Low-filler or filler-free construction material formulations
The integration of water-insoluble cellulose fiber gels into dry building material formulations addresses the scarcity and resource inefficiency of fillers by enhancing mortar properties and achieving standard-compliant tensile strengths, even with reduced filler content, through their role as temporary fillers and in conjunction with hydraulically setting binders and polymers.
Patent Information
- Application Number
- PCT/EP2023/059827
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-17
AI Technical Summary
Conventional dry building material formulations rely heavily on fillers, which are scarce in some regions and resource-intensive, necessitating a reduction or elimination of filler content while maintaining mortar strength and processing properties, especially in terms of tensile strength and freeze-thaw resistance.
Incorporating water-insoluble cellulose fiber gels as dispersible powders or dispersions into the formulations, which act as temporary fillers and improve mortar properties, allowing for reduced or eliminated filler content, and using hydraulically setting binders and polymers to achieve desired fresh and solid mortar characteristics.
The use of water-insoluble cellulose fiber gels enables the production of mortars with improved processing properties, long open time, and enhanced tensile strengths that meet or exceed standard specifications, including C2 and S2 standards, while reducing the need for fillers and optimizing resource efficiency.
Smart Images

Figure IMGF000025_0001 
Figure IMGF000026_0001 
Figure IMGF000026_0002
Abstract
Description
[0001] Low-filler or filler-free building material formulations
[0002] The invention relates to low-filler or filler-free dry building material formulations, polymer compositions containing polymer powder and water-insoluble cellulose fiber gels, as well as corresponding low-filler or filler-free fresh mortars and hardened mortars and their use, for example, as adhesives or coatings, in particular tile adhesives, leveling compounds, screeds or reinforcing compounds for thermal insulation composite systems.
[0003] Common dry building material formulations currently contain, in addition to mineral binders such as cement and additives, usually fillers as the main quantitative component, as described, for example, in US2013 / 0143023, US8846157 or US10239789. Mixing the dry building material formulations with water produces fresh mortar. After the fresh mortar has set, hardened mortar is obtained. An example of additives are polymers in the form of water-redispersible powders (polymer powders), which are powder compositions that are accessible by drying the corresponding aqueous polymer dispersions in the presence of protective colloids. Due to this manufacturing process, the finely divided polymer resin of the dispersion is coated with a sufficient amount of a water-soluble protective colloid. During drying, the protective colloid acts like a coating that prevents the particles from sticking together.When the polymer powder is redispersed in water, the protective colloid dissolves again in water and an aqueous dispersion of the original polymer particles is formed (Schulze J. in TIZ, No. 9, 1985).
[0004] However, fillers are a scarce or increasingly scarce commodity in some regions of the world. Furthermore, there is a growing demand for more resource-efficient, sustainable construction. Therefore, the aim is to reduce or even completely eliminate the filler content in dry building material formulations. However, the fresh mortar should, if possible, exhibit the usual processing properties, and the hardened mortar properties should also meet or, if possible, exceed the standard specifications, particularly the C2 standard according to EN 12004.
[0005] Against this background, the task was to provide dry building material formulations, fresh mortar and hardened mortar with at least a reduced filler content, whereby the fresh mortar should be easy to process, have a long open time and, in addition, the hardened mortar should have advantageous adhesive tensile strengths after freeze-thaw cycles but also in standard climates and preferably meet the C2 standard.
[0006] Surprisingly, the problem was solved with building material formulations or mortars that contained one or more water-insoluble cellulose fiber gels in the form of dispersible powders or dispersions. Such building material formulations or mortars produce the desired fresh and hardened mortar properties even when relatively large amounts of water are used for mixing. Water can act as a so-called temporary filler in the fresh mortars, which is at least partially released again during the formation of the hardened mortar and is thus ecologically sustainable. It was precisely through the use of the water-insoluble cellulose fiber gels that mortar with the desired fresh and hardened mortar properties was obtained.Conventional thickeners swell in water and have a water-retaining effect in mortars. Although they are usually used to adjust the processing properties of fresh mortars, they are not sufficient to produce workable fresh mortars in the case of filler-free or filler-free mortars. Instead, they result in fresh mortars that are too sticky and therefore unworkable. Superabsorbents also produced unstable fresh mortars that collapsed and were therefore unapplicable. Fibers have so far been used to reduce the tendency of hardened mortars to crack, but not to stabilize filler-free or filler-free fresh mortars or to regulate the water balance of fresh mortars. Conventional fibers act like fillers in fresh mortars.
[0007] The invention relates to dry building material formulations containing one or more hydraulically setting binders , one or more polymers of ethylenically unsaturated monomers in the form of water - redispersible powders ( polymer powders ) and optionally one or more additives , characterized in that
[0008] < 9 wt . -% , based on the total weight of the dry building material formulations, of fillers and one or more water-insoluble cellulose fiber gels in the form of dispersible powders.
[0009] The water-insoluble cellulose fiber gel in the form of dispersible powders has average particle sizes of preferably 0.1 to 1000 pm, particularly preferably 1 to 750 pm, and most preferably 10 to 500 pm. The average particle sizes are determined by means of laser light diffraction and laser light scattering using the LS 13320 measuring device from Beckmann-Coulter, preferably in accordance with the device manufacturer's instructions after adequate dilution of the aqueous dispersions with demineralized water.
[0010] The grain fractions described below refer to the determination method using sieve analysis according to DIN EN ISO 4610 with an air jet sieve with mesh sizes of 150 pm, 71 pm and 32 pm respectively.
[0011] The grain fraction of the water-insoluble cellulose fiber gel in the form of dispersible powders with diameters of > 150 pm is preferably < 50%, particularly preferably < 30% and most preferably < 15%.
[0012] The grain fraction of the water-insoluble cellulose fiber gel in
[0013] Form of dispersible powders with diameters of > 71 pm is preferably < 75%, more preferably < 50% and most preferably < 35%.
