The method generates and recovers carbon dioxide from inorganic acid reactions with lithium-ion battery materials to produce high-quality lithium carbonate, reducing emissions and costs, thus overcoming the impurity and emission challenges of current lithium carbonate production techniques.
Patent Information
- Application Number
- PCT/JP2024/013089
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-28
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Current methods for producing lithium carbonate from recycled lithium-ion battery materials result in low-quality lithium carbonate due to impurities and high carbon dioxide emissions, as they involve burning processes that generate hydrogen fluoride, nitrogen oxides, and sulfur compounds.
A method that generates carbon dioxide by reacting an inorganic acid with a carbonate-containing raw material, recovers the carbon dioxide, and then uses it to produce lithium carbonate, thereby reducing emissions and impurities, employing a system with a reaction tank, carbon dioxide recovery device, and lithium carbonate production tank.
This method produces high-quality lithium carbonate while minimizing carbon dioxide emissions and costs, effectively addressing the impurity and emission issues of existing processes.
Smart Images

Figure JP2024013089_03102024_PF_FP_ABST
Abstract
Description
Lithium carbonate manufacturing method and lithium carbonate manufacturing apparatus
[0001] The present invention relates to a method and an apparatus for producing lithium carbonate. This application claims priority based on Japanese Patent Application No. 2023-58132 filed on March 31, 2023, and Japanese Patent Application No. 2024-53899 filed on March 28, 2024, the contents of which are incorporated herein by reference.
[0002] In recent years, there has been a demand to reduce greenhouse gas emissions from electric vehicles and the lithium-ion batteries used in them throughout their entire lifecycle, from sourcing raw materials to disposal and recycling.
[0003] When recovering resources such as lithium from lithium-ion batteries, it is common to use a recycled raw material called black mass, which is obtained by firing and pulverizing lithium-ion batteries.
[0004] As a method for recovering lithium from black mass, for example, Patent Document 1 focuses on lithium aluminate contained in black mass and discloses a method for recovering lithium by leaching black mass containing lithium aluminate in an acidic solution.
[0005] Patent Document 2 discloses a method in which an active material powder obtained by pulverizing a lithium ion battery is burned, the carbon content in the active material powder is burned and converted into carbon dioxide, and then the burned active material powder is wet-dissolved to recover lithium.
[0006] Patent No. 6998241 JP 2022-168616
[0007] The lithium recovery method disclosed in Patent Document 1 discloses that after recovering lithium, lithium is carbonated to obtain lithium carbonate, but does not take into consideration reducing greenhouse gases such as carbon dioxide in the process of obtaining lithium carbonate.
[0008] Patent Document 2 discloses that lithium carbonate is obtained by introducing carbon dioxide obtained by burning carbon in an active material powder into a lithium-containing solution obtained by wet dissolution. That is, a method for reducing carbon dioxide emissions by utilizing carbon dioxide generated by burning carbon in an active material powder as a carbonate source for obtaining lithium carbonate is being studied.
[0009] However, the active material powder obtained by pulverizing lithium-ion batteries contains many impurities, and the gas components generated when the active material powder is burned contain not only carbon dioxide but also hydrogen fluoride, nitrogen oxides, sulfur compounds, etc. The hydrogen fluoride, nitrogen oxides, and sulfur compounds in the gas components are easily incorporated as impurities, which poses a problem of reducing the purity of the lithium carbonate.
[0010] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a method for producing lithium carbonate and an apparatus for producing lithium carbonate that can produce high-quality lithium carbonate while reducing carbon dioxide emission and usage costs.
[0011] In order to solve the above-mentioned problems, the present invention is characterized by having any one of the following aspects: (1) A method for producing lithium carbonate, comprising: a carbon dioxide generating step of adding an inorganic acid to a raw material containing a carbonate to generate carbon dioxide, a carbon dioxide recovering step of recovering the carbon dioxide, and a lithium carbonate producing step of adding the recovered carbon dioxide to a lithium-containing liquid to obtain lithium carbonate.
[0012] (2) The method for producing lithium carbonate according to (1), wherein, in the carbon dioxide recovery step, gaseous carbon dioxide is absorbed in an alkaline solution to recover the carbon dioxide.
[0013] (3) The method for producing lithium carbonate according to (1), wherein the carbon dioxide recovery step recovers the carbon dioxide by capturing gaseous carbon dioxide.
