Gas absorbent-supporting porous substrate

A porous base material with macropores and mesopores, loaded with an amine compound and polyether composition, enhances carbon dioxide absorption and desorption efficiency, addressing the limitations of existing materials by maintaining high fluidity and amine compound efficiency.

WO2024204666A1PCT designated stage expired Publication Date: 2024-10-03MITSUI MINING & SMELTING CO LTD

Patent Information

Application Number
PCT/JP2024/012943
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing carbon dioxide absorbent materials using porous substrates with mesopores have limited amine compound loading, resulting in low carbon dioxide absorption capacity and slow gas desorption at low temperatures, requiring thermal energy for efficient desorption.

Method used

A porous base material with both macropores and mesopores, supporting a gas absorbent composition containing an amine compound and a polyether, which enhances gas absorption capacity and desorption rate by maintaining high fluidity and increasing the amine compound's efficiency.

Benefits of technology

The proposed solution significantly increases the carbon dioxide absorption capacity and desorption rate, reducing the thermal energy required for gas desorption and improving the overall efficiency of the gas absorbent material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012943_03102024_PF_FP_ABST
    Figure JP2024012943_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a gas absorbent-supporting porous substrate comprising: a porous substrate having at least macropores; and a gas absorbent supported in at least some pores in the porous substrate. The gas absorbent is a composition containing an amine compound and a polyether. When the pore volume of mesopores in the porous substrate is Vs and the pore volume of mesopores in the gas absorbent-supporting porous substrate is Vsa, the ratio of Vsa to Vs, i.e., Vsa / Vs, is 0.60 or less. When the pore volume of the macropores in the porous substrate is Vm and the pore volume of macropores in the gas absorbent-supporting porous substrate is Vma, the ratio of Vma to Vm, i.e., Vma / Vm, is 0.50 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Gas absorbent-supporting porous substrate

[0001] The present invention relates to a gas absorbent-supporting porous substrate, and also to an acid gas absorbent and a carbon dioxide absorbent each comprising a gas absorbent-supporting porous substrate.

[0002] In recent years, with the growing awareness of environmental issues, carbon dioxide, NO and NO contained in exhaust gases have become increasingly 2 Nitrogen oxides such as SO and SO 2 The emission of sulfur oxides such as carbon dioxide is becoming a problem. For example, carbon dioxide separation and capture technology, which is one of the causes of global warming, has attracted attention, and studies are underway to separate and capture carbon dioxide emitted from thermal power plants and steelworks. One known carbon dioxide separation and capture technology is a method that uses a carbon dioxide absorbent in which an amine compound is supported on a porous material.

[0003] For example, Patent Document 1 describes an amino compound-supported porous substrate for adsorbing carbon dioxide, in which a porous substrate having mesopores is exposed to an atmosphere in which the amino compound is in a gaseous state, thereby supporting the amino compound inside the mesopores.

[0004] JP 2015-113337 A

[0005] However, carbon dioxide absorbents using porous substrates, particularly those using porous substrates having mesopores, have the problem that the amount of amine compound that contributes to the carbon dioxide absorption capacity is small relative to the total amount of amine compound supported, from the viewpoint of the diffusibility and flowability of the gas to be passed through.Furthermore, there is also the problem that the rate at which the absorbed gas is desorbed at low temperatures is slow, and therefore, heat costs are required for efficient desorption.

[0006] Therefore, an object of the present invention is to provide a gas absorbent-supporting porous substrate that can overcome the various drawbacks of the prior art described above.

[0007] The present invention provides a gas absorbent-supported porous substrate comprising: a porous substrate having at least macropores and mesopores; and a gas absorbent supported in at least some of the pores of the porous substrate, wherein the gas absorbent is a composition containing an amine compound and a polyether; and wherein Vs is the pore volume per unit volume of the porous substrate of mesopores in the porous substrate measured by mercury porosimetry in a pore diameter range of more than 2.0 nm and less than 50 nm; and Vsa is the pore volume per unit volume of the gas absorbent-supported porous substrate of mesopores in the gas absorbent-supported porous substrate measured by mercury porosimetry in a pore diameter range of more than 2.0 nm and less than 50 nm; the ratio Vsa / Vs of Vsa to Vs is 0.60 or less; and Vm is the pore volume per unit volume of the porous substrate of macropores in the porous substrate measured by mercury porosimetry in a pore diameter range of 50 nm or more and 10 μm or less; The present invention provides a gas absorbent-supported porous substrate in which, when Vma is the pore volume of macropores in the gas absorbent-supported porous substrate per unit volume of the gas absorbent-supported porous substrate as measured by mercury intrusion porosimetry in a pore diameter range of 50 nm to 10 μm, the ratio Vma / Vm of Vma to Vm is 0.50 or more.

[0008] FIG. 1 is a schematic diagram showing an enlarged view of a main part of a porous substrate used in the present invention.

[0009] The present invention will be described below with reference to the drawings based on preferred embodiments thereof. The present invention relates to a porous substrate supported on a gas absorbent. In the present invention, the gas absorbent is supported on at least a portion of the pores of the porous substrate. Porous substrates supported on an amine compound as a gas absorbent are conventionally known, but one of the features of the gas absorbent-supported porous substrate of the present invention is the use of a composition containing an amine compound and a polyether (hereinafter also referred to as a "gas absorbing composition") as the gas absorbent. By using such a gas absorbent, when the gas absorbent-supported porous substrate of the present invention absorbs a gas, the polyether can dissolve or disperse the compound produced by the reaction between the gas and the amine compound. Due to this, the fluidity of the gas absorbent supported on the porous substrate can be maintained high after gas absorption, so that the amine compound supported on the porous substrate can react efficiently with the gas, thereby increasing the gas absorption amount of the gas absorbent-supported porous substrate. Furthermore, because the fluidity of the gas absorbent supported in the porous substrate is maintained high even after gas absorption, the desorption rate of the gas absorbed by the porous substrate can be increased.

[0010] The amine compound contained in the gas absorbing composition has a chemical structure containing a primary amino group (-NH 2 ), secondary amino group (-NHR 5 ), tertiary amino group (—NR 5 R 6 ), quaternary ammonium group (-N + R 5 R 6 R 7 ) can be used without any particular limitation. 5 , R 6 and R 7are each independently, for example, a substituted or unsubstituted alkyl group, a substituted or unsubstituted aryl group, or the like. The alkyl group is, for example, an alkyl group having 1 to 10 carbon atoms. The alkyl group may be linear or branched. The aryl group is, for example, a monocyclic, bicyclic, or tricyclic aromatic hydrocarbon ring group having 6 to 14 carbon atoms. Examples of the aryl group include a phenyl group and a naphthyl group. Examples of substituents that the alkyl group or aryl group may have include a hydroxyl group and a halogen atom. The halogen atom is selected from a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. The amine compound may be, for example, a monoamine-type amine compound having one amino group per molecule of the amine compound, or a polyamine-type amine compound having two or more amino groups per molecule of the amine compound.

