less than 10%.
[0049] Rate of change B3 (%) = (|P B '-Q B '| / Q B ')×100...(B3)
[0050] PB Q′: the second resonance frequency of the laminated glass in the portion of the laminated glass from the position of 0 mm to the position of 25 mm from the first end toward the second end B ': Secondary resonance frequency of the laminated glass in a portion of the laminated glass from a position 100 mm to a position 125 mm from the first end toward the second end
[0051] Rate of change B4 (%) = (|R B '-S B '| / S B ')×100...(B4)
[0052] R B ': the secondary resonance frequency S of the laminated glass in the portion of the laminated glass from the position of 0 mm to the position of 25 mm from the second end toward the first end B ': Secondary resonance frequency of the laminated glass in a portion of the laminated glass from a position 100 mm to a position 125 mm from the second end toward the first end
[0053] The interlayer film for laminated glass according to the present invention can improve vibration damping in the high frequency range at the edge portions of the laminated glass that correspond to the edge portions of the interlayer film.
[0054] In the laminated glass according to the present invention, vibration damping properties in the high frequency range can be improved at the edge portions of the laminated glass.
[0055] Fig. 1 is a cross-sectional view schematically showing an interlayer film for laminated glass according to a first embodiment of the present invention. Fig. 2 is a cross-sectional view schematically showing an interlayer film for laminated glass according to a second embodiment of the present invention. Fig. 3 is a cross-sectional view schematically showing an example of laminated glass using the interlayer film for laminated glass shown in Fig. 1. Fig. 4 is a cross-sectional view schematically showing an example of laminated glass using the interlayer film for laminated glass shown in Fig. 2.
[0056] The present invention will be described in detail below.
[0057] (Interlayer Film for Laminated Glass) The interlayer film for laminated glass according to the present invention (sometimes abbreviated as "interlayer film" in this specification) is used in laminated glass.
[0058] The interlayer film has a one-layer structure or a two- or more-layer structure. The interlayer film may have a one-layer structure or a two- or more-layer structure. The interlayer film may have a two-layer structure, a two- or more-layer structure, a three-layer structure, or a three- or more-layer structure. The interlayer film may have a structure of 10 or fewer layers, or a structure of 5 or fewer layers. The interlayer film may include only a first layer. The interlayer film may include a first layer and a second layer disposed on a first surface side of the first layer. The interlayer film may include a first layer, a second layer disposed on the first surface side of the first layer, and a third layer disposed on a second surface side of the first layer opposite the first surface side. The interlayer film may be a single-layer interlayer film or a multi-layer interlayer film. The structure of the interlayer film may be partially different. For example, the interlayer film may have a portion having a single-layer structure and a portion having a multi-layer structure.
[0059] The interlayer film has a first end (one end) and a second end (the other end) opposite the first end. The first end and the second end are opposite ends of the interlayer film. The interlayer film has an MD direction and a TD direction. The interlayer film is obtained, for example, by extrusion molding and is an extrusion molded product (preferably a melt extrusion molded product). The MD direction is the flow direction of the interlayer film during production. The TD direction is a direction perpendicular to the flow direction of the interlayer film during production and perpendicular to the thickness direction of the interlayer film. The first end and the second end are opposite ends of the interlayer film in the TD direction.
[0060] The above interlayer film is used to produce the following laminated glasses P, Q, R, and S. Note that depending on the distance between the first end and the second end of the interlayer film, laminated glass Q and laminated glass S may be the same.
[0061] Laminated glass P: A laminated glass obtained by placing the portion of the interlayer film from 0 mm to 25 mm from the first end toward the second end between two sheets of green glass with a thickness of 2.0 mm. The position 0 mm from the first end toward the second end is the position of the first end of the interlayer film.
[0062] Laminated glass Q: A laminated glass obtained by placing the portion of the interlayer film extending from the first end toward the second end, from a position 100 mm to a position 125 mm, between two sheets of green glass having a thickness of 2.0 mm.
[0063] Laminated glass R: A laminated glass obtained by placing the portion of the interlayer film from 0 mm to 25 mm from the second end toward the first end between two sheets of green glass with a thickness of 2.0 mm. The position 0 mm from the second end toward the first end is the position of the second end of the interlayer film.
[0064] Laminated glass S: A laminated glass obtained by placing the portion of the interlayer film extending from the second end toward the first end, from a position 100 mm to a position 125 mm, between two sheets of green glass having a thickness of 2.0 mm.
[0065] The laminated glasses P, Q, R, and S can be produced, for example, as follows.
[0066] Method for producing laminated glass P: An interlayer film for producing laminated glass P is prepared by, for example, cutting out a portion of the interlayer film from the first end to the second end, from the 0 mm position to the 25 mm position. The interlayer film for producing laminated glass P is sandwiched between two 2.0 mm-thick green glass sheets conforming to JIS R3208 to obtain a laminate. The obtained laminate is placed in a rubber bag and degassed at a vacuum of 0.08 MPa for 20 minutes. The degassed laminate is then transferred to an oven and vacuum-pressed at 90°C for 30 minutes to pre-press the laminate. The pre-pressed laminate is then pressed in an autoclave at 140°C and a pressure of 1.3 MPa for 20 minutes to obtain laminated glass P.
[0067] Method for producing laminated glass Q: An interlayer film for producing laminated glass Q is prepared by, for example, cutting out a portion of the interlayer film from the first end portion to a position 100 mm to 125 mm from the second end portion. Laminated glass Q is obtained in the same manner as in the method for producing laminated glass P, except that this interlayer film for producing laminated glass Q is used.
[0068] Method for producing laminated glass R: An interlayer film for producing laminated glass R is prepared by, for example, cutting out a portion of the interlayer film from the second end portion to a position from 0 mm to 25 mm toward the first end portion from the interlayer film. Laminated glass R is obtained in the same manner as the method for producing laminated glass P, except that this interlayer film for producing laminated glass R is used.
[0069] Method for producing laminated glass S: An interlayer film for producing laminated glass S is prepared by, for example, cutting out a portion of the interlayer film from the second end portion to a position 100 mm to 125 mm from the first end portion. Laminated glass S is obtained in the same manner as the method for producing laminated glass P, except that this interlayer film for producing laminated glass S is used.
[0070] The laminated glasses P, Q, R, and S may be obtained by the following method.
[0071] An interlayer film is sandwiched between two 2.0 mm thick green glass sheets conforming to JIS R3208 to obtain a laminate. The obtained laminate is placed in a rubber bag and degassed at a vacuum of 0.08 MPa for 20 minutes. The degassed laminate is then transferred to an oven and vacuum-pressed at 90°C for 30 minutes to pre-bond the laminate. The pre-bonded laminate is then compressed in an autoclave at 140°C and a pressure of 1.3 MPa for 20 minutes to obtain laminated glass X. The obtained laminated glass X is cut at predetermined positions to obtain laminated glasses P, Q, R, and S.
[0072] The width of each of the laminated glasses P, Q, R, and S was 25 mm. The length of each of the laminated glasses P, Q, R, and S was 300 mm, which is suitable for measuring the secondary loss factor and secondary resonance frequency described below.
[0073] When the above laminated glasses P, Q, R, and S are obtained, the interlayer film satisfies the following configuration A or the following configuration B.
[0074] Configuration A: The rate of change A1 represented by the following formula (A1) is less than 10%, and the rate of change A2 represented by the following formula (A2) is less than 10%.
[0075] Rate of change A1 (%) = (|P A -Q A | / Q A )×100...(A1)
[0076] P A : Secondary loss coefficient of the laminated glass P A : Secondary loss coefficient of the laminated glass Q
[0077] Rate of change A2 (%) = (|R A -S A | / S A )×100...(A2)
[0078] R A : Secondary loss coefficient of the laminated glass R A : Secondary loss coefficient of the laminated glass S
[0079] Configuration B: The rate of change B1 represented by the following formula (B1) is less than 10%, and the rate of change B2 represented by the following formula (B2) is less than 10%.
[0080] Change rate B1 (%) = (|P B -Q B | / Q B )×100...(B1)
[0081] P B : Secondary resonance frequency Q of the laminated glass P B : Secondary resonance frequency of the laminated glass Q
[0082] Rate of change B2 (%) = (|R B -S B | / S B )×100...(B2)
[0083] R B : Secondary resonance frequency of the laminated glass R B : Secondary resonance frequency of the laminated glass S
[0084] The interlayer film according to the present invention has the above-described configuration, and therefore can improve vibration damping in the high frequency range at the edge portion of the laminated glass that corresponds to the edge portion of the interlayer film.
[0085] Interlayer films are generally produced by extrusion molding. The present inventors have found that in laminated glass produced using an interlayer film produced by extrusion molding (particularly an interlayer film having a structure of two or more layers), it may not be possible to improve vibration damping in the high frequency range (e.g., 1000 Hz or higher and 3000 Hz or lower) at the edge portions of the laminated glass corresponding to the edge portions of the interlayer film.
[0086] The present inventors conducted extensive research into the causes of the above-mentioned problems and discovered the following (1) and (2). (1) In extrusion molding, even if the layers of an interlayer film can be molded with the desired thickness ratio in the central portion, the layers may not be molded with the desired thickness ratio in the edge portions on both sides of the interlayer film that face each other in the transverse direction. For example, even if the layers are extrusion molded to have a uniform thickness, the thickness of each layer is likely to vary in the edge portions on both sides of the interlayer film that face each other in the transverse direction, resulting in a change in the thickness ratio. In particular, the thickness of the interlayer film's intermediate layer is likely to be unintentionally reduced in the edge portions on both sides of the interlayer film that face each other in the transverse direction. (2) Unintentional changes in the thickness ratio of each layer in the edge portions of the interlayer film reduce the vibration damping properties in the high-frequency range at the edge portions of the laminated glass.
[0087] As a result of extensive research, the inventors have found that an interlayer film that satisfies the above-mentioned configuration A or B can improve vibration-damping properties in the high-frequency range at the edge portions of the laminated glass that correspond to the edge portions of the interlayer film.
[0088] In order to maintain high vibration-damping properties in the high-frequency range at the edge portions, it is also possible to cut off the entire portion of the interlayer film where the layers do not have the desired thickness ratio, and then use the cut interlayer film to manufacture laminated glass. However, this method generates a large amount of waste material.
[0089] In contrast, the interlayer film according to the present invention can improve vibration damping in the high frequency range while contributing to a reduction in scrap material.
[0090] The interlayer film according to the present invention can improve vibration damping in the high frequency range at the edge portions of the laminated glass, thereby improving vibration damping in the high frequency range throughout the laminated glass.
[0091] The interlayer film may satisfy the above-mentioned configuration A, may satisfy the above-mentioned configuration B, or may satisfy both the above-mentioned configurations A and B. From the viewpoint of more effectively exerting the effects of the present invention, the interlayer film preferably satisfies the above-mentioned configuration B, and more preferably satisfies the above-mentioned configurations A and B.
[0092] In an interlayer film that satisfies the above-mentioned configuration A, the rate of change A1 expressed by the above-mentioned formula (A1) is less than 10%, and the rate of change A2 expressed by the above-mentioned formula (A2) is less than 10%.
[0093] The rate of change A1 is preferably greater than 0%, more preferably 1% or greater, even more preferably 1.8% or greater, even more preferably 2% or greater, particularly preferably 3% or greater, most preferably 4% or greater, and preferably 9.7% or less, more preferably 9% or less, even more preferably 8% or less, even more preferably 7% or less, and particularly preferably 6% or less. When the rate of change A1 exceeds the lower limit or is equal to or greater than the lower limit, the generation of scrap material during the production of the interlayer film can be effectively suppressed. When the rate of change A1 is equal to or less than the upper limit, the effects of the present invention can be more effectively exhibited. The range of the rate of change A1 can be set by appropriately selecting the upper limit and the lower limit.
[0094] In an interlayer film satisfying the above-mentioned configuration A, it is preferable that the rate of change A1 satisfies the above-mentioned lower limit or upper limit in at least a portion of the region in the MD. In an interlayer film satisfying the above-mentioned configuration A, it is more preferable that when the secondary loss factors of a laminated glass P having a length of 300 mm in the MD and a laminated glass Q having a length of 300 mm in the MD are measured, the rate of change A1 satisfies the above-mentioned lower limit or upper limit. In an interlayer film satisfying the above-mentioned configuration A, it is even more preferable that when the secondary loss factors of two laminated glasses P having a length of 300 mm in the MD and two laminated glasses Q having a length of 300 mm in the MD, both made from a section of 600 mm in the MD, are measured, the rate of change A1 calculated from the average value of the secondary loss factors of each measured section satisfies the above-mentioned lower limit or upper limit. In an interlayer film satisfying the above-mentioned configuration A, when the secondary loss factors of three sheets of laminated glass P each having a length of 300 mm in the MD and three sheets of laminated glass Q each having a length of 300 mm in the MD, which are fabricated from a section of 900 mm in the MD, are measured, it is particularly preferable that the rate of change A1 calculated from the average value of the secondary loss factors in each measured section satisfies the above-mentioned lower limit or upper limit.In an interlayer film satisfying the above-mentioned configuration A, when the secondary loss factors of three sheets of laminated glass P each having a length of 300 mm in the MD and three sheets of laminated glass Q each having a length of 300 mm in the MD, which are fabricated from a section of 900 mm in the MD, are measured, it is most preferable that the rate of change A1 calculated from the secondary loss factors in each measured section satisfies the above-mentioned lower limit or upper limit, respectively.
[0095] The secondary loss coefficient of the laminated glass P (P A ) is preferably 0.20 or more, more preferably 0.25 or more, even more preferably 0.30 or more, and particularly preferably 0.35 or more. A When the secondary loss coefficient (P A The secondary loss coefficient (P) of the laminated glass P may be 0.80 or less, 0.75 or less, 0.70 or less, 0.65 or less, 0.60 or less, 0.55 or less, 0.50 or less, or 0.45 or less.A The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0096] The secondary loss coefficient of the laminated glass Q (Q A The secondary loss factor (Q) is preferably 0.20 or more, more preferably 0.30 or more, and even more preferably 0.35 or more. A When the secondary loss coefficient (Q ) of the laminated glass Q is equal to or greater than the above lower limit, the sound insulation of the laminated glass Q can be further improved. A The secondary loss coefficient (Q ) of the laminated glass Q may be 0.55 or less, 0.50 or less, or 0.45 or less. A The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0097] The rate of change A2 is preferably greater than 0%, more preferably 1% or greater, even more preferably 1.2% or greater, even more preferably 2% or greater, particularly preferably 3% or greater, most preferably 4% or greater, and preferably 9% or less, more preferably 8% or less, even more preferably 7% or less, even more preferably 6.9% or less, and particularly preferably 6% or less. When the rate of change A2 exceeds the lower limit or is equal to or greater than the lower limit, the generation of scrap material during the production of the interlayer film can be effectively suppressed. When the rate of change A2 is equal to or less than the upper limit, the effects of the present invention can be even more effectively exhibited. The range of the rate of change A2 can be set by appropriately selecting the upper limit and the lower limit.
[0098] In an interlayer film satisfying the above-mentioned configuration A, it is preferable that the rate of change A2 satisfies the above-mentioned lower limit or upper limit in at least a portion of the region in the MD. In an interlayer film satisfying the above-mentioned configuration A, it is more preferable that when the secondary loss factors of a laminated glass R having a length of 300 mm in the MD and a laminated glass S having a length of 300 mm in the MD are measured, the rate of change A2 satisfies the above-mentioned lower limit or upper limit. In an interlayer film satisfying the above-mentioned configuration A, it is even more preferable that when the secondary loss factors of two laminated glasses R having a length of 300 mm in the MD and two laminated glasses S having a length of 300 mm in the MD, both made from a section of 600 mm in the MD, are measured, the rate of change A2 calculated from the average value of the secondary loss factors of each measured section satisfies the above-mentioned lower limit or upper limit. In an interlayer film satisfying the above-mentioned configuration A, when the secondary loss factors of three sheets of laminated glass R each having a length of 300 mm in the MD and three sheets of laminated glass S each having a length of 300 mm in the MD, which are fabricated from a section of 900 mm in the MD, are measured, it is particularly preferable that the rate of change A2 calculated from the average value of the secondary loss factors in each measured section satisfies the above-mentioned lower limit or upper limit. In an interlayer film satisfying the above-mentioned configuration A, when the secondary loss factors of three sheets of laminated glass R each having a length of 300 mm in the MD and three sheets of laminated glass S each having a length of 300 mm in the MD, which are fabricated from a section of 900 mm in the MD, are measured, it is most preferable that the rate of change A2 calculated from the secondary loss factors in each measured section satisfies the above-mentioned lower limit or upper limit, respectively.
[0099] The secondary loss coefficient of the laminated glass R (R A ) is preferably 0.20 or more, more preferably 0.25 or more, even more preferably 0.30 or more, and particularly preferably 0.35 or more. A When the secondary loss coefficient (R A The secondary loss coefficient (R ) of the laminated glass R may be 0.80 or less, 0.75 or less, 0.70 or less, 0.65 or less, 0.60 or less, 0.55 or less, 0.50 or less, or 0.45 or less.A The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0100] The secondary loss coefficient of the laminated glass S (S A ) is preferably 0.20 or more, more preferably 0.30 or more, and even more preferably 0.35 or more. A When the secondary loss coefficient (S A The secondary loss coefficient (S A The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0101] In an interlayer film that satisfies the above-mentioned configuration B, the rate of change B1 expressed by the above-mentioned formula (B1) is less than 10%, and the rate of change B2 expressed by the above-mentioned formula (B2) is less than 10%.
[0102] The rate of change B1 is preferably greater than 0%, more preferably 1% or greater, even more preferably 1.8% or greater, even more preferably 2% or greater, particularly preferably 3% or greater, most preferably 4% or greater, and preferably 9% or less, more preferably 8% or less, even more preferably 7.9% or less, even more preferably 7% or less, and particularly preferably 6% or less. When the rate of change B1 exceeds the lower limit or is equal to or greater than the lower limit, the generation of scrap material during the production of the interlayer film can be effectively suppressed. When the rate of change B1 is equal to or less than the upper limit, the effects of the present invention can be more effectively exhibited. The range of the rate of change B1 can be set by appropriately selecting the upper limit and the lower limit.
