A catalyst for non-thermal plasma ammonia production and its preparation method and application
The metal-based catalyst for non-thermal plasma ammonia production from CH4 and N2 addresses the energy and environmental drawbacks of existing methods by enabling efficient ammonia synthesis at room temperature and atmospheric pressure, reducing CO2 emissions and safety hazards.
Patent Information
- Application Number
- PCT/IB2024/053604
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-17
AI Technical Summary
Current ammonia production methods, such as the Haber-Bosch process, are energy-intensive and generate high CO2 emissions, and alternative technologies using H2 or H2O face challenges like safety hazards and corrosion, limiting their economic competitiveness and environmental impact.
A metal-based catalyst is developed for non-thermal plasma ammonia production, specifically designed for direct conversion of CH4 and N2, using a dielectric barrier discharge plasma reactor with a catalyst prepared by loading metals like Cu, Zn, or Ag on inorganic oxide supports, allowing for efficient ammonia production at room temperature and atmospheric pressure without the need for H2 or H2O.
This method achieves high efficiency in converting natural gas and nitrogen to ammonia with low energy consumption and reduced CO2 emissions, overcoming safety and corrosion issues associated with H2 and H2O, and provides a more economical and environmentally friendly route for ammonia production.
Smart Images

Figure IB2024053604_17102024_PF_FP_ABST
Abstract
Description
[0001] A catalyst for non-thermal plasma ammonia production and its preparation method and application
[0002] Field of the invention
[0003] The present invention belongs to the field of sustainable green chemical technology, and specifically relates to a metal-based catalyst for non-thermal plasma ammonia production and its preparation method and application.
[0004] Background of the invention
[0005] Ammonia is a critically important fertilizer and chemical product that is vital to the global food supply. There is also a trend towards ammonia as a highly promising non-carbon energy carrier and transportation fuel. Ammonia consists of 17.6 % hydrogen by mass, so it can be used as an indirect hydrogen storage compound. In addition, the energy density of ammonia is about 4.32 kWh-L-1, showing a capacity comparable to that of methanol and almost twice that of liquid hydrogen. Prototype vehicles running on pure ammonia and gasoline-ammonia fuel modifications have recently been designed. Another important advantage of using pure ammonia is that dependence on fossil fuels can be reduced by using synthetic "sustainable fuel sources". Further, future short-term storage such as batteries could be buffered by long-term energy storage molecules with high energy content and density such as ammonia.
[0006] Large-scale production of ammonia still relies heavily on the capital- and energy-intensive Haber-Bosch (H-B) process, which produces about 500 million tons of ammonia per year globally. In the H-B route, a mixture of hydrogen (H2) and nitrogen (N2) catalyzes the reaction through the use of an iron-based catalyst modified with K2O and AI2O3. At the same time, considering that the reaction to produce ammonia releases a certain amount of heat, the reaction is often carried out at temperatures in the range of 300-500° C, and 150-200 bar of pressure are required to shift the reaction equilibrium in favor of the ammonia production in the H-B process. The production of ammonia is very energy intensive and costly, partly because hydrogen does not occur naturally and needs to be produced using the very energy-intensive reforming of natural gas, which results in the emission of about 1 .87 tons of the greenhouse gas CO2 per ton of ammonia. A single pass results in a conversion efficiency of only 15% for N2 and H2. Therefore, recovery of unreacted syngas is often required to achieve an overall conversion efficiency of 97%. Despite this high conversion efficiency, the process is still an energy-intensive chemical process, and the H-B process is responsible for about 1 % of global GHG emissions and about 1.4% of global energy consumption. These values increase further if CO2 emissions associated with natural gas reforming (e.g. hydrogen production from CH4) are included. In recent years, a variety of new technologies have been developed to produce ammonia, including electrochemical, biochemical, photochemical and plasma technologies. In the last decades, a large number of non-thermal plasma (NTP)-assisted ammonia syntheses performed by N2 and H2 have been reported, and many studies have shown that ammonia can be produced at low temperatures (400-500 K) and atmospheric pressures when the NTP is coupled in tandem with a catalyst. However, considering that H2 does not exist in nature, it needs to be produced by natural gas reforming and the process generates a large amount of carbon emissions, which reduces economic competitiveness. Recently, several research groups have investigated the plasma-driven production of ammonia from N2 and H2O. However, utilizing H2O as the H2 feed theoretically requires at least 1 .5 tons of water stoichiometry per ton of ammonia and adds at least 20% to the actual water consumption due to process losses and emissions. As a result, electrochemical and non-thermal plasma technologies for ammonia production from N2 and H2O will be limited in arid regions such as Australia and the Middle East, and corrosion problems in pipeline and reactor systems due to seawater further limit their water source applications. Simultaneously, the water vapor reforming process with CH4 is energy intensive and results directly in very high annual CO2 emissions. Meanwhile, the reaction needs to be carried out at 800-1000° C, which also further increases the energy consumption of the process and the CO2 emissions, and the resulting H2 also needs to be stored and transported, which poses certain safety risks. For the foregoing reasons, it is more valuable to provide a method for the direct production of ammonia from CH4 and N2 than such combined techniques. And utilizing natural gas, whose main component is CH4, as an alternative hydrogen source would have very considerable economic benefits.
