Catalyst for synergistic removal of nitrogen oxides and co, preparation method therefor and use

Through the core-shell structure catalyst of high-entropy oxide and CePO4, the problems of narrow temperature window and poor sulfur resistance of the catalyst in the existing technology when synergistically removing nitrogen oxides and carbon monoxide are solved, and a wide temperature window, high activity, and High stability catalytic effect, reducing costs and improving CO conversion rate.

WO2024207996A1PCT designated stage expired Publication Date: 2024-10-10ZHEJIANG UNIV

Patent Information

Application Number
PCT/CN2024/083168
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-07
Filing Date
2024-03-22
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing catalysts have problems with NH3 oxidation at high temperatures due to improved redox performance when synergistically removing nitrogen oxides and carbon monoxide. They have narrow temperature windows, poor sulfur resistance, high cost, and poor stability.

Method used

A core-shell structure catalyst using high-entropy oxides as the core and CePO4 as the shell is prepared by a hydrothermal method. The CePO4 shell adsorbs NH3 to avoid contact with high-entropy oxides, improves redox performance and sulfur resistance, and achieves a wide temperature window and high Activity and high stability.

Benefits of technology

It achieves efficient and coordinated removal of nitrogen oxides and carbon monoxide in a wide temperature range, reduces costs, improves the stability and sulfur resistance of the catalyst, avoids NH3 oxidation at high temperatures, and maintains a high CO conversion rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

Disclosed in the present invention are a catalyst for synergistic removal of nitrogen oxides and CO, a preparation method therefor and the use. The catalyst has a core-shell structure with aluminum oxide and / or titanium oxide loaded with a high-entropy oxide as the core and CePO4 as the shell. The preparation method comprises: performing vibratory ball milling, washing, drying and calcining on aluminum isopropoxide and / or titanium isopropoxide, chlorides of five or more different metal elements and P123 and / or PEG, stirring the obtained high-entropy oxide inner core and a gel of H3PO4 and Ce (NO3)3, and performing vibratory ball milling, drying and calcining, so as to obtain a high-entropy oxide loaded with CePO4 seeds; preparing, by using ammonia water, a clear solution containing pyrophosphate and Ce(NO3)3 in equal stoichiometric ratios, then adding the high-entropy oxide loaded with the CePO4 seeds and urea and / or TPAH to form a slurry, and, after hydrothermal reaction, washing, drying and calcining the solid, so as to obtain the catalyst for synergistic removal of nitrogen oxides and CO.
Need to check novelty before this filing date? Find Prior Art

Description

Catalyst capable of synergistically removing nitrogen oxides and CO, preparation method thereof, and application thereof Technical Field

[0001] The present invention relates to the field of air pollution control technology, in particular to a method for synergistically removing nitrogen oxides (NO x ) and carbon monoxide (CO) catalyst, preparation method and application thereof. Background Art

[0002] NO x As air pollutants, NO and CO coexist extensively in many industrial flue gases, such as coal-fired power plants, steel industry coke ovens, biomass boilers, etc. x It is O3 and PM 2.5 In addition to causing harm to human health, CO also causes environmental problems such as ozone holes and greenhouse effects. x and CO are of great significance to environmental protection and human health.

[0003] Currently, about NO x The collaborative removal of NH3 and CO mostly adopts CO-SCR (CO selective catalytic reduction) technology, but in practice, industrial flue gas is mostly in an oxygen-rich environment, which will seriously inhibit the occurrence of CO-SCR reaction and reduce the denitrification efficiency. In addition, the use of precious metal materials such as Ir-based materials also has disadvantages such as high cost and poor stability. The simultaneous NH3-SCR reaction and CO oxidation reaction on the same catalyst can effectively avoid the above problems, so it has also become a collaborative removal of NO. x and CO.

[0004] Regarding the simultaneous occurrence of NH3-SCR reaction and CO oxidation reaction, in order to achieve efficient CO removal efficiency, the catalyst must have high redox performance. High redox performance will cause NH3 oxidation to occur at high temperature, which will reduce the denitrification efficiency and narrow the temperature window for synergistic removal. Therefore, this is also the main problem in the current catalyst design. In addition, the actual industrial flue gas components are complex, and the sulfur resistance of the catalyst is also a key factor that needs to be considered in catalyst design. Therefore, a NO catalyst with a wide temperature window, high activity and high stability has been developed. x The synergistic removal catalyst of CO has broad application prospects and development significance.

[0005] The Chinese patent document with publication number CN114192158A discloses a method for producing CO and NO x Preparation method of synergistic removal catalyst, copper, manganese, iron, cerium ions are loaded on the surface of vanadium tungsten titanium catalyst, in the removal of NO xAt the same time, CO oxidation is also achieved, but the catalyst has problems such as a narrow denitrification temperature window (NO removal efficiency is only about 80% at 250°C) and poor sulfur resistance.