[0103] In an interlayer film satisfying the above-mentioned configuration B, it is preferable that the rate of change B1 satisfies the above-mentioned lower limit or upper limit in at least a portion of the region in the MD. In an interlayer film satisfying the above-mentioned configuration B, it is more preferable that when the secondary resonance frequencies of a laminated glass P having a length of 300 mm in the MD and a laminated glass Q having a length of 300 mm in the MD are measured, the rate of change B1 satisfies the above-mentioned lower limit or upper limit. In an interlayer film satisfying the above-mentioned configuration B, it is even more preferable that when the secondary resonance frequencies of two laminated glasses P having a length of 300 mm in the MD and two laminated glasses Q having a length of 300 mm in the MD, both made from a 600 mm section in the MD, are measured, the rate of change B1 calculated from the average value of the secondary resonance frequencies in each measured section satisfies the above-mentioned lower limit or upper limit. In an interlayer film satisfying the above-mentioned configuration B, it is particularly preferable that, when the secondary resonance frequencies of three sheets of laminated glass P and three sheets of laminated glass Q each having a length of 300 mm in the MD, which are fabricated from a section of 900 mm in the MD, are measured, the rate of change B1 calculated from the average value of the secondary resonance frequencies in each measured section satisfies the above-mentioned lower limit or upper limit.In an interlayer film satisfying the above-mentioned configuration B, it is most preferable that, when the secondary resonance frequencies of three sheets of laminated glass P and three sheets of laminated glass Q each having a length of 300 mm in the MD, which are fabricated from a section of 900 mm in the MD, are measured, the rate of change B1 calculated from the secondary resonance frequencies in each measured section satisfies the above-mentioned lower limit or upper limit, respectively.
[0104] The secondary resonance frequency of the laminated glass P (P B The secondary resonance frequency (P) is preferably 600 Hz or more, more preferably 700 Hz or more, even more preferably 720 Hz or more, particularly preferably 760 Hz or more, and is preferably 1000 Hz or less, more preferably 900 Hz or less, and even more preferably 840 Hz or less. B When the secondary resonance frequency (P) of the laminated glass P is equal to or greater than the lower limit and equal to or less than the upper limit, the sound insulation of the laminated glass P can be further improved. B The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0105] The secondary resonance frequency (Q B The secondary resonance frequency (Q B When the secondary resonance frequency (Q ) of the laminated glass Q is equal to or greater than the lower limit and equal to or less than the upper limit, the sound insulation of the laminated glass Q can be further improved. B The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0106] The rate of change B2 is preferably greater than 0%, more preferably 1% or greater, even more preferably 1.8% or greater, even more preferably 2% or greater, particularly preferably 3% or greater, most preferably 4% or greater, and preferably 9% or less, more preferably 8% or less, even more preferably 7.5% or less, even more preferably 7% or less, and particularly preferably 6% or less. When the rate of change B2 exceeds the lower limit or is equal to or greater than the lower limit, the generation of scrap material during the production of the interlayer film can be effectively suppressed. When the rate of change B2 is equal to or less than the upper limit, the effects of the present invention can be even more effectively exhibited. The range of the rate of change B2 can be set by appropriately selecting the upper limit and the lower limit.
[0107] In an interlayer film satisfying the above-mentioned configuration B, it is preferable that the rate of change B2 satisfies the above-mentioned lower limit or upper limit in at least a portion of the region in the MD. In an interlayer film satisfying the above-mentioned configuration B, it is more preferable that when the secondary resonance frequencies of a laminated glass R having a length of 300 mm in the MD and a laminated glass S having a length of 300 mm in the MD are measured, the rate of change B2 satisfies the above-mentioned lower limit or upper limit. In an interlayer film satisfying the above-mentioned configuration B, it is even more preferable that when the secondary resonance frequencies of two laminated glasses R having a length of 300 mm in the MD and two laminated glasses S having a length of 300 mm in the MD, which are fabricated from a 600 mm section in the MD, are measured, the rate of change B2 calculated from the average value of the secondary resonance frequencies in each measured section satisfies the above-mentioned lower limit or upper limit. In an interlayer film satisfying the above-mentioned configuration B, it is particularly preferable that, when the secondary resonance frequencies of three sheets of laminated glass R and three sheets of laminated glass S each having a length of 300 mm in the MD, which are fabricated from a section of 900 mm in the MD, are measured, the rate of change B2 calculated from the average value of the secondary resonance frequencies in each measured section satisfies the above-mentioned lower limit or upper limit.In an interlayer film satisfying the above-mentioned configuration B, it is most preferable that, when the secondary resonance frequencies of three sheets of laminated glass R and three sheets of laminated glass S each having a length of 300 mm in the MD, which are fabricated from a section of 900 mm in the MD, are measured, the rate of change B2 calculated from the secondary resonance frequencies in each measured section satisfies the above-mentioned lower limit or upper limit, respectively.
[0108] The secondary resonance frequency (R B The secondary resonance frequency (R B When the secondary resonance frequency (R ) of the laminated glass R is equal to or greater than the lower limit and equal to or less than the upper limit, the sound insulation of the laminated glass R can be further improved. B The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0109] The secondary resonance frequency (S B The secondary resonance frequency (S) is preferably 600 Hz or more, more preferably 700 Hz or more, even more preferably 720 Hz or more, particularly preferably 760 Hz or more, and is preferably 1000 Hz or less, more preferably 900 Hz or less, and even more preferably 840 Hz or less. B When the secondary resonance frequency (S ) of the laminated glass S is equal to or greater than the lower limit and equal to or less than the upper limit, the sound insulation of the laminated glass S can be further improved. B The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0110] The secondary resonance frequency and secondary loss factor of the laminated glasses P, Q, R, and S can be measured as follows: The secondary resonance frequency and secondary loss factor of the laminated glasses P, Q, R, and S can be measured simultaneously.
[0111] The laminated glasses P, Q, R, and S are stored for four weeks in an environment with a temperature of 23±2°C and a humidity of 25±5%. After storage, the laminated glasses P, Q, R, and S are vibrated in a constant temperature chamber at 20°C using a vibration generator for damping tests (Spectris's "Pertable Vibration Exciter Type 4809" or equivalent). The obtained vibration characteristics are amplified using a mechanical impedance measuring device (Spectris's "75 VA Power Amplifier Type 2718" or equivalent), and the vibration spectrum is subjected to FFT analysis to determine the secondary resonance frequency and secondary loss factor. The analysis software used can be Spectris's "PULSE LabShop" (or equivalent).
[0112] Suitable methods for obtaining an interlayer film that satisfies the above-mentioned configuration A or the above-mentioned configuration B include, for example, (1) a method of cutting a predetermined position from the end in the TD direction of an interlayer film (interlayer film before cutting) produced by extrusion molding, and (2) a method of obtaining an interlayer film that satisfies the below-described configuration C.
[0113] Hereinafter, specific embodiments of the present invention will be described with reference to the drawings.
[0114] Fig. 1 is a cross-sectional view schematically showing an interlayer film for laminated glass according to a first embodiment of the present invention, in which a cross section of an interlayer film 11 in the thickness direction is shown.
[0115] The interlayer film 11 shown in FIG. 1 is a multilayer interlayer film having a structure of two or more layers. The interlayer film 11 is used to obtain laminated glass. The interlayer film 11 is an interlayer film for laminated glass. The interlayer film 11 includes a first layer 1, a second layer 2, and a third layer 3. The second layer 2 is disposed and laminated on a first surface 1a of the first layer 1. The third layer 3 is disposed and laminated on a second surface 1b of the first layer 1 opposite the first surface 1a. The first layer 1 is an interlayer. The second layer 2 and the third layer 3 are each protective layers, and in this embodiment, are surface layers. The first layer 1 is disposed and sandwiched between the second layer 2 and the third layer 3. Therefore, the interlayer film 11 has a multilayer structure (second layer 2 / first layer 1 / third layer 3) in which the second layer 2, first layer 1, and third layer 3 are laminated in this order.
[0116] The intermediate film 11 has a first end 11a and a second end 11b. The first end 11a and the second end 11b are end portions on both sides facing each other in the TD direction of the intermediate film 11. In FIG. 1 , the left-right direction is the TD direction, and the front-to-back direction is the MD direction.
[0117] The end face of the first end 11a includes an end face of the first layer 1, an end face of the second layer 2, and an end face of the third layer 3. The end face of the first end 11a is composed of an end face of the first layer 1, an end face of the second layer 2, and an end face of the third layer 3. The end face of the second end 11b includes an end face of the first layer 1, an end face of the second layer 2, and an end face of the third layer 3. The end face of the second end 11b is composed of an end face of the first layer 1, an end face of the second layer 2, and an end face of the third layer 3.
[0118] The intermediate film 11 has a rectangular cross-sectional shape in the thickness direction. The thickness of the intermediate film 11 is approximately uniform. The thickness of the intermediate film 11 at the first end 11a is the same as the thickness of the intermediate film 11 at the second end 11b. The first layer 1 has, from the first end 11a to the second end 11b, a region of increasing thickness, a region of approximately uniform thickness, and a region of decreasing thickness, in this order. The second layer 2 and the third layer 3 each have, from the first end 11a to the second end 11b, a region of decreasing thickness, a region of approximately uniform thickness, and a region of increasing thickness, in this order.
[0119] The aforementioned laminated glass P can be obtained by placing a portion P of the interlayer film 11 extending from the first end 11a to the second end 11b, from 0 mm to 25 mm, between two sheets of 2.0 mm thick green glass. The aforementioned laminated glass Q can be obtained by placing a portion Q of the interlayer film 11 extending from the first end 11a to the second end 11b, from 100 mm to 125 mm, between two sheets of 2.0 mm thick green glass. The aforementioned laminated glass R can be obtained by placing a portion R of the interlayer film 11 extending from the second end 11b to the first end 11a, from 0 mm to 25 mm, between two sheets of 2.0 mm thick green glass. The aforementioned laminated glass S can be obtained by placing a portion S of the interlayer film 11 extending from the second end 11b to the first end 11a, from 100 mm to 125 mm, between two sheets of 2.0 mm thick green glass.
[0120] The intermediate film 11 satisfies the above-described configuration A or the above-described configuration B.
[0121] It should be noted that other layers may be disposed between the second layer 2 and the first layer 1, and between the first layer 1 and the third layer 3. Examples of other layers include layers containing polyethylene terephthalate, etc. It is preferable that the second layer 2 and the first layer 1, and the first layer 1 and the third layer 3 are directly laminated to each other.
[0122] 2 is a cross-sectional view schematically illustrating an interlayer film for laminated glass according to a second embodiment of the present invention, showing a cross section in the thickness direction of an interlayer film 11A.
[0123] The interlayer film 11A shown in FIG. 2 is a multilayer interlayer film having a structure of two or more layers. The interlayer film 11A is used to obtain laminated glass. The interlayer film 11A is an interlayer film for laminated glass. The interlayer film 11A includes a first layer 1A, a second layer 2A, and a third layer 3A. The second layer 2A is disposed and laminated on a first surface 1Aa of the first layer 1A. The third layer 3A is disposed and laminated on a second surface 1Ab opposite the first surface 1Aa of the first layer 1A. The first layer 1A is an interlayer. The second layer 2A and the third layer 3A are each protective layers, and in this embodiment, are surface layers. The first layer 1A is disposed and sandwiched between the second layer 2A and the third layer 3A. Therefore, the intermediate film 11A has a multilayer structure in which the second layer 2A, the first layer 1A, and the third layer 3A are laminated in this order (second layer 2A / first layer 1A / third layer 3A).
[0124] The intermediate film 11A has a first end 11a and a second end 11b. The first end 11a and the second end 11b are end portions on both sides of the intermediate film 11A that face each other in the TD direction. In Figure 2, the left-right direction is the TD direction, and the front-to-back direction is the MD direction.
[0125] The end face of the first end portion 11a includes an end face of the first layer 1A, an end face of the second layer 2A, and an end face of the third layer 3A. The end face of the first end portion 11a is composed of an end face of the first layer 1A, an end face of the second layer 2A, and an end face of the third layer 3A. The end face of the second end portion 11b includes an end face of the first layer 1A, an end face of the second layer 2A, and an end face of the third layer 3A. The end face of the second end portion 11b is composed of an end face of the first layer 1A, an end face of the second layer 2A, and an end face of the third layer 3A.
[0126] The intermediate film 11A has a wedge-shaped cross section in the thickness direction. The thickness of the intermediate film 11A is not uniform. The thickness of the intermediate film 11A at the first end 11a is different from the thickness of the intermediate film 11A at the second end 11b. The thickness of the intermediate film 11A at the second end 11b is greater than the thickness of the intermediate film 11A at the first end 11a. The first layer 1A has, from the first end 11a to the second end 11b, a region of increasing thickness, a region of approximately uniform thickness, and a region of decreasing thickness, in this order. The second layer 2A and the third layer 3A each have, from the first end 11a to the second end 11b, a first region of increasing thickness, a second region of increasing thickness, and a third region of increasing thickness, in this order. The amount of increase in thickness of the second layer 2A in the first region is different from the amount of increase in thickness of the second layer 2A in the second region. The amount of increase in thickness of the second layer 2A in the second region is different from the amount of increase in thickness of the second layer 2A in the third region. The amount of increase in thickness of the third layer 3A in the first region is different from the amount of increase in thickness of the third layer 3A in the second region. The amount of increase in thickness of the third layer 3A in the second region is different from the amount of increase in thickness of the third layer 3A in the third region.
[0127] The aforementioned laminated glass P can be obtained by placing a portion P of the interlayer film 11A extending from 0 mm to 25 mm toward the first end 11a and the second end 11b between two sheets of 2.0 mm-thick green glass. The aforementioned laminated glass Q can be obtained by placing a portion Q of the interlayer film 11A extending from 100 mm to 125 mm toward the first end 11a and the second end 11b between two sheets of 2.0 mm-thick green glass. The aforementioned laminated glass R can be obtained by placing a portion R of the interlayer film 11A extending from 0 mm to 25 mm toward the second end 11b and the first end 11a between two sheets of 2.0 mm-thick green glass. The aforementioned laminated glass S can be obtained by placing a portion S of the interlayer film 11A extending from 100 mm to 125 mm toward the second end 11b and the first end 11a between two sheets of 2.0 mm-thick green glass.
[0128] The intermediate film 11A satisfies the above-described configuration A or the above-described configuration B.
[0129] The cross-sectional shape of the interlayer film in the thickness direction may be rectangular or wedge-shaped. The wedge shape may be a shape in which the thickness changes at a constant rate from one end of the interlayer film to the other end, or a shape in which the thickness changes at a non-constant rate from one end of the interlayer film to the other end. The thickness of the interlayer film at the first end and the thickness of the interlayer film at the second end may be the same or different. The thickness of the interlayer film at the first end may be greater or smaller than the thickness of the interlayer film at the second end.
[0130] The cross-sectional shape of the first layer in the thickness direction may be rectangular or wedge-shaped. The thickness of the first layer at the first end and the thickness of the first layer at the second end may be the same or different. The thickness of the first layer at the first end may be greater or smaller than the thickness of the first layer at the second end.
[0131] The cross-sectional shape of the second layer in the thickness direction may be rectangular or wedge-shaped. The thickness of the second layer at the first end and the thickness of the second layer at the second end may be the same or different. The thickness of the second layer at the first end may be greater or smaller than the thickness of the second layer at the second end.
[0132] The cross-sectional shape of the third layer in the thickness direction may be rectangular or wedge-shaped. The thickness of the third layer at the first end and the thickness of the third layer at the second end may be the same or different. The thickness of the third layer at the first end may be greater or smaller than the thickness of the third layer at the second end.
[0133] The first layer may be a surface layer of the interlayer film, or an intermediate layer of the interlayer film. When the interlayer film has a structure of three or more layers, the first layer is an intermediate layer of the interlayer film. The second layer may be a surface layer of the interlayer film, or an intermediate layer of the interlayer film. The second layer is preferably a surface layer of the interlayer film. The third layer may be a surface layer of the interlayer film, or an intermediate layer of the interlayer film. The third layer is preferably a surface layer of the interlayer film. The second layer and the third layer are preferably surface layers of the interlayer film, respectively.
[0134] The interlayer film preferably has layers having different glass transition temperatures. The glass transition temperature of the first layer is preferably different from the glass transition temperature of the second layer. The glass transition temperature of the first layer is preferably different from the glass transition temperature of the third layer. The glass transition temperature of the second layer and the glass transition temperature of the third layer may be the same or different.
[0135] From the viewpoint of further improving the sound insulation of the laminated glass, the glass transition temperature of the first layer is preferably lower than the glass transition temperature of the second layer. From the viewpoint of further improving the sound insulation of the laminated glass, the glass transition temperature of the first layer is preferably lower than the glass transition temperature of the third layer. From the viewpoint of further improving the sound insulation of the laminated glass, the first layer is preferably the layer with the lowest glass transition temperature. From the viewpoint of further improving the sound insulation of the laminated glass, it is preferable that the second layer is the layer with the highest glass transition temperature, and it is more preferable that the second layer and the third layer are each the layer with the highest glass transition temperature.
[0136] The glass transition temperature of the layer having the highest glass transition temperature is preferably 32°C or higher, more preferably 35°C or higher, even more preferably 37°C or higher, particularly preferably 38°C or higher, and preferably 50°C or lower, more preferably 45°C or lower, and even more preferably 40°C or lower. When the glass transition temperature is equal to or higher than the lower limit, configuration B is more likely to be satisfied. When the glass transition temperature is equal to or higher than the lower limit, the vibration damping properties of the laminated glass can be further improved. When the glass transition temperature is equal to or higher than the lower limit and equal to or lower than the upper limit, the handleability of the interlayer film can be improved and the sound insulation of the laminated glass can be further improved. The range of the glass transition temperature of the layer having the highest glass transition temperature can be set by appropriately selecting the upper limit and the lower limit.
[0137] The glass transition temperature of the first layer is preferably −20° C. or higher, more preferably −10° C. or higher, even more preferably 0° C. or higher, and preferably 20° C. or lower, more preferably 10° C. or lower, and even more preferably 5° C. or lower. When the glass transition temperature is equal to or higher than the lower limit, the structure B is more likely to be satisfied. When the glass transition temperature is equal to or higher than the lower limit, the vibration damping properties of the laminated glass can be further improved. When the glass transition temperature is equal to or higher than the lower limit and equal to or lower than the upper limit, the handleability of the interlayer film can be improved and the sound insulation of the laminated glass can be further improved. The range of the glass transition temperature of the first layer can be set by appropriately selecting the upper limit and the lower limit.
[0138] The glass transition temperature of the second layer is preferably 32°C or higher, more preferably 35°C or higher, even more preferably 37°C or higher, particularly preferably 38°C or higher, and preferably 50°C or lower, more preferably 45°C or lower, and even more preferably 40°C or lower. When the glass transition temperature is equal to or higher than the lower limit, the structure B is more likely to be satisfied. When the glass transition temperature is equal to or higher than the lower limit, the vibration damping properties of the laminated glass can be further improved. When the glass transition temperature is equal to or higher than the lower limit and equal to or lower than the upper limit, the handleability of the interlayer film can be improved and the sound insulation of the laminated glass can be further improved. The range of the glass transition temperature of the second layer can be set by appropriately selecting the upper limit and the lower limit.