[0007] Based on the current research status, in the process of ammonia synthesis technology, the steam reforming of CH4 needs to be conducted at high temperatures, leading to issues such as high energy consumption and high CO2 emissions. In existing studies, by coupling non-thermal plasma with catalysts, it is possible to produce ammonia at low temperatures (400-500 K) and atmospheric pressure. However, the issue of using H2 and H2O as reaction feedstock still cannot be resolved. H2 poses safety hazards during storage and transportation, while H2O leads to technical problems such as corrosion of pipeline and reactors.
[0008] Summary of the invention
[0009] The inventors have found that a metal-based catalyst for non-thermal plasma ammonia production and a preparation method and application thereof for the direct production of ammonia by CH4 and N2 under the action of the metal-based catalyst of the invention provide improved properties for non-thermal plasma ammonia production.
[0010] In a first aspect of the invention there is provided a method of preparing a metal-based catalyst for ammonia production, preferably for ammonia production using a non-thermal plasma, comprising the steps of: (i) loading a metal substance, which contains a metal, on a support material; (ii) optionally drying the material of step (i); and (iii) calcination of the material of step (i) or of step (ii), thereby obtaining the metal-based catalyst for ammonia production.
[0011] In a second aspect of the invention there is provided a metal-based catalyst for producing ammonia obtainable by or obtained by the method of invention according to the first aspect.
[0012] In a third aspect of the invention there is provided a use of the metal-based catalyst of the invention according to the second aspect for ammonia production, preferably for ammonia production using a non-thermal plasma. In a fourth aspect of the invention there is provided a method of producing ammonia, preferably using a non-thermal plasma, comprising the steps of:
[0013] (i) providing a metal-based catalyst according to the second aspect of the invention into a dielectric barrier discharge plasma reactor, and
[0014] (ii) converting CH4 and N2 to NH3 under non-thermal plasma reaction conditions in said dielectric barrier discharge plasma reactor using said metal-based catalyst.
[0015] Legend to the figures
[0016] FIG. 1 shows a schematic diagram of a dielectric barrier discharge non-thermal plasma reactor used in the present invention. Wherein, 1-nitrogen; 2-methane; 3-high voltage electrode; 4-optical emission spectrometer; 5-dielectric barrier discharge plasma reactor; 6-ground electrode; 7- cold trap; 8-micro-GC; 9-plasma generator.
[0017] Detailed description of the invention
[0018] In order to overcome the above mentioned drawbacks, this present invention has been conducted with the aims of providing a catalyst for non-thermal plasma ammonia production and a preparation method and application thereof for the direct production of ammonia by CH4 and N2 under the action of a metal-based catalyst for non-thermal plasma ammonia production to solve drawbacks of existing ammonia synthesis technology whose feedstock would use H2 or H2O, and H2 is a safety hazard in the process of storing and transporting, and H2O will lead to the pipe and reactor system corrosion.
[0019] Embodiments
[0020] In a preferred embodiment, the loading of the metal on the support material of step (i) is carried out using one of a wet impregnation (Wl) process or Incipient wetness impregnation (IWI) process or an excess impregnation process.
[0021] In a preferred embodiment, said metal is one or more selected from Cu, Zn, Ag, Ni, Fe, Ru, Rh and Co, more preferably selected from Cu, Zn and Ag.
[0022] In a preferred embodiment, said support material comprises orconsists essentially of an inorganic oxide. In a preferred embodiment, said support material is one or more selected of AI2O3 , SiC>2 , TiC>2, Zeolites, Y molecular sieves and ZSM-5 molecular sieves.
[0023] In a preferred embodiment, said metal substance is loaded on the support material at a metal mass percentage of 0.1 % to 10%, preferably 1 % to 5%, based on the weight of the support material.
[0024] In a preferred embodiment, the drying condition of step (ii) is at 75-150 °C, preferably for 1-24 hours.
[0025] In a preferred embodiment, the calcining conditions of step (iii) calcining temperature of 100-800°C, preferably 200-800°C, more preferably at 300-700°C.
[0026] In a preferred embodiment, the calcining conditions of step (iii) comprises a heating increase rate of 1- 20 °C / min to attain the calcining temperature. In a preferred embodiment, the calcinating conditions of step (iii) comprises maintaining the calcining temperature for 3-5 hours.
[0027] In a preferred embodiment, the atmosphere for calcination of step (iii) is air or nitrogen.
[0028] In a preferred embodiment, said support material has particles with a diameter of 1 to 1 .5 mm and / or a length of 3 to 5 mm and / or a specific BET surface area of 50 to 500 m2 / g, preferably 150 to 350 m2 / g.
[0029] In a preferred embodiment, step (i) comprises adding the metal substance to the support material in the form of a water-soluble salt thereof, preferably wherein the water-soluble salt is one or more selected of a nitrate salt, a sulfate salt and a chloride salt.
[0030] Embodiments of the method of the third aspect
[0031] In a preferred embodiment, said non-thermal plasma reaction conditions of step (ii) are generated by the dielectric barrier discharge plasma reactor at a power of 5 - 30W, preferably 5 - 20W.
