Method for recovering large-particle calcium fluoride from fluorine-containing wastewater

By carrying out impurity removal treatment and crystal seed activation in fluorine-containing acidic wastewater, combined with the use of crystal growth accelerators, the problem of difficulty in ensuring the quality of calcium fluoride recovery from high-concentration fluorine-containing acidic wastewater has been successfully solved, achieving high purity and large particles. The recovery of calcium fluoride simplifies the process and avoids secondary pollution.

WO2024212734A1PCT designated stage expired Publication Date: 2024-10-17ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO

Patent Information

Application Number
PCT/CN2024/080103
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-11
Filing Date
2024-03-05
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing technology is difficult to recover high-quality calcium fluoride products when treating high-concentration fluorine-containing acidic wastewater. The process flow is complex and there is a risk of secondary pollution.

Method used

By removing impurities from fluorine-containing acidic wastewater, activating calcium fluoride-containing crystal seeds, adding a crystal growth accelerator under preset conditions, adjusting pH and stirring, settling, filtering and drying, large particle fluoride is obtained. calcium.

Benefits of technology

It achieves the recovery of high-purity, large-particle calcium fluoride while discharging wastewater fluoride up to the standard, simplifying the process, avoiding secondary pollution, and ensuring high-quality recovery of calcium fluoride.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024080103_17102024_PF_FP_ABST
    Figure CN2024080103_17102024_PF_FP_ABST
Patent Text Reader

Abstract

A method for recovering large-particle calcium fluoride from fluorine-containing wastewater. The method comprises: subjecting fluorine-containing acidic wastewater to an impurity removal treatment to obtain pure fluorine-containing wastewater; activating a seed crystal containing calcium fluoride to obtain an activated seed crystal; adding the activated seed crystal to the pure fluorine-containing wastewater, adding a calcium-containing regulator according to a preset calcium-fluorine ratio, and then adding a crystal growth promoter according to a preset mass ratio to obtain a reaction solution; and adjusting the pH of the reaction solution at a preset reaction temperature, stirring the reaction solution, and subjecting same to sedimentation, filtration and drying to obtain large-particle calcium fluoride, wherein the adding amount of the activated seed crystal is 5-10 times the concentration of fluorine ions in the pure fluorine-containing wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

A method for recovering large-particle calcium fluoride from fluoride-containing wastewater

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to Chinese patent application No. 2023103854864 filed on April 11, 2023, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present disclosure relates to the field of wastewater treatment, and in particular to a method for recovering large-particle calcium fluoride from fluoride-containing wastewater. Background Art

[0004] Fluoride is an essential trace element for the human body to maintain normal physiological activities. A moderate amount of fluoride promotes the calcification of teeth and bones, aids in the conduction of nerve impulses, and promotes enzyme metabolism. However, excessive fluoride poses serious risks to humans, soil, animals, and plants. The World Health Organization stipulates that the upper limit of fluoride content in drinking water is 1.5 mg / L. The "Integrated Wastewater Discharge Standard" sets the fluoride ion content limit at 10 mg / L, while the "Drinking Water Quality Hygiene Standard" sets the fluoride content limit at 1 mg / L. Conventional treatment methods for fluoride-containing wastewater, such as chemical precipitation and flocculation precipitation, produce large amounts of sludge with high water content and low purity of calcium fluoride, making it unusable as a product. Discharge into the environment poses serious risks to humans, soil, animals, and plants, and also results in a waste of fluoride resources. Recovering fluoride from wastewater as fluoride would not only solve the problem of wastewater defluoridation, but also achieve fluoride resource recovery, which is of great significance.

[0005] However, existing technologies for recovering fluorine from fluoride-containing acidic wastewater suffer from varying degrees of complexity, difficulty ensuring the quality of recovered calcium fluoride, and the risk of secondary contamination. Therefore, developing a method that can simultaneously treat high-concentration fluoride-containing acidic wastewater and recover high-quality calcium fluoride products is a pressing technical challenge.

[0006] Summary of the Invention

[0007] The present disclosure provides a method for recovering large-particle calcium fluoride from fluorine-containing wastewater, so as to solve the technical problem in the prior art of recovering fluorine from fluorine-containing acidic wastewater while simultaneously recovering high-quality calcium fluoride products.

