Negative electrode and lithium battery comprising same
The use of an amorphous carbon electrodeposition inducing layer with high nitrogen content in lithium batteries addresses the issue of lithium dendrite growth, enhancing cycle stability and energy density by promoting uniform lithium deposition.
Patent Information
- Application Number
- PCT/KR2024/003729
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-07-03
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium metal batteries suffer from short circuits due to the growth of lithium dendrites, which deteriorate the lifespan characteristics, as carbon-based anode materials do not change volume during charging and discharging, limiting their stability and cycle performance.
A cathode with an electrodeposition inducing layer containing amorphous carbon with a nitrogen content greater than 1% by weight, which uniformly deposits lithium ions, preventing the formation and growth of dendrites.
The solution enhances the cycle characteristics and stability of lithium batteries by ensuring uniform lithium deposition, reducing the occurrence of short circuits and improving energy density.
Smart Images

Figure KR2024003729_03102024_PF_FP_ABST
Abstract
Description
Cathode and lithium battery containing same
[0001] It relates to a cathode and a lithium battery including the same.
[0002] Lithium batteries currently on the market primarily use carbon-based anode materials, such as graphite. Carbon-based anode materials exhibit no volume change during charge and discharge, contributing to the stability of lithium batteries. Graphite's theoretical capacity is relatively small, at around 372 mAh / g.
[0003] Lithium metal can be used as an anode active material. Lithium metal has a very high theoretical electrical capacity of approximately 3860 mAh / g. During charge / discharge, lithium metal can form dendrites on its surface due to side reactions with the electrolyte. These dendrites can grow and cause short circuits between the anode and cathode. Consequently, the lifespan of lithium batteries containing lithium metal deteriorates.
[0004] A method for improving the life characteristics of a lithium battery containing lithium metal is required.
[0005] One aspect is to provide a new structure of cathode.
[0006] Another aspect is to provide a lithium battery comprising a cathode of a novel structure.
[0007] According to the implementation example
[0008] negative current collector; and
[0009] A cathode current collector is disposed on the electrodeposition induction layer, and includes a first carbon-based material;
[0010] The above first carbon-based material is amorphous carbon containing a nitrogen element,
[0011] A cathode is provided, wherein the content of nitrogen element exceeds 1 wt% with respect to the total weight of the above-described electrodeposition induction layer.
[0012] According to another implementation example,
[0013] anode; cathode as above; and
[0014] A lithium battery is provided, including an electrolyte disposed between the positive electrode and the negative electrode.
[0015] According to one aspect, by adopting a negative electrode having a new structure, it is possible to provide a lithium battery with improved cycle characteristics by uniformly depositing lithium.
[0016] Figure 1 is a cross-sectional view of a cathode according to an exemplary embodiment.
[0017] Figure 2 is a cross-sectional view of a cathode according to another exemplary embodiment.
[0018] Figure 3 is a schematic diagram of a lithium metal battery according to an exemplary embodiment.
[0019] Figure 4 is a schematic diagram of a lithium metal battery according to an exemplary embodiment.
[0020] Figure 5 is a schematic diagram of a lithium metal battery according to an exemplary embodiment.
[0021] FIG. 6 is a cross-sectional view of a lithium metal battery including a solid electrolyte layer according to another exemplary embodiment.
[0022] Figure 7 is a cross-sectional view of a lithium metal battery including a solid electrolyte layer according to another exemplary embodiment.
[0023] Figure 8a is an SEM image of the cathode when a lithium electrodeposition layer begins to form on the electrodeposition-inducing layer according to Example 1.
[0024] Figure 8b is an SEM image of the cathode after a lithium electrodeposition layer is formed on the electrodeposition-inducing layer according to Example 1.
[0025] Figure 9a is an SEM image of the cathode when a lithium electrodeposition layer began to form on the electrodeposition-inducing layer according to Comparative Example 3.
[0026] Figure 9b is an SEM image of the cathode after a lithium electrodeposition layer is formed on the electrodeposition-inducing layer according to Comparative Example 3.
[0027] In a lithium-free anode lithium metal battery, which is a lithium battery, a lithium deposited layer containing lithium is precipitated and dissolved between the anode current collector and the electrolyte layer during the charge / discharge process. As the charge / discharge of the lithium-free metal battery is repeated, the lithium deposited layer includes impurities remaining in the electrode, decomposition products of the electrolyte, etc. Therefore, the surface of the lithium deposited layer becomes rough and hard due to the inclusion of these impurities. Lithium dendrites are deposited on the lithium deposited layer having this rough surface. These lithium dendrites continuously grow during the charge / discharge process, which can cause a short circuit between the positive and negative electrodes.
[0028] The negative electrode according to one aspect has a new structure, which allows lithium to be uniformly deposited and suppresses the formation of lithium dendrites on the negative electrode, thereby suppressing the occurrence of short circuits in a lithium battery using such a negative electrode, thereby improving the cycle characteristics.
[0029]
[0030] The present inventive concept described below is capable of various modifications and embodiments. Specific embodiments are illustrated in the drawings and described in detail. However, this is not intended to limit the present inventive concept to specific embodiments, but rather to encompass all modifications, equivalents, or alternatives within the technical scope of the present inventive concept.
[0031] The terminology used below is only used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. Hereinafter, the terms "comprises" or "has" and the like are intended to indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, but should be understood to not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. The " / " used below may be interpreted as "and" or "or" depending on the context.
[0032] In order to clearly express various layers and regions in the drawings, the thickness is shown enlarged or reduced. Similar parts are designated by the same drawing reference numerals throughout the specification. When a part such as a layer, film, region, or plate is said to be "on" or "above" another part throughout the specification, this includes not only cases where it is directly above the other part, but also cases where there is another part in between. Terms such as first, second, etc. may be used throughout the specification to describe various components, but the components should not be limited by the terms. The terms are used only for the purpose of distinguishing one component from another. In this specification and the drawings, components having substantially the same functional configuration are referred to by the same reference numerals, and redundant descriptions are omitted.
[0033] In the present disclosure, the "particle diameter" of a particle refers to the average diameter when the particle is spherical, and refers to the average major axis length when the particle is non-spherical. The particle diameter of a particle can be measured using a particle size analyzer (PSA). The "particle diameter" of a particle is, for example, the average particle diameter. The average particle diameter is, for example, the median particle diameter (D50). The median particle diameter (D50) is the size of a particle corresponding to 50% of the cumulative volume, calculated from the side of particles having a small particle size in a size distribution of particles measured, for example, by laser diffraction.
[0034] In this disclosure, “metal” includes both metals and metalloids such as silicon and germanium, in their elemental or ionic states.
[0035] In this disclosure, “alloy” means a mixture of two or more metals.
[0036] In the present disclosure, “positive electrode material” means a positive electrode material capable of undergoing lithiation and delithiation.
[0037] In the present disclosure, “negative electrode active material” means a negative electrode material capable of undergoing lithiation and delithiation.
[0038] In the present disclosure, “lithiation” and “lithiating” mean a process of adding lithium to a positive electrode active material or a negative electrode active material.
[0039] In the present disclosure, “delithiation” and “delithiate” mean a process of removing lithium from a positive electrode active material or a negative electrode active material.
[0040] In this disclosure, “charging” and “charging” mean a process of providing electrochemical energy to a battery.
[0041] In this disclosure, “discharging” and “discharging” mean the process of removing electrochemical energy from a battery.
[0042] In the present disclosure, “positive electrode” and “cathode” mean an electrode at which electrochemical reduction and lithiation occur during a discharge process.
[0043] In the present disclosure, “cathode” and “anode” mean electrodes where electrochemical oxidation and delithiation occur during a discharge process.
[0044]
[0045] Below, a negative electrode and a lithium battery including the same according to exemplary embodiments are described in more detail.
[0046] [cathode]
[0047] According to one embodiment, a negative electrode includes: a negative current collector; and an electrodeposition inducing layer disposed on the negative current collector and including a first carbon-based material; wherein the first carbon-based material is an amorphous carbon including a nitrogen element, and the content of the nitrogen element with respect to the total weight of the electrodeposition inducing layer may be greater than 1 wt%. In this case, the content of the nitrogen element with respect to the total weight of the first carbon-based material may be greater than 10 wt%. For example, the electrodeposition inducing layer including the first carbon-based material including the nitrogen element may uniformly electrodeposit lithium ions on the electrodeposition inducing layer. For example, in the electrodeposition inducing layer including the first carbon-based material including the nitrogen element, lithium ions may preferentially bind to the nitrogen element, so that lithium ions are electrodeposited on the surface of the first carbon-based material, and thus lithium ions may be uniformly electrodeposited on the electrodeposition inducing layer. As lithium ions are uniformly deposited on the electrodeposition-inducing layer, the density of the lithium electrodeposition layer formed on the electrodeposition-inducing layer is improved, so that the energy density of a lithium battery including the negative electrode can be improved. The first carbon-based material including a nitrogen element can uniformly deposit lithium ions on the surface of the electrodeposition-inducing layer, thereby effectively preventing the generation and / or growth of lithium dendrites. The stability of the negative electrode including the electrodeposition-inducing layer including the first carbon-based material including the nitrogen element and the lithium battery employing the same is improved, and the cycle characteristics of the lithium battery are improved.
[0048] In contrast, the electrodeposition-inducing layer including the first carbon-based material that does not contain a nitrogen element or has a nitrogen element content of 10 wt% or less based on the total weight of the first carbon-based material may not cause uniform electrodeposition of lithium ions, since the content of the nitrogen element contained in the electrodeposition-inducing layer corresponds to 1 wt% or less. Accordingly, the density of the lithium electrodeposition layer formed on the electrodeposition-inducing layer may decrease, so that the energy density of the negative electrode including the electrodeposition-inducing layer including the first carbon-based material including the nitrogen element and the lithium battery employing the same may decrease. In addition, the electrodeposition-inducing layer including the first carbon-based material that does not contain a nitrogen element or has a low nitrogen element content may not cause uniform electrodeposition of lithium ions on the electrodeposition-inducing layer, making it difficult to effectively suppress the generation and / or growth of lithium dendrites on the surface of the electrodeposition-inducing layer. The stability of a negative electrode and a lithium battery including an electrodeposition-inducing layer including a first carbon-based material that does not contain a nitrogen element or has a low nitrogen element content may be reduced, and the cycle characteristics of the lithium battery may be reduced.
[0049] Referring to FIG. 1, the negative electrode (20) includes a negative electrode current collector (21); and an electrodeposition-inducing layer (22) disposed on the negative electrode current collector (21) and including a first carbon-based material, wherein the first carbon-based material is amorphous carbon including a nitrogen element, and the content of the nitrogen element is greater than 1 wt% with respect to the total weight of the electrodeposition-inducing layer.
[0050] Referring to FIG. 2, the negative electrode (20) includes: a negative electrode current collector (21); an electrodeposition-inducing layer (22) disposed on the negative electrode current collector (21) and including a first carbon-based material; and a lithium electrodeposition layer (23) disposed on the electrodeposition-inducing layer (22), wherein the first carbon-based material is amorphous carbon including a nitrogen element, and the content of the nitrogen element is greater than 1 wt% with respect to the total weight of the electrodeposition-inducing layer.
[0051]
[0052] [Cathode: Negative current collector]
[0053] Referring to FIGS. 1 and 2, the negative electrode (20) includes a negative electrode collector (21).
