Separator for electrochemical device, and electrochemical device comprising same

The use of a separator with a porous polymer substrate and a coating layer composed of acrylic acid, acrylamide, and inorganic particles addresses the dimensional instability of lithium secondary battery separators, achieving low heat shrinkage and maintaining structural integrity under high-temperature wet conditions.

WO2024204992A1PCT designated stage expired Publication Date: 2024-10-03LG ENERGY SOLUTION LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/000984
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-01-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium secondary battery separators experience significant dimensional instability and heat shrinkage under high-temperature wet conditions, leading to electrode exposure and reduced adhesion, especially in lithium secondary batteries where the polymer binder content is low to accommodate varying battery types.

Method used

A separator with a porous polymer substrate and a porous coating layer containing an acrylic acid-based binder, an acrylamide-based binder, and inorganic particles, where the inorganic particles comprise 90% to 96% of the coating layer by weight, and the binder ratio is optimized to provide dimensional stability and ion conductivity while minimizing polymer binder content.

Benefits of technology

The separator achieves reduced heat shrinkage rates of 5% or less in a dry state and 10% or less in a wet state, preventing electrode exposure and maintaining structural integrity under high-temperature conditions, thus enhancing the reliability and performance of lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

The present invention relates to a separator for an electrochemical device, comprising a porous polymer substrate and a porous coating layer formed on at least one surface of the porous polymer substrate, wherein the porous coating layer comprises an acrylic binder, an acrylamide-based binder and inorganic particles, the porous coating layer comprises approximately 90-96 wt% of the inorganic particles on the basis of the total weight of the porous coating layer, and the weight ratio of the acrylic binder and the acrylamide-based binder is approximately 3:7 to 7:3.
Need to check novelty before this filing date? Find Prior Art

Description

Separator for electrochemical devices and electrochemical devices containing the same

[0001] This application is based upon and claims the benefit of priority from Korean Patent Application No. 10-2023-0038631, filed with the Korean Intellectual Property Office on March 24, 2023, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a separator for an electrochemical device and an electrochemical device including the same.

[0003] Electrochemical devices convert chemical energy into electrical energy using electrochemical reactions. Recently, electrochemical devices including lithium secondary batteries, which have high energy density and voltage, long cycle life, and can be used in various fields, are widely used.

[0004] A lithium secondary battery may include an electrode assembly manufactured with a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, and the electrode assembly may be manufactured by being housed in a case together with an electrolyte. The separator may include a porous coating layer including a polymer binder and inorganic particles on at least one surface of a porous substrate. The inorganic particles may be connected to other inorganic particles by the polymer binder to form an interstitial volume, and lithium ions may move through the interstitial volume. In addition to fixing the inorganic particles, the polymer binder may provide adhesiveness to the porous coating layer, and the porous coating layer may be adhered to the porous substrate and the electrode, respectively.

[0005] The purpose of the present invention is to provide a separator for an electrochemical device having a reduced dimensional change rate in a high-temperature wet state, a method for manufacturing the same, and an electrochemical device including the separator.

[0006] The present invention relates to obtaining a separation membrane that secures dimensional stability under high temperature and wet conditions while maintaining a relatively low content of polymer binder in a porous coating layer.

[0007] One aspect of the present invention provides a separator for an electrochemical device, comprising a porous polymer substrate and a porous coating layer formed on at least one surface of the porous polymer substrate, wherein the porous coating layer comprises an acrylic acid-based binder, an acrylamide-based binder, and inorganic particles, wherein the porous coating layer comprises about 90 wt% to 96 wt% of the inorganic particles based on the total weight of the porous coating layer, and wherein the weight ratio of the acrylic acid-based binder and the acrylamide-based binder is about 3:7 to 7:3.

[0008] The weight average molecular weight of the above acrylamide-based binder may be about 400,000 to 1,000,000.

[0009] The above porous coating layer is formed by coating a coating slurry containing the acrylic acid-based binder, the acrylamide-based binder, inorganic particles, a dispersant, and a dispersion medium on the porous polymer substrate, and the pH of the coating slurry may be 3 to 9.

[0010] The above acrylic acid-based binder may contain, as a repeating unit, one or more monomers selected from the group consisting of acrylic acid and methacrylic acid.

[0011] The above acrylamide-based binder may include, as a repeating unit, one or more monomers selected from the group consisting of acrylamide, methacrylamide, N-ethylacrylamide, ethylmethacrylamide, N-propylacrylamide, N-isopropylacrylamide, N-isopropylmethacrylamide, N-butylacrylamide, and N-butylmethacrylamide.

[0012] In the porous coating layer, the content of the acrylic acid-based binder may be greater than or equal to the content of the acrylamide-based binder.

[0013] Another aspect of the present invention provides an electrochemical device comprising an anode, a cathode, and a separator disposed between the anode and the cathode, wherein the separator is a separator for another electrochemical device on the one side.

[0014] The above electrochemical device may be a lithium secondary battery.

[0015] The above electrochemical device may further include an electrolyte solution including a solvent in which ethylene carbonate (EC) / ethyl methyl carbonate (EMC) is mixed in a weight ratio of about 3 / 7 or a solvent in which ethylene carbonate (EC) / ethyl methyl carbonate (EMC) / dimethyl carbonate (DMC) is mixed in a weight ratio of about 20 / 5 / 75.

[0016] The separator for an electrochemical device according to the present invention can provide improved dimensional stability in a dry state and a wet state impregnated with an electrolyte. For example, the separator has a dry state thermal shrinkage of about 5% or less under a high temperature condition of 200°C or higher, and a wet state thermal shrinkage of about 10% or less under a high temperature condition of 130°C or higher, thereby preventing electrode exposure due to thermal shrinkage of the separator.

[0017] Hereinafter, each component of the present invention will be described in more detail so that a person having ordinary skill in the art to which the present invention pertains can easily practice it; however, this is only an example, and the scope of the rights of the present invention is not limited by the following contents.

[0018] The term "comprises" as used herein is used to list materials, compositions, devices, and methods useful in the present invention, but is not limited to the listed examples.

[0019] As used herein, the terms "about," "approximately," and "substantially" are used to mean a range or approximation of a numerical value or degree, taking into account inherent manufacturing and material tolerances, and are used to prevent infringers from unfairly exploiting the disclosure, which includes precise or absolute numerical values ​​provided to aid understanding of the present invention.

[0020] As used herein, “electrochemical device” may refer to a primary battery, a secondary battery, a super capacitor, etc.

[0021] As used herein, “wet state” may mean a state in which the separator is impregnated with at least a portion of the electrolyte, and “dry state” may mean a dry state in which the separator is not impregnated with the electrolyte.

[0022] As used herein, “durability” may mean a property of the binder to exhibit adhesive strength or mechanical strength as its original properties without swelling or deformation when in contact with an electrolyte.