[0032] In a preferred embodiment, said non-thermal plasma reaction conditions of step (ii) comprise a reaction pressure of 0.1 - 5 atmosphere, preferably less than 3 atmosphere, more preferably about 1 atmosphere.
[0033] In a preferred embodiment, said non-thermal plasma reaction conditions of step (ii) comprise a reaction temperature of 200 - 500 K, preferably 250 - 350 K, more preferably about room temperature.
[0034] In a preferred embodiment, step (ii) comprises providing a volume ratio of CH4:N2 of 4:1 to 1 :2, preferably 3:1 to 1 :1 , more preferably about 2:1 .
[0035] In a preferred embodiment, step (ii) comprises providing a flow rate of CH4 of 5 to 30 seem and / or providing a flow rate of N2 of 1 to 15 seem, preferably 3 to 15 seem.
[0036] In order to achieve the above goal, the present invention is realized by using any one or more of the following technical solutions:
[0037] The present invention discloses a method of preparing a metal-based catalyst for non-thermal plasma ammonia production, in which a metal substance is loaded on a support material in embodiments using an equal wet impregnation (Wl) or Incipient wetness impregnation (IWI) method. Wl is a catalyst synthesis method where a support material absorbs a precursor solution containing the desired active phase, offering simplicity and versatility in catalyst preparation. IWI uniformly distributes an active component onto a support material by saturating it with a precursor solution until reaching its incipient wetness point, ensuring maximum absorption. After drying, calcination, the catalyst for non- thermal plasma ammonia production is obtained;
[0038] The metal is preferably selected from one or more of Cu, Zn or Ag; the support material is preferably selected from one or more of AI2O3 , SiC>2 , TiC>2, Zeolites, Y molecular sieves and ZSM-5 molecular sieves;
[0039] The metal substance is preferably loaded on the support material at a metal mass percentage of 1% to 5%.
[0040] Preferably, the drying condition is 1 to 24 h at 75 to 150°C. Preferably, the calcination conditions are a calcining temperature of 300 - 700 °C and / or a heating rate of 1-20 °C / min to attain the calcining temperature, and calcination for 3-5 h at the calcining temperature.
[0041] Further, preferably the atmosphere for calcination is air or nitrogen
[0042] Preferably, the particles of the support material have a diameter of 1 to 1 .5 mm, and / or a length of 3 to 5 mm and / or a specific surface area of 150 to 350 m2 / g.
[0043] Preferably, the metal is added to the support material in the form of a water-soluble salt, the water-soluble salt being a nitrate, sulfate or chloride.
[0044] The present invention also discloses catalysts for non-thermal plasma ammonia production made by the above preparation method or obtainable by the above preparation method.
[0045] The present invention also discloses the application of the above catalyst for non-thermal plasma ammonia production in ammonia production, wherein a catalyst for non-thermal plasma ammonia production is added under non-thermal plasma reaction conditions in a dielectric barrier discharge plasma reactor to efficiently convert CPU and N2 to NH3; the dielectric barrier discharge plasma generator is preferably operated at a power range of 5 to 20W.
[0046] Compared with the current existing techniques, the present invention has the following beneficial effects:
[0047] The present invention discloses embodiments of a method of preparing a metal-based catalyst for non-thermal plasma ammonia production, using IWI or Wl method to load metal on the support material in order to achieve a good metal dispersion effect, the metal is preferably Cu, Zn or Ag, which are metals with better plasma activity; the support material is one or more of AI2O3, SiC>2, TiC>2, Y molecular sieve and ZSM-5 molecular sieve; these stable support materials can provide rich pore structure; the metal is loaded with a mass percentage of 1 %~5% to obtain the active component with certain metal loadings, and after drying and removing most of the water, the catalyst structure comprises the metal. These stable support materials can provide rich pore structure; the metal is preferably loaded on the support material with a mass percentage of 1 % - 5% to obtain the active component with a certain metal loading, and the catalyst for non-thermal plasma ammonia production is prepared by optionally drying to remove most of the water and calcining to generate the metal oxide structure. The catalyst is characterized by large specific surface area, large mesopore volume and uniform metal dispersion. And the catalyst produced by the present invention has excellent CH4 and nitrogen conversion ability, can make natural gas and nitrogen and other raw materials efficiently converted to ammonia, while only a small amount of coke is produced, without the use of H2 and H2O, can be used at room temperature, normal pressure, using dielectric barrier discharge plasma reactor at low plasma power, natural gas and nitrogen can be efficiently converted to ammonia, the natural gas conversion of 5.9-56.4%, and 0.5% - 8.1 % for N2 conversion is shown in exemplary embodiments. Meanwhile, the production rate of ammonia may reach 12.9 - 96.5 pmol-h’1. The reaction process does not require the use of H2 or H2O, which effectively solves the safety hazards of H2 in the storage and transportation process and the technical problems of corrosion of the pipeline and the reactor system that H2O will cause.
[0048] Further, the drying conditions are preferably 1 to 24 h at 75 to 150 °C to ensure that majority water is removed to obtain a dried solid material. Further, in preferred embodiments the support material has a particle diameter of 1 to 1 .5 mm, and / or a length of 3 to 5 mm, and / or a specific BET surface area of 150 to 350 m2 / g. Said dimensions can have a good match with the reactor size.
