Nitrogen fixation with water enabled by non-thermal plasma catalytic
The non-thermal plasma catalytic method using a dielectric barrier discharge reactor with a metal-based catalyst efficiently converts nitrogen and water into ammonia, addressing the energy and carbon challenges of the Haber-Bosch process and providing a sustainable ammonia production solution.
Patent Information
- Application Number
- PCT/IB2024/053603
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-17
AI Technical Summary
The ammonia production industry is energy-intensive and carbon-heavy due to the Haber-Bosch process, which requires high temperatures and pressures, and relies on fossil fuels for hydrogen production, resulting in significant greenhouse gas emissions and energy consumption, while alternative methods like electrochemistry and plasma-based production face challenges in efficiency and economic viability.
A non-thermal plasma catalytic method using a dielectric barrier discharge reactor with a metal-based catalyst, such as Co/SiC, to convert nitrogen and water into ammonia at lower temperatures and pressures, reducing energy consumption and carbon footprint by eliminating the need for hydrogen production from fossil fuels.
This method achieves a 20% conversion of nitrogen to ammonia with a production rate of at least 100 pmol/h, offering a more sustainable and economically viable alternative by integrating with renewable energy and reducing greenhouse gas emissions.
Smart Images

Figure IB2024053603_17102024_PF_FP_ABST
Abstract
Description
NITROGEN FIXATION WITH WATER ENABLED BY NON-THERMAL PLASMACATALYTICFIELD
[0001] The present invention is directed toward the production of ammonia from water and nitrogen (N2) enabled by non-thermal plasma catalytic.BACKGROUND
[0002] The ammonia industry is crucial for the global supply of food via the economical production of fertilizers, and it allows the development of catalytic chemistry and technologies with ammonia as a promising carbon-free energy carrier and transport fuel. Ammonia consists of 17.6 wt % of hydrogen, and thereby, it can be used as an indirect hydrogen storage compound. Moreover, ammonia’s energy density is approximately 4.32 kWh.L'1, showing a capacity equivalency to methanol and almost double that of liquid hydrogen.
[0003] Automobiles operating on pure ammonia and gasoline-ammonia fuel modifications have recently been hypothesized and are near to being prototyped. An important advantage of using pure ammonia is the resulting diminished reliance on fossil fuels by changing to a “sustainable fuel source” that can be manufactured synthetically. Soon synthetic low-carbon fuels will be needed as a response to the current environmental emergency, and ammonia is among such synthetic fuels. Short-term storage such as batteries can be buffered by long-term energy storage molecules with high energy content and density like ammonia.
[0004] The massive production of ammonia remains heavily dependent on the capital and energy- intensive Haber-Bosch (HB) process, which secures around 500 million tons of ammonia produced annually. In the HB route, a mixture of hydrogen (H2) and nitrogen gas (N2) is passed over an ironbased catalyst promoted with K2O and AI2O3. Given the exothermic nature of N2 reduction, it requires a temperature of 300-500 °C to improve the kinetics and a pressure of 150-200 atm to shift the reaction equilibrium to be in favor of the ammonia product.
[0005] Ammonia production via the H-B process is highly energy-and cost-consumption partially due to the hydrogen source derived from highly endothermic natural gas reforming. Steam reforming of coal or natural gas such as methane (CH4) provides the inlet hydrogen stream for ammonia production via the H-B process leading to around 1.87 tons of the greenhouse gas CO2 released per ton of ammonia. A single pass results in a conversion efficiency of only 15% for both N2 and H2. Therefore, recycling of unreacted synthesis gas is often required to achieve an overall 97% conversion efficiency.
[0006] Despite such high conversion efficiency, the HB route with recycled gas remains energy intensive, and the entire process scheme needed to achieve reaction conversion of 97% is complex. The HB accounts for about 1% of global greenhouse gas emissions and is responsible for approximately 1.4% of global energy consumption. These values increase further if CO2 emissions associated with the reforming of natural gas such as CH4 to produce H2 are included.
[0007] Ammonia can also be produced from other processes such as electrochemistry, biochemistry, photochemistry, and plasma. Biochemistry retains its very fundamental progress and photochemistry displays very low efficiency, electrochemistry and plasma for ammonia production are mostly studied.
[0008] The use of H2O as a H2 source in the synthesis of ammonia is undoubtedly a promising approach in a sustainable and economical way of electrochemical process. Suitable synergy between the electrode and electrolyte is required to secure the system feasibly and applicably. It is also important to note that the limited development of electrochemical-mediated ammonia synthesis is due to the challenge in using proper controls, standards, and experimental methods to definitively prove that ammonia is truly synthesized by N2 reduction. Although several detailed protocols for proof of genuine electrochemistry have been reported; nonetheless, the majority of the recent reports are unable to meet the mandatory requirement to qualify as reliable results. Detailed assessment of the current state of electrochemistry is fraught with visible difficulties owing to several issues in the experimental methods and results presentation.
[0009] Non-thermal plasma (NTP)-assisted ammonia synthesis from N2 and H2 have been intensively reported over the last few decades and many studies have demonstrated that ammonia can be produced at low temperature (400-500 K) and atmospheric pressure when NTP is in tandem with a catalyst. Unlike the H-B process where the commercial iron-based catalyst is hard to be replaced or developed further at least soon, the complexity of plasma and catalyst that can alterammonia production significantly opens huge rooms for catalyst development to bring plasma catalytic ammonia production to the industrial level.
[0010] The ability to activate N2 at mild conditions enables small-scale, decentralized fertilizer and / or energy carrier vehicle production compatible with intermittent renewable energy. It can be said that we could make ammonia when the sun is shining, or the wind is blowing. Life cycle assessments have predicted that efficient plasma technologies would be more sustainable than the conventional fixation, particularly when integrating with renewable energy.
[0011] The favorable sustainability, nonetheless, cannot be translated to economic competitiveness given the large carbon footprint of natural gas reforming for H2 feed production. Several research groups have recently investigated plasma-driven ammonia production from N2 and H2O. Nevertheless, a low NIL production rate is still challenging.
[0012] The use of ultrapure H2 feed and large centralized production plants still challenges economic viability. Hydrogen is exclusively derived from the reforming of fossil hydrocarbons, and mostly CH4, resulting in annual CO2 emissions of 300 Mt (around 1.5% of greenhouse gas emissions. The energy cost of H2 production originates from the energy-intensive methane reforming processes operated at 800-10000C. The produced H2 also needs to be stored and transported, posing safety concerns, and high downstream costs. The current world is preferably shifting to low-or even zero-carbon emission processes, allowing for the removal of any emissions, particularly those from manufacturing.
