Semiconductor light-receiving element and method for manufacturing semiconductor light-receiving element
The semiconductor light-receiving device employs a digital alloy structure with alternately laminated Si and AlAs layers on an InP substrate to address noise and reliability issues in APDs, achieving low noise and high reliability through effective lattice strain management and crystal quality improvement.
Patent Information
- Application Number
- PCT/JP2023/014682
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-17
AI Technical Summary
Current semiconductor photodetectors, such as APDs, face challenges in achieving low noise and high reliability due to lattice mismatch issues and crystal defects, particularly when forming Ge absorption layers on Si substrates or Si multiplication layers on InP substrates, which affect their noise performance and reliability.
A semiconductor light-receiving device is developed with a digital alloy structure comprising alternately laminated Si and AlAs layers on an InP substrate, incorporating an electric field relaxation layer and a light absorption layer, using MOVPE to form a high-quality multiplication layer that reduces noise and enhances reliability.
The solution enables the creation of a semiconductor light-receiving element with low noise and excellent reliability, capable of high-speed operation by effectively managing lattice mismatch and crystal defects, thereby improving the signal-to-noise ratio and manufacturing feasibility.
Smart Images

Figure JP2023014682_17102024_PF_FP_ABST
Abstract
Description
Semiconductor light receiving element and method for manufacturing the same
[0001] The present disclosure relates to a semiconductor light receiving element and a method for manufacturing the semiconductor light receiving element.
[0002] In recent years, the data center market has seen remarkable growth due to the spread of businesses that handle large amounts of data, video content, and other such services. This has led to an increase in demand for optical communication devices required for large-volume data communications. Avalanche photodiodes (APDs), which offer superior performance, are essential optical communication devices on the receiving side of communication data, not only for short-distance communications but also for long-distance communications between data centers.
[0003] The APD used on the receiving side generates photocarriers consisting of electron-hole pairs from the optical signal received during data communication and is capable of amplifying the photocarriers themselves. Therefore, by using an APD, it is possible to restore an accurate optical signal on the receiving side even during long-distance transmission where signal strength deteriorates. In addition, the use of an APD eliminates the need for an external carrier amplifier on the receiving side, which is necessary when using a normal photodetector, making it possible to miniaturize communication equipment. For this reason, APDs are used as semiconductor photodetectors even for short-distance communications.
[0004] A main APD device structure used in current optical communications is the SACM (Separate Absorption, Charge and Multiplication Avalanche Photodiode) type APD structure, in which a layer that receives signal light and generates photocarriers is separated from a layer that multiplies the generated photocarriers. As an SACM APD structure, a structure formed on an InP substrate and including an InGaAs absorption layer that receives signal light and generates photocarriers, an AlInAs multiplication layer that multiplies the generated carriers, and an electric field relaxation layer that controls the electric field strength of the multiplication layer so that the photocarriers can be avalanche multiplied is particularly used. Photocarriers generated in the InGaAs absorption layer are reverse-biased, and electrons are conducted into the AlInAs multiplication layer, where the photocarriers are avalanche-amplified, thereby enabling the amplification of optical signals (see Patent Document 1).
[0005] As communication speeds increase, there is a demand for APDs that can operate with even lower noise than current APDs. To achieve this, it is necessary to reduce the Hall noise generated in the multiplication layer. To achieve this, APDs that suppress Hall noise during multiplication by using a germanium (Ge) absorption layer and a Si multiplication layer formed on a silicon (Si) substrate have recently begun to be used (Non-Patent Document 1).
[0006] Patent No. 4166560 Patent No. 1983-276272 Patent No. 2730472
[0007] M. Huang, et. al. , “Germanium on Silicon Avalanche Photodiode.” IEEE Journal of Selected Topics In Quantum Electronics, Vol. 24, No. 2,3800911,2018. M. Daoudi, et. al. ,”Si-delta doping and spacer thickness effects on the electronic properties in Si-delta-doped AlGaAs / GaAs HEMT structures,” Superlattices and Microstructures, Vol. 51, pp. 497-505, 2012. J. Zheng, et. al. , “Digital Alloy InAlAs Avalanche Photodopdes,” IEEE Journal of Lightwave Technology, Vol. 36, No. 17, pp. 3580-3585, 2018. D. C. Houghton, et. al. ,”Comparison of chemical beam epitaxy and metalorganic chemical vapor deposition for highly strained multiple quantum well InGaAsP / InP 1.5μm lasers. Crystal Growth, Vol. 136, pp. 56-63, 1994.
[0008] However, even now, it is extremely difficult to obtain a high-quality Ge absorption layer thicker than 1 μm due to lattice mismatch in the Ge absorption layer grown on a Si substrate. In other words, SiGe-APDs using Si substrates have problems with reliability and manufacturing technology. From the standpoint of high reliability, an AlInAs multiplication layer on an InP substrate, which is a III-V mixed crystal semiconductor material, is excellent as a multiplication layer for electron-multiplying APDs, but its noise performance is inferior to that of APDs with a Si multiplication layer.
[0009] Therefore, in order to form a Si multiplication layer on an InP substrate that is expected to reduce noise, for example, in the APD described in Patent Document 2, an attempt is made to use an InP substrate, form a light absorption layer using a III-V group alloy semiconductor having a lattice constant that is an integer ratio to the lattice constant of Si, and form the Si multiplication layer on top of the InP substrate. However, in such a structure, not only the Si multiplication layer but also the III-V group alloy semiconductor light absorption layer itself is lattice mismatched, making it difficult to obtain a high level of crystal quality that functions as a multiplication layer, and there are concerns about the reliability of the APD.
[0010] Furthermore, the semiconductor photodetector described in Patent Document 3 does not use an InP substrate, but rather describes growing a high-quality Si multiplication layer on a Si substrate, followed by forming an amorphous InGaAs layer as a light absorption layer. However, with this device structure and manufacturing method, the amorphous InGaAs layer has a high density of crystal defects, which causes a large dark current due to the crystal defects, and also raises concerns about the reliability of the APD.
[0011] In addition to the above, devices (particularly RF devices) that exhibit excellent characteristics have been realized by depositing Si itself two-dimensionally using a technique called delta doping, which involves doping Si at a high concentration in two dimensions, as in the invention described in Non-Patent Document 2. However, since APDs require a film thickness on the order of several tens of nanometers as the region where avalanche amplification occurs, there was a problem in that δ doping could not achieve a thicker film due to factors such as deterioration of the surface condition.
[0012] Recently, a paper was published stating that a technology called Digital Alloy, which makes it possible to control crystal growth at the atomic layer level, can be used to obtain semiconductors with material properties different from conventional materials for alloy semiconductor materials made of III-V alloy semiconductors (Non-Patent Document 3). By applying the Digital Alloy technology, it is possible to realize structures with material properties that have never been seen before by controlling the layer thickness of two materials with different lattice constants at the atomic layer level.
[0013] However, simply selecting and layering crystalline materials does not result in good crystal quality due to crystal defects caused by structural stress due to lattice mismatch, etc. To obtain a high-quality APD capable of high-speed operation, it is necessary to form a silicon (Si) layer on an alloy semiconductor substrate with a thickness sufficient to enable avalanche multiplication, and this is made possible by appropriately selecting materials to be layered at the atomic layer level.