[0014] (4) The method for producing lithium carbonate according to any one of (1) to (3), wherein the raw material contains a lithium compound.
[0015] (5) The method for producing lithium carbonate according to any one of (1) to (3), wherein the raw material is a lithium ion battery fired powder obtained by firing and pulverizing a lithium ion battery.
[0016] (6) The method for producing lithium carbonate according to any one of (1) to (5), wherein the inorganic acid is at least one selected from the group consisting of sulfuric acid, hydrochloric acid, and nitric acid.
[0017] (7) The method for producing lithium carbonate according to any one of (1) to (5), wherein the carbon dioxide generation step is carried out under a temperature condition of 10°C or higher and 40°C or lower, and under a pH condition of pH 6 or lower.
[0018] (8) An apparatus for producing lithium carbonate, comprising: a reaction tank that generates carbon dioxide using a raw material containing a carbonate and an inorganic acid; a carbon dioxide capture device that captures the carbon dioxide; and a lithium carbonate production tank that supplies carbon dioxide from the carbon dioxide capture device to a lithium-containing liquid to produce lithium carbonate.
[0019] (9) The apparatus for producing lithium carbonate according to (8), wherein the carbon dioxide recovery device is a device that captures gaseous carbon dioxide.
[0020] (10) The apparatus for producing lithium carbonate according to (8), wherein the carbon dioxide recovery device is a device that captures carbon dioxide by causing an alkaline solution to absorb gaseous carbon dioxide.
[0021] According to the present invention, it is possible to provide a method for producing lithium carbonate and an apparatus for producing lithium carbonate that can produce high-quality lithium carbonate while reducing carbon dioxide emissions and usage costs.
[0022] 1 is a flowchart showing a stepwise configuration of a lithium carbonate manufacturing method according to an embodiment of the present invention;
[0023] Hereinafter, a method for producing lithium carbonate and an apparatus for producing lithium carbonate according to one embodiment of the present invention will be described with reference to the drawings. Note that each embodiment shown below is specifically described to provide a better understanding of the gist of the invention, and does not limit the present invention unless otherwise specified.
[0024] (Method for Producing Lithium Carbonate) As shown in Fig. 1 , the method for producing lithium carbonate of this embodiment includes at least a carbon dioxide generation step S1 of adding an inorganic acid to a raw material containing a carbonate to generate carbon dioxide, a carbon dioxide recovery step S2 of recovering the carbon dioxide, and a lithium carbonate production step S5 of adding the recovered carbon dioxide to a lithium-containing liquid to obtain lithium carbonate. In the method for producing lithium carbonate of this embodiment, the carbon dioxide generation step S1 may be a leaching step of leaching lithium ions from a raw material containing a carbonate. In this case, the method for producing lithium carbonate of this embodiment may include a solid-liquid separation step S3 of separating a leachate generated in the carbon dioxide generation step S1 from a leachate residue, and an impurity removal step S5 of removing impurities from the leachate separated in the solid-liquid separation step S3.
[0025] The method for producing lithium carbonate according to the present embodiment is preferably carried out using an apparatus for producing lithium carbonate 10 shown in Fig. 2. The apparatus for producing lithium carbonate 10 used in the present embodiment has at least a reaction tank (leaching tank) 11, a carbon dioxide capture device 13, and a lithium carbonate production tank 14. The apparatus for producing lithium carbonate 10 according to the present embodiment may also have a solid-liquid separation tank 12.
[0026] (Carbon dioxide generating step: S1) In the carbon dioxide generating step S1, an inorganic acid is added to a raw material containing a carbonate to generate carbon dioxide. In this embodiment, the raw material may contain a lithium compound, and the carbonate may be a lithium compound. Examples of the carbonate include one or more selected from the group consisting of lithium carbonate, cobalt carbonate, nickel carbonate, aluminum carbonate, and calcium carbonate.
[0027] More specifically, examples of raw materials containing carbonate include lithium ion battery sintered powder (black mass) formed from used lithium ion batteries collected as recycled raw materials, and lithium ion battery sintered powder (black mass) formed from scrap generated in the manufacturing process of lithium ion batteries.
[0028] The positive electrode active material of lithium-ion batteries is lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganese oxide (LiMn 2 O 4 The negative electrode active material may contain a lithium compound such as lithium titanate. The electrolyte may contain lithium hexafluorophosphate (LiPF 6 ) and lithium tetrafluoroborate (LiBF 4 ) and other lithium compounds.
[0029] Among these lithium compounds, lithium compounds bonded with trivalent cobalt, nickel, or manganese (lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganese oxide (LiMn 2 O 4 ) are hardly soluble in inorganic acids such as sulfuric acid, which convert them into divalent ions. Therefore, it is preferable to heat and thermally decompose the lithium compound bonded to the trivalent cobalt, nickel, or manganese, and convert the lithium in the lithium compound with the trivalent cobalt, nickel, or manganese into lithium carbonate. During the thermal decomposition process, the lithium in the lithium compound bonded to the trivalent cobalt, nickel, or manganese reacts with carbon dioxide produced during the thermal decomposition process to form lithium carbonate (Li 2 CO 3 ) is also produced. The lithium compound derived from the electrolyte also reacts with the carbon dioxide produced during the thermal decomposition process to produce lithium carbonate (Li 2 CO 3 ) is generated.
[0030] First Method: Lithium Carbonate (Li2 CO 3 In a first method for obtaining a lithium-ion battery sintered powder (black mass) containing aluminum, a used lithium-ion battery is discharged and then directly placed in a pyrolysis furnace, and the lithium-ion battery is thermally decomposed by heating, for example, in a temperature range of about 400°C to 600°C for about 30 minutes to 5 hours, preferably in a superheated steam atmosphere or a non-oxidizing atmosphere such as nitrogen. Pyrolysis of a lithium-ion battery under the above-mentioned conditions of atmosphere, temperature, and time is preferred because the aluminum contained in the lithium-ion battery becomes embrittled without melting.
[0031] In the thermal decomposition of the lithium ion battery of this embodiment, the exterior case of the lithium ion battery is melted or embrittled to separate and recover, and the binder is decomposed to make the positive electrode active material and the current collector separable from each other. Furthermore, in the thermal decomposition of the lithium ion battery of this embodiment, the lithium compound bonded to trivalent cobalt, nickel, or manganese in the positive electrode active material is thermally decomposed to generate a thermal decomposition product. Then, carbon dioxide generated during the thermal decomposition reacts with lithium in the thermal decomposition product to produce lithium carbonate (Li 2 CO 3 ) is generated.
[0032] Next, the pyrolyzed product of the lithium-ion battery is crushed. The crushed electrode active material after the pyrolysis is broken into fine first crushed material having a particle size of approximately less than 1 mm. For example, the crushing process can be carried out using a shear crusher such as a biaxial shear crusher or an impact crusher such as a hammer mill, either alone or in combination.
[0033] Next, the crushed material of the thermal decomposition product of the lithium-ion battery is classified using a sieve with an appropriate mesh size, for example, into fine particles of less than 1 mm, preferably 0.5 mm or less, and coarse particles larger than that. For classification, for example, a vibrating sieve with a mesh size of 0.1 mm to 1.0 mm, preferably 0.1 mm to 0.5 mm, may be used. This classification allows for separation of the metal chunks of the exterior case and metal foil derived from the current collector contained in the coarse particles from the thermal decomposition product of the electrode active material contained in the fine particles.
[0034] By the above steps, a lithium-ion battery sintered powder (black mass) containing the lithium carbonate of this embodiment and having a particle size of 1 mm or less can be obtained. The proportion of lithium carbonate contained in the black mass is, for example, about 1% by mass or more and 10% by mass or less, which is suitable for generating carbon dioxide.
[0035] Second Method: Lithium Carbonate (Li 2 CO 3 In a second method for obtaining a lithium-ion battery sintered powder (black mass) containing the lithium-ion battery sintered powder (black mass), first, used lithium-ion batteries are immersed in salt water to remove the internal charge of the lithium-ion batteries. The lithium-ion batteries from which the internal charge has been removed are then dried and crushed to obtain second crushed pieces of a size that allows for accurate separation of the positive electrode active material inside the lithium-ion battery from the outer case. Crushing can be performed using, for example, a uniaxial crusher. The concentration of the salt water used to remove the internal charge of the lithium-ion batteries is not particularly limited. The mesh size of the screen of the uniaxial crusher is preferably 6 mm or more and 10 mm or less in diameter. When the mesh size of the screen is within this range, the positive electrode active material inside the lithium-ion battery can be sufficiently separated from the outer case.
[0036] Next, the second crushed material is classified using a sieve with an appropriate mesh size to recover the positive electrode active material from the second crushed material. For example, the positive electrode active material inside the lithium ion battery and the exterior case contained in the second crushed material can be separated by sieving using a vibrating sieve with a mesh size of 0.25 mm to 2.8 mm.
[0037] Another method for separating used lithium-ion batteries into the positive electrode active material inside the lithium-ion battery and the exterior case includes a method using an immersion crushing device immersed in an immersion liquid. Specifically, used lithium-ion batteries are crushed using the immersion crushing device, and lightweight crushed materials such as the exterior case (plastic portion) of the crushed lithium-ion battery are suspended, causing metals containing the positive electrode active material to precipitate, and the precipitate is recovered to recover the positive electrode active material. The immersion liquid is preferably an aqueous solution containing at least one selected from sodium hydroxide, calcium hydroxide, and lithium hydroxide, and has a pH of 8 or higher. When the immersion liquid contains at least one salt selected from sodium hydroxide, calcium hydroxide, and lithium hydroxide, residual charge in the lithium-ion battery can be released in the immersion liquid.
[0038] As described above, the positive electrode active material recovered using the uniaxial crusher or the immersion crusher is placed in a pyrolysis furnace and heated, preferably in a superheated steam atmosphere or a non-oxidizing atmosphere such as nitrogen, for example, at a temperature range of about 400°C to 600°C for about 1 hour to 2 hours, to react the lithium in the lithium compound combined with trivalent cobalt, nickel, or manganese with carbon dioxide generated during the pyrolysis process to produce lithium carbonate (Li 2 CO 3 When the thermal decomposition of the positive electrode active material is carried out under the above-mentioned conditions of atmosphere, temperature, and time, metals such as aluminum contained in the positive electrode active material are embrittled without melting, which is preferable.
[0039] Lithium carbonate (Li 2 CO 3 The pyrolyzate containing the lithium carbonate of the present embodiment can be classified using a sieve with appropriate openings, as in the first method, to obtain a lithium ion battery fired powder (black mass) having a particle size of 1 mm or less, which contains the lithium carbonate of the present embodiment.
[0040] Lithium carbonate (Li 2 CO 3 The second method for obtaining black mass containing sulphur dioxide is preferred because it allows for a greater reduction in the amount of exhaust gas.
[0041] Third Method: Lithium Carbonate (Li 2 CO 3 In a third method for obtaining a lithium-ion battery sintered powder (black mass) containing the above-mentioned sintered powder, black mass is obtained from scrap generated in the manufacturing process of lithium-ion batteries, such as scraps of sheet-like positive electrode material or black powder that is a defective lithium-ion battery.
[0042] For example, black mass can be obtained by thermally decomposing, crushing, and classifying scrap generated in the manufacturing process of lithium ion batteries in the same manner as in the first method. Alternatively, black mass can be obtained by crushing scrap generated in the manufacturing process of lithium ion batteries using a uniaxial crusher or an immersion crusher in the same manner as in the second method, recovering the positive electrode active material from the crushed material, thermally decomposing the positive electrode active material, and then classifying it.
[0043] In the carbon dioxide generation step S1 of this embodiment, for example, lithium ion battery fired powder (black mass) containing lithium carbonate as a carbonate salt obtained by any of the first to third methods described above is used as a raw material.
[0044] In this embodiment, the black mass is placed in a resin reaction tank (leaching tank) 11, and water and an inorganic acid are then added to the reaction tank 11, followed by stirring and shaking. Note that the black mass may be finely pulverized or attrition-pulverized in the reaction tank 11 to improve the reaction efficiency.
[0045] As the inorganic acid, it is preferable to use one or more selected from the group consisting of sulfuric acid, hydrochloric acid, and nitric acid. In the reaction tank 11, it is preferable to mix the raw material black mass, water, and inorganic acid, and adjust the pH to a level at which lithium carbonate dissolves. The pH at which lithium carbonate dissolves is, for example, preferably about pH 6 or less, more preferably in the range of pH 2 to pH 5. At pH 6 or less, lithium carbonate dissolves and carbon dioxide is generated. On the other hand, at a pH below 2, the solubility of lithium carbonate does not change, and the amount of carbon dioxide generated does not change either. When lithium carbonate dissolves, one or more reactions selected from the decomposition reactions shown in the following formulas (1) to (3) proceed, and carbon dioxide is generated (carbon dioxide generation step S1). Li2 CO 3 +H 2 SO 4 →Li 2 SO 4 (liquid phase)+H 2 O (liquid phase) + CO 2 (Gas) (1) Li 2 CO 3 +2HCl → 2LiCl (liquid phase) +H 2 O (liquid phase) + CO 2 (Gas) (2) Li 2 CO 3 +2HNO 3 →2LiNO 3 (liquid phase)+H 2 O (liquid phase) + CO 2 (Gas) (3)
[0046] The carbon dioxide generation step is preferably carried out at room temperature (10 to 40°C, preferably 18 to 25°C). In the conventional method of generating carbon dioxide by burning carbon in the active material powder in a lithium ion battery, the reaction temperature is high and hydrogen fluoride, nitrogen oxides (NO X ), and sulfur compounds are simultaneously generated. Therefore, when the gas components obtained by the conventional method are used in the subsequent lithium carbonate production step, the quality of the lithium carbonate is deteriorated. As described above, the gas generated in the carbon dioxide generation step S1 of the present embodiment is a non-combustible gas, and therefore, hydrogen fluoride, nitrogen oxides (NO X ), and sulfur compounds.
[0047] Within the temperature condition range of the carbon dioxide generation step S1 of this embodiment, the gas generated when black mass, water, and inorganic acid are mixed to generate carbon dioxide contains carbon dioxide, hydrogen, oxygen, etc. On the other hand, if the temperature is below room temperature, the problem of carbon dioxide generation being difficult arises. The component composition of the gas generated in the carbon dioxide generation step S1 of this embodiment is, for example, carbon dioxide: 95 vol% to 98 vol%, hydrogen: 1 vol% to 2 vol%, and the balance: oxygen, etc. The gas components can be measured by gas chromatography.
[0048] The reaction time in the reaction tank 11 may be, for example, in the range of 30 minutes to 20 hours. If the reaction time is less than 30 minutes, there is a concern that the lithium carbonate contained in the black mass will not react sufficiently with the inorganic acid. Furthermore, if the reaction time exceeds 20 hours, there is a concern that the reaction will not proceed any further, resulting in a decrease in treatment efficiency.
[0049] As described above, the components contained in the gas obtained in the carbon dioxide generation step S1 of this embodiment are carbon dioxide, oxygen, hydrogen, etc. Oxygen and hydrogen do not generate impurities in the lithium carbonate production step S5. Therefore, when the carbon dioxide obtained in the carbon dioxide generation step S1 of this embodiment is used as a carbon dioxide source in the subsequent lithium carbonate production step S5, high-quality lithium carbonate can be obtained without removing impurities in the gas.
[0050] In the carbon dioxide generation step S1 of this embodiment, leaching of lithium compounds into the liquid phase simultaneously proceeds. For example, lithium carbonate contained in the black mass reacts with an inorganic acid and migrates to the leachate (liquid phase) in the form of lithium sulfate, lithium chloride, lithium nitrate, etc. Next, a calcium compound is added to neutralize the black mass to separate it from cobalt and nickel. Because the calcium compound added during neutralization is eluted and the black mass contains lithium fluoride in addition to lithium carbonate, the leachate contains impurities such as calcium and fluorine. Meanwhile, the leaching residue (solid phase) obtained after leaching contains the carbon, cobalt, nickel, etc. contained in the black mass.
[0051] (Carbon dioxide capture step: S2) Next, in the carbon dioxide capture step S2, the carbon dioxide generated in the carbon dioxide generation step S1 is captured. As the carbon dioxide capture device 13 for capturing carbon dioxide, either a gas capture device that captures carbon dioxide in gaseous form and captures it, or an alkaline solution tank that absorbs and captures gaseous carbon dioxide with an alkaline solution can be used.
[0052] When gaseous carbon dioxide is collected by the gas collection device 13, the carbon dioxide can be used as it is in the subsequent lithium carbonate production step S5. Therefore, carbon dioxide is supplied from the gas collection device to the lithium carbonate production tank 14 through a gas supply pipe (not shown).
