Nanoporous graphite, precursor thereof, and electrochemical device including same

Nanoporous graphite with controlled nanopores addresses the durability and stability issues of two-dimensional graphene-based separators by maintaining stable interlayer distance and enhancing selective permeability, suitable for various separation and electrochemical applications.

WO2024205144A1PCT designated stage expired Publication Date: 2024-10-03KOREA ADVANCED INST OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003625
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-21
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing two-dimensional graphene-based separators for gas and water treatment face issues with durability and long-term stability due to easy peeling and expansion of interlayer distance under harsh conditions, leading to reduced selective separation efficiency.

Method used

Development of nanoporous graphite with controlled nanopores on its surface, characterized by specific Raman and X-ray diffraction features, and a method involving intercalation compounds and chemical oxidation to create stable nanopores, enhancing selective permeability and durability.

Benefits of technology

The nanoporous graphite maintains stable interlayer distance and improves selective permeability and durability, maintaining high performance even under harsh conditions and long-term use, suitable for applications in water treatment, gas separation, and electrochemical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003625_03102024_PF_FP_ABST
    Figure KR2024003625_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention pertains to a nanoporous graphite that significantly improves selective permeability to a target substance when used as a separator and can exhibit excellent durability due to the interlayer spacing being reliably maintained even under severe conditions or long-term use. The nanoporous graphite contains a plurality of nanopores on at least one surface of a graphite layer and has a diffraction peak corresponding to the (002) crystal plane of graphite, and at least one of the plurality of nanopores is located in-plane in the graphite layer.
Need to check novelty before this filing date? Find Prior Art

Description

Nanoporous graphite, precursors thereof, and electrochemical devices comprising the same

[0001] The present invention relates to nanoporous graphite containing nano-sized pores, precursors thereof, and applications thereof.

[0002] Carbon materials are widely used in various industrial fields such as water treatment, gas separation, and energy devices.

[0003] Among these, research on separation membranes using two-dimensional structures such as graphene is actively being conducted in the field of separation membranes, such as gas separation membranes, water treatment separation membranes, ion separation membranes, and secondary battery separation membranes that selectively transmit ions or specific substances.

[0004] Among the membrane structures based on two-dimensional structures, research is being conducted continuously on the use of single-layer graphene oxide (GO) or multi-layer graphene oxide in which multiple single layers are stacked to improve selectivity or permeability for the target substance to be separated.

[0005] For example, research has been conducted to improve the permeation flux or selectivity for a specific gas mixture by including functionalized graphene such as graphene oxide on a porous support. However, in the case of a composite membrane simply layered with graphene oxide, such as when manufacturing a composite membrane by coating graphene oxide, there is a problem of low durability due to the phenomenon of easy peeling off by external physical and / or chemical stimuli.

[0006] In addition, when using multilayer graphene oxide under conditions in which an aqueous medium or solvent exists, there is a disadvantage in that the interlayer distance in the multilayer structure included in the separation membrane expands, drastically reducing the efficiency of selective separation of the target substance, and the long-term stability of the separation membrane is poor, limiting its industrial use.

[0007] Accordingly, there is a need to develop a new structural material that can improve the selective penetration efficiency of the target substance while efficiently suppressing performance degradation even during long-term use due to excellent durability.

[0008] An object of the present invention is to provide nanoporous graphite in which the interlayer distance is stably maintained even under harsh conditions or long-term use.

[0009] Another object of the present invention is to provide a nanoporous graphite precursor capable of enabling the production of the aforementioned nanoporous graphite.

[0010] Another object of the present invention is to provide various applications of the nanoporous graphite described above.

[0011] The present invention provides nanoporous graphite, characterized in that the nanoporous graphite includes a plurality of nanopores on at least one surface of a graphite layer, has a diffraction peak due to a (002) crystal plane of graphite in X-ray diffraction analysis, and at least one of the plurality of nanopores is located on an in-plane inside the graphite layer.

[0012] In the nanoporous graphite according to the present invention, the nanoporous graphite may include a D' band in a Raman spectrum.

[0013] In the nanoporous graphite according to the present invention, the Raman spectrum of the nanoporous graphite is I d / I g The intensity ratio can be between 0.3 and 1.5.

[0014] In the nanoporous graphite according to the present invention, the nanoporous graphite may include a D' band having a stronger scattering intensity than the D band in a Raman spectrum.

[0015] In the nanoporous graphite according to the present invention, the nanoporous graphite may include a D' band having a stronger scattering intensity than the 2D band in a Raman spectrum.

[0016] In the nanoporous graphite according to the present invention, the FWHM of the diffraction peak due to the (002) crystal plane of graphite in the X-ray diffraction analysis of the nanoporous graphite may be 5° or less.

[0017] In the nanoporous graphite according to the present invention, the average diameter of the nanopores may be 500 nm or less.

[0018] In the nanoporous graphite according to the present invention, after the nanoporous graphite is exfoliated into graphene, five or more nanopores may be included in a 50 nm x 50 nm image observed with a transmission electron microscope.

[0019] In the nanoporous graphite according to the present invention, the nanoporous graphite can satisfy the following equation 1.

[0020] (Formula 1)

[0021] SNPG / SG ≤ 10

[0022] (SNPG stands for the BET surface area of ​​nanoporous graphite, and SG stands for the BET surface area of ​​pristine graphite)

[0023] In the nanoporous graphite according to the present invention, the nanoporous graphite has a diameter of 20 m 2 / g or less can have a BET surface area.

[0024] In the nanoporous graphite according to the present invention, the size of the nanopores can be controlled by a chemical oxidation reaction.

[0025] In the nanoporous graphite according to the present invention, the nanoporous graphite has a diameter of 0.1 cm 3 / g or less can have a pore volume.

[0026] In the nanoporous graphite according to the present invention, the intensity of the peak of C-O-C, C-O, or C-O bond energy according to X-ray photoelectron spectroscopy may be lower than the intensity of the peak of C-C and C-C bond energy.

[0027] The present invention provides a separator, wherein the separator comprises the nanoporous graphite.

[0028] In the separation membrane according to the present invention, the separation membrane may be used for water treatment, solvent nanofiltration, gas separation, or ion separation.

[0029] The present invention provides an electrochemical device, wherein the electrochemical device comprises the nanoporous graphite described above.

[0030] The present invention provides a graphite precursor, characterized in that the graphite precursor includes Cr on at least one side of a graphite layer, includes a D' band in a Raman spectrum, and has two or more diffraction peaks diffracted at an angle lower than a diffraction angle 2θ due to a (002) crystal plane of graphite in an X-ray diffraction analysis.

[0031] In the graphite precursor according to the present invention, the graphite precursor may include a D band having a weaker scattering intensity than the 2D band in the Raman spectrum.

[0032] In the graphite precursor according to the present invention, the Cr may be included in an amount of 3 wt% or less of the total weight of the nanoporous graphite precursor.

[0033] The present invention provides a method for producing nanoporous graphite, the method for producing nanoporous graphite comprising: (S1) a step of producing a nanoporous graphite precursor by positioning one or more intercalating compounds on the upper side of at least one surface of graphite; (S2) a step of reacting the intercalating compound with an unsaturated bond between carbon atoms of the graphite; and (S3) a step of forming nanopores due to the reaction of the step (S2); wherein the intercalating compound induces nanopores at the positions of the saturated bonds.

[0034] In the method for producing nanoporous graphite according to the present invention, the intercalating compound is CrO2Cl2; Cr2O3; FeCl3; and a compound comprising the same; may be selected from the group consisting of:

[0035] In the method for producing nanoporous graphite according to the present invention, the reaction in step (S2) may be an oxidation reaction.

[0036] In the method for producing nanoporous graphite according to the present invention, the reaction of step (S2) can be performed under acidic conditions.

[0037] In the method for producing nanoporous graphite according to the present invention, the step (S2) can be performed by adding an oxidizing agent.

[0038] In the method for producing nanoporous graphite according to the present invention, the oxidizing agent may include KMnO4.

[0039] The nanoporous graphite according to the present invention includes a plurality of nanopores on at least one side of a graphite layer, has a diffraction peak due to the (002) crystal plane of graphite in X-ray diffraction analysis, and is characterized in that at least one of the plurality of nanopores is located on an in-plane inside the graphite layer, so that when used as a separation membrane, not only can the selective permeability for a target substance be significantly improved, but also has the advantage of excellent durability in which the interlayer distance is stably maintained even under harsh conditions or for long-term use.