[0014] The grain fraction of the water-insoluble cellulose fiber gel in the form of dispersible powders with diameters of > 32 pm is preferably 5% to 95%, particularly preferably 15% to 90% and most preferably 25% to 80%.
[0015] The water-insoluble cellulose fiber gels in the form of aqueous dispersions have a viscosity of preferably 500 to 10,000 mPa.s, particularly preferably 1,000 to 5,000 mPa.s and most preferably 1,500 to 3,000 mPa.s (Brookfield viscosity, 2% dispersion in water, at 20 revolutions and 20°C (activation: 5 cm dissolver disk, 2,000 rpm, 6 min).
[0016] The fibers of the fiber gel preferably have a length of 0.1 pm to 1,000 pm, particularly preferably 0.5 pm to 750 pm, and most preferably 1 pm to 500 pm. The fibers of the fiber gel preferably have a fiber diameter of < 10 pm.
[0017] The water-insoluble cellulose fiber gel in the form of dispersible powders has a density of preferably 0.5 to 1.5 g / cm 3 , particularly preferably 0.8 to 1.3 g / cm 3 and most preferably 1.0 to 1.2 g / cm 3 (determined using a helium pycnometer) .
[0018] The water-insoluble cellulose fiber gel in the form of dispersible powders has a bulk density of preferably 200 to 1,000 g / L, particularly preferably 250 to 700 g / L (determined according to EN ISO 60).
[0019] The water-insoluble cellulose fiber gel in the form of dispersible powders has a water absorption capacity as a weight ratio of water-insoluble cellulose fiber gel to water of preferably 1 to 10 to 1 to 200, more preferably 1 to 20 to 1 to 150, particularly preferably 1 to 25 to 1 to 100 and most preferably 1 to 30 to 1 to 75. The water absorption capacity is determined by placing the water-insoluble cellulose fiber gel in the form of a dispersible powder into a paper filter moistened with water, then saturating the water-insoluble cellulose fiber gel with water by adding water and allowing excess water to drip off through the moistened paper filter.The water absorption capacity is determined as the difference between the weight of the moistened paper filter before addition of the water-insoluble cellulose fiber gel and the weight of the moistened paper filter containing the water-insoluble cellulose fiber gel saturated with water. The determination is carried out at 21 °C and 50% relative humidity.
[0020] The water-insoluble cellulose fiber gel in the form of dispersible powders has a water retention capacity of preferably 65% to 99%, particularly preferably 75% to 97%, and most preferably 80% to 95%. The water retention capacity is determined in accordance with DIN 18555, Part 7, using the filter plate method. According to the standard, the water retention capacity is the percentage of water remaining in the mortar after 5 minutes following capillary water removal through an absorbent substrate.
[0021] The cellulose of the water-insoluble cellulose fiber gel is preferably in crystalline, particularly microcrystalline form.
[0022] The water-insoluble cellulose fiber gel is present in water preferably in colloidal form or in the form of a hydrogel.
[0023] The water-insoluble cellulose fiber gel is preferably thixotropic.
[0024] The water-insoluble cellulose fiber gel is preferably based on one or more water-insoluble microcrystalline celluloses (MCCs) and one or more water-soluble dispersants. This is crucial for the fiber gel aspect. The gel is generally activated by mixing in water under the influence of shear forces. During shear activation in water, the water-insoluble MCC is dispersed, while the water-soluble dispersant is dissolved and acts as a "spacer" between the MCC particles, preventing their agglomeration.
[0025] Suitable raw materials for producing water-insoluble microcrystalline cellulose (MCC) include cellulose from natural sources such as grass, potatoes, cotton, or wood pulp, preferably rice, grain, or corn, particularly preferably in the form of straw, and most preferably wheat straw or seaweed. Water-insoluble microcrystalline cellulose (MCC) can be obtained, for example, by enzymatic treatment, steam explosion, or in particular chemical treatment of raw material and, if appropriate, mechanical comminution such as milling or grinding, if appropriate sifting, if appropriate fractionating, if appropriate compacting, if appropriate neutralizing, and if appropriate purifying. Chemical treatment is preferably carried out by treatment with mineral acids such as sulfuric acid, hydrobromic acid, or, in particular, hydrochloric acid.Such a treatment preferably involves depolymerization or hydrolysis of the raw material. Highly reactive amorphous regions are preferably hydrolyzed, releasing water-insoluble microcrystalline cellulose (MCC).
[0026] Water-soluble dispersants for the water-insoluble cellulose fiber gel include, for example, guar gum, locust bean gum, sodium alginate, carrageenan, potassium alginate, xanthan gum, tragacanth gum, karaya gum, gum arabic, agar, konjac, starch, maltodextrin, inulin, and cellulose derivatives such as carboxymethylcellulose or cellulose ethers, especially hydroxymethylcellulose, methylcellulose, and hydroxypropylmethylcellulose. Carboxymethylcellulose (CMC) and xanthan gum are preferred.
[0027] Water-insoluble microcrystalline cellulose (MCC) and water-soluble dispersants can generally be mixed in dry or aqueous form and optionally subsequently dried, for example by spray drying. The gel is generally activated by mixing in water under shear forces. Activation can be carried out beforehand or during the mixing of the dry building material formulations according to the invention.
[0028] Water-insoluble cellulose fiber gels in the form of dispersible powders are also commercially available, for example under the name Arbocel gel, in particular Arbocel P 3500 F (trade name of J. Rettenmaier).
[0029] Examples of hydraulically setting binders are cements, in particular Portland cement (CEM I), Portland slag cement (CEM II), blast furnace cement (CEM III), pozzolana cement (CEM IV), composite cement (CEM V), Portland silicate dust cement, Portland slate cement, Portland limestone cement, trass cement, slag cement, magnesia cement, phosphate cement, blast furnace cement, mixed cements (composite cements), filling cements or rapid-setting cement, or fly ash or hydraulic lime. Preferred cements are Portland cement, aluminate cement, slag cement, mixed cements and filling cements, or hydraulic lime.