[0049] Further, the metal is added to the support material in the form of a water-soluble salt to facilitate the next step of conversion; the water-soluble salt is a nitrate, sulfate, or chloride, which facilitates dissolution in water to form a solution.
[0050] The present invention also discloses a catalyst for non-thermal plasma ammonia production made by the above preparation method, which has excellent natural gas and nitrogen conversion capability, and can efficiently convert natural gas and nitrogen into ammonia at room temperature and pressure using a dielectric-barrier discharge plasma reactor at low plasma power, such as with an ammonia production rate of 96 pmol-fr1or more.
[0051] The present invention also discloses the application of the above catalyst for non-thermal plasma ammonia production in ammonia production, utilizing the catalyst for non-thermal plasma ammonia production to introduce methane and nitrogen into a dielectric-barrier discharge non-thermal plasma reactor, to realize high-efficiency conversion of methane and nitrogen under milder reaction conditions and lower power consumption, and to efficiently convert natural gas and nitrogen into high value ammonia, providing a more economical technical route to reduce carbon emissions in the ammonia production process and achieve carbon neutrality.
[0052] In addition, natural gas is a relatively clean and abundant natural resource, the main component of which is methane, which has high thermodynamic and kinetic inertness due to the high symmetry structure and high C-H bond energy (425 kJ / mol) of the methane molecule, but the activation and high efficiency utilization of methane is still at a relatively low level, and natural gas is currently still mainly used for fuel purposes in real life. The present invention employs dielectric barrier discharge (DBD) non- thermal plasma (NTP) technology, which can deliver energetic substances, to activate and convert methane and nitrogen molecules, e.g. in natural gas, into ammonia and other high value-added products. The conversion of natural gas and nitrogen under non-thermal plasma technology is realized with low operating costs and mild reaction conditions: under the conditions described in the present invention, at least 96.5 pmol-fr1of ammonia can be produced, and 56.4% methane conversion and 8.1 % nitrogen conversion can be achieved. It does not require the use of H2 and substantially improves a series of problems in the existing Haber-Bosch process, such as high energy consumption, high investment costs, complex process routes, high reaction pressures, and high plant costs, and provides a new technological route for the preparation of ammonia as well as for the efficient utilization of methane.
[0053] Exemplary embodiments
[0054] In order to better understand the embodiments of the present invention, the technical solutions in the embodiments of the present invention will be described clearly and completely in the following in conjunction with the accompanying drawing in the exemplary embodiments of the present invention, and it is obvious that the described embodiments are only a part of the embodiments of the present invention and not all of the possible embodiments or examples of the invention. Based on the embodiments in the present invention, all other embodiments obtained by a person of ordinary skill without making creative labor shall fall within the scope of protection of the present invention.
[0055] It is to be noted that the terms "first", "second", etc., In the specification and claims of the present invention and the accompanying drawings referred to above are used to distinguish similar objects and need not be used to describe a particular order or sequence. It should be understood that the data so used may be interchanged, where appropriate, so that the embodiments of the present invention described herein can be practiced in an order otherthan those illustrated or described herein. In addition, the terms "comprising" and "having", and any variations thereof, are intended to cover non-exclusive embodiments, e.g., a process, method, system, product or apparatus comprising a series of steps or units need not be limited to those steps or units clearly listed but may include steps or units that are not clearly listed, but rather may include embodiments that are not clearly listed, units, but may include other steps or units that are not clearly listed or that are inherent to those processes, methods, products or equipment.
[0056] For the present disclosure, the phrase “A and / or B” means (A), (B), or (A and B). For the present disclosure, the phrase “A, B, and / or C” means (A), (B), (C), (A and B), (A and C), (B and C), or (A, B and C).
[0057] The singular forms “a”, “an”, and “the” as used herein should be construed to include plural referents unless the content clearly dictates otherwise. It should also be noted that the term “or” is generally employed in its broadest sense, that is as meaning “and / or” unless the content clearly dictates otherwise. The terms “comprising”, “including”, “having” and the like, as used with respect to embodiments of the present disclosure, are synonymous. Such expressions should be construed in an open, inclusive sense, meaning that the embodiment described includes the recited features, butthat it does not exclude the presence of other features, as long as they do not render the embodiment unworkable.
[0058] The terms “about”, “approximately”, “substantially” and the like, as used with respect to embodiments of the present disclosure indicate that the value or range is interpreted as being as accurate as the method used to measure it. Where such terms are applied to a structural unit the expression containing the terms is to be interpreted as a technical feature being produced within the technical tolerance of the method of manufacture.
[0059] Whenever reference is made throughout this document to a compound which is a salt, this should be construed to include the anhydrous form as well as any solvates (in particular hydrates) of this compound.
[0060] In accordance with the invention, the BET surface area as referred to herein is determined at a temperature of 77K using a sample of 0.1-0.5g. The BET surface area as referred to herein is determined using nitrogen. A preferred analysis method to determine the BET surface area comprises heating samples to 400 °C for a desorption cycle prior to surface area analysis. A suitable and thus preferred analysis apparatus for determining the BET surface area is a Micromeritics Gemini VII 2390 Surface Analyzer preferably equipped with a Micromeritics FlowPrep 060 flowing-gas degassing unit.