[0040] FIG. 1a, FIG. 1b and FIG. 1c are drawings showing X-ray diffraction patterns, Raman spectra and XPS spectra for graphite and GIC of Preparation Examples 1 to 3, respectively, and FIG. 1d is a drawing showing the Cr content included in Preparation Examples 1 to 3 calculated through XPS analysis.

[0041] Figure 2 is a schematic diagram illustrating a series of processes for manufacturing nanoporous graphite using graphite as a starting material.

[0042] FIG. 3a is a diagram showing a transmission electron microscope image of Example 1 and a corresponding energy dispersive spectroscopy (EDS) mapping image, and FIGS. 3b and 3c are diagrams showing a high-resolution transmission electron microscope (HR-TEM) image of Example 1 and a corresponding fast Fourier transform (FFT) pattern, respectively.

[0043] Figures 4a and 4b are drawings showing the Raman spectrum and C1s XPS spectrum for the carbon body, respectively, and Figure 4c is a drawing showing the X-ray diffraction pattern for the carbon body, respectively.

[0044] FIG. 5a is a diagram showing the FT-IR spectra of graphite, Preparation Example 3, Comparative Example 1, Example 1, Example 2, Example 3, and Example 4, and FIG. 5b and FIG. 5c are diagrams showing the water contact angle and zeta potential of Examples 1 to 4, respectively.

[0045] FIG. 6a is a drawing showing high-resolution transmission electron microscope (HR-TEM) images of Example 1, Example 2, and Comparative Example 3, and FIG. 6b is a drawing showing the pore size distribution results of Example 1 and Example 2.

[0046] Figures 7a and 7b are diagrams showing N2 adsorption-desorption isotherms and BJH (Barrett-Joyner-Halenda) pore size distributions for Examples 1 and 2, respectively.

[0047] Figure 8 is a schematic diagram illustrating the pore formation process of nanoporous graphite.

[0048] FIGS. 9a, 9b, and 9c are drawings showing an optical image, a top-view scanning electron microscope (SEM) image, and a cross-section SEM image, respectively, of a membrane manufactured according to Example 5.

[0049] FIG. 10a, FIG. 10b and FIG. 10c are schematic diagrams showing the results of changes in the interlayer structure of carbon bodies included in the membranes of Example 5 and Comparative Example 4 under conditions of aqueous solutions containing various ions, the results of changes in the interlayer structure according to the concentration of ions and the phenomenon of interlayer distance expansion under pure H2O conditions, respectively.

[0050] FIG. 11a and FIG. 11b are drawings showing XRD patterns measured after the membrane of Example 5 was immersed in pure water for 1 day and 60 days, respectively, and schematically showing the interlayer distance expansion phenomenon under pure water (pure H2O) conditions for Comparative Example 4 and Example 5.

[0051] FIG. 12a and FIG. 12b are drawings comparing XRD patterns measured after immersing the membranes of Examples 5 to 8 in a dry state and in pure water for 24 hours, respectively, and drawings comparing interlayer distances calculated from XRD patterns measured after immersing each membrane in 0.1 M of each ionic solution (NaCl, Na2SO4, LiCl, CaCl2, MgCl2, K3[Fe(CN)6], and AlCl2) for 24 hours.

[0052] Figures 13a and 13b are diagrams showing the ion permeability characteristics of the membranes of Examples 5 to 8, respectively, according to the ion permeability and the anion-to-cation valence ratios included in the ion solution.

[0053] Figures 14a and 14b are diagrams comparing the performance results of Example 5 according to a continuous forward osmosis desalination test for 24 hours and the ion rejection rate according to a continuous forward osmosis desalination test for 1 day and 7 days, respectively.

[0054] Figures 15a and 15b are diagrams showing the performance evaluation results of a separation membrane according to the concentration of a NaCl solution and the performance evaluation results of a separation membrane according to the pH change of a NaCl solution, respectively.

[0055] Figures 16a and 16b are drawings showing the performance evaluation results for the membrane of Example 5 according to a continuous forward osmosis desalination test for 30 days using a 0.1 M NaCl solution and a 1 M NaCl solution as feed solutions, respectively, and the performance evaluation results for the membrane of Example 5 according to the thickness of the membrane using a 0.1 M NaCl solution.

[0056] Figure 17 is a schematic diagram illustrating the mechanism of desalination using a membrane containing nanoporous graphite.

[0057] The nanoporous graphite of the present invention will be described in detail with reference to the attached drawings below.

[0058] The drawings presented below are provided as examples to ensure that those skilled in the art can fully understand the spirit of the present invention. Therefore, the present invention is not limited to the drawings presented below and may be embodied in other forms. The drawings presented below may be exaggerated to clarify the spirit of the present invention.

[0059] At this time, if there is no other definition in the technical and scientific terms used, they have the meaning commonly understood by a person of ordinary skill in the technical field to which this invention belongs, and the description of known functions and configurations that may unnecessarily obscure the gist of the present invention is omitted in the following description and attached drawings.

[0060] Additionally, the singular forms used in the specification and the appended claims are intended to include the plural forms as well, unless the context clearly dictates otherwise.

[0061] In this specification and the appended claims, the terms first, second, etc. are not used in a limiting sense but are used to distinguish one component from another.

[0062] In this specification and the appended claims, the terms “include” or “have” mean that a feature or component described in the specification is present, and unless specifically limited, does not preclude the possibility that one or more other features or components may be added.

[0063] In this specification and the appended claims, when a part such as a film (layer), region, component, etc. is said to be on or above another part, it includes not only the case where it is directly above and in contact with another part, but also the case where another film (layer), another region, another component, etc. is interposed therebetween.

[0064] A numerical range as used herein includes a lower bound and an upper bound and all values ​​within that range, increments logically derived from the shape and width of the defined range, all doubly delimited values, and all possible combinations of upper and lower bounds of numerical ranges delimited in different shapes.

[0065] The terms “about,” “substantially,” and the like, as used in this specification and the appended claims, are used in a sense of numerical value or approximation to numerical values ​​when manufacturing and material tolerances inherent in the meanings stated are presented, and are used to prevent unscrupulous infringers from unfairly exploiting disclosures that state precise or absolute values ​​in order to aid understanding of this specification and the appended claims.

[0066] Hereinafter, the nanoporous graphite of the present invention, the nanoporous graphite precursor, the electrochemical device including the same, and the components of the electrochemical device will be described in detail.

[0067] The present invention provides nanoporous graphite, characterized in that the nanoporous graphite includes a plurality of nanopores on at least one surface of a graphite layer, has a diffraction peak due to a (002) crystal plane of graphite in X-ray diffraction analysis, and at least one of the plurality of nanopores is located on an in-plane inside the graphite layer.

[0068] According to one embodiment, the nanoporous graphite may include a D' band in a Raman spectrum. The nanoporous graphite may mean that the graphite layer includes one or more nanopores on a plane, i.e., on an in-plane, within the layer, including the D' band in the Raman spectrum.

[0069] According to one embodiment, the Raman spectrum of the nanoporous graphite is I d / I gThe intensity ratio can be 0.3 to 1.5. I of the Raman spectrum of the nanoporous graphite d / I g The intensity ratio may be 0.3 or more, 0.4 or more, 0.5 or more, or 0.6 or more, and the upper limit may be 2.0 or less, 1.5 or less, 1.3 or less, or 1.2 or less. Specifically, the I of the Raman spectrum of the nanoporous graphite d / I g The intensity ratio can be 0.3 to 2.0, 0.4 to 1.5, 0.5 to 1.3 or 0.6 to 1.2. I of the Raman spectrum of the nanoporous graphite d / I g When the strength ratio satisfies the above-described range, it can significantly improve the selective permeability to the target substance when used as a separation membrane due to fewer defects, and can also exhibit excellent durability in which the interlayer distance is stably maintained even under harsh conditions or for long-term use.

[0070] According to one embodiment, the nanoporous graphite may include a D' band having a stronger scattering intensity than the D band in a Raman spectrum.

[0071] Specifically, the D' band may be a peak that appears when the graphite layer contains defects and nanopores in the aromatic carbon structure. Therefore, a single layer of the nanoporous graphite may have a D' band higher than the D band, thereby maintaining high crystallinity and indicating that nanopores are formed.