[0030] Examples of fast-setting cements are aluminate cement, calcium sulfoaluminate cements and high alumina cements.
[0031] Preferred are Portland cement CEM I, Portland slag cement CEM II / AS, CEM II / BS, Portland limestone cement CEM II / A-LL, Portland fly ash cement CEM II / AV, Portland fly ash slag cement CEM II / B-SV or blast furnace cement CEM III / A, CEM III / B, CEM III / B and fast-setting cement, in particular aluminate cement.
[0032] The dry building material formulations are based on hydraulically setting binders to an extent of preferably 50 to 99 wt.%, more preferably 60 to 98 wt.%, particularly preferably 70 to 97 wt.%, most preferably 80 to 96 wt.%, and most preferably 85 to 95 wt.%, based on the total weight of the dry building material formulations. In a preferred embodiment, the dry building material formulations contain fast-setting cement, such as aluminate cement, and additionally one or more hydraulically setting binders other than fast-setting cement, in particular Portland cements. Fast-setting cement, in particular in combination with other hydraulically setting binders, is particularly advantageous for achieving the object of the invention.
[0033] The dry building material formulations are preferably based on 0 to 25 wt.%, particularly preferably 1 to 20 wt.%, and most preferably 5 to 15 wt.% of rapid-setting cement, based on the total weight of the dry building material formulations. The dry building material formulations are preferably based on 1 to 40 wt.%, particularly preferably 3 to 25 wt.%, and most preferably 5 to 15 wt.% of rapid-setting cement, based on the total weight of the hydraulically setting binders used.
[0034] Preferred dry building material formulations contain one or more retarders, particularly if they also contain fast-setting cement. Retarders are preferably selected from the group comprising saccharides, hydroxy compounds having 1 to 25 carbon atoms, carboxylic acid compounds having 1 to 25 carbon atoms or their salts, hydroxycarboxylic acid compounds having 1 to 25 carbon atoms or their salts, phosphonic acids or their salts, and phosphoric acids or their salts. Preferred salts are alkali metal, alkaline earth metal, or ammonium salts, such as sodium, potassium, magnesium, calcium, or ammonia salts. Examples of suitable carboxylic acid compounds are oxalic acid, tartaric acid, gluconic acid, heptonic acid, gallic acid, citric acid, succinic acid, sebacic acid, salicylic acid, pimelic acid, hematic acid, or malic acid. Tartaric acid, gluconic acid and citric acid are preferred.Examples of suitable hydroxy compounds are pentaerythritol, sorbitol, sucrose, glucose, fructose, or disaccharides such as sucrose. Fructose and sucrose (cane sugar) are preferred. Examples of suitable phosphonic acids or phosphoric acids or their salts are tetrasodium and tetrapotassium pyrophosphate, and sodium hexametaphosphate (Graham's salt).
[0035] Preferred retarders are hydroxycarboxylic acid compounds, phosphonic acids, or phosphoric acids, or their respective salts. Most preferred retarders are gluconic acid, tartaric acid, and citric acid, or their respective salts.
[0036] The dry building material formulations preferably contain 0.01 to 5 wt.%, particularly preferably 0.05 to 1 wt.% and most preferably 0.1 to 0.5 wt.% retarder, based on the total weight of the dry building material formulations.
[0037] The dry building material formulations can also contain one or more thickeners, for example polysaccharides such as cellulose ethers and modified cellulose ethers, cellulose esters, starch ethers, guar gum, xanthan gum, polycarboxylic acids such as polyacrylic acid and its partial esters, casein and associative thickeners. Preferred cellulose ethers are methylcellulose ethers. The thickeners are generally different from the water-insoluble cellulose fiber gels according to the invention. Any thickeners are generally present separately from the water-insoluble cellulose fiber gels according to the invention. The thickeners have molecular weights of preferably > 4000 g / mol, particularly preferably > 10000 g / mol and most preferably > 20000 g / mol. The dry building material formulations are based preferably < 5 wt. %, particularly preferably 0.1 to 3 wt. % and most preferably 0.3 to 1 wt.-% of thickeners, based on the total weight of the dry building material formulations.
[0038] Examples of fillers include quartz sand, quartz flour, calcium carbonate, dolomite, clay, chalk, hydrated lime, talc, or mica, as well as lightweight fillers such as pumice, foam glass, aerated concrete, perlite, vermiculite, and carbon nanotubes (CNTs). Quartz sand, quartz flour, calcium carbonate, chalk, or hydrated lime are preferred. Fillers preferably have a diameter of > 100 μm, especially > 1 mm.
[0039] The dry building material formulations preferably contain <5 wt.% and particularly preferably <1 wt.% fillers, based on the total weight of the dry building material formulations. Most preferably, no filler is added to the dry building material formulations. Most preferably, the dry building material formulations do not contain any filler.
[0040] Common additives for dry building material formulations include, for example, setting accelerators, fibers, water repellents, preservatives, film-forming aids, dispersants, foam stabilizers, air-entraining agents, defoamers, and flame retardants (e.g., aluminum hydroxide). For clarification, additives do not include water-insoluble cellulose fiber gels according to the invention.