[0011] The amine compound may be, for example, a low molecular weight compound or a polymer compound. Examples of the low molecular weight compound include aliphatic amines and aromatic amines. Examples of the aliphatic amine include chain aliphatic amines and cyclic aliphatic amines, such as ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, bis(2-hydroxypropyl)amine, N,N'-bis(2-hydroxyethyl)ethylenediamine, monoethanolamine, diethanolamine, diisopropanolamine, methylamine, dimethylamine, diethylamine, methyldiethanolamine, methylethanolamine, piperidine, piperazine, and 2-aminoethylpiperazine. Examples of the aromatic amine include 2-picolylamine, aniline, and m-xylenediamine. Examples of the polymer compound include linear polyethyleneimine and branched polyethyleneimine. The weight average molecular weight of the polymer compound is preferably from 300 to 10,000, more preferably from 300 to 5,000, even more preferably from 300 to 3,000, and still more preferably from 300 to 1,000. These amine compounds may be used alone or in combination of two or more.

[0012] Among these amine compounds, it is preferable to use polyamines, primary amines, secondary amines, tertiary amines, quaternary ammonium, aromatic amines, and polyimines, because they can be easily supported on the porous substrate and have a high acid gas absorption capacity when the amine compound-supported porous substrate of the present invention is used, for example, as an acid gas absorbent.

[0013] In the gas absorbent-supported porous substrate of the present invention, the mass ratio of the amine compound to the mass of the porous substrate is preferably 0.15 or more. This allows the gas absorption amount of the gas absorbent-supported porous substrate to be sufficiently increased. From this perspective, the mass ratio of the amine compound to the mass of the porous substrate is more preferably 0.20 or more, and even more preferably 0.25 or more. Since the larger the amount of amine compound supported, the larger the gas absorption amount tends to be, there is no particular limitation on the upper limit of the mass ratio of the amine compound to the mass of the porous substrate. However, from the viewpoint of ensuring a sufficient amount of polyether supported on the porous substrate and from the viewpoint of sufficiently suppressing leakage of the amine compound from the porous substrate due to an excessive amount of amine compound, the mass ratio of the amine compound to the mass of the porous substrate is preferably 10 or less, more preferably 5.0 or less, even more preferably 2.0 or less, even more preferably 1.0 or less, even more preferably 0.9 or less, and particularly preferably 0.8 or less.

[0014] Next, the polyether contained in the gas absorbing composition will be described. As described above, the polyether dissolves or disperses the compound produced by the reaction of the gas with the amine compound, thereby enhancing the fluidity of the gas absorbent after gas absorption. In other words, in the gas absorbent-supported porous substrate of the present invention, the fluidity of the gas absorbent is high even after gas absorption, so that unreacted amine compounds circulate within the gas absorbent and easily move to the surface of the gas absorbent. As a result, the proportion of amino groups contributing to gas absorption among the amino groups possessed by the amine compound supported on the porous substrate (hereinafter also referred to as "amine efficiency") increases, resulting in a high gas absorption amount. Furthermore, due to the increased fluidity of the gas absorbent, the product of the reaction between the absorbed gas and the amine compound circulates within the gas absorbent and easily moves to the surface of the gas absorbent, thereby increasing the desorption rate of the absorbed gas. In order to make these effects more pronounced, it is preferable that the polyether and the amine compound are compatible, and it is more preferable that the polyether and the amine compound are compatible at the temperature at which the gas absorbent-supported porous substrate is subjected to gas adsorption and desorption. The temperature at which gas is adsorbed and desorbed is not particularly limited, and an appropriate temperature can be selected depending on the type of gas to be adsorbed and desorbed, the environment in which the gas is used, and the like.

[0015] In this specification, the amine efficiency is calculated by dividing the gas absorption amount of the gas absorbent-supported porous substrate by the theoretical value of the nitrogen atom content per unit mass of the gas absorbent-supported porous substrate (hereinafter also referred to as "theoretical nitrogen atom content").Specific measurement methods will be described in the examples below.

[0016] The polyether is preferably a polyether represented by the following formula (1) or (2): 1 -(O-A 1 ) n1 -OR 2 (1) R 1 O-(A 1 -O) n1 -R 3 -(O-A 2 ) n2 -OR 2 (2)

[0017] In formulas (1) and (2), A 1 and A 2 represents an alkylene group. 1 and R 2 R each independently represents a hydrogen atom or an alkyl group. 3 represents an alkylene group which may be substituted with X. X is *-(O-A 3 ) n3 -OR 4 Represents. A 3 represents an alkylene group. 4 represents a hydrogen atom or an alkyl group. * represents a bond. n1, n2, and n3 represent the number of repetitions.

[0018] In formulas (1) and (2), A 1 , A 2 and A 3 The alkylene groups represented by the formula (1) each independently have preferably 2 to 10 carbon atoms, more preferably 2 to 8 carbon atoms, and even more preferably 2 to 6 carbon atoms. Specific examples of such alkylene groups include an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a trimethylene group, and a tetramethylene group. 1 represents an ethylene group, and 1 , A 2 and A 3 Among polyethers in which A represents an ethylene group, those other than polyethylene glycol are also called "polyethylene glycol derivatives." 1 represents a propylene group, and 1 , A 2 and A 3 Among polyethers in which represents a propylene group, those other than polypropylene glycol are also called "polypropylene glycol derivatives."

[0019] In formulas (1) and (2), R 1 and R 2Examples of the alkyl group represented by the formula (I) include alkyl groups having 1 to 6 carbon atoms. Specific examples of such alkyl groups include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, and a 1-methylethyl group.

[0020] In formulas (1) and (2), R 3 The alkylene group represented by the formula (I) preferably has 2 or more and 10 or less carbon atoms, more preferably 2 or more and 6 or less carbon atoms, and even more preferably 2 or more and 4 or less carbon atoms. Specific examples of such alkylene groups include those represented by the formula (I) above. 1 , A 2 and A 3 Specific examples of alkylene groups represented by the following formulas can be given. 3 is preferably a trimethylene group. 3 The alkylene group represented by the formula (I) may be unsubstituted with X or may be substituted with one or more Xs.

[0021] In formulas (1) and (2), the repeat numbers represented by n1, n2, and n3 are each independently preferably 4 to 30, more preferably 4 to 20, and even more preferably 4 to 15. When the repeat number n is 4 or more, volatilization of the polyether can be sufficiently suppressed. Furthermore, by setting the repeat numbers n1, n2, and n3 to 30 or less, the fluidity of the polyether can be increased.

[0022] From the same viewpoint, the weight average molecular weight of the polyether is preferably 200 or more and 2,000 or less, more preferably 200 or more and 1,500 or less, and even more preferably 200 or more and 1,000 or less.

[0023] The polyether may be, for example, a diol type or a triol type. In this specification, a diol type polyether refers to a polyether having two hydroxyl groups. As a diol type polyether, for example, in the above formula (1), A 1 is an ethylene group, and R 1 and R 2Another example is polyethylene glycol in which A is a hydrogen atom. 1 is a propylene group, and R 1 and R 2 In this specification, the term "triol-type polyether" refers to a polyether having three hydroxyl groups. Examples of triol-type polyethers include polypropylene glycols in which R 3 is replaced by one X, and A 1 , A 2 and A 3 is a propylene group, and R 1 , R 2 and R 4 is a hydrogen atom.