[0139] The glass transition temperature of the third layer is preferably 32°C or higher, more preferably 35°C or higher, even more preferably 37°C or higher, particularly preferably 38°C or higher, and preferably 50°C or lower, more preferably 45°C or lower, and even more preferably 40°C or lower. When the glass transition temperature is equal to or higher than the lower limit, configuration B is more likely to be satisfied. When the glass transition temperature is equal to or higher than the lower limit, the vibration damping properties of the laminated glass can be further improved. When the glass transition temperature is equal to or higher than the lower limit and equal to or lower than the upper limit, the handleability of the interlayer film can be improved and the sound insulation of the laminated glass can be further improved. The range of the glass transition temperature of the third layer can be set by appropriately selecting the upper limit and the lower limit.
[0140] The tan δ at the glass transition temperature of the layer having the lowest glass transition temperature is preferably 1.2 or more, more preferably 1.3 or more, even more preferably 1.4 or more, and particularly preferably 2.0 or more. When the tan δ is equal to or greater than the lower limit, the vibration damping properties of the laminated glass can be further improved. Note that the tan δ at the glass transition temperature of the layer having the lowest glass transition temperature may be 4.0 or less, or may be 3.0 or less. The range of tan δ at the glass transition temperature of the layer having the lowest glass transition temperature can be set by appropriately selecting the upper limit and the lower limit.
[0141] The tan δ at the glass transition temperature of the first layer is preferably 1.2 or more, more preferably 1.3 or more, even more preferably 1.4 or more, and particularly preferably 2.0 or more. When the tan δ is equal to or greater than the lower limit, the vibration damping properties of the laminated glass can be further improved. The tan δ at the glass transition temperature of the first layer may be 4.0 or less, or may be 3.0 or less. The range of tan δ at the glass transition temperature of the first layer can be set by appropriately selecting the upper limit and the lower limit.
[0142] The tan δ at the glass transition temperature of the second layer is preferably 0.40 or more, more preferably 0.45 or more, and even more preferably 0.50 or more. When the tan δ is equal to or greater than the lower limit, the vibration damping of the laminated glass can be further improved. The tan δ at the glass transition temperature of the second layer may be 4.0 or less, or may be 3.0 or less. The range of tan δ at the glass transition temperature of the second layer can be set by appropriately selecting the upper limit and the lower limit.
[0143] The tan δ at the glass transition temperature of the third layer is preferably 0.40 or more, more preferably 0.45 or more, and even more preferably 0.50 or more. When the tan δ is equal to or greater than the lower limit, the vibration damping of the laminated glass can be further improved. The tan δ at the glass transition temperature of the third layer may be 4.0 or less, or may be 3.0 or less. The range of tan δ at the glass transition temperature of the third layer can be set by appropriately selecting the upper limit and the lower limit.
[0144] The glass transition temperature and tan δ are determined by viscoelasticity measurement, which is specifically carried out as follows.
[0145] The interlayer film is sandwiched between two 100 μm-thick polyethylene terephthalate films (PET films, e.g., "Lumirror H10" manufactured by Toray Industries, Inc.) to obtain a laminate. The resulting laminate is sandwiched between two 2.0 mm-thick green glass sheets, placed in a rubber bag, and degassed at a vacuum of 0.08 MPa for 20 minutes. After degassing, the degassed container is transferred to an oven and vacuum-pressed at 90°C for 30 minutes to pre-bond the laminate. After pre-bonding, the laminate is compressed in an autoclave at 140°C and a pressure of 1.3 MPa for 20 minutes to obtain a test specimen. The test specimen is stored for 4 weeks in an environment at a temperature of 23±2°C and a humidity of 25±5%. After storage, the green glass and PET film are peeled off, and the viscoelasticity is measured using a viscoelasticity measuring device (TA Instruments' "ARES-G2" viscoelasticity measuring device, or equivalent). Using parallel plates with a diameter of 8 mm as a jig, measurements are made under the following conditions: shear mode, temperature reduction from 100°C to -20°C at a cooling rate of 3°C / min, frequency of 1 Hz, and strain of 1%. In the obtained measurement results, the peak temperature of the loss tangent is taken as the glass transition temperature Tg (°C), and the value of the loss tangent at the glass transition temperature is taken as tan δ at the glass transition temperature. When the interlayer film has multiple layers, the test specimen is prepared in an integrated state without separation, and measurements are performed. The peak tan δ and glass transition temperature, etc., derived from each layer are read from the measurement results. In the case of laminated glass, the laminated glass is cooled with liquid nitrogen or the like, and then the laminated glass member and the interlayer film are peeled off. The peeled interlayer film is used to prepare the test specimen by the above-mentioned method. The viscoelasticity measurement is performed using this test specimen.
[0146] The end face of the first end portion preferably has an end face of the layer with the lowest glass transition temperature, more preferably has an end face of the layer with the lowest glass transition temperature and an end face of the layer with the highest glass transition temperature. The end face of the second end portion preferably has an end face of the layer with the lowest glass transition temperature, more preferably has an end face of the layer with the lowest glass transition temperature and an end face of the layer with the highest glass transition temperature. In this case, the above-mentioned configurations A and B can be easily satisfied.
[0147] The end face of the first end portion preferably includes an end face of the first layer, more preferably includes an end face of the first layer and an end face of the second layer, and even more preferably includes an end face of the first layer, an end face of the second layer, and an end face of the third layer. The end face of the second end portion preferably includes an end face of the first layer, more preferably includes an end face of the first layer and an end face of the second layer, and even more preferably includes an end face of the first layer, an end face of the second layer, and an end face of the third layer. In this case, it becomes easier to preferably satisfy the above-mentioned configurations A and B.
[0148] From the viewpoint of suitably satisfying the above-mentioned configuration A and the above-mentioned configuration B, the interlayer film preferably has the following configuration C.
[0149] Configuration C: The rate of change C1 represented by the following formula (C1) is greater than 0% and not greater than 50%, and the rate of change C2 represented by the following formula (C2) is greater than 0% and not greater than 50%.
[0150] Rate of change C1 (%) = (|T P -T Q | / T Q )×100...(C1)
[0151] T P : The ratio of the thickness of the layer with the lowest glass transition temperature at a position 12.5 mm from the first end toward the second end to the thickness of the interlayer film at a position 12.5 mm from the first end toward the second end, T Q : The ratio of the thickness of the layer with the lowest glass transition temperature at a position 112.5 mm from the first end toward the second end to the thickness of the interlayer film at a position 112.5 mm from the first end toward the second end
[0152] Rate of change C2 (%) = (|T R -T S | / T S )×100...(C2)
[0153] T R: The ratio of the thickness of the layer with the lowest glass transition temperature at a position 12.5 mm from the second end toward the first end to the thickness of the interlayer film at a position 12.5 mm from the second end toward the first end, T S : The ratio of the thickness of the layer with the lowest glass transition temperature at a position 112.5 mm from the second end toward the first end to the thickness of the interlayer film at a position 112.5 mm from the second end toward the first end
[0154] The rate of change C1 is preferably greater than 0%, more preferably 1% or more, even more preferably 5% or more, even more preferably 10% or more, particularly preferably 14.3% or more, and preferably 50% or less, more preferably 40% or less, even more preferably 36% or less, even more preferably 30% or less, and particularly preferably 20% or less. In this case, it becomes easier to suitably satisfy the above-mentioned configurations A and B. The range of the rate of change C1 can be set by appropriately selecting the above-mentioned upper limit value and the above-mentioned lower limit value.
[0155] The ratio of the thickness of the layer with the lowest glass transition temperature at a position 12.5 mm from the first end toward the second end to the thickness of the interlayer film at a position 12.5 mm from the first end toward the second end is defined as a ratio (T P ) is the ratio (T P ) is "(thickness of the layer with the lowest glass transition temperature at a position 12.5 mm from the first end toward the second end) / (thickness of the interlayer film at a position 12.5 mm from the first end toward the second end)". P ) is preferably 0.05 or more, more preferably 0.07 or more, even more preferably 0.09 or more, particularly preferably 0.13 or more, and preferably 0.27 or less, more preferably 0.20 or less, even more preferably 0.16 or less. P When the ratio (T PWhen the ratio (T ) is equal to or less than the upper limit, the mechanical strength of the interlayer film can be further increased. In addition, when producing laminated glass, unintended slippage of the glass under high temperature conditions such as in an autoclave can be suppressed. P The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0156] The ratio of the thickness of the layer with the lowest glass transition temperature at a position 112.5 mm from the first end toward the second end to the thickness of the interlayer film at a position 112.5 mm from the first end toward the second end is defined as a ratio (T Q ) is the ratio (T Q ) is "(thickness of the layer with the lowest glass transition temperature at a position 112.5 mm from the first end toward the second end) / (thickness of the interlayer film at a position 112.5 mm from the first end toward the second end)". Q ) is preferably 0.05 or more, more preferably 0.07 or more, even more preferably 0.09 or more, particularly preferably 0.13 or more, and preferably 0.27 or less, more preferably 0.20 or less, even more preferably 0.16 or less. Q When the ratio (T Q When the ratio (T ) is equal to or less than the upper limit, the mechanical strength of the interlayer film can be further increased. In addition, when producing laminated glass, unintended slippage of the glass under high temperature conditions such as in an autoclave can be suppressed. Q The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0157] The rate of change C2 is preferably greater than 0%, more preferably 1% or more, even more preferably 5% or more, even more preferably 10% or more, particularly preferably 14.3% or more, and preferably 50% or less, more preferably 40% or less, even more preferably 36% or less, even more preferably 30% or less, and particularly preferably 20% or less. In this case, it becomes easier to suitably satisfy the above-mentioned configurations A and B. The range of the rate of change C2 can be set by appropriately selecting the above-mentioned upper limit value and the above-mentioned lower limit value.
[0158] The ratio of the thickness of the layer with the lowest glass transition temperature at a position 12.5 mm from the second end toward the first end to the thickness of the interlayer film at a position 12.5 mm from the second end toward the first end is defined as a ratio (T R ) is the ratio (T R ) is "(thickness of the layer with the lowest glass transition temperature at a position 12.5 mm from the second end toward the first end) / (thickness of the interlayer film at a position 12.5 mm from the second end toward the first end)". R ) is preferably 0.05 or more, more preferably 0.07 or more, even more preferably 0.09 or more, particularly preferably 0.13 or more, and preferably 0.27 or less, more preferably 0.20 or less, even more preferably 0.16 or less. R When the ratio (T R When the ratio (T ) is equal to or less than the upper limit, the mechanical strength of the interlayer film can be further increased. In addition, when producing laminated glass, unintended slippage of the glass under high temperature conditions such as in an autoclave can be suppressed. R The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0159] The ratio of the thickness of the layer with the lowest glass transition temperature at a position 112.5 mm from the second end toward the first end to the thickness of the interlayer film at a position 112.5 mm from the second end toward the first end is defined as a ratio (T S ) is the ratio (T S ) is "(thickness of the layer with the lowest glass transition temperature at a position 112.5 mm from the second end toward the first end) / (thickness of the interlayer film at a position 112.5 mm from the second end toward the first end)". S ) is preferably 0.05 or more, more preferably 0.07 or more, even more preferably 0.09 or more, particularly preferably 0.13 or more, and preferably 0.27 or less, more preferably 0.20 or less, even more preferably 0.16 or less. SWhen the ratio (T S When the ratio (T ) is equal to or less than the upper limit, the mechanical strength of the interlayer film can be further increased. In addition, when producing laminated glass, unintended slippage of the glass under high temperature conditions such as in an autoclave can be suppressed. S The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0160] The maximum thickness of the interlayer film is preferably 0.15 mm or more, more preferably 0.25 mm or more, even more preferably 0.5 mm or more, particularly preferably 0.8 mm or more, and is preferably 4 mm or less, more preferably 3.8 mm or less, and even more preferably 3.6 mm or less. The range of the maximum thickness of the interlayer film can be set by appropriately selecting the upper limit and the lower limit.
[0161] From the viewpoint of practical use and of sufficiently increasing adhesive strength and penetration resistance, the maximum thickness of the surface layer in the interlayer film is preferably 20 μm or more, more preferably 25 μm or more, even more preferably 50 μm or more, and preferably 2000 μm or less, more preferably 1800 μm or less. The range of the maximum thickness of the surface layer in the interlayer film can be set by appropriately selecting the above upper limit and lower limit.
[0162] From the viewpoint of practical use and of sufficiently increasing penetration resistance, the maximum thickness of the layer (intermediate layer) disposed between the two surface layers of the interlayer film is preferably 40 μm or more, more preferably 60 μm or more, even more preferably 80 μm or more, and preferably 200 μm or less, more preferably 150 μm or less. The range of the maximum thickness of the layer (intermediate layer) disposed between the two surface layers of the interlayer film can be set by appropriately selecting the above upper limit and lower limit.
[0163] When the thickness of the intermediate film at the first end and the thickness of the intermediate film at the second end are different, the thickness of the intermediate film at the second end is preferably larger than the thickness of the intermediate film at the first end, more preferably larger by 0.01 mm or more, even more preferably larger by 0.05 mm or more, particularly preferably larger by 0.1 mm or more, preferably larger by 5 mm or less, more preferably larger by 4.8 mm or less, and even more preferably larger by 4.6 mm or less. The difference between the thickness of the intermediate film at the second end and the thickness of the intermediate film at the first end can be set by appropriately selecting the upper limit and the lower limit.
[0164] When used in laminated glass for a head-up display (HUD), from the viewpoint of improving the display, the interlayer film preferably has a portion whose cross section in the thickness direction is wedge-shaped.
[0165] To prevent double images, the wedge angle θ of the interlayer film can be appropriately set according to the installation angle of the laminated glass. The wedge angle θ is the wedge angle of the entire interlayer film.
[0166] The wedge angle θ of the interlayer film is the interior angle at the intersection of a straight line connecting the surface portion (first surface portion) on one side of the interlayer film between the maximum and minimum thickness portions of the interlayer film and a straight line connecting the surface portion (second surface portion) on the other side of the interlayer film between the maximum and minimum thickness portions of the interlayer film.
[0167] In addition, if there are multiple maximum thickness portions, multiple minimum thickness portions, the maximum thickness portion is in a fixed region, or the minimum thickness portion is in a fixed region, the maximum thickness portion and the minimum thickness portion for determining the wedge angle θ are selected so that the wedge angle θ to be determined is largest.
[0168] From the viewpoint of more effectively suppressing ghosting, the wedge angle θ of the interlayer film is preferably 0.05 mrad or more, more preferably 0.1 mrad (0.00575 degrees) or more, and even more preferably 0.2 mrad (0.0115 degrees) or more. Furthermore, when the wedge angle θ is equal to or greater than the above-mentioned lower limit, a laminated glass suitable for vehicles with a large windshield installation angle, such as trucks and buses, can be obtained. The range of the wedge angle θ of the interlayer film can be set by appropriately selecting the upper limit value and the lower limit value described below.
[0169] From the viewpoint of more effectively suppressing ghosting, the wedge angle θ of the interlayer film is preferably 2 mrad (0.1146 degrees) or less, more preferably 0.7 mrad (0.0401 degrees) or less. Furthermore, when the wedge angle θ is equal to or less than the above upper limit, a laminated glass suitable for vehicles with a small windshield installation angle, such as sports cars, can be obtained. The range of the wedge angle θ of the interlayer film can be set by appropriately selecting the above upper limit and lower limit.
[0170] The wedge angle (θ) of the interlayer and the thickness of the interlayer may be measured by a contact thickness measuring instrument "TOF-4R" (manufactured by Yamabun Denki Co., Ltd.).
[0171] The thickness of the interlayer film is measured using the above-mentioned measuring device at a film transport speed of 2.15 mm / min to 2.25 mm / min over the shortest distance from the first end to the second end.
[0172] The thickness of each layer of the intermediate film can be measured using an instrument such as "SE-3000" (manufactured by SELMIC).
[0173] The thickness of each layer of the interlayer film can be measured as follows: The interlayer film is cut in the thickness direction at the measurement position using a razor, cutter, etc. The cut surface of the interlayer film is observed using the measuring device described above, and then the thickness of each layer is measured using calculation software included in the accompanying software.
[0174] An example of a measuring device that can be used to measure the wedge angle (θ) of the interlayer film after it has been formed into laminated glass, the thickness of the interlayer film, and the thickness of each layer of the interlayer film is the non-contact multilayer film thickness measuring device "OPTIGAUGE" (manufactured by Lumetrics, Inc.). When using such a measuring device, the thickness of the interlayer film can be measured in the laminated glass state.
[0175] The interlayer film is preferably used in laminated glass for a head-up display (HUD). The interlayer film is preferably an interlayer film for a HUD. The interlayer film preferably has a display corresponding area corresponding to the display area of the HUD.
[0176] Hereinafter, details of the first layer, the second layer, and the third layer that constitute the interlayer film according to the present invention, as well as details of each component contained in the first layer, the second layer, and the third layer, will be described.
[0177] (Resin) The interlayer film preferably contains a resin (hereinafter may be referred to as resin (0)). The interlayer film preferably contains a thermoplastic resin (hereinafter may be referred to as thermoplastic resin (0)) as the resin (0). The interlayer film preferably contains a polyvinyl acetal resin (hereinafter may be referred to as polyvinyl acetal resin (0)) as the thermoplastic resin (0). The first layer preferably contains a resin (hereinafter may be referred to as resin (1)). The first layer preferably contains a thermoplastic resin (hereinafter may be referred to as thermoplastic resin (1)) as the resin (1). The resin in the first layer is preferably a thermoplastic resin. The first layer preferably contains a polyvinyl acetal resin (hereinafter may be referred to as polyvinyl acetal resin (1)) as the thermoplastic resin (1). The second layer preferably contains a resin (hereinafter may be referred to as resin (2)). The second layer preferably contains a thermoplastic resin (hereinafter may be referred to as thermoplastic resin (2)) as the resin (2). The resin in the second layer is preferably a thermoplastic resin. The second layer preferably contains a polyvinyl acetal resin (hereinafter may be referred to as polyvinyl acetal resin (2)) as the thermoplastic resin (2). The third layer preferably contains a resin (hereinafter may be referred to as resin (3)). The third layer preferably contains a thermoplastic resin (hereinafter may be referred to as thermoplastic resin (3)) as the resin (3). The resin in the third layer is preferably a thermoplastic resin. The third layer preferably contains a polyvinyl acetal resin (hereinafter may be referred to as polyvinyl acetal resin (3)) as the thermoplastic resin (3). The resin (1), the resin (2), and the resin (3) may be the same or different. The thermoplastic resin (1), the thermoplastic resin (2), and the thermoplastic resin (3) may be the same or different from each other. In order to further improve sound insulation, it is preferable that the resin (1) is different from the resins (2) and (3).Since sound insulation is further improved, it is preferable that the thermoplastic resin (1) is different from the thermoplastic resin (2) and the thermoplastic resin (3). The polyvinyl acetal resin (1), the polyvinyl acetal resin (2), and the polyvinyl acetal resin (3) may be the same or different. Since sound insulation is further improved, it is preferable that the polyvinyl acetal resin (1) is different from the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3). Each of the resins (0), (1), (2), and (3) may be used alone or in combination of two or more. Each of the thermoplastic resins (0), (1), (2), and (3) may be used alone or in combination of two or more. The polyvinyl acetal resin (0), the polyvinyl acetal resin (1), the polyvinyl acetal resin (2), and the polyvinyl acetal resin (3) may each be used alone or in combination of two or more.
