Stainless steel composite plate with excellent appearance, and preparation method therefor

By using technologies such as surface treatment, isolating agents and intermittent cooling in the preparation process of stainless steel composite panels, the problems of poor plate shape and poor interface bonding quality have been solved, efficient and environmentally friendly stainless steel composite panel production has been achieved, and the product quality has been improved. Mechanical properties and corrosion resistance.

WO2024212404A1PCT designated stage expired Publication Date: 2024-10-17INST OF RES OF IRON & STEEL JIANGSU PROVINCE +3

Patent Information

Application Number
PCT/CN2023/111060
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2023-08-03
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing stainless steel composite panels have problems such as poor plate shape, poor interface bonding quality and surface defects during the preparation process, especially environmental pollution and poor product quality caused by explosive composite technology.

Method used

A stainless steel composite plate preparation method with excellent plate shape is adopted, including the steps of composite billet preparation, composite billet rolling and composite plate separation and straightening. Through surface treatment, use of isolation agents, vacuum welding and intermittent cooling and other technologies, the composite plate is ensured The plate shape and interface bonding quality.

Benefits of technology

It achieves the excellent plate shape, interface bonding quality and high production efficiency of stainless steel composite panels, avoids environmental pollution and surface defects caused by explosive composite technology, and improves the mechanical properties and corrosion resistance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023111060_17102024_PF_FP_ABST
    Figure CN2023111060_17102024_PF_FP_ABST
Patent Text Reader

Abstract

A stainless steel composite plate with an excellent appearance, and a preparation method therefor. The method comprises three main steps, i.e., composite blank preparation, composite blank rolling, and composite plate separation and straightening, wherein in the step of composite blank preparation, three instances of vacuumizing and two instances of vacuum breaking are performed on a composite blank by means of a seamless steel pipe, and finally the vacuum degree is less than or equal to 10^-2 Pa; in the step of composite blank rolling, intermittent cooling and straightening are performed, and stacking cooling is performed using two steel plates which are at T^f-150°C to T^f+150°C; and in the step of composite plate separation and straightening, flattening is performed using a flattening machine, a transverse flattening force F1 being equal to ν×a×b×c^transverse×σ^transverse / (d×(ν-c^transverse / a)), and a longitudinal flattening force F2 being equal to a×b×c^longitudinal×σ^longitudinal / (d+c^longitudinal). The composite plate has an excellent appearance and an excellent interfacial bonding quality, the degree of unevenness is less than or equal to 3 mm / m, the composite interfacial bonding rate is 100%, the shear strength is greater than or equal to 300 MPa, and the yield and production efficiency are high.
Need to check novelty before this filing date? Find Prior Art

Description

Stainless steel composite plate with excellent plate shape and preparation method thereof Technical Field

[0001] The invention belongs to the technical field of steel material preparation, and relates to a stainless steel composite plate with excellent plate shape and a preparation method thereof. Background Art

[0002] With the continuous development of science and industry, ordinary alloys or a single metal can no longer meet the comprehensive performance requirements of industrial development. Composite plates have come into being. Stainless steel composite plates are composite materials with stainless steel as the cladding layer and carbon steel or low-alloy steel as the base layer, combined through a specific process method. They have both the corrosion resistance of the cladding layer and the good mechanical properties of the base layer. They reduce the consumption of precious metals and significantly lower the cost of the project. They can save resources and reduce costs without reducing the use effect (mechanical strength, corrosion resistance, etc.), achieving a perfect combination of low cost and high performance. With good economic and social benefits, they are widely used in petrochemical, pressure vessels, medical equipment, papermaking, water conservancy, bridges and other industries.

[0003] Chinese patent application CN110064835A discloses a method for explosively welding TMCP bridge steel and stainless steel clad plates. In this application, the stainless steel and bridge steel are bonded together using explosive welding. This explosive bonding creates vibration, noise, and smoke pollution, and the resulting stainless steel clad plate exhibits poor shape and interface quality.

[0004] Summary of the Invention

[0005] The object of the present invention is to provide a stainless steel composite plate and a preparation method thereof, wherein the stainless steel composite plate has excellent plate shape and interface bonding quality.

[0006] To achieve the above-mentioned object of the invention, one embodiment of the present invention provides a method for preparing a stainless steel composite plate with excellent plate shape, which comprises the following steps:

[0007] 1) Composite blank preparation

[0008] Prepare two carbon steel billets with a thickness of T1, a length of L1, and a width of W1 as base materials; and prepare two stainless steel billets with a thickness of T2, a length of L2 < L1, and a width of W2 < W1 as composite materials;

[0009] performing surface treatment on at least one surface of each of the two substrates and the two composite materials;

[0010] Apply a release agent to one surface of a composite material;

[0011] Assembling the blanks in the order of stacking substrate, composite, composite, and substrate; wherein the composite is placed in the center relative to the substrate, the surfaces of the substrate and composite that are in contact with each other are both surfaces that have undergone the surface treatment, and the surface coated with the release agent faces the other composite;

[0012] Prepare four sealing strips with a width of W3 = 2T2-1 ~ 2mm, and place the sealing strips against the four sides of the two composite materials. Perform gas shielded welding between adjacent sealing strips and between the sealing strips and the base material, so that the two base materials and the sealing strips form a whole, thereby obtaining a composite blank base material;

[0013] A circular hole is machined on the seal strip at the groove on the side of the composite billet base, and a seamless steel pipe is welded at the circular hole;

[0014] Performing surfacing welding on the grooves on four sides of the composite billet base;

[0015] The composite billet is subjected to three vacuuming and two breaking processes through the seamless steel pipe, and finally the vacuum degree is ≤10 -2 Pa; then the seamless steel pipe is sealed to obtain a composite billet;

[0016] 2) Composite billet rolling

[0017] The obtained composite billet is heated and then subjected to two-stage controlled rolling of rough rolling + finishing rolling;

[0018] After rolling, the composite plate enters an ultra-fast cooling system for intermittent cooling. The ultra-fast cooling system has 24 cooling manifolds arranged at intervals of 1 m along the roller table. The cooling distance of each cooling manifold is 1 m. When the composite plate passes through the ultra-fast cooling system, the opening and closing states of all 24 cooling manifolds are controlled by opening N cooling manifolds and then closing M cooling manifolds. The cooling water pressure is 0.15-0.30 MPa, the cooling rate is 3-15°C / s, and the final cooling temperature is 380-590°C. Wherein N is 2, 3 or 4, and M is 2, 3 or 4.

[0019] After the composite plate leaves the ultra-fast cooling system, it enters the straightening machine for straightening. The straightened composite plate is placed at a temperature of T f -150℃~T f The stack cooling is carried out between two steel plates at +150℃, and the stack cooling time is 0.4min / mm×t0±5min, where t0 is the thickness of the composite plate. After the stack cooling is completed, the composite plate is cooled naturally on the cooling bed; wherein, T f =550+30Si-20Mn+15Cr-15Ni+10Mo, where the element symbols in this formula represent 100 times the mass percentage of each element in the substrate;

[0020] 3) Composite plate separation and straightening

[0021] Cut the edge of the composite board to remove the part other than the seal, and separate the composite board into two small composite boards;

[0022] Place the composite board with the composite layer facing upwards on the flattening machine for flattening. When flattening horizontally, control the flattening force of the flattening machine to be F1 = ν × a × b × c. 横 ×σ 横 / (d×(ν-c 横 / a)); When flattening longitudinally, control the flattening force F2 = a × b × c 纵 ×σ 纵 / (d+c 纵 ); where a is the width of the composite board, b is the thickness of the composite board, c 横 It is the unevenness per meter of the composite board in the horizontal direction, in mm, c 纵 is the unevenness per meter of the composite board in the longitudinal direction, in mm, d is the working distance of the flattening machine, σ 横 is the tensile yield strength of the composite plate in the transverse direction, σ 纵 is the tensile yield strength of the composite plate in the longitudinal direction, ν is the Poisson's ratio;

[0023] Finally, the composite plate is cold straightened to obtain the finished single-sided stainless steel composite plate.

[0024] Preferably, the step of "three-way vacuuming and two-way breaking of the composite blank through the seamless steel pipe, and finally making the vacuum degree ≤10 -2 Pa” is specifically:

[0025] First, connect the seamless steel pipe to the vacuum pump to evacuate the composite billet to a vacuum degree of ≤10 -2 Pa, then maintain the pressure for more than 4 hours; then connect the seamless steel pipe to the nitrogen device, break the composite billet and fill it with nitrogen;

[0026] After that, the seamless steel pipe is reconnected to the vacuum pump to evacuate the composite billet to a vacuum degree of ≤10 -1 Pa, no pressure maintenance; then connect the seamless steel pipe to the nitrogen device, break the composite billet and fill it with nitrogen;

[0027] Finally, the seamless steel pipe is connected to the vacuum pump for the third time to evacuate the composite billet to a vacuum degree of ≤10 -2 Pa.

[0028] Preferably, the step of "heating the obtained composite billet and then performing two-stage controlled rolling of rough rolling + finishing rolling" is specifically as follows:

[0029] The obtained composite blank is heated at a soaking temperature of 1150-1220°C, a total heating time of ≥1.2 min / mm×t, where t is the thickness of the composite blank, and a soaking section holding time of 30 min-50 min;

[0030] A two-stage controlled rolling process of rough rolling + finishing rolling is adopted. In the rough rolling stage, the starting rolling temperature is ≤1050°C, the final rolling temperature is ≥980°C, transverse rolling is performed first and then longitudinal rolling, at least one pass reduction is ≥35mm during longitudinal rolling, the total rough rolling reduction is 40-60%, and the rough rolling stage is ended when the thickness of the intermediate billet is 2.5-3.5 times the target thickness of the composite plate; then the intermediate billet is allowed to warm up, during which water cooling is carried out, and the finishing rolling stage is started when the surface temperature of the intermediate billet drops below 860°C; the final rolling temperature of the finishing rolling stage is ≥780°C, the total finishing rolling reduction is 55-75%, and the composite plate is obtained.

[0031] Preferably, the step of "heating the obtained composite billet and then performing two-stage controlled rolling of rough rolling + finishing rolling" is specifically as follows:

[0032] The obtained composite blank is heated in five stages, including preheating, first heating, second heating, third heating and soaking. The preheating temperature is ≤850°C, the residence time is (0.45-0.55) min / mm×t, the first heating temperature is 1030-1090°C, the residence time is (0.35-0.45) min / mm×t, the second heating temperature is 1100-1160°C, the residence time is (0.25-0.35) min / mm×t, the third heating temperature is 1140-1180°C, the residence time is (0.15-0.25) min / mm×t, the soaking temperature is 1170-1210°C, the residence time is (0.10-0.20) min / mm×t, and t is the thickness of the composite blank.

[0033] A two-stage controlled rolling method of rough rolling + finishing rolling is adopted, in which longitudinal rolling is adopted for the first pass, and the rolling reduction is ≥46mm; transverse rolling is adopted from the second pass until the composite billet is rolled to the target width of the final composite plate in the nth pass, and the rolling reduction in the second pass is ≥25mm; longitudinal rolling is adopted from the n+1th pass, and the rolling reduction in the n+1th pass is ≥30mm; during the entire rough rolling stage, the rolling temperature of the first pass is ≥1060℃, the start rolling temperature of the remaining passes is ≤1050℃, and the final rolling temperature is ≥1000℃; the rough rolling stage is terminated when the thickness of the intermediate billet is 2.5 to 3.5 times the target thickness of the composite plate, and the intermediate billet is kept warm, during which water cooling is carried out. When the surface temperature of the intermediate billet drops below 840℃, the finishing rolling stage begins, and the start rolling temperature of the finishing rolling stage is 810℃ to 840℃, and the final rolling temperature is 780℃ to 810℃.

[0034] Preferably, the step of "heating the obtained composite billet and then performing two-stage controlled rolling of rough rolling + finishing rolling" is specifically as follows:

[0035] The obtained composite blank is heated in four stages: preheating, first heating, second heating and soaking. The preheating temperature is 950-1000°C, the residence time is 0.3 min / mm×t, the first heating temperature is 1050-1100°C, the second heating temperature is 1120-1180°C, the soaking temperature is 1150-1200°C, and the total residence time of the first heating, second heating and soaking is 1.5 min / mm×t+20-40 min, where t is the thickness of the composite blank.