[0072] According to one embodiment, the nanoporous graphite may include a D' band having a stronger scattering intensity than the 2D band in a Raman spectrum.

[0073] Specifically, the 2D band may be a peak that appears when the crystal structure of each layer of the nanoporous graphite is maintained. Accordingly, the nanoporous graphite may mean that the interlayer crystal structure has high crystallinity and appropriate nanopores because the 2D band is maintained and the D' band is higher than the 2D band.

[0074] According to one embodiment, the FWHM of the diffraction peak due to the (002) crystal plane of graphite in the X-ray diffraction analysis may be 5° or less. The FWHM of the diffraction peak due to the (002) crystal plane of graphite in the X-ray diffraction analysis may be 0.1° or more, 0.5° or more, or 1° or more, and an upper limit may be 10° or less, 5° or less, or 3° or less. Specifically, the FWHM of the diffraction peak due to the (002) crystal plane of graphite in the X-ray diffraction analysis may be 0.1 to 10°, 0.5 to 5°, or 1 to 3°. The X-ray diffraction peak in the (002) crystal plane of the nanoporous graphite may maintain high crystallinity while having a large number of pores, thereby satisfying the above-described full width at half maximum (FWHM).

[0075] According to one embodiment, the average diameter of the nanopores included in the nanoporous graphite may be 500 nm or less. The average diameter of the nanopores included in the nanoporous graphite may be 1,000 nm or less, 500 nm or less, 200 nm or less, 100 nm or less, or 50 nm or less, and a lower limit may be 0.1 nm or more, 1 nm or more, or 5 nm or more. Specifically, the average diameter of the nanopores included in the nanoporous graphite may be 0.1 to 1,000 nm, 1 to 500 nm, 1 to 200 nm, 1 to 100 nm, 1 to 50 nm, or 5 to 50 nm. The nanopores may have a diameter within the above-described range to improve material transfer and / or solvent transport properties, thereby increasing permeability to a target substance.

[0076] According to one embodiment, after peeling off one layer of graphene included in the nanoporous graphite, a 50 nm x 50 nm image observed with a scanning electron microscope (SEM) may include 5 or more nanopores. The number of nanopores included in the 50 nm x 50 nm image observed with a transmission electron microscope after peeling off one layer of graphene included in the nanoporous graphite may be 1 or more, 2 or more, 3 or more, 5 or more, or 10 or more, and an upper limit may be 500 or less, 200 or less, 100 or less, 50 or less, or 20 or less. Specifically, after peeling off one layer of graphene included in the nanoporous graphite, the number of nanopores in a 50 nm x 50 nm image observed with a transmission electron microscope may be 1 to 500, 2 to 200, 3 to 100, 5 to 50, or 10 to 20. The number of nanopores described above refers to the density of the nanopores, and the nanopores included in the nanoporous graphite may have a density in the above-described range to improve material transfer and / or solvent transport properties, thereby increasing permeability to a target substance.

[0077] According to one embodiment, the nanoporous graphite can satisfy the following equation 1.

[0078] (Formula 1)

[0079] SNPG / SG ≤ 10

[0080] (In Equation 1, SNPG represents the BET surface area of ​​nanoporous graphite, and SG represents the BET surface area of ​​pristine graphite.)

[0081] The value of SNPG / SG of the above formula 1 may be 20 or less, 10 or less, 5 or less, 3 or less, or 2 or less, and as a lower limit, may be greater than 1.0. Specifically, the value of SNPG / SG of the above formula 1 may be greater than 1.0 and less than 20, greater than 1.0 and less than 10, greater than 1.0 and less than 5, greater than 1.0 and less than 3, or greater than 1.0 and less than 2.

[0082] The above pristine graphite refers to general graphite, and the nanoporous graphite has a highly stacked and dense crystal structure of graphene, and thus can satisfy the range described in Equation 1. However, despite having a highly stacked and dense structure, the porous graphite has a large number of pores, and thus can have higher permeability to target substances and higher durability than general graphite materials.

[0083] According to one embodiment, the nanoporous graphite has a thickness of 20 m 2 / g or less. The BET surface area of ​​the above nanoporous graphite is 20 m 2 / g or less, 10 m 2 / g or less or 5 m 2 / g or less, with a lower limit of 0.1 m 2 / g or more, 1 m 2 / g or more or 2 m 2 / g or more. Specifically, the BET specific surface area of ​​the nanoporous graphite is 0.1 to 20 m 2 / g, 1 to 10 m 2 / g or 2 to 5 m 2 / g. The nanoporous graphite has a highly layered and dense structure, and thus can have a BET specific surface area within the above-described range. Nevertheless, the nanoporous graphite has a large number of pores, and thus can have higher permeability to target substances and higher durability than typical graphite materials.

[0084] According to one embodiment, the size of the nanopores can be controlled by a chemical oxidation reaction.

[0085] As a non-limiting example, CrO2Cl2 or the like is inserted between the planes of each graphene included in the nanoporous graphite, i.e., intercalated, and the CrO2Cl2 inserted between layers under acidic conditions reacts with double-bonded carbon to break the double bonds, thereby causing strain in the carbon lattice to form defects and pores. More specifically, the CrO2Cl2 can form sp of the graphene included in the nanoporous graphite. 2 The nanopores can be induced by inducing local cleavage of the domain. At this time, the size of the nanopores can be determined by the concentration of CrO2Cl2 and the treatment time, etc. Meanwhile, the oxidizing agent that induces the chemical oxidation reaction may be KMnO4, etc., but the present invention is not limited thereto.

[0086] According to one embodiment, the nanoporous graphite has a diameter of 0.1 cm 3 / g or less. The pore volume of the nanoporous graphite is 0.20 cm 3 / g or less, 0.10 cm 3 / g or less or 0.05 cm 3 / g or less, with a lower limit of 0.001 cm 3 / g or more, 0.05 cm 3 / g or more or 0.01 cm 3 / g or more. Specifically, the pore volume of the nanoporous graphite is 0.001 to 0.20 cm 3 / g, 0.05 to 0.10 cm 3 / g or 0.01 to 0.05 cm 3 / g. The nanoporous graphite may have high mass transfer efficiency and durability despite having a low pore volume in the above-described range due to pores appropriately formed between the planes of graphene included in the nanoporous graphite.

[0087] According to one embodiment, the intensity of the peak of C-O-C, C-O, or C(-O)-O binding energy according to X-ray photoelectron spectroscopy (XPS) of the nanoporous graphite may be lower than the intensity of the peak of C-O-C and C-C binding energy. Specifically, since the nanopores included in the nanoporous graphite may be generated by a chemical oxidation reaction as described above, the peak including the oxygen functional group of the X-ray photoelectron spectroscopy may be greater than the carbon peak. In the case of general pristine graphite that does not satisfy this, the pores are not densely located between layers but are randomly located, so that the remarkable effect according to the present invention may not be exhibited.

[0088] The present invention provides a separator, wherein the separator comprises nanoporous graphite according to the present invention. When describing the separator, it is understood that the separator comprises the aforementioned nanoporous graphite, and thus the separator according to the present invention encompasses all of the properties described above regarding nanoporous graphite.

[0089] Hereinafter, the separation membrane of the present invention will be described in more detail.

[0090] According to one embodiment, the separation membrane may be used for water treatment, solvent nanofiltration, gas separation, or ion separation. Specifically, the separation membrane may have high mass transfer efficiency, permeability to target substances, and high durability due to the inclusion of the nanoporous graphite described above. Accordingly, the separation membrane may be used for the aforementioned purposes, but the present invention is not limited thereto.

[0091] According to one embodiment, the nanoporous graphite can be included in electrode active materials, supercapacitor electrodes, electrochemical devices, and the like.

[0092] Specifically, the electrode active material may be included in a negative electrode for a secondary battery, a supercapacitor electrode, etc. The electrode active material includes the nanoporous graphite described above, and since the nanoporous graphite can have significantly high material transfer efficiency and durability as described above, it may be included in the negative electrode for a secondary battery, a supercapacitor electrode, etc. to improve the performance and durability of the secondary battery and the supercapacitor.

[0093] Additionally, specifically, the electrochemical device may be an electrochemical sensor, an electrochemical catalyst, or an energy storage device. As described above, the nanoporous graphite exhibits remarkable effects, such as high mass transfer efficiency and high durability, and thus can be applied to the electrochemical device described above.