[0024] From the viewpoints of compatibility with the amine compound and easy availability, it is preferable to use polyethylene glycol, polypropylene glycol, or a derivative thereof as the polyether, it is more preferable to use polyethylene glycol or a triol-type polypropylene glycol derivative, and it is particularly preferable to use polyethylene glycol.

[0025] The mass ratio of the polyether to the mass of the amine compound in the gas absorbing composition is preferably 0.05 or more and 10 or less, more preferably 0.10 or more and 5.00 or less, and even more preferably 0.50 or more and 3.00 or less.By setting the mass ratio of the polyether to the mass of the amine compound to 0.05 or more, the above-mentioned effect of the polyether can be more reliably obtained.In addition, by setting the mass ratio of the polyether to the mass of the amine compound to 10 or less, a sufficient amount of the amine compound can be supported on the porous substrate, so that the gas absorption amount of the gas absorbent-supported porous substrate of the present invention can be increased.

[0026] From the same viewpoint, the ratio of the mass of the polyether to the mass of the porous substrate is preferably 0.05 or more and 10 or less, more preferably 0.10 or more and 5.00 or less, even more preferably 0.10 or more and 2.00 or less, even more preferably 0.10 or more and 1.00 or less, and even more preferably 0.10 or more and 0.80 or less.

[0027] The ratio of the mass of the gas absorbent to the mass of the porous substrate is preferably 0.20 or more, more preferably 0.25 or more, and even more preferably 0.30 or more. It is preferable that the ratio of the total mass of the amine compound and polyether to the mass of the porous substrate is within the above-mentioned numerical range. By setting the ratio of the mass of the gas absorbent to the mass of the porous substrate to 0.20 or more, the gas absorption amount of the gas absorbent-supported porous substrate can be sufficiently increased. In addition, since the amount of gas absorbent supported tends to increase as the amount of gas absorbent increases, there is no upper limit for the ratio of the mass of the gas absorbent to the mass of the porous substrate. However, by setting the ratio of the mass of the gas absorbent to the mass of the porous substrate to 10 or less, leakage of the gas absorbent from the porous substrate due to an excessive amount of gas absorbent can be sufficiently suppressed. In addition, since a sufficient amount of voids can be secured in the porous substrate, the gas desorption rate can be increased. From this viewpoint, the ratio of the mass of the gas absorbent to the mass of the porous substrate is more preferably 5.0 or less, even more preferably 2.0 or less, even more preferably 1.8 or less, and particularly preferably 1.6 or less.

[0028] From the viewpoint of ensuring sufficient gas absorption, the nitrogen atom content of the gas absorbent-supported porous substrate is preferably 2.5% by mass or more and 30.0% by mass or less, more preferably 3.0% by mass or more and 30.0% by mass or less, even more preferably 4.0% by mass or more and 25.0% by mass or less, and even more preferably 4.5% by mass or more and 20.0% by mass or less. From the same viewpoint, the nitrogen atom content per unit mass of the gas absorbent-supported porous substrate contained in the gas absorbent-supported porous substrate of the present invention is preferably 2.1 mmol / g or more and 21.4 mmol / g or less, more preferably 2.9 mmol / g or more and 17.9 mmol / g or less, and even more preferably 3.2 mmol / g or more and 14.3 mmol / g or less. The nitrogen atom content and nitrogen atom content of the gas absorbent-supported porous substrate can be measured, for example, using an oxygen, nitrogen, and hydrogen analyzer ONH836 manufactured by LECO Japan LLC.

[0029] The gas absorbing composition used in the present invention may be used in combination with an antioxidant to increase its fluidity and make it easier to support inside the pores. Examples of antioxidants include ascorbic acid, hydroquinone, 3,5-dibutyl-4-hydroxytoluene, butylhydroxyanisole, and α-tocopherol. These additives may be added singly or in combination of two or more.

[0030] Next, the porous substrate used in the present invention (that is, the porous substrate in a state before supporting the gas absorbent) will be described. As the porous substrate, for example, the porous substrate described in WO 2022 / 163834 can be used. The porous substrate used in the present invention advantageously has at least macropores and mesopores. As a result, the gas absorbent-supported porous substrate of the present invention reliably ensures a gas passage, so that the gas absorption amount and gas desorption rate are high. Macropores in a porous substrate generally refer to pores having a pore diameter of 50 nm or more among the pores possessed by the porous substrate. The porous substrate used in the present invention has a controlled pore diameter distribution of the macropores possessed by the porous substrate. In detail, the porous substrate used in the present invention has a mode pore diameter Dm of macropores measured by mercury intrusion in a pore diameter range of 50 nm or more and 10 μm or less, preferably 0.05 μm or more and 3.0 μm or less. By setting the mode pore diameter Dm of the macropores within this range, the amine efficiency, gas absorption amount, and gas desorption rate of the gas absorbent-supported porous substrate used in the present invention can be further improved. From the viewpoint of making this advantage even more pronounced, the mode pore diameter Dm of the macropores of the porous substrate used in the present invention, measured by mercury intrusion porosimetry in a pore diameter range of 50 nm to 10 μm, is more preferably 0.07 μm to 2.0 μm, and even more preferably 0.10 μm to 1.5 μm.

[0031] The porous substrate used in the present invention preferably has a controlled pore volume of macropores. Specifically, the porous substrate used in the present invention has a pore volume Vm of the macropores of the porous substrate measured by mercury intrusion porosimetry in a pore diameter range of 50 nm to 10 μm, preferably 0.20 mL / mL to 0.70 mL / mL per unit volume of the porous substrate. By setting the pore volume of the macropores in this range, the porous substrate used in the present invention has a higher compressive strength when formed into a molded body. In addition, when a gas absorbent is supported on the porous substrate used in the present invention, it is possible to increase the amine efficiency, gas absorption amount, and gas desorption rate. From the viewpoint of making this advantage even more pronounced, the porous substrate used in the present invention has a pore volume Vm of macropores, measured by mercury intrusion porosimetry in a pore diameter range of 50 nm to 10 μm, per unit volume of the porous substrate, of more preferably 0.30 mL / mL to 0.65 mL / mL, and even more preferably 0.40 mL / mL to 0.60 mL / mL.

[0032] On the other hand, the pore volume Vma of the macropores in the gas absorbent-supported porous substrate of the present invention when the porous substrate supports the gas absorbent is preferably 0.10 mL / mL or more and 0.70 mL / mL or less, more preferably 0.15 mL / mL or more and 0.65 mL / mL or less, and even more preferably 0.20 mL / mL or more and 0.60 mL / mL or less per unit volume of the gas absorbent-supported porous substrate. By setting the pore volume Vma of the macropores in the gas absorbent-supported porous substrate within this range, it is possible to further improve both the gas absorption ability of the gas absorbent-supported porous substrate and the diffusibility of the gas to be circulated.

