Preparation of near-infrared luminescent nd and yb synchronously and highly-doped core-shell structure nanocrystal and use thereof in immunochromatographic test
Patent Information
- Application Number
- PCT/CN2023/141917
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2023-12-26
- Publication Date
- 2024-10-17
AI Technical Summary
Existing immunochromatography test strips have low sensitivity and low signal-to-noise ratio, mainly due to light absorption and autofluorescence interference, making it difficult to achieve highly sensitive and accurate biomarker detection in complex biological samples.
By preparing β-phase NaNdF4:Yb@NaLuF4 core-shell structure nanocrystals, the absorption capacity of the nanocrystals for 808nm light and the utilization rate of excitation energy are improved, efficient near-infrared emission is achieved, and background interference is reduced. High-brightness near-infrared luminescent Nd3+ and Yb3+ co-doped core-shell structure nanocrystals are used as fluorescent probes to construct an immunochromatographic detection method with no background interference and high sensitivity.
It significantly increases the quantum yield of nanocrystals to 35.5%, achieves background-free and highly sensitive detection, enhances the ability to detect disease indicators in complex samples, and improves the accuracy and reliability of detection results.
Smart Images

Figure CN2023141917_17102024_PF_FP_ABST
Abstract
Description
Preparation of near-infrared luminescent Nd and Yb simultaneously highly doped core-shell nanocrystals and their application in immunochromatographic detection Technical Field
[0001] The present invention belongs to the technical field of immunological detection, and specifically relates to the preparation of near-infrared luminescent Nd and Yb synchronously highly doped core-shell structure nanocrystals and their application in immunochromatographic detection. Background Art
[0002] As the most common point-of-care testing method in the world, lateral flow analysis (LFA) has attracted great attention in academic research and industrial manufacturing due to its advantages such as rapid reading, low cost and ease of use. Among them, the most common LFA is the immunochromatographic test strip. However, immunochromatographic test strips based on gold nanoparticles, latex beads and europium fluorescent microspheres still have problems with low sensitivity and low signal-to-noise ratio. This is because the nitrocellulose membrane (NM) of the test strip and the blood and plasma sample matrices have high light absorption and autofluorescence interference. Therefore, the development of an immunochromatographic test strip that can eliminate light absorption and autofluorescence interference is necessary to achieve sensitive and accurate quantitative detection of biomarkers in complex biological matrices (such as plasma, whole blood, urine and fecal samples).
[0003] As a new generation of luminescent materials, rare earth down-conversion nanocrystals have the following advantages: (1) large Stokes shift and narrow emission spectrum half-peak width, which can realize multi-index and multi-detection; (2) high fluorescence quantum yield, no photobleaching, good photostability, and can be repeatedly detected; (3) the excitation light and emission light are mostly in the near-infrared region, with strong light penetration ability and no background interference, which can realize no background interference and high signal-to-noise ratio detection. 3+ and Yb 3+ The excitation light and emission light of the co-doped nanocrystals are near-infrared light 800nm excitation and near-infrared light 980nm excitation, respectively. It is a potential fluorescent material for detecting disease indicators in complex samples without background interference.
[0004] Studies have shown that rare earth ions Nd 3+ and Yb 3+ There is a strong energy transfer efficiency between Nd 3+ and Yb 3+ The mass production rate of co-doped nanocrystals has reached 20.7%. 3+ and Yb 3+The near-infrared emission brightness of co-doped nanocrystals to meet the needs of high-sensitivity detection is still a direction worth exploring. A large number of studies have shown that the luminescence efficiency of rare earth nanocrystals is affected by surface defects of the nanocrystals and the doping concentration of rare earth ions. Therefore, constructing an inert shell and optimizing the doping concentration of rare earth ions are effective methods to improve the luminescence efficiency of rare earth nanocrystals. For example, Chinese invention patents CN111044493A and CN110514825A provide a core-shell structure α-phase NaLnF4:Nd,Yb@CaF2 / NaLnF4 and α-phase NaYF4:Yb,Nd@NaYF4 nanocrystal probes, respectively. However, the maximum mass yield of the near-infrared luminescence of the above-mentioned nanocrystal probes is only 20.7%. At the same time, the luminescence efficiency of the α-phase used is significantly lower than that of the β-phase because the arrangement of the doped rare earth ions in the α-phase and β-phase is significantly different. In addition, the main matrix components used in these methods contain other Ln elements, including Y, Gd, or Lu. The doping of these elements will affect the content, arrangement, and inter-ion distance of the Nd and Yb elements in the nanocrystals, thereby hindering the efficient absorption and utilization of the excitation energy of the nanocrystals, and ultimately resulting in the inability to further increase the luminescence intensity of the nanocrystals. Therefore, it is necessary to improve the nanocrystals to further enhance their absorption capacity for 808nm light and the utilization rate of the excitation energy, so as to achieve highly sensitive detection with zero background signal interference in the immunochromatographic detection method.