[0013] Because of the foregoing, it would be advantageous to provide a process for direct ammonia production from H2Oand N2 is more beneficial than such combination technologies and even with a combination between water splitting and ammonia production, at least by eliminating H2 production step from these endothermic processes and complexed cooling, compression, and separation units, which required to separate and convey produced H2 for subsequent ammonia production step. Chemical production processes with less equipment investments and lower total energy consumption are undoubtedly in high demand of development.
[0014] The utilization of methane, the principal component of natural gas, as an alternative H2 source can be applied for N2 fixation can produce extra value-added products that can compensate for the cost.
[0015] Dielectric barrier discharge (DBD) non-thermal plasma (NPT) which can provide highly energetic species is a good candidate for activating H2O and N2 to ammonia and other value-added products.BRIEF SUMMARY
[0016] In accordance with embodiments described herein, a method of ammonia production from H2O and N2 enabled by NTP catalytic. The method comprises introducing the H2O and N2 feedstock to a DBD plasma reactor in the presence of a metal-based catalyst structure, where the metal-based catalyst structure comprises a metal loaded or present on support structure, such as, but not limited to a silica support structure. The method reported herein is able to convert at least 20 % of N2 to ammonia at a production rate of at least 100 pmol.tr1(3% yield) from the feedstock.
[0017] The above and still further features and advantages of the present invention will become apparent upon consideration of the following detailed description of specific embodiments thereof.
[0018] In a first aspect of the invention is provided a method for ammonia production comprising the steps of:(i) providing a first feedstock comprising N2 gas;(ii) providing a second feedstock comprising H2O;(iii) providing a reaction chamber comprising a metal-based catalyst;(iv) submitting the first feedstock of step (i) and the second feedstock of step (ii) to said reaction chamber;(v) subjecting the first and second feedstock to plasma in the reaction chamber comprising said metal-based catalyst, thereby forming ammonia; wherein the reaction chamber is a non-thermal plasma reactor and / or the plasma is a non-thermal plasma.
[0019] In another aspect, the invention provides a method for ammonia production further comprising a regeneration process of a metal-based catalyst, wherein the regeneration process comprises:a. rinsing the metal-based catalyst with a regeneration liquid, preferably the regeneration liquid comprises a polar organic solvent and most preferably the regeneration liquid comprises a polar organic solvent selected from acetone, propanol, ethyl acetate, methyl ethyl ketone and combinations thereof; b. optionally drying the metal-based catalyst obtained in step a.; c. calcining the metal-based catalyst to a temperature between 300 to 600 °C, preferably between 350 to 500 °C, preferably for at least 2 hour (at least 3 hours), and / or in an atmosphere comprising or consisting of H2 and Ar, preferably wherein the atmosphere is provided as a gas flow having a flowrate of 100 to 200 mL / min; thereby regenerating the metal-based catalyst.
[0020] In another aspect, the invention provides a catalyst for ammonia production, preferably ammonia production using a non-thermal plasma reaction process comprising: a support structure; and a metal from the group consisting of Cu, Co, Zn, Mn, Y, Fe, Ru, Pd, Os, Ir, Pt or combinations thereof (preferably Co), wherein the metal is present on the support structure; and wherein the metal-based catalyst has a pellet form.
[0021] In another aspect, the invention provides a metal-based catalyst obtainable by a wet impregnation method, preferably using a water-soluble precursor of said metal.
[0022] In another aspect, the invention provides a dielectric barrier discharge plasma reactor for ammonia production comprising: a reaction chamber comprising a structure of metal-based catalyst particles; a first supply to the reaction chamber; a second supply to the reaction chamber; wherein the first supply and second supply to the reaction chamber are in a counter-current configuration, wherein preferably the metal-based catalyst particles are the catalyst particles as described herein.
[0023] In another aspect, the invention provides a method for non-thermal plasma ammonia production using N2 gas and a second feedstock source characterized in that the conditions of non- thermal plasma include at least one, preferably two and most preferably three of the following conditions:• a frequency between 5 to 60 kHz;• a pressure between 0.5 to 2 atm;• a reaction temperature between 200 to 600 k; wherein the method is carried out using the dielectric barrier discharge plasma reactor as described herein.BRIEF DESCRIPTION OF THE DRAWINGS
[0024] FIG. 1 depicts a plot of simulated plasma-assisted ammonia production from H2O and N2 as described herein. 1 -Dielectric barrier discharge plasma reactor, 2-reservoir for second supply source, 3-pump, 4-quartz tube reactor, 5-ground electrode, 6-reservoir for first supply source, 7- cold trap, 8-TAN, 9-Micro-GC, 10-Optical Emission Spectroscopy (OES), 11 -plasma generator, 12-Oscilloscope, 13-high voltage electrode, 14-high voltage probe, 15-voltage probe, 16-current probe.DETAILED DESCRIPTION
[0025] In the following detailed description, while aspects of the disclosure are disclosed, alternate embodiments of the present disclosure and their equivalents may be devised without parting from the spirit or scope of the present disclosure. It should be noted that any discussion herein regarding “one embodiment”, “an embodiment”, “an exemplary embodiment”, and the like indicate that the embodiment described may include a particular feature, structure, or characteristic and that such feature, structure, or characteristic may not necessarily be included in every embodiment. In addition, references to the foregoing do not necessarily comprise a reference to the same embodiment. Finally, irrespective of whether it is explicitly described, one of ordinary skill in the art would readily appreciate that each of the particular features, structures, or characteristics of thegiven embodiments may be utilized in connection or combination with those of any other embodiment discussed herein.
[0026] Various operations may be described as multiple discrete actions or operations in turn, in a manner that is most helpful in understanding the claimed subject matter. However, the order of description should not be construed to imply that these operations are necessarily order-dependent. In particular, these operations may not be performed in the order of presentation. Operations described may be performed in a different order than the described embodiment. Various additional operations may be performed and / or described operations may be omitted in additional embodiments.
[0027] For the present disclosure, the phrase “A and / or B” means (A), (B), or (A and B). For the present disclosure, the phrase “A, B, and / or C” means (A), (B), (C), (A and B), (A and C), (B and C), or (A, B and C).