[0023] In the electrode assembly that constitutes a secondary battery, the separator is a film material that has the function of isolating the two electrodes (anode / cathode) to prevent electrical short circuits caused by physical contact, and providing a passage for ions to move between the two electrodes through the electrolyte contained within the micropores, thereby providing ion conductivity.

[0024] The porous coating layer formed on one side of the separator contains a polymer binder and inorganic particles and can prevent thermal shrinkage of the porous polymer substrate. The separator including the porous coating layer exhibits excellent dimensional stability in a dry state without an electrolyte, but in a wet state where the separator is impregnated with an electrolyte, the polymer binder may swell due to the electrolyte, or the adhesive strength of the polymer binder may decrease when the separator is exposed to a temperature of about 130℃ or higher depending on the operating conditions of the lithium secondary battery including the separator. That is, in such a high-temperature wet state, the adhesive strength of the porous coating layer decreases and the separator tends to shrink significantly. For example, a cylindrical battery that inserts the electrode assembly into a case while the electrode assembly is wound and tensioned requires relatively less adhesive strength between the electrode and the separator than a pouch-type battery, so there is a problem that the dimensional stability in the wet state is lowered due to a small content of polymer binder.

[0025] The present invention provides a separation membrane having improved dimensional stability under high temperature and wet conditions while maintaining a relatively low content of polymer binder in the porous coating layer.

[0026] One specific example of the present invention provides a separator for an electrochemical device, comprising a porous polymer substrate and a porous coating layer formed on at least one surface of the porous polymer substrate, wherein the porous coating layer includes an acrylic acid-based binder, an acrylamide-based binder, and inorganic particles, wherein the porous coating layer includes the inorganic particles at about 90 wt% to 96 wt% based on the total weight of the porous coating layer, and the weight ratio of the acrylic acid-based binder and the acrylamide-based binder is about 3:7 to 7:3.

[0027] The porous polymer substrate may be a porous membrane having a plurality of pores formed therein, which electrically insulates the positive and negative electrodes to prevent short circuits. For example, when the electrochemical device is a lithium secondary battery, the porous polymer substrate may be an ion-conductive barrier that blocks electrical contact between the positive and negative electrodes while allowing lithium ions to pass through. At least a portion of the pores may form a three-dimensional network that connects the surface and the interior of the porous polymer substrate, and a fluid may pass through the porous polymer substrate through the pores.

[0028] The porous polymer substrate may use a material that is physically and chemically stable with respect to the organic solvent electrolyte. For example, the porous polymer substrate may include, but is not limited to, a resin such as a polyolefin-based resin such as polyethylene, polypropylene, and polybutylene, polyvinyl chloride, polyethylene terephthalate, polycycloolefin, polyethersulfone, polyamide, polyimide, polyimideamide, nylon, polytetrafluoroethylene, and copolymers or mixtures thereof. For example, a polyolefin-based resin may be used. Polyolefin-based resins can be processed into a relatively thin thickness and are easy to apply a coating slurry, making them suitable for manufacturing electrochemical devices with a higher energy density.

[0029] The porous polymer substrate may have a single-layer or multi-layer structure. The porous polymer substrate may include two or more polymer resin layers having different melting points (Tm), thereby providing a shutdown function in the event of a high-temperature runaway of the battery. For example, the porous polymer substrate may include a polypropylene layer having a relatively high melting point and a polyethylene layer having a relatively low melting point. The porous polymer substrate may have a three-layer structure in which polypropylene, polyethylene, and polypropylene are laminated in that order. The polyethylene layer melts when the temperature of the battery rises above a predetermined temperature, thereby shutting down the pores, thereby preventing thermal runaway of the battery.

[0030] The thickness of the porous polymer substrate may be approximately 1 ㎛ to 100 ㎛. For example, the thickness of the porous polymer substrate may be approximately 10 ㎛ to 90 ㎛, 20 ㎛ to 80 ㎛, 30 ㎛ to 70 ㎛, or 40 ㎛ to 60 ㎛. For example, the thickness of the polymer substrate may be approximately 1 ㎛ to 30 ㎛. For example, the thickness of the polymer substrate may be approximately 5 ㎛ to 15 ㎛, or 8 ㎛ to 13 ㎛. By controlling the thickness of the porous polymer substrate within the above-described range, the volume of the electrochemical device can be minimized while electrically insulating the positive and negative electrodes, thereby increasing the amount of active material included in the electrochemical device.

[0031] The porous polymer substrate may include pores having an average diameter of approximately 0.01 μm to 1 μm. For example, the size of the pores included in the porous polymer substrate may be approximately 0.01 μm to 0.09 μm, 0.02 μm to 0.08 μm, 0.03 μm to 0.07 μm, or 0.04 μm to 0.06 μm. For example, the size of the pores may be approximately 0.02 μm to 0.06 μm. By controlling the pore size of the porous polymer substrate within the above-described range, the air permeability and ionic conductivity of the entire manufactured membrane can be controlled.

[0032] The porous polymer substrate may have a permeability of approximately 10 s / 100cc or more and 100 s / 100cc or less. For example, the permeability of the porous polymer substrate may be approximately 10 s / 100cc or more and 90 s / 100cc or less, 20 s / 100cc or more and 80 s / 100cc or less, 30 s / 100cc or more and 70 s / 100cc or less, or 40 s / 100cc or more and 60 s / 100cc or less. For example, the permeability of the porous polymer substrate may be approximately 50 s / 100cc or more and 70 s / 100cc or less. When the permeability of the porous polymer substrate is within the above-described range, the permeability of the manufactured separator may be provided within a range suitable for securing the output and cycle characteristics of the electrochemical device.

[0033] The above air permeability (s / 100cc) means the time (in seconds) it takes for 100cc of air to pass through a porous polymer substrate or membrane of a predetermined area under a constant pressure. The above air permeability can be measured using an air permeability tester (Gurley densometer) according to ASTM D 726-58, ASTM D726-94 or JIS-P8117. For example, using a 4110N device from Gurley, air at a pressure of 0.304 kPa or air at a pressure of 1.215 kN / m 2100 cc of air under the pressure of water occupies 1 square inch (or 6.54 cm 2 ) can be used to measure the time it takes for 100 cc of air to pass through a 1-square-inch sample under a constant pressure of 4.8 inches of water at room temperature. For example, using the ASAHI SEIKO EG01-55-1MR equipment, the time it takes for 100 cc of air to pass through a 1-square-inch sample can be measured.

[0034] The porous polymer substrate may have a porosity of approximately 10 vol% to 60 vol%. For example, the porosity of the porous polymer substrate may be approximately 15 vol% to 55 vol%, 20 vol% to 50 vol%, 25 vol% to 45 vol%, or 30 vol% to 40 vol%. For example, the porosity of the porous polymer substrate may be approximately 30 vol% to 50 vol%. When the porosity of the porous polymer substrate is within the above-described range, the ionic conductivity of the manufactured separator may be provided within a range suitable for securing the output and cycle characteristics of the electrochemical device.