[0094] However, the nanoporous graphite according to the present invention is not limited to the above-described uses, and it can also be applied to various industrial fields to which the remarkable effects of the nanoporous graphite according to the present invention can be applied.

[0095] The present invention provides a nanoporous graphite precursor, characterized in that the nanoporous graphite precursor includes Cr on at least one side of a graphite layer, includes a D' band in a Raman spectrum, and has two or more diffraction peaks diffracted at an angle lower than 2θ, a diffraction angle due to a (002) crystal plane of graphite, in an X-ray diffraction analysis.

[0096] In describing the above nanoporous graphite precursor, the nanoporous graphite precursor may be an intermediate in the manufacturing process of the above-described nanoporous graphite, and the D' band and the (002) crystal plane of the graphite may be the same as or similar to the terms described above in the nanoporous graphite, and therefore the nanoporous graphite precursor according to the present invention includes all of the contents described above in the nanoporous graphite.

[0097] Hereinafter, the nanoporous graphite precursor according to the present invention will be described in more detail.

[0098] According to one embodiment, the above-described nanoporous graphite can be produced by a graphite intercalation reaction of Cr in the nanoporous graphite precursor. As in the non-limiting example described above, CrO2Cl2 or the like is inserted, i.e., intercalated, between the planes of each graphene included in the above-described nanoporous graphite, and then a chemical oxidation reaction proceeds, thereby producing the above-described nanoporous graphite.

[0099] According to one embodiment, the Cr, i.e., chromium atoms, may be included in an amount of 3 wt% or less based on the total weight of the nanoporous graphite precursor. The Cr, i.e., chromium atoms, may be included in an amount of 10 wt% or less, 5 wt% or less, or 3 wt% or less based on the total weight of the nanoporous graphite precursor, and as a lower limit, may be included in an amount of 0.1 wt% or more, 0.5 wt% or more, or 1 wt% or more. Specifically, the Cr, i.e., chromium atoms, may be included in an amount of 0.1 to 10 wt%, 0.5 to 5 wt%, or 1 to 3 wt% based on the total weight of the nanoporous graphite precursor. The Cr included in the nanoporous graphite precursor is included within the above-described range, so that the pore size and pore distribution of the nanoporous graphite described above can be appropriately controlled.

[0100] In addition, it goes without saying that the Cr contained in the above nanoporous graphite precursor can be removed after pore creation, thereby producing the above-described nanoporous graphite.

[0101] The present invention provides a method for producing nanoporous graphite, the method for producing nanoporous graphite comprising: (S1) a step of producing a nanoporous graphite precursor by positioning one or more intercalating compounds on the upper side of at least one surface of graphite; (S2) a step of reacting the intercalating compound with an unsaturated bond between carbon atoms of the graphite; and (S3) a step of forming nanopores due to the reaction of the step (S2); wherein the intercalating compound induces nanopores at the positions of the saturated bonds.

[0102] In describing the method for producing the above nanoporous graphite, the method for producing the above nanoporous graphite may be the method for producing the above-described nanoporous graphite; and the graphite and nanopores, etc. may be the same as or similar to the terms described above in the nanoporous graphite and nanoporous graphite precursor, and therefore the method for producing nanoporous graphite according to the present invention includes all the contents described above in the nanoporous graphite and nanoporous graphite precursor.

[0103] Hereinafter, the method for manufacturing nanoporous graphite of the present invention will be described in detail.

[0104] As described above, as a non-limiting example, the intercalating compound is inserted between the planes of each graphene included in the nanoporous graphite, i.e., intercalated, and the intercalating compound inserted between layers under acidic conditions can react with double-bonded carbon to break the double bonds and induce strain in the carbon lattice to form defects and pores. More specifically, the intercalating compound can form sp of the graphene included in the nanoporous graphite. 2 The above nanopores can be induced by inducing local cleavage of the domain.

[0105] According to one embodiment, the intercalating compound is CrO2Cl2; Cr2O3; FeCl3; and a compound including the same; and at least one may be selected from the group including the intercalating compound. The intercalating compound may be selected from the chemical species described above and may form the nanopores between the planes of each graphene included in the graphite.

[0106] According to one embodiment, the reaction in step (S2) may be an oxidation reaction. As described above, in step (S2), the intercalating compound may react with double-bonded carbon to break the double bonds contained in the graphene. At this time, the process in which the double bonds of an unsaturated hydrocarbon are broken to become a saturated hydrocarbon or the process in which double bonds are removed to create pores or defects may be performed by an oxidation reaction.

[0107] According to one embodiment, the oxidation reaction may be performed by further adding an oxidizing agent. Specifically, the intercalating compound intercalated between the planes of the graphene included in the graphite may be oxidized by the oxidizing agent under acidic conditions, thereby generating the nanopores. As a non-limiting example, the oxidizing agent may include KMnO4, etc., but the present invention is not limited thereto.

[0108] According to one embodiment, the reaction of step (S2) may be performed under acidic conditions. As described above, the reaction of step (S2) may be an oxidation reaction and may be performed by adding an oxidizing agent. At this time, in order to facilitate the oxidation reaction, the reaction of step (S2) may be performed under acidic conditions of pH less than 7. As a non-limiting example, the nanoporous graphite precursor may be dispersed in water (H-2O), and an oxidizing agent, KMnO4, and sulfuric acid (H2SO4), may be added to the aqueous solution in which the precursor is dispersed, thereby performing the reaction under acidic conditions and conditions in which the oxidizing agent is added.

[0109] According to one embodiment, the amount of the oxidizing agent added may be 0.01 to 10 equivalents based on 1 equivalent of the intercalating compound included in the nanoporous graphite precursor. The amount of the oxidizing agent added may be 0.01 equivalents or more, 0.05 equivalents or more, 0.1 equivalents or more, 0.2 equivalents or more, 0.5 equivalents or more, or 1 equivalent or more based on 1 equivalent of the intercalating compound included in the nanoporous graphite precursor, and the upper limit may be 100 equivalents or less, 50 equivalents or less, 30 equivalents or less, 20 equivalents or less, 10 equivalents or less, or 5 equivalents or less. Specifically, the amount of the oxidizing agent added may be 0.01 to 100 equivalents, 0.05 to 50 equivalents, 0.1 to 30 equivalents, 0.2 to 20 equivalents, 0.5 to 10 equivalents, or 1 to 5 equivalents based on 1 equivalent of the intercalating compound included in the nanoporous graphite precursor. The amount of the oxidizing agent added may be adjusted within the above-described range, but may vary depending on various conditions such as the chemical species of the additive, the chemical species of the intercalating compound, and the pH during the manufacturing process, and therefore the present invention is not limited to the above-described amount of the oxidizing agent added.

[0110] Hereinafter, the nanoporous graphite according to the present invention will be described in more detail through examples. However, the following examples are merely references for explaining the present invention in detail, and the present invention is not limited thereto, and may be implemented in various forms.

[0111] Additionally, unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein is merely for the purpose of describing specific embodiments and is not intended to be limiting of the present invention.

[0112]

[0113] (Manufacturing Example 1) Preparation of precursor for nanoporous graphite

[0114] To prepare nanoporous graphite, 1 g of graphite and 10 g of Cr2O3 were added to a 25 mL flask, and then 10 mL of HCl was slowly added to prepare a mixture.

[0115] The mixture was stirred for 2 hours to cause an intercalation reaction to form CrO2Cl2 between the graphite layers.

[0116] Afterwards, the obtained product in which CrO2Cl2 was formed between graphite layers was vacuum filtered, washed with deionized water, and dried in an oven at 60°C to produce a graphite intercalation compound (GIC), which is a precursor of nanoporous graphite.

[0117]

[0118] (Manufacturing Example 2)

[0119] The same procedure as Manufacturing Example 1 was followed, except that the mixture was stirred for 5 hours to perform an intercalation reaction.

[0120]

[0121] (Manufacturing Example 3)

[0122] The same procedure as Manufacturing Example 1 was followed, except that the mixture was stirred for 20 hours to perform an intercalation reaction.

[0123]

[0124] (Experimental Example 1) Structural Analysis of Graphite Intercalation Compound (GIC)

[0125] The structures of each manufactured GIC were compared through X-ray diffraction (XRD) analysis, X-ray photoelectron spectroscopy (XPS) analysis, and Raman analysis.

