Protective dielectric layers for enhancing reliability of vacuum ultraviolet lamps

The integration of protective dielectric layers and a regenerable component in VUV lamps enhances their reliability and longevity by resisting degradation and restoring transmission, addressing the short lifespan issues of VUV lamps with lithium fluoride windows.

WO2024206809A1PCT designated stage expired Publication Date: 2024-10-03THE RGT UNIV OF MICHIGAN
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/US2024/022212
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Vacuum ultraviolet (VUV) lamps, particularly those using lithium fluoride windows, have short lifetimes due to susceptibility to moisture and color center formation, leading to reduced transmission and increased costs, as they degrade quickly under the harsh conditions within the ionization chamber and external environments.

Method used

A VUV lamp design incorporating a transmissive window with multiple layers, including a primary layer of magnesium fluoride, calcium fluoride, or lithium fluoride, and a protective dielectric layer of silicon dioxide, silicon nitride, or aluminum oxide, which enhances transmission while resisting degradation from ions, electrons, and moisture, and a regenerable component that uses heat or deep ultraviolet radiation to restore transmission.

Benefits of technology

The solution extends the lifetime of VUV lamps by maintaining greater than 60% transmission and significantly delaying degradation, allowing for prolonged reliable operation and reduced maintenance, while the regenerable component restores transmission, effectively addressing the limitations of existing VUV window materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2024022212_03102024_PF_FP_ABST
    Figure US2024022212_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Vacuum ultraviolet (VUV) lamps are provided having an ultraviolet radiation chamber that generates ultraviolet photons with a gas selected from the group consisting of: argon (Ar), krypton (Kr), xenon (Xe), and combinations thereof. A transmissive window is disposed adjacent to the ultraviolet radiation chamber and permits ultraviolet photons to pass therethrough. The transmissive window comprises a primary layer of a first material selected from the group consisting of: magnesium fluoride, calcium fluoride, lithium fluoride, and combinations thereof. At least one protective layer comprises a transmissive dielectric material selected from the group consisting of: silicon dioxide (SiO2), silicon nitride (Si3N4), aluminum oxide (Al2O3), and combinations thereof. Methods of making the VUV lamps, as well as regenerable VUV lamps with a regenerator component, such as a heater or deep ultraviolet (DUV) radiation source are also provided. The VUV lamps may be incorporated into photoionization detectors (PIDs), including microfabricated microfluidic PIDs.
Need to check novelty before this filing date? Find Prior Art

Description

PROTECTIVE DIELECTRIC LAYERS FOR ENHANCING RELIABILITY OF VACUUM ULTRAVIOLET LAMPSGOVERNMENT SUPPORT

[0001] This invention was made with government support under ROl-OHOl 1082 awarded by the Centers for Disease Control and Prevention and under FA8650-19-C-9101 awarded by the U.S. Air Force Materiel Command. The government has certain rights in the invention.CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of U.S. Provisional Application No. 63 / 456,127, filed on March 31, 2023. The entire disclosure of the above application is incorporated herein by reference.FIELD

[0003] The present disclosure relates to protective dielectric layers for enhancing reliability and robustness of vacuum ultraviolet lamps (VUV) for applications, such as microfluidic photoionization detectors (PID).BACKGROUND

[0004] This section provides background information related to the present disclosure which is not necessarily prior art.

[0005] A photoionization detector (PID) is a type of non-destructive vapor analyte detector that can be used in conjunction with gas chromatography (GC) for analysis of volatile organic compounds (VOCs) and other analyte compounds. In a PID, vapor molecules are ionized inside an ionization chamber by ultra-violet (UV) radiation generated by a UV lamp. For example, vacuum ultraviolet (VUV) lamps are widely used in many applications, especially, in gas analysis, in which gas molecules are ionized by the VUV photons emitted by the lamp and subsequently detected. Thus, ions generated in the ionization chamber may then be driven to electrodes to generate current. The UV lamp is typically filled with low pressure argon, krypton, xenon, or other gases to produce UV light under external electrical excitation. For example, an argon (Ar) lamp can emit photons with energy up to 11.7 eV (106 nm in wavelength) and krypton (Kr) can emit photons with energy up to 10.6 eV (117 nm in wavelength).

[0006] In the UV lamps, sealing windows (i.e., UV transmission windows) are formed with specialized materials, such as calcium fluoride, magnesium fluoride, or lithium fluoride. Suchmaterials have a relatively high transmission coefficient within the range of wavelengths of UV radiation / photons (or photon energies) of interest. Usually, a magnesium fluoride (MgF2) window is used for krypton lamps and other lamps whose photon energy is lower than 10.6 eV (or wavelength longer than 117 nm). However, for an argon lamp, a MgF2 window’s transmission decreases significantly near 106 nm. Therefore, a lithium fluoride (LiF) window, which has a higher transmission near 106 nm, needs to be used. In addition to MgF2 and LiF, CaF2 is also used as a VUV transmission window.

[0007] However, these VUV window materials are relatively expensive and susceptible to water etching, crystal solarization, and the yellowing effect due to UV damage, all of which degrade the UV lamp (and hence PID) performance and shorten its lifetime. The LiF window in particular is highly susceptible to moisture (hygroscopic effect) and color center formation caused by highly energetic ions and VUV photons. While a MgF2 window may last a few thousand hours of operation, an LiF window can last only about 100 hours, which makes an argon VUV lamp very expensive and its lifetime notoriously short. It would be advantageous to provide robust VUV windows having reduced susceptibility to moisture and reactivity to plasma in the ionization chamber to enhance lifetime of the VUV lamp.SUMMARY

[0008] This section provides a general summary of the disclosure, and is not a comprehensive disclosure of its full scope or all of its features.

[0009] In certain aspects the present disclosure relates to a vacuum ultraviolet (VUV) lamp. The VUV lamp may comprise an ultraviolet radiation chamber that is configured to generate ultraviolet photons that comprises a gas selected from the group consisting of: argon (Ar), krypton (Kr), xenon (Xe), and combinations thereof. The VUV lamp may also comprise a transmissive window disposed adjacent to the ultraviolet radiation chamber that permits the ultraviolet photons to pass from the ultraviolet radiation chamber therethrough. The transmissive window comprises multiple layers including a primary layer comprising a first material selected from the group consisting of: magnesium fluoride, calcium fluoride, lithium fluoride, and combinations thereof, and at least one protective layer disposed adjacent to the primary layer that comprises a transmissive dielectric material.

[0010] In one aspect, the transmissive dielectric material is selected from the group consisting of: silicon dioxide (SiCL), silicon nitride (SisN4), aluminum oxide (AI2O3), and combinations thereof.

[0011] In one aspect, the primary layer defines a first side facing the ultraviolet radiation chamber and a second side opposite to the first side. The at least one protective layer is disposed adjacent to the second side.

[0012] In one aspect, the primary layer defines a first side facing the ultraviolet radiation chamber and a second side opposite to the first side. The at least one protective layer comprises a first protective layer disposed adjacent to the first side and a second protective layer disposed adjacent to the second side.

[0013] In one aspect, the at least one protective layer transmits greater than or equal to about 60% of the ultraviolet photons generated in the ultraviolet radiation chamber.

[0014] In one aspect, the at least one protective layer has a thickness of less than or equal to about 500 nm.

[0015] In one aspect, the at least one protective layer has a thickness of greater than or equal to about 0.5 nm to less than or equal to about 10 nm.

[0016] In one aspect, the transmissive window comprises the primary layer and an interlayer assembly disposed on a side opposite to the ultraviolet radiation chamber. The interlayer assembly comprises a first protective layer, an interlayer comprising the first material selected from the group consisting of: magnesium fluoride, calcium fluoride, lithium fluoride, and combinations thereof disposed adjacent to the first protective layer. The interlayer assembly further includes a second protective layer disposed on a side of the interlayer opposite to the first protective layer.

[0017] The present disclosure further relates to a regenerable vacuum ultraviolet (VUV) lamp that may comprise an ultraviolet radiation chamber that is configured to generate ultraviolet photons that comprises a gas selected from the group consisting of: argon (Ar), krypton (Kr), xenon (Xe), and combinations thereof. The regenerable VUV lamp further comprises a transmissive window disposed adjacent to the ultraviolet radiation chamber that permits the ultraviolet photons to pass from the ultraviolet radiation chamber therethrough. The transmissive window comprises multiple layers including a primary layer comprising a first material selected from the group consisting of: magnesium fluoride, calcium fluoride, lithium fluoride, and combinations thereof, and at least one protective layer disposed adjacent to the primary layer that comprises a transmissive dielectric material. The regenerable VUV lamp further comprises a regenerator component disposed in proximity to the transmissive window. The regenerator component has a first operational state and a second operational state. In the first operational state, the regenerator component is dormant and in a second operational state, the regenerator component is configured to selectively generate heat or deep ultraviolet (DUV) radiation directedtowards the transmissive window to enhance or restore transmission of the ultraviolet photons through the transmissive window.

[0018] In one aspect, the transmissive dielectric material is selected from the group consisting of: silicon dioxide (SiCh), silicon nitride (SisN4), aluminum oxide (AI2O3), and combinations thereof.

[0019] In one aspect, the regenerator component comprises a heater.

[0020] In one aspect, the regenerator component comprises a source of deep ultraviolet (DUV) radiation.

[0021] In one aspect, the regenerator component comprises a heater and a source of deep ultraviolet (DUV) radiation.

[0022] In one aspect, the transmissive window is sealed to the ultraviolet radiation chamber by a high-temperature seal capable of withstanding temperatures of greater than or equal to about 350°C.

[0023] In one aspect, the primary layer defines a first side facing the ultraviolet radiation chamber and a second side opposite to the first side, wherein the at least one protective layer is disposed adjacent to the second side.

[0024] In one aspect, the primary layer defines a first side facing the ultraviolet radiation chamber and a second side opposite to the first side. The at least one protective layer comprises a first protective layer disposed adjacent to the first side and a second protective layer disposed adjacent to the second side.

[0025] In one aspect, the at least one protective layer has a thickness of less than or equal to about 500 nm.

[0026] In one aspect, the at least one protective layer has a thickness of greater than or equal to about 0.5 nm to less than or equal to about 10 nm.

[0027] The present disclosure further relates to a photoionization detector (PID). The PID comprises an ionization chamber having an inlet that receives a fluid sample and an outlet through which the fluid sample exits the ionization chamber. The PID also comprises a first electrode and a distinct second electrode in electrical communication with the ionization chamber. The PID comprises an ultraviolet radiation chamber that is configured to generate ultraviolet photons that comprises a gas selected from the group consisting of: argon (Ar), krypton (Kr), xenon (Xe), and combinations thereof. Further, a transmissive window is disposed between the ionization chamber and the ultraviolet radiation chamber that permits the ultraviolet photons to pass from the ultraviolet radiation chamber into the ionization chamber. The transmissive window comprises multiple layers including a primary layer comprising a first material selected from the groupconsisting of: magnesium fluoride, calcium fluoride, lithium fluoride, and combinations thereof. At least one protective layer is disposed adjacent to the primary layer comprising a transmissive dielectric material.

[0028] In one aspect, the transmissive dielectric material is selected from the group consisting of: silicon dioxide (SiCh), silicon nitride (SiaN4), aluminum oxide (AI2O3), and combinations thereof.

[0029] In one aspect, the ionization chamber is a microfluidic ionization chamber having one or more microfluidic channels each having a total volume of less than about 10 pL.

[0030] In one aspect, the primary layer defines a first side facing the ultraviolet radiation chamber and a second side opposite to the first side facing the ionization chamber. The at least one protective layer is disposed adjacent to the second side.

[0031] In one aspect, the primary layer defines a first side facing the ultraviolet radiation chamber and a second side opposite to the first side facing the ionization chamber. The at least one protective layer comprises a first protective layer disposed adjacent to the first side and a second protective layer disposed adjacent to the second side.

[0032] In one aspect, the at least one protective layer has a thickness of less than or equal to about 500 nm.

[0033] In one aspect, the at least one protective layer has a thickness of greater than or equal to about 0.5 nm to less than or equal to about 10 nm.

[0034] Further areas of applicability will become apparent from the description provided herein. The description and specific examples in this summary are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure.DRAWINGS

[0035] The drawings described herein are for illustrative purposes only of selected embodiments and not all possible implementations, and are not intended to limit the scope of the present disclosure.