[0033] In the gas absorbent-supported porous substrate of the present invention, the ratio Vma / Vm of the pore volume Vma of the macropores of the gas absorbent-supported porous substrate per unit volume of the porous substrate to the pore volume Vm of the macropores of the porous substrate per unit volume of the porous substrate is 0.50 or more. This makes it possible to achieve both the gas absorption capacity and the diffusibility of the gas to be circulated, and also to increase the gas desorption rate. From this perspective, Vma / Vm is more preferably 0.60 or more, even more preferably 0.70 or more, and even more preferably 0.75 or more. Ideally, Vma / Vm is 1.00, but it may be, for example, 0.99 or less.

[0034] The porous substrate used in the present invention has mesopores in addition to the above-mentioned macropores. Mesopores generally refer to pores having a pore diameter of more than 2 nm and less than 50 nm among the pores of the porous substrate. The porous substrate used in the present invention has macropores and mesopores, which improves the gas absorption ability and the gas absorbent loading efficiency. In order to make this advantage more pronounced, the porous substrate used in the present invention has a mode pore diameter Ds of mesopores measured by mercury porosimetry in a pore diameter range of more than 2.0 nm and less than 50.0 nm, preferably more than 2.0 nm and less than 50.0 nm, more preferably 7.0 nm or more and 40.0 nm or less, more preferably 10.0 nm or more and 35.0 nm or less, and even more preferably 12.0 nm or more and 35.0 nm or less.

[0035] The porous substrate used in the present invention preferably has a controlled mesopore volume. Specifically, the porous substrate used in the present invention has a mesopore volume Vs measured by mercury intrusion porosimetry in a pore diameter range of more than 2.0 nm and less than 50 nm, which is preferably 0.05 mL / mL or more and 0.50 mL / mL or less per unit volume of the porous substrate. Due to the mesopore volume being in this range, the porous substrate used in the present invention has high compressive strength when molded. Furthermore, when a gas absorbent is supported on the porous substrate used in the present invention, it becomes a gas absorbent-supported porous substrate having high amine efficiency, gas absorption amount and gas desorption rate. From the viewpoint of making this advantage even more pronounced, the porous substrate used in the present invention preferably has a mesopore volume Vs, measured by mercury intrusion porosimetry in the pore diameter range of more than 2.0 nm and less than 50 nm, of 0.10 mL / mL or more and 0.40 mL / mL or less, even more preferably 0.10 mL / mL or more and 0.35 mL / mL or less, and even more preferably 0.10 mL / mL or more and 0.20 mL / mL or less.

[0036] On the other hand, in the gas absorbent-supported porous substrate of the present invention in a state in which the porous substrate supports a gas absorbent, the pore volume Vsa of the mesopores measured by mercury porosimetry in the range of pore diameters of more than 2.0 nm and less than 50 nm is, per unit volume of the gas absorbent-supported porous substrate, preferably 0.01 mL / mL or more and 0.30 mL / mL or less, more preferably 0.01 mL / mL or more and 0.25 mL / mL or less, even more preferably 0.01 mL / mL or more and 0.20 mL / mL or less, and even more preferably 0.01 mL / mL or more and 0.15 mL / mL or less. Due to the pore volume Vsa of the mesopores in the gas absorbent-supported porous substrate being in such a range, the gas absorbent-supported porous substrate can have both gas absorption ability and diffusibility of the gas to be circulated.

[0037] In the gas absorbent-supported porous substrate of the present invention, the ratio Vsa / Vs of the pore volume Vsa of the mesopores of the gas absorbent-supported porous substrate per unit volume of the porous substrate to the pore volume Vs of the mesopores of the porous substrate per unit volume of the porous substrate is 0.60 or less. This allows the gas absorption amount of the gas absorbent-supported porous substrate to be sufficiently increased. From this viewpoint, Vsa / Vs is more preferably 0.50 or less, even more preferably 0.45 or less, and even more preferably 0.20 or less. There is no particular restriction on the lower limit of Vsa / Vs, but from the viewpoint of achieving both gas absorption ability and diffusibility of the gas to be circulated, Vsa / Vs may be 0.02 or more, 0.03 or more, 0.04 or more, or 0.05 or more.

[0038] Vma / Vm and Vsa / Vs can be calculated by measuring the pore volume of the macropores and the pore volume of the mesopores of the gas absorbent-supported porous substrate and the porous substrate not supported with the gas absorbent. The gas absorbent supported on the porous substrate can be removed without deforming the skeletal structure of the porous substrate, for example, by firing at 600 ° C. or less in an air atmosphere. Therefore, it is preferable to measure the pore volume of the porous substrate not supported with the gas absorbent after firing the gas absorbent-supported porous substrate at 600 ° C. or less in an air atmosphere.

[0039] The pore volume per unit volume of the above-mentioned porous substrate and gas absorbent-supporting porous substrate can be calculated using the pore volume per unit mass measured using a conventional method and the bulk density. The bulk density can be measured, for example, by mercury intrusion porosimetry.

[0040] The porous substrate used in the present invention has a total pore volume Vt measured by mercury porosimetry, preferably 0.55 mL / mL or more and 0.95 mL / mL or less per unit volume of the porous substrate. Due to having such a pore volume, the porous substrate used in the present invention has high compressive strength when formed into a molded body. Furthermore, when a gas absorbent is supported on the porous substrate used in the present invention, it is possible to improve the amine efficiency, gas absorption amount, and gas desorption rate. From the viewpoint of making this advantage more pronounced, the porous substrate used in the present invention has a total pore volume Vt measured by mercury porosimetry, preferably 0.55 mL / mL or more and 0.90 mL / mL or less, more preferably 0.60 mL / mL or more and 0.85 mL / mL or less, and even more preferably 0.60 mL / mL or more and 0.80 mL / mL.

[0041] On the other hand, the total pore volume in the gas absorbent-supported porous substrate of the present invention when the porous substrate supports a gas absorbent will depend on the type of gas absorbent supported and the amount of gas absorbent supported, but the total pore volume Va measured by mercury porosimetry is preferably 0.05 mL / mL or more and 0.80 mL / mL or less per unit volume of the gas absorbent-supported porous substrate. By having such a pore volume, the gas absorbent-supported porous substrate can have both gas absorption ability and diffusibility of the gas to be circulated. From the viewpoint of making this advantage more pronounced, the gas absorbent-supported porous substrate used in the present invention has a total pore volume Va measured by mercury porosimetry per unit volume of the gas absorbent-supported porous substrate, more preferably 0.10 mL / mL or more and 0.75 mL / mL or less, and even more preferably 0.20 mL / mL or more and 0.75 mL / mL or less.

[0042] When the porous substrate used in the present invention has macropores and mesopores, it is preferable that the value of Dm / Ds, which is the ratio of the most frequent pore diameter Dm of the macropores to the most frequent pore diameter Ds of the mesopores, is 1 or more and 1500 or less, since this provides the advantage of improving gas absorption capacity. In addition, by having both macropores and mesopores, the macropores can serve as a receiver for any gas absorbent that leaks out of the mesopores, thereby providing the advantage of suppressing leakage of the gas absorbent from the porous substrate. From the viewpoint of making this advantage even more pronounced, the value of Dm / Ds is more preferably 2 or more and 1000 or less, and even more preferably 3 or more and 500 or less, and 5 or more and 200 or less.