[0014] The present disclosure has been made to solve the above-mentioned problems, and has as its object to provide a semiconductor light-receiving element that is low noise and has excellent reliability, and a method for manufacturing the same.
[0015] A semiconductor light receiving element according to the present disclosure includes: a semiconductor substrate; a digital alloy multiplication layer formed on the semiconductor substrate and having a digital alloy structure in which a first semiconductor layer made of a superlattice layer composed of group IV atoms and a second semiconductor layer having a band gap energy larger than that of the first semiconductor layer are alternately stacked; an electric field relaxation layer formed on the digital alloy multiplication layer and relaxing an electric field; and a light absorption layer formed on the electric field relaxation layer and absorbing incident light.
[0016] A method for manufacturing a semiconductor light-receiving element according to the present disclosure includes the steps of: epitaxially growing, on an n-type InP substrate, an n-type AlInAs buffer layer; a digital alloy multiplication layer having a digital alloy structure in which a Si layer or a layer containing Si, each having a thickness N times (1≦N≦20) the thickness of a monolayer, and an AlAs layer, each having a thickness M times (1≦M≦20) the thickness of a monolayer, are alternately stacked multiple times; a p-type AlInAs field relaxation layer; an n-type InGaAs light absorption layer; an i-type AlInAs window layer; an n-type InP window layer; and a p-type InGaAs contact layer by MOVPE; and forming Zn selective diffusion regions in parts of the n-type InP window layer and the i-type AlInAs window layer.
[0017] According to the semiconductor light-receiving element and the method for manufacturing the semiconductor light-receiving element disclosed herein, it is possible to form a high-quality digital alloy type multiplication layer containing group IV atoms on a semiconductor substrate, thereby achieving the effects of obtaining a semiconductor light-receiving element that is low noise and has excellent reliability, and of easily manufacturing such a semiconductor light-receiving element.
[0018] FIG. 1 is a cross-sectional view showing the element structure of a semiconductor light-receiving element according to a first embodiment. FIG. 2 is a diagram showing the relationship between the excess noise coefficient and the multiplication factor. FIG. 3 is a cross-sectional view showing the element structure of a semiconductor light-receiving element according to a second embodiment. FIG. 4 is a diagram showing the calculation results of the effective stress τ when the composition ratio of Si and AlAs is changed in a digital alloy type stacked structure of Si and AlAs in the semiconductor light-receiving element according to the second embodiment. FIG. 5 is a cross-sectional view showing the element structure of a semiconductor light-receiving element according to a third embodiment. FIG. 6 is a cross-sectional view showing the element structure of a semiconductor light-receiving element according to a fourth embodiment. FIG. 7 is a diagram showing the relationship between the Si sheet carrier concentration and the Si material supply amount. FIG. 8 is a cross-sectional view showing the element structure of a semiconductor light-receiving element according to a fifth embodiment.
[0019] 1 is a cross-sectional view showing the structure of a semiconductor light-receiving element 100 according to the first embodiment. An SACM-type APD is given as an example of the semiconductor light-receiving element 100 according to the first embodiment.
[0020] The semiconductor light-receiving element 100 according to the first embodiment is a semiconductor device having a carrier concentration of 1 to 5×10 18 cm -3 an n-type AlInAs buffer layer 3 having a thickness of 0.1 to 0.5 μm; an i-type Si-AlAs digital alloy multiplication layer 4 having a thickness of 0.05 to 0.2 μm and consisting of a digital alloy structure in which i-type Si layers (for example, a thickness of 2 ML) and i-type AlAs layers (for example, a thickness of 2 ML) are alternately stacked multiple times; and an i-type Si-AlAs digital alloy multiplication layer 4 having a carrier concentration of 0.5 to 1×10 18 cm -3 and a p-type AlInAs field relaxation layer 5 having a layer thickness of 0.05 to 0.15 μm and a carrier concentration of 1 to 5×10 15 cm -3and an n-type InGaAs light absorption layer 6 having a thickness of 1.0 to 1.5 μm, an i-type AlInAs window layer 7 having a thickness of 0.05 to 1 μm, and a carrier concentration of 0.1 to 5×10 15 cm -3 and an n-type InP window layer 8 having a thickness of 0.5 to 1.0 μm and a carrier concentration of 1 to 5×10 18 cm -3 and a p-type InGaAs contact layer 9 having a ring shape and a thickness of 0.1 to 0.5 μm.
[0021] The semiconductor light-receiving element 100 according to the first embodiment further includes a Zn selective diffusion region 10 (p-type conductive region) provided in a part of the n-type InP window layer 8 and the i-type AlInAs window layer 7, a SiNx surface protective film 11 provided on the surface of the n-type InP window layer 8 including the surface of the Zn selective diffusion region 10, an n-type electrode 1 provided on the back surface of the n-type InP substrate 2, and a p-type electrode 12 provided on the surface of the annular p-type InGaAs contact layer 9.
[0022] The semiconductor light-receiving element 100 according to the first embodiment is characterized in that it is configured as an i-type Si-AlAs digital alloy multiplication layer 4 having a digital alloy structure in which i-type Si layers and i-type AlAs layers are alternately stacked multiple times. In the explanation of each embodiment, the composition ratio of AlInAs and InGaAs constituting each layer except the multiplication layer is not specified, but it is desirable that both have a composition ratio that lattice matches with the n-type InP substrate 2.
[0023] The i-type Si layer mentioned above refers to a silicon superlattice layer having a layer thickness N times (1≦N≦20) that of a silicon monoatomic layer. The i-type Si layer is also referred to as the first semiconductor layer 30a, the i-type AlAs layer is also referred to as the second semiconductor layer 30b, and the i-type Si-AlAs digital alloy multiplication layer 4 is also simply referred to as the digital alloy multiplication layer.
[0024] In the above description, the i-type Si-AlAs digital alloy multiplication layer 4 is exemplified by a multiplication layer formed by alternately stacking multiple i-type Si layers each having a thickness equivalent to two monolayers (ML), i.e., 2 ML i-type Si layers and 2 ML i-type AlAs layers. However, the thickness of the i-type Si layers may be within a range of N times the thickness of a monolayer (1≦N≦20), and the thickness of the i-type AlAs layers may be within a range of M times the thickness of a monolayer (1≦M≦20). It is even more preferable if the thickness of the i-type Si layers is within a range of N times the thickness of a monolayer (1≦N≦6), and the thickness of the i-type AlAs layers is within a range of M times the thickness of a monolayer (1≦M≦6). For the i-type Si-AlAs digital alloy multiplication layer 4, when the i-type Si layers and i-type AlAs layers are alternately stacked multiple times, the number of stacking times is preferably in the range of 5 to 300.
[0025] <Method for Manufacturing Semiconductor Photodetector According to First Embodiment> The semiconductor photodetector 100 according to the first embodiment can be manufactured by forming each semiconductor layer on an InP substrate using a crystal growth method such as metal organic vapor phase epitaxy (MOVPE) or molecular beam epitaxy (MBE). A method for manufacturing an SACM-type APD, which is an example of the semiconductor photodetector 100 according to the first embodiment, will be described below.