[0035] The above porosity refers to the volume ratio of pores to the total volume of the porous polymer substrate. The porosity can be measured by methods known in the art. For example, it can be measured by the BET (Brunauer Emmett Teller) measurement method using nitrogen gas adsorption, the capillary flow porosimetry method, or the water or mercury intrusion method.

[0036] The above porous coating layer is formed on at least one surface of the above porous polymer substrate and includes a polymer binder and inorganic particles, and the polymer particles may include an acrylic acid-based binder and an acrylamide-based binder.

[0037] The porous coating layer may be formed by coating at least one surface of a porous polymer substrate with a coating slurry containing an acrylic acid-based binder, an acrylamide-based binder, inorganic particles, a dispersant, and a dispersion medium. For example, the separator may be manufactured by applying the coating slurry to at least one surface of a porous polymer substrate and then drying to remove the dispersion medium. The porous coating layer includes an interstitial volume in which the inorganic particles are connected by the acrylic acid-based binder and the acrylamide-based binder, and allows lithium ions to pass therethrough while adhering to the porous polymer substrate to prevent thermal shrinkage of the porous polymer substrate.

[0038] The above coating slurry can include a dispersion medium to dissolve or disperse at least a portion of the acrylic acid-based binder or the acrylamide-based binder, and can disperse inorganic particles. The coating slurry can be used in which the polymer binder and inorganic particles are uniformly dispersed by controlling the type and content of the dispersion medium. For example, the dispersion medium can be one selected from the group consisting of water, ethanol, acetone, isopropyl alcohol (IPA), dimethylacetamide (DMAc), dimethylformamide (DMF), N-methyl-2-pyrrolidone (NMP), acetonitrile, and combinations thereof. Using the above-described type of dispersion medium, a porous coating layer in which inorganic particles are uniformly dispersed can be formed.

[0039] The above coating slurry can contain a dispersant to maintain a uniformly dispersed state of the acrylic acid-based binder, the acrylamide-based binder, and the inorganic particles. For example, the dispersant can contain at least one selected from the group consisting of a soluble polyamine, a soluble amine compound, fatty acids, fatty alcohols, sorbitan fatty acid ester, tannic acid, pyrogallic acid, and polyacrylic acid. For example, the dispersant can be a polyacrylic acid-based polymer dispersant. By using the above-described type of dispersant, the stability of the coating slurry can be improved, and the uniformity of the porous coating layer formed with the coating slurry can be secured.

[0040] The dispersant may be included in an amount of approximately 0.01 wt% to 5 wt% based on the total weight of the coating slurry. For example, the content of the dispersant may be included in an amount of 0.1 wt% to 4 wt%, 0.5 wt% to 3 wt%, or 1 wt% to 2 wt%. For example, the content of the dispersant may be approximately 3 wt% to 5 wt%. By controlling the content of the dispersant within the above-described range, uniform dispersion and stability of the polymer binder and inorganic particles included in the coating slurry can be achieved.

[0041] The coating slurry including the dispersant may have a pH of about 3 to 9. For example, the pH of the coating slurry may be about 3.5 to 8.5, 4.0 to 8.0, 4.5 to 7.5, 5.0 to 7.0, or 5.5 to 6.5. For example, the pH of the coating slurry may be about 5.5 to 8.5, or about 6.0 to 8.0. The pH of the coating slurry may be adjusted by changing the type or properties of the dispersant. For example, the dispersant may be a polyacrylic acid-based polymer dispersant, and the pH of the coating slurry may be adjusted by adjusting the degree of substitution of the polyacrylic acid-based polymer dispersant. For example, in the polyacrylic acid-based polymer dispersant, -COOH may be replaced with -COOH. - Na + By controlling the degree of substitution, the pH of the coating slurry can be controlled. By controlling the pH of the coating slurry within the above-described range, the adhesion to inorganic particles can be improved through uniform dispersion of the polymer binder, particularly the acrylic acid-based binder, contained in the coating slurry, thereby reducing thermal shrinkage of the porous coating layer and the separator comprising the same.

[0042] The coating slurry including the above dispersant may have a viscosity of about 10 cps or more and 500 cps or less. For example, the viscosity of the coating slurry may be about 50 cps or more and 450 cps or less, 100 cps or more and 400 cps or less, 150 cps or more and 350 cps or less, or 200 cps or more and 300 cps or less. For example, the viscosity of the coating slurry may be about 10 cps or more and 100 cps or less, or about 10 cps or more and 50 cps or less. When the viscosity of the coating slurry exceeds 500 cps, lumps having an average particle size (D99) of about 100 ㎛ are formed, making it difficult to manufacture a separation membrane through continuous application to a porous polymer substrate, thereby making it impossible to secure productivity.

[0043] The above coating slurry may further include additives such as a surfactant, an antifoaming agent, a flame retardant, and a wetting agent. The additives may be included in an amount of about 0 wt% to about 10 wt% based on the total weight of the coating slurry. For example, the content of the additive may be about 0.01 wt% to about 9 wt%, 0.1 wt% to about 8 wt%, 1 wt% to about 7 wt%, 2 wt% to about 6 wt%, or 3 wt% to about 5 wt%. For example, the content of the additive may be about 1 wt% to about 5 wt%. By controlling the content of the additive within the above-described range, the dimensional stability and flame retardancy of the porous coating layer formed by the coating slurry can be secured.

[0044] The dispersion medium included in the above coating slurry may be removed by drying or heating after the porous coating layer is formed. For example, the porous coating layer may include the dispersion medium at 5 ppm or less. For example, the porous coating layer may be composed of an acrylic acid-based binder, an acrylamide-based binder, inorganic particles, and a dispersant. In the process of removing the dispersion medium, a plurality of pores may be formed on the surface and inside of the porous coating layer. The pores may include an interstitial volume formed by connecting adjacent inorganic particles by the acrylic acid-based binder, the acrylamide-based binder, or both, and may have a structure that forms a three-dimensional network through which a fluid can pass.

[0045] The thickness of the porous coating layer may be approximately 1 ㎛ to 15 ㎛. For example, the thickness of the porous coating layer may be approximately 2 ㎛ to 14 ㎛, 3 ㎛ to 13 ㎛, 4 ㎛ to 12 ㎛, 5 ㎛ to 11 ㎛, 6 ㎛ to 10 ㎛, or 7 ㎛ to 9 ㎛. For example, the thickness of the porous coating layer may be approximately 1 ㎛ to 5 ㎛. For example, the thickness of the porous coating layer may be approximately 1.5 ㎛ to 3.5 ㎛. By controlling the thickness of the porous coating layer within the above-described range, shrinkage of the porous polymer substrate can be minimized and stable adhesion to the porous polymer substrate can be achieved.