[0036] FIGS. 1A-1B. FIG. 1A illustrates the mechanisms that cause a transmissive window (e.g., LiF window) to lose its vacuum ultraviolet (VUV) transmission ability in a VUV lamp. FIG. IB shows photographs of a yellowing effect on the transmissive window of the VUV lamp after experiencing degradation.

[0037] FIGS. 2A-2D illustrate variations of dielectric-coated VUV windows for VUV lamps that can protect the VUV window from ions, excited gas molecules, electrons, and water vapor molecules inside and / or outside of the lamp chamber (or plasma chamber). The dielectriccoating can be applied on either or both sides of the VUV window with the same or different materials and with the same or different thicknesses. FIG. 2A shows a cross-sectional view of a vacuum ultraviolet (VUV) light prepared in accordance with certain aspects of the present disclosure to have a transmissive window with a protective dielectric coating on a bottom side. FIG. 2B shows a cross-sectional view of another variation of a vacuum ultraviolet (VUV) light prepared in accordance with certain aspects of the present disclosure having a transmissive window with a protective dielectric coating on top and bottom sides. FIG. 2C shows a cross- sectional view of another variation of a vacuum ultraviolet (VUV) light prepared in accordance with certain aspects of the present disclosure having a transmissive window with a protective interlayer assembly that includes a first and second dielectric coating on top and bottom sides around a primary layer. The protective interlayer assembly is disposed adjacent to a second window primary layer. FIG. 2B shows an illustration of an embodiment of a regenerable vacuum ultraviolet (VUV) lamp with a regenerator component (e.g., a heater or DUV) disposed near the VUV transmissive window for selectively regenerating it.

[0038] FIGS. 3A-3B. In FIG. 3 A, a VUV device structure for characterizing silica VUV transmission using a commercial krypton lamp and a magnesium fluoride interlayer coated with various thicknesses (0 to 100 nm) of silica is shown. In FIG. 3B, silica coatings having thicknesses of 10 nm, 25 nm, 50 nm, and 100 nm are tested. A normalized signal obtained by the DUT versus ionization potentials for different thicknesses of silica coating is shown.

[0039] FIGS. 4A-4C. FIG. 4A shows a setup used to characterize the PID lifetime. A flame ionization detector (FID), which is assumed to have no degradation, is fluidically connected to the SIPID as the calibration detector. FIG. 4B shows a krypton (Kr) containing UV lamp based PIDs for lifetime test shows - (1) a control PID without any interlayer (z.e., the Kr lamp is directly placed and sealed on the top of the microfluidic chip); (2) a PID with a bare LiF interlayer; (3) a PID with a LiF interlayer coated with 10 nm silica on both sides. Note that only the bottom surface of the interlayer is exposed to microfluidic channels and hence the ambient environment. The top surface is sealed by surrounding UV-epoxy, which is assumed to have no water vapor coming from outside. FIG. 4C shows signal over aging time obtained by the three devices in FIG. 4B. The signals from each device are normalized to its 0thhour data. The PIDs are aged in ambient with temperature of 19.7±0.7°C and relative humidity of 41.5+10.4%. The signal of the PIDs is periodically measured using benzene (Ionization Potential = 9.2 eV). The Kr lamps and the FID are turned off during aging intervals. Error bars are obtained with 3 measurements.

[0040] FIGS. 5A-5F. FIG. 5 A shows simulating Argon plasma aging. (Left) Conceptual design of an argon lamp with silica coating on built-in LiF facing inward. (Right) The aging effectsin an Argon-lamp setting illustrated on the left are simulated by placing (1) bare and (2) silica- coated LiF interlayers inside an Argon plasma chamber. FIG. 5B shows a device structure for testing VUV degradation of bare and silica-coated LiF interlayers after they are aged in the Argon plasma chamber in FIG. 5A. During the test, an adhesive tape is used to sandwich the LiF interlayer between the Argon lamp and the microfluidic chip. The LiF interlayer is disassembled after each test and placed back to the Argon plasma chamber for further aging. In FIG. 5C, a normalized signal of the device in FIG. 5B with respect to the argon plasma aging time for both bare and silica-coated LiF interlayer (10 nm coated on both sides) using heptane (IP = 10.1 eV) as the analyte. The signal is normalized to that obtained at the Oth hour for each interlayer. The testing protocol is the same as described and shown in FIGS. 4A-4C. FIGS. 5D-5F are transmission spectra of a bare and silica-coated LiF (5 nm and 10 nm on both sides) interlayers at different Argon plasma aging times. F and M refer to F color center and M color center, respectively.

[0041] FIGS. 6A-6C. Transmission spectra of aged built-in LiF using (FIG. 6A) thermal bleaching (annealing at 350°C in ambient) and (FIG. 6B) deep ultraviolet (DUV) bleaching (illuminated under 2400 pW / cm2at 245 nm in ambient) for a regenerable VUV window. All aged LiF samples are dissembled from in-situ aged Argon lamps. Inset in FIG. 6A shows the photos of the built-in LiF sample at 0thhour and after 40 hours of thermal bleaching. F and M refer to F color center and M color center, respectively. FIG. 6C shows F band (250 nm) transmission versus bleaching time of aged built-in LiF samples extracted from FIGS. 6 A and 6B, respectively. The arrows in FIGS. 6A and 6B indicate the F band trend during thermal and DUV bleaching processes.

[0042] FIGS. 7A-7B. A device structure for testing the VUV transmission enhancement of an aged built-in LiF interlayer by thermal bleaching in a regenerable VUV unit is shown in FIG. 7A. The aged built-in LiF interlayer is dissembled from an aged Argon lamp and thermally bleached (annealing at 350°C in ambient). FIG. 7B shows VUV transmission enhancement versus thermal bleaching time. Heptane (Ionization Potential = 10.1 eV) is used as the test analyte. Inset: corresponding UV-VIS transmission spectra of the tested built-in LiF at different bleaching times.

[0043] FIGS. 8A-8D. FIG. 8D shows a generic device structure of a silica-integrated photoionization detector (SIPID) including a vacuum ultraviolet (VUV) lamp, an interlayer of silica-coated VUV window, and a microfluidic channel as part of the PID. The VUV lamps are commercially available, which come with a 1 -mm- thick built-in MgF2 and LiF transmissive window for a Krypton (Kr) and Argon (Ar) lamp, respectively. FIG. 8B shows a photograph of a microfluidic chip bonded with a 10 nm- silica-coated 0.5 mm thick MgF2 interlayer. FIG. 8Cshows a micrograph of the center of the spiral microfluidic channel in FIG. 8B. The labeled Cr and Au are on the top MgF2 window and the bottom silicon, respectively. FIG. 8D show a microfabrication process - (I) anodic bonding; (II) e-beam evaporation and lift-off; (III) deep reactive-ion etching (DRIE); (IV) plasma-enhanced chemical vapor deposition (PECVD); (V) evaporation and Au / Cr etch; (VI) Au- Au cold- welding.

[0044] FIGS. 9A-9D. FIG. 9A shows a device structure of an SIPID using a commercial Kr lamp and a MgF2 interlayer coated with various thicknesses (0 to 100 nm) of protective silica layers. FIG. 9B shows a setup used to characterize the silica VUV transmission. The analytes with a range of ionization potentials (IPs) were injected via a bench-top gas chromatography (GC) injector. Two Kr-based PIDs were connected in series. The one without silica coating (z.e., 0 nm silica thickness) was used to calibrate the signal obtained by the other one (e.g... the device under test - DUT) coated with various thicknesses of silica. FIG. 9C shows normalized signal obtained by the DUT versus ionization potentials for different thicknesses of silica coating. The normalization is defined as the ratio of peak areas of respective analytes (with corresponding ionization potentials) between the DUT with a silica coating and the DUT having a bare interlayer without any coating. FIG. 9D shows a normalized signal, which reflects the overall VUV transmission efficiency of the silica coating, extracted from FIG. 9C for different silica coating thicknesses. A single exponential function (exp(-k*x)) is used to fit each curve at respective ionization potentials for extracting the corresponding pseudo-absorption coefficients. Inset: pseudo-absorption coefficient vs. ionization potential. The vertical dashed line indicates 10.6 eV. Error bars were obtained with 3 measurements.

[0045] FIGS. 10A-10C. FIG. 10A shows a schematic of a system setup used to characterize the PID lifetime. A flame ionization detector (FID), assumed to have no degradation, was fluidically connected to the SIPID as the calibration detector. FIG. 10B shows a Kr lamp based PIDs for lifetime test - (1) control PID without any interlayer (e.g., the Kr lamp was directly placed and sealed on the top of the microfluidic chip); (2) PID with a bare LiF interlayer; (3) PID with a LiF interlayer coated with 10 nm silica on both sides in accordance with certain aspects of the present disclosure. Note that only the bottom surface of the interlayer was exposed to microfluidic channels and hence the ambient environment. The top surface was sealed by surrounding UV-epoxy, which is assumed to have no water vapor coming from outside. FIG. 10C shows signal over aging time obtained by the three devices in FIG. 10B. The signals from each device are normalized to its relative sensitivity (z.e., PID / FID) at the 0thhour. The PIDs were aged in ambient with a temperature of 19.7±0.7°C and relative humidity of 41.5+10.4%. The signal of the PIDs was periodically measured using benzene (IP = 9.2 eV). The Kr lamps and the FID wereturned off without carrier gas during aging intervals. Error bars were obtained with 3 measurements.

[0046] FIGS. 11A-11D. FIG. 11A shows a signal of Ar-SIPIDs (with and without silica) for heptane (IP = 10.1 eV) versus time. The signals from each device are normalized to its relative sensitivity at the 0thhour. Inset: Ar lamp based SIPIDs (Ar-SIPID) with (1) bare EiF interlayer as a control and (2) silica-coated (10 nm) EiF interlayer. The normalized signals for two other analytes, toluene (8.8 eV) and dichloromethane (11.3 eV). The aging protocol was the same as in FIG. 10C that the plasma was only turned on during each measurement point. FIG. 11B shows a normalized signal of another Ar-SIPID in continuous operation (z.e., the Ar lamp was turned on throughout the aging experiment) versus aging time for benzene (IP = 9.2 eV) and dichloromethane (DCM, IP = 11.3 eV). Dash lines are the fitting curves of a single exponential decay function (A*exp(-k*x)+C). The exponential decay constants are k = 0.53 h'1and 1.14 h'1for benzene and DCM, respectively. A and C are fitting constants. FIG. 11C shows transmission spectra of pristine EiF, aged interlayer EiF, and aged built-in EiF. F and M refer to the F color center and M color center, respectively. The aged interlayer and the built-in EiF windows were dissembled from the 700-hour aged control Ar-SIPID (z.e. , without silica). The inset shows a photo of the dissembled aged built-in EiF window. FIG. 1 ID shows a conceptual illustration of different degradation agents generated by Argon plasma and their exposure to built-in and interlayer EiF windows - (1) Ar*: Argon excited state; (2) Ar+: Argon ion; (3) e": electron; (4) hv: VUV photon.

[0047] FIGS. 12A-12F. FIG. 12A shows a schematic simulating Ar plasma aging. On the left is a conceptual design of an Ar lamp with silica coating on built-in EiF facing inward. On the right, the aging effects in an Argon-lamp setting illustrated on the left were simulated by placing (1) bare and (2) silica-coated EiF interlayers inside an Argon plasma chamber. FIG. 12B shows a device structure for testing VUV degradation of bare and silica-coated EiF interlayers after they were aged in an Argon plasma chamber in FIG. 12A. During the test, a stretchable tape was used to sandwich the EiF interlayer between the Argon lamp and the microfluidic chip. After each test, the EiF interlayer was disassembled and placed back in the Argon plasma chamber for further aging. FIG. 12C shows a normalized signal of the device in FIG. 12B with respect to the argon plasma aging time for both bare and silica-coated EiF interlayer (10 nm coated on both sides) using benzene (IP = 9.2 eV) as the analyte. The signal is normalized to the relative sensitivity obtained at the 0thhour for each interlayer. Error bars were obtained with 3 measurements. FIGS. 12D-12F show transmission spectra of a bare and silica-coated EiF (5 nm and 10 nm on both sides) interlayer at different Ar plasma aging times. An inset in FIG. 12F shows the photos of agedsamples of bare, 5 nm silica-coated, and 10 nm silica-coated LiF. F and M in FIG. 12D refer to the F color center and the M color center, respectively.