[0126] FIG. 1a, FIG. 1b and FIG. 1c are drawings showing X-ray diffraction patterns, Raman spectra and XPS spectra for graphite and GIC of Preparation Examples 1 to 3, respectively, and FIG. 1d is a drawing showing the Cr content included in Preparation Examples 1 to 3 calculated through XPS analysis.

[0127] Referring to Fig. 1a, in Manufacturing Examples 1 to 3, it was observed that there were two diffraction peaks diffracted at an angle lower than the diffraction angle 2θ due to the (002) crystal plane of graphite.

[0128] It was observed that both Manufacturing Examples 1 to 3 included a first peak located at a diffraction angle approximately 0.4 degrees lower than the diffraction angle 2θ due to the (002) crystal plane of graphite among the two diffraction peaks, and the diffraction angles at which the second peak was located were different.

[0129] It was observed that the second peaks of Manufacturing Examples 1, 2, and 3 were located at diffraction angles that were about 0.9 degrees, about 1.8 degrees, and about 2.2 degrees lower, respectively, than the diffraction angle corresponding to the (002) crystal plane of graphite.

[0130] From this, it can be seen that the interlayer space of graphite becomes wider and larger as more CrO2Cl2 is formed between the graphite layers as the intercalation reaction time increases, but the crystal structure of graphite is still maintained.

[0131] These characteristics can be seen more clearly by examining the Raman spectrum in Fig. 1b.

[0132] Referring to Figure 1b, it was observed that all of Manufacturing Examples 1 to 3 included a D band with a weaker scattering intensity than the 2D band, similar to graphite, whereas, unlike graphite, it had a scattering intensity of about 1596 cm -1 It was observed that the D' band was included in the Raman shift.

[0133] That is, it can be seen that even though CrO2Cl2 is intercalated between graphite layers to form GIC, structural defects are practically not formed, and the crystal structure of graphite is maintained almost identically. In addition, it can be seen that GIC includes both a region with a wide interlayer space where CrO2Cl2 is located and a region with a narrow interlayer space where CrO2Cl2 is not located due to the intercalated CrO2Cl2.

[0134] Looking at FIGS. 1c and 1d, it can be seen that as the intercalation reaction time increases, more CrO2Cl2 is formed between the graphite layers, which increases the Cr content. As shown in FIG. 1c, in Preparation Examples 1 to 3, an O 1s peak is observed along with the Cr 2p peak, which can be seen to originate from the intercalated CrO2Cl2. In addition, it was confirmed that the GICs of Preparation Examples 1, 2, and 3 contained 1.71 wt%, 2.01 wt%, and 2.13 wt% of Cr, respectively.

[0135] From these results, GIC of Manufacturing Example 3 was used as a precursor for manufacturing nanoporous graphite.

[0136]

[0137] (Example 1) Preparation of nanoporous graphite

[0138] 100 mg of GIC of Manufacturing Example 3 was dissolved in 10 mL of sulfuric acid and stirred at room temperature (23°C) for 2 hours to prepare a precursor solution. Subsequently, the temperature of the precursor solution was increased to 35°C in an oil bath, and a mixture containing KMnO4, an oxidizing agent, was added to the precursor solution and stirred for 2 hours.

[0139] At this time, GIC: KMnO4 was added so that the weight ratio of the oxidizing agent KMnO4 was 1:1.

[0140] Afterwards, the stirred mixture was placed in an ice bath, and deionized water and hydrogen peroxide were slowly added to stop the reaction so that the temperature did not rise. The resulting compound was purified with 10% hydrochloric acid, and then centrifuged to obtain the product, which was washed several times using deionized water.

[0141] Next, the solution containing the washed product was sonicated for 1 hour, centrifuged at 5000 rpm for 1 hour, and the supernatant obtained was freeze-dried to produce nanoporous graphite.

[0142] A series of processes for manufacturing nanoporous graphite using pristine graphite as a starting material is schematically illustrated in Figure 2.

[0143]

[0144] (Example 2)

[0145] The same procedure as Example 1 was followed, except that KMnO4 was added so that the weight ratio of GIC:KMnO4 was 1:1.25.

[0146]

[0147] (Example 3)

[0148] The same procedure as Example 1 was followed, except that KMnO4 was added so that the weight ratio of GIC:KMnO4 was 1:1.5.

[0149]

[0150] (Example 4)

[0151] The same procedure as Example 1 was followed, except that KMnO4 was added so that the weight ratio of GIC:KMnO4 was 1:2.

[0152]

[0153] (Example 5)

[0154] The same procedure as Example 1 was followed, except that KMnO4 was added so that the weight ratio of GIC:KMnO4 was 1:0.25.

[0155]

[0156] (Example 6)

[0157] The same procedure as Example 1 was followed, except that KMnO4 was added so that the weight ratio of GIC:KMnO4 was 1:0.5.

[0158]

[0159] (Comparative Example 1)

[0160] The same procedure as Example 1 was followed, except that the oxidizing agent KMnO4 was not added.

[0161]

[0162] (Comparative Example 2)

[0163] The same procedure as Example 1 was followed, except that graphite, not GIC, was used and KMnO4 was added so that the weight ratio of graphite: KMnO4 was 1:1.

[0164]

[0165] (Comparative Example 3)

[0166] The same procedure was followed as in the conventional Hummers method, except that the mixture was stirred for 15 hours with KMnO4 added so that the weight ratio of graphite:KMnO4 was 1:3.5.

[0167]

[0168] (Experimental Example 2) Structural Analysis of Nanoporous Graphite

[0169] FIG. 3a is a diagram showing a transmission electron microscope image of Example 1 and a corresponding energy dispersive spectroscopy (EDS) mapping image, and FIGS. 3b and 3c are diagrams showing a high-resolution transmission electron microscope (HR-TEM) image of Example 1 and a corresponding fast Fourier transform (FFT) pattern, respectively.

[0170] As shown in Fig. 3a, it is observed that the signal related to oxygen is measured low, indicating that the oxidation reaction by the oxidizing agent is effectively suppressed.

[0171] In addition, referring to FIGS. 3b and 3c, it was observed that the nanoporous graphite of Example 1 included nanopores, and mainly contained sp2 carbon domains as the main structure, and it was confirmed that sp3 carbon domains due to local oxygen bonding existed.

[0172] Additionally, it can be seen from the hexagonal FFT pattern derived from the HR-TEM image that the graphene crystal structure is maintained.

[0173] Figures 4a and 4b are drawings showing the Raman spectrum and C1s XPS spectrum for the carbon body, respectively, and Figure 4c is a drawing showing the X-ray diffraction pattern for the carbon body, respectively.

[0174] First, referring to the Raman spectrum of Fig. 4a, unlike the GIC of the manufacturing example described above, in the case of Comparative Example 1, the Raman spectrum is 1340 cm -1 The intensity of the D band peak located at the Raman shift of 1570 cm increases, and the intensity of the G band peak (1570 cm -1 The formation of defects and nanopores in the aromatic carbon structure can be seen from the appearance of a broad D' band peak (located at Raman shift) and a single 2D peak (2700 cm -1 The presence of Raman shifts indicates that nanopores are formed while maintaining the crystal structure of graphite.

[0175] On the other hand, in the case of Example 1, it was observed that a D band peak with a sharp increase in intensity was present along with a broad 2D band peak compared to Comparative Example 1, and it was confirmed that the G band peak was red-shifted. It can be seen that this is due to the presence of a mixture of sp2 bonded carbon and sp3 bonded carbon, which is consistent with the results of the HR-TEM image analysis described above.

[0176] As the concentration of the oxidizing agent increases, the sp3 carbon domain area increases, so the intensity of the D band peak gradually decreases and the red-shifted G band, i.e., the peak of the D' band, appears broad.

[0177] Additionally, it was confirmed that the ratio (ID / IG) of the intensity of the D band peak (ID) and the intensity of the G band peak (IG) of graphite, Manufacturing Example 3, Comparative Example 1, Example 1, Example 2, Example 3, Example 4, and Comparative Example 2 was 0.072, 0.14, 0.48, 1.09, 1.04, 0.87, 0.81, and 0.95, respectively.