[0026] On the surface of an n-type InP substrate 2, an n-type AlInAs buffer layer 3, an i-type Si-AlAs digital alloy multiplication layer 4 having a digital alloy structure in which i-type Si layers (2 ML thick) and i-type AlAs layers (2 ML thick) are alternately stacked multiple times, a p-type AlInAs electric field relaxation layer 5, an n-type InGaAs light absorption layer 6, an i-type AlInAs window layer 7, an n-type InP window layer 8, and a p-type InGaAs contact layer 9 are sequentially grown by crystal growth using MOVPE.
[0027] When MOVPE is used as the epitaxial crystal growth method, the crystal growth temperature is preferably about 550°C, but may be within the temperature range of 500°C to 600°C.
[0028] In the wafer process after epitaxial crystal growth, reactive ion etching, CVD (Chemical Vapor Deposition), evaporation, etc. are used to process the element region, form films, and form electrodes, thereby forming the element structure required to function as an SACM-type APD. The wafer process is described in detail below.
[0029] After epitaxial crystal growth, an SiOx film is formed on the surface of the wafer by a CVD method, etc. The SiOx film is an insulating film and functions as a diffusion mask.
[0030] Using photolithography and etching techniques, a circular pattern mask with a diameter of 20 μm is used for patterning to form circular openings in the SiOx film. Zn selective diffusion regions 10 are formed in parts of the n-type InP window layer 8 and the i-type AlInAs window layer 7 by, for example, diffusing zinc (Zn) from the openings into the semiconductor layer using the SiOx film as a diffusion mask. The tip of the Zn selective diffusion region 10 within the semiconductor layer is located in the i-type AlInAs window layer 7. The Zn selective diffusion region 10 functions as a p-type conductive region. After the Zn selective diffusion region 10 is formed, the SiOx film is removed by wet etching or dry etching.
[0031] Next, photolithography and etching techniques are used to process the p-type InGaAs contact layer 9 by reactive ion etching or the like so that it remains in a ring shape with a width of about 3.0 to 5.0 μm on the Zn selective diffusion region 10 .
[0032] After processing the p-type InGaAs contact layer 9, a SiNx surface protective film 11 is formed on the wafer surface by a CVD method or the like. Then, photolithography and etching are used to remove only the SiNx surface protective film 11 on the surface of the p-type InGaAs contact layer 9. The SiNx surface protective film 11 also functions as an anti-reflection film.
[0033] A metal material such as Ti / Au is deposited on the surface of the p-type InGaAs contact layer 9 by vapor deposition or the like to form a p-type electrode 12 .
[0034] Finally, the back surface of the n-type InP substrate 2 is ground, and then a metal material such as AuGeNi is deposited by evaporation or the like to form the n-type electrode 1. This completes the method for manufacturing the SACM-type APD, which is an example of the semiconductor photodetector 100 according to the first embodiment.
[0035] <Operation of Semiconductor Photodetector According to First Embodiment> The operation of the SACM type APD, which is an example of the semiconductor photodetector 100 according to the first embodiment fabricated by the above-described manufacturing method, will be described below.
[0036] First, a reverse bias voltage is applied from the outside so that the n-type electrode 1 provided on the back side of the n-type InP substrate 2 of the SACM APD, which is an example of the semiconductor photodetector 100, is positive and the p-type electrode 12 provided on the front side is negative. The reverse bias voltage is set to a voltage value that sufficiently generates avalanche amplification.
[0037] When a SACM APD is applied with a reverse bias voltage and light of 1.3 μm or 1.55 μm wavelength, which is a wavelength band used in optical communications, is incident on the Zn selective diffusion region 10, which is a p-type conductive region, from the p-type electrode 12 side, the light is absorbed in the n-type InGaAs light absorption layer 6, generating photocarriers (electron-hole pairs). With a reverse bias voltage applied, the electrons move to the n-type electrode 1 side and the holes move to the p-type electrode 12 side.
[0038] In an SACM APD to which a reverse bias voltage is applied, the electric field strength is controlled by the p-type AlInAs field buffer layer 5 so that avalanche amplification occurs when electrons are conducted into the i-type Si-AlAs digital alloy multiplication layer 4. In the i-type Si-AlAs digital alloy multiplication layer 4, electrons are ionized to generate new electron-hole pairs, and the newly generated electrons and holes further cause a chain reaction of ionization, resulting in avalanche amplification of the electrons and holes, i.e., avalanche amplification. In other words, electrons, which are photocarriers, are multiplied by the avalanche amplification effect in the i-type Si-AlAs digital alloy multiplication layer 4, making it possible to amplify the received optical signal.
[0039] <Function of the semiconductor light receiving element according to the first embodiment> The characteristics of the semiconductor light receiving element can be expressed by the S / N ratio, which is the ratio of signal to noise. An APD with excellent reception sensitivity has a large S / N ratio. The signal strength due to the photocurrent generated by light absorption is expressed as i s , the shot noise, which is a noise component generated inside the semiconductor light receiving element such as dark current, is i Ns , the thermal noise generated by the thermal noise amplitude due to the peripheral circuits is i Nt In this case, the S / N ratio of the semiconductor light receiving element is expressed by the following equation (1).
[0040] In particular, when the semiconductor light receiving element is an APD, the photocarriers generated by light absorption are multiplied, resulting in a signal intensity i s This increases the S / N ratio, making it possible to receive signals in long-distance communications.
[0041] Next, the elementary charge of electrons is q, the avalanche multiplication factor is M, and the average current flowing through the avalanche region of the APD is I p , the dark current multiplied in the avalanche region is I dM , excess noise factor x, bandwidth B, Boltzmann constant k, temperature T, external circuit resistance R L Then, the S / N ratio is calculated using the following equation (2).
[0042]
[0043] In equation (2), the main factor that deteriorates the S / N ratio is the multiplied dark current I, which is determined by the APD component on the denominator side. dM and the excess noise factor x included in the power of the multiplication factor M. Dark current I dM is a dark current generated when photocarriers are multiplied, and therefore is highly dependent on the crystal quality of the APD. In particular, in SiGe-APDs, the dark current increases due to crystal defects that arise in the Ge absorption layer due to the difference in lattice constant between Ge and Si, which causes a deterioration in the S / N ratio of the APD.
[0044] Regarding the excess noise factor x, which affects another characteristic of the APD, the relationship expressed by the following equation (3) holds between the excess noise factor F and the multiplication factor M.
[0045] From equation (3), it can be seen that if the excess noise factor F is known, the excess noise figure x can be calculated using the multiplication factor M. In an SACM-type APD, the excess noise factor F is expressed by the following equation (4) using the impact ionization rate ratio k, which indicates the multiplication factor ratio between holes and electrons.
[0046]
[0047] From equation (4), it can be seen that the smaller the impact ionization rate ratio k, the smaller the excess noise factor F and the smaller the excess noise exponent x, resulting in a larger S / N ratio and therefore superior noise characteristics. Figure 2 is a diagram showing the relationship between the excess noise factor F and the multiplication factor M. In general, the impact ionization rate ratio k is a value specific to the material, and for Si, k = 0.1, which is smaller than the k = 0.2 for AlInAs. Therefore, as shown in Figure 2, Si is more advantageous in terms of noise characteristics.
[0048] However, since the SiGe-APD uses Ge for the absorption layer, as mentioned above, shot noise (I dM As a result, variations in crystal quality or characteristics during manufacturing can often result in the failure to obtain a desired S / N ratio.