[0005] Summary of the Invention
[0006] In order to overcome the above-mentioned shortcomings of the prior art, the present invention is to 3+ and Yb 3+ The preparation method of co-doped core-shell structure nanocrystals was improved by synthesizing β-phase NaNdF4:Yb@NaLnF4 core-shell structure nanocrystals, thereby greatly improving its absorption capacity of 808nm excitation light and increasing the sensitizing ion Nd in the nanocrystals. 3+ The utilization rate of excitation energy is improved, thus achieving efficient emission of nanocrystals at 980nm (mass production rate is as high as 35.5%), and overcoming the existing Nd 3+ and Yb 3+ The co-doped core-shell structure nanocrystals have insufficient near-infrared light emission intensity. 3+ and Yb 3+ Co-doped core-shell structured nanocrystals NaNdF4:Yb@NaLuF4 are used as fluorescent recognition probes to establish an immunochromatographic detection method. Compared with the existing near-infrared immunochromatographic method, its fluorescent marker has comparable stability, stronger fluorescence emission, and better sensitivity in the detection results, thus enabling background-free, highly sensitive immunochromatographic detection of various indicators in the fields of medicine, agriculture, and food safety.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] The first aspect of the present invention provides a high-brightness near-infrared luminescent β-phase Nd 3+ and Yb 3+ The method for preparing co-doped core-shell structure nanocrystals comprises the following steps:
[0009] S1. Preparation of core NaNdF4:Yb:
[0010] S11. Weigh rare earth acetate Ln(CH3COO)3, wherein neodymium acetate Nd(CH3COO)3 accounts for 40% and ytterbium acetate Yb(CH3COO)3 accounts for 60%, add oleic acid and 1-octadecene, and heat to 150-180°C under an inert gas atmosphere until all the solids are dissolved, thereby obtaining a rare earth precursor solution;
[0011] S12, adding a methanol solution containing sodium hydroxide and a methanol solution containing ammonium fluoride to the rare earth precursor solution, stirring and mixing under an inert gas atmosphere, heating the solution to 120° C. to remove methanol in the solution; finally, heating the solution to 290-310° C. and maintaining the reaction for 50-70 minutes;
[0012] S13. After the reaction is completed, the solution is cooled to room temperature, and then the precipitate is collected by centrifugation to obtain the core NaNdF4:Yb60%; finally, the NaNdF4:Yb60% nanocrystals are dispersed in cyclohexane for later use;
[0013] S2. Preparation of NaNdF4:Yb60%@NaLuF4 core-shell structure:
[0014] S21, adding lutetium oxide Lu2O3 to an aqueous solution containing trifluoroacetic acid; heating to 90-110°C until the solid is completely dissolved, and then continuing to heat until the solution is completely evaporated to dryness, thereby obtaining a solid powder of lutetium trifluoroacetate;
[0015] S22, adding sodium trifluoroacetate Na(CF3COO)3, oleic acid, 1-octadecene, and the NaNdF4:Yb60% cyclohexane solution prepared in step S13 to the lutetium trifluoroacetate solid powder; heating to 110-130°C under an inert gas atmosphere and holding for 20-40 minutes to remove cyclohexane and water in the system; then heating to 290-310°C and reacting for 50-70 minutes to epitaxially grow a NaLuF4 shell layer;
[0016] S23, after the solution is cooled to room temperature, the precipitate is collected by centrifugation to obtain the high-brightness near-infrared luminescent β-phase Nd 3+ and Yb 3+Co-doped core-shell structured nanocrystals, namely NaNdF4:Yb60%@NaLuF4 core-shell structured nanocrystals, referred to as β-NaNdF4:Yb@NaLnF4.
[0017] Near-infrared luminescent β-phase Nd prepared by the method of the present invention 3+ and Yb 3+ The co-doped nanomaterial includes a core, and the core is an inorganic matrix doping ion; the inorganic matrix core is NaLnF4, Ln=Yb 3+ and Nd 3+ Co-doping ions; the inorganic matrix core cannot contain other Ln elements (Ln=Y 3+ 、Gd 3+ 、Er 3+ 、Ho 3+ or Ce 3+ Any one or more of); The near-infrared luminescent rare earth nanomaterial further comprises a shell layer, which is one or more layers, coated outside the core; The matrix of the shell layer comprises NaLnF4, wherein Ln=Yb 3+ .
[0018] The present invention adopts the method of accelerating phase transformation to realize the sensitization of Nd 3+ and luminescent ion Yb 3+ At the same time, high concentration doping, in which the sensitizing ion Nd 3+ and luminescent ion Yb 3+ The doping ratios of Yb and dapoxies are 40% and 60% respectively. This doping ratio not only ensures the high absorption capacity of nanocrystals for 808nm, but also increases the absorption capacity of the luminescent center Yb 3+ The quantum yield of the resulting nanocrystals, which fully utilize the excitation energy, reached 35.5%, significantly higher than the previously reported highest yield of 20.7%. Furthermore, using these highly luminescent near-infrared nanocrystals as immunofluorescent probes to prepare immunochromatographic test strips, they established an immunochromatographic method for detecting disease markers in complex samples such as feces, blood, and urine with high sensitivity and without background interference.
[0019] Preferably, in step S11, the ratio of the rare earth acetate to oleic acid and 1-octadecene is 1-3 mmol:7.5 mL:15 mL.
[0020] Preferably, in step S12, the molar concentration of the methanol solution containing sodium hydroxide is 0.2-0.5 mmol / mL, and the molar concentration of the methanol solution containing ammonium fluoride is 0.3-0.5 mmol / mL.
[0021] Preferably, in step S12, the volume ratio of the methanol solution containing sodium hydroxide to the methanol solution containing ammonium fluoride is 1:1.
[0022] Preferably, in step S21, the usage ratio of lutetium oxide to trifluoroacetic acid aqueous solution is 0.5-2 mmol / 10-20 mL, and the volume fraction of trifluoroacetic acid aqueous solution is 50%.
[0023] Preferably, in step S22, the usage ratio of the sodium trifluoroacetate, oleic acid, 1-octadecene and NaNdF4:Yb60% cyclohexane solution is 1-3 mmol:10 mL:10 mL:10-20 mL, and the molar concentration of the NaNdF4:Yb60% cyclohexane solution is 0.1-0.2 mmol / mL.
[0024] The second aspect of the present invention provides a high-brightness near-infrared luminescent β-phase Nd prepared by the preparation method described in the first aspect. 3+ and Yb 3+ Co-doped core-shell nanocrystals.
[0025] The third aspect of the present invention provides the high-brightness near-infrared luminescent β-phase Nd 3+ and Yb 3+ Application of co-doped core-shell nanocrystals in immunochromatographic detection.
[0026] The fourth aspect of the present invention provides a high brightness near infrared light emitting β-phase Nd 3+ and Yb 3+ A luminescent lateral flow test strip for serum markers co-doped with core-shell structured nanocrystals, characterized in that the lateral flow test strip is a high-brightness near-infrared luminescent β-phase Nd 3+ and Yb 3+ Co-doped core-shell structure nanocrystals are used as immune markers, and the lateral flow test strip is composed of high-brightness near-infrared luminescent β-phase Nd 3+ and Yb 3+ The co-doped core-shell structure nanocrystals, a polyvinyl chloride support backing, a detection pad, a conjugation pad, a sample pad, and a water-absorbing pad are composed of a conjugation pad loaded with a high-brightness near-infrared luminescent β-phase Nd modified with a binding antibody or a target protein. 3+ and Yb 3+ Highly bright near-infrared luminescent β-phase Nd co-doped core-shell nanocrystal probe and anti-quality control antibody modified 3+ and Yb 3+ Co-doped core-shell structured nanocrystal probes.