[0046] The acrylic acid-based binder can bind inorganic particles included in the porous coating layer and provide adhesion to the porous polymer substrate of the porous coating layer. The acrylic acid-based binder may contain, as a repeating unit, one or more monomers selected from the group consisting of acrylic acid and methacrylic acid. For example, the acrylic acid-based binder may be polyacrylic acid (PAA).

[0047] When the acrylic acid-based binder is included in a coating slurry, the dispersibility thereof can be determined by the pH concentration of the coating slurry. When the pH of the coating slurry is 3 to 9, the binding of inorganic particles by the acrylic acid-based binder and the resulting dimensional stability of the porous coating layer can be secured.

[0048] The weight average molecular weight (Mw) of the acrylic acid-based binder may be approximately 50,000 or more and 400,000 or less. For example, the weight average molecular weight of the acrylic acid-based binder may be approximately 100,000 or more and 350,000 or less, 150,000 or more and 300,000 or less, or 200,000 or more and 250,000 or less. For example, the weight average molecular weight of the acrylic acid-based binder may be approximately 100,000 or more and 200,000 or less. By controlling the weight average molecular weight of the acrylic acid-based binder within the above-described range, it is possible to realize dense bonding of the inorganic particles through uniform mixing with the inorganic particles in the porous coating layer, thereby reducing the thermal shrinkage rate of the separator.

[0049] In the present invention, the weight average molecular weight of the polymer binder can be measured by gel permeation chromatography (GPC: gel permeation chromatography, PL GPC220, Agilent Technologies). For example, the weight average molecular weight can be measured using an Agilent High Temperature RI detector under the conditions of a PL Olexis (Polymer Laboratories) column (column temperature: 160°C), TCB (Trichlorobenzene) as a solvent, a sample concentration of 1.0 mg / mL, a flow rate of 1.0 mL / min, and an injection volume of 200 μL (corrected by a third-order function, standard: Polystyrene).

[0050] The acrylamide-based binder may be included in a porous coating layer to provide durability of the porous coating layer against an electrolyte. The acrylamide-based binder may include, as a repeating unit, one or more monomers selected from the group consisting of acrylamide, methacrylamide, N-ethylacrylamide, ethylmethacrylamide, N-propylacrylamide, N-isopropylacrylamide, N-isopropylmethacrylamide, N-butylacrylamide, and N-butylmethacrylamide. The butylacrylamide may collectively refer to sec-butylacrylamide and tert-butylacrylamide, and the butylmethacrylamide may collectively refer to sec-butylmethacrylamide and tert-butylmethacrylamide. For example, the acrylamide-based binder may be polyacrylamide (PAM).

[0051] The weight average molecular weight (Mw) of the acrylamide-based binder may be approximately 400,000 or more and 1,000,000 or less. For example, the weight average molecular weight of the acrylamide-based binder may be approximately 450,000 or more and 950,000 or less, 500,000 or more and 900,000 or less, 550,000 or more and 850,000 or less, 600,000 or more and 800,000 or less, or 650,000 or more and 750,000 or less. For example, the weight average molecular weight of the acrylamide-based binder may be approximately 400,000 or more and 900,000 or less. By controlling the weight average molecular weight of the acrylamide-based binder within the above-described range, the viscosity of the coating slurry may not exceed 500 cps, thereby forming a porous coating layer and reducing the thermal shrinkage rate of the separator.

[0052] The porous coating layer may contain the acrylic acid-based binder and the acrylamide-based binder in a weight ratio of about 3:7 to 7:3. For example, the porous coating layer may contain the acrylic acid-based binder and the acrylamide-based binder in a weight ratio of about 4:6 to 6:4, for example, in a weight ratio of about 4.5:5.5 to 5.5:4.5. For example, the porous coating layer may satisfy the above-described range, and the content of the acrylic acid-based binder may be greater than the content of the acrylamide-based binder. For example, the porous coating layer may contain the acrylic acid-based binder and the acrylamide-based binder in a weight ratio of about 6:4 to 5:5.

[0053] The acrylic acid-based binder can easily interact with inorganic particles compared to the acrylamide-based binder, thereby contributing to the formation of the interstitial volume described above. For example, the acrylic acid-based binder can exhibit electrostatic attraction to inorganic particles or form hydrogen bonds through a carboxyl group. The acrylamide-based binder exhibits a greater modulus than the acrylic acid-based binder, thereby contributing to securing durability by maintaining the structure of the porous coating layer even when the separator is in a wet state impregnated with an electrolyte. By adjusting the contents of the acrylic acid-based binder and the acrylamide-based binder within the above-described range, the formation of the interstitial volume by the acrylic acid-based binder and the structural stability of the porous coating layer by the acrylamide-based binder can be simultaneously secured. A separator having a porous coating layer satisfying the above-described range can have reduced thermal shrinkage in a wet state. If the content of the acrylic acid-based binder is greater than the above-described range, the structural stability of the porous coating layer in a wet state may decrease, resulting in rapid thermal shrinkage. If the content of the acrylamide-based binder is greater, the inorganic particles may not be sufficiently bound in a dry state, resulting in rapid thermal shrinkage.

[0054] The above porous coating layer contains an acrylic acid-based binder and an acrylamide-based binder, and does not contain a copolymer of the acrylic acid-based binder and the acrylamide-based binder. The mixed use of the acrylic acid-based binder and the acrylamide-based binder makes it easy to control the weight average molecular weight and content ratio of the individual binders compared to the use of the copolymer, so that the advantages according to the weight average molecular weight range and the advantages according to the content range can be easily achieved simultaneously.

[0055] The porous coating layer may contain the inorganic particles in an amount of about 90 wt% to 96 wt% based on the total weight of the porous coating layer. For example, the content of the inorganic particles based on the total weight of the porous coating layer may be about 90.5 wt% to 95.5 wt%, 91.0 wt% to 95.0 wt%, 91.5 wt% to 94.5 wt%, 92.0 wt% to 94.0 wt%, or 92.5 wt% to 93.5 wt%. For example, the porous coating layer may contain the inorganic particles in an amount of about 93 wt% to 96 wt%. In the above-described range, a separator having mechanical strength suitable for a cylindrical battery and having reduced thermal shrinkage in a wet state can be manufactured. Meanwhile, even if the content of the inorganic particles relative to the total weight of the porous coating layer deviates from the aforementioned range to some extent within the error range, for example, slightly below 90 wt% or slightly exceeding 96 wt% within the error range, it still does not deviate from the spirit of the present invention.

[0056] The above inorganic particles can be used as electrochemically stable particles. The above inorganic particles can be used in the operating voltage range of the electrochemical device (e.g., Li / Li +There is no particular limitation as long as no oxidation and / or reduction reaction occurs at 0 to 5 V as a standard. In particular, when using inorganic particles with a high dielectric constant as inorganic particles, it can contribute to increasing the degree of dissociation of electrolyte salt, such as lithium salt, in the liquid electrolyte, thereby improving the ionic conductivity of the electrolyte. For the reasons described above, it is preferable that the inorganic particles include high-dielectric constant inorganic particles having a dielectric constant of about 5 or more, for example, about 10 or more. Non-limiting examples of inorganic particles having a dielectric constant of 5 or more include BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT, 0 <x<1, 0<y<1), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3(PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, Al(OH)3, SiC, AlOOH, TiO2 or mixtures thereof.