[0041] Examples of fibers are natural organic fibers, in particular cotton, hemp, jute, flax, wood, cellulose, viscose, leather or sisal fibers; synthetic organic fibers, in particular viscose fibers, polyamide fibers, polyester fibers, polyacrylonitrile fibers, Dralon fibers, polyethylene fibers, polypropylene fibers, polyvinyl alcohol fibers or aramid fibers; inorganic fibers, in particular glass fibers, carbon fibers, mineral wool fibers or metal fibers. The fibers have a length of preferably 0.1 μm to 16 mm, preferably 0.5 μm to 1 mm, particularly preferably 1 μm to 500 μm. The fibers have a fiber diameter of preferably <10 μm. Fibers generally do not exist in the form of a gel in water. Fibers preferably do not swell in water. Fibers behave like a filler in the fresh mortars according to the invention. The fibers are generally different from the water-insoluble cellulose fiber gels of the invention.The dry building material formulations preferably do not contain fibers. Examples of setting accelerators are aluminum compounds, silicates, (alkali) earth hydroxides, nitrates, nitrites, sulfates, borates, or carboxylic acids. Preferred setting accelerators are aluminum salts, aluminates, alkali silicates such as water glass, alkali formates, potassium hydroxide, or calcium hydroxide (Ca(OH)2). The dry building material formulations preferably do not contain any setting accelerators.
[0042] The additives can be used in the amounts customary for this purpose, for example 0 to 25 wt.%, preferably 0.05 to 15 wt.% and most preferably 0.1 to 10 wt.%, based on the total weight of the building material dry formulations.
[0043] The dry building material formulations generally contain preferably 0.5 to 30 wt. %, more preferably 1 to 25 wt. %, even more preferably 2 to 20 wt. %, particularly preferably 3 to 15 wt. %, and most preferably 4 to 10 wt. % of polymers of ethylenically unsaturated monomers in the form of water-redispersible powders (polymer powders), in each case based on the total weight of the dry building material formulations. The polymer powders also contribute to achieving the object of the invention, particularly with regard to the hardened mortar properties.
[0044] Suitable polymers of ethylenically unsaturated monomers include, for example, those based on one or more monomers from the group comprising vinyl esters, (meth)acrylic acid esters, vinyl aromatics, olefins, 1,3-dienes, and vinyl halides, and optionally other monomers copolymerizable therewith. The polymers are preferably not crosslinked.
[0045] Suitable vinyl esters are those of carboxylic acids having 1 to 15 carbon atoms. Preferred are vinyl acetate, vinyl propionate, vinyl butyrate, vinyl 2-ethylhexanoate, vinyl laurate, 1-methylvinyl acetate, vinyl pivalate, and vinyl esters of a-branched monocarboxylic acids having 9 to 11 carbon atoms, for example VeoVa9. R or VeoVal0 R (Trade names of the company Resolution). Vinyl acetate is particularly preferred. Suitable monomers from the group of acrylic acid esters or methacrylic acid esters are esters of unbranched or branched alcohols having 1 to 15 C atoms. Preferred methacrylic acid esters or acrylic acid esters are methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, n-butyl acrylate, n-butyl methacrylate, t-butyl acrylate, t-butyl methacrylate, 2-ethylhexyl acrylate. Methyl acrylate, methyl methacrylate, n-butyl acrylate, t-butyl acrylate and 2-ethylhexyl acrylate are particularly preferred.
[0046] Preferred vinylaromatics are styrene, methylstyrene, and vinyltoluene. The preferred vinyl halide is vinyl chloride. The preferred olefins are ethylene and propylene, and the preferred dienes are 1,3-butadiene and isoprene.
[0047] If desired, 0.1 to 5% by weight, based on the total weight of the monomer mixture, of auxiliary monomers can be copolymerized. Preference is given to using 0.5 to 2.5% by weight of auxiliary monomers. Examples of auxiliary monomers are ethylenically unsaturated mono- and dicarboxylic acids, preferably acrylic acid, methacrylic acid, fumaric acid, and maleic acid; ethylenically unsaturated carboxylic acid amides and nitriles, preferably acrylamide and acrylonitrile; mono- and diesters of fumaric acid and maleic acid, such as the diethyl and diisopropyl esters, and maleic anhydride; ethylenically unsaturated sulfonic acids or their salts, preferably vinylsulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid.Further examples are pre-crosslinking comonomers such as polyethylenically unsaturated comonomers, for example diallyl phthalate, divinyl adipate, diallyl maleate, allyl methacrylate or triallyl cyanurate, or post-crosslinking comonomers, for example acrylamidoglycolic acid (AGA), methylacrylamidoglycolic acid methyl ester (MAGME), N-methylolacrylamide (NMA), N-methylolmethacrylamide, N-methylolallylcarbamate, alkyl ethers such as isobutoxy ether or esters of N-methylolacrylamide, N-methylolmethacrylamide and N-methylolallylcarbamate. Epoxy-functional comonomers such as glycidyl methacrylate and glycidyl acrylate are also suitable. Further examples are silicon-functional comonomers such as acryloxypropyltri(alkoxy)- and methacryloxypropyltri(alkoxy)-silanes, vinyltrialkoxysilanes and vinylmethyldialkoxysilanes, where ethoxy and ethoxypropylene glycol ether residues may be present as alkoxy groups.Monomers with hydroxy or CO groups may also be mentioned, for example methacrylic acid and acrylic acid hydroxyalkyl esters such as hydroxyethyl, hydroxypropyl or hydroxybutyl acrylate or methacrylate as well as compounds such as diacetone acrylamide and acetylacetoxyethyl acrylate or methacrylate.
[0048] The monomer selection or the selection of the weight fractions of the comonomers is carried out such that a glass transition temperature Tg of -25°C to +25°C, preferably -10°C to +10°C, particularly preferably -10°C to 0°C results. The glass transition temperature Tg of the polymers can be determined in a known manner using differential scanning calorimetry (DSC). The Tg can also be approximately predicted using the Fox equation. According to Fox TG, Bull. Am. Physics Soc. 1, 3, page 123 (1956), the following applies: 1 / Tg = xl / Tgl + x2 / Tg2 + ... + xn / Tgn, where xn is the mass fraction (wt. % / 100) of monomer n, and Tgn is the glass transition temperature in Kelvin of the homopolymer of monomer n. Tg values for homopolymers are listed in Polymer Handbook 2nd Edition, J. Wiley & Sons, New York (1975).
[0049] Preference is given to copolymers of vinyl acetate with 1 to 50% by weight of ethylene; copolymers of vinyl acetate with 1 to 50% by weight of ethylene and 1 to 50% by weight of one or more further comonomers from the group consisting of vinyl esters having 1 to 12 carbon atoms in the carboxylic acid radical, such as vinyl propionate, vinyl laurate, vinyl esters of alpha-branched carboxylic acids having 9 to 13 carbon atoms, such as VeoVa9, VeoValO, VeoVall; copolymers of vinyl acetate, 1 to 50% by weight of ethylene and preferably 1 to 60% by weight of (meth)acrylic esters of unbranched or branched alcohols having 1 to 15 carbon atoms, in particular n-butyl acrylate or 2-ethylhexyl acrylate; and copolymers with 30 to 75% by weight of vinyl acetate, 1 to 30% by weight of vinyl laurate or vinyl ester of an alpha-branched carboxylic acid having 9 to 11 C atoms, and 1 to 30% by weight of (meth)acrylic acid esters of unbranched or branched alcohols having 1 to 15 C atoms, in particular n-butyl acrylate or 2-ethylhexyl acrylate, which also contain 1 to 40% by weight.-% ethylene; copolymers with vinyl acetate, 1 to 50% by weight of ethylene and 1 to 60% by weight of vinyl chloride; it being possible for the polymers to also contain the auxiliary monomers mentioned in the amounts mentioned, and the data in % by weight add up to 100% by weight in each case.
[0050] Also preferred are (meth)acrylic acid ester polymers, such as copolymers of n-butyl acrylate or 2-ethylhexyl acrylate or copolymers of methyl methacrylate with n-butyl acrylate and / or 2-ethylhexyl acrylate; styrene-acrylic acid ester copolymers with one or more monomers from the group methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate; vinyl acetate-acrylic acid ester copolymers with one or more monomers from the group methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate and optionally ethylene; styrene-1,3-butadiene copolymers; where the polymers may also contain the auxiliary monomers mentioned in the amounts mentioned, and the data in wt.% add up to 100 wt.% in each case.
[0051] Most preferred are copolymers with vinyl acetate and 5 to 50% by weight of ethylene, or copolymers with vinyl acetate, 1 to 50% by weight of ethylene and 1 to 50% by weight of a vinyl ester of a-branched monocarboxylic acids having 9 to 11 C atoms, or copolymers with 30 to 75% by weight of vinyl acetate, 1 to 30% by weight of vinyl laurate or vinyl ester of an alpha-branched carboxylic acid having 9 to 11 C atoms, and 1 to 30% by weight of (meth)acrylic acid esters of unbranched or branched alcohols having 1 to 15 C atoms, which also contain 1 to 40% by weight of ethylene, or copolymers with vinyl acetate, 5 to 50% by weight of ethylene and 1 to 60% by weight of vinyl chloride. The polymers are generally prepared in an aqueous medium and preferably by the suspension or, in particular, the emulsion polymerization process—as described, for example, in DE-A 102008043988. The polymers are obtained in the form of aqueous dispersions.Common emulsifiers and / or, preferably, protective colloids can be used in the polymerization, as described in DE-A 102008043988. Thus, polymers in the form of protective colloid-stabilized aqueous dispersions are preferred. The protective colloids can be anionic or, preferably, cationic or nonionic. Combinations of cationic and nonionic protective colloids are also preferred. Preferred nonionic protective colloids are polyvinyl alcohols. Preferred cationic protective colloids are polymers that carry one or more cationic charges, as described, for example, in EW Flick, Water Soluble Resins - an Industrial Guide, Noyes Publications, Park Ridge, NJ, 1991. Preferred protective colloids are polyvinyl alcohols, especially partially saponified or fully saponified polyvinyl alcohols with a degree of hydrolysis of 80 to 100 mol%.Partially saponified polyvinyl alcohols with a degree of hydrolysis of 80 to 94 mol% and a Höppler viscosity of 1 to 30 mPas in a 4% aqueous solution (Höppler method at 20°C, DIN 53015) are particularly preferred. The protective colloids mentioned are accessible by methods known to those skilled in the art and are generally added during polymerization in a total amount of 1 to 20 wt.%, based on the total weight of the monomers.
[0052] The polymers in the form of aqueous dispersions can be converted into corresponding water-redispersible powders, as described, for example, in DE-A 102008043988. A drying aid is generally used in a total amount of 3 to 30% by weight, preferably 5 to 20% by weight, based on the polymeric constituents of the dispersion. The aforementioned polyvinyl alcohols are preferred as drying aids. Thus, polymers in the form of protective colloid-stabilized, water-redispersible powders are preferred. The dispersions can be dried, for example, by fluidized-bed drying, freeze-drying, or spray-drying. The dispersions are preferably spray-dried. Spray-drying is carried out in conventional spray-drying systems, with atomization being possible using single-, dual-, or multi-component nozzles or with a rotating disk.The outlet temperature is generally selected in the range of 45°C to 120°C, preferably 60°C to 90°C, depending on the system, the Tg of the resin, and the desired degree of drying. The viscosity of the feed to be atomized is adjusted via the solids content to achieve a value of < 500 mPas (Brookfield viscosity at 20 revolutions and 23°C), preferably < 250 mPas. The solids content of the dispersion to be atomized is preferably 30 to 75 wt.% and particularly preferably 50 to 60 wt.%.
[0053] During atomization, a content of up to 1.5% by weight of antifoam, based on the polymer, has often proven advantageous. To increase storage stability by improving blocking stability, particularly in the case of polymer powders with a low glass transition temperature, the resulting polymer powder can be treated with one or more antiblocking agents (anticaking agents), preferably 1 to 30% by weight, based on the total weight of polymeric constituents. Examples of antiblocking agents are Ca or Mg carbonate, talc, gypsum, silica, kaolins such as metakaolin, and silicates with particle sizes preferably in the range from 10 nm to 10 pm. Antiblocking agents are generally not fillers within the meaning of the present invention. Antiblocking agents are generally different from the abovementioned fillers. The abovementioned fillers preferably do not comprise antiblocking agents.
[0054] To improve the application properties, additional additives such as pigments, fillers, foam stabilizers, hydrophobizing agents or cement plasticizers can be added during drying. The invention further relates to processes for producing dry building material formulations by mixing one or more hydraulically setting binders, one or more polymers of ethylenically unsaturated monomers in the form of water-redispersible powders and, if appropriate, one or more additives, characterized in that one or more water-insoluble cellulose fiber gels in the form of dispersible powders and, if appropriate, fillers are additionally added, with the proviso that the proportion of fillers added is < 9% by weight, based on the total weight of the dry building material formulations.
[0055] Preferably no fillers are added.
[0056] The production of dry building material formulations is not tied to any particular procedure or mixing device. For example, dry building material formulations can be obtained by mixing and homogenizing the individual components of the building material formulations in conventional powder mixing devices.
[0057] The dry building material formulations according to the invention are therefore in the form of dry mixes. The dry building material formulations are generally produced without the addition of water or in the absence of water. The amount of water required for the use of the dry building material formulations is added in generally known quantities prior to application. The application mixture can be mixed and homogenized, for example, using mortar, concrete mixers, or plastering machines or stirrers.
[0058] In an alternative process for producing the dry building material formulations, premixes are first prepared from at least two components of the dry building material formulations, which are then blended with one or more other components of the dry building material formulations. Preferred premixes contain one or more water-insoluble cellulose fiber gels in the form of dispersible powders and one or more polymers in the form of water-redispersible powders.
[0059] A further object of the invention are polymer compositions obtainable by mixing one or more water-insoluble cellulose fiber gels and one or more polymers of ethylenically unsaturated monomers.
[0060] With such compositions, the object of the invention can be achieved in a particularly advantageous manner.
[0061] The invention further relates to processes for producing the polymer compositions, characterized in that one or more polymers of ethylenically unsaturated monomers and one or more water-insoluble cellulose fiber gels are mixed.
[0062] The polymer compositions are preferably in the form of aqueous dispersions and particularly preferably in the form of water-redispersible powders. It is preferred that the water-insoluble cellulose fiber gels are present or introduced in the form of aqueous dispersions and particularly in the form of dispersible powders. It is also preferred that the polymers are present or introduced in the form of aqueous dispersions and particularly in the form of water-redispersible powders.
[0063] The polymer compositions preferably contain 10 to 90 wt.%, particularly preferably 20 to 70 wt.% and most preferably 30 to 50 wt.% of water-insoluble cellulose fiber gels, based on the dry weight of the polymers of ethylenically unsaturated monomers.
[0064] The polymer compositions preferably contain > 50 wt .%, particularly preferably > 80 wt .% and even more preferably > 90 wt .% of water-insoluble cellulose fiber gels and polymers, based on the dry weight of the polymer compositions.
[0065] Furthermore, the polymer compositions may contain one or more additives, such as the above-mentioned thickeners, retarders, setting accelerators, fibers, hydrophobicizing agents, preservatives, film-forming aids, dispersants, foam stabilizers, air-entraining agents, defoamers, and flame retardants (e.g., aluminum hydroxide). For the avoidance of doubt, additives do not comprise any water-insoluble cellulose fiber gels according to the invention. Preferably, no fibers are present.
[0066] The additives may be present, for example, in an amount of 0 to 25% by weight, preferably 0.05 to 15% by weight and most preferably 0.1 to 10% by weight, based on the total weight of the polymer compositions.
[0067] Most preferably, the polymer compositions consist of water-insoluble cellulose fiber gels in the form of dispersible powders and polymers of ethylenically unsaturated monomers in the form of water-redispersible powders.
[0068] The mixing of the polymers of ethylenically unsaturated monomers and the water-insoluble cellulose fiber gels is not tied to any particular procedure or device and can be carried out in conventional mixing containers. For example, polymers in the form of aqueous dispersions are converted into water-redispersible powders by drying, and then water-insoluble cellulose fiber gels are added. The water-insoluble cellulose fiber gels are preferably added after the polymer dispersions have been dried. If desired, the water-insoluble cellulose fiber gels can be metered into the spray dryer after the polymer dispersion has been dried, optionally together with other additives that can be mixed in conventionally, such as, for example, antiblocking agents, defoamers, foam stabilizers, fillers, dyes, biocides, and thickeners.
[0069] The invention further relates to processes for producing fresh mortars by a) mixing dry building material formulations with water or b) mixing a component b1) containing one or more hydraulically setting binders, optionally one or more fillers, optionally one or more additives and optionally water with a component b2) containing one or more polymers of ethylenically unsaturated monomers in the form of aqueous dispersions, optionally one or more fillers, optionally one or more additives and optionally additionally water and optionally a component b3) containing one or more fillers and optionally water, wherein at least one of the components b1) to b3), in particular component b2), contains one or more water-insoluble cellulose fiber gels in the form of dispersible powders, and wherein a total of 0 to 9 wt.-%, based on the dry weight of the fresh mortar, of fillers are added. Preferably, no fillers are added. It is preferred that none of the components b1) to b3) contain fillers.
[0070] A further subject of the invention are fresh mortars obtainable by the aforementioned processes a) or b).
[0071] Another subject of the invention are fresh mortars based on the dry building material formulations according to the invention and water.