[0049] In contrast, in electron multiplying APDs using an InP substrate, InGaAs is used for the absorption layer and AlInAs for the multiplication layer. Both crystals are materials that are lattice-matched to the InP substrate, so crystal defects are unlikely to occur, making it possible to manufacture APDs that are low-noise and highly reliable.
[0050] In order to further improve the S / N ratio of the APD, the digital alloy technology disclosed in Non-Patent Document 2, that is, the technology of stacking different materials at atomic layer level thicknesses, is used to stack a III-V group alloy semiconductor such as AlAs or InAs at atomic layer level thicknesses while including Si in the multiplication layer, thereby enabling the crystal growth of a multiplication layer with a smaller impact ionization rate ratio k than that of conventional materials.
[0051] Since Si has a smaller lattice constant than InP or GaAs substrates, which are semiconductor materials used in the optical communication band, when growing a layered structure such as a multiplication layer containing Si, the lattice constant of the III-V mixed crystal semiconductor material must be larger than that of Si. Furthermore, since a high-quality absorption layer can be formed simultaneously with the formation of the multiplication layer, shot noise can be suppressed, making it possible to consistently manufacture APDs with higher sensitivity than conventional SACM-type APDs.
[0052] In the first embodiment, a case where a material containing Si and an AlAs layer, which is a semiconductor material different from Si, are stacked in the multiplication layer has been described as an example. Similar effects can be obtained by using a mixed crystal semiconductor material composed of a group III atomic material and a group V atomic material, such as InP, GaP, AlP, InAs, GaAs, InSb, GaSb, or AlSb, as the material for the multiplication layer. Furthermore, the crystalline material is not limited to binary compounds. Similar effects can also be obtained by stacking ternary or quaternary mixed crystal semiconductor materials, such as InGaAs, AlInAs, GaAsSb, AlGaInAs, or AlGaAsSb, at the atomic level.
[0053] As an example of the layer thickness of the layers constituting the digital alloy structure, a structure in which layers are stacked in 2ML units is given. However, the layer thickness is a critical film thickness that allows crystal growth without generating crystal defects on the base substrate, for example, a layer thickness of up to 5 nm, and any combination of layer thicknesses may be used as long as it is within a range in which the necessary constituent materials of the multiplication layer can be crystallized. Furthermore, the Si-AlAs digital alloy multiplication layer may not be i-type, i.e., undoped, as shown in the example above, but may be an n-type Si-AlAs digital alloy multiplication layer or a p-type Si-AlAs digital alloy multiplication layer by doping the entire Si-AlAs digital alloy multiplication layer with n-type or p-type impurities.
[0054] In the above example, the Zn selective diffusion region 10, which is a p-type conductive region, is formed by Zn diffusion. However, any atom that imparts p-type conductivity, other than Zn, may be used, such as Cd or Be. The Zn diffusion method may be a solid-phase diffusion method using ZnO or a Zn vapor-phase diffusion method using a crystal growth furnace. Alternatively, instead of the Zn selective diffusion region 10, a p-type contact layer may be grown by crystal growth.
[0055] In the above example, a front-illuminated structure has been described in which light to be detected is incident on the Zn selective diffusion region 10, which is a p-type conductive region, from the p-electrode 12 side. Conversely to the front-illuminated structure, a back-illuminated structure can be used in which the n-electrode 1 on the back side of the n-type InP substrate 2 is opened using a circular pattern, and light is incident from the n-type InP substrate 2 side. Furthermore, a side-illuminated structure in which light is incident from the end face of the n-type light absorption layer can also be used in which the same effect is achieved.
[0056] Effect of First Embodiment As described above, according to the semiconductor light-receiving element and the method for manufacturing a semiconductor light-receiving element according to the first embodiment, the multiplication layer is formed of a Si-AlAs digital alloy type multiplication layer having a digital alloy structure in which Si layers made of Si superlattice layers and AlAs layers are alternately stacked multiple times. This brings about the effect that a semiconductor light-receiving element with low noise and excellent reliability can be obtained, and the effect that such a semiconductor light-receiving element can be easily manufactured.
[0057] Second Embodiment <Element Structure of Semiconductor Photodetector According to Second Embodiment> Fig. 3 is a cross-sectional view showing the element structure of a semiconductor photodetector 110 according to the second embodiment. An SACM type APD is given as an example of the semiconductor photodetector 110 according to the second embodiment.
[0058] The semiconductor light-receiving element 110 according to the second embodiment is a semiconductor device having a carrier concentration of 1 to 5×10 18 cm -3an n-type AlInAs buffer layer 3 having a thickness of 0.1 to 0.5 μm; an i-type Si-AlAs digital alloy multiplication layer 4a having a thickness of 0.05 to 0.2 μm and consisting of a digital alloy structure in which i-type Si layers (for example, a thickness of 2 ML) and i-type AlAs layers (for example, a thickness of 4 ML) are alternately stacked multiple times; and an i-type Si-AlAs digital alloy multiplication layer 4b having a carrier concentration of 0.5 to 1×10 18 cm -3 and a p-type AlInAs field relaxation layer 5 having a layer thickness of 0.05 to 0.15 μm and a carrier concentration of 1 to 5×10 15 cm -3 and an n-type InGaAs light absorption layer 6 having a thickness of 1.0 to 1.5 μm, an i-type AlInAs window layer 7 having a thickness of 0.05 to 1 μm, and a carrier concentration of 0.1 to 5×10 15 cm -3 and an n-type InP window layer 8 having a thickness of 0.5 to 1.0 μm and a carrier concentration of 1 to 5×10 18 cm -3 and a p-type InGaAs contact layer 9 having a ring shape and a thickness of 0.1 to 0.5 μm.
[0059] The semiconductor light-receiving element 110 according to the second embodiment further includes a Zn selective diffusion region 10 (p-type conductive region) provided in a part of the n-type InP window layer 8 and the i-type AlInAs window layer 7, a SiNx surface protective film 11 provided on the surface of the n-type InP window layer 8 including the surface of the Zn selective diffusion region 10, an n-type electrode 1 provided on the back surface of the n-type InP substrate 2, and a p-type electrode 12 provided on the surface of the annular p-type InGaAs contact layer 9.
[0060] The semiconductor light-receiving element 110 according to the second embodiment is characterized in that the multiplication layer has a digital alloy structure in which i-type Si layers, each having a thickness N times (1≦N≦20) the thickness of a monolayer, and i-type AlAs layers, each having a thickness M times (1≦M≦20) the thickness of a monolayer, are alternately stacked multiple times, and the i-type Si-AlAs digital alloy multiplication layer 4 a has a relationship in which the number of monolayers M constituting the i-type AlAs layer is larger than the number of monolayers N constituting the i-type Si layer (N<M).
[0061] The i-type Si layer mentioned above refers to a silicon superlattice layer having a layer thickness N times (1≦N≦20) that of a silicon monoatomic layer. The i-type Si layer is also referred to as the first semiconductor layer 31a, the i-type AlAs layer as the second semiconductor layer 31b, and the i-type Si-AlAs digital alloy multiplication layer 4a is also simply referred to as the digital alloy multiplication layer.