[0028] The singular forms “a”, “an”, and “the” as used herein should be construed to include plural referents unless the content clearly dictates otherwise. It should also be noted that the term “or” is generally employed in its broadest sense, that is as meaning “and / or” unless the content clearly dictates otherwise.
[0029] The terms “comprising”, “including”, “having” and the like, as used with respect to embodiments of the present disclosure, are synonymous. Such expressions should be construed in an open, inclusive sense, meaning that the embodiment described includes the recited features, but that it does not exclude the presence of other features, as long as they do not render the embodiment unworkable.
[0030] The terms “about”, “approximately”, “substantially” and the like, as used with respect to embodiments of the present disclosure indicate that the value or range is interpreted as being as accurate as the method used to measure it. Where such terms are applied to a structural unit the expression containing the terms is to be interpreted as a technical feature being produced within the technical tolerance of the method of manufacture.
[0031] Whenever reference is made throughout this document to a compound which is a salt, this should be construed to include the anhydrous form as well as any solvates (in particular hydrates) of this compound.
[0032] The term ‘residence time’ is to be interpreted as the reactor volume divided by the volumetric flow rate thus giving the total time that the material has spent inside the reactor. As will be understood by those skilled in the art, where there are multiple inflows or outflows, then the sum of the outflows or inflows is used to determine the residence time.
[0033] In accordance with the invention, the BET surface area as referred to herein is determined at a temperature of 77K using a sample of 0.1-0.5g. The BET surface area as referred to herein is determined using nitrogen. A preferred analysis method to determine the BET surface area comprises heating samples to 400 °C for a desorption cycle prior to surface area analysis. A suitable and thus preferred analysis apparatus for determining the BET surface area is a Micromeritics Gemini VII 2390 Surface Analyzer preferably equipped with a Micromeritics FlowPrep 060 flowing-gas degassing unit.
[0034] In accordance with the invention, particle size distribution as referred to herein was determined by transmission electron microscopy (STEM) analysis performed using theFEI Tecnai F20 system with a Field emission gun (FEG) operating at 200 kV, accompanied by a 4k Gatan CCD camera. A preferred analysis method to determine the particle size distribution comprises placing approximately 0.05 g of the sample dispersed in ethanol and supported on holey carbon placed on a 200 mesh Cu grid, and subsequently capturing the images. High-resolution transmission electron microscope (HRTEM) images were acquired for the fresh and spent Ir / GaN samples. This analysis took place on the FEI Talos F200X, a high-resolution scanning / transmission electron microscope operational within the range of 80 to 200 kV. The microscope was equipped with a high-angle annular dark field (HAADF) detector for Z contrast imaging, as well as a Super X-EDX detector for compositional analysis.
[0035] In accordance with the invention, the particle size distribution characteristics of the metal on the support structure of the catalyst are determined by transmission electron microscopy energy- dispersive x-ray (TEM-EDX).
[0036] For the purposes of the present disclosure, the ideal gas law is assumed such that the vol% of a gas is considered as equal to the mol%.
[0037] The importance of using alternative feedstocks to ultrapure H2 for ammonia production has been previously noted herein. In accordance with example embodiments described herein,processes are described for effective ammonia production from H2O and N2 and utilizing a suitable metal-based catalyst and NTP. As described herein, a metal-based catalyst structure is provided in the ammonia production process that comprises a metal loaded or present on a support structure. The presence of the specified metal-based catalyst, preferably including Co, enhances the activation of N2, particularly under synergisms of catalyst and plasma regime.
[0038] Figure 1 illustrates an exemplary reactor (1) which can be used for the production of ammonia as described herein. The reactor comprises a reservoir for the first supply source (6) and a second reservoir for the second supply source (2) which are introduced into the plasma reactor. The pump (3) is used to control the flow rate and pressure of the supply source to the reactor. The reactor comprises a quartz tube reactor (4) which forms the main chamber of the plasma reactor. The plasma generator (11) is responsible for generating the dielectric barrier discharge plasma within the quartz reactor by creating an electric field using both the ground electrode (5) and the high voltage electrode (13). During operation, Optical Emission Spectroscopy (OES) (10) is used to analyse the light emitted by plasma and provides information about the excited species present in the plasma and their concentrations. Similarly, the oscilloscope (12) is used to monitor the characteristics of the electrical discharge (e.g. voltage, current waveforms) and control the plasma generation process. The cold trap (7) is used to capture and condense any vaporized or gaseous products that are formed during the plasma treatment. The reaction products can thus be analysed by micro-GC (9) and / or by the Total Acid Number TAN (8) to determine the acidity of the reaction products or residual materials.Method for Ammonia Production
[0039] In a first aspect of the invention is provided a method for ammonia production comprising the steps of:(i) providing a first feedstock comprising N2 gas;(ii) providing a second feedstock comprising H2O;(iii) providing a reaction chamber comprising a metal-based catalyst;(iv) submitting the first feedstock of step (i) and the second feedstock of step (ii) to said reaction chamber;(v) subjecting the first and second feedstock to plasma in the reaction chamber comprising said metal-based catalyst, thereby forming ammonia; wherein the reaction chamber is a non-thermal plasma reactor and / or the plasma is a non-thermal plasma.
[0040] In preferred embodiment, in step (v) in the non-thermal plasma reactor ionized N2 gas is created within a relatively low-temperature reactor by applying an electric field.
[0041] In preferred embodiments, the second feedstock provided in step (iii) is gaseous. The second feedstock is thus provided as water vapour.
[0042] In other embodiments, the second feedstock provided in step (iii) is liquid.
[0043] In highly preferred embodiments of the invention, the second feedstock comprising H2O is not seawater.
[0044] In preferred embodiments, the volume ratio of N2 gas of the first and H2O of the second feedstock provided in step (iii) is at least 1: 1 respectively, preferably at least 1:2 respectively, preferably at least 1:3 respectively, preferably at least 1 :4 respectively, preferably at 1:5 respectively. In highly preferred embodiments, the volume ratio of N2 gas of the first and H2O of the second feedstock provided in step (iii) is at least 1 :1 respectively, preferably at least 1:2 respectively, preferably at least 1:3 respectively, preferably at least 1:4 respectively, preferably at 1:5 respectively. In said preferred embodiments, the H2O of the second feedstock is preferably provided as a vapour.
[0045] In other embodiments the volume ratio oflS gas of the first and H2O of the second feedstock is at least 10: 1, preferably at least 50: 1, more preferably at least 100:1, even more preferably at least 150:1 and most 200: 1 respectively. In some embodiments, the feed flowrate of the first feedstock is at least 10 seem and the feed flowrate of the second feedstock is at least 0.1 seem. In some embodiments, the volume ratio of N2 gas of the first and H2O of the second feedstock is at least 10:1, preferably at least 50:1, more preferably at least 100: 1, even more preferably at least 150: 1 and most 200:1 respectively. In said preferred embodiments, the H2O of the second feedstock is preferably provided as a liquid.
[0046] In other embodiments the volumetric flow rate of N2 gas of the first and H2O of the second feedstock is at least 10: 1, preferably at least 50:1, more preferably at least 100:1, even more preferably at least 150:1 and most 200: 1 respectively. In some embodiments, the feed flowrate of the first feedstock is at least 10 seem and the feed flowrate of the second feedstock is at least 0.1 seem. In some embodiments, the volumetric flow rate of N2 gas of the first and H2O of the second feedstock is at least 10: 1, preferably at least 50:1, more preferably at least 100:1, even more preferably at least 150:1 and most 200:1 respectively. In said preferred embodiments, the H2O of the second feedstock is preferably provided as a liquid.
[0047] In preferred embodiments, step (v) of the method is conducted at temperatures between 150 to 500 K, preferably between 200 to 450 K, even more preferably between 250 and 400 K and most preferably between 275 and 350 K. In some embodiments, step (v) of the method is conducted at temperatures between 150 to 700 K, preferably between 200 to 600 K, more preferably between 250 to 500 K.
[0048] In some embodiments, step (v) is conducted at a plasma power of at least 2 W, preferably at least 3 W, even more preferably at least 4 W, even more preferably at least 5 W, even more preferably at least 6W and most preferably at least 7 W. Step (v) is conducted at plasma powers in the range of 2 to 12 W, preferably in the range of 4 to 11W, even more preferably in the range of 6 to 10 W and most preferably in the range of 7 to 8 W. In some embodiments, step (v) is conducted at a plasma power of at least 1 W / pg(NI h), preferably at least 2 W / pg(NI h), more preferably at least 3 W / pg(NI h) and most preferably at least 4 W / pg(NI h).
[0049] In some embodiments, step (v) is carried out in the reaction chamber which is configured as batch, fixed-bed continuous flow or moving bed mode.
[0050] The method described herein results in a conversion of at least about 5 % N2, preferably at least 10% N2, preferably at least 16% N2, preferably at least 20 %. The process described herein results in an ammonia production rate of at least 1 pmol.h'1, preferably at least 10 pmol.h'1, more preferably at least 50 pmol.h'1, even more preferably at least 100 pmol.h'1. The process described herein results in an ammonia production rate of at least 150 pmol.h'1, preferably at least 200 pmol.h'1, preferably at least 250pmol.tr1and most preferably at least 300 pmol.h'1. The process described herein results in preferred embodiments in NH4NO3 production, preferably of at least0.1 mM.1T1, preferably at least 0.2 mM.h'1, preferably at least 0.5 mM.h'1, preferably at least 0.54 mM.h'1, preferably at least 0.6 mM.h'1which is competitive with that achieved from plasma- assisted ammonia production from hydrogen and nitrogen.
[0051] In preferred embodiments, the energy yield for ammonia is at least 0.01 g.kWh^g'1, preferably at least 0.02 g.kWh^g'1, more preferably at least 0.05 g.kWh^g'1, and most preferably at least 0.07 g.kWh^g'1. In preferred embodiments, the energy yield for ammonia is at least 0.08 g.kWh^g'1, preferably at least 0.1 g.kWh^g'1, preferably at least 0.2 g.kWh^g'1, even more preferably at least 0.5 g.kWh^g'1and most preferably at least 0.7 g.kWh^g'1.
[0052] In preferred embodiments, the residence time of step (v) in the reaction chamber is at least 0.1 seconds, preferably at least 1 minute, even more preferably at least 10 minutes and most preferably at least 30 minutes.
[0053] Any N2 fixation with other feedstocks can be promoted and beneficial from the ammonia production process described herein.
[0054] In a different aspect of the invention is provided a regeneration process of a metal-based catalyst comprising: a. rinsing the metal-based catalyst with a regeneration liquid, preferably the regeneration liquid comprises a polar organic solvent and most preferably the regeneration liquid comprises a polar organic solvent selected from acetone, propanol, ethyl acetate, methyl ethyl ketone and combinations thereof; b. optionally drying the metal-based catalyst obtained in step a. ; c. calcining the metal-based catalyst to a temperature between 300 to 600 °C, preferably between 350 to 500 °C, preferably for at least 2 hour (at least 3 hours), and / or in an atmosphere comprising or consisting of H2 and Ar, preferably wherein the atmosphere is provided as a gas flow having a flowrate of 100 to 200 mL / min; thereby regenerating the metal-based catalyst provided in step (iii).
[0055] Metal-based catalyst structures as described herein can also be regenerated, either before or after a period of use, to enhance the performance of the catalyst structure. The regeneration process comprises rinsing the metal-based catalyst with acetone and drying in the air to remove acetone (e.g., drying at 100 °C to about 200 °C, e.g., about 150 °C, for at least 1 hour, e.g., about 3 hoursor greater), and calcination (heating in the air) at a temperature of at least about 400 °C for a sufficient period of time, e.g., at least about 2 hours (e.g., about 3 hours or greater) in a mixture of FF / Ar with a flowrate in range of 100 to 200 mL / min. The regeneration process can also be repeated any number of times depending upon a particular application. For a metal-based catalyst structure that has been used, e.g., in a plasma-assisted process for ammonia production, the regeneration process (e.g., single regeneration, twice regeneration, etc.) can be used to regenerate or refresh the metal-based catalyst structure such that its performance is enhanced in relation to the performance of the metal-based catalyst structure before the regeneration process. In particular, the performance of the catalytic reaction for the metal-based catalyst structure can improve when subjected to a regeneration process and after the metal-based catalyst structure has been used in long-term industrial applications. While not bound by any theory, the active catalytic sites in the metal-based catalysts may be further activated during the regeneration process. In the regeneration process, metal migration may take place to achieve a better dispersion, resulting in improved catalytic performance. The regeneration process can be repeated a plurality of times (e.g., regenerated twice, regenerated three times, etc.) for a particular application to enhance the catalytic performance of the metal-based catalyst structure.Metal-based Catalyst for Ammonia Production
[0056] In a different aspect of the invention is provided a metal-based catalyst for ammonia production, preferably ammonia production using a non-thermal plasma reaction process comprising:• a support structure; and• a metal selected from the group consisting of Cu, Co, Zn, Mn, Y, Fe, Ru, Pd, Os, Ir, Pt or combinations thereof, preferably the metal is selected from of Cu, Co, Zn, Mn or combinations thereof, preferably the metal is Co, wherein the metal is present on the support structure; and wherein the metal-based catalyst has a pellet form.
[0057] As will be understood by those skilled in the art, the advantages of pelletized catalysts include an improved mass transfer, reduced catalyst attrition, improved ease of handing and facile scalability for industrial purposes.
[0058] Metal-based catalysts which are considered to be of a particular utility in the context of the present invention, are described in CN202310394220A, the contents of which are incorporated herein by reference. According to CN202310394220A, some metal -based catalysts suitable for the non-thermal plasma production of ammonia include those comprising a Cu,Zn or Ag metal, loaded or present on a support material (or support structure) such as AI2O3, SiCh, TiCh, Zeolites, Y molecular sieves and ZSM-5 molecular sieves. The methods of preparation of such catalysts are also incorporated herein. Furthermore, the metal-based catalysts disclosed in CN202310394220A and which are incorporated by reference, can be utilized in a pellet form.
[0059] In preferred embodiments, the support structure of the metal-based catalyst comprises or consists essentially of a material is selected from AI2O3 , SiCh , TiCh , Y-molecular sieves and ZSM-5 molecular sieves.
[0060] In some embodiments, the support structure is a zeolite, commonly used zeolites in non- thermal plasma applications include ZSM-5, Beta zeolite (BEA), Y zeolite (FAU), mordenite (MOR), SAPO-34, FER zeolite (FER), ZSM-22 or combinations thereof and which may be used as support structures in the metal-based catalyst.
[0061] In preferred embodiments, the support structure of the metal-based catalyst, preferably the SiO2 support structure, has a BET surface area in the range of 100 and 250 m2 / g, preferably in the range of 120 m2 / g and 200 m2 / g, preferably in the range of 150 m2 / g and 175 m2 / g. In some embodiments, the support structure of the metal-based catalyst, preferably the SiO2 support structure, has a BET surface area in the range of 50 to 500 m2 / g, preferably in the range of 100 to 400 m2 / g, more preferably in the range of 150 to 350 m2 / g.
[0062] In preferred embodiments, the metal-based catalyst has a BET surface area in the range of 100 and 250 m2 / g, preferably in the range of 120 m2 / g and 200 m2 / g, preferably in the range of 150 m2 / g and 175 m2 / g.
[0063] In preferred embodiments, the support structure of the metal-based catalyst has particles with one, preferably two and most preferably three of the following characteristics:• a diameter between 0.5 and 3.0 mm, preferably between 1.0 and 2.5 mm and more preferably between 1.0 and 2.0 mm;• a length between 2 and 10 mm, preferably between 4 and 6 mm and most preferably between 3 and 5 mm;• a specific surface area between 50 and 450 m2 / g, preferably between 100 and 400 m2 / g, even more preferably between 150 and 350 m2 / g.
[0064] In preferred embodiments, the metal-based catalyst has particles with one, preferably two and most preferably three of the following characteristics:• a diameter between 0.5 and 3.0 mm, preferably between 1.0 and 2.5 mm and more preferably between 1.0 and 2.0 mm;• a length between 2 and 10 mm, preferably between 4 and 6 mm and most preferably between 3 and 5 mm;• a specific surface area between 50 and 450 m2 / g, preferably between 100 and 400 m2 / g, even more preferably between 150 and 350 m2 / g.
[0065] In highly preferred embodiments, the support structure of the metal-based catalyst has a substantially uniform cylindrical morphology.
[0066] A metal-based catalyst structure that has been determined to be very useful in ammonia production and for methane conversion comprises a silica support structure loaded with Co. The choice of the particular metal species provided in the metal-based catalyst for plasma-assisted ammonia process was achieved as a result of careful analysis based upon the specific N2 conversion as well as how Co metal species behave in the metal-based catalyst structure for a particular plasma-driven ammonia production process. A series of Co / SiCh catalysts with controlled metal loading of 1 wt.% have been developed to activate H2O and N2 to ammonia. It has been determined unexpectedly that the presence of the Co / SiCh in the plasma described herein provides a synergistic effect in conversion of H2O and N2 to ammonia.
[0067] In preferred embodiments, the mass content of the metal in the metal-based catalyst is between 0.1 wt.% and 25 wt.%, preferably between 0.5 wt.% and 15 wt.%, and even more preferably between 0.5 wt.% and 7.5 wt.% by total mass of the metal-based catalyst. In otherembodiments, the mass content of the metal in the metal-based catalyst is between 0.1 wt.% and 25 wt.%, preferably between 0.5 wt.% and 15 wt.%, and even more preferably between 0.5 wt.% and 7.5 wt.% by total mass of the support structure.
[0068] The metal-based catalyst described herein can be synthesized by using the wet impregnation method. In such embodiments, the metal-based catalyst as described herein elsewhere is obtainable by a wet impregnation method, preferably using a water-soluble precursor salt of said metal. The SiCh support in extruded cylinder form can be ordered commercially. The SiCh material can further have a BET surface area in the range of 120 m2 / g and 200 m2 / g.
[0069] In example embodiments, the metal-based catalyst support structure has a uniform cylindrical morphology, such as a uniform Co nanoparticle morphology. The Co / SiCh catalyst structure has a surface area of 100 to 150 m2 / g, a pore volume of 0.3 to 0.8 mL / g. Thus, in some embodiments, the metal-based catalyst has a BET surface area between 50 and 200 m2 / g, preferably a BET surface area between 75 and 150 m2 / g. The Co nanoparticle has a smooth surface and a narrow particle size distribution, preferably in the range of 10 to 100 nm, more preferably in the range of 20 to 80 nm, even more preferably within the range of 30 to 70 nm.
[0070] In some embodiments, the metal-based catalyst has one, preferably two, and even more preferably three of the following characteristics:• a BET surface area between 50 and 200 m2 / g, preferably BET a surface area between 100 and 150 m2 / g;• a pore volume between 0.1 to 1 mL / g, preferably between 0.5 to 0.8 mL / g;• a particle size distribution between 2 to 50 nm, preferably between 2 to 10 nm of the metal being present in the catalyst.