[0072] Preferably, 10 to 300 wt.%, more preferably 20 to 200 wt.%, even more preferably 25 to 150 wt.%, particularly preferably 30 to 100 wt.%, very particularly preferably 35 to 75 wt.%, most preferably 40 to 70 wt.%, and most preferably 45 to 60 wt.% of water are introduced, based on the total weight of the dry building material formulations or based on the dry weight of the fresh mortar. The amount of water preferably includes any water introduced by polymers of ethylenically unsaturated monomers in the form of aqueous dispersions.
[0073] Preferably, 25 to 90 wt.%, particularly preferably 40 to 80 wt.% and most preferably 60 to 70 wt.% of dry building material formulations are used, based on the total weight of the fresh mortar.
[0074] Preferably, the fresh mortars are based on 0.1 to 20 wt.%, more preferably 0.5 to 10 wt.%, particularly preferably 1 to 8 wt.% and most preferably 3.5 to 6 wt.% of polymers of ethylenically unsaturated monomers, in particular in the form of water-redispersible powders, based on the total weight of the fresh mortars.
[0075] The fresh mortar has a density of preferably 0.8 to 2.0 g / cm 3 , particularly preferably 1.0 to 1.8 g / cm 3 and most preferably 1.3 to 1.7 g / cm 3 (Determination method: pressure compensation method according to DIN 18555 Part 2).
[0076] The fresh mortar has an air void content of preferably 1 to 20%, more preferably 5 to 18%, particularly preferably 10 to 17% and most preferably 12 to 16% (determination method: pressure equalization method according to DIN 18555 Part 2).
[0077] In process alternative a), the mixing of the dry building material formulations with water is not tied to any particular procedure or mixing device and can be carried out in a conventional manner.
[0078] In the case of alternative b), 2K systems, i.e., two-component systems, are preferred. Particularly preferred are components b1) and b2) alone. Most preferably, no further components, especially no component b3), are added.
[0079] The water-insoluble cellulose fiber gels are preferably contained in components bl) and / or b2), in particular exclusively in component bl).
[0080] Water is preferably contained in components b1) and / or b2), in particular exclusively in component b2).
[0081] The production of fresh mortar according to process alternative b) is not tied to any particular procedure or mixing device. Fresh mortar can be obtained, for example, by mixing and homogenizing the individual components using mixing devices, such as mortar or concrete mixers, plastering machines, or stirrers.
[0082] In general, the fresh mortar is applied immediately after its production in a conventional manner, in particular without any further processing step.
[0083] Another object of the invention is hardened mortar obtainable by setting the fresh mortar.
[0084] After 28 days in standard climate (23°C, 50% relative humidity), the hardened mortar has a dry bulk density of preferably 600 to 1300 g / L, more preferably 700 to 1200 g / L, particularly preferably 800 to 1100 g / L and most preferably 900 to 1000 g / L (determination method: based on EN 1015-6).
[0085] The dry building material formulations, fresh mortar, or hardened mortar, are particularly suitable for the production of construction adhesives, self-leveling compounds, plasters, fillers, joint mortars, sealing slurries, or external thermal insulation composite systems. Among construction adhesives, tile adhesives, skim coats, full thermal insulation adhesives or embedding mortars, or plasters in general are preferred applications for the dispersion powder compositions. Preferred areas of application are self-leveling compounds; self-leveling floor leveling compounds and screeds are particularly preferred.
[0086] Using the procedure according to the invention, fillers can be partially or even completely dispensed with in mortars. Surprisingly, despite this considerable intervention in the mortar structure, fresh mortar and hardened mortar with the desired properties are still obtained. The fresh mortars are pliable, show advantageous flow, have low tackiness and have a particularly long open time, which is an important processing property for the user. The hardened mortars are characterized by advantageous mechanical properties, in particular they have very good adhesive tensile strengths, especially after storage in standard climatic conditions or after freeze-thaw cycles. But good values are also achieved after storage in water or heat. The hardened mortars therefore also meet the requirements of the C2 standard. The hardened mortars also achieve high tear strengths, which also meet the S2 standard.All this can be achieved with a significantly reduced polymer content compared to filler-containing formulations.
[0087] Furthermore, mortars according to the invention have a lower density than conventional mortars with standard filler quantities, which, for example, facilitates the processing of fresh mortar. Furthermore, the mortars are very economical, based on the use of the dry components.
[0088] All this is achieved by the addition of the water-insoluble cellulose fiber gels according to the invention. Water can, for example, act as a temporary filler in the mortars according to the invention, which is at least partially released again during the setting of the fresh mortar.
[0089] The following examples serve to further illustrate the invention. Preparation of the dry building material formulations:
[0090] The dry building material formulations of the (comparative) examples were prepared from the recipes given in Table 1 by intensive mixing at 23°C and 50% relative humidity.
[0091] Table 1: Recipes of the building material dry formulations:
[0092] The components of the dry building material formulations:
[0093] - Milke CEM I 52, 5R: Portland cement;
[0094] - Tylose (trade name of SE Tylose): methyl cellulose;
[0095] - VINNAPAS 5010 N (trade name of Wacker Chemie): water-redispersible, polyvinyl alcohol-stabilised vinyl acetate-ethylene copolymer;
[0096] - Arbocel (trade name of J. Rettenmaier & Söhne): water-insoluble cellulose fibre gel in the form of a dispersible powder;
[0097] - Fondue La farge (trade name of Imerys): calcium aluminate cement (quick-setting cement).
[0098] Preparation of fresh mortar:
[0099] The dry building material formulations of the (comparative) examples were mixed with the water quantities specified in Table 2 per 1000 parts by weight of the respective dry building material formulation. Table 2: Fresh mortar:
[0100] Testing the fresh mortar properties:
[0101] Determination of the open time of fresh mortar:
[0102] The open time of the fresh mortars of the (comparative) examples was determined according to EN 12004 (test standards EN 1348 and EN 1346) 30 minutes after mixing with water.
