Dry negative electrode film, and dry negative electrode and lithium battery comprising same
The dry negative electrode film with a core-shell structure addresses the solvent-related issues in conventional lithium battery electrodes by reducing internal resistance and improving mechanical strength, resulting in improved lithium battery performance and stability.
Patent Information
- Application Number
- PCT/KR2024/003348
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional lithium battery electrodes manufactured using slurry-based methods require excessive solvents, leading to high internal resistance and low mechanical strength, which hinders miniaturization and performance enhancement.
A dry negative electrode film with a core-shell structure, where the core is made of carbon-based materials and the shell includes a composite of metal oxides and carbon-based materials, is used to reduce internal resistance and improve mechanical strength, thereby enhancing the cycling characteristics of lithium batteries.
The dry negative electrode film achieves reduced internal resistance, improved mechanical properties, and enhanced cycle characteristics, leading to more efficient and stable lithium battery performance.
Smart Images

Figure KR2024003348_03102024_PF_FP_ABST
Abstract
Description
Dry negative electrode film, dry negative electrode and lithium battery comprising the same
[0001] The present invention relates to a dry negative electrode film, a dry negative electrode including the same, and a lithium battery.
[0002] To accommodate the miniaturization and high-performance of various devices, lithium batteries are becoming increasingly important not only for their miniaturization and weight reduction, but also for their high energy density. In other words, high-capacity lithium batteries are becoming increasingly important.
[0003] Electrodes manufactured from slurries containing solvents use an excessive amount of solvent during electrode manufacture, so a dry method that excludes the use of such organic solvents is being considered.
[0004] One aspect is to provide a novel dry cathode film having improved cycling characteristics due to reduced internal resistance and improved mechanical strength.
[0005] Another aspect is to provide a dry cathode comprising the above dry cathode film.
[0006] Another aspect is to provide a lithium battery comprising the above dry negative electrode.
[0007] According to one aspect,
[0008] A dry negative electrode active material, and a dry binder, wherein the dry negative electrode active material comprises a composite negative electrode active material comprising a core; and a shell disposed along a surface of the core, wherein the core comprises a carbon-based material; a mixture of a carbon-based material and a silicon-based active material; a composite of a carbon-based material and a silicon-based active material; or a combination thereof, and wherein the shell comprises a composite comprising at least one first metal oxide and a first carbon-based material, wherein the first metal oxide is disposed within a first carbon-based material matrix, and wherein the first metal oxide is represented by the chemical formula M a O b(0 <a≤3, 0<b<4, a가 1, 2, 또는 3 이면, b는 정수가 아님)로 표시되며, 상기 M은 원소주기율표 2족 내지 16족 중에서 선택된 하나 이상의 금속인, 건식 음극 필름이 제공된다.
[0009] According to another embodiment, a dry negative electrode is provided, which includes a negative electrode collector; and the above-described dry negative electrode film disposed on one or both sides of the negative electrode collector.
[0010] The above negative electrode current collector includes a substrate; and an interlayer disposed between the substrate and the dry negative electrode film, wherein the interlayer includes a carbon-based conductive material.
[0011] According to another aspect, it includes an anode, a cathode, and an electrolyte disposed between the anode and the cathode,
[0012] The above cathode is the dry cathode described above,
[0013] A lithium battery is provided, wherein the electrolyte comprises a liquid electrolyte, a solid electrolyte, or a combination thereof.
[0014] According to one aspect, the internal resistance of the dry negative electrode film is reduced and the mechanical properties are improved, thereby improving the initial efficiency and cycle characteristics of a lithium battery employing such a dry negative electrode film.
[0015] Figure 1 is a cross-sectional schematic diagram of a dry cathode cathode active material according to one embodiment.
[0016] Figure 2 is a cross-sectional schematic diagram of a dry cathode cathode active material according to another embodiment.
[0017] Figure 3a illustrates the structure of a dry cathode-separator subassembly according to an embodiment.
[0018] Figure 3b illustrates the structure of a dry cathode-separator subassembly according to another embodiment.
[0019] Figure 4a is a cross-sectional view showing a laminated structure of a dry negative electrode for a lithium battery according to an embodiment.
[0020] Figure 4b is a cross-sectional view showing a laminated structure of a dry negative electrode for a lithium battery according to another embodiment.
[0021] Figure 4c is a cross-sectional view showing a laminated structure of a dry negative electrode for a lithium battery according to another embodiment.
[0022] Figure 5 is a schematic diagram of a lithium battery according to an embodiment.
[0023] Figure 6 is a schematic diagram of a lithium battery according to another embodiment.
[0024] Figure 7 is a schematic diagram of a lithium battery according to another embodiment.
[0025] <Explanation of symbols for major parts of the drawing>
[0026] 1 lithium battery 2 cathode
[0027] 3 positive electrode 4 separator
[0028] 5 Battery case 6 Cap assembly
[0029] 7 Battery structure 8 Electrode tab
[0030] 10 cores 20 shells
[0031] 21. First metal oxide 22. First carbon-based material
[0032] 23 Second carbon-based material 100 Dry negative electrode active material
[0033] Various embodiments are illustrated in the accompanying drawings. However, the present invention may be embodied in many different forms and should not be construed as limited to the embodiments described herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. Like reference numerals in the drawings indicate like elements.
[0034] When a component is referred to as being "on" another component, it can be understood that it is either directly on top of the other component or that other components may be intervening between them. Conversely, when a component is referred to as being "directly on" another component, no intervening components are present.
[0035] Although the terms "first," "second," "third," etc. may be used herein to describe various components, elements, regions, layers, and / or zones, these components, elements, regions, layers, and / or zones should not be limited by these terms. These terms are used only to distinguish one component, element, region, layer, or zone from another component, element, region, layer, or zone. Thus, a first component, element, region, layer, or zone described below may be referred to as a second component, element, region, layer, or zone without departing from the teachings of this specification.
[0036] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the invention. As used herein, the singular forms "a," "an," and "the" are intended to include the plural forms including "at least one," unless the content clearly dictates otherwise. "At least one" should not be construed as limiting to the singular. As used herein, the term "and / or" includes any and all combinations of one or more of the listed items. The terms "comprises" and / or "comprising" as used in the detailed description specify the presence of stated features, regions, integers, steps, operations, components, and / or ingredients, but do not preclude the presence or addition of one or more other features, regions, integers, steps, operations, components, ingredients, and / or groups thereof.
[0037] Spatially relative terms such as "below," "under," "bottom," "above," "above," and "top" may be used herein to readily describe the relationship of one component or feature to another. It will be understood that spatially relative terms are intended to encompass different orientations of the device when in use or operation in addition to the orientations depicted in the drawings. For example, if the device in the drawings were turned over, a component described as "below" or "below" another component or feature would then be oriented "above" the other component or feature. Thus, the exemplary term "below" can encompass both the above and below orientations. The device can be arranged in other orientations (rotated 90 degrees or otherwise rotated), and the spatially relative terms used herein can be interpreted accordingly.
[0038] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure pertains. Furthermore, it will be understood that terms defined in commonly used dictionaries should be interpreted to have a meaning consistent with their meaning within the context of the relevant art and the present disclosure, and not in an idealized or overly formal sense.
[0039] Exemplary embodiments are described herein with reference to cross-sectional drawings that are schematic representations of idealized embodiments. As such, variations from the shapes depicted are to be expected, for example, as a result of manufacturing techniques and / or tolerances. Therefore, the embodiments described herein should not be construed as limited to the specific shapes of regions as depicted herein, but should encompass variations in shapes resulting from, for example, manufacturing. For example, regions depicted or described as flat may typically have rough and / or non-linear features. Moreover, angles depicted as sharp may be rounded. Therefore, the regions depicted in the drawings are schematic in nature, and their shapes are not intended to depict the precise shapes of the regions, nor are they intended to limit the scope of the claims.
[0040] "Group" means a group in the periodic table of elements according to the International Union of Pure and Applied Chemistry ("IUPAC") Group 1-18 classification system.
[0041] The term "dry" as used herein refers to a state in which the material does not function properly even when in contact with or without a solvent, such as a process solvent. For example, a dry conductive material refers to a conductive material that functions properly without the need for contact with a solvent, or a conductive material that does not contain a solvent. For example, a dry binder refers to a conductive material that functions properly without the need for contact with a solvent, a binder that does not contain a solvent, etc. For example, a binder that is not mixed with a solvent and is in a liquid state at room temperature can be referred to as a dry binder.
[0042] In this specification, "particle size" refers to the average diameter when the particle is spherical, and the average major axis length when the particle is non-spherical. Particle size can be measured using a particle size analyzer (PSA). "Particle size" refers to the average particle diameter, for example. "Average particle size" refers to the median particle diameter, D50, for example.
[0043] D50 is the size of the particle corresponding to 50% of the cumulative volume, calculated from the particle side with a smaller particle size in the particle size distribution measured by laser diffraction.
[0044] D90 is the size of the particle corresponding to 90% of the cumulative volume, calculated from the particle side with a smaller particle size in the particle size distribution measured by laser diffraction.
[0045] D10 is the size of the particle corresponding to 10% of the cumulative volume, calculated from the particle side with a small particle size in the particle size distribution measured by laser diffraction.
[0046] The average particle diameter (D50) can be measured by a method suitable to those skilled in the art, such as a particle size analyzer, transmission electron microscope image, scanning electron microscope, or field emission scanning electron microscope (FE-SEM). In some embodiments, data analysis is performed using a dynamic light scattering measurement device, and the number of particles is counted by particle size range, and the average particle diameter (D50) value can be easily obtained from the following: calculation. In the present invention, "diameter" refers to the particle diameter or average particle diameter when the particle is spherical, and "diameter" refers to the major axis length or average major axis length when the particle is spherical.
[0047] In this disclosure, “metal” includes both metals and metalloids such as silicon and germanium, in their elemental or ionic states.
[0048] In this disclosure, “alloy” means a mixture of two or more metals.
[0049] In the present disclosure, “electrode active material” means an electrode material capable of undergoing lithiation and delithiation.
[0050] In the present disclosure, “positive electrode material” means a positive electrode material capable of undergoing lithiation and delithiation.
[0051] In the present disclosure, “negative electrode active material” means a negative electrode material capable of undergoing lithiation and delithiation.
[0052] In the present disclosure, “lithiation” and “lithiating” mean a process of adding lithium to an electrode active material.
[0053] In the present disclosure, “delithiation” and “delithiate” mean a process of removing lithium from an electrode active material.
[0054] In this disclosure, “charging” and “charging” mean a process of providing electrochemical energy to a battery.
[0055] In this disclosure, “discharging” and “discharging” mean the process of removing electrochemical energy from a battery.
[0056] In the present disclosure, “positive electrode” and “cathode” mean an electrode at which electrochemical reduction and lithiation occur during a discharge process.
[0057] In the present disclosure, “cathode” and “anode” mean electrodes where electrochemical oxidation and delithiation occur during a discharge process.
[0058] While specific implementations have been described, alternatives, modifications, variations, improvements, and substantial equivalents that are not currently anticipated or unforeseen may occur to the applicant or those skilled in the art. Accordingly, the appended claims, as filed and as amended, are intended to encompass all such alternatives, modifications, variations, improvements, and substantial equivalents.
[0059]
[0060] Hereinafter, a dry negative electrode film, a dry negative electrode including the same, and a lithium battery according to exemplary embodiments will be described in more detail.
[0061] When mixing active material, conductive material, and binder in a dry manner to manufacture an anode plate using a dry anode, there is a problem that the conductive material in the form of nanoparticles is bound to the binder and the conductive material is excessively aggregated and bound to the active material, resulting in an uneven mixing of the active material, conductive material, and binder, resulting in high plate resistance and low tensile strength. In contrast, by using a manufacturing method according to one embodiment, a dry anode film in which a binder and a conductive material are uniformly bonded to the surface of the active material in the manufacturing process of a dry electrode plate is provided, thereby improving the resistance reduction effect and providing a dry anode film with enhanced tensile strength, a dry anode including the same, and a lithium battery.
[0062] A dry negative electrode film according to an embodiment comprises a dry negative electrode active material and a dry binder, wherein the dry negative electrode active material comprises a core; and a shell disposed along a surface of the core, wherein the core comprises a carbon-based material; a mixture of a carbon-based material and a silicon-based active material; a composite of a carbon-based material and a silicon-based active material; or a combination thereof, and wherein the shell contains a composite comprising at least one first metal oxide and a first carbon-based material, wherein the first metal oxide is disposed within a first carbon-based material matrix, and wherein the first metal oxide has the chemical formula M. a O b (0 <a≤3, 0<b<4, a가 1, 2, 또는 3 이면, b는 정수가 아님)로 표시되며, 상기 M은 원소주기율표 2족 내지 16족 중에서 선택된 하나 이상의 금속이다.
[0063] Referring to FIG. 1, the dry negative electrode active material (100) includes a core (10) and a shell (20) arranged continuously or discontinuously along the surface of the core (10).
[0064] The core (10) contains a carbon-based material; a mixture of a carbon-based material and a silicon-based active material; a composite of a carbon-based material and a silicon-based active material; or a combination thereof, and the shell (20) can cover all or part of the core (10).
[0065] The shell (20) includes a first metal oxide (21) and a first carbon-based material (22). The dry negative electrode active material is, for example, an electrode active material that is not impregnated, dissolved, or dispersed in a process solvent during the dry negative electrode film manufacturing process.
[0066] Since the dry negative electrode active material has a core / shell structure and the shell includes the first carbon-based material, the dry negative electrode active material and the dry binder can be more uniformly mixed. Accordingly, agglomeration of the dry binder within the dry negative electrode film can be suppressed, and the dry binder can be uniformly distributed three-dimensionally. By suppressing local resistance regions within the dry negative electrode film, the imbalance in current density can be reduced, and the overall internal resistance of the dry electrode film can be reduced.
[0067] Since the dry negative electrode active material has a core / shell structure and the shell includes a first carbon-based material, the interfacial resistance between the dry negative electrode active materials can be reduced. Since the dry negative electrode active material has a core / shell structure and the shell includes a first carbon-based material, the internal resistance of the dry negative electrode film can be reduced. Since the dry negative electrode active material has a core / shell structure and the shell includes a first carbon-based material, the bonding strength between the dry negative electrode active material and the dry binder can be improved. Since the dry composite negative electrode active material has a core / shell structure and the shell includes a first carbon-based material, the mechanical properties, such as the tensile strength, of the dry negative electrode film can be improved. Since the internal resistance of the dry negative electrode film is reduced and the mechanical properties are improved, the cycle characteristics of a lithium battery including such a dry negative electrode film can be improved.
[0068] Since the shell includes the first metal oxide, the ionic conductivity can be improved compared to a shell made of a carbon-based material, and as a result, the ionic conductivity of the dry negative electrode active material can be improved.
[0069] The dry negative electrode active material has a core / shell structure, and the shell can be arranged continuously or discontinuously along the surface of the core. The shell can be more uniformly arranged on the core by including a first metal oxide arranged in a first carbon-based material matrix. The shell can be more uniformly arranged on the core without aggregation by being introduced onto the core from, for example, a composite including the first metal oxide arranged in the first carbon-based material matrix. The shell uniformly arranged on the core effectively blocks contact between the core and the electrolyte, thereby preventing side reactions due to contact between the core and the electrolyte. In addition, the formation of a resistive layer on the core surface can be suppressed by suppressing cation mixing due to contact between the core and the electrolyte. In addition, the introduction of the shell on the core can suppress the elution of transition metal ions from the core, in a core including a transition metal. The first carbon-based material can be, for example, a crystalline carbon-based material. The first carbon-based material can be, for example, a carbon-based nanostructure. The first carbon-based material may be, for example, a carbon-based two-dimensional nanostructure. The first carbon-based material may be, for example, graphene. For example, a shell comprising graphene and / or a matrix thereof is flexible, and thus easily accommodates changes in the volume of the dry negative electrode material during charge and discharge, thereby suppressing the occurrence of cracks within the dry negative electrode material. Since graphene has high electronic conductivity, the interfacial resistance between the dry negative electrode material and the electrolyte is reduced. Therefore, despite the introduction of a shell comprising graphene, an increase in the internal resistance of the lithium battery can be suppressed. In contrast, conventional carbon-based materials that do not include a first metal oxide are easily agglomerated, making it difficult to uniformly arrange them on the core of the dry negative electrode material.Additionally, since the first carbon-based material matrix is derived from, for example, a graphene matrix, it has a relatively low density and high porosity compared to conventional carbon-based materials derived from graphite-based materials.
[0070] The dry cathode active material has a core / shell structure. The shell includes a first metal oxide, and the metal included in the first metal oxide may be, for example, one or more selected from Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se. The first metal oxide may be, for example, Al2O z (0 <z<3), NbO x (0 <x<2.5), MgO x (0 <x<1), Sc2O z (0 <z<3), TiO y (0 <y<2), ZrO y (0 <y<2), V2O z (0 <z<3), WO y (0 <y<2), MnO y (0 <y<2), Fe2O z (0 <z<3), Co3O w (0 <w<4), PdO x (0 <x<1), CuO x (0 <x<1), AgO x (0 <x<1), ZnO x (0 <x<1), Sb2O z (0 <z<3), 및 SeO y (0 <y<2) 중에서 선택된 하나 이상일 수 있다. 제1 탄소계 재료 메트릭스 내에 이러한 제1 금속산화물이 배치됨에 의하여 코어 상에 배치된 쉘의 균일성이 향상되고, 건식 음극활물질의 내전압성(high-voltage resistance)이 더욱 향상된다. 쉘은 예를 들어 제1 금속산화물로서 Al2O x (0 <x<3)를 포함한다.
