Polymer material containing chemically modified polysaccharide

A water-soluble, antibacterial hydrogel is achieved by forming hydrogen bonds between a hydrophilic chitosan derivative and a neutral polysaccharide, addressing the challenge of creating chitosan-based hydrogels with improved mechanical and antibacterial properties for various biomedical applications.

WO2024214274A1PCT designated stage expired Publication Date: 2024-10-17SMART TISSUES KK
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/015143
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Conventional methods struggle to create hydrogels with chitosan that are water-soluble while maintaining antibacterial properties, as chitosan is insoluble in water and organic solvents.

Method used

A polymer material composed of a hydrophilic chitosan derivative and a neutral hydrophilic polysaccharide, such as methacrylated dextran, that form hydrogen bonds and can be photocrosslinked to create a water-soluble, antibacterial hydrogel.

Benefits of technology

The resulting hydrogel exhibits improved mechanical properties and maintains antibacterial activity, making it suitable for applications in bioprinting, tissue engineering, and drug delivery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

[Problem] To provide a biological material using chitosan, especially a hydrogel material, having mechanical properties applicable to various uses while maintaining the antibacterial properties of chitosan. [Solution] It was discovered that, by using a polymer material containing a hydrophilic chitosan derivative and two kinds of neutral, hydrophilic polysaccharides capable of forming a hydrogen bond between the chitosan derivative and the molecule, a hydrogel having mechanical properties applicable to various uses while maintaining the antibacterial properties of chitosan can be obtained by a means such as photocrosslinking.
Need to check novelty before this filing date? Find Prior Art

Description

Chemically modified polysaccharide-containing polymeric materials

[0001] The present invention relates to polymeric materials comprising chemically modified polysaccharides that crosslink with each other to form antimicrobial hydrogels, bioprinting matrices comprising the polymeric materials, and other uses.

[0002] Bacterial infections represent one of the world's largest public healthcare challenges. Specifically, wound infections, one of the most common infectious diseases, are a major cause of morbidity and mortality. Meanwhile, contamination of cell cultures by bacteria and other microorganisms remains a major concern for researchers, especially in 3D culture systems, where detection by visual tracking is more complex than in conventional 2D cultures. One of the most common methods for preventing bacterial contamination in vitro is the use of antibiotics. However, previous studies have raised concerns that antibiotics may induce changes in gene expression and regulation within cells.

[0003] Chitosan, a cationic polysaccharide derived from chitin, is a renewable polymer that is biodegradable, biocompatible, non-toxic, and antibacterial, and is expected to find applications in fields such as medicine, cosmetics, the food industry, and agriculture (e.g., Non-Patent Document 1). However, because most of the sugar units of chitosan contain primary amino groups, it is insoluble in water, organic solvents, and alkaline solutions, although it is soluble in dilute acids.

[0004] Therefore, it has been difficult to create materials such as hydrogels that contain water as a solvent while maintaining the antibacterial properties of chitosan.

[0005] Dash et al., Progress in Polymer Science, Vol. 36, 981-1014, 2011

[0006] Therefore, an object of the present invention is to provide a biomaterial, particularly a hydrogel material, that uses chitosan and has mechanical properties that make it applicable to a variety of uses while maintaining the antibacterial properties of chitosan.

[0007] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have found that by using a polymer material containing two types of polysaccharides, namely, a hydrophilic chitosan derivative and a neutral hydrophilic polysaccharide capable of forming intermolecular hydrogen bonds with the hydrophilic chitosan derivative, it is possible to obtain a hydrogel having mechanical properties applicable to a variety of uses by means of photocrosslinking or the like while maintaining the antibacterial properties of chitosan, and have thus completed the present invention.