[0036] After the composite billet leaves the heating furnace, it is first descaled with high-pressure water and then rolled. During the rolling process, transverse rolling is adopted starting from the first pass until the composite billet is rolled to a width of Wt+0~40mm by the nth pass, where Wt is the target width of the composite plate, and the total reduction rate up to this point is ≥30%. Longitudinal rolling is adopted starting from the n+1th pass, and the rolling reduction rate of the n+1th pass is ≥20%. When the thickness of the intermediate billet is 2.5~3.5 times the target thickness of the composite plate, it is started to wait for temperature. When the surface temperature of the intermediate billet drops below 880℃, rolling is resumed until the rolling is completed, and the final rolling temperature is T r ±20℃, the total reduction rate of the entire rolling process is ≥75%; The element symbols in this formula represent 100 times the mass percentage of each element in the base material.

[0037] Preferably, in the intermittent cooling:

[0038] When the thickness of the composite plate is less than 54 mm, the roller speed of the ultra-fast cooling system is 0.4-0.8 m / s, the 1st to 4th groups of cooling manifolds are opened, the 5th to 6th groups of cooling manifolds are not opened, the 7th to 8th groups of cooling manifolds are opened, the 9th to 10th groups of cooling manifolds are not opened, the 11th to 12th groups of cooling manifolds are opened, the 13th to 14th groups of cooling manifolds are not opened, the 15th to 16th groups of cooling manifolds are opened, the 17th to 18th groups of cooling manifolds are not opened, the 19th to 20th groups of cooling manifolds are opened, the 21st to 22nd groups of cooling manifolds are not opened, and the 23rd to 24th groups of cooling manifolds are opened; the composite plate passes through the ultra-fast cooling system once, completing intermittent cooling;

[0039] When the thickness of the composite plate is greater than 54 mm, the roller speed of the ultra-fast cooling system is greater than 0.2 m / s and less than 0.6 m / s, the first to fourth groups of cooling manifolds are opened, the fifth to eighth groups of cooling manifolds are not opened, the ninth to twelfth groups of cooling manifolds are opened, the thirteenth to sixteenth groups of cooling manifolds are not opened, the seventeenth to twentieth groups of cooling manifolds are opened, the twenty-first to twenty-second groups of cooling manifolds are not opened, and the twenty-third to twenty-fourth groups of cooling manifolds are opened; the composite plate passes through the ultra-fast cooling system once, completing intermittent cooling.

[0040] Preferably, in the intermittent cooling:

[0041] When the thickness of the composite plate is ≥70mm, the roller speed of the ultra-rapid cooling system is 0.4-0.9m / s. The composite plate first enters the ultra-rapid cooling system in the forward direction. When its head reaches the 24th group of cooling headers, the rollers reverse and the composite plate passes through the ultra-rapid cooling system in the reverse direction and exits from the ultra-rapid cooling system inlet, completing intermittent cooling.

[0042] The 1st to 4th groups of cooling manifolds are open, the 5th to 8th groups of cooling manifolds are not open, the 9th to 12th groups of cooling manifolds are open, the 13th to 16th groups of cooling manifolds are not open, the 17th to 20th groups of cooling manifolds are open, the 21st to 22nd groups of cooling manifolds are not open, and the 23rd to 24th groups of cooling manifolds are open.

[0043] Preferably, the step of "placing the straightened composite plate at a temperature of T f -150℃~T f In the process of “stack cooling between two steel plates at +150℃”, the length and width of the steel plates used are both greater than those of the large composite plate, and the thickness of the steel plates used is twice that of the large composite plate.

[0044] Preferably, in the step of "coating a release agent on one surface of a composite material", the release agent used is a coating solution containing silicon oxide and magnesium oxide, wherein the mass ratio of silicon oxide to magnesium oxide is 3:1;

[0045] The amount of the release agent applied is 20 μg / m 2 , y is the thickness ratio of the composite blank to the composite plate;

[0046] Before the step of "assembling the blanks in the order of stacking the substrate, the composite material, the composite material, and the substrate", the composite material coated with the release agent is placed in a trolley furnace for heating and drying. The drying temperature is 340-360°C and the drying time is 35-45 minutes.

[0047] Preferably, in the step of "applying a release agent on one surface of a composite material", the components of the release agent used are as follows: 25-35% silicon nitride, 5-10% thermosetting amino resin, and 55-70% water in a mass ratio;

[0048] The thickness of the release agent is 0.2-0.5mm;

[0049] Before the step of "assembling the blanks in the order of stacking the substrate, the composite material, the composite material, and the substrate", the composite material coated with the release agent is heated and dried at a temperature of 100 to 250°C for 20 to 40 minutes.

[0050] Preferably, the step of "substituting surface treatment on at least one surface of each of the two substrates and the two composite materials" comprises:

[0051] Milling one surface of two substrates in a manner of relative shape complementation to form an irregular concave-convex surface comprising X planes sequentially connected in a transverse direction, wherein the substrate is a non-uniform thickness blank with a non-monotonically varying thickness in the transverse direction, and wherein the length L12 of the irregular concave-convex surface is equal to L1 and the total width W12 is greater than W1; or milling the one surface of two substrates into an irregular concave-convex surface comprising X planes sequentially connected in a longitudinal direction, wherein the substrate is a non-uniform thickness blank with a non-monotonically varying thickness in the longitudinal direction, and wherein the total length L12 of the irregular concave-convex surface is greater than L1 and the width W12 is equal to W1; X ≥ 2;

[0052] One surface of each composite material is ground and polished to remove surface oxide scale; and then each composite material is bent to match the corresponding irregular concave and convex surface.

[0053] Preferably, the step of "substituting surface treatment on at least one surface of each of the two substrates and the two composite materials" comprises:

[0054] Grinding and polishing one surface of each composite material to remove surface oxide scale; and,

[0055] In a manner of relative shape complementarity, one surface of the two substrates is milled and ground, and the surface is processed into a transverse inclined surface with a length L11=L1 and a width W11>W1, and the substrate is a non-uniform thickness blank with a thickness gradient in the transverse direction, or the surface is processed into a longitudinal inclined surface with a length L11>L1 and a width W11=W1, and the substrate is a non-uniform thickness blank with a thickness gradient in the longitudinal direction.

[0056] Preferably, the step of "substituting surface treatment on at least one surface of each of the two substrates and the two composite materials" comprises:

[0057] One surface of each substrate and each composite material is ground and polished to remove surface oxide scale. After grinding and polishing, the substrate and composite material are both blanks of equal thickness.

[0058] Preferably, in the “composite is placed centrally relative to the substrate”, the distance from the side edge of the composite material in the transverse direction to the corresponding side edge of the substrate is half the width difference between the contact surface of the composite material and the substrate, and the distance from the side edge of the composite material in the longitudinal direction to the corresponding side edge of the substrate is half the length difference between the contact surface of the composite material and the substrate.

[0059] To achieve the above-mentioned object of the invention, one embodiment of the present invention provides a stainless steel composite plate with excellent plate shape, and the composite plate is prepared by the above-mentioned preparation method.

[0060] Preferably, the unevenness of the composite plate is ≤3 mm / m, the composite interface bonding rate is 100%, and the shear strength is ≥300 MPa.

[0061] Preferably, the unevenness of the composite plate is ≤2 mm / m, the composite interface bonding rate is 100%, and the shear strength is ≥360 MPa.

[0062] Preferably, the impact energy at 0°C is ≥240J, the impact energy at -20°C is ≥200J, and the impact energy at -40°C is ≥150J.

[0063] Preferably, the Vickers hardness difference of the base layer of the composite plate in the thickness direction is ≤10, the head, middle and tail strength difference is ≤40 MPa, and the strength difference of the entire plate is ≤40 MPa.

[0064] Compared with the prior art, the beneficial effects of the present invention are: on the one hand, in the entire preparation method, through specific control of the process, the corrosion resistance and mechanical strength of the stainless steel composite plate are guaranteed, and the corrosion resistance and mechanical properties are avoided from being deteriorated during the rolling process of the composite billet; on the other hand, the problems of poor plate shape, poor interface bonding quality, and poor surface quality of the existing thick plates of stainless steel composite plates are solved, so that the stainless steel composite plate has excellent plate shape and interface bonding quality, the unevenness of the composite plate is ≤3mm / m, the composite interface bonding rate is 100%, the shear strength is ≥300MPa, and obvious surface defects such as pits and scratches caused by the existing explosive composite technology are avoided; on the other hand, the yield rate in the production process is high and the production efficiency is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] For the sake of clarity in presentation and description, in the various drawings of the present invention, certain dimensions of structures or parts are exaggerated relative to other structures or parts. Therefore, these drawings are only used to illustrate the basic structure of the subject matter of the present invention.

[0066] FIG1a is a schematic cross-sectional view of a steel billet according to a first embodiment of the billet surface treatment step of the present invention;

[0067] FIG1 b is a schematic transverse cross-sectional view of a steel billet according to a second embodiment of the billet surface treatment step of the present invention, wherein the change in surface shape after the surface treatment is indicated by dot-dash lines;

[0068] FIG1c is a schematic longitudinal cross-sectional view of a steel billet according to a third embodiment of the billet surface treatment step of the present invention, wherein the change in surface shape after the surface treatment is indicated by dot-dash lines;

[0069] FIG1d is a schematic transverse cross-sectional view of a steel billet according to a fourth embodiment of the billet surface treatment step of the present invention, and illustrates the changes in surface shape before (A) and after (B) the surface treatment;

[0070] FIG1e is a schematic longitudinal cross-sectional view of a steel billet according to a fifth embodiment of the billet surface treatment step of the present invention, and illustrates the changes in surface shape before (A) and after (B) the surface treatment;

[0071] FIG2a is a schematic cross-sectional view of the composite blank corresponding to FIG1a;

[0072] FIG2b is a schematic transverse cross-sectional view of the composite blank corresponding to FIG1b;

[0073] FIG2c is a schematic longitudinal cross-sectional view of the composite blank corresponding to FIG1c;

[0074] FIG2d is a schematic transverse cross-sectional view of the composite blank corresponding to FIG1d;

[0075] FIG2e is a schematic longitudinal cross-sectional view of the composite blank corresponding to FIG1e;

[0076] FIG3a is a flow chart of a first embodiment of the overall steps of composite billet rolling according to the present invention;

[0077] FIG3 b is a flow chart of a second embodiment of the overall steps of composite billet rolling according to the present invention;

[0078] FIG3 c is a flow chart of a third embodiment of the overall steps of composite billet rolling according to the present invention;

[0079] FIG4 a is a schematic cross-sectional view of two composite plates rolled from the composite billet of FIG2 a ;

[0080] FIG4 b is a schematic transverse cross-sectional view of two composite plates rolled from the composite billet of FIG2 b ;

[0081] FIG4c is a schematic longitudinal cross-sectional view of two composite plates rolled from the composite billet of FIG2c;

[0082] FIG4 d is a schematic transverse cross-sectional view of two composite plates rolled from the composite billet of FIG2 d ;

[0083] FIG4e is a schematic longitudinal cross-sectional view of two composite plates rolled from the composite billet of FIG2e DETAILED DESCRIPTION

[0084] As mentioned in the background, existing stainless steel clad plates suffer from poor shape and interface bonding due to manufacturing process issues. To address these technical issues, the present invention provides a method for preparing a single-sided stainless steel clad plate with excellent shape, as well as a single-sided stainless steel clad plate prepared using this method.

[0085] Specifically, the preparation method includes three steps: composite billet preparation, composite billet rolling, and composite plate separation and straightening. These three steps are introduced below one by one.

[0086] The overall steps of preparing the composite blank include the following sub-steps:

[0087] Prepare two carbon steel billets with a thickness of T1, a length of L1, and a width of W1 as base materials; and prepare two stainless steel billets with a thickness of T2, a length of L2, and a width of W2 as composite materials;

[0088] performing surface treatment on at least one surface of each of the two substrates and the two composite materials;

[0089] Apply a release agent to one surface of a composite material;

[0090] Assemble the blanks in the order of stacking base material, composite material, composite material and base material;

[0091] Prepare four sealing strips with a width of W3, where W3 = 2T2 - 1 to 2 mm, and place the sealing strips against the four sides of the two composite materials. Perform gas shielded welding between adjacent sealing strips and between the sealing strips and the base material, so that the two base materials and the sealing strips form a whole, thereby obtaining a composite blank base material.

[0092] A circular hole is machined on the seal strip at the groove on the side of the composite billet base, and a seamless steel pipe is welded at the circular hole;

[0093] Performing surfacing welding on the grooves on four sides of the composite billet base;

[0094] The composite billet is subjected to three vacuuming and two breaking processes through the seamless steel pipe, and finally the vacuum degree is ≤10 -2 Pa; and then the seamless steel pipe is sealed to obtain a composite billet.

[0095] Furthermore, the above steps are described in detail as follows.

[0096] The step of “preparing two carbon steel billets of length L1 and width W1 as base materials; and preparing two stainless steel billets of length L2 and width W2 as composite materials” is also a billet preparation step.

[0097] The carbon steel billet used as the base material has a thickness of T1, a length of L1, and a width of W1, that is, a rectangular billet. Similarly, the stainless steel billet used as the composite material has a thickness of T2, a length of L2, and a width of W2, that is, a rectangular billet.

[0098] Furthermore, L2<L1, W2<W1, and the length and width of the composite material are both smaller than those of the base material. Preferably, L2=L1-L0, W2=W1-W0, and the preferred value ranges of L0 and W0 are 90-150 mm, respectively.

[0099] As a preferred solution, the carbon steel billet's surface oxide scale penetration depth and surface pit depth are both ≤0.3mm, and its roughness is ≤3mm / m. The stainless steel billet's surface is scratch-free and its roughness is ≤2mm / m. This prevents billets with significant surface or shape defects from entering the composite panel production line.

[0100] As a preferred embodiment, the stainless steel billet is preferably austenitic stainless steel. Its chemical composition, by mass percentage, is: C ≤ 0.15%, Si ≤ 1.00%, Mn ≤ 2.00%, P ≤ 0.045%, S ≤ 0.030%, Ni: 6.0-22.0%, Cr: 16.0-26.0%, Mo ≤ 3.0%, with the balance being Fe and unavoidable impurities. Using a stainless steel billet with this chemical composition can further enhance the performance of the composite plate, particularly the corrosion resistance of the composite layer, while maintaining the aforementioned technical effects. For example, the composite layer of the composite plate (i.e., the composite material obtained by rolling) exhibits no intergranular corrosion cracking after being boiled in a sulfuric acid-copper sulfate solution for 20 hours and then bent 180°.

[0101] It should be noted that the chemical compositions of the two stainless steel billets may be the same or different, and only one of them may adopt the chemical composition provided by the above preferred solution, or both of them may adopt the chemical composition provided by the above preferred solution, or neither of them may adopt the chemical composition provided by the above preferred solution.

[0102] As a preferred embodiment, the chemical composition of the carbon steel billet is, in percentage by mass: C: 0.03-0.16%, Si: 0.11-0.29%, Mn: 1.31-1.54%, P≤0.018%, S≤0.0030%, Cr: 0.06-0.29%, Nb: 0.011-0.034%, Ti: 0.011-0.019%, Al: 0.030-0.040%, and the rest is Fe and unavoidable impurities.

[0103] Further preferably, the chemical composition of the carbon steel billet is, in percentage by mass: C: 0.08-0.12%, Si: 0.16-0.24%, Mn: 1.36-1.44%, P≤0.015%, S≤0.0025%, Cr: 0.11-0.19%, Ni: 0.06-0.14%, Nb: 0.016-0.024%, Ti: 0.011-0.019%, Al: 0.030-0.040%, and the rest is Fe and unavoidable impurities.

[0104] More preferably, the chemical composition of the carbon steel billet is, in percentage by mass: C: 0.05-0.09%, Si: 0.14-0.22%, Mn: 1.41-1.49%, P≤0.012%, S≤0.0020%, Cr: 0.16-0.24%, Ni: 0.11-0.19%, Mo: 0.11-0.19%, Nb: 0.021-0.029%, Ti: 0.011-0.019%, Al: 0.030-0.040%, and the rest is Fe and unavoidable impurities.

[0105] Another preferred embodiment is that the chemical composition of the carbon steel billet is, in percentage by mass: C: 0.03-0.07%, Si: 0.11-0.19%, Mn: 1.46-1.54%, P≤0.010%, S≤0.0015%, Cr: 0.21-0.29%, Ni: 0.16-0.24%, Cu: 0.16-0.24%, Mo: 0.16-0.24%, Nb: 0.026-0.034%, Ti: 0.011-0.019%, Al: 0.030-0.040%, and the rest is Fe and unavoidable impurities.

[0106] Similar to the description of the aforementioned stainless steel plates, the chemical compositions of the two carbon steel billets may be the same or different. Only one of the two carbon steel billets may adopt the chemical composition provided by the above preferred scheme, or both of the two carbon steel billets may adopt the chemical composition provided by the above preferred scheme, or neither of the two carbon steel billets may adopt the chemical composition provided by the above preferred scheme.

[0107] Next, regarding the step of "subjecting a surface treatment to at least one surface of each of the two substrates and the two composite materials," that is, the blank surface treatment step, the present invention provides five preferred embodiments, which are respectively introduced below.

[0108] <First embodiment of the blank surface treatment step>

[0109] In this embodiment, one surface of each substrate and each composite material is ground and polished to remove the surface oxide scale and reveal the metallic luster. In this way, after grinding and polishing, the substrate and the composite material are both blanks of equal thickness.

[0110] As shown in FIG1a , for example, surface p1a of substrate 11a and surface p2a of substrate 12a are ground and polished using a grinding wheel, belt sander, or milling machine to remove surface oxide scale and reveal a metallic luster. Surface p3a of prepared composite material 21a and surface p4a of composite material 22a are ground and polished using a wire wheel to remove surface oxide scale and reveal a metallic luster.

[0111] As will be seen from the following text, during assembly, the surface that has been surface treated (polished in this embodiment) is used as the surface where the substrate and the composite material are in contact with each other, for example, surface p1a and surface p3a are in contact with each other, and surface p4a and surface p2a are in contact with each other, so that the interface bonding quality can be guaranteed.

[0112] <Second embodiment of the blank surface treatment step>

[0113] In this embodiment, similar to the first embodiment, one surface of each composite material (e.g., surface p3b of composite material 21b and surface p4b of composite material 22b in FIG. 1b ) is ground and polished to remove surface oxide scale and expose metallic luster, which will not be described in detail.

[0114] In this embodiment, what is different from the aforementioned first embodiment is the surface treatment of the substrate: referring to FIG1b , the surface p1b of the substrate 11b is milled to process the surface p1b into a surface p1b0, which is a transverse inclined surface with a length L11=L1 and a width W11>W1. Accordingly, the substrate 11b is processed into a non-uniform thickness blank with a thickness gradient in the transverse direction (i.e., in the width direction). That is, after the substrate 11b is milled, the height of the substrate 11b gradually increases from one side to the other side in the width direction. Similarly, the surface p2b of the substrate 12b is milled to process the surface p2b into a surface p2b0, which is a transverse inclined surface with a length L11=L1 and a width W11>W1. Accordingly, the substrate 12b is processed into a non-uniform thickness blank with a thickness gradient in the transverse direction.

[0115] The milling of surface p2b of substrate 12b and surface p1b of substrate 11b is performed in a manner that complements their relative shapes. This means that the processed surface p2b0 and surface p1b0 are complementary in shape when facing each other. For example, the lateral inclination angle of surface p2b0 (e.g., the angle with the original surface p2b) is equal to the lateral inclination angle of surface p1b0 (e.g., the angle with the original surface p1b). This ensures that the upper and lower surfaces of the composite blank are parallel during subsequent assembly.

[0116] It is understandable that after the above-mentioned milling process, the surface oxide scales on the surface p1b of the substrate 11b and the surface p2b of the substrate 12b can also be removed, revealing the metallic luster.

[0117] As can be seen from the following text, when assembling, by using the surface that has been surface treated (milling in this embodiment) as the surface where the base material and the composite material are in contact with each other, for example, surface p1b0 and surface p3b are in contact with each other, and surface p4b and surface p2b0 are in contact with each other, the interface bonding quality can be ensured as in the aforementioned first embodiment, and this embodiment can also be further used to prepare non-uniform thickness composite plates with a lateral thickness gradient, so as to improve the applicable scenarios and scope of the composite plates.

[0118] <Third Embodiment of Blank Surface Treatment Step>

[0119] This embodiment is essentially the same as the second embodiment described above (including the surface treatments on surfaces p3c and p4c), differing only in that the substrate thickness gradient in the second embodiment is changed to a longitudinal (i.e., lengthwise) gradient in thickness. These differences are described below; other similarities are discussed in the second embodiment and will not be repeated here.

[0120] Referring to FIG1c , surface p1c of substrate 11c is milled to form surface p1c0, which is a longitudinally inclined surface with a length L11 greater than L1 and a width W11 equal to W1. Accordingly, substrate 11c is processed into a non-uniform thickness blank with a longitudinally varying thickness. Similarly, surface p2c of substrate 12c is milled to form surface p2c0, which is a longitudinally inclined surface with a length L11 greater than L1 and a width W11 equal to W1. Accordingly, substrate 12c is processed into a non-uniform thickness blank with a longitudinally varying thickness.

[0121] The milling of surface p2c of substrate 12c and surface p1c of substrate 11c is performed in a manner that complements their relative shapes. For example, the longitudinal inclination angle of surface p2c0 (e.g., the angle with the original surface p2c) is equal to the longitudinal inclination angle of surface p1c0 (e.g., the angle with the original surface p1c). This ensures that the upper and lower surfaces of the composite blank are parallel during subsequent assembly.

[0122] <Fourth embodiment of the blank surface treatment step>

[0123] In this embodiment, one surface of each substrate is milled to form an irregular concave-convex surface comprising X planes connected sequentially in the transverse direction. The substrate is a non-uniform thickness blank having a non-monotonically varying thickness in the transverse direction. The length of the irregular surface is L12 = L1 and the total width is W12 > W1.

[0124] For example, referring to Figure 1d, the surface p1d of the substrate 11d is milled and processed from the horizontal surface in Figure 1d (A) to the irregular concave-convex surface p1d0 shown in Figure 1d (B). The irregular concave-convex surface p1d0 specifically includes X planes connected in sequence along the horizontal direction, where X≥2. In the figure, there are 8 planes. It can be seen from the figure that the 1st, 3rd, 5th, and 7th of these 8 planes from the left to the right side of the figure are all horizontal inclined surfaces, and the 2nd, 4th, 6th, and 8th are all horizontal planes. Of course, this is only an example, and the implementation can also be changed to X taking other numbers, or not including horizontal planes but only including horizontal inclined surfaces, etc.

[0125] 1d, by milling the surface p1d, the base material 11d is processed into a non-uniform thickness blank with a non-monotonically varying thickness in the transverse direction.

[0126] The length L12 of the irregular concave-convex surface p1d0 is L1, which means that it has not changed due to milling. The total width W12 of the irregular concave-convex surface p1d0 is greater than W1. It can be understood that the total width W12 is the sum of the widths of the X planes.

[0127] Correspondingly, referring to FIG1d , surface p2d of substrate 12d is also milled, transforming surface p2d from the horizontal surface shown in FIG1d(A) into the irregular concave-convex surface p2d0 shown in FIG1d(B). The milling of surface p2d of substrate 12d and surface p1d of substrate 11d is performed in a manner that complements their relative shapes. This means that the milled surface p2d0 and surface p1d0 are complementary in shape when facing each other.

[0128] Based on the complementary relative shapes, the irregular concave-convex surface p2d0 also specifically includes X planes connected in sequence along the transverse direction, exemplified in the figure as eight planes. The length L12 of the irregular concave-convex surface p2d0 is equal to L1, indicating that it remains unchanged due to milling. The total width W12 of the irregular concave-convex surface p2d0 is greater than W1. It can be understood that the total width W12 is the sum of the widths of the X planes of the irregular concave-convex surface p2d0.

[0129] Referring to Figure 1d, milling of surface p2d transforms substrate 12d into a non-uniformly thick blank with a non-monotonically varying thickness in the transverse direction. Due to the complementary shapes of irregular concave-convex surface p2d0 and irregular concave-convex surface p1d0, if milled substrates 12d and 11d are placed opposite each other, the sum of their thicknesses remains constant. This ensures that the upper and lower surfaces of the composite blank remain parallel during subsequent assembly.

[0130] The above describes the surface treatment of the two substrates in this embodiment. The following describes the surface treatment of the two composite materials.

[0131] In this embodiment, the surface p3d of the prepared composite material 21d is ground and polished with a wire wheel to remove the surface oxide scale and reveal the metallic luster; similarly, the surface p4d of the prepared composite material 22d is ground and polished with a wire wheel to remove the surface oxide scale and reveal the metallic luster.