[0057] In addition, inorganic particles having lithium ion transfer capability, i.e., inorganic particles containing lithium element but having the function of transferring lithium ions without storing lithium, can be used. Non-limiting examples of inorganic particles having lithium ion transfer capability include lithium phosphate (Li3PO4), lithium titanium phosphate (Li). x Ti y (PO4)3, 0 < x <2, 0 < y <3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3), 14Li2O-9Al2O3-38TiO2-39P2O5, etc. (LiAlTiP) x O ySeries glass (0 <x < 4, 0 < y < 13), 리튬란탄티타네이트(Li x La y TiO3, 0 < x <2, 0 <y <3), Li 3.25 Ge 0.25 P 0.75 Lithium germanium thiophosphate (Li) such as S4 x Ge y P z S w , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), lithium nitride (Li 3 N ), etc. x N y , 0 < x <4, 0 < y < 2), SiS2 series glass (Li) such as Li3PO4-Li2S-SiS2 x Si y S z , 0 < x < 3, 0 <y < 2, 0 < z < 4), LiI-Li2S-P2S5등과 같은 P2S5계열 glass(Li x P y S z , 0 < x < 3, 0< y < 3, 0 < z < 7) or mixtures thereof.

[0058] In addition, as the inorganic particles, inorganic particles having flame retardancy can be used to impart flame retardant properties to the separator or to prevent a rapid increase in temperature inside the electrochemical device. Non-limiting examples of inorganic particles having flame retardancy include Sb2O3, Sb2O4, Sb2O5, SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, Zn2SnO4, ZnSnO3, ZnSn(OH)6, ZrO2, Y2O3, SiO2, Al2O3, AlOOH, Al(OH)3, SiC, TiO2, H3BO3, HBO2, and mixtures thereof.

[0059] The average particle diameter (D50) of the above-mentioned inorganic particles may be approximately 50 nm to 5,000 nm. For example, the average particle diameter (D50) of the above-mentioned inorganic particles may be approximately 100 nm to 4,500 nm, 200 nm to 4,000 nm, 300 nm to 3,000 nm, 400 nm to 2,000 nm, or 500 nm to 1,000 nm. If the average particle diameter of the inorganic particles is less than approximately 50 nm, as the specific surface area increases, an additional polymer binder is required for bonding between the inorganic particles, which is disadvantageous in terms of electrical resistance. If the average particle diameter of the inorganic particles exceeds 5,000 nm, the uniformity of the surface of the coating layer is lowered, and damage to the porous polymer substrate or electrode may occur during lamination.

[0060] The aspect ratio of the above-described inorganic particles may be approximately 1 or more and 2 or less. For example, the aspect ratio of the above-described inorganic particles may be approximately 1.1 or more and 1.9 or less, 1.2 or more and 1.8 or less, 1.3 or more and 1.7 or less, or 1.4 or more and 1.6 or less. By controlling the aspect ratio of the above-described inorganic particles within the above-described range, it is possible to form a porous coating layer including an interstitial volume that facilitates the movement of the polymer binder through the pores between the inorganic particles and ultimately enables the movement of lithium ions.

[0061] The BET surface area of ​​the above inorganic particles is approximately 5 m 2 / g or more 25 m 2 / g or less. For example, the BET surface area of ​​the inorganic particles is about 6 m 2 / g or more 24 m 2 / g or less, 7 m 2 / g or more 23 m 2 / g or less, 8 m 2 / g or more 22 m 2 / g or less, 9 m 2 / g or more 21 m 2 / g or less, 10 m 2 / g or more than 20 m 2 / g or less, 11 m 2 / g or more than 19 m 2 / g or less, 12 m 2 / g or more than 18 m 2 / g or less, 13 m 2 / g or more than 17 m 2 / g or less or 14 m 2 / g or more 26 m 2 / g or less. By controlling the BET specific surface area of ​​the inorganic particles within the above-described range, the movement of the polymer binder through the pores between the inorganic particles can be controlled.

[0062] The separator for the electrochemical device may have a permeability of approximately 50 s / 100cc or more and 150 s / 100cc or less. For example, the permeability of the separator may be approximately 60 s / 100cc or more and 140 s / 100cc or less, 70 s / 100cc or more and 130 s / 100cc or less, 80 s / 100cc or more and 120 s / 100cc or less, or 90 s / 100cc or more and 110 s / 100cc or less. For example, the permeability of the separator may be approximately 100 s / 100cc or more and 120 s / 100cc or less. When the permeability of the separator is within the above-described range, the output, stability, and cycle characteristics of the electrochemical device can be secured.

[0063] The thermal shrinkage of the separator for the electrochemical device may be approximately 10% or less. For example, the dry state thermal shrinkage of the separator may be 5% or less, and the wet state thermal shrinkage may be 10% or less. For example, the dry state thermal shrinkage may be a dimensional change rate based on when the separator is exposed to 200°C for 30 minutes, and the wet state thermal shrinkage may be a dimensional change rate based on when the separator is exposed to 135°C for 30 minutes in a state in which the separator is impregnated with an electrolyte. For example, the dry state thermal shrinkage of the separator may be approximately 5% or less in both the MD direction and the TD direction, and the wet state thermal shrinkage may be approximately 10% or less in both the MD direction and the TD direction.

[0064] When a cell is manufactured using the above electrochemical device separator, the cell may have an electrical resistance of approximately 0.5 Ohm or more and 1.5 Ohm or less. For example, the electrical resistance of the cell may be approximately 0.6 Ohm or more and 1.4 Ohm or less, 0.7 Ohm or more and 1.3 Ohm or less, 0.8 Ohm or more and 1.2 Ohm or less, or 0.9 Ohm or more and 1.1 Ohm or less. For example, the electrical resistance of the cell may be approximately 0.6 Ohm or more and 0.8 Ohm or less.

[0065]

[0066] Another specific example of the present invention provides an electrochemical device comprising a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the separator is a separator for the electrochemical device of the above-described specific example. The electrochemical device can be manufactured by inserting and sealing an electrode assembly comprising the positive electrode, the negative electrode, and the separator interposed between the positive electrode and the negative electrode into a case or pouch. An electrolyte may be injected into the case or pouch before sealing to impregnate the electrode assembly with the electrolyte. The shape of the case or pouch is not limited. For example, the electrochemical device can be a cylindrical, square, coin-shaped, or pouch-shaped lithium secondary battery.

[0067] The positive electrode and the negative electrode may be coated by applying and drying an electrode active material on at least one surface of each current collector. The current collector may be a material that is conductive and does not cause a chemical change in the electrochemical device. For example, the current collector for the positive electrode may be, but is not limited to, aluminum, nickel, titanium, sintered carbon, stainless steel; aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc.; and the like. For example, the current collector for the negative electrode may be, but is not limited to, copper, nickel, titanium, sintered carbon, stainless steel; copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc.; and the like. The current collector may be in various forms, such as a metal plate, film, foil, net, porous body, or foam body.

[0068] The positive electrode has a positive electrode current collector and a positive electrode active material layer including a positive electrode active material, a conductive material, and a binder resin on at least one surface of the positive electrode current collector. The positive electrode active material is a layered compound such as lithium manganese oxide (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; chemical formula Li 1+x Mn 2-x Lithium manganese oxides such as O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; chemical formula LiNi 1-x M x Ni-site type lithium nickel oxide represented by O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga and x = 0.01 to 0.3); chemical formula LiMn 1-x M xA lithium manganese composite oxide represented by O2 (wherein, M = Co, Ni, Fe, Cr, Zn or Ta, and x = 0.01 to 0.1) or Li2Mn3MO8 (wherein, M = Fe, Co, Ni, Cu or Zn); LiMn2O4 in which a portion of Li in the chemical formula is replaced by an alkaline earth metal ion; a disulfide compound; or a mixture of two or more of Fe2(MoO4)3.

[0069] The above negative electrode has a negative electrode current collector and a negative electrode active material layer including a negative electrode active material, a conductive material, and a binder resin on at least one surface of the current collector. The negative electrode includes carbon such as lithium metal oxide, non-graphitizable carbon, and graphite carbon as the negative electrode active material; LixFe2O3(0≤x≤1), Li x WO2(0≤x≤1), Si, SiO x (0 <x<2), SiC, Si 합금 등의 실리콘계 재료; Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of group 1, 2, and 3 of the periodic table, halogens; 0 <x≤1; 1≤y≤3; 1≤z≤8) 등의 금속 복합 산화물; 리튬 금속; 리튬 합금; 주석계 합금; SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, 및 Bi2O5등의 금속 산화물; 폴리아세틸렌 등의 도전성 고분자; Li-Co-Ni 계 재료; 티타늄 산화물 중 선택된 1종 또는 2종 이상의 혼합물을 포함할 수 있다.

[0070] The conductive material may be one or a mixture of two or more conductive materials selected from the group consisting of graphite, carbon black, carbon fibers or metal fibers, metal powders, conductive whiskers, conductive metal oxides, carbon nanotubes, activated carbon, and polyphenylene derivatives. The carbon nanotubes have a graphite sheet in the shape of a cylinder with a nano-sized diameter, and sp 2 It has a bonding structure, and exhibits the characteristics of a conductor or a semiconductor depending on the angle and structure at which the graphite plane is rolled. Carbon nanotubes can be classified into single-walled carbon nanotubes (SWCNTs), double-walled carbon nanotubes (DWCNTs), and multi-walled carbon nanotubes (MWCNTs) depending on the number of bonds forming the wall, and these carbon nanotubes can be appropriately selected depending on the use of the dispersion. For example, it can be one selected from the group consisting of natural graphite, artificial graphite, super-p, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, Denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide, or a mixture of two or more conductive materials among these.

[0071] As the above binder resin, a binder resin commonly used in electrodes of electrochemical devices can be used. Non-limiting examples of such binder resins include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-cotrichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate. Examples thereof include, but are not limited to, cellulose acetatepropionate, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, and carboxyl methyl cellulose.

[0072] The above electrolyte is A + B - As a salt with the same structure as A + is Li + , Na +, K + Contains ions composed of alkali metal cations or combinations thereof, such as B - is PF6 - , BF4 - , Cl - , Br - , I - , ClO4 - , AsF6 - , CH3CO2 - , CF3SO3 - , N(CF3SO2)2 - , C(CF2SO2)3 - A salt comprising an anion such as or a combination thereof may be dissolved or dissociated in an organic solvent comprising propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma butyrolactone (γ-butyrolactone) or a mixture thereof.

[0073] For example, the electrolyte may include a solvent having a weight ratio of EC / EMC of approximately 3 / 7 or a solvent having a weight ratio of ethylene carbonate (EC) / ethyl methyl carbonate (EMC) / dimethyl carbonate (DMC) of approximately 20 / 5 / 75, and the dimensional stability of the separator according to the specific example may be maximized.

[0074] The electrochemical device including the electrode assembly may be a lithium secondary battery. The battery may be used as a unit cell, and may be used as a battery module including the unit cell, a battery pack including the battery module, or a device including the battery pack as a power source. The devices may include, but are not limited to, small devices such as computers, mobile phones, and power tools; electric vehicles including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs) that are powered by an electric motor; electric two-wheeled vehicles including electric bicycles (E-bikes) and electric scooters; electric golf carts; and power storage systems.

[0075]

[0076] Another specific embodiment of the present invention provides a method for manufacturing a separator for an electrochemical device, comprising the step of forming a porous coating layer comprising an acrylic acid-based binder, an acrylamide-based binder, and inorganic particles on at least one surface of a porous polymer substrate. Any content overlapping with that described in the above-described separator for an electrochemical device will be replaced with the description of the preceding specific embodiment.

[0077] The step of forming the porous coating layer may include preparing a coating slurry including an acrylic acid-based binder and an acrylamide-based binder as polymer binders, inorganic particles, a dispersant, and a dispersion medium, applying the coating slurry to a porous polymer substrate, and drying the coating slurry. For example, the coating slurry may be prepared by first mixing the acrylamide-based binder, inorganic particles, a dispersant, and a dispersion medium, and then adding the acrylic acid-based binder to prevent agglomeration and precipitation of the acrylamide-based binder and the acrylic acid-based binder.

[0078] The step of forming the porous coating layer may further include a step of corona discharge treating at least one surface of the porous polymer substrate before applying the coating slurry to the porous polymer substrate. The step of corona discharge treating at least one surface of the porous polymer substrate can prevent a decrease in the bonding strength between the surface of the porous polymer substrate and the surface of the coating layer at high temperatures, and can prevent a decrease in the bonding strength between the surface of the polymer substrate and the surface of the coating layer due to an electrolyte.

[0079] The corona discharge treatment may be a treatment of at least one surface of the porous polymer substrate with a voltage of 0.1 kV or more and 10 kV or less in air. For example, the corona discharge treatment may be a treatment with a voltage of 0.2 kV or more and 9 kV or less, 0.3 kV or more and 8 kV or less, 0.4 kV or more and 7 kV or less, 0.5 kV or more and 6 kV or less, 0.6 kV or more and 5 kV or less, 0.7 kV or more and 4 kV or less, 0.8 kV or more and 3 kV or less, 0.9 kV or more and 2 kV or less, or 1.0 kV or more and 2 kV or less in air. For example, the corona discharge treatment may be a treatment with a voltage of 1.8 kV in air. By controlling the applied voltage of the corona discharge treatment within the above-described range, an appropriate number of functional groups can be formed on the surface of the polymer substrate, and damage to the surface of the polymer substrate can be prevented.