[0008] According to some embodiments of the present disclosure, a method for recovering large-particle calcium fluoride from fluoride-containing wastewater includes: removing impurities from fluoride-containing acidic wastewater to obtain pure fluoride-containing wastewater; activating calcium fluoride seed crystals to obtain activated seed crystals; adding the activated seed crystals to the pure fluoride-containing wastewater, and adding a calcium-containing regulator according to a preset calcium-fluoride ratio, and then adding a crystal growth promoter at a preset mass ratio to obtain a reaction solution; and adjusting the pH of the reaction solution at a preset reaction temperature, stirring, and then settling, filtering and drying to obtain large-particle calcium fluoride, wherein the amount of the activated seed crystals added is 5 to 10 times the fluoride ion concentration in the pure fluoride-containing wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present disclosure and, together with the description, serve to explain the principles of the present disclosure.

[0010] In order to more clearly illustrate the embodiments of the present disclosure or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0011] FIG1 is a schematic flow diagram of a method for recovering large-particle calcium fluoride from fluoride-containing wastewater according to some embodiments of the present disclosure;

[0012] FIG2 is a detailed schematic diagram of a method for recovering large-particle calcium fluoride from fluoride-containing wastewater according to some embodiments of the present disclosure;

[0013] FIG3 is a phase diagram of large-particle calcium fluoride obtained by a method for recovering large-particle calcium fluoride from fluoride-containing wastewater according to some embodiments of the present disclosure;

[0014] FIG4 is a particle size distribution diagram of large-particle calcium fluoride obtained by a method for recovering large-particle calcium fluoride from fluoride-containing wastewater according to some embodiments of the present disclosure. DETAILED DESCRIPTION

[0015] To make the objectives, technical solutions, and advantages of the embodiments of the present disclosure more clear, the technical solutions in some embodiments will be clearly and completely described below in conjunction with the accompanying drawings in some embodiments. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without making any creative efforts shall fall within the scope of protection of the present disclosure.

[0016] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present disclosure can be purchased from the market or prepared by existing methods.

[0017] The method for recovering calcium fluoride from fluorine-containing acidic wastewater in the related art includes:

[0018] (1) A method for treating high-concentration fluorine-containing wastewater and recovering fluorine, wherein two reaction tanks are sequentially set up, chemical gypsum and calcium chloride are added to each tank, and fluoride ions in the fluorine-containing wastewater are converted into calcium fluoride precipitates. The discharged wastewater is then filtered through a fluorite sand filter tank to ensure that the wastewater meets discharge standards. Calcium fluoride is also recovered at the same time. However, the calcium fluoride product obtained by this method cannot be effectively separated from calcium sulfate, and the quality of the calcium fluoride is unstable;

[0019] (2) A method for producing calcium fluoride using high-fluorine-containing industrial wastewater. This method uses calcium hydroxide and calcium chloride to jointly precipitate fluoride ions in the fluoride-containing wastewater. The precipitated product is passed through an inclined plate sedimentation tank, concentrated and filtered to obtain a mixed solid product with a calcium fluoride content of 30%-35%. The treated wastewater is passed through a precision filter to ensure that the effluent meets discharge standards. The calcium fluoride obtained by this method has low purity and low utilization value.

[0020] (3) A method for multi-stage treatment of high-concentration fluorine-containing wastewater and in-situ preparation of high-purity CaF2. The principle of this method is to first remove impurities from the high-concentration fluorine-containing wastewater, specifically by adding barium chloride to remove SO4 2- , add oxidant to remove organic matter, add Fe 2+ The activated carbon is used to remove heavy metal ions, and then the fluoride-containing wastewater after impurity removal enters a lime bed containing calcium oxide. A two-step process of in-situ crystallization of some calcium sulfate and in-situ generation of CaF2 is used to form fluoride-containing sludge with a high calcium fluoride content. Although this method improves the purity of calcium fluoride in the fluoride-containing sludge, it is easy to bring about the risk of excessive heavy metals due to the addition of barium salts during the treatment process. In addition, the process flow of the method is cumbersome and the operation is complicated.