[0178] Examples of the resin include a cured product of a thermosetting resin and a thermoplastic resin.
[0179] Examples of the thermoplastic resin include polyvinyl acetal resin, ethylene-vinyl acetate copolymer resin, ethylene-acrylic acid copolymer resin, polyurethane resin, (meth)acrylic resin, polyolefin resin, ionomer resin, polyvinyl alcohol resin, etc. Thermoplastic resins other than these may also be used.
[0180] The polyvinyl acetal resin can be produced, for example, by acetalizing polyvinyl alcohol (PVA) with an aldehyde. The polyvinyl acetal resin is preferably an acetalized product of polyvinyl alcohol. The polyvinyl alcohol can be obtained, for example, by saponifying polyvinyl acetate. The degree of saponification of the polyvinyl alcohol is generally within the range of 70 mol% to 99.9 mol%.
[0181] The average degree of polymerization of the polyvinyl alcohol (PVA) is preferably 200 or more, more preferably 500 or more, even more preferably 1500 or more, even more preferably 1600 or more, particularly preferably 2600 or more, and most preferably 2700 or more, and is preferably 5000 or less, more preferably 4000 or less, and even more preferably 3500 or less. When the average degree of polymerization is at least the lower limit, the penetration resistance of the laminated glass is further improved. When the average degree of polymerization is at most the upper limit, the interlayer film is easily formed. The range of the average degree of polymerization can be set by appropriately selecting the upper limit and the lower limit.
[0182] The average degree of polymerization of the polyvinyl alcohol is determined by a method in accordance with JIS K6726 "Testing methods for polyvinyl alcohol."
[0183] The number of carbon atoms in the acetal group contained in the polyvinyl acetal resin is not particularly limited. The aldehyde used in producing the polyvinyl acetal resin is not particularly limited. The number of carbon atoms in the acetal group in the polyvinyl acetal resin is preferably 3 to 5, and more preferably 3 or 4. When the number of carbon atoms in the acetal group in the polyvinyl acetal resin is 3 or more, the glass transition temperature of the interlayer film is sufficiently low. The number of carbon atoms in the acetal group in the polyvinyl acetal resin may be 4 or 5.
[0184] The aldehyde is not particularly limited. In general, an aldehyde having 1 to 10 carbon atoms is suitably used. Examples of the aldehyde having 1 to 10 carbon atoms include propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-valeraldehyde, 2-ethylbutyraldehyde, n-hexylaldehyde, n-octylaldehyde, n-nonylaldehyde, n-decylaldehyde, formaldehyde, acetaldehyde, and benzaldehyde. The aldehyde is preferably propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-hexylaldehyde, or n-valeraldehyde, more preferably propionaldehyde, n-butyraldehyde, or isobutyraldehyde, and even more preferably n-butyraldehyde. The above aldehydes may be used alone or in combination of two or more.
[0185] The hydroxyl group content (hydroxyl group amount) of the polyvinyl acetal resin (0) is preferably 15 mol% or more, more preferably 18 mol% or more, and preferably 40 mol% or less, more preferably 35 mol% or less. When the hydroxyl group content is equal to or greater than the lower limit, the adhesive strength of the interlayer film is further increased. When the hydroxyl group content is equal to or less than the upper limit, the flexibility of the interlayer film is increased, making it easier to handle. The range of the hydroxyl group content can be set by appropriately selecting the upper limit and the lower limit.
[0186] The hydroxyl group content (hydroxyl group amount) of the polyvinyl acetal resin (1) is preferably 17 mol% or more, more preferably 20 mol% or more, even more preferably 22 mol% or more, and preferably 28 mol% or less, more preferably 27 mol% or less, even more preferably 25 mol% or less, and particularly preferably 24 mol% or less. When the hydroxyl group content is equal to or greater than the lower limit, the mechanical strength of the interlayer film is further increased. In particular, when the hydroxyl group content of the polyvinyl acetal resin (1) is 20 mol% or more, the reaction efficiency is high and productivity is excellent, and when it is 28 mol% or less, the sound insulation of the laminated glass is further improved. Furthermore, when the hydroxyl group content is equal to or less than the upper limit, the flexibility of the interlayer film is increased, making it easier to handle. The range of the hydroxyl group content can be set by appropriately selecting the upper and lower limits.
[0187] The hydroxyl group content (hydroxyl group amount) of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) is preferably 25 mol% or more, more preferably 28 mol% or more, more preferably 30 mol% or more, even more preferably 31.5 mol% or more, even more preferably 32 mol% or more, and particularly preferably 33 mol% or more. The hydroxyl group content (hydroxyl group amount) of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) is preferably 38 mol% or less, more preferably 37 mol% or less, even more preferably 36.5 mol% or less, and particularly preferably 36 mol% or less. When the hydroxyl group content is above the lower limit, the adhesive strength of the interlayer film is further increased. When the hydroxyl group content is below the upper limit, the flexibility of the interlayer film is increased, making it easier to handle. The range of the hydroxyl group content can be set by appropriately selecting the upper and lower limits.
[0188] From the viewpoint of further improving sound insulation, the hydroxyl group content of the polyvinyl acetal resin (1) is preferably lower than the hydroxyl group content of the polyvinyl acetal resin (2). From the viewpoint of further improving sound insulation, the hydroxyl group content of the polyvinyl acetal resin (1) is preferably lower than the hydroxyl group content of the polyvinyl acetal resin (3). The absolute value of the difference between the hydroxyl group content of the polyvinyl acetal resin (1) and the hydroxyl group content of the polyvinyl acetal resin (2) is defined as absolute value A, and the absolute value of the difference between the hydroxyl group content of the polyvinyl acetal resin (1) and the hydroxyl group content of the polyvinyl acetal resin (3) is defined as absolute value B. From the viewpoint of further improving sound insulation, the absolute values A and B are each preferably 1 mol% or more, more preferably 5 mol% or more, even more preferably 9 mol% or more, particularly preferably 10 mol% or more, and most preferably 12 mol% or more. Each of the absolute value A and the absolute value B is preferably 20 mol % or less. The range of the absolute value A and the range of the absolute value B can be set by appropriately selecting the upper limit value and the lower limit value.
[0189] The hydroxyl group content of the polyvinyl acetal resin is a molar fraction calculated by dividing the amount of ethylene groups having hydroxyl groups by the total amount of ethylene groups in the main chain, and is expressed as a percentage. The amount of ethylene groups having hydroxyl groups can be measured, for example, in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral."
[0190] The degree of acetylation (amount of acetyl groups) of the polyvinyl acetal resin (0) is preferably 0.1 mol% or more, more preferably 0.3 mol% or more, even more preferably 0.5 mol% or more, and preferably 30 mol% or less, more preferably 25 mol% or less, and even more preferably 20 mol% or less. When the degree of acetylation is at least the lower limit, the compatibility between the polyvinyl acetal resin and the plasticizer is enhanced. When the degree of acetylation is at most the upper limit, the moisture resistance of the interlayer film and laminated glass is enhanced. The range of the degree of acetylation can be set by appropriately selecting the upper limit and the lower limit.
[0191] The degree of acetylation (amount of acetyl groups) of the polyvinyl acetal resin (1) is preferably 0.01 mol% or more, more preferably 0.1 mol% or more, even more preferably 7 mol% or more, even more preferably 9 mol% or more, preferably 30 mol% or less, more preferably 25 mol% or less, even more preferably 24 mol% or less, and particularly preferably 20 mol% or less. When the degree of acetylation is at least the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is improved. When the degree of acetylation is at most the upper limit, the moisture resistance of the interlayer film and laminated glass is improved. In particular, when the degree of acetylation of the polyvinyl acetal resin (1) is 0.1 mol% or more and 25 mol% or less, the penetration resistance is excellent. The range of the degree of acetylation can be set by appropriately selecting the upper and lower limits.
[0192] The acetylation degree (acetyl group amount) of each of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) is preferably 0.01 mol% or more, more preferably 0.5 mol% or more, and preferably 10 mol% or less, more preferably 2 mol% or less. When the acetylation degree is equal to or greater than the lower limit, the compatibility between the polyvinyl acetal resin and the plasticizer is enhanced. When the acetylation degree is equal to or less than the upper limit, the moisture resistance of the interlayer film and laminated glass is enhanced. The range of the acetylation degree can be set by appropriately selecting the upper limit and the lower limit.
[0193] The degree of acetylation is a molar fraction calculated by dividing the amount of ethylene groups having acetyl groups by the total amount of ethylene groups in the main chain, and is expressed as a percentage. The amount of ethylene groups having acetyl groups can be measured, for example, in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral."
[0194] The degree of acetalization of the polyvinyl acetal resin (0) (the degree of butyralization in the case of a polyvinyl butyral resin) is preferably 60 mol% or more, more preferably 63 mol% or more, and preferably 85 mol% or less, more preferably 75 mol% or less, and even more preferably 70 mol% or less. When the degree of acetalization is equal to or greater than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetalization is equal to or less than the upper limit, the reaction time required to produce the polyvinyl acetal resin is shortened. The range of the degree of acetalization can be set by appropriately selecting the upper limit and the lower limit.
[0195] The degree of acetalization of the polyvinyl acetal resin (1) (the degree of butyralization in the case of a polyvinyl butyral resin) is preferably 47 mol% or more, more preferably 60 mol% or more, and preferably 85 mol% or less, more preferably 80 mol% or less, and even more preferably 75 mol% or less. When the degree of acetalization is equal to or greater than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetalization is equal to or less than the upper limit, the reaction time required to produce the polyvinyl acetal resin is shortened. The range of the degree of acetalization can be set by appropriately selecting the upper and lower limits.
[0196] The degree of acetalization of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) (the degree of butyralization in the case of a polyvinyl butyral resin) is preferably 55 mol% or more, more preferably 60 mol% or more, and preferably 75 mol% or less, more preferably 71 mol% or less. When the degree of acetalization is equal to or greater than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetalization is equal to or less than the upper limit, the reaction time required to produce the polyvinyl acetal resin is shortened. The range of the degree of acetalization can be set by appropriately selecting the upper limit and the lower limit.
[0197] The degree of acetalization is determined as follows. First, the amount of ethylene groups to which hydroxyl groups are bonded and the amount of ethylene groups to which acetyl groups are bonded are subtracted from the total amount of ethylene groups in the main chain to determine the value. The obtained value is divided by the total amount of ethylene groups in the main chain to determine the molar fraction. The value expressed as a percentage of this molar fraction is the degree of acetalization.
[0198] The hydroxyl group content (hydroxyl group amount), acetalization degree (butyralization degree), and acetylation degree are preferably calculated from the results of measurements made in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral." However, measurements made in accordance with ASTM D1396-92 may also be used. When the polyvinyl acetal resin is a polyvinyl butyral resin, the hydroxyl group content (hydroxyl group amount), acetalization degree (butyralization degree), and acetylation degree can be calculated from the results of measurements made in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral."
[0199] The content of polyvinyl acetal resin in 100% by weight of resin contained in the interlayer film is preferably 10% by weight or more, more preferably 30% by weight or more, even more preferably 50% by weight or more, even more preferably 70% by weight or more, particularly preferably 80% by weight or more, and most preferably 90% by weight or more. The content of polyvinyl acetal resin in 100% by weight of resin contained in the interlayer film is preferably 100% by weight or less. The main component (50% by weight or more) of the resin in the interlayer film is preferably polyvinyl acetal resin. The range of the content of the polyvinyl acetal resin can be set by appropriately selecting the upper and lower limits.
[0200] The content of the polyvinyl acetal resin in 100% by weight of the resin contained in the first layer is preferably 10% by weight or more, more preferably 30% by weight or more, even more preferably 50% by weight or more, even more preferably 70% by weight or more, particularly preferably 80% by weight or more, and most preferably 90% by weight or more. The content of the polyvinyl acetal resin in 100% by weight of the resin contained in the first layer is preferably 100% by weight or less. The main component (50% by weight or more) of the resin in the first layer is preferably polyvinyl acetal resin. The range of the content of the polyvinyl acetal resin can be set by appropriately selecting the upper and lower limits.
[0201] The content of the polyvinyl acetal resin in 100% by weight of the resin contained in the second layer is preferably 10% by weight or more, more preferably 30% by weight or more, even more preferably 50% by weight or more, even more preferably 70% by weight or more, particularly preferably 80% by weight or more, and most preferably 90% by weight or more. The content of the polyvinyl acetal resin in 100% by weight of the resin contained in the second layer is preferably 100% by weight or less. The main component (50% by weight or more) of the resin in the second layer is preferably a polyvinyl acetal resin. The range of the content of the polyvinyl acetal resin can be set by appropriately selecting the upper and lower limits.
[0202] The content of the polyvinyl acetal resin in 100% by weight of the resin contained in the third layer is preferably 10% by weight or more, more preferably 30% by weight or more, even more preferably 50% by weight or more, even more preferably 70% by weight or more, particularly preferably 80% by weight or more, and most preferably 90% by weight or more. The content of the polyvinyl acetal resin in 100% by weight of the resin contained in the third layer is preferably 100% by weight or less. The main component (50% by weight or more) of the resin in the third layer is preferably a polyvinyl acetal resin. The range of the content of the polyvinyl acetal resin can be set by appropriately selecting the upper and lower limits.
[0203] (Plasticizer) From the viewpoint of further increasing the adhesive strength of the interlayer film, the interlayer film preferably contains a plasticizer (hereinafter, sometimes referred to as plasticizer (0)). The first layer preferably contains a plasticizer (hereinafter, sometimes referred to as plasticizer (1)). The second layer preferably contains a plasticizer (hereinafter, sometimes referred to as plasticizer (2)). The third layer preferably contains a plasticizer (hereinafter, sometimes referred to as plasticizer (3)). When the thermoplastic resin contained in the interlayer film is a polyvinyl acetal resin, it is particularly preferable that the interlayer film (each layer) contains a plasticizer. The layer containing a polyvinyl acetal resin preferably contains a plasticizer.
[0204] The plasticizer is not particularly limited. Any conventionally known plasticizer can be used as the plasticizer. Only one type of plasticizer may be used, or two or more types may be used in combination.
[0205] Examples of the plasticizer include organic ester plasticizers such as monobasic organic acid esters and polybasic organic acid esters, organic phosphate plasticizers, and organic phosphite plasticizers. The plasticizer is preferably an organic ester plasticizer. The plasticizer is preferably a liquid plasticizer.
[0206] Examples of the monobasic organic acid ester include glycol esters obtained by reacting glycol with a monobasic organic acid. Examples of the glycol include triethylene glycol, tetraethylene glycol, and tripropylene glycol. Examples of the monobasic organic acid include butyric acid, isobutyric acid, caproic acid, 2-ethylbutyric acid, heptyl acid, n-octylic acid, 2-ethylhexyl acid, n-nonylic acid, decylic acid, and benzoic acid.
[0207] Examples of the polybasic organic acid ester include ester compounds of a polybasic organic acid and an alcohol having a linear or branched structure and having 4 to 8 carbon atoms. Examples of the polybasic organic acid include adipic acid, sebacic acid, and azelaic acid.
[0208] Examples of the organic ester plasticizer include triethylene glycol di-2-ethylpropanoate, triethylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylhexanoate, triethylene glycol dicaprylate, triethylene glycol di-n-octanoate, triethylene glycol di-n-heptanoate, tetraethylene glycol di-n-heptanoate, dibutyl sebacate, dioctyl azelate, dibutyl carbitol adipate, ethylene glycol di-2-ethylbutyrate, 1,3-propylene glycol di-2-ethylbutyrate, 1,4-butylene glycol di-2-ethylbutyrate, and diethylene glycol di-2-ethylbutylene. Examples of suitable organic ester plasticizers include diethylene glycol di-2-ethylhexanoate, dipropylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylpentanoate, tetraethylene glycol di-2-ethylbutyrate, diethylene glycol dicaprylate, diethylene glycol dibenzoate, dipropylene glycol dibenzoate, dihexyl adipate, dioctyl adipate, hexylcyclohexyl adipate, a mixture of heptyl adipate and nonyl adipate, diisononyl adipate, diisodecyl adipate, heptylnonyl adipate, dibutyl sebacate, oil-modified alkyd sebacate, and a mixture of a phosphate ester and an adipate. Organic ester plasticizers other than those listed above may also be used as the organic ester plasticizer. Furthermore, adipate esters other than the above-mentioned adipate esters may also be used as the adipate ester.
[0209] Examples of the organic phosphoric acid plasticizer include tributoxyethyl phosphate, isodecylphenyl phosphate, and triisopropyl phosphate.
[0210] The plasticizer is preferably a diester plasticizer represented by the following formula (1):
[0211]
[0212] In the above formula (1), R1 and R2 each represent an organic group having 2 to 10 carbon atoms, R3 represents an ethylene group, an isopropylene group, or an n-propylene group, and p represents an integer of 3 to 10. In the above formula (1), R1 and R2 each preferably represent an organic group having 5 to 10 carbon atoms, and more preferably represent an organic group having 6 to 10 carbon atoms.
[0213] The plasticizer preferably includes triethylene glycol di-2-ethylhexanoate (3GO), triethylene glycol di-2-ethylbutyrate (3GH), or triethylene glycol di-2-ethylpropanoate. The plasticizer more preferably includes triethylene glycol di-2-ethylhexanoate (3GO) or triethylene glycol di-2-ethylbutyrate (3GH), and even more preferably includes triethylene glycol di-2-ethylhexanoate (3GO).
[0214] The content of the plasticizer contained in the interlayer film is preferably 5 parts by weight or more, more preferably 25 parts by weight or more, even more preferably 30 parts by weight or more, and preferably 45 parts by weight or less, more preferably 40 parts by weight or less, even more preferably 38 parts by weight or less, and particularly preferably 36 parts by weight or less, per 100 parts by weight of the resin (0) contained in the interlayer film. When the content of the plasticizer is at least the above-mentioned lower limit, the penetration resistance of the laminated glass is further improved. When the content of the plasticizer is at most the above-mentioned upper limit, it is easy to adjust the glass transition temperature of the interlayer film within the above-mentioned range. Furthermore, the transparency of the interlayer film is further improved. The range of the content of the plasticizer can be set by appropriately selecting the above-mentioned upper limit and lower limit.