[0061] For the purposes of the present disclosure, the ideal gas law is assumed such that the vol% of a gas is considered as equal to the mol%. The invention is described in further detail below in conjunction with the accompanying drawing Figure 1 .
[0062] Example A
[0063] In an exemplary embodiment of the method of synthesizing ammonia at ambient temperature and pressure by means of a non-thermal plasma technique, the method comprising efficiently converting CH4 and N2 to ammonia under non-thermal plasma reaction conditions, under mild reaction conditions and with the assistance of a catalyst. The catalyst is a metal-loaded inorganic oxide material, wherein the metal is one or more of Cu, Zn, Ag, Ni, Fe, Ru, Rh and Co, and the inorganic oxide is one or more of AI2O3, SiC>2, TiC>2, Zeolites, Y molecular sieve, and ZSM-5 molecular sieve, and the metal loading is from 1 % to 5% by weight in terms of the weight of the support material.
[0064] The reaction atmosphere is a mixture of nitrogen and methane, and the reaction temperature is room temperature, and the reaction pressure is 1 atmosphere.
[0065] A further improvement of the present invention is that the reactor system used is a dielectric barrier discharge plasma reactor, a schematic diagram of which is shown in Figure 1.
[0066] In embodiments, a method is provided of preparing a catalyst for ammonia production using non-thermal plasma technology, comprising the steps of:
[0067] 1) Selection of suitable inorganic oxides as support materials.
[0068] 2) Multiple metal-loaded (transition) metal oxide catalysts were obtained by loading metals on the support material according to the Wl process or the IWI process.
[0069] A further improvement of the present invention is that the support material is a commercially available material such as SiC>2 with suitable pore size and specific BET surface area.
[0070] A further improvement of the present invention is that, in step 2), the loading metal is selected as Cu, Zn, Ag, Ni, Fe, Ru, Rh or Co metal substance, water-soluble salt thereof, and loaded onto the support material with a metal loading of 1 % to 5% by weight, dried at 75 - 150 °C for 1 - 24 h, and then raised to 300 - 700 °C in accordance with the heating rate of 1 - 20 °C / min and calcined under an atmosphere of air or the catalyst was calcined under nitrogen atmosphere for 3 - 5 h to obtain the final catalyst.
[0071] The catalyst is further improved in that the water-soluble salt is nitrate, sulfate or chloride.
[0072] The present invention has been found to enable the efficient conversion of feedstocks such as natural gas and nitrogen to ammonia in the presence of specific metal-loaded catalysts, while generating only a small amount of coke.
[0073] To summary, in preferred examples of the method of preparing a catalyst for non-thermal plasma ammonia production, said method comprising the following steps:
[0074] (1) Select shaped support material with a particle diameter of 1 to 1 .5 mm, a length of 3 to 5 mm and a specific BET surface area of 150 to 350m2 / g.
[0075] 2) Preparation of metal-loaded catalysts, the present invention realizes obtaining the desired metal loading using a process selected from an IWI process, a Wl process, an excess impregnation method (and similar processes). Preferred water-soluble salts of preferred active metal substances (Cu, Zn, Ag, Ni, Fe Ru, Rh or Co) including nitrates, sulfates, chlorides, etc. or combinations of the above substances are dissolved in water, 1 % to 5% by weight of the metal mass loaded into the support, dried at 75 to 150 °C for 1 to 24 h, and then calcined under air or nitrogen atmosphere at 300 to 700 °C (attained with a temperature increase rate of 1 to 20 °C / min) under air or nitrogen atmosphere, and then calcined for 3 to 5 h to obtain the final catalyst.
[0076] In further embodiments, the invention provides the following step(s):
[0077] (3) Catalyst application: Using the dielectric barrier discharge non-thermal plasma reactor shown in Fig. 1 , a certain amount of catalyst was firstly loaded into the reactor, and the flow rates of CF and N2 were controlled to be about 10 to 50 seem respectively so as to realize the reaction atmosphere CH4 :N2 according to a volume ratio of 2:1 to 1 :1 , and the temperature and pressure of the reaction were at room temperature and 1 atmosphere. The power of the non-thermal plasma generator was set at 5 to 20 W. The gaseous and liquid products were collected, and their product distribution was studied.
[0078] The highly porous supports in the present invention include one or more of mesoporous TiC>2, porous AI2O3, porous SiC>2, zeolites, ZSM-5 molecular sieves and Y molecular sieves. In the present invention, the use of metals suitable for loadings including, but not limited to, Cu, Zn, Ag, Ni, Fe, Ru, Rh, Co can substantially improve the reaction performance of the catalyst, and the metal mass percentage of the metal loading is preferably in the range 1 % to 5% by weight based on the weight of the support structure.
[0079] Example 1
[0080] Catalysts with a mass percentage of 5% Cu / SiC>2 were prepared according to the following: Cylindrical shaped SiC>2 supports with substantially uniform dimensions from Sigma Aldrich were used as the catalyst support material with a diameter of 1 mm, a length of 5 mm and a specific BET surface area of 350 m2 / g.