[0043] When the porous substrate used in the present invention has macropores and mesopores, as shown in Figure 1, the porous substrate 1 preferably has a co-continuous structure of a skeleton 3 in which mesopores 4 are formed and macropores 2. In the porous substrate 1 shown in Figure 1, the skeleton 3 and the macropores 2 each have a continuous three-dimensional network structure and are entangled with each other, thereby forming a co-continuous structure of the skeleton 3 and the macropores 2. The fact that the porous substrate 1 has a co-continuous structure of the skeleton 3 and the macropores 2 can be confirmed by observing the surface or cross section of the porous substrate 1 with a scanning electron microscope (hereinafter also referred to as "SEM").

[0044] The skeleton 3 shown in FIG. 1 is a portion made of the material that constitutes the porous substrate 1. The material that constitutes the porous substrate 1 may be, for example, an oxide ceramic containing a metalloid element or a metal element. An example of the metalloid element is silicon. An example of the oxide ceramic containing silicon is silica (SiO 2 ) can be mentioned. Examples of metal elements include aluminum, tin, and zinc, as well as transition metal elements such as cerium, titanium, zirconium, vanadium, chromium, iron, cobalt, nickel, palladium, platinum, copper, silver, and gold. Among these, aluminum, tin, cerium, titanium, and zirconium are preferred from the viewpoint of ease of manufacturing the porous substrate 1. Examples of oxide ceramics containing aluminum, tin, cerium, titanium, or zirconium include alumina (Al2 O 3 ), tin oxide (SnO 2 ), ceria (CeO 2 ), titania (TiO 2 ) and zirconia (ZrO 2 ) etc.

[0045] When the oxide ceramic contains silicon, aluminum, tin, zinc or a transition metal element, the oxide ceramic may further contain, in addition to the silicon, aluminum, tin, zinc or transition metal element, an element selected from alkali metal elements such as lithium and sodium, alkaline earth metal elements such as magnesium and calcium, rare earth elements such as lanthanum, scandium, yttrium and gadolinium, and the like.

[0046] The shape of the porous substrate used in the present invention is not particularly limited. The porous substrate may be, for example, spherical, polyhedral, columnar, or flat, or any combination thereof. When the gas absorbent-supported porous substrate of the present invention is used as a gas absorbent, as described below, the porous substrate is preferably a molded body from the viewpoint of reducing pressure loss. When the porous substrate is a molded body, appropriate voids are generated between the porous substrates, making it possible to efficiently absorb gas without causing excessive pressure loss. The shape of the molded body is not particularly limited. For example, it may be a columnar, spherical, polyhedral, or flat shape, as described below, or any combination thereof.

[0047] When the porous substrate is a columnar molded body, the porous substrate may be a columnar body having a convex curved side surface, such as a circular cylinder or an elliptical cylinder. Alternatively, the porous substrate may be a polygonal prism such as a quadrangular prism, a hexagonal prism, or an octagonal prism, that is, a columnar body having a side surface composed of multiple flat surfaces. When the porous substrate is a columnar body, the columnar body may be missing a portion. For example, the cross section of the columnar body may be a shape missing a portion, such as a circle, an ellipse, or a polygon. In addition, when referring to a "columnar body," the end faces at the upper and lower ends of the columnar body in the height direction are geometrically flat, but in the present invention, the end faces do not need to be flat in the strict sense, and may have a curved portion (a convex curved portion and / or a concave curved portion) within the range that can be considered a columnar body.

[0048] When the porous substrate is a columnar molded body, its average diameter, i.e., the average diameter of the cross section when the columnar body is cut in a direction perpendicular to the height direction of the columnar body, is preferably 1.5 mm or more, more preferably 2.5 mm or more, even more preferably 3.0 mm or more, even more preferably 3.5 mm or more, and even more preferably 4.0 mm or more. On the other hand, the upper limit of the average diameter of the columnar body is preferably 20 mm or less, more preferably 14 mm or less, even more preferably 12 mm or less, even more preferably 10 mm or less, and even more preferably 8.0 mm or less. By setting the average diameter of the columnar body within this range, the durability of the columnar body can be improved and the amount of gas absorbent carried can be increased. Note that when the cross section when the columnar body is cut in a direction perpendicular to the height direction of the columnar body is not circular, the above-mentioned average diameter means the circle equivalent diameter for the area of ​​the cross section.

[0049] The porous substrate used in the present invention can be produced, for example, by the method described in WO 2022 / 163834.

[0050] There are no particular limitations on the method for supporting a gas absorbent on the porous substrate used in the present invention. For example, a solution is prepared by mixing the gas absorbent with a solvent compatible with it, and this solution is mixed with the porous substrate to allow the solution to penetrate into the pores of the porous substrate. The solvent of the solution containing the porous substrate is then distilled off under reduced pressure, and the solution is dried by heating, leaving the gas absorbent in the pores of the porous substrate. Another non-chemically bonded modification method involves placing the gas absorbent and the porous substrate in an autoclave with them spaced apart, and then evacuating the autoclave and filling it with vapor of the gas absorbent, thereby introducing the gas absorbent into the pores of the porous substrate.

[0051] The gas absorbent-supported porous substrate of the present invention is used to absorb various gases by taking advantage of the properties of the amine compound supported thereon. In particular, an absorbent comprising the gas absorbent-supported porous substrate of the present invention can be suitably used as an absorbent for acidic gases such as carbon dioxide, nitrogen oxides, and sulfur oxides, utilizing chemical adsorption by amino groups. In particular, the gas absorbent-supported porous substrate of the present invention has the advantage of high amine efficiency and gas absorption capacity due to the gas absorbent containing polyether. Therefore, the gas to be treated and the pressure conditions during use can be selected from a wide range. In particular, when the gas absorbent-supported porous substrate of the present invention is a molded body, the synergistic effect of its shape and the macropores of the porous substrate significantly reduces pressure loss when gas is passed through it, thereby offering the advantage of being able to treat large amounts of gas to be treated containing a low concentration of the gas to be absorbed. For example, when atmospheric air is used as the gas to be treated, it is possible to treat large amounts of atmospheric carbon dioxide at high speed. This is extremely advantageous from the viewpoint of preventing global warming by removing carbon dioxide from the atmosphere, and complying with emission regulations by removing carbon dioxide from gases emitted from business establishments.

[0052] Acidic gases such as carbon dioxide, nitrogen oxides, and sulfur oxides absorbed in the gas absorbent-supported porous substrate of the present invention are desorbed by heating the gas absorbent-supported porous substrate. As described above, the gas absorbent-supported porous substrate of the present invention has the advantage that the fluidity of the gas absorbent is high even after gas absorption, resulting in a high gas desorption rate and allowing for rapid reuse as a gas absorbent. In particular, the gas absorbent-supported porous substrate of the present invention has high fluidity without being heated to high temperatures, so gas desorption proceeds quickly even when the gas absorbent-supported porous substrate is heated at a relatively low temperature. This reduces the heat cost during gas desorption and suppresses material deterioration of the gas absorbent-supported porous substrate due to exposure to high heat. The desorbed carbon dioxide can be used, for example, as a raw material for synthesizing various organic compounds, such as methane, propylene, and gasoline. Alternatively, the gas absorbent-supported porous substrate that has absorbed carbon dioxide can be stored for long periods in a storage facility. The desorbed nitrogen oxides can also be used, for example, as a raw material for synthesizing nitric acid. The released sulfur oxides are used as raw materials for synthesis of, for example, hydrogen sulfide or sulfuric acid.