[0132] Furthermore, to match the surface shape of substrates 11d and 12d, after removing the surface oxide scale, this embodiment also bends each composite material to match the corresponding irregular concave-convex surface. For example, composite material 21d is bent to match the corresponding irregular concave-convex surface p1d0, facilitating contact during subsequent assembly. For another example, composite material 22d is bent to match the corresponding irregular concave-convex surface p2d0, facilitating contact during subsequent assembly.

[0133] The surface treatment of this embodiment can ensure the interface bonding quality as in the aforementioned first embodiment, and can also be further used to prepare non-uniform thickness composite plates with non-monotonically varying transverse thicknesses, so as to improve the applicable scenarios and scope of the composite plates, enhance the corrosion resistance compared to existing steel plates, and avoid frequent welding and dissimilar welding between composite plates of different thicknesses.

[0134] <Fifth Embodiment of the Blank Surface Treatment Step>

[0135] The difference between this embodiment and the aforementioned fourth embodiment is that the thickness of the substrate in the transverse direction in the fourth embodiment is changed to the thickness of the substrate in the longitudinal direction in this embodiment.

[0136] For example, referring to Figure 1e, the surface p1e of the substrate 11e is milled and processed to transform the surface p1e from the horizontal surface in Figure 1e(A) into the irregular concave-convex surface p1e0 shown in Figure 1e(B). The irregular concave-convex surface p1e0 specifically includes X planes connected in sequence along the longitudinal direction, where X≥2. In the figure, there are 8 planes. It can be seen from the figure that the 1st, 3rd, 5th, and 7th of these 8 planes from the left to the right side of the figure are all longitudinal inclined surfaces, while the 2nd, 4th, 6th, and 8th are all horizontal planes. Of course, this is only an example, and the implementation can also be changed to X taking other numbers, or not including horizontal planes but only including longitudinal inclined surfaces, etc.

[0137] 1e, by milling the surface p1e, the base material 11e is processed into a non-uniform thickness blank with a non-monotonically varying thickness in the longitudinal direction.

[0138] The width W12 of the irregular concave-convex surface p1e0 is equal to W1, which means it has not changed due to milling. The total length L12 of the irregular concave-convex surface p1e0 is greater than L1. It can be understood that the total length L12 is the sum of the lengths of the X planes.

[0139] Correspondingly, referring to FIG1e , surface p2e of substrate 12e is also milled, transforming surface p2e from the horizontal surface shown in FIG1e(A) into the irregular concave-convex surface p2e0 shown in FIG1e(B). The milling of surface p2e of substrate 12e and surface p1e of substrate 11e is performed in a manner that complements their relative shapes, i.e., the milled surface p2e0 and surface p1e0 are complementary in shape when facing each other.

[0140] According to the relative shape complementarity, the irregular concave-convex surface p2e0 also specifically includes X planes connected in sequence along the longitudinal direction, exemplified as 8 planes in the figure. The width W12 of the irregular concave-convex surface p2e0 is equal to W1, and the total length L12 is greater than L1.

[0141] Referring to Figure 1e, by milling surface p2e, substrate 12e is processed into a non-uniform thickness blank with a non-monotonically varying thickness in the longitudinal direction. Due to the complementary shapes of irregular concave-convex surface p2e0 and irregular concave-convex surface p1e0, if milled substrates 12e and 11e are placed opposite each other, the sum of their thicknesses remains constant. This ensures that the upper and lower surfaces of the composite blank are parallel during subsequent assembly.

[0142] The above describes the surface treatment of the two substrates in this embodiment. The following describes the surface treatment of the two composite materials.

[0143] In this embodiment, the surface p3e of the prepared composite material 21e is ground and polished with a wire wheel to remove the surface oxide scale and reveal the metallic luster; similarly, the surface p4e of the prepared composite material 22e is ground and polished with a wire wheel to remove the surface oxide scale and reveal the metallic luster.

[0144] Furthermore, to match the surface shape of substrates 11e and 12e, after removing the surface oxide scale, this embodiment also bends each composite material to match the corresponding irregular concave-convex surface. For example, composite material 21e is bent to match the corresponding irregular concave-convex surface p1e0, facilitating contact during subsequent assembly. For another example, composite material 22e is bent to match the corresponding irregular concave-convex surface p2e0, facilitating contact during subsequent assembly.

[0145] Similar to the aforementioned fourth embodiment, this embodiment can also improve the applicable scenarios and scope of the composite plate, enhance the corrosion resistance compared to the existing steel plate, and avoid frequent welding and dissimilar welding between composite plates of different thicknesses.

[0146] The above introduces five preferred implementation methods of the blank surface treatment steps in the overall step of preparing the composite blank. Although only one surface of each of the substrate and the composite material is treated, it should be noted that no matter which of the above five implementation methods is used, the other surfaces of each substrate and composite material can be further treated to remove the oxide scale. Although this additional treatment to remove the oxide scale is not necessary to achieve the technical effect of the present invention, it may be better; for example, in addition to descaling the surface of the substrate facing the composite material, the surface of the substrate facing away from the composite material (i.e., the surface of the composite plate) can also be descaled.

[0147] The following will continue to introduce other sub-steps of the overall steps for preparing the composite blank.

[0148] The step of "applying a release agent on one surface of a composite material" is also a step of applying a release agent.

[0149] Among them, combined with the above, it can be seen that in the previous billet surface treatment step, the surface of the composite material that will be in contact with the substrate during assembly is subjected to surface treatment such as grinding and polishing in order to ensure the interface bonding quality of the composite plate; and the purpose of the release agent coating step is to use the release agent to avoid the surfaces of one composite material and another composite material that are in contact during assembly from bonding during the subsequent composite billet rolling step, which makes it difficult to separate them in the end.

[0150] Based on this, a release agent is applied to one of the two composite materials. If, during the previous blank surface treatment step, one surface of the selected composite material was surface treated and the other was not, then during this release agent application step, the release agent is applied to the "untreated" surface. If, as mentioned above, both surfaces of the selected composite material were surface treated during the previous blank surface treatment step, then during this release agent application step, the release agent is applied to the surface that is intended to face the other composite material during assembly. For example, using Figure 1a as an example, the release agent can be applied to surface p6a of composite material 22a or surface p5a of composite material 21a.

[0151] Regarding the release agent, two preferred implementations are provided here, which are introduced below respectively.

[0152] <First embodiment of the release agent>

[0153] In this embodiment, the release agent is a coating liquid containing silicon oxide and magnesium oxide, wherein the mass ratio of silicon oxide to magnesium oxide is 3: 1. The release agent of this embodiment can achieve a good isolation effect, ensuring the subsequent separation of the two composite board plates.

[0154] A method for preparing the release agent is provided, comprising mixing release agent powder, binder powder, and water in a mass ratio of 27:3:70 to obtain a fluid release agent coating solution. The release agent powder comprises silicon oxide and magnesium oxide, mixed in a mass ratio of 3:1. The binder powder comprises polyvinyl alcohol and thermosetting phenolic resin, mixed in a mass ratio of 1:1.

[0155] When the release agent is applied to the surface of the composite material, the amount of the release agent applied is 20 μg / m 2 , that is, the weight of the release agent per unit area of ​​the composite surface is 20 μmg. Wherein, y is the ratio of the thickness of the composite billet produced in the composite billet preparation step to the thickness of the composite plate subsequently rolled, which is also known as the composite billet rolling reduction ratio.

[0156] Furthermore, based on this embodiment, after the release agent is applied and before the subsequent assembly (that is, before the step of "assembling in the stacking order of substrate, composite, composite, and substrate"), the composite material coated with the release agent is placed in a trolley furnace for heating and drying. The drying temperature is 340-360°C and the drying time is 35-45 minutes.

[0157] <Second embodiment of the release agent>

[0158] In this embodiment, the release agent comprises, by weight, 25-35% silicon nitride, 5-10% thermosetting amino resin, and 55-70% water. Compared to existing release agents, and even compared to the first embodiment of the release agent described above, this release agent not only achieves excellent isolation, ensuring the subsequent separation of the two composite board panels, but also boasts strong chemical stability and high-temperature and thermal shock resistance from the active ingredient, silicon nitride. The thermosetting amino resin, serving as the binder, cures at low temperatures, is non-toxic, and achieves strong adhesion with minimal usage. Consequently, the release agent is inexpensive, simple to operate, and offers excellent isolation and adhesion properties.

[0159] Here, a preferred preparation method of the release agent is provided, comprising: first placing 5-10% silicon nitride (by weight percentage) in a container such as a beaker, then pouring in 15-25% water and stirring; after the silicon nitride has no granularity and no bubbles, pouring in 2-3% thermosetting amino resin and continuing to stir; when it becomes viscous, continue to pour in the remaining silicon nitride and water, stir for 3-5 minutes, and then pour in the remaining thermosetting amino resin; when it is stirred until it becomes viscous, the release agent is prepared.

[0160] When the release agent is applied on the surface of the composite material, the thickness of the release agent applied is 0.2 to 0.5 mm.

[0161] Furthermore, based on this embodiment, after the release agent is applied and before subsequent assembly, the composite material coated with the release agent is heated and dried at a temperature of 100 to 250° C. for 20 to 40 minutes.

[0162] Next, after completing the release agent application step, the step of "assembling the blanks in the stacking order of substrate, composite material, composite material, and substrate" is introduced.

[0163] This step of "assembling the blanks in the order of substrate, composite, composite, and substrate" is also the blank assembly step. In addition to the stacking order of substrate, composite, composite, and substrate, the following conditions must also be met:

[0164] 1) The surfaces of the substrate and the composite material that are in contact with each other are all surfaces that have undergone the surface treatment; for example, in the first embodiment of the blank surface treatment step described above, referring to FIG. 2a, the surface p2a of the substrate 12a and the surface p4a of the composite material 22a are in contact with each other, and the surface p1a of the substrate 11a and the surface p3a of the composite material 21a are in contact with each other; in the second embodiment of the blank surface treatment step described above, referring to FIG. 2b, the surface p1b0 and the surface p3b are in contact with each other, and the surface p4b and the surface p2b0 are in contact with each other; in the third embodiment of the blank surface treatment step described above, referring to FIG. 2c, the surface of the substrate 11c is in contact with each other. The surface p1c and the surface p3c of the composite material 21c are in contact with each other, and the surface p2c of the substrate 12c and the surface p4c of the composite material 22c are in contact with each other. In the fourth embodiment of the blank surface treatment step described above, referring to FIG. 2d , the irregular concave-convex surface p1d0 and the surface p3d of the composite material 21d are in contact with each other, and the irregular concave-convex surface p2d0 and the surface p4d of the composite material 22d are in contact with each other. In the fifth embodiment of the blank surface treatment step described above, referring to FIG. 2e , the irregular concave-convex surface p1e0 and the surface p3e of the composite material 21e are in contact with each other, and the irregular concave-convex surface p2e0 and the surface p4e of the composite material 22e are in contact with each other.

[0165] 2) The surface coated with the release agent faces the other composite material; for example, referring to FIG2a , one of the surfaces p6a and p5a is coated with a release agent 30a; referring to FIG2b , one of the surfaces p6b and p5b is coated with a release agent 30b; referring to FIG2c , one of the surfaces p6c ​​and p5c is coated with a release agent 30c; referring to FIG2d , one of the surfaces p6d and p5d is coated with a release agent 30d; referring to FIG2e , one of the surfaces p6e and p5e is coated with a release agent 30e; it should be noted that in FIG2a to 2e , for ease of understanding and explanation, the thickness of the release agent between the two composite materials (for example, reference numerals 30a, 30b, 30c, 30d, and 30e in FIG2a to 2e ) is exaggerated for illustration, that is, the ratio of the release agent thickness to the substrate thickness, the composite material thickness, and the seal width mentioned later is exaggerated;

[0166] 3) The composite material is placed in the center relative to the substrate; in this regard, the previous article introduced that the length and width of the composite material are smaller than the length and width of the substrate, L2<L1, W2<W1. When assembling, the distances from the two sides of the composite material in the horizontal direction to the corresponding two sides of the substrate are equal, and the distances from the two sides of the composite material in the longitudinal direction to the corresponding two sides of the substrate are also equal.

[0167] The following describes the three points respectively for the five embodiments of the blank surface treatment steps described above. Furthermore, since the composite blank is generally symmetrically arranged vertically, only one set of substrate + composite material in the composite blank is used as an example for description, such as the set above.

[0168] Regarding the first embodiment of the blank surface treatment step described above, referring to Figure 2a, the length L1 and width W1 of the surface p1a of the substrate 11a, the length L2 and width W2 of the surface p3a of the composite 21a, L2 = L1-L0, W2 = W1-W0, and the preferred value ranges of L0 and W0 are 90-150 mm, respectively; in the assembled state, the distance from the lateral side of the composite 21a (corresponding to the long side of the surface p3a) to the lateral side of the substrate 11a (corresponding to the long side of the surface p1a) is half of W0, and the distance from the longitudinal side of the composite 21a (corresponding to the short side of the surface p3a) to the longitudinal side of the substrate 11a (corresponding to the short side of the surface p1a) is half of L0.

[0169] Regarding the second embodiment of the blank surface treatment step described above, referring to FIG2b , the length L11 and width W11 of the surface p1b0 of the substrate 11b, the length L2 and width W2 of the surface p3b of the composite 21b, L2=L11-L0, W2=W11-W0, and the preferred value ranges of L0 and W0 are 90-150 mm, respectively; in the assembled state, the distance from the transverse side of the composite 21b (corresponding to the long side of the surface p3b) to the transverse side of the substrate 11b (corresponding to the long side of the surface p1b0) is half of W0, and the distance from the longitudinal side of the composite 21b (corresponding to the short side of the surface p3b) to the longitudinal side of the substrate 11b (corresponding to the short side of the surface p1b0) is half of L0.

[0170] Regarding the third embodiment of the blank surface treatment step described above, referring to FIG2c , the length L11 and width W11 of the surface p1c0 of the substrate 11c, the length L2 and width W2 of the surface p3c of the composite 21c, L2=L11-L0, W2=W11-W0, and the preferred value ranges of L0 and W0 are 90-150 mm, respectively; in the assembled state, the distance from the lateral side of the composite 21c (corresponding to the long side of the surface p3c) to the lateral side of the substrate 11c (corresponding to the long side of the surface p1c0) is half of W0, and the distance from the longitudinal side of the composite 21c (corresponding to the short side of the surface p3c) to the longitudinal side of the substrate 11c (corresponding to the short side of the surface p1c0) is half of L0.

[0171] Regarding the fourth embodiment of the blank surface treatment step described above, referring to FIG2d , the length L12 and width W12 of the irregular concave-convex surface p1d0 of the substrate 11d, the length L2 and width W2 of the surface p3d of the composite 21d, L2=L12-L0, W2=W12-W0, and the preferred value ranges of L0 and W0 are 90 to 150 mm, respectively; in the assembled state, the distance from the lateral side of the composite 21d (corresponding to the long side of the surface p3d) to the lateral side of the substrate 11d (corresponding to the long side of the irregular concave-convex surface p1d0) is half of W0, and the distance from the longitudinal side of the composite 21d (corresponding to the short side of the surface p3d) to the longitudinal side of the substrate 11d (corresponding to the short side of the irregular concave-convex surface p1d0) is half of L0.

[0172] For the fifth embodiment of the blank surface treatment step described above, referring to Figure 2e, the length L12 and width W12 of the irregular concave-convex surface p1e0 of the substrate 11e, the length L2 and width W2 of the surface p3e of the composite 21e, L2 = L12-L0, W2 = W12-W0, and the preferred value ranges of L0 and W0 are 90 to 150 mm, respectively; in the assembled state, the distance from the lateral side of the composite 21e (corresponding to the long side of the surface p3e) to the lateral side of the substrate 11e (corresponding to the long side of the irregular concave-convex surface p1e0) is half of W0, and the distance from the longitudinal side of the composite 21e (corresponding to the short side of the surface p3e) to the longitudinal side of the substrate 11e (corresponding to the short side of the irregular concave-convex surface p1e0) is half of L0.

[0173] The above describes the assembly step. In a preferred embodiment, after the assembly step, the four stacked billets are placed in a four-column hydraulic press. The opposing surfaces of the two substrates (i.e., the upper surface of the upper substrate and the lower surface of the lower substrate) are pressurized to a pressure of 500 tons or more. This ensures closer contact between adjacent billets.

[0174] Furthermore, in the step "Prepare four sealing strips of width W3, place them against the four sides of the two composite materials, and perform gas shielded welding between adjacent sealing strips and between the sealing strips and the base material, so that the two base materials and the sealing strips form a single integral body, thereby obtaining a composite billet base," the placement of the sealing strips allows the four stacked steel billets to be connected into a single composite billet base. Specifically, referring to Figures 2a-2e, the composite billet base comprises: two base materials forming the upper and lower surfaces, two composite materials located in the middle, and four sealing strips forming four frames surrounding the two composite materials and connecting the two base materials. In Figures 2a-2e, the sealing strips are labeled 40a, 40b, 40c, 40d, and 40e, respectively.

[0175] The width of the seal is W3 = 2T2-1 ~ 2mm. A seal of this width is used to wrap the upper and lower composite materials at the same time, thereby improving the wrapping effect. It should be noted here that, as mentioned above, for the sake of ease of understanding and explanation, the thickness of the release agent (such as the numbers 30a, 30b, 30c, 30d and 30e) is magnified in Figures 2a to 2e. Accordingly, the width of the seal shown in Figures 2a to 2e is shown to be larger than the sum of the thicknesses of the two composite materials, but this is only because the thickness of the release agent is magnified. In fact, the width of the seal is W3 = 2T2-1 ~ 2mm, that is, the width of the seal is slightly smaller than the sum of the thicknesses of the two composite materials by 1 to 2mm.

[0176] Furthermore, among the four seals, two seals are respectively attached to the two side edges of the two composite materials in the horizontal direction, with a length L31 = L2-1 ~ 2mm; the other two seals are respectively attached to the two side edges of the two composite materials in the longitudinal direction, with a length L32 = W2-1 ~ 2mm.

[0177] Preferably, the thickness T3 of the seal is 12-15 mm.

[0178] Each seal strip can be formed by directly cutting it from a steel plate according to the thickness T3, width W3, and length L31 or L32 without welding, or it can be formed by welding multiple seal strips of different lengths together, for example, the seal strips at the longitudinal side edges of the two composite materials in the fourth embodiment of the blank surface treatment step described above, and the seal strips at the transverse side edges of the two composite materials in the fifth embodiment of the blank surface treatment step described above.

[0179] As a preferred embodiment, in this step, before performing gas shielded welding between adjacent seals or between a seal and a substrate, both ends and both sides of each seal may be ground and polished to remove surface oxide scale and improve welding effect; and / or, both ends and both sides of each seal may be grooved first.

[0180] Furthermore, as a preferred embodiment, in the step of "gas shielded welding is performed between adjacent seals and between the seal and the substrate", the welding speed is 300-360 mm / min, and the interpass temperature during the welding process is controlled to be 135-165°C.

[0181] In gas shielded welding, the shielding gas is 75-80% Ar + 20-25% CO2 by volume.

[0182] Next, for the step of "machining a circular hole on the seal at the groove on the side of the composite blank base, and welding a seamless steel pipe at the circular hole", the groove described therein is a groove formed between the two base materials and outside the seal; in this step, a circular hole is machined to weld the seamless steel pipe to facilitate subsequent vacuuming of the inside of the composite blank.

[0183] As a preferred embodiment, the circular hole is processed in the middle of the short side (ie, the side in the longitudinal direction) of the composite blank base blank, but the present invention is not limited thereto.

[0184] As a preferred embodiment, the diameter of the circular hole is 8 to 12 mm; accordingly, the outer diameter of the seamless steel pipe is consistent with the diameter of the circular hole, which is 8 to 12 mm, the wall thickness is 1.2 to 2 mm, and the length is 200 to 400 mm.

[0185] Next, the step of "surfacing the grooves on the four sides of the composite base blank" employs submerged arc surfacing. As will be appreciated, this surfacing process forms a rectangular filler layer outside the four frames formed by the seal strips. See Figures 2a to 2e, where the filler layers formed by the surfacing are designated 50a, 50b, 50c, 50d, and 50e, respectively.

[0186] As a preferred method, before cladding, the flux is baked at 350°C for 2 hours and then held at 150°C for 1 hour. During the cladding process, the interpass temperature is controlled at 135-165°C, and the welding speed is 420-480 mm / min. This submerged arc cladding technology, combined with the previous sealing and gas shielded welding, secures the four steel billets together, ensuring joint strength and preventing cracking during the subsequent composite billet rolling process. This further enhances the interface bonding, while maintaining the aforementioned quality advantages of the composite plate.

[0187] In addition, during the cladding welding process, before each welding construction, the weld attachments need to be cleaned to keep the weld clean; after welding is completed, the insulation cotton is covered for insulation.

[0188] Next, the step of "using the seamless steel pipe to perform three vacuuming and two breaking of the composite billet, and finally making the vacuum degree ≤10 -2 Pa" is preferably:

[0189] First, connect the seamless steel pipe to the vacuum pump, connect the seamless steel pipe to the space inside the composite blank (such as the surface gap between the composite material and the base material, the surface gap between the composite materials, the end face gap between the composite material and the seal, etc.), and evacuate the composite blank to a vacuum degree of ≤10 -2 Pa, and then maintain the pressure for more than 4 hours; then connect the seamless steel pipe to a nitrogen device (such as a nitrogen generator, a nitrogen tank), which will break the air in the composite billet and fill the space inside the composite billet with nitrogen;

[0190] After that, the seamless steel pipe is reconnected to the vacuum pump to evacuate the composite billet to a vacuum degree of ≤10 -1Pa, no pressure maintenance; then connect the seamless steel pipe to the nitrogen device, break the composite billet and fill it with nitrogen;

[0191] Finally, the seamless steel pipe is connected to the vacuum pump for the third time to evacuate the composite billet to a vacuum degree of ≤10 -2 Pa.

[0192] In this way, the air in the space can be prevented from causing surface oxidation at the composite interface during subsequent composite billet rolling, thereby ensuring the bonding quality of the composite interface.

[0193] Furthermore, in this step, the seamless steel pipe is sealed by a method currently available in the steel industry, such as heating and flattening the seamless steel pipe with a flame gun to achieve sealing.

[0194] The above describes in detail the overall steps for preparing the composite billet. Specific settings such as surface treatment, three vacuum extractions and two air breaks, welding, and sealing lay the foundation for the subsequent composite billet to obtain excellent interface bonding quality and surface quality during subsequent rolling. The setting of the isolation agent is more conducive to the smooth separation of the two composite small plates.

[0195] The above describes in detail the overall steps for preparing the composite billet. As previously mentioned, the preparation method of the present invention further includes the overall step of rolling the composite billet after the overall step of preparing the composite billet. The present invention provides three implementation methods of the overall step of rolling the composite billet, each of which is described in detail below.

[0196] <First embodiment of the overall step of composite billet rolling>

[0197] In this embodiment, referring to FIG3a , the composite billet rolling process includes the following sub-steps:

[0198] The obtained composite blank is heated at a soaking temperature of 1150-1220°C, a total heating time of ≥1.2 min / mm×t, where t is the thickness of the composite blank, and a soaking section holding time of 30 min-50 min;

[0199] A two-stage controlled rolling process of rough rolling and finishing rolling is adopted. In the rough rolling stage, the starting rolling temperature is ≤1050°C and the final rolling temperature is ≥980°C. The horizontal rolling is performed first and then the longitudinal rolling. During the longitudinal rolling, at least one pass has a reduction of ≥35mm. The total rough rolling reduction is 40-60%. The rough rolling stage is terminated when the thickness of the intermediate billet is 2.5-3.5 times the target thickness of the composite plate. The intermediate billet is then cooled by water. When the surface temperature of the intermediate billet drops below 860°C, the finishing rolling stage is started. The final rolling temperature of the finishing rolling stage is ≥780°C, and the total finishing reduction is 55-75% to obtain the composite plate.

[0200] After rolling, the composite plate enters an ultra-fast cooling system for intermittent cooling. The ultra-fast cooling system has 24 cooling manifolds arranged at intervals of 1 m along the roller table. The cooling distance of each cooling manifold is 1 m. When the composite plate passes through the ultra-fast cooling system, the opening and closing states of all 24 cooling manifolds are controlled by opening N cooling manifolds and then closing M cooling manifolds. The cooling water pressure is 0.15-0.30 MPa, the cooling rate is 3-15°C / s, and the final cooling temperature is 380-590°C. Wherein N is 2, 3 or 4, and M is 2, 3 or 4.

[0201] After the composite plate leaves the ultra-fast cooling system, it enters the straightening machine for straightening. The straightened composite plate is placed at a temperature of T f -150℃~T f The stack cooling is carried out between two steel plates at +150℃, and the stack cooling time is 0.4min / mm×t0±5min, where t0 is the thickness of the composite plate. After the stack cooling is completed, the cooling bed on the composite plate is naturally cooled to room temperature; wherein, T f =550+30Si-20Mn+15Cr-15Ni+10Mo, where the element symbols in this formula represent 100 times the mass percentage of each element in the substrate;

[0202] At this point, the overall step of rolling the composite billet is completed and the overall step of separating and straightening the composite billet is entered.

[0203] Compared with the prior art, this embodiment:

[0204] First, the heating and rolling technology used, through the control of the heating temperature, heating time, holding time, various temperatures during rolling, reduction, cooling temperature, cooling rate and other parameters, can not only ensure the mechanical properties of the final composite plate, but also avoid the corrosion resistance of the composite layer from being reduced during the preparation process of the composite plate;

[0205] On the other hand, by adopting the intermittent cooling method, when the large composite plate passes through the ultra-fast cooling system, it travels in the alternating opening and closing of the cooling manifolds, so that each part of the large composite plate will be cooled, turned red, cooled, turned red... and so on, until the large composite plate leaves the ultra-fast cooling system; in this way, in the cooling-turning red cycle of the large composite plate, the carbon steel substrate continuously undergoes phase change and self-tempering effect, and the phase change reaction gradually penetrates into the core until the entire carbon steel substrate completes the phase change; this intermittent cooling process is different from conventional reciprocating cooling. The turning red and self-tempering of reciprocating cooling occur after the surface or near-surface layer has completed the phase change. The temperature difference or cooling rate between the surface and the core is large, and the microstructure and mechanical properties are different. The difference is also quite large. However, in the intermittent cooling process of this embodiment, at the same time, some parts of the composite plate are in a cooling state, while some parts are in a red-hot / self-tempering state. Moreover, each part of the composite plate is alternately cooled and red-hot / self-tempered over time, so that the differences in temperature, cooling rate, structure, and performance between the surface and core of the composite plate are relatively small. For example, the Vickers hardness difference of the base layer of the final composite plate in the thickness direction is ≤10, the strength difference between the head, middle and tail is ≤40MPa, and the strength difference of the entire plate is ≤40MPa. At the same time, the intermittent cooling can further improve the plate shape of the composite plate, that is, the unevenness is low. Even if straightening is not performed after cooling and the plate is directly cooled on the cooling bed, an excellent plate shape can be obtained.

[0206] On the other hand, stack cooling, especially the temperature of the two steel plates and the stack cooling time during stack cooling, can further improve the structure, performance and plate shape of the final composite plate compared to the first embodiment described above.

[0207] Furthermore, in the intermittent cooling: if the thickness of the composite plate is less than 54 mm, for example, when the thickness is 10-54 mm, the roller speed of the ultra-fast cooling system is 0.4-0.8 m / s, the 1st to 4th groups of cooling manifolds are opened, the 5th to 6th groups of cooling manifolds are not opened, the 7th to 8th groups of cooling manifolds are opened, the 9th to 10th groups of cooling manifolds are not opened, the 11th to 12th groups of cooling manifolds are opened, the 13th to 14th groups of cooling manifolds are not opened, the 15th to 16th groups of cooling manifolds are opened, the 17th to 18th groups of cooling manifolds are not opened, the 19th to 20th groups of cooling manifolds are opened, the 21st to 22nd groups of cooling manifolds are not opened, and the 23rd to 24th groups of cooling manifolds are opened; the composite plate passes through the ultra-fast cooling system once, and the intermittent cooling is completed.

[0208] Further preferably, during the intermittent cooling, if the thickness of the composite plate is greater than 54 mm, for example, greater than 54 mm and less than 70 mm, the roller speed of the ultra-rapid cooling system is greater than 0.2 m / s and less than 0.6 m / s, the first to fourth groups of cooling manifolds are opened, the fifth to eighth groups of cooling manifolds are closed, the ninth to twelfth groups of cooling manifolds are opened, the thirteenth to sixteenth groups of cooling manifolds are closed, the seventeenth to twentieth groups of cooling manifolds are opened, the twenty-first to twenty-second groups of cooling manifolds are closed, and the twenty-third to twenty-fourth groups of cooling manifolds are opened; the composite plate passes through the ultra-rapid cooling system once, completing the intermittent cooling. In this way, shape and uniformity control of thick stainless steel composite plates is achieved, overcoming the production difficulties of existing thick stainless steel composite plates.

[0209] Preferably, during the intermittent cooling, when the thickness of the composite plate slab is ≥70 mm, for example, when the thickness is 70 mm to 110 mm, the roller speed of the ultra-rapid cooling system is 0.4 to 0.9 m / s. The composite plate slab first enters the ultra-rapid cooling system entrance in the forward direction. When its head reaches the 24th group of cooling manifolds, the rollers reverse, and the composite plate slab passes through the ultra-rapid cooling system in the reverse direction and exits the ultra-rapid cooling system entrance, completing the intermittent cooling. Furthermore, preferably, the 1st to 4th groups of cooling manifolds are opened, the 5th to 8th groups of cooling manifolds are closed, the 9th to 12th groups of cooling manifolds are opened, the 13th to 16th groups of cooling manifolds are closed, the 17th to 20th groups of cooling manifolds are opened, the 21st to 22nd groups of cooling manifolds are closed, and the 23rd to 24th groups of cooling manifolds are opened. In this way, the shape control and uniformity control of the extra-thick stainless steel composite plate are achieved, overcoming the production difficulties of existing extra-thick stainless steel composite plates.

[0210] Furthermore, in this embodiment, the step of "placing the straightened composite plate at a temperature of T f -150℃~T f In the process of “stack cooling between two steel plates at +150℃”, the length and width of the steel plates used are both greater than those of the large composite plate, and the thickness of the steel plates used is twice that of the large composite plate.

[0211] <Second embodiment of the overall step of composite billet rolling>

[0212] This embodiment, referring to FIG3b , differs from the first embodiment of the composite billet rolling process in that the heating and rolling steps, while the post-rolling steps (including intermittent cooling, straightening, stack cooling, and natural cooling on a cooling bed) are identical to those of the first embodiment of the composite billet rolling process, are not described in detail here. The following describes only the steps that differ from the first embodiment of the composite billet rolling process (i.e., the heating and rolling steps).

[0213] Specifically, in this embodiment, the heating step of the composite billet rolling process is as follows:

[0214] The obtained composite blank is heated in five stages, including preheating, first heating, second heating, third heating and soaking. The preheating temperature is ≤850°C, the residence time is (0.45~0.55) min / mm×t, the first heating temperature is 1030~1090°C, the residence time is (0.35~0.45) min / mm×t, the second heating temperature is 1100~1160°C, the residence time is (0.25~0.35) min / mm×t, the third heating temperature is 1140~1180°C, the residence time is (0.15~0.25) min / mm×t, the soaking temperature is 1170~1210°C, the residence time is (0.10~0.20) min / mm×t, and t is the thickness of the composite blank.

[0215] The rolling steps of the composite billet rolling process are as follows:

[0216] A two-stage controlled rolling method of rough rolling + finishing rolling is adopted, in which longitudinal rolling is adopted for the first pass, and the rolling reduction is ≥46mm; transverse rolling is adopted from the second pass until the composite billet is rolled to the target width of the final composite plate in the nth pass, and the rolling reduction in the second pass is ≥25mm; longitudinal rolling is adopted from the n+1th pass, and the rolling reduction in the n+1th pass is ≥30mm; during the entire rough rolling stage, the rolling temperature of the first pass is ≥1060℃, the start rolling temperature of the remaining passes is ≤1050℃, and the final rolling temperature is ≥1000℃; the rough rolling stage is terminated when the thickness of the intermediate billet is 2.5 to 3.5 times the target thickness of the composite plate, and the intermediate billet is kept warm, during which water cooling is carried out. When the surface temperature of the intermediate billet drops below 840℃, the finishing rolling stage begins, and the start rolling temperature of the finishing rolling stage is 810℃ to 840℃, and the final rolling temperature is 780℃ to 810℃.

[0217] Compared with the prior art, this embodiment also adopts intermittent cooling and stack cooling, and accordingly also has the beneficial effects brought by the intermittent cooling process and stack cooling process. Please refer to the introduction of the first embodiment of the composite billet rolling general steps in the previous text. Furthermore, compared with the prior art, the heating process of this embodiment can better control the heating rate of the composite billet in each section, ensure the uniform heating of the billet, avoid the composite billet cracking and air leakage due to the difference in thermal properties of the composite material and the composite material, and thus ensure the interface bonding effect; furthermore, the rolling process of this embodiment adopts the method of first longitudinal rolling, then transverse rolling, and then longitudinal rolling for rough rolling, which can ensure the realization of large reduction rolling, so that the core of the composite billet is effectively penetrated, promotes the deformation of the core, and ensures the bonding rate of the composite interface; when waiting for temperature, an instant cooling device is used for cooling, which reduces the waiting time and improves the rolling efficiency. At the same time, it avoids the waiting time being too long and the growth of the carbon steel substrate grains; the temperature control in the finishing rolling stage can refine the grains and ensure that the composite plate has good low-temperature impact toughness.

[0218] <Third embodiment of the overall step of composite billet rolling>

[0219] This embodiment, referring to FIG. 3c , differs from the first embodiment of the composite billet rolling process in that the heating and rolling steps, while the post-rolling steps (including intermittent cooling, straightening, stack cooling, and natural cooling on a cooling bed) are identical to those of the first embodiment of the composite billet rolling process and are not described in detail here. The following describes only the steps that differ from the first embodiment of the composite billet rolling process (i.e., the heating and rolling steps).

[0220] Specifically, in this embodiment, the heating step of the composite billet rolling process is as follows:

[0221] The obtained composite blank is heated in four stages, namely preheating, first heating, second heating and equalizing. The preheating temperature is 950-1000°C, the residence time is 0.3 min / mm×t, the first heating temperature is 1050-1100°C, the second heating temperature is 1120-1180°C, the equalizing temperature is 1150-1200°C, and the total residence time of the first heating, second heating and equalizing is 1.5 min / mm×t+20-40 min, where t is the thickness of the composite blank.

[0222] The rolling steps of the composite billet rolling process are as follows:

[0223] After the composite billet leaves the heating furnace, it is first descaled with high-pressure water and then rolled. During the rolling process, transverse rolling is adopted starting from the first pass until the composite billet is rolled to a width of Wt+0~40mm by the nth pass, where Wt is the target width of the composite plate, and the total reduction rate up to this point is ≥30%. Longitudinal rolling is adopted starting from the n+1th pass, and the rolling reduction rate of the n+1th pass is ≥20%. When the thickness of the intermediate billet is 2.5~3.5 times the target thickness of the composite plate, it is started to wait for temperature. When the surface temperature of the intermediate billet drops below 880℃, rolling is resumed until the rolling is completed, and the final rolling temperature is T r ±20℃, the total reduction rate of the entire rolling process is ≥75%; The element symbols in this formula represent 100 times the mass percentage of each element in the base material.

[0224] Compared to the prior art, this embodiment also utilizes intermittent cooling and stack cooling, and accordingly possesses the beneficial effects of these processes. For details, see the first embodiment of the composite billet rolling process described above. Furthermore, compared to the prior art, the heating process of this embodiment ensures that the composite billet is fully heated, reducing deformation resistance during rolling. Furthermore, the rolling process of this embodiment not only reduces deformation resistance during widening, but also achieves a good metallurgical bond between the composite material and the substrate, effectively ensuring the interfacial bonding strength of the composite plate, and furthermore, achieving excellent performance of the composite plate.

[0225] The above describes in detail the overall steps of rolling the composite billet. As mentioned above, the preparation method of the present invention also includes the overall step of separating and straightening the composite plate. Specifically, the overall step of separating and straightening the composite plate includes the following sub-steps:

[0226] The large composite plate obtained in the above composite billet rolling process is cut with a plasma cutter to remove the portion other than the seal, and the large composite plate is separated into two small composite plates, one above the other.

[0227] Place the composite board with the composite layer facing upwards on the flattening machine for flattening. When flattening horizontally, control the flattening force of the flattening machine to be F1 = ν × a × b × c. 横 ×σ 横 / (d×(ν-c 横 / a)); When flattening longitudinally, control the flattening force F2 = a × b × c 纵 ×σ 纵 / (d+c 纵 ); where a is the width of the composite board, b is the thickness of the composite board, c 横 It is the unevenness per meter of the composite board in the horizontal direction, in mm, c 纵is the unevenness per meter of the composite board in the longitudinal direction, in mm, d is the working distance of the flattening machine, σ 横 is the tensile yield strength of the composite plate in the transverse direction, σ 纵 is the tensile yield strength of the composite plate in the longitudinal direction, ν is the Poisson's ratio;

[0228] Finally, the composite plate is cold straightened to obtain the finished single-sided stainless steel composite plate.