[0048] FIGS. 13A-13B. FIG. 13A shows transmission spectra of aged built-in and interlayer LiF using thermal bleaching (annealing at 350 °C in ambient). The aged LiF samples were dissembled from the Ar-SIPID after 700 h of aging shown in FIG. 11B. F and M refer to the F color center and the M color center, respectively. An inset in FIG. 13A shows the photos of the built-in LiF sample at the 0thhour and after 40 hours of thermal bleaching. The arrows in FIG. 13A indicate the F band trend during thermal bleaching process. FIG. 13B shows VUV transmission enhancement versus thermal bleaching time. Heptane (IP = 10.1 eV) was used as the test analyte. Inset: corresponding UV-VIS transmission spectra of the tested built-in LiF at different thermal bleaching times. An aged built-in LiF was dissembled from an aged Ar-lamp and bleached by thermal annealing. The VUV enhancement is normalized to the relative sensitivity obtained at the 0thhour. Error bars were obtained with 3 measurements.

[0049] Corresponding reference numerals indicate corresponding parts throughout the several views of the drawings.DETAILED DESCRIPTION

[0050] Example embodiments are provided so that this disclosure will be thorough, and will fully convey the scope to those who are skilled in the art. Numerous specific details are set forth such as examples of specific compositions, components, devices, and methods, to provide a thorough understanding of embodiments of the present disclosure. It will be apparent to those skilled in the art that specific details need not be employed, that example embodiments may be embodied in many different forms and that neither should be construed to limit the scope of the disclosure. In some example embodiments, well-known processes, well-known device structures, and well-known technologies are not described in detail.

[0051] The terminology used herein is for the purpose of describing particular example embodiments only and is not intended to be limiting. As used herein, the singular forms “a,” “an,” and “the” may be intended to include the plural forms as well, unless the context clearly indicates otherwise. The terms “comprises,” “comprising,” “including,” and “having,” are inclusive and therefore specify the presence of stated features, elements, compositions, steps, integers, operations, and / or components, but do not preclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups thereof. Although the open-ended term “comprising,” is to be understood as a non-restrictive term used to describe and claim various embodiments set forth herein, in certain aspects, the term may alternatively beunderstood to instead be a more limiting and restrictive term, such as “consisting of’ or “consisting essentially of.” Thus, for any given embodiment reciting compositions, materials, components, elements, features, integers, operations, and / or process steps, the present disclosure also specifically includes embodiments consisting of, or consisting essentially of, such recited compositions, materials, components, elements, features, integers, operations, and / or process steps. In the case of “consisting of,” the alternative embodiment excludes any additional compositions, materials, components, elements, features, integers, operations, and / or process steps, while in the case of “consisting essentially of,” any additional compositions, materials, components, elements, features, integers, operations, and / or process steps that materially affect the basic and novel characteristics are excluded from such an embodiment, but any compositions, materials, components, elements, features, integers, operations, and / or process steps that do not materially affect the basic and novel characteristics can be included in the embodiment.

[0052] Any method steps, processes, and operations described herein are not to be construed as necessarily requiring their performance in the particular order discussed or illustrated, unless specifically identified as an order of performance. It is also to be understood that additional or alternative steps may be employed, unless otherwise indicated.

[0053] When a component, element, or layer is referred to as being “on,” “engaged to,” “connected to,” or “coupled to” another element or layer, it may be directly on, engaged, connected or coupled to the other component, element, or layer, or intervening elements or layers may be present. In contrast, when an element is referred to as being “directly on,” “directly engaged to,” “directly connected to,” or “directly coupled to” another element or layer, there may be no intervening elements or layers present. Other words used to describe the relationship between elements should be interpreted in a like fashion (e.g., “between” versus “directly between,” “adjacent” versus “directly adjacent,” etc.). As used herein, the term “and / or” includes any and all combinations of one or more of the associated listed items.

[0054] Although the terms first, second, third, etc. may be used herein to describe various steps, elements, components, regions, layers and / or sections, these steps, elements, components, regions, layers and / or sections should not be limited by these terms, unless otherwise indicated. These terms may be only used to distinguish one step, element, component, region, layer or section from another step, element, component, region, layer or section. Terms such as “first,” “second,” and other numerical terms when used herein do not imply a sequence or order unless clearly indicated by the context. Thus, a first step, element, component, region, layer or section discussed below could be termed a second step, element, component, region, layer or section without departing from the teachings of the example embodiments.

[0055] Spatially or temporally relative terms, such as “before,” “after,” “inner,” “outer,” “beneath,” “below,” “lower,” “above,” “upper,” and the like, may be used herein for ease of description to describe one element or feature's relationship to another element(s) or feature(s) as illustrated in the figures. Spatially or temporally relative terms may be intended to encompass different orientations of the device or system in use or operation in addition to the orientation depicted in the figures.

[0056] Throughout this disclosure, the numerical values represent approximate measures or limits to ranges to encompass minor deviations from the given values and embodiments having about the value mentioned as well as those having exactly the value mentioned. Other than in the working examples provided at the end of the detailed description, all numerical values of parameters (e.g., of quantities or conditions) in this specification, including the appended claims, are to be understood as being modified in all instances by the term “about” whether or not “about” actually appears before the numerical value. “About” indicates that the stated numerical value allows some slight imprecision (with some approach to exactness in the value; approximately or reasonably close to the value; nearly). If the imprecision provided by “about” is not otherwise understood in the art with this ordinary meaning, then “about” as used herein indicates at least variations that may arise from ordinary methods of measuring and using such parameters. For example, “about” may comprise a variation of less than or equal to 5%, optionally less than or equal to 4%, optionally less than or equal to 3%, optionally less than or equal to 2%, optionally less than or equal to 1%, optionally less than or equal to 0.5%, and in certain aspects, optionally less than or equal to 0.1%.

[0057] In addition, disclosure of ranges includes disclosure of all values and further divided ranges within the entire range, including endpoints and sub-ranges given for the ranges.

[0058] Example embodiments will now be described more fully with reference to the accompanying drawings.

[0059] Photoionization detectors (PIDs) are widely used for detecting volatile organic compounds (VOCs). Additionally, benefiting from its small footprint, lamp-based PIDs have been implemented in many field applications like environmental monitoring, industrial hygiene, and healthcare, and the like. Conventionally, a VUV lamp is filled with low-pressure xenon (Xe, VUV photon energy up to 9.9 eV), krypton (Kr, up to 10.6 eV), or argon (Ar, up to 11.7 eV). Usually, a MgF2 window is used for Kr and other lamps whose emitted photon energy is lower than 10.6 eV (or, equivalently, wavelength >117 nm). However, for an Ar lamp, which emits 11.7 eV (106 nm in wavelength) photons and can ionize the VOCs whose ionization potential is higher than 10.6 eV, a LiF window, which has a high transmission near 11.7 eV, needs to be used.

[0060] All these VUV windows, particularly, the LiF window, are highly susceptible to moisture (hygroscopicity) and color center formation (solarization) caused by highly energetic ions and VUV photons. While a MgF2 window provides reliable operation over 3,000 hours, a LiF window lasts only approximately 300 hours due to higher hygroscopicity, faster solarization, and fill gas leak resulting from the larger mismatch of the LiF thermal expansion coefficient (CTE) to the glass lamp housing.

[0061] FIG. 1A generally illustrates the mechanisms that cause a vacuum ultraviolet lamp 20 having a transmissive window 26 (e.g., LiF or other window materials) that loses its VUV transmission ability. In FIG. 1A, an ultraviolet radiation chamber 22 contains a noble gas 34 used to generate ultraviolet photons that pass through the transmissive window 26 into an exterior environment 28. An inner side of the transmissive window 26 is exposed to the gas 24 in the ultraviolet radiation chamber 22. During operation, the gas 24 in the ultraviolet radiation chamber 22 may have various ions and excited atoms (here, shown as argon (Ar+) ions and reactive and / or excited atoms (Ar*)), electrons (e"), and VUV (hv) photons, all of which can chemically react with and attack the transmissive window 26. An outer side of the transmissive window 26 (on a side opposite to the ultraviolet radiation chamber) is exposed to VUV photons and the external environment 28. Thus, the outer side of the transmissive window 26 may react with moisture (water molecules) present in the external environment 28.

[0062] FIG. IB shows photographs of a yellowing effect on the transmissive window of the VUV lamp that indicates a significantly reduced transmission for a transmissive (e.g., LiF) window mounted in an argon lamp after 700 hours in an ambient environment, during which the argon lamp is turned for only a couple of hours.

[0063] In various aspects, the present disclosure provides a VUV lamp design that can protect the lamp from the attack generated by ions, electrons, and excited gas molecules within the lamp chamber, and moisture outside of the lamp chamber, while still ensuring good VUV transmission from the ultraviolet radiation chamber, for example, greater than or equal to about 60% and optionally greater than or equal to about 70% of photons ranging from 8.5 to 11.5 eV. By way of example, one suitable design is illustrated in FIG. 2A showing a vacuum ultraviolet (VUV) lamp 30 that includes an ultraviolet radiation chamber 32 filled with a gas 34. The ultraviolet radiation chamber 32 is configured to generate ultraviolet radiation or ultraviolet photons (hv). The gas 34 may be an inert gas selected from the group consisting of: argon (Ar), krypton (Kr), xenon (Xe), and combinations thereof. In certain variations, the ultraviolet radiation chamber is a microfluidic chamber and has a total volume of less than about 10 microliters (pL). By way of example only, FIG. 2A shows the gas 34 as being argon that generates argon ions (Ar+),reactive argon molecules (Ar*), electrons (e‘), and photons (hv). The gas may have a reduced pressure within the ultraviolet radiation chamber 32. The ultraviolet radiation chamber 32 is sealed at a terminal end by a transmissive window 40 that retains gas 34 inside the ultraviolet radiation chamber 32 but permits ultraviolet photons (hv) to pass therethrough.

[0064] The light source / VUV lamp 30 thus generates light or electromagnetic radiation / photons, which are directed through the transmissive window 40 towards a target (such as an ionization chamber in a photoionization detector device). Particularly suitable light generated in the ultraviolet radiation chamber 32 falls within the ultraviolet electromagnetic radiation spectrum. In certain variations, the light may be ultraviolet radiation (UV) (including ultraviolet A, ultraviolet B, ultraviolet C, near ultraviolet, middle ultraviolet, far ultraviolet, extreme ultraviolet, and vacuum ultraviolet) having a wavelength of greater than or equal to about 10 nm to less than or equal to about 400 nm. In still other variations, the light may be ultraviolet radiation with wavelengths in a range of greater than or equal to about 100 nm to less than or equal to about 400 nm (including ultraviolet A, ultraviolet B, ultraviolet C). Notably, the light may be filtered light, focused light, polarized light, or may be extra- spectral or a mixture of different wavelengths.

[0065] According to various aspects of the present disclosure, the transmissive window 40 includes a primary layer 50, which may be considered to be a conventional transmissive window for a VUV lamp. The primary layer 50 may thus be formed of a material selected from the group consisting of: magnesium fluoride (MgF2), calcium fluoride (CaF2), lithium fluoride (LiF), and combinations thereof. In accordance with various aspects of the present disclosure, the primary layer 50 of the transmissive window 40 further comprises at least one protective layer 60 disposed adjacent to the primary layer 50. The protective layer 60 may comprise a transmissive dielectric material. The transmissive dielectric material is transmissive to ultraviolet radiation / photons and further resists reaction with water and plasma or other reactive molecules present in the ultraviolet radiation chamber. In certain aspects, the transmissive dielectric material may be selected from the group consisting of: silicon dioxide (SiCT), silicon nitride (SisN4), aluminum oxide (AI2O3), and combinations thereof. By transmissive layer, it is meant that the material is transparent to ultraviolet electromagnetic radiation so that greater than or equal to about 60 % of target wavelengths, for example, in the range of greater than or equal to about 100 nm to less than or equal to about 400 nm, transmit therethrough. Notably, in the variation shown in FIG. 2A, this protective layer 60 may be applied to a prefabricated VUV lamp having an existing primary layer 50 transmissive window.