[0054] The material constituting the negative electrode current collector (21) may be any material that does not react with lithium, i.e., does not form an alloy or compound with lithium, and has conductivity. The negative electrode current collector (21) is, for example, a metal or an alloy. The negative electrode current collector (210) may be made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel (SUS), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
[0055] The negative electrode current collector (21) includes, for example, a first metal substrate. The first metal substrate includes, or is made of, the first metal as a main component. The first metal substrate includes, or is made of, the first metal as a main component. The content of the first metal included in the first metal substrate is, for example, 90 wt% or more, 95 wt% or more, 99 wt% or more, or 99.9 wt% or more, based on the total weight of the first metal substrate. The first metal substrate may be made of, for example, a material that does not react with lithium, i.e., does not form an alloy and / or compound with lithium.
[0056] The first metal is not necessarily limited to, for example, copper (Cu), nickel (Ni), stainless steel (SUS), iron (Fe), and cobalt (Co), and any metal that can be used as a current collector in the relevant technical field can be used. The first metal substrate may be composed of, for example, one of the above-described metals, or may be composed of an alloy of two or more metals. The first metal substrate is, for example, in the form of a sheet or foil. The thickness of the negative electrode current collector (21) may be, for example, 5 ㎛ to 50 ㎛, 10 ㎛ to 50 ㎛, 10 ㎛ to 40 ㎛, or 10 ㎛ to 30 ㎛, but is not necessarily limited to this range, and may be selected according to the characteristics of the required lithium battery.
[0057] The negative electrode collector (21) may further include a coating layer (not shown) containing a second metal on the first metal substrate.
[0058] The negative electrode current collector (21) may include, for example, a first metal substrate; and a coating layer disposed on the first metal substrate and including a second metal. The second metal has a higher Mohs hardness than the first metal. That is, since the coating layer including the second metal is harder than the substrate including the first metal, deterioration of the first metal substrate can be prevented. The Mohs hardness of the material constituting the first metal substrate is, for example, 5.5 or less. The Mohs hardness of the first metal is, for example, 5.5 or less, 5.0 or less, 4.5 or less, 4.0 or less, 3.5 or less, or 3.0 or less. The Mohs hardness of the first metal may be, for example, 2.0 to 6.0. The coating layer includes the second metal. The coating layer includes, for example, the second metal as a main component or is made of the second metal. The content of the second metal included in the coating layer is, for example, 90 wt% or more, 95 wt% or more, 99 wt% or more, or 99.9 wt% or more based on the total weight of the coating layer. The coating layer may be composed of, for example, a material that does not react with lithium, i.e., does not form an alloy and / or compound with lithium. The Mohs hardness of the material constituting the coating layer is, for example, 6.0 or more. For example, the Mohs hardness of the second metal is 6.0 or more, 6.5 or less, 7.0 or more, 7.5 or more, 8.0 or more, 8.5 or more, or 9.0 or more. The Mohs hardness of the second metal may be, for example, 6.0 to 12. If the Mohs hardness of the second metal is excessively low, it may be difficult to suppress deterioration of the negative electrode current collector. If the Mohs hardness of the second metal is excessively high, processing may not be easy. The second metal is, for example, one or more selected from titanium (Ti), manganese (Mn), niobium (Nb), tantalum (Ta), iridium (Ir), vanadium (V), rhenium (Re), osmium (Os), tungsten (W), chromium (Cr), boron (B), ruthenium (Ru), and rhodium (Rh).The coating layer may be composed of, for example, one of the above-described metals, or may be composed of an alloy of two or more metals. The difference in Mohs hardness between the first metal included in the first metal substrate and the second metal included in the coating layer may be, for example, 2 or more, 2.5 or more, 3 or more, 3.5 or more, or 4 or more. Since the first metal and the second metal have such a difference in Mohs hardness, deterioration of the negative electrode current collector can be more effectively suppressed. The coating layer may have a single-layer structure or a multi-layer structure of two or more layers. The coating layer may have a two-layer structure including, for example, a first coating layer and a second coating layer. The coating layer may have a three-layer structure including, for example, a first coating layer, a second coating layer, and a third coating layer. The thickness of the coating layer may be, for example, 10 nm to 1 ㎛, 50 nm to 500 nm, 50 nm to 200 nm, or 50 nm to 150 nm. If the thickness of the coating layer is too thin, it may be difficult to suppress the uneven growth of the lithium-containing metal layer. As the thickness of the coating layer increases, the cycle characteristics of the lithium battery improve. However, if the thickness of the coating layer is too thick, the energy density of the lithium battery decreases and the formation of the coating layer may not be easy. The coating layer may be formed on the first metal substrate by, for example, a vacuum deposition method, a sputtering method, a plating method, etc., but is not necessarily limited to these methods, and any method capable of forming a coating layer in the relevant technical field may be used.
[0059] For example, the negative electrode current collector (21) may have a reduced thickness compared to the negative electrode current collector included in a conventional negative electrode. Therefore, the negative electrode according to the present disclosure is distinguished from the conventional electrode including a thick film current collector, for example, by including a thin film current collector. By employing a thin film current collector having a reduced thickness in the electrode according to one embodiment, the thickness of the lithium electrodeposition layer in the negative electrode including the thin film current collector may be relatively increased. As a result, the energy density of a lithium battery employing such an electrode is increased. The thickness of the negative electrode current collector (21) may be, for example, less than 15 um, 14.5 um or less, or 14 um or less. The thickness of the negative electrode current collector (110, 210) may be, for example, less than 0.1 um to 15 um, 1 um to 14.5 um, 2 um to 14 um, 3 um to 14 um, 5 um to 14 um, or 10 um to 14 um.
[0060] The negative electrode current collector (21) may have a form selected from, for example, a sheet, a foil, a film, a plate, a porous body, a mesoporous body, a body containing through holes, a polygonal ring body, a mesh body, a foam body, and a non-woven body, but is not necessarily limited to these forms, and any form used in the relevant technical field is possible.
[0061] The negative electrode current collector (21) may include, for example, a base film and a metal substrate layer disposed on one or both sides of the base film. The negative electrode current collector (21) includes a substrate, and the substrate may have a structure including, for example, a base film and a metal substrate layer disposed on one or both sides of the base film. An intermediate layer may additionally be disposed on the metal substrate layer.
[0062] For example, the base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film can melt when a short circuit occurs, thereby suppressing a sudden increase in current. The base film may be, for example, an insulator. The metal substrate layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal substrate layer may act as an electrochemical fuse, which may be cut in the event of an overcurrent to prevent a short circuit. The limit current and maximum current can be controlled by controlling the thickness of the metal substrate layer. The metal substrate layer may be plated or deposited on the base film. When the thickness of the metal substrate layer is reduced, the limit current and / or maximum current of the negative electrode current collector (21) decreases, thereby improving the stability of the lithium metal battery in the event of a short circuit. A lead tab may be added on the metal substrate layer for external connection. The lead tab may be welded to the metal substrate layer or the metal substrate layer / base film laminate by ultrasonic welding, laser welding, spot welding, etc. During welding, the base film and / or the metal substrate layer may be melted, so that the metal substrate layer may be electrically connected to the lead tab. In order to make the welding of the metal substrate layer and the lead tab more solid, a metal chip may be added between the metal substrate layer and the lead tab. The metal chip may be a thin piece of the same material as the metal of the metal substrate layer. The metal chip may be, for example, a metal foil, a metal mesh, etc.The metal piece may be, for example, aluminum foil, copper foil, SUS foil, etc. After arranging the metal piece on the metal substrate layer, the lead tab may be welded to the metal piece / metal substrate layer laminate or the metal piece / metal substrate layer / base film laminate by welding the metal piece with the lead tab. During welding, the base film, the metal layer, and / or the metal piece may melt, so that the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal substrate layer. The base film may have a thickness of, for example, 1 to 50 ㎛, 1.5 to 50 ㎛, 1.5 to 40 ㎛, or 1 to 30 ㎛. When the base film has a thickness in this range, the weight of the negative electrode assembly can be more effectively reduced. The melting point of the base film may be, for example, 100 to 300°C, 100 to 250°C or less, or 100 to 200°C. Since the base film has a melting point within this range, the base film can be melted and easily bonded to the lead tab during the process of welding the lead tab. To improve the adhesion between the base film and the metal substrate layer, a surface treatment such as corona treatment may be performed on the base film. The thickness of the metal substrate layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to ㎛. Since the metal substrate layer has a thickness within this range, conductivity can be maintained while ensuring the stability of the negative electrode. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness within this range, the connection between the metal layer and the lead tab can be performed more easily. By having this structure, the negative electrode collector (21) can reduce the weight of the electrode and consequently improve the energy density.
[0063]
[0064] [Cathode: Electrodeposition-inducing layer]
[0065] Referring to FIGS. 1 and 2, the negative electrode (20) includes a negative electrode current collector (21); and an electrodeposition-inducing layer (22) disposed on the negative electrode current collector (21). The electrodeposition-inducing layer (22) includes a first carbon-based material. The first carbon-based material is an amorphous carbon containing a nitrogen element, and the content of the nitrogen element exceeds 1 wt% with respect to the total weight of the electrodeposition-inducing layer (22). Since the electrodeposition-inducing layer (22) includes the first carbon-based material containing a nitrogen element, lithium metal can be more uniformly electrodeposited on the electrodeposition-inducing layer. In particular, since the content of the nitrogen element exceeds 1 wt% with respect to the total weight of the electrodeposition-inducing layer, the density of the lithium electrodeposition layer formed on the electrodeposition-inducing layer increases, and the generation and / or growth of lithium dendrites can be effectively prevented.
[0066] According to one embodiment, the content of the nitrogen element is 1.1 wt% or more, 1.2 wt% or more, 1.1 wt% to 10 wt%, or 1.2 wt% to 10 wt% based on the total weight of the electrodeposition-inducing layer.
[0067] According to one embodiment, the content of the nitrogen element in the first carbon-based material may be greater than 10 wt%, greater than 11 wt%, or greater than 12 wt% based on the total weight of the first carbon-based material. When the content of the nitrogen element in the first carbon-based material satisfies the above range, the content of the nitrogen element in the electrodeposition-inducing layer (22) of greater than 1 wt% can be more easily satisfied.
[0068] According to one embodiment, the first carbon-based material may be a carbide of a polymer containing a nitrogen element. For example, the first carbon-based material may be a carbide prepared by carbonizing a polymer containing a nitrogen element at a temperature of 800°C or higher. For example, the carbonization of the polymer containing a nitrogen element may be performed at a temperature of 800°C or higher in a nitrogen atmosphere for 3 hours or longer.
[0069] According to one embodiment, the polymer including the nitrogen element may include sulfurized polyacrylonitrile (SPAN). For example, the sulfurized polyacrylonitrile may have improved structural stability by including a three-dimensionally cross-linked condensed ring. In particular, the sulfurized polyacrylonitrile may include a plurality of nitrogen (N) elements derived from nitrile groups included in the three-dimensionally cross-linked condensed ring. Since the nitrogen element included in the sulfurized polyacrylonitrile is included in the condensed ring, even when the sulfurized polyacrylonitrile is carbonized at a temperature of 800°C or higher, the nitrogen element remains in the carbonized product, and accordingly, a first carbon-based material in which the content of the nitrogen element in the first carbon-based material exceeds 10 wt% with respect to the total weight of the first carbon-based material can be more easily prepared. In addition, the electrodeposition-inducing layer (22) including the first carbon-based material in which the nitrogen element content in the first carbon-based material exceeds 10 wt% with respect to the total weight of the first carbon-based material can more easily have a nitrogen element content exceeding 1 wt%. For example, the nitrogen element contained in the first carbon-based material can react with lithium ions during a charge / discharge process to form a lithium nitride such as Li3N, and this lithium nitride can uniformly electrodeposit lithium ions on the electrodeposition-inducing layer.
