Preparation method for Anti-static polyimide resin

By using a combination of naphthalene ring structure, aromatic diamine, and naphthalene dianhydride in polyimide resin to form a π conjugated structure, the problem of performance attenuation and powder drop caused by conductive modifiers in the existing technology is solved. , realizing polyimide resin with high anti-static properties and mechanical properties, expanding its application fields.

WO2024212818A1PCT designated stage expired Publication Date: 2024-10-17HUANGSHAN JUXIN NEW MATERIALS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/084362
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-03-28
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

The performance of existing anti-static polyimide resin materials is attenuated after adding conductive modifiers, and the powder falls off during use, affecting product yield, and cannot meet the high anti-static performance requirements in specific fields.

Method used

By using naphthalene diamine containing a naphthalene ring structure to react with aromatic diamine and dianhydride at room temperature and under nitrogen protection conditions, a polyimide resin with a π conjugated structure is formed, and the amount of naphthalene diamine is controlled to be no less than that of naphthalene. The dosage of diamine and aromatic diamine accounts for 40%. The antistatic effect can be achieved without adding antistatic additives, and the performance is improved by using dianhydride containing naphthalene ring.

Benefits of technology

It achieves the additive-free anti-static effect of the body, avoids the problems of color difference and unstable performance caused by conductive modifiers, improves the mechanical properties of the material, and expands the application fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2024084362-APPB-I100001
    Figure PCTCN2024084362-APPB-I100001
Patent Text Reader

Abstract

The present invention relates to the technical field of high polymer materials. Disclosed is a preparation method for an anti-static polyimide resin. The preparation method comprises the following steps: step S1, at room temperature and under the condition of nitrogen protection, adding aromatic diamine and naphthalene diamine into an organic solvent, stirring until aromatic diamine and naphthalene diamine are completely dissolved, then adding aromatic dianhydride in batches, stirring to undergo a reaction at the room temperature for 9-18 h, and then adding 4-phenylethynylphthalic anhydride to undergo an end-capping reaction for 6-10 h to obtain an end-capped polyamic acid solution; and step S2, performing imidization treatment on the end-capped polyamic acid solution to obtain polyimide powder, cleaning by using ethanol and then performing suction filtration, and performing drying treatment for 3-5 h to obtain the anti-static polyimide resin. The present invention uses naphthalene diamine having a naphthalene ring structure, so that a prepared polyimide resin material has certain electrical property, can achieve an anti-static effect, and also has excellent mechanical property.
Need to check novelty before this filing date? Find Prior Art

Description

[Article 91, 02.04.2024] A method for preparing an antistatic polyimide resin Technical Field

[0001] The invention belongs to the technical field of polymer materials, and particularly relates to an antistatic polyimide resin and a preparation method thereof. Background Art

[0002] Polyimide resins have high strength and excellent resistance to high and low temperatures, making them an excellent representative of high-performance polymer materials. However, in certain specific applications, they still require additives or modifiers to enhance and modify their properties to meet the requirements. For example, in specialty electronics, electrical appliances, semiconductors, and specialized industrial fields, high antistatic performance requirements are placed on various polyimide materials. A variety of antistatic polyimide materials have been developed in the prior art, but almost all antistatic polyimide resin profiles currently on the market achieve their antistatic properties through the use of additives or modifiers, such as graphite, indium tin oxide (ITO), tin dioxide, titanium nitride, etc.

[0003] The addition of conductive modifiers to polyimide resin materials can lead to a certain degree of degradation in performance. Powder droplets during dynamic use can affect product yield. Therefore, conductive filler-modified antistatic polyimide resins cannot meet the current demands of specific applications. Therefore, developing a new polyimide resin with superior overall performance and inherent antistatic properties, particularly an antistatic polyimide resin that can be widely used in electronics, electrical appliances, semiconductors, and specialty industries, is of great significance. Summary of the Invention

[0004] The object of the present invention is to provide an antistatic polyimide resin and a preparation method thereof, so as to solve the problems in the background technology.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing an antistatic polyimide resin comprises the following steps:

[0007] Step S1, adding aromatic diamine and naphthalene diamine to an organic solvent at room temperature under nitrogen protection, stirring until completely dissolved, adding aromatic dianhydride in batches, stirring and reacting at room temperature for 9-18 hours, and then adding 4-phenylethynylphthalic anhydride to cap the reaction for 6-10 hours to obtain a capped polyamic acid solution;

[0008] Step S2: imidizing the blocked polyamic acid solution to obtain polyimide powder, washing with ethanol, filtering, and drying for 3-5 hours to obtain an antistatic polyimide resin.