[0178] Next, looking at the C1s XPS spectrum of Fig. 4b, in the case of Comparative Example 1, since no oxidizing agent was added, no oxygen-related peaks were observed, and only typical carbon bond peaks were present. From this, it can be seen that the chemical structure of graphite is maintained during the nanopore formation process.

[0179] When an oxidizing agent is added, it is observed that the C=O bond peak (287.8 eV) and C=O(O) (288.9 eV) bond peaks begin to appear in addition to the CO peak located at a binding energy of 286.2 eV, indicating the additional presence of epoxide groups, hydroxyl groups, and carboxyl groups.

[0180] Specifically, in all of Examples 1 to 4 and Comparative Example 2, it was confirmed that the intensity of the peak of the C-O-C, C-O, or C(=O)-O bond energy was smaller than the intensity of the peak of the C-C and C-C bond energy, and it was confirmed that the intensity of the bond peak related to the functional group containing oxygen increased as the concentration of the oxidizing agent increased, and in particular, it was confirmed that it was the strongest in Comparative Example 2.

[0181] More specifically, it was confirmed that the ratio of the intensity of the COC bond peak in Example 1 to the intensity of the C=C and CC bond peaks was 1:4.5, and the ratios of the intensities for the same bond peaks in Examples 2, 3, 4, and Comparative Example 2 were 1:2.4, 1:1.5, 1:1.4, and 1:1.2, respectively.

[0182] When comparing Example 1 and Comparative Example 2, it was confirmed that oxidation was inhibited by the GIC of Example 1 even when the same concentration of oxidizing agent was added.

[0183] These results were confirmed to be consistent with the results of Fourier Transform Infrared Spectroscopy (FT-IR) analysis.

[0184] Meanwhile, referring to FIG. 4c, the results of X-ray diffraction analysis of carbon bodies according to Comparative Example 1, Manufacturing Example 3, Example 1, Example 5, and Example 6 were examined, and it was confirmed that the carbon bodies according to Comparative Example 1, Manufacturing Example 3, Example 1, Example 5, and Example 6 had a diffraction peak due to the graphite (002) crystal plane. Therefore, it was confirmed that Comparative Example 1, Manufacturing Example 3, Example 1, Example 5, and Example 6 well maintained the layered structure of graphite.

[0185] In addition, it was confirmed that the oxidation peak of graphite located at 10 to 15° increased as the amount of KMnO4, an oxidizing agent, increased. This means that the nanopores contained in the graphite, which are generated as the graphite is oxidized, increased, and it was confirmed that the carbon body according to Manufacturing Example 3 and Comparative Example 1, which did not use an oxidizing agent, did not show a diffraction peak located at 10 to 15°.

[0186] FIG. 5a is a diagram showing the FT-IR spectra of graphite, Preparation Example 3, Comparative Example 1, Example 1, Example 2, Example 3, and Example 4, and FIG. 5b and FIG. 5c are diagrams showing the water contact angle and zeta potential of Examples 1 to 4, respectively.

[0187] Referring to the FT-IR spectrum of Fig. 5a, in the case of Manufacturing Example 3, 1560 cm -1 Specific aromatic carbon peak at wavenumber 1000 cm -1 and 1130 cm -1 It can be seen that CrO2Cl2 intercalant is inserted between the layers from the peak corresponding to the C-Cl vibration mode at the wavenumber. In addition, referring to the cases of Examples 1 to 4, OH (600 cm -1 and 1074 cm -1 ), COC (1230 cm -1 ) and COOH (1675 cm -1 ) It can be seen that the intensity of the peak containing oxygen functional groups becomes stronger as the concentration of the added oxidizing agent increases.

[0188] As is known, the wettability and hydrophilic properties of carbon bodies such as graphene are affected by the content of oxygen functional groups included in the carbon body. As shown in Fig. 5b, the water contact angle of Example 1, which contains a limited number of oxygen functional groups, was 75°, whereas Example 4, which contains a relatively larger amount of oxygen functional groups, showed a water contact angle of 33°.

[0189] In addition, when comparing the zeta potential values ​​as shown in Fig. 5c, it was observed that Example 1 still exhibited a zeta potential characteristic of -53 mV despite containing a small amount of oxygen functional groups. This characteristic can be advantageous when dispersing nanoporous graphite in water or a solvent for application, and can also further enhance the ion rejection rate effect when applied to the treatment of solutions with low ionic strength.

[0190] FIG. 6a is a drawing showing high-resolution transmission electron microscope (HR-TEM) images of Example 1, Example 2, and Comparative Example 3, and FIG. 6b is a drawing showing the pore size distribution results of Example 1 and Example 2.

[0191] As shown in Fig. 6a, it was confirmed that a large number of nanopores existed in Examples 1 and 2, whereas in the case of Comparative Example 3, it was found that almost no nanopores were formed.

[0192] That is, it can be seen that the formation of nanopores is due to the CrO2Cl2 intercalant inserted between the layers. In addition, as illustrated in Fig. 6b, it was confirmed that the oxidizing agent added during the nanoporous graphite manufacturing process can additionally etch the nanopores to form larger pores.

[0193] FIG. 7a and FIG. 7b are diagrams showing N2 adsorption-desorption isotherms and BJH (Barrett-Joyner-Halenda) pore size distributions for Example 1 and Example 2, respectively, and the pore characteristics calculated using the BET (Brunauer-Emmett-Teller) method from the analysis results of the diagrams related to the pores are summarized in Table 1 below.

[0194] SampleS BET (m 2 / g)S external (m 2 / g)S micro (m 2 / g)V total (cm 3 / g)V external (cm 3 / g)V macro (cm 3 / g) Example 22.282.220.060.00740.00720.0002 Example 12.862.610.250.00980.00970.0001

[0195] Referring to FIG. 7a, FIG. 7b and Table 1, it can be seen that the pores are exposed due to the dense crystal structure of the highly stacked nanoporous graphite containing graphene.

[0196] Additionally, when compared to the BET surface area of ​​pristine graphite, the ratio of the BET surface area of ​​nanoporous graphite to the BET surface area of ​​pristine graphite is 3.59 m 2 / g was confirmed.

[0197] As described above, it can be seen that the nanopores included in the nanoporous graphite are formed by CrO2Cl2 inserted between the layers.

[0198] Specifically, referring to Fig. 8, which schematically illustrates the pore formation process of nanoporous graphite, after the formation of graphite interlayer compound (GIC) in which the interlayer distance is increased by CrO2Cl2 inserted into the interlayer, under acidic conditions, the interlayer-inserted CrO2Cl2 reacts with double-bonded carbon to break the double bonds, thereby inducing strain in the carbon lattice to form defects or to favor oxidation by an oxidizing agent. However, since oxidation by an oxidizing agent is carried out by a diffusive-controlled process, the interlayer-inserted CrO2Cl2 can control the content of oxygen functional groups by oxidation by inhibiting the diffusion of the oxidizing agent.

[0199] In addition, it can be seen that the pore size can be controlled by a chemical oxidation reaction by an oxidizing agent.

[0200]

[0201] (Examples 5 to 8) Preparation of membrane

[0202] The nanoporous graphite of Examples 1, 2, 3, and 4 was used to manufacture membranes of Examples 5, 6, 7, and 8, respectively.

[0203] Each nanoporous graphite dispersion (0.01 mg / mL) in deionized water was coated on a polyethersulfone (PES) porous polymer support (47 mm, pore size: 200 nm, Sterlitech) using vacuum filtration, and then dried at 25°C to manufacture each membrane.

[0204]

[0205] (Comparative Example 4)

[0206] The same process as that of manufacturing a membrane in Example 5 was performed, except that the membrane was manufactured using the carbon body of Comparative Example 2.

[0207]

[0208] (Experimental Example 3) Analysis of changes in the interlayer structure of the membrane

[0209] FIGS. 9a, 9b, and 9c are drawings showing an optical image, a top-view scanning electron microscope (SEM) image, and a cross-section SEM image, respectively, of a membrane manufactured according to Example 5.

[0210] Referring to FIGS. 9a, 9b, and 9c, it can be seen that the manufactured separator is flexible and has excellent bending resistance characteristics, and it was confirmed that an active layer including nanoporous graphite with a thickness of 50 nm was formed.