[0215] The content of the plasticizer (1) contained in the first layer relative to 100 parts by weight of the resin (1) contained in the first layer is defined as content (1). The content (1) is preferably 50 parts by weight or more, more preferably 55 parts by weight or more, even more preferably 60 parts by weight or more, and preferably 100 parts by weight or less, more preferably 90 parts by weight or less, even more preferably 85 parts by weight or less, and particularly preferably 80 parts by weight or less. When the content (1) is equal to or greater than the lower limit, the flexibility of the interlayer film is increased, making the interlayer film easier to handle. When the content (1) is equal to or less than the upper limit, the penetration resistance of the laminated glass is further improved. The range of the content (1) can be set by appropriately selecting the upper limit and the lower limit.
[0216] The content of the plasticizer (2) contained in the second layer relative to 100 parts by weight of the resin (2) contained in the second layer is defined as content (2). The content of the plasticizer (3) contained in the third layer relative to 100 parts by weight of the resin (3) contained in the third layer is defined as content (3). The contents (2) and (3) are each preferably 5 parts by weight or more, more preferably 10 parts by weight or more, even more preferably 15 parts by weight or more, even more preferably 20 parts by weight or more, particularly preferably 24 parts by weight or more, most preferably 25 parts by weight or more, preferably 45 parts by weight or less, more preferably 40 parts by weight or less, even more preferably 35 parts by weight or less, particularly preferably 34 parts by weight or less, and most preferably 33 parts by weight or less. When the contents (2) and (3) are at least the lower limits, the flexibility of the interlayer film is increased, making the interlayer film easier to handle. When the contents (2) and (3) are at most the upper limits, the penetration resistance of the laminated glass is further improved. The range of the content (2) and the range of the content (3) can be set by appropriately selecting the upper limit value and the lower limit value.
[0217] In order to improve the sound insulation of the laminated glass, the content (1) is preferably greater than the content (2), and the content (1) is preferably greater than the content (3).
[0218] The absolute value of the difference between the content (2) and the content (1), and the absolute value of the difference between the content (3) and the content (1), are each preferably 10 parts by weight or more, more preferably 15 parts by weight or more, even more preferably 20 parts by weight or more, particularly preferably 25 parts by weight or more, and preferably 80 parts by weight or less, more preferably 75 parts by weight or less, even more preferably 70 parts by weight or less, even more preferably 65 parts by weight or less, even more preferably 60 parts by weight or less, even more preferably 55 parts by weight or less, even more preferably 50 parts by weight or less, particularly preferably 45 parts by weight or less, and most preferably 40 parts by weight or less. When the absolute value of the difference is equal to or greater than the lower limit and equal to or less than the upper limit, the sound insulation of the laminated glass can be further improved. The range of the absolute value of the difference can be set by appropriately selecting the upper limit and the lower limit.
[0219] (Heat-shielding material) The intermediate film preferably contains a heat-shielding material. The first layer preferably contains a heat-shielding material. The second layer preferably contains a heat-shielding material. The third layer preferably contains a heat-shielding material. Only one type of heat-shielding material may be used, or two or more types may be used in combination.
[0220] The heat-shielding material preferably contains at least one component X selected from a phthalocyanine compound, a naphthalocyanine compound, and an anthracyanine compound, or contains heat-shielding particles. In this case, the heat-shielding material may contain both the component X and the heat-shielding particles.
[0221] Component X: The interlayer film preferably contains at least one component X selected from a phthalocyanine compound, a naphthalocyanine compound, and an anthracyanine compound. The first layer preferably contains the component X. The second layer preferably contains the component X. The third layer preferably contains the component X. The component X is a heat-shielding material. Only one type of component X may be used, or two or more types may be used in combination.
[0222] There are no particular restrictions on the component X. As the component X, conventionally known phthalocyanine compounds, naphthalocyanine compounds, and anthracyanine compounds can be used.
[0223] Examples of the component X include phthalocyanine, phthalocyanine derivatives, naphthalocyanine, naphthalocyanine derivatives, anthracyanine, and anthracyanine derivatives. The phthalocyanine compound and the phthalocyanine derivative preferably have a phthalocyanine skeleton. The naphthalocyanine compound and the naphthalocyanine derivative preferably have a naphthalocyanine skeleton. The anthracyanine compound and the anthracyanine derivative preferably have an anthracyanine skeleton.
[0224] From the viewpoint of further improving the heat-shielding properties of the interlayer film and laminated glass, the component X is preferably at least one selected from the group consisting of phthalocyanine, phthalocyanine derivatives, naphthalocyanine, and naphthalocyanine derivatives, and more preferably at least one of phthalocyanine and phthalocyanine derivatives.
[0225] From the viewpoint of effectively improving the heat-shielding properties and maintaining a higher visible light transmittance for a long period of time, the component X preferably contains a vanadium atom or a copper atom. The component X preferably contains a vanadium atom, and also preferably contains a copper atom. The component X is more preferably at least one of a phthalocyanine containing a vanadium atom or a copper atom and a derivative of a phthalocyanine containing a vanadium atom or a copper atom. From the viewpoint of further improving the heat-shielding properties of the interlayer film and laminated glass, the component X preferably has a structural unit in which an oxygen atom is bonded to a vanadium atom.
[0226] The content of component X in 100 wt% of the interlayer film or 100 wt% of the layer containing component X (first layer, second layer, or third layer) is preferably 0.001 wt% or more, more preferably 0.005 wt% or more, even more preferably 0.01 wt% or more, particularly preferably 0.02 wt% or more, preferably 0.2 wt% or less, more preferably 0.1 wt% or less, even more preferably 0.05 wt% or less, and particularly preferably 0.04 wt% or less. When the content of component X is equal to or greater than the above-mentioned lower limit and equal to or less than the above-mentioned upper limit, the heat-shielding properties are sufficiently high and the visible light transmittance is sufficiently high. For example, it is possible to achieve a visible light transmittance of 70% or more. The range of the content of component X can be set by appropriately selecting the above-mentioned upper limit and lower limit.
[0227] Heat-shielding particles: The interlayer film preferably contains heat-shielding particles. The first layer preferably contains heat-shielding particles. The second layer preferably contains heat-shielding particles. The third layer preferably contains heat-shielding particles. The heat-shielding particles are a heat-shielding material. Use of the heat-shielding particles can effectively block infrared rays (heat rays). Only one type of the heat-shielding particles may be used, or two or more types may be used in combination.
[0228] From the viewpoint of further enhancing the heat-shielding properties of the laminated glass, the heat-shielding particles are more preferably metal oxide particles, and the heat-shielding particles are preferably particles formed from a metal oxide (metal oxide particles).
[0229] Infrared rays, which have wavelengths of 780 nm or more, which are longer than visible light, have a smaller amount of energy than ultraviolet rays. However, infrared rays have a large thermal effect, and when infrared rays are absorbed by a substance, they are released as heat. For this reason, infrared rays are generally called heat rays. By using the above heat-shielding particles, infrared rays (heat rays) can be effectively blocked. Here, heat-shielding particles refer to particles that can absorb infrared rays.
[0230] Specific examples of the heat-shielding particles include metal oxide particles such as aluminum-doped tin oxide particles, indium-doped tin oxide particles, antimony-doped tin oxide particles (ATO particles), gallium-doped zinc oxide particles (GZO particles), indium-doped zinc oxide particles (IZO particles), aluminum-doped zinc oxide particles (AZO particles), niobium-doped titanium oxide particles, tungsten oxide particles (sodium-doped tungsten oxide particles, cesium-doped tungsten oxide particles, thallium-doped tungsten oxide particles, rubidium-doped tungsten oxide particles, etc.), tin-doped indium oxide particles (ITO particles), tin-doped zinc oxide particles, and silicon-doped zinc oxide particles; and lanthanum hexaboride (LaB 6 ) particles, etc. Heat-shielding particles other than these may also be used. Metal oxide particles are preferred because of their high heat-ray shielding function, and ATO particles, GZO particles, IZO particles, ITO particles, or tungsten oxide particles are more preferred, with ITO particles or tungsten oxide particles being particularly preferred. In particular, tin-doped indium oxide particles (ITO particles) are preferred because of their high heat-ray shielding function and ease of availability, and tungsten oxide particles are also preferred.
[0231] From the viewpoint of further improving the heat-shielding properties of the interlayer film and laminated glass, the tungsten oxide particles are preferably metal-doped tungsten oxide particles. The "tungsten oxide particles" include metal-doped tungsten oxide particles. Specific examples of the metal-doped tungsten oxide particles include sodium-doped tungsten oxide particles, cesium-doped tungsten oxide particles, thallium-doped tungsten oxide particles, and rubidium-doped tungsten oxide particles.
[0232] From the viewpoint of further improving the heat-shielding properties of the interlayer film and laminated glass, cesium-doped tungsten oxide particles are particularly preferred. From the viewpoint of further improving the heat-shielding properties of the interlayer film and laminated glass, the cesium-doped tungsten oxide particles are represented by the formula: Cs 0.33 WO 3 Preferably, the tungsten oxide particles are represented by the formula:
[0233] The average particle size of the heat-shielding particles is preferably 0.01 μm or more, more preferably 0.02 μm or more, and preferably 0.1 μm or less, more preferably 0.05 μm or less. When the average particle size is equal to or greater than the lower limit, the heat ray shielding property is sufficiently high. When the average particle size is equal to or less than the upper limit, the dispersibility of the heat-shielding particles is high. The range of the average particle size can be set by appropriately selecting the upper limit and the lower limit.
[0234] The "average particle size" refers to the volume average particle size. The average particle size can be measured using a particle size distribution analyzer ("UPA-EX150" manufactured by Nikkiso Co., Ltd.) or the like.
[0235] The content of the heat-shielding particles (particularly the content of tungsten oxide particles) in 100 wt % of the interlayer film or 100 wt % of the layer containing the heat-shielding particles (first layer, second layer, or third layer) is preferably 0.01 wt % or more, more preferably 0.1 wt % or more, even more preferably 1 wt % or more, particularly preferably 1.5 wt % or more, preferably 6 wt % or less, more preferably 5.5 wt % or less, even more preferably 4 wt % or less, particularly preferably 3.5 wt % or less, and most preferably 3 wt % or less. When the content of the heat-shielding particles is equal to or greater than the above lower limit and equal to or less than the above upper limit, the heat-shielding property is sufficiently high and the visible light transmittance is sufficiently high. The range of the content of the heat-shielding particles can be set by appropriately selecting the above upper limit and the above lower limit.
[0236] (Metal Salt) The interlayer film preferably contains at least one metal salt of an alkali metal salt and an alkaline earth metal salt (hereinafter, sometimes referred to as metal salt M). The first layer preferably contains the metal salt M. The second layer preferably contains the metal salt M. The third layer preferably contains the metal salt M. The alkaline earth metals refer to six metals: Be, Mg, Ca, Sr, Ba, and Ra. The use of the metal salt M makes it easy to control the adhesion between the interlayer film and a laminated glass member such as a glass plate, or the adhesion between each layer in the interlayer film. Only one type of metal salt M may be used, or two or more types may be used in combination.
[0237] The metal salt M preferably contains at least one metal selected from the group consisting of Li, Na, K, Rb, Cs, Mg, Ca, Sr, and Ba. The metal salt M contained in the interlayer film preferably contains at least one metal selected from the group consisting of K and Mg.
[0238] Furthermore, alkali metal salts of organic acids having 2 to 16 carbon atoms and alkaline earth metal salts of organic acids having 2 to 16 carbon atoms can be used as the metal salt M. The metal salt M may include a magnesium salt of a carboxylic acid having 2 to 16 carbon atoms or a potassium salt of a carboxylic acid having 2 to 16 carbon atoms.
[0239] Examples of the magnesium salts of carboxylic acids having 2 to 16 carbon atoms and the potassium salts of carboxylic acids having 2 to 16 carbon atoms include magnesium acetate, potassium acetate, magnesium propionate, potassium propionate, magnesium 2-ethylbutyrate, potassium 2-ethylbutanoate, magnesium 2-ethylhexanoate, and potassium 2-ethylhexanoate.
[0240] The total content of Mg and K in the interlayer film or the layer containing the metal salt M (first layer, second layer, or third layer) is preferably 5 ppm or more, more preferably 10 ppm or more, and even more preferably 20 ppm or more, and is preferably 300 ppm or less, more preferably 250 ppm or less, and even more preferably 200 ppm or less. When the total content of Mg and K is equal to or greater than the above-mentioned lower limit and equal to or less than the above-mentioned upper limit, the adhesion between the interlayer film and the laminated glass member (e.g., glass plate) or the adhesion between the layers in the interlayer film can be more effectively controlled. The range of the total content of Mg and K can be set by appropriately selecting the above-mentioned upper limit and lower limit.
[0241] (Ultraviolet ray blocking agent) The interlayer film preferably contains an ultraviolet ray blocking agent. The first layer preferably contains an ultraviolet ray blocking agent. The second layer preferably contains an ultraviolet ray blocking agent. The third layer preferably contains an ultraviolet ray blocking agent. By using an ultraviolet ray blocking agent, the visible light transmittance of the laminated glass is more unlikely to decrease even after long-term use. Only one type of ultraviolet ray blocking agent may be used, or two or more types may be used in combination.
[0242] The ultraviolet screening agent includes an ultraviolet absorbing agent, and the ultraviolet screening agent is preferably an ultraviolet absorbing agent.
[0243] Examples of the ultraviolet screening agent include ultraviolet screening agents containing metal atoms, ultraviolet screening agents containing metal oxides, ultraviolet screening agents having a benzotriazole structure (benzotriazole compounds), ultraviolet screening agents having a benzophenone structure (benzophenone compounds), ultraviolet screening agents having a triazine structure (triazine compounds), ultraviolet screening agents having a malonic acid ester structure (malonic acid ester compounds), ultraviolet screening agents having an oxalic acid anilide structure (oxalic acid anilide compounds), and ultraviolet screening agents having a benzoate structure (benzoate compounds).
[0244] Examples of the ultraviolet shielding agent containing the metal atom include platinum particles, platinum particles whose surfaces are coated with silica, palladium particles, and palladium particles whose surfaces are coated with silica. The ultraviolet shielding agent is preferably not a heat-shielding particle.
[0245] The ultraviolet screening agent is preferably an ultraviolet screening agent having a benzotriazole structure, an ultraviolet screening agent having a benzophenone structure, an ultraviolet screening agent having a triazine structure, or an ultraviolet screening agent having a benzoate structure, more preferably an ultraviolet screening agent having a benzotriazole structure or an ultraviolet screening agent having a benzophenone structure, and even more preferably an ultraviolet screening agent having a benzotriazole structure.
[0246] Examples of the ultraviolet screening agent containing a metal oxide include zinc oxide, titanium oxide, and cerium oxide. Furthermore, the surface of the ultraviolet screening agent containing a metal oxide may be coated. Examples of the coating material for the surface of the ultraviolet screening agent containing a metal oxide include insulating metal oxides, hydrolyzable organosilicon compounds, and silicone compounds.
[0247] Examples of the insulating metal oxide include silica, alumina, zirconia, etc. The insulating metal oxide has a band gap energy of, for example, 5.0 eV or more.
[0248] Examples of the ultraviolet screening agent having a benzotriazole structure include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole ("Tinuvin P" manufactured by BASF), 2-(2'-hydroxy-3',5'-di-t-butylphenyl)benzotriazole ("Tinuvin 320" manufactured by BASF), 2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole ("Tinuvin 326" manufactured by BASF), and 2-(2'-hydroxy-3',5'-di-amylphenyl)benzotriazole ("Tinuvin 328" manufactured by BASF). Due to their excellent ultraviolet screening performance, the ultraviolet screening agent is preferably an ultraviolet screening agent having a benzotriazole structure containing a halogen atom, and more preferably an ultraviolet screening agent having a benzotriazole structure containing a chlorine atom.
[0249] Examples of the ultraviolet screening agent having a benzophenone structure include octabenzone ("Chimassorb 81" manufactured by BASF).
[0250] Examples of the ultraviolet screening agent having a triazine structure include "LA-F70" manufactured by ADEKA Corporation and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol ("Tinuvin 1577FF" manufactured by BASF).
[0251] Examples of the ultraviolet screening agent having a malonic acid ester structure include dimethyl 2-(p-methoxybenzylidene)malonate, tetraethyl-2,2-(1,4-phenylenedimethylidene)bismalonate, and 2-(p-methoxybenzylidene)-bis(1,2,2,6,6-pentamethyl-4-piperidinyl)malonate.
[0252] Commercially available ultraviolet screening agents having the malonic acid ester structure include Hostavin B-CAP, Hostavin PR-25, and Hostavin PR-31 (all manufactured by Clariant).
[0253] Examples of the ultraviolet screening agent having an oxalic acid anilide structure include oxalic acid diamides having an aryl group substituted on the nitrogen atom, such as N-(2-ethylphenyl)-N'-(2-ethoxy-5-t-butylphenyl)oxalic acid diamide, N-(2-ethylphenyl)-N'-(2-ethoxy-phenyl)oxalic acid diamide, and 2-ethyl-2'-ethoxy-oxalanilide ("Sanduvor VSU" manufactured by Clariant).
[0254] Examples of the ultraviolet screening agent having a benzoate structure include 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate ("Tinuvin 120" manufactured by BASF).
[0255] The content of the ultraviolet screening agent in 100 wt% of the interlayer film or 100 wt% of the layer containing the ultraviolet screening agent (first layer, second layer, or third layer) is preferably 0.1 wt% or more, more preferably 0.2 wt% or more, even more preferably 0.3 wt% or more, particularly preferably 0.5 wt% or more, preferably 2.5 wt% or less, more preferably 2 wt% or less, even more preferably 1 wt% or less, and particularly preferably 0.8 wt% or less. When the content of the ultraviolet screening agent is equal to or greater than the lower limit, the decrease in visible light transmittance after a period of time is further suppressed. When the content of the ultraviolet screening agent is equal to or less than the upper limit, the decrease in visible light transmittance of the interlayer film and laminated glass after a period of time is significantly suppressed. The range of the content of the ultraviolet screening agent can be set by appropriately selecting the upper limit and the lower limit.
[0256] (Antioxidant) The interlayer film preferably contains an antioxidant. The first layer preferably contains an antioxidant. The second layer preferably contains an antioxidant. The third layer preferably contains an antioxidant. Only one type of antioxidant may be used, or two or more types may be used in combination.
[0257] Examples of the antioxidant include phenol-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants. The phenol-based antioxidants are antioxidants having a phenol skeleton. The sulfur-based antioxidants are antioxidants containing sulfur atoms. The phosphorus-based antioxidants are antioxidants containing phosphorus atoms.