[0081] Next, CU(NO3)2-6H2O (Sigma Aldrich) salt was dissolved in deionized water to form a metal precursor solution, and SiC>2 support was impregnated with an equal volume of the metal precursor solution to achieve a Cu metal loading of 5%, and the impregnated solids were subsequently dried at 75 °C for 24 h and calcined using a ramping rate of 20 °C / min. The 5% Cu / SiC>2 catalyst was obtained by calcining in static air at 550 °C for 4 h after the ramping rate of 20 °C / min, and 4 g of the obtained catalyst was taken and filled in the reactor.
[0082] The ammonia synthesis experiments with nitrogen and methane were carried out using methane and nitrogen as two independent gas paths, with a volume ratio of CF : N2 of 2:1 , and controlling the flow rates of 6.6 seem and 3.3 seem, respectively, and controlling the pressures to be at atmospheric pressure and the temperatures to be at room temperature, and controlling the power of the plasma generator to be 20 W. The ammonia synthesis experiments were carried out using methane and nitrogen as two independent gas paths. Under these conditions, a methane conversion of 56.4%, a nitrogen conversion of 8.1 %, and an ammonia production rate of 96.5 pmol-h-1of the reaction product were obtained.
[0083] Example 2 Cu / SiC>2 catalysts with a mass percentage of 5% were prepared according to the following: cylindrical shaped SiC>2 supports with substantially homogeneous dimensions from Fisher Scientific were used as catalyst support materials with a diameter of 1 mm, a length of 3 mm and a specific BET surface area of 150 m2 / g.
[0084] Next, Cu(NOs) 2-6H2 O salt was dissolved in deionized water to form a metal precursor solution, SiC>2 support was impregnated with an equal volume of the metal precursor solution to achieve a Cu metal loading of 5%, and the impregnated solid was subsequently dried at 150 °C for 1 h and calcined in nitrogen at 300 °C for 5 h after a ramping rate of 1°C / min to obtain a 5% of Cu / SiC>2 catalyst was obtained and 4 g of the obtained catalyst was taken and filled in the reactor.
[0085] The ammonia synthesis experiments with nitrogen and methane were carried out using methane and nitrogen as two independent gas paths, CF : N2 with a volume ratio of 2:1 , and the flow rates were adjusted and controlled as shown in Table 1 , and the flow rates were controlled to be 13.2 seem and 6.6 seem respectively, and the pressures were controlled to be at atmospheric pressure, the temperatures to be at room temperature, and the power of the plasma generator to be 20 W. The results were measured and presented in Table 1 , and the ammonia production rates were measured and presented in Table 1. The results such as feedstock conversion, ammonia generation rate was measured and listed in Table 1 .
[0086] Example 3
[0087] Catalysts with a mass percentage of 5% Cu / SiC>2 were prepared according to the following: cylindrical shaped SiC>2 supports with uniform dimensions from Sigma Aldrich were used as the catalyst support material, with a diameter of 1 .3 mm, a length of 4 mm and a specific BET surface area of 250 m2 / g.
[0088] Next, Cu(NOs) 2-6H2 O salt was dissolved in deionized water to form a metal precursor solution, and SiC>2 support was impregnated with an equal volume of the metal precursor solution to achieve a Cu metal loading of 5%, and the impregnated solids were subsequently dried at 150 °C for 1 h and calcined in static nitrogen at 700 °C for 3 h after a ramping rate of 10 °C / min. The 5% Cu / SiC>2 catalyst was obtained, and 4 g of the obtained catalyst was taken and filled in the reactor.
[0089] The ammonia synthesis experiments with nitrogen and methane were carried out using methane and nitrogen as two independent gas paths with a volume ratio of 2:1 for CH4 : N2 and their flow rates were controlled to be 20 seem and 10 seem, respectively, the pressure was controlled to be at atmospheric pressure and the temperature to be at room temperature, and the power of the plasma generator was adjusted and controlled as shown in Table 1. The results such as feedstock conversion, ammonia generation rate were measured and listed in Table 1.
[0090] The flow rates of methane and nitrogen were adjusted and controlled to 6.6 seem and 3.3 seem, respectively, but the plasma power was changed to 10W or 15W to carry out ammonia synthesis experiments with nitrogen and methane. The results such as feedstock conversion, ammonia generation rate were measured and listed in Table 1 .
[0091] Example 4 Zn / SiC>2 or 1 % Ag / SiC>2 catalysts with a mass percentage of 2% were prepared according to the following: cylindrical shaped SiC>2 supports with homogeneous dimensions from Sigma Aldrich were used as the catalyst support material with a diameter of 1 .3 mm, a length of 4 mm and a specific BET surface area of 250 m2 / g.
[0092] Next, ZnSC orAgNOs salt was dissolved in deionized water to form a metal precursor solution, SiC>2 support was impregnated with an equal volume of the metal precursor solution to achieve a Zn metal loading of 2% or a 1 % loading of Ag, and the impregnated solids were subsequently dried at 110 °C for 3 h and calcined in static air at 550 °C for 4 h after a ramping rate of 10 °C / min, to obtain 2% Zn / SiC>2 or 1 % Ag / SiC>2 catalyst in mass percentage and 4 g of obtained catalyst was taken and filled in the reactor.
[0093] The ammonia synthesis experiments with nitrogen and methane were carried out using methane and nitrogen as two separate gas paths with a volume ratio of 2:1 for CH4 : N2 and respectively controlling the flow rate as shown in Table 1 , controlling its pressure to atmospheric pressure, temperature to room temperature and controlling the power of the plasma generator as shown in Table 1. The results such as feedstock conversion, ammonia generation rate were measured and listed in Table 1 .
[0094] Example 5
[0095] Catalysts with a mass percentage of 2% Zn / AI2O3 or 1 % Ag / AI2O3 were prepared according to the following: cylindrical shaped AI2O3 supports with uniform dimensions from Sigma Aldrich were used as the catalyst support material with a diameter of 1 .2 mm, a length of 5 mm and a specific BET surface area of 300 m2 / g.
[0096] Next, ZnCh or AgNOs salt was dissolved in deionized water to form a metal precursor solution, SiC>2 support was impregnated with an equal volume of the metal precursor solution to achieve a Zn metal loading of 2% or a 1 % loading of Ag, and the impregnated solids were subsequently dried at 110 °C for 12 h and calcined at 550 °C for 4 h in static air after a ramping rate of 10 °C / min. A catalyst with a mass percentage of 2% Zn / SiC>2 or 1% Ag / SiC>2 was obtained and 4 g of the obtained catalyst was taken and filled in the reactor.
[0097] The ammonia synthesis experiments with nitrogen and methane were carried out using methane and nitrogen as two separate gas paths with a volume ratio of 2:1 for CH4 : N2 and respectively controlling the flow rate as shown in Table 1 , controlling its pressure to atmospheric pressure, temperature to room temperature and controlling the power of the plasma generator as shown in Table 1. The results such as feedstock conversion, ammonia generation rate were measured and listed in Table 1 .
[0098] Example 6
[0099] Catalysts with a mass percentage of 5% CU / AI2O3, 5% Cu / TiC>2, 5% Cu / Y, 5% Cu / ZSM-5 were prepared according to the following: cylindrical shaped AI2O3 supports with uniform dimensions from Sigma Aldrich were used as the catalyst support material or powdered TiC>2 , Y, ZSM-5 molecular sieves, which were prepared in the laboratory by using silica sols. The shaped supports were prepared with a diameter of 1 .2 mm, a length of 5 mm and a specific BET surface area of 300 m2 / g.
[0100] Next, Cu(NOs) 2-6H2O salt was dissolved in deionized water to form metal precursor solutions, and different supports were impregnated with equal volumes of the metal precursor solutions to achieve a Cu metal loading of 5%, and then the impregnated solids were dried at 110 °C for 12 h and calcined in static air at 550 °C for 3 h after a heating rate of 15 °C / min. The Cu-containing catalysts with different supports were obtained: 5% CU / AI2O3, 5% Cu / TiC>2, 5% Cu / Y, 5% Cu / ZSM-5 catalysts in mass percentage and 4 g of catalysts were taken out and filled in the reactor.
[0101] The ammonia synthesis experiments with nitrogen and methane were carried out using methane and nitrogen as two separate gas paths with a volume ratio of 1 :1 for CH4 : N2 and respectively controlling the flow rate as shown in Table 1 , controlling its pressure to atmospheric pressure, temperature to room temperature and controlling the power of the plasma generator as shown in Table 1. The results such as feedstock conversion, rate of ammonia generation were measured and listed in Table 1 .
[0102] Table 1. Performance evaluation results of different catalysts under different reaction conditions
[0103] Table 1 shows the results of the performance evaluation of different catalysts under different reaction conditions, from which it can be seen that the different catalysts for the preparation of ammonia from the co-conversion of nitrogen and natural gas varied greatly, and the flow rates of the two gas phases, as well as the power of the plasma generator, all had a significant effect on the conversion of methane and nitrogen, as well as the rate of ammonia generation. Under optimal conditions, the methane conversion can reach 56.4%, the nitrogen conversion can reach 8.1 %, and the ammonia production rate can reach 96.5 pmol h-1.
[0104] Referring to FIG. 1 for a schematic diagram of the dielectric barrier discharge non-thermal plasma reactor used in the present invention, it can be seen from the figure that the reactor is a dielectric barrier discharge plasma reactor 5, which utilizes the high voltage generated by the high voltage electrodes 3 of the plasma generator 9 to form a plasma, and at the same time, the grounding electrodes 6 are grounded for safety, while the optical emission spectrometer 4 is utilized to monitor the spectra generated therein and to study the reaction mechanism involved. Nitrogen supplied by nitrogen source 1 is fed into the gas and methane of methane source 2 is fed into the gas, and its relative flow rate can be adjusted by a flow meter, and ammonia can be generated in the reactor after the two gases are mixed into it, and it can be detected and analyzed by using micro-GC 8 after separation through a cold trap 7. In summary, the reactor is operated by connecting the high voltage electrode 3 to a high voltage alternating current, and a high voltage electric field will be formed between the high voltage and low voltage electrodes. When passing through the high voltage electric field, methane of methane source 2 and nitrogen of nitrogen source 1 will be polarized by the electric field. At the same time, electrons will be accelerated in the high-voltage electric field and will collide with the reactant molecules, resulting in the breaking of chemical bonds in the reactants, thus realizing the activation of methane and nitrogen at low temperatures at atmospheric pressure and the generation of ammonia.