[0080] The step of forming the porous coating layer may include coating the porous polymer substrate by applying the coating slurry. For example, the coating may be formed by a method such as a bar coater, a wire bar coater, a roll coater, a spray coater, a spin coater, an inkjet coater, a screen coater, a reverse coater, a gravure coater, a knife coater, a slot die coater, a hot melt coater, a comma coater, a direct metering coater, etc., but is not limited thereto. For example, the step of forming the coating layer may be to simultaneously coat the coating slurry on both sides of the porous polymer substrate using a bar coater or a slot die coater.

[0081] The step of forming the porous coating layer may include applying the coating slurry to a porous polymer substrate and then drying or heating the coating layer to evaporate the dispersion medium included in the coating layer. The removal of the dispersion medium may be performed at a temperature that can evaporate only the dispersion medium included in the coating layer without deforming the polymer binder included in the coating layer. For example, the removal of the dispersion medium may be performed by heating the coating layer to a predetermined temperature, but ensuring that the temperature of the surface of the coating layer does not exceed 60°C. When heating the coating layer under the above conditions, thermal energy may be first used to heat and phase-change the dispersion medium, and may not be used to deform the polymer binder.

[0082]

[0083] Hereinafter, the present invention will be described in more detail through specific examples and experimental examples. The following examples and experimental examples are intended to illustrate the present invention, and the present invention is not limited by the following examples and experimental examples.

[0084] Example 1

[0085] Preparation of coating slurry

[0086] At room temperature (25℃), 5.4 g (solid content 10%) of acrylamide-based binder (polyacrylamide, Mw: 900,000) and 30 g of Al2O3 (particle size: 500 nm) as inorganic particles were added to 67 mL of water in a 250 mL wide-mouth round bottle, and then beads were added and the bottle was shaken to mix.

[0087] 2.1 g (solid content 25%) of an acrylic acid binder (polyacrylic acid, Mw: 350,000) and 1.1 g (solid content 42%) of a polyacrylic acid polymer dispersant were added to the bottle above, stirred twice with a shaker (for a total of 2 hours), and then 0.2 g (solid content 100%) of a wetting agent was added and stirred for another 15 minutes with a shaker to prepare a slurry.

[0088] The above slurry was filtered to remove lumps, and a coating slurry having a solid content of 30% and a pH of 7.0 was prepared.

[0089] Preparation of porous polymer substrates

[0090] A polyethylene film measuring 20 cm × 30 cm and having a thickness of 10 ㎛ was used as the porous polymer substrate.

[0091] Manufacturing of membranes

[0092] The coating slurry was coated on both sides of a polyethylene film using a bar coater to form a coating layer with a thickness of 1.5 μm for each coating.

[0093] By applying airflow to a polyethylene film on which a coating layer was formed and repeating the process of removing the dispersion medium five times, a separation membrane with a total thickness of 13 μm was manufactured.

[0094] Comparative Example 1

[0095] A separation membrane was manufactured in the same manner as in Example 1, except that the pH of the coating slurry was adjusted to 2.5 by using a polyacrylic acid polymer dispersant (solid content 25%) having a different degree of substitution from the dispersant of Example 1 when manufacturing the coating slurry.

[0096] Example 2

[0097] A membrane was manufactured using the same method as in Example 1, except that polyacrylamide (Mw: 400,000, solid content 15%) was used as an acrylamide-based binder when manufacturing the coating slurry.

[0098] Comparative Example 2

[0099] A membrane was manufactured in the same manner as in Example 1, except that polyacrylamide (Mw: 1,200,000, solid content 5%) was used as an acrylamide-based binder when manufacturing the coating slurry.

[0100] Example 3

[0101] A membrane was manufactured in the same manner as in Example 1, except that 3 g of polyacrylic acid (solid content 25%) and 0.32 g of polyacrylamide (solid content 10%) were used in the preparation of the coating slurry.

[0102] Example 4

[0103] A membrane was manufactured in the same manner as in Example 1, except that 1.3 g of polyacrylic acid (solid content 25%) and 7.6 g of polyacrylamide (solid content 10%) were used in the preparation of the coating slurry.

[0104] Comparative Example 3

[0105] A membrane was manufactured in the same manner as in Example 1, except that 4.3 g of polyacrylic acid (solid content 25%) was used when manufacturing the coating slurry, and no acrylamide-based binder was used.

[0106] Comparative Example 4

[0107] A membrane was manufactured in the same manner as in Example 1, except that 11 g of polyacrylamide (solid content 10%) was used when manufacturing the coating slurry and no acrylic acid binder was used.

[0108]

[0109] Experimental Example 1. Confirmation of Membrane Properties According to Coating Slurry Properties

[0110] The properties of the membrane manufactured according to Example 1 and Comparative Example 1 were confirmed and are shown in Table 1 below.

[0111] Confirmed improvement in dry state heat shrinkage

[0112] The membranes of the examples and comparative examples were prepared as specimens measuring 5 cm × 5 cm, respectively. After storing them in a convection oven at 200°C for 30 minutes, the thermal shrinkage ratios in the MD and TD directions were calculated according to the equation [(length of the initial specimen - length after storing @200°C / 0.5 h) / (length of the initial specimen)] × 100 (%).

[0113] Confirmed improvement in wet state heat shrinkage

[0114] The membranes of the examples and comparative examples were prepared as 5 cm × 5 cm specimens and each was inserted into an aluminum pouch measuring 7 cm × 10 cm. 1 g of the following electrolyte was injected into the pouch, and the pouch was sealed.

[0115] The electrolyte 1 used herein was a solvent containing ethylene carbonate (EC) / ethyl methyl carbonate (EMC) mixed at a weight ratio of 3 / 7, 2 wt% of vinylene carbonate (VC) as an additive, and lithium salt LiPF61 M.

[0116] The electrolyte 2 used above contained a solvent containing ethylene carbonate (EC) / ethyl methyl carbonate (EMC) / dimethyl carbonate (DMC) mixed at a weight ratio of approximately 20 / 5 / 75. After storing the sealed pouch in a 135°C convection oven for 30 minutes, the separator was taken out, and the Machine Direction (MD) and Transverse Direction (TD) thermal shrinkage ratios were calculated according to [(length of initial specimen - length after storing @135°C / 0.5 h) / (length of initial specimen)] × 100 (%).

[0117] Comparative Example 1 Example 1 Coating slurry pH 2.5 7.0 PAA:PAM weight ratio 5:5 5:5 Thickness of membrane (㎛) 13.0 13.0 Dry state thermal shrinkage @ 200℃ / 0.5h (MD(%) / TD(%)) 59 / 57 3 / 3 Electrolyte 1 Wet state thermal shrinkage @ 135℃ / 0.5h (MD(%) / TD(%)) 18 / 18 6 / 5 Electrolyte 2 Wet state thermal shrinkage @ 135℃ / 0.5h (MD(%) / TD(%)) 19 / 18 6 / 5

[0118]

[0119] Experimental Example 2. Confirmation of the properties of the membrane according to the molecular weight of the acrylamide-based binder.