[0258] The antioxidant is preferably a phenol-based antioxidant or a phosphorus-based antioxidant.
[0259] Examples of the phenolic antioxidant include 2,6-di-t-butyl-p-cresol (BHT), butylhydroxyanisole (BHA), 2,6-di-t-butyl-4-ethylphenol, stearyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2'-methylenebis-(4-methyl-6-butylphenol), 2,2'-methylenebis-(4-ethyl-6-t-butylphenol), 4,4'-butylidene-bis-(3-methyl-6-t-butylphenol), 1,1,3-tris-(2-methyl-hydroxy-5- Examples of antioxidants include tetrakis[methylene-3-(3',5'-butyl-4-hydroxyphenyl)propionate]methane, 1,3,3-tris-(2-methyl-4-hydroxy-5-t-butylphenol)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis(3,3'-t-butylphenol)butyric acid glycol ester, and bis(3-t-butyl-4-hydroxy-5-methylbenzenepropanoate)ethylenebis(oxyethylene). One or more of these antioxidants are preferably used.
[0260] Examples of the phosphorus-based antioxidant include tridecyl phosphite, tris(tridecyl)phosphite, triphenyl phosphite, trinonylphenyl phosphite, bis(tridecyl)pentaerythritol diphosphite, bis(decyl)pentaerythritol diphosphite, tris(2,4-di-t-butylphenyl)phosphite, bis(2,4-di-t-butyl-6-methylphenyl)ethyl ester phosphorous acid, and 2,2'-methylenebis(4,6-di-t-butyl-1-phenyloxy)(2-ethylhexyloxy)phosphorus, etc. One or more of these antioxidants are preferably used.
[0261] Examples of commercially available antioxidants include "IRGANOX 245" manufactured by BASF, "IRGAFOS 168" manufactured by BASF, "IRGAFOS 38" manufactured by BASF, "Sumilizer BHT" manufactured by Sumitomo Chemical Co., Ltd., "H-BHT" manufactured by Sakai Chemical Industry Co., Ltd., and "IRGANOX 1010" manufactured by BASF.
[0262] In order to maintain a high visible light transmittance of the interlayer film and laminated glass for a long period of time, the content of the antioxidant is preferably 0.03 wt% or more, and more preferably 0.1 wt% or more, based on 100 wt% of the interlayer film or 100 wt% of the layer containing the antioxidant (first layer, second layer, or third layer). Furthermore, since the effect of adding the antioxidant becomes saturated, the content of the antioxidant is preferably 2 wt% or less, based on 100 wt% of the interlayer film or 100 wt% of the layer containing the antioxidant (first layer, second layer, or third layer). The range of the antioxidant content can be set by appropriately selecting the upper and lower limits.
[0263] (Light stabilizer) The interlayer film preferably contains a light stabilizer. The first layer preferably contains a light stabilizer. The second layer preferably contains a light stabilizer. The third layer preferably contains a light stabilizer. Only one type of light stabilizer may be used, or two or more types may be used in combination.
[0264] The light stabilizer is preferably a hindered amine light stabilizer.
[0265] Examples of the hindered amine light stabilizer include a hindered amine light stabilizer in which a carbon atom, an alkoxy group, or a hydrogen atom is bonded to a nitrogen atom of a piperidine structure. From the viewpoint of further suppressing discoloration, a hindered amine light stabilizer in which a carbon atom or an alkoxy group is bonded to a nitrogen atom of a piperidine structure is preferred. The hindered amine light stabilizer is preferably a hindered amine light stabilizer in which a carbon atom is bonded to a nitrogen atom of a piperidine structure, and is also preferably a hindered amine light stabilizer in which an alkoxy group is bonded to a nitrogen atom of a piperidine structure. The hindered amine light stabilizer in which a carbon atom is bonded to a nitrogen atom of a piperidine structure may be a hindered amine light stabilizer in which an alkyl group or an alkylene group is bonded to a nitrogen atom of a piperidine structure. The hindered amine light stabilizer in which a carbon atom is bonded to a nitrogen atom of a piperidine structure may be a hindered amine light stabilizer in which an alkyl group is bonded to a nitrogen atom of a piperidine structure, or may be a hindered amine light stabilizer in which an alkyl group is bonded to a nitrogen atom of a piperidine structure.
[0266] Examples of the hindered amine light stabilizer in which a carbon atom is bonded to the nitrogen atom of the piperidine structure include "Tinuvin 765" and "Tinuvin 622SF" manufactured by BASF, and "ADK STAB LA-52" manufactured by ADEKA. Examples of the hindered amine light stabilizer in which an alkoxy group is bonded to the nitrogen atom of the piperidine structure include "Tinuvin XT-850FF" and "Tinuvin XT-855FF" manufactured by BASF, and "ADK STAB LA-81" manufactured by ADEKA. Examples of the hindered amine light stabilizer in which a hydrogen atom is bonded to the nitrogen atom of the piperidine structure include "Tinuvin 770DF" manufactured by BASF, and "Hostavin N24" manufactured by Clariant.
[0267] From the viewpoint of further suppressing discoloration, the molecular weight of the light stabilizer is preferably 2,000 or less, more preferably 1,000 or less, and even more preferably 700 or less.
[0268] The content of the light stabilizer in 100% by weight of the interlayer film or 100% by weight of the layer containing the light stabilizer (first layer, second layer, or third layer) is preferably 0.0025% by weight or more, more preferably 0.025% by weight or more, and preferably 0.5% by weight or less, more preferably 0.3% by weight or less. When the content of the light stabilizer is equal to or greater than the above lower limit and equal to or less than the above upper limit, discoloration is effectively suppressed. The range of the content of the light stabilizer can be set by appropriately selecting the above upper limit and lower limit.
[0269] (Other Components) The interlayer film, the first layer, the second layer, and the third layer may each contain components other than the above-mentioned components, as necessary. Examples of the other components include colorants (pigments, dyes, etc.), coupling agents, dispersants, surfactants, flame retardants, antistatic agents, adhesion modifiers other than metal salts, moisture-resistant agents, fluorescent brighteners, and infrared absorbers. Each of these other components may be used alone or in combination of two or more.
[0270] (Other Details of the Interlayer Film for Laminated Glass) The distance between the first end and the second end of the interlayer film is preferably 0.5 m or more, more preferably 0.8 m or more, particularly preferably 1.0 m or more, and preferably 3.0 m or less, more preferably 2.0 m or less, particularly preferably 1.5 m or less. The range of this distance can be set by appropriately selecting the upper and lower limits.
[0271] The interlayer film may be wound into a roll of the interlayer film. The roll may include a winding core and the interlayer film wound around the outer periphery of the winding core.
[0272] The method for producing the interlayer film is not particularly limited. In the case of a single-layer interlayer film, the method for producing the interlayer film includes extruding a resin composition using an extruder. In the case of a multi-layer interlayer film, the method for producing the interlayer film includes, for example, forming each layer using a resin composition for each layer, and then laminating the resulting layers. Furthermore, the method for producing the interlayer film includes co-extruding the resin compositions for each layer using an extruder to laminate the layers. A production method using extrusion molding is preferred because it is suitable for continuous production.
[0273] In view of excellent production efficiency of the interlayer film, it is preferable that the second layer and the third layer contain the same polyvinyl acetal resin. In view of excellent production efficiency of the interlayer film, it is more preferable that the second layer and the third layer contain the same polyvinyl acetal resin and the same plasticizer. In view of excellent production efficiency of the interlayer film, it is even more preferable that the second layer and the third layer are formed from the same resin composition.
[0274] The method for manufacturing the interlayer film preferably includes an extrusion step of obtaining a pre-cut interlayer film by extrusion molding, and a cutting step of cutting the pre-cut interlayer film at a predetermined position from one end in the TD direction. In the cutting step, the pre-cut interlayer film is preferably cut at a predetermined position from one end in the TD direction and at a predetermined position from the other end in the TD direction. In this case, an interlayer film satisfying the above-mentioned configuration A or B can be suitably obtained.
[0275] The interlayer film preferably has an uneven shape on at least one of its two surfaces. The interlayer film more preferably has an uneven shape on both surfaces. The method for forming the uneven shape is not particularly limited, and examples thereof include lip embossing (melt fracture), embossing roll, calender roll, and profile extrusion.
[0276] (Laminated Glass) The laminated glass according to the present invention includes a first laminated glass member, a second laminated glass member, and an interlayer film. In the laminated glass according to the present invention, the interlayer film is disposed between the first laminated glass member and the second laminated glass member.
[0277] The laminated glass preferably comprises a first laminated glass member, a second laminated glass member, and the above-described interlayer film.
[0278] The laminated glass has a first end (one end) and a second end (the other end) opposite the first end. The first end and the second end are opposite ends of the laminated glass. It is preferable that the first end and the second end of the laminated glass correspond to opposite ends of the interlayer film in the transverse direction.
[0279] The laminated glass preferably satisfies the following configuration A' or B'. In this case, vibration damping properties in the high frequency range can be improved at the edge portions of the laminated glass.
[0280] Configuration A': The rate of change A3 represented by the following formula (A3) is less than 10%, and the rate of change A4 represented by the following formula (A4) is less than 10%.
[0281] Rate of change A3 (%) = (|P A '-Q A '| / Q A ')×100...(A3)
[0282] P A Q′: Secondary loss coefficient of the laminated glass in a portion of the laminated glass from the position of 0 mm to the position of 25 mm from the first end toward the second end A ': Secondary loss coefficient of the laminated glass in a portion of the laminated glass from a position 100 mm to a position 125 mm from the first end toward the second end
[0283] Rate of change A4 (%) = (|R A '-S A '| / S A ')×100...(A4)
[0284] R A ': secondary loss coefficient S of the laminated glass in a portion of the laminated glass from the position of 0 mm to the position of 25 mm from the second end toward the first end A ': Secondary loss coefficient of the laminated glass in a portion of the laminated glass from a position 100 mm to a position 125 mm from the second end toward the first end
[0285] Configuration B': The rate of change B3 represented by the following formula (B3) is less than 10%, and the rate of change B4 represented by the following formula (B4) is less than 10%.
[0286] Rate of change B3 (%) = (|P B '-Q B '| / Q B ')×100...(B3)
[0287] P B Q′: the second resonance frequency of the laminated glass in the portion of the laminated glass from the position of 0 mm to the position of 25 mm from the first end toward the second end B ': Secondary resonance frequency of the laminated glass in a portion of the laminated glass from a position 100 mm to a position 125 mm from the first end toward the second end
[0288] Rate of change B4 (%) = (|R B '-S B '| / S B ')×100...(B4)
[0289] R B ': the secondary resonance frequency S of the laminated glass in the portion of the laminated glass from the position of 0 mm to the position of 25 mm from the second end toward the first end B ': Secondary resonance frequency of the laminated glass in a portion of the laminated glass from a position 100 mm to a position 125 mm from the second end toward the first end
[0290] The laminated glass may satisfy the above-mentioned Structure A', may satisfy the above-mentioned Structure B', or may satisfy both the above-mentioned Structure A' and the above-mentioned Structure B'. From the viewpoint of more effectively exerting the effects of the present invention, the laminated glass preferably satisfies the above-mentioned Structure B', and more preferably satisfies the above-mentioned Structure A' and the above-mentioned Structure B'.
[0291] In the laminated glass satisfying the above-mentioned configuration A', the rate of change A3 expressed by the above-mentioned formula (A3) is less than 10%, and the rate of change A4 expressed by the above-mentioned formula (A4) is less than 10%.
[0292] The rate of change A3 is preferably greater than 0%, more preferably 1% or more, even more preferably 1.8% or more, even more preferably 2% or more, particularly preferably 3% or more, most preferably 4% or more, and preferably 9.7% or less, more preferably 9% or less, even more preferably 8% or less, even more preferably 7% or less, and particularly preferably 6% or less. When the rate of change A3 exceeds the lower limit or is equal to or greater than the lower limit, the generation of scrap material during the production of laminated glass can be effectively suppressed. When the rate of change A3 is equal to or less than the upper limit, the effects of the present invention can be more effectively exhibited. The range of the rate of change A3 can be set by appropriately selecting the upper limit and the lower limit.
[0293] The secondary loss coefficient of the laminated glass (P A The secondary loss factor (P A When the second loss coefficient (P A The secondary loss coefficient (P A The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0294] The secondary loss coefficient of the above laminated glass (Q A The secondary loss factor (Q ′) is preferably 0.20 or more, more preferably 0.25 or more, even more preferably 0.30 or more, and particularly preferably 0.35 or more. A When the second loss coefficient (Q ′) of the laminated glass is equal to or greater than the lower limit, the sound insulation of the laminated glass can be further improved. A The secondary loss coefficient (Q ′) of the laminated glass may be 0.80 or less, 0.75 or less, 0.70 or less, 0.65 or less, 0.60 or less, 0.55 or less, 0.50 or less, or 0.45 or less. A The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0295] The change rate A4 is preferably greater than 0%, more preferably 1% or more, even more preferably 1.8% or more, even more preferably 2% or more, particularly preferably 3% or more, most preferably 4% or more, and preferably 9% or less, more preferably 8% or less, even more preferably 7% or less, even more preferably 6.9% or less, and particularly preferably 6% or less. When the change rate A4 exceeds the lower limit or is equal to or greater than the lower limit, the generation of scrap material during the production of laminated glass can be effectively suppressed. When the change rate A4 is equal to or less than the upper limit, the effects of the present invention can be more effectively exhibited. The range of the change rate A4 can be set by appropriately selecting the upper limit and the lower limit.
[0296] The secondary loss coefficient (R A The secondary loss factor (R ′) is preferably 0.20 or more, more preferably 0.25 or more, even more preferably 0.30 or more, and particularly preferably 0.35 or more. A When the second loss coefficient (R ′) of the laminated glass is equal to or greater than the lower limit, the sound insulation of the laminated glass can be further improved. AThe secondary loss coefficient (R ′) of the laminated glass may be 0.80 or less, 0.75 or less, 0.70 or less, 0.65 or less, 0.60 or less, 0.55 or less, 0.50 or less, or 0.45 or less. A The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0297] The secondary loss coefficient (S A The secondary loss factor (S A When the second loss coefficient (S A The secondary loss coefficient (S A The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0298] In the laminated glass satisfying the above-mentioned configuration B', the rate of change B3 expressed by the above-mentioned formula (B3) is less than 10%, and the rate of change B4 expressed by the above-mentioned formula (B4) is less than 10%.
[0299] The change rate B3 is preferably greater than 0%, more preferably 1% or more, even more preferably 1.8% or more, even more preferably 2% or more, particularly preferably 3% or more, most preferably 4% or more, and preferably 9% or less, more preferably 8% or less, even more preferably 7.9% or less, even more preferably 7% or less, and particularly preferably 6% or less. When the change rate B3 exceeds the lower limit or is equal to or greater than the lower limit, the generation of scrap material during the production of laminated glass can be effectively suppressed. When the change rate B3 is equal to or less than the upper limit, the effects of the present invention can be more effectively exhibited. The range of the change rate B3 can be set by appropriately selecting the upper limit and the lower limit.
[0300] The secondary resonance frequency (P B The secondary resonance frequency (P B When the secondary resonance frequency (P B The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0301] The secondary resonance frequency (Q B The secondary resonance frequency (Q ′) is preferably 500 Hz or more, more preferably 600 Hz or more, even more preferably 700 Hz or more, particularly preferably 720 Hz or more, most preferably 760 Hz or more, and is preferably 1000 Hz or less, more preferably 900 Hz or less, and even more preferably 840 Hz or less. B When the secondary resonance frequency (Q ′) is equal to or greater than the above lower limit and equal to or less than the above upper limit, the sound insulation of the laminated glass can be further improved. B The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0302] The change rate B4 is preferably greater than 0%, more preferably 1% or more, even more preferably 1.8% or more, even more preferably 2% or more, particularly preferably 3% or more, most preferably 4% or more, and preferably 9% or less, more preferably 8% or less, even more preferably 7.4% or less, even more preferably 7% or less, and particularly preferably 6% or less. When the change rate B4 exceeds the lower limit or is equal to or greater than the lower limit, the generation of scrap material during the production of laminated glass can be effectively suppressed. When the change rate B4 is equal to or less than the upper limit, the effects of the present invention can be more effectively exhibited. The range of the change rate B4 can be set by appropriately selecting the upper limit and the lower limit.
[0303] The secondary resonance frequency (R B The secondary resonance frequency (R ′) is preferably 500 Hz or more, more preferably 600 Hz or more, even more preferably 700 Hz or more, particularly preferably 720 Hz or more, most preferably 760 Hz or more, and is preferably 1000 Hz or less, more preferably 900 Hz or less, and even more preferably 840 Hz or less. B When the secondary resonance frequency (R ′) is equal to or greater than the above lower limit and equal to or less than the above upper limit, the sound insulation of the laminated glass can be further improved. B The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0304] The secondary resonance frequency (S B The secondary resonance frequency (S ′) is preferably 500 Hz or more, more preferably 600 Hz or more, even more preferably 700 Hz or more, particularly preferably 720 Hz or more, most preferably 760 Hz or more, and is preferably 1000 Hz or less, more preferably 900 Hz or less, and even more preferably 840 Hz or less. B When the secondary resonance frequency (S ′) is equal to or greater than the above lower limit and equal to or less than the above upper limit, the sound insulation of the laminated glass can be further improved. B The range of (a) can be set by appropriately selecting the above upper limit value and the above lower limit value.
[0305] The secondary loss factor and secondary resonance frequency of the laminated glass can be measured by the same method as the method for measuring the secondary loss factor and secondary resonance frequency of the laminated glasses P, Q, R, and S. In the laminated glass, if the thickness of the first laminated glass member is different from the thickness of the second laminated glass member, the secondary loss factor and secondary resonance frequency are measured by applying vibration from the surface of the thicker laminated glass member.
[0306] FIG. 3 is a cross-sectional view that schematically shows an example of laminated glass that uses the interlayer film for laminated glass shown in FIG.
[0307] The laminated glass 31 shown in Fig. 3 includes a first laminated glass member 21, a second laminated glass member 22, and an interlayer film 11. The interlayer film 11 is disposed and sandwiched between the first laminated glass member 21 and the second laminated glass member 22.
[0308] A first laminated glass member 21 is laminated on a first surface of the interlayer film 11. A second laminated glass member 22 is laminated on a second surface opposite the first surface of the interlayer film 11. The first laminated glass member 21 is laminated on the outer surface of the second layer 2. The second laminated glass member 22 is laminated on the outer surface of the third layer 3.
[0309] The laminated glass 31 has a first end 31 a and a second end 31 b. The first end 31 a of the laminated glass 31 corresponds to the first end of the interlayer film 11, and the second end 31 b of the laminated glass 31 corresponds to the second end of the interlayer film 11.