[0105] The above content is only to illustrate the technical ideas of the present invention, cannot be used to limit the scope of protection of the present invention, all in accordance with the technical ideas put forward by the present invention, any changes made on the basis of the technical program, fall within the scope of protection of the claims of the present invention.
Claims
CLAIMS1. A method of preparing a metal-based catalyst for ammonia production, preferably for ammonia production using a non-thermal plasma, comprising the steps of:(i) loading a metal substance, which contains a metal, on a support material;(ii) optionally drying the material of step (i); and(iii) calcination of the material of step (i) or of step (ii), thereby obtaining the metal-based catalyst for ammonia production.
2. The method of preparing a metal-based catalyst of claim 1 , wherein the loading of the metal on the support material of step (i) is carried out using one of a wet impregnation (Wl) process, an Incipient wetness impregnation (IWI) process or an excess impregnation process.
3. The method of preparing a metal-based catalyst of any one of the preceding claims, wherein said metal is one or more selected from Cu, Zn, Ag, Ni, Fe, Ru, Rh and Co, preferably selected from Cu, Zn and Ag.
4. The method of preparing a metal-based catalyst of any one of the preceding claims, wherein said support material is one or more material selected of AI2O3 , SiC>2 , TiC>2 , Zeolites, Y molecular sieves and ZSM-5 molecular sieves.
5. The method of preparing a metal-based catalyst of any one of the preceding claims, wherein said metal substance is loaded on the support material at a metal mass percentage of 0.1 % to 10%, preferably 1 % to 5%, based on the weight of the support material.
6. The method of preparing a metal-based catalyst of any one of the preceding claims, wherein the drying condition of step (ii) is at 75-150 °C, preferably for 1-24 hours.
7. The method of preparing a metal-based catalyst of any one of the preceding claims, wherein the calcining conditions of step (iii) comprises a calcining temperature of 100-800°C, preferably of 300- 700°C.
8. The method of preparing a metal-based catalyst of claim 7, wherein the calcining conditions of step (iii) comprises a heating increase rate of 1-20 °C / min to attain the calcining temperature.
9. The method of preparing a metal-based catalyst of any one of the preceding claims 7 - 8, wherein the calcinating conditions of step (iii) comprises maintaining the calcining temperature for 3-5 hours.
10. The method of preparing a metal-based catalyst of any one of the preceding claims, wherein the atmosphere for calcination of step (iii) is air or nitrogen.
11. The method of preparing a metal-based catalyst of any one of the preceding claims, wherein said support material has particles with a diameter of 1 to 1 .5 mm and / or a length of 3 to 5 mm and / or a specific BET surface area of 50 to 500 m2 / g, preferably 150 to 350 m2 / g.
12. The method of preparing a metal-based catalyst of any one of the preceding claims, wherein step (i) comprises adding the metal substance to the support material in the form of a water-soluble salt thereof, preferably wherein the water-soluble salt is one or more selected of a nitrate salt, a sulfate salt and a chloride salt.
13. A metal-based catalyst for producing ammonia obtainable by or obtained by the method of preparation of any one of claims 1 to 12.
14. Use of the metal-based catalyst as claimed in claim 13 for ammonia production, preferably for ammonia production using a non-thermal plasma.
15. Method of producing ammonia, preferably using a non-thermal plasma, comprising the steps of:(i) providing a metal-based catalyst as claimed in claim 13 into a dielectric barrier discharge plasma reactor, and(ii) converting CH4 and N2 to NH3 under non-thermal plasma reaction conditions in said dielectric barrier discharge plasma reactor using said catalyst.
16. Method according to claim 15, wherein said non-thermal plasma reaction conditions of step (ii) comprise a reaction pressure of 0.1 - 5 atmosphere, preferably less than 3 atmosphere, more preferably about 1 atmosphere.
17. Method according to any one of the claims 15 -16, wherein said non-thermal plasma reaction conditions of step (ii) comprise a reaction temperature of 200 - 700 K, preferably 250 - 350 K, more preferably about room temperature.
18. Method according to any one of the claims 15 -17, wherein step (ii) comprises providing a volume ratio of CH4:N2 of 4:1 to 1 :2, preferably 3:1 to 1 :1 , more preferably about 2:1 .
19. Method according to any one of the claims 15 -18, wherein step (ii) comprises providing a flow rate of CH4 of 5 to 30 seem and / or providing a flow rate of N2 of 1 to 15 seem, preferably 3 to 15 seem.
Citation Information
Patent Citations
Method and device for preparing ammonia by cooperation of dielectric barrier discharge low-temperature plasma and catalyst
CN110372006A
Method for co-producing ammonia, amine compounds and hydrogen by catalytically converting methane and nitrogen through plasma
CN116002713A
Catalyst on silica support
GB929212A
Non-thermal plasma synthesis of ammonia
WO2009025835A1
Cited By
Synthetic ammonia system based on utilization of methane and nitrogen
CN119657031A
Preparation method of selective deoxidizing electrode and application of selective deoxidizing electrode in electrocatalytic synthesis of ammonia
CN120330759A
Application of synthesis ammonia catalyst based on Silicalite-1
CN122230783A