[0071] The shell may further comprise one or more second metal oxides. The second metal oxides may be, for example, of the formula Ma O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시될 수 있으며, 상기 M은 원소주기율표 2족 내지 13족, 제15족 및 16족 중에서 선택된 하나 이상의 금속이다. 제2 금속산화물은 예를 들어 상기 제1 금속산화물과 동일한 금속을 포함할 수 있다. 제2 금속산화물의 a 와 c의 비율인 c / a가 상기 제1 금속산화물의 a 와 b의 비율인 b / a에 비하여 더 큰 값을 가질 수 있다. 예를 들어, c / a > b / a. The second metal oxide can be disposed within the first carbon-based material matrix. The second metal oxide is selected from, for example, Al2O3, NbO, NbO2, Nb2O5, MgO, Sc2O3, TiO2, ZrO2, V2O3, WO2, MnO2, Fe2O3, Co3O4, PdO, CuO, AgO, ZnO, Sb2O3, and SeO2. The first metal oxide is, for example, a reduction product of the second metal oxide. The first metal oxide is obtained by reducing part or all of the second metal oxide. Therefore, the first metal oxide has a lower oxygen content and a lower oxidation number of the metal compared to the second metal oxide. For example, the shell is the first metal oxide Al2O x (0 <x<3) 및 제2 금속산화물인 Al2O3를 포함한다.
[0072] The shell includes, for example, at least one selected from a first metal oxide and a second metal oxide, and the particle size of at least one selected from the first metal oxide and the second metal oxide may be, for example, 0.1 nm to 100 nm, 0.5 nm to 100 nm, 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 30 nm, 5 nm to 30 nm, or 10 nm to 30 nm. The first metal oxide and / or the second metal oxide may be more uniformly distributed within the first carbon-based material matrix by having particle sizes in the nano-range. If the particle size of at least one of the first metal oxide and the second metal oxide is excessively increased, the thickness of the shell may increase, thereby increasing the internal resistance of the composite negative electrode active material. If the particle size of at least one of the first metal oxide and the second metal oxide is excessively decreased, uniform dispersion may be difficult.
[0073] The shell may include a first metal oxide and / or a second metal oxide and may include a first carbon-based material. The first carbon-based material may be arranged in a direction protruding from a surface of the first metal oxide and / or the second metal oxide. The first carbon-based material may be arranged in a direction protruding from the surface of the first metal oxide and / or the second metal oxide by growing directly from the surface of the first metal oxide and / or the second metal oxide. The first carbon-based material arranged in a direction protruding from the surface of the first metal oxide and / or the second metal oxide is, for example, a carbon-based two-dimensional nanostructure, a carbon-based flake, or graphene.
[0074] The thickness of the shell is 5 ㎛ or less, for example, 0.1 nm to 5 ㎛, 0.5 nm to 5 ㎛, 1 nm to 5 ㎛, 1 nm to 1 ㎛, 1 nm to 500 nm, 1 nm to 200 nm, 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 30 nm, or 1 nm to 20 nm. When the shell has a thickness in this range, the electronic conductivity of the dry negative electrode including the dry negative electrode active material can be further improved and the internal resistance can be further reduced.
[0075] The shell may have a single-layer structure or a multi-layer structure. The multi-layer structure may have, for example, a two-layer structure, a three-layer structure, or a four-layer structure. The multi-layer structure may, for example, have different types of metals in the first metal oxide contained in each layer.
[0076] The content of the shell may be, for example, 5 wt% or less, 0.01 wt% to 5 wt%, 0.01 wt% to 3 wt%, 0.01 wt% to 2 wt%, or 0.01 wt% to 1 wt% of the total weight of the dry negative electrode active material. The content of the first metal oxide may be, for example, 3 wt% or less, 0.006 wt% to 3 wt%, 0.06 wt% to 1.8 wt%, 0.006 wt% to 1.2 wt%, or 0.006 wt% to 0.6 wt% of the total weight of the dry negative electrode active material. When the dry negative electrode active material includes the shell and the first metal oxide in these content ranges, the cycle characteristics of the lithium battery are further improved.
[0077] The shell disposed along the surface of the core is, for example, a dry coating layer. The shell can be introduced onto the core by, for example, a dry method such as milling. The shell disposed along the surface of the core can include, for example, one or more selected from a composite comprising a first metal oxide and a first carbon-based material, for example, graphene, and a milling result of the composite. The first metal oxide is disposed within a matrix of the first carbon-based material, for example, a graphene matrix.
[0078] The shell is made from a composite comprising, for example, a first metal oxide and a first carbon-based material, for example, graphene. The composite may further comprise a second metal oxide in addition to the first metal oxide. The composite may comprise, for example, two or more types of the first metal oxide. The composite may comprise, for example, two or more types of the first metal oxide and two or more types of the second metal oxide.
[0079] The composite may include at least one selected from a first metal oxide and a second metal oxide. The particle size of at least one selected from the first metal oxide and the second metal oxide may be from 0.1 nm to 100 nm, from 0.5 nm to 100 nm, from 1 nm to 100 nm, from 1 nm to 50 nm, from 1 nm to 30 nm, from 5 nm to 30 nm, or from 10 nm to 30 nm. Since the first metal oxide and / or the second metal oxide have particle sizes in the nano-range, they can be more uniformly distributed within the first carbon-based material matrix of the composite. Therefore, the composite can be uniformly coated on the core without agglomeration to form a shell. In addition, since the first metal oxide and / or the second metal oxide have particle sizes in the range, they can be more uniformly arranged on the core. Therefore, since the first metal oxide and / or the second metal oxide are uniformly arranged on the core, the withstand voltage characteristics can be more effectively exhibited. The particle size of the first metal oxide and / or the second metal oxide is measured using, for example, a laser diffraction method or a dynamic light scattering method measuring device. The particle size is measured using, for example, a laser scattering particle size distribution meter (for example, Horiba LA-920), and is the value of the median particle size (D50) when 50% of the small particle size is accumulated in volume conversion. The uniformity deviation of at least one selected from the first metal oxide and / or the second metal oxide may be 3% or less, 2% or less, or 1% or less.
[0080] The uniformity can be determined, for example, by X-ray photoelectron spectroscopy (XPS). Accordingly, at least one selected from the first metal oxide and the second metal oxide can be uniformly distributed within the composite with a deviation of 3% or less, 2% or less, or 1% or less.
[0081] The dry cathode active material comprises a core, and the core comprises, for example, a carbon-based material; a mixture of a carbon-based material and a silicon-based active material; a composite of a carbon-based material and a silicon-based active material; or a combination thereof.
[0082] In the mixture of a carbon-based material and a silicon-based active material or the composite of a carbon-based material and a silicon-based active material, the content of the silicon-based active material is 5 to 20 wt%, 7 to 18 wt%, 10 to 17 wt%, or 10 to 15 wt% based on 10 wt% of the total weight of the mixture of the carbon-based material and the silicon-based active material or the composite of the carbon-based material and the silicon-based active material.
[0083] The carbonaceous material is crystalline carbon, amorphous carbon, or a combination thereof, wherein the crystalline carbon is at least one selected from the group consisting of natural graphite, artificial graphite, graphene, fullerene, and carbon nanotubes, and the amorphous carbon is at least one selected from the group consisting of pitch carbon, soft carbon, hard carbon, mesophase pitch carbide, calcined coke, and carbon fiber.
[0084] The precursor of the above amorphous carbon may be coal-based pitch, mesophase pitch, petroleum-based pitch, coal-based oil, petroleum-based heavy oil, or a polymer resin such as a phenol resin, a furan resin, or a polyimide resin.
[0085] The above silicon-based active material is a Si alloy, a silicon-containing structure, a silicon-containing compound, or a combination thereof.
[0086] The above silicon-containing compound is SiO2, SiOx (0 <x<2), SiC, 또는 그 조합이며, 상기 실리콘 함유 구조체가 실리콘 복합 구조체를 포함한다.
[0087] According to one embodiment, the silicon-based active material contains a silicon composite structure. The silicon composite structure may be a silicon-carbon composite or may include a silicon-carbon composite.
[0088] The silicon-carbon composite is a silicon-carbon composite including silicon particles and a first carbon-based material, a silicon-carbon composite including a core in which silicon particles and a second carbon-based material are mixed and a third carbon-based material surrounding the core, or a combination thereof.
[0089] The first carbon-based material to the third carbon-based material are independently crystalline carbon, amorphous carbon, or a combination thereof. The silicon-carbon composite includes a core comprising silicon particles and crystalline carbon, and an amorphous carbon coating layer positioned on the surface of the core.
[0090] When the silicon-carbon composite described above is used as a silicon-based active material, the secondary battery can exhibit high capacity and stable cycle characteristics.
[0091] In the silicon-carbon composite including the silicon particles and the first carbon-based material, the content of the silicon particles may be 30 wt% to 70 wt%, 30 wt% to 60 wt%, for example, 40 wt% to 50 wt%. Alternatively, the silicon-based active material may include a silicon-carbon composite including a core in which silicon particles and a second carbon-based material are mixed and a third carbon-based material surrounding the core. By using such a silicon-carbon composite, a secondary battery can realize a very high capacity while improving the capacity retention rate, and in particular, can improve the high-temperature life characteristics. In the present specification, the average particle diameter (D50) means the diameter of particles having a cumulative volume of 50 volume% in a particle size distribution.
[0092] Additionally, with respect to 100 wt% of the silicon-carbon composite, the third carbon-based material may be included in an amount of 1 wt% to 50 wt%, and the silicon particles may be included in an amount of 30 wt% to 70 wt%. The second carbon-based material may be included in an amount of 20 wt% to 69 wt%. When the contents of the silicon particles, the third carbon-based material, and the second carbon-based material are within the above ranges, the discharge capacity of the secondary battery is excellent and the capacity retention rate is improved.
[0093] The particle size of the above silicon particles is 10 nm to 30 um, for example, 10 nm to 1000 nm, or 20 nm to 150 nm. When the average particle size of the silicon particles is within the above range, volume expansion occurring during charge and discharge can be suppressed or reduced, and electron transfer interruption due to particle fragmentation during charge and discharge can be prevented.
[0094] In the above silicon-carbon composite, for example, the second carbon-based material may be crystalline carbon and the third carbon-based material may be amorphous carbon. That is, the silicon-carbon composite is a silicon-carbon composite including a core comprising silicon particles and crystalline carbon and an amorphous carbon coating layer positioned on the surface of the core.
[0095] A silicon-carbon composite may be, for example, a silicon-carbon nanocomposite. A silicon-carbon nanocomposite refers to a composite in which at least one of silicon and carbon has a nanoscale size of less than 1 μm. For example, a silicon-carbon nanocomposite may be a composite composed of silicon nanoparticles and carbon nanoparticles.
[0096] The silicon-containing compound may include, for example, silicon, a silicon alloy, silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, or combinations thereof. The silicon-containing compound may include, for example, SiO x (0 <x<2)를 포함할 수 있다.
[0097] The silicon alloy comprises silicon and an element of an alkali metal, an alkaline earth metal, a group 13 to 16 element, a transition metal, a rare earth element, or a combination thereof. The element is, for example, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, or a combination thereof.
[0098] According to another embodiment, a silicon composite structure comprises: porous silicon secondary particles; and first carbon flakes disposed on the porous silicon secondary particles; wherein the porous silicon secondary particles are aggregates of a plurality of silicon composite primary particles, and the silicon composite primary particles comprise silicon; silicon dioxide (SiO2) and / or silicon suboxide (SiO) disposed on the silicon. x , 0 <x<2); 및 상기 실리콘 디옥사이드 (SiO2) 및 / 또는 실리콘 서브옥사이드 상에 배치되는 제2 탄소 플레이크를 포함할 수 있다.
[0099] A silicon composite structure includes porous silicon secondary particles containing aggregates of a plurality of silicon composite primary particles, and first carbon flakes disposed on the porous silicon secondary particles. The first carbon flakes disposed on the porous silicon secondary particles may be disposed to cover at least one surface of the porous silicon secondary particles. The first carbon flakes may be directly disposed on the porous silicon secondary particles. The first carbon flakes may be directly grown on silicon suboxide of the porous silicon secondary particles. The first carbon flakes may be directly grown from the surface of the porous silicon secondary particles and disposed directly on the surface of the porous silicon secondary particles. The first carbon flakes may completely or partially cover the surface of the porous silicon secondary particles. The coverage of the first carbon flake is, for example, 5 to 100%, 10 to 99%, 20 to 95%, or 40 to 90% based on the total surface area of the porous silicon secondary particle. The carbon of the first carbon flake exists on the surface of the porous silicon secondary particle and effectively buffers the volume change of the porous silicon secondary particle. The size of the porous silicon secondary particle may be, for example, 1 to 20 μm, 2 to 18 μm, or 3 to 10 μm. The size of the first carbon flake may be, for example, 1 to 200 nm, 5 to 150 nm, or 10 to 100 nm. Here, the size means the diameter or the major axis length.
[0100] The silicon composite primary particle comprises silicon; silicon, silicon suboxide (SiO) disposed on at least one surface of the silicon; x, 0<x<2); 및 상기 실리콘 서브옥사이드의 일면 상에 배치된 제2 탄소 플레이크를 포함한다. 실리콘은 예를 들어, 판상형, 침상형, 구형, 또는 이들의 조합 형태일 수 있다. 실리콘은 그 형상이 제한되지 않으며, 예를 들어 스피어, 나노와이어, 침상, 막대형, 입자, 나노튜브, 나노로드, 웨이퍼(wafer), 및 나노리본, 또는 이들의 조합물이다. 실리콘의 평균 사이즈는 예를 들어 10 nm 내지 1 ㎛, 10 nm 내지 500 nm, 20 내지 150 nm, 또는 100 nm 이다. 실리콘의 평균 사이즈는 실리콘이 구형 입자인 경우에는 평균입경이고, 비구형 입자, 예를 들어 판상 입자 또는 침상형 입자인 경우에는 장축 길이, 길이 또는 두께를 의미할 수 있다. 실리콘 복합체 일차 입자에서 실리콘 상에 배치되는 실리콘 서브옥사이드(SiOx) (0<x<2)는 실리콘의 적어도 일면을 커버하도록 배치될 수 있다. 실리콘 서브옥사이드는 실리콘 상에 직접적으로 배치될 수 있다. 실리콘 서브옥사이드는 실리콘의 표면을 전체적으로 또는 부분적으로 커버할 수 있다. 실리콘 서브옥사이드의 커버율은 예를 들어 실리콘의 전체 표면적을 기준으로 하여 예를 들어 1 내지 100 %, 5 내지 99 %, 10 내지 95 %, 또는 20 내지 90 % 일 수 있다. 실리콘 서브옥사이드 상에 배치되는 제2 탄소 플레이크는 실리콘 서브옥사이드의 적어도 일 면을 커버하도록 배치될 수 있다. 제2 탄소 플레이크는 실리콘 서브옥사이드 상에 직접적으로 배치될 수 있다. 제2 탄소 플레이크는 상기 실리콘 서브옥사이드의 표면으로부터 직성장되어 실리콘 서브옥사이드의 표면에 직접적으로 배치될 수 있다. 제2 탄소 플레이크는 예를 들어 실리콘 서브옥사이드의 표면을 전체적으로 또는 부분적으로 커버할 수 있다.The coverage of the second carbon flakes may be, for example, 10 to 100%, 10 to 99%, 20 to 95%, or 40 to 90% based on the total surface area of the silicon suboxide. The carbon of the second carbon flakes exists on the surface of the silicon and / or silicon suboxide and can effectively buffer the volume change of the silicon composite primary particle. The size of the second carbon flakes may be, for example, 1 to 200 nm, 5 to 150 nm, or 10 to 100 nm. Here, the size means the diameter or the major axis length.
[0101] A silicon composite structure includes porous silicon secondary particles and second carbon flakes disposed on the porous silicon secondary particles. The second carbon flakes may be disposed to completely or partially cover the porous silicon secondary particles. For example, the second carbon flakes may be disposed to completely or partially surround the porous silicon secondary particles. The porous silicon secondary particles include first carbon flakes disposed on silicon composite primary particles. When the volume of the silicon composite structure expands / shrinks, silicon included in the porous silicon secondary particles can maintain contact with the first carbon flakes and / or the second carbon flakes. Since the porous secondary particles include pores, they can act as an internal buffer space when the volume of the silicon composite structure expands / shrinks. Therefore, unlike conventional silicon-based negative electrode materials, the silicon composite structure can effectively accommodate a change in volume of the silicon composite structure during charge / discharge while suppressing an increase in internal resistance.
[0102] The porosity of the silicone composite structure can be, for example, 60% or less, 30% to 60%. Alternatively, the silicone composite structure can be nonporous. A nonporous structure can have, for example, a porosity of 10% or less, 5% or less. A nonporous structure can have, for example, a porosity of 0.01% to 5%, or 0%. Porosity can be measured by mercury porosimetry or nitrogen adsorption.
[0103] The silicon composite structure may have, for example, a non-spherical shape. The sphericity of the silicon composite structure may be, for example, 0.9 or less. The sphericity of the silicon composite structure is, for example, 0.7 to 0.9, 0.8 to 0.9, or 0.85 to 0.9. The circularity is, for example, 4πA / P. 2 (A is the area, P is the perimeter) is determined by
[0104] The silicon composite structure includes first carbon flakes and second carbon flakes. The first carbon flakes and the second carbon flakes may be, for example, the same carbon flakes. The first carbon flakes and the second carbon flakes may be any carbon-based material having a flake shape. The first carbon flakes and the second carbon flakes may independently be graphene, graphite, carbon fibers, graphitic carbon, graphene oxide, or a mixture thereof. The porous composite structure may include, for example, first graphene and second graphene as the first carbon flakes and the second carbon flakes. The first graphene and the second graphene may each have a structure such as a nanosheet, a membrane (or film), or a flake. A nanosheet refers to a shape formed in an irregular state on silicon suboxide or porous silicon secondary particles with a thickness of about 1000 nm or less, for example, 1 to 1000 nm. A film is a form that is continuously and uniformly formed on silicon suboxide or porous silicon secondary particles.
[0105] The silicon-containing structure may further include a carbon-based coating layer disposed on the silicon composite structure. The carbon-based coating layer can improve the physical stability of the silicon composite structure and more effectively prevent side reactions between silicon and the electrolyte during charge and discharge. The carbon-based coating layer may include, for example, a first amorphous carbon. The carbon-based coating layer may include a high-density first amorphous carbon. The first amorphous carbon may include, for example, pitch carbon, soft carbon, hard carbon, mesophase pitch carbide, calcined coke, carbon fiber, or a mixture thereof. The carbon-based coating layer may further include crystalline carbon. By further including crystalline carbon, the carbon-based coating layer can more effectively perform a buffering function against volume changes of the silicon composite structure. The crystalline carbon may be, for example, natural graphite, artificial graphite, graphene, fullerene, carbon nanotube, or a mixture thereof. The thickness of the carbon coating layer can be, for example, 1 nm to 5000 nm, 10 nm to 2000 nm or 5 nm to 2500 nm.