[0066] Thus, the transmissive VUV window 40 is coated with the protective dielectric layer 50 that is transmissive to UV photons (such as silica, silicon nitride, or aluminum oxide) and may be disposed on either side or both sides of the primary layer 50. If the dielectric protective layer / coatings 60 are on both sides, the same or different dielectric materials with the same or different thicknesses can be used. In various aspects, the protective layer 60 may be a thin film layer or coating, for example, having a maximum average thickness of less than or equal to about 500 nm, optionally less than or equal to about 400 nm, optionally less than or equal to about 300 nm, optionally less than or equal to about 250 nm, optionally less than or equal to about 200 nm, optionally less than or equal to about 150 nm, optionally less than or equal to about 100 nm, optionally less than or equal to about 75 nm, optionally less than or equal to about 50 nm, optionally less than or equal to about 25 nm, and in certain variations, optionally less than or equal to about 20 nm. In certain variations, each protective layer 60 may respectively have an average thickness of greater than or equal to about 0.5 nm to less than or equal to about 500 nm, optionally of greater than or equal to about 0.5 nm to less than or equal to about 250 nm, optionally greater than or equal to about 0.5 nm to less than or equal to about 100 nm, optionally greater than or equal to about 0.5 nm to less than or equal to about 50 nm, optionally greater than or equal to about 0.5 nm to less than or equal to about 25 nm, optionally greater than or equal to about 0.5 nm to less than or equal to about 20 nm, and in certain variations, optionally greater than or equal to about 0.5 nm to less than or equal to about 10 nm. Where multiple protective layers (like 60) are included for the transmissive window, they may be compositionally distinct from one another or the same compositionally. Further, where multiple protective layers or coatings are used, they may have the same or distinct thicknesses from one another.

[0067] This dielectric protective coating 60 forms a thin but dense layer that blocks ions, excited gas molecules, electrons, and water vapor molecules from coming into contact with the primary layer 50, thus protecting the primary layer 50 to enhance the reliability of the VUV window 40 and hence the whole VUV lamp 30 lifetime. The protective coating 60 may be deposited via various coating methods, including any microfabrication process for dielectric deposition, such as plasma-enhanced chemical vapor deposition (PECVD), sputtering, atomic layer deposition (ALD), and the like. The VUV lamp 30 may be a discharge chamber in a PID device, as will be described further below.

[0068] Notably, in certain aspects, the transmissive window assembly 40 including at least a primary layer 50 and at least one protective layer 60 comprising a transmissive dielectric material has a transmissivity for ultraviolet photons of greater than or equal to about 60%, optionally greater than or equal to about 70%, optionally greater than or equal to about 75%, optionallygreater than or equal to about 80%, and in certain variations, optionally greater than or equal to about 85%.

[0069] It should be noted that while thin metal coatings (for example, a few nanometers in thickness) had been known to be VUV transmissive and previously used to coat the exterior side of a VUV window, these metal coatings suffer from a few drawbacks. First, a thin metal coating on the outer window surface in the nanometer thickness range may not form a dense and continuous protective layer, but rather may have pinholes and defects which still allow water vapor molecules to go through the pores in the metal coating and attack the VUV window. Second, in some cases a metal coating on the outer window surface cannot be used because it may cause an electrical short circuit (such as in the case where it is integrated into a microfluidic photoionization detector, in which the metal coating is in electrical contact with the two electrodes, such as electrically conductive silicon walls). Third, a metal coating cannot be used on the inner side of the VUV window, as it may destroy plasma generation in the VUV chamber. Fourth, a thin metal coating tends to degrade faster (e.g., corrosion) in high humidity atmosphere by itself compared to the dielectrics provided by the present disclosure, so that it impairs the overall VUV transmission. Lastly, relatively stable metals, such as gold, are costly for large scale manufacturing.

[0070] FIGS. 2B-2D show alternative variations of VUV lamps prepared in accordance with various aspects of the present disclosure. To the extent that the components are the same as those described in the context of FIG. 2A, unless otherwise addressed, these components and their properties will not be repeated herein for brevity. FIG. 2B shows a first variation of a vacuum ultraviolet (VUV) lamp 30A. In FIG. 2B, a transmissive window 40A defines a first side 42 exposed to an ultraviolet radiation chamber 32 and an opposite second side 44 that faces an external environment 46. The transmissive window 40A includes not only a primary layer 50 and a first protective layer 60 comprising a transparent dielectric material (discussed above) disposed on the second side 44, but also a second protective layer 62 comprising a transparent dielectric material (discussed above) on the second side 44. In this variation, the transmissive window 40A is protected from both the plasma and reactive species from gas 34 inside the ultraviolet radiation chamber 32 on the first side 42 as well as being protected from moisture and reactive species in the external environment 46 on the second side 44. However, the transmissive window 40A still permits ultraviolet photons (hv) to pass therethrough, for example, having the transmissivity levels described above, for example, permitting greater than or equal to about 60% and in certain variations, optionally greater than or equal to about 70% or more of photons to pass.

[0071] FIG. 2C shows a second variation of a vacuum ultraviolet (VUV) lamp 30B. In FIG. 2C, a transmissive window 40B defines a first side 42 exposed to an ultraviolet radiation chamber 32 and an opposite second side 44 that faces an external environment 46. The transmissive window 40B includes not only a first primary layer 50 as described above on the first side 42 of transmissive window 40B, but further includes a protective interlayer assembly 70 on the second side 44. The protective interlayer assembly 70 includes a first protective layer 60 comprising a transparent dielectric material (discussed above), a second primary layer 52 like the primary layer 50 described above, and a second protective layer 64 also comprising a transparent dielectric material (discussed above). In this variation, the transmissive window 40B is protected from moisture and reactive species in the external environment 46 on the second side 44. However, the transmissive window 40B still permits ultraviolet photons (hv) to pass therethrough, for example, having the transmissivity levels described above, for example, permitting greater than or equal to about 60% and in certain variations, optionally greater than or equal to about 70% or more of photons to pass. Notably, in the variation shown in FIG. 2C, like in FIG. 2A, this protective interlayer assembly 70 may be applied to a prefabricated VUV lamp having an existing first primary layer 50 transmissive window.

[0072] While the aforementioned embodiments incorporating protective dielectric coating(s) increase the VUV window lifetime, the VUV window may still degrade over time due to long durations of operation. To further extend the VUV window and the lamp lifetime, FIG. 2D shows another embodiment of a regenerable vacuum ultraviolet (VUV) lamp 30D. To the extent that the components of the VUV lamp 30D are the same as those described in the context of FIG. 2A, unless otherwise addressed, these components and their properties will not be repeated herein for brevity. Notably, any of the VUV lamp embodiments previously described, including those in the context of FIGS. 2A-2C, may be used in such a regenerable VUV lamp 30D. A transmissive window 40D is shown by way of example that includes a primary layer 50, a first protective layer 60 comprising a transparent dielectric material (discussed above), and a second protective layer 62 comprising a transparent dielectric material (discussed above). A regenerator component 80 is disposed adjacent to an ultraviolet radiation chamber 34 and transmissive window 40D. The regenerator component 80 may be a heater and / or a deep ultraviolet (DUV) radiation generator. The regenerator component 80 may be integrated into the VUV lamp assembly or housing. The regenerator component 80 may have a first state and a second state. In the first operational state, the regenerator component 80 may be dormant or off. In the circumstance where the transmissive window 40D yellows or transmission of photons otherwise diminishes, the regenerator component 80 can be activated into a second operational state. Theregenerator component 80 is configured to selectively generate waves 82, for example, heat or deep ultraviolet (DUV) radiation (e.g., having a wavelength of about 245 nm), directed towards the transmissive window 40D. The exposure to the waves 82, whether heat or DUV radiation, can enhance or restore transmission of the ultraviolet photons through the transmissive window 40D. For example, the VUV transmissive window 40D can be heated to a predetermined temperature (e.g., from greater than ambient up to about 350°C) for a certain amount of time (where the higher the temperature during heating, the less time is required). Notably, the heating temperature may be limited by the sealant used on the transmissive window 40D, so that in circumstances where a high temperature sealant / adhesive or other high-temperature stable bonding technique is used, the regenerator component 80 heater may be used at higher temperatures, potentially exceeding 350°C for shorter durations. The VUV transmissive winder 40D may be illuminated for a predetermined amount of time by VUV radiation, or a combination of both heating and DUV radiation can regenerate the VUV transmissive window 40D so that it recovers its VUV transmission ability.

[0073] In certain aspects, the present disclosure contemplates methods of making a robust vacuum ultraviolet (VUV) lamp. Such a method may comprise applying a transmissive dielectric material coating via a deposition process to one or more surfaces of a primary layer for a transmissive window for a VUV lamp. In certain variations, the method also comprises applying a second transmissive dielectric material coating via a deposition process on another surface of the primary layer. Suitable deposition processes include atomic layer deposition (ALD), physical vapor deposition (PVD), chemical vapor deposition (CVD), including plasma enhanced CVD, and the like. In certain aspects, the surface coating of the transmissive dielectric material may be applied by an atomic layer deposition (ALD) process that can coat the primary layer of the transmissive window, such as lithium fluoride or magnesium fluoride, with a conformal layer that comprises the dielectric oxide-based layer, such as silicon dioxide (SiCL) or aluminum oxide (AI2O3) or alternatively a nitride-based layer, such as silicon nitride (SisN4). ALD is a self-limiting process for chemical deposition of ultrathin films on a substrate and typically involves subjecting the target substrate to self- saturating surface reactions. The surface reactions may be conducted sequentially and / or in an alternating fashion, depending on the composition and structure of the film desired.

[0074] ALD can be conducted in an apparatus having a vacuum deposition chamber with a holder for the substrate (or in the case of large- volume production, with two rotating rolls for roll-to-roll processing), at least one vapor source (known as the precursor) and various controls by which the substrate may be individually subjected to the vapor source. Such controls may include heaters, coolers, flow routing and valves, for controlling the amount of exposure of thesubstrate to the vapor source. The ALD process for deposition of surface coating onto regions of the primary material of the transmissive window may involve reaction of the surface in a deposition chamber with a single vapor of precursor materials or reaction of the surface with multiple vapors introduced sequentially and having the precursors of the surface coating. Suitable precursors may include organic and inorganic metallic compounds. The vapor may be pulsed into the vacuum deposition chamber on a carrier gas and may be rapidly purged, e.g., by vacuum pumping and / or flushing with an inert gas. Such pulsing of the vapor and purging of the system may be performed to control the dose of the precursor vapor to which the substrate is exposed.

[0075] Generally, the ALD process is performed at elevated temperatures and reduced pressures. Temperature within the deposition chamber is desirably high enough that reaction between the substrate and the precursors in the vapor occurs, while also preventing condensation of the vapor onto the surface. As non-limiting examples, the reaction space in the deposition chamber may have a temperature of room temperature (e.g., approximately 21 °C) to about 600°C (for depositing coating directly on the primary layer) and the operating pressure may be between about 1 Pa to about 5,000 Pa.

[0076] As the ALD process is conducted, a single atomic layer of the surface coating material may be bound to the primary layer surface via surface reactions, thereby providing a monoatomic coating. With sequential or alternating reactions, composite layers may be formed. Furthermore, additional atomic monolayers may be grown over the monoatomic layer, thereby forming a surface coating having greater thicknesses.

[0077] The ALD process is illustrative of one technique for forming transmissive dielectric coatings on a transmissive window, but other deposition processes may likewise be used.

[0078] The present disclosure also contemplates a robust photoionization detector (PID), which may be a microfluidic PIC. Such a PID may comprise an ionization chamber having an inlet that receives a fluid sample and an outlet through which the fluid sample exits the ionization chamber. Further, a first electrode and a distinct second electrode in electrical communication with the microfluidic ionization chamber. The PID also includes an integrated vacuum ultraviolet (VUV) lamp prepared in accordance with various aspects of the present disclosure described above. For example, the PID may have an ultraviolet radiation chamber that is configured to generate ultraviolet photons that comprises a gas selected from the group consisting of: argon (Ar), krypton (Kr), xenon (Xe), and combinations thereof. Further, there is a transmissive window disposed between the ionization chamber and the ultraviolet radiation chamber that permits the ultraviolet photons to pass from the ultraviolet radiation chamber into the ionization chamber. Thetransmissive window comprises multiple layers including a primary layer comprising a first material selected from the group consisting of: magnesium fluoride, calcium fluoride, lithium fluoride, and combinations thereof, and at least one protective layer disposed adjacent to the primary layer comprising a transmissive dielectric material selected from the group consisting of: silicon dioxide (S i O2), silicon nitride (SisN4), aluminum oxide (AI2O3), and combinations thereof. Any of the VUV lamp variations described above, including the regenerable VUV lamp with a regenerator component, may be incorporated into the PID device.