[0070] For example, the above-described yellow-modified polyacrylonitrile can be manufactured by heating raw material powders including, for example, sulfur powder and polyacrylonitrile powder in a sealed, non-oxidizing atmosphere. When the sulfur powder and polyacrylonitrile powder are heated, a ring closure reaction in which the polyacrylonitrile is three-dimensionally crosslinked to form a fused ring, for example, a six-membered ring, and a reaction between sulfur and polyacrylonitrile simultaneously proceed, so that a yellow-modified polyacrylonitrile in which sulfur is bonded to the fused ring can be obtained. In this case, the fused ring may include a nitrogen element. Accordingly, when preparing a first carbon-based material by carbonizing a polymer including a yellow-modified polyacrylonitrile, since the nitrogen element included in the condensation ring of the yellow-modified polyacrylonitrile remains without being decomposed during the carbonization process, the content of the nitrogen element included in the first carbon-based material can easily satisfy more than 10 wt%. The electrodeposition-inducing layer including the first carbon-based material including the nitrogen element can more easily satisfy the content of the nitrogen element included in the electrodeposition-inducing layer exceeding 1 wt%, thereby uniformly depositing a lithium element on the electrodeposition-inducing layer.
[0071] According to one embodiment, the first carbon-based material may be an amorphous carbon that further includes elemental sulfur. For example, when the first carbon-based material further includes elemental sulfur, the nitrogen element can be more easily retained during the process of preparing the first carbon-based material.
[0072] For example, the first carbon-based material may be a carbide of a polymer containing nitrogen and sulfur elements. For example, carbonization of a polymer containing nitrogen and sulfur elements may be performed at a temperature of 800°C or higher in a nitrogen atmosphere.
[0073] According to one embodiment, the polymer including the nitrogen element and the sulfur element may include a sulfur-modified polyacrylonitrile. For example, the sulfur-modified polyacrylonitrile may include a condensation ring in which a plurality of sulfur elements are continuously bonded. For example, the sulfur-modified polyacrylonitrile may include a condensation ring formed by continuously bonding three or more sulfur elements. In this case, the condensation ring in which the sulfur elements are continuously bonded may include a nitrogen element. Accordingly, the polymer including the sulfur-modified polyacrylonitrile includes a large amount of the nitrogen element contained in the condensation ring, and since the nitrogen element remains without being decomposed during the carbonization process of the polymer, the nitrogen element content in the first carbon-based material may increase. In addition, since the sulfur element contained in the polymer is decomposed and removed during the carbonization process, the proportion of the nitrogen element in the polymer may further increase.
[0074] According to one embodiment, the content of elemental sulfur in the first carbon-based material may be 0.1 to 50 wt%.
[0075] According to one embodiment, when the first carbon-based material includes elemental sulfur, the electrodeposition-inducing layer (22) including the first carbon-based material may further include Li2S. Li2S may be, for example, 1×10 -5 Since it has an ionic conductivity of S / cm or more, it can provide additional ionic conductivity to the electrodeposition induction layer (22). Li2S can be derived from elemental sulfur contained in the first carbon-based material. Li2S can be generated, for example, by a reaction between elemental sulfur contained in the first carbon-based material and lithium ions during charging of a lithium battery. Since the electrodeposition induction layer (22) additionally contains Li2S, the ionic conductivity of the electrodeposition induction layer (22) can increase.
[0076] According to one embodiment, the intensity ratio of the D peak to the G peak (Id / Ig) obtained by the Raman analysis spectrum of the first carbon-based material may be 0.8 to 1.5. From this, it can be confirmed that the first carbon-based material is an amorphous carbon in the range of the intensity ratio of the D peak to the G peak (Id / Ig) value.
[0077] According to one embodiment, the first carbon-based material may be, for example, in the form of particles. The average particle diameter of the first carbon-based material may be, for example, 50 nm to 10 μm, or 500 nm to 10 μm. Since the first carbon-based material has an average particle diameter within this range, lithium ions can be more uniformly deposited on the electrodeposition-inducing layer.
[0078] The content of the first carbon-based material may be, for example, 1 to 99 wt%, 10 to 90 wt%, 20 to 80 wt%, 20 to 50 wt%, or 30 to 50 wt% based on the total weight of the electrodeposition-inducing layer (21). Since the electrodeposition-inducing layer (22) includes the first carbon-based material in this range, the cycle characteristics of a lithium battery including the electrodeposition-inducing layer (22) can be further improved.
[0079] The electrodeposition-inducing layer (22) may further include a second carbon-based material. For example, the electrodeposition-inducing layer (22) may further include a second carbon-based material that is distinct from the first carbon-based material. The electrodeposition-inducing layer (22) may include, for example, a first carbon-based material and a second carbon-based material, and the first carbon-based material and the second carbon-based material may be different from each other. The second carbon-based material may be, for example, a carbon-based conductive material. By further including the second carbon-based material in the electrodeposition-inducing layer (22), the internal resistance of the electrodeposition-inducing layer (22) may be reduced and conductivity may be imparted to the protective layer.
[0080] According to one embodiment, the dispersibility of the first carbon-based material can be improved by further including a second carbon-based material in the electrodeposition-inducing layer (22). Accordingly, lithium ions can be more uniformly deposited on the electrodeposition-inducing layer (22), thereby more effectively preventing the deposition and / or growth of local lithium dendrites. For example, the second carbon-based material can act as a carbon-based dispersant.
[0081] According to one embodiment, the second carbon-based material may be, for example, amorphous carbon. Since the electrodeposition-inducing layer (22) includes the second carbon-based material that is amorphous carbon, lithium ions can move more quickly through the surface of the amorphous carbon. The second carbon-based material may be porous or non-porous. The second carbon-based material may be, for example, in the form of particles. The second carbon-based material may be, for example, spherical particles, plate-shaped particles, needle-shaped particles, or a combination thereof. The second carbon-based material particles may have, for example, an irregular shape. The average particle diameter of the second carbon-based material may be, for example, 10 nm to 500 nm, 10 nm to 300 nm, 10 nm to 200 nm, 10 nm to 100 nm 10 nm to 50 nm, 30 nm to 50 nm, or 40 nm to 50 nm. By having the above-described second carbon-based material having a particle size within this range, the cycle characteristics of a lithium battery including an electrodeposition-inducing layer can be further improved. The particle size of the above-described carbon-based material can be measured using, for example, laser diffraction, a scanning electron microscope, a transmission electron microscope, or an elemental force microscope.
[0082] According to one embodiment, the second carbon-based material may include carbon black, acetylene black, Denka black, Ketjen black, carbon nanotubes, carbon nanofibers, carbon nanobelts, graphene, graphene oxide, fullerene, activated carbon, carbon fibers, or a combination thereof. For example, the second carbon-based material may include carbon black, acetylene black, Denka black, Ketjen black, or a combination thereof.
[0083] The content of the second carbon-based material may be, for example, 1 to 99 wt%, 10 to 50 wt%, or 20 to 40 wt% based on the total weight of the electrodeposition-inducing layer. By including the second carbon-based material in this range in the electrodeposition-inducing layer (22), the cycle characteristics of a lithium battery including the electrodeposition-inducing layer (22) can be further improved.
[0084] According to one embodiment, the ratio of the content of the first carbon-based material to the content of the second carbon-based material may be 1:99 to 99:1, 10:90 to 90:10, 1:99 to 50:50, or 10:90 to 50:50.
[0085] The electrodeposition-inducing layer (22) may further include, for example, a metal oxide. The electrodeposition-inducing layer (22) may, for example, simultaneously include the first carbon-based material and the metal oxide. The electrodeposition-inducing layer (22) may, for example, simultaneously include the first carbon-based material, the second carbon-based material, and the metal oxide. The electrodeposition-inducing layer (22) including the first carbon-based material and the metal oxide is, for example, an organic-inorganic composite layer. By further including the metal oxide in the electrodeposition-inducing layer (22), the strength and / or elasticity of the electrodeposition-inducing layer (22) may be improved. Since the durability of the electrodeposition-inducing layer (22) is improved, the cycle characteristics of a lithium battery including the electrodeposition-inducing layer (22) may be further improved.
[0086] The metal oxide may be, for example, in the form of particles. The shape of the metal oxide particles is not particularly limited. The metal oxide particles may be, for example, spherical particles, plate-shaped particles, needle-shaped particles, or a combination thereof. The metal oxide particles may have, for example, an irregular shape. The average particle diameter of the metal oxide may be, for example, 100 nm to 2 ㎛, 200 nm to 1 ㎛, or 400 nm to 1 ㎛. When the metal oxide has a particle diameter in this range, the cycle characteristics of the lithium battery including the electrodeposition-inducing layer (22) can be further improved. The metal oxide may be, for example, porous or non-porous. The metal oxide may be, for example, crystalline or amorphous.
[0087] The metal oxide may include, but is not necessarily limited to, Nb2O5, TiO2, Al2O3, SiO2, BaTiO3, MOF (Metal Organic Framework), POSS (Polyhedral Oligomeric Silsesquioxanes), Li2CO3, Li3PO4, Li2O, montmorillonite, ZrO2, CeO2, Mn3O4 or a combination thereof, for example, and any metal oxide used in the art may be used.
[0088] The metal oxide may have, for example, lithiophilicity. A metal oxide having lithium affinity can react with lithium ions during the charge and discharge process of a lithium battery. The metal oxide may include, for example, a pseudo-capacitive oxide that reacts with lithium to form a lithium metal oxide. The oxide providing pseudo-capacity may be, for example, Nb2O5, TiO2, etc. Nb2O5 may have a crystal structure belonging to the orthorhombic system. Nb2O5 may react with lithium ions during the charge process of a lithium battery to form Li xNb2O5(0 <x<1)를 형성할 수 있다. 의사용량성 산화물은 예를 들어 의사커패시터(pseudo capacitor)로 작용함에 의하여 전착유도층(22) 상에 리튬을 저장 및 / 또는 분산시키는 역할을 수행할 수 있다. 의사용량성 산화물을 포함하는 전착유도층(22)의 리튬 이온 전도 특성이 향상되고 리튬의 편재화(localization)가 방지되어, 전착유도층(22) 상에 리튬 이온이 보다 균일하게 전착될 수 있다.
[0089] The metal oxide content may be, for example, 5 to 60 parts by weight, 10 to 50 parts by weight, 10 to 40 parts by weight, or 10 to 30 parts by weight of the metal oxide relative to 100 parts by weight of the first carbon-based material. The metal oxide content included in the electrodeposition-inducing layer (22) may be, for example, 1 to 40 wt%, 5 to 30 wt%, or 5 to 20 wt% relative to the total weight of the protective layer. Since the electrodeposition-inducing layer (22) includes a metal oxide in this range, the cycle characteristics of a lithium battery including the electrodeposition-inducing layer (22) can be further improved.
[0090] The electrodeposition-inducing layer (22) may include, for example, 5 to 40 parts by weight of a metal oxide and 50 to 100 parts by weight of a second carbon-based material relative to 100 parts by weight of the first carbon-based material. Since the electrodeposition-inducing layer (22) has such a composition, the cycle characteristics of a lithium battery including the electrodeposition-inducing layer (22) may be further improved.