[0006] The US patent publication number US2018250661A1 discloses a method for simultaneously removing NO from flue gas. x The precious metal Pd was introduced into commercial catalysts to achieve the conversion of NO x and CO synergistic removal, but the catalyst introduces precious metals, which has the disadvantages of high cost and poor resistance.

[0007] Chinese patent documents with publication numbers CN113649020A, CN113694933A, and CN114308053A disclose titanium oxide denitrification catalysts loaded with high entropy oxides, which focus on low-temperature denitrification below 250°C, have a narrow denitrification window, and are not suitable for medium- and high-temperature denitrification above 300°C.

[0008] Summary of the Invention

[0009] The present invention provides a catalyst that can synergistically remove nitrogen oxides and CO, which has excellent characteristics such as wide temperature window, high activity, and high stability, and realizes low-cost synergistic control of NO x and CO, overcoming the problems of excessive oxidation of NH3 at high temperatures and catalyst resistance caused by the improvement of the redox performance of current catalysts.

[0010] A catalyst capable of synergistically removing nitrogen oxides and CO has a core-shell structure with aluminum oxide and / or titanium oxide loaded with high entropy oxide as the core and CePO4 as the shell.

[0011] The present invention adopts a core-shell structure to solve the above technical problems, and wraps a high entropy oxide with high redox performance inside CePO4. Among them, CePO4 is a good medium and low temperature denitrification catalyst that can achieve NO x Highly efficient removal of NH3. Furthermore, due to its strong acidity, CePO4 effectively adsorbs NH3 from flue gas, preventing it from coming into contact with the high-entropy oxide in the core, thereby effectively reducing its over-oxidation at high temperatures. Furthermore, both CePO4 and high-entropy oxide exhibit excellent sulfur resistance, enabling them to maintain a good synergistic removal efficiency in actual industrial flue gas.

[0012] In the catalyst, the high entropy oxide is preferably an oxide of at least four metal elements among Co, Zn, Mn, Mg, Ni, and Fe and Cu, and the metal elements are in an equimolar ratio.

[0013] Further preferably, the molar ratio of Cu element to CePO4 in the high entropy oxide is 1:2-10.

[0014] The present invention also provides a method for preparing the catalyst capable of synergistically removing nitrogen oxides and CO, comprising the steps of:

[0015] (1) Aluminum isopropoxide and / or titanium isopropoxide and chlorides of five or more different metal elements are used as precursors, P123 (polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer) and / or PEG (polyethylene glycol) are added as templates, and the mixture is subjected to vibration ball milling, washing, drying, and calcining to obtain a high entropy oxide core;

[0016] (2) adjusting the pH of a mixed solution containing H3PO4 and Ce(NO3)3 in a molar ratio of 1:1 to 9-11 with aqueous ammonia, stirring thoroughly to form a gel, and then stirring the high entropy oxide core obtained in step (1) with the mixed solution, vibrating ball milling, drying, and calcining to obtain a high entropy oxide loaded with CePO4 seeds;

[0017] (3) providing a mixed solution containing pyrophosphoric acid and Ce(NO3)3 in equal stoichiometric ratios, adding ammonia water to obtain a clear solution, and then adding the high entropy oxide loaded with CePO4 crystal seeds obtained in step (2) and urea and / or TPAH (tetrapropylammonium hydroxide) to form a slurry. After the hydrothermal reaction, the solid is washed, dried, and calcined to obtain the catalyst that can synergistically remove nitrogen oxides and CO.

[0018] In the preparation method of the present invention, first prepare high entropy oxide by high-speed vibration ball milling, then load a layer of CePO4 on the high entropy oxide core, and finally grow CePO4 shell by hydrothermal method. When NH3 contacts the catalyst, the CePO4 of the shell can well adsorb NH3 as solid acid to avoid contact with the high entropy oxide of the core, and NH3-SCR reaction occurs in the outer layer of the catalyst. At the same time, the core high entropy oxide of the catalyst has a higher oxidation performance and can achieve a higher CO conversion rate. The core-shell structure catalyst prepared has CO oxidation in the inner layer of the catalyst, and adsorbs NH3 in the outer layer to avoid contact with the oxide of the inner layer and the occurrence of NH3 oxidation. The excellent characteristics of the high entropy oxide of the core structure have excellent SO2 resistance due to its huge configurational entropy, and previous studies have also shown that the shell of CePO4 also has good SO2 resistance. Therefore, the catalyst of this structure can effectively avoid NH3 oxidation under high temperature while achieving high CO oxidation performance. At the same time, the catalyst material has certain sulfur resistance. The CePO4 in the outer layer also has a certain protective effect for the high entropy oxide of the core, and is an excellent catalyst with a wide temperature window, high activity and high stability.