[0310] The end face of the first end 31a includes the end face of the first laminated glass member 21, the end face of the first layer 1, the end face of the second layer 2, the end face of the third layer 3, and the end face of the second laminated glass member 22. The end face of the first end 31a is composed of the end face of the first laminated glass member 21, the end face of the first layer 1, the end face of the second layer 2, the end face of the third layer 3, and the end face of the second laminated glass member 22. The end face of the second end 31b is composed of the end face of the first laminated glass member 21, the end face of the first layer 1, the end face of the second layer 2, the end face of the third layer 3, and the end face of the second laminated glass member 22.
[0311] For the laminated glass 31, the second-order loss factor and second-order resonance frequency of the laminated glass 31 can be measured in a portion P of the laminated glass 31 from 0 mm to 25 mm toward the first end 31 a and the second end 31 b. For the laminated glass 31, the second-order loss factor and second-order resonance frequency of the laminated glass 31 can be measured in a portion Q of the laminated glass 31 from 100 mm to 125 mm toward the first end 31 a and the second end 31 b. For the laminated glass 31, the second-order loss factor and second-order resonance frequency of the laminated glass 31 can be measured in a portion R of the laminated glass 31 from 0 mm to 25 mm toward the second end 31 b and the first end 31 a. For the laminated glass 31, the second-order loss factor and second-order resonance frequency of the laminated glass 31 can be measured in a portion S of the laminated glass 31 from 100 mm to 125 mm toward the second end 31 b and the first end 31 a.
[0312] FIG. 4 is a cross-sectional view that schematically shows an example of laminated glass that uses the interlayer film for laminated glass shown in FIG. 2 .
[0313] The laminated glass 31A shown in Fig. 4 includes a first laminated glass member 21A, a second laminated glass member 22A, and an interlayer film 11A. The interlayer film 11A is disposed and sandwiched between the first laminated glass member 21A and the second laminated glass member 22A.
[0314] A first laminated glass member 21A is laminated on a first surface of the interlayer film 11A. A second laminated glass member 22A is laminated on a second surface opposite the first surface of the interlayer film 11A. The first laminated glass member 21A is laminated on the outer surface of the second layer 2A. The second laminated glass member 22A is laminated on the outer surface of the third layer 3A.
[0315] The laminated glass 31A has a first end 31a and a second end 31b. The first end 31a of the laminated glass 31A corresponds to the first end of the interlayer film 11A, and the second end 31b of the laminated glass 31A corresponds to the second end of the interlayer film 11A.
[0316] The end face of the first end portion 31a includes the end face of the first laminated glass member 21A, the end face of the first layer 1A, the end face of the second layer 2A, the end face of the third layer 3A, and the end face of the second laminated glass member 22A. The end face of the first end portion 31a is composed of the end face of the first laminated glass member 21A, the end face of the first layer 1A, the end face of the second layer 2A, the end face of the third layer 3A, and the end face of the second laminated glass member 22A. The end face of the second end portion 31b includes the end face of the first laminated glass member 21A, the end face of the first layer 1A, the end face of the second layer 2A, the end face of the third layer 3A, and the end face of the second laminated glass member 22A. The end face of the second end portion 31b is composed of the end face of the first laminated glass member 21A, the end face of the first layer 1A, the end face of the second layer 2A, the end face of the third layer 3A, and the end face of the second laminated glass member 22A.
[0317] For the laminated glass 31A, the secondary loss factor and secondary resonance frequency of the laminated glass 31A can be measured in a portion P of the laminated glass 31A extending from 0 mm to 25 mm toward the first end 31a and the second end 31b. For the laminated glass 31A, the secondary loss factor and secondary resonance frequency of the laminated glass 31A can be measured in a portion Q of the laminated glass 31A extending from 100 mm to 125 mm toward the first end 31a and the second end 31b. For the laminated glass 31A, the secondary loss factor and secondary resonance frequency of the laminated glass 31A can be measured in a portion R of the laminated glass 31A extending from 0 mm to 25 mm toward the second end 31b and the first end 31a. In the laminated glass 31A, the secondary loss factor and secondary resonant frequency of the laminated glass 31A can be measured in a portion S of the laminated glass 31A from a position 100 mm to a position 125 mm from the second end 31b toward the first end 31a.
[0318] The laminated glass may be a head-up display. When the laminated glass is a head-up display, the laminated glass has a display area for the head-up display. The display area is an area where information can be displayed well.
[0319] A head-up display system can be obtained using the head-up display. The head-up display system includes the laminated glass and a light source device for irradiating the laminated glass with light for image display. The light source device can be attached to the dashboard of a vehicle, for example. An image can be displayed by irradiating the display area of the laminated glass with light from the light source device.
[0320] The first laminated glass member is preferably a first glass plate, and the second laminated glass member is preferably a second glass plate.
[0321] Examples of the first and second laminated glass members include glass plates and PET (polyethylene terephthalate) films. The laminated glass includes not only laminated glass in which an interlayer film is sandwiched between two glass plates, but also laminated glass in which an interlayer film is sandwiched between a glass plate and a PET film or the like. The laminated glass is a laminate including glass plates, and preferably includes at least one glass plate. It is preferable that the first laminated glass member and the second laminated glass member are each a glass plate or a PET film, and that the laminated glass includes a glass plate as at least one of the first laminated glass member and the second laminated glass member. It is particularly preferable that both the first and second laminated glass members are glass plates.
[0322] Examples of the glass plate include inorganic glass and organic glass. Examples of the inorganic glass include float glass, heat-absorbing glass, heat-reflecting glass, polished glass, patterned glass, lined glass, and green glass. The organic glass is a synthetic resin glass that replaces inorganic glass. Examples of the organic glass include polycarbonate plates and poly(meth)acrylic resin plates. Examples of the poly(meth)acrylic resin plates include polymethyl(meth)acrylate plates.
[0323] The thickness of each of the first laminated glass member and the second laminated glass member is preferably 1 mm or more, preferably 5 mm or less, and more preferably 3 mm or less. When the laminated glass member is a glass plate, the thickness of the glass plate is preferably 0.5 mm or more, more preferably 0.7 mm or more, and preferably 5 mm or less, and more preferably 3 mm or less. From the viewpoint of reducing the frequency response function (FRF) value of the entire laminated glass at 1000 Hz to 3000 Hz and further improving vibration damping in the high frequency range (e.g., 1000 Hz to 3000 Hz), it is preferable that the thickness of each of the first laminated glass member and the second laminated glass member is small. For example, the thickness of each of the first laminated glass member and the second laminated glass member is preferably 2 mm or less, more preferably 1.8 mm or less, and even more preferably 1.6 mm or less. When the laminated glass member is a PET film, the thickness of the PET film is preferably 0.03 mm or more, and preferably 0.5 mm or less.
[0324] The thickness of the first laminated glass member and the thickness of the second laminated glass member may be the same or different.
[0325] The FRF value of the laminated glass is not particularly limited, and may be, for example, 10 dB or less, 6 dB or less, 5 dB or less, 4 dB or less, 3 dB or less, 2 dB or less, 1 dB or less, 0 dB or less, or -7 dB or less. The lower the FRF value, the better the vibration damping, so the lower limit is not particularly limited. From the viewpoint of improving vibration damping and bubbling resistance while also improving vibration damping, the FRF value of the laminated glass may be, for example, -20 dB or more or -10 dB or more. The FRF value of the laminated glass can be measured by the method described in the Examples section below. In the laminated glass, when the thickness of the first laminated glass member and the thickness of the second laminated glass member are different, the FRF value is measured by applying vibration from the surface of the thicker laminated glass member. The range of the FRF value of the laminated glass can be set by appropriately selecting the upper and lower limits.
[0326] The method for producing the laminated glass is not particularly limited. The laminated glass can be produced, for example, as follows. First, an interlayer film is sandwiched between the first laminated glass member and the second laminated glass member to obtain a laminate. Next, the air remaining between the first laminated glass member, the second laminated glass member, and the interlayer film is removed, for example, by passing the obtained laminate through a pressure roll or placing it in a rubber bag and suctioning it under reduced pressure. Thereafter, a pre-bonded laminate is obtained by pre-bonding at about 70°C to 110°C. Next, the pre-bonded laminate is placed in an autoclave or pressed at about 120°C to 150°C and a pressure of 1 MPa to 1.5 MPa. In this manner, a laminated glass can be obtained.
[0327] The interlayer film and the laminated glass can be used in automobiles, railway vehicles, aircraft, ships, buildings, etc. The interlayer film and the laminated glass can also be used for applications other than these. The interlayer film and the laminated glass are preferably interlayer films and laminated glass for vehicles or buildings, and more preferably interlayer films and laminated glass for vehicles. The interlayer film and the laminated glass can be used for automobile windshields, side windows, rear windows, roof glass, backlight glass, etc. The interlayer film and the laminated glass are preferably used in automobiles. The interlayer film is preferably used to obtain laminated glass for automobiles.
[0328] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0329] The polyvinyl acetal resin used was acetalized using n-butylaldehyde having a carbon number of 4. The degree of acetalization (degree of butyralization), degree of acetylation, and hydroxyl group content of the polyvinyl acetal resin were measured by a method conforming to JIS K6728 "Testing Methods for Polyvinyl Butyral." Note that when measured by ASTM D1396-92, the values shown were similar to those obtained by the method conforming to JIS K6728 "Testing Methods for Polyvinyl Butyral."
[0330] The following materials were prepared:
[0331] (Resins) PVB1: Polyvinyl acetal resin (polyvinyl butyral resin), average degree of polymerization 1700, hydroxyl group content 30 mol%, acetylation degree 0.7 mol%, acetalization degree (butyralization degree) 69.3 mol% PVB2: Polyvinyl acetal resin (polyvinyl butyral resin), average degree of polymerization 3000, hydroxyl group content 24 mol%, acetylation degree 12 mol%, acetalization degree (butyralization degree) 64 mol% PVB3: Polyvinyl acetal resin (polyvinyl butyral resin), average degree of polymerization 3300, hydroxyl group content 23.5 mol%, acetylation degree 18.5 mol%, acetalization degree (butyralization degree) 58 mol%
[0332] (Plasticizer) 3GO: Triethylene glycol di-2-ethylhexanoate
[0333] (Metal salt) Mg mixture (a 50:50 (weight ratio) mixture of magnesium 2-ethylbutyrate and magnesium acetate)
[0334] (UV Screening Agent) Tinuvin 326: 2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole ("Tinuvin 326" manufactured by BASF)
[0335] (Antioxidant) BHT: 2,6-di-t-butyl-p-cresol
[0336] Example 1 Preparation of resin composition for forming first layer: The following components were blended and thoroughly kneaded with a mixing roll to obtain a resin composition for forming the first layer.
[0337] PVB3: 100 parts by weight; 3GO: 60 parts by weight; Mg mixture: an amount that results in a magnesium content of 70 ppm in the resulting first layer; Tinuvin 326: an amount that results in a magnesium content of 0.2% by weight in the resulting first layer; BHT: an amount that results in a magnesium content of 0.2% by weight in the resulting first layer.
[0338] Preparation of resin composition for forming second layer and third layer: The following components were blended and thoroughly kneaded with a mixing roll to obtain a resin composition for forming the second layer and the third layer.
[0339] PVB1: 100 parts by weight; 3GO: 32.5 parts by weight; Mg mixture: an amount that results in a magnesium content of 70 ppm in the second and third layers; Tinuvin 326: an amount that results in a magnesium content of 0.2% by weight in the second and third layers; BHT: an amount that results in a magnesium content of 0.2% by weight in the second and third layers.
[0340] Preparation of Interlayer Film: The resin composition for forming the first layer and the resin compositions for forming the second and third layers were co-extruded using a co-extruder to obtain an interlayer film before cutting. The co-extrusion conditions were set to ensure that the first, second, and third layers each had a uniform thickness. The interlayer film before cutting was then cut using a score cutter at a position 25 mm inward from one end in the TD direction and a position 25 mm inward from the other end in the TD direction. In this way, a rectangular interlayer film (760 μm thick) having a first end and a second end and a three-layer structure (second layer / first layer / third layer) was obtained. The first end and the second end are opposite ends of the interlayer film in the TD direction, and the distance between the first end and the second end is 1092 mm.
[0341] In the table, "Cutting position (1)" is the distance from one end of the interlayer film in the TD direction to the cutting position. Also, "Cutting position (2)" in the table is the distance from the other end of the interlayer film in the TD direction to the cutting position.
[0342] Preparation of laminated glass: The obtained interlayer film was sandwiched between two sheets of green glass 2.0 mm thick, 50 cm wide, and 40 cm long, conforming to JIS R3208, to obtain a laminate. The obtained laminate was placed in a rubber bag and degassed at a vacuum of 0.08 MPa for 20 minutes, and then transferred to an oven in the degassed state and held at 90°C for a further 30 minutes for vacuum pressing to pre-bond the laminate. The pre-bonded laminate was then pressed in an autoclave at 140°C and a pressure of 1.3 MPa for 20 minutes to obtain laminated glass.
[0343] (Examples 2 to 6 and Comparative Examples 1 and 2) Rectangular interlayer films (760 μm thick) having a first end and a second end and a three-layer structure (second layer / first layer / third layer) were obtained in the same manner as in Example 1, except that the type of resin, the amount of plasticizer, and the cutting position of the interlayer film before cutting were changed as shown in the table. In the table, cutting positions (1) and (2) of 0 mm indicate that no cutting was performed. The metal salts, ultraviolet ray blocking agents, and antioxidants were used in the same types and amounts as in Example 1. Laminated glass was also obtained in the same manner as in Example 1.
[0344] Example 7 Preparation of resin composition for forming first layer: The following components were blended and thoroughly kneaded with a mixing roll to obtain a resin composition for forming the first layer.
[0345] PVB3: 100 parts by weight; 3GO: 60 parts by weight; Mg mixture: an amount that results in a magnesium content of 70 ppm in the resulting first layer; Tinuvin 326: an amount that results in a magnesium content of 0.2% by weight in the resulting first layer; BHT: an amount that results in a magnesium content of 0.2% by weight in the resulting first layer.
[0346] Preparation of resin composition for forming second layer and third layer: The following components were blended and thoroughly kneaded with a mixing roll to obtain a resin composition for forming the second layer and the third layer.
[0347] PVB1: 100 parts by weight; 3GO: 32.5 parts by weight; Mg mixture: an amount that results in a magnesium content of 70 ppm in the second and third layers; Tinuvin 326: an amount that results in a magnesium content of 0.2% by weight in the second and third layers; BHT: an amount that results in a magnesium content of 0.2% by weight in the second and third layers.
[0348] Preparation of Interlayer Film: The resin composition for forming the first layer and the resin compositions for forming the second and third layers were co-extruded using a co-extruder to obtain an interlayer film before cutting. The co-extrusion conditions were designed to ensure that the first layer had a uniform thickness, and that the thickness of each of the second and third layers increased from one end to the other in the TD direction. The interlayer film before cutting was then cut using a score cutter at a position 25 mm inward from one end in the TD direction and a position 25 mm inward from the other end in the TD direction. In this way, a wedge-shaped interlayer film having a first end and a second end and a three-layer structure (second layer / first layer / third layer) was obtained. The first end and the second end are opposite ends of the interlayer film in the TD direction, and the distance between the first end and the second end was 1092 mm.
[0349] Preparation of Laminated Glass: Laminated glass was obtained in the same manner as in Example 1 using the obtained interlayer film.
[0350] Examples 8 and 9 and Comparative Example 3 Wedge-shaped interlayer films having a first end and a second end and a three-layer structure (second layer / first layer / third layer) were obtained in the same manner as in Example 7, except that the type of resin, the amount of plasticizer, and the cutting position of the interlayer film before cutting were changed as shown in the table. In the table, cutting positions (1) and (2) of 0 mm mean that no cutting was performed. The metal salts, ultraviolet ray blocking agents, and antioxidants used were the same types and in the same amounts as in Example 7. Laminated glass was also obtained in the same manner as in Example 7.
[0351] (Examples 10 and 11) Preparation of laminated glass: Laminated glass was obtained in the same manner as in Example 1, except that the interlayer film obtained in Example 3 was used and two sheets of green glass having the thicknesses shown in the table below were used.
[0352] (Evaluation) (1) Viscoelasticity Measurement (Glass Transition Temperature and Tan δ at Glass Transition Temperature) The obtained interlayer was sandwiched between two 100 μm thick polyethylene terephthalate films (PET film, "Lumirror H10" manufactured by Toray Industries, Inc.) to obtain a laminate. The obtained laminate was sandwiched between two 2.0 mm thick green glass sheets, placed in a rubber bag, and degassed for 20 minutes at a vacuum of 0.08 MPa. After degassing, the degassed product was transferred to an oven and further held at 90°C for 30 minutes to vacuum press the laminate to pre-press the laminate. After pre-pressing, the laminate was pressed in an autoclave at 140°C and a pressure of 1.3 MPa for 20 minutes to obtain a test specimen. The obtained test specimen was stored for 4 weeks in an environment of 23±2°C and 25±5% humidity. After storage, the green glass and PET film were peeled off, and the viscoelasticity was measured using an "ARES-G2" viscoelasticity measuring device manufactured by TA Instruments. Using a parallel plate with a diameter of 8 mm as a jig, measurements were performed in shear mode under conditions of decreasing the temperature from 100°C to -20°C at a rate of 3°C / min, a frequency of 1 Hz, and a strain of 1%. In the measurement results obtained, the peak temperature of the loss tangent was defined as the glass transition temperature Tg (°C), and the value of the loss tangent at the glass transition temperature was defined as tan δ at the glass transition temperature.
[0353] (2) Thickness The thickness of the obtained interlayer film was measured as follows.
[0354] (a) Thickness at the first end (b) Thickness at the second end (c) Thickness of the layer (first layer) having the lowest glass transition temperature at a position 12.5 mm from the first end toward the second end (d) Thickness of the interlayer film at a position 12.5 mm from the first end toward the second end (e) Thickness of the layer (first layer) having the lowest glass transition temperature at a position 112.5 mm from the first end toward the second end (f) Thickness of the interlayer film at a position 112.5 mm from the first end toward the second end (g) Thickness of the layer (first layer) having the lowest glass transition temperature at a position 12.5 mm from the second end toward the first end (h) Thickness of the interlayer film at a position 12.5 mm from the second end toward the first end (i) Thickness of the layer (first layer) having the lowest glass transition temperature at a position 112.5 mm from the second end toward the first end (j) Thickness of the interlayer at a position 112.5 mm from the second end toward the first end
[0355] Furthermore, the following thickness ratios were calculated from the thicknesses (c) to (j) above.