[0211] FIG. 10a, FIG. 10b and FIG. 10c are schematic diagrams showing the results of changes in the interlayer structure of carbon bodies included in the membranes of Example 5 and Comparative Example 4 under conditions of aqueous solutions containing various ions, the results of changes in the interlayer structure according to the concentration of ions and the phenomenon of interlayer distance expansion under pure H2O conditions, respectively.

[0212] At this time, the result of the change in the interlayer structure of Fig. 10a was compared using the interlayer distance calculated from the XRD pattern measured after immersing each membrane in the dried state and each ion solution (NaCl, Na2SO4, LiCl, CaCl2, MgCl2, K3[Fe(CN)6], and AlCl2) of pure and 0.1 M concentrations for 24 hours, and the result of the change in the interlayer structure of Fig. 10b was compared using the interlayer distance calculated from the XRD pattern measured after immersing each membrane in each ion solution (NaCl, Na2SO4, and MgCl2) of concentrations of 0.01 M, 0.1 M, and 1 M, respectively.

[0213] First, referring to FIG. 10a, the interlayer distance of the membrane of Example 5 was observed to increase by 1.4 Å from the interlayer distance of the dry membrane (7.5 Å) to 8.9 Å after being immersed in pure water, whereas the interlayer distance of the membrane of Comparative Example 4 was observed to increase by 3.6 Å from 7.9 Å to 11.5 Å after being immersed in pure water. This indicates that the interlayer distance of the membrane of Comparative Example 4 expanded by approximately 2.6 times more than that of the membrane of Example 5, resulting in a significant decrease in interlayer distance stability when immersed in pure water.

[0214] In addition, the degree of change in the interlayer structure is affected by the ions inserted between the layers, and it can be seen that the change in the interlayer distance of Example 5 and Comparative Example 4 occurs the most in the MgCl2 ion solution. In the case of Example 5, it was confirmed that the interlayer distance expanded by a maximum of 2.91 Å from 7.5 Å to 10.41 Å, whereas in Comparative Example 4, the interlayer distance expanded by a maximum of 6.02 Å from 7.9 Å to 13.92 Å, similarly confirming that the interlayer distance expanded to a maximum of about 2.1 times more than that of Example 5.

[0215] In general, in the field of water treatment, ion rejection capacity can be defined by the interlayer distance of the separation membrane, and stabilizing the interlayer distance has the advantage of improving the ion rejection rate and reliability at the same time.

[0216] Additionally, referring to FIG. 10b, it was confirmed that the interlayer distance of the membrane of Example 5 was suppressed to 10 Å or less even under various concentrations of ionic solutions, but in the case of the membrane of Comparative Example 4, the interlayer distance was expanded to a maximum of 14 Å, and it was confirmed that the stability according to the concentration of the ionic solution also decreased.

[0217] FIG. 11a and FIG. 11b are drawings showing XRD patterns measured after the membrane of Example 5 was immersed in pure water for 1 day and 60 days, respectively, and schematically showing the interlayer distance expansion phenomenon under pure water (pure H2O) conditions for Comparative Example 4 and Example 5.

[0218] As shown in Fig. 11a, the nanoporous graphite included in the membrane of Example 5 was not exfoliated even after being immersed in pure water for 60 days, and the interlayer distance based on the XRD pattern was also maintained, confirming that the stability of the interlayer distance was maintained for a long period of time.

[0219] These results, as shown in Fig. 11b, indicate that the membrane of Example 5 can effectively maintain a narrow capillary shape (interlayer distance) by enhancing the interlayer interaction through pi-pi (ππ interaction) because the functional groups containing oxygen contained in the nanoporous graphite are limited in a pure or ionic solution.

[0220] FIG. 12a and FIG. 12b are drawings comparing XRD patterns measured after immersing the membranes of Examples 5 to 8 in a dry state and in pure water for 24 hours, respectively, and drawings comparing interlayer distances calculated from XRD patterns measured after immersing each membrane in 0.1 M of each ionic solution (NaCl, Na2SO4, LiCl, CaCl2, MgCl2, K3[Fe(CN)6], and AlCl2) for 24 hours.

[0221] Referring to FIGS. 12a and 12b, it can be seen that the more oxygen-containing functional groups are included in the nanoporous graphite included in the separation membrane, the greater the degree of change due to expansion of the interlayer distance.

[0222] Thus, controlled oxidation is essential for the production of nanoporous graphite with limited oxygen-containing functional groups along with pore formation in graphite, especially in the field of desalination under high salinity conditions, because the ion rejection rate is enhanced depending on the steric effect between the interlayer distance and the hydrated shell.

[0223]

[0224] (Experimental Example 4) Comparative Analysis of Membrane Performance

[0225] To compare the performance of each manufactured membrane, ion permeation tests and forward osmosis desalination tests were performed.

[0226] At this time, the ion permeation test and forward osmosis desalination test were performed using an H-type cell divided into a feed region and a permeation region, and each separation membrane was positioned in the middle of each region divided so as to face the feed region.

[0227] The ion permeation test was performed by filling the feed area and the permeation area with 80 mL of deionized water and each ion solution (KCl, NaCl, Na2SO4, LiCl, CaCl2, MgCl2, and K3[Fe(CN)6]), respectively, and then performing the test for 24 hours. After that, the ion conductivity in the permeation area was measured to compare and evaluate the ion permeation rate.

[0228] Figures 13a and 13b are diagrams showing the ion permeability characteristics of the membranes of Examples 5 to 8, respectively, according to the ion permeability and the anion-to-cation valence ratios included in the ion solution.

[0229] Referring to FIGS. 13a and 13b, in the case of Examples 7 and 8, the monovalent ion (K + , Na + , and Li + ) and multivalent ions ((SO4 2-, Ca 2+ , Mg 2+ , Al 3+ , Fe(CN)6 3- ) was observed to exhibit relatively high ion permeability for all, resulting in poor selectivity for ion exclusion.

[0230] On the other hand, in the case of the membrane of Example 5 containing nanoporous graphite with limited functional groups containing oxygen by controlled oxidation, it can be seen that the permeability for monovalent ions and polyvalent ions is reduced by 3 to 5 times, which can significantly improve the efficiency of ion exclusion present in an aqueous solution.

[0231] The forward osmosis desalination test was performed similarly to the ion permeation test, using an H-type cell with feed and draw regions divided into sections, with the membrane of Example 5 positioned in the middle of each section. 80 mL of 0.1 M ion solutions (KCl, NaCl, Na2SO4, LiCl, MgCl2) were used as the feed solution, and 80 mL of 2 M sucrose solution was used as the draw solution.

[0232] At this time, the ion rejection rate R(%) was calculated using the following equation 2.

[0233]

[0234] (Formula 2)

[0235] R(%) = 1 - (C ep / C f ) x 100

[0236] (C in Equation 2 ep is the concentration of the drawn salt, and C f is the ion concentration in the feed solution.)

[0237]

[0238] The concentration of the salt drawn here was calculated using the following equation 3.

[0239]

[0240] (Formula 3)

[0241] C ep = (C p (V draw +ΔV)) / ΔV

[0242] (C in Equation 3 p is the concentration of salt in the draw solution, and V draw is the volume of the draw solution, and ΔV is the change in volume of the draw solution.)

[0243]

[0244] Figures 14a and 14b are diagrams comparing the performance results of Example 5 according to a continuous forward osmosis desalination test for 24 hours and the ion rejection rate according to a continuous forward osmosis desalination test for 1 day and 7 days, respectively.

[0245] As shown in Fig. 14a, it was confirmed that the ion rejection rate for monovalent ions and polyvalent ions was 99.5% or higher regardless of the type of ion, and the water flux was also 0.75 to 0.92 LMH, demonstrating excellent membrane performance. As shown in Fig. 14b, it can be seen that the ion rejection rate characteristic of 99.5% or higher was still maintained even after 7 days of continuous forward osmosis desalination testing, confirming that the durability of the membrane is also excellent.

[0246] Additionally, the performance of the separation membrane was compared and evaluated according to the concentration and pH conditions of the ion solution.

[0247] Figures 15a and 15b are diagrams showing the performance evaluation results of a separation membrane according to the concentration of NaCl solution and the performance evaluation results of a separation membrane according to the pH change of the NaCl solution, respectively.

[0248] Referring to Fig. 15a, it was observed that even in the case of 0.01 to 1 M NaCl solution, an ion rejection rate characteristic of 99.4% or more was shown, and it was observed that even in the case of a highly concentrated 2 M NaCl solution, the ion rejection rate characteristic was maintained at 90.5% or more.