[0019] In step (1), the molar ratio of the aluminum isopropoxide and / or titanium isopropoxide to the chloride is preferably 2:1-10.

[0020] In step (1), preferably, the chlorides are all divalent metal chlorides and must contain CuCl2.

[0021] In step (1), the mass ratio of the template to the precursor is preferably 0.1-1:1.

[0022] In step (1), the calcination temperature is preferably 380-420° C., and the calcination time is preferably 3-5 h.

[0023] In step (2), the calcination temperature is preferably 380-420° C., and the calcination time is preferably 3-5 h.

[0024] In step (2), the mass percentage of CePO4 seeds in the high entropy oxide loaded with CePO4 seeds is preferably 5%-20%.

[0025] In step (3), the molar ratio of urea and / or TPAH to Ce(NO3)3 is preferably 1-10:1.

[0026] In step (3), the temperature of the hydrothermal reaction is preferably 120-200° C., and the time is preferably 8-24 h.

[0027] In step (3), the calcination temperature is preferably 380-420° C., and the calcination time is preferably 3-5 h.

[0028] As a general inventive concept, the present invention also provides the use of the catalyst in the synergistic removal of nitrogen oxides and CO by selective catalytic reduction.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1) The core-shell structure catalyst prepared by the present invention can achieve a wide temperature window for NO x The synergistic removal of CO and NH3 can effectively avoid the NH3 oxidation problem caused by the improved redox performance of the catalyst.

[0031] 2) The catalyst prepared by the present invention has a certain sulfur resistance in both the core and shell structures, which improves the stability of the catalyst and can meet complex working conditions under actual conditions.

[0032] 3) The present invention uses transition metal precursors to simultaneously achieve NO x The synergistic removal of CO and CO reduces the cost of synergistic removal of pollutants. DETAILED DESCRIPTION

[0033] The present invention will be further described below with reference to specific examples. It should be understood that these examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention.

[0034] Example 1

[0035] Catalyst preparation:

[0036] (1) Copper chloride, nickel chloride, ferrous chloride, cobalt chloride, and magnesium chloride were mixed with aluminum isopropoxide and PEG-4000 in equal molar ratios. The mixture was ball-milled at 30 Hz for 120 min, washed with ethanol, dried in vacuo at 40°C, and then calcined at 400°C for 4 h to obtain a high-entropy oxide core. The amounts of each component added were as follows: total molar weight of metal chloride: molar weight of aluminum isopropoxide = 5:3.33; 0.4 g of PEG-4000 was added to 5 mmol of metal chloride;

[0037] (2) adjusting a mixed solution of phosphoric acid and cerium nitrate hexahydrate in a molar ratio of 1:1 to pH 10 with concentrated ammonia water, stirring thoroughly to form a gel, and then adding the core prepared in step (1) to the gel and stirring thoroughly, wherein the mass percentage of CePO4 is 5%, and the stirred sample is again subjected to high-speed vibration ball milling. After the ball milling, the sample is allowed to stand for a period of time and then vacuum dried at 40°C, and then calcined at 400°C for 4h to form a high-entropy oxide supported by CePO4 seeds;

[0038] (3) An equal stoichiometric amount of cerium nitrate solution was added dropwise to the pyrophosphoric acid solution, and the pH of the solution was adjusted to 4 with aqueous ammonia. The high entropy oxide supported by CePO4 seeds prepared in step (2) and urea were added, with 2 mol of urea added per mol of cerium nitrate. The mixture was then stirred for 30 min and hydrothermally heated at 180°C for 12 h. The obtained sample was washed, vacuum-dried, and calcined at 400°C for 4 h to obtain a high entropy oxide@CePO4 catalyst. The molar ratio of Cu element to CePO4 in the high entropy oxide was 1:10.

[0039] Catalyst activity test:

[0040] Activity experiments were conducted in a fixed-bed reactor with a catalyst loading of 2.3 mL and a particle size of 40-60 mesh. Initial gas concentrations were: NO = NH3 = 600 ppm, CO = 1200 ppm, O2 = 5 vol%, H2O = 5 vol%, with N2 as the balance gas, and a gas space velocity (GHSV) of 40,000 h-1. -1 When the reaction temperature was 280°C, the NO conversion rate was 99.6%, the N2 selectivity was 99.8%, and the CO conversion rate was 64.3%. When the reaction temperature was 380°C, the NO conversion rate was 99.3%, the CO conversion rate was 100%, and the N2 selectivity was 100%.