[0027] Preferably, the anti-quality control antibody comprises a goat anti-chicken IgY antibody.
[0028] The fifth aspect of the present invention provides the high-brightness near-infrared light emitting β-phase Nd 3+ and Yb 3+ A method for preparing a lateral flow test strip for luminescent detection of serum markers co-doped with core-shell structured nanocrystals comprises the following steps:
[0029] (1) β-NaNdF4:Yb@NaLnF4 probe surface modification recognition marker
[0030] The functional modification in S1 and β-NaNdF4:Yb@NaLnF4 is carboxyl modification, and the method used is ligand exchange method:
[0031] S11, the cyclohexane solution of β-NaNdF4:Yb@NaLnF4 core-shell structure nanocrystals was thoroughly mixed with ethanol and a 0.1 M hydrochloric acid aqueous solution, and ultrasonicated for 30 min to remove the oleic acid ligands on the surface of the nanocrystals;
[0032] The β-NaNdF4:Yb@NaLnF4 core-shell structured nanocrystal solutions prepared in S12 and S11 were centrifuged (10000 r / min, 30 min) to collect the ligand-free β-NaNdF4:Yb@NaLnF4 core-shell structured nanocrystals and redissolved in 10 mL of deionized water;
[0033] S13, adding the β-NaNdF4:Yb@NaLnF4 core-shell structure nanocrystals resuspension prepared in S12 dropwise to an aqueous solution containing polyacrylic acid, and stirring at room temperature for 60 min to obtain polyacrylic acid-modified β-NaNdF4:Yb@NaLnF4 core-shell structure nanocrystals;
[0034] S14. Collect the polyacrylic acid modified β-NaNdF4:Yb@NaLnF4 core-shell structured nanocrystals prepared in S12 by centrifugation and disperse them in 10-20 mL of deionized water.
[0035] S2. Functionalized binding and recognition of the target binding antibody or target protein in β-NaNdF4:Yb@NaLnF4
[0036] S21. Take the amino- or carboxyl-functionalized near-infrared luminescent β-NaNdF4:Yb@NaLnF4 nanomaterial obtained in step S14, add MES buffer, centrifuge, and discard the supernatant; and redisperse the precipitated β-NaNdF4:Yb@NaLnF4 nanomaterial in MES buffer.
[0037] S22, add EDC / SulFo-NHS to the β-NaNdF4:Yb@NaLnF4 nanomaterial buffer obtained in S21 and activate for 10-60 min. Centrifuge to obtain the precipitate, and then redisperse it in the buffer.
[0038] S23. Add the binding antibody or target protein that recognizes and detects the target to the activated β-NaNdF4:Yb@NaLnF4 nanomaterial buffer obtained in S22, react at room temperature for 1-3 hours, then add a blocking agent for blocking and react for 0.5-2 hours.
[0039] S24, centrifuge the antibody- or target protein-modified β-NaNdF4:Yb@NaLnF4 nanomaterial buffer obtained in S23, take the precipitate (i.e., the β-phase Nd4:Yb@NaLnF4 nanomaterial labeled with the detection target recognition antibody labeled with the near-infrared luminescent rare earth nanomaterial) 3+ and Yb 3+ Co-doped nanomaterials) were dispersed in PBS or other buffer and stored at 4°C.
[0040] At the same time, the same method was used to prepare the quality control antibody modified high-brightness near-infrared luminescent β-phase Nd 3+ and Yb 3+ Co-doped core-shell structured nanocrystal probes.
[0041] (2) Assembly of a near-infrared tomography detection card based on β-NaNdF4:Yb@NaLnF4 nanomaterials
[0042] S11. Preparation of the detection pad: stick the nitrocellulose membrane to the middle of the polyvinyl chloride support floor for later use, then use coating buffer (PB buffer, 10mM, pH=7.4) to dilute the detection target recognition antibody and quality control antibody to 0.5-5mg / mL, and then use a gold spray film scribing instrument to evenly draw the detection target recognition antibody and quality control antibody on the detection line and quality control line of the nitrocellulose membrane of the polyvinyl chloride support bottom plate at a film speed of 10-80mm / s and a film volume of 1μL / cm. The marked polyvinyl chloride support bottom plate is placed in a 37°C blower drying oven for 24 hours and set aside.
[0043] S12. Pretreatment of the conjugate pad: Soak the polyester fiber membrane in PB buffer (10 mM, pH 7.4) containing S9 surfactant, casein, PVP-K30, and Tween-20 for 2-4 h. After drying at 37°C, cut the glass fiber membrane into strips 10 mm wide and 300 mm long using an automatic cutting machine.
[0044] S13. Preparation of conjugate pad: Add 1% (v / v) binding antibody or target protein modified β-NaNdF4:Yb@NaLnF4 nanomaterial dispersion obtained in step (1) and 2% (v / v) quality control antibody modified β-NaNdF4:Yb@NaLnF4 nanomaterial dispersion to the gold spray diluent [containing 10% (w / v) sucrose, 0.3% (w / v) bovine serum albumin (BSA), 0.5% (w / v) polyvinyl pyrrolidone (PVP K-30), 5% (w / v) S9 surfactant, 0.03% (v / v) Proclin-3000); use a gold spray film instrument to evenly spray the conjugate pad pretreated previously at a spray speed of 50 mm / s and a spray volume of 4 uL / cm, and then place the prepared conjugate pad in a 37°C air drying oven to dry for 24 h for use.
[0045] S14. Preparation of sample pad: Soak the glass fiber membrane in PB buffer (10 mM, pH = 7.4) containing S9 surfactant, casein, PVP-K30, and Tween-20 for 2 to 4 hours; cut the glass fiber membrane after drying at 37°C into strips with a width of 21 mm and a length of 300 mm using an automatic cutting instrument; when adding samples, directly add blood, urine, and other samples containing the target to be tested.