[0021] (4) A method and apparatus for treating fluorine-containing wastewater, which introduces a fluidized bed crystallization reactor. Utilizing the principle of induced crystallization, calcium fluoride precipitates with large particles and low water content can be recovered. However, the equipment requirements are high, the process is complex, and the process conditions are difficult to control.

[0022] (5) A method for graded treatment of fluorine-containing acidic wastewater and recovery of calcium fluoride resources, wherein calcium-containing alkaline substances (one or more of quicklime, carbide slag or lime milk) are added to the fluorine-containing wastewater, followed by the addition of calcium chloride, inhibitors and collectors, and the removal of impurity foam in the fluorine-containing wastewater by combining the inhibitors and collectors with aeration flotation, followed by filtration and drying to obtain calcium fluoride particles. The inhibitor is one or two of water glass, acidic water glass, and tannic acid, and the collector is one or a mixture of two or more fatty acid organic substances such as oleic acid, sodium oleate, sodium petroleum sulfonate, and sodium lauryl sulfate. This method relies solely on flotation to remove impurities in the sludge, resulting in poor removal effect and poor quality of the recovered calcium fluoride, with the highest purity being 92.3%;

[0023] (6) A method for recycling and reusing fluorine-containing wastewater based on calcium fluoride-induced precipitation, wherein the total molar number of fluoride ions in the treated fluorine-containing wastewater is calculated first; and the total molar number of fluoride ions in the treated fluorine-containing wastewater is calculated according to the molar ratio n(Ca 2+ / F - )=1.0. Calcium chloride, calcium fluoride at a rate of 5.0 g / L, and polyacrylamide (PAM) as a coagulant aid are added to fluoride-containing wastewater. After stirring, the mixture is allowed to settle to obtain sludge water. The sludge water is separated, and the obtained sludge portion can be returned to the fourth step as calcium fluoride precipitation nuclei for reuse. The remaining sludge is extracted with calcium fluoride for reuse in the preparation of fluorine-containing products. The obtained sludge has a moisture content of less than 50%, and the content of recyclable calcium fluoride is greater than 80%. This method has a high moisture content in the sludge and low purity of the recovered calcium fluoride.

[0024] Therefore, overall, the existing fluorine recovery technology for fluorine-containing wastewater has problems to varying degrees, such as complex process flow, difficulty in ensuring the quality of calcium fluoride recovery, and the risk of secondary pollution.

[0025] Seed crystal growth promoters in related technologies include:

[0026] (1) A method for preparing coarse-grained aluminum hydroxide from an ammonium aluminum sulfate solution, wherein the seed growth promoter is sodium dodecylsulfonate or sodium dodecylbenzenesulfonate or a mixture thereof, and the addition amount is 400 to 600 ppm;

[0027] (2) A method for efficient comprehensive utilization of arsenic alkali residue resources, wherein the crystal growth promoter is citric acid, and the amount of citric acid is measured at a concentration of 30-100 mg / L in a leachate containing sodium carbonate and sodium arsenate;

[0028] (3) A potassium sulfate crystal growth promoter and its application, wherein the crystal growth promoter comprises sodium tripolyphosphate, diammonium hydrogen phosphate, magnesium sulfate, urea and sodium sulfate;

[0029] (4) A process for preparing large-particle food-grade calcium hydrogen phosphate, wherein the particle promoter comprises one or two of K2CO3, KOH, K3C6H5O7, or K2C2O4, and the amount added is 1.5-3.5% of the total mass of the calcium carbonate suspension and the phosphoric acid solution;

[0030] (5) A method for improving the filtration performance of ferrous sulfate, wherein the accelerator is either ferrous sulfate heptahydrate or cellulose, and the addition amount is 0.1%-5.0% by weight of the titanium clearing liquid;

[0031] (6) A method for eliminating the periodic refinement of the particle size of the seed product, wherein the aluminum hydroxide trace crystal growth promoter is a mixture of fatty acid and sodium dodecylbenzene sulfonate, wherein the mass fraction of the fatty acid is 20-60%, the mass fraction of the sodium dodecylbenzene sulfonate is 40-80%, and the fatty acid molecular formula is C n H 2n +COOH, n=16 or 18, added in an amount to achieve a volume concentration of 10-300 ppm in the solution.