[0356] Ratio (T P ): Ratio of thickness (c) to thickness (d) (thickness (c) / thickness (d)) Ratio (T Q ): Ratio of thickness (e) to thickness (f) (thickness (e) / thickness (f)) Ratio (T R ): Ratio of thickness (g) to thickness (h) (thickness (g) / thickness (h)) Ratio (T S ): Ratio of thickness (i) to thickness (j) (thickness (i) / thickness (j))
[0357] In addition, the calculated ratio (T P ), ratio (T Q ), ratio (T R ) and the ratio (T S ) and the rate of change C1 and the rate of change C2 were calculated according to the above-mentioned formulas (C1) and (C2).
[0358] (3) Secondary Loss Factor and Secondary Resonance Frequency of Laminated Glass The obtained interlayer film was cut out at predetermined positions to obtain an interlayer film for producing laminated glass P, an interlayer film for producing laminated glass Q, an interlayer film for producing laminated glass R, and an interlayer film for producing laminated glass S. The cut interlayer film was sandwiched between two 2.0 mm thick green glass sheets (25 mm x 300 mm) conforming to JIS R3208 to obtain a laminate. The obtained laminate was placed in a rubber bag and degassed at a vacuum of 0.08 MPa for 20 minutes. The degassed laminate was then transferred to an oven and held at 90°C for 30 minutes to perform vacuum pressing, thereby pre-pressing the laminate. The pre-pressed laminate was then pressed in an autoclave at 140°C and a pressure of 1.3 MPa for 20 minutes to obtain the following laminated glasses P, Q, R, and S.
[0359] Laminated glass P: A laminated glass obtained by placing the portion of the interlayer film extending from the first end toward the second end, from the 0 mm position to the 25 mm position, between two sheets of green glass having a thickness of 2.0 mm.
[0360] Laminated glass Q: A laminated glass obtained by placing the portion of the interlayer film extending from the first end toward the second end, from a position 100 mm to a position 125 mm, between two sheets of green glass having a thickness of 2.0 mm.
[0361] Laminated glass R: A laminated glass obtained by placing the portion of the interlayer film extending from the second end portion toward the first end portion, from the position of 0 mm to the position of 25 mm, between two sheets of green glass having a thickness of 2.0 mm.
[0362] Laminated glass S: A laminated glass obtained by placing the portion of the interlayer film extending from the second end toward the first end, from a position 100 mm to a position 125 mm, between two sheets of green glass having a thickness of 2.0 mm.
[0363] The secondary loss factor and secondary resonance frequency of the obtained laminated glasses P, Q, R, and S were measured as follows.
[0364] The laminated glasses P, Q, R, and S were stored for 4 weeks in an environment with a temperature of 23±2°C and a humidity of 25±5%. After storage, the laminated glasses P, Q, R, and S were vibrated in a thermostatic chamber at 20°C using a vibration generator for damping tests (Spectris's "Pertable Vibration Exciter Type 4809"). The obtained vibration characteristics were amplified using a mechanical impedance measuring device (Spectris's "75 VA Power Amplifier Type 2718"), and the vibration spectrum was subjected to FFT analysis to determine the secondary resonance frequency and secondary loss factor. The analysis software used was Spectris's "PULSE LabShop."
[0365] From the measurement results, the rates of change A1, A2, B1 and B2 were calculated according to the above-mentioned formulas (A1), (A2), (B1) and (B2).
[0366] (4) Vibration Damping in the High Frequency Range at the Edge Portion of Laminated Glass (FRF) Using the interlayer films obtained in Examples 1 to 11 and Comparative Examples 1 to 3, the vibration damping in the high frequency range at the edge portion of the laminated glass was measured by the following method.
[0367] (4-1) Preparation of Laminated Glass for Evaluation The obtained interlayer film was cut as follows to obtain interlayer films for evaluation 1 to 4. Note that the obtained interlayer film was cut out while being shifted slightly in the MD direction to obtain interlayer films for evaluation 1 to 4.
[0368] Evaluation interlayer film 1: An evaluation interlayer film having a size of 50 cm width (TD direction) x 40 cm length (MD direction), which is the interlayer film portion from the 0 mm position to the 500 mm position from the first end of the interlayer film toward the second end.
[0369] Evaluation interlayer film 2: An evaluation interlayer film having a size of 50 cm width (TD direction) x 40 cm length (MD direction), which is the interlayer film portion extending from the first end of the interlayer film to the position 100 mm to 600 mm from the first end toward the second end of the interlayer film.
[0370] Evaluation interlayer film 3: An evaluation interlayer film having a size of 50 cm width (TD direction) x 40 cm length (MD direction), which is the interlayer film portion from the second end of the interlayer film to the position of 0 mm to 500 mm toward the first end.
[0371] Evaluation interlayer film 4: An evaluation interlayer film having a size of 50 cm wide (TD direction) x 40 cm long (MD direction), which is the interlayer film portion from the second end of the interlayer film to a position 100 mm to 600 mm from the first end.
[0372] The obtained evaluation interlayer films 1 to 4 were sandwiched between two sheets of green glass conforming to JIS R3208, measuring 2.0 mm thick, 50 cm wide, and 40 cm long, to obtain a laminate. The obtained laminate was placed in a rubber bag and degassed at a vacuum of 0.08 MPa for 20 minutes. The degassed laminate was then transferred to an oven and vacuum-pressed at 90°C for 30 minutes to pre-bond the laminate. The pre-bonded laminate was then compressed in an autoclave at 140°C and a pressure of 1.3 MPa for 20 minutes to produce evaluation laminated glasses 1 to 4 corresponding to the evaluation interlayer films 1 to 4, respectively. However, in Examples 10 and 11, evaluation laminated glasses 1 to 4 were produced under the above-described conditions using two sheets of green glass conforming to JIS R3208, measuring 50 cm wide and 40 cm long, and having the thicknesses shown in Table 10 below.
[0373] (4-2) Measurement of Frequency Response Function (FRF) The horizontal direction of the obtained laminated glass for evaluation was defined as the x direction, and the vertical direction was defined as the y direction. The coordinates (x, y) of the four corners of the laminated glass for evaluation were defined as coordinates (0, 0), coordinates (0, 40), coordinates (50, 0), and coordinates (50, 40), respectively. The coordinates (x, y) were located x cm horizontally and y cm vertically from the coordinate (0, 0). The area between the coordinates (0, 0) and coordinates (0, 40) was the edge of the laminated glass for evaluation. The position of coordinates (5, 5) was used as the acceleration pickup position, and an accelerometer for measuring acceleration was installed at the position of coordinates (5, 5). The position of coordinates (35, 5) was set as H1, and the position of coordinates (5, 35) was set as H10. An arc was set from H1 to H10 with the position of coordinates (5, 5) (acceleration pickup position) as the center, and H2 to H9 were set at equal intervals on the arc. H1 was used as the excitation point, and vibration was applied five times with an impact hammer. The FRF (response to excitation (F) (m / s 2 ) was arithmetically averaged to calculate the average FRF (H1) at H1. Similarly, the average FRF (H2) at H2, the average FRF (H3) at H3, ..., the average FRF (H10) at H10 was calculated. The average FRF (H1) to average FRF (H10) were arithmetically averaged to determine the average FRF (H1 to H10). The average FRF (H1 to H10) was averaged over a range of 1000 Hz to 3000 Hz and then converted to a dB value, which was used as the "FRF value of the evaluation laminated glass." Note that the "edge of the evaluation laminated glass" refers to the edge of the interlayer film on the first edge side in the evaluation laminated glasses 1 and 2, and refers to the edge of the interlayer film on the second edge side in the evaluation laminated glasses 3 and 4.
[0374] The laminated glass on which the accelerometer was installed was suspended by soft rubber and the measurements were performed in a free-free state. The analysis software used was "BKConnect" manufactured by Spectris. The accelerometer used was "352C68" manufactured by PCB PIEZOTRONICS. The impact hammer used was "086C01" (aluminum head) manufactured by PCB PIEZOTRONICS.
[0375] The absolute value of the difference between the FRF value of evaluation laminated glass 1 and the FRF value of evaluation laminated glass 2, and the absolute value of the difference between the FRF value of evaluation laminated glass 3 and the FRF value of evaluation laminated glass 4 were calculated, and the vibration damping properties (FRF) in the high frequency range at the edge portions of the laminated glasses were evaluated according to the following criteria.
[0376] [Evaluation criteria for vibration damping in the high frequency range (FRF) at the edge portion of laminated glass] ∘: The absolute value of the difference is less than 0.7; ×: The absolute value of the difference is 0.7 or more.
[0377] (5) Measurement of frequency response function (FRF) at the center of laminated glass Using the interlayer films obtained in Examples 3, 10, and 11, the frequency response function (FRF) at the center of the laminated glass corresponding to the center of the interlayer film was measured by the following method.
[0378] (5-1) Preparation of Laminated Glass for Evaluation An interlayer film for evaluation was obtained, which was the interlayer film portion from the following first position to the following second position of the interlayer film, having a size of 50 cm width (TD direction) × 40 cm length (MD direction).
[0379] First position: 25 cm from the center of the interlayer in the TD direction toward the first end. Second position: 25 cm from the center of the interlayer in the TD direction toward the second end.
[0380] The obtained evaluation interlayer film was sandwiched between two sheets of green glass conforming to JIS R3208, measuring 50 cm wide and 40 cm long, and having the thickness shown in Table 10 below, to obtain a laminate. The obtained laminate was placed in a rubber bag and degassed at a vacuum of 0.08 MPa for 20 minutes, and then transferred to an oven in the degassed state, where it was further vacuum-pressed at 90°C for 30 minutes to pre-bond the laminate. The pre-bonded laminate was then compressed in an autoclave for 20 minutes under conditions of 140°C and a pressure of 1.3 MPa, to produce an evaluation laminated glass corresponding to the evaluation interlayer film.
[0381] (5-2) Measurement of Frequency Response Function (FRF) The FRF value of the evaluation laminated glass was determined in the same manner as in the above-mentioned "(4-2) Measurement of Frequency Response Function (FRF)".
[0382] The interlayer structure and results are shown in Tables 1 to 10 below.
[0383]
[0384]
[0385]
[0386]
[0387]
[0388]
[0389]
[0390]
[0391]
[0392]
[0393] DESCRIPTION OF SYMBOLS 1, 1A... First layer 1a, 1Aa... First surface 1b, 1Ab... Second surface 2, 2A... Second layer 3, 3A... Third layer 11, 11A... Interlayer 11a... First end 11b... Second end 21, 21A... First laminated glass member 22, 22A... Second laminated glass member 31, 31A... Laminated glass 31a... First end 31b... Second end P... Portion from the first end to the second end, from 0 mm to 25 mm Q... Portion from the first end to the second end, from 100 mm to 125 mm R... Portion from the second end to the first end, from 0 mm to 25 mm S... Portion from the second end to the first end, from 100 mm to 125 mm
Claims
1. An interlayer film for laminated glass, the interlayer film having a first end and a second end opposite the first end, wherein when a laminated glass P is obtained by disposing a portion of the interlayer film from a position of 0 mm to a position of 25 mm from the first end toward the second end between two pieces of green glass having a thickness of 2.0 mm, a laminated glass Q is obtained by disposing a portion of the interlayer film from a position of 100 mm to a position of 125 mm from the first end toward the second end between two pieces of green glass having a thickness of 2.0 mm, a laminated glass R is obtained by disposing a portion of the interlayer film from a position of 0 mm to a position of 25 mm from the second end toward the first end between two pieces of green glass having a thickness of 2.0 mm, and a laminated glass S is obtained by disposing a portion of the interlayer film from a position of 100 mm to a position of 125 mm from the second end toward the first end between two pieces of green glass having a thickness of 2.0 mm, the following configuration A or the following configuration B is satisfied. Configuration A: The rate of change A1 represented by the following formula (A1) is less than 10%, and the rate of change A2 represented by the following formula (A2) is less than 10%. Rate of change A1 (%) = (|P A -Q A | / Q A )×100...(A1) P A Q: Secondary loss coefficient of the laminated glass P A : Secondary loss coefficient change rate A2 (%) of the laminated glass Q = (|R A -S A | / S A )×100...(A2) R A : Secondary loss coefficient of the laminated glass R S A : Secondary loss coefficient of the laminated glass S. Configuration B: The rate of change B1 represented by the following formula (B1) is less than 10%, and the rate of change B2 represented by the following formula (B2) is less than 10%. Rate of change B1 (%) = (|P B -Q B | / Q B )×100...(B1) P B : Secondary resonance frequency of the laminated glass P Q B : The rate of change in the secondary resonance frequency of the laminated glass Q B2 (%) = (|R B -S B | / S B )×100...(B2) R B : Secondary resonance frequency of the laminated glass R S B : Secondary resonance frequency of the laminated glass S 2. The interlayer film for laminated glass according to claim 1, wherein said configuration A is satisfied.
3. The interlayer film for laminated glass according to claim 1, wherein said configuration B is satisfied.
4. The interlayer film for laminated glass according to claim 1, wherein the configuration A and the configuration B are satisfied.
5. The interlayer film for laminated glass according to any one of claims 1 to 4, comprising a first layer containing a resin and a second layer containing a resin, the second layer being disposed on the first surface side of the first layer.
6. The interlayer film for laminated glass according to claim 5, wherein the resin in the first layer is a thermoplastic resin, and the resin in the second layer is a thermoplastic resin.
7. The interlayer film for laminated glass according to claim 5 or 6, further comprising a third layer containing a resin, the third layer being disposed on a second surface side opposite to the first surface side of the first layer.
8. The interlayer film for laminated glass according to claim 7, wherein the resin in the third layer is a thermoplastic resin.
9. The interlayer film for laminated glass according to any one of claims 5 to 8, wherein the first layer and the second layer have different glass transition temperatures.
10. The interlayer film for laminated glass according to any one of claims 5 to 9, wherein the layer having the highest glass transition temperature has a glass transition temperature of 32°C or higher.
11. The interlayer film for laminated glass according to claim 10, wherein the layer having the highest glass transition temperature has a glass transition temperature of 37° C. or higher.
12. The interlayer film for laminated glass according to any one of claims 5 to 11, wherein the second layer is a surface layer of the interlayer film, and the second layer is a layer having the highest glass transition temperature.
13. The interlayer film for laminated glass according to any one of claims 5 to 12, wherein the layer having the lowest glass transition temperature has a tan δ of 1.2 or more at the glass transition temperature.
14. The interlayer film for laminated glass according to claim 13, wherein tan δ at the glass transition temperature of the layer with the lowest glass transition temperature is 1.4 or more.
15. The interlayer film for laminated glass according to any one of claims 5 to 14, wherein the first layer is the layer having the lowest glass transition temperature.
16. The interlayer film for laminated glass according to any one of claims 5 to 15, wherein the end face of the first end portion has an end face of the layer having the lowest glass transition temperature, and the end face of the second end portion has an end face of the layer having the lowest glass transition temperature.
17. The interlayer film for laminated glass according to any one of claims 5 to 16, which satisfies the following configuration C. Configuration C: The rate of change C1 represented by the following formula (C1) is greater than 0% and less than or equal to 50%, and the rate of change C2 represented by the following formula (C2) is greater than 0% and less than or equal to 50%. Rate of change C1 (%) = (|T P -T Q | / T Q )×100...(C1) T P : The ratio of the thickness of the layer having the lowest glass transition temperature at a position 12.5 mm from the first end toward the second end to the thickness of the interlayer at a position 12.5 mm from the first end toward the second end T Q : The ratio of the thickness of the layer having the lowest glass transition temperature at a position 112.5 mm from the first end toward the second end to the thickness of the interlayer at a position 112.5 mm from the first end toward the second end. Change rate C2 (%) = (| T R -T S | / T S )×100...(C2) T R : The ratio of the thickness of the layer having the lowest glass transition temperature at a position 12.5 mm from the second end toward the first end to the thickness of the interlayer at a position 12.5 mm from the second end toward the first end, T S : The ratio of the thickness of the layer having the lowest glass transition temperature at a position 112.5 mm from the second end toward the first end to the thickness of the interlayer at a position 112.5 mm from the second end toward the first end 18. The interlayer film for laminated glass according to any one of claims 1 to 17, comprising a resin and a plasticizer, the content of the plasticizer contained in the interlayer film being 36 parts by weight or less per 100 parts by weight of the resin contained in the interlayer film.
19. The interlayer film for laminated glass according to any one of claims 1 to 18, wherein the cross-sectional shape of the interlayer film in the thickness direction is wedge-shaped.
20. A laminated glass comprising: a first laminated glass component; a second laminated glass component; and the interlayer film for laminated glass according to any one of claims 1 to 19, wherein the interlayer film for laminated glass is disposed between the first laminated glass component and the second laminated glass component.
21. A laminated glass having a first end and a second end opposite the first end, wherein the following configuration A' or the following configuration B' is satisfied. Configuration A': The rate of change A3 represented by the following formula (A3) is less than 10%, and the rate of change A4 represented by the following formula (A4) is less than 10%. Rate of change A3 (%) = (|P A '-Q A '| / Q A ')×100...(A3) P A Q′: secondary loss coefficient of the laminated glass in a portion of the laminated glass from the position of 0 mm to the position of 25 mm from the first end toward the second end A ': rate of change A4 (%) of the secondary loss coefficient of the laminated glass in the portion of the laminated glass from the position of 100 mm to the position of 125 mm from the first end toward the second end A '-S A '| / S A ')×100...(A4) R A ': secondary loss coefficient S of the laminated glass in a portion of the laminated glass from the position of 0 mm to the position of 25 mm from the second end toward the first end A Configuration B′: Secondary loss coefficient of the laminated glass in a portion of the laminated glass from a position of 100 mm to a position of 125 mm from the second end toward the first end. Configuration B′: A rate of change B3 represented by the following formula (B3) is less than 10%, and a rate of change B4 represented by the following formula (B4) is less than 10%. Rate of change B3 (%)=(|P B '-Q B '| / Q B ')×100...(B3) P B Q′: the secondary resonance frequency of the laminated glass in a portion of the laminated glass from the position of 0 mm to the position of 25 mm from the first end toward the second end B ': rate of change B4 (%) of secondary resonance frequency of the laminated glass in a portion of the laminated glass from a position of 100 mm to a position of 125 mm from the first end toward the second end = (|R B '-S B '| / S B ')×100...(B4) R B ': the secondary resonance frequency S of the laminated glass in a portion of the laminated glass from the position of 0 mm to the position of 25 mm from the second end toward the first end B ': secondary resonance frequency of the laminated glass in a portion of the laminated glass from a position 100 mm to a position 125 mm from the second end toward the first end
Citation Information
Patent Citations
Viscoelastic plastic interlayer for vibroacoustic damping and glazing unit comprising such an interlayer
WO2013175101A1
Cut interlayer film for laminated glass
JP1985021834A
JP1988195551U
Polyvinyl acetal-based resin film, and multilayer structure
JP2013091793A
Interlayer film for laminated glass, and laminated glass
WO2016125896A1