Catalyst for preparing higher aliphatic alcohol from synthesis gas, and preparation method therefor and use thereof
By using small-sized, multi-scale porous molybdenum sulfide materials and alkali metal modification technology, the problems of low active site concentration and slow reactant diffusion of MoS2-based catalysts are solved, and high-activity and high-selectivity catalytic effects for high-carbon alcohols are achieved. Syngas production of higher carbon alcohols provides a more promising catalyst solution.
Patent Information
- Application Number
- PCT/CN2023/112561
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2023-08-11
- Publication Date
- 2024-10-17
AI Technical Summary
Existing MoS2-based synthesis gas catalysts for high-carbon alcohol production have low catalytic activity and selectivity due to the large size of nanosheets, low concentration of edge sulfur vacancy active sites, and lack of multi-scale pore structure, and the diffusion of reactants and product molecules is difficult. , limiting its application prospects.
Small-sized, multi-scale porous molybdenum sulfide materials are used, grown through a template method and modified with alkali metals for synthesis gas to produce higher carbon alcohols, forming rich edge sulfur vacancies and multi-scale pore structures to promote the diffusion of reactants and product molecules. Contact with the active site to avoid secondary side reactions.
The activity of the catalyst and the selectivity of high-carbon alcohols are significantly improved, and the catalytic effect of high carbon monoxide conversion rate and good stability is achieved, which has good industrial application prospects and commercial value.
Smart Images

Figure CN2023112561_17102024_PF_FP_ABST
Abstract
Description
A catalyst for preparing higher alcohols from synthesis gas, and its preparation method and application Technical Field
[0001] The present invention relates to a catalyst for preparing higher alcohols from synthesis gas, a preparation method and an application thereof, and belongs to the field of chemistry and chemical engineering. Background Art
[0002] Higher carbon alcohols are generally C 2+ Alcohols can be used as solvents, chemical raw materials, alternative fuels, and fuel additives. The increasing scarcity of petroleum resources has necessitated the development of novel routes for converting non-oil-based carbon resources into carbon-containing chemicals or fuels. Among these, converting non-oil-based carbon resources such as coal, natural gas, biomass, and even CO2 into higher-carbon alcohols via syngas (primarily a mixture of CO and H2, with a small amount of CO2) is a particularly attractive approach.
[0003] At present, for the reaction of synthesizing high-carbon alcohols from synthesis gas, researchers have developed several catalyst systems including modified Rh-based catalysts, Mo-based catalysts, modified methanol synthesis catalysts and modified Fischer-Tropsch synthesis catalysts. Among them, molybdenum sulfide (MoS2)-based catalysts have attracted widespread attention due to their relatively low price and unique sulfur resistance. After a lot of optimization, the overall selectivity of molybdenum sulfide-based catalysts in catalyzing the conversion of synthesis gas to alcohols has been able to reach a high level, but methanol is still usually the main alcohol product, and its selectivity often accounts for more than 50% of the total alcohols, which greatly limits the application prospects of molybdenum sulfide-based catalysts. People usually improve the activity and C of molybdenum sulfide-based catalysts by adding a second transition metal (such as Fe, Co, Ni, Rh, etc.). 2+ Although the reaction is selective for alcohol, the formation of large amounts of hydrocarbon by-products is often difficult to avoid, and the reaction process often faces the loss of the second transition metal component caused by the formation of carbonyl compounds or the deactivation caused by the sintering of the second transition metal.
[0004] The production of higher alcohols from syngas involves the cleavage of CO bonds and the coupling of C—C bonds. The edge sulfur vacancy active sites of MoS2-based catalysts are crucial for these two key steps, directly affecting the activity and selectivity of the reaction. However, most of the currently reported MoS2-based catalysts for the production of higher alcohols from syngas use H2S as the sulfur source. Simply loading MoS2 on carbon or oxide supports results in large MoS2 nanosheets with a low concentration of edge sulfur vacancy active sites. Furthermore, the lack of a multiscale pore structure hinders the diffusion of reactant and product molecules, resulting in low activity and selectivity. Designing novel molybdenum sulfide-based catalysts to increase the concentration of edge sulfur vacancy active sites and the diffusion rate of molecules within the pores, thereby achieving high activity and selectivity for higher alcohols, is of great significance for the industrial application of syngas to higher alcohols.
[0005] Summary of the Invention
[0006] The purpose of the present invention is to provide a catalyst for preparing higher carbon alcohols from synthesis gas, and its preparation method and application. The present invention is the first to use small-sized, multi-scale porous molybdenum sulfide materials for preparing higher carbon alcohols from synthesis gas, significantly reducing the size of molybdenum sulfide nanosheets, increasing the concentration of active sites of edge sulfur vacancies, and realizing the controllable construction of multi-scale porous structures of molybdenum sulfide materials, promoting the diffusion of molecules in the pores, thereby breaking through key technical bottlenecks such as low active site concentration and slow diffusion of reactant and product molecules in the molybdenum sulfide catalyst system. In addition, the small-sized, multi-scale porous molybdenum sulfide catalyst disclosed in the present invention has a self-supporting effect and does not require any carrier assistance. The catalyst exhibits the characteristics of high carbon monoxide conversion rate, high selectivity for higher carbon alcohols, good stability, etc., and has good industrial application prospects and commercial value.
[0007] The present invention discloses a method for preparing a catalyst for producing higher carbon alcohols from synthesis gas, in which a small-sized, multi-scale porous molybdenum sulfide material is grown on a suitable template, and after modification with an alkali metal, it is used to produce higher carbon alcohols from synthesis gas. The molybdenum sulfide synthesized by this method is arranged in an array and exhibits a small lateral size, so it has abundant edge sulfur vacancies, making it highly active. In addition, the method disclosed by the present invention can enable the synthesized molybdenum sulfide material to completely replicate the template structure, and by adjusting the properties of the template itself and its interaction with the precursor, the pore structure of the synthesized molybdenum sulfide material can be regulated. Through the catalyst preparation method disclosed by the present invention, the controllable construction of multi-scale porous molybdenum sulfide materials with one-dimensional linear pores, two-dimensional linear cross pores or three-dimensional spherical pores and their composite pore structures can be achieved. The synthesized molybdenum sulfide catalyst has a multi-scale pore structure, which promotes the diffusion of reactant and product molecules, enables the reactant molecules to fully contact the active sites; and enables the product molecules to quickly detach from the catalyst bed, inhibits the occurrence of secondary side reactions, and significantly improves the catalytic activity and selectivity.
[0008] Summary of the invention is as follows:
[0009] The present invention provides a catalyst for producing higher alcohols from synthesis gas. The catalyst is a small-sized, multi-scale porous molybdenum sulfide material with abundant sulfur vacancies at the edges of the molybdenum sulfide. The porous pore framework of the molybdenum sulfide material is formed by stacking molybdenum sulfide nanosheets. The size of the molybdenum sulfide nanosheets is 0.5-15 nm. The multi-scale porous structure of the molybdenum sulfide material is composed of at least one of mesopores or macropores formed by stacking molybdenum sulfide nanosheets, and micropores formed by stacking molybdenum sulfide nanosheets. The inner diameter of the micropores is 0.2-2 nm, and the average inner diameter of the mesopores or macropores is 2-1000 nm, preferably 6-400 nm. Further preferably, the average inner diameter of the mesopores is 6-50 nm, and the average inner diameter of the macropores is 50-400 nm. The mesopores or macropores are at least one of one-dimensional linear pores, two-dimensional linear intersecting pores, and three-dimensional spherical pores.
[0010] The present invention further provides a catalyst for producing higher alcohols from syngas. The catalyst is an alkali metal-modified, small-sized, multi-scale porous molybdenum sulfide material with abundant sulfur vacancies at the edges of the molybdenum sulfide. The porous pore framework of the porous molybdenum sulfide material is formed by the molybdenum sulfide itself, without a carrier or template.
[0011] The molybdenum sulfide in the above material has a nanosheet structure, and the size of the nanosheet is 0.5 to 15 nm, which is a small-sized molybdenum sulfide.
[0012] The multi-scale porous structure is composed of micropores (inner diameter 0.2 to 2 nm) between molybdenum sulfide nanosheets and mesopores or macropores formed by the skeleton support of molybdenum sulfide nanosheets, or both. The average inner diameter of the mesopores or macropores is 2 to 1000 nm; the mesopores or macropores are at least one of one-dimensional linear pores, two-dimensional linear cross pores and three-dimensional spherical pores; the preferred average inner diameter of the mesopores or macropores is 6 to 400 nm.
[0013] The present invention also provides a method for preparing a catalyst for synthesizing higher alcohols from syngas. The method comprises selecting a suitable template A, uniformly dispersing a molybdenum source B on the template A or a surface-treated template A*, then introducing a sulfur source C, and reacting the molybdenum source B and the sulfur source C at high temperature in situ to obtain a reaction product D in a one-step process. The reaction product D is then transferred to a post-treatment liquid E for treatment to remove the template, followed by filtration and washing to obtain a small-sized, multi-scale porous molybdenum sulfide material F. The molybdenum sulfide material F is then uniformly mixed with an alkali metal additive G to obtain a catalyst H for synthesizing higher alcohols from syngas.
[0014] The template A is at least one of silica spheres, silica nanowires, SBA-15, KIT-6, alumina nanowires, titanium oxide nanowires, titanium oxide nanospheres, and titanium oxide nanotubes, and the diameters of the above-mentioned oxide spheres, oxide nanowires, and oxide nanotubes are 2 to 400 nm; the molybdenum source B is at least one of ammonium molybdate, sodium molybdate, potassium molybdate, phosphomolybdic acid, sodium phosphomolybdate, potassium phosphomolybdate, molybdenum chloride, and molybdenum acetylacetonate; the sulfur source C is thiourea, sulfur, sodium sulfide, potassium sulfide, hydrogen sulfide, ammonium tetrathiomolybdate, carbon disulfide, dimethyl sulfoxide, At least one of thioacetamide, cysteine, methionine, and thiol; the molar ratio of molybdenum atoms to sulfur atoms in the feeding amount of the molybdenum source B and the sulfur source C is 1:1 to 1:500; the post-treatment liquid E is at least one of hydrofluoric acid solution, sulfuric acid solution, hydrochloric acid solution, nitric acid solution, sodium hydroxide solution, potassium hydroxide solution, and ammonia solution; the alkali metal additive G is at least one of the hydroxide or metal salt compound of lithium, sodium, potassium, and cesium, preferably potassium carbonate or potassium hydroxide; the molar ratio of the alkali metal additive G to the alkali metal atoms to the molybdenum atoms in molybdenum sulfide is 0.02 to 5.
[0015] The surface treatment method for obtaining the template A* is at least one of hydroxylation, amination, carboxylation, and alkylation.
[0016] The method for uniformly dispersing the molybdenum source B on the template A or the surface-treated template A* is at least one of ultrasonic dispersion, mixed grinding, and ball milling, and the steps are as follows:
[0017] (a) The specific steps of the ultrasonic dispersion method are as follows: (1) first adding the template A or A* to a dispersant and ultrasonically dispersing for 0.5 to 6 hours. The dispersant is water, methanol, ethanol, propanol, acetone, or a mixed solution thereof; the concentration of the template and the dispersant in the dispersion is 1 g / L to 1000 g / L; (2) adding the molybdenum source B to the above dispersion and ultrasonically dispersing for 0.5 to 6 hours.
[0018] The ultrasonic frequency of the ultrasonic dispersion method is 10 to 300 kHz.
[0019] (b) The specific steps of the mixing and grinding method are as follows: the template A or A* and the molybdenum source B are mixed and placed in a mortar, and the mixed grinding is performed for 0.5 to 6 hours.
[0020] (c) The ball milling method comprises the following steps: mixing the template A or A* with the molybdenum source B in a ball milling jar, and milling the jar in a ball mill for 2 to 50 hours. The ball milling jar is made of at least one of polytetrafluoroethylene, zirconium oxide, stainless steel, agate, and cemented carbide; the ball milling balls are at least one of zirconium oxide balls, stainless steel balls, agate balls, and cemented carbide balls; the ball-to-material ratio is 200:1 to 10:1 (mass ratio); and the ball milling speed is 200 to 1500 rpm.
[0021] The molybdenum sulfide material F and the alkali metal additive G are mixed by at least one of a liquid phase dispersion stirring method, a mixed grinding method, and a ball milling method, and the steps are as follows:
[0022] (d) The specific steps of the liquid phase dispersion and stirring method are: (1) dissolving the alkali metal additive G in a solvent to form a solution, wherein the solvent is at least one of water, methanol, ethanol, acetone, and N,N-dimethylformamide (DMF); (2) adding the molybdenum sulfide material F to the above solution and ultrasonically dispersing it for 0.5 to 6 hours to form a dispersion liquid; (3) placing the above dispersion liquid at 25 to 150° C. and stirring it until dry, thereby achieving uniform mixing of the molybdenum sulfide material F and the alkali metal additive G.
[0023] The ultrasonic frequency of the liquid phase dispersion stirring method is 10 to 300 kHz.
[0024] (e) The specific steps of the mixed grinding method are as follows: the molybdenum sulfide material F and the alkali metal additive G are mixed and placed in a mortar, and the mixed grinding is performed for 0.5 to 6 hours.
[0025] (f) The ball milling method comprises the following steps: mixing the molybdenum sulfide material F and the alkali metal additive G in a ball milling jar, and milling the jar in a ball mill for 2 to 50 hours. The ball milling jar is made of at least one of polytetrafluoroethylene, zirconium oxide, stainless steel, agate, and cemented carbide; the ball milling balls are at least one of zirconium oxide balls, stainless steel balls, agate balls, or cemented carbide balls; the ball-to-material ratio is 200:1 to 10:1 (mass ratio); and the ball milling speed is 200 to 1500 rpm.
[0026] The catalyst for preparing higher alcohols from synthesis gas provided by the present invention is suitable for one or more of a fixed bed reactor, a fluidized bed reactor, a moving bed reactor, a slurry bed reactor, and a tank reactor.
[0027] Before being used in the synthesis gas to produce higher alcohols reaction, the catalyst is pretreated in an inert atmosphere, a reducing atmosphere, or a mixture of the two at 180-600°C for 0.5-50 hours. This not only increases the concentration of sulfur vacancy active sites, but also allows the alkali metal promoter to diffuse rapidly on the catalyst surface, interacting more evenly with the sulfur vacancy active sites. The inert atmosphere is at least one of nitrogen, argon, helium, and neon; the reducing atmosphere is at least one of hydrogen, carbon monoxide, and hydrogen sulfide; the synthesis gas is at least one of CO / H2 and CO / CO2 / H2; and the higher alcohol is at least one of an alcohol containing two or more carbon atoms.
[0028] Compared with the prior art, the beneficial effects of the synthesis gas to higher alcohols catalyst provided by the present invention and its preparation method and application are mainly reflected in the following aspects:
[0029] (1) Conventional MoS2-based catalysts for synthesizing higher alcohols from syngas have large nanosheets and a low concentration of edge sulfur vacancy active sites. The present invention utilizes the strong interaction between the template and the precursor to arrange the synthesized molybdenum sulfide in an array, completely replicating the template structure and exhibiting a smaller lateral size, resulting in a catalyst with abundant edge sulfur vacancy active sites.
[0030] (2) Traditional MoS2-based catalysts for producing high-carbon alcohols from synthesis gas lack a multi-scale pore structure, making it difficult for reactants and product molecules to diffuse. The present invention regulates the pore structure of the synthesized molybdenum sulfide material by adjusting the properties of the template itself and its interaction with the precursor, thereby achieving the controllable construction of multi-scale porous molybdenum sulfide materials with one-dimensional linear pores, two-dimensional linear cross pores or three-dimensional spherical pores and their composite pore structures. The constructed multi-scale pore structure can promote the diffusion of reactant and product molecules, allowing the reactant molecules to fully contact the active sites; and enable the product molecules to quickly detach from the catalyst bed, thereby suppressing the occurrence of secondary side reactions and significantly improving the catalytic activity and selectivity.
[0031] (3) This invention is the first to utilize small-sized, multi-scale porous molybdenum sulfide materials for the production of higher alcohols from syngas, overcoming key technical bottlenecks such as low active site concentration and slow diffusion of reactant and product molecules in molybdenum sulfide catalyst systems. The catalyst provided by this invention exhibits high carbon monoxide conversion, high selectivity for higher alcohols, and good stability, possessing promising industrial application prospects and commercial value. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] FIG1 is a TEM image of catalysts MoS2-1 to 11 in Examples and Comparative Examples;
[0033] According to the size statistics of molybdenum sulfide nanosheets, the sizes of MoS2-1-4 and MoS2-8-10 are all less than 10nm; while the sizes of MoS2-5-7 and MoS2-11 are all greater than 20nm, and even greater than 200nm. TEM images, XRD patterns, and corresponding catalytic properties have been analyzed in detail in the Examples and Comparative Examples.
[0034] FIG2 is an XRD spectrum of catalysts MoS2-1 to 11 in the examples and comparative examples;
[0035] Figure 3 is an O2 adsorption infrared spectrum of the catalysts MoS2-2 and MoS2-7 in the examples and comparative examples, where 900-980 cm -1 The peak is the characteristic peak of O2 adsorption by sulfur vacancies at the edge of MoS2, 800 cm -1 The wide packet nearby is the characteristic peak of O2 adsorption by in-plane sulfur vacancies. The results show that MoS2-2 has abundant edge sulfur vacancies. DETAILED DESCRIPTION
[0036] The following examples illustrate the catalyst for preparing higher alcohols from synthesis gas provided by the present invention, its preparation method, and its application, but the present invention is not limited thereto.
[0037] Regarding the mixing method of the template and the precursor, such as non-specific template, ultrasonic dispersion, mixed grinding and ball milling achieve similar results, so the following examples and comparative examples all take ultrasonic dispersion as an example.
[0038] Example 1
[0039] 1200 mg of ammonium molybdate and 5333 mg of a silica sphere dispersion (30 wt.% silica in ethylene glycol, with a silica sphere diameter of approximately 100-200 nm) were uniformly dispersed in 100 mL of deionized water and ultrasonically dispersed for 6 hours at a frequency of 120 kHz. The sample was then stirred to dryness at room temperature and then dried in a vacuum oven at 120°C. The dried sample was then sealed with 20 mL of carbon disulfide in a 100 mL stainless steel autoclave under argon and reacted at 450°C for 6 hours. The resulting product was treated in a potassium hydroxide solution at 80°C for 24 hours to remove the silica template. The product was then washed with anhydrous ethanol and deionized water until neutral and then dried in an oven at 80°C to obtain the catalyst, designated MoS2-1.
[0040] According to XRD characterization, MoS2-1 is a typical 2H-MoS2 structure, and there is no XRD signal of silica, indicating that the template has been completely removed and the MoS2-1 catalyst does not contain a carrier or a template. According to TEM characterization, MoS2-1 completely replicates the silica sphere template, and the MoS2 nanosheets are stacked to form a three-dimensional macroporous skeleton with an inner diameter of about 150nm; in addition, the MoS2 nanosheets form micropores (stacked pores) through stacking. This multi-scale pore structure is conducive to the mass transfer of reactants, products and intermediate molecules. The statistical results based on TEM characterization show that the average size of MoS2 nanosheets is about 6.2nm. The small size of MoS2 nanosheets gives it abundant edge sulfur vacancies, thus exhibiting high activity and high selectivity.
[0041] Example 2
[0042] 1600 mg of ammonium molybdate tetrahydrate and 2500 mg of SBA-15 (pore inner diameter approximately 6-13 nm) were uniformly dispersed in 100 mL of deionized water and ultrasonically dispersed for 12 hours at 120 kHz. The sample was then stirred to dryness at room temperature and then dried in an 80°C oven overnight. The dried sample was then sealed with 40 mL of carbon disulfide in a 100 mL stainless steel autoclave under argon and reacted at 500°C for 12 hours. The resulting product was treated in hydrofluoric acid solution at room temperature for 8 hours to remove the SBA-15 template. The product was then washed with anhydrous ethanol and deionized water until neutral and then dried in an 80°C oven to obtain the catalyst, designated MoS2-2.
[0043] According to XRD characterization, MoS2-2 has a typical 2H-MoS2 structure and no XRD signal of silica, indicating that the template has been completely removed and the MoS2-2 catalyst does not contain a carrier or template. According to TEM characterization, MoS2-2 completely replicates the SBA-15 template. The MoS2 nanosheets are arranged in an orderly manner along the original spatial structure of SBA-15 to form a one-dimensional linear structure, forming a mesoporous skeleton with an inner diameter of about 10nm. In addition, the MoS2 nanosheets form micropores (stacked pores) through stacking. This multi-scale pore structure is conducive to the mass transfer of reactants, products and intermediate molecules. The statistical results based on TEM characterization show that the average size of MoS2 nanosheets is about 3.6nm. The small size of MoS2 nanosheets gives it abundant edge sulfur vacancies, thus exhibiting high activity and high selectivity.
[0044] Example 3
[0045] 1200 mg of ammonium molybdate tetrahydrate and 2500 mg of SiO2 microspheres (approximately 400 nm in diameter) were uniformly dispersed in 100 mL of deionized water and ultrasonically dispersed for 6 hours at a frequency of 120 kHz. The sample was then stirred to dryness at room temperature and then dried in a 120°C oven overnight. The dried sample was then sealed with 20 mL of carbon disulfide in a 100 mL stainless steel autoclave under argon and reacted at 450°C for 6 hours. The resulting product was treated in potassium hydroxide solution at 80°C for 24 hours to remove the SiO2 template. The product was then washed with anhydrous ethanol and deionized water until neutral and then dried in an 80°C oven to obtain the catalyst, designated MoS2-3.
[0046] According to XRD characterization, MoS2-3 has a typical 2H-MoS2 structure and no XRD signal of silica, indicating that the template has been completely removed and the MoS2-3 catalyst does not contain a carrier or a template. According to TEM characterization, MoS2-3 completely replicates the silica microsphere template, and the MoS2 nanosheets are stacked to form a three-dimensional macroporous skeleton with an inner diameter of about 400nm; in addition, the MoS2 nanosheets form micropores (stacked pores) through stacking. This multi-scale pore structure is conducive to the mass transfer of reactants, products and intermediate molecules. The statistical results based on TEM characterization show that the average size of MoS2 nanosheets is about 5.5nm. The small size of MoS2 nanosheets gives it abundant edge sulfur vacancies, thus exhibiting high activity and high selectivity.
[0047] Example 4
[0048] 1200mg of ammonium molybdate tetrahydrate and 2500mg of amination-treated SiO2 microspheres (diameter approximately 400nm) were uniformly dispersed in 100mL of deionized water and ultrasonically dispersed for 6 hours at an ultrasonic frequency of 120kHz. The mixture was then stirred to dryness at room temperature and then dried in a 120°C oven overnight. The dried sample was then packaged with 20mL of carbon disulfide in a 100mL stainless steel autoclave under argon protection and reacted at 450°C for 6 hours. The resulting product was treated in a hydrofluoric acid solution and potassium hydroxide solution at 80°C for 24 hours to remove the SiO2 template. The product was then washed with anhydrous ethanol and deionized water until neutral, and then dried in an 80°C oven to obtain the catalyst, which was designated as MoS2-4.
[0049] According to XRD characterization, MoS2-4 is a typical 2H-MoS2 structure, and there is no XRD signal of silica, indicating that the template has been completely removed and the MoS2-4 catalyst does not contain a carrier or template. According to TEM characterization, MoS2-4 completely replicates the silica microsphere template, and the MoS2 nanosheets are stacked to form a three-dimensional macroporous skeleton with an inner diameter of approximately 400nm; in addition, the MoS2 nanosheets form micropores (stacked pores) through stacking. This multi-scale pore structure is conducive to the mass transfer of reactants, products and intermediate molecules. Due to the amino treatment, the interaction between the molybdenum precursor and the surface of the silica sphere template is enhanced, avoiding polymerization during the high-temperature synthesis process, thereby further reducing the size of the synthesized MoS2 nanosheets. Statistical results based on TEM characterization show that the average size of the MoS2 nanosheets is about 3.8nm. The small size of the MoS2 nanosheets gives it abundant edge sulfur vacancies, thus exhibiting high activity and high selectivity.
[0050] Comparative Example 1
[0051] 1235.9 mg of ammonium molybdate tetrahydrate and 2283.6 mg of thiourea were dissolved and dispersed in 35 mL of deionized water to form a uniform solution. The solution was then sealed in a 100 mL reactor and reacted at 400 ° C for 4 hours. The product was -1 The product was stirred in a potassium hydroxide solution at 60°C for 3 hours, washed with anhydrous ethanol and deionized water until neutral, and then dried in an oven at 80°C to obtain a catalyst, which was recorded as MoS2-5.
[0052] XRD characterization revealed that MoS2-5 exhibits a typical 2H-MoS2 structure, with no support or template present in the catalyst. TEM characterization revealed that MoS2-5 exhibits a flower-like structure, with MoS2 nanosheets exhibiting large horizontal dimensions. TEM-based statistical results indicate that the average size of the MoS2 nanosheets is >100 nm. These large MoS2 nanosheets lack edge sulfur vacancies, resulting in relatively low selectivity for higher alcohols.
[0053] Comparative Example 2
[0054] 900 mg of ammonium molybdate tetrahydrate and 10 mL of carbon disulfide were placed in a 40 mL stainless steel autoclave under argon protection and reacted at 400 °C for 4 hours. -1 The product was stirred in a potassium hydroxide solution at 60°C for 3 hours, washed with anhydrous ethanol and deionized water until neutral, and then dried in an oven at 80°C to obtain a catalyst, which was recorded as MoS2-6.
[0055] According to XRD characterization, MoS2-6 has a typical 2H-MoS2 structure, and the catalyst does not contain a carrier or template. Since no carrier and no solvent were introduced, ammonium molybdate could not be effectively dispersed during the high-temperature synthesis process. According to TEM characterization, MoS2-6 is aggregated as a whole, and its MoS2 nanosheets have large horizontal dimensions. The statistical results based on TEM characterization show that the average size of MoS2 nanosheets is >30nm. The large size of MoS2 nanosheets makes them lack edge sulfur vacancies, thus showing relatively low selectivity for higher carbon alcohols.
[0056] Comparative Example 3
[0057] 900 mg of ammonium molybdate tetrahydrate was dissolved in 20 mL of deionized water to form a uniform solution. The above solution and 10 mL of carbon disulfide were then sealed in a 40 mL stainless steel autoclave under argon protection and reacted at 400 ° C for 4 hours. The product was 6 mol L -1 The product was stirred in a potassium hydroxide solution at 60°C for 3 hours, washed with anhydrous ethanol and deionized water until neutral, and then dried in an oven at 80°C to obtain a catalyst, which was recorded as MoS2-7.
[0058] XRD characterization revealed that MoS2-7 exhibits a typical 2H-MoS2 structure, with no support or template present in the catalyst. TEM characterization revealed that MoS2-7 exhibits a flower-like structure, with MoS2 nanosheets exhibiting large horizontal dimensions. TEM-based statistical results indicate that the average size of the MoS2 nanosheets is >20 nm. These large MoS2 nanosheets lack edge sulfur vacancies, resulting in relatively low selectivity for higher alcohols.
[0059] Comparative Example 4
[0060] 1600 mg of ammonium molybdate tetrahydrate and 2500 mg of SBA-15 (pore inner diameter approximately 6-13 nm) were dispersed in 100 mL of deionized water, stirred to dryness at room temperature, and then dried in an 80°C oven overnight. The dried sample was then sealed with 40 mL of carbon disulfide in a 100 mL stainless steel autoclave under argon and reacted at 500°C for 12 hours. The resulting product was treated in hydrofluoric acid solution at room temperature for 8 hours to remove the SBA-15 template. The product was then washed with anhydrous ethanol and deionized water until neutral, and then dried in an 80°C oven to obtain the catalyst, designated MoS2-8.
[0061] According to XRD characterization, MoS2-8 has a typical 2H-MoS2 structure and no XRD signal of silica, indicating that the template has been completely removed and the MoS2-8 catalyst does not contain a carrier or template. According to TEM characterization, although MoS2-8 can replicate part of the SBA-15 template, most of the MoS2 nanosheets are still separated from the original SBA-15 structure and appear aggregated, causing the original pores to be blocked. The statistical results based on TEM characterization show that the average size of the MoS2 nanosheets is about 4nm. Although the size of the nanosheets in MoS2-8 is close to that of MoS2-2, it does not have a complete one-dimensional ordered linear structure and most of the pores are blocked, resulting in restricted diffusion of reactants, products and intermediate molecules in the pores. Therefore, the activity and selectivity of higher carbon alcohols are much lower than those of MoS2-2.
[0062] Comparative Example 5
[0063] 1600 mg of ammonium molybdate tetrahydrate was physically mixed with 2500 mg of SBA-15 (pore inner diameter approximately 6-13 nm). The resulting mixture was then sealed in a 100-mL stainless steel autoclave with 40 mL of carbon disulfide under argon and reacted at 500°C for 12 hours. The resulting product was treated in hydrofluoric acid solution at room temperature for 8 hours to remove the SBA-15 template. The product was then washed with anhydrous ethanol and deionized water until neutral and then dried in an oven at 80°C to obtain the catalyst, designated MoS2-9.
[0064] According to XRD characterization, MoS2-9 has a typical 2H-MoS2 structure and no XRD signal of silica, indicating that the template has been completely removed and the MoS2-9 catalyst does not contain a carrier or template. According to TEM characterization, MoS2-9 hardly replicates the pore structure of the SBA-15 template, and the MoS2 nanosheets are aggregated. The statistical results based on TEM characterization show that the average size of the MoS2 nanosheets is about 4nm. Although the size of the nanosheets in MoS2-9 is close to that of MoS2-2, because the MoS2 nanosheets are aggregated and do not have a complete one-dimensional ordered linear structure, the diffusion of reactants, products and intermediate molecules is restricted, so the activity and selectivity of higher carbon alcohols are much lower than those of MoS2-2.
[0065] Comparative Example 6
[0066] 1200 mg of ammonium molybdate was physically mixed with 5333 mg of a dispersion of silica spheres (30 wt% silica in ethylene glycol, with silica spheres approximately 100-200 nm in diameter). The resulting mixture was then sealed with 20 mL of carbon disulfide in a 100 mL stainless steel autoclave under argon and reacted at 450°C for 6 hours. The resulting product was treated in potassium hydroxide solution at 80°C for 24 hours to remove the silica template. The product was then washed with anhydrous ethanol and deionized water until neutral, and then dried in an oven at 80°C to obtain the catalyst, designated MoS2-10.
[0067] According to XRD characterization, MoS2-10 has a typical 2H-MoS2 structure and no XRD signal of silica, indicating that the template has been completely removed and the MoS2-10 catalyst does not contain a carrier or a template. According to TEM characterization, MoS2-10 hardly replicates the pore structure of the silica template, and the MoS2 nanosheets are aggregated. The statistical results based on TEM characterization show that the average size of the MoS2 nanosheets is about 6.5nm. Although the size of the nanosheets in MoS2-10 is close to that of MoS2-1, because the MoS2 nanosheets are aggregated and do not have a complete three-dimensional macroporous structure, the diffusion of reactants, products and intermediate molecules is restricted, so the activity and selectivity of higher carbon alcohols are much lower than those of MoS2-1.
[0068] Comparative Example 7
[0069] Commercial molybdenum disulfide (CAS No.: 1317-33-5) was used as a comparative sample and recorded as MoS2-11.
[0070] According to XRD characterization, MoS2-11 has a typical 2H-MoS2 structure with high crystallinity and does not contain a carrier or template. According to TEM characterization, MoS2-11 presents a large lamellar structure. The statistical results based on TEM characterization show that the average size of MoS2 nanosheets is >200nm. The large size of MoS2 nanosheets makes them lack edge sulfur vacancies, thus showing relatively low selectivity for higher carbon alcohols.
[0071] Comparison
[0072] The MoS2-based catalyst used in the present invention completely replicates the pores of SBA-15 and SiO2 spheres, forming a multi-scale pore structure. Comparisons of MoS2-2 with MoS2-8 and MoS2-9, as well as MoS2-1 with MoS2-10, clearly demonstrate the important role of the multi-scale pore structure formed after the complete replication of the template in improving catalyst activity and selectivity for higher alcohols. Furthermore, a performance comparison of a series of MoS2-based catalysts modified with different alkali metals revealed that K-modified MoS2-based catalysts prepared with potassium carbonate or potassium hydroxide as additives exhibited superior performance, with the K / Mo molar ratio of 0.2 exhibiting the best performance.
[0073] The method of adding alkali metal is:
[0074] The above MoS2-1 to 11 were ultrasonically dispersed in 50 mL of deionized water for 3 hours, followed by the addition of an appropriate amount of alkali metal salt or hydroxide solution and continued ultrasonic dispersion for 3 hours. The samples were then stirred to dryness at room temperature and dried at 80°C to obtain alkali metal-modified MoS2 samples, which were designated as Cat-XYZ, where X corresponds to MoS2-1 to 11, Y is the alkali metal salt or hydroxide used, and Z is the molar ratio of the alkali metal to Mo.
[0075] The alkali metal-modified catalysts in Table 1 all used potassium carbonate as a promoter, and the K / Mo molar ratio was 0.2, so they were abbreviated as Cat-1 to Cat-11.
[0076] MoS2-2 was ultrasonically dispersed in 50 mL of deionized water for 3 hours. An appropriate amount of the alkali metal salt or hydroxide solution shown in Table 2 was then added and ultrasonic dispersion continued for another 3 hours. The mixture was then stirred to dryness at room temperature and dried at 80°C to obtain the alkali metal-modified MoS2-2 sample.
[0077] MoS2-2 was ultrasonically dispersed in 50 mL of deionized water for 3 hours. Subsequently, different amounts of potassium carbonate solutions listed in Table 3 were added and ultrasonic dispersion was continued for another 3 hours. The mixture was then stirred to dryness at room temperature and dried at 80°C to obtain alkali metal-modified MoS2-2 samples.
[0078] The application of alkali metal modified catalysts takes a fixed bed reactor as an example, and the specific steps are as follows:
[0079] Before filling the catalyst, the catalyst was formed into particles of 250-600 μm. Then 200 mg of catalyst was loaded into the reaction tube and a pressure of 1 bar and 30 mL min was introduced. -1 H2 was pretreated at 300℃ for 1 hour. When the temperature dropped to the reaction temperature (240℃ for example), the reaction gas was switched to a CO / H2 ratio of 1 / 2 (containing 4% Ar as an internal standard substance to calculate the CO conversion rate) and pressurized to 50 bar. The reaction gas space velocity was 3000 mL g cat. -1 h -1 For example, the reaction products were analyzed online using a gas chromatograph, with TCD and FID detectors used for qualitative and quantitative analysis, respectively. The specific reaction performance is listed in Table 1.
[0080] Table 1 Catalyst performance evaluation results
[0081] Table 2 Properties of MoS2-2 samples modified with different alkali metals Note: The molar ratio of alkali metal to Mo is 0.2
[0082] Table 3 Properties of MoS2-2 samples modified with different potassium carbonate contents
Claims
1. A catalyst for preparing higher alcohols from synthesis gas, It is characterized in that The catalyst is a small-sized, multi-scale porous molybdenum sulfide material with abundant sulfur vacancies at the edge of molybdenum sulfide. The pore framework of the porous molybdenum sulfide material is formed by the accumulation of molybdenum sulfide nanosheets, and the size of the molybdenum sulfide nanosheets is 0.5-15nm. The multi-scale porous structure of the porous molybdenum sulfide material is composed of at least one of mesopores and macropores formed by the accumulation of molybdenum sulfide nanosheets and micropores formed by the accumulation of molybdenum sulfide nanosheets, the inner diameter of the micropores is 0.2-2nm, the average inner diameter of the mesopores and macropores is 2-1000nm, and the mesopores or macropores are at least one of one-dimensional linear pores, two-dimensional linear cross pores and three-dimensional spherical pores.
2. A catalyst for preparing higher alcohols from synthesis gas, It is characterized in that The catalyst is a small-sized, multi-scale porous molybdenum sulfide material modified by an alkali metal, which has abundant sulfur vacancies at the edge of molybdenum sulfide; the porous channel skeleton of the porous molybdenum sulfide material is formed by molybdenum sulfide itself; the size of the nanosheet of the molybdenum sulfide material is 0.5 to 15 nm; The multi-scale porous structure is composed of micropores with an inner diameter of 0.2 to 2 nm between molybdenum sulfide nanosheets and mesopores or macropores formed by the support of the molybdenum sulfide nanosheet skeleton, or both. The average inner diameter of the mesopores and macropores is 2 to 1000 nm; the mesopores or macropores are at least one of one-dimensional linear pores, two-dimensional linear cross pores and three-dimensional spherical pores.
3. A catalyst for preparing higher alcohols from synthesis gas according to claim 2, It is characterized in that The average inner diameter of the mesopores and macropores is 6-400nm.
4. A method for preparing the catalyst according to claim 2 or 3, It is characterized in that By selecting a suitable template A, the molybdenum source B is uniformly dispersed on the template A or the template A* after surface treatment, and then the sulfur source C is introduced, and the molybdenum source B and the sulfur source C are reacted in situ at high temperature to obtain a reaction product D in one step, and then the reaction product D is transferred to a post-treatment liquid E for treatment to wash away the template, and the small-sized, multi-scale porous molybdenum sulfide material F is obtained by suction filtration and washing, and the molybdenum sulfide material F is uniformly mixed with an alkali metal additive G to obtain a synthesis gas to high carbon alcohol catalyst H; The method of uniformly dispersing the molybdenum source B on the template A or the surface-treated template A* is at least one of an ultrasonic dispersion method, a mixed grinding method, and a ball milling method; The alkali metal auxiliary agent G is at least one of potassium hydroxide or metal salt compounds.
5. The method for preparing the catalyst according to claim 4, Features The template A is at least one of silica spheres, silica nanowires, SBA-15, KIT-6, alumina nanowires, titanium oxide nanowires, titanium oxide nanospheres, and titanium oxide nanotubes, and the diameters of the above-mentioned oxide spheres, oxide nanowires, and oxide nanotubes are 2 to 400 nm; the molybdenum source B is at least one of ammonium molybdate, sodium molybdate, potassium molybdate, phosphomolybdic acid, sodium phosphomolybdate, potassium phosphomolybdate, molybdenum chloride, and molybdenum acetylacetonate; the sulfur source C is thiourea, sulfur, sodium sulfide, potassium sulfide, hydrogen sulfide, ammonium tetrathiomolybdate, carbon disulfide, dimethyl sulfoxide, thioacetamide, cysteine, At least one of methionine and thiol; the molar ratio of molybdenum atoms to sulfur atoms in the molybdenum source B and the sulfur source C is 1:1 to 1:500; the catalyst synthesis temperature is 180 to 600°C, and the synthesis time is 0.5 to 48 hours; the post-treatment liquid E is at least one of hydrofluoric acid solution, sulfuric acid solution, hydrochloric acid solution, nitric acid solution, sodium hydroxide solution, potassium hydroxide solution, and ammonia solution; the post-treatment time is 0.5 to 48 hours; the alkali metal additive G is potassium carbonate or potassium hydroxide; the molar ratio of the alkali metal additive G to the alkali metal atoms in molybdenum sulfide to the molybdenum atoms is 0.02 to 5.
6. The method for preparing the catalyst according to claim 4, Features The method for obtaining the template A* through surface treatment is at least one of hydroxylation, amination, carboxylation and alkylation.
7. The method for preparing the catalyst according to claim 4, Features The method of uniformly dispersing the molybdenum source B on the template A or the surface-treated template A* is at least one of an ultrasonic dispersion method, a mixed grinding method, and a ball milling method; The specific steps of the ultrasonic dispersion method are: (1) first adding the template A or A* into a dispersant, and ultrasonically dispersing for 0.5 to 6 hours, wherein the dispersant is water, methanol, ethanol, propanol, acetone, or a mixed solution thereof, and the concentration of the dispersion formed by the template and the dispersant is 1 g / L to 1000 g / L; (2) adding the molybdenum source B into the above dispersion, and ultrasonically dispersing for 0.5 to 6 hours; The ultrasonic frequency of the ultrasonic dispersion method is 10 to 300 kHz; The specific steps of the mixed grinding method are: mixing the template A or A* and the molybdenum source B in a mortar, and mixing and grinding for 0.5 to 6 hours; The specific steps of the ball milling method are: mixing the template A or A* and the molybdenum source B and placing them in a ball milling jar, placing the ball milling jar on a ball mill and ball milling for 2 to 50 hours, the material of the ball milling jar is at least one of polytetrafluoroethylene, zirconium oxide, stainless steel, agate, and cemented carbide, the ball milling balls are at least one of zirconium oxide balls, stainless steel balls, agate balls, or cemented carbide balls, the ball-to-material ratio of the ball milling balls to the sum of the template and the molybdenum source is 200:1 to 10:1 (mass ratio); the ball milling speed is 200 to 1500 rpm.
8. The method for preparing the catalyst according to claim 4, Features The molybdenum sulfide material F and the alkali metal additive G are mixed by at least one of a liquid phase dispersion stirring method, a mixed grinding method, and a ball milling method; The specific steps of the liquid phase dispersion and stirring method are as follows: (1) dissolving the alkali metal additive G in a solvent to form a solution, wherein the solvent is at least one of water, methanol, ethanol, acetone, and N,N-dimethylformamide (DMF); (2) adding the molybdenum sulfide material F to the above solution, and ultrasonically dispersing for 0.5 to 6 hours to form a dispersion; (3) placing the above dispersion at 25 to 150° C. and stirring until dry, thereby achieving uniform mixing of the molybdenum sulfide material F and the alkali metal additive G; The ultrasonic frequency of the liquid phase dispersion stirring method is 10 to 300 kHz; The specific steps of the mixed grinding method are: mixing the molybdenum sulfide material F and the alkali metal additive G in a mortar, and mixing and grinding for 0.5 to 6 hours; The specific steps of the ball milling method are: mixing the molybdenum sulfide material F and the alkali metal additive G in a ball milling jar, The material of the ball mill is at least one of polytetrafluoroethylene, zirconium oxide, stainless steel, agate and cemented carbide. The ball milling balls are at least one of zirconium oxide balls, stainless steel balls, agate balls and cemented carbide balls. The ball-to-material ratio of the ball milling balls to the sum of the molybdenum sulfide material F and the alkali metal additive G is 200:1-10:1 (mass ratio). The ball milling speed is 200-1500 rpm.
9. Use of the catalyst according to claims 1 to 3 in the reaction of synthesizing higher alcohols from synthesis gas, Features: The catalyst is used for preparing high-carbon alcohols from synthesis gas and is suitable for one or more of a fixed bed reactor, a fluidized bed reactor, a moving bed reactor, a slurry bed reactor and a kettle reactor.
10. Use of the catalyst according to claim 9 in the reaction of synthesizing higher alcohols from synthesis gas, Features: The catalyst is pretreated at 180-600°C for 0.5-50 hours in an inert atmosphere, a reducing atmosphere or a mixed atmosphere of the two before being used in the synthesis gas to produce higher alcohols reaction; the inert atmosphere is at least one of nitrogen, argon, helium and neon; the reducing atmosphere is at least one of hydrogen, carbon monoxide and hydrogen sulfide; the synthesis gas is CO / H 2 and CO / CO 2 / H 2 At least one of the following: high carbon alcohols are at least one of the alcohols containing more than 2 carbon atoms.
Citation Information
Patent Citations
Preparation method and application of molybdenum sulfide catalyst using SBA-15 as carrier for producing low-carbon alcohols from synthetic gas
CN102351641A
Carbon-supported catalysts for production of higher alcohols from syngas
CN103313785A
Preparation method of heteroatom doped porous molybdenum disulfide coated graphene
CN110479311A
Molybdenum disulfide with three-dimensional hierarchical pore structure and preparation method and application thereof
CN111841579A
Catalyst composition formulated for synthesis of alcohols and method of preparing the same
US8815963B1
Cited By
KOH-loaded molybdenum disulfide photo-thermal catalyst as well as preparation method and application thereof
CN120605741A