[0032] In general, different types of seed crystal growth have their own specific crystal growth promoters, but no research or reports on calcium fluoride seed crystal growth promoters were found.

[0033] Therefore, how to provide a method that can treat high-concentration fluorine-containing acidic wastewater and recover high-quality calcium fluoride products is a technical problem that urgently needs to be solved.

[0034] FIG1 is a flow diagram of a method for recovering large-particle calcium fluoride from fluoride-containing wastewater according to some embodiments of the present disclosure. As shown in FIG1 , a method for recovering large-particle calcium fluoride from fluoride-containing wastewater according to some embodiments of the present disclosure comprises: step S1. removing impurities from fluoride-containing acidic wastewater to obtain pure fluoride-containing wastewater; step S2. activating calcium fluoride-containing seed crystals to obtain activated seed crystals; step S3. adding the activated seed crystals to the pure fluoride-containing wastewater, and adding a calcium-containing regulator according to a preset calcium-fluoride ratio, and then adding a crystal growth promoter at a preset mass ratio to obtain a reaction solution; and step S4. adjusting the pH of the reaction solution at a preset reaction temperature, stirring the reaction solution, and then settling, filtering and drying the reaction solution to obtain large-particle calcium fluoride. The amount of activated seed crystals added is 5 to 10 times the fluoride ion concentration in the pure fluoride-containing wastewater.

[0035] In some embodiments, the positive effect of controlling the amount of activated seed crystals added to be 5 to 10 times the fluoride ion concentration in the pure fluoride-containing wastewater is that within this range, sufficient activated seed crystals are ensured to be added, which can effectively control the growth of calcium fluoride crystals during the reaction process, allowing subsequent homogeneous nucleation to form and obtain large calcium fluoride particles.

[0036] FIG2 is a detailed schematic diagram of a method for recovering large particles of calcium fluoride from fluoride-containing wastewater according to some embodiments of the present disclosure. As shown in FIG2 , in some optional embodiments, the activation of calcium fluoride-containing seed crystals includes the steps of:

[0037] S201. Sieving calcium fluoride to a particle size of <30 μm to obtain a sieved material;

[0038] S202. Add a seed crystal activator to the sieved material, perform ultrasonic treatment, and then filter and dry to obtain activated seed crystals.

[0039] In some embodiments, the specific steps of activating the calcium fluoride-containing seed crystals are defined as follows: first, the calcium fluoride is sieved to obtain a sieved material with a small particle size, and then a seed crystal activator is added to the sieved material, and ultrasonication is performed, so that the seed crystal activator can fully activate the sieved material containing calcium fluoride.

[0040] At the same time, the addition of a seed crystal activator can achieve etching of the seed crystal surface and reset of the surface micro-electric field, making the seed crystal more conducive to continued growth and expansion of the crystal, thereby subsequently obtaining large-particle calcium fluoride.

[0041] In some optional embodiments, the liquid-to-solid ratio of the seed crystal activator to the sieved material is 2 to 5:1.

[0042] In some embodiments, the positive effect of controlling the liquid-solid ratio of the seed crystal activator to the sieved material to be 2 to 5:1 is that within this liquid-solid ratio range, the activation effect of the seed crystal activator on the calcium fluoride in the sieved material can be ensured, and the activated seed crystals can be obtained in combination with subsequent ultrasound.

[0043] In some optional embodiments, the seed crystal activator includes at least one of fatty alcohol polyoxyethylene ether, acetic acid, ammonium bifluoride, ammonium chloride, and sodium fluoride.

[0044] In some embodiments, controlling the specific type of the seed crystal activator can ensure sufficient activation of the calcium fluoride-containing screening material.

[0045] In some optional embodiments, the power of the ultrasound is 10w to 100w.

[0046] In some embodiments, controlling the specific power of ultrasound can not only ensure complete mixing of the seed crystal activator and the sieved material, but also ensure that the seed crystal activator can effectively change the micro-electric field distribution of the solution and the surface activity of the crystal growth surface, making it more conducive to the continued growth and expansion of the crystals, thereby obtaining large particles of calcium fluoride.

[0047] In some optional embodiments, the crystal growth promoter includes at least one of sodium glycocholate, triglyceride, ethanol, lauryl glucoside, gluconic acid, magnesium trichloride, and copper chloride.