[0053] The above-described embodiments of the present invention encompass the following technical ideas. [1] A gas absorbent-supported porous substrate comprising: a porous substrate having at least macropores and mesopores; and a gas absorbent supported in at least some of the pores of the porous substrate, wherein the gas absorbent is a composition containing an amine compound and a polyether; wherein Vs is the pore volume per unit volume of the porous substrate of mesopores in the porous substrate measured by mercury porosimetry in a pore diameter range of more than 2.0 nm and less than 50 nm; and Vsa is the pore volume per unit volume of the gas absorbent-supported porous substrate of mesopores in the gas absorbent-supported porous substrate measured by mercury porosimetry in a pore diameter range of more than 2.0 nm and less than 50 nm; the ratio Vsa / Vs of Vsa to Vs is 0.60 or less; and Vm is the pore volume per unit volume of the porous substrate of macropores in the porous substrate measured by mercury porosimetry in a pore diameter range of 50 nm or more and 10 μm or less;

[0023] A gas absorbent-supported porous substrate, wherein the ratio Vma / Vm of Vma to Vm is 0.50 or more, where Vma is the pore volume of macropores in the gas absorbent-supported porous substrate per unit volume of the gas absorbent-supported porous substrate, as measured by mercury intrusion porosimetry in a pore diameter range of 50 nm to 10 μm. [2] A gas absorbent-supported porous substrate according to [1], wherein the nitrogen atom content is 2.5 mass% to 30 mass%. [3] A gas absorbent-supported porous substrate according to [1] or [2], wherein the ratio of the mass of the polyether to the mass of the amine compound is 0.05 to 10. [4] A gas absorbent-supported porous substrate according to any one of [1] to [3], wherein the ratio of the mass of the gas absorbent to the mass of the porous substrate is 0.20 or more. [5] A gas absorbent-supported porous substrate according to any one of [1] to [4], wherein the amine compound and the polyether are compatible. [6] The gas absorbent-supporting porous substrate according to any one of [1] to [5], wherein the polyether is a polyether represented by the following formula (1) or (2): 1 -(O-A 1 ) n -OR 2 (1) R1 O-(A 1 -O) n1 -R 3 -(O-A 2 ) n2 -OR 2 (2) In the formula, A 1 and A 2 represents an alkylene group, and R 1 and R 2 each independently represents a hydrogen atom or an alkyl group, R 3 represents an alkylene group which may be substituted with X, and X is *-(O-A 3 ) n3 -OR 4 represents A 3 represents an alkylene group, and R 4 represents a hydrogen atom or an alkyl group, * represents a bond, and n1, n2, and n3 represent the number of repetitions. [7] The gas absorbent-supported porous substrate according to any one of [1] to [6], wherein the polyether is a polyether having a weight-average molecular weight of 200 to 2,000. [8] The gas absorbent-supported porous substrate according to any one of [1] to [7], wherein the porous substrate has a total pore volume measured by mercury intrusion porosimetry of 0.55 mL / mL to 0.95 mL / mL. [9] The gas absorbent-supported porous substrate according to any one of [1] to [8], wherein the porous substrate has a co-continuous structure of a skeleton in which the mesopores are formed and the macropores.

[10] The gas absorbent-supported porous substrate according to any one of [1] to [9], wherein the skeleton of the porous substrate contains an element selected from silicon, aluminum, tin, cerium, titanium, and zirconium.

[11] The gas absorbent-supported porous substrate according to any one of [1] to

[10] , wherein the porous substrate is a molded body.

[12] An acidic gas absorbent, comprising the gas absorbent-supported porous substrate according to any one of [1] to

[11] .

[13] A carbon dioxide absorbent, comprising the gas absorbent-supported porous substrate according to any one of [1] to

[11] .

[0054] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "% by mass."

[0055] [Example 1] (1) Production of Porous Substrate The porous substrate of this example was prepared by the production method described in Japanese Patent No. 6,924,338. 2,052 g of polyethylene glycol 10,000, 2,160 g of urea, 14.5 g of acetic acid, and 24 kg of water were added to a 100 L container and stirred at room temperature for 30 minutes to prepare an aqueous polyethylene glycol solution. A sol liquid preparation system consisting of two liquid transfer pumps, a static mixer, and a cooling piping section (2 ° C) was fed with an aqueous polyethylene glycol solution at a rate of 90 mL per minute and tetramethoxysilane at a rate of 45 mL per minute, and mixed and cooled within the system to obtain a mixed solution. The mixed solution was collected in a stirring tank cooled to 15 ° C and stirred for 30 minutes. After stirring, the sol liquid was fed into a 600 mL container, a mold for forming cylindrical pellets with a diameter of 4.6 mm was added, and a polysiloxane gel was produced by heating in a warm bath at 30 ° C.

[0056] The resulting polysiloxane gel was then added to a reaction vessel containing 100 mL of 3 mol / L urea water and heated under reflux for 12 hours. After the reaction was completed, the resulting polysiloxane gel was washed with water and dried for 12 hours in a dryer set at 60 ° C. After drying, it was baked at 600 ° C. for 5 hours in an air atmosphere to obtain a cylindrical porous substrate with a diameter of 4.6 mm. The length of the resulting porous substrate was adjusted by cutting it so that the aspect ratio was 1.5.

[0057] The structure of the obtained porous substrate was observed with an SEM (JSM-7900F manufactured by JEOL), and it was confirmed that the substrate had a co-continuous structure of a silica skeleton with mesopores and macropores.

[0058] (2) Supporting of Gas Absorbent Polyethyleneimine 600 (weight average molecular weight 600) was used as the amine compound, and polyethylene glycol 200 (weight average molecular weight 200) was used as the polyether. Hereinafter, polyethyleneimine is also referred to as "PEI" and polyethylene glycol is also referred to as "PEG". PEI600 and PEG200 were compatible. 3.5 g of PEI600 and 3.5 g of PEG200 were dissolved in 10.5 mL of water to prepare an aqueous solution of the gas absorbent, and then 2.5 g of the previously prepared porous substrate was added to the aqueous solution. After leaving it standing overnight, water was removed at 100 ° C. under reduced pressure to obtain a gas absorbent-supported porous substrate in which a gas absorbent containing PEI600 and PEG200 was supported in the pores of the porous substrate.