[0062] In the above description, the i-type Si-AlAs digital alloy multiplication layer 4a is exemplified by a multiplication layer formed by alternately stacking multiple i-type Si layers each having a layer thickness equivalent to two monolayers (ML), i.e., 2 ML i-type Si layers and 4 ML i-type AlAs layers. The relationship (N<M) is satisfied, where the number of monolayers M constituting the i-type AlAs layers is greater than the number of monolayers N constituting the i-type Si layers. The thickness of the i-type Si layers may be within the range of N times the number of monolayers (1≦N≦20), and the thickness of the i-type AlAs layers may be within the range of M times the number of monolayers (1≦M≦20). It is even more preferable if the thickness of the i-type Si layers is within the range of N times the number of monolayers (1≦N≦6), and the thickness of the i-type AlAs layers is within the range of M times the number of monolayers (1≦M≦6). In the case where the i-type Si—AlAs digital alloy multiplication layer 4 is formed by alternately laminating the i-type Si layers and the i-type AlAs layers multiple times, the number of laminations is preferably in the range of 5 to 300 times.
[0063] <Method for manufacturing semiconductor light receiving element according to embodiment 2> The method for manufacturing the semiconductor light receiving element 110 according to embodiment 2 is almost the same as the method for manufacturing the semiconductor light receiving element 100 according to embodiment 1, so a detailed description of the manufacturing method will be omitted.
[0064] <Function of the Semiconductor Photodetector According to the Second Embodiment> In an APD, a layer structure is generally formed by crystal growth above the multiplication layer, from the electric field relaxation layer to the p-type contact layer, with a total layer thickness of about 2 μm. If crystal defects occur within the crystals that make up the layer structure, dark current increases and shot noise increases, deteriorating the S / N ratio of the APD and raising concerns about reliability.
[0065] The multiplication layer formed by the digital alloy technology disclosed in this application is formed by alternately stacking Si and other semiconductor materials, which have a lattice constant that does not match that of the semiconductor substrate, at the atomic layer level. Therefore, it is necessary to alternately stack layers of compressive strain and layers of tensile strain to reduce stress in the entire crystal growth layer.
[0066] In a structure in which two different materials are alternately and repeatedly laminated, the effective stress τ according to a mechanical equilibrium model, which serves as a guideline for when dislocations occur, can be calculated using the following equation (5) based on the description in Non-Patent Document 4.
[0067]
[0068] The meaning of each symbol in equation (5) is as follows: Ψ: angle between the interface and the slip plane λ: angle between the dislocation line and the Burgers spectrum ν: Poisson's ratio μ x : Shear modulus of compressive strain layer μ y : Shear modulus of tensile strain layer μ xy : Average shear modulus of the repeated laminated portion b: Burger spectrum θ: Angle between the dislocation line and the Burger spectrum β: Core parameter x: Amount of strain in the compressively strained layer h: Thickness of the compressively strained layer y: Amount of strain in the tensilely strained layer H: Thickness of the tensilely strained layer Z: Thickness of the strain relaxation layer N: Number of compressively strained layers L: Calculated value of Nh + (N-1)H
[0069] By normalizing the calculated effective stress τ and configuring the layer structure so that the effective stress τ is 0 or less, high-quality APDs without dislocations can be grown. Figure 4 shows the calculation results of the effective stress τ when the composition ratio of the Si layer to the AlAs layer is changed in a digital alloy-type stacked structure made of Si layers and AlAs layers. When the Si layer is set to one atomic layer and the atomic layer of the AlAs layer is changed to one to three atomic layers, it can be seen that increasing the stacked composition ratio of the AlAs layer to the Si layer reduces the effective stress τ. In Figure 4, the vertical axis represents the effective stress τ in arbitrary units, and the horizontal axis represents the film thickness of the stacked structure.
[0070] The effective stress τ during crystal growth of a digital alloy multiplication layer containing Si acts to alleviate the stress of the entire laminate structure by stacking a material with a larger lattice constant than Si. However, since the materials that make up the laminate structure are themselves lattice-mismatched, the effective stress τ applied to the entire semiconductor light-receiving element gradually increases, so it is necessary to control the film thickness of the entire laminate structure to a critical film thickness at which crystal defects do not occur or less.
[0071] In the second embodiment, a combination of a Si layer and an AlAs layer has been described as an example of the digital alloy multiplication layer. Instead of the AlAs layer, a III-V group alloy semiconductor material other than AlAs may be applied. Furthermore, the III-V group alloy semiconductor material may be a ternary alloy semiconductor or a quaternary alloy semiconductor. The digital alloy multiplication layer need not be undoped, but may be doped, for example, p-type or n-type.
[0072] Effect of Second Embodiment As described above, according to the semiconductor light-receiving element of the second embodiment, the multiplication layer has a digital alloy structure in which Si layers, each having a thickness N times the monolayer, and AlAs layers, each having a thickness M times the monolayer, are alternately stacked multiple times, and the multiplication layer is an Si-AlAs digital alloy type having a relationship in which the number M of monolayers constituting the AlAs layers is greater than the number N of monolayers constituting the Si layers. Therefore, stress generated in the multiplication layer containing Si can be alleviated, and an effect is achieved in which a semiconductor light-receiving element having low noise and excellent reliability is obtained.
[0073] Third Embodiment <Element Structure of Semiconductor Photodetector According to Third Embodiment> Fig. 5 is a cross-sectional view showing the element structure of a semiconductor photodetector 120 according to the third embodiment. As an example of the semiconductor photodetector 120 according to the third embodiment, a SACM type APD is given.
[0074] The semiconductor light-receiving element 120 according to the third embodiment is a semiconductor device having a carrier concentration of 1 to 5×10 18 cm -3The n-type AlInAs buffer layer 3 has a thickness of 0.1 to 0.5 μm, the i-type Si-AlAs digital alloy multiplication layer 4 has a thickness of 0.05 to 0.2 μm and is made of a digital alloy structure in which an i-type Si layer (for example, a thickness of 2 ML) and an i-type AlAs layer (for example, a thickness of 2 ML) are alternately stacked multiple times, and the i-type Al x Ga y In 1-x-y As (x=0.25, y=0.218) transition layer 22 and a carrier concentration of 0.5 to 1×10 18 cm -3 and a p-type AlInAs field relaxation layer 5 having a layer thickness of 0.05 to 0.15 μm and a carrier concentration of 1 to 5×10 15 cm -3 and an n-type InGaAs light absorption layer 6 having a thickness of 1 to 1.5 μm, an i-type AlInAs window layer 7 having a thickness of 0.05 to 1 μm, and a carrier concentration of 0.1 to 5×10 15 cm -3 and an n-type InP window layer 8 having a thickness of 0.5 to 1 μm and a carrier concentration of 1 to 5×10 18 cm -3 and a p-type InGaAs contact layer 9 having a ring shape and a thickness of 0.1 to 0.5 μm.
[0075] The semiconductor light-receiving element 120 according to the third embodiment further includes a Zn selective diffusion region 10 provided in a part of the n-type InP window layer 8 and the i-type AlInAs window layer 7, a SiNx surface protective film 11 provided on the surface of the n-type InP window layer 8 including the surface of the Zn selective diffusion region 10, an n-type electrode 1 provided on the back surface of the n-type InP substrate 2, and a p-type electrode 12 provided on the surface of the annular p-type InGaAs contact layer 9.