[0079] In certain variations, the ionization chamber is a microfluidic ionization chamber having one or more microfluidic channels each having a total volume of less than about 10 pL.

[0080] In certain aspects, the present disclosure provides microfluidic photoionization detectors (pPID) based on silicon chips that are able to rapidly and sensitively detect volatile compounds. In the past, applications of pPID were limited by the manual assembly process that involves using a glue that may potentially outgas and clog the fluidic channel, and by the short lifetime of the vacuum ultraviolet (VUV) lamps (especially, Argon lamps). Here, the present disclosure contemplates in certain variations, a gold-gold cold welding-based microfabrication process to integrate ultrathin (10 nm) silica into pPID. The silica coating not only enables direct bonding of the VUV window to silicon under amicable conditions, but also works as a moisture and plasma exposure barrier for the primary layer of VUV windows (e.g., MgF2 and LiF) that are highly susceptible to hygroscopicity and solarization. Detailed characterization of the silica coating is provided in the examples below, showing that the 10 nm silica coating allows 40% to 80% VUV transmission from 8.5 eV to 11.5 eV. It is further shown that the silica-protected pPID maintains 90% of its original sensitivity after 2,200 hours of exposure to ambient conditions (with a temperature of 19.7±0.7°C and a relative humidity of 41.5+10.4 %), compared to 39% without silica. Furthermore, Argon plasma inside an Argon VUV lamp was identified as the dominant degradation source (other than moisture effect) for the LiF window with color centers formation in UV-VIS and VUV transmission spectra. Ultrathin silica is also effective in protecting the LiF from Argon plasma exposure. Lastly, thermal annealing (350°C in ambient) was found to bleach the color centers and restore VUV transmission of degraded LiF windows effectively.

[0081] Examples

[0082] Example 1

[0083] Silica (SiCL) is used as the example dielectric for demonstration throughout this example. First, the reduction of VUV transmission by the thin silica coating on a transmissive window is examined. In FIG. 3A, a device structure for characterizing silica VUV transmission using a commercial Kr lamp and a MgF2 interlayer coated with various thicknesses (0 to 100 nm)of silica formed through plasma-enhanced chemical vapor deposition is shown. Two Kr-based PIDs are connected in series. The one without silica coating (z.e., 0 nm silica coating thickness) is used to calibrate the signal obtained by the other one (e.g., the device under test - DUT) coated with various thicknesses of silica. A bench-top gas chromatography injector is used for injection of a range of analytes with ionization potentials from 8.5 to 10.5 eV. In FIG. 3B, silica coatings having thicknesses of 10 nm, 25 nm, 50 nm, and 100 nm are tested. A normalized signal obtained by the DUT versus ionization potentials for different thicknesses of silica coating is shown. The normalization is defined as the ratio of peak areas of respective analytes between DUT and the calibration PID at corresponding ionization potentials. Thus, a normalized signal is equivalent to the VUV transmission, so that a 10 nm silica coating yields the VUV transmission of approximately 75%. With increasing thickness of silica coating, the VUV transmission becomes smaller.

[0084] The moisture exposure barrier performance of the protective transmissive dielectric layers (e.g., when silica is coated outside of the VUV window) of the thin silica is examined by comparing the lifetime of devices shown in FIGS. 4A-4C. The device with a 10 nm silica-coated LiF interlayer still has 83% signal strength at the aging time of 1,900 hours, in comparison to the faster degradation of a control device having 43% signal strength and the device with a bare LiF interlayer (without silica coating) having only 33% signal strength at the same aging time. Over the course of aging, the device with the bare LiF shows the fastest degradation followed by the control device with built-in MgF2 window exposed. The results suggest that the 10 nm silica effectively delays the degradation of the VUV window stack including both LiF and MgF2 windows.

[0085] Next, the performance of the protective coatings comprising the transmissive dielectric materials as barriers to argon plasma exposure (e.g., when silica is coated inside of the VUV window) is examined. An argon plasma chamber is used for simulating the in-situ aging of the LiF window installed on an Argon lamp as shown in FIG. 5A for qualitative demonstration of silica protection of VUV windows from Argon plasma exposure. The VUV transmission change is extracted by inserting the bare and silica-coated LiF as interlayers to a Kr-based PID as shown in FIG. 5B. As shown in FIG. 5C, the silica-coated LiF prepared in accordance with certain aspects of the present disclosure shows an enhanced reliability with a normalized VUV transmission over 100% at the aging time of 12 hours, compared to the bare LiF with only 50% at the same aging time. FIGS. 5D-5F demonstrate the UV-VIS transmission spectra of the bare, 5 nm, and 10 nm silica-coated LiF samples. In the bare LiF, the color centers (F and M band) are developed right after the first 1.5 hours of aging, and the transmission deteriorates upon further aging. In contrast,both 5 nm and 10 nm silica-coated LiF windows show a recovery of F band (which develops during the silica sputtering where Argon is used as the ion source) after the first 1.5 hours of aging, and then the spectra remains stable over the rest of aging time. The recovery of the F band of the silica-coated LiF is consistent with the increasing VUV transmission of silica-coated LiF after 2 hours of aging in FIG. 5C. The results suggest that a thin silica layer can protect the LiF from transmission loss in both VUV and UV-VIS spectra regions caused by argon plasma exposure.

[0086] As noted above, the protective barrier layers may have different thicknesses of silica or other transmissive dielectrics for VUV windows, so that the transmissive window is protected when exposed to moisture and plasma (e.g., argon, krypton, xenon). In addition, in addition to CVD, other fabrication techniques can be used, for example, atomic layer deposition (ALD), that can serve to form a higher density of dielectric for better protection of the primary layer of the transmissive window.

[0087] Example 2

[0088] In addition to protection for enhancing the lifetime of VUV lamps, methods for regenerating the aged VUV windows and hence VUV lamps are explored with following examples.

[0089] First, recovering the transmission (e.g., bleaching) is demonstrated in the UV-VIS regime. As shown in FIGS. 6A-6C, both thermal bleaching (annealing at 350°C in ambient) and deep ultraviolet (DUV) bleaching (illuminated under 2400 pW / cm2at 245 nm in ambient) effectively recovers the UV-VIS transmission of aged LiF transmissive windows by eliminating or reducing the F and M color centers.

[0090] To further examine the effectiveness of bleaching in the VUV regime, an aged built-in LiF transmissive window is inserted as an interlayer in a device structure as shown in FIG. 7A for extracting its VUV transmission recovery by thermal annealing. FIG. 7B suggests that the VUV transmission enhances approximately 5-fold with concomitant approximate 20% UV-VIS transmission restoration at the F band (near 250 nm). These results suggest that by either thermal or DUV bleaching, the UV-VIS and VUV transmission of aged VUV windows can be recovered selectively and simultaneously.

[0091] It should be noted that the above annealing (or bleaching) temperature (350°C) may degrade the adhesive or sealant bonding of the built-in LiF transmissive window to the glass housing of the Argon lamp. For applications where a stable high-temperature adhesive, sealant, or other stable bonding technique is used for adhering and sealing the transmissive window to the remainder of the UV irradiation chamber, higher annealing (or bleaching) temperatures may be used for the regenerating process. For in-situ bleaching of an aged Argon lamp, a lower annealingtemperature or DUV bleaching procedures, or the combination of both may be more practical. To realize thermal bleaching at high temperatures (about 350°C), thermally stable high temperature bonding between VUV windows and VUV lamp body is needed to withstand a high annealing (or bleaching) temperature. As will be described below, in certain variations, the high temperature bonding may be done via a glue-free technique.

[0092] Example 3

[0093] In this example, a silicon chip-based microfluidic PID (pPID) with a spiral channel and a VUV lamp placed on top of it is formed and tested. Due to its flow-through nature and small ionization chamber volume, the pPID has fast responses (approximately 0.01 s). Additionally, a sub-picogram detection limit was achieved. However, as background, previous pPIDs are manually assembled by pressing the lamp’s bottom (e.g., MgF2 transmissive window) against the top of the microfluidic chip and then sealing the edges with a UV curable glue. This process is subject to human errors that may cause gas leakage and a low yield (e.g., glues may accidentally clog the channels), making the entire process less amenable to mass production. Further, the UV curable glue may potentially outgas and produce a background signal. Therefore, it is desirable to integrate a VUV window on top of the microfluidic chip glue-free. Unfortunately, most established hermetic bonding techniques (e.g., eutectic, anodic, and fusion) are not applicable for bonding transmissive window materials like MgF2 or EiF with silicon, since fluoride glass is easy to crack at the high temperatures required for processing (>350°C) due to the large thermal mismatch.

[0094] This example further shown in FIGS. 8A-8D explores (1) glue-free bonding between a VUV lamp and a silicon chip for future high-yield mass production; and (2) increased lifetime of a VUV lamp and hence PID, especially an Ar-based lamp with a EiF window. Here, an integrated pPID with a VUV window coated with an ultrathin (10 nm thick) protective silica layer is formed. A new microfabrication process based on cold welding was developed, enabling a silica-coated VUV window to be bonded directly on top of a silicon chip and resulting in reliable and high-yield assembly of a pPID amenable to industrial- scale production. Additionally, the ultrathin silica coating maintains a good VUV transmission while offering strong protection of a VUV window against humid ambient environments. 40-80% of the original sensitivity (z.e., without the silica coating) was achieved for the VOCs of various ionization potentials (IP, 8.5 - 11.5 eV). Using silica as the protective moisture barrier, it is shown that the silica-protected pPID maintains 90% of its original sensitivity after 2,200 hours of exposure to ambient conditions / environment, as compared to 39% without the protective silica layer.

[0095] Degradation mechanisms of the LiF window in an Ar lamp are also investigated, which show Ar plasma exposure as the dominant degradation source other than the commonly believed moisture effect. Furthermore, ultrathin silica was demonstrated as an effective barrier layer protecting LiF windows from Ar plasma, suggesting a new Ar lamp design according to certain aspects of the present disclosure provide increased lamp lifetime. Finally, thermal bleaching was explored to effectively restore the VUV transmission of degraded LiF windows for future design and manufacturing of regenerable VUV lamps and PIDs.

[0096] Analytical standard grade VOC analytes were purchased from Sigma Aldrich (St. Louis, MO). P-type / Boron Prime silicon (Si) wafers (100 mm in diameter, 400 pm thick, 0.001- 0.053 Q-cm, double-sided-polished (DSP)) were from Ultrasil. Borofloat 33 Pyrex glass wafers (P / N 517) were from University Wafer. Single crystal MgF2 and LiF substrates (<100> orientation, 10 x 10 x 0.5 mm in dimension, DSP, Ra (surface roughness) < 1.5 nm) were from BIOTAIN CRYSTAL CO., LIMITED. Kr VUV lamp (P / N 043-257) was from MOCON (part of AMETEK). Ar VUV lamp (P / N 050-0001-000 (RAE)) was from EQUIPCO. UV-curable epoxy (P / N NOA 68T) was from Norland Products. The transformer (P / N ZS1052(H)-ND) for Kr lamp excitation was from Digikey. The transformer (10KV High Frequency High Voltage Transformer Booster Coil Inverter) for Ar lamp excitation was from eBay. All materials were used as purchased without further purification or modification.