[0091] According to one embodiment, the electrodeposition-inducing layer (22) may further include a binder. Since the electrodeposition-inducing layer (22) includes the first carbon-based material and the binder, the bonding strength between the first carbon-based material may be further improved. Since the electrodeposition-inducing layer (22) includes the binder, the electrodeposition-inducing layer (22) may maintain a certain shape and the mechanical strength of the electrodeposition-inducing layer (22) may be improved.
[0092] The binder may be, for example, a non-conductive binder or a conductive binder. The conductive binder may be, for example, an ionically conductive binder, an electronically conductive binder, or a combination thereof.
[0093] Binders include, for example, polystyrene sulfonate (PSS), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP, polyvinylidene fluoride-hexafluoropropylene), polyvinyl fluoride (PVF, polyvinylidene fluoride), poly(meth)acrylic acid, poly(meth)acrylate, polymethyl methacrylate (PMMA, poly(methylmethacrylate), polyethylene oxide (PEO, polyethylene oxide), polyethylene glycol (PEG), polyacrylonitrile (PAN), acrylonitrile-styrene-butadiene copolymer, polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), polyaniline, and polyacetylene, polytetrafluoroethylene (PTFE), styrene-butadiene rubber (SBR), Polyimide (PI), polyamideimide (PAI), carboxymethylcellulose (CMC), polyvinyl chloride (PVC), polyacrylonitrile (PAN), modified polyphenylene oxide (PPO), polyethylene (PE), polypropylene (PP), etc., but are not necessarily limited thereto. The ion-conducting binder may include polar functional groups.Ion-conducting binders containing polar functional groups include, for example, Nafion, Aquivion, Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone sulfone) (SPAEKKS), sulfonated poly(aryl ether ketone) (SPAEK), poly[bis(benzimidazobenzisoquinolinones)] (SPBIBI), poly(styrene sulfonate) (PSS), lithium 9,10-Diphenylanthracene-2-sulfonate (lithium 9,10-diphenylanthracene-2-sulfonate, DPASLi. + ) etc. Electronically conductive binders include, for example, polyacetylene, polythiophene, polypyrrole, poly(p-phenylene), poly(phenylenevinylene), poly(phenylenesulfide), polyaniline, etc.
[0094] The binder may be, for example, an acrylic binder or a fluorinated binder. The fluorinated binder included in the electrodeposition-inducing layer (22) may be, for example, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), etc. For example, the acrylic binder included in the electrodeposition-inducing layer (22) may be, for example, poly(meth)acrylic acid, poly(meth)acrylate, polymethyl(meth)acrylate, polyacrylonitrile, acrylonitrile-styrene-butadiene copolymer, etc.
[0095] The binder content may be, for example, 1 to 30 parts by weight, 5 to 30 parts by weight, or 10 to 30 parts by weight of the binder relative to 100 parts by weight of the first carbon-based material. The binder content included in the electrodeposition-inducing layer (22) may be, for example, 1 to 25 wt%, or 5 to 20 wt% relative to the total weight of the electrodeposition-inducing layer (22). By including a binder in this range in the electrodeposition-inducing layer (22), the cycle characteristics of a lithium battery including the electrodeposition-inducing layer (22) may be further improved.
[0096] The thickness of the electrodeposition-inducing layer (22) may be, for example, 1 ㎛ to 50 ㎛, 3 ㎛ to 20 ㎛, 5 ㎛ to 20 ㎛, or 7 ㎛ to 15 ㎛, but is not necessarily limited to this range and may be adjusted according to the shape, capacity, etc. of the required lithium battery. If the thickness of the electrodeposition-inducing layer (22) is too small, it may be difficult to perform the function of the electrodeposition-inducing layer (22). If the thickness of the electrodeposition-inducing layer (22) is excessively increased, the internal resistance may increase and the energy density of the lithium battery may decrease.
[0097]
[0098] [Cathode: Lithium electrodeposition layer]
[0099] Referring to FIG. 2, the negative electrode (20) includes a negative electrode current collector (21); an electrodeposition induction layer (22) disposed on the negative electrode current collector (21); and a lithium electrodeposition layer (23) disposed on the electrodeposition induction layer (22), wherein the lithium electrodeposition layer (23) includes lithium metal or a lithium alloy.
[0100] The lithium electrodeposition layer (23) may include a lithium electrodeposition layer (23) formed by lithium metal being plated on the electrodeposition-inducing layer (22) by charging after the negative electrode (20) is introduced into the lithium battery together with the positive electrode and the electrolyte. The lithium electrodeposition layer (23) may include, for example, lithium metal or a lithium alloy.
[0101] For example, the lithium alloy is an alloy of lithium and another metal that can be alloyed with lithium, and may be, for example, a lithium-silver alloy, a lithium-zinc alloy, a lithium-magnesium alloy, a lithium-tin alloy, etc.
[0102] According to one embodiment, the lithium electrodeposition layer (23) may include a spherical lithium metal or a spherical lithium alloy. For example, since the lithium electrodeposition layer (23) is formed on the electrodeposition-inducing layer (22) including the first carbon-based material including nitrogen atoms, electrodeposition of lithium ions is induced by the nitrogen atoms, and thus, the spherical lithium metal or lithium alloy may be electrodeposited on the electrodeposition-inducing layer (22). Accordingly, the lithium electrodeposition layer (23) may include a spherical lithium metal or lithium alloy.
[0103] According to one embodiment, the average particle diameter (D50) of the lithium metal or lithium alloy of the embodiment may be 0.1 to 15 μm, 0.1 to 12 μm, 0.1 to 10 μm, 1 to 15 μm, 2 to 15 μm, 3 to 15 μm, or 3 to 10 μm.
[0104] The thickness of the lithium electrodeposition layer (23) may be, for example, 50 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, 1 μm to 50 μm, 1 μm to 40 μm, 5 μm to 40 μm, or 10 μm to 35 μm. For example, when the lithium electrodeposition layer (23) has a thickness within this range, the energy density of the lithium battery can be further improved.
[0105] According to one embodiment, the thickness of the lithium electrodeposition layer (23) at maximum charge may be 35 µm or less, 30 µm or less, 28 µm or less, 10 to 35 µm, 10 to 30 µm, or 10 to 28 µm.
[0106] According to one embodiment, the density of the lithium electrodeposition layer (23) may be 0.3 g / cc to 0.5 g / cc.
[0107]
[0108] [Cathode: Anode interlayer]
[0109] Referring to FIGS. 1 and 2, the negative electrode (20) may optionally further include an anode interlayer (not shown) disposed between the negative electrode current collector (21) and the electrodeposition induction layer (22). By additionally including the anode interlayer in the negative electrode (20), the generation and / or growth of lithium dendrites in the negative electrode (20) can be more effectively suppressed. The anode interlayer may be omitted.
[0110] The negative electrode intermediate layer may include, for example, a negative electrode active material and a binder. The negative electrode active material is a negative electrode material that can be lithiated and delithiated. The negative electrode active material included in the negative electrode intermediate layer has, for example, a particle form. The negative electrode active material having a particle form has an average particle diameter, for example, 10 nm to 4 ㎛, 10 nm to 1 ㎛, 10 nm to 500 nm, 10 nm to 100 nm, or 20 nm to 80 nm. When the negative electrode active material has an average particle diameter in this range, reversible plating and / or dissolution of lithium may be facilitated during charge and discharge. The average particle diameter of the negative electrode active material is, for example, a median diameter (D50) measured using a laser particle size distribution analyzer.
[0111] The negative electrode active material included in the negative electrode intermediate layer may include, for example, at least one selected from a carbon-based negative electrode active material and a metal or metalloid negative electrode active material. The carbon-based negative electrode active material may be, for example, amorphous carbon. Examples of the carbon-based negative electrode active material include, but are not limited to, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, etc., and any material classified as amorphous carbon in the relevant technical field may be used. Amorphous carbon is carbon that has no crystallinity or very low crystallinity, and is distinguished from crystalline carbon or graphite-based carbon. The metal or metalloid negative electrode active material includes, but is not limited to, one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn), and any metal or metalloid negative electrode active material that forms an alloy or compound with lithium in the relevant technical field may be used. For example, nickel (Ni) does not form an alloy with lithium, and therefore is not a metal negative electrode active material in the present specification. The negative electrode intermediate layer includes a type of negative electrode active material among these negative electrode active materials, or includes a mixture of a plurality of different negative electrode active materials. The negative electrode intermediate layer may include, for example, a mixture of amorphous carbon and one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The mixing ratio of the mixture may be, for example, 10:1 to 1:2, 10:1 to 1:1, 7:1 to 1:1, 5:1 to 1:1, or 4:1 to 2:1 by weight.The negative electrode active material included in the negative electrode intermediate layer may include a mixture of first particles made of, for example, amorphous carbon and second particles made of a metal or a metalloid. The metal includes, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The content of the second particles is 8 to 60 wt%, 10 to 50 wt%, 15 to 40 wt%, or 20 to 30 wt% based on the total weight of the mixture. When the second particles have a content in this range, the cycle characteristics of, for example, a lithium battery are further improved.
[0112] The binder included in the negative electrode intermediate layer is, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited thereto, and any binder used in the relevant technical field may be used. The binder may be composed of a single binder or a plurality of different binders. When the negative electrode intermediate layer does not include a binder, the negative electrode intermediate layer can be easily separated from the negative electrode current collector (21). The content of the binder included in the negative electrode intermediate layer may be, for example, 1 to 20 wt% based on the total weight of the negative electrode intermediate layer.
[0113] The thickness of the negative electrode intermediate layer may be, for example, 1 ㎛ to 20 ㎛, 1 ㎛ to 15 ㎛, or 2 ㎛ to 10 ㎛, or 3 ㎛ to 7 ㎛. The thickness of the negative electrode intermediate layer may be, for example, 1% to 50%, 1% to 30%, 1% to 10%, or 1% to 5% of the thickness of the positive electrode active material layer. If the thickness of the negative electrode intermediate layer is too thin, lithium dendrites formed between the negative electrode intermediate layer and the negative electrode current collector may collapse the negative electrode intermediate layer, making it difficult to improve the cycle characteristics of the lithium battery. If the thickness of the negative electrode intermediate layer increases excessively, the energy density of a lithium battery employing the negative electrode (20) may decrease, and it may be difficult to improve the cycle characteristics. If the thickness of the negative electrode intermediate layer decreases, for example, the charge capacity of the negative electrode intermediate layer also decreases. The charge capacity of the negative electrode intermediate layer may be, for example, 0.1% to 50%, 1% to 30%, 1% to 10%, 1% to 5%, or 1% to 2% of the charge capacity. If the charge capacity of the negative electrode intermediate layer is too small, lithium dendrites formed between the negative electrode intermediate layer and the negative electrode current collector may collapse the negative electrode intermediate layer, making it difficult to improve the cycle characteristics of the lithium battery. If the charge capacity of the negative electrode intermediate layer increases excessively, the energy density of the lithium battery using the negative electrode (20) may decrease and it may be difficult to improve the cycle characteristics. The charge capacity of the positive electrode active material layer is obtained by multiplying the charge capacity density (mAh / g) of the positive electrode active material by the mass of the positive electrode active material in the positive electrode active material layer. When multiple types of positive electrode active materials are used, the charge capacity density × mass value is calculated for each positive electrode active material, and the sum of these values is the charge capacity of the positive electrode active material layer. The charge capacity of the negative electrode intermediate layer is also calculated in the same way. That is, the charge capacity of the negative electrode intermediate layer is obtained by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the negative electrode intermediate layer. When multiple types of negative electrode active materials are used, the charge capacity density Х mass value is calculated for each negative electrode active material, and the sum of these values is the capacity of the negative electrode intermediate layer.Here, the charge capacity density of the positive and negative electrode materials is the capacity estimated using an all-solid-state half-cell using lithium metal as a counter electrode. The charge capacity of the positive electrode active material layer and the negative electrode intermediate layer is directly measured by measuring the charge capacity using the all-solid-state half-cell. The charge capacity density is obtained by dividing the measured charge capacity by the mass of each active material. Alternatively, the charge capacity of the positive electrode active material layer and the negative electrode intermediate layer may be the initial charge capacity measured at the first charge cycle.
[0114]
[0115] [Lithium battery]
[0116] According to one embodiment, a lithium battery includes a positive electrode; the above-described negative electrode; and an electrolyte disposed between the positive electrode and the negative electrode. For example, the negative electrode includes an electrodeposition-inducing layer including the above-described first carbon-based material. By including the above-described negative electrode, the lithium battery can simultaneously provide improved capacity and excellent lifespan characteristics. The lithium battery may be, but is not limited to, a lithium primary battery, a lithium secondary battery, a lithium-sulfur battery, a lithium-air battery, a lithium metal battery, a non-anode lithium metal battery, etc., and any lithium battery used in the art is possible.
[0117] Lithium batteries are manufactured by, for example, the following exemplary methods, but are not necessarily limited to these methods and are adjusted according to required conditions.
[0118] (cathode)
[0119] A cathode including an electrodeposition-inducing layer including the first carbon-based material described above is prepared.
[0120] (anode)
[0121] First, a positive electrode active material composition is prepared by mixing a positive electrode active material, a conductive agent, a binder, and a solvent. The prepared positive electrode active material composition is directly coated and dried on an aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon. Alternatively, the positive electrode active material composition is cast on a separate support, and then the film obtained by peeling from the support is laminated on the aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon.
[0122] The cathode active material is a lithium-containing metal oxide, and any one commonly used in the art can be used without limitation. For example, one or more types of composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof can be used, and specific examples thereof include Li a A 1-b B b D2 (in the above formula, 0.90 ≤ a ≤ 1, and 0 ≤ b ≤ 0.5); Li a E 1-b B b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B b O 4-c D c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li aNi 1-b-c Co b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a MnGb O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (wherein 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) A compound represented by any one of the chemical formulas Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used.
[0123] In the chemical formula representing the above-described compound, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. It is also possible to use a compound having a coating layer added to the surface of the above-described compound, or it is also possible to use a mixture of the above-described compound and the compound having a coating layer added. The coating layer added to the surface of the above-mentioned compound includes a coating element compound of, for example, an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element of the coating element. The compound forming the coating layer is amorphous or crystalline. The coating elements included in the coating layer are Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method for forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method includes, for example, spray coating and dipping. Since the specific coating method is well understood by those working in the relevant field, a detailed description thereof will be omitted.
[0124] The cathode active material is, for example, Li a Ni x Co y M z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0.8≤x<1, 0 <y≤0.3, 0<z≤0.3, 및 x+y+z=1이고, M은 망간(Mn), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), LiNi x Co y Mn z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Al z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Mn z Al w O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2, 0<w≤0.2, 및 x+y+z+w=1), Li a Co x M y O 2-b A b (1.0≤a≤1.2, 0≤b≤0.2, 0.9≤x≤1, 0≤y≤0.1, and x+y=1, M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, and A is F, S, Cl, Br or a combination thereof), Li a Ni x Mn y M' z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0 <x≤0.3, 0.5≤y<1, 0<z≤0.3, 및 x+y+z=1이고, M'는 코발트(Co), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), Li a M1 x M2 y PO 4-b X b (In the above chemical formula 7, 0.90 ≤a ≤1.1, 0≤x≤0.9, 0≤y≤0.5, 0.9 <x+y<1.1, 0≤b≤2 이며, M1이 크롬(Cr), 망간(Mn), 철(Fe), 코발트(Co), 니켈(Ni), 구리(Cu), 지르코늄(Zr) 또는 이들의 조합이며, M2가 마그네슘(Mg), 칼슘(Ca), 스트론튬(Sr), 바륨(Ba), 티탄(Ti), 아연(Zn), 보론(B), 니오븀(Nb), 갈륨(Ga), 인듐(In), 몰리브덴(Mo), 텅스텐(W), 알루미늄(Al), 실리콘(Si), 크롬(Cr), 바나듐(V), 스칸듐(Sc), 이트륨(Y) 또는 이들의 조합이며, X가 O, F, S, P 또는 이들의 조합), Li a M3 z PO4 (0.90≤a≤1.1, 0.9≤z≤1.1, and M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof).
[0125] The conductive material may include, but is not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. Any conductive material used in the relevant technical field may be used. Alternatively, the anode may not include a separate conductive material, for example.
[0126] As the binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the above polymers, styrene butadiene rubber polymer, etc. are used, and as the solvent, N-methylpyrrolidone (NMP), acetone, water, etc. are used, but are not necessarily limited to these, and any solvent used in the relevant technical field may be used.
[0127] It is also possible to form pores inside the electrode plate by further adding a plasticizer or a pore forming agent to the positive electrode active material composition.
[0128] The contents of the cathode active material, conductive agent, binder, and solvent used in the cathode are at levels typically used in lithium batteries. Depending on the intended use and configuration of the lithium battery, one or more of the conductive agent, binder, and solvent may be omitted.
[0129] The binder content included in the positive electrode may be 0.1 wt% to 10 wt% or 0.1 wt% to 5 wt% of the total weight of the positive electrode active material layer. The positive electrode active material content included in the positive electrode may be 80 wt% to 99 wt%, 90 wt% to 99 wt% or 95 wt% to 99 wt% of the total weight of the positive electrode active material layer.
[0130] (Separator)
[0131] Next, a separator to be inserted between the positive and negative electrodes is prepared.
[0132] Any separator commonly used in lithium batteries can be used. For example, a separator with low resistance to ion migration and excellent electrolyte absorption capacity is used. The separator may be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or combinations thereof, and may be in the form of a nonwoven or woven fabric. For lithium-ion batteries, a rollable separator, such as polyethylene or polypropylene, is used, while for lithium-ion polymer batteries, a separator with excellent organic electrolyte absorption capacity is used.
[0133] The separator is manufactured by the following exemplary methods, but is not limited to these methods and may be adjusted according to required conditions.
[0134] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated and dried on the electrode to form a separator. Alternatively, the separator composition is cast on a support and dried, and then a separator film peeled from the support is laminated on the electrode to form a separator.
[0135] The polymer used in separator manufacturing is not particularly limited; any polymer used as a binder for electrode plates can be used. Examples include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or mixtures thereof.
[0136] (electrolyte)
[0137] Next, the electrolyte is prepared.
[0138] The electrolyte may be, for example, a liquid electrolyte, a solid electrolyte, a gel electrolyte, or a combination thereof.
[0139] The electrolyte is, for example, an organic electrolyte. An organic electrolyte is prepared by dissolving a lithium salt in an organic solvent, for example.
[0140] Any organic solvent used in the relevant technical field may be used. Examples of the organic solvent include propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.
[0141] Lithium salts are all possible if they are used as lithium salts in the relevant technical field. Lithium salts include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(1≤x≤20, 1≤y≤20), LiCl, LiI or a mixture thereof. The concentration of the lithium salt is, for example, 0.1 M to 5.0 M.
[0142] The solid electrolyte is, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof.
[0143] Solid electrolytes are, for example, oxide-based solid electrolytes. Oxide-based solid electrolytes are Li 1+x+y Al x Ti 2-x Si y P 3-y O 12(0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(O≤x<1, O≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M = Te, Nb, or Zr, x is an integer from 1 to 10) is one or more selected from. The solid electrolyte is manufactured by a sintering method, etc. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M doped LLZO, M=Ga, W, Nb, Ta, or Al, 0≤x≤10, 0 <a<2) 중에서 선택된 가넷계(Garnet-type) 고체전해질이다.
[0144] The sulfide-based solid electrolyte may include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles may include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles may be Li2S or P2S5. Sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixing molar ratio of Li2S to P2S5 may be, for example, in a range of about 50:50 to about 90:10. In addition, Li3PO4, halogen, halogen compound, Li 2+2x Zn 1??x GeO4("LISICON", 0≤x<1), Li 3+y PO 4-x N x( "LIPON", 0 <x<4, 0<y<3), Li 3.25 Ge 0.25 P 0.75 S4("ThioLISICON"), Li2O-Al2O3-TiO2-P2O 5( An inorganic solid electrolyte prepared by adding "LATP") etc. to an inorganic solid electrolyte of Li2S-P2S5, SiS2, GeS2, B2S3, or a combination thereof can be used as a sulfide solid electrolyte. Non-limiting examples of sulfide solid electrolyte materials include Li2S-P2S5; Li2S-P2S5-LiX (X=halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S -P2S5-Z m S n(0 <m<10, 0<n<10, Z=Ge, Zn 또는 Ga); Li2S-GeS2; Li2S-SiS2-Li3PO4; 및 Li2S-SiS2-Li p FOR q (0 <p<10, 0<q<10, M=P, Si, Ge, B, Al, Ga 또는 In)을 포함한다. 이와 관련하여, 황화물계 고체전해질 재료는 황화물계 고체전해질 물질의 원료 시작 물질(예를 들면, Li2S, P2S5, 등)을 용융 담금질법(melt quenching method), 기계적 밀링법 등에 의해 처리함으로써 제조될 수 있다. 또한, 소성(calcinations) 공정이 상기 처리 후에 수행될 수 있다. 황화물계 고체전해질은 비정질이거나, 결정질이거나, 이들이 혼합된 상태일 수 있다.
[0145] A polymer solid electrolyte is an electrolyte that includes, for example, a mixture of a lithium salt and a polymer, or a polymer having an ion-conducting functional group. A polymer solid electrolyte is, for example, a polymer electrolyte that does not include a liquid electrolyte.Polymers included in the polymer solid electrolyte include, for example, polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyethylene oxide (PEO), poly(styrene-b-ethylene oxide) block copolymer (PS-PEO), poly(styrene-butadiene), poly(styrene-isoprene-styrene), poly(styrene-b-divinylbenzene) block copolymer, poly(styrene-ethylene oxide-styrene) block copolymer, polystyrene sulfonate (PSS), polyvinyl fluoride (PVF), polymethyl methacrylate (PMMA), poly(methylmethacrylate), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), polyacrylonitrile (PAN), Polyaniline, polyacetylene, Nafion, Aquivion, Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone sulfone) (SPAEKKS), sulfonated poly(aryl ether ketone) (SPAEK), poly[bis(benzimidazobenzisoquinolinones)] (SPBIBI), poly(styrene sulfonate) (PSS), lithium 9,10-Diphenylanthracene-2-sulfonate (lithium 9,10-diphenylanthracene-2-sulfonate, DPASLi. +) or a combination thereof, but is not limited thereto, and any polymer electrolyte used in the art may be used. The lithium salt may be any lithium salt that can be used in the art. The lithium salt may be, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(x and y are each 1 to 20), LiCl, LiI or a mixture thereof.
[0146] A gel electrolyte is, for example, a gel polymer electrolyte. A gel polymer electrolyte is, for example, an electrolyte that includes a liquid electrolyte and a polymer, or an organic solvent and a polymer having an ion-conducting functional group. The liquid electrolyte can be, for example, an ionic liquid, a mixture of a lithium salt and an organic solvent, a mixture of an ionic liquid and an organic solvent, or a mixture of a lithium salt, an ionic liquid, and an organic solvent. The polymer can be selected from the polymers used in solid polymer electrolytes. The organic solvent can be selected from the organic solvents used in liquid electrolytes. The lithium salt can be selected from the lithium salts used in solid polymer electrolytes. An ionic liquid refers to a salt that is liquid at room temperature or a room-temperature molten salt that has a melting point below room temperature and is composed only of ions. The ionic liquid may comprise at least one selected from compounds comprising, for example, a) at least one cation selected from ammonium, pyrrolidinium, pyridinium, pyrimidinium, imidazolium, piperidinium, pyrazolium, oxazolium, pyridazinium, phosphonium, sulfonium, triazolium, and mixtures thereof, and b) at least one anion selected from BF4-, PF6-, AsF6-, SbF6-, AlCl4-, HSO4-, ClO4-, CH3SO3-, CF3CO2-, Cl-, Br-, I-, BF4-, SO4-, CF3SO3-, (FSO2)2N-, (C2F5SO2)2N-, (C2F5SO2)(CF3SO2)N-, and (CF3SO2)2N-. A gel polymer electrolyte can be formed by impregnating a polymer solid electrolyte into an electrolyte solution within a lithium battery. The gel electrolyte may further include inorganic particles.
[0147]
[0148] (lithium battery)
[0149] Referring to FIG. 3, a lithium battery (1) according to an embodiment includes a positive electrode (3), the above-described negative electrode (2), and a separator (4). The positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An organic electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing the lithium battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.
[0150] Referring to FIG. 4, a lithium battery (1) according to one embodiment includes a positive electrode (3), the aforementioned negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2), and the positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, but may be, for example, a cylindrical shape, a thin film shape, etc.
[0151] Referring to FIG. 5, a lithium battery (1) according to an embodiment includes a positive electrode (3), the aforementioned negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2) to form a battery structure. A battery structure (7) is stacked in a bi-cell structure and then accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding a current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, and may be, for example, a cylindrical shape, a thin film shape, etc.
[0152] A pouch-type lithium metal battery corresponds to the lithium batteries of FIGS. 3 to 5, each of which uses a pouch as a battery case. The pouch-type lithium battery includes one or more battery structures. A separator is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are laminated in a bi-cell structure, then impregnated with an organic electrolyte, and accommodated and sealed in a pouch to complete the pouch-type lithium battery. For example, although not shown in the drawings, the above-described positive electrode, negative electrode, and separator may be simply laminated and accommodated in a pouch in the form of an electrode assembly, or may be wound or folded into a jelly-roll-shaped electrode assembly and then accommodated in a pouch. Subsequently, an organic electrolyte is injected into the pouch and sealed to complete the lithium battery.
[0153] The lithium battery of the present disclosure has excellent discharge capacity and lifespan characteristics, as well as high energy density, and is therefore used in, for example, electric vehicles (EVs). For example, it is used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). It is also used in applications requiring large amounts of power storage, such as electric bicycles and power tools.
[0154] Lithium batteries are stacked in multiple layers to form a battery module, and the multiple battery modules form a battery pack. Such a battery pack can be used in any device requiring high capacity and high output. For example, it can be used in laptops, smartphones, electric vehicles, etc. The battery module includes, for example, multiple batteries and a frame that holds them. The battery pack includes, for example, multiple battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. The multiple battery packs are controlled by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.
[0155]
[0156] A lithium battery containing a solid electrolyte is described in more detail below.
[0157] (all-solid-state lithium battery)
[0158] The lithium battery may be, for example, an all-solid-state lithium battery including a solid electrolyte. By including the above-described negative electrode, the all-solid-state lithium battery can simultaneously provide improved capacity and excellent lifespan characteristics.
[0159] All-solid-state lithium batteries are manufactured, for example, by the following exemplary methods, but are not necessarily limited to these methods and are adjusted according to required conditions.
[0160] Referring to FIGS. 6 and 7, the all-solid-state lithium battery (1) includes a positive electrode (10); the aforementioned negative electrode (20); and a solid electrolyte layer (30) disposed between the positive electrode (10) and the negative electrode (20). The solid electrolyte layer (30) includes, for example, an inorganic solid electrolyte. The solid electrolyte layer (30) includes, for example, a sulfide-based solid electrolyte or an oxide-based solid electrolyte.
[0161] (cathode)
[0162] A negative electrode containing the lithium metal or lithium alloy described above is prepared.
[0163] (anode)
[0164] Referring to FIGS. 6 and 7, the positive electrode (10) includes a positive electrode current collector (11) and a positive electrode active material layer (12) disposed on the positive electrode current collector. The positive electrode active material layer (12) includes a positive electrode active material. The positive electrode active material refers to the lithium battery section described above.
[0165] The positive electrode active material layer (12) may further include a solid electrolyte in addition to the positive electrode active material. The solid electrolyte included in the positive electrode (10) may be the same as or different from the solid electrolyte included in the solid electrolyte layer (30). For details on the solid electrolyte included in the positive electrode (10), refer to the solid electrolyte layer (30) section. The solid electrolyte used in the positive electrode active material layer (12) may have a smaller D50 average particle size than the solid electrolyte used in the solid electrolyte layer (30). For example, the D50 average particle size of the solid electrolyte used in the positive electrode active material layer (12) may be 90% or less, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, or 20% or less of the D50 average particle size of the solid electrolyte used in the solid electrolyte layer (30). The average D50 particle size of the solid electrolyte used in the positive electrode active material layer (12) may be, for example, 0.1 µm to 2 µm, 0.2 µm to 1.5 µm, or 0.3 µm to 1.0 µm. The content of the solid electrolyte included in the positive electrode active material layer (12) may be 1 to 15 wt%, 5 to 15 wt%, or 8.0 to 12.0 wt% of the total weight of the positive electrode active material layer (12).
[0166] The positive electrode active material layer (12) may include a binder. The binder may be, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., but is not necessarily limited thereto and may be any binder that can be used in the relevant technical field. The content of the binder included in the positive electrode active material layer (12) may be, for example, 0.1 to 5 wt%, 0.5 to 3 wt%, or 1.0 to 2.0 wt% of the total weight of the positive electrode active material layer (12).
[0167] The cathode active material layer (12) may include a conductive material. The conductive material may be, for example, a carbon-based conductive material or a metal-based conductive material. The conductive material is not necessarily limited to graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon tube, metal powder, etc., and any conductive material that can be used as a conductive material in the relevant technical field may be used. The content of the conductive material included in the cathode active material layer (12) may be, for example, 0.1 to 10 wt%, 0.5 to 5 wt%, or 1.0 to 4.0 wt% of the total weight of the cathode active material layer (12). In addition to the above-described cathode active material, solid electrolyte, binder, and conductive material, the cathode active material layer (12) may further include additives such as fillers, coating agents, dispersants, and ion conductive aids.
[0168] The positive electrode current collector (11) may be, for example, a plate or foil made of aluminum (Al), indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector (11) may be omitted. The positive electrode current collector (11) may further include a carbon layer disposed on one or both sides of the metal substrate. By additionally disposing the carbon layer on the metal substrate, the metal of the metal substrate is prevented from being corroded by the solid electrolyte included in the positive electrode layer, and the interface resistance between the positive electrode active material layer (12) and the positive electrode current collector (11) may be reduced. The thickness of the carbon layer may be, for example, 1 µm to 5 µm, 1 µm to 4 µm, or 1 µm to 3 µm. If the carbon layer is too thin, it may be difficult to completely block contact between the metal substrate and the solid electrolyte. If the carbon layer is too thick, the energy density of the all-solid-state secondary battery may decrease. The carbon layer may include amorphous carbon, crystalline carbon, etc. The thickness of the positive electrode current collector (11) including the metal substrate and optionally the carbon layer may be, for example, 10 ㎛ to 50 ㎛, 10 ㎛ to 40 ㎛, or 10 ㎛ to 30 ㎛, but is not necessarily limited to this range, and may be selected depending on the characteristics of the all-solid-state lithium battery required.
[0169] Although not shown in the drawing, the positive electrode (10) may further include a positive electrode current collector (11), a positive electrode active material layer (12) disposed on the positive electrode current collector, and an inactive member disposed on one side of the positive electrode active material layer. The area of the positive electrode active material layer (12) may be smaller than the area of the solid electrolyte layer (30) in contact with the positive electrode active material layer (12). The inactive member may be disposed to surround the side of the positive electrode active material layer (12) to correct an area error between the positive electrode active material layer (12) and the solid electrolyte layer (30). The inactive member is a member that does not contain an electrochemically active material, for example, an electrode active material. The electrode active material is a material that absorbs / releases lithium. The inactive member is a member made of a material other than the electrode active material and used in the relevant technical field. The inert member surrounds the side surface of the positive electrode active material layer (12) and can be in contact with the solid electrolyte layer (30). Since the inert member surrounds the side surface of the positive electrode active material layer (12) and is in contact with the solid electrolyte layer (30), cracks in the solid electrolyte layer (30) that occur due to a pressure difference during the pressing process in the solid electrolyte layer (30) that does not come into contact with the positive electrode active material layer (12) can be effectively suppressed. Since the area of the inert member compensates for the difference between the area of the positive electrode active material layer (12) and the area of the solid electrolyte layer (30), cracks in the solid electrolyte layer (30) that occur due to a pressure difference during the pressing process can be effectively suppressed. The inert member can be disposed between the positive electrode current collector (11) and the solid electrolyte layer (30) that face each other. The inert member can serve as a filler that fills the space between the positive electrode current collector (11) and the solid electrolyte layer (30) that face each other. The inert member may include at least one selected from a lithium ion insulator and a lithium ion conductor. The inert member may be an electronic insulator. That is, the inert member may not be an electronic conductor.The inert member may be an organic material, an inorganic material, or an organic-inorganic composite material. The organic material may be, for example, a polymer. The inorganic material may be, for example, a ceramic such as a metal oxide. The organic-inorganic composite material may be a composite of a polymer and a metal oxide. The inert member may include, for example, at least one selected from the group consisting of an insulating polymer, an ion-conducting polymer, an insulating inorganic material, an oxide-based solid electrolyte, and a sulfide-based solid electrolyte. The inert member may be, for example, an olefin-based polymer such as polypropylene (PP) or polyethylene (PE). The inert member (40) may be, for example, a gasket. The thickness of the inert member may be the same as or similar to the thickness of the positive electrode active material layer (12).
[0170] (solid electrolyte layer)
[0171] Referring to FIGS. 6 to 7, a solid electrolyte layer (30) is disposed between the positive electrode (10) and the negative electrode (20) and includes, for example, a sulfide-based solid electrolyte.
[0172] Sulfide-based solid electrolytes include, for example, Li2S-P2S5, Li2S-P2S5-LiX, where X is a halogen element, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n , m, n are positive numbers, Z is one of Ge, Zn or Ga, Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q , p, q are positive numbers, M is one of P, Si, Ge, B, Al, Ga In, Li 7-x PS 6-x Cl x , 0 ≤x ≤2, Li 7-x PS 6-xBr x , 0 ≤x ≤2, and Li 7-x PS 6-x I x , may include at least one selected from 0 ≤x ≤2. The sulfide-based solid electrolyte is manufactured by treating starting materials such as Li2S and P2S5 by a melting rapid cooling method or a mechanical milling method. In addition, heat treatment may be performed after the treatment. The solid electrolyte may be amorphous, crystalline, or a mixture thereof. In addition, the solid electrolyte may be, for example, a material including sulfur (S), phosphorus (P), and lithium (Li) as constituent elements among the above-described sulfide-based solid electrolyte materials. For example, the solid electrolyte may be a material including Li2S-P2S5. When using a material including Li2S-P2S5 as a sulfide-based solid electrolyte material forming the solid electrolyte, the mixing molar ratio of Li2S and P2S5 is, for example, in the range of Li2S: P2S5= 50:50 to 90:10.