[0076] The semiconductor light receiving element 120 according to the third embodiment has a multiplication layer made of an i-type Si—AlAs digital alloy multiplication layer 4 having a digital alloy structure, and a 15 nm thick i-type AlInAs layer between the i-type Si—AlAs digital alloy multiplication layer 4 and the p-type AlInAs field relaxation layer 5. x Ga y In 1-x-y The feature is that an As transition layer 22 is provided. x Gay In 1-x-y The layers other than the As transition layer 22 are the same as the layers in the semiconductor light-receiving device 100 according to the first embodiment.
[0077] <Method of Manufacturing a Semiconductor Photodetector According to the Third Embodiment> The method of manufacturing a semiconductor photodetector 120 according to the third embodiment is to further form an i-type Al layer between the i-type Si—AlAs digital alloy multiplication layer 4 and the p-type AlInAs field relaxation layer 5 having a digital alloy structure during epitaxial crystal growth. x Ga y In 1-x-y The manufacturing method differs from that of the semiconductor light-receiving element 100 according to the first embodiment only in that the As transition layer 22 is grown as a crystal, and therefore a detailed description of the manufacturing method will be omitted.
[0078] <Function of the Semiconductor Photodetector According to the Third Embodiment> In an electron multiplying APD, photocarriers generated when light is incident on the APD are conducted from the absorption layer to the multiplication layer through a layer to which a reverse bias is applied, and upon reaching the multiplication layer, the electrons are avalanche-multiplied, amplifying the carriers. The use of a multiplication layer containing Si can change the amount of band discontinuity that occurs between the absorption layer and the multiplication layer, potentially creating a band barrier that inhibits high-speed response. The band discontinuity hinders high-speed response, particularly when the multiplication factor is small and the voltage is low.
[0079] Therefore, in the semiconductor light receiving element 120 according to the third embodiment, an AlInAs quaternary alloy semiconductor material having a band gap energy value intermediate between the band gap energy of the multiplication layer and the band gap energy of the relaxation layer is provided between the i-type Si—AlAs digital alloy type multiplication layer 4 and the p-type AlInAs electric field relaxation layer 5. x Ga y In 1-x-y By using As (x = 0.25, y = 0.22) and inserting a transition layer with a thickness of about 15 nm, the band barrier when electrons are conducted to the multiplication layer can be reduced. As a result, high-speed response of the semiconductor light-receiving element 120 is possible. In addition to this effect, by growing a crystal layer with a different composition from the multiplication layer above the multiplication layer, it is expected that the effective stress τ of the entire layer structure can be partially alleviated.
[0080] In the third embodiment, an i-type Al x Ga y In 1-x-y Although an As layer was used, other alloy semiconductor materials may be used as long as they have an intermediate bandgap energy value relative to the bandgap energies of the absorption layer, buffer layer, and multiplication layer. Furthermore, if the transition layer is constructed by combining layers with the same composition as the layers that make up the digital alloy structure, it becomes easier to control crystal growth. The transition layer may be other than undoped, and may be doped, for example, p-type or n-type.
[0081] <Effects of Third Embodiment> As described above, according to the semiconductor light receiving element of the third embodiment, an i-type AlInAs layer is formed between the Si-AlAs digital alloy type multiplication layer and the p-type AlInAs field relaxation layer. x Ga y In 1-x-y The provision of the As transition layer effectively reduces the band barrier occurring between the Si-AlAs digital alloy multiplication layer and the p-type AlInAs field relaxation layer, improving carrier conductivity and resulting in a semiconductor light-receiving element capable of high-speed operation.
[0082] 6 is a cross-sectional view showing the structure of a semiconductor light-receiving element 130 according to embodiment 4. An SACM-type APD is given as an example of the semiconductor light-receiving element 130 according to embodiment 4.
[0083] The semiconductor light-receiving element 130 according to the fourth embodiment is a semiconductor device having a carrier concentration of 1 to 5×10 18 cm -3 an n-type AlInAs buffer layer 3 having a thickness of 0.1 to 0.5 μm; an i-type SiAs-AlAs digital alloy multiplication layer 4b having a thickness of 0.05 to 0.2 μm and consisting of a digital alloy structure in which i-type SiAs layers (for example, a thickness of 2 ML) and i-type AlAs layers (for example, a thickness of 2 ML) are alternately stacked multiple times; and a carrier concentration of 0.5 to 1×10 18 cm -3 and a p-type AlInAs field relaxation layer 5 having a layer thickness of 0.05 to 0.15 μm and a carrier concentration of 1 to 5×1015 cm -3 and an n-type InGaAs light absorption layer 6 having a thickness of 1.0 to 1.5 μm, an i-type AlInAs window layer 7 having a thickness of 0.05 to 1 μm, and a carrier concentration of 0.1 to 5×10 15 cm -3 and an n-type InP window layer 8 having a thickness of 0.5 to 1.0 μm and a carrier concentration of 1 to 5×10 18 cm -3 and a p-type InGaAs contact layer 9 having a ring shape and a thickness of 0.1 to 0.5 μm.
[0084] The semiconductor light-receiving element 130 according to the fourth embodiment further includes a Zn selective diffusion region 10 (p-type conductive region) provided in a part of the n-type InP window layer 8 and the i-type AlInAs window layer 7, a SiNx surface protective film 11 provided on the surface of the n-type InP window layer 8 including the surface of the Zn selective diffusion region 10, an n-type electrode 1 provided on the back surface of the n-type InP substrate 2, and a p-type electrode 12 provided on the surface of the annular p-type InGaAs contact layer 9.
[0085] The semiconductor light-receiving element 130 according to the fourth embodiment is characterized in that the multiplication layer is composed of an i-type SiAs-AlAs digital alloy multiplication layer 4b having a digital alloy structure in which i-type SiAs layers and i-type AlAs layers are alternately stacked multiple times.
[0086] The i-type SiAs layer mentioned above refers to a SiAs superlattice layer made of a compound of Si and As and having a layer thickness N times (1≦N≦20) that of a SiAs monoatomic layer. The i-type SiAs layer is also called the first semiconductor layer 32a, the i-type AlAs layer is also called the second semiconductor layer 32b, and the i-type SiAs-AlAs digital alloy multiplication layer 4b is also simply called the digital alloy multiplication layer.
[0087] In the above description, the i-type SiAs-AlAs digital alloy multiplication layer 4b is exemplified as a multiplication layer formed by alternately stacking multiple i-type SiAs layers each having a thickness equivalent to two monolayers (ML), i.e., 2 ML i-type SiAs layers and 2 ML i-type AlAs layers. The thickness of the i-type SiAs layers may be within a range of N times the thickness of a monolayer (1≦N≦20), and the thickness of the i-type AlAs layers may be within a range of M times the thickness of a monolayer (1≦M≦20). It is even more preferable if the thickness of the i-type SiAs layers is within a range of N times the thickness of a monolayer (1≦N≦6), and the thickness of the i-type AlAs layers is within a range of M times the thickness of a monolayer (1≦M≦6). In the case where the i-type SiAs-AlAs digital alloy multiplication layer 4b is formed by alternately laminating the i-type SiAs layers and the i-type AlAs layers multiple times, the number of laminations is preferably in the range of 5 to 300 times.
[0088] <Method for Manufacturing Semiconductor Photodetector According to Fourth Embodiment> The semiconductor photodetector 130 according to the fourth embodiment can be manufactured by forming each semiconductor layer on an InP substrate using MOVPE. A method for manufacturing an SACM-type APD, which is an example of the semiconductor photodetector 130 according to the fourth embodiment, will be described below.