[0008] That is, in one aspect, the present invention provides: <1> a polymer material comprising: a) a first polysaccharide having repeating units containing two types of sugar units, d-glucosamine and N-acetyl-d-glucosamine, the first polysaccharide having a structure in which at least a portion of the amino groups in the d-glucosamine are substituted with sites having carboxyl groups to form amide bonds; and b) a second polysaccharide having a structure in which at least a portion of the hydroxyl groups in the repeating units are substituted with functional groups selected from the group consisting of acrylic groups and methacrylic groups, the first polysaccharide and the second polysaccharide both being water-soluble and capable of forming a hydrogel by crosslinking with each other; <2> the polymer material according to claim 1, in which hydrogen bonds are formed between the first polysaccharide and the second polysaccharide; <3> The polymer material according to <1> above, wherein the carboxyl group-containing moiety in the first polysaccharide contains a sugar acid formed by oxidizing a monosaccharide and / or a disaccharide; <4> The polymer material according to <2> above, wherein the sugar acid contains a galactosyl group; <5> The polymer material according to <2> above, wherein the sugar acid is selected from the group consisting of lactobionic acid, threonic acid, xylonic acid, and gluconic acid derivatives having one or more sugar structures; <6> The polymer material according to <1> above, wherein the introduction rate of the carboxyl group-containing moiety in the first polysaccharide is 1 to 10%; <7> The polymer material according to <1> above, wherein the functional group in the second polysaccharide is a methacrylic group; <8> The polymer material according to <1> above, wherein the first polysaccharide has a weight-average molecular weight (Mw) in the range of 50 to 2000 kDa; <9> The polymer material according to the above <1>, wherein the second polysaccharide has a weight-average molecular weight (Mw) in the range of 4 to 2000 kDa; <10> The polymer material according to the above <1>, wherein the first polysaccharide has antibacterial activity; <11> The polymer material according to the above <1>, wherein the first polysaccharide is a modified polysaccharide of a cationic polysaccharide; <12> The polymer material according to the above <10>, wherein the cationic polysaccharide is chitosan or a chitosan derivative; <13> The polymer material according to the above <1>, wherein the first polysaccharide comprises the following repeating unit: <14> The polymer material according to the above <1>, wherein the second polysaccharide is a modified polysaccharide of a neutral water-soluble polysaccharide; <15> The polymer material according to the above <13>, wherein the neutral water-soluble polysaccharide comprises a repeating unit selected from the group consisting of glucose, galactose, mannose, and combinations thereof; <16> The polymer material according to the above <1>, wherein the second polysaccharide is selected from the group consisting of dextran, chitosan, locust bean gum, caregeenan, and derivatives thereof; <17> The polymer material according to the above <1>, wherein the second polysaccharide comprises the following repeating unit: <18> The polymer material according to the above <1>, wherein the second polysaccharide is a methacrylated dextran at least partially containing the following repeating unit: <19> The polymer material according to the above <1>, wherein the molar ratio of the first polysaccharide to the second polysaccharide is in the range of 1:0.1 to 1:10; <20> The polymer material according to the above <1>, wherein the first polysaccharide and the second polysaccharide have the same polymer backbone and optionally have different chemical modifications; <21> The polymer material according to the above <1>, further comprising a crosslinking agent; <22> The polymer material according to the above <21>, wherein the crosslinking agent is a water-soluble photocrosslinking agent; and <23> The polymer material according to the above <1>, for use as a matrix in bioprinting; for encapsulating proteins, particles, or exosomes; or for drug delivery.

[0009] In another aspect, the present invention also relates to a bioprinting matrix comprising the above-mentioned gel material and uses thereof, and provides: <24> a bioprinting matrix comprising the polymer material according to any one of the above <1> to <23>, wherein the first polysaccharide and the second polysaccharide are crosslinked to each other during bioprinting to form a hydrogel; <25> a bioprinting matrix according to the above <24>, which has antibacterial activity and low toxicity; and <26> use of the polymer material according to any one of the above <1> to <23> or the matrix according to the above <24> or <25> in bioprinting; encapsulation of proteins, particles, or exosomes; or drug delivery.

[0010] According to the present invention, it is possible to obtain an antibacterial composite hydrogel that has mechanical properties applicable to various applications by means of photocrosslinking, etc., while maintaining the antibacterial properties of chitosan. The mechanical properties of such hydrogels are improved by the formation of hydrogen bonds between two types of polysaccharides contained in the polymer material.

[0011] Furthermore, the polymer material of the present invention is biocompatible, water-soluble, and antibacterial, and can easily gel upon irradiation with light, making it useful as a matrix for 3D bioprinting. These properties make it applicable to a wide range of applications, including protein encapsulation and drug delivery, tissue engineering, cell culture, drug discovery and screening, in vitro research, tissue regeneration, and regenerative medicine.

[0012] Figure 1 shows FTIR spectra of chitosan (CH) and modified chitosan (LACH). Figure 2 shows a graph showing the inhibitory activity of chitosan (CH) and modified chitosan (LACH) against E. coli growth in the presence of chitosan (CH) and modified chitosan (LACH). The final polysaccharide concentrations in the graph are in % wt / v. Figure 3A shows a graph of bacterial growth rate in the presence of polysaccharide, and Figure 3B shows an image of CFU on an agar plate after 24 hours of incubation. Figure 4 shows a graph showing the enzymatic degradation behavior of the hydrogel. Figure 5 shows the printing characteristics of the LACH / DEXMA solution: Figure 5A shows an image of continuous filament formation (shear-thinning behavior) as the precursor polymer solution is extruded; Figure 5B shows a screenshot of the print preview; Figure 5C shows an image of the bioprinting process; Figure 5D shows an image of the printed construct; and Figure 5E shows an image of the square area used to calculate the printing characteristics. Figure 6 is a graph showing cell viability in gel-forming polysaccharides (gel precursor polymers). Figure 7 is a graph showing cell viability in photocrosslinked gels. Figure 8 is a flow diagram showing the procedure for the protein release assay of Example 7. Figure 9 is a graph showing the kinetic profile of protein release from photocrosslinked gels.

[0013] The following describes embodiments of the present invention. The scope of the present invention is not limited to these descriptions, and other than the following examples, the present invention can be implemented with appropriate modifications within the scope that does not depart from the spirit of the present invention.

[0014] 1. Polymer Material of the Present Invention The polymer material of the present invention comprises a) a first polysaccharide and b) a second polysaccharide, both of which are water-soluble and capable of forming a hydrogel by crosslinking with each other.

[0015] 1-1. First Polysaccharide The first polysaccharide of the present invention is a polysaccharide having repeating units containing two types of sugar units, d-glucosamine and N-acetyl-d-glucosamine. The first polysaccharide has a structure in which at least a portion of the amino groups in the d-glucosamine are substituted with sites having carboxyl groups to form amide bonds. This chemical modification can increase the water solubility of the first polysaccharide.

[0016] In a preferred embodiment, the "carboxyl group-containing moiety" includes a sugar acid formed by oxidation of a monosaccharide and / or a disaccharide. Such a sugar acid preferably contains a galactosyl group. For example, the sugar acid may be selected from the group consisting of lactobionic acid, threonic acid, xylonic acid, and gluconic acid derivatives having one or more sugar structures.

[0017] In a preferred embodiment, the first polysaccharide may be a modified cationic polysaccharide. Typical examples of such cationic polysaccharides include, but are not limited to, chitosan and chitosan derivatives. Chitosan and chitosan derivatives are preferred because of their antibacterial activity.

[0018] A non-limiting example of the first polysaccharide is a galactosylated chitosan that at least partially comprises the following repeating units:

[0019] Here, the introduction rate of the carboxyl group-containing moiety in the first polysaccharide can be preferably 1 to 10%. This makes it possible to increase the water solubility of the first polysaccharide while maintaining the inherent properties of the first polysaccharide, such as antibacterial activity. Here, the "introduction rate" refers to the proportion of amino groups in the first polysaccharide that are substituted with the carboxyl group-containing moiety.

[0020] The first polysaccharide also preferably has a weight average molecular weight (Mw) in the range of 50 to 2000 kDa.

[0021] 1-2. Second Polysaccharide The second polysaccharide of the present invention has a structure in which at least a portion of the hydroxyl groups in the repeating unit are substituted with a functional group selected from the group consisting of an acrylic group and a methacrylic group. The functional group is a methacrylic group. The presence of such a functional group can increase the water solubility of the second polysaccharide.

[0022] The second polysaccharide is preferably a modified polysaccharide of a neutral water-soluble polysaccharide. That is, the first polysaccharide is preferably a cationic polysaccharide, whereas the second polysaccharide is preferably neutral and uncharged. This is preferable from the viewpoint of preventing electrostatic interactions with the first polysaccharide and avoiding pH dependency in solubility.

[0023] The neutral water-soluble polysaccharide may be, for example, a polysaccharide containing a repeating unit selected from the group consisting of glucose, galactose, mannose, and combinations thereof. More specifically, the second polysaccharide may be selected from the group consisting of dextran, chitosan, locust bean gum, carrageenan, and derivatives thereof, and may have the above-mentioned functional group. Preferably, the second polysaccharide is dextran, chitosan, or a derivative thereof.

[0024] A non-limiting example of the second polysaccharide is a methacrylated dextran that includes, at least in part, the following repeating units: (In the formula, n is a natural number from 2 to 1000.)

[0025] In another preferred embodiment, the second polysaccharide may include, but is not limited to, methacrylated chitosan, which at least partially comprises the following repeating units:

[0026] The second polysaccharide may preferably have a weight average molecular weight (Mw) in the range of 4 to 2000 kDa.

[0027] In the present invention, both the first polysaccharide and the second polysaccharide are water-soluble polysaccharides. Typically, the first polysaccharide is the above-mentioned galactosylated chitosan, and the second polysaccharide is methacrylated dextran or methacrylated chitosan.

[0028] For example, when the first polysaccharide is a chitosan and the second polysaccharide is a dextran, hydrogen bonds can be formed between the amino groups of the chitosan and the hydroxyl groups of the dextran. These hydrogen bonds are weaker than the electrostatic interactions of other polyanionic polymers. The antibacterial properties of chitosan are derived from the electrostatic interactions between the amino groups of the sugar moiety and the negatively charged cell walls of bacterial cells. Therefore, the antibacterial properties of chitosan can be maintained by using a neutral dextran or the like as the first polysaccharide.

[0029] In another preferred embodiment, the first and second polysaccharides have the same polymer backbone and may optionally have different chemical modifications, such as a combination of a galactosylated chitosan as the first polysaccharide and a methacrylated chitosan as the second polysaccharide.

[0030] In a preferred embodiment, the molar ratio of the first polysaccharide to the second polysaccharide in the polymer material of the present invention is preferably in the range of 1:0.1 to 1:10. However, this molar ratio can be appropriately changed depending on the type of polysaccharide, etc., from the viewpoint of ease of hydrogel formation, as described below. For example, the first polysaccharide can have a concentration typically in the range of 10 to 100 mg / ml, preferably 25 to 50 mg / ml, and the second polysaccharide can have a concentration typically in the range of 30 to 200 mg / ml, preferably 50 to 100 mg / ml.

[0031] Also in a preferred embodiment, the first polysaccharide and the second polysaccharide have the same polymer backbone, optionally with different chemical modifications.

[0032] 1-3. Other Components The first polysaccharide and the second polysaccharide contained in the polymer material of the present invention can form a hydrogel by crosslinking with each other. Therefore, the polymer material of the present invention can contain an optional crosslinking agent in addition to the first and second polysaccharides. The crosslinking agent can be added at a concentration preferably in the range of 1 to 10 mg / ml, more preferably 2 to 5 mg / ml.

[0033] Such crosslinking agents may be those known in the art, such as photopolymerization initiators or water-soluble azo polymerization initiators, such as 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (Irgacure 2959) and 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide (VA-086)].

[0034] Preferably, the crosslinking agent contained in the polymer material of the present invention is a water-soluble photocrosslinking agent. The light irradiation time for photocrosslinking is not particularly limited, but is typically in the range of 1 to 30 minutes.

[0035] In this specification, the term "gel" generally refers to a dispersion system of polymers that has high viscosity and has lost fluidity, and in which the storage modulus G' and loss modulus G" satisfy the relationship G'≧G". A gel that uses water as a solvent is called a "hydrogel".

[0036] The polymeric materials of the present invention are applicable to a wide range of applications, including tissue engineering, cell culture, drug discovery and screening, in vitro research, tissue regeneration, and regenerative medicine. More specifically, such applications include, for example, matrices for bioprinting; encapsulation of proteins, particles, or exosomes; and drug delivery.

[0037] In particular, the polymer material of the present invention is biocompatible, water-soluble, and antibacterial, and can easily gel upon irradiation with light or other means, making it useful as a matrix for 3D bioprinting. Therefore, the present invention also provides a bioprinting matrix that includes the above polymer material and forms a hydrogel by crosslinking the first polysaccharide and the second polysaccharide with each other during bioprinting. The matrix is ​​characterized by its antibacterial activity and low toxicity.

[0038] In another aspect, the present invention provides the use of the polymer material or the matrix in bioprinting; encapsulation of proteins, particles or exosomes; or drug delivery.

[0039] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0040] 1. Preparation of Polymer Material The polymer material of the present invention was prepared and a hydrogel was formed from the polymer material according to the following procedure.

[0041] [Reaction 1: Synthesis of Water-Soluble Chitosan] A water-soluble chitosan material corresponding to the first polysaccharide was prepared by introducing hydrophilic functional groups into chitosan. Specifically, as shown in Scheme 1, chitosan was reacted with lactobionic acid (galactosylation reaction) to modify the amino groups in the chitosan molecule. This reaction yielded a soluble galactosylated chitosan that was soluble up to 60 mg / ml in buffers in the physiological pH range.

[0042]

[0043] The formation of galactosylated chitosan was confirmed by FTIR. The wavenumber region used for the measurement was 4000 to 1000 cm -1 Figure 1 shows the FTIR spectra of chitosan before (left: CH) and after modification with lactobionic acid (LA) (right: LACH). The most representative change that confirms the successful chemical modification is the 1653 cm peak, which corresponds to the stretching of the CO bond of the acetamide group of chitosan.-1 From 1625 cm -1 and the shift of the absorption band to 1597 cm corresponding to the amino groups of polysaccharides. -1 From 1532 cm -1 These changes are due to the formation of new amide bonds between the amino group of CH and the carboxyl group of LA.

[0044] Reaction 2: Modification of the Second Polysaccharide The second polysaccharide of the present invention involves methacrylation by reaction of hydroxyl groups present in the starting polysaccharide with methacrylic anhydride (MA) or glycidyl methacrylate (GMA), which introduces double bond moieties into the second polysaccharide that can be converted to crosslinks by UV light activation.

[0045] Specifically, dextran (DEX) was reacted with glycidyl methacrylate (GMA) to obtain methacrylated dextran (DEXMA), as shown in Scheme 2. The reaction was confirmed by NMR.

[0046] Reaction 1 The results were confirmed by H-NMR (solvent: DMSO-d 6 As a result, the proton peaks in the δ range of 5 to 4.4 ppm represent the anomeric protons in the anhydroglucose units of dextran. The peaks of the acrylic group (-CH=CH2), which are not present in unmodified dextran, appeared in the δ range of 5.6 to 6.3 ppm, indicating that methacrylated dextran was obtained.

[0047] [Reaction 3: Mixing of the first and second polysaccharides] Next, the water-soluble chitosan (LACH: the first polysaccharide) synthesized above was mixed with methacrylated dextran (DEXMA: the second polysaccharide), which resulted in the formation of hydrogen bonds between the amino groups of LACH and the hydroxyl groups of DEXMA, as shown in Scheme 3.

[0048] [Reaction 4: Addition of Photocrosslinker] A water-soluble photocrosslinker was added to the mixture of the first and second polysaccharides, and then the mixture was irradiated with light for a short period of time to cause gelation. The photocrosslinker may be a compound that is activated by UV or visible light.

[0049] 2. Investigation of gelation conditions The first and second polysaccharides, LACH and DEXMA, synthesized above, were dissolved in PBS and photocrosslinked in the presence of Irgacure 2959 or VA-086 (2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide]) as a crosslinker. Photocrosslinking was performed by irradiating a 30 μL polymer droplet with 365 nm light at 5 mW / cm. 2 The light source was irradiated at an intensity of 1000 nm at a distance of 5 cm from the light source. Table 1 shows the results of photocrosslinking using multiple concentrations of LACH with various molecular weights and DEXMA with various concentrations. Irgacure 2959 and VA-086 gave the same results at all concentrations.

[0050]

[0051] As shown in Table 1, the molecular weight of chitosan, the raw material for LACH, did not affect gelation. Under the LACH conditions used in the experiment, the minimum DEXMA concentration required for gel formation was 50 mg / ml. Lower photoinitiator concentrations or lower DEXMA concentrations tended to increase the exposure time required for gelation. Under the highest photoinitiator concentration (5 mg / ml), gel formation occurred within 1 minute at almost all LACH / DEXMA ratios. The optimal condition (number 7) in Table 1 was selected based on the potential toxicity of the photoinitiator, gelation time, and polymer ratio.

[0052] 3. Antibacterial Properties Chitosan is known to have antibacterial properties. To confirm that the modified chitosan (LACH) synthesized above also maintains its antibacterial properties, its bactericidal activity against the Gram-negative bacterium Escherichia coli (E. coli) was examined. The optical density (OD) measurement method of bacterial culture was used to estimate the cell density in liquid culture in the presence or absence of polysaccharide samples at various time points. Specifically, bacteria were cultured at 1 x 10 8The bacteria were resuspended in LB medium at a concentration of CFU / ml, and 300 μl aliquots of bacterial broth were added to 2700 μl of medium containing CH, LACH, or control. The cultures were incubated at 37°C with moderate agitation. Subsequently, 100 μL of the culture medