Olivine cathode active material for lithium secondary battery and manufacturing method thereof
The use of ferric oxide and lithium dihydrogen phosphate in a spray-drying process with a carbon coating addresses the complexities and costs of existing LFP production methods, enhancing the electrochemical performance and thermal stability of lithium iron phosphate positive electrode active materials for lithium secondary batteries.
Patent Information
- Application Number
- PCT/KR2024/004036
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-29
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
The existing methods for manufacturing lithium iron phosphate (LFP) positive electrode active materials for lithium secondary batteries are complex, generate toxic by-products, and result in high costs due to the use of certain iron raw materials, while also facing issues like pipe clogging and reduced productivity from recrystallization growth during the spraying process.
A method involving the use of ferric oxide as an iron raw material, lithium dihydrogen phosphate, and a spray-drying process with a slurry obtained by wet milling, where the LiH2PO4 is added to prevent pipe clogging and improve productivity, and a carbon coating is applied to enhance electronic conductivity and lithium diffusion.
This approach results in an LFP positive electrode active material with improved electrochemical performance, reduced process complications, and lower production costs, while maintaining excellent thermal stability and lifespan characteristics.
Smart Images

Figure KR2024004036_03102024_PF_FP_ABST
Abstract
Description
Olivine-based cathode active material for lithium secondary batteries and method for producing the same
[0001] The present invention relates to a method for producing an olivine-based positive electrode active material for a lithium secondary battery, an olivine-based positive electrode active material produced thereby, and a lithium secondary battery including the same.
[0002]
[0003] As the electric vehicle market gains momentum, the cathode active material market, which accounts for more than 40% of the cost of lithium-ion batteries, is also experiencing rapid annual growth. Automobiles are categorized into six tiers based on overall length: segment A for vehicles under 3,500 mm and segment F for those over 5,000 mm. Accordingly, even for battery-powered electric vehicles, cathode active materials are used differently depending on the grade and driving range.
[0004] For electric vehicles with a range exceeding 600 km on a single charge, high-energy-density lithium-ion batteries are required, necessitating the use of high-nickel NCM cathode active materials. For ranges around 400 km, mid-nickel NCM cathode active materials are used. However, for electric vehicles with lower ranges and relatively low prices, the use of materials with lower energy density but higher safety and longevity is advantageous from a cost perspective.
[0005] Lithium iron phosphate (LiIonP) is an olivine structure composed of FeO6 octahedral sites and PO4 tetrahedral sites, and is a material in which lithium ions are inserted and deintercalated through a one-dimensional pathway. This material is mainly composed of Li, Fe, and P, and has a price advantage due to the lower cost of metal minerals compared to NCA or NCM materials that mainly use Ni and Co. In addition, the strong PO bond makes the structure stable, so there is no oxygen dissociation at high temperatures during charging, and it has the advantage of excellent thermal stability. In addition, it has excellent life characteristics, and many electric vehicles using it have been produced in China.
[0006] However, since lithium ion insertion and de-insertion occurs by one-dimensional diffusion, the primary particles must be manufactured in nano size, and since the material itself has no electrical conductivity, a uniform carbon coating must be provided on the surface. Carbon can be coated on the surface of lithium iron phosphate particles and between particles. Carbon coated on the surface of lithium iron phosphate improves electronic conductivity, but has the problem of inhibiting lithium diffusion. Therefore, there is a need to develop carbon-coated lithium iron phosphate that can simultaneously improve electronic conductivity and lithium diffusion.
[0007] Lithium iron phosphate (LFP) is known to be manufactured by various methods, including hydrothermal synthesis using LiOH, FeSO4, and (NH4)3PO4; spray drying using Li2CO3 and FePO4 precursors; and milling of Li2CO3 and FePO4. However, these manufacturing methods have problems such as the generation of toxic byproducts such as ammonia, complicated post-treatment processes, and high unit prices of iron raw materials.
[0008] In order to solve the above problems, the applicant's patent application (KR10-2022-0182881) proposes a method for manufacturing an LFP cathode active material for lithium secondary batteries by using ferric oxide (Fe2O3), a by-product of the steel industry, as an iron raw material, and lithium dihydrogen phosphate (LiH2PO4) and wet milling the resulting slurry, which is then spray-dried. However, the above manufacturing method has a problem in that a large amount of dry material adheres to the wall of the device due to LiH2PO4 recrystallization growth during the spraying process, which clogs the pipes and reduces overall productivity.
[0009] Therefore, there is a need to develop a method for economically and efficiently manufacturing lithium iron phosphate (LFP) cathode active materials with excellent electrochemical performance without process problems.
[0010]
[0011] In one embodiment of the present invention, a method for manufacturing an olivine-based cathode active material having excellent output characteristics, a cathode active material manufactured therefrom, and a lithium secondary battery using the same are provided.
[0012]
[0013] An olivine-based positive electrode active material precursor according to one embodiment of the present invention is a precursor derived from a mixed raw material having an average particle diameter of 4.0 µm to 13.0 µm, including a lithium raw material, an iron raw material, and a phosphorus raw material, and can satisfy the following relational expression 1.
[0014] [Relationship 1]
[0015] 60.0 ≤ M LFP *D pc ≤ 85.0
[0016] (In the above relation 1, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and D pc is the crystal grain size (nm) of the precursor.)
[0017] The above precursor has a crystal grain size (D) obtained by XRD analysis.pc ) may be 75.0 nm to 95.0 nm.
[0018] The precursor may further comprise carbon in excess of 0.20 wt% based on the total weight.
[0019] The above precursor may have a phase fraction of lithium iron phosphate (LiFePO4) of 94.5% or more.
[0020] The precursor may have a phase fraction of lithium phosphate (Li3PO4) of 4.5% or less, a phase fraction of iron oxide (Fe2O3) of 3.5% or less, and a phase fraction of iron tetraoxide (Fe3O4) of 4.5% or less.
[0021] In one embodiment of the present invention, an olivine-based positive electrode active material for a lithium secondary battery includes a core portion containing lithium metal phosphate; and a carbon coating layer positioned on the surface of the core portion; and can satisfy the following relationship 2.
[0022] [Relationship 2]
[0023] 0.20 ≤ D50*Dc^2*C / 1000 ≤ 0.50
[0024] (In the above equation 2, D50 is the average particle size (㎛) of the olivine-based positive electrode active material, Dc is the crystal grain size (nm) in the olivine-based positive electrode active material, and C is the carbon weight percentage (%) in the olivine-based positive electrode active material.)
[0025] In one embodiment of the present invention, an olivine-based cathode active material for a lithium secondary battery is derived from the olivine-based cathode active material precursor,
[0026] The following relationship 3 can be satisfied.
[0027] [Relationship 3]
[0028] 1.00 ≤ M LFP *D50 ^2 ≤ 2.85
[0029] (In the above relational expression 3, M LFPis the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and D50 is the average particle size (㎛) of the olivine-based positive electrode active material.
[0030] In one embodiment of the present invention, an olivine-based positive electrode active material for a lithium secondary battery is derived from the olivine-based positive electrode active material precursor, and can satisfy the following relationship 4.
[0031] [Relationship 4]
[0032] 0.75 ≤ M LFP *C*100 / D50≤ 1.50
[0033] (In the above relational expression 4, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, D50 is the average particle size (㎛) of the olivine-based cathode active material, and C is the weight percentage (%) of carbon in the olivine-based cathode active material.
[0034] In one embodiment of the present invention, an olivine-based positive electrode active material for a lithium secondary battery is derived from the olivine-based positive electrode active material precursor, and can satisfy the following relationship 5.
[0035] [Relationship 5]
[0036] 17.0 ≤ M LFP * D50*C / Dc*10^5≤ 30.0
[0037] (In the above relation 5, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, D50 is the average particle size (㎛) of the olivine-based cathode active material, C is the carbon weight percentage (%) in the olivine-based cathode active material, and Dc is the crystal grain size (nm) in the olivine-based cathode active material.
[0038] In one embodiment of the present invention, an olivine-based positive electrode active material for a lithium secondary battery is derived from the olivine-based positive electrode active material precursor, and can satisfy the following relationship 6.
[0039] [Relationship 6]
[0040] 12.0 ≤ M LFP^2*C*1000≤ 29.0
[0041] (In the above relational expression 6, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and C is the weight percentage (%) of carbon in the olivine-based cathode active material.
[0042] The above positive electrode active material may have a crystal grain size (Dc) of 90.0 nm to 130.0 nm obtained by XRD analysis.
[0043] The above positive electrode active material may have a carbon content of 0.45 wt% to 3.0 wt% based on the total weight.
[0044] The above positive electrode active material may have an average particle diameter (D50) of 1.0 to 10.0 μm.
[0045] The above positive electrode active material can be represented by the following chemical formula 1.
[0046] [Chemical Formula 1]
[0047] Li x (Fe y M 1-y )PO4
[0048] (In the above chemical formula 1,
[0049] 0.95≤x≤1.1, 0.9≤y≤1, 0.95≤x / y≤1.1,
[0050] M is at least one selected from the group consisting of Mn, Co, Ni, Cu, Zn, Mg, Cr, V, Mo, Ti, Al, Nb, B, W, and Ga.)
[0051] According to another embodiment of the present invention, a method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery includes the steps of: mixing and calcining a lithium raw material, an iron raw material, and a phosphorus raw material to manufacture a precursor including lithium iron phosphate (LiFePO4); mixing and milling the precursor, a carbon additive, a dispersant, and a solvent to manufacture a slurry; spray-drying the slurry to obtain a spray-dried product; calcining the spray-dried product in a reducing atmosphere to obtain a calcined product; and pulverizing and separating the calcined product to obtain a final olivine-based positive electrode active material, and can satisfy the following relational expression 7.
[0052] [Relationship 7]
[0053] 21.5 ≤ M LFP *D50_s ≤ 25.5
[0054] (In the above relational expression 7, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and D50_s is the average particle size (㎛) of the spray-dried product.
[0055] The method for manufacturing the above olivine-based positive electrode active material for a lithium secondary battery can satisfy the following relationship 8.
[0056] [Relationship 8]
[0057] 2.20 ≤ M LFP * D50_c*Dc_c / 1000≤ 2.90
[0058] (In the above relational expression 8, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, D50_c is the average particle size (㎛) of the sintered product, and Dc_c is the crystal grain size (nm) in the sintered product.)
[0059] The method for manufacturing the above olivine-based positive electrode active material for a lithium secondary battery can satisfy the following relationship 9.
[0060] [Relationship 9]
[0061] 0.28 ≤ M LFP^2*C_c*D50_c ≤ 0.50
[0062] (In the above relational expression 9, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, C_c is the weight percentage (%) of carbon in the sintered product, and D50_c is the average particle size (㎛) of the sintered product.
[0063] The method for manufacturing the above olivine-based positive electrode active material for a lithium secondary battery can satisfy the following relationship 3.
[0064] [Relationship 3]
[0065] 1.00 ≤ M LFP *D50 ^2 ≤ 2.85
[0066] (In the above relational expression 3, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and D50 is the average particle size (㎛) of the olivine-based positive electrode active material.
[0067] The method for manufacturing the above olivine-based positive electrode active material for a lithium secondary battery can satisfy the following relationship 4.
[0068] [Relationship 4]
[0069] 0.75 ≤ M LFP *C*100 / D50≤ 1.50
[0070] (In the above relational expression 4, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, D50 is the average particle size (㎛) of the olivine-based cathode active material, and C is the weight percentage (%) of carbon in the olivine-based cathode active material.
[0071] The method for manufacturing the above olivine-based positive electrode active material for a lithium secondary battery can satisfy the following relationship 5.
[0072] [Relationship 5]
[0073] 17.0 ≤ M LFP * D50*C / Dc*10^5≤ 30.0
[0074] (In the above relation 5, M LFPis the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, D50 is the average particle size (㎛) of the olivine-based cathode active material, C is the carbon weight percentage (%) in the olivine-based cathode active material, and Dc is the crystal grain size (nm) in the olivine-based cathode active material.
[0075] The method for manufacturing the above olivine-based positive electrode active material for a lithium secondary battery can satisfy the following relationship 6.
[0076] [Relationship 6]
[0077] 12.0 ≤ M LFP ^2*C*1000≤ 29.0
[0078] (In the above relational expression 6, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and C is the weight percentage (%) of carbon in the olivine-based cathode active material.
[0079] In the step of manufacturing a precursor including lithium iron phosphate (LiFePO4) by mixing and calcining a lithium raw material, an iron raw material, and a phosphorus raw material, the phase fraction of lithium iron phosphate (LiFePO4) in the manufactured precursor may be 94.5% or more.
[0080] In the step of preparing a slurry by mixing and milling the above precursor, carbon additive, dispersant, and solvent, the average particle diameter of the solid material in the slurry may be 0.9 ㎛ to 1.20 ㎛.
[0081] The crystal grain size (Dc_c) of the fired product obtained in the step of firing the spray-dried product in a reducing atmosphere to obtain a fired product may be 90.0 nm to 130 nm, and the average particle diameter (D50_c) of the fired product may be 22.0 μm to 24.0 μm.
[0082] In the step of spray-drying the above slurry to obtain a spray-dried product, the average particle diameter of the spray-dried product may be 24.0 μm to 26.0 μm.
[0083] In the step of crushing and separating the above-mentioned sintered material to obtain a final olivine-based positive electrode active material, the average particle diameter (D50) of the separated final olivine-based positive electrode active material may be 1.0 µm to 10.0 µm.
[0084] The above iron raw material is ferric oxide (Fe2O3), and the average particle size (D50) of the ferric oxide (Fe2O3) may be in the range of 0.1 ㎛ to 2.6 ㎛ and the maximum particle size (Dmax) may be 10 ㎛ or less.
[0085] The above lithium raw material and phosphorus raw material are lithium dihydrogen phosphate (LiH2PO4), and the average particle size (D50) of the lithium dihydrogen phosphate (LiH2PO4) may be in the range of 1 µm to 100 µm.
[0086] In the step of mixing and calcining the above lithium raw material, iron raw material, and phosphorus raw material to manufacture a precursor including lithium iron phosphate (LiFePO4), when mixing the lithium raw material, iron raw material, and phosphorus raw material, the following mixing relationship can be satisfied.
[0087] [Mixed Relationship]
[0088] (Diameter of container (cm)*PI*2 < R(RPM) < (Diameter of container (cm)*PI*10
[0089] (Here PI is the circumference constant.)
[0090] According to another embodiment of the present invention, a positive electrode for a lithium secondary battery may include a current collector; and a positive electrode active material layer positioned on at least one surface of the current collector and including an olivine-based positive electrode active material for a lithium secondary battery.
[0091] A lithium secondary battery according to another embodiment of the present invention may include the positive electrode.
[0092]
[0093] According to the present invention, there is an advantage in that an olivine-based positive electrode active material having excellent discharge characteristics and charge / discharge efficiency can be manufactured.
[0094]
[0095] Figure 1 shows the results of particle size analysis of the raw material Fe2O3 according to Example 1.
[0096] Figure 2 shows the results of particle size analysis of the raw material Fe2O3 according to Example 2 and Comparative Example 1.
[0097] Figure 3 shows the results of particle size analysis of the raw material Fe2O3 according to Example 3.
[0098] Figure 4 shows the results of particle size analysis of the raw material Fe2O3 according to Comparative Example 2.
[0099]
[0100] In this specification, the terms first, second, and third, etc. are used to describe various parts, components, regions, layers, and / or sections, but are not limited thereto. These terms are used only to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, a first part, component, region, layer, or section described below may be referred to as a second part, component, region, layer, or section without departing from the scope of the present invention.
[0101] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the present invention. As used herein, the singular forms "singular" and "comprising" include plural forms as well, unless the context clearly dictates otherwise. The word "comprising" as used herein specifies a particular feature, region, integer, step, operation, element, and / or component, but does not exclude the presence or addition of other features, regions, integers, steps, operations, elements, and / or components.
[0102] When a part is referred to as being "on" or "over" another part, it can be directly on or over the other part, or there may be other parts intervening. Conversely, when a part is referred to as being "directly on" another part, there are no other parts intervening.
[0103] Although not defined otherwise, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by those of ordinary skill in the technical field to which the present invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with the relevant technical literature and the present disclosure, and are not to be construed as ideal or overly formal unless otherwise defined.
[0104] In this specification, the term "combination(s) thereof" described in the expression in the Makushi format means one or more mixtures or combinations selected from the group consisting of the components described in the expression in the Makushi format, and means including any one or more selected from the group consisting of said components.
[0105] In this specification, the positive electrode active material or compound may be in the form of a secondary particle formed by agglomeration of a plurality of primary particles, and the term “primary particle” means the smallest particle unit that can be distinguished as a single lump when observing the cross-section of the positive electrode active material through a scanning electron microscope (SEM), and may be formed of a single crystal grain or a plurality of crystal grains.
[0106] In this specification, “crystal grain” means a distinct region in which atoms within a primary particle form a lattice structure with a certain direction.
[0107] In this specification, the average particle diameter (D50) of the positive electrode active material, etc., was measured using a conventional PSA (Particle size analysis) that measures the particle diameter of a particle material, and a detailed description thereof is omitted.
[0108] In this specification, the crystal grain size can be calculated by the following Scherrer equation (Equation 1).
[0109] τ=(K*λ) / (β*coaθ) (1)
[0110] In the above equation 1, K is a shape factor, λ is an x-ray wavelength, β is a full width at half maximum, and θ is a Bragg angle. In the present invention, the shape factor is generally 1.0, and may vary depending on the crystallite.
[0111]
[0112] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.
[0113]
[0114] 1. Olivine-based cathode active material precursor
[0115] An olivine-based positive electrode active material precursor for a lithium secondary battery according to one embodiment of the present invention is a precursor derived from a mixed raw material having an average particle diameter of 4.0 µm to 13.0 µm, including a lithium raw material, an iron raw material, and a phosphorus raw material, and can satisfy the following relational expression 1.
[0116] [Relationship 1]
[0117] 60.0 ≤ M LFP *D pc ≤ 85.0
[0118] (In the above relation 1, M LFPis the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and D pc is the crystal grain size (nm) of the precursor.)
[0119] The calculated value of the above relational expression 1 may be 60.0 to 85.0, and specifically, may be 70.0 to 85.0.
[0120] If the calculated value of relational expression 1 satisfies the above range, Fe 2+ The fraction of Fe is improved, thereby preventing loss of Fe due to magnetic separation during the wet milling process, and thus enabling the production of a crystal structure with an accurate composition of the olivine-based positive electrode active material, which is desirable because it can improve the charge / discharge capacity characteristics of a lithium secondary battery using the same.
[0121]
[0122] An olivine-based positive electrode active material precursor for a lithium secondary battery according to one embodiment of the present invention may include lithium iron phosphate (LiFePO4), and the phase fraction of lithium iron phosphate (LiFePO4) in the precursor may be 94.5% or more.
[0123] An olivine-based cathode active material precursor according to one embodiment of the present invention may further include carbon. The carbon content may exceed 0.20 wt%, and specifically, may be 0.25 wt% or more, based on the total weight of the precursor.
[0124] When the carbon content in the positive electrode active material precursor satisfies the above range, it is preferable because it can improve the electronic conductivity of the positive electrode active material.
[0125] An olivine-based positive electrode active material precursor according to one embodiment of the present invention may include lithium phosphate (Li3PO4), and the fraction of lithium phosphate (Li3PO4) in the precursor may be 4.5% or less, specifically 4.0% or less, or 3.5% or less.
[0126] An olivine-based positive electrode active material precursor according to one embodiment of the present invention may include iron oxide (Fe2O3), and the fraction of iron oxide (Fe2O3) in the precursor may be 3.5% or less, and specifically, 3.0% or less, 2.5% or less, or 2.0% or less.
[0127] An olivine-based positive electrode active material precursor according to one embodiment of the present invention may include iron tetroxide (Fe3O4), and the fraction of iron tetroxide (Fe3O4) in the precursor may be 3.5% or less, and specifically, 3.0% or less, 2.5% or less, or 2.0% or less.
[0128] When the phase fractions of lithium iron phosphate (LiFePO4), lithium phosphate (Li3PO4), iron oxide (Fe2O3), and iron tetroxide (Fe3O4) in the positive electrode active material precursor satisfy the above range, the impurity content in the final olivine-based positive electrode active material is reduced, and carbon is more effectively diffused and coated on the surface and / or inside of the positive electrode active material particles, thereby improving the electrochemical characteristics of a battery to which it is applied.
[0129] In this specification, the phase fractions of each composition can be obtained from XRD Rietveld structural analysis, such as the fractions of LFP, Fe2O3, Fe3O4, and Li3PO4 phases.
[0130]
[0131] 2. Olivine-based cathode active material
[0132] An olivine-based positive electrode active material for a lithium secondary battery according to another embodiment of the present invention may include a core portion; and a carbon coating layer positioned on the surface of the core portion.
[0133] The above core portion may contain lithium metal phosphate.
[0134] An olivine-based positive electrode active material for a lithium secondary battery according to another embodiment of the present invention can satisfy the following relationship 2.
[0135] [Relationship 2]
[0136] 0.20 ≤ D50*Dc^2*C / 1000 ≤ 0.50
[0137] In the above equation 2, D50 is the average particle size (㎛) of the olivine-based positive electrode active material, Dc is the crystal grain size (nm) in the olivine-based positive electrode active material, and C is the carbon weight percentage (%) in the olivine-based positive electrode active material.
[0138] In the above relational expression 2, the calculated value of D50*Dc^2*C / 1000 can be 0.20 to 0.50, and specifically, 0.25 to 0.40, 0.26 to 0.37.
[0139]
[0140] When the olivine-based positive electrode active material satisfies the above relational expression 2, the carbon content and crystal grain size can be controlled simultaneously to obtain excellent electronic conductivity and lithium ion transfer speed, and the average particle size of the positive electrode active material can be controlled to improve the specific surface area of the positive electrode active material and the density of the positive electrode active material layer, thereby improving the charge / discharge performance of the battery using the positive electrode active material, which is desirable.
[0141]
[0142] The average particle diameter (D50) of the above olivine-based positive electrode active material may be 1.0 to 10.0 μm, and specifically, 1.0 to 2.0 μm. When the average particle diameter of the olivine-based positive electrode active material satisfies the above range, it is preferable because the discharge capacity of the battery can be improved.
[0143] The crystal grain size (Dc) of the above olivine-based positive electrode active material may be 90.0 nm to 130.0 nm, and specifically, 100.0 nm to 130.0 nm, 100.0 nm to 120.0 nm, or 105.0 nm to 115.0 nm. When the crystal grain size (Dc) of the olivine-based positive electrode active material satisfies the above range, the charge / discharge characteristics of a lithium secondary battery to which it is applied can be improved, which is preferable.
[0144] The olivine-based positive electrode active material may contain 0.45 wt% to 3.0 wt% of carbon based on the total weight, and specifically, 1.0 wt% to 2.5 wt%. When the olivine-based positive electrode active material contains carbon within the above range, it is preferable because it improves electronic conductivity and simultaneously prevents a decrease in lithium ion movement speed, thereby improving the charge / discharge capacity characteristics of a lithium secondary battery to which it is applied.
[0145] The above olivine-based positive electrode active material may be a secondary particle formed by agglomerating a plurality of primary particles.
[0146] When the average particle diameter (D50) of the olivine-based positive electrode active material satisfies the above range, it is preferable because the charge / discharge capacity characteristics of a lithium secondary battery to which it is applied can be improved.
[0147]
[0148] A carbon coating layer may be formed between the primary particles, but is not limited thereto. However, it is preferable when the carbon coating layer is formed between the primary particles because it is advantageous for improving the charge and discharge capacity of a lithium secondary battery.
[0149] The above carbon content was measured using a high-precision carbon / sulfur analyzer. Specifically, the content of carbon oxide and sulfur generated by burning the sample in an oxygen stream with a combustible agent was detected, and the content was measured for 100 parts by weight of the entire olivine-based positive electrode active material for lithium secondary batteries.
[0150]
[0151] An olivine-based positive electrode active material according to another embodiment of the present invention may be derived from the above-described olivine-based positive electrode active material precursor (hereinafter referred to as precursor).
[0152] The above olivine-based positive electrode active material can satisfy the following relationship 3.
[0153] [Relationship 3]
[0154] 1.00 ≤ MLFP *D50 ^2 ≤ 2.85
[0155] In the above relation 3, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and D50 is the average particle diameter (㎛) of the final olivine-based cathode active material.
[0156] Meanwhile, in the above relational expression 3, M LFP *D50 ^2 The calculated value may be from 1.00 to 2.85, specifically from 2.00 to 2.85, and from 2.10 to 2.80.
[0157] When the above relational expression 3 is satisfied, it is possible to form a crystal structure with an accurate composition of an olivine-based positive electrode active material, and it is preferable to improve the charge / discharge capacity characteristics of a lithium secondary battery using the same.
[0158]
[0159] The above olivine-based positive electrode active material can satisfy the following relationship 4.
[0160] [Relationship 4]
[0161] 0.75 ≤ M LFP *C*100 / D50≤ 1.50
[0162] In the above relational expression 4, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, D50 is the average particle diameter (㎛) of the olivine-based cathode active material, and C is the carbon weight percentage (%) of the final olivine-based cathode active material.
[0163]
[0164] Meanwhile, in the above relational expression 4, M LFP The calculated value of *C*100 / D50 can be between 0.75 and 1.50, and specifically between 0.80 and 1.40.
[0165] When the above relational expression 4 is satisfied, it is possible to form a crystal structure of the exact composition of the olivine-based positive electrode active material, and a carbon coating of excellent quality is formed, thereby improving electronic conductivity and preventing a decrease in lithium ion movement speed, thereby improving the charge / discharge characteristics of a lithium secondary battery using the same, which is preferable.
[0166]
[0167] The above olivine-based positive electrode active material can satisfy the following relationship 5.
[0168] [Relationship 5]
[0169] 17.0 ≤ M LFP * D50*C / Dc*10^5≤ 30.0
[0170] In the above relation 5, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, D50 is the average particle size (㎛) of the olivine-based cathode active material, C is the carbon weight percentage (%) in the olivine-based cathode active material, and Dc is the crystal grain size (nm) in the olivine-based cathode active material.
[0171] Meanwhile, in the above relational expression 5, M LFP * The calculated value of D50*C / Dc*100 can be 17.0 to 30.0, and specifically 20.0 to 30.0.
[0172] When the above relational expression 5 is satisfied, it is possible to form a crystal structure of the exact composition of the olivine-based positive electrode active material, and a carbon coating of excellent quality is formed, thereby improving electronic conductivity and preventing a decrease in lithium ion movement speed, thereby improving the charge / discharge characteristics of a lithium secondary battery to which it is applied, which is preferable.
[0173]
[0174] The above olivine-based positive electrode active material can satisfy the following relationship 6.
[0175] [Relationship 6]
[0176] 12.0 ≤ M LFP^2*C*1000≤ 29.0
[0177] In the above relation 6, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and C is the weight percentage (%) of carbon in the olivine-based cathode active material.
[0178] Meanwhile, in the above relational expression 6, M LFP The calculated value of ^2*C*1000 can be between 12.0 and 29.0, specifically between 12.0 and 25.0, and between 13.0 and 20.0.
[0179] When the above relational expression 6 is satisfied, the formation of a crystal structure with an accurate composition of the olivine-based positive electrode active material is possible, and Fe 3+ It is desirable to improve the quality of carbon coating by reducing the amount of carbon used in carbon thermal reduction, and to form a high-quality carbon coating, thereby improving electronic conductivity, thereby improving the charge / discharge characteristics of lithium secondary batteries to which it is applied.
[0180]
[0181] The olivine-based positive electrode active material according to the present invention can be represented by the following chemical formula 1.
[0182] [Chemical Formula 1]
[0183] Li x (Fe y M 1-y )PO4
[0184] In the above chemical formula 1, 0.95≤x≤1.1, 0.9≤y≤1.0, 0.95≤x / y≤1.15, and M is at least one selected from the group consisting of Mn, Co, Ni, Cu, Zn, Mg, Cr, V, Mo, Ti, Al, Nb, B, W, and Ga.
[0185]
[0186] 3. Manufacturing method of olivine-based positive electrode active material
[0187] A method for manufacturing an olivine-based positive electrode active material precursor for a lithium secondary battery according to one embodiment of the present invention may include the steps of: mixing and firing a lithium raw material, an iron raw material, and a phosphorus raw material to manufacture a precursor including lithium iron phosphate (LiFePO4); mixing and milling the precursor, a carbon additive, a dispersant, and a solvent to manufacture a slurry; spray-drying the slurry to obtain a spray-dried product; and firing the spray-dried product in a reducing atmosphere to obtain an olivine-based positive electrode active material having a carbon coating layer formed thereon.
[0188] 3.1 Preparation of olivine-based cathode active material precursor
[0189] The step of mixing and calcining the above lithium raw material, iron raw material, and phosphorus raw material to produce a precursor including lithium iron phosphate (LiFePO4) may include the step of mixing and milling lithium dihydrogen phosphate (LiH2PO4), ferric oxide (Fe2O3), and a carbon-containing dispersant to obtain a mixture; and the step of calcining the mixture in a reducing atmosphere to obtain a precursor including lithium iron phosphate (LiFePO4).
[0190] First, a step of obtaining a mixture by mixing and milling lithium dihydrogen phosphate (LiH2PO4), ferric oxide (Fe2O3), and a carbon-containing dispersant is performed.
[0191] The above lithium dihydrogen phosphate (LiH2PO4) can be obtained by reacting lithium phosphate (Li3PO4), which is generated in an intermediate step of lithium carbonate or lithium hydroxide used in the production of cathode materials for lithium-ion batteries from salt lakes and ore lithium, with a phosphoric acid (H3PO4) solution. The above ferric oxide (Fe2O3) can be recovered and used from steel pickling wastewater, thereby reducing or suppressing the generation of wastewater, thereby producing an olivine-based cathode active material in an environmentally friendly manner. The above lithium dihydrogen phosphate (LiH2PO4) may have an average particle diameter (D50) in the range of 1 μm to 100 μm, specifically in the range of 30 μm to 100 μm, and more specifically in the range of 45 μm to 100 μm.
[0192] The above iron (II) oxide (Fe2O3) may be a powder having a maximum particle size (Dmax) of 10㎛ or less, and an average particle diameter (D50) of 0.1㎛ to 2.6㎛.
[0193] The above lithium dihydrogen phosphate (LiH2PO4) has a melting point of about 100°C, and is liquefied under heating conditions, and the iron (Fe2O3) oxide reaction proceeds. If the size of the iron (Fe2O3) oxide particles is large or the size difference between the lithium dihydrogen phosphate (LiH2PO4) particle size and the iron (Fe2O3) oxide particle size is large, the degree of uniform mixing with lithium dihydrogen phosphate (LiH2PO4) is reduced. Accordingly, during reduction calcination, it is difficult for the Li ions and PO4 ions of the liquefied LiH2PO4 to penetrate into the iron (Fe2O3) oxide particles, so that a large amount of impurity phase is formed, which causes a deterioration in the quality of the olivine-based cathode active material.
[0194] Therefore, the maximum particle size (Dmax), average particle diameter (D50) of the above iron oxide (Fe2O3) and lithium dihydrogen phosphate (LiH2PO4) are advantageous in reducing the impurity content and manufacturing an olivine-based positive electrode active material with excellent quality when the average particle diameter (D50) satisfies the above range.
[0195] The mass percentage of the solid organic material relative to the total mass of lithium dihydrogen phosphate (LiH2PO4) and iron (Fe2O3) may be in the range of 1 wt% to 10 wt%.
[0196] The carbon-containing dispersant may be a carbon-containing organic compound, and specifically, may be at least one selected from citric acid, fumaric acid, adipic acid, succinic acid, tartaric acid, glutarinc acid, maleic acid, oxalic acid, malonic acid, or ascorbic acid.
[0197] More specifically, the carbon-containing dispersant may be citric acid.
[0198] The above carbon-containing dispersant can prevent agglomeration between particles and also form a carbon coating layer on the surface of the product particles.
[0199] The above lithium dihydrogen phosphate (LiH2PO4), ferric oxide (Fe2O3), and carbon-containing dispersant can be introduced into a grinding device and mixed and milled. Specifically, the above lithium dihydrogen phosphate (LiH2PO4), ferric oxide (Fe2O3), and organic compound can be introduced into a grinding device and milled while being mixed.
[0200] In the present invention, the grinding device may be a grinding device such as an air jet mill, a hammer, a screen mill, a fine impact mill, a ball mill, or a vibrator mill, and specifically, may be a fine impact mill.
[0201] The mixing speed (R) of the above lithium dihydrogen phosphate (LiH2PO4), ferric oxide (Fe2O3), and dispersant can satisfy the following mixing relationship.
[0202] [Mixed Relationship]
[0203] (Diameter of container (cm)*PI*2 < R(RPM) < (Diameter of container (cm)*PI*10
[0204] Meanwhile, the mixing speed (R) is the rotation speed per minute, and mixing is advantageous in a range that satisfies the above relationship depending on the diameter of the container.
[0205] When the mixing speed satisfies the above mixing relationship, uniform grinding and mixing of the mixture can be achieved.
[0206] The above-described fin impact mill device can rotate two fin disks in the same or opposite direction at 4,000 RPM to 10,000 RPM, and specifically at 8,000 RPM to 10,000 RPM. Meanwhile, an inert gas can be continuously supplied into the inside of the fin impact mill device to form a reducing atmosphere inside the fin impact mill device.
[0207] Specifically, it can be performed in an inert gas atmosphere or a reducing gas atmosphere. The inert gas atmosphere or reducing gas atmosphere can be performed while continuously supplying at least one gas selected from high-purity nitrogen gas, high-purity argon (100%) gas, a mixture of hydrogen and nitrogen gas, a mixture of hydrogen and argon gas, or coke oven gas. When dry mixing milling is performed in the above atmosphere, it is advantageous in improving the quality of the olivine-based positive electrode active material by preventing unnecessary reactions and agglomeration of materials during the reaction process of the raw materials.
[0208] A step of mixing and milling lithium dihydrogen phosphate (LiH2PO4), ferric oxide (Fe2O3), and a carbon-containing dispersant and calcining the mixture obtained in a reducing atmosphere is performed to obtain a precursor containing lithium iron phosphate (LiFePO4).
[0209] Specifically, the process can be performed by loading the mixture into a kiln and continuously supplying an inert gas atmosphere or a reducing gas. The inert gas or reducing gas can be supplied in a volume of 3.8% to 40% of the kiln volume per minute. The inert gas or reducing gas is omitted here as it has been previously described.
[0210] Meanwhile, by heating the kiln at a heating rate ranging from 2.5°C / min to 10°C / min, the temperature inside the kiln can be raised to a temperature of 350°C or higher, specifically, to a temperature ranging from 350°C to 650°C. In addition, the temperature can be maintained in the above temperature range for 1 hour to 8 hours, specifically, by maintaining the temperature for 4 hours to 7 hours, a precursor containing lithium iron phosphate can be obtained.
[0211] If calcination is performed at a temperature below the above temperature range or for a time shorter than the above calcination time range, the olivine structure may not be properly formed. Furthermore, if calcination is performed at a temperature higher than the above temperature range or for a time longer than the above calcination time range, the problem of over-calcination and reduced activity of the positive electrode active material may occur.
[0212] Meanwhile, a step of grinding the precursor obtained above may be additionally performed. This is advantageous in improving the quality of the olivine-based positive electrode active material ultimately obtained by preparing a uniformly dispersed slurry in the wet mixing milling step described below.
[0213]
[0214] After performing a step of calcining the above mixture in a reducing atmosphere to obtain a precursor, a step of pulverizing the obtained precursor to obtain a precursor powder may be additionally performed. Meanwhile, the obtained precursor powder may be separated into a lithium iron phosphate compound powder having a maximum particle size (Dmax) of 45 ㎛ or less and an average particle size (D50) of 4.0 ㎛ to 13.0 ㎛ using a 325 mesh or 400 mesh sieve.
[0215] The crystal grain size of the precursor may be 75.0 nm to 95 nm, specifically 75.0 nm to 90 nm, 75.0 nm to 85 nm. Since the crystal grain size of the precursor satisfies the above range, the crystal grain size of the finally manufactured olivine-based positive electrode active material is controlled to the target range of the present invention, thereby improving the discharge capacity of a lithium secondary battery using the same, which is preferable.
[0216] The characteristics of the precursor have been explained in detail above, so a duplicate explanation will be omitted here.
[0217]
[0218] 3.2 Manufacturing of olivine-based cathode active materials
[0219] (Slurry manufacturing)
[0220] A step of preparing a slurry by mixing and milling the above precursor, carbon additive, dispersant, and solvent can be performed.
[0221] The total mass percentage of the carbon additive and dispersant relative to the total mass of the precursor, carbon additive and dispersant may be greater than 1 wt% and less than 15 wt%, and specifically may be in the range of 5 wt% to 12 wt%.
[0222] Meanwhile, the mass ratio of the carbon additive to the mass of the dispersant may be greater than 1 and less than 17, and specifically may be in the range of 4 to 16.
[0223] The above carbon additive can form a carbon coating layer and can penetrate into the inside of the positive electrode active material. The above carbon additive can be at least one selected from glucose, sucrose, fructose, lactose, and maltose, and more specifically, glucose can be used.
[0224] The amount of the carbon additive mixed is not particularly limited as long as it can produce an olivine-based positive electrode active material with excellent output of the present invention.
[0225] The above dispersant may be at least one selected from citric acid, fumaric acid, adipic acid, succinic acid, tartaric acid, glutarinc acid, maleic acid, oxailic acid, malonic acid, or ascorbic acid.
[0226] The above dispersant may specifically be citric acid.
[0227] The solvent may be ethanol, water, distilled water or deionized water. Specifically, it may be deionized water (DIW).
[0228] Meanwhile, additionally, one or more selected from among Mn, Co, Ni, Cu, Zn, Mg, Cr, V, Mo, Ti, Al, Nb, B, W, or Ga may be mixed.
[0229]
[0230] The above precursor, dispersant, and carbon additive can be introduced into a solvent-loaded bead mill milling device, mixed, and then milled for 30 minutes to 1 hour using a wet milling method to prepare a slurry. Wet milling can be performed by introducing zirconium beads (ZrO2 beads) having an average diameter ranging from 0.1 mm to 0.5 mm into a reactor in an amount similar to the mass of the solid material. Here, the solid material refers to the precursor, dispersant, and carbon additive. At this time, the milling linear speed of the milling pin can be in the range of 7 m / s to 14 m / s, and the wet bead milling can be performed at a circulation speed of 200 mL / min so that the internal slurry continuously moves into and out of the reactor.
[0231] The above precursor, dispersant, carbon additive, and solvent are continuously fed into the bead mill device, and can be continuously fed at a volume of 20% to 50% of the volume of the bead mill device per minute. By performing wet milling under the above conditions, the entire process is advantageously carried out stably and continuously.
[0232] The average particle diameter of the solid material in the slurry manufactured through the above wet milling may be 0.9 µm to 1.20 µm, specifically 1.0 µm to 1.10 µm. When the average particle diameter of the solid material in the slurry satisfies the above range, the primary particle and crystal grain size of the material obtained in the subsequent spray drying process can be controlled to the range targeted by the present invention, thereby producing an olivine-based positive electrode active material capable of ultimately improving the discharge capacity of the battery, which is preferable.
[0233] (Spray drying)
[0234] Next, a step of spray drying the slurry to obtain a spray dried product is performed.
[0235] The above spray drying can be performed by spraying the slurry into a spray dryer. The spray dryer can be a nozzle-type atomizer spray dryer or a disk rotary atomizer spray dryer.
[0236] When using a disk rotary atomizer spray dryer, the slurry can be supplied at an input speed equivalent to the evaporation amount standard of the atomizer dryer while spraying the slurry into the spray dryer at a disk rotation speed of 15,000 RPM to 30,000 RPM. At this time, the hot air inlet temperature of the spray dryer can be maintained in the range of 150 to 400°C, and the outlet temperature can be maintained in the range of 80 to 150°C.
[0237] When using a nozzle-type atomizer spray dryer, the air pressure supplied to the spray nozzle can range from 0.15 MPa to 0.3 MPa. The slurry is supplied at an input rate equivalent to the evaporation rate standard of the nozzle-type atomizer dryer. At this time, spray drying can be performed while maintaining the hot air inlet temperature of the spray dryer in the range of 150 to 400°C and the outlet temperature in the range of 80 to 150°C.
[0238] In one embodiment of the present invention, in the step of spray-drying the slurry to obtain a spray-dried product, the average particle diameter (D50_s) of the spray-dried product may be 24.0 μm to 26.0 μm, specifically 24.0 μm to 25.5 μm. When the average particle diameter of the spray-dried product satisfies the above range, it is preferable because it is possible to control the particle diameter range of the positive electrode active material targeted in the present invention in the post-sintering process, and it is easy to control the target particle diameter through the jet mill process, and ultimately, it is possible to manufacture an olivine-based positive electrode active material capable of improving the discharge capacity of a battery.
[0239] The above spray-dried product can satisfy the following relationship 7.
[0240] [Relationship 7]
[0241] 21.5 ≤ M LFP *D50_s ≤ 25.5
[0242] In the above relational expression 7, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and D50_s is the average particle diameter (㎛) of the spray-dried product.
[0243] Meanwhile, in the above relational expression 7, M LFP *The calculated value of D50 can be between 21.5 and 25.5, and specifically between 23.0 and 25.0.
[0244] If the above relation 7 is satisfied, Fe 2+ The fraction is improved to prevent loss of Fe due to magnetic separation during a wet milling process, thereby enabling the production of a crystal structure with an accurate composition of the olivine-based positive electrode active material, and improving the charge / discharge capacity characteristics of a lithium secondary battery using the same, which is desirable.
[0245]
[0246] (Firing)
[0247] Next, a step of calcining the spray-dried product in a reducing atmosphere to obtain an olivine-based positive electrode active material having a carbon coating layer formed thereon is performed.
[0248] The spray-dried product obtained through the above spray-drying process can be loaded into a kiln and then calcined while continuously supplying reducing gas or inert gas.
[0249] Specifically, after the above spray-dried product is loaded into a kiln, an inert gas atmosphere or a reducing gas is continuously supplied, so that the process can be performed in a reducing atmosphere. Here, the inert gas or reducing gas is omitted as it has been previously explained.
[0250] Meanwhile, the inert gas or reducing gas can be continuously supplied at a volume range of 3.8% to 40% per minute based on the volume inside the sintering furnace in which the positive electrode active material precursor material is loaded, thereby performing sintering.
[0251] Meanwhile, by heating the kiln at a heating rate ranging from 1°C / min to 10°C / min, the temperature inside the kiln can be raised to a temperature of 500°C or higher, specifically, to a temperature ranging from 500°C to 700°C. In addition, the temperature can be maintained in the above temperature range for 1 hour to 12 hours, specifically, for 4 hours to 7 hours to obtain a sintered product.
[0252] If calcination is performed at a temperature below the above temperature range or for a time shorter than the above calcination time range, the olivine structure may not be properly formed. Furthermore, if calcination is performed at a temperature higher than the above temperature range or for a time longer than the above calcination time range, the problem of over-calcination and reduced activity of the positive electrode active material may occur.
[0253] In one embodiment of the present invention, the average particle diameter (D50_c) of the sintered material may be 22.0 µm to 24.0 µm, and specifically, 22.2 µm to 23.8 µm.
[0254] The crystal grain size (Dc_c) of the above-mentioned product may be 90.0 nm to 130.0 nm, and specifically, 100.0 nm to 130.0 nm, 100.0 nm to 120.0 nm, or 105.0 nm to 115.0 nm.
[0255] The above-mentioned sintered material may contain 0.45 wt% to 3.0 wt% of carbon (C_c) based on the total weight, and specifically, 1.0 wt% to 2.5 wt%.
[0256] The above-mentioned material can satisfy the following relationship 8.
[0257] [Relationship 8]
[0258] 2.20 ≤ M LFP * D50_c*Dc_c / 1000≤ 2.90
[0259] In the above relational expression 8, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, D50_c is the average particle diameter (㎛) of the sintered product, and Dc_c is the crystal grain size (nm) in the sintered product.
[0260] Meanwhile, in the above relational expression 8, M LFP The calculated value of *D50*Dc_c / 1000 can be between 2.20 and 2.90, and specifically between 2.30 and 2.60.
[0261] If the above relation 8 is satisfied, Fe 2+ The fraction of Fe is improved, thereby preventing loss of Fe due to magnetic separation during a wet milling process, and thus enabling the production of a crystal structure with an accurate composition of the sintered product, i.e., an olivine-based positive electrode active material, and improving the charge / discharge capacity characteristics of a lithium secondary battery using the same, which is desirable.
[0262] The above-mentioned material can satisfy the following relationship 9.
[0263] [Relationship 9]
[0264] 0.28 ≤ M LFP ^2*C_c*D50_c ≤ 0.50
[0265] In the above equation 9, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, C_c is the weight percentage (%) of carbon in the sintered product, and D50_c is the average particle diameter (㎛) of the sintered product.
[0266] Meanwhile, in the above relational expression 9, M LFP The calculated value of ^2*C_c* D50_c can be between 0.28 and 0.50, and specifically between 0.29 and 0.47.
[0267] If the above relation 9 is satisfied, Fe 2+The fraction of Fe is improved to prevent loss of Fe due to magnetic separation during the wet milling process, thereby enabling the production of the sintered product, i.e., the olivine-based positive electrode active material, with a crystal structure of the exact composition, and Fe 3+ It is desirable to improve the quality of the carbon coating by reducing the amount of carbon used in the carbon thermal reduction, improve electronic conductivity, and prevent the reduction of the lithium ion movement speed, thereby improving the charge / discharge characteristics of the lithium secondary battery to which it is applied.
[0268] A step of calcining the above mixture in a reducing atmosphere to obtain an olivine-based positive electrode active material having a carbon coating layer formed thereon is performed, and then the obtained olivine-based positive electrode active material having a carbon coating layer formed thereon is pulverized using a jet mill or the like, and then sieved to finally manufacture an olivine-based positive electrode active material having a controlled particle size. The calcined material can be pulverized using a jet mill by operating it at a separator condition of 8,000 RPM to 15,000 RPM and spraying air at a pressure of 4.5 to 6.0 bar, specifically 5.0 to 5.3 bar.
[0269] The average particle diameter (D50) of the finally manufactured olivine-based positive electrode active material may be 1.0 to 10.0 μm, and specifically, 1.0 to 5.0 μm, 1.0 to 2.0 μm, or 1.0 to 1.8 μm.
[0270] The crystal grain size (Dc) of the above olivine-based positive electrode active material may be 90.0 nm to 130.0 nm, and specifically, 100.0 nm to 130.0 nm, 100.0 nm to 120.0 nm, or 105.0 nm to 115.0 nm.
[0271] The above olivine-based positive electrode active material may contain 0.45 wt% to 3.0 wt% of carbon (C) based on the total weight, and specifically, 1.0 wt% to 2.5 wt%.
[0272] The above-mentioned final manufactured olivine-based positive electrode active material can satisfy the following relationship 3.
[0273] [Relationship 3]
[0274] 1.00 ≤ M LFP *D50 ^2 ≤ 2.85
[0275] In the above relation 3, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and D50 is the average particle diameter (㎛) of the final olivine-based cathode active material.
[0276] Meanwhile, in the above relational expression 3, M LFP *D50 ^2 The calculated value may be from 1.00 to 2.85, specifically from 2.00 to 2.85, and from 2.10 to 2.80.
[0277] If the above relation 3 is satisfied, Fe 2+ The fraction is improved to prevent loss of Fe due to magnetic separation during a wet milling process, thereby enabling the production of a crystal structure with an accurate composition of the olivine-based positive electrode active material, and improving the charge / discharge capacity characteristics of a lithium secondary battery using the same, which is desirable.
[0278]
[0279] The above-mentioned final manufactured olivine-based positive electrode active material can satisfy the following relationship 4.
[0280] [Relationship 4]
[0281] 0.75 ≤ M LFP *C*100 / D50≤ 1.50
[0282] In the above relational expression 4, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, D50 is the average particle diameter (㎛) of the olivine-based cathode active material, and C is the carbon weight percentage (%) of the final olivine-based cathode active material.
[0283]
[0284] Meanwhile, in the above relational expression 4, MLFP The calculated value of *C*100 / D50 can be between 0.75 and 1.50, and specifically between 0.80 and 1.40.
[0285] If the above relation 4 is satisfied, Fe 2+ The fraction of Fe is improved to prevent loss of Fe due to magnetic separation during the wet milling process, thereby enabling the production of the crystal structure of the olivine-based positive electrode active material with an accurate composition, and Fe 3+ It is desirable to improve the quality of carbon coating by reducing the amount of carbon used in carbon thermal reduction, improve electronic conductivity, and prevent a decrease in lithium ion movement speed, thereby improving the charge / discharge characteristics of lithium secondary batteries to which it is applied.
[0286]
[0287] The above-mentioned final manufactured olivine-based positive electrode active material can satisfy the following relationship 5.
[0288] 17.0 ≤ M LFP * D50*C / Dc*10^5≤ 30.0
[0289] In the above relation 5, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, D50 is the average particle size (㎛) of the olivine-based cathode active material, C is the carbon weight percentage (%) in the olivine-based cathode active material, and Dc is the crystal grain size (nm) in the olivine-based cathode active material.
[0290] Meanwhile, in the above relational expression 5, M LFP * The calculated value of D50*C / Dc*100 can be 17.0 to 30.0, and specifically 20.0 to 30.0.
[0291] If the above relation 5 is satisfied, Fe 2+ The fraction of Fe is improved to prevent loss of Fe due to magnetic separation during the wet milling process, thereby enabling the production of the crystal structure of the olivine-based positive electrode active material with an accurate composition, and Fe 3+It is desirable to improve the quality of carbon coating by reducing the amount of carbon used in carbon thermal reduction, improve electronic conductivity, and prevent a decrease in lithium ion movement speed, thereby improving the charge / discharge characteristics of lithium secondary batteries to which it is applied.
[0292]
[0293] The above-mentioned final manufactured olivine-based positive electrode active material can satisfy the following relationship 6.
[0294] [Relationship 6]
[0295] 12.0 ≤ M LFP ^2*C*1000≤ 29.0
[0296] In the above relation 6, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and C is the weight percentage (%) of carbon in the olivine-based cathode active material.
[0297] Meanwhile, in the above relational expression 6, M LFP The calculated value of ^2*C*1000 can be between 12.0 and 29.0, specifically between 13.0 and 20.0.
[0298] If the above relation 6 is satisfied, Fe 2+ The fraction of Fe is improved to prevent loss of Fe due to magnetic separation during the wet milling process, thereby enabling the production of the crystal structure of the olivine-based positive electrode active material with an accurate composition, and Fe 3+ It is desirable to improve the quality of carbon coating by reducing the amount of carbon used in carbon thermal reduction, improve electronic conductivity, and prevent a decrease in lithium ion movement speed, thereby improving the charge / discharge characteristics of lithium secondary batteries to which it is applied.
[0299]
[0300] 4. Bipolar
[0301] In another embodiment of the present invention, a positive electrode is provided, which includes a current collector and a positive electrode active material layer positioned on at least one surface of the current collector and manufactured according to the method for manufacturing an olivine-based positive electrode active material described above.
[0302] The characteristics of the positive electrode active material constituting the positive electrode active material layer are the same as described above. Therefore, a detailed description of the positive electrode active material will be omitted.
[0303] The above-mentioned current collector may be selected from the group consisting of, for example, aluminum foil, nickel foil, stainless steel foil, titanium foil, nickel foam, aluminum foam, a polymer substrate coated with a conductive metal, and combinations thereof.
[0304] Meanwhile, the positive electrode active material layer may include a binder and a conductive material.
[0305] At this time, the binder plays a role of improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one kind alone or a mixture of two or more kinds thereof may be used, but is not limited thereto. The binder may be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.
[0306] And, the conductive material is used to provide conductivity to the electrode, and in the battery to be constructed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One type alone or a mixture of two or more types among these may be used, but the present invention is not limited thereto. The conductive material may typically be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.
[0307] The above positive electrode can be manufactured according to a conventional positive electrode manufacturing method, except that the above positive electrode active material is used.
[0308] Specifically, the positive electrode can be manufactured by applying a composition for forming a positive electrode active material layer, including the positive electrode active material described above and optionally a binder, a conductive agent, or a solvent, on a positive electrode current collector, followed by drying and rolling. At this time, the types and contents of the positive electrode active material, binder, and conductive agent are as described above.
[0309] The solvent may be a solvent generally used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the positive electrode.
[0310] Alternatively, the positive electrode may be manufactured by casting the composition for forming the positive electrode active material layer on a separate support, and then laminating the resulting film on a positive electrode current collector by peeling it off from the support.
[0311] The structure and manufacturing method of the positive electrode are not limited in the present invention.
[0312]
[0313] 5. Lithium secondary battery
[0314] In another embodiment of the present invention, a lithium secondary battery including the positive electrode is provided.
[0315] The lithium secondary battery may specifically include a positive electrode, a negative electrode positioned opposite the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, wherein the positive electrode is as described above. In addition, the lithium secondary battery may optionally further include a battery container that houses an electrode assembly including the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.
[0316] In the above lithium secondary battery, the negative electrode may include a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.
[0317] The negative electrode current collector may be selected from the group consisting of, for example, copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.
[0318] The negative electrode active material layer may optionally include a binder and a conductive material together with the negative electrode active material. As an example, the negative electrode active material layer may be manufactured by applying a composition for forming a negative electrode active material layer comprising the negative electrode active material and optionally a binder and a conductive material onto a negative electrode current collector and drying the composition, or by casting the negative electrode forming composition onto a separate support and then laminating the resulting film onto a negative electrode current collector by peeling the film off from the support.
[0319] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples thereof include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, and Al alloy; metallic oxides capable of doping and dedoping lithium, such as SiOβ (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical, or fiber-like forms, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes.
[0320] The above binder and conductive material may be the same as those described above for the positive electrode.
[0321] Next, depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. Such separators may include polyethylene, polypropylene, polyvinylidene fluoride, or multilayer films of two or more layers thereof, and mixed multilayer films such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator may also be used.
[0322] In addition, in the lithium secondary battery, examples of the electrolyte include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.
[0323] Specifically, the organic liquid electrolyte may include an organic solvent and a lithium salt.
[0324] The organic solvent may be used without any particular limitation as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; Carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (wherein R is a C2 to C20 linear, branched, or cyclic hydrocarbon group, and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, a carbonate solvent is preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery and a linear carbonate compound having low viscosity (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate, etc.) is more preferable.In this case, the performance of the electrolyte may be improved when the cyclic carbonate and the chain carbonate are mixed and used in a volume ratio of about 1:1 to about 1:9.
[0325] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2. LiCl, LiI, or LiB(C2O4)2. It is preferable that the concentration of the lithium salt be used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.
[0326] The structure and manufacturing method of the battery are not limited in the present invention.
[0327] As described above, a lithium secondary battery including a cathode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention, and is therefore useful in portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0328] Hereinafter, embodiments of the present invention will be described in more detail through examples. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited to the following examples.
[0329]
[0330] (Manufacture of positive electrode active material: Examples 1 to 5 and Comparative Examples 1 to 4)
[0331] (Raw material mixing) Lithium dihydrogen phosphate (LiH2PO4) powder, iron (Fe2O3) powder, and a dispersant were placed in a mixing milling device, and dry mixing milled to obtain mixed raw material powder. The iron (Fe2O3) oxide was recycled from steel pickling wastewater.
[0332] (Precursor manufacturing) After the above mixed raw material powders are charged into a high-temperature kiln, they are heated to 650℃ at a heating rate of 5℃ / min while supplying nitrogen gas in the range of 0.1L / min to 300L / min, maintained for 6 hours, and then naturally cooled to room temperature. The cooled material is pulverized using a milling machine, and a lithium iron phosphate-containing precursor powder can be separated through dry processing with the maximum particle size (Dmax) and average particle diameter (D50) controlled using a sieve.
[0333] (Slurry preparation) The separated precursor powder containing lithium iron phosphate having an average particle size (D50) of 45㎛ or less, citric acid, glucose, and deionized water are introduced into a bead mill. Zirconium beads (ZrO2 beads) having an average diameter ranging from 0.1 mm to 0.5 mm are introduced into the bead mill, and milled at a milling linear speed of 7 m / s to 14 m / s to prepare a slurry. At this time, the materials are introduced into the bead mill to account for 20% to 50% of the internal volume of the bead mill.
[0334] (Spray drying) The slurry was sprayed into a spray dryer using a disk atomizer while rotating the disk at 15,000 RPM to 30,000 RPM, and the spray dryer inlet temperature was set to 150°C to 400°C and the outlet temperature was set to 80°C to 150°C, thereby producing an olivine-based positive electrode active material.
[0335] (Reduction firing) 30 g of the powder obtained by the above spray drying was placed in an alumina saga, and firing was performed for 5 hours under conditions of maintaining 650°C in a nitrogen atmosphere to produce a fired product.
[0336] (crushing and separation)
[0337] The above-mentioned sintered material was pulverized using a jet mill operating at 12,000 RPM under separator conditions and spraying air at a pressure of 5.3 bar, and finally, a carbon-coated olivine-based positive electrode active material was manufactured.
[0338]
[0339] Table 1 below summarizes the mixed mass and mixed mass percentage of lithium dihydrogen phosphate (LiH2PO4), ferric oxide (Fe2O3), and carbon-containing dispersant (citric acid) according to Examples 1 to 5 and Comparative Examples 1 to 4, the average particle size (D50) of lithium dihydrogen phosphate (LiH2PO4), ferric oxide (Fe2O3), and the average particle size (D50) of the lithium iron phosphate compound obtained by grinding and sieving the lithium iron phosphate compound obtained after reduction and calcination. Here, the average particle size (D50) of the lithium iron phosphate compound obtained by sieving was controlled by varying the mesh size of the sieve.
[0340] Raw Material WeightRaw Material Weight PercentRaw Material Average Particle Size (D50)Raw Material D50 Ratio (LiH2PO4: Fe2O3)Mixed Raw Material Average Particle Size (D50)LiH2PO4Fe2O3Citric AcidLiH2PO4Fe2O3Citric AcidLiH2PO4Fe2O3(g)(g)(wt%)(wt%)(wt%)(um)(um)(㎛)Example 1681.96515.7511052.10%39.40%8.40%450.80564.03Example 2681.96515.7511052.10%39.40%8.40%910.801148.92Example 3681.96515.7511052.10%39.40%8.40%1002.543912.02Example 4681.96515.7511052.10%39.40%8.40%911.03888.92Example 5681.96515.7511052.10%39.40%8.40%911.038812.02Comparative Example 1681.96515.7511052.10%39.40%8.40%910.109102.02Comparative Example 2681.96515.7511052.10%39.40%8.40%3002.9010335.15Comparative Example 3681.96515.7511052.10%39.40%8.40%911.03888.92Comparative Example 4681.96515.7511052.10%39.40%8.40%911.03888.92
[0341] Referring to Table 1 above, Examples 1 to 5 and Comparative Examples 3 to 4 showed that the average particle size (D50) of the raw material, ferric oxide (Fe2O3), was in the range of 0.1 ㎛ to 2.6 ㎛, and the average particle size (D50) of the lithium iron phosphate compound finally obtained through dry mixing milling and reduction firing was in the range of 4.0 ㎛ to 13.0 ㎛. In the case of Comparative Example 1, the average particle size (D50) of the raw material, ferric oxide (Fe2O3), was 0.8 ㎛, but the average particle size (D50) of the lithium iron phosphate compound finally obtained through dry mixing milling and reduction firing was 2.02 ㎛, which was smaller than the range of 4.0 ㎛ to 13.0 ㎛. In addition, in the case of Comparative Example 2, the average particle size (D50) of the raw material, ferric oxide (Fe2O3), was 2.9 ㎛, exceeding the range of 0.1 ㎛ to 2.6 ㎛, and the average particle size (D50) of the lithium iron phosphate compound finally obtained through dry mixing milling and reduction firing was 151.45 ㎛, which was larger than the range of 4.0 ㎛ to 13.0 ㎛.
[0342] FIG. 1 shows the results of particle size analysis of raw material Fe2O3 according to Example 1, FIG. 2 shows the results of particle size analysis of raw material Fe2O3 according to Example 2 and Comparative Example 1, FIG. 3 shows the results of particle size analysis of raw material Fe2O3 according to Example 3, and FIG. 4 shows the results of particle size analysis of raw material Fe2O3 according to Comparative Example 2.
[0343] Referring to FIGS. 1 to 3, it can be confirmed that the maximum particle size of the raw material Fe2O3 according to Examples 1 to 3 and Comparative Example 1 is 10 μm or less.
[0344] Referring to Fig. 4, it can be confirmed that the maximum particle size of the raw material Fe2O3 according to Comparative Example 2 is larger than 10㎛.
[0345]
[0346] Table 2 below shows the crystal grain size of lithium iron phosphate-containing precursors according to Examples 1 to 5 and Comparative Examples 1 to 4, the measured values of the phase fraction of each composition, and the calculated values of Equation 1.
[0347] Mixed raw material average particle size (D50_m, ㎛)Carbon content (wt%)Crystal grain size (D pc, nm)LFP phase fraction (M LFP, %)Fe2O3 phase fraction(%)Fe3O4 phase fraction(%)Li3PO4 phase fraction(%)Relationship equation 1M LFP *D pc (nm)Example 14.030.3378.894.51.803.774.5Example 28.920.2784.498.600.90.583.2Example 312.020.3480.396.81.401.877.7Example 48.920.2784.498.600.90.583.2Example 512.020.2784.498.600.90.583.2Comparative Example 12.020.207180.73.810.64.957.3Comparative Example 235.150.069986.41.66.75.385.5Comparative Example Comparative Example 48.920.2784.498.600.90.583.2
[0348] Referring to Table 2 above, it can be confirmed that the precursors according to Examples 1 to 5 have an average particle diameter (D50_m) of the mixed raw material of 4.03 ㎛ to 12.02 ㎛, which falls within the range of 4.0 ㎛ to 13.0 ㎛, and the calculated value of Relationship 1 is 74.5 to 83.2, which falls within the range of 70.0 to 85.0.
[0349]
[0350] Table 3 below shows the weight and weight percentage of materials used in the step of preparing slurries using precursor powders, citric acid, glucose, and deionized water according to Examples 1 to 5 and Comparative Examples 1 to 4, and the average particle diameter (D50) analysis values of solid materials in the final prepared slurry. Here, the solid content ratio means the total mass percentage of the lithium iron phosphate compound, dispersant (citric acid), and carbon additive (glucose) with respect to the total weight of the slurry.
[0351] Precursor (g)Citric Acid (g)Glucose (g)DIW (g)Solid contentPrecursor (wt%)Citric Acid (wt%)Glucose (wt%)Slurry internal solidsD50 (㎛)Example 11501.58.750032.0%93.6%0.9%5.4%1.068Example 21501.58.750032.0%93.6%0.9%5.4%1.067Example 31501.58.750032.0%93.6%0.9%5.4%1.068Example 41501.56.550031.6%94.9%0.9%4.1%1.082Example 51501.518.250033.9%88.4%0.9%10.7%1.073Comparative Example 11501.58.750032.0%93.6%0.9%5.4%0.803Comparative Example 21501.58.750032.0%93.6%0.9%5.4%1.212Comparative Example 31501.5050030.3%99.0%1.0%0.0%1.031Comparative Example 41501.52550035.3%85.0%0.8%14.2%1.042
[0352] Referring to Table 3 above, in Examples 1 to 5 and Comparative Examples 1 to 2, the mass percentage of the total mass of citric acid and glucose (citric acid + glucose) relative to the total mass of the lithium iron phosphate compound, dispersant (citric acid), and carbon additive (glucose) was found to be 5.00 wt% to 11.60 wt%, which is within the range of 4.5 wt% to 12.0 wt%.
[0353] In addition, Examples 1 to 5 and Comparative Examples 1 to 2 showed that the mass ratio of glucose to citric acid mass was 4.56 to 11.89, which was within the range of 4 to 16.
[0354] Comparative Example 3 showed that the mass percentage of the total mass of citric acid and glucose (citric acid + glucose) with respect to the total mass of the lithium iron phosphate compound, dispersant (citric acid), and carbon additive (glucose) was 1.00 wt%, which was less than the range of 4.5 wt% to 12.0 wt%, and since glucose was not mixed, the mass ratio of glucose to the mass of citric acid was 0, which was less than the range of 4 to 16.
[0355] Comparative Example 4 showed that the mass percentage of the total mass of citric acid and glucose (citric acid + glucose) relative to the total mass of the lithium iron phosphate compound, dispersant (citric acid), and carbon additive (glucose) was 15.00 wt%, which was greater than the range of 4.5 wt% to 12.0 wt%, and the mass ratio of glucose to the mass of citric acid was 17.75, which was greater than the range of 4 to 16.
[0356] Table 4 below shows the results of measuring the average particle size of the spray-dried product according to Examples 1 to 5 and Comparative Examples 1 to 4, the average particle size of the sintered product obtained by firing the spray-dried product, the crystal grain size, and the carbon content.
[0357] In addition, the calculated values of relational expressions 7 to 9 are shown.
[0358] LFP phase fraction (MLFP, %)Spray-dried productAverage particle size (D50_s, ㎛)Sintered productAverage particle size (D50_c, ㎛)Sintered product grain size (Dc, ㎚)Sintered product carbon content (C, %)Relationship equation 7M LFP *D50_s (㎛) relational expression 8MLFP * D50_c*Dc_c / 1000 (㎛ 2 ) Relationship 9M LFP ^2*C_c*D50_c(㎛) 94.525.423.21071.83%24.002.350.379 98.625.323.11071.77%24.952.440.398 96.824.123.31141.84%23.332.570.402 98.624.622.41091.36%24.262.410.296 98.624.823.51092.02%24.452.530.462 80.724.321.6811.70%19.611.410.239 86.424.623.21491.56%21.252.990.270 98.626.124.61350.40%25.733.270.096 98.626.826.1843.01%26.422.160.764
[0359] Referring to Table 4 above, the average particle diameter (D50_c) of the sintered products manufactured according to Examples 1 to 5 was in the range of 22.4 μm to 23.5 μm, and the carbon content was found to be almost similar, in the range of 1.36 wt% to 2.02 wt%.
[0360] In the case of Comparative Example 1, where the average particle diameter (D50_m) of the mixed raw material was 2.02㎛, the average particle diameter (D50_c) of the sintered product was 21.6㎛, which was somewhat smaller than that of Examples 1 to 5, and the carbon content was 1.70 wt%, which was similar to that of Examples 1 to 5.
[0361] In the case of Comparative Example 2, where the average particle diameter (D50_m) of the mixed raw material was 35.15㎛, the average particle diameter (D50_c) of the sintered product was 23.2㎛, which was similar to that of Examples 1 to 5, and the carbon content was 1.56 wt%, which was similar to that of Examples 1 to 5.
[0362] In the case of Comparative Example 3, where Glucose was not mixed in the wet mixing milling step, the average particle diameter (D50_c) of the sintered product was 24.6 ㎛, which was slightly larger than that of Examples 1 to 5, and the carbon content was 0.40 wt%, which was lower than that of Examples 1 to 5.
[0363] In the case of Comparative Example 4, in which the amount of Citric acid and Glucose mixed was large and the Glucose / Citric acid mass ratio was high in the wet mixing milling step, the average particle diameter (D50_c) of the sintered product was 26.1 ㎛, which was larger than that of Examples 1 to 5, and the carbon content was 3.01 wt%, which was larger than that of Examples 1 to 5.
[0364] Referring to Table 4 above, it can be confirmed that the calculated value of relational expression 7 of the positive electrode active materials manufactured according to Examples 1 to 5 is 23.33 to 24.95, which is within the range of 21.5 to 25.5, the calculated value of relational expression 8 is 2.35 to 2.57, which is within the range of 2.20 to 2.90, and the calculated value of relational expression 9 is 0.296 to 0.462, which is within the range of 0.28 to 0.50.
[0365] On the other hand, in the case of the positive electrode active materials manufactured according to Comparative Examples 1 to 4, it can be confirmed that the calculated value of relational expression 7 is outside the range of 21.5 to 25.5, the calculated value of relational expression 8 is outside the range of 2.20 to 2.90, and the calculated value of relational expression 9 is outside the range of 0.28 to 0.50.
[0366] Table 5 below shows the results of measuring the average particle diameter, crystal grain size, and carbon content of the final olivine-based positive electrode active materials obtained after grinding and separation according to Examples 1 to 5 and Comparative Examples 1 to 4.
[0367] In addition, the calculated values of relational expressions 2 to 6 are shown.
[0368]
[0369] LFP phase fraction (MLFP, %)Average particle size of positive electrode active material (D50, ㎛)Crystalline size of positive electrode active material (Dc, nm)Carbon content of positive electrode active material (C, %)Relationship equation 2D50*Dc^2*C / 1000(nm) 3 ) Relationship 3M LFP *D50 ^2 (㎛ 2 )Relationship 4MLFP* C*100 / D50 (㎛)Relationship 5MLFP* D50*C / Dc*10^5Relationship 6M LFP ^2*C*1000Example 194.51.541071.83%0.3232.241.1224.8916.34Example 298.61.51071.77%0.3042.221.1624.4717.21Example 396.81.521141.84%0.3632.241.1723.7517.24Example 498.61.6831091.36%0.2722.790.8020.7013.22Example 598.61.4821092.02%0.3562.171.3427.0819.64Comparative Example 180.70.851811.70%0.0950.581.6114.4111.07Comparative Example 286.41.831491.56%0.6342.890.7416.5511.65Comparative Example 398.62.3141350.40%0.1695.280.176.763.89Comparative Example 498.60.898843.01%0.1910.803.3031.7329.26
[0370] Referring to Table 5 above, it can be confirmed that the calculated value of equation 2 of the positive electrode active materials manufactured according to Examples 1 to 5 is 0.272 to 0.363, which is included in the range of 0.20 to 0.50, the calculated value of equation 3 is 2.17 to 2.79, which is included in the range of 1.0 to 2.85, the calculated value of equation 4 is 0.80 to 1.34, which is included in the range of 0.75 to 1.50, the calculated value of equation 5 is 20.70 to 27.08, which is included in the range of 17.0 to 30.0, and the calculated value of equation 6 is 16.34 to 19.64, which is included in the range of 12.0 to 29.0.
[0371]
[0372] On the other hand, in the case of the positive electrode active materials manufactured according to Comparative Examples 1 to 4, it can be confirmed that the calculated value of relational expression 2 is outside the range of 0.20 to 0.50, the calculated value of relational expression 3 is outside the range of 1.0 to 2.85, the calculated value of relational expression 4 is outside the range of 0.75 to 1.50, the calculated value of relational expression 5 is outside the range of 17.0 to 30.0, and the calculated value of relational expression 6 is outside the range of 12.0 to 29.0.
[0373]
[0374] (Preparation of positive electrode active material: Example 6)
[0375] An olivine-based positive electrode active material was manufactured in the same manner as Example 1, except that the following mixing relationship was satisfied in the raw material mixing step.
[0376] Specifically, it proceeded as follows.
[0377] In the dry step, raw materials, lithium dihydrogen phosphate (LiH2PO4) powder and ferric oxide (Fe2O3) powder, were mixed in a molar ratio of 3:1.5, and citric acid was mixed in an amount ranging from 1 wt% to 2.5 wt% of the total mass of the lithium dihydrogen phosphate (LiH2PO4) powder and ferric oxide (Fe2O3) powder, and uniformly mixed and milled using a ball mill or powder mixer to obtain a mixed raw material powder. At this time, the mixing speed of the lithium dihydrogen phosphate (LiH2PO4) powder, ferric oxide (Fe2O3), and citric acid satisfies the following mixing relationship expressed by the internal volume of the ball mill or powder mixer.
[0378] [Mixed Relationship]
[0379] (Diameter of container (cm)*PI*2 < R(RPM) < (Diameter of container (cm)*PI*10
[0380] Here, PI is the circumferential constant.
[0381] After the above mixed powder is loaded into a high-temperature calcination furnace, nitrogen gas is supplied in the range of 0.1 L / min to 300 L / min, heated to 650°C at a heating rate of 5°C / min, maintained for 6 hours, and then naturally cooled to room temperature to manufacture a primary calcined product, i.e., a precursor, through a dry step.
[0382] Next, using the primary calcined material, the slurry was prepared, spray dried, reduced calcined, pulverized, and separated in the same manner as in Example 1 to prepare the final olivine-based positive electrode active material.
[0383] The average particle size of the final olivine-based positive electrode active material obtained at this time was controlled to 1.0 to 2.0 μm.
[0384] (Manufacturing of positive electrode active material: Comparative Example 5)
[0385] A mixed raw material was prepared by performing the mixing step in the same manner as in Example 6.
[0386] After the above mixed raw material is charged into a high-temperature kiln, nitrogen gas is supplied in the range of 0.1 L / min to 300 L / min, and the mixture is heated to 650°C at a heating rate of 5°C / min, maintained for 6 hours, and then naturally cooled to room temperature to manufacture an olivine-based positive electrode active material through a dry step.
[0387] Through the crushing and separation process, the average particle size of the final produced olivine-based positive electrode active material was controlled to 1.0 to 2.0 μm.
[0388]
[0389] (Manufacturing of positive electrode active material: Comparative example 6)
[0390] Citric acid (2.1 wt% based on the total mass of lithium dihydrogen phosphate (LiH2PO4) powder and ferric oxide (Fe2O3) powder) and glucose (5.8 wt% based on the total mass of lithium dihydrogen phosphate (LiH2PO4) powder and ferric oxide (Fe2O3) powder) were mixed with lithium dihydrogen phosphate (LiH2PO4) powder and ferric oxide (Fe2O3) powder, and then mixed with deionized water to manufacture a positive electrode active material by performing only the wet step of Example 6. That is, a positive electrode active material was manufactured by performing only the wet step without performing the dry step of Example 6 using the above raw materials.
[0391] At this time, the material attached to the inner wall of the spray dryer was a large amount of mixed dry material due to LiH2PO4 recrystallization growth and Fe2O3, and when 1 kg of slurry was injected and spray-dried, it was measured that about 300 g was attached to the inner wall of the spray dryer.
[0392] It can be confirmed that the mass of the positive electrode active material lost by being attached to the wall of the device during the spray drying process according to Example 6 was significantly reduced to about 3 wt% of the mass of the positive electrode active material lost according to Comparative Example 6.
[0393]
[0394] (Coin-shaped half-cell manufacturing)
[0395] Using the LFP cathode active material manufactured according to the above examples and comparative examples, a CR2032 coin cell was manufactured and then electrochemical evaluation was conducted.
[0396] Specifically, a slurry for manufacturing an electrode plate was prepared by mixing LFP cathode active material:conductive material (Super P):binder (PVDF) in a mass ratio of 90:5:5 in an NMP (N-Methyl-2-pyrrolidone) solvent and adjusting the slurry viscosity.
[0397] The above-mentioned slurry was coated on a 15 μm thick Al foil using a doctor blade, dried, and rolled to manufacture a positive electrode plate. Here, the electrode loading amount was approximately 10 mg / cm2 The ideal was the density of the polar plate was about 2 g / cm 3 That's all for now.
[0398] 1M LiPF6 and EC:DMC:EMC=3:4:3 (vol%) were mixed as electrolyte, and then 1.5 wt% of vinylene carbonate (VC) was added. Coin-type half-cells were manufactured using PP separators and lithium anodes (200 μm, Honzo metal), and aged at room temperature for 10 hours. The measured voltage range was 3.65 V to 2.5 V, and the evaluation was conducted with a 1C reference capacity of 150 mAh / g.
[0399] The results of battery characteristic evaluations using the positive electrode active materials according to Examples 1 to 5 and Comparative Examples 1 to 4 are summarized in Table 6 below.
[0400] Charge capacityDischarge capacityEfficiencyDischarge capacity(mAh / g@0.1C)(mAh / g@0.1C)%(mAh / g@1C)Example 1160.8158.398.40%142.7Example 2162160.499.00%146.7Example 3161158.398.30%142.6Example 4161.9159.198.30%143.1Example 5160.1155.997.40%146.3Comparative example 1156.2152.797.70%138.2Comparative example 2156.8153.397.80%138.2Comparative example 3150.4150.299.90%78.3 Comparative example 4149.9149.699.80%91.7
[0401] Referring to Table 6 above, in the case of batteries using the LFP positive electrode active materials according to Examples 1 to 5, it was confirmed that the charge capacity was 160 mAh / g or more at a charge current of 0.1 C, and the discharge capacity was 155 mAh / g. In addition, it was confirmed that the charge capacity was 140 mAh / g or more at a charge current of 1 C.
[0402] On the other hand, in the case of batteries using LFP positive electrode active materials according to Comparative Examples 1 to 4, the charge capacity was in the range of 149.9 mAh / g to 156.8 mAh / g at a charge current of 0.1 C, and the discharge capacity was in the range of 149.6 mAh / g to 153.3 mAh / g, which were confirmed to be lower than those of Examples 1 to 5. In addition, the charge capacity was found to be in the range of 78.3 mAh / g to 138.2 mAh / g at a charge current of 1 C.
[0403] In the case of Comparative Example 2, the reason for the low charge and discharge capacity is thought to be that the difference in particle size of the initial raw materials, lithium dihydrogen phosphate (LiH2PO4) and ferric oxide (Fe2O3), is large, the mixing uniformity is low, and the Li ions and PO4 ions of the liquefied lithium dihydrogen phosphate (LiH2PO4) during the reduction and calcination process do not efficiently penetrate into the interior of the ferric oxide (Fe2O3) particles.
[0404] In the case of Comparative Example 3, the reason for the low charge and discharge capacity is thought to be that the amount of Glucose, a raw material for forming the carbon coating layer, mixed was small, so the carbon coating layer was not formed effectively.
[0405]
[0406] The results of battery characteristic evaluation using the positive electrode active materials according to Example 6 and Comparative Examples 5 to 6 are summarized in Table 7 below.
[0407] Charge capacityDischarge capacityEfficiency(mAh / g@0.1C)(mAh / g@0.1C)%Example 6162160.499.0Comparative example 5157.7154.297.8Comparative example 6156.8155.799.3
[0408] Referring to Table 7 above, in the case of a battery using the LFP positive electrode active material according to Example 6, it was confirmed that the charge capacity was 162 mAh / g and the discharge capacity was 160.4 mAh / g at a charge current of 0.1 C.
[0409] On the other hand, in the case of the battery using the LFP positive electrode active material according to Comparative Example 5, the charge capacity was 157.7 mAh / g at a charge current of 0.1 C, and the discharge capacity was 154.2 mAh / g, and in the case of the battery using the LFP positive electrode active material according to Comparative Example 6, the charge capacity was 156.8 mAh / g at a charge current of 0.1 C, and the discharge capacity was 155.7 mAh / g.
[0410] From this, it can be confirmed that the battery using the LFP positive electrode active material manufactured according to Example 6 of the present invention has excellent charge and discharge capacities.
[0411] In addition, it can be confirmed that when manufacturing an LFP cathode active material through the dry and wet steps of the present invention, the problem of reduced productivity due to attachment to the equipment surface can be solved.
[0412]
[0413] The present invention is not limited to the above-described embodiments, but can be manufactured in a variety of different forms. Those skilled in the art will appreciate that the present invention can be implemented in other forms without altering the technical spirit or essential characteristics of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive.
[0414] Accordingly, the actual scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A precursor derived from a mixed raw material having an average particle size of 4.0㎛ to 13.0㎛, including a lithium raw material, an iron raw material, and a phosphorus raw material. An olivine-based positive electrode active material precursor satisfying the following relational expression 1. [Relationship 1] 60.0 ≤ M LFP *D pc ≤ 85.0 (In the above relation 1, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and D pc is the crystal grain size (nm) of the precursor.) 2. In paragraph 1, The above precursor has a crystal grain size (D) obtained by XRD analysis. pc ) is 75.0 nm to 95.0 nm, Olivine-based cathode active material precursor.
3. In paragraph 1, The precursor further comprises carbon exceeding 0.20 wt% based on the total weight, Olivine-based cathode active material precursor.
4. In paragraph 1, The above precursor has a phase fraction of lithium iron phosphate (LiFePO4) of 94.5% or more. Olivine-based cathode active material precursor.
5. In paragraph 1, The above precursor has a phase fraction of lithium phosphate (Li3PO4) of 4.5% or less. Olivine-based cathode active material precursor.
6. In paragraph 1, The above precursor has a phase fraction of iron oxide (Fe2O3) of 3.5% or less. Olivine-based cathode active material precursor.
7. In paragraph 1, The above precursor has a phase fraction of iron tetroxide (Fe3O4) of 4.5% or less. Olivine-based cathode active material precursor.
8. A core portion containing lithium metal phosphate; and A carbon coating layer positioned on the surface of the core portion; An olivine-based positive electrode active material for a lithium secondary battery satisfying the following relational expression 2. [Relationship 2] 0.20 ≤ D50*Dc^2*C / 1000 ≤ 0.50 (In the above equation 2, D50 is the average particle size (㎛) of the olivine-based positive electrode active material, Dc is the crystal grain size (nm) in the olivine-based positive electrode active material, and C is the carbon weight percentage (%) in the olivine-based positive electrode active material.) 9. It is derived from the olivine-based positive electrode active material precursor of any one of the first to seventh clauses, An olivine-based positive electrode active material for a lithium secondary battery satisfying the following relational expression 3. [Relationship 3] 1.00 ≤ M LFP *D50 ^2 ≤ 2.85 (In the above relational expression 3, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and D50 is the average particle size (㎛) of the olivine-based positive electrode active material.
10. It is derived from the olivine-based positive electrode active material precursor of any one of the first to seventh clauses, An olivine-based positive electrode active material for a lithium secondary battery satisfying the following relational expression 4. [Relationship 4] 0.75 ≤ M LFP *C*100 / D50≤ 1.50 (In the above relational expression 4, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, D50 is the average particle size (㎛) of the olivine-based cathode active material, and C is the weight percentage (%) of carbon in the olivine-based cathode active material.
11. It is derived from the olivine-based positive electrode active material precursor of any one of the first to seventh clauses, An olivine-based positive electrode active material for a lithium secondary battery satisfying the following relational expression 5. [Relationship 5] 17.0 ≤ M LFP * D50*C / Dc*10^5≤ 30.0 (In the above relational expression 5, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, D50 is the average particle size (㎛) of the olivine-based cathode active material, C is the carbon weight percentage (%) in the olivine-based cathode active material, and Dc is the crystal grain size (nm) in the olivine-based cathode active material.
12. It is derived from the olivine-based positive electrode active material precursor of any one of the first to seventh clauses, An olivine-based positive electrode active material for a lithium secondary battery satisfying the following relational expression 6. [Relationship 6] 12.0 ≤ M LFP ^2*C*1000≤ 29.0 (In the above relational expression 6, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and C is the weight percentage (%) of carbon in the olivine-based cathode active material.
13. In paragraphs 8 to 12, The above cathode active material has a crystal grain size (Dc) of 90.0 nm to 130.0 nm as determined by XRD analysis. Olivine-based cathode active material for lithium secondary batteries.
14. In paragraphs 8 to 12, The above positive electrode active material has a carbon content of 0.45 wt% to 3.0 wt% based on the total weight. Olivine-based cathode active material for lithium secondary batteries.
15. In paragraphs 8 to 12, The above positive electrode active material has an average particle diameter (D50) of 1.0 to 10.0㎛. Olivine-based cathode active material for lithium secondary batteries.
16. In paragraphs 8 to 12, The above positive electrode active material is an olivine-based positive electrode active material for a lithium secondary battery represented by the following chemical formula 1: [Chemical Formula 1] Li x (Fe y M 1-y )PO4 (In the above chemical formula 1, 0.95≤x≤1.1, 0.9≤y≤1, 0.95≤x / y≤1.1, M is at least one selected from the group consisting of Mn, Co, Ni, Cu, Zn, Mg, Cr, V, Mo, Ti, Al, Nb, B, W, and Ga.) 17. A step of mixing and calcining lithium raw material, iron raw material, and phosphorus raw material to manufacture a precursor including lithium iron phosphate (LiFePO4); A step of preparing a slurry by mixing and milling the above precursor, carbon additive, dispersant, and solvent; A step of spray drying the above slurry to obtain a spray dried product; A step of calcining the above spray-dried product in a reducing atmosphere to obtain a calcined product; and A step of crushing and separating the above-mentioned material to obtain a final olivine-based positive electrode active material; It satisfies the following relational expression 7, A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery. [Relationship 7] 21.5 ≤ M LFP *D50_s ≤ 25.5 (In the above relational expression 7, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and D50_s is the average particle size (㎛) of the spray-dried product.
18. A step of manufacturing a precursor including lithium iron phosphate (LiFePO4) by mixing and calcining lithium raw material, iron raw material, and phosphorus raw material; A step of preparing a slurry by mixing and milling the above precursor, carbon additive, dispersant, and solvent; A step of spray drying the above slurry to obtain a spray dried product; A step of calcining the above spray-dried product in a reducing atmosphere to obtain a calcined product; and A step of crushing and separating the above-mentioned material to obtain a final olivine-based positive electrode active material; It satisfies the following relational expression 8, A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery. [Relationship 8] 2.20 ≤ M LFP * D50_c*Dc_c / 1000≤ 2.90 (In the above relational expression 8, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, D50_c is the average particle size (㎛) of the sintered product, and Dc_c is the crystal grain size (nm) in the sintered product.) 19. A step of manufacturing a precursor including lithium iron phosphate (LiFePO4) by mixing and calcining lithium raw material, iron raw material, and phosphorus raw material; A step of preparing a slurry by mixing and milling the above precursor, carbon additive, dispersant, and solvent; A step of spray drying the above slurry to obtain a spray dried product; A step of calcining the above spray-dried product in a reducing atmosphere to obtain a calcined product; and A step of crushing and separating the above-mentioned material to obtain a final olivine-based positive electrode active material; It satisfies the following relation 9, A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery. [Relationship 9] 0.28 ≤ M LFP ^2*C_c*D50_c ≤ 0.50 (In the above relational expression 9, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, C_c is the weight percentage (%) of carbon in the sintered product, and D50_c is the average particle size (㎛) of the sintered product.
20. A step of manufacturing a precursor including lithium iron phosphate (LiFePO4) by mixing and calcining lithium raw material, iron raw material, and phosphorus raw material; A step of preparing a slurry by mixing and milling the above precursor, carbon additive, dispersant, and solvent; A step of spray drying the above slurry to obtain a spray dried product; A step of calcining the above spray-dried product in a reducing atmosphere to obtain a calcined product; and A step of crushing and separating the above-mentioned material to obtain a final olivine-based positive electrode active material; It satisfies the following relational expression 3, A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery. [Relationship 3] 1.00 ≤ M LFP *D50 ^2 ≤ 2.85 (In the above relational expression 3, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and D50 is the average particle size (㎛) of the olivine-based positive electrode active material.
21. A step of manufacturing a precursor including lithium iron phosphate (LiFePO4) by mixing and calcining lithium raw material, iron raw material, and phosphorus raw material; A step of preparing a slurry by mixing and milling the above precursor, carbon additive, dispersant, and solvent; A step of spray drying the above slurry to obtain a spray dried product; A step of calcining the above spray-dried product in a reducing atmosphere to obtain a calcined product; and A step of crushing and separating the above-mentioned material to obtain a final olivine-based positive electrode active material; It satisfies the following relational expression 4, A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery. [Relationship 4] 0.75 ≤ M LFP *C*100 / D50≤ 1.50 (In the above relational expression 4, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, D50 is the average particle size (㎛) of the olivine-based cathode active material, and C is the weight percentage (%) of carbon in the olivine-based cathode active material.
22. A step of manufacturing a precursor including lithium iron phosphate (LiFePO4) by mixing and calcining lithium raw material, iron raw material, and phosphorus raw material; A step of preparing a slurry by mixing and milling the above precursor, carbon additive, dispersant, and solvent; A step of spray drying the above slurry to obtain a spray dried product; A step of calcining the above spray-dried product in a reducing atmosphere to obtain a calcined product; and A step of crushing and separating the above-mentioned material to obtain a final olivine-based positive electrode active material; It satisfies the following relation 5, A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery. [Relationship 5] 17.0 ≤ M LFP * D50*C / Dc*10^5≤ 30.0 (In the above relational expression 5, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, D50 is the average particle size (㎛) of the olivine-based cathode active material, C is the carbon weight percentage (%) in the olivine-based cathode active material, and Dc is the crystal grain size (nm) in the olivine-based cathode active material.
23. A step of manufacturing a precursor including lithium iron phosphate (LiFePO4) by mixing and calcining lithium raw material, iron raw material, and phosphorus raw material; A step of preparing a slurry by mixing and milling the above precursor, carbon additive, dispersant, and solvent; A step of spray drying the above slurry to obtain a spray dried product; A step of calcining the above spray-dried product in a reducing atmosphere to obtain a calcined product; and A step of crushing and separating the above-mentioned material to obtain a final olivine-based positive electrode active material; It satisfies the following relation 6, A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery. [Relationship 6] 12.0 ≤ M LFP ^2*C*1000≤ 29.0 (In the above relational expression 6, M LFP is the phase fraction of lithium iron phosphate (LiFePO4) in the precursor, and C is the weight percentage (%) of carbon in the olivine-based cathode active material.
24. In paragraphs 17 to 23, The phase fraction of lithium iron phosphate (LiFePO4) in the above precursor is 94.5% or more, A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery.
25. In paragraphs 17 to 23, In the step of preparing a slurry by mixing and milling the above precursor, carbon additive, dispersant and solvent, The average particle size of the solid material in the above slurry is 0.9㎛ to 1.20㎛. A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery.
26. In paragraphs 17 to 23, The crystal grain size (Dc) of the above-mentioned material is 90.0 nm to 130 nm. A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery.
27. In paragraphs 17 to 23, The average particle diameter (D50_c) of the above-mentioned product is 22.0㎛ to 24.0㎛. A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery.
28. In paragraphs 17 to 23, In the step of spray drying the above slurry to obtain a spray dried product, The average particle diameter of the above spray-dried product is 24.0㎛ to 26.0㎛. A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery.
29. In paragraphs 17 to 23, In the step of crushing and separating the above-mentioned material to obtain the final olivine-based positive electrode active material, The average particle diameter (D50) of the above separated final olivine-based positive electrode active material is 1.0㎛ to 10.0㎛. A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery.
30. In paragraphs 17 to 23, The above iron raw material is ferric oxide (Fe2O3), The average particle size (D50) of the above iron oxide (Fe2O3) is in the range of 0.1㎛ to 2.6㎛ and the maximum particle size (Dmax) is 10㎛ or less. A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery.
31. In paragraphs 17 to 23, The above lithium raw material and phosphorus raw material are lithium dihydrogen phosphate (LiH2PO4), The average particle size (D50) of the above lithium dihydrogen phosphate (LiH2PO4) is in the range of 1㎛ to 100㎛. A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery.
32. In paragraphs 17 to 23, In the step of mixing and calcining the above lithium raw material, iron raw material and phosphorus raw material to manufacture a precursor including lithium iron phosphate (LiFePO4), When mixing the above lithium raw material, iron raw material and phosphorus raw material, the following mixing relationship is satisfied: A method for manufacturing an olivine-based positive electrode active material for a lithium secondary battery. [Mixed Relationship] (Diameter of container (cm)*PI*2 < R(RPM) < (Diameter of container (cm)*PI*10 (Here PI is the circumference constant.) 33. The entire house; and A cathode active material layer comprising an olivine-based cathode active material for a lithium secondary battery according to any one of claims 8 to 16, located on at least one surface of the above-mentioned collector; Cathode for lithium secondary batteries.
34. Containing a positive electrode for a lithium secondary battery according to Article 33, Lithium secondary battery.
Citation Information
Patent Citations
Carbon composite of lithium / Iron / Phosphorus-based complex oxide, production method therefor, positive pole activating material for lithium secondary battery, and lithium secondary battery
JP2003292308A
Method for producing iron lithium phosphate
KR101337140B1
Lithium iron phosphate powder manufacturing method, olivine structured lithium iron phosphate powder, cathode sheet using said lithium iron phosphate powder, and non-aqueous ...
KR1020110007112A
PRODUCTION METHOD OF FePO4 USING pH CONTROL, AND PRODUCTION METHOD OF LiFePO4 / C FOR POSITIVE ELECTRODE OF LITHIUM SECONDARY BATTERY
KR1020140021791A
Cathode for lithium secondary battery, preparation method thereof, and lithium secondary battery comprising the same
KR1020150024704A
Cited By
Preparation method of lithium iron phosphate positive electrode material, positive electrode material, pole piece and battery
CN120172377A
Preparation method and application of high-temperature-resistant lithium iron phosphate positive electrode material based on solid solution reaction
CN120757091A
Methods for preparing composite positive electrode active materials, composite positive electrode active materials, and rechargeable lithium batteries
EP4841703A1
High performance LFP cell with active material composite for high rate applications
US20260312149A1