[0048] In some embodiments, controlling the specific type of crystal growth promotion can effectively change the solution micro-electric field distribution and the surface activity of the crystal growth surface, making it more conducive to the continued growth and expansion of the crystals, thereby obtaining large-particle calcium fluoride products.

[0049] In some optional embodiments, the calcium-containing regulator includes calcium chloride and / or clarified lime water.

[0050] In some embodiments, controlling the specific type of calcium-containing regulator can not only provide a portion of calcium ions, but also preliminarily improve the pH value of the pure fluoride-containing wastewater, thereby facilitating the subsequent use of crystal growth promoters to promote the formation and growth of crystals.

[0051] In some optional embodiments, the preset calcium-fluorine ratio is 1.05-1.15; the preset mass ratio is 0.01‰-0.5‰.

[0052] In some embodiments, the preset calcium-fluorine ratio is controlled to be 1.05-1.15 and the preset mass ratio is 0.01‰-0.5‰. Within this range, the growth of the crystal can be effectively controlled and the generation of heterogeneous nucleation can be effectively avoided, thereby ensuring uniform growth of the crystal and obtaining a large-particle calcium fluoride product.

[0053] In some optional embodiments, the preset reaction temperature is 10° C. to 30° C.; and / or the pH is 6.0 to 9.0.

[0054] In some embodiments, controlling the specific preset reaction temperature and pH can, on the one hand, adjust the solubility and pH of the reaction solution so that a large amount of calcium fluoride product can be subsequently precipitated. On the other hand, by adjusting the specific conditions of the reaction solution, the growth of crystals can be controlled, effectively avoiding the generation of heterogeneous nucleation.

[0055] In some optional embodiments, the stirring includes first stirring and second stirring, the first stirring time is 5 minutes to 10 minutes, the second stirring time is 0.5 hours to 1 hour, and the rotation speed of the first stirring is greater than the second stirring.

[0056] In some embodiments, the specific manner and time of stirring are controlled. On the one hand, a first stirring at a faster speed can be combined with a second stirring at a slower speed to ensure uniform dispersion of the solute in the reaction solution. On the other hand, the first stirring and the second stirring can be used to ensure uniform crystal growth, thereby obtaining a large-particle calcium fluoride product.

[0057] The present disclosure will be further described below with reference to specific examples. It should be understood that these examples are intended to illustrate the present disclosure only and are not intended to limit the scope of the present disclosure. Experimental methods in the following examples where specific conditions are not specified are generally measured in accordance with national standards. If no corresponding national standards are available, the methods were performed in accordance with commonly used international standards, conventional conditions, or conditions recommended by the manufacturer.

[0058] Example 1

[0059] Fluoride-containing acidic wastewater with a fluoride ion concentration of 1500 mg / L was treated for impurity removal. Chemically pure calcium fluoride with a particle size of less than 30 μm was activated with a mixture of fatty alcohol polyoxyethylene ether and acetic acid at a liquid-solid ratio of 2:1 and ultrasonic wave 100W. Then, 5 times the fluoride ion concentration in the solution was added to the purified fluoride-containing wastewater after impurity removal, and the calcium-fluoride molar ratio n(Ca 2+ / F - )=1.15, and adding clear lime water and calcium fluoride crystal growth promoter to the impurity-removed solution at a ratio of 0.5‰ of the total mass of the solution to obtain a reaction solution. The crystal growth promoter is composed of triglyceride, ethanol, and gluconic acid.

[0060] The temperature of the reaction solution was controlled at 30°C, and the pH value was adjusted to 9.0. The mixture was stirred rapidly for 5 minutes, then slowly stirred for 1 hour, and fully settled, filtered, and the filter cake was dried at 105°C. Figure 3 is a phase diagram of large-particle calcium fluoride in a method for recovering large-particle calcium fluoride from fluoride-containing wastewater according to some embodiments of the present disclosure. As shown in Figure 3, large-particle calcium fluoride was obtained, and the fluoride ion concentration in the filtrate was less than 10 mg / L, which met the emission standards. The purity of the recovered large-particle calcium fluoride reached 98.12%. Figure 4 is a particle size distribution diagram of large-particle calcium fluoride in a method for recovering large-particle calcium fluoride from fluoride-containing wastewater according to some embodiments of the present disclosure. As shown in Figure 4, D90 = 71.223 μm.