[0009] Furthermore, the usage ratio of the organic solvent, aromatic diamine, naphthalenediamine, aromatic dianhydride and 4-phenylethynylphthalic anhydride is 500-600 mL: 0.11-0.17 mol: 0.11-0.18 mol: 0.285-0.295 mol: 0.0008-0.002 mol; and the usage of naphthalenediamine is not less than 40% of the molar sum of the usage of naphthalenediamine and aromatic diamine.

[0010] Furthermore, the aromatic diamine is one of 4,4'-diaminodiphenyl ether, 1,3-bis(4'-aminophenoxy)benzene and 3,3',5,5'-tetramethylbenzidine.

[0011] Furthermore, the naphthalene diamine is one of 1,4-naphthalene diamine, 1,5-naphthalene diamine, 1,6-naphthalene diamine, 1,7-naphthalene diamine, 2,6-naphthalene diamine, and 2,7-naphthalene diamine, preferably 1,5-naphthalene diamine or 2,6-naphthalene diamine.

[0012] Furthermore, the aromatic dianhydride is composed of one or more of 3,3',4,4'-biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride and 2,3,6,7-naphthalenetetracarboxylic dianhydride in any proportion; preferably, the aromatic dianhydride contains one of 1,4,5,8-naphthalenetetracarboxylic dianhydride and 2,3,6,7-naphthalenetetracarboxylic dianhydride, which can further improve the antistatic properties of the obtained polyimide resin.

[0013] Furthermore, one method of the imidization treatment is:

[0014] 100-200 mL of an organic solvent is added to the blocked polyamic acid solution and stirred to reduce the viscosity of the blocked polyamic acid solution. A mixture of acetic anhydride and triethylamine in a volume ratio of 1:2 is then added, and the mixture is reacted for 20-24 hours and then precipitated in an ethanol aqueous solution.

[0015] Furthermore, the organic solvent is a mixture of one or more of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone in any proportion.

[0016] Furthermore, another method of the imidization treatment is:

[0017] Add 100-200 mL of water-carrying agent to the blocked polyamic acid solution, heat it in an oil bath at 180°C until no water is separated from the water separator, then cool it to below 60°C and use a centrifuge to remove the organic solvent.

[0018] Furthermore, the water-carrying agent is one of toluene, xylene, trimethylbenzene and dichlorobenzene.

[0019] Furthermore, the temperature of the drying process is 150° C., and the vacuum degree is above -0.09 MPa, preferably -0.095 MPa.

[0020] An antistatic polyimide resin is prepared by the above preparation method.

[0021] Beneficial effects of the present invention:

[0022] The present invention uses naphthalene diamine containing a naphthalene ring structure to prepare a polyimide resin. By controlling the amount of naphthalene diamine to be no less than 40% of the molar sum of the amounts of naphthalene diamine and aromatic diamine, the prepared polyimide resin can achieve an antistatic effect without adding any antistatic additives or modifiers. The principle is that the naphthalene rings overlap to form a closed conjugated large π bond, and after polymerization, alternating units of the π conjugated structure are formed on the polyimide main chain. By controlling the content of the naphthalene diamine monomer, the polyimide resin material has certain electrical properties and can achieve the antistatic effect of the material. In addition, by using a dianhydride containing a naphthalene ring in combination, the antistatic performance of the polyimide resin of the present invention can be further improved.

[0023] Because no conductive modifier is required, there is no problem of product color difference caused by inconsistent addition of the conductive modifier, nor is there any problem of unstable antistatic effect and deterioration of material mechanical properties caused by uneven dispersion of the conductive modifier. The antistatic polyimide resin prepared by the present invention not only has an excellent antistatic effect but also has good mechanical properties. It can be used in the preparation of antistatic polyimide resin profiles, further expanding the application field of this material.