[0106] The silicon-containing structure may further comprise, for example, a second amorphous carbon disposed within the silicon composite structure. For example, the silicon composite structure may comprise porous silicon secondary particles, and the second amorphous carbon may be disposed within the pores of the porous silicon secondary particles. The second amorphous carbon may be disposed between a plurality of silicon composite primary particles constituting the porous silicon secondary particles. The silicon composite primary particles may comprise, for example, silicon; silicon dioxide (SiO2) and / or silicon suboxide (SiO) disposed on the silicon. x, 0 <x<2); 및 실리콘 디옥사이드(SiO2) 및 / 또는 실리콘 서브옥사이드 상에 배치되는 제2 탄소 플레이크; 및 제2 탄소 플레이크 상에 배치되는 제2 비정질 탄소를 포함할 수 있다. 실리콘 복합 구조체는 그 내부의 기공에 치밀한 제2 비정질 탄소가 채워짐에 의하여 비다공성 구조를 갖는 밀집 구조체를 가질 수 있다. 실리콘 복합 구조체가 이러한 비다공성 구조를 가짐에 의하여, 충방전시 전해액과의 부반응이 더욱 감소될 수 있으며, 실리콘의 부피 변화를 더욱 효과적으로 완화할 수 있다. 제2 비정질 탄소는 예를 들어 피치카본, 소프트카본, 하드카본, 메조페이스 피치 탄화물, 소성된 코크스, 탄소섬유 또는 이들의 혼합물을 포함할 수 있다.
[0107] In the silicon composite structure, the mixing ratio of the total weight of the first carbon, which is the sum of the carbon of the first carbon flakes and the carbon of the second carbon flakes, and the weight of the second carbon, which is the carbon of the carbon-based coating layer, may be, for example, 30:1 to 1:3, 20:1 to 1:1, or 10:1 to 1:0.9. By having the first carbon and the second carbon having the mixing ratio in this range, a lithium battery having improved cycle characteristics can be provided. The mixing ratio of the first carbon and the second carbon can be confirmed through thermogravimetric analysis. The first carbon is associated with a peak appearing in the range of 700 to 750°C, and the second carbon is associated with a peak appearing in the range of 600 to 650°C. The thermogravimetric analysis is performed, for example, at a heating rate of about 10°C / min, in an air atmosphere at a temperature in the range of 25 to 1,000°C. The first carbon is, for example, crystalline carbon, and the second carbon is, for example, amorphous carbon. The mixing ratio of the total weight of the carbon of the first carbon flake and the carbon of the second carbon flake and the total weight of the first amorphous carbon and the second amorphous carbon may be, for example, 1:99 to 99:1, 1:20 to 80:1, or 1:1 to 1:10.
[0108] The core is a silicon-containing negative electrode active material, which is a silicon-containing compound, SiO. x (0 <x<2)를 포함할 수 있다. SiO x (0 <x<2)의 평균 입경은 예를 들어 1 ㎛ 이상, 3 ㎛ 이상, 또는 5 ㎛ 이상일 수 있다. SiO x (0 <x<2)의 평균 입경은 예를 들어 1 ㎛ 내지 30 ㎛, 3 ㎛ 내지 20 ㎛, 또는 5 ㎛ 내지 15 ㎛ 일 수 있다. 예를 들어 코어는 실리콘 함유 화합물 SiO2를 함유할 수 있다.
[0109] The shell contains a composite comprising a first metal oxide; and a first carbon-based material.
[0110] First carbon-based materials, such as graphene, have high electronic conductivity, which can reduce the interfacial resistance between the dry negative electrode material and the electrolyte. Therefore, despite the introduction of a shell comprising the first carbon-based material, the increase in internal resistance of the lithium battery is suppressed or reduced.
[0111] The first carbon-based material included in the shell is derived from a graphene matrix, and therefore has a relatively low density and high porosity compared to conventional carbon-based materials derived from graphite-based materials. The d002 interplanar distance of the first carbon-based material included in the shell of the dry negative electrode active material may be, for example, 3.38 Å or more, 3.45 Å or more, 3.50 Å or more, 3.60 Å or more, 3.80 Å or more, or 4.00 Å or more. The d002 interplanar distance of the first carbon-based material included in the shell of the dry negative electrode active material may be, for example, 3.38 to 4.0 Å, 3.38 to 3.8 Å, 3.38 to 3.6 Å, 3.38 to 3.5 Å, or 3.38 to 3.45 Å. In contrast, the d002 interplanar distance of a conventional carbon-based material derived from a graphite-based material may be, for example, 3.38 Å or less, or 3.35 to 3.38 Å. Since the first metal oxide has a high voltage resistance, deterioration of the core can be prevented during charge / discharge at high voltage. The shell may include, for example, one type of the first metal oxide or two or more different types of the first metal oxides. As a result, the cycle characteristics of a lithium battery including the above-described dry negative electrode active material are improved, and volume change can be suppressed.
[0112] The shell may include, for example, a first carbon-based material, and the core may include, for example, a silicon-containing negative electrode active material, such as a silicon-containing structure and / or a silicon-containing compound. For example, the first carbon-based material may be composited with the silicon-containing structure and / or the silicon-containing compound through a mechanochemical reaction. The first carbon-based material may be chemically bound to the silicon-containing structure and / or the silicon-containing compound, for example, through a chemical bond. The core and the shell are composited by chemically bonding the first carbon-based material disposed in the shell and the silicon-containing structure and / or the silicon-containing compound disposed in the core through a chemical bond. Therefore, the composite negative electrode active material is distinguished from a simple physical mixture of the first carbon-based material and the silicon-containing structure and / or the silicon-containing compound. The first metal oxide and the carbon-based material included in the shell may also be chemically bound through a chemical bond. Here, the chemical bond is, for example, a covalent bond or an ionic bond.
[0113] The composite includes a first carbon-based material. The first carbon-based material has, for example, a branched structure, and at least one metal oxide selected from a first metal oxide and a second metal oxide may be distributed within the branched structure of the first carbon-based material. The branched structure of the first carbon-based material includes, for example, a plurality of particles of the first carbon-based material in contact with each other. The first carbon-based material having the branched structure may provide various conductive paths. The first carbon-based material may be, for example, graphene. The graphene has, for example, a branched structure, and at least one metal oxide selected from a first metal oxide and a second metal oxide may be distributed within the branched structure of the graphene. The branched structure of the graphene includes, for example, a plurality of graphene particles in contact with each other. The graphene having the branched structure may provide various conductive paths.
[0114] The first carbon-based material has, for example, a spherical structure, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure. The size of the spherical structure of the first carbon-based material may be 50 nm to 300 nm. There may be a plurality of first carbon-based materials having a spherical structure. Since the first carbon-based material has a spherical structure, the composite may have a rigid structure. The first carbon-based material may be, for example, graphene. The graphene has, for example, a spherical structure, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure. The size of the spherical structure of the graphene may be 50 nm to 300 nm. There may be a plurality of graphene having a spherical structure. Since the graphene has a spherical structure, the composite may have a rigid structure.
[0115] The first carbon-based material may have, for example, a spiral structure in which a plurality of spherical structures are connected, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure of the spiral structure. The size of the spiral structure of the first carbon-based material may be 500 nm to 100 um. Since the first carbon-based material has a spiral structure, the composite may have a rigid structure. The first carbon-based material may be, for example, graphene. The graphene may have, for example, a spiral structure in which a plurality of spherical structures are connected, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure of the spiral structure. The size of the spiral structure of the graphene may be 500 nm to 100 um. Since the graphene has a spiral structure, the composite may have a rigid structure.
[0116] The first carbon-based material may have, for example, a cluster structure in which a plurality of spherical structures are aggregated, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure of the cluster structure. The size of the cluster structure of the first carbon-based material may be from 0.5 mm to 10 cm. Since the first carbon-based material has the cluster structure, the composite may have a rigid structure. The first carbon-based material may be, for example, graphene. The graphene may have, for example, a cluster structure in which a plurality of spherical structures are aggregated, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure of the cluster structure. The size of the cluster structure of the graphene may be from 0.5 mm to 10 cm. Since the graphene has the cluster structure, the composite may have a rigid structure.
[0117] The composite may be, for example, a faceted-ball structure, and at least one selected from a first metal oxide and a second metal oxide may be distributed within or on the surface of the structure. Since the composite is a faceted-ball structure, the composite can be easily coated on the irregular surface of the core.
[0118] The composite may be, for example, a planar structure, and at least one selected from a first metal oxide and a second metal oxide may be distributed within or on the surface of the planar structure. Since the composite is such a two-dimensional planar structure, the composite can be easily coated on the irregular surface of the core.
[0119] The first carbon-based material may extend from the first metal oxide by a distance of 10 nm or less and may include at least 1 to 20 layers of the first carbon-based material. For example, a first carbon-based material having a total thickness of 12 nm or less may be disposed on the first metal oxide by stacking a plurality of first carbon-based material layers. For example, the total thickness of the carbon-based material may be 0.6 nm to 12 nm. The first carbon-based material may be, for example, graphene. The graphene may extend from the first metal oxide by a distance of 10 nm or less and may include at least 1 to 20 layers of graphene. For example, a graphene having a total thickness of 12 nm or less may be disposed on the first metal oxide by stacking a plurality of graphene layers. For example, the total thickness of the graphene may be 0.6 nm to 12 nm.
[0120] The shell may further comprise a second carbonaceous material that is fibrous carbon. The second carbonaceous material may comprise fibrous carbon.
[0121] By further including a second carbon-based material in the shell, which is a fibrous carbon, the conducting path of the negative electrode active material can be further lengthened. The second carbon-based material can form a three-dimensional conductive network between a plurality of composite negative electrode active materials, thereby reducing the internal resistance of the negative electrode including the negative electrode active material. By fixing the fibrous carbon on the negative electrode active material, a uniform and stable three-dimensional conductive network can be formed between the plurality of negative electrode active materials. Therefore, the high-rate characteristics of a lithium battery including a negative electrode active material including the second carbon-based material can be improved.
[0122] The aspect ratio of the second carbon-based material may be 10 or greater, for example, 10 to 100,000, 10 to 80,000, 10 to 50,000, 10 to 10,000, 10 to 5000, 10 to 1000, 10 to 500, 10 to 100, or 10 to 50. The aspect ratio of the second carbon-based material is, for example, the ratio of the length of the major axis passing through the center of the second carbon-based material, i.e., the length of the second carbon-based material, to the length of the minor axis perpendicular to the major axis, i.e., the diameter of the second carbon-based material.
[0123] The diameter of the second carbon-based material may be, for example, 1 nm to 50 nm, 1 nm to 30 nm, or 1 nm to 10 nm. When the diameter of the second carbon-based material is within the above range, the absolute number of strands per volume is reduced, thereby enabling uniform dispersion without a minimal reduction in internal resistance.
[0124] The length of the second carbon-based material can be, for example, 100 nm to 1000 μm, 100 nm to 500 μm, 100 nm to 100 μm, 100 nm to 50 μm, 100 nm to 10 μm, 100 nm to 5 μm, 100 nm to 2 μm, 100 nm to 1 μm, 100 nm to 500 nm, or 100 nm to 300 nm. The length of the second carbon-based material can be, for example, 500 nm to 1000 μm, 500 nm to 500 μm, 500 nm to 100 μm, 500 nm to 50 μm, 500 nm to 10 μm, 500 nm to 5 μm, or 500 nm to 2 μm. When the length of the second carbon-based material is within the above range, an effective conductive path can be provided without reducing the internal resistance of the electrode.
[0125] The second carbon-based material may include, for example, carbon nanofibers, carbon nanotubes, or a combination thereof.
[0126] The carbon nanotube may include, for example, a carbon nanotube primary structure, a carbon nanotube secondary structure formed by agglomeration of a plurality of carbon nanotube primary particles, or a combination thereof.
[0127] A carbon nanotube primary structure is a single carbon nanotube unit.
[0128] The carbon nanotube primary structure can include, for example, a single-walled carbon nanotube (SWCNT), a double-walled carbon nanotube (DWCNT), a multi-walled carbon nanotube (MWCNT), or a combination thereof. The diameter of the carbon nanotube primary structure can be, for example, 1 nm to 20 nm, 1 nm to 15 nm, or 2 nm to 10 nm. The length of the carbon nanotube primary structure can be, for example, 100 nm to 2 μm, 100 nm to 1 μm, 100 nm to 500 nm, 100 nm to 400 nm, 100 nm to 300 nm, or 200 nm to 300 nm. The diameter and length of the carbon nanotube primary structure can be measured by scanning electron microscope (SEM) images or laser diffraction.
[0129] A carbon nanotube secondary structure is a structure formed by assembling carbon nanotube primary structures, wholly or partially, to form a bundle or bundle shape. The carbon nanotube secondary structure may include, for example, a bundle-type carbon nanotube, a rope-type carbon nanotube, or a combination thereof. The diameter of the carbon nanotube secondary structure may be, for example, 2 nm or more or 3 nm or more. The diameter of the carbon nanotube secondary structure may be, for example, 50 nm or less, 30 nm or less, or 10 nm or less. The diameter of the carbon nanotube secondary structure may be, for example, 50 nm or less, 30 nm or less, or 10 nm or less. The diameter of the carbon nanotube secondary structure may be, for example, 2 nm to 50 nm, 2 nm to 30 nm, or 2 nm to 20 nm. The length of the carbon nanotube secondary structure can be, for example, 500 nm to 1000 μm, 500 nm to 500 μm, 500 nm to 200 μm, 500 nm to 100 μm, or 500 nm to 50 μm. The diameter and length of the carbon nanotube secondary structure can be measured using a scanning electron microscope (SEM) image, an optical microscope, or laser diffraction. The carbon nanotube secondary structure can be converted into a carbon nanotube primary structure, for example, by dispersing it in a solvent or the like, and then used in the manufacture of a dry negative electrode active material.
[0130] The content of the second carbon-based material may be, for example, 0.1 wt% to 50 wt%, 1 wt% to 40 wt%, or 5 wt% to 30 wt% based on the total weight of the first carbon-based material and the second carbon-based material. When the dry negative electrode active material includes the first carbon-based material and the second carbon-based material in this range, a conduction path is more effectively secured within the dry composite negative electrode active material, so that the internal resistance of the dry negative electrode active material can be further reduced. As a result, the cycle characteristics of a lithium battery including the dry negative electrode active material can be further improved. The content of the second carbon-based material may be, for example, 0.001 wt% to 5 wt%, 0.01 wt% to 3 wt%, or 0.01 wt% to 1 wt% based on the total weight of the dry negative electrode active material. By including a second carbon-based material within this range in the dry anode active material, a conductive path is secured within the composite anode active material, further reducing the internal resistance of the dry anode active material. Consequently, the cycle characteristics of a lithium battery including the dry anode active material can be further improved.
[0131] The specific surface area of the dry cathode active material is, for example, 1 m 2 / g to 100 m 2 / g, 1 m 2 / g to 50 m 2 / g, or 1 m 2 / g to 30 m 2 / g. Since the composite negative electrode active material has a specific surface area in this range, the cycle characteristics of a lithium battery employing the composite negative electrode active material can be further improved. The average particle diameter (D50) of the composite negative electrode active material is, for example, 1 ㎛ to 30 ㎛, 3 ㎛ to 20 ㎛, or 5 ㎛ to 15 ㎛. The particle diameter (D10) of the composite negative electrode active material is, for example, 0.1 ㎛ to 10 ㎛, 0.5 ㎛ to 10 ㎛, or 1 ㎛ to 10 ㎛. The particle diameter (D90) of the composite negative electrode active material is, for example, 10 ㎛ to 50 ㎛, 10 ㎛ to 30 ㎛, or 10 ㎛ to 25 ㎛. When the composite negative electrode active material has an average particle size (D50), particle size (D10), and / or particle size (D90) in this range, the cycle characteristics of a lithium battery employing such a dry negative electrode can be further improved.
[0132] The content of the dry conductive material included in the dry negative electrode film is, for example, 0.1 to 5 wt%, 0.5 to 5 wt%, or 1 to 5 wt% based on the total weight of the dry negative electrode film. By including the dry conductive material in this range in the dry negative electrode film, the conductivity of the dry negative electrode film is improved, and the cycle characteristics of a lithium battery including the dry negative electrode film can be improved.
[0133] Dry cathode films are, for example, self-standing films. Dry cathode films can maintain a film form without a support, for example. Therefore, dry cathode films can be prepared as separate self-standing films and then placed on electrode current collectors. Since dry cathode films are manufactured through a dry process, they do not contain any intentionally added process solvents. For example, they do not contain residual processing solvents. While trace amounts of unintended solvents may remain in the dry cathode film, these solvents are not intentionally added process solvents. Therefore, dry cathode films are distinguished from wet electrode films, which are manufactured by mixing components and process solvents and then drying to remove some or all of the process solvent.
[0134] In a dry negative electrode film according to an embodiment, the first dry negative electrode film includes a mixture of a carbon-based material and a silicon-based active material as a core of a dry composite negative electrode active material; a composite of a carbon-based material and a silicon-based active material; or a combination thereof, and the second dry negative electrode film includes a carbon-based material as a core of a dry composite negative electrode active material, and the contents of the binder and the composite of the first dry negative electrode film are equal to or greater than the contents of the binder and the composite of the second dry negative electrode film, respectively. In some embodiments, the content of the binder of the first dry negative electrode film is equal to (e.g., equal to) or greater than the content of the binder of the second dry negative electrode film. In some embodiments, the amount of the composite of the first dry negative electrode film is equal to (e.g., equal to) or greater than the content of the composite of the second dry negative electrode film.
[0135] The above second dry negative electrode film may further include a conductive material. The conductive material may be a composite (GB), Denka black, summer black, superfi, carbon nanotubes, activated carbon, carbon molecular sieves, graphene, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers, carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives, etc. Here, the composite is the same as a composite including at least one first metal oxide and a first carbon-based material constituting the shell of the composite negative electrode active material, and therefore, a description thereof will be omitted.
[0136] The dry negative electrode film comprises a first dry negative electrode film disposed adjacent to a negative electrode current collector and a second dry negative electrode film disposed on the first dry negative electrode film, wherein the first dry negative electrode film comprises a mixture of a carbon-based material and a silicon-based active material as a core of a dry composite negative electrode active material; a composite of a carbon-based material and a silicon-based active material; or a combination thereof, and the second dry negative electrode film comprises a mixture of a carbon-based compound and a silicon-based active material; a composite of a carbon-based compound and a silicon-based active material; or a combination thereof as a core of a dry negative electrode active material, wherein the content of the composite (GB) and the binder of the first dry negative electrode film is equal to or greater than the content of the composite and the binder of the second dry negative electrode film, and wherein the content of the mixture of the carbon-based material and the silicon-based active material; the composite of the carbon-based material and the silicon-based active material; or a combination thereof in the first dry negative electrode film is greater than the content of the mixture of the carbon-based material and the silicon-based active material; the composite of the carbon-based material and the silicon-based active material; or a combination thereof in the second dry negative electrode film. A composite of a carbon-based material and a silicon-based active material; or a combination thereof, which is equal to or greater than the content of the composite. In some embodiments, the amount of binder in the first dry negative electrode film is equal to (e.g., equal to) the content of the binder in the second dry negative electrode film, or greater than the amount of the composite (GB) in the first dry negative electrode film. The dry negative electrode film has the same content (e.g., equal to) or greater than the content of the composite (GB) in the second dry negative electrode film. In some embodiments, the content of the carbon-based material in the first dry negative electrode film is equal to (e.g., equal to) the content of the carbon-based material in the second dry negative electrode film, and the content of silicon is greater than or equal to the content of the carbon-based material in the second dry negative electrode film. The content of the silicon-based active material in the first dry negative electrode film is equal to (e.g., equal to) or greater than the content of the silicon-based active material in the second dry negative electrode film.
[0137] The first dry negative electrode film includes a carbon-based material and a silicon-based active material as a core of a dry composite negative electrode active material, and the silicon-based active material includes a silicon composite structure. The second dry negative electrode film includes a carbon-based material as a core of a dry composite negative electrode active material, and the contents of the binder and the composite of the first dry negative electrode film are equal to or greater than the contents of the binder and the composite of the second dry negative electrode film.
[0138] The above dry negative electrode film includes a first dry negative electrode film disposed adjacent to a negative electrode current collector and a second dry negative electrode film disposed on the first dry negative electrode film, wherein the first dry negative electrode film includes a carbon-based material and a silicon-based active material as a core of a dry composite negative electrode active material, and the second dry negative electrode film includes a carbon-based material and a silicon-based active material as a core of a dry negative electrode active material. Here, the silicon-based active materials of the first dry negative electrode film and the second dry negative electrode film include a silicon composite structure. The binder content of the first dry negative electrode film is equal to or greater than the binder content of the second dry negative electrode film, and the composite (GB) content of the first dry negative electrode film is equal to or greater than the composite content of the second dry negative electrode film.
[0139] The content of the carbon-based material in the first dry negative electrode film is equal to or greater than the content of the carbon-based material in the second dry negative electrode film. And the content of the silicon-based active material in the first dry negative electrode film is equal to or greater than the content of the silicon-based active material in the second dry negative electrode film.
[0140] The structure of a dry cathode-separator subassembly employing a dry cathode film according to an embodiment will be described with reference to the attached drawings.
[0141] Referring to FIG. 3a, the dry negative electrode-separator subassembly (200) has a structure in which a first dry negative electrode film (20a) is laminated on a negative electrode current collector (20), a second dry negative electrode film (20b) is laminated on top of the first dry negative electrode film (20a), and a separator (4) is laminated on top of the first dry negative electrode film (20a).
[0142] The dry cathode-separator subassembly (200) shown in FIG. 3b differs from the case of FIG. 3a only in that an intermediate layer (30) is disposed between the cathode current collector (20) and the first dry cathode film (20a).
[0143] Figures 4a to 4c show a laminated structure of a dry cathode according to an embodiment, and specifically show the composition of the first dry cathode and the second dry cathode.
[0144] According to an embodiment, as shown in Fig. 4a, the first dry negative electrode film (20a) includes a composite negative electrode active material in which a shell containing a complex (GB1) is coated on graphite, which is a carbon-based material, which is the first negative electrode active material, a silicon composite structure (SCN) as the second negative electrode active material, and polytetrafluoroethylene (PTFE1) as a dry binder. The second dry negative electrode film (20b) includes a composite negative electrode active material in which a shell containing a complex (GB2) is coated on graphite, which is the first negative electrode active material, a silicon composite structure (SCN) as the second negative electrode active material, and polytetrafluoroethylene (PTFE2) as a dry binder.
[0145] The above silicon composite structure is a silicon-carbon composite including silicon particles and a first carbon-based material, a silicon-carbon composite including a core in which silicon particles and a second carbon-based material are mixed and a third carbon-based material surrounding the core, or a combination thereof.
[0146] The contents of PTFE1 and GB1 of the first dry negative electrode film (20a) are adjusted to be equal to or greater than the contents of PTFE2 and GB2 of the second dry negative electrode film (20b), respectively (PTFE1 ≥ PTFE2, GB1 ≥ GB2). Within these ranges, the dry negative electrode film can be effectively prevented from being peeled off from the negative electrode current collector, and the growth of lithium dendrites away from the negative electrode current collector can be induced to be small.
[0147] The mixing weight ratio of PTFE1 and PTFE2 is not limited, but is 10:1 to 1.1:1, 9.5:1 to 1.3:1, 9:1 to 1.5:1, 9:1 to 1.5:1, 6:1 to 1.5:1, 5:1 to 1.8:1, or 4:1 to 2:1.
[0148] The mixing weight ratio of GB1 and GB2 is not limited, but is 10:1 to 1.1:1, 9.5:1 to 1.3:1, 9:1 to 1.5:1, 9:1 to 1.5:1, 6:1 to 1.5:1, 5:1 to 1.8:1, or 4:1 to 2:1.
[0149] In the first dry cathode film and the second dry cathode film, the content of the silicon composite structure is 5 to 20 parts by weight, 11 to 18 parts by weight, or 12 to 15 parts by weight based on 100 parts by weight of the total content of the graphite and silicon composite structure.
[0150] According to another embodiment, as shown in FIG. 4b, the first dry negative electrode film (20a) includes a composite negative electrode active material in which a shell containing a complex (GB1) is coated on graphite as the first negative electrode active material, a silicon composite structure as the second negative electrode active material, and polytetrafluoroethylene (PTFE1) as a dry binder. The second dry negative electrode film (20a) includes a composite negative electrode active material in which a shell containing a complex (GB2) is coated on graphite as the first negative electrode active material, a silicon composite structure as the second negative electrode active material, and polytetrafluoroethylene (PTFE2) as a dry binder.
[0151] The SCN1 content of the first dry negative electrode film is controlled to be greater than the SCN2 content of the second dry negative electrode film. When the SCN1 content is controlled to be greater than the SCN2 content, the PTFE1 and GB1 contents of the first dry negative electrode film are controlled to be equal to or greater than the PTFE2 and GB2 contents of the second dry negative electrode film, respectively (SCN1 ≥ SCN2, PTFE1 ≥ PTFE2, GB1 ≥ GB2). Within these ranges, the volume expansion of the dry negative electrode film can be suppressed, and the growth of lithium dendrites in the negative electrode film far from the current collector can be induced to be small.
[0152] The mixing weight ratio of the contents of SCN1 of the first dry cathode film and SCN2 of the second dry cathode film is not limited, but is 10:1 to 1.1:1, 9.5:1 to 1.3:1, 9:1 to 1.5:1, 9:1 to 1.5:1, 6:1 to 1.5:1, 5:1 to 1.8:1, or 4:1 to 2:1.
[0153] When the silicon content of the first dry negative electrode film is greater than that of the second dry negative electrode film, the electrode expansion rate is reduced, dendrite formation is reduced during rapid charging, electrolyte invasion characteristics are improved, electrode detachment is reduced, and higher electrode stability can be secured with less binder. In addition, when the contents of PTFE1 and GB1 of the first dry negative electrode film are adjusted to be equal to or greater than the contents of PTFE2 and GB2 of the second dry negative electrode film, peeling of the dry negative electrode film from the negative electrode current collector can be effectively prevented, and lithium dendrite growth away from the negative electrode current collector can be induced to be small.
[0154] According to another embodiment, as shown in FIG. 4c, the second dry negative electrode film (20b) disposed far from the negative electrode collector (20) includes a first composite negative electrode active material containing a graphite core / composite (GB1) shell as a negative electrode active material and PTFE1 as a binder, and the first dry negative electrode film (20a) disposed at a position adjacent to the negative electrode collector (20) uses a first composite negative electrode active material in which a shell containing a composite (GB1) is coated on graphite as a dry composite negative electrode active material, a second composite negative electrode active material containing a silicon composite structure (SCN) as a core / composite (GB2) as a shell, and PTFE2 as a binder.
[0155] The total content of graphite and silicon composite structure (SCN) of the first dry cathode film can be significantly controlled compared to the content of graphite of the second dry cathode film.
[0156] The mixing weight ratio of the total content of the graphite and silicon composite structure (SCN) of the first dry negative electrode film to the content of the graphite of the second dry negative electrode film is not limited, but is 10:1 to 1.1:1, 9.5:1 to 1.3:1, 9:1 to 1.5:1, 9:1 to 1.5:1, 6:1 to 1.5:1, 5:1 to 1.8:1, or 4:1 to 2:1.
[0157] For example, in the first composite negative electrode active material, the content of the composite (GB1) can be controlled to be greater than that of the composite (GB2), and the content of the binder PTFE1 can be controlled to be equal to or greater than that of the binder PTFE2 (PTFE1 ≥ PTFE2, GB1 ≥ GB2). By forming such a structure, it is possible to control volume expansion and form a structure that induces small lithium dendrite growth on the side far from the current collector.
[0158] The mixing weight ratio of PTFE1 and PTFE2 and the mixing weight ratio of GB1 and GB2 in FIG. 4b and FIG. 4c are as described in FIG. 4a.
[0159] The first dry negative electrode film and the second dry negative electrode film of FIGS. 4A to 4C may further include a conductive material. For example, the second dry negative electrode film of FIG. 4C includes a first composite negative electrode active material containing a graphite core / composite (GB1) shell as a negative electrode active material and PTFE1 as a binder, and the second dry negative electrode film may further include a conductive material. A composite (GB) or the like may be used as the conductive material. Here, the composite is the same as a composite including one or more first metal oxides and a first carbon-based material constituting the shell of the composite negative electrode active material, and therefore, a description thereof will be omitted.
[0160] In the dry cathode including the above-described dry cathode film, the first dry cathode film and
[0161] The thickness of the second dry cathode film can be formed at a ratio of 1:3 to 3:1, 1:2 to 2:1, or 1:1.
[0162] According to an embodiment, the dry cathode film has a multilayer structure of two or more layers, two to five layers, or two to three layers, and is capable of forming a thick film.
[0163] The term "solvent-free" as used herein refers to a component that excludes any amount of residual processing solvent to function properly. In one embodiment, the dry negative electrode film is a self-standing film, and the dry negative electrode film is free of residual processing solvent, for example, is solvent-free.
[0164] The tensile strength of the dry negative electrode film according to one embodiment may be, for example, 450 kPa or more, 500 kPa or more, 700 kPa or more, or 1000 kPa or more at 25°C. This tensile strength is before rolling. The tensile strength of the dry negative electrode film before rolling may be, for example, 500 kPa to 5000 kPa, 600 kPa to 5000 kPa, 700 kPa to 5000 kPa, or 800 kPa to 5000 kPa at 25°C.
[0165] The tensile strength of the dry negative electrode film after rolling at 25°C can be 1000 kPa or more, 1050 kPa or more, 1200 kPa or more, or 1500 kPa or more. The tensile strength of the dry negative electrode film after rolling at 25°C can be, for example, 1000 kPa to 5000 kPa, 1050 kPa to 5000 kPa, 1090 kPa to 5000 kPa, 1200 kPa to 5000 kPa, or 1800 kPa to 5000 kPa. Since the dry negative electrode film has a tensile strength in the above-described range, the structural stability of the dry negative electrode film can be improved. Therefore, the dry negative electrode film can maintain a stable three-dimensional conductive network during the charge and discharge process, thereby improving the reversibility of the electrode reaction. The high tensile strength of the dry negative electrode film within this range can enhance the mechanical strength of the dry negative electrode film. The enhanced mechanical strength of the dry negative electrode film can suppress or reduce localized deterioration due to volume changes during charge and discharge of an electrode comprising the dry negative electrode film and a lithium battery comprising the same. Consequently, the cycle characteristics of the lithium battery can be improved.
[0166] The dry cathode film comprises the above-described dry cathode active material, providing improved cycle characteristics and reduced volume change.
[0167] A method for manufacturing a dry negative electrode includes, for example, a step of preparing a dry mixture by dry mixing a dry composite negative electrode active material and a dry binder; a step of providing a negative electrode current collector; a step of disposing an intermediate layer on one surface of the negative electrode current collector; and a step of disposing the dry mixture on the intermediate layer and rolling it to obtain a dry negative electrode film, thereby manufacturing a negative electrode having a negative electrode active material layer disposed on one surface of the negative electrode current collector.
[0168] First, a dry mixture is prepared by dry mixing a composite negative electrode active material and a dry binder.
[0169] When preparing the dry mixture, additional dry conductive agent may be included.
[0170] Dry mixing means mixing without a process solvent. A process solvent is, for example, a solvent used in the preparation of an electrode slurry. A process solvent is, for example, water, NMP, etc., but is not limited thereto, and is not limited as long as it is a process solvent used in the preparation of an electrode slurry. Dry mixing can be performed using a stirrer at a temperature of, for example, 25 to 65°C. Dry mixing can be performed using a stirrer at a rotation speed of, for example, 10 to 10,000 rpm, or 100 to 10,000 rpm. Dry mixing can be performed using a stirrer for, for example, 1 to 200 minutes, or 1 to 150 minutes. The composite negative electrode active material is a dry composite negative electrode active material.
[0171] Dry mixing may be performed, for example, more than once. First, a first mixture may be prepared by first dry mixing the dry composite negative electrode active material and the dry binder. A dry conductive material may be further added during the preparation of the first mixture. The first dry mixing may be performed, for example, at a temperature of 25 to 65°C, at a rotation speed of 2000 rpm or less, or 500 to 2000 rpm, for 15 minutes or less, for example, 5 to 15 minutes. The first dry mixing may allow the dry composite negative electrode active material and the dry binder to be uniformly mixed. Subsequently, the second mixture may be prepared by second dry mixing the dry composite negative electrode active material and the dry binder. The secondary dry mixing can be performed, for example, at a temperature of 25 to 65°C, or 25 to 65°C, at a rotation speed of 4000 rpm or more, or 4000 to 9000 rpm, for 10 minutes or more, or 10 to 60 minutes. The secondary dry mixing can yield a dry mixture comprising a fibrillated dry binder.
[0172] The stirrer is, for example, a kneader. The stirrer includes, for example, a chamber; one or more rotating shafts disposed inside the chamber and rotating; and blades rotatably coupled to the rotating shafts and disposed in the longitudinal direction of the rotating shafts. The blades may be, for example, one or more selected from a ribbon blade, a sigma blade, a jet (Z) blade, a dispersion blade, and a screw blade. By including the blades, a dry negative electrode composite active material, a dry conductive material, and a dry binder can be effectively mixed without a solvent, thereby producing a dough-like mixture.
[0173] The prepared dry mixture can be extruded into a sheet form by feeding it into an extrusion device. The pressure during extrusion is, for example, 4 MPa to 100 MPa, or 10 MPa to 90 MPa. The obtained sheet-form extruded product is a dry negative electrode film as a sheet for the negative electrode active material layer. By repeating this process, a dry negative electrode film having a multilayer structure can be easily manufactured.
[0174] Dry conductive materials include, but are not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. Any material used as a conductive material in the relevant technical field may be used. The conductive material is, for example, a carbon-based conductive material. A dry conductive material is a conductive material that does not come into contact with a process solvent.
[0175] According to one embodiment, the dry binder includes a fluorine-based binder.
[0176] Dry binders include, but are not limited to, vinylidene fluoride / hexafluoropropylene copolymers, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the aforementioned polymers, styrene butadiene rubber-based polymers, etc., and any polymer used in the art may be used. An example of a dry binder is polytetrafluoroethylene (PTFE). The term "dry binder" is a binder that does not come into contact with a process solvent.
[0177] In some embodiments, the dry binder may be a fibrillated binder. As used herein, the term "fibrillation" refers to a process of converting fibers of a material (e.g., grinding or pulverizing) into individual units of material smaller than the fibers. In one embodiment, the dry binder may have a glass transition temperature (Tg) of from about 15°C to about 100°C.
[0178] It is also possible to form pores inside the negative electrode active material layer by further adding a plasticizer or pore former to the dry mixture.
[0179] The contents of the dry composite negative electrode active material, dry conductive agent, and dry binder used in the negative electrode active material layer are used in the same range as when manufacturing a wet negative electrode. Next, a negative electrode current collector is provided.
[0180] Although not shown in the drawing, the negative electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film may be liquefied when a short circuit occurs, thereby suppressing a rapid increase in current. The base film may be, for example, an insulator. The metal layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof.
[0181] The metal layer can act as an electrochemical fuse and be cut off in case of overcurrent to prevent a short circuit. The limit current and the maximum current can be controlled by adjusting the thickness of the metal layer. The metal layer can be plated or deposited on the base film. When the thickness of the metal layer is reduced, the limit current and / or the maximum current of the negative electrode current collector (521b, 522b) decreases, thereby improving the stability of the lithium battery in case of a short circuit. A lead tab can be added on the metal layer for connection to the outside. The lead tab can be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, etc. During welding, the base film and / or the metal layer melt, so that the metal layer can be electrically connected to the lead tab. To strengthen the welding between the metal layer and the lead tab, a metal chip can be added between the metal layer and the lead tab. The metal piece may be a thin piece of the same material as the metal of the metal layer. The metal piece may be, for example, a metal foil, a metal mesh, etc. The metal piece may be, for example, aluminum foil, copper foil, SUS foil, etc. After the metal piece is placed on the metal layer, the lead tab may be welded to the metal piece / metal layer laminate or the metal piece / metal layer / base film laminate. During welding, the base film, the metal layer, and / or the metal piece may melt, so that the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal layer. The base film may have a thickness of, for example, 1 to 50 μm, 1.5 to 50 μm, 1.5 to 40 μm, or 1 to 30 μm. When the base film has a thickness in this range, the weight of the electrode assembly can be more effectively reduced.The melting point of the base film may be, for example, 100°C to 300°C, 100°C to 250°C, or 100°C to 200°C. Since the base film has a melting point within this range, the base film can be melted and easily bonded to the lead tab during the process of welding the lead tab. To improve the adhesion between the base film and the metal layer, a surface treatment such as corona treatment may be performed on the base film. The thickness of the metal layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to ㎛. Since the metal layer has a thickness within this range, the stability of the electrode assembly can be secured while maintaining conductivity. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness within this range, the connection between the metal layer and the lead tab can be performed more easily. By having this structure as the negative electrode collector, the weight of the electrode can be reduced, and as a result, the energy density can be improved.
[0182] The negative current collector is, for example, aluminum foil.
[0183] Next, an intermediate layer is placed on at least one surface of the negative electrode collector. The intermediate layer may include a carbon-based conductive material and a binder. The intermediate layer may be omitted.
[0184] The carbon-based conductive material may be or include a fibrous carbon-based material, a particulate carbon-based material, or a combination thereof. The aspect ratio of the fibrous carbon-based material and the particulate carbon-based material may independently be greater than or equal to 10, for example, from about 10 to about 100,000, from about 10 to about 80,000, from about 10 to about 50,000, from about 10 to about 100,000, from about 10,000, from about 10 to about 5000, from about 10 to about 100, or from about 10 to about 50.
[0185] Next, a dry negative electrode film, which is a sheet for a negative electrode active material layer prepared on an intermediate layer, is placed and rolled to manufacture a negative electrode having a negative electrode active material layer placed on one surface of a negative electrode current collector. The intermediate layer is placed between the negative electrode current collector and the negative electrode active material layer.
[0186] Rolling can be done by, but is not limited to, a roll press, a flat plate press, etc. The pressure during rolling is, for example, 0.1 ton / cm. 2 10.0 ton / cm 2 However, it is not limited to this range. If the pressure during rolling is excessively high, cracks may occur in the negative electrode collector. If the pressure during rolling is excessively low, the bonding strength between the negative electrode collector and the negative electrode active material layer may be reduced.
[0187] A lithium battery according to another embodiment employs a negative electrode including the above-described dry negative electrode film.
[0188] By adopting the above-described negative electrode, a lithium battery provides improved interfacial resistance, cycle characteristics and reduced volume change.
[0189] Lithium batteries are manufactured by, for example, the following exemplary methods, but are not necessarily limited to these methods and are adjusted according to required conditions.
[0190] First, a dry cathode is manufactured according to the cathode manufacturing method described above.
[0191] Next, a cathode active material composition is prepared, comprising a mixture of a cathode active material, a conductive agent, a binder, and a solvent. The cathode active material composition is directly coated and dried on a cathode current collector to produce a cathode plate. Alternatively, the cathode active material composition can be cast on a separate support, and then a film peeled from the support can be laminated onto an aluminum current collector to produce a cathode plate.
[0192] The cathode active material is a lithium-containing metal oxide, and any one commonly used in the art can be used without limitation. For example, the cathode active material can be at least one compound oxide of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof. The cathode active material can include, for example, at least one selected from the group consisting of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, and lithium manganese oxide, but is not necessarily limited thereto, and any one used as a cathode active material of a lithium battery in the art can be used.
[0193] The cathode active material is, for example, Li a A 1-b B b D2 (in the above formula, 0.90 ≤ a ≤ 1.8, and 0 ≤ b ≤ 0.5); Li a E 1-b B b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B b O 4-c D c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B c D α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B c O 2-α F α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b Bc O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c D α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a MnG bO2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) It may include a compound represented by any one of the chemical formulas Fe2(PO4)3(0 ≤ f ≤ 2); and LiFePO4.
[0194] In the chemical formula described above, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof.
[0195] It is also possible to use a compound having a coating layer added to the surface of the above-mentioned compound, or it is also possible to use a mixture of the above-mentioned compound and a compound having a coating layer added. The coating layer added to the surface of the above-mentioned compound includes, for example, a coating element compound of an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element of the coating element. The compound forming the coating layer is amorphous or crystalline. The coating elements included in the coating layer are Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof. The method for forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method includes, for example, spray coating and dipping. Since specific coating methods are well understood by those working in the relevant field, a detailed description thereof will be omitted.
[0196] The cathode active material is, for example, LiNiO2, LiCoO2, LiMn x O 2x (x=1, 2), LiNi 1-x Mn x O2(0 <x<1), LiNi 1-x-y Co x Mn y O2(0≤x≤0.5, 0≤y≤0.5), LiFeO2, V2O5, TiS, MoS, etc. can be used.
[0197] The cathode active material is, for example, Li a Ni x Co y M z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0.8≤x<1, 0≤y≤0.3, 0 <z≤0.3, x+y+z=1, M은 망간(Mn), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al) 및 보론(B)으로 이루어진 군으로부터 선택된 하나 이상, A는 F, S, Cl, Br 또는 이들의 조합), LiNi x Co y Mr z O2(0.8≤x≤0.95, 0 <y≤0.2, 0<z≤0.2 및 x+y+z=1), LiNi x Co y Al z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2, x+y+z=1), LiNi x Co y Al v Mr w O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <v≤0.2, 0<w≤0.2, x+y+v+w=1), Li a Ni x Mr y m' z O 2-b A b (1.0≤a≤1.2, 0≤b≤0.2, 0 <x≤0.3, 0.5≤y<1, 0<z≤0.3, 및 x+y+z=1, M'는 코발트(Co), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합, A는 F, S, Cl, Br 또는 이들의 조합) 등이 사용될 수 있다.
[0198] In the positive electrode active material composition, the conductive agent, binder, and solvent may be the same as those used in the negative electrode active material composition. Meanwhile, it is also possible to form pores within the electrode plate by further adding a plasticizer to the positive electrode active material composition and / or the negative electrode active material composition.
[0199] The contents of the cathode active material, conductive agent, binder, and solvent are at levels typically used in lithium batteries. Depending on the intended use and configuration of the lithium battery, one or more of the conductive agent, binder, and solvent may be omitted.
[0200] The binder content included in the positive electrode may be, for example, 0.1 to 10 wt% or 0.1 to 5 wt% of the total weight of the positive electrode active material layer. The conductive material content included in the positive electrode may be, for example, 0.1 to 10 wt% or 0.1 to 5 wt% of the total weight of the positive electrode active material layer. The positive electrode active material content included in the positive electrode may be, for example, 70 wt% to 99 wt%, 90 wt% to 99 wt%, or 95 wt% to 99 wt% of the total weight of the positive electrode active material layer.
[0201] The positive electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. By having such a structure, the positive electrode current collector can reduce the weight of the electrode and consequently improve the energy density of the lithium battery.
[0202] Next, a separator to be inserted between the positive and negative electrodes is prepared.
[0203] Any separator commonly used in lithium batteries can be used. For example, a separator with low resistance to ion migration and excellent electrolyte absorption capacity is used. The separator may be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or combinations thereof, and may be in the form of a nonwoven or woven fabric. For lithium-ion batteries, a rollable separator, such as polyethylene or polypropylene, is used, while for lithium-ion polymer batteries, a separator with excellent organic electrolyte absorption capacity is used.
[0204] The separator is manufactured by the following exemplary methods, but is not limited to these methods and may be adjusted according to required conditions.
[0205] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated and dried on the electrode to form a separator. Alternatively, the separator composition is cast on a support and dried, and then a separator film peeled from the support is laminated on the electrode to form a separator.
[0206] The polymer used in separator manufacturing is not particularly limited; any polymer used as a binder for electrode plates can be used. Examples include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or mixtures thereof.
[0207] Next, the electrolyte is prepared.
[0208] The electrolyte is, for example, an organic electrolyte. An organic electrolyte is prepared by dissolving a lithium salt in an organic solvent, for example.
[0209] Any organic solvent used in the relevant technical field may be used. Examples of the organic solvent include propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.
[0210] Lithium salts are all possible if they are used as lithium salts in the relevant technical field. Lithium salts include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(FSO2)2N, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(1≤x≤20, 1≤y≤20), LiCl, LiI or mixtures thereof.
[0211] Alternatively, the electrolyte is a solid electrolyte. Examples of solid electrolytes include, but are not limited to, boron oxide, lithium oxynitride, and the like, and any solid electrolyte used in the relevant technical field may be used. The solid electrolyte is formed on the cathode, for example, by a method such as sputtering, or a separate solid electrolyte sheet is laminated on the cathode.
[0212] The solid electrolyte is, for example, an oxide-based solid electrolyte or a sulfide-based solid electrolyte.
[0213] Solid electrolytes are, for example, oxide-based solid electrolytes. Oxide-based solid electrolytes are Li 1+x+y Alx Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(O≤x<1, O≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M = Te, Nb, or Zr, x is an integer from 1 to 10) is one or more selected from. The solid electrolyte is manufactured by a sintering method, etc. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10, 0<a<2) is a garnet-type solid electrolyte selected from among.
[0214] The sulfide-based solid electrolyte may include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles may include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles may be Li2S or P2S5. Sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixing molar ratio of Li2S to P2S5 may be, for example, in a range of about 50:50 to about 90:10. In addition, Li3PO4, halogen, halogen compound, Li 2+2x Zn 1-x GeO4("LISICON", 0≤x<1), Li 3+y PO 4-x N x ("LIPON", 0 <x<4, 0<y<3), Li 3.25 Ge 0.25 P 0.75 S4("ThioLISICON"), Li2O-Al2O3-TiO2-P2O 5( An inorganic solid electrolyte prepared by adding "LATP") etc. to an inorganic solid electrolyte of Li2S-P2S5, SiS2, GeS2, B2S3, or a combination thereof can be used as a sulfide solid electrolyte. Non-limiting examples of sulfide solid electrolyte materials include Li2S-P2S5; Li2S-P2S5-LiX (X=halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S -P2S5-Z m S n(0 <m<10, 0<n<10, Z=Ge, Zn 또는 Ga); Li2S-GeS2; Li2S-SiS2-Li3PO4; 및 Li2S-SiS2-Li p MO q (0 <p<10, 0<q<10, M=P, Si, Ge, B, Al, Ga 또는 In)을 포함한다. 이와 관련하여, 황화물계 고체전해질 재료는 황화물계 고체전해질 물질의 원료 시작 물질(예를 들면, Li2S, P2S5등)을 용융 담금질법(melt quenching method), 기계적 밀링법 등에 의해 처리함으로써 제조될 수 있다. 또한, 소성(calcinations) 공정이 상기 처리 후에 수행될 수 있다. 황화물계 고체전해질은 비정질이거나, 결정질이거나, 이들이 혼합된 상태일 수 있다.
[0215] Referring to FIG. 5, a lithium battery (1) according to an embodiment includes a positive electrode (3), a negative electrode (2), and a separator (4). The positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An organic electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing the lithium battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.
[0216] Referring to FIG. 6, a lithium battery (1) according to an embodiment includes a positive electrode (3), a negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2), and the positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, but may have, for example, a cylindrical shape, a thin film shape, etc.
[0217] Referring to FIG. 7, a lithium battery (1) according to an embodiment includes a positive electrode (3), a negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2) to form a battery structure. The battery structure (7) is stacked in a bi-cell structure and then accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, but may be, for example, a cylindrical shape, a thin film shape, etc.
[0218] A pouch-type lithium battery corresponds to the lithium batteries of FIGS. 5 to 7, each of which uses a pouch as a battery case. The pouch-type lithium battery includes one or more battery structures. A separator is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are laminated in a bi-cell structure, then impregnated with an organic electrolyte, and accommodated and sealed in a pouch to complete the pouch-type lithium battery. For example, although not shown in the drawings, the above-described positive electrode, negative electrode, and separator may be simply laminated and accommodated in a pouch in the form of an electrode assembly, or may be wound or folded into a jelly-roll-shaped electrode assembly and then accommodated in a pouch. Subsequently, an organic electrolyte is injected into the pouch and sealed to complete the lithium battery.
[0219] Lithium batteries are used in electric vehicles (EVs) due to their excellent cycle life and high-rate characteristics. For example, they are used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). They are also used in applications requiring large amounts of power storage, such as electric bicycles and power tools.
[0220] Lithium batteries are stacked in multiple layers to form a battery module, and the multiple battery modules form a battery pack. Such a battery pack can be used in any device requiring high capacity and high output. For example, it can be used in laptops, smartphones, electric vehicles, etc. The battery module includes, for example, multiple batteries and a frame that holds them. The battery pack includes, for example, multiple battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. The multiple battery packs are controlled by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.
[0221] A dry negative electrode according to another embodiment comprises: an electrode current collector; and the above-described dry negative electrode film disposed on one or both sides of the electrode current collector.
[0222] By including a dry cathode film in the dry cathode, the internal resistance of the dry cathode is reduced and the mechanical properties are improved.
[0223] The electrode current collector may include, for example, a substrate.
[0224] The material constituting the substrate may be any material that does not react with lithium, i.e., does not form an alloy or compound with lithium, and has conductivity. The substrate may be, for example, a metal or an alloy. The substrate may be made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel (SUS), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), or an alloy thereof. The substrate may have a form selected from, for example, a sheet, a foil, a film, a plate, a porous body, a mesoporous body, a body containing through-holes, a polygonal ring body, a mesh body, a foam body, and a non-woven body, but is not necessarily limited to these forms, and any form used in the relevant technical field may be used.
[0225] The electrode current collector may include, for example, a substrate; and an interlayer disposed between the substrate and the dry negative electrode film. The interlayer may include, for example, a carbon-based conductive material.
[0226] The interlayer is, for example, directly disposed on one or both sides of the substrate. Therefore, no other layers may be disposed between the substrate and the interlayer. By directly disposing the interlayer on one or both sides of the substrate, the bonding strength between the substrate and the dry cathode film can be further enhanced.
[0227] The thickness of the intermediate layer is, for example, 0.01 to 30%, 0.1 to 30%, 0.5 to 30%, 1 to 25%, 1 to 20%, 1 to 15%, 1 to 10%, 1 to 5%, or 1 to 3% of the thickness of the substrate. The thickness of the intermediate layer is, for example, 10 nm to 5 ㎛, 50 nm to 5 ㎛, 200 nm to 4 ㎛, 500 nm to 3 ㎛, 500 nm to 2 ㎛, 500 nm to 1.5 ㎛, or 700 nm to 1.3 ㎛. When the intermediate layer has a thickness in this range, the bonding force between the substrate and the dry negative electrode film is further improved, and an increase in interfacial resistance is suppressed.
[0228] The intermediate layer includes, for example, a carbon-based conductive material. The carbon-based conductive material included in the intermediate layer may be selected from carbon-based conductive materials used in dry cathode films. The intermediate layer may include the same carbon-based conductive material used in the dry cathode film. By including a carbon-based conductive material in the intermediate layer, the intermediate layer may be, for example, a conductive layer.
[0229] The intermediate layer may additionally include, for example, a binder. By additionally including a binder in the intermediate layer, the bonding strength between the substrate and the dry negative electrode film can be further improved. The binder included in the intermediate layer may be, for example, a conductive binder or a non-conductive binder. The conductive binder may be, for example, an ion-conductive binder and / or an electron-conductive binder. A binder having both ion-conductive and electron-conductive properties may be classified as either an ion-conductive binder or an electron-conductive binder.
[0230] The binder included in the intermediate layer may be selected from binders used in dry negative electrode films. The intermediate layer may include the same binder as the binder used in the dry negative electrode film. The binder included in the intermediate layer is, for example, a fluorinated binder. The fluorinated binder included in the intermediate layer is, for example, polyvinylidene fluoride (PVDF). The intermediate layer may be, for example, a binding layer including a binder. The intermediate layer may be, for example, a conductive layer including a binder and a carbon-based conductive material.
[0231] The intermediate layer can be disposed on the substrate, for example, dry or wet. The intermediate layer can be disposed on the substrate dry, for example, by deposition such as CVD or PVD. The intermediate layer can be disposed on the substrate wet, for example, by spin coating, dip coating, or the like. The intermediate layer can be disposed on the substrate, for example, by depositing a carbon-based conductive material on the substrate by deposition. A dry-coated intermediate layer is composed of a carbon-based conductive material and may not include a binder. The intermediate layer can be disposed on the substrate, for example, by coating a composition comprising a carbon-based conductive material, a binder, and a solvent on the surface of the substrate and drying it. The intermediate layer can have a single-layer structure or a multi-layer structure including a plurality of layers, for example, a two-layer structure, a three-layer structure, or a four-layer structure.
[0232] The dry cathode film included in the dry cathode corresponds to the electrode active material layer.
[0233] The dry negative electrode includes a dry negative electrode film, and the dry negative electrode film includes a dry negative electrode active material having the core / shell structure described above.
[0234] The dry negative electrode active material having the core / shell structure described above includes a carbon-based material in the core; a mixture of a carbon-based material and a silicon-based active material; a composite of a carbon-based material and a silicon-based active material; or a combination thereof, and includes a first metal oxide and a first carbon-based material in the shell.
[0235] The dry negative electrode active material may additionally include a conventional dry negative electrode active material in addition to the dry negative electrode active material having the core / shell structure described above. Any conventional dry negative electrode active material commonly used in the art may be used without limitation.