[0089] Using MOVPE at a growth temperature of 550° C., the following are grown sequentially by crystal growth on the surface of the n-type InP substrate 2: an n-type AlInAs buffer layer 3; an i-type SiAs-AlAs digital alloy multiplication layer 4b having a digital alloy structure in which i-type SiAs layers (2 ML thick) and i-type AlAs layers (2 ML thick) are alternately stacked multiple times; a p-type AlInAs electric field relaxation layer 5; an n-type InGaAs light absorption layer 6; an i-type AlInAs window layer 7; an n-type InP window layer 8; and a p-type InGaAs contact layer 9.
[0090] When growing the i-type SiAs layer by MOVPE, the Si source is silane (SiH 4 ) and As material arsine (AsH 3 ) is used as the raw material gas.
[0091] When MOVPE is used as the epitaxial crystal growth method, the crystal growth temperature is preferably about 550°C, but may be within the temperature range of 500°C to 600°C.
[0092] The wafer process after epitaxial crystal growth is the same as in the first embodiment, and therefore a detailed description thereof will be omitted.
[0093] <Function of the semiconductor light receiving element according to the fourth embodiment> When stacking a multiplication layer containing Si at the atomic layer level, it may be difficult to form a film of simple Si depending on the crystal growth method. In particular, in the MOVPE method, it is very difficult to form a film of simple Si in a crystal growth furnace. As a countermeasure for this, for example, silane (SiH 4 ), as well as arsine (AsH 3 ), or phosphine (PH 3 ) are simultaneously introduced into a crystal growth furnace and reacted to form a layer made of a compound such as a SiAs layer or a SiP layer, which can have a structure that is easier to form than a layer made of simple silicon.
[0094] As an example, the relationship between the carrier concentration of the Si sheet and the amount of Si material supplied is shown in Figure 7. By controlling the crystal growth temperature and the amount of semiconductor material supplied in this way, it becomes possible to form a structure in which semiconductor layers made of Si and other elements are stacked, instead of Si layers stacked at the atomic layer level, and therefore it is possible to obtain the same effect as in the first embodiment.
[0095] In the fourth embodiment, silane (SiH 4 However, any material containing Si can be used as a material for crystal growth regardless of whether it is solid, liquid, or gas. In the fourth embodiment, arsine (AsH 3 ) was used, but any solid or liquid material containing As can be used as a material for crystal growth. Furthermore, if a compound with Si can be formed using a raw material containing a group V atomic material other than As, such as P or Sb, a similar effect can be obtained. Furthermore, the crystal growth method can be the MBE method as well as the MOVPE method.
[0096] Effect of Fourth Embodiment As described above, according to the semiconductor photodetector and the method for manufacturing a semiconductor photodetector according to the fourth embodiment, a SiAs-AlAs digital alloy type multiplication layer having a digital alloy structure in which SiAs layers and AlAs layers are alternately stacked multiple times is provided as the multiplication layer, which brings about the effect that a semiconductor photodetector with low noise and excellent reliability can be obtained, and the effect that such a semiconductor photodetector can be manufactured more easily.
[0097] Fifth Embodiment <Element Structure of Semiconductor Photodetector According to Fifth Embodiment> Fig. 8 is a cross-sectional view showing the element structure of a semiconductor photodetector 140 according to the fifth embodiment. An SACM type APD is given as an example of the semiconductor photodetector 140 according to the fifth embodiment.
[0098] The semiconductor light-receiving element 140 according to the fifth embodiment is a semiconductor device having a carrier concentration of 1 to 5×10 18 cm -3 an n-type AlInAs buffer layer 3 having a thickness of 0.1 to 0.5 μm; an i-type Si-Ge digital alloy multiplication layer 4c having a thickness of 0.05 to 0.2 μm and consisting of a digital alloy structure in which i-type Si layers (for example, a thickness of 2 ML) and i-type Ge layers (for example, a thickness of 2 ML) are alternately stacked multiple times; and a carrier concentration of 0.5 to 1×10 18 cm -3 and a p-type AlInAs field relaxation layer 5 having a layer thickness of 0.05 to 0.15 μm and a carrier concentration of 1 to 5×10 15 cm -3 and an n-type InGaAs light absorption layer 6 having a thickness of 1.0 to 1.5 μm, an i-type AlInAs window layer 7 having a thickness of 0.05 to 1 μm, and a carrier concentration of 0.1 to 5×10 15 cm -3 and an n-type InP window layer 8 having a thickness of 0.5 to 1.0 μm and a carrier concentration of 1 to 5×10 18 cm -3 and a p-type InGaAs contact layer 9 having a ring shape and a thickness of 0.1 to 0.5 μm.
[0099] The semiconductor light-receiving element 140 according to the fifth embodiment further includes a Zn selective diffusion region 10 (p-type conductive region) provided in a part of the n-type InP window layer 8 and the i-type AlInAs window layer 7, a SiNx surface protective film 11 provided on the surface of the n-type InP window layer 8 including the surface of the Zn selective diffusion region 10, an n-type electrode 1 provided on the back surface of the n-type InP substrate 2, and a p-type electrode 12 provided on the surface of the annular p-type InGaAs contact layer 9.
[0100] The semiconductor light receiving element 140 according to the fifth embodiment is characterized in that the multiplication layer is composed of an i-type Si-Ge digital alloy multiplication layer 4c having a digital alloy structure in which i-type Si layers and i-type Ge layers are alternately stacked multiple times.
[0101] The i-type Si layer refers to a silicon superlattice layer having a layer thickness N times (1≦N≦20) that of a silicon monoatomic layer, and the i-type Ge layer refers to a silicon superlattice layer having a layer thickness M times (1≦M≦20) that of a germanium monoatomic layer. The i-type Si layer is also referred to as the first group IV atomic superlattice layer 33a, the i-type Ge layer is also referred to as the second group IV atomic superlattice layer 33b, and the i-type Si-Ge digital alloy multiplication layer 4c is also simply referred to as the digital alloy multiplication layer.
[0102] In the above description, the i-type Si—Ge digital alloy multiplication layer 4c is exemplified as a multiplication layer formed by alternately stacking multiple i-type Si layers each having a thickness equivalent to two monolayers (ML), i.e., 2ML i-type Si layers and 2ML i-type Ge layers. However, the thickness of the i-type Si layers may be within a range of N times the thickness of a monolayer (1≦N≦20), and the thickness of the i-type Ge layers may be within a range of M times the thickness of a monolayer (1≦M≦20). It is even more preferable if the thickness of the i-type Si layers is within a range of N times the thickness of a monolayer (1≦N≦6), and the thickness of the i-type Ge layers is within a range of M times the thickness of a monolayer (1≦M≦6). For the i-type Si—Ge digital alloy multiplication layer 4c, when the i-type Si layers and i-type Ge layers are alternately stacked multiple times, the number of stacking times is preferably in the range of 5 to 300.
[0103] <Method for Manufacturing Semiconductor Photodetector According to Fifth Embodiment> The semiconductor photodetector 140 according to the fifth embodiment can be manufactured by forming each semiconductor layer on an InP substrate using MOVPE. A method for manufacturing an SACM-type APD, which is an example of the semiconductor photodetector 140 according to the fifth embodiment, will be described below.