[0229] In this way, by regulating the flattening force of the flattening machine, the present invention can achieve plate shape control of the composite plate, which is easy to operate and has excellent effects.

[0230] The portion outside the seal in the step of "cutting the edge of the composite plate to remove the portion outside the seal" refers to the edge of the composite plate, which is converted from the seal and filler layer in the composite billet mentioned above after the composite billet rolling step. By removing this portion, the stainless steel cladding is exposed. Without this portion's connecting function, the composite plate is separated into two small composite plates, one above the other.

[0231] Referring to Figures 4a-4e, corresponding to the five embodiments of the blank surface treatment steps described above, Figures 4a-4e illustrate the cross-sectional shapes of two corresponding single-sided composite sheet panels (i.e., the final composite sheet). Each resulting composite sheet panel consists of a cladding layer and a base layer. The cladding layer is rolled from the original composite material, and the base layer is rolled from the original base material. Therefore, in Figures 4a-4e, the cladding layer is still labeled with the number of the original composite material, and the base layer is still labeled with the number of the original base material. Among them, referring to Figure 4a, based on the first embodiment of the blank surface treatment step described above, the prepared single-sided stainless steel composite plate is an equal thickness plate with a total thickness of 5 to 55 mm, a base thickness of 4 to 45 mm, and a composite layer thickness of 1 to 10 mm; referring to Figures 4b to 4e, based on the second to fifth embodiments of the blank surface treatment steps described above, the prepared single-sided stainless steel composite plate is a non-equal thickness plate, the maximum total thickness of the composite plate (corresponding to the thickest position of the composite plate) is 7 to 55 mm and the minimum value (corresponding to the thinnest position of the composite plate) is 5 to 47 mm, the maximum base thickness is 6 to 45 mm (corresponding to the thickest position of the composite plate) and the minimum value (corresponding to the thinnest position of the composite plate) is 4 to 37 mm, and the composite layer thickness is 1 to 10 mm.

[0232] Furthermore, the present invention provides a single-sided stainless steel composite plate, which is prepared by the preparation method of any one of the embodiments described above. It has both excellent mechanical properties and corrosion resistance, and has excellent plate shape, interface bonding quality, uniformity, impact toughness and surface quality compared to the existing technology.

[0233] Specifically, the single-sided stainless steel composite plate according to one embodiment of the present invention was sampled in accordance with GB / T 2975-Steel and Steel Products-"Sampling Location and Preparation of Specimens for Mechanical Properties Tests", and:

[0234] In terms of plate shape, the test is carried out in accordance with GB / T 709- "Dimensions, shape, weight and allowable deviations of hot-rolled steel plates and strips". The unevenness of the composite plate is ≤3mm / m, and even ≤2mm / m.

[0235] In terms of interface bonding quality, according to GB / T 6396-Test Methods for Mechanical and Process Properties of Composite Steel Plates, a tensile test was conducted on the composite plate. The composite interface bonding rate of the composite plate was 100%, and the shear strength was ≥300MPa, and even the shear strength was ≥360MPa.

[0236] In terms of mechanical properties, tensile tests were conducted in accordance with GB / T 6396-"Test methods for mechanical and process properties of composite steel plates" and GB / T 228.1-"Tensile tests on metallic materials - Part 1: Test methods at room temperature". The yield strength of the composite plate is ≥345MPa, the tensile strength is ≥490MPa, the elongation after fracture is ≥18%, and the yield strength ratio is ≤0.85. The Vickers hardness difference in the thickness direction of the base layer of the composite plate is ≤10, the head-middle-tail strength difference is ≤40MPa, and the strength difference across the entire plate is ≤40MPa.

[0237] According to GB / T 6396-"Test Methods for Mechanical and Process Properties of Composite Steel Plates" and GB / T 229-"Charpy Pendulum Impact Test Method for Metallic Materials", the composite plate is tested to have an impact energy of ≥120J at 0°C, ≥120J at -20°C, and ≥120J at -40°C. Furthermore, the composite plate may have an impact energy of ≥240J at 0°C, ≥200J at -20°C, and ≥150J at -40°C.

[0238] Sampling was carried out in accordance with GB / T 2975-Steel and Steel Products-"Sampling Location and Preparation of Specimens for Mechanical Properties Tests", and testing was carried out in accordance with GB / T 6396-"Test Methods for Mechanical and Process Properties of Composite Steel Plates". The composite plate had no cracks when bent outward 180° and no cracks when bent inward 180°.

[0239] Sampling was carried out in accordance with GB / T 6396-Test Methods for Mechanical and Process Properties of Composite Steel Plates, and testing was conducted in accordance with GB / T 4334-Corrosion of Metals and Alloys—Test Methods for Intergranular Corrosion of Austenitic and Ferritic-Austenitic (Duplex) Stainless Steels. The composite plate was boiled in a sulfuric acid-copper sulfate solution for 20 hours and bent 180°. No intergranular corrosion cracks were observed in the composite layer.

[0240] The detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present invention. They are not intended to limit the scope of protection of the present invention. Any equivalent implementation methods or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

[0241] The beneficial effects of the present invention are further illustrated below through a plurality of embodiments. Of course, these embodiments are only a part of the many variations of the present invention, but not all of them.

[0242] In these embodiments, the steel types and chemical compositions of the selected composite materials and substrates are shown in Table 1. “-” indicates that the corresponding elements were not actively added during the preparation of the steel billet (the content was zero or close to zero).

[0243] Table 1

[0244] The substrates and composite materials listed in Table 1 above were used in accordance with the overall steps for preparing a composite blank in the preparation method of the present invention to produce a composite blank. For the composite blanks of each example, the substrate, composite material, composite blank thickness, and composite blank type used are shown in Table 2. In the "Composite Blank Type" column of Table 2, "①," "②," "③," "④," and "⑤" respectively indicate that the composite blank was prepared according to the first, second, third, fourth, and fifth embodiments of the blank surface treatment steps described above.

[0245] Table 2

[0246] Furthermore, for each example, the composite billet rolling steps of the preparation method of the present invention were implemented, with specific parameters shown in Tables 3 and 4. In the "Heating + Rolling Implementation Method" column of Table 3, "I," "II," and "III," respectively, indicate that the corresponding example was implemented according to the first, second, and third implementation methods of the composite billet rolling steps described above.

[0247] Table 3

[0248] Table 4

[0249] Furthermore, the above-described embodiments were implemented according to the overall steps of separating and straightening the composite plate of the present invention to produce single-sided stainless steel composite plate products. The total thickness, base layer thickness, cladding layer thickness, and base layer microstructure of the composite plate products of these embodiments are shown in Table 5. The columns for composite plate thickness and base layer thickness in Table 5 indicate ranges, representing minimum to maximum thicknesses.

[0250] Table 5

[0251] Furthermore, using the sampling and testing standards disclosed above, samples of the composite panels from various examples were sampled and tested. All examples demonstrated a 100% interfacial bonding rate, a passing 180° inward bend (no cracks), and a passing 180° outward bend (no cracks). Furthermore, after being boiled in a sulfuric acid-copper sulfate solution for 20 hours and then bent 180°, the composite layer showed no intergranular corrosion cracks. Other performance test results are shown in Table 6.

[0252] Table 6

[0253] To summarize, compared with the prior art, the present invention has the following advantages: on the one hand, in the entire preparation method, the corrosion resistance and mechanical strength of the stainless steel composite plate are guaranteed through specific control of the process, and the degradation of the corrosion resistance and mechanical properties during the rolling process of the composite billet is avoided; on the other hand, the problems of poor plate shape, poor interface bonding quality, and poor surface quality of the existing thick plates of stainless steel composite plates are solved, so that the stainless steel composite plate has excellent plate shape and interface bonding quality, and avoids obvious surface defects such as pits and scratches caused by the existing explosive composite technology; on the other hand, the yield rate in the production process is high and the production efficiency is high.

Claims

1. A method for preparing a stainless steel composite plate, characterized in that: The following steps are involved: 1) Composite blank preparation Prepare two carbon steel billets with a thickness of T1, a length of L1, and a width of W1 as base materials; and prepare two stainless steel billets with a thickness of T2, a length of L2<L1, and a width of W2<W1 as composite materials; Performing surface treatment on at least one surface of each of the two substrates and the two composite materials; Apply a release agent to one surface of a composite material; The blanks are assembled in the order of stacking substrate, composite material, composite material, and substrate; wherein the composite material is placed in the center relative to the substrate, the surfaces of the substrate and the composite material that are in contact with each other are both surfaces that have undergone the surface treatment, and the surface coated with the release agent faces the other composite material; Prepare four seals with a width of W3 = 2T2-1 ~ 2mm, attach the seals to the four sides of the two composite materials, perform gas shielded welding between adjacent seals and between the seals and the substrate, so that the two substrates and the seals form a whole, and obtain a composite blank base blank; A circular hole is machined on the seal strip at the groove on the side of the composite blank base, and a seamless steel pipe is welded at the circular hole; Performing surfacing welding on the grooves on four sides of the composite blank base blank; The composite billet is subjected to three vacuum extractions and two air breaks through the seamless steel pipe, and finally the vacuum degree is ≤10 -2 Pa; then the seamless steel pipe is sealed to obtain a composite billet; 2) Composite billet rolling The obtained composite billet is heated, and then subjected to two-stage controlled rolling of rough rolling + finishing rolling; After rolling, the composite plate enters the ultra-fast cooling system for intermittent cooling: the ultra-fast cooling system has 24 groups of cooling manifolds arranged at intervals of 1m along the roller, and the cooling distance of each group of cooling manifolds is 1m. When the composite plate passes through the ultra-fast cooling system, the opening and closing states of all 24 groups of cooling manifolds are controlled in a manner of opening N groups of cooling manifolds and then not opening M groups of cooling manifolds. The cooling water pressure is 0.15-0.30MPa, the cooling rate is 3-15℃ / s, and the final cooling temperature is 380-590℃; wherein N is 2, 3 or 4, and M is 2, 3 or 4; After the composite plate leaves the ultra-fast cooling system, it directly enters the straightening machine for straightening. The straightened composite plate is placed at a temperature of T f -150℃~T f The stack cooling is carried out between two steel plates at +150℃, and the stack cooling time is 0.4min / mm×t0±5min, where t0 is the thickness of the composite plate. After the stack cooling is completed, the composite plate is cooled naturally on the cooling bed; wherein, T f =550+30Si-20Mn+15Cr-15Ni+10Mo, the element symbols in this formula represent 100 times the mass percentage of each element in the substrate; 3) Composite plate separation and straightening The edge of the large composite board is cut to remove the portion other than the seal, and the large composite board is separated into two small composite boards, an upper one and an lower one; Place the composite board with the composite layer facing upwards on the flattening machine for flattening. When flattening horizontally, control the flattening of the flattening machine. Force F1 = ν × a × b × c 横 ×σ 横 / (d×(ν-c 横 / a)); When flattening longitudinally, control the flattening force of the flattening machine F2 = a×b×c 纵 ×σ 纵 / (d+c 纵 ), where a is the width of the composite board, b is the thickness of the composite board, and c is 横 It is the unevenness per meter of the composite board in the horizontal direction, in mm, c 纵 is the unevenness per meter of the composite board in the longitudinal direction, in mm, d is the working distance of the flattening machine, σ 横 is the tensile yield strength of the composite plate in the transverse direction, σ 纵 is the tensile yield strength of the composite plate in the longitudinal direction, ν is the Poisson's ratio; Finally, the small composite plate is cold straightened to obtain a finished single-sided stainless steel composite plate.

2. The method for preparing a stainless steel composite plate according to claim 1, characterized in that: Step "Through the seamless steel pipe, the composite blank is subjected to three vacuum extractions and two air breaks, and finally the vacuum degree is ≤10 -2 Pa” is specifically: First, connect the seamless steel pipe to the vacuum pump to evacuate the composite billet to a vacuum degree of ≤10 -2 Pa, and then maintain the pressure for more than 4 hours; next, connect the seamless steel pipe to the nitrogen device, break the composite billet, and fill it with nitrogen; After that, the seamless steel pipe is reconnected to the vacuum pump to evacuate the composite billet to a vacuum degree of ≤10 -1 Pa, without pressure maintenance; then the seamless steel pipe is connected to the nitrogen device, the composite billet is vented and filled with nitrogen; Finally, the seamless steel pipe is connected to the vacuum pump for the third time to evacuate the composite billet to a vacuum degree of ≤10 -2 Pa.