[0173] The sulfide-based solid electrolyte may include, for example, an argyrodite type solid electrolyte represented by the following chemical formula 1:
[0174] <Chemical Formula 1>
[0175] Li + 12-n-x A n+ X 2- 6-x Y - x
[0176] In the above formula, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb or Ta, X is S, Se or Te, Y is Cl, Br, I, F, CN, OCN, SCN or N3, and 1 ≤n ≤5, 0 ≤x ≤2. The sulfide-based solid electrolyte is, for example, Li 7-x PS 6-x Clx , 0 ≤x ≤2, Li 7-x PS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-x I x , 0≤x≤2. The sulfide-based solid electrolyte may be, for example, an argyrodite-type compound including at least one selected from Li6PS5Cl, Li6PS5Br, and Li6PS5I. The density of the argyrodite-type solid electrolyte may be 1.5 to 2.0 g / cc. Since the argyrodite-type solid electrolyte has a density of 1.5 g / cc or more, the internal resistance of the all-solid-state secondary battery is reduced, and penetration of the solid electrolyte layer by Li can be effectively suppressed.
[0177] The elastic modulus, i.e., Young's modulus, of the sulfide-based solid electrolyte may be, for example, 35 GPa or less, 30 GPa or less, 27 GPa or less, 25 GPa or less, or 23 GPa or less. The elastic modulus, i.e., Young's modulus, of the sulfide-based solid electrolyte may be, for example, 10 to 35 GPa, 10 to 30 GPa, 10 to 27 GPa, 10 to 25 GPa, or 10 to 23 GPa. Since the sulfide-based solid electrolyte has an elastic modulus in this range, the temperature and / or pressure required for sintering, etc. is reduced, and thus sintering of the solid electrolyte can be performed more easily.
[0178] The average D50 particle size of the solid electrolyte used in the solid electrolyte layer (30) may be, for example, 1 μm to 10 μm, 1.5 μm to 7 μm, or 2 μm to 5 uμm.
[0179] The content of the sulfide-based solid electrolyte included in the solid electrolyte layer (30) may be, for example, 97 to 100 wt%, 98 to 99.9 wt%, or 98.5 to 99.0 wt% of the total weight of the solid electrolyte layer (30).
[0180] The solid electrolyte layer (30) may further include, for example, a binder. The binder included in the solid electrolyte layers (30, 30a, 30b) may be, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., but is not limited thereto, and any binder used in the relevant technical field may be used. The binder of the solid electrolyte layer (30) may be the same as or different from the binder included in the positive electrode active material layer (12) and the negative electrode active material layer (22).
[0181] The content of the binder included in the solid electrolyte layer (30) may be, for example, 0.1 to 3 wt%, 0.5 to 2 wt%, or 1.0 to 2.0 wt% of the total weight of the solid electrolyte layer (30).
[0182] Referring to FIGS. 6 and 7, the all-solid-state lithium battery (1) includes a solid electrolyte layer (30), a positive electrode layer (10) disposed on one surface of the solid electrolyte layer (30), and a negative electrode layer (20) disposed on the other surface of the solid electrolyte layer (30). The positive electrode layer (30) includes a positive electrode active material layer (12) in contact with the solid electrolyte layer (30) and a positive electrode current collector (11) in contact with the positive electrode active material layer (12), and the negative electrode layer (20) includes a negative electrode active material layer (22) in contact with the solid electrolyte layer (30) and a negative electrode current collector (21) in contact with the negative electrode active material layer (22). For example, an all-solid-state lithium battery (1) is formed by arranging a positive electrode active material layer (12) and a negative electrode active material layer (22) on both sides of a solid electrolyte layer (30), and arranging a positive electrode current collector (11) and a negative electrode current collector (21) on the positive electrode active material layer (12) and the negative electrode active material layer (22), respectively, to complete an all-solid-state lithium metal battery (30). Alternatively, an all-solid-state lithium metal battery (40) is formed by sequentially stacking a negative electrode active material layer (22), a solid electrolyte layer (30), a positive electrode active material layer (12), and a positive electrode current collector (11) on the negative electrode current collector (21).
[0183]
[0184] [Cathode manufacturing method]
[0185] According to another embodiment, a method for manufacturing an anode for a lithium metal battery comprises the steps of: providing an anode current collector; and providing an electrodeposition-inducing layer on the anode current collector, wherein the electrodeposition-inducing layer comprises a first carbon-based material having a nitrogen element content exceeding 1 wt% with respect to the total weight of the first carbon-based material. A lithium battery comprising an anode manufactured by this method provides improved cycle characteristics.
[0186] First, a negative electrode current collector is provided. The negative electrode current collector refers to the negative electrode portion described above. For example, copper foil is provided as the negative electrode current collector.
[0187] Next, an electrodeposition-inducing layer is provided on the negative electrode current collector. The electrodeposition-inducing layer can be provided, for example, by mixing the above-described first carbon-based material and a binder with a solvent to prepare a slurry, then coating the slurry on a metal substrate, and drying it. The electrodeposition-inducing layer can be provided, for example, by mixing the above-described first carbon-based material, the second carbon-based material, and a binder with a solvent to prepare a slurry, then coating the slurry on a metal substrate, and drying it.
[0188] The coating method is not particularly limited and can be coated using a doctor blade or the like. The slurry may include, for example, the first carbon-based material described above, a binder, and a solvent. The slurry may further include a second carbon-based material. The slurry may further include a metal oxide. The slurry may include, for example, the first carbon-based material, the second carbon-based material, a binder, and a solvent described above. The slurry may include, for example, the first carbon-based material, the metal oxide, the second carbon-based material, the binder, and the solvent. For the metal oxide, the second carbon-based material, and the binder, refer to the negative electrode section described above. The solvent may be an organic solvent. The solvent may be, for example, NMP, but is not necessarily limited thereto, and any solvent used in the relevant technical field may be used.
[0189] According to one embodiment, the first carbon-based material described above can be manufactured by carbonizing a polymer containing a nitrogen element. For example, the first carbon-based material described above can be manufactured directly by carbonizing sulfurized polyacrylonitrile (SPAN).
[0190] For example, a yellow-modified polyacrylonitrile can be manufactured by the following method. A mixed raw material comprising polyacrylonitrile powder and sulfur powder is heated. The mixed raw material can be mixed using a general mixing device such as a mixer, mortar, or ball mill. A simple mixture of sulfur and polyacrylonitrile can be used as the mixed raw material. Alternatively, the mixed raw material can be formed into pellets and used. The mixed raw material may consist solely of polyacrylonitrile and sulfur (S), or may further include general materials such as a conductive material applicable to the negative electrode.
[0191] By heating the mixed raw materials in the heat treatment process, sulfur (S) contained in the mixed raw materials is introduced into the structure of polyacrylonitrile. The heat treatment process can be performed in a closed system or an open system. In order to suppress the loss of sulfur (S) vapor, it can be performed in a closed system. The atmosphere of the heat treatment process can be an atmosphere that does not hinder the acceptance of sulfur (S) into polyacrylonitrile, such as an atmosphere that does not contain hydrogen and a non-oxidizing atmosphere. If hydrogen is present in the heat treatment atmosphere, sulfur (S) can be removed from the reaction system by reacting with hydrogen in the reaction system and converting to hydrogen sulfide. By heat treating in a non-oxidizing atmosphere, sulfur in a vapor state reacts with polyacrylonitrile simultaneously with the ring closure reaction of polyacrylonitrile, thereby obtaining sulfur-modified polyacrylonitrile (SPAN). A non-oxidizing atmosphere includes a reduced pressure state with a low oxygen concentration that does not allow oxidation to proceed, an inert gas atmosphere such as nitrogen or argon, a sulfur gas atmosphere, etc. In a sealed non-oxidizing atmosphere, for example, the mixed raw material can be placed in a container that maintains a seal that does not allow sulfur (S) vapor to be lost, and the inside of the container can be heated under a reduced pressure or inert gas atmosphere. Alternatively, the mixed raw material can be heated in a vacuum-packed state using a material such as an aluminum laminate film that is difficult to react with sulfur vapor. The heat treatment temperature of the mixed raw material in the heat treatment process can be a temperature at which sulfur can be introduced into polyacrylonitrile and the resulting yellowed polyacrylonitrile is not denatured. The heat treatment temperature can be 250 to 500°C, 250 to 400°C, or 250 to 300°C. The heat treatment temperature can be a temperature higher than the temperature at which sulfur (S) vaporizes. Vaporization refers to the phase change of sulfur from a liquid or solid to a gas, and can occur by boiling, evaporation, sublimation, etc. For example, the melting point of α-sulfur (S, tetragonal sulfur) is 112.8℃, the melting point of β-sulfur (S, monotonic sulfur) is 119.6℃, and the melting point of γ-sulfur (S, monotonic sulfur) is 106.8℃. The boiling point of sulfur (S) is 444.7℃. Since the vapor pressure of sulfur is high, if the temperature of the mixed raw material is 150℃ or higher, the generation of sulfur vapor can be confirmed with the naked eye. If the temperature of the mixed raw material is 150℃ or higher, reflux of sulfur is possible. When refluxing sulfur during the heat treatment process, a reflux device can be used. Even if the sulfur content in the mixed raw material is excessive, a sufficient amount of sulfur (S) can be introduced to polyacrylonitrile during the heat treatment process. When using an excessive amount of sulfur for polyacrylonitrile, the disadvantages caused by elemental sulfur can be prevented by removing elemental sulfur from the heat treatment result after the heat treatment process. The adverse effects can be suppressed. When the polyacrylonitrile and sulfur in the mixed raw materials are mixed in a weight ratio of 1:2 to 1:10, a sufficient amount of sulfur can be introduced into the polyacrylonitrile through a simple sulfur removal process in which the heat-treated result after the heat treatment process is heated at 200°C to 250°C under reduced pressure, while suppressing the adverse effects of the remaining simple sulfur. If the simple sulfur removal process is not performed on the heat-treated result after the heat treatment process, the heat-treated result can be used as a yellowed polyacrylonitrile as it is. If the simple sulfur removal process is performed on the heat-treated result after the heat treatment process, the heat-treated result after the simple sulfur removal process can be used as a yellowed polyacrylonitrile. The simple sulfur removal process can be, for example, 1 to 6 hours. When yellowed polyacrylonitrile is heated from room temperature to 900°C at a heating rate of 20°C / min, the mass loss determined by thermogravimetric analysis is less than 10% at 400°C. In contrast, when a mixture of sulfur powder and polyacrylonitrile powder is heated under the same conditions, the mass loss begins around 120°C, and when the temperature exceeds 200°C, a large mass loss occurs due to rapid loss of sulfur.Sulfur (S) in the yellow-modified polyacrylonitrile exists in a stable state combined with polyacrylonitrile, or exists as simple sulfur, but is trapped in the cross-linked structure when polyacrylonitrile is ring-closed by heating, and is thus in a state in which it is difficult to evaporate even when heated. The manufactured yellow-modified polyacrylonitrile may be in a powder state.