[0053] When recovering carbon dioxide using an alkaline solution tank, an aqueous sodium hydroxide solution is used as the alkaline solution, and carbon dioxide (gas) is introduced into the aqueous sodium hydroxide solution to recover carbon dioxide. The concentration of the aqueous sodium hydroxide solution preferred for recovering carbon dioxide is 1 mol / L or more and 18 mol / L or less. When carbon dioxide is introduced into the aqueous sodium hydroxide solution, carbon dioxide is recovered as sodium bicarbonate, as shown in the following formulas (4) and (5). CO 2 + 2NaOH → Na 2 CO 3 +H 2 O (4) Na 2 CO 3 +CO 2 +H 2 O → 2NaHCO 3 (5)
[0054] (Solid-Liquid Separation Step: S3) In the solid-liquid separation step S3 of this embodiment, the leaching solution (liquid phase) obtained in the carbon dioxide generation step S1 is separated from the leaching residue (solid phase). For example, the solid-liquid separation can be performed by filtering the solid-liquid mixture obtained in the carbon dioxide generation step S1 using a filtration device to separate the solid and liquid phases. By performing the solid-liquid separation step S3, it is possible to obtain a solid phase containing carbon, cobalt, nickel, etc. contained in the black mass, and a leaching solution (liquid phase) in which lithium carbonate is dissolved in the form of lithium sulfate, lithium chloride, or lithium nitrate.
[0055] The solid phase obtained by the solid-liquid separation step S3 can then be leached using sulfuric acid or the like to leach and recover each metal from insoluble substances such as carbon (graphite) contained in the solid phase.
[0056] (Impurity Removal Step: S4) In the impurity removal step S4 of this embodiment, impurities are removed from the leachate (liquid phase) separated in the solid-liquid separation step S3. In this embodiment, lithium-ion battery fired powder (black mass) is leached with one or more inorganic acids selected from the group consisting of sulfuric acid, hydrochloric acid, and nitric acid, and impurities such as calcium ions and fluoride ions coexist in the leachate. If calcium ions coexist in the leachate, they react with carbon dioxide to produce calcium carbonate in the subsequent lithium carbonate production step S5, thereby reducing the purity of lithium carbonate. Furthermore, if fluoride ions coexist in the leachate, they produce lithium fluoride in the subsequent lithium carbonate production step S5, thereby reducing the purity of lithium carbonate. Therefore, in this embodiment, it is desirable to remove impurities such as calcium ions and fluoride ions from the leachate (liquid phase) separated in the solid-liquid separation step S3.
[0057] In the impurity removal step S4, it is preferable to first remove fluoride ions from the leachate. As a method for removing fluoride ions, a calcium salt is added to the leachate to form calcium fluoride (CaF 2 The calcium fluoride method involves precipitating calcium fluoride from the aqueous solution of fluoride ions and separating the fluoride ions as a solid, and the adsorption method involves adsorbing the fluoride ions onto aluminum hydroxide, or both of these methods.
[0058] In the calcium fluoride method, one or more calcium salts selected from calcium chloride, calcium carbonate, calcium hydroxide, and calcium sulfate can be used. By adding any of the calcium salts to a leachate containing fluoride ions, calcium fluoride (CaF 2 ) precipitates and precipitates. This reaction reduces the fluoride ion concentration in the leachate.
[0059] The adsorption method involves removing fluoride ions from a leachate containing fluoride ions by adsorbing them onto the surface of aluminum hydroxide in the leachate, and then separating the aluminum hydroxide precipitate with the adsorbed fluoride ions, thereby reducing the fluoride ion concentration in the leachate. In the adsorption method, aluminum sulfate or aluminum chloride may be added to the leachate containing fluoride ions. The leachate of this embodiment contains lithium ions, and adding aluminum sulfate or aluminum chloride precipitates aluminum hydroxide. In this case, the pH of the leachate is preferably in the range of pH 6 to pH 8. A pH of 6 to pH 8 can reduce the solubility of the precipitated aluminum hydroxide while adsorbing fluoride ions onto the aluminum hydroxide, thereby increasing the purity of the lithium carbonate obtained in the subsequent lithium carbonate production step S5. If the pH of the leachate is outside the range of pH 6 to pH 8, aluminum ions remain in the leachate, adversely affecting the subsequent lithium carbonate production step S5.
[0060] In the impurity removal step S4 of this embodiment, sodium carbonate (Na 2 CO 3 When sodium carbonate is added to the leaching solution, calcium ions in the leaching solution react with the sodium carbonate to form calcium carbonate (CaCO 3 ) precipitates, and calcium ions can be separated as solids. By separating calcium ions in this way, the calcium ion concentration in the leachate can be reduced, and the purity of lithium carbonate obtained in the subsequent lithium carbonate production step S5 can be increased.
[0061] The leachate separated in the solid-liquid separation step S3 contains heavy metal ions (Fe 3+ , Mn 2+ , Ni 2+ , Co 2+ When the leachate contains heavy metal ions, the concentration of heavy metal ions in the leachate can be reduced by precipitating or adsorbing the heavy metal ions using any of the above-mentioned calcium fluoride method, adsorption method, and calcium carbonate generation method.
[0062] (Lithium carbonate production step: S5) In the lithium carbonate production step S5 of the present embodiment, the carbon dioxide recovered in the carbon dioxide recovery step S2 is introduced into the leachate from which impurities have been removed in the impurity removal step S4 to precipitate lithium carbonate, and the lithium carbonate precipitate is separated, thereby obtaining lithium carbonate. That is, the leachate is used as a lithium-containing liquid.
[0063] In the lithium carbonate production step S5 of this embodiment, the carbon dioxide recovered in the carbon dioxide recovery step S2 is used as a carbon dioxide source. The carbon dioxide recovered in the carbon dioxide recovery step S2 is the carbon dioxide contained in the gas generated in the preceding carbon dioxide generation step S1. The gas generated in the carbon dioxide generation step S1 of this embodiment contains oxygen, hydrogen, and the like in addition to carbon dioxide. However, the gas also contains hydrogen fluoride, nitrogen oxides (NO X ), and sulfur compounds. Therefore, in the lithium carbonate production step S5 of the present embodiment, no impurities are produced, and high-quality lithium carbonate can be obtained.
[0064] Furthermore, in the lithium carbonate production step S5 of the present embodiment, carbon dioxide generated when the lithium compound contained in the black mass is leached into a liquid phase using an inorganic acid is used as the carbon dioxide source. This makes it possible to reduce the amount of carbon dioxide emitted into the atmosphere when recycling lithium-ion batteries and to reduce the cost of carbon dioxide when producing lithium carbonate.
[0065] In the lithium carbonate production step S5 of the present embodiment, it is preferable to introduce the gaseous carbon dioxide recovered using the gas collection device in the carbon dioxide recovery step S2 directly into the leaching solution in which any of lithium sulfate, lithium chloride, and lithium nitrate is dissolved, through a gas supply pipe. When lithium carbonate is precipitated using gaseous carbon dioxide, components that affect the reaction for precipitating lithium carbonate are not introduced into the leaching solution, and higher quality lithium carbonate can be produced.
[0066] In the lithium carbonate production step S5, the carbon dioxide recovered with the aqueous sodium hydroxide solution in the carbon dioxide recovery step S2 may be used as a carbon dioxide source. In this case, the carbon dioxide recovered with the aqueous sodium hydroxide solution obtained in the carbon dioxide recovery step S2 may be added to a leachate in which any one of lithium sulfate, lithium chloride, and lithium nitrate is dissolved. In this method, carbon dioxide can be recovered and stored in the aqueous sodium hydroxide solution (alkaline solution tank), preventing carbon dioxide from being emitted as a gas. Furthermore, in this method, the reaction for producing lithium carbonate proceeds more quickly than in a method in which gaseous carbon dioxide is introduced. Therefore, the cost of carbon dioxide in lithium carbonate production can be more effectively reduced.
[0067] In the lithium carbonate production step S5 of the present embodiment, as the carbon dioxide source, only gaseous carbon dioxide recovered using a gas collection device may be used, only carbon dioxide recovered using an aqueous sodium hydroxide solution may be used, or both of them may be used.
[0068] In the above-described embodiment, lithium-ion battery sintered powder (black mass) formed using lithium-ion batteries recovered as recycled raw materials is used as the carbonate-containing raw material, but other materials such as incineration residue, dust, sludge, etc. may also be used. Furthermore, in the above-described embodiment, a leachate obtained by leaching black mass with an inorganic acid is used as the lithium-containing liquid for obtaining lithium carbonate, but a lithium-containing liquid generated when cathode scraps or an electrolyte are leached with acid may also be used.