[0059] [Examples 2 to 9] A gas absorbent-supporting porous substrate was obtained in the same manner as in Example 1, except that the type and amount of the amine compound and the type and amount of the polyether were as shown in Table 1. The polyethers used in Examples 7, 8, and 9 are as follows. Example 7: A 1 represents an ethylene group, and R 1 and R 2 represents a methyl group and has a weight-average molecular weight of 200 (hereinafter also referred to as "Me2(PEG200)"). Example 8: Polypropylene glycol 400 (weight-average molecular weight 400, hereinafter also referred to as "diol type PPG400"). Example 9: Polyether in which R 3 represents a trimethylene group substituted with X at the 2-position, and A 1 , A 2 and A 3 represents a propylene group, R 1 , R 2 and R 4 represents a hydrogen atom and has a weight-average molecular weight of 300 (hereinafter also referred to as "triol-type PPG300"). In Example 5, polyethyleneimine 300 (weight-average molecular weight 300, hereinafter also referred to as "PEI300") was used as the amine compound. In all Examples, the amine compound and polyether used were compatible with each other.

[0060] [Comparative Example 1] A gas absorbent consisting of only an amine compound, without using a polyether, was supported on a porous substrate at a mass ratio of 1: 1. Otherwise, a gas absorbent-supported porous substrate was obtained in the same manner as in Example 1.

[0061] [Comparative Examples 2 and 3] Mesoporous silica CARiACT Q-10 (manufactured by Fuji Silysia Chemical Ltd.) was used as the porous substrate. The amounts of the amine compound and polyether supported were as shown in Table 1. Except for this, a gas absorbent-supporting porous substrate was obtained in the same manner as in Example 1.

[0062] Comparative Examples 4 and 5 The amounts of the amine compound and polyether supported were as shown in Table 1. Except for this, the same procedure as in Example 1 was carried out to obtain a gas absorbent-supporting porous substrate.

[0063] [Evaluation] For the porous substrates used in the Examples and Comparative Examples, the pore volume Vm of the macropores, the pore volume Vs of the mesopores, the total pore volume Vt, the most frequent pore diameter Dm of the macropores, and the most frequent pore diameter Ds of the mesopores were measured by the following methods. The porous substrates used in Comparative Examples 2 and 3 were mesoporous silica, and the most frequent pore diameter of the macropores was not measured, and therefore is indicated as "-" in Table 1. For the gas absorbent-supported porous substrates obtained in the Examples and Comparative Examples, the pore volume Vma of the macropores, the pore volume Vsa of the mesopores, and the total pore volume Va were measured by the same methods. Furthermore, for the gas absorbent-supported porous substrates obtained in the Examples and Comparative Examples, the nitrogen atom content, nitrogen atom content, carbon dioxide absorption amount, amine efficiency, and carbon dioxide desorption rate were measured by the following methods. The results are shown in Tables 1 and 2 below. Note that in Comparative Example 2, the amount of gas absorbent used was too large relative to the pore volume of the porous substrate, causing the gas absorbent to overflow, and some items could not be evaluated. The measurement results of items that could not be evaluated are marked as "measurable" in Tables 1 and 2.

[0064] [Pore volume Vt, Vm, Vs, Va, Vma, Vsa, Va] The pore volume was measured by mercury intrusion porosimetry using a mercury porosimeter (Micromeritics "Autopore IV9520"). In mercury intrusion porosimetry, pressure was applied to the pores of the porous substrate and the gas absorbent-supported porous substrate to inject mercury, and the pore volume per unit mass was determined from the pressure and the amount of mercury injected. The pore volume per unit mass was multiplied by the bulk density measured by the following method to calculate the pore volume per unit volume. In each example and comparative example, the pore volumes Vm and Vma of the macropores were analyzed by mercury intrusion porosimetry in the pore range having a diameter of 50 nm or more and 10 μm or less, and the pore volumes Vs and Vsa of the mesopores were analyzed by mercury intrusion porosimetry in the pore range having a diameter of more than 2 nm and less than 50 nm. The total pore volumes Vt and Va were the sum of the pore volumes of macropores and mesopores.

[0065] [Bulk density] Using a mercury porosimeter (Micromeritics "Autopore IV9520"), the bulk density of the porous substrate and the gas absorbent-supported porous substrate was measured by mercury intrusion porosimetry under the following measurement conditions and procedures. (Measurement conditions) "Mercury parameters; advancing contact angle: 130.0 degrees, receding contact angle: 130.0 degrees, surface tension: 485.0 mN / m (485.0 dynes / cm), mercury density: 13.5335 g / mL", "low pressure parameters; exhaust pressure: 50 μmHg, exhaust time: 5.0 min, mercury injection pressure: 0.0035 MPa, equilibrium time: 10 seconds", "high pressure parameters; equilibrium time: 10 seconds", "intrusion volume: adjusted to 25% or more and 90% or less", "measurement environment: 20 ° C". (Measurement Procedure) (1) Approximately 0.5 g of sample was weighed and placed in the sample cell, and the weighed value was entered. (2) The range of 0.0048 to 0.2068 MPa was measured in the low-pressure section. (3) The range of 0.2068 to 255.1060 MPa was measured in the high-pressure section. (4) The pore size distribution was calculated from the mercury injection pressure and mercury injection amount. (2), (3), and (4) were performed automatically using the software provided with the device. The bulk density was calculated using the software from the pore size distribution calculated as described above. The bulk density was determined by referencing "Bulk Density at 0.0035 MPa" on the software.

[0066] [Most frequent pore diameter Dm of macropores] Using a mercury porosimeter (Micromeritics "Autopore IV9520"), the most frequent pore diameter Dm of macropores was measured by mercury intrusion. In mercury intrusion, pressure is applied to the pores of the porous substrate to inject mercury, and the pore volume and specific surface area are determined from the pressure and the amount of mercury injected. The pore diameter was calculated from the relationship between the pore volume and the specific surface area when the pores are assumed to be cylindrical. In this specification, the mercury intrusion method was used to analyze a pore range having a diameter of 50 nm or more and 10 μm or less.

[0067] [Modular pore diameter Ds of mesopores] As with the modal pore diameter of macropores, the modal pore diameter Ds of mesopores was measured by mercury intrusion porosimetry using a mercury porosimeter (Micromeritics' "Autopore IV9520") In this specification, the mesopores were analyzed in the range of diameters greater than 2 nm and less than 50 nm by mercury intrusion porosimetry.

[0068] [Nitrogen atom content and nitrogen atom content] The nitrogen atom content and nitrogen atom content of the gas absorbent-supported porous substrate were quantified using an oxygen, nitrogen, and hydrogen analyzer ONH836 manufactured by LECO Japan LLC. In Examples 7 to 9, no measurement was performed, and the measurement results were indicated as "-". Note that the nitrogen atom content may exceed the theoretical nitrogen atom content value described below due to the influence of bias in the supported gas absorbent.

[0069] [Amount of carbon dioxide absorption] The amount of carbon dioxide absorption was measured using a BELCAT II adsorption amount and adsorption rate measuring device manufactured by Microtrac-Bell. 0.1 g of a gas absorbent-supported porous substrate was placed in a sample cell and pretreated at 120 ° C. for 30 minutes under a helium flow of 50 sccm. After pretreatment, the temperature of the sample chamber was set to 25 ° C., and a gas with a carbon dioxide concentration of 4 vol% was passed through at 50 sccm for 25 minutes. Thereafter, the flow of carbon dioxide was stopped, helium was passed through at 50 sccm, and the temperature was raised to 100 ° C. at a heating rate of 10 ° C. / min and maintained for 30 to 60 minutes. The amount of carbon dioxide absorption was calculated from the peak area detected by TCD at this time.