[0097] Microfluidic photoionization detector (pPID) fabrication

[0098] FIG. 8A shows the pPID configuration. The Si and glass wafers were cleaned using piranha solution and then anodically bonded. 30 nm chromium (Cr) / 200 nm gold (Au) were lithographically patterned and evaporated onto the silicon surface using a lift-off process. Another layer of photoresist (PR) was patterned for deep reactive-ion etching (DRIE) through the Si to form microchannels having a cross-section of 390 pm (width) x 400 pm (depth), a wall thickness of 40 pm, and a length of 3.9 cm. The entire spiral channel had an overall size of 4 mm in diameter (see FIG. 8B). The wafer was then diced. Further, a pre-determined thickness of SiO2 was deposited as a protective layer on a MgF2 substrate (z.e., the VUV window) via plasma-enhanced vapor deposition (PECVD), which was used as an interlayer in FIG. 8A. 30 nm Cr / 200 nm Au was evaporated and wet-etched with a pattern matching that of the Si microchannel. Finally, the microfluidic die and the MgF2 die were piranha cleaned and then Au- Au cold-welded through a flip chip bonder at 150°C and under a pressure of 2 MPa in ambient condition for 10 minutes (see FIG. 8C) for the cold- welded interface). As shown in FIG. 8B, the microfluidic die was designed larger than the MgF2 die such that the gold electrodes on the silicon were exposed and accessible for wire bonding. Note that the microfluidic chip described herein was designed for the Kr lampassembly (z.e., Kr pPID). For the Ar lamp (z.e., Ar pPID), due to a larger lamp size, the spiral channel was modified and had a larger overall size of 7 mm in diameter with a length of 10 cm. For the LiF interlayer, due to the restriction of processing LiF in cleanroom facilities, SiCF was sputtered on a LiF substrate, and the silica-coated LiF substrate was then mechanically fixed on the microfluidic chip using UV-curable epoxy. However, the similar microfabrication process developed for the MgF2 interlayer is in principle applicable.

[0099] Next, the integrated microfluidic chip was electrically packaged on a printed circuit board by wire bonding the two gold electrode contacts with aluminum wires of 50 pm diameter using a wedge bonder. Then, two 10 cm long guard columns were inserted into the inlet and outlet ports, respectively, and hermetically sealed with UV-curable epoxy. Finally, the Kr (or Ar) lamps with built-in MgF2 (or LiF) windows were mounted on top of the integrated MgF2 (or LiF) interlayer window and sealed with UV-curable epoxy. Adhesive copper tapes were then applied to the VUV lamps to form two excitation electrodes facing each other for plasma generation. An in-house developed circuit was used for plasma generation and readout.

[0100] pPID sensitivity and reliability characterization

[0101] The sensitivity of the pPIDs was evaluated using an Agilent 6890 benchtop gas chromatography (GC) equipped with a thermal injector and a flame ionization detector (FID). 99.999% Helium was used as the carrier gas with a flow rate of 3 mL / min. All measurements were done at room temperature with only guard columns for fluidic connections. For reliability measurement, the pPID was fluidically connected to the FID in series, which served as the calibration detector assuming no degradation. The analytes were injected through the thermal injector (250°C) with a reference FID signal in the range of 200 pA to 500 pA to ensure similar and consistent injections for each measurement. The relative sensitivity of a pPID under test is defined as the ratio of peak areas of pPID over FID. The time evolution of the relative sensitivity over certain aging conditions (e.g., moisture or plasma exposure) was recorded in reliability tests.

[0102] Aging condition for moisture reliability test

[0103] Between relative sensitivity measurements, the pPIDs were aged with plasma turning off and without carrier gas flow in the lab ambient with a temperature of 19.7+0.7 °C and a relative humidity of 41.5+10.4 % recorded by a thermometer in-situ.

[0104] Argon plasma chamber setup for Ar plasma exposure reliability test

[0105] An Ar plasma chamber (Harrick Plasma PDC-32G) was used to simulate LiF substrate degradation when exposed to plasma inside an Ar lamp. The RF plasma chamber was first pumped down to a low pressure below the atmosphere. 99.999% Ar gas was then fed into thechamber in a constant flow = 150 mL / min before the RF power was turned. The LiF substrates were placed at the same location inside the chamber during each aging cycle.

[0106] UV-VIS transmission characterization

[0107] The transmission spectra of the MgF2 and LiF substrates were taken a Woollam M-2000 ellipsometer from 190 nm to 900 nm.

[0108] Atomic force microscopy (AFM) characterization

[0109] Surface roughness of the MgF2 substrates before and after silica coating was characterized using a Bruker ICON AFM with tapping mode in the air. The scan area was 5 pm x 5 pm. Multiple positions on each sample were scanned for consistency.

[0110] Crystalline structure characterization by X-ray diffraction (XRD)

[0111] The crystalline structure of LiF and MgF2 was determined by XRD technique. The samples were measured in reflection mode on a Rigaku Ultima 4 system. A parallel beam of Cu K-alpha excitation obtained from Rigaku's patented CBO (Cross-Beam-Optics) device was used as an X-ray source. X-ray tube runs at 40 kV and 44 mA. Cu K-beta was filtered by a 20-micron Ni foil.

[0112] LiF transmission restoration by thermal bleaching and DUV bleaching

[0113] Degraded LiF windows were thermally bleached by thermal annealing the sample on a hot plate at 350°C in ambient conditions. Note that since the LiF window is susceptible to thermal shock, the LiF samples were first placed on the hotplate at room temperature before ramping to high temperatures. The Deep UV (DUV) bleaching was achieved by placing the sample under the illumination of 2400 pW / cm2at 245 nm (UVP UVG-11 P / N 95-0016-14) in ambient. The UV lamp’s illumination power was calibrated using a UV meter. The DUV illumination also generated additional heat that raised the temperature of the sample in contact with the UV lamp surface to approximately 50°C.

[0114] Chemical composition characterization by X-ray photoelectron spectroscopy (XPS)

[0115] XPS spectra of fresh and aged LiF were collected using a Kratos Axis Ultra XPS with a monochromated Al Ka X-ray source (10 mA, 12 kV). The spot size was 700 pm x 300 pm. An Argon ion sputtering source with a sputtering rate of 0.025 nm / s was used for depth profiling. The sputtering duration was 1000 seconds (corresponding to 25 nm) for each depth step. Survey scans were used to quantify the atomic compositions at each depth. Core scans of Li 1 s level were used to investigate the binding environment of Li at each depth. The binding energies were calibrated to that of adventitious surface carbon (284.8 eV). The fresh LiF was measured rightafter being unpacked from a vacuum bag. The LiF were aged in the lab ambient (z.e., temperature = 19.7+0.7 °C and relative humidity = 41.5+10.4 %) for 1000 hours before measurement.

[0116] Silica integrated microfluidic photoionization detector device structure and fabrication

[0117] FIG. 8A depicts a generic device structure of a silica-integrated microfluidic photoionization detector (SIPID). To protect the VUV window, an interlayer was formed by coating silica on the VUV window surface facing the microfluidic channel, i.e., the side exposed to ambient moisture and VOC analytes during detection in the PID device. The interlayer was then integrated onto the microfluidic chip through gold-gold cold-welding using lithographically- patterned gold as the intermediate adhesive layer. Note that the counter gold layer on the microfluidic chip also serves the electrode contacts accessible for wire bond packaging. As an example, FIGS. IB and 1C show a 10 nm-silica-coated MgF2 window integrated microfluidic chip with the full microfabrication process illustrated in FIG. ID.

[0118] Unlike traditional hermetic bonding methods (e.g., anodic and eutectic) requiring high temperatures (>300 °C) for long periods (> 1 hour), cold welding allows for a low-temperature (150°C) bonding process in a short time (10 minutes) to prevent VUV window cracking caused by the large thermal expansion coefficient (CTE) mismatch (CTEsi = 2.6; CTEMgF2 = 13.7; CTEUF = 37; unit: 10'6 / K). On the other hand, compared to other low-temperature bonding techniques (e.g., polymer bonding) that cannot achieve a hermetic seal due to the gas permeable nature, the gold cold- welded interface in the SIPID provides a leak-free encapsulation that can sustain a flow rate up to 40 mL / min, sufficient for most applications in gas chromatography. It is noteworthy that, compared to manual glue bonding of individual dies, cold welding can be applied at the wafer level, resulting in increased yield and reduced cost per chip.

[0119] The commercial PID lamp, which comes with a 1 mm thick built-in VUV window (MgF2 for a Kr lamp and LiF for an Ar lamp), was then mechanically attached on top of the integrated interlayer using UV curable glue along the lamp’s circumferential edge such that both the bottom surface of the lamp’s built-in VUV window and the top surface of the interlayer VUV window are sealed from ambient. Note that although the glue was still used here for simplicity and convenience, unlike previous designs, in the design of this example, the VUV lamp was easily attached to the top of the interlayer and the glue was no longer in contact with the microfluidic chip beneath, and therefore, potential outgassing and clogging issues are avoided. Other packaging techniques (e.g., 3D printing) can also be employed to make a lamp fixture and completely avoid using glue if needed. For future manufacturing, the built-in VUV window on a commercial lampcan be pre-coated with silica and subsequently cold-welded to the silicon microfluidic chip without using an interlayer.

[0120] Silica VUV transmission

[0121] The silica coating on a VUV window may compromise the overall VUV transmission. In certain aspects, the protective dielectric (silica) coating is ultrathin to minimize its VUV absorption but is also sufficiently thick to ensure a uniform and dense coverage on the MgF2 or LiF window for efficiently blocking moisture permeation. To characterize the VUV transmission of the silica coating, a series of Kr lamp (10.6 eV) based SIPIDs (see FIG. 9A) were constructed with various thicknesses of silica coating (via PECVD) on the MgF2 interlayer. As shown in the system schematic in FIG. 9B, various analytes with a range of ionization potentials (IPs) were injected and then detected by two Kr-based PIDs connected in series. The first PID did not have an interlayer and was used to calibrate the downstream SIPIDs (z.e., the device under test - DUT) due to the non-destructive and flow-through nature of our PID. The interlayers in the DUT had various silica coating thicknesses ranging from 0 nm (z.e., just a bare 0.5 mm MgF2 window) to 100 nm.

[0122] In FIG. 9C, the VUV transmission of the silica coating can be extracted by further normalizing the peak area to that obtained with the 0 nm silica coating. It is found that a 10 nm silica coating retains 70-80% of the original sensitivity (in other words, 70-80% overall VUV transmission). In general, with the increased silica coating thickness, the sensitivity for the analytes with lower ionization potentials (such as IP = 8.56 and 8.82 eV) decays more slowly than for those with higher ionization potentials (such as IP = 10.18 and 10.47 eV), as shown in the inset of FIG. 9D. This can be explained as follows. First, the Kr-lamp has multiple VUV photon emission energies with the highest being 10.6 eV. The analytes with lower ionization potentials can be ionized (and subsequently detected) by not only 10.6 eV photons, but also the emitted photons with other lower energies. In contrast, the analytes with high ionization potentials (such as 10.18 and 10.47 eV) can only be ionized by 10.6 eV photons. Furthermore, silica’s VUV absorption increases with increased VUV photon energy (e.g., decreased VUV photon wavelength) in the range of 8.5 - 10.5 eV. Consequently, the detection of analytes having lower ionization potentials is less impacted by the silica coating than that of those having ionization potentials closer to 10.6 eV (see the inset in FIG. 9D). The pseudo-absorption coefficient of the silica coating at 10.6 eV is estimated to be 4.5 x 105cm'1by using the decay curve of the analyte with 10.47 eV ionization potential in FIG. 9D and a single exponential curve fit, in general agreement with the previous studies that show an absorption coefficient of 6 x 105cm'1at 10.6 eV for silica. Note that only the analyte whose ionization potential is close to 10.6 eV can be used toextract the silica absorption coefficient at 10.6 eV since only 10.6 eV photons can ionize it, as discussed previously.

[0123] Furthermore, to ensure uniform coverage of an ultrathin 10 nm silica coating on the MgF2 window, the surface morphology of bare and 10 nm-silica-coated MgF2 windows was examined using AFM. The surface roughness remained the same before (RMS = 0.9 nm) and after (RMS = 0.8 nm) silica coating suggesting a pin-hole free ultrathin silica layer on MgF2.

[0124] The VUV transmission of the silica coating beyond 10.6 eV was further investigated using Ar lamps (with the highest emission energy of 11.7 eV) and LiF windows with a similar device structure, i.e., replacing Kr lamps (MgF2 interlayer) with Ar lamps (LiF interlayer). Due to restrictions on processing LiF in our cleanroom facility, silica could only be sputtered on the LiF substrates instead of using PECVD. In Figure S3(A), 10 nm sputtered silica shows 40-60% of original sensitivity (i.e., overall VUV transmission) for the analytes with the ionization potential ranging from 8.5 eV to 11.5 eV. The -20% discrepancy compared to a PECVD coating is likely caused by the extrinsic VUV transmission loss of the host LiF substrate due to its exposure to Ar plasma during the sputtering process, as evidenced by the LiF color center formation after sputtering (see Figure S3(B)).