[0041] Example 2

[0042] Catalyst preparation:

[0043] (1) Copper chloride, nickel chloride, ferrous chloride, cobalt chloride, and magnesium chloride were mixed with aluminum isopropoxide and PEG-4000 in equal molar ratios. The mixture was ball-milled at 30 Hz for 120 min, washed with ethanol, dried in vacuo at 40°C, and then calcined at 400°C for 4 h to obtain a high-entropy oxide core. The amounts of each component added were as follows: total molar weight of metal chloride: molar weight of aluminum isopropoxide = 5:3.33; 0.4 g of PEG-4000 was added to 5 mmol of metal chloride;

[0044] (2) adjusting a mixed solution of phosphoric acid and cerium nitrate hexahydrate in a molar ratio of 1:1 to pH 10 with concentrated ammonia water, stirring thoroughly to form a gel, and then adding the core prepared in step (1) to the gel and stirring thoroughly, wherein the mass percentage of CePO4 is 5%, and the stirred sample is again subjected to high-speed vibration ball milling. After the ball milling, the sample is allowed to stand for a period of time and then vacuum dried at 40°C, and then calcined at 400°C for 4h to form a high-entropy oxide supported by CePO4 seeds;

[0045] (3) An equal stoichiometric amount of cerium nitrate solution was added dropwise to the pyrophosphoric acid solution, and the pH of the solution was adjusted to 4 with aqueous ammonia. The high entropy oxide supported by CePO4 seeds prepared in step (2) and urea were added, with 2 mol of urea added per mol of cerium nitrate. The mixture was then stirred for 30 min and hydrothermally heated at 180°C for 12 h. The obtained sample was washed, vacuum-dried, and calcined at 400°C for 4 h to obtain a high entropy oxide@CePO4 catalyst. The molar ratio of Cu element to CePO4 in the high entropy oxide was 1:5.

[0046] Catalyst activity test:

[0047] Activity experiments were conducted in a fixed-bed reactor with a catalyst loading of 2.3 mL and a particle size of 40-60 mesh. Initial gas concentrations were: NO = NH3 = 600 ppm, CO = 1200 ppm, O2 = 5 vol%, H2O = 5 vol%, with N2 as the balance gas, and GHSV = 40,000 h-1. -1 When the reaction temperature was 280°C, the NO conversion rate was 99.8%, the N2 selectivity was 100%, and the CO conversion rate was 91.3%. When the reaction temperature was 380°C, the NO conversion rate was 98.7%, the CO conversion rate was 100%, and the N2 selectivity was 99.7%.

[0048] Example 3

[0049] Catalyst preparation:

[0050] (1) Copper chloride, nickel chloride, manganese chloride, cobalt chloride, and zinc chloride were mixed with aluminum isopropoxide and PEG-4000 in equal molar ratios. The mixture was ball-milled at 30 Hz for 120 min, washed with ethanol, dried in vacuo at 40°C, and then calcined at 400°C for 4 h to obtain a high-entropy oxide core. The amounts of each component added were as follows: total molar weight of metal chloride: molar weight of aluminum isopropoxide = 5:3.33; 0.4 g of PEG-4000 was added to 5 mmol of metal chloride;

[0051] (2) adjusting a mixed solution of phosphoric acid and cerium nitrate hexahydrate in a molar ratio of 1:1 to pH 10 with concentrated ammonia water, stirring thoroughly to form a gel, and then adding the core prepared in step (1) to the gel and stirring thoroughly, wherein the mass percentage of CePO4 is 5%, and the stirred sample is again subjected to high-speed vibration ball milling. After the ball milling, the sample is allowed to stand for a period of time and then vacuum dried at 40°C, and then calcined at 400°C for 4h to form a high-entropy oxide supported by CePO4 seeds;

[0052] (3) An equal stoichiometric amount of cerium nitrate solution was added dropwise to the pyrophosphoric acid solution, and the pH of the solution was adjusted to 4 with aqueous ammonia. The high entropy oxide supported by CePO4 seeds prepared in step (2) and urea were added, with 2 mol of urea added per mol of cerium nitrate. The mixture was then stirred for 30 min and hydrothermally heated at 180°C for 12 h. The obtained sample was washed, vacuum-dried, and calcined at 400°C for 4 h to obtain a high entropy oxide@CePO4 catalyst. The molar ratio of Cu element to CePO4 in the high entropy oxide was 1:5.

[0053] Catalyst activity test:

[0054] Activity experiments were conducted in a fixed-bed reactor with a catalyst loading of 2.3 mL and a particle size of 40-60 mesh. Initial gas concentrations were: NO = NH3 = 600 ppm, CO = 1200 ppm, O2 = 5 vol%, H2O = 5 vol%, with N2 as the balance gas, and GHSV = 40,000 h-1. -1 When the reaction temperature was 280°C, the NO conversion rate was 99.7%, the N2 selectivity was 99.9%, and the CO conversion rate was 92.8%. When the reaction temperature was 380°C, the NO conversion rate was 97.2%, the CO conversion rate was 100%, and the N2 selectivity was 98.4%.

[0055] Example 4

[0056] Catalyst preparation:

[0057] (1) Copper chloride, nickel chloride, ferrous chloride, cobalt chloride, and zinc chloride were mixed with aluminum isopropoxide and PEG-4000 in equal molar ratios. The mixture was ball-milled at 30 Hz for 120 min, washed with ethanol, dried in vacuo at 40°C, and then calcined at 400°C for 4 h to obtain a high-entropy oxide core. The amounts of each component added were as follows: total molar weight of metal chloride: molar weight of aluminum isopropoxide = 5:3.33; 0.4 g of PEG-4000 was added to 5 mmol of metal chloride;

[0058] (2) adjusting a mixed solution of phosphoric acid and cerium nitrate hexahydrate in a molar ratio of 1:1 to pH 10 with concentrated ammonia water, stirring thoroughly to form a gel, and then adding the core prepared in step (1) to the gel and stirring thoroughly, wherein the mass percentage of CePO4 is 5%, and the stirred sample is again subjected to high-speed vibration ball milling. After the ball milling, the sample is allowed to stand for a period of time and then vacuum dried at 40°C, and then calcined at 400°C for 4h to form a high-entropy oxide supported by CePO4 seeds;

[0059] (3) An equal stoichiometric amount of cerium nitrate solution was added dropwise to the pyrophosphoric acid solution, and the pH of the solution was adjusted to 4 with aqueous ammonia. The high entropy oxide supported by CePO4 seeds prepared in step (2) and urea were added, with 2 mol of urea added per mol of cerium nitrate. The mixture was then stirred for 30 min and hydrothermally heated at 180°C for 12 h. The obtained sample was washed, vacuum-dried, and calcined at 400°C for 4 h to obtain a high entropy oxide@CePO4 catalyst. The molar ratio of Cu element to CePO4 in the high entropy oxide was 1:5.

[0060] Catalyst activity test:

[0061] Activity experiments were conducted in a fixed-bed reactor with a catalyst loading of 2.3 mL and a particle size of 40-60 mesh. Initial gas concentrations were: NO = NH3 = 600 ppm, CO = 1200 ppm, O2 = 5 vol%, H2O = 5 vol%, with N2 as the balance gas, and GHSV = 40,000 h-1. -1 When the reaction temperature was 280°C, the NO conversion rate was 99.6%, the N2 selectivity was 99.9%, and the CO conversion rate was 92.1%. When the reaction temperature was 380°C, the NO conversion rate was 98.2%, the CO conversion rate was 100%, and the N2 selectivity was 98.8%.

[0062] Example 5

[0063] Catalyst preparation:

[0064] (1) Copper chloride, nickel chloride, manganese chloride, cobalt chloride, and ferrous chloride were mixed with aluminum isopropoxide and PEG-4000 in equal molar ratios. The mixture was ball-milled at 30 Hz for 120 min, washed with ethanol, dried in vacuo at 40°C, and then calcined at 400°C for 4 h to obtain a high-entropy oxide core. The amounts of each component added were as follows: total molar weight of metal chloride: molar weight of aluminum isopropoxide = 5:3.33; 0.4 g of PEG-4000 was added to 5 mmol of metal chloride;

[0065] (2) adjusting a mixed solution of phosphoric acid and cerium nitrate hexahydrate in a molar ratio of 1:1 to pH 10 with concentrated ammonia water, stirring thoroughly to form a gel, and then adding the core prepared in step (1) to the gel and stirring thoroughly, wherein the mass percentage of CePO4 is 5%, and the stirred sample is again subjected to high-speed vibration ball milling. After the ball milling, the sample is allowed to stand for a period of time and then vacuum dried at 40°C, and then calcined at 400°C for 4h to form a high-entropy oxide supported by CePO4 seeds;

[0066] (3) An equal stoichiometric amount of cerium nitrate solution was added dropwise to the pyrophosphoric acid solution, and the pH of the solution was adjusted to 4 with aqueous ammonia. The high entropy oxide supported by CePO4 seeds prepared in step (2) and urea were added, with 2 mol of urea added per mol of cerium nitrate. The mixture was then stirred for 30 min and hydrothermally heated at 180°C for 12 h. The obtained sample was washed, vacuum-dried, and calcined at 400°C for 4 h to obtain a high entropy oxide@CePO4 catalyst. The molar ratio of Cu element to CePO4 in the high entropy oxide was 1:5.