[0120] The condition of the membranes manufactured according to Examples 1 to 2 and Comparative Example 2 was confirmed, and the physical properties of each membrane were confirmed and shown in Table 2 below. The method for confirming each physical property is the same as in the previous experimental example.

[0121] Comparative Example 2 Example 1 Example 2 PAM weight average molecular weight 1,200,000 900,000 400,000 PAA:PAM weight ratio 5:55:55:5 Thickness of membrane (㎛) 13.0 13.0 13.0 Dry state thermal shrinkage @ 200℃ / 0.5h (MD(%) / TD(%)) Coating not possible due to increased viscosity of coating slurry (>500 cps) 3 / 3 3 / 2 Electrolyte 1 Wet state thermal shrinkage @ 135℃ / 0.5h (MD(%) / TD(%)) 6 / 5 5 / 5 Electrolyte 2 Wet state thermal shrinkage @ 135℃ / 0.5h (MD(%) / TD(%)) 6 / 5 5 / 5

[0122]

[0123] Experimental Example 3. Confirmation of the properties of the membrane according to the weight ratio of acrylic acid binder and acrylamide binder.

[0124] The condition of the membranes manufactured according to Examples 1, 3, and 4 and Comparative Examples 3 to 4 was confirmed, and the physical properties of each membrane were confirmed and shown in Table 3 below. The method for confirming each physical property is the same as in the previous experimental example.

[0125] Comparative Example 3 Example 3 Example 1 Example 4 Comparative Example 4 PAA:PAM weight ratio 10:07:35:53:70:10 Thickness of membrane (㎛) 13.0 13.0 13.0 13.0 13.0 Dry state thermal shrinkage @ 200℃ / 0.5h (MD(%) / TD(%)) 1 / 13 / 23 / 35 / 55 5 / 50 Wet state thermal shrinkage in electrolyte 1 @ 135℃ / 0.5h (MD(%) / TD(%)) 27 / 25 6 / 56 / 56 / 51 5 / 13 Wet state thermal shrinkage in electrolyte 2 @ 135℃ / 0.5h (MD(%) / TD(%)) 18 / 20 6 / 56 / 55 / 51 4 / 12

[0126]

[0127] While the present invention has been described above with reference to preferred embodiments, it will be understood by those skilled in the art or those with ordinary knowledge in the art that various modifications and changes can be made to the present invention without departing from the spirit and technical scope of the present invention as set forth in the claims below. Accordingly, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be defined by the claims.

Claims

1. Comprising a porous polymer substrate and a porous coating layer formed on at least one surface of the porous polymer substrate, The above porous coating layer includes an acrylic acid-based binder, an acrylamide-based binder, and inorganic particles. The porous coating layer comprises 90 to 96 wt% of the inorganic particles based on the total weight of the porous coating layer, A separator for an electrochemical device, wherein the weight ratio of the acrylic acid-based binder and the acrylamide-based binder is 3:7 to 7:

3.

2. In paragraph 1, A separator for an electrochemical device, wherein the weight average molecular weight of the acrylamide-based binder is 400,000 to 1,000,000.

3. In paragraph 1, The above porous coating layer is, A coating slurry containing the acrylic acid binder, the acrylamide binder, inorganic particles, a dispersant, and a dispersion medium is formed by coating the porous polymer substrate. A separator for an electrochemical device, wherein the pH of the above coating slurry is 3 to 9.

4. In paragraph 1, A separator for an electrochemical device, wherein the acrylic acid-based binder comprises, as a repeating unit, one or more monomers selected from the group consisting of acrylic acid and methacrylic acid.

5. In paragraph 1, A separator for an electrochemical device, wherein the acrylamide-based binder comprises, as a repeating unit, at least one monomer selected from the group consisting of acrylamide, methacrylamide, N-ethylacrylamide, ethylmethacrylamide, N-propylacrylamide, N-isopropylacrylamide, N-isopropylmethacrylamide, N-butylacrylamide, and N-butylmethacrylamide.

6. In paragraph 1, A separator for an electrochemical device, wherein the content of the acrylic acid-based binder in the porous coating layer is greater than or equal to the content of the acrylamide-based binder.

7. An electrochemical device comprising a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, The above separator Comprising a porous polymer substrate and a porous coating layer formed on at least one surface of the porous polymer substrate, The above porous coating layer includes an acrylic acid-based binder, an acrylamide-based binder, and inorganic particles. The porous coating layer comprises 90 to 96 wt% of the inorganic particles based on the total weight of the porous coating layer, An electrochemical device wherein the weight ratio of the acrylic acid-based binder and the acrylamide-based binder is 3:7 to 7:

3.

8. In paragraph 7, An electrochemical device further comprising an electrolyte solution comprising a solvent in which ethylene carbonate (EC) / ethyl methyl carbonate (EMC) is mixed in a weight ratio of 3 / 7 or a solvent in which ethylene carbonate (EC) / ethyl methyl carbonate (EMC) / dimethyl carbonate (DMC) is mixed in a weight ratio of 20 / 5 / 75.

9. In paragraph 7, An electrochemical device wherein the weight average molecular weight of the acrylamide-based binder is 400,000 to 1,000,000.

10. In paragraph 7, The above porous coating layer is, A coating slurry containing the acrylic acid binder, the acrylamide binder, inorganic particles, a dispersant, and a dispersion medium is formed by coating the porous polymer substrate. An electrochemical device, wherein the pH of the above coating slurry is 3 to 9.

11. In paragraph 7, An electrochemical device, wherein the acrylic acid-based binder comprises, as a repeating unit, one or more monomers selected from the group consisting of acrylic acid and methacrylic acid.

12. In paragraph 7, An electrochemical device, wherein the acrylamide-based binder comprises, as a repeating unit, at least one monomer selected from the group consisting of acrylamide, methacrylamide, N-ethylacrylamide, ethylmethacrylamide, N-propylacrylamide, N-isopropylacrylamide, N-isopropylmethacrylamide, N-butylacrylamide, and N-butylmethacrylamide.

13. In paragraph 7, An electrochemical device, wherein the content of the acrylic acid-based binder in the porous coating layer is greater than or equal to the content of the acrylamide-based binder.

Citation Information

Patent Citations

  • Separator for electrochemical device and electrochemical device comprising the same

    KR1020240143399A

  • Cell(Cellular) Phone auxiliary battery with memory card reader

    KR1020200137123A

  • Stabilized composition comprising hydroquinone or its derivative

    KR1020220057415A

  • Binder for secondary battery, composite separator and secondary battery prepared by using the same

    KR102368234B1

  • Manufacturing apparatus for display

    KR102825565B1