[0236] Any dry negative electrode active material that can be used as a negative electrode active material of a lithium battery in the relevant technical field can be used. For example, it includes at least one selected from the group consisting of lithium metal, metals alloyable with lithium, transition metal oxides, non-transition metal oxides, and carbon-based materials. Metals alloyable with lithium include, for example, Si, Sn, Al, Ge, Pb, Bi, Sb Si-Y alloy (wherein Y is an alkali metal, an alkaline earth metal, a group 13 element, a group 14 element, a transition metal, a rare earth element, or a combination thereof, and is not Si), Sn-Y alloy (wherein Y is an alkali metal, an alkaline earth metal, a group 13 element, a group 14 element, a transition metal, a rare earth element, or a combination thereof, and is not Sn), etc. Element Y is, for example, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, or a combination thereof. Transition metal oxides are, for example, lithium titanium oxide, vanadium oxide, lithium vanadium oxide, etc. Non-transition metal oxides are, for example, SnO2, SiO x(0 <x<2) 등이다. 탄소계 재료는 예를 들어 결정질 탄소, 비정질 탄소 또는 이들의 혼합물이다. 결정질 탄소는 예를 들어 무정형, 판상, 린편상(flake), 구형 또는 섬유형의 천연 그래파이트 또는 인조 그래파이트와 같은 그래파이트다. 비정질 탄소는 예를 들어 소프트 카본(soft carbon: 저온 소성 탄소) 또는 하드 카본(hard carbon), 메조페이스 피치(mesophase pitch) 탄화물, 소성된 코크스 등이다.
[0237] The cathode active material may be, for example, one or more of a composite oxide of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof, and specific examples are as described above.
[0238] A dry cathode is, for example, a dry cathode. A dry cathode includes a dry cathode film, and a dry cathode film includes a dry cathode active material.
[0239] According to another embodiment, a lithium battery includes a first electrode; a second electrode; and an electrolyte disposed between the first electrode and the second electrode, wherein the first electrode, the second electrode, or a combination thereof is the dry negative electrode described above.
[0240] The cycle characteristics of a lithium battery are improved by having a dry negative electrode having reduced internal resistance and improved mechanical properties.
[0241] A lithium battery may include, for example, a dry negative electrode, or a dry negative electrode and a dry positive electrode. A lithium battery may include, for example, a dry negative electrode and a wet positive electrode, or a dry positive electrode and a dry negative electrode.
[0242] A lithium battery includes an electrolyte, and the electrolyte may include, for example, a liquid electrolyte, a solid electrolyte, a gel electrolyte, or a combination thereof.
[0243] Liquid electrolytes are, for example, organic electrolytes. Organic electrolytes are prepared by dissolving lithium salts in organic solvents.
[0244] Any organic solvent used in the relevant technical field may be used. Examples of the organic solvent include propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.
[0245] Lithium salts are all possible if they are used as lithium salts in the relevant technical field. Lithium salts include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (where x and y are natural numbers), LiCl, LiI, or mixtures thereof.
[0246] The solid electrolyte may include, for example, an inorganic solid electrolyte, an organic solid electrolyte, an organic-inorganic composite solid electrolyte, or a combination thereof.
[0247] The solid electrolyte may include, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer-based solid electrolyte, or a combination thereof.
[0248] The solid electrolyte may be, but is not limited to, boron oxide, lithium oxynitride, etc., and any solid electrolyte used in the relevant technical field may be used. The solid electrolyte may be formed on the cathode by, for example, sputtering or a separate solid electrolyte sheet may be laminated on the cathode.
[0249] Oxide solid electrolytes include, for example, Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT, 0≤x<1, 0≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M = Te, Nb, or Zr, 0≤x≤10), Li 3+x La3Zr 2-y My O 12 (M doped LLZO, M=Ga, W, Nb, Ta, Al or a combination thereof, 0≤x≤10, 0 <y<2), Li7La3Zr 2-x Ta x O 12 (0 <x<2, LLZ-Ta), 또는 이들의 조합을 포함한다. 산화물계 고체전해질은 예를 들어 가넷계(Garnet-type) 고체전해질이다. 산화물계 고체전해질은 소결법 등에 의하여 제작된다.
[0250] Oxide-based solid electrolytes include, for example, Li7La3Zr2O 12 (LLZO), Li 6.5 La3Zr 1.5 Ta 0.5 O 12 , Li 1.3 Al 0.3 Ti 1.7 (PO4)3, Li 0.34 La 0.51 TiO 2.94 , Li 1.07 Al 0.69 Ti 1.46 (PO4)3, 50Li4SiO4-50Li2BO3, 90Li3BO3-10Li2SO4, Li 2.9 PO 3.3 N 0.46 , or a combination thereof.
[0251] Sulfide-based solid electrolytes include, for example, Li2S-P2S5, Li2S-P2S5-LiX, where X is a halogen element, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n , m, n are positive numbers, Z is one of Ge, Zn or Ga, Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MOq , p, q are positive numbers, M is one of P, Si, Ge, B, Al, Ga In, Li 7-x PS 6-x Cl x , 0≤x≤2, Li 7-x PS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-x I x , at least one selected from 0≤x≤2. The sulfide-based solid electrolyte is manufactured by treating starting materials such as Li2S and P2S5 by a melting rapid cooling method or a mechanical milling method. In addition, heat treatment may be performed after such treatment. The sulfide-based solid electrolyte may be amorphous, crystalline, or a mixture thereof.
[0252] The sulfide-based solid electrolyte may include, for example, an argyrodite type solid electrolyte represented by the following chemical formula 9:
[0253] <Chemical Formula 9>
[0254] Li + 12-n-x A n+ X 2- 6-x Y - x
[0255] In the above formula, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb, or Ta, X is S, Se, or Te, Y is Cl, Br, I, F, CN, OCN, SCN, or N3, and 1≤n≤5, 0≤x≤2.
[0256] Sulfide-based solid electrolyte is Li 7-x PS 6-x Cl x , 0≤x≤2, Li 7-x PS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-xI x , may be an argyrodite-type compound including at least one selected from 0≤x≤2. In particular, the sulfide-based solid electrolyte included in the solid electrolyte may be an argyrodite-type compound including at least one selected from Li6PS5Cl, Li6PS5Br, and Li6PS5I.
[0257] The polymer-based solid electrolyte may be, for example, a solid electrolyte comprising an ion-conducting polymer and a lithium salt, a solid electrolyte comprising an ionic liquid polymer and a lithium salt, or a combination thereof.7
[0258] An ion-conducting polymer is a polymer that contains an ion-conducting repeating unit in its main chain or side chain. The ion-conducting repeating unit is a unit having ion conductivity, and may be, for example, an alkylene oxide unit, a hydrophilic unit, etc. The ion-conducting polymer may contain, for example, an ether monomer, an acrylic monomer, a methacrylic monomer, a siloxane monomer, or a combination thereof as the ion-conducting repeating unit. The ion-conducting polymer may be, for example, polyethylene oxide, polypropylene oxide, polymethyl methacrylate, polyethyl methacrylate, polydimethylsiloxane, polyacrylic acid, polymethacrylic acid, polymethyl acrylate, polyethyl acrylate, poly-2-ethylhexyl acrylate, polybutyl methacrylate, poly-2-ethylhexyl methacrylate, polydecylacrylate, polyethylenevinylacetate, or a combination thereof. The ion-conducting polymer can be, for example, polyethylene oxide (PEO), polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), polyvinyl sulfone, or a combination thereof.
[0259] Polymeric ionic liquids (PILs) include, for example, i) one or more cations selected from ammonium, pyrrolidinium, pyridinium, pyrimidinium, imidazolium, piperidinium, pyrazolium, oxazolium, pyridazinium, phosphonium, sulfonium, triazole and mixtures thereof, and ii) BF4-, PF6-, AsF6-, SbF6-, AlCl4-, HSO4-, ClO4-, CH3SO3-, CF3CO2-, (CF3SO2)2N-, Cl-, Br-, I-, SO4 - , PF6-, ClO4-, CF3SO3-, CF3CO2-, (C2F5SO2)2N-, (C2F5SO2)(CF3SO2)N-, NO3 - , Al2Cl7 - , AsF6 - , SbF6 - , CF3COO - , CH3COO - , CF3SO3 - , (CF3SO2)3C - , (CF3CF2SO2)2N - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , SF5CF2SO3 - , SF5CHFCF2SO3 - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (O(CF3)2C2(CF3)2O)2PO -And may contain repeating units comprising one or more anions selected from (CF3SO2)2N-. The ionic liquid polymer may be, for example, poly(diallyldimethylammonium)TFSI, poly(1-allyl-3-methylimidazolium trifluoromethanesulfonylimide), poly(N-methyl-N-propylpiperidinium bis(trifluoromethanesulfonyl)imide), or a combination thereof.
[0260] Lithium salts include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, Li(FSO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(1≤x≤20, 1≤y≤20), LiCl, LiI or a combination thereof.
[0261] A method for manufacturing a dry cathode according to another embodiment is provided.
[0262] A method for manufacturing a dry cathode comprises the steps of providing a dry cathode film; and the steps of disposing the dry electrode film on one or both sides of an electrode current collector.
[0263] The step of providing a dry negative electrode film includes a step of preparing a dry mixture by dry mixing a dry negative electrode active material and a dry binder; and a step of forming the dry mixture to prepare a dry negative electrode film.
[0264] First, a dry mixture is prepared by dry mixing the negative electrode active material and the dry binder. For example, a dry mixture is prepared by dry mixing the dry negative electrode active material and the dry binder.
[0265] The above dry mixture may further include a dry conductive agent.
[0266] Dry mixing means mixing without a process solvent. A process solvent is, for example, a solvent used in the preparation of an electrode slurry. The process solvent is not limited to, but includes, water, NMP, etc., and is not limited to, any process solvent used in the preparation of an electrode slurry. Dry mixing can be performed using a stirrer at a temperature of, for example, 15°C to 65°C and a rotation speed of 10 to 10,000 rpm. Dry mixing can be performed using a stirrer for, for example, 1 to 200 minutes.
[0267] Dry mixing may be performed, for example, more than once. First, a first dry mixture may be prepared by first dry mixing a dry negative active material, a dry conductive material, and a dry binder. The first dry mixing may be performed, for example, at a temperature of 25 to 65°C, at a rotation speed of 10 to 2000 rpm or less, for a time of 15 minutes or less. Subsequently, the first dry mixture may be additionally dry mixed a second time to prepare a second mixture. The second dry mixing may be performed, for example, at a temperature of 25 to 65°C, at a rotation speed of 3000 to 9000 rpm, for a time of 10 to 60 minutes. By the second dry mixing, a dry mixture including a fibrillated dry binder may be obtained.
[0268] The stirrer is, for example, a kneader. The stirrer includes, for example, a chamber; one or more rotating shafts disposed inside the chamber and rotating; and blades rotatably coupled to the rotating shaft and disposed in the longitudinal direction of the rotating shaft. The blades may be, for example, one or more selected from a ribbon blade, a sigma blade, a jet (Z) blade, a dispersion blade, and a screw blade. By including the blades, an electrode active material, a dry conductive material, and a dry binder can be effectively mixed without a solvent to produce a dough-like mixture.
[0269] Dry binders include, for example, vinylidene fluoride / hexafluoropropylene copolymers, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the aforementioned polymers, and styrene butadiene rubber-based polymers. The dry binder may be selected from among the dry binders used in the above-described dry negative electrode films.
[0270] Dry conductive materials include, but are not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. Any material used as a conductive material in the relevant technical field may be used. The conductive material is, for example, a carbon-based conductive material. The dry conductive material may be selected from among the dry conductive materials used in the above-described dry cathode film.
[0271] It is also possible to form pores inside the electrode plate by adding a plasticizer or pore former to the dry mixture.
[0272] The contents of dry negative electrode active material, dry binder, and dry conductive material used in the dry negative electrode film are at levels typically used in lithium batteries.
[0273] A dry cathode film includes a dry cathode active material as the cathode active material. The dry cathode active material refers to the dry cathode film described above. A dry cathode film uses a dry cathode active material as the cathode active material. The dry cathode active material refers to the dry cathode film described above.
[0274] Next, the dry mixture is molded to prepare a dry cathode film.
[0275] The prepared dry mixture can be fed into an extrusion device and extruded into a sheet or film form. The pressure during extrusion is, for example, 4 MPa to 100 MPa.
[0276] Next, an electrode current collector is provided in which an intermediate layer is disposed on one or both sides of the substrate.
[0277] The step of providing an electrode current collector having an intermediate layer disposed on one or both sides of a substrate includes, for example, the step of providing a substrate; and the step of disposing the intermediate layer on one or both sides of the substrate.
[0278] The substrate of the electrode current collector refers to the electrode current collector section described above. The substrate of the positive electrode current collector is, for example, aluminum foil. The substrate of the negative electrode current collector is, for example, copper foil.
[0279] The step of disposing an intermediate layer on one or both sides of a substrate includes dry coating and / or wet coating. Dry coating involves, for example, coating a carbon-based conductive material and / or a precursor thereof on one or both sides of an electrode current collector by vapor deposition or the like. The vapor deposition is performed at a temperature ranging from room temperature to high temperature and a pressure ranging from normal pressure to vacuum. The intermediate layer disposed by dry coating may not include a binder if it is made of a carbon-based material. Wet coating involves, for example, coating a composition comprising a carbon-based conductive material and a binder on one or both sides of an electrode current collector. The composition includes, for example, a carbon-based conductive material, a binder, and a process solvent. For details on the carbon-based conductive material and binder, refer to the electrode section described above. The process solvent may be selected from solvents used in the preparation of an electrode slurry. The process solvent is removed by drying after the composition is coated on the electrode current collector. The coating method may include, but is not limited to, spin coating, dip coating, or the like, and any coating method used in the art may be used.
[0280] Next, the dry negative electrode films are simultaneously or sequentially placed on one or both sides of the electrode collector to manufacture a dry negative electrode.
[0281] A rolling step may be added during and / or after placing the dry negative electrode film on one or both sides of the electrode collector.
[0282] Rolling can be performed using, but is not limited to, a roll press or a flat plate press. The pressure during rolling is, for example, 1.0 to 10.0 ton / cm. If the pressure during rolling is excessively high, cracks may occur in the electrode current collector. If the pressure during rolling is excessively low, the bonding strength between the electrode current collector and the dry negative electrode film may be reduced.
[0283] Lithium batteries are manufactured by, for example, the following exemplary methods, but are not limited to these methods and may vary depending on the required conditions.
[0284] First, one or both of the positive electrode and the negative electrode can be manufactured according to the above-described dry negative electrode manufacturing method. Alternatively, when one of the positive electrode and the negative electrode is manufactured using the above-described electrode manufacturing method, the other electrode can be manufactured using a wet manufacturing method. For example, the other electrode can be manufactured by manufacturing an electrode slurry containing an electrode active material, a conductive material, a binder, and a solvent, coating the manufactured electrode slurry on an electrode current collector, and drying it. The conductive material and binder included in the electrode manufactured using the wet manufacturing method can be selected from the conductive material and binder used in manufacturing the above-described dry negative electrode.
[0285] Next, a separator to be inserted between the positive and negative electrodes is prepared.
[0286] The step of providing a dry negative electrode film includes a step of preparing a dry mixture by dry mixing a dry negative electrode active material and a dry binder as described above; and a step of forming the dry mixture to prepare a dry negative electrode film.
[0287] Dry cathode active materials can be formed during the dry mixing process of the core and composite.
[0288] The composite comprises at least one first metal oxide; and a first carbon-based material, wherein the first metal oxide is disposed within a first carbon-based material matrix, and the first metal oxide has the chemical formula M. a O b (0 <a≤3, 0<b<4, a가 1, 2, 또는 3 이면, b는 정수가 아님)로 표시되며, 상기 M은 원소주기율표 2족 내지 16족 중에서 선택된 하나 이상의 금속이다.
[0289] The step of providing a complex includes, for example, the step of supplying a reaction gas consisting of a carbon source gas to a structure including a metal oxide and performing a heat treatment to provide a complex. The step of providing a complex includes, for example, M a O c(0 <a≤3, 0<c≤4, a가 1, 2 또는 3인 경우, b가 정수임)로 표시되는 1 종 이상의 제2 금속산화물에 탄소 공급원 기체로 이루어진 반응 가스를 공급하고 열처리하여 복합체를 제조하는 단계를 포함하며, 상기 M은 원소주기율표 제2 족 내지 제13 족, 제15 족 및 제16 족 중에서 선택된 하나 이상의 금속이다.
[0290] The carbon source gas is a gas composed of a compound represented by the following chemical formula 10, or at least one mixed gas selected from the group consisting of a compound represented by the following chemical formula 10, a compound represented by the following chemical formula 11, and an oxygen-containing gas represented by the following chemical formula 12.
[0291] <Chemical Formula 10>
[0292] C n H (2n+2-a) [OH] a
[0293] In the above chemical formula 10, n is 1 to 20, a is 0 or 1;
[0294] <Chemical Formula 11>
[0295] C n H 2n
[0296] In the above chemical formula 11, n is 2 to 6;
[0297] <Chemical Formula 12>
[0298] C x H y O z
[0299] In the above chemical formula 12, x is 0 or an integer from 1 to 20, y is 0 or an integer from 1 to 20, and z is 1 or 2.
[0300] The compound represented by Chemical Formula 10 and the compound represented by Chemical Formula 11 are at least one selected from the group consisting of methane, ethylene, propylene, methanol, ethanol, and propanol. The oxygen-containing gas represented by Chemical Formula 12 includes, for example, carbon dioxide (CO2), carbon monoxide (CO), water vapor (H2O), or a mixture thereof.
[0301] M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물에 탄소 공급원 기체로 이루어진 반응 가스를 공급하고 열처리하는 단계 이후에 질소, 헬륨 및 아르곤으로 이루어진 군으로부터 선택된 하나 이상의 불활성 기체를 이용한 냉각 단계를 더 거칠 수 있다. 냉각 단계는 상온(20-25℃)으로 조절하는 단계를 말한다. 탄소 공급원 기체는 질소, 헬륨, 아르곤으로 이루어진 군으로부터 선택된 하나 이상의 불활성 기체를 포함할 수 있다.
[0302] In the manufacturing method of the composite, the process of growing carbon-based materials, such as graphene, depending on the gas phase reaction can be performed under various conditions.