[0061] Example 2

[0062] Comparing Example 2 with Example 1, the difference between Example 2 and Example 1 is:

[0063] Fluoride-containing acidic wastewater with a fluoride ion concentration of 2500 mg / L was treated for impurity removal. Chemically pure calcium fluoride with a particle size of less than 30 μm was activated with a mixture of ammonium chloride and sodium fluoride at a liquid-solid ratio of 3:1 and ultrasonic 10W. Then, 10 times the fluoride ion concentration in the solution was added to the purified fluoride-containing wastewater after impurity removal, and the calcium-fluoride molar ratio n(Ca 2+ / F -)=1.05, and adding calcium chloride and calcium fluoride crystal growth promoters to the impurity-removed solution at a concentration of 0.01‰ of the total mass of the solution to obtain a reaction solution. The crystal growth promoter consists of lauryl glucoside and copper chloride.

[0064] The reaction solution temperature was controlled at 10°C, the pH value was adjusted to 6.0, and the mixture was first stirred rapidly for 10 minutes and then slowly stirred for 0.5 hours. The mixture was fully settled, filtered, and the filter cake was dried at 105°C to obtain large-particle calcium fluoride. The fluoride ion concentration of the filtrate was less than 10 mg / L, meeting the emission standards. The purity of the recovered large-particle calcium fluoride reached 98.03%, and D90 was 72.681 μm.

[0065] Example 3

[0066] Comparing Example 3 with Example 1, the difference between Example 3 and Example 1 is:

[0067] Fluoride-containing wastewater with a fluoride ion concentration of 800 mg / L was treated for impurity removal. Chemically pure calcium fluoride with a particle size of less than 30 μm was activated with a mixture of fatty alcohol polyoxyethylene ether and ammonium bifluoride at a liquid-solid ratio of 5:1 and ultrasonic wave 60W. Then, 6 times the fluoride ion concentration in the solution was added to the purified fluoride-containing wastewater after impurity removal, and the calcium-fluoride molar ratio was adjusted to n(Ca 2+ / F - )=1.10, and adding calcium chloride and calcium fluoride crystal growth promoters to the impurity-removed solution at a rate of 0.2‰ of the total mass of the solution to obtain a reaction solution, wherein the crystal growth promoter consists of sodium glycocholate and magnesium trichloride.

[0068] The solution temperature was controlled at 20°C, the pH value was adjusted to 8.0, the mixture was first stirred rapidly for 8 minutes, then stirred slowly for 0.8 hours, and the mixture was fully settled, filtered, and the filter cake was dried at 105°C to obtain large-particle calcium fluoride. The fluoride ion concentration of the filtrate was less than 10 mg / L, meeting the emission standards. The purity of the recovered large-particle calcium fluoride reached 98.23%, and D90 was 73.002 μm.

[0069] Example 4

[0070] Comparing Example 4 with Example 1, the difference between Example 4 and Example 1 is:

[0071] Fluoride-containing wastewater with a fluoride ion concentration of 120 mg / L was treated for impurity removal. Chemically pure calcium fluoride with a particle size of less than 30 μm was activated with a mixture of fatty alcohol polyoxyethylene ether, acetic acid and sodium fluoride under the conditions of liquid-solid ratio of 4:1 and ultrasonic wave 80W. Then, 7 times the fluoride ion concentration in the solution was added to the purified fluoride-containing wastewater after impurity removal, and the calcium fluoride molar ratio n (Ca 2+ / F -)=1.12, and adding calcium chloride and calcium fluoride crystal growth promoters to the impurity-removed solution at a ratio of 0.3‰ of the total mass of the solution to obtain a reaction solution, wherein the crystal growth promoter consists of ethanol and copper chloride.

[0072] The solution temperature was controlled at 15°C, the pH value was adjusted to 7.0, the mixture was first stirred rapidly for 7 minutes, then stirred slowly for 0.6 hours, and the mixture was fully settled, filtered, and the filter cake was dried at 105°C to obtain large-particle calcium fluoride. The fluoride ion concentration of the filtrate was less than 10 mg / L, meeting the emission standards. The purity of the recovered large-particle calcium fluoride reached 98.15%, and D90 was 72.452 μm.