[0104] Using MOVPE at a growth temperature of 550° C., the following are grown by crystal growth in sequence on the surface of the n-type InP substrate 2: an n-type AlInAs buffer layer 3; an i-type Si—Ge digital alloy multiplication layer 4 c having a digital alloy structure in which i-type Si layers (2 ML thick) and i-type Ge layers (2 ML thick) are alternately stacked multiple times; a p-type AlInAs electric field relaxation layer 5; an n-type InGaAs light absorption layer 6; an i-type AlInAs window layer 7; an n-type InP window layer 8; and a p-type InGaAs contact layer 9.
[0105] When growing the i-type Si layer by MOVPE, the Si source is silane (SiH 4 ) is used as a source gas. When growing the i-type Ge layer by MOVPE, germane (GeH 4 ) is used as the raw material gas.
[0106] When MOVPE is used as the epitaxial crystal growth method, the crystal growth temperature is preferably about 550°C, but may be within the temperature range of 500°C to 600°C.
[0107] The wafer process after epitaxial crystal growth is the same as in the first embodiment, and therefore a detailed description thereof will be omitted.
[0108] <Function of the semiconductor photodetector according to the fifth embodiment> In addition to the combination of Si and group V atomic material shown in the first embodiment, the same effect as the APD can be expected even if the group V atomic material is replaced with Ge or carbon (C), which is a group IV atomic material. Because Ge or C is the same group IV atomic material as Si, it can also be expected to have the effect of partially improving interface control during crystal growth. Furthermore, if Ge or C is used, the band gap value can be changed more than with the above-mentioned Si material, and therefore it becomes possible to control the energy barrier of electrons in the conduction band, as explained in the third embodiment.
[0109] <Effects of Semiconductor Photodetector According to Fifth Embodiment> As described above, according to the semiconductor photodetector according to the fifth embodiment, a Si-Ge digital alloy type multiplication layer having a digital alloy structure in which Si layers and Ge layers are alternately stacked multiple times is provided as the multiplication layer. This reduces the energy barrier when carriers are conducted from the absorption layer to the multiplication layer containing Si, thereby providing an effect of obtaining a semiconductor photodetector capable of high-speed operation.
[0110] Although the present disclosure describes various exemplary embodiments and examples, the various features, aspects, and functions described in one or more embodiments are not limited to application to a particular embodiment, but may be applied to the embodiments alone or in various combinations.
[0111] Therefore, countless variations not illustrated are conceivable within the scope of the technology disclosed in the present specification, including, for example, cases where at least one component is modified, added, or omitted, and cases where at least one component is extracted and combined with components of another embodiment.
[0112] 1 n-type electrode, 2 n-type InP substrate, 3 n-type AlInAs buffer layer, 4 i-type Si-AlAs digital alloy multiplication layer, 4a i-type Si-AlAs digital alloy multiplication layer, 4b i-type SiAs-AlAs digital alloy multiplication layer, 4c i-type Si-Ge digital alloy multiplication layer, 5 p-type AlInAs field relaxation layer, 6 n-type InGaAs light absorption layer, 7 i-type AlInAs window layer, 8 n-type InP window layer, 9 p-type InGaAs contact layer, 10 Zn selective diffusion region, 12 p-type electrode, 22 i-type Al x Ga y In 1-x-y As transition layer, 30a, 31a, 32a; first semiconductor layer, 30b, 31b, 32b; second semiconductor layer, 33a; first group IV atomic superlattice layer, 33b; second group IV atomic superlattice layer, 100, 110, 120, 130, 140; semiconductor light-receiving element
Claims
1. A semiconductor light receiving element comprising: a semiconductor substrate; a digital alloy type multiplication layer formed on the semiconductor substrate and having a digital alloy structure in which a first semiconductor layer made of a superlattice layer composed of Group IV atoms and a second semiconductor layer having a larger band gap energy than the first semiconductor layer are alternately stacked; an electric field relaxation layer formed on the digital alloy type multiplication layer and relaxing the electric field; and a light absorption layer formed on the electric field relaxation layer and absorbing incident light.
2. The semiconductor light-receiving element according to claim 1, characterized in that the first semiconductor layer is a Si superlattice layer having a layer thickness N times (1≦N≦20) that of a Si monolayer, and the second semiconductor layer has a layer thickness M times (1≦M≦20) that of a monolayer and is a layer made of a semiconductor having a lattice constant larger than that of Si.
3. The semiconductor light-receiving element according to claim 2, wherein the second semiconductor layer has a thickness greater than that of the first semiconductor layer.
4. The semiconductor light-receiving element according to claim 1, wherein the first semiconductor layer is a Si-containing superlattice layer made of Si and group V atoms and having a layer thickness N times (1≦N≦20) that of a monoatomic layer, and the second semiconductor layer is made of a III-V group mixed crystal semiconductor and has a layer thickness M times (1≦M≦20) that of a monoatomic layer.
5. A semiconductor light-receiving element according to any one of claims 1 to 3, characterized in that the second semiconductor layer is made of a III-V group mixed crystal semiconductor.
6. A semiconductor light-receiving element comprising: a semiconductor substrate; a digital alloy type multiplication layer formed on the semiconductor substrate and having a digital alloy structure in which a first group IV atomic superlattice layer made of first group IV atoms and having a layer thickness N times (1≦N≦20) that of a monoatomic layer and a second group IV atomic superlattice layer made of second group IV atoms different from the first group IV atoms and having a layer thickness M times (1≦M≦20) that of a monoatomic layer are alternately laminated; an electric field relaxation layer formed on the digital alloy type multiplication layer and relaxing an electric field; and a light absorption layer formed on the electric field relaxation layer and absorbing incident light.
7. A semiconductor light-receiving element according to any one of claims 1 to 6, characterized in that a transition layer for relaxing distortion is provided between said digital alloy type multiplication layer and said electric field relaxation layer.
8. A method for manufacturing a semiconductor light-receiving element, comprising: a step of epitaxially growing, on an n-type InP substrate, an n-type AlInAs buffer layer, a digital alloy type multiplication layer having a digital alloy structure in which a Si layer or a layer containing Si, each having a thickness N times (1≦N≦20) a monolayer, and an AlAs layer having a thickness M times (1≦M≦20) a monolayer, are alternately stacked multiple times, a p-type AlInAs electric field relaxation layer, an n-type InGaAs light absorption layer, an i-type AlInAs window layer, an n-type InP window layer, and a p-type InGaAs contact layer, in sequence by MOVPE; and a step of forming a Zn selective diffusion region in a portion of the n-type InP window layer and the i-type AlInAs window layer.
9. The method for producing a semiconductor light-receiving element according to claim 8, wherein the crystal growth temperature by said MOVPE method is within the range of 500° C. to 600° C.
10. The method for producing a semiconductor light-receiving element according to claim 8 or 9, characterized in that silane is used as a source gas for Si during crystal growth of the Si layer or the layer containing Si by the MOVPE method.
Citation Information
Patent Citations
1.55-micron wave band avalanche photodetector and preparation method thereof
CN114361285A
Semiconductor photodetector
JP1982036876A
Light receiving semiconductor device
JP2002170983A
Method for forming strained silicon material with improved thermal conductivity
JP2008509562A
semiconductor optical modulator
JP7220837B1