[0192] The first carbon-based material can be prepared by carbonizing the manufactured yellow-modified polyacrylonitrile. For example, the yellow-modified polyacrylonitrile can be carbonized by heating it at a temperature of 800°C or higher under nitrogen conditions for 2 to 6 hours. The first carbon-based material manufactured by carbonizing the yellow-modified polyacrylonitrile can be an amorphous carbon with a nitrogen element content exceeding 1 wt% based on the total weight of the first carbon-based material.
[0193]
[0194] The present invention is explained in more detail through the following examples and comparative examples. However, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.
[0195] Example 1: Cu-based / C-SPAN-containing electrodeposition-induced layer cathode
[0196] (Preparation of the first carbon material)
[0197] Sulfurized polyacrylonitrile (SPAN) having an average particle size (D50) of 0.1 ㎛ and a dark brown color was prepared by grinding and mixing sulfur powder and polyacrylonitrile powder and heat-treating at 350°C for 6 hours.
[0198] The above-mentioned yellow-modified polyacrylonitrile was carbonized in a nitrogen atmosphere at 850°C for 4 hours to prepare a black first carbon-based material (c-SPAN). The content of nitrogen atoms in the manufactured first carbon-based material was 12 wt% based on the total weight of the first carbon-based material.
[0199] (Cathode manufacturing)
[0200] A mixture was prepared by preparing 0.19 g of the first carbon-based material, 1.71 g of Denka Black as the second carbon-based material, and 0.033 g of polyvinylidene fluoride (PVDF) as the binder, and then dry mixing at 2,000 rpm for 5 minutes using a Thinky mixer. A slurry was prepared by adding a solvent (NMP) to the mixture. The slurry was coated on a copper current collector using a doctor blade, and dried in a vacuum oven at 80°C to prepare a negative electrode. The negative electrode had a structure in which a 10 ㎛ thick electrodeposition-inducing layer was coated on a copper current collector. The content of nitrogen element included in the electrodeposition-inducing layer, measured through XPS analysis, was 1.2 wt% with respect to the total weight of the electrodeposition-inducing layer.
[0201] (Polar electrode manufacturing)
[0202] LiCoO2 powder and carbon conductive material (Super-P; Timcal Ltd.) were uniformly mixed at a weight ratio of 90:5, and then a PVDF (polyvinylidene fluoride) binder solution was added to prepare a positive electrode active material slurry so that the weight ratio of active material:carbon conductive material:binder = 90:5:5.
[0203] The manufactured slurry was coated on a 15 ㎛ thick aluminum substrate using a doctor blade, dried under reduced pressure at 120°C, and rolled using a roll press to form a sheet to manufacture a positive electrode.
[0204] (Manufacturing of coin cells)
[0205] A polypropylene separator (Celgard 3510) was placed between the positive and negative electrodes manufactured above, and an electrolyte was injected to manufacture a coin cell.
[0206] As an electrolyte, a solution containing 1.15 M LiPF6 dissolved in EC (ethylene carbonate) + EMC (ethyl methyl carbonate) + DMC (dimethyl carbonate) (2:4:4 volume ratio) was used.
[0207]
[0208] Comparative Example 1: Cu-based / C-PAN-containing electrodeposition-induced layer cathode
[0209] A negative electrode and a coin cell were manufactured in the same manner as in Example 1, except that the first carbon-based material was prepared as a non-carbonized sulfurized polyacrylonitrile (SPAN). The nitrogen content contained in the sulfurized polyacrylonitrile (SPAN), which is the first carbon-based material, was 10 wt% based on the total weight of the sulfurized polyacrylonitrile (SPAN), and the nitrogen element content contained in the electrodeposition-inducing layer including the sulfurized polyacrylonitrile (SPAN) was 1 wt%.
[0210] Comparative Example 2: Cathode containing Cu substrate / Denka Black
[0211] A negative electrode and a coin cell were manufactured in the same manner as in Example 1, except that Denkablack was used as the first carbon-based material instead of carbonized yellow-modified polyacrylonitrile (c-SPAN), and an electrodeposition induction layer containing only Denkablack was manufactured.
[0212] Comparative Example 3: Cu-based cathode
[0213] A cathode and coin cell were manufactured in the same manner as in Example 1, except that the electrodeposition induction layer was not placed.
[0214]
[0215] Evaluation Example 1: SEM Measurement
[0216] Coin cells manufactured in Example 1 and Comparative Example 3 were charged under constant current at a current of 0.1 C rate at 25°C until the voltage reached 4.2 V (vs. Li), thereby forming a lithium electrodeposition layer on the electrodeposition-inducing layer. The negative electrodes according to Example 1 and Comparative Example 3 were observed by SEM when the lithium electrodeposition layer began to form on the electrodeposition-inducing layer and after the lithium electrodeposition layer was formed (@SOC 100).
[0217] Fig. 8a is an SEM image of the negative electrode when a lithium electrodeposition layer began to form on the electrodeposition-inducing layer according to Example 1. Fig. 8b is an SEM image of the negative electrode after a lithium electrodeposition layer was formed on the electrodeposition-inducing layer according to Example 1. Fig. 9a is an SEM image of the negative electrode when a lithium electrodeposition layer began to form on the electrodeposition-inducing layer according to Comparative Example 3. Fig. 9b is an SEM image of the negative electrode after a lithium electrodeposition layer was formed on the electrodeposition-inducing layer according to Comparative Example 3.
[0218] Referring to FIGS. 8a, 8b, 9a and 9b, Example 1 including an electrodeposition-inducing layer including a first carbon-based material has a lithium electrodeposition layer having a spherical shape including lithium metal, so that lithium ions are uniformly deposited on the electrodeposition-inducing layer compared to Comparative Example 3.
[0219] Accordingly, in the lithium battery according to Example 2, a lithium electrodeposition layer having a thickness of 25 μm was formed on the electrodeposition-inducing layer with a higher density than that of Comparative Example 5, in which the lithium electrodeposition layer had a thickness of 38 μm, while the remaining capacity was 100%.
[0220]
[0221] Evaluation Example 2: Nucleation overpotential and short circuit time measurements
[0222] Nucleation overpotential and short circuit time were measured for coin cells according to Example 1 and Comparative Examples 1 to 3. The coin cell is a half cell composed of a Cu foil counter electrode coated with Li metal and an electrodeposition induction layer, and measurements were made by repeating charge and discharge cycles.
[0223] The measurement results are shown in Table 1 below.
[0224] Anode current collector / Electrodeposition induction layer Nucleation overpotential (mV) Short circuit time (hr) Example 1 Cu substrate / C-SPAN+Denka black (1:9) 4799 Comparative example 1 Cu substrate / SPAN+Denka black (1:9) 5840 Comparative example 2 Cu substrate / Denka black (10) 6027 Comparative example 3 Cu substrate 5572
[0225] As shown in Table 1, the lithium battery of Example 1 had a reduced nucleation overpotential at which a lithium electrodeposition layer can be initially formed when lithium ions are deposited on the negative electrode, and an increased short circuit time, compared to the lithium batteries of Comparative Examples 1 to 3.
[0226] It was determined that the lithium battery of Example 1 included an electrodeposition-inducing layer with a nitrogen content satisfying a specific range, so that lithium was uniformly deposited and lithium ion conductivity characteristics were further improved.
[0227]
[0228] While exemplary embodiments have been described in detail with reference to the attached drawings, the present invention is not limited to these examples. It is self-evident that those skilled in the art to which the present invention pertains can devise various modifications or variations within the scope of the technical concepts described in the patent claims, and these also naturally fall within the technical scope of the present invention.
[0229] [Explanation of symbols]
[0230] 1 lithium battery 2, 20 cathode
[0231] 3, 10 positive electrode 4 separator
[0232] 5 Battery case 6 Cap assembly
[0233] 7 Battery structure 8 Electrode tab
[0234] 11. Anode current collector 12. Anode active material layer
[0235] 21 Negative current collector 22 Electrodeposition induction layer
[0236] 23 Lithium electrodeposition layer 30 Solid electrolyte layer
Claims
1. Negative current collector; and A cathode current collector is disposed on the electrodeposition induction layer, and includes a first carbon-based material; The above first carbon-based material is amorphous carbon containing a nitrogen element, A cathode in which the content of the nitrogen element exceeds 1 wt% with respect to the total weight of the electrodeposition-inducing layer.
2. In paragraph 1, A cathode in which the content of the nitrogen element is 1.1 wt% to 10 wt% based on the total weight of the electrodeposition-inducing layer.
3. In paragraph 1, The above first carbon-based material is a cathode, which is a carbide of a polymer containing a nitrogen element.
4. In paragraph 3, The polymer containing the above nitrogen element is a cathode including carbonized sulfurized polyacrylonitrile (c-SPAN).
5. In paragraph 1, The above first carbon-based material is an amorphous carbon that further contains a sulfur element, and is a cathode.
6. In paragraph 5, A cathode, wherein the content of sulfur element in the first carbon-based material is 0.1 to 50 wt%.
7. In paragraph 5, The above electrodeposition induction layer further comprises Li2S, the cathode.
8. In paragraph 1, A cathode, wherein the intensity ratio of the D peak to the G peak (Id / Ig) obtained by the Raman analysis spectrum of the first carbon-based material is 0.8 to 1.
5.
9. In paragraph 1, A cathode, wherein the average particle diameter of the first carbon-based material is 100 nm to 10 ㎛.
10. In paragraph 1, A cathode, wherein the above-mentioned electrodeposition-inducing layer further includes a second carbon-based material, and the second carbon-based material is a carbon-based conductive material.
11. In paragraph 10, A cathode, wherein the second carbon-based material comprises carbon black, denka black, ketjen black, carbon nanotubes, carbon nanofibers, carbon nanobelts, fullerenes, activated carbon, carbon fibers, or a combination thereof.
12. In paragraph 10, A cathode in which the content ratio of the first carbon-based material included in the electrodeposition-inducing layer to the content ratio of the second carbon-based material is 1:99 to 99:
1.
13. In paragraph 1, A cathode, wherein the above electrodeposition-inducing layer further comprises a binder.
14. In paragraph 13, The above binder is a cathode comprising a fluorine-based binder or an acrylic-based binder.
15. In paragraph 13, A negative electrode for a lithium metal battery, wherein the electrodeposition-inducing layer comprises 1 to 30 parts by weight of the binder based on 100 parts by weight of the first carbon-based material.
16. In paragraph 1, A cathode having a thickness of the above electrodeposition-inducing layer of 1 ㎛ to 50 ㎛.
17. In paragraph 1, A negative electrode further comprising a lithium electrodeposition layer disposed on the electrodeposition-inducing layer.
18. In paragraph 17, A negative electrode having a thickness of the lithium electrodeposition layer of 50㎛ or less.
19. Anode; a cathode according to any one of claims 1 to 18; and A lithium battery comprising an electrolyte disposed between the positive electrode and the negative electrode.
20. In paragraph 19, A lithium battery, wherein the electrolyte is a liquid electrolyte, a gel electrolyte, a solid electrolyte, or a combination thereof.
Citation Information
Patent Citations
Negative electrode and lithium ion battery and lithium ion battery
JP2019175864A
Method of manufacturing electrode active material of lithium secondary battery
KR1020130057804A
Negative current collector for all-solid-state battery and negative electrode for all-solid-state battery comprising same
WO2022055335A1