[0046] S15. Assembly of the immunochromatographic test strip: Remove the polyvinyl chloride support base of the nitrocellulose membrane with the antibody fixed thereon, attach the prepared S13 conjugate pad to the end near the test line of the nitrocellulose membrane, attach the absorbent pad to the end near the quality control line of the nitrocellulose membrane, and attach the sample pad prepared in S14 to the other end of the prepared conjugate pad. Leave a 2mm overlap between each component to complete the assembly of the test strip.
[0047] S16. Preparation of immunochromatographic test paper card: Use an automatic strip cutter to cut the assembled test paper into 4.00 mm wide test strips, and load the test strips into a plastic card shell; obtain an immunochromatographic test paper card with near-infrared luminescence of β-NaNdF4:Yb@NaLnF4 nanomaterial (based on high-brightness near-infrared light emitting β-phase Nd 3+ and Yb 3+ Co-doped core-shell structured nanocrystals for luminescent detection of serum markers (lateral flow test strips).
[0048] Compared with the prior art, the present invention has the following beneficial effects:
[0049] The present invention discloses a method for preparing near-infrared luminescent Nd and Yb synchronously highly doped core-shell structure nanocrystals, and synthesizes Nd without other Ln elements by utilizing a scheme of accelerating phase transition. 3+ and Yb 3+ At the same time, the highly doped nanocrystals. This solution solves the problem of Nd 3+and Yb 3+ The lattice mismatch problem was solved, and Nd 3+ and Yb 3+ Co-doped nanocrystals, on the other hand, realize Nd 3+ and Yb 3+ At the same time, high concentration doping was determined to be Nd 3+ and Yb 3+ The doping ratios of the nanocrystals were 40% and 60%, respectively. Under these doping ratios, the nanocrystals achieved high absorption of 808 nm and fully utilized the excitation energy of 808 nm, ultimately greatly improving the near-infrared light emission intensity of the core-shell nanocrystals at 980 nm (30 times higher than the core-shell structure α-NaYF4:Nd60%,Yb7%@CaF2 nanocrystals disclosed in Chinese invention patent CN110514825B). The fluorescence quantum yield was as high as 35.5%, significantly higher than that reported in the literature (Cao C, Xue M, Zhu X, Yang P, Feng W, Li F. Energy Transfer Highway in Nd 3+ -Sensitized Nanoparticles for Efficient Near-Infrared Bioimaging. ACS Appl Mater Interfaces. 2017 Jun 7; 9(22): 18540-18548) reported that α-NaLnF4:Nd,Yb@CaF2 / NaLnF4 has a luminescence intensity of 20.7%. Then, this high-brightness near-infrared luminescent nanocrystal is used to construct a fluorescent immunoprobe to construct an immunochromatographic test strip, thereby achieving high-sensitivity detection of disease indicators in complex samples without background interference. Specifically, the present invention has the following advantages:
[0050] (1) The present invention adopts the method of accelerating phase transformation to synthesize β-phase NaNdF4:Yb@NaLuF4 core-shell structure nanocrystals with regular morphology and uniform particle size. 3+ Doping achieves high absorption of 808nm photons. 3+ →Yb 3+ The efficient energy transfer and high concentration of Yb 3+ Doping enables the nanocrystals to fully utilize the absorption of 808nm photons, making them emit 980nm near-infrared light with high brightness. The coating of NaLnF4 inert shell suppresses the high concentration of Yb 3+The surface defect quenching phenomenon caused by doping was finally achieved by preparing NaNdF4:Yb60%@NaLnF4 nanocrystals that emit high-brightness near-infrared light at 980nm. These high-brightness near-infrared-emitting nanocrystals can be used as immunofluorescent markers to facilitate highly sensitive immunochromatographic detection. Compared with existing near-infrared immunochromatographic methods, NaNdF4:Yb60%@NaLnF4 nanocrystals have stronger near-infrared emission and higher sensitivity.
[0051] (2) When the NaNdF4:Yb60%@NaLuF4 nanocrystal immunochromatographic test strip provided by the present invention is used to detect actual body fluid markers, an appropriate amount of body fluid sample is dripped onto the sample pad. After a period of reaction, the luminescence of the test strip is detected using a handheld portable detection instrument (808nm excitation, 980nm emission). Because the excitation and emission spectra of the NaNdF4:Yb60%@NaLuF4 nanocrystal fluorescent probe are both in the near-infrared region, interference with the detected fluorescent signal from various small and large molecules in the cellulose membrane and body fluids is eliminated. This enables the immunochromatographic detection method to achieve highly sensitive real-time detection of various indicators in complex samples such as blood, urine, and feces without background signal interference. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 is the XRD diffraction pattern of core-shell structure NaNdF4:Yb60%@NaLuF4 nanocrystals;
[0053] FIG2 is a transmission electron micrograph of core-shell structured NaNdF4:Yb60%@NaLuF4 nanocrystals (the bar graph represents the size of the core-shell structured nanocrystals);
[0054] Figure 3 is a comparison of the fluorescence spectra of core-shell structured NaNdF4:Yb60%@NaLuF4 nanocrystals and conventional NaYF4:Nd20%,Yb10%@NaYF4 nanocrystals;
[0055] FIG4 is a comparison of the fluorescence spectra of the core-shell structure NaNdF4:Yb60%@NaLuF4 nanocrystals and the core-shell structure NaYF4:Nd60%,Yb7%@NaYF4 disclosed in patent CN110514825B;
[0056] Figure 5 is a schematic diagram of an immunochromatographic test strip using core-shell structured NaNdF4:Yb60%@NaLuF4 nanocrystals as fluorescent immunolabeling [① is the sample pad, ② is the binding pad, ③ is the test line (T line), ④ is the quality control line (C line), and ⑤ is the absorbent pad];
[0057] FIG6 is a physical picture of an immunochromatographic test strip using core-shell structured NaNdF4:Yb60%@NaLuF4 nanocrystals as fluorescent immunolabeling;
[0058] Figure 7 is a curve showing the relationship between the concentration of SARS-CoV-2 neutralizing antibodies detected by an immunochromatographic test strip using core-shell structure NaNdF4:Yb60%@NaLuF4 nanocrystals as fluorescent immunolabeling and the ratio of the fluorescence intensity of the test line (T line) to the quality control line (C line). DETAILED DESCRIPTION
[0059] The following is a further description of specific embodiments of the present invention. It should be noted that the description of these embodiments is intended to facilitate understanding of the present invention and does not constitute a limitation of the present invention. In addition, the technical features involved in the various embodiments of the present invention described below may be combined with each other as long as they do not conflict with each other.
[0060] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.
[0061] Example 1 Preparation and Luminescence Properties of Near-Infrared Luminescent Nd and Yb Synchronously Highly Doped Core-Shell Structure Nanocrystals (NaNdF4:Yb60%@NaLuF4 Core-Shell Structure Nanocrystals)
[0062] 1. Preparation of core NaNdF4:Yb60%:
[0063] 1) Add 0.4 mmol of neodymium acetate (Nd(CH3COO)3) and 0.6 mmol of ytterbium acetate (Yb(CH3COO)3) to a three-necked flask containing 7.5 mL of oleic acid (OA) and 15 mL of 1-octadecene (ODE). Under a nitrogen atmosphere, heat to 100°C for 10 minutes to remove moisture and oxygen. Then heat to 160°C for 60 minutes until all the solids are dissolved. Finally, cool to room temperature to obtain a rare earth precursor solution.
[0064] 2) First, 10 mL of a methanol solution containing 2.5 mmol of sodium hydroxide (NaOH) was slowly added to the rare earth precursor solution in the three-necked flask and vigorously stirred for 20 minutes. Then, 10 mL of a methanol solution containing 4 mmol of ammonium fluoride (NH4F) was slowly added thereto. Under a nitrogen atmosphere, the mixture was vigorously stirred for 60 minutes. The mixture was then heated to 120°C for 30 minutes to remove methanol, oxygen, and moisture from the system. Finally, the temperature was raised to 300°C for 60 minutes.
[0065] 3) After the reaction is complete, allow the solution to cool naturally to room temperature and transfer it to a 50 mL centrifuge tube. Add 5 mL of anhydrous ethanol, shake and mix thoroughly, and centrifuge at 7500 rpm for 5 minutes. Repeat the washing and centrifugation operation with anhydrous ethanol 2-3 times to obtain the precipitate, which is the nuclear NaNdF4:Yb60%;
[0066] The obtained core NaNdF4:Yb60% was redispersed in 10 mL of cyclohexane to obtain a NaNdF4:Yb60% dispersion (molar concentration of 0.1 mmol / mL) for later use.
[0067] 2. Preparation of core-shell NaNdF4:Yb60%@NaLuF4:
[0068] 1) Add 1 mmol of lutetium oxide (Lu2O3) to a three-necked flask containing 5 mL of deionized water (H2O) and 5 mL of trifluoroacetic acid (CF3COOH). Heat to 98°C and allow to react until the solution is completely transparent and the solid is completely dissolved. Then, evaporate to dryness to remove all water to obtain a solid powder of lutetium trifluoroacetate. Cool to room temperature and set aside.
[0069] 2) To the three-necked flask containing the lutetium trifluoroacetate solid powder, 2 mmol of sodium trifluoroacetate (CF3COONa), 15 mL of oleic acid (OA), 15 mL of 1-octadecene (ODE), and 10 mL of the NaNdF4:Yb60% dispersion (0.1 mmol / mL) from step 1 were added. The mixture was heated to 120°C under a nitrogen atmosphere for 30 minutes to remove cyclohexane and water from the system. The mixture was then heated to 300°C for 60 minutes to form an epitaxial NaLuF4 inert shell layer.
[0070] 3) After the solution is cooled to room temperature, 10 mL of anhydrous ethanol is added and washed by shaking. The mixture is then centrifuged at 8000 rpm for 5 min. The washing with anhydrous ethanol and the centrifugation operation are repeated 2-3 times to obtain the core-shell structured NaNdF4:Yb60%@NaLuF4 precipitate.
[0071] The prepared core-shell structured NaNdF4:Yb60%@NaLuF4 nanocrystals were redispersed in 10 mL of cyclohexane to obtain a NaNdF4:Yb60%@NaLuF4 core-shell structured nanocrystal dispersion (0.1 mmol / mL) for later use.
[0072] First, the NaNdF4:Yb60%@NaLuF4 core-shell nanocrystals prepared in this example were subjected to XRD diffraction analysis. As can be seen from the XRD diffraction spectrum in Figure 1, the NaNdF4:Yb60%@NaLuF4 nanocrystals have a hexagonal crystal structure.
[0073] Next, the NaNdF4:Yb60%@NaLuF4 core-shell structured nanocrystals prepared in this example were observed under a transmission electron microscope. As shown in Figure 2, the core-shell structured NaNdF4:Yb60%@NaLuF4 nanocrystals are monodispersed, round particles with regular morphology and uniform particle size, with a diameter of 17 nm.
[0074] In addition, the emission spectra of the NaNdF4:Yb60%@NaLuF4 core-shell structure nanocrystals prepared in this example, the core-shell structure α-NaYF4:Nd60%,Yb7%@CaF2 nanocrystals disclosed in patent CN110514825B, and the core-shell structure β-NaYF4:Nd60%,Yb7%@NaYF4 nanocrystals reported in the literature (Feng Xu, et al. Rare-earth Doped Nanoparticles with Narrow NIR-II Emission for Optical Imaging with Reduced Autofluorescence. Chem. Res. Chinese Universities, 2021, 37(4), 943―950) under 808nm excitation were analyzed. As shown in Figure 3, the near-infrared luminescence of the core-shell structured β-NaYF4:Nd60%,Yb7%@NaYF4 nanocrystals at 980nm is enhanced by 3.0 times compared to the emission spectrum of the core-shell structured β-NaYF4:Nd60%,Yb7%@NaYF4 nanocrystals at 808nm. Figure 4 shows that the near-infrared luminescence of the core-shell structured α-NaYF4:Nd60%,Yb7%@CaF2 nanocrystals at 980nm is enhanced by 30 times compared to the emission spectrum of the core-shell structured α-NaYF4:Nd60%,Yb7%@NaLuF4 nanocrystals at 808nm.
[0075] Finally, the relative fluorescence quantum yield of the NaNdF4:Yb60%@NaLuF4 core-shell structure nanocrystals prepared in this example was calculated. The absorbance of the DMSO solution of NaNdF4:Yb60%@NaLuF4 (0.1 mg / mL, DCNPs solution) and the DMSO solution of ICG (0.1 mg / mL, ICG solution) at 808 nm of the excitation light source was measured using an ultraviolet absorption spectrometer and recorded as A DCNPs and A ICG Afterwards, the emission spectra of NaNdF4:Yb60%@NaLuF4 DMSO solution (0.1 mg / mL) and ICG DMSO solution (0.1 mg / mL) under 808 nm excitation were measured using a near-infrared fluorescence spectrometer, and the emission peak areas of NaNdF4:Yb60%@NaLuF4 core-shell nanocrystals and near-infrared fluorescent dye ICG were calculated and recorded as F DCNPs and F ICG The relative fluorescence quantum yield is calculated by the formula QY DCNPs =35.5%. The calculation formula is as follows:
[0076] and
[0077] Among them, QY ICG represents the fluorescence quantum yield of the organic fluorescent dye ICG in DMSO solution. The value is 13% according to the literature review; n DCNPs and n ICG represent the refractive indices of DCNPs solution and ICG solution, respectively.
[0078] Example 2 Preparation of High Brightness Near-Infrared Luminescent Immunochromatographic Test Strips
[0079] The immunochromatographic test strip of this embodiment is prepared using the NaNdF4:Yb60%@NaLuF4 core-shell structure nanocrystals in Example 1 as an immune marker. The test strip consists of a sample pad, a conjugation pad, a water-absorbing pad, a detection pad, and a polyvinyl chloride support base.
[0080] The test pad is composed of a nitrocellulose membrane containing a test line and a quality control line: the test line is a line drawn in parallel on the nitrocellulose membrane using a certain amount (3.5-4.2L) of serum indicator antibody solution, and the quality control line is a line drawn in parallel on the nitrocellulose membrane using a certain amount (3.5-4.5L) of sheep anti-chicken IgY antibody solution. The line width of the test line and the quality control line are both 1-1.2mm, and the drop volume is 1-1.2mL / cm;
[0081] The conjugate pad is composed of a polyester cellulose membrane loaded with binding antibodies or target protein modified NaNdF4:Yb60%@NaLuF4 core-shell structure nanocrystal probes and chicken IgY antibody modified NaNdF4:Yb60%@NaLuF4 core-shell structure nanocrystal probes.
[0082] The detection pad is pasted on the middle part of the polyvinyl chloride supporting base plate, and the conjugation pad is pasted on the end of the detection pad close to the detection line; the sample pad is pasted on the other end of the conjugation pad; and the absorbent pad is pasted on the end of the quality control line of the detection pad. Its structure is shown in Figures 5 and 6.
[0083] The preparation method of the above-mentioned immunochromatographic test strip comprises the following steps:
[0084] 1. Preparation of NaNdF4:Yb60%@NaLuF4 core-shell structure nanocrystal probes modified with antibodies or target proteins and NaNdF4:Yb60%@NaLuF4 core-shell structure nanocrystal probes modified with chicken IgY antibodies (i.e., preparation of rare earth down-conversion near-infrared second-region luminescence probes)
[0085] 1) To the NaNdF4:Yb60%@NaLuF4 core-shell structure nanocrystal dispersion (10 mL, 0.1 mmol / mL) prepared in Example 1, 10 mL of HCl solution (0.1 M) and 10 mL of anhydrous ethanol were added, and after oscillation and mixing at room temperature, the oleic acid ligand was removed by ultrasonication for 30 min; then, the ligand-free NaNdF4:Yb60%@NaLuF4 nanocrystals were collected by centrifugation (10000 r / min, 30 min); then, the ligand-free NaNdF4:Yb60%@NaLuF4 nanocrystals were washed by centrifugation with deionized water (10000 r / min, 20 min), and the operation was repeated 2 to 3 times; the ligand-free NaNdF4:Yb60%@NaLuF4 nanocrystals were redispersed in 10 mL of deionized water. The mixture was then added dropwise to 10 mL of deionized water containing 50 mg of polyacrylic acid (PAA) and vigorously stirred at room temperature for 60 min. After the reaction was completed, the polyacrylic acid-modified NaNdF4:Yb60%@NaLuF4 nanocrystals (i.e., PAA-NaNdF4:Yb60%@NaLuF4 nanocrystals) were collected by centrifugation (10,000 r / min, 30 min) and washed by centrifugation with deionized water (10,000 r / min, 20 min). The operation was repeated 2 to 3 times and then redispersed in 10 mL of deionized water to obtain a PAA-NaNdF4:Yb60%@NaLuF4 nanocrystal dispersion (0.1 mmol / mL).
[0086] 2) 100 μL of PAA-NaNdF4:Yb60%@NaLuF4 nanocrystal dispersion (0.1 mmol / mL) was added to a 1.5 mL EP tube, and then 1 mL of MES buffer (pH = 6.0) was added for washing. The supernatant was removed by centrifugation (15000 rpm, 15 min), and the PAA-NaNdF4:Yb60%@NaLuF4 nanocrystals were redispersed in 1 mL of MES buffer (pH = 6.0). 400 μL of MES buffer (pH = 6.0) containing 40 μg of EDC and 400 μL of MES buffer (pH = 6.0) containing 70 μg of EDC were added to the above solution. SulFo-NHS was added to MES buffer (pH = 6.0), and then placed on a mixer to react for 30 minutes. After the reaction was completed, the supernatant was removed by centrifugation (15000r / min, 15min), and the PAA-NaNdF4:Yb60%@NaLuF4 nanocrystals activated by SulFo-NHS were resuspended in 1mL MES buffer (pH = 6.0);
[0087] To the resulting nanocrystal suspension, 60 mg of RBD protein (novel coronavirus antigen) or chicken IgY antibody was added and the suspension was allowed to react on a mixer for 90 min. 1 mL of blocking buffer [Tris buffer (pH = 8.0, 10 mM) containing 1% (w / v) bovine serum albumin (BSA)] was then added and the suspension was allowed to react on a mixer for another 60 min to block other unreacted activation sites. The suspension was centrifuged (15,000 rpm, 15 min) and the supernatant was removed to collect the RBD protein or chicken IgY antibody-coupled NaNdF4:Yb60%@NaLuF4 nanocrystals.
[0088] The RBD protein or chicken IgY antibody-coupled NaNdF4:Yb60%@NaLuF4 nanocrystals were washed with final washing buffer [Tris buffer (pH = 8.0, 10 mM) containing 1% (w / v) bovine serum albumin (BSA), 0.1% (v / v) Tween-20, and 0.03% (v / v) Proclin-300], and then redispersed in 100 uL of final washing buffer to obtain a NaNdF4:Yb60%@NaLuF4 nanocrystal dispersion (0.1 mmol / mL) coupled to RBD protein or chicken IgY antibody for later use.
[0089] 2. The steps for assembling the near-infrared two-zone luminescent immunochromatographic test strip are as follows:
[0090] 1) Sample Pad Preparation: Soak the glass fiber membrane in PB buffer (10 mM, pH 7.4) containing 1% (v / v) Tween-20 for 2–4 h. Then, dry the membrane in a 37°C air drying oven for 24 h. Cut the dried glass fiber membrane into strips 21 mm wide and 300 mm long using an automated cutting machine. Place the prepared sample pad in a drying oven until ready for use.
[0091] 2) Pretreatment of the conjugate pad: Soak the polyester fiber membrane in PB buffer (10 mM, pH 7.4) containing 1% (v / v) Tween-20 for 2-4 hours. Then, dry the membrane in a 37°C air drying oven for 24 hours. Cut the dried glass fiber membrane into strips 10 mm wide and 300 mm long using an automatic cutter. Place the pretreated conjugate pad in the drying oven until ready for use.
[0092] 3) Preparation of the test pad: First, a nitrocellulose membrane was attached to the middle of a polyvinyl chloride support base plate and set aside. Angiotensin-converting enzyme 2 (ACE2) and goat anti-chicken IgY antibody were diluted to 1 mg / mL using coating buffer (PB buffer (10 mM, pH = 7.4)). Then, a gold-sprayed streaker was used to evenly streak the 1 mg / mL angiotensin-converting enzyme 2 solution and goat anti-chicken IgY antibody solution onto the test and control lines of the nitrocellulose membrane on the polyvinyl chloride support base plate at a streaking speed of 50 mm / s and a streaking volume of 1 uL / cm. The streaked polyvinyl chloride support base plate was placed in a 37°C air drying oven and dried for 24 h before use.
[0093] 4) Preparation of the conjugate pad: 1% (v / v) RBD protein-conjugated NaNdF4:Yb60%@NaLuF4 nanocrystal dispersion and 2% (v / v) chicken IgY antibody-conjugated NaNdF4:Yb60%@NaLuF4 nanocrystal dispersion were added to a gold spray diluent [Tris buffer (20 mM, pH = 7.4) containing 10% (w / v) sucrose, 0.3% (w / v) bovine serum albumin (BSA), 0.5% (w / v) polyvinylpyrrolidone (PVP K-30), 5% (w / v) S9 surfactant, and 0.03% (v / v) Proclin-3000]. The gold was evenly sprayed onto the pretreated conjugate pad using a gold sprayer at a spray speed of 50 mm / s and a spray volume of 4 uL / cm. The prepared conjugate pad was then dried in a 37°C air drying oven for 24 h before use.
[0094] 5) Assembly of the immunochromatographic test strip: Remove the polyvinyl chloride support base of the nitrocellulose membrane with the antibody fixed thereon, attach the prepared conjugate pad to the end near the test line of the nitrocellulose membrane, attach the absorbent pad to the end near the quality control line of the nitrocellulose membrane, and attach the prepared sample pad to the other end of the prepared conjugate pad; the overlap distance between each component is 2 mm, and the test strip assembly is complete; use an automatic strip cutter to cut the assembled test strip into 4.00 mm wide test strips, load the test strips into a plastic card holder, and obtain a high-brightness near-infrared luminescent immunochromatographic test strip, also known as a high-brightness near-infrared luminescent Nd and Yb co-doped core-shell structure nanocrystal SARS-CoV-2 neutralizing antibody assay test strip.
[0095] 3. The method of using the immunochromatographic test strip prepared in this example with the high-brightness near-infrared second-region luminescent NaNdF4:Yb60%@NaLuF4 core-shell structure nanocrystals as immunofluorescence labeling probes is as follows: 50 μL of blood sample and 80 μL of sample buffer [containing 0.85% (w / v) sodium chloride (NaCl), 0.5% (v / v) Triton 100 (TX-100), 0.1% (v / v) Tween-20 (T-20), 0.1% (w / v) S9 The surfactant Tris buffer (100 mM, pH = 8.0) was shaken and mixed, then added to the sample pad and allowed to stand for chromatography for 15 minutes. The fluorescence signals of the test line and the quality control line in the test strip at 980 nm were then detected using a handheld detection instrument. A standard curve was prepared based on the measured fluorescence intensity and the concentration of SARS-CoV-2 neutralizing antibodies in the standard sample. The fluorescence intensity of the test sample was compared with the standard curve to obtain the concentration of SARS-CoV-2 neutralizing antibodies in the sample.
[0096] Example 3 Detection Limit of High-Brightness Near-Infrared Luminescence Immunochromatographic Test Strip
[0097] The detection limit of the high-brightness near-infrared luminescent immunochromatographic test strip prepared in Example 2 for determining SARS-CoV-2 neutralizing antibodies was investigated. The specific method is as follows:
[0098] 1) The SARS-CoV-2 neutralizing antibody standard was added to the sample buffer [Tris buffer (100 mM, pH = 8.0) containing 0.85% (w / v) sodium chloride (NaCl), 0.5% (v / v) Triton 100 (TX-100), 0.1% (v / v) Tween-20 (T-20), 0.1% (w / v) S9 surfactant] to prepare SARS-CoV-2 neutralizing antibody concentrations of 0 μg / mL, 0.6 μg / mL, 0.13 μg / mL, 0.25 μg / mL, 0.5 μg / mL, 1 μg / mL, 2 μg / mL, 4 μg / mL, 8 μg / mL, and 16 μg / mL, respectively;
[0099] 2) 100 μL of sample solution of each concentration was added to the sample well of the reagent card (immunochromatographic test strip prepared in Example 2). The chromatography reaction was allowed to stand at room temperature for 15 minutes. The 980 nm emission light signal intensity was collected at the test line and quality control line of the near-infrared second zone luminescence immunochromatographic test strip using a handheld detection instrument. The test results of the samples at each SARS-CoV-2 neutralizing antibody concentration and the corresponding standard curve are shown in Figure 7. As can be seen from Figure 7, the detection limit of the immunochromatographic test strip is 0.11 μg / mL, and the repeatability is good.