[0073] Example 5

[0074] Comparing Example 5 with Example 1, the difference between Example 5 and Example 1 is:

[0075] Fluoride-containing wastewater with a fluoride ion concentration of 500 mg / L was treated for impurity removal. Chemically pure calcium fluoride with a particle size of less than 30 μm was activated with fatty alcohol polyoxyethylene ether at a liquid-solid ratio of 4:1 and ultrasonic 90W. The impurity-removed solution was added in an amount 8 times the fluoride ion concentration in the solution, and the calcium-fluoride molar ratio n(Ca 2+ / F - )=1.13, and adding clarified lime water and a calcium fluoride crystal growth promoter to the impurity-removed solution at a ratio of 0.4‰ of the total mass of the solution to obtain a reaction solution, wherein the crystal growth promoter consists of sodium glycocholate, triglyceride, copper chloride and magnesium trichloride.

[0076] The solution temperature was controlled at 25°C, the pH value was adjusted to 7.0, the mixture was first stirred rapidly for 9 minutes, then stirred slowly for 0.7 hours, and the mixture was fully settled, filtered, and the filter cake was dried at 105°C to obtain large-particle calcium fluoride. The fluoride ion concentration of the filtrate was less than 10 mg / L, meeting the emission standards. The purity of the recovered large-particle calcium fluoride reached 98.05%, and D90 was 72.013 μm.

[0077] According to one or more technical solutions of some embodiments of the present disclosure, at least the following technical effects or advantages are achieved:

[0078] (1) According to some embodiments of the present disclosure, a method for recovering large-particle calcium fluoride from fluorine-containing wastewater can recover high-purity, large-particle calcium fluoride while achieving fluorine discharge standards in the wastewater. The overall process is simple, easy to operate, and there is no secondary pollution.

[0079] (2) According to some embodiments of the present disclosure, a method for recovering large-particle calcium fluoride from fluoride-containing wastewater is provided. By adding a seed crystal activator, etching of the seed crystal surface and resetting of the surface micro-electric field can be achieved, making the seed crystal more conducive to continued crystal growth.

[0080] (3) According to some embodiments of the present disclosure, a method for recovering large-particle calcium fluoride from fluoride-containing wastewater is provided. By adding a regulator with a reasonable calcium-fluoride ratio to the solution and controlling other process conditions, the growth of crystals can be effectively controlled, and the generation of heterogeneous nucleation can be effectively avoided.

[0081] (4) According to some embodiments of the present disclosure, a method for recovering large-particle calcium fluoride from fluoride-containing wastewater can effectively change the solution micro-electric field distribution and the surface activity of the crystal growth surface by adding a crystal growth promoter, making it more conducive to the continued growth and expansion of the crystal.

[0082] According to some embodiments of the present disclosure, a method for recovering large-particle calcium fluoride from fluoride-containing wastewater comprises the following steps: first, the fluoride-containing acidic wastewater is subjected to impurity removal treatment, and then activated seed crystals are reacted with the impurity-removed fluoride-containing acidic wastewater. The relationship between the amount of activated seed crystals added and the fluoride ion concentration in the impurity-removed fluoride-containing acidic wastewater is controlled. Simultaneously, a calcium-containing regulator is added to preliminarily adjust the pH and provide some calcium ions. Crystals in the activated seed crystals are used to generate and precipitate part of calcium fluoride in the fluoride-containing acidic wastewater solution. The addition of a crystal growth promoter can effectively change the solution micro-electric field distribution and the surface activity of the crystal growth surface, making it more conducive to the continued growth and expansion of crystals in the activated seed crystals, thereby ensuring that the crystals in the activated seed crystals gradually grow and precipitate a sufficient amount of calcium fluoride to form a large-particle calcium fluoride product, thereby achieving the recovery of fluorine from the fluoride-containing acidic wastewater while recovering a high-quality calcium fluoride product.