[0249] In the case of water flow rate, it can be seen that it gradually decreases as the concentration of the ion solution increases. This is because the concentration difference between the feed solution and draw solution areas decreases, which reduces the osmotic pressure effect. In particular, when the concentration of the ion solution is the same or higher than that of the draw solution, the driving force that enables water movement is low, so the ion rejection rate characteristic appears low in the case of a highly concentrated ion solution.

[0250] As shown in Fig. 15b, it was confirmed that the ion rejection rate characteristic of 99.5% or more was maintained even under harsh conditions such as alkaline and acidic conditions during continuous forward osmosis desalination tests for 7 days.

[0251] Furthermore, the long-term durability of the membrane was evaluated by conducting a forward osmosis desalination test for 30 days, and the performance according to the thickness of the membrane was further compared and analyzed.

[0252] At this time, the thickness of the separation membrane refers to the thickness of the nanoporous graphite layer coated on the PES porous polymer support.

[0253] Figures 16a and 16b are drawings showing the performance evaluation results for the membrane of Example 5 according to a continuous forward osmosis desalination test for 30 days using a 0.1 M NaCl solution and a 1 M NaCl solution as feed solutions, respectively, and the performance evaluation results for the membrane of Example 5 according to the thickness of the membrane using a 0.1 M NaCl solution.

[0254] As shown in Fig. 16a, even after a long-term test for 30 days, the ion rejection rates in the feed solutions of 0.1 M NaCl and 1 M NaCl were maintained at excellent levels of 99.8% and 98%, respectively, and the water flow rate was also confirmed to be stable.

[0255] Referring to Fig. 16b, when the thickness of the membrane is 20 nm and 10 nm, the water flow rate increases to 2.21 LMH and 4.42 LMH, respectively, and the ion rejection rate is 96% and 84%, respectively. The decrease in the ion rejection rate is believed to be due to the increase in defects due to the decrease in the membrane thickness, but the 84% ion rejection rate characteristic still shows excellent performance based on the two-dimensional membrane.

[0256] As described above, the excellent ion rejection performance of the separation membrane according to the present invention is due to the modulation of the interlayer distance due to the nanopores contained in the nanoporous graphite and limited oxidation.

[0257] Figure 17 is a schematic diagram illustrating the mechanism of desalination using a membrane containing nanoporous graphite.

[0258] As illustrated in Figure 17, nanoporous graphite can be formed by controlled oxidation, which includes both nanopores and sp3 regions with expanded interlayer spacing. Thus, nanoporous graphite can include sp3 regions with expanded interlayer spacing and sp2 regions with relatively narrow interlayer spacing, along with a two-dimensional network of interconnected pores.

[0259] At this time, nanoporous graphite has a structure that includes pores that are smaller or similar in size to the hydrated ion size, and sp3 and sp2 regions with different interlayer distances, thereby providing resistance to ion permeation due to the steric effect and increasing the permeation selectivity of ions. In addition, water that is limited to a relatively narrow interlayer distance region can shorten the movement path of water or effectively reduce the tortuosity of the movement path by the pore structure, thereby further enhancing the selective exclusion effect of ions.

[0260]

[0261] Although the present invention has been described through specific matters and limited examples as described above, these are provided only to help a more general understanding of the present invention, and the present invention is not limited to the above examples, and those skilled in the art to which the present invention pertains can make various modifications and variations based on this description.

[0262] Therefore, the idea of ​​the present invention should not be limited to the described embodiments, and all things that are equivalent or equivalent to the claims described below as well as the claims are considered to fall within the scope of the idea of ​​the present invention.

Claims

1. Nanoporous graphite characterized in that it includes a plurality of nanopores on at least one side of a graphite layer, has a diffraction peak due to the (002) crystal plane of graphite in X-ray diffraction analysis, and at least one of the plurality of nanopores is located on an in-plane inside the graphite layer.

2. In paragraph 1, The above nanoporous graphite is a nanoporous graphite containing a D' band in a Raman spectrum.

3. In paragraph 1, I of the Raman spectrum of the above nanoporous graphite d / I g Nanoporous graphite having a strength ratio of 0.3 to 1.

5.

4. In paragraph 1, The above nanoporous graphite is a nanoporous graphite including a D' band having a stronger scattering intensity than the D band in a Raman spectrum.

5. In paragraph 1, The above nanoporous graphite is a nanoporous graphite comprising a D' band having a stronger scattering intensity than the 2D band in a Raman spectrum.

6. In paragraph 1, Nanoporous graphite, wherein the FWHM of the diffraction peak due to the (002) crystal plane of graphite in the X-ray diffraction analysis of the above nanoporous graphite is 5° or less.

7. In paragraph 1, Nanoporous graphite, wherein the average diameter of the above nanopores is 500 nm or less.

8. In paragraph 1, Nanoporous graphite, wherein at least five nanopores are included in a 50 nm x 50 nm image observed with a transmission electron microscope after the nanoporous graphite is exfoliated into graphene.

9. In paragraph 1, The above nanoporous graphite is a nanoporous graphite that satisfies the following equation 1. (Formula 1) SNPG / SG ≤ 10 (SNPG stands for the BET surface area of ​​nanoporous graphite, and SG stands for the BET surface area of ​​pristine graphite) 10. In paragraph 1, The above nanoporous graphite is 20 m 2 Nanoporous graphite having a BET surface area of ​​less than / g.

11. In paragraph 1, Nanoporous graphite, wherein the size of the above nanopores is controlled by a chemical oxidation reaction.

12. In paragraph 1, The above nanoporous graphite is 0.1 cm 3 Nanoporous graphite having a pore volume of less than / g.

13. In paragraph 1, The above nanoporous graphite is a nanoporous graphite in which the intensity of the peak of C-O-C, C-O, or C-O bonding energy according to X-ray photoelectron spectroscopy is lower than the intensity of the peak of C-O-C and C-C bonding energy.

14. A separation membrane comprising nanoporous graphite according to paragraph 1.

15. In paragraph 14, The above separation membrane is a separation membrane for water treatment, solvent nanofiltration, gas separation or ion separation.

16. An electrochemical device comprising nanoporous graphite according to any one of claims 1 to 13.

17. Contains Cr on at least one side of the graphite layer, and includes a D' band in the Raman spectrum, A nanoporous graphite precursor characterized by having two or more diffraction peaks diffracted at an angle lower than the diffraction angle 2θ due to the (002) crystal plane of graphite in X-ray diffraction analysis.

18. In paragraph 17, A nanoporous graphite precursor comprising a D band having a weaker scattering intensity than a 2D band in the above Raman spectrum.

19. In paragraph 17, A nanoporous graphite precursor, wherein the Cr is contained in an amount of 3 wt% or less of the total weight of the nanoporous graphite precursor. 20.(S1) A step of preparing a nanoporous graphite precursor by positioning one or more intercalating compounds on the upper side of at least one surface of graphite; (S2) a step in which the intercalating compound reacts with the carbon-carbon unsaturated bonds contained in the graphite; and (S3) a step in which nanopores are formed due to the reaction of the above step (S2); including; A method for producing nanoporous graphite, wherein the intercalating compound causes nanopores at the location of the saturated bond.

21. In paragraph 20, The above intercalating compound is CrO2Cl2; Cr2O3; FeCl3; A method for producing nanoporous graphite, wherein at least one compound is selected from the group consisting of: and a compound comprising the same.

22. In paragraph 20, A method for producing nanoporous graphite, wherein the reaction in the above step (S2) is an oxidation reaction.

23. In paragraph 20, A method for producing nanoporous graphite, wherein the reaction of the above step (S2) is performed under acidic conditions.

24. In paragraph 20, A method for producing nanoporous graphite, wherein the above step (S2) is performed by adding an oxidizing agent.

25. In paragraph 24, A method for producing nanoporous graphite, wherein the oxidizing agent comprises KMnO4.

Citation Information

Patent Citations

  • Alkali metal battery having an integral 3D graphene-carbon-metal hybrid foam-based electrode

    CN109314225A

  • Electrode active material for capacitor, and capacitor using said electrode active material

    KR1020150063373A

  • Supercapacitor having an integral 3D graphene-carbon hybrid foam-based electrode

    KR1020180099735A