[0070] [Amine efficiency] The amount of carbon dioxide absorbed measured by the above method was divided by the theoretical nitrogen atom content of the gas absorbent-supported porous substrate to calculate the amine efficiency. A higher amine efficiency indicates a higher proportion of amino groups contributing to gas absorption among the amino groups possessed by the amine compound supported on the porous substrate.

[0071] [Theoretical nitrogen atom content and theoretical nitrogen atom content] The theoretical nitrogen atom content (mmol / g) of the porous substrate supporting gas absorbent is calculated by multiplying the amount (mmol) of amine compound supported by the amine value of this amine compound, and dividing the result (mmol) by the mass (g) of the porous substrate supporting gas absorbent.In addition, by using the atomic weight of nitrogen atom, the theoretical nitrogen atom content (mmol / g) of the porous substrate supporting gas absorbent is converted into theoretical nitrogen atom content (%).

[0072] [Carbon dioxide desorption rate] The carbon dioxide desorption rate was evaluated using a BELCAT II adsorption amount and adsorption rate measuring device manufactured by Microtrac-Bell. 0.1 g of a gas absorbent-supported porous substrate was placed in a sample cell and pretreated at 120 ° C. for 30 minutes under a helium flow of 50 sccm. After pretreatment, the temperature of the sample chamber was set to 25 ° C., and a gas with a carbon dioxide concentration of 4 vol% was passed through at 50 sccm for 25 minutes. Thereafter, the flow of carbon dioxide was stopped, helium was passed through at 50 sccm, and the temperature was raised to 100 ° C. at a heating rate of 10 ° C. / min and maintained for 30 to 60 minutes. From the peak area detected by the TCD at this time, 90% of the amount of carbon dioxide absorbed relative to the total amount of carbon dioxide was calculated, and the desorption rate at 100 ° C. was calculated by dividing by the time from the start of desorption until 90% of the carbon dioxide amount was desorbed. Further, the desorption rate at 80°C was calculated in the same manner as in the above measurement, except that the temperature was raised to 80°C instead of 100°C.

[0073]

[0074]

[0075] As is clear from the results shown in Tables 1 and 2, the gas absorbent-supported porous substrates of each Example, which used a porous substrate having macropores and mesopores and a gas absorbent consisting of a composition containing an amine compound and a polyether, and which had Vsa / Vs and Vma / Vm within the specified ranges, had superior amine efficiency and carbon dioxide desorption rate than the gas absorbent-supported porous substrates of each Comparative Example. In particular, as shown in Table 2, it can be seen that the gas absorbent-supported porous substrate of the present invention has an excellent gas desorption rate at a relatively low temperature of 80 ° C.

[0076] According to the present invention, there is provided a gas absorbent-supporting porous substrate which has a high gas absorption amount and a high desorption rate of the absorbed gas.

Claims

1. A gas absorbent-supported porous substrate comprising a porous substrate having at least macropores and mesopores, and a gas absorbent supported in at least some of the pores of the porous substrate, wherein the gas absorbent is a composition containing an amine compound and a polyether, and the pore volume per unit volume of the porous substrate of the mesopores of the porous substrate measured by mercury intrusion porosimetry in a pore diameter range of more than 2.0 nm and less than 50 nm is Vs, and the pore volume per unit volume of the gas absorbent-supported porous substrate of the mesopores of the gas absorbent-supported porous substrate measured by mercury intrusion porosimetry in a pore diameter range of more than 2.0 nm and less than 50 nm is Vsa, the ratio Vsa / Vs of Vsa to Vs is 0.60 or less, and the pore volume per unit volume of the porous substrate of the macropores of the porous substrate measured by mercury intrusion porosimetry in a pore diameter range of 50 nm or more and 10 μm or less is Vm, A gas absorbent-supported porous substrate, in which the pore volume of macropores in the gas absorbent-supported porous substrate per unit volume of the gas absorbent-supported porous substrate, as measured by mercury intrusion porosimetry in a pore diameter range of 50 nm to 10 μm, is taken as Vma, and the ratio Vma / Vm of Vma to Vm is 0.50 or more.

2. A gas absorbent-supporting porous substrate as described in claim 1, in which the nitrogen atom content is 2.5 mass % or more and 30.0 mass % or less.

3. The gas absorbent-supporting porous substrate according to claim 1, wherein the ratio of the mass of said polyether to the mass of said amine compound is 0.05 or more and 10 or less.

4. A gas absorbent-supporting porous substrate according to claim 1, wherein the ratio of the mass of said gas absorbent to the mass of said porous substrate is 0.20 or more.

5. The gas absorbent-supporting porous substrate according to claim 1, wherein said amine compound and said polyether are compatible with each other.

6. The gas absorbent-supporting porous substrate according to claim 1, wherein the polyether is a polyether represented by the following formula (1) or (2): 1 - (O-A 1 ) n1 -OR 2 (1) R 1 O-(A 1 -O) n1 -R 3 - (O-A 2 ) n2 -OR 2 (2) In the formula, A 1 and A 2 represents an alkylene group; R 1 and R 2 each independently represents a hydrogen atom or an alkyl group; R 3 represents an alkylene group which may be substituted with X, and X is *-(O-A 3 ) n3 -OR 4 represents, 3 represents an alkylene group; R 4 represents a hydrogen atom or an alkyl group, * represents a bond, and n1, n2 and n3 represent the number of repetitions.

7. The gas absorbent-supporting porous substrate according to claim 1, wherein the polyether has a weight average molecular weight of 200 or more and 2,000 or less.

8. The gas absorbent-supporting porous substrate according to claim 1, wherein the porous substrate has a total pore volume measured by mercury intrusion porosimetry of 0.55 mL / mL or more and 0.95 mL / mL or less.

9. The gas absorbent-supporting porous substrate according to claim 1, wherein the porous substrate has a co-continuous structure of the skeleton in which the mesopores are formed and the macropores.

10. The gas absorbent-supporting porous substrate according to claim 1, wherein the skeleton of the porous substrate comprises an element selected from silicon, aluminum, tin, cerium, titanium and zirconium.

11. The gas absorbent-supporting porous substrate according to claim 1, wherein the porous substrate is a molded body.

12. An acid gas absorbent comprising a gas absorbent-supporting porous substrate according to any one of claims 1 to 11.

13. A carbon dioxide absorbent comprising a gas absorbent-supporting porous substrate according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Amino compound-carried porous material, and method for producing the same

    JP2015113337A

  • Apparatus and method for producing sol, gel and porous silica body

    JP6924338B1

  • Porous body, adsorptive material containing said porous body, and method for removing metal and / or metal ion using said adsorptive material

    WO2022163834A1

  • Adsorbent, filtering media, and air filter

    JP2008200648A

  • Monolithic organic porous material, method for producing the same, and monolithic organic porous ion exchanger

    JP2009221428A

Cited By

  • Carbon dioxide absorbing material and method for producing same

    WO2026225428A1