[0100] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. It is apparent to those skilled in the art that various changes, modifications, substitutions, and variations of these embodiments may be made without departing from the principles and spirit of the present invention, and the changes still fall within the scope of protection of the present invention.
Claims
1. A high-brightness near-infrared luminescent β-phase Nd 3+ and Yb 3+ The method for preparing co-doped core-shell structure nanocrystals is characterized by: The following steps are involved: S1. Preparation of core NaNdF4:Yb: S11, weighing rare earth acetate, wherein neodymium acetate accounts for 40% and ytterbium acetate accounts for 60%, adding oleic acid and 1-octadecene, and heating to 150-180° C. in an inert gas atmosphere until all the solids are dissolved, thereby obtaining a rare earth precursor solution; S12, adding a methanol solution containing sodium hydroxide and a methanol solution containing ammonium fluoride to the rare earth precursor solution, stirring and mixing under an inert gas atmosphere, heating the solution to 120° C. to remove methanol in the solution; finally, heating the solution to 290-310° C. and maintaining the reaction for 50-70 minutes; S13, after the reaction is completed, the solution is cooled to room temperature, and then the precipitate is collected by centrifugation to obtain the core NaNdF4:Yb60%; finally, the NaNdF4:Yb60% nanocrystals are dispersed in cyclohexane for later use; S2. Preparation of NaNdF4:Yb60%@NaLuF4 core-shell structure: S21, adding lutetium oxide to an aqueous solution containing trifluoroacetic acid; heating to 90-110° C. until the solid is completely dissolved, and then continuing to heat until the solution is completely evaporated to obtain lutetium trifluoroacetate solid powder; S22, adding sodium trifluoroacetate, oleic acid, 1-octadecene and the NaNdF4:Yb60% cyclohexane solution prepared in step S13 to the lutetium trifluoroacetate solid powder; heating to 110-130° C. under an inert gas atmosphere and maintaining for 20-40 min to remove cyclohexane and water in the system; and then heating to 290-310° C. and reacting for 50-70 min to epitaxially grow a NaLuF4 shell layer; S23, after the solution is cooled to room temperature, the precipitate is collected by centrifugation to obtain the high-brightness near-infrared luminescent β-phase Nd 3+ and Yb 3+ Co-doped core-shell nanocrystals.
2. A high-brightness near-infrared luminescent β-phase Nd according to claim 1 3+ and Yb 3+ The method for preparing co-doped core-shell structure nanocrystals is characterized by: In step S11, the usage ratio of the rare earth acetate to oleic acid and 1-octadecene is 1-3 mmol:7.5 mL:15 mL.
3. A high-brightness near-infrared luminescent β-phase Nd according to claim 1 3+ and Yb 3+ The method for preparing co-doped core-shell structure nanocrystals is characterized by: In step S12, the molar concentration of the methanol solution containing sodium hydroxide is 0.2-0.5 mmol / mL, and the molar concentration of the methanol solution containing ammonium fluoride is 0.3-0.5 mmol / mL.
4. A high-brightness near-infrared luminescent β-phase Nd according to claim 1 3+ and Yb 3+ The method for preparing co-doped core-shell structure nanocrystals is characterized by: In step S12, the volume ratio of the methanol solution containing sodium hydroxide to the methanol solution containing ammonium fluoride is 1:
1.
5. A high-brightness near-infrared luminescent β-phase Nd according to claim 1 3+ and Yb 3+ The method for preparing co-doped core-shell structure nanocrystals is characterized by: In step S21, the dosage ratio of lutetium oxide to trifluoroacetic acid aqueous solution is 0.5-2 mmol / 10-20 mL, and the volume fraction of trifluoroacetic acid aqueous solution is 50%.
6. A high-brightness near-infrared luminescent β-phase Nd according to claim 1 3+ and Yb 3+ The method for preparing co-doped core-shell structure nanocrystals is characterized by: In step S22, the dosage ratio of the sodium trifluoroacetate, oleic acid, 1-octadecene and NaNdF4:Yb60% cyclohexane solution is 1-3mmol:10mL:10mL:10-20mL, and the molar concentration of the NaNdF4:Yb60% cyclohexane solution is 0.1-0.2mmol / mL.
7. High-brightness near-infrared luminescent β-phase Nd prepared by the preparation method according to any one of claims 1 to 6 3+ and Yb 3+ Co-doped core-shell nanocrystals.
8. The high-brightness near-infrared luminescent β-phase Nd as claimed in claim 7 3+ and Yb 3+ Application of co-doped core-shell structured nanocrystals in immunochromatographic detection.
9. A high-brightness near-infrared light-emitting β-phase Nd 3+ and Yb 3+ A serum marker luminescent detection lateral flow test strip co-doped with core-shell structure nanocrystals, characterized in that: The lateral flow test strip is made of the high brightness near-infrared luminescent β-phase Nd 3+ and Yb 3+ Co-doped core-shell structure nanocrystals are used as immune markers. The lateral flow test strip is composed of high-brightness near-infrared luminescent β-phase Nd 3+ and Yb 3+ The invention is composed of a co-doped core-shell structure nanocrystal, a polyvinyl chloride support back plate, a detection pad, a conjugation pad, a sample pad, and a water-absorbing pad, wherein the conjugation pad is loaded with a high-brightness near-infrared luminescent β-phase Nd modified with a binding antibody or a target protein. 3+ and Yb 3+ High-brightness near-infrared luminescent β-phase Nd co-doped core-shell nanocrystal probe and anti-quality control antibody modified 3+ and Yb 3+ Co-doped core-shell structured nanocrystal probes.
10. A method according to claim 9 based on high brightness near infrared light emission β-phase Nd 3+ and Yb 3+ A serum marker luminescent detection lateral flow test strip co-doped with core-shell structure nanocrystals, characterized in that: The anti-quality control antibody includes goat anti-chicken IgY antibody.