[0067] Catalyst activity test:

[0068] Activity experiments were conducted in a fixed-bed reactor with a catalyst loading of 2.3 mL and a particle size of 40-60 mesh. Initial gas concentrations were: NO = NH3 = 600 ppm, CO = 1200 ppm, O2 = 5 vol%, H2O = 5 vol%, with N2 as the balance gas, and GHSV = 40,000 h-1. -1 When the reaction temperature was 280°C, the NO conversion rate was 99.8%, the N2 selectivity was 100%, and the CO conversion rate was 92.6%. When the reaction temperature was 380°C, the NO conversion rate was 98%, the CO conversion rate was 100%, and the N2 selectivity was 98.5%.

[0069] Example 6

[0070] Catalyst preparation:

[0071] (1) Copper chloride, nickel chloride, manganese chloride, cobalt chloride, ferrous chloride, and magnesium chloride were mixed with aluminum isopropoxide and PEG-4000 in equal molar ratios. The mixture was ball-milled at 30 Hz for 120 min, washed with ethanol, dried in vacuo at 40°C, and then calcined at 400°C for 4 h to obtain a high-entropy oxide core. The amounts of each component added were as follows: total molar weight of metal chloride: molar weight of aluminum isopropoxide = 5:3.33; 0.4 g of PEG-4000 was added to 5 mmol of metal chloride;

[0072] (2) adjusting a mixed solution of phosphoric acid and cerium nitrate hexahydrate in a molar ratio of 1:1 to pH 10 with concentrated ammonia water, stirring thoroughly to form a gel, and then adding the core prepared in step (1) to the gel and stirring thoroughly, wherein the mass percentage of CePO4 is 5%, and the stirred sample is again subjected to high-speed vibration ball milling. After the ball milling, the sample is allowed to stand for a period of time and then vacuum dried at 40°C, and then calcined at 400°C for 4h to form a high-entropy oxide supported by CePO4 seeds;

[0073] (3) An equal stoichiometric amount of cerium nitrate solution was added dropwise to the pyrophosphoric acid solution, and the pH of the solution was adjusted to 4 with aqueous ammonia. The high entropy oxide supported by CePO4 seeds prepared in step (2) and urea were added, with 2 mol of urea added per mol of cerium nitrate. The mixture was then stirred for 30 min and hydrothermally heated at 180°C for 12 h. The obtained sample was washed, vacuum-dried, and calcined at 400°C for 4 h to obtain a high entropy oxide@CePO4 catalyst. The molar ratio of Cu element to CePO4 in the high entropy oxide was 1:5.

[0074] Catalyst activity test:

[0075] Activity experiments were conducted in a fixed-bed reactor with a catalyst loading of 2.3 mL and a particle size of 40-60 mesh. Initial gas concentrations were: NO = NH3 = 600 ppm, CO = 1200 ppm, O2 = 5 vol%, H2O = 5 vol%, with N2 as the balance gas, and GHSV = 40,000 h-1. -1 When the reaction temperature was 280°C, the NO conversion rate was 99.7%, the N2 selectivity was 100%, and the CO conversion rate was 94.2%. When the reaction temperature was 380°C, the NO conversion rate was 95.5%, the CO conversion rate was 100%, and the N2 selectivity was 97.2%.

[0076] Example 7

[0077] Catalyst preparation:

[0078] (1) Copper chloride, nickel chloride, magnesium chloride, cobalt chloride, zinc chloride, and ferrous chloride were mixed with aluminum isopropoxide and PEG-4000 in equal molar ratios. The mixture was ball-milled at 30 Hz for 120 min, washed with ethanol, dried in vacuo at 40°C, and then calcined at 400°C for 4 h to obtain a high-entropy oxide core. The amounts of each component added were as follows: total molar weight of metal chloride: molar weight of aluminum isopropoxide = 5:3.33; 0.4 g of PEG-4000 was added to 5 mmol of metal chloride;

[0079] (2) adjusting a mixed solution of phosphoric acid and cerium nitrate hexahydrate in a molar ratio of 1:1 to pH 10 with concentrated ammonia water, stirring thoroughly to form a gel, and then adding the core prepared in step (1) to the gel and stirring thoroughly, wherein the mass percentage of CePO4 is 5%, and the stirred sample is again subjected to high-speed vibration ball milling. After the ball milling, the sample is allowed to stand for a period of time and then vacuum dried at 40°C, and then calcined at 400°C for 4h to form a high-entropy oxide supported by CePO4 seeds;

[0080] (3) An equal stoichiometric amount of cerium nitrate solution was added dropwise to the pyrophosphoric acid solution, and the pH of the solution was adjusted to 4 with aqueous ammonia. The high entropy oxide supported by CePO4 seeds prepared in step (2) and urea were added, with 2 mol of urea added per mol of cerium nitrate. The mixture was then stirred for 30 min and hydrothermally heated at 180°C for 12 h. The obtained sample was washed, vacuum-dried, and calcined at 400°C for 4 h to obtain a high entropy oxide@CePO4 catalyst. The molar ratio of Cu element to CePO4 in the high entropy oxide was 1:5.

[0081] Catalyst activity test:

[0082] Activity experiments were conducted in a fixed-bed reactor with a catalyst loading of 2.3 mL and a particle size of 40-60 mesh. Initial gas concentrations were: NO = NH3 = 600 ppm, CO = 1200 ppm, O2 = 5 vol%, H2O = 5 vol%, with N2 as the balance gas, and GHSV = 40,000 h-1. -1 When the reaction temperature was 280°C, the NO conversion rate was 99.5%, the N2 selectivity was 99.8%, and the CO conversion rate was 94.3%. When the reaction temperature was 380°C, the NO conversion rate was 95.4%, the CO conversion rate was 100%, and the N2 selectivity was 96.7%.

[0083] Example 8

[0084] Catalyst preparation:

[0085] (1) Copper chloride, nickel chloride, manganese chloride, cobalt chloride, zinc chloride, iron chloride, and magnesium chloride were mixed with aluminum isopropoxide and PEG-4000 in equal molar ratios. The mixture was ball-milled at 30 Hz for 120 min, washed with ethanol, dried in vacuo at 40°C, and then calcined at 400°C for 4 h to obtain a high-entropy oxide core. The amounts of each component added were as follows: total molar weight of metal chloride: molar weight of aluminum isopropoxide = 5:3.33; 0.4 g of PEG-4000 was added to 5 mmol of metal chloride;

[0086] (2) adjusting a mixed solution of phosphoric acid and cerium nitrate hexahydrate in a molar ratio of 1:1 to pH 10 with concentrated ammonia water, stirring thoroughly to form a gel, and then adding the core prepared in step (1) to the gel and stirring thoroughly, wherein the mass percentage of CePO4 is 5%, and the stirred sample is again subjected to high-speed vibration ball milling. After the ball milling, the sample is allowed to stand for a period of time and then vacuum dried at 40°C, and then calcined at 400°C for 4h to form a high-entropy oxide supported by CePO4 seeds;

[0087] (3) An equal stoichiometric amount of cerium nitrate solution was added dropwise to the pyrophosphoric acid solution, and the pH of the solution was adjusted to 4 with aqueous ammonia. The high entropy oxide supported by CePO4 seeds prepared in step (2) and urea were added, with 2 mol of urea added per mol of cerium nitrate. The mixture was then stirred for 30 min and hydrothermally heated at 180°C for 12 h. The obtained sample was washed, vacuum-dried, and calcined at 400°C for 4 h to obtain a high entropy oxide@CePO4 catalyst. The molar ratio of Cu element to CePO4 in the high entropy oxide was 1:5.

[0088] Catalyst activity test:

[0089] Activity experiments were conducted in a fixed-bed reactor with a catalyst loading of 2.3 mL and a particle size of 40-60 mesh. Initial gas volume concentrations were: NO = NH3 = 600 ppm, CO = 1200 ppm, O2 = 5 vol%, H2O = 5 vol%, SO2 = 100 ppm (when used), with N2 as the balance gas. GHSV = 40,000 h -1 At a reaction temperature of 280°C, the NO conversion rate was 99.9%, the N2 selectivity was 100%, and the CO conversion rate was 95.6%. At a reaction temperature of 380°C, the NO conversion rate was 94.3%, the CO conversion rate was 100%, and the N2 selectivity was 96.4%. When 100 ppm SO2 was introduced into the reaction gas, at 280°C, the NO conversion rate was 96.2%, the N2 selectivity was 98.6%, and the CO conversion rate was 79.3%. At 380°C, the NO conversion rate was 100%, the CO conversion rate was 100%, and the N2 selectivity was 100%.

[0090] Comparative Example 1

[0091] Catalyst preparation:

[0092] A high entropy oxide core was prepared according to the method of Example 8 and CePO4 was prepared by a hydrothermal method. After preparation, the two were dry-mixed to not form the core-shell structure of the present invention. The molar ratio of Cu element to CePO4 in the high entropy oxide was 1:5.

[0093] Catalyst activity test:

[0094] Catalyst activity was tested under the same conditions as in Example 8. At a reaction temperature of 280°C, the NO conversion was 99.8%, the N2 selectivity was 100%, and the CO conversion was 96%. At a reaction temperature of 380°C, the NO conversion was 76.4%, the CO conversion was 100%, and the N2 selectivity was 80.2%. When 100 ppm of SO2 was introduced into the reaction gas, at 280°C, the NO conversion was 96.1%, the N2 selectivity was 99.8%, and the CO conversion was 61.4%. At 380°C, the NO conversion was 100%, the CO conversion was 91.5%, and the N2 selectivity was 100%.