[0071] Metals, alternative or in addition to Co, that can also be selected and provided in the support structure include silver (Ag), zinc (Zn), cobalt (Co), nickel (Ni), cerium (Ce), Copper (Cu), Manganese (Mn), Yttrium (Y), Iron (Fe), Ruthenium (Ru), Palladium (Pd), Osmium (Os), Iridium (Ir) and Platinum (Pt) and any combinations thereof. Each metal dopant or the combination of metal dopants can be provided within the metal-based catalyst structure (e.g., in metal or metal oxide form) in various amounts. For example, Co can be provided in the catalyst support in an amount from about 5 wt%. It is noted that the term weight percentage (wt%) of metal within acatalyst structure, as described herein, refers to the mass of a particular metal element divided by the mass of the catalyst support (i.e., the mass of the catalyst support material before metal loading, such as the weight of a SiCh support material) and then multiplied by 100 (to obtain a percentage value).
[0072] The support structure comprising a SiCh material can be doped with a suitable amount of Co metal in the following manner. Metal salt can be dissolved in deionized water to form an aqueous solution of a metal precursor at a suitable concentration within the solution. Metal precursor salt that can be used to form the catalyst structure includes, without limitation, chlorides, nitrates, and sulfates. The metal precursors in the solution are then loaded into the porous support material to achieve a desired amount of metal within the catalyst structure. Any suitable loading process can be performed to load metals within the support material. Some non-limiting examples of metal loading processes include impregnation, where an active metal precursor is first dissolved in an aqueous or organic solution, the metal-containing solution is then added to catalyst support and the solvent is then removed by evaporation.
[0073] Depending upon the loading process, the resultant metal-loaded catalyst structure can be dried at a temperature between about 60 °C to about 80 °C for a period of time between about 2 hours to about 24 hours. The dried catalyst structure can then be subjected to calcination under a mixture of 5%H2 / Ar with a flowrate from 100 to 200 mL / min at a temperature ranging from about 300 °C to about 700 °C and at a suitable ramped or stepped increased heating rate (e.g., heating rate increases the temperature at about 3°C / min to about 10 °C / min), where such calcination temperatures, times and heating rates can be modified depending upon the type or types of metals doped into the catalyst structure as well as reaction conditions associated with the use of the catalyst structure.
[0074] The resultant metal-loaded catalyst structure is suitable for use in plasma-assisted ammonia production from H2O and N2 (and / or other N2 fixation or CH4 conversion processes) under several different types of operational conditions. The catalyst structure can be utilized, e.g., for H2O conversion, ammonia production, and / or another hydrocarbon conversions in a number of different types of reactor systems including, without limitation, batch reactor systems, continuous tubular reactors (CTR), continuous stirred-tank reactors (CSTR), semi-batch reactors, varying catalyticreactors such as fixed bed, trickle-bed, moving bed, rotating bed, fluidized bed, slurry reactors, a non-thermal plasma reactor, and any combinations thereof.Dielectric Barrier Discharge Plasma Reactor for Ammonia Production
[0075] In a different aspect of the invention is provided a dielectric barrier discharge plasma reactor for ammonia production comprising: a reaction chamber comprising a structure of metal-based catalyst particles; a first supply to the reaction chamber; a second supply to the reaction chamber; wherein the first supply and second supply to the reaction chamber are in a counter-current configuration wherein the metal-based catalyst particles are the catalyst as described herein.
[0076] In some embodiments of the invention, the dielectric barrier discharge plasma reactor is provided wherein the reaction chamber is a fluidized bed plasma reactor and / or the structure of metal-based catalyst particles is a fluidized bed.
[0077] In some embodiments of the invention, the dielectric barrier discharge plasma reactor is provided wherein the first supply to the reaction chamber is a gas and the second supply to the reaction chamber is a liquid. In such embodiments, the first supply to the reaction chamber is preferably N2 gas whilst the second supply to the reaction chamber is H2O. The second supply to the reaction chamber can either be gaseous or liquid.Method of Operating the Dielectric Barrier Discharge Plasma Reactor for Ammonia Production
[0078] In a different aspect of the invention is provided a method for non-thermal plasma ammonia production from N2 gas and a second feedstock source characterized in that the conditions of non- thermal plasma include at least one, preferably two of the following conditions: a frequency between 5 to 60 kHz;a pressure between 0.5 to 2 atm;
[0079] a reaction temperature between 300 to 600 K.In a different aspect of the invention is provided a method for non-thermal plasma ammonia production from N2 gas and a second feedstock source characterized in that the conditions of non-thermal plasma include at least one, preferably two of the following conditions: a frequency between 5 to 60 kHz; a pressure between 0.5 to 2 atm; a reaction temperature between 300 to 600 K wherein a dielectric barrier discharge plasma reactor is used comprising: a reaction chamber comprising a structure of metal-based catalyst particles; a first supply to the reaction chamber; a second supply to the reaction chamber; wherein the first supply and second supply to the reaction chamber are in a counter-current configuration and wherein the metal-based catalyst particles are the catalyst as described herein.
[0080] A method for non-thermal plasma ammonia production according to claim 1 characterized in that the conditions of non-thermal plasma in step (v) include at least one, preferably two and most preferably three of the following conditions:• a frequency between 5 to 60 kHz;• a pressure between 0.5 to 2 atm; a reaction temperature between 300 to 600 K.
[0081] Examples of a metal-based catalyst structure and methods for plasma-driven ammonia production from H2O and N2 are now described.
[0082] Synthesis of a Co / SiOz catalyst structure[0083JA SiC>2 support with uniform cylindrical morphology was purchased from Sigma Aldrich. The Co metal supported on SiCh catalysts were prepared by wet impregnation method. The copper nitrate salt (Sigma Aldrich) was dissolved into deionized water to make a precursor solution. The SiC>2 was added to the solution to obtain 5 wt.% Co to SiCh. The mixture was mixed at 40-60 rpm and at 40-60 °C by using a rotatory. The amount of Co in the catalyst structure varied from 1 -20 wt%.
[0084] The Co / SiCh catalysts formed were used for testing efficacy in plasma-assisted ammonia production from H2O and N2. The H2O and N2 gases were directly used from purchase as direct feedstocks (i.e., without further treatment) for plasma ammonia synthesis. Ammonia production processes can occur at operating temperatures of at least about 4W or greater. The operating pressure for the ammonia process was at 1 bar.