[0125] Ultrathin silica as the moisture barrier

[0126] The reliability of PIDs was tested using the setup in FIG. 10A. An FID was connected downstream in series with the PID and used as the calibration detector. The relative sensitivity of the PID under test is defined as the ratio of peak areas of PID over FID. The reliability of the PID was evaluated using the time evolution of its relative sensitivity under certain aging conditions.

[0127] To examine the silica protection performance on VUV windows against moisture, a hybrid device architecture of SIPID is designed - in which the more hygroscopic LiF window (with or without silica) was selected as the interlayer exposed to ambient to amplify the moisture effect (since MgF2 window is less susceptible to moisture); and the Kr lamp was employed as the VUV source due to its known superior robustness to an Ar lamp. Therefore, other possible degradation mechanisms associated with an Ar lamp could be ruled out and the VUV light source was deemed stable throughout the test. As shown in FIG. 10B, two SIPIDs (one with a bare LiF interlayer and the other with a 10 nm silica double-coated LiF interlayer) and a control device without interlayer were tested. Note that the 10 nm silica coating on the top LiF interlayer surface was for precaution only, which was essentially unnecessary as its perimeter was sealed by UV- epoxy that has a very low water vapor transmission rate. The PIDs were aged in ambient with a temperature of 19.7+0.7 °C and a relative humidity of 41.5+10.4%, which translates to a dew point= 8.0±1.8°C. This dew point is close to the annual average value recorded at Detroit Metro Airport station in Michigan. The signal (z.e., relative sensitivity) of the PIDs was periodically measured using benzene (IP = 9.2 eV). Between two consecutive measurements (z.e., during an aging cycle), the PIDs were not in operation with the Kr lamp (z.e., plasma) and carrier gas being turned off.

[0128] FIG. 10C shows the moisture reliability of the three devices. During the initial 50- 100 hours, all three devices underwent a significant drop in sensitivity, which recovered after 200 hours. Although the exact cause of this anomaly is unknown, by way of non-limiting theory, it may be attributed to an initial “bum-in” phase of the pPID. The silica-coated LiF device prepared in accordance with certain aspects of the present disclosure maintained its sensitivity at 90% after 2,200 hours of aging. In comparison, both the control device and bare LiF device degraded to 45% and 39%, respectively, with the same aging time. The bare LiF device underwent the fastest degradation among the three devices in the first 800 hours, after which the sensitivity plateaued at approximately 40%. The control device (z.e., the one with a built-in MgF2 window only) shared a similar trend reaching the 40% plateau with a slower degradation rate. The results suggest that the LiF window experiences faster degradation when exposed to ambient than the MgF2 window (control), while the eventual VUV transmission loss after a long term is similar for both windows. In contrast, the silica-coated LiF window (or interlayer) according to certain aspects of the present disclosure shows no obvious degradation trend with only 10% VUV loss when sensitivity plateaued, attesting to the effective moisture protection of the 10 nm silica coating for VUV windows.

[0129] To understand the role of silica as the moisture barrier, X-ray photoelectron spectroscopy (XPS) depth profiling was performed to examine the moisture degradation mechanism of LiF. It was found that the chemical compositions (e.g., atomic compositions of elements Li, F, and O) of both fresh and aged LiF substrates (e.g., exposed to ambient for 1000 hours) stayed almost constant from the top surface to 200 nm deep into the bulk. Consistently, the binding energy of Li 1 s level also remained relatively unchanged from surface to bulk. These results suggest that LiF crystals remained chemically unaltered even when exposed to a moisture dosage that had caused significant loss in VUV transmission. A previous study showed that LiF experienced significantly increased surface roughness when exposed to humidity, suggesting that the VUV transmission loss may be due to the stronger surface scattering. Therefore, ultrathin silica acts as a barrier to prevent moisture from being in contact with LiF, and as a surface passivation layer to maintain the morphology of LiF surface.

[0130] Study of Ar based SIPID

[0131] Ultrathin silica integration to the LiF interlayers in the Ar lamp based SIPIDs (Ar- SIPID) is further demonstrated, as shown in the inset of FIG. 11 A, to examine whether Ar lamp lifetime could be improved. FIG. 11A demonstrates the moisture reliability test of control and silica-coated Ar-SIPIDs. The aging protocol was the same as previously described in FIGS. 10A- 10C. Surprisingly, both devices degraded almost identically over 700 hours of aging regardless of silica protection. Compared to the results using the Kr lamps in FIG. 10C, Ar-SIPIDs’ sensitivity had a faster degradation rate without plateauing. In addition, it was visually observed that the built-in LiF windows in both Ar lamps of the tested Ar-SIPIDs appeared yellowish just after about 50 hours of aging, and such yellowish discoloration was manifested throughout the whole bulk crystal of LiF. All evidence suggests that there are new degradation mechanisms in the Ar lamp itself that are faster than the moisture-induced degradation discussed previously.

[0132] As part of this experiment, it was discovered that a major new degradation source turns out to be the Ar plasma generated inside the Ar lamp. To decouple its impact from the moisture reliability test performed before, another control device (z.e., Ar-SIPID without silica) was constructed and it was aged with Ar plasma being turned on continuously. As evidenced in FIG. 1 IB, with constant Ar plasma aging, the Ar-SIPID demonstrated an accelerated exponentiallike decay, taking only 2 hours to drop to 75% and 30% for benzene (IP = 9.2 eV and dichloromethane (DCM, IP = 11.3 eV), respectively. In addition, the yellowish discoloration of the built-in LiF window has also developed (not necessarily requiring 2 hours). Such results indicate that the dominant aging of Ar-SIPIDs in FIG. 11 A could be attributed to the accumulated short-term (approximately 30 minutes) Ar plasma exposure when it was turned on during the measurements at each aging test time point. Additionally, throughout 700 hours of moisture aging, the sensitivity loss for DCM is faster than toluene (IP = 8.8 eV) and heptane (10.1 eV, FIG. 11 A), consistent with the trend observed in FIG. 11B with accelerated Ar plasma exposure, that is, the sensitivity decays faster for the analytes whose ionization potentials are closer to the maximum emitted photon energy of Ar plasma (11.7 eV), as discussed in FIG. 9D for the Kr plasma case.

[0133] To better understand the degradation mechanism of the LiF windows in the Ar- SIPID, the built-in LiF window as well as the interlayer LiF window were dissembled from the 700-hour aged control Ar-SIPID (z.e., without silica) for further characterizations. From the transmission spectra in FIG. 11C, the aged built-in LiF window shows two dominant signature color centers of LiF (labeled as F and M), which render its yellowish appearance as seen in the inset of FIG. 11C. These color center formations result from high energy irradiations (e.g. , X-rays, Extreme UV (EUV), VUV, heavy ions, protons, electrons, etc.). Opposite to the significantlydeteriorated built-in LiF window, the directly contacted LiF interlayer underneath only developed a small F center without any visual discoloration, indicative of different degradation mechanisms. As illustrated in FIG. 11D, the built-in LiF window was directly exposed to all four species generated by Ar plasma inside the lamp body - (1) Ar*: Argon excited state; (2) Ar+: Argon ion; (3) e": electron; and (4) hv: VUV photon (e.g., 11.7 eV). In contrast, the LiF interlayer was only subject to the VUV photons transmitted through the built-in window. The above comparison suggests that the combination of Ar excited states, Ar ions, and electrons might play a more detrimental role to the LiF than VUV photons. However, it is also worth noting that the dose of VUV photons (hence the damage) incident on the LiF interlayer is lower than that on the native built-in LiF window during aging, especially after the built-in window became yellowish. Indeed, a similar effect was observed previously when a VUV-transmissive indium thin film was coated on the LiF substrate exposed to Ar discharge. It was found that the ratios of the initial slopes of the decay curves (e.g., VUV transmission of the LiF) closely matched the ratios of the initially transmitted intensities determined by the thickness of the indium thin film.

[0134] Ultrathin silica as the Ar plasma protective layer

[0135] The fact that the LiF interlayer suffered only mild degradation from Ar plasma with the shielding of the built-in window described above suggests a design to eventually integrate an ultrathin dielectric (e.g., silica) coating on the inner (top) surface of the built-in LiF transmissive window in an Ar lamp as depicted in FIGS. 12A-12B would be advantageous. Unlike vulnerable LiF, silica is not susceptible to any color center formation and has one of the lowest sputtering yields of any standard materials when exposed to Ar plasma (meaning that silica can withstand Ar plasma very well). Combined with its decent transmission in VUV as described before, the ultrathin silica layer thus serves to protect LiF from Ar plasma.

[0136] Limited by the inability to build an actual Ar lamp in-house, Ar plasma aging on the bare and silica-coated LiF substrates using a commercial Ar plasma chamber is performed, which simulated the actual environment inside an Ar lamp as illustrated in FIG. 12A. After aging in the plasma chamber, the LiF substrates were inserted as an additional interlayer into a Kr lamp based PID device, as illustrated in FIG. 12B, to extract the VUV transmission loss. Once again, a Kr lamp is used (instead of an Ar lamp) to provide a stable VUV source, as discussed previously. In addition, a stretchable tape instead of UV-epoxy was used for easy removal of the assembled VUV lamp and the interlayer between two consecutive aging cycles. The overall VUV transmission loss is hence inferred as the said PID sensitivity loss, assuming that other components in the stack (z.e., the Kr lamp and MgF2 interlayer) stayed intact.

[0137] In FIG. 12C, the 10 nm silica-coated LiF substrate remained stable (with a 15% increase in fact) after 11.5 hours of exposure to Ar plasma. In contrast, the bare LiF decreased to 60% of its original VUV transmission for the same aging. FIGS. 12D-12F present the UV-VIS spectra obtained simultaneously with another batch of substrates, showing that bare LiF progressively developed the F and M color centers with overall transmission loss, resulting in visual discoloration after 13 hours of aging (see the inset in FIG. 12F). In contrast, the silica- coated LiF substrates showed an initial F color center as-sputtered, which in fact partially recovered after the first 1.5 hours of aging, and the overall transmission stayed relatively stable without developing any other new color centers. Compared to small fluctuations in the transmission spectra of the 5 nm silica-coated LiF substrate, the 10 nm sample presents an almost constant overall transmission during aging. As mentioned before, the initial F color center of the silica-coated samples is caused by the sputtering process using Ar plasma, as further evidenced by the lower transmission value of the F center (wavelength: 250 nm) in 10 nm coating (0.73) than that of 5 nm (0.78). Note that the phenomenon of an initial partial recovery of the F center is consistent with the small increase of the VUV transmission observed in FIG. 12C, which also occurred right after the first 2 hours of aging. Such color center healing is attributed to the UV bleaching effect by the UV photons inside the Ar plasma chamber.

[0138] The above experiments using an Ar plasma chamber suggest that ultrathin silica effectively prevents VUV transmission loss of and color center formation in LiF from plasma exposure and thus can potentially be integrated on the inner surface (e.g., facing plasma) of a LiF (and MgF2) window to increase the Ar (and Kr) lamp lifetime. In contrast, other VUV transmissive thin films, such as indium and gold, are not suitable, because their metallic nature would disrupt the dielectric environment for dielectric-barrier-discharge plasma to form inside a VUV lamp and because thin metal coatings may not fully cover and protect the underlying surface of the UV window.

[0139] Example 4

[0140] Restoration of aged LiF windows by thermal and DUV bleaching

[0141] This example explores restoring degraded VUV transmission and color centers for a transmissive window in a VUV lamp. The unaltered single-crystal morphology of the degraded built-in LiF suggests that the observed color centers could be attributed as a recoverable crystallographic defect in which an anionic vacancy is occupied by one or more unpaired electrons that can therefore absorb light and generate color centers. It is known that such color centers developed in alkali halide crystals can be bleached by thermal annealing or DUV illumination.These two methods are thus used to restore two pairs of aged built-in LiF windows and their corresponding aged LiF interlayers in FIG. 11 A.