[0303] According to the first condition, for example, M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물이 배치된 반응기에 먼저 메탄을 공급하고 열처리온도(T)까지 승온처리한다. 열처리 온도(T)까지의 승온 시간은 10 분 내지 4 시간이고 열처리온도(T)는 700 ℃ 내지 1100 ℃ 범위이다. 열처리온도(T)에서 반응 시간 동안 열처리를 실시한다. 반응시간은 예를 들어 4 시간 내지 8 시간이다. 열처리된 결과물을 상온으로 냉각시켜 복합체를 제조한다. 열처리온도(T)에서 상온까지 냉각하는 과정에 걸치는 시간은 예를 들어 1 시간 내지 5 시간이다.
[0304] According to the second condition, for example, Ma O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물이 배치된 반응기에 먼저 수소를 공급하고 열처리온도(T)까지 승온 처리한다. 열처리 온도(T)까지의 승온 시간은 10 분 내지 4 시간이고 열처리온도(T)는 700 ℃ 내지 1100 ℃ 범위이다. 열처리온도(T)에서 일정 반응 시간 동안 열처리한 후 메탄 가스를 공급하고 잔여 반응 시간 동안 열처리를 실시한다. 반응시간은 예를 들어 4 시간 내지 8 시간이다. 열처리된 결과물을 상온으로 냉각시켜 복합체를 제조한다. 냉각하는 과정에서 질소를 공급한다. 열처리온도(T)에서 상온까지 냉각하는 과정에 걸치는 시간은 예를 들어 1 시간 내지 5 시간이다.
[0305] According to the third condition, for example, M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물이 배치된 반응기에 먼저 수소를 공급하고 열처리온도(T)까지 승온 처리한다. 열처리 온도(T)까지의 승온 시간은 10 분 내지 4 시간이고 열처리온도(T)는 700 ℃ 내지 1100 ℃ 범위이다. 열처리온도(T)에서 일정 반응 시간 동안 열처리한 후 메탄과 수소의 혼합 가스를 공급하고 잔여 반응 시간 동안 열처리를 실시한다. 반응시간은 예를 들어 4 시간 내지 8 시간이다. 열처리된 결과물을 상온으로 냉각시켜 복합체를 제조한다. 냉각하는 과정에서 질소를 공급한다. 열처리온도(T)에서 상온까지 냉각하는 과정에 걸치는 시간은 예를 들어 1 시간 내지 5 시간이다.
[0306] In the process of manufacturing a composite, if the carbon source gas contains water vapor, a composite having excellent conductivity can be obtained. The content of water vapor in the gas mixture is not limited and is, for example, 0.01% to 10% by volume based on 100% by volume of the total carbon source gas. The carbon source gas is, for example, methane; a mixed gas containing methane and an inert gas; or a mixed gas containing methane and an oxygen-containing gas.
[0307] The carbon source gas can be, for example, methane; a mixture of methane and carbon dioxide; or a mixture of methane, carbon dioxide, and water vapor. In the mixture of methane and carbon dioxide, the molar ratio of methane to carbon dioxide is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. In the mixture of methane, carbon dioxide, and water vapor, the molar ratio of methane, carbon dioxide, and water vapor is about 1:0.20 to 0.50:0.01 to 1.45, about 1:0.25 to 0.45:0.10 to 1.35, or about 1:0.30 to 0.40:0.50 to 1.0.
[0308] The carbon source gas is, for example, carbon monoxide or carbon dioxide. The carbon source gas is, for example, a mixture of methane and nitrogen. In the mixture of methane and nitrogen, the molar ratio of methane to nitrogen is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. The carbon source gas may not include an inert gas such as nitrogen.
[0309] The heat treatment pressure can be selected considering the heat treatment temperature, the composition of the gas mixture, and the desired amount of carbon coating. The heat treatment pressure can be controlled by adjusting the amount of the incoming gas mixture and the amount of the outgoing gas mixture. The heat treatment pressure is, for example, 0.5 atm or more, 1 atm or more, 2 atm or more, 3 atm or more, 4 atm or more, or 5 atm or more. The heat treatment pressure is, for example, 0.5 atm to 10 atm, 1 atm to 10 atm, 2 atm to 10 atm, 3 atm to 10 atm, 4 atm to 10 atm, or 5 atm to 10 atm.
[0310] The heat treatment time is not particularly limited and can be appropriately adjusted depending on the heat treatment temperature, the pressure during the heat treatment, the composition of the gas mixture, and the desired amount of carbon coating. For example, the reaction time at the heat treatment temperature is, for example, 10 minutes to 100 hours, 30 minutes to 90 hours, or 50 minutes to 40 hours. For example, as the heat treatment time increases, the amount of carbon deposited, for example, the amount of graphene (carbon), increases, and thus the electrical properties of the composite may improve. However, this trend may not necessarily be directly proportional to time. For example, after a certain period of time, carbon deposition, for example, graphene deposition, may no longer occur or the deposition rate may decrease.
[0311] Through the gas phase reaction of the carbon source gas described above, M is produced even at relatively low temperatures. a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물 및 그 환원 생성물인 M a O b(0 <a≤3, 0<b<4, a는 1, 2, 또는 3이며, b 는 정수가 아님)로 표시되는 제1 금속산화물 중에서 선택된 하나 이상에 균일한 탄소계 재료의 코팅 예를 들어 그래핀 코팅을 제공함에 의하여 복합체가 얻어진다.
[0312] The composite is a matrix of carbon-based materials having one or more structures selected from, for example, a spherical structure, a spiral structure in which multiple spherical structures are connected, a cluster structure in which multiple spherical structures are aggregated, and a sponge structure, for example, a graphene matrix and M arranged within the graphene matrix. a O b (0 <a≤3, 0<b<4, a는 1, 2, 또는 3이며, b 는 정수가 아님)로 표시되는 제1 금속산화물 및 M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물 중에서 선택된 하나 이상을 포함한다.
[0313] The content of the dry binder is 1 to 10 wt%, 1 to 5 wt%, or 1.5 to 3.5 wt%, or 1.5 to 3 wt%, based on 100 wt% of the total content of the core, composite, and dry binder.
[0314] The content of the composite including at least one selected from the first metal oxide and the first carbon-based material may be about 5 wt% or less based on the total weight of the dry negative electrode film.
[0315] The present invention is further described in detail through the following examples and comparative examples. However, these examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.
[0316] (Manufacture of composites)
[0317] Manufacturing Example 1: Al2O3@Gr composite
[0318] Al2O3 particles (average particle size: approximately 20 nm) were placed inside the reactor, and then CH4 was supplied into the reactor at approximately 300 sccm and 1 atm for approximately 30 minutes, and the temperature inside the reactor was increased to 1000°C at a heating rate of approximately 23°C / min.
[0319] Then, heat treatment was performed by maintaining the temperature for 7 hours. Then, the supply of CH4 was stopped and the internal temperature of the reactor was adjusted to room temperature (25℃) to produce Al2O3 particles and its reduction product, Al2O z (0 <z<3) 입자가 그래핀에 매립된 복합체를 얻었다.
[0320] The alumina content of the composite was 60 wt%.
[0321] Manufacturing Example 2: Al2O3@Gr composite
[0322] A composite was manufactured in the same manner as in Manufacturing Example 1, except that Al2O3 particles (average particle diameter: approximately 200 nm) were used instead of Al2O3 particles (average particle diameter: approximately 20 nm).
[0323] Manufacturing Example 3: SiO2@Gr composite
[0324] SiO2 particles (average particle diameter: approximately 15 nm) were placed inside the reactor, and then CH4 was supplied into the reactor at approximately 300 sccm and 1 atm for approximately 30 minutes, and the temperature inside the reactor was raised to 1000°C.
[0325] Then, heat treatment was performed by maintaining the temperature for 7 hours. Then, the internal temperature of the reactor was adjusted to room temperature (20-25℃) to produce SiO2 particles and its reduction product, SiO y (0 <y<2) 입자가 그래핀에 매립된 복합체를 얻었다.
[0326] (Manufacture of silicon-based negative electrode active material)
[0327] Manufacturing Example 4
[0328] Flake graphite (SFG6) (Timcal, AG) (particle size: 4 μm, specific surface area: 17 m2 / g), pitch, and silicon were wet mixed in a weight ratio of 2:25:73 using isopropyl alcohol (IPA) and spray dried. The dried resultant was then carbonized at 900°C to obtain a silicon-carbon composite (SCN) (D50: approximately 13 μm).
[0329] (Manufacturing of lithium batteries (full cells), dry cathode)
[0330] Example 1: Dry cathode film comprising graphite, GB 0.5%, and binder
[0331] (Manufacture of dry cathode)
[0332] Graphite as the first negative electrode active material, polytetrafluoroethylene (PTFE) as a dry binder, and the composite (GB) prepared in Manufacturing Example 1 were introduced into a blade mixer at a weight ratio of 97.5:2.0:0.5, and then primary dry mixing was performed at a speed of 1200 rpm at 25°C for 10 minutes to prepare a first dry mixture in which the dry negative electrode active material and the dry binder were uniformly mixed.
[0333] Next, to allow fiberization (e.g., fibrillization) of the binder to occur, the first mixture was further mixed at 25°C and 5000 rpm for 20 minutes to prepare a second mixture. No separate solvent was used in the preparation of the first and second mixtures.
[0334] The prepared second mixture was fed into an extruder and extruded to prepare a dry negative electrode film, a self-standing film of a negative electrode active material layer in the form of a sheet. The pressure during extrusion was 50 MPa. The dry negative electrode film contained a composite negative electrode active material having a structure in which a shell including a composite and / or a milling result thereof was coated on a graphite core.
[0335] A first laminate was prepared by placing a carbon layer as an interlayer on one side of a 12 ㎛ thick copper thin film and placing the interlayer on one side of a second positive electrode collector.
[0336] The intermediate layer was prepared by coating a composition containing a carbon conductive material (Danka black) and polyvinylidene fluoride (PVDF) on an aluminum thin film and then drying it. The thickness of the intermediate layer disposed on one side of the aluminum thin film was approximately 1 μm.
[0337] A dry negative electrode film, which is a self-supporting negative electrode active material layer, was placed on the middle layer of the prepared first laminate and rolled to manufacture a negative electrode.
[0338] (Manufacturing of positive electrode)
[0339] Composite cathode active material LiNi 0.91 Co 0.05 Al 0.04 A mixture of O2 (hereinafter referred to as NCA91), carbon conductive agent (Denka Black), and polyvinylidene fluoride (PVDF) in a weight ratio of 96:2:2 was mixed with N-methylpyrrolidone (NMP) in an agate mortar to prepare a slurry.
[0340] The slurry was bar-coated on an aluminum current collector to a thickness of 40 μm, dried at room temperature, and then dried again under vacuum conditions at 120°C and rolled to manufacture a positive electrode.
[0341] (Manufacturing of coin cells)
[0342] Coin cells were manufactured using the positive and negative electrodes manufactured above, using a polypropylene separator (Celgard 3510) and a solution containing 1.15 M LiPF6 and 1.5 wt% vinylene carbonate (VC) dissolved in EC (ethylene carbonate) + EMC (ethyl methyl carbonate) + DMC (dimethyl carbonate) (2:4:4 volume ratio) as an electrolyte.
[0343] Example 2: Dry cathode film containing graphite, SCN, GB 0.5%, and binder
[0344] Graphite as the first negative electrode active material, the silicon composite structure (SCN) used in Manufacturing Example 4 as the second negative electrode active material, polytetrafluoroethylene (PTFE) as a dry binder, and the composite (GB) prepared in Manufacturing Example 1 were introduced into a blade mixer at a weight ratio of 81.5:15:3:0.5, and then first dry mixing was performed at 25°C and a speed of 1200 rpm for 10 minutes to prepare a first dry mixture in which the dry positive electrode active material, dry conductive agent, and dry binder were uniformly mixed.
[0345] The dry negative electrode film contains a first composite negative electrode active material having a structure in which a shell including a composite and / or a milling result thereof is coated on a graphite core, and a second composite negative electrode active material having a structure in which a shell including a composite and / or a milling result thereof is coated on an SCN core.
[0346] Example 3
[0347] Coin cells were manufactured in the same manner as in Example 1, except that the cathode was manufactured according to the following process.
[0348] (Manufacturing of cathode)
[0349] Graphite as the first negative electrode active material, the silicon composite structure (SCN) used in Manufacturing Example 4 as the second negative electrode active material, polytetrafluoroethylene (PTFE) as a dry binder, and the composite (GB) prepared in Manufacturing Example 1 were introduced into a blade mixer at a weight ratio of 40.5:7.5:1:0.2, and then primary dry mixing was performed at a speed of 1200 rpm at 25°C for 10 minutes to prepare a first dry mixture in which the dry positive electrode active material and the dry binder were uniformly mixed.
[0350] Next, to allow the fiberization of the binder to proceed, the first mixture was further mixed at a speed of 5000 rpm at 25°C for 20 minutes to prepare a second mixture. No separate solvent was used in the preparation of the first and second mixtures.
[0351] The prepared second mixture was fed into an extruder and extruded to prepare a first dry negative electrode film as a self-standing film of a negative electrode active material layer in the form of a sheet. The pressure during extrusion was 50 MPa. The dry negative electrode film contained a composite negative electrode active material having a structure in which a shell including a composite and / or a milling result thereof was coated on a graphite core.
[0352] Separately, a second dry negative electrode film was manufactured in the same manner as above, except that the weight ratio of graphite as the first negative electrode active material, the silicon composite structure (SCN) used in Manufacturing Example 4 as the second negative electrode active material, polytetrafluoroethylene (PTFE) as the dry binder, and the composite (GB) prepared in Manufacturing Example 1 was changed to 40.5:7.5:2:0.3 when manufacturing the second dry mixture for forming the second dry negative electrode film.
[0353] A first laminate was prepared by placing a carbon layer as an interlayer on one side of a 12 ㎛ thick copper thin film and placing the interlayer on one side of a second positive electrode collector.
[0354] The intermediate layer was prepared by coating a composition containing a carbon conductive material (Danka black) and polyvinylidene fluoride (PVDF) on an aluminum thin film and then drying it. The thickness of the intermediate layer disposed on one side of the aluminum thin film was approximately 1 μm.
[0355] A first dry cathode film and a second dry cathode film were sequentially placed on the intermediate layer of the prepared first laminate, and rolled to manufacture a dry cathode (copper thin film / intermediate layer (carbon layer) / first dry cathode film / second dry cathode film).
[0356] Example 4
[0357] A coin cell was manufactured in the same manner as in Example 2, except that the cathode shown in Fig. 4c was manufactured according to the following process.
[0358] (Manufacture of dry cathode)
[0359] Graphite, the silicon composite structure (SCN) used in Manufacturing Example 4 as the second negative electrode active material, polytetrafluoroethylene (PTFE) as a dry binder, and the composite (GB) prepared in Manufacturing Example 1 were placed in a blade mixer at a weight ratio of 40.75:15:2:0.3, and then first dry mixing was performed at 25°C and a speed of 1200 rpm for 10 minutes to prepare a first dry mixture in which the dry positive electrode active material and the dry binder were uniformly mixed.
[0360] Next, to allow the fiberization of the binder to proceed, the first mixture was further mixed at a speed of 5000 rpm at 25°C for 20 minutes to prepare a second mixture. No separate solvent was used in the preparation of the first and second mixtures.
[0361] The prepared second mixture was fed into an extruder and extruded to prepare a first dry negative electrode film as a self-standing film of a negative electrode active material layer in the form of a sheet. The pressure during extrusion was 50 MPa. The dry negative electrode film contained a composite negative electrode active material having a structure in which a shell including a composite and / or a milling result thereof was coated on a graphite core.
[0362] Separately, a second dry negative electrode film was manufactured in the same manner as above, except that the weight ratio of graphite as the first negative electrode active material, polytetrafluoroethylene (PTFE) as the dry binder, and the composite (GB) prepared in Manufacturing Example 1 was changed to 40.75:1:0.2 when manufacturing the first dry mixture.
[0363] A first laminate was prepared by placing a carbon layer as an interlayer on one side of a 12 ㎛ thick copper thin film and placing the interlayer on one side of a second positive electrode collector.
[0364] The intermediate layer was prepared by coating a composition containing a carbon conductive material (Danka black) and polyvinylidene fluoride (PVDF) on an aluminum thin film and then drying it. The thickness of the intermediate layer disposed on one side of the aluminum thin film was approximately 1 μm.
[0365] A first dry cathode film and a second dry cathode film were sequentially placed on the intermediate layer of the prepared first laminate, and rolled to manufacture a dry cathode (copper thin film / intermediate layer (carbon layer) / first dry cathode film / second dry cathode film).
[0366] Example 5
[0367] Coin cells were manufactured in the same manner as in Example 3, except that the cathode shown in Fig. 4b was manufactured according to the following manufacturing process.
[0368] (Manufacturing of cathode)
[0369] Graphite as the first negative electrode active material, the silicon composite structure (SCN) used in Manufacturing Example 4 as the second negative electrode active material, polytetrafluoroethylene (PTFE) as a dry binder, and the composite (GB) prepared in Manufacturing Example 1 were introduced into a blade mixer at a weight ratio of 40.5:7:1:0.2, and then primary dry mixing was performed at a speed of 1200 rpm at 25°C for 10 minutes to prepare a first dry mixture in which the dry positive electrode active material and the dry binder were uniformly mixed.
[0370] Next, to allow the fiberization of the binder to proceed, the first mixture was further mixed at a speed of 5000 rpm at 25°C for 20 minutes to prepare a second mixture. No separate solvent was used in the preparation of the first and second mixtures.
[0371] The prepared second mixture was fed into an extruder and extruded to prepare a first dry negative electrode film as a self-standing film of a negative electrode active material layer in the form of a sheet. The pressure during extrusion was 50 MPa. The dry negative electrode film contained a composite negative electrode active material having a structure in which a shell including a composite and / or a milling result thereof was coated on a graphite core.
[0372] Separately, a second dry negative electrode film was manufactured in the same manner as above, except that the weight ratio of graphite as the first negative electrode active material, the silicon composite structure (SCN) used in Manufacturing Example 4 as the second negative electrode active material, polytetrafluoroethylene (PTFE) as the dry binder, and the composite (GB) prepared in Manufacturing Example 1 was changed to 40.5:8:2:0.3 when manufacturing the second dry mixture for forming the second dry negative electrode film.
[0373] A first laminate was prepared by placing a carbon layer as an interlayer on one side of a 12 ㎛ thick copper thin film and placing the interlayer on one side of a second positive electrode collector.