[0024] The present invention can realize the imidization of polyamic acid by using both chemical method and thermal method, the synthesis method is simple, does not require ultra-high temperature and high pressure, the synthesis process is mild, and the production safety is higher. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts shall fall within the scope of protection of the present invention. Example

[0026] An antistatic polyimide resin is prepared by the following steps:

[0027] Step S1, add 500mL N,N-dimethylformamide to a 1000mL glass flask, add 35.4g 4,4'-diaminodiphenyl ether and 18.70g 1,5-naphthalene diamine at room temperature, and mechanically stir under nitrogen atmosphere until the above substances are completely dissolved, then slowly add 25.80g 3,3',4,4'-biphenyltetracarboxylic dianhydride and 44.73g pyromellitic dianhydride, respectively, stir and react for 12h, then add 0.5g 4-phenylethynylphthalic anhydride to cap the reaction for 10h to obtain a blocked polyamic acid solution;

[0028] Step S2, adding 120mL of N,N-dimethylformamide to the polyamic acid solution and stirring to mix, then adding 35mL of triethylamine and 70mL of acetic anhydride for imidization treatment, reacting for 24 hours, and precipitating in an ethanol aqueous solution to obtain a polyimide powder, which is then washed with ethanol and filtered, and dried at a temperature of 150°C and a vacuum degree of -0.095MPa for 3 hours to obtain an antistatic polyimide resin. Example

[0029] An antistatic polyimide resin is prepared by the following steps:

[0030] Step S1, 500mL N,N-dimethylacetamide was added to a 1000mL glass flask, and 48.82g 1,3-bis(4'-aminophenoxy)benzene and 23.18g 1,5-naphthalene diamine were added at room temperature. Under nitrogen atmosphere, the mixture was mechanically stirred until the above substances were completely dissolved. Then, 15.71g 1,4,5,8-naphthalenetetracarboxylic dianhydride was slowly added. After stirring and reacting at room temperature for 6h, 51.10g pyromellitic dianhydride was slowly added. The stirring reaction was continued for 3h, and then 0.2g 4-phenylethynylphthalic anhydride was added for end-capping reaction for 6h to obtain a blocked polyamic acid solution;

[0031] Step S2, adding 150mL of toluene to the polyamic acid solution, heating in an oil bath at 180°C until almost no water is separated in the water separator, cooling to below 60°C, removing the solvent by centrifuge to obtain polyimide powder, and then washing with ethanol and filtering, and drying at a temperature of 150°C and a vacuum degree of -0.095MPa for 4h to obtain an antistatic polyimide resin. Example

[0032] An antistatic polyimide resin is prepared by the following steps:

[0033] Step S1, add 600mL N-methylpyrrolidone to a 1000mL glass flask, add 28.17g 3,3',5,5'-tetramethylbenzidine and 27.81g 1,5-naphthalene diamine at room temperature, and mechanically stir under nitrogen atmosphere until the above substances are completely dissolved, then slowly add 23.57g 2,3,6,7-naphthalenetetracarboxylic dianhydride, stir and react at room temperature for 6h, then slowly add 60.34g 3,3',4,4'-biphenyltetracarboxylic dianhydride, continue stirring and reacting for 12h, and then add 0.5g 4-phenylethynylphthalic anhydride to cap the reaction for 6h to obtain a blocked polyamic acid solution;

[0034] Step S2, adding 200 mL of N-methylpyrrolidone to the blocked polyamic acid solution and stirring to mix, then adding 35 mL of triethylamine and 70 mL of acetic anhydride for imidization treatment, reacting for 20 hours, and precipitating in an ethanol aqueous solution to obtain a polyimide powder, which is then washed with ethanol and filtered, and dried at a temperature of 150 ° C and a vacuum degree of -0.095 MPa for 3 hours to obtain an antistatic polyimide resin.

[0035] The polyimide resins prepared in Examples 1 to 3 were pressed into standard bars using a four-post plate vulcanizer under the same pressing conditions. The standard bars were then subjected to performance tests for elongation at break, volume resistivity, tensile strength, flexural strength, unnotched impact strength, and hardness. The test results are shown in Table 1.