[0069] (Lithium Carbonate Manufacturing Apparatus) As shown in FIG. 2 , the lithium carbonate manufacturing apparatus 10 of this embodiment has at least a reaction tank (leaching tank) 11, a carbon dioxide capture device 13, and a lithium carbonate production tank 14. The lithium carbonate manufacturing apparatus 10 of this embodiment may further have a solid-liquid separation tank 12. The reaction tank (leaching tank) 11 of this embodiment may be any reaction tank that can generate carbon dioxide from a raw material containing a carbonate using one or more inorganic acids selected from the group consisting of sulfuric acid, hydrochloric acid, and nitric acid. The carbon dioxide capture device 13 may be either or both of a gas capture device and an alkaline solution tank. The solid-liquid separation tank 12 may be a separation device, such as a filtration device, that separates a solid-liquid mixture generated in the reaction tank (leaching tank) 11 into solid and liquid. The lithium carbonate production tank 14 has a carbon dioxide supply means for supplying the carbon dioxide recovered in the carbon dioxide recovery device 13, and a leachate supply means for supplying the leachate separated in the solid-liquid separation tank 12 and containing any one of lithium sulfate, lithium chloride, and lithium nitrate dissolved therein, and may be any reaction tank capable of producing lithium carbonate.
[0070] According to the method for producing lithium carbonate and the apparatus for producing lithium of the present invention, high-quality lithium carbonate can be obtained while reducing carbon dioxide emissions and usage costs, thereby contributing to the reduction of greenhouse gases.
[0071] 10: Lithium carbonate production apparatus 11: Reaction tank (leaching tank) 12: Solid-liquid separation tank 13: Carbon dioxide recovery device 14: Lithium carbonate production tank
Claims
1. A method for producing lithium carbonate, comprising: a carbon dioxide generating step of generating carbon dioxide by adding an inorganic acid to a raw material containing a carbonate; a carbon dioxide recovering step of recovering the carbon dioxide; and a lithium carbonate producing step of adding the recovered carbon dioxide to a lithium-containing liquid to obtain lithium carbonate.
2. The method for producing lithium carbonate according to claim 1, wherein in the carbon dioxide recovery step, gaseous carbon dioxide is absorbed in an alkaline solution to recover the carbon dioxide.
3. The method for producing lithium carbonate according to claim 1, wherein the carbon dioxide recovery step recovers the carbon dioxide by capturing gaseous carbon dioxide.
4. The method for producing lithium carbonate according to claim 1, wherein the raw material contains a lithium compound.
5. The method for producing lithium carbonate according to claim 1, wherein the raw material is a lithium ion battery sintered powder obtained by sintering and pulverizing a lithium ion battery.
6. The method for producing lithium carbonate according to claim 1, wherein the inorganic acid is at least one selected from the group consisting of sulfuric acid, hydrochloric acid, and nitric acid.
7. The method for producing lithium carbonate according to claim 1, wherein in the carbon dioxide generation step, the temperature condition is in the range of 10°C or higher and 40°C or lower, and the pH condition is pH 6 or lower.
8. An apparatus for producing lithium carbonate, comprising: a reaction tank that generates carbon dioxide using a raw material containing a carbonate and an inorganic acid; a carbon dioxide capture device that captures the carbon dioxide; and a lithium carbonate production tank that supplies carbon dioxide from the carbon dioxide capture device to a lithium-containing liquid to produce lithium carbonate.
9. The apparatus for producing lithium carbonate according to claim 8, wherein the carbon dioxide capture device is a device for capturing gaseous carbon dioxide.
10. The apparatus for producing lithium carbonate according to claim 8, wherein the carbon dioxide recovery device is a device that captures carbon dioxide by causing an alkaline solution to absorb gaseous carbon dioxide.
Citation Information
Patent Citations
Method for treating waste lithium-ion battery
JP2022168616A
Game machine
JP2023058132A
Cancer determination device, cancer information acquiring method, and program
JP2024053899A
Lithium recovery method
JP6998241B2
Method for manufacturing high-purity nickel sulfate
WO2023286683A1
Cited By
Method for recovering lithium carbonate from wastewater containing impurity lithium fluoride mother liquor
CN121005454A