[0085] Reactor and reaction conditions for plasma-assisted ammonia production from H2O and Nz.
[0086] A packed bed catalytic reactor made of quartz tube was used for testing ammonia production under conditions as noted herein. A plasma generator can provide a power up to 700W was used. The reaction conditions apply to the process data as described herein and outlined in Tables 1.
[0087] The feedstock used in the ammonia production was H2O and N2 with different total flowrate from 10 to 50 seem and different H2O / N2 volumetric ratios such as from 1.0 to 5.0.
[0088] The position of the metal-based catalyst bed was in a middle section of a reactor tube for the reactor, where the reactor tube was filled with quartz wool at the top and the bottom of the catalyst bed. The reactor was loaded with 0.1 g of metal-based catalyst pellets (formed as previously described herein) and feedstock passed the metal-based catalysts with a down-flow mode with no inert diluent. The plasma power was started from 5W, the reaction pressure was 1 bar, inlet gas flow rate was 10 seem N2 and H2O flowrate (liquid flow) was from 0.05 to 0.2 seem. Four grams (0.1 g) of metal-based catalyst was loaded for each reaction with a reaction time on stream of 8 hours.
[0089] A control reaction were conducted with the packed bed plasma reactor using H2O and N2 without metal-based catalyst was performed in all conditions.
[0090] Characterization of data obtained from processes.
[0091] The necessary data to determine gas conversion was acquired by using a micro gas chromatography (Agilent Micro-GC 490).
[0092] A Thermographic Analysis (TGA) signal along with a simultaneously collected Differential Scanning Calorimetry (DSC) signal combined with a simultaneous thermal analyzer (PerkinElmer STA 6000) of the spent catalyst was verify the carbon formation on the catalyst.
[0093] The ammonia production was analyzed via titration method by using a Metrohm 848 Titrino Plus. Each measurement was performed triplicate.
[0094] Liquid products were analyzed by using gas chromatography-mass spectrometry (GC-MS) (PerkinElmer Clarus SQ 8T).
[0095] In situ plasma reaction was characterized by using optical emission spectroscopy (AvSpec- ULS2048CL-EVO, USA). The wavelength was recorded from 200 to 1000 nm.
[0096] Ammonia-temperature programmed desorption (NH3-TPD) was performed to determine the surface acidity of Co / SiCh catalysts on a chemisorption analyzer (Finesorb-3010). Typically, 0.2 g catalyst was put into a U-type quartz tube and both ends were filled with quartz wool. To remove the adsorbed impurities, temperature-programmed oxidation (TPO) test was first performed, in which the tube was heated up to 600 °C and held for 30 minutes with a ramp rate of 20 °C min under 5%02 / He gas flow (flow rate 30 seem). Then, the system was cooled down to 120 °C and ammonia adsorption was conducted by feeding 10% NFF / He for 30 minutes (flow rate 25 seem). Next, the physisorbed ammonia was flushed out by He gas flow for 30 minutes (flow rate 30 seem). Finally, the desorption of ammonia was carried out from 120 °C to 800 °C with a ramping rate of 20 °C min4and held at 800 °C for 10 minutes. The desorbed ammonia was monitored by a thermal conductivity detector (TCD) and the amount was quantified by peak integration of the corresponding calibrated TCD signal. Nitrogen adsorption-desorption analysis of catalysts was carried out on an ASAP 2020 Plus surface area and porosimeter system (Micromeritics). The sample was first degassed at 350 °C for 4 hours with a temperature ramping rate of 10 °C min4and a vacuum level of 20 pmHg. The analysis was then performed in liquid nitrogen to get a 56-point adsorption-desorption isotherm. The total surface area was calculated by the BET method and the total pore volume was calculated at 0.995 relative pressure.[00971Plasma-driven ammonia production
[0098] As previously noted herein, a comparison of the performance of the Co / SiCh was employed for plasma-driven of ammonia production from H2O and N2.
[0099] A control experiment, in which plasma-driven reaction between H2O and N2 was performed in an empty tube showed no ammonia production even at the highest plasma power used in this work (7.36W).
[0100] As shown in Table 1 herein, when the Co / SiCh catalyst was packed in the reactor, ammonia was detected.
[0101] Table 1 : Plasma-based ammonia production performance at H2O flowrate of 0.1 seem and N2 flowrate of 10 seem, and different testsThe N2 conversion obtained was around 9.5 % and ammonia production was of 175.3 pmol / h. Ammonia production yield was calculated by the ammonia production yield on N2 conversion and it was almost 16% and the energy yield was 0.45 g / kW.h. It has been reported that nitrous oxide such as N2O was formed from the plasma driven N2 fixation with water by wetting N2 gas with water [1, 2], An extra downstream process to produce HNO3 from nitrous oxide is required to deal with such greenhouse gas. In-liquid plasma could form NH4NO3, which is an important fertilizer. In this primary work, we also analyzed NH4NO3 formation qualitatively and quantitatively, and the NH4NO3 was 0.54 mM / h. The in-liquid plasma route primarily displays high potential for ammonia and fertilizer production directly with less carbon emission.
[0102] Thus, the use of a metal-based catalyst structure as described herein that includes a combination of Co / SiCh provides a significantly enhanced production of ammonia. The use of a methane environment also produces other value-added products as described herein.
[0103] While the invention has been described in detail and with reference to specific embodiments thereof, it will be apparent to one skilled in the art that various changes and modifications can be made therein without departing from the spirit and scope thereof.
[0104] Thus, it is intended that the present invention covers the modifications and variations of this invention provided they come within the scope of the appended claims and their equivalents.
Claims
Claims1. A method for ammonia production comprising the steps of:(i) providing a first feedstock comprising N2 gas;(ii) providing a second feedstock comprising H2O;(iii) providing a reaction chamber comprising a metal-based catalyst;(iv) submitting the first feedstock of step (i) and the second feedstock of step (ii) to said reaction chamber;(v) subjecting the first and second feedstock to plasma in the reaction chamber comprising said metal-based catalyst, thereby forming ammonia; wherein the reaction chamber is a non-thermal plasma reactor and / or the plasma is a non-thermal plasma.
2. The method according to any one of claims 1 , wherein the second feedstock provided in step (iii) is gaseous.
3. The method according to any one of claims 1 or 2, wherein the second feedstock provided in step (iii) is liquid.
4. The method according to any one of claim 1 to 3, wherein the volume ratio of N2 gas of the first and H2O of the second feedstock provided in step (iii) is at least 1 : 1 respectively, preferably at least 1 :2 and most preferably from 1: 1 to 1:5.