[0374] The intermediate layer was prepared by coating a composition containing a carbon conductive material (Danka black) and polyvinylidene fluoride (PVDF) on an aluminum thin film and then drying it. The thickness of the intermediate layer disposed on one side of the aluminum thin film was approximately 1 μm.
[0375] A first dry cathode film and a second dry cathode film were sequentially placed on the intermediate layer of the prepared first laminate, and rolled to manufacture a dry cathode (copper thin film / intermediate layer (carbon layer) / first dry cathode film / second dry cathode film).
[0376] Comparative Example 1: Preparation of a wet cathode
[0377] (Manufacturing of cathode)
[0378] Graphite as the first negative active material, polytetrafluoroethylene (PTFE) as a binder, and the composite (GB) prepared in Manufacturing Example 1 as a conductive material were placed in a blade mixer at a weight ratio of 96.5:3:0.5, mixed at 25°C and 1200 rpm for 10 minutes, and then water was added thereto and mixed to obtain a negative active material slurry.
[0379] After applying the above negative active material slurry to copper foil, a film was formed using a doctor blade to a coating thickness of 20 μm, vacuum-dried at 130°C for 3 hours, and then rolled to manufacture a negative electrode.
[0380] Comparative Example 2: Preparation of a dry cathode
[0381] A dry cathode was manufactured in the same manner as Example 1, except that Denka Black was used instead of the composite manufactured in Manufacturing Example 1 when manufacturing the first dry mixture.
[0382] Comparative Example 3: Preparation of a dry cathode
[0383] A dry negative electrode was manufactured in the same manner as in Example 2, except that only the silicon composite structure (SCN) used in Manufacturing Example 4 was used instead of the graphite, which is the first negative electrode active material, and the silicon composite structure (SCN) used in Manufacturing Example 4, which is the second negative electrode active material, when manufacturing the first dry mixture.
[0384] Evaluation Example 1: Tensile Strength Evaluation
[0385] For each of the dry negative electrode films manufactured in Examples 1-4 and Comparative Examples 2-3, specimens for measuring tensile strength according to ASTM D 638 (216 mm (Length) × 19±0.5 mm (Width) × 3.18±0.38 mm (Depth)) were manufactured. Tensile strength was measured by performing a tensile strength test according to the ASTM D 638 method. The measurement results are shown in Table 1 below.
[0386] Classification Tensile strength [kPa] Rolling voltage After rolling Example 16301050 Example 27001090 Example 310001500 Example 48001200 Example 511001800 Comparative example 150100 Comparative example 2400960 Comparative example 3650990
[0387] As shown in Table 1, the dry negative electrode film of Example 1-5 showed improved mechanical strength compared to the dry negative electrode film of Comparative Example 1-3.
[0388] It was determined that the dry cathodes of Examples 1 and 2 were better than the dry cathodes of Comparative Examples 1 and 2 because each component was uniformly distributed, the binder was more uniformly distributed within the dry cathode film, and the fiberized binder more effectively bound the composite cathode active material.
[0389] Evaluation Example 2: Compound Resistance Evaluation
[0390] For each of the dry cathodes manufactured in Example 1-5 and Comparative Example 1-3, the composite resistance was measured using an electrode resistance measurement system (Hioki, RM2610) at 25°C, and the measurement results are shown in Table 3 below.
[0391] In an electrode resistance measurement system (Hioki, RM2610), the probe was positioned so that the negative electrode active material layer of the negative electrode faced the probe, a constant current was passed through the surface of the negative electrode active material layer, and the volume resistivity of the negative electrode active material layer and the interfacial resistance between the negative electrode active material layer and the negative electrode current collector were measured from the surface potential distribution. The volume resistivity of the negative electrode active material layer was regarded as the composite resistance of the negative electrode active material layer.
[0392] Evaluation Example 3: Interface Resistance Evaluation
[0393] For each of the dry cathodes manufactured in Example 1-5 and Comparative Example 1-3, the interface resistance was measured using an electrode resistance measurement system (Hioki, RM2610) at 25°C, and the measurement results are shown in Table 2 below.
[0394] In an electrode resistance measurement system (Hioki, RM2610), a probe was placed on the negative electrode so that the negative electrode active material layer of the negative electrode faced the probe, a constant current was passed through the surface of the negative electrode active material layer, and the volume resistivity of the negative electrode active material layer and the interfacial resistance between the negative electrode active material layer and the negative electrode current collector were measured from the surface potential distribution.
[0395] Distinctive resistance [Ωcm]Interface resistance [Ωcm 2 ]Embodiment 10.0350.002Embodiment 20.0250.002Embodiment 30.0150.001Embodiment 40.020.002Embodiment 50.0110.001Comparative Example 10.0680.05Comparative Example 20.1210.004Comparative Example 30.080.003
[0396] As shown in Table 2, the dry cathode of Example 1-5 had a reduced composite resistance compared to the dry cathode of Comparative Example 1-3.
[0397] It was determined that the dry negative electrode of Example 1-5 had improved electronic conductivity and / or ionic conductivity within the dry negative electrode film by including a composite negative electrode active material in which a shell including a composite is uniformly arranged on a core.
[0398] It was determined that the wet cathode of Comparative Example 1 and the dry cathode of Comparative Examples 2-3 had reduced electronic conductivity and / or ionic conductivity because they did not include the composite cathode active material described above.
[0399] As shown in Table 2, the dry cathode of Example 1-5 had a reduced interfacial resistance compared to the dry cathode of Comparative Example 1-3.
[0400] Evaluation Example 4: Adhesion of the polar plate
[0401] Using an adhesion tester (UTM, Instron), each dry cathode specimen manufactured in Example 1-5 and Comparative Example 1-3 was cut into 150 mm × 15 mm, and the force was measured when the electrode was attached to a double-sided adhesive tape and then detached by 90°. The results are shown in Table 3 below.
[0402] Adhesive force of the polarizing plate [gf / mm] Example 13.5 Example 24.0 Example 35.9 Example 44.8 Example 56.8 Comparative Example 12.95 Comparative Example 21.47 Comparative Example 32.8
[0403] As shown in Table 3, the wet negative electrode of Comparative Example 1 showed improved adhesion to the electrode plate compared to the dry negative electrode films of Comparative Examples 2 and 3, as shown in Table 3. However, it was found that the dry negative electrode films of Examples 1-5 showed improved adhesion to the electrode plate compared to the wet negative electrode of Comparative Example 1 and the dry negative electrodes of Comparative Examples 2-3.
[0404] Evaluation Example 5: Evaluation of charge-discharge characteristics at room temperature (25°C)
[0405] The lithium batteries manufactured in Examples 1 to 5 and Comparative Examples 1-3 were charged at a constant current of 0.1 C rate at 25°C until the voltage reached 4.5 V (vs. Li), and then cut-off at a current of 0.02 C rate while maintaining 4.5 V in constant voltage mode. Subsequently, the batteries were discharged at a constant current of 0.1 C rate until the voltage reached 2.75 V (vs. Li) during discharge (formation cycle).
[0406] The lithium battery, which had undergone a Mars cycle, was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.5 V (vs. Li), and then cut-off at a current of 0.02 C rate while maintaining 4.5 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.2 C rate until the voltage reached 2.75 V (vs. Li) (1 st cycle). These cycles are 50 th The cycle was repeated under the same conditions (50 repetitions).
[0407] In all charge / discharge cycles, a 10-minute pause was provided after each charge / discharge cycle. Some of the results of the room-temperature charge / discharge experiments are shown in Table 4 below. The initial efficiency is defined by Equation 1 below, and the capacity retention rate is defined by Equation 2 below.
[0408] <Formula 1>
[0409] Initial efficiency [%] = [Discharge capacity in the Martian cycle / Charge capacity in the Martian cycle] × 100
[0410] <Formula 2>
[0411] Capacity retention rate [%] = [50 th Discharge capacity in cycles / 1 st Discharge capacity in cycle] × 100
[0412] Classification Initial Efficiency (%) Capacity Retention Rate [%] Example 186.293 Example 284.593 Example 385.194.5 Example 485.596.8 Example 585.898.9 Comparative Example 186.490 Comparative Example 279.282 Comparative Example 378.256
[0413] As shown in Table 4, the lithium batteries of Examples 1 to 5 had improved life characteristics compared to the lithium batteries of Comparative Examples 1 to 2.
[0414] These improved life characteristics were determined to be due to the suppression of the formation of a solid electrolyte membrane (SEI) on the surface and / or inside the negative electrode active material by the composite coating, thereby suppressing the internal resistance of the lithium battery.
[0415] Evaluation Example 6: XPS (X-ray photoelectron spectroscopy) spectrum evaluation
[0416] During the manufacturing process of the composite manufactured in Manufacturing Example 1, XPS spectra were measured over time using Qunatum 2000 (Physical Electronics). XPS spectra of C 1s orbitals and Al 2p orbitals were measured for the samples before heating, after 1 minute, after 5 minutes, after 30 minutes, after 1 hour, and after 4 hours, respectively. At the beginning of heating, only the peak for the Al 2p orbital appeared, and the peak for the C 1s orbital did not appear. After 30 minutes, the peak for the C 1s orbital appeared clearly, and the size of the peak for the Al 2p orbital decreased significantly.
[0417] After 30 minutes, a peak for the C 1s orbital due to the C-C bond and C=C bond caused by the growth of graphene was clearly observed near 284.5 eV.
[0418] As the reaction time elapsed, the oxidation number of aluminum decreased, and the peak position of the Al 2p orbital shifted toward lower binding energy (eV).
[0419] Therefore, as the reaction progresses, graphene grows on the Al2O3 particles, and Al2O, a reduction product of Al2O3, x (0 <x<3)가 생성됨을 확인하였다.
[0420] The average carbon and aluminum contents were measured through XPS analysis results in 10 areas of the composite sample manufactured in Manufacturing Example 1. The deviation of the aluminum content in each area was calculated based on the measurement results. The deviation of the aluminum content was expressed as a percentage of the average value, and this was called uniformity. The percentage of the deviation of the aluminum content to the average value, i.e. the uniformity of the aluminum content, was 1%. Therefore, it was confirmed that alumina was uniformly distributed in the composite manufactured in Manufacturing Example 1.
Claims
1. Contains a dry negative electrode active material and a dry binder, The above dry negative electrode active material contains a composite negative electrode active material including a core; and a shell arranged along the surface of the core, The above core comprises a carbon-based material; a mixture of a carbon-based material and a silicon-based active material; a composite of a carbon-based material and a silicon-based active material; or a combination thereof, The above shell contains a composite including at least one first metal oxide and a first carbon-based material, The first metal oxide is disposed within the first carbon-based material matrix, The above first metal oxide has the chemical formula M a O b (0 <a≤3, 0<b<4, a가 1, 2, 또는 3 이면, b는 정수가 아님)로 표시되며, 상기 M은 원소주기율표 2족 내지 16족 중에서 선택된 하나 이상의 금속인, 건식 음극 필름.
2. In the first paragraph, the dry negative electrode film has a multilayer structure of two or more layers.
3. In the first paragraph, the dry negative electrode film includes a first dry negative electrode film and a second dry negative electrode film, A dry negative electrode film, wherein the binder content and the composite content of the first dry negative electrode film are greater than the binder content and the composite content of the second dry negative electrode film, respectively.
4. In the first paragraph, the dry negative electrode film is a self-standing film, and the dry negative electrode film is free of residual processing solvent. A dry negative electrode film having a tensile strength before rolling of 450 kPa or more and a tensile strength after rolling of 1000 kPa or more.
5. A dry negative electrode film in accordance with paragraph 1, wherein the content of the complex is 5 wt% or less based on the total weight of the dry negative electrode film.
6. In the first paragraph, the metal included in the first metal oxide is at least one metal selected from among Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se. The above first metal oxide is Al2O z (0 <z<3), NbO x (0 <x<2.5), MgO x (0 <x<1), Sc2O z (0 <z<3), TiO y (0 <y<2), ZrO y (0 <y<2), V2O z (0 <z<3), WO y (0 <y<2), MnO y (0 <y<2), Fe2O z (0 <z<3), Co3O w (0 <w<4), PdO x (0 <x<1), CuO x (0 <x<1), AgO x (0 <x<1), ZnO x (0 <x<1), Sb2O z (0 <z<3), 및 SeO y (0 <y<2) 중에서 선택되는 하나 이상인, 건식 음극 필름.
7. In the first paragraph, the shell further includes a second metal oxide, The second metal oxide has the chemical formula M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3 이면, c는 정수임)로 표시되며, The second metal oxide contains the same metal as the first metal oxide, The ratio of a and c of the second metal oxide, c / a, has a greater value than the ratio of a and b of the first metal oxide, b / a, A dry cathode film, wherein the second metal oxide is disposed within the first carbon-based material matrix.
8. In the 7th paragraph, the second metal oxide is selected from Al2O3, NbO, NbO2, Nb2O5MgO, Sc2O3, TiO2, ZrO2, V2O3, WO2, MnO2, Fe2O3, Co3O4, PdO, CuO, AgO, ZnO, Sb2O3, and SeO2, A dry cathode film, wherein the first metal oxide is a reduction product of the second metal oxide.
9. In paragraph 1, the carbon-based material is crystalline carbon, amorphous carbon, or a combination thereof, The above crystalline carbon is at least one selected from the group consisting of natural graphite, artificial graphite, graphene, fullerene, and carbon nanotube, A dry cathode film wherein the amorphous carbon is at least one selected from the group consisting of pitch carbon, soft carbon, hard carbon, mesophase pitch carbide, calcined coke, and carbon fiber.
10. In the first paragraph, the silicon-based active material is a Si alloy, a silicon-containing structure, a silicon-containing compound, or a combination thereof. The above silicon-containing compound is SiO2, SiOx (0 <x<2), SiC, 또는 그 조합이며, A dry cathode film wherein the above silicon-containing structure comprises a silicon composite structure.
11. In the 10th paragraph, the silicon-based active material includes a silicon-based composite structure, A dry cathode film, wherein the silicon-based composite structure comprises a silicon-carbon composite including silicon particles and a first carbon-based material, a silicon-carbon composite including a core in which silicon particles and a second carbon-based material are mixed and a third carbon-based material surrounding the core, or a combination thereof.
12. In the first paragraph, the dry binder comprises a fibrillized binder, The above dry binder includes a fluorine-based binder, The glass transition temperature (T) of the above dry binder g ) is 15 to 100 ℃, A dry negative electrode film, wherein the dry binder content is 0.1 to 5 wt% based on the total weight of the dry negative electrode film.
13. In the first paragraph, the dry cathode film further includes a dry conductive material, The above dry conductive material includes a carbon-based conductive material, The above carbon-based conductive material includes a fibrous carbon-based material having an aspect ratio of 10 or more, a particulate carbon-based material having an aspect ratio of less than 10, or a combination thereof. A dry negative electrode film, wherein the dry conductive material content is 0.1 to 5 wt% based on the total weight of the dry negative electrode film.
14. Negative current collector; and A dry negative electrode comprising a dry negative electrode film according to any one of claims 1 to 13, which is disposed on one or both sides of the negative electrode collector.
15. In the 14th paragraph, the negative electrode collector comprises a substrate; and an interlayer disposed between the substrate and the dry negative electrode film, A dry cathode, wherein the intermediate layer comprises a carbon-based conductive material.
16. In the 14th paragraph, the dry negative electrode film includes a first dry negative electrode film disposed adjacent to the negative electrode collector and a second dry negative electrode film disposed on top of the first dry negative electrode film. A dry cathode, wherein the content of the composite and the content of the binder of the first dry cathode film are greater than the content of the composite and the content of the binder of the second dry cathode film, respectively.
17. In the 16th paragraph, the first dry negative electrode film is a carbon-based material as a core of a dry composite negative electrode active material. Contains silicon-based active materials, The above silicon-based active material includes a silicon composite structure, The above second dry negative electrode film includes a carbon-based material as a core of a dry composite negative electrode active material, A dry negative electrode, wherein the binder content of the first dry negative electrode film is equal to or greater than the binder content of the second dry negative electrode film, and the composite content of the first dry negative electrode film is equal to or greater than the composite content of the second dry negative electrode film.
18. In the 14th paragraph, the dry negative electrode film includes a first dry negative electrode film disposed adjacent to the negative electrode collector and a second dry negative electrode film disposed on the first dry negative electrode film. The above first dry negative electrode film includes a carbon-based material and a silicon-based active material as a core of a dry composite negative electrode active material, The above second dry negative electrode film includes a carbon-based material and a silicon-based active material as a core of a dry negative electrode active material, The silicon-based active material of the first dry negative electrode film and the second dry negative electrode film includes a silicon composite structure, The binder content of the first dry negative electrode film is equal to or greater than the binder content of the second dry negative electrode film, The content of the composite (GB) of the first dry cathode film is equal to or greater than the content of the composite of the second dry cathode film, A dry negative electrode, wherein the content of the carbon-based material in the first dry negative electrode film is equal to or greater than the content of the carbon-based material in the second dry negative electrode film, and the content of the silicon-based active material in the first dry negative electrode film is equal to or greater than the content of the silicon-based active material in the second dry negative electrode film.
19. Contains an anode, a cathode, and an electrolyte disposed between the anode and the cathode, The above cathode is a dry cathode according to Article 15, The above electrolyte comprises a liquid electrolyte, a solid electrolyte, a gel electrolyte or a combination thereof, A lithium battery, wherein the solid electrolyte comprises an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof.
20. In paragraph 19, the positive electrode includes a positive electrode collector, and the negative electrode includes a negative electrode collector. The above positive electrode collector and negative electrode collector each include a base film and a metal layer disposed on one or both sides of the base film, The above base film comprises a polymer, and the polymer comprises polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, A lithium battery, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
Citation Information
Patent Citations
High-capacity hard carbon fast-charging negative electrode material as well as preparation method and application thereof
CN114695894A
Anode active material for lithium secondary batteries and method of preparing for the same and lithium secondary batteries comprising the same
KR1020100127433A
Process for preparation of anode active material
KR1020120081556A
Negative active material, and negative electrode and lithium battery containing the material
KR1020140104067A
Method and apparatus for spatial audio reproduction using directional room impulse responses interpolation
KR1020230121007A