[0095] By comparing Comparative Example 1 with Example 8, it can be found that the advantages of the core-shell structure of the present invention are reflected in two aspects: 1. The NO conversion rate is high at high temperature, while the CO conversion rate can also be maintained at low temperature; 2. The anti-sulfur effect on CO oxidation is good and the oxidation rate is high.

[0096] In addition, it should be understood that after reading the above description of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A catalyst capable of synergistically removing nitrogen oxides and CO, characterized in that: It has a core-shell structure with aluminum oxide and / or titanium oxide loaded with high entropy oxide as the core and CePO4 as the shell, and a layer of CePO4 is also loaded on the core; The high entropy oxide is an oxide of at least four metal elements among Co, Zn, Mn, Mg, Ni, and Fe and Cu.

2. The catalyst according to claim 1, characterized in that In the high entropy oxide, each metal element is in an equal molar ratio.

3. The catalyst according to claim 2, characterized in that The molar ratio of the Cu element to CePO4 in the high entropy oxide is 1:2-10.

4. The method for preparing the catalyst according to any one of claims 1 to 3, characterized in that: Includes steps: (1) using aluminum isopropoxide and / or titanium isopropoxide and chlorides of five or more different metal elements as precursors, adding P123 and / or PEG as templates, performing vibration ball milling, washing, drying, and calcining to obtain a high entropy oxide core; (2) adjusting the pH of a mixed solution containing H3PO4 and Ce(NO3)3 in a molar ratio of 1:1 to 9-11 with aqueous ammonia, stirring the solution thoroughly to form a gel, and then stirring the high entropy oxide core obtained in step (1) with the solution thoroughly, vibrating and ball milling, drying, and calcining to obtain a high entropy oxide loaded with CePO4 seeds; (3) providing a mixed solution containing pyrophosphoric acid and Ce(NO3)3 in an equal stoichiometric ratio, adding aqueous ammonia to obtain a clear solution, then adding the high entropy oxide loaded with CePO4 seeds obtained in step (2) and urea and / or TPAH to form a slurry, and after a hydrothermal reaction, washing, drying, and calcining the solid to obtain the catalyst that can synergistically remove nitrogen oxides and CO.

5. The preparation method according to claim 4, characterized in that: In step (1): The molar ratio of the aluminum isopropoxide and / or titanium isopropoxide to the chloride is 2:1-10; The chlorides are all divalent metal chlorides and must contain CuCl2; The mass ratio of the template to the precursor is 0.1-1:1; The calcination temperature is 380-420° C. and the calcination time is 3-5 hours.

6. The preparation method according to claim 4, characterized in that: In step (2): The calcination temperature is 380-420°C and the calcination time is 3-5h; In the high entropy oxide loaded with CePO4 crystal seeds, the mass percentage of CePO4 crystal seeds is 5%-20%.

7. The preparation method according to claim 4, characterized in that: In step (3): The molar ratio of urea and / or TPAH to Ce(NO3)3 is 1-10:1; The temperature of the hydrothermal reaction is 120-200°C and the time is 8-24h; The calcination temperature is 380-420° C. and the calcination time is 3-5 hours.

8. Use of the catalyst according to any one of claims 1 to 3 in the synergistic removal of nitrogen oxides and CO by selective catalytic reduction.

Citation Information

Patent Citations

  • Pyrophosphate catalyst of cerium for selectively catalyzing and reducing nitrogen oxides and preparation method thereof

    CN101642715A

  • Denitration catalyst taking high-entropy oxide as active component as well as preparation and application of denitration catalyst

    CN114308053A

  • Catalyst capable of synergistically removing nitrogen oxides and CO as well as preparation method and application of catalyst

    CN116673047A

  • Core-shell support, method for producing the same, catalyst for purification of exhaust gas using the core-shell support, method for producing the same, and method for purification of exhaust gas using the catalyst for purification of exhaust gas

    US20180021758A1

  • METHOD OF PREPARING CATALYST FOR LOW-TEMPERATURE SYNERGISTIC CATALYTIC PURIFICATION OF NOx AND HCN IN FLUE GAS, AND USE THEREOF

    US20200197922A1

Cited By

  • Heavy metal and sulfur poisoning resistant denitration and CO / CH removal synergistic multifunctional catalyst synthesized in one step through solid-phase high-speed high-pressure ball milling method and application of denitration and CO / CH removal synergistic multifunctional catalyst

    CN118925789A

  • High-entropy metal alkene catalyst for ammoxidation as well as preparation method and application of high-entropy metal alkene catalyst

    CN119565634A

  • Preparation method of high-entropy material as well as product and application of high-entropy material

    CN119819319A

  • Method for catalytic oxidation of carbon monoxide based on plasma hydroxylation high-entropy metal oxide catalytic material

    CN121467053A

  • A method for catalytic oxidation of carbon monoxide based on a plasma hydroxylated high-entropy metal oxide catalytic material

    CN121467053B