[0083] Various embodiments of the present disclosure may be presented in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of the present disclosure; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numbers within the range. For example, the description of a range from 1 to 6 should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0084] In the present disclosure, unless otherwise specified, the directional words used, such as "upper" and "lower", specifically refer to the directions of the drawings in the accompanying drawings. In addition, in the description of the present disclosure, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second" are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" refers to one or more, and "plurality" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple.

[0085] The foregoing description is intended only to provide specific embodiments of the present disclosure, intended to enable those skilled in the art to understand and implement the present disclosure. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present disclosure. Therefore, the present disclosure is not to be limited to the embodiments shown herein, but is to be construed in the broadest manner consistent with the principles and novel features claimed herein.

Claims

1. A method for recovering large-particle calcium fluoride from fluoride-containing wastewater, include: The fluorine-containing acidic wastewater is treated to remove impurities to obtain pure fluorine-containing wastewater; activating the seed crystals containing calcium fluoride to obtain activated seed crystals; Adding the activated seed crystals to the pure fluorine-containing wastewater, adding a calcium-containing regulator according to a preset calcium-fluorine ratio, and then adding a crystal growth promoter according to a preset mass ratio to obtain a reaction solution; and Adjusting the pH of the reaction solution at a preset reaction temperature, stirring the reaction solution, and then settling, filtering and drying the reaction solution to obtain large-particle calcium fluoride; Wherein, the added amount of the activated seed crystal is 5 to 10 times the fluoride ion concentration in the pure fluoride-containing wastewater.

2. The method according to claim 1, in, The activation of the seed crystal containing calcium fluoride comprises the steps of: Screening calcium fluoride until the particle size is less than 30 μm to obtain a screened material; A seed crystal activator is added to the sieved material, and the mixture of the seed crystal activator and the sieved material is ultrasonicated, and then the mixture of the seed crystal activator and the sieved material after ultrasonication is filtered and dried to obtain activated seed crystals.

3. The method according to claim 2, in, The liquid-to-solid ratio of the seed activator to the screening material is 2 to 5:

1.

4. The method according to claim 2, in, The seed activator includes at least one of fatty alcohol polyoxyethylene ether, acetic acid, ammonium bifluoride, ammonium chloride and sodium fluoride.

5. The method according to claim 2, in, The power of the ultrasound is 10w-100w.

6. The method according to claim 1, in, The crystal growth promoter includes at least one of sodium glycocholate, triglyceride, ethanol, lauryl glucoside, gluconic acid, magnesium trichloride and copper chloride.

7. The method according to claim 1, in, The calcium-containing regulator includes calcium chloride and / or clarified lime water.

8. The method according to claim 1, in, The preset calcium-fluorine ratio is 1.05-1.15; the preset mass ratio is 0.01‰-0.5‰.

9. The method according to claim 1, in, The preset reaction temperature is 10°C to 30°C; and / or, The pH value is 6.0 to 9.

0.

10. The method according to claim 1, in, The stirring includes first stirring and second stirring, the first stirring lasts for 5 minutes to 10 minutes, the second stirring lasts for 0.5 hours to 1 hour, and the rotation speed of the first stirring is greater than that of the second stirring.

Citation Information

Patent Citations

  • Method and device for treating fluorine-containing waste water

    CN101941752A

  • Method for crystal form CaF2 production through rare earth wastewater resource comprehensive recovery

    CN109574313A

  • Defluorination method for fluorine-containing wastewater

    CN113264602A

  • Method for stage treatment of fluorine-containing acidic wastewater and recovery of calcium fluoride resource

    CN115583752A

  • Method for recovering large-particle calcium fluoride from fluorine-containing wastewater

    CN116588963A

Cited By

  • Method for recovering phosphate radicals, fluorine ions and sulfate radicals from ardealite washing water step by step

    CN120553897A

  • Lanthanum-loaded fluorite ball seed crystal and method for treating fluorine-containing wastewater by using lanthanum-loaded fluorite ball seed crystal

    CN120695718A

  • Lanthanum-loaded fluorite spherical seed and method for treating fluorine-containing wastewater by using the same

    CN120695718B

  • Processing method of safe fluorgypsum powder

    CN121377580A

  • Integrated wastewater crystallization and defluorination device with composite rotational flow cooperating with seed crystal activation

    CN122464578A