[0103] The test results are shown in Table 3.
[0104] Table 3: Open time of fresh mortar:
[0105] Example 1 according to the invention shows a significant improvement in open time compared to Comparative Examples 1 and 2.
[0106] The fresh mortar of comparative example 3 had a tough consistency, was not spreadable, could not be levelled and was therefore not workable.
[0107] Testing the hardened mortar properties:
[0108] Testing the tensile strength of the hardened mortar:
[0109] The bond tensile strength of the hardened mortars of the (comparative) examples was determined according to EN 12004.
[0110] The test results are summarized in Table 4. Table 4 : Tensile strength of the hardened mortars : a) Testing after 28 days of storage under standard climate conditions in accordance with EN 12004; b) Testing after 7 days of storage under standard climate conditions and 21 days of storage in water in accordance with EN 12004; c) Testing after 14 days of storage under standard climate conditions, 14 days of storage in heat at 70 ° C and after 1 day of storage under standard climate conditions in accordance with EN 12004; d) Testing after freeze-thaw storage in accordance with EN 12004.
[0111] The hardened mortar of Example 1 showed considerably better adhesive tensile strengths after standard storage and after freeze-thaw cycles than Comparative Example 1 and thus exceeded the requirements for a C2 adhesive.
[0112] Compared to Comparative Example 2, Example 1 also demonstrated significantly improved tensile strength after freeze-thaw cycles, even though Comparative Example 2 used twice the amount of polymer powder as in Example 1. Thus, the adhesives according to the invention also exceed the requirements for S2 adhesives.
[0113] Testing the tensile strength of the hardened mortar:
[0114] The ultimate tensile strength was determined for the hardened mortars of the (comparative) examples according to EN 12004. The measurement error for this measurement is 0.3. The results are shown in Table 5.
[0115] The mortar of Example 1 contained the same amount of polymer as Comparative Example 1 but showed much better tensile strength.
[0116] Example 1 and Comparative Example 2 gave comparable values within the scope of measurement accuracy, although in Comparative Example 2 almost twice the amount of polymer was used than in Example 1.
[0117] Table 5: Tensile strength of the hardened mortars:
Claims
Patent claims:
1. Building material dry formulations containing one or more hydraulically setting binders, one or more polymers of ethylenically unsaturated monomers in the form of water-redispersible powders and optionally one or more additives, characterized in that < 9 wt.%, based on the total weight of the dry building material formulations, of fillers and one or more water-insoluble cellulose fiber gels in the form of dispersible powders.
2. Building material dry formulations according to claim 1, characterized in that the water-insoluble cellulose fiber gel in the form of dispersible powders contains a grain fraction with diameters of > 32 pm at 5% to 95%.
3. Building material dry formulations according to claim 1 or 2, characterized in that the water-insoluble cellulose fiber gels have a viscosity of 500 to 10,000 mPa.s (determined as Brookfield viscosity, in 2% dispersion in water, at 20 revolutions and 20°C).
4. Building material dry formulations according to claims 1 to 3, characterized in that the water-insoluble cellulose fiber gels in the form of dispersible powders have a water absorption capacity as a weight ratio of water-insoluble cellulose fiber gel to water of 1 to 10 to 1 to 200.
5. Building material dry formulations according to claims 1 to 4, characterized in that the water-insoluble cellulose fiber gels in the form of dispersible powders have a water retention capacity of 65% to 99%.
6. Building material dry formulations according to claims 1 to 5, characterized in that the water-insoluble cellulose fiber gel is based on one or more water-insoluble microcrystalline celluloses and one or more water-soluble dispersants.
7. Dry building material formulations according to claims 1 to 6, characterized in that the dry building material formulations are based on 50 to 99 wt.% hydraulically setting binders, based on the total weight of the dry building material formulations.
8. Dry building material formulations according to claims 1 to 7, characterized in that the dry building material formulations contain fast-setting cement and also one or more hydraulically setting binders different from fast-setting cement.
9. A process for the production of dry building material formulations by mixing one or more hydraulically setting binders, one or more polymers of ethylenically unsaturated monomers in the form of water-redispersible powders and, if appropriate, one or more additives, characterized in that one or more water-insoluble cellulose fiber gels in the form of dispersible powders and, if appropriate, fillers are additionally added, with the proviso that the proportion of fillers added is < 9% by weight, based on the total weight of the dry building material formulations.
10. A process for the preparation of dry building material formulations according to claim 9, characterized in that no fillers are added.
11. Polymer compositions containing one or more water-insoluble cellulose fiber gels and one or more polymers of ethylenically unsaturated monomers.
12. Polymer compositions according to claim 11, characterized in that they contain > 50 wt.% of water-insoluble cellulose fiber gels and polymers of ethylenically unsaturated monomers, based on the dry weight of the polymer compositions.
13. Fresh mortar based on the dry building material formulations according to claims 1 to 8 and water, wherein the fresh mortar has a density of 0.8 to 2.0 g / cm 3 (Determination method: pressure compensation method according to DIN 18555 Part 2).
14. Hardened mortar obtainable by setting the fresh mortar according to claim 13, wherein the hardened mortar has a dry bulk density of 600 to 1300 g / L (determined according to EN 1015-6 after 28 days in standard climate at 23°C and 50% relative humidity).
15. Use of the dry building material formulations of claims 1 to 8 for the production of construction adhesives, leveling compounds, plasters, fillers, joint mortars, sealing slurries or thermal insulation composite systems.
Citation Information
Patent Citations
Fiber-containing mortar composition
DE102008043988A1
Fiber-containing concrete compositions
US10239789B2
Coating Compositions For Producing Permanently Flexible Coatings
US20130143023A1
Production of solid materials based on hydraulically setting coating agents
US8846157B2
Cellulose gel / acrylic acid series polymer composition
CN101906233A