[0036] Table 1

[0037]

[0038] As can be seen from the test data in Table 1, the antistatic polyimide resins prepared in Examples 1 to 3 have a low volume resistivity, and the volume resistivity of the materials prepared in Examples 2 and 3 is much lower than that of the material prepared in Example 1, which proves that the use of a dianhydride containing a naphthalene ring can further improve the antistatic performance of the polyimide resin of the present invention; and the antistatic polyimide resins prepared in Examples 1 to 3 have good mechanical properties, meet the preparation of antistatic polyimide resin profiles, and expand the application field of this material.

[0039] It should be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus.

[0040] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing an antistatic polyimide resin, characterized in that: The following steps are involved: Step S1, adding aromatic diamine and naphthalene diamine to an organic solvent at room temperature and under nitrogen protection, stirring until completely dissolved, adding aromatic dianhydride in batches, stirring and reacting at room temperature for 9-18 hours, and then adding 4-phenylethynylphthalic anhydride for end-capping reaction for 6-10 hours to obtain an end-capped polyamic acid solution; Step S2, imidizing the blocked polyamic acid solution to obtain polyimide powder, washing with ethanol, filtering, and drying for 3-5 hours to obtain antistatic polyimide resin.

2. The method for preparing an antistatic polyimide resin according to claim 1, characterized in that: The dosage ratio of the organic solvent, aromatic diamine, naphthalenediamine, aromatic dianhydride and 4-phenylethynylphthalic anhydride is 500-600 mL: 0.11-0.17 mol: 0.11-0.18 mol: 0.285-0.295 mol: 0.0008-0.002 mol; and the dosage of naphthalenediamine is not less than 40% of the sum of the molar dosages of naphthalenediamine and aromatic diamine.

3. The method for preparing an antistatic polyimide resin according to claim 1, characterized in that: The aromatic diamine is one of 4,4'-diaminodiphenyl ether, 1,3-di(4'-aminophenoxy)benzene and 3,3',5,5'-tetramethylbenzidine.

4. The method for preparing an antistatic polyimide resin according to claim 1, characterized in that: The naphthalenediamine is one of 1,4-naphthalenediamine, 1,5-naphthalenediamine, 1,6-naphthalenediamine, 1,7-naphthalenediamine, 2,6-naphthalenediamine and 2,7-naphthalenediamine.

5. The method for preparing an antistatic polyimide resin according to claim 1, characterized in that: The aromatic dianhydride is composed of one or more of 3,3',4,4'-biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride and 2,3,6,7-naphthalenetetracarboxylic dianhydride in any proportion.

6. The method for preparing an antistatic polyimide resin according to claim 1, characterized in that: The imidization treatment: 100-200 mL of an organic solvent is added to the blocked polyamic acid solution, and the mixture is stirred and mixed. Then, a mixture of acetic anhydride and triethylamine in a volume ratio of 1:2 is added, and the mixture is reacted for 20-24 hours and then precipitated in an ethanol aqueous solution.

7. The method for preparing an antistatic polyimide resin according to claim 6, characterized in that: The organic solvent is a mixture of one or more of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone in any proportion.

8. The method for preparing an antistatic polyimide resin according to claim 1, characterized in that: The imidization treatment is: Add 100-200 mL of water-carrying agent to the blocked polyamic acid solution, heat in an oil bath at 180° C. until no water is separated from the water separator, then cool to below 60° C. and remove the solvent using a centrifuge.

9. The method for preparing an antistatic polyimide resin according to claim 8, characterized in that: The water-carrying agent is one of toluene, xylene, trimethylbenzene and dichlorobenzene.

10. An antistatic polyimide resin, characterized in that: Prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Polyimide composite material and preparation method thereof

    CN104403313A

  • Method for preparing carbon fiber-polyimide composite material

    CN104629365A

  • FPC substrate polyimide film special for LED and preparation method thereof

    CN110437615A

  • Anti-static polyimide resin and preparation method thereof

    CN116333312A

  • copolyimide

    JP1986258835A