5. The method according to any one of claims 1 to 3, wherein the volume ratio of N2 gas of the first and H2O of the second feedstock provided in step (iii) is at least 50: 1 respectively, preferably at least 100: 1, and most preferably from 200: 1 to 50: 1.
6. The method according to any one of claims 1 to 5, wherein additionally NH4NO3 is produced during step (v), preferably wherein the method yields NH4NO3 of at least 0.5 mM.h'1.
7. The method according to any one of the preceding claims, wherein the method yields ammonia at about 1 to about 500 pmol.h’1, preferably at least 200 pmol.h'1.
8. The method according to any one of the preceding claims, wherein the energy yield for ammonia is at least 0.01 g.kWh^g'1, preferably at least 0.1 g.kWh^g’1.
9. The method according to any one of the preceding claims, wherein step (v) is conducted at temperatures between 150 to 700 K, preferably between 200 to 450 K.
10. The method according to any one of the preceding claims, wherein step (v) is carried out in the reaction chamber configured as batch, fixed-bed continuous flow or moving-bed mode.
11. The method according to any one of the preceding claims, wherein the residence time of step (v) in the reaction chamber is at least 0.1 seconds, preferably at least 10 minutes.
12. The method according to any one of the preceding claims, further comprising a regeneration process, wherein the regeneration process comprises: a. rinsing the metal-based catalyst with a regeneration liquid, preferably the regeneration liquid comprises a polar organic solvent and most preferably the regeneration liquid comprises a polar organic solvent selected from acetone, propanol, ethyl acetate, methyl ethyl ketone and combinations thereof; b. optionally drying the metal-based catalyst obtained in step a.; c. calcining the metal-based catalyst to a temperature between 300 to 600 °C, preferably between 350 to 500 °C, preferably for at least 2 hour (at least 3 hours), and / or in an atmosphere comprising or consisting of H2 and Ar, preferably wherein the atmosphere is provided as a gas flow having a flowrate of 100 to 200 mL / min; thereby regenerating the metal-based catalyst provided in step (iii).
13. A metal-based catalyst for ammonia production, preferably ammonia production using a nonthermal plasma reaction process, comprising: a support structure; and a metal selected from the group consisting of Cu, Co, Zn, Mn, Y, Fe, Ru, Pd, Os, Ir, Pt or combinations thereof, preferably a metal selected from Cu, Co, Zn, Mn or combinations thereof, and most preferably Co, wherein the metal is present on the support structure; and wherein the metal-based catalyst has a pellet form.
14. The metal-based catalyst according to claim 13, wherein the support structure comprises or consists essentially of a material is selected from AI2O3, SiCh, TiCh, zeolites, Y molecular sieves and ZSM-5 molecular sieves.
15. The metal-based catalyst according to claim 13 or 14, wherein the support structure, preferably the SiCh support structure, has a BET surface area in the range of 120 m2 / g and 200 m2 / g.
16. The metal-based catalyst according to any one of claims 13 to 15, wherein the support structure has a substantially uniform cylindrical morphology.
17. The metal-based catalyst according to of any one of claims 13 to 16, wherein the mass content of the metal in the catalyst lies between 0.1 wt.% and 25 wt.% based on the mass of the support structure, preferably between 0.5 wt.% and 15 wt.% based on the mass of the support structure, more preferably between 0.5 wt.% and 7.5 wt.% based on the mass of the support structure.
18. The metal-based catalyst according to any one of claims 13 to 17, wherein the metal-based catalyst has one, preferably two and most preferably three of the following characteristics:• a BET surface area between 50 and 200 m2 / g, preferably BET a surface area between 100 and 150 m2 / g;• a pore volume between 0.1 to 1 mL / g, preferably between 0.5 to 0.8 mL / g;• a particle size distribution of the metal particles is between 2 to 50 nm, preferably between 2 to 10 nm.
19. The catalyst according to any one of claims 13 to 18, obtainable by a wet impregnation method, preferably using a water-soluble precursor salt of said metal.
20. Use of the catalyst according any one of claims 13 to 19, for the conversion of a gas comprising N2 to ammonia in the presence of non-thermal plasma, preferably provided by a dielectric barrier discharge reactor, preferably wherein the conversion of N2 to ammonia is at least 10%, more preferably at least 12%.
21. A dielectric barrier discharge plasma reactor for ammonia production comprising: a reaction chamber comprising a structure of metal-based catalyst particles;a first supply to the reaction chamber; a second supply to the reaction chamber; wherein the first supply and second supply to the reaction chamber are in a counter-current configuration, wherein preferably the metal-based catalyst particles are the metal-based catalyst according to any one of claims 13 to 20.
22. The dielectric barrier discharge plasma reactor according to claim 21, wherein the reaction chamber is a fluidized bed plasma reactor and / or the structure of metal-based catalyst particles is a fluidized bed.
23. The dielectric barrier discharge plasma reactor according to claim 21 or 22, wherein the first supply to the reaction chamber is a gas and the second supply to the reaction chamber is a liquid.
24. The dielectric barrier discharge plasma reactor according to any one of claims 21 to 23, wherein the plasma power is provided from renewable sources, preferably plasma power from solar or wind sources.
25. A method for non-thermal plasma ammonia production according to claim 1 characterized in that the conditions of non-thermal plasma in step (v) include at least one, preferably two and most preferably three or four of the following conditions:• a power between 1 to 200 W;• a frequency between 5 to 60 kHz;• a pressure between 0.5 to 2 atm;• a reaction temperature between 300 to 600 K.
26. A method for non-thermal plasma ammonia production using a dielectric barrier discharge plasma reactor according to any one of claims 21 to 24, from N2 gas and a second feedstock source characterized in that the conditions of non-thermal plasma include at least one, preferably two and most preferably three of the following conditions:• a frequency between 5 to 60 kHz; a pressure between 0.5 to 2 atm;• a reaction temperature between 300 to 600 K
Citation Information
Patent Citations
Non-thermal plasma synthesis with carbon component
US20140105807A1
Ammonia synthesis using plasma-produced electrons
US20190292063A1
Methods and compositions for microwave catalytic ammonia synthesis
US20200079656A1
Bicycle-handle
US471932A
Non-thermal plasma synthesis of ammonia
WO2009025835A1