[0142] FIG. 13A shows the thermal bleaching results. In the severely aged built-in LiF window, the F center was eliminated after 68 hours of bleaching, while the M center disappeared much faster in only 3 hours. The interlayer LiF also had a fast recovery (3 hours) of its much less degraded F center. The F band recovery rates can be inferred. Both F bands in either built-in or interlayer LiF were recovered by thermal bleaching. As a result, the yellowish aged LiF window became clear again (see the pictures in the inset of FIG. 13 A. Compared to the complete elimination of color centers by thermal bleaching, DUV bleaching can only partially reduce the F center and M center of the degraded built-in LiF window at a slower rate as shown. In fact, the F center was blue-shifted as it recovered, which might indicate formation of new color centers caused by the DUV itself. Nevertheless, the F center in the aged interlayer LiF was restored entirely by DUV bleaching.

[0143] Next, whether such bleaching could restore the transmission in the VUV range concomitantly with the UV-VIS range is qualitatively examined by using a device structure similar to that shown in FIG. 12B. “Built-in LiF” refers to the similarly aged LiF window removed from an Ar lamp that was exposed to Ar plasma and visually discolored. By thermal bleaching (FIG. 13B), the VUV transmission of an aged built-in LiF window enhanced progressively approximately 5 times at IP = 10.1 eV accompanied with its F center recovered from 60% to 80% (FIG. 13B inset). In contrast, DUV bleaching was not as effective for recovering VUV transmission, despite significant restoration was seen in the UV-VIS range. Therefore, thermal bleaching is considered an effective bleaching method throughout VUV to UV-VIS range, while in these experiments, DUV bleaching only appears to cure the color centers in the UV-VIS range.

[0144] Lastly, the possibility to thermally recover an aged Ar lamp in situ by placing its intact built-in LiF window directly on the surface of a 350°C hotplate in ambient conditions is explored. However, the bonding between the lamp glass body and the built-in LiF window failed after just 20 minutes of annealing, which led to Ar gas leakage from inside and rendered the lamp useless. However, as noted above, a new bonding method that can withstand high temperatures (not necessarily 350 °C) may be used to substitute for conventional adhesives / sealants to implement such VUV window restoration methods provided by certain aspects of the present disclosure.

[0145] Example 5

[0146] Another variation of a protective coating for a transmissive window is explored in this example. More specifically, a transmissive dielectric protective layer comprising siliconnitride (S13N4) is used. PECVD silicon nitride coating is tested as it is theorized to have better performance as a moisture barrier than silica. While silicon nitride did offer protection, only 50% of the original sensitivity was obtained for a 10 nm thick coating, which is about 30% lower than a silica coating of the same thickness. Metallic coatings such as a thin film of sputtered Cr (2.5 nm) / Au (2.5 nm) were previously reported that allowed for > 50% VUV transmission on an MgF2 window, but they have questionable moisture protection effectiveness due to the discontinuous and island-like surface typically formed by ultrathin metals. As noted above, a thin metal coating cannot be used for a pPID design described herein as it would short the silicon electrodes of the microfluidic chip underneath.

[0147] In various aspects, the present disclosure provides microfabrication processes that form devices having VUV window with protective silicon coatings bonded under ambient conditions, so that VUV lamps can be directly integrated onto pPIDs for future high yield mass production. In such embodiments, the ultrathin silica protective coating was shown to be an effective barrier for both moisture and plasma exposure with good VUV transmission. The silica coating was prepared by widely employed deposition techniques (namely PECVD and sputtering) without further processing. Other techniques (e.g., atomic layer deposition) could form superior quality silica coatings that could further enhance the performance. Thus, the present disclosure contemplates more robust VUV lamps having enhanced lifetimes by coating ultrathin transmissive dielectric materials, like silica, on both sides of the VUV window - the outer silica layer for moisture protection and the inner for plasma shielding. Such a new type of VUV lamp and the corresponding PID will significantly reduce the maintenance effort in field applications under harsh environments and broaden the detection range of VOCs beyond 10.6 eV (Kr-based PID) by using a reliable Ar-based PID (up to 11.7 eV).

[0148] The foregoing description of the embodiments has been provided for purposes of illustration and description. It is not intended to be exhaustive or to limit the disclosure. Individual elements or features of a particular embodiment are generally not limited to that particular embodiment, but, where applicable, are interchangeable and can be used in a selected embodiment, even if not specifically shown or described. The same may also be varied in many ways. Such variations are not to be regarded as a departure from the disclosure, and all such modifications are intended to be included within the scope of the disclosure.

Claims

CLAIMSWhat is claimed is:

1. A vacuum ultraviolet (VUV) lamp comprising: an ultraviolet radiation chamber that is configured to generate ultraviolet photons that comprises a gas selected from the group consisting of: argon (Ar), krypton (Kr), xenon (Xe), and combinations thereof; and a transmissive window disposed adjacent to the ultraviolet radiation chamber that permits the ultraviolet photons to pass from the ultraviolet radiation chamber therethrough, wherein the transmissive window comprises multiple layers including a primary layer comprising a first material selected from the group consisting of: magnesium fluoride, calcium fluoride, lithium fluoride, and combinations thereof, and at least one protective layer disposed adjacent to the primary layer that comprises a transmissive dielectric material.

2. The vacuum ultraviolet (VUV) lamp of claim 1 , wherein the transmissive dielectric material is selected from the group consisting of: silicon dioxide (SiCh), silicon nitride (SisN4), aluminum oxide (AI2O3), and combinations thereof.

3. The vacuum ultraviolet (VUV) lamp of claim 1, wherein the primary layer defines a first side facing the ultraviolet radiation chamber and a second side opposite to the first side, wherein the at least one protective layer is disposed adjacent to the second side.

4. The vacuum ultraviolet (VUV) lamp of claim 1, wherein the primary layer defines a first side facing the ultraviolet radiation chamber and a second side opposite to the first side, wherein the at least one protective layer comprises a first protective layer disposed adjacent to the first side and a second protective layer disposed adjacent to the second side.

5. The vacuum ultraviolet (VUV) lamp of claim 1, wherein the at least one protective layer transmits greater than or equal to about 60% of the ultraviolet photons generated in the ultraviolet radiation chamber.

6. The vacuum ultraviolet (VUV) lamp of claim 1, wherein the at least one protective layer has a thickness of less than or equal to about 500 nm.

7. The vacuum ultraviolet (VUV) lamp of claim 1, wherein the at least one protective layer has a thickness of greater than or equal to about 0.5 nm to less than or equal to about 10 nm.

8. The vacuum ultraviolet (VUV) lamp of claim 1, wherein the transmissive window comprises the primary layer and an interlayer assembly disposed on a side opposite to the ultraviolet radiation chamber, wherein the interlayer assembly comprises a first protective layer, an interlayer comprising the first material selected from the group consisting of: magnesium fluoride, calcium fluoride, lithium fluoride, and combinations thereof disposed adjacent to the firstprotective layer, and a second protective layer disposed on a side of the interlayer opposite to the first protective layer.

9. A regenerable vacuum ultraviolet (VUV) lamp comprising: an ultraviolet radiation chamber that is configured to generate ultraviolet photons that comprises a gas selected from the group consisting of: argon (Ar), krypton (Kr), xenon (Xe), and combinations thereof; a transmissive window disposed adjacent to the ultraviolet radiation chamber that permits the ultraviolet photons to pass from the ultraviolet radiation chamber therethrough, wherein the transmissive window comprises multiple layers including a primary layer comprising a first material selected from the group consisting of: magnesium fluoride, calcium fluoride, lithium fluoride, and combinations thereof, and at least one protective layer disposed adjacent to the primary layer that comprises a transmissive dielectric material; and a regenerator component disposed in proximity to the transmissive window, wherein the regenerator component has a first state and a second state, wherein in the first state the regenerator component is dormant and in a second state the regenerator component is configured to selectively generate heat or deep ultraviolet (DUV) radiation directed towards the transmissive window to enhance or restore transmission of the ultraviolet photons through the transmissive window.

10. The regenerable vacuum ultraviolet (VUV) lamp of claim 9, wherein the transmissive dielectric material is selected from the group consisting of: silicon dioxide (SiCh), silicon nitride (SisN4), aluminum oxide (AI2O3), and combinations thereof.

11. The regenerable vacuum ultraviolet (VUV) lamp of claim 9, wherein the regenerator component comprises a heater.

12. The regenerable vacuum ultraviolet (VUV) lamp of claim 9, wherein the regenerator component comprises a source of deep ultraviolet (DUV) radiation.

13. The regenerable vacuum ultraviolet (VUV) lamp of claim 9, wherein the regenerator component comprises a heater and a source of deep ultraviolet (DUV) radiation.

14. The regenerable vacuum ultraviolet (VUV) lamp of claim 9, wherein the transmissive window is sealed to the ultraviolet radiation chamber by a high-temperature seal capable of withstanding temperatures of greater than or equal to about 350°C.

15. The regenerable vacuum ultraviolet (VUV) lamp of claim 9, wherein the primary layer defines a first side facing the ultraviolet radiation chamber and a second side opposite to the first side, wherein the at least one protective layer is disposed adjacent to the second side.

16. The regenerable vacuum ultraviolet (VUV) lamp of claim 9, wherein the primary layer defines a first side facing the ultraviolet radiation chamber and a second side opposite to the first side, wherein the at least one protective layer comprises a first protective layer disposed adjacent to the first side and a second protective layer disposed adjacent to the second side.

17. The regenerable vacuum ultraviolet (VUV) lamp of claim 9, wherein the at least one protective layer has a thickness of less than or equal to about 500 nm.

18. The regenerable vacuum ultraviolet (VUV) lamp of claim 9, wherein the at least one protective layer has a thickness of greater than or equal to about 0.5 nm to less than or equal to about 10 nm.19 A photoionization detector (PID) comprising: an ionization chamber having an inlet that receives a fluid sample and an outlet through which the fluid sample exits the ionization chamber; a first electrode and a distinct second electrode in electrical communication with the ionization chamber; an ultraviolet radiation chamber that is configured to generate ultraviolet photons that comprises a gas selected from the group consisting of: argon (Ar), krypton (Kr), xenon (Xe), and combinations thereof; and a transmissive window disposed between the ionization chamber and the ultraviolet radiation chamber that permits the ultraviolet photons to pass from the ultraviolet radiation chamber into the ionization chamber, wherein the transmissive window comprises multiple layers including a primary layer comprising a first material selected from the group consisting of: magnesium fluoride, calcium fluoride, lithium fluoride, and combinations thereof, and at least one protective layer disposed adjacent to the primary layer comprising a transmissive dielectric material.

20. The photoionization detector (PID) of claim 19, wherein the transmissive dielectric material is selected from the group consisting of: silicon dioxide (SiCh), silicon nitride (SisN4), aluminum oxide (AI2O3), and combinations thereof.

21. The photoionization detector (PID) of claim 19, wherein the ionization chamber is a microfluidic ionization chamber having one or more microfluidic channels each having a total volume of less than about 10 pL.

22. The photoionization detector (PID) of claim 19, wherein the primary layer defines a first side facing the ultraviolet radiation chamber and a second side opposite to the first side facing the ionization chamber, wherein the at least one protective layer is disposed adjacent to the second side.

23. The photoionization detector (PID) of claim 19, wherein the primary layer defines a first side facing the ultraviolet radiation chamber and a second side opposite to the first side facing the ionization chamber, wherein the at least one protective layer comprises a first protective layer disposed adjacent to the first side and a second protective layer disposed adjacent to the second side.

24. The photoionization detector (PID) of claim 19, wherein the at least one protective layer has a thickness of less than or equal to about 500 nm.

25. The photoionization detector (PID) of claim 19, wherein the at least one protective layer has a thickness of greater than or equal to about 0.5 nm to less than or equal to about 10 nm.

Citation Information

Patent Citations

  • A method for ionizing gases using UV irradiation and electrons, a method for identifying gases, and an apparatus therefor.

    JP2013541701A

  • Microfluidic photoionization detector

    KR1020180003579A

  • Photo ionization detector for gas chromatography having two separately ionizing sources and methods of use

    US20140132277A1

  • Photoionization detector ultraviolet lamp

    US20200292496A1

  • Integrated micro-photoionization detector with an ultrathin ultraviolet transmission window

    US20210341422A1