3. The method for preparing a stainless steel composite plate according to claim 1, characterized in that: The step of "heating the obtained composite billet, and then performing two-stage controlled rolling of rough rolling + finishing rolling" is specifically as follows: The obtained composite blank is heated, the soaking temperature is 1150-1220°C, the total heating time is ≥1.2min / mm×t, t is the thickness of the composite blank, and the soaking section holding time is 30min-50min; A two-stage controlled rolling method of rough rolling + finishing rolling is adopted. In the rough rolling stage, the starting rolling temperature is ≤1050°C, the final rolling temperature is ≥980°C, the rolling is first performed transversely and then longitudinally, at least one pass of longitudinal rolling has a reduction of ≥35mm, the total reduction of rough rolling is 40-60%, and the rough rolling stage is ended when the thickness of the intermediate billet is 2.5-3.5 times the target thickness of the composite plate. After that, the intermediate billet is cooled by water during the temperature-keeping period. When the surface temperature of the intermediate billet drops below 860°C, the finishing rolling stage is started. The final rolling temperature of the finishing rolling stage is ≥780°C, the total reduction of finishing rolling is 55-75%, and the composite plate is obtained.

4. The method for preparing a stainless steel composite plate according to claim 1, characterized in that: The step of "heating the obtained composite billet, and then performing two-stage controlled rolling of rough rolling + finishing rolling" is specifically as follows: The obtained composite blank is heated in five stages, including preheating, first heating, second heating, third heating and soaking, wherein the preheating temperature is ≤850°C, the residence time is (0.45-0.55) min / mm×t, the first heating temperature is 1030-1090°C, the residence time is (0.35-0.45) min / mm×t, the second heating temperature is 1100-1160°C, the residence time is (0.25-0.35) min / mm×t, the third heating temperature is 1140-1180°C, the residence time is (0.15-0.25) min / mm×t, the soaking temperature is 1170-1210°C, the residence time is (0.10-0.20) min / mm×t, and t is the thickness of the composite blank; A two-stage controlled rolling method of rough rolling + finishing rolling is adopted, wherein the first pass adopts longitudinal rolling with a rolling reduction of ≥46mm; transverse rolling is adopted from the second pass until the composite billet is rolled to the target width of the final composite plate in the nth pass, and the rolling reduction in the second pass is ≥25mm; longitudinal rolling is adopted from the n+1th pass, and the rolling reduction in the n+1th pass is ≥30mm; during the entire rough rolling stage, the rolling temperature of the first pass is ≥1060℃, the start rolling temperature of the remaining passes is ≤1050℃, and the final rolling temperature is ≥1000℃; when the intermediate billet thickness is rolled to 2.5 to 3.5 times the target thickness of the composite plate After the rough rolling stage, the steel is kept warm and cooled by water. When the surface temperature of the intermediate billet drops below 840°C, the finishing rolling stage begins. The starting rolling temperature of the finishing rolling stage is 810°C to 840°C, and the final rolling temperature is 780°C to 810°C.

5. The method for preparing a stainless steel composite plate according to claim 1, characterized in that: The step of "heating the obtained composite billet, and then performing two-stage controlled rolling of rough rolling + finishing rolling" is specifically as follows: The obtained composite blank is heated by a four-stage method of preheating, first heating, second heating and soaking, the preheating temperature is 950-1000°C, the residence time is 0.3min / mm×t, the first heating temperature is 1050-1100°C, the second heating temperature is 1120-1180°C, the soaking temperature is 1150-1200°C, and the total residence time of the first heating, second heating and soaking is 1.5min / mm×t+20-40min, t is the thickness of the composite blank; After the composite billet leaves the heating furnace, it is first descaled with high-pressure water and then rolled; during rolling, transverse rolling is adopted from the first pass until the composite billet is rolled to a width of Wt+0~40mm in the nth pass, where Wt is the target width of the composite plate, and the total reduction rate up to this point is ≥30%; longitudinal rolling is adopted from the n+1th pass, and the rolling reduction rate of the n+1th pass is ≥20%; when the thickness of the intermediate billet is 2.5~3.5 times the target thickness of the composite plate, the temperature is waited, and when the surface temperature of the intermediate billet drops below 880℃, the rolling is resumed until the rolling is completed, and the final rolling temperature is T r ±20℃, the total reduction rate of the whole rolling process is ≥75%; The element symbols in this formula represent 100 times the mass percentage of each element in the base material.

6. The method for preparing a stainless steel composite plate according to claim 1, characterized in that: In the intermittent cooling: When the thickness of the composite plate is below 54 mm, the roller speed of the ultra-fast cooling system is 0.4-0.8 m / s, the 1st to 4th groups of cooling manifolds are opened, the 5th to 6th groups of cooling manifolds are not opened, the 7th to 8th groups of cooling manifolds are opened, the 9th to 10th groups of cooling manifolds are not opened, the 11th to 12th groups of cooling manifolds are opened, the 13th to 14th groups of cooling manifolds are not opened, the 15th to 16th groups of cooling manifolds are opened, the 17th to 18th groups of cooling manifolds are not opened, the 19th to 20th groups of cooling manifolds are opened, the 21st to 22nd groups of cooling manifolds are not opened, and the 23rd to 24th groups of cooling manifolds are opened; the composite plate passes through the ultra-fast cooling system once, and intermittent cooling is completed; When the thickness of the large composite plate is greater than 54 mm, the roller speed of the ultra-fast cooling system is greater than 0.2 m / s and less than 0.6 m / s, the 1st to 4th groups of cooling manifolds are opened, the 5th to 8th groups of cooling manifolds are not opened, the 9th to 12th groups of cooling manifolds are opened, the 13th to 16th groups of cooling manifolds are not opened, the 17th to 20th groups of cooling manifolds are opened, the 21st to 22nd groups of cooling manifolds are not opened, and the 23rd to 24th groups of cooling manifolds are opened; the large composite plate passes through the ultra-fast cooling system once, and intermittent cooling is completed.

7. The method for preparing a stainless steel composite plate according to claim 1, characterized in that: In the intermittent cooling: When the thickness of the large composite plate is ≥70mm, the roller speed of the ultra-fast cooling system is 0.4-0.9m / s. The large composite plate first enters the ultra-fast cooling system in the forward direction. When its head reaches the 24th group of cooling manifolds, the roller reverses, and the large composite plate passes through the ultra-fast cooling system in the reverse direction and leaves the ultra-fast cooling system inlet to complete intermittent cooling.

8. The method for preparing a stainless steel composite plate according to claim 1, characterized in that: Step 1: Place the straightened composite board at a temperature of T f -150℃~T f In the process of "stack cooling between two steel plates at +150℃", the length and width of the steel plate used are greater than the length and width of the large composite plate, and the thickness of the steel plate used is twice the thickness of the large composite plate.

9. The method for preparing a stainless steel composite plate according to claim 1, characterized in that: In the step of "coating a release agent on one surface of a composite material", the release agent used is a coating liquid containing silicon oxide and magnesium oxide, wherein the mass ratio of silicon oxide to magnesium oxide is 3:1; The amount of the release agent applied is 20 μg / m 2 , y is the thickness ratio of the composite blank to the composite plate; Before the step of "assembling the blanks in the stacking order of substrate, composite material, composite material, and substrate", the composite material coated with the release agent is placed in a trolley furnace for heating and drying, the drying temperature is 340-360°C, and the drying time is 35-45 minutes.

10. The method for preparing a stainless steel composite plate according to claim 1, characterized in that: In the step of "applying a release agent on one surface of a composite material", the components of the release agent used are as follows: 25-35% silicon nitride, 5-10% thermosetting amino resin, and 55-70% water in a mass ratio; The thickness of the release agent is 0.2-0.5mm; Before the step of "assembling the blanks in the stacking order of substrate, composite material, composite material, and substrate", the composite material coated with the release agent is heated and dried at a temperature of 100 to 250°C for 20 to 40 minutes.

11. The method for preparing a stainless steel composite plate according to claim 1, characterized in that: The step of "substituting surface treatment on at least one surface of each of the two substrates and the two composites" comprises: In a relative shape complementary manner, one surface of the two substrates is milled and ground, and the surface is processed into an irregular concave-convex surface including X planes connected in sequence in the transverse direction, and the substrate is a non-uniform thickness blank with non-monotonic thickness change in the transverse direction, and the length L12 of the irregular concave-convex surface is L1=L1 and the total width W12>W1; or, the surface is processed into an irregular concave-convex surface including X planes connected in sequence in the longitudinal direction, and the substrate is a non-uniform thickness blank with non-monotonic thickness change in the longitudinal direction, and the total length L12 of the irregular concave-convex surface is L1>L1 and the width W12=W1; X≥2; One surface of each composite material is ground and polished to remove the surface oxide scale; and then each composite material is bent to match the corresponding irregular concave and convex surface.

12. The method for preparing a stainless steel composite plate according to claim 1, characterized in that: The step of "substituting surface treatment on at least one surface of each of the two substrates and the two composites" comprises: Grinding and polishing one surface of each composite material to remove surface oxide scale; and, In a relative shape-complementary manner, one surface of the two substrates is milled and ground to form a transversely inclined surface with a length L11=L1 and a width W11>W1, and the substrate is a non-uniform thickness blank with a thickness gradient in the transverse direction; or the surface is milled and ground to form a longitudinally inclined surface with a length L11>L1 and a width W11=W1, and the substrate is a non-uniform thickness blank with a thickness gradient in the longitudinal direction.

13. The method for preparing a stainless steel composite plate according to claim 1, characterized in that: The step of "substituting surface treatment on at least one surface of each of the two substrates and the two composites" comprises: One surface of each substrate and each composite material is ground and polished to remove the surface oxide scale. After grinding and polishing, the substrate and the composite material are both blanks of equal thickness.

14. The method for preparing a stainless steel composite plate according to claim 1, characterized in that: In the aforementioned “the composite material is placed centrally relative to the substrate”, the distance from the side edge of the composite material in the transverse direction to the corresponding side edge of the substrate is half of the width difference between the contact surface of the composite material and the substrate, and the distance from the side edge of the composite material in the longitudinal direction to the corresponding side edge of the substrate is half of the length difference between the contact surface of the composite material and the substrate.

15. A stainless steel composite plate, characterized in that: The unevenness of the composite plate is ≤3 mm / m, the composite interface bonding rate is 100%, and the shear strength is ≥300 MPa.

16. The stainless steel composite plate according to claim 15, characterized in that: The unevenness of the composite plate is ≤2 mm / m, and the shear strength is ≥360 MPa.

17. The stainless steel composite plate according to claim 15, characterized in that: Impact energy at 0℃ ≥240J, impact energy at -20℃ ≥200J, impact energy at -40℃ ≥150J.

18. The stainless steel composite plate according to claim 15, characterized in that: The Vickers hardness difference of the base layer of the composite board in the thickness direction is ≤10, the strength difference of the head, the middle and the tail is ≤40MPa, and the strength difference of the whole board is ≤40MPa.

19. The stainless steel composite plate according to claim 15, characterized in that: The composite board is a plate of equal thickness with a total thickness of 5 to 55 mm, comprising a base layer with a thickness of 4 to 45 mm and a composite layer with a thickness of 1 to 10 mm.

20. The stainless steel composite plate according to claim 15, characterized in that: The composite board comprises a composite layer of equal thickness and a base layer of unequal thickness, wherein the thickness of the composite layer is 1 to 10 mm; The thickness of the base layer in the transverse or longitudinal direction varies non-monotonically, and its composite surface includes irregular concave-convex surfaces of X planes connected sequentially in the transverse direction; or, the thickness of the base layer in the transverse or longitudinal direction varies monotonically, and its composite surface is an inclined surface.

Citation Information

Patent Citations

  • Explosive welding manufacturing method for TMCP type bridge steel stainless steel composite sheet

    CN110064835A

  • Manufacture method of metal composite board

    CN101992568A

  • Meshing type composite plate vacuum rolling preparation method

    CN103272842A

  • Stainless steel and carbon steel composite plate and production method thereof

    CN104441822A

  • Preparation method for asymmetrical wide hot-rolled metal composite plates

    CN105458005A

Cited By

  • Production method for improving yield of nickel steel composite plate

    CN119747389A

  • Production method of hot-rolled copper-steel bimetal composite plate

    CN120696217A

  • Rolling method, device, medium and equipment for optimizing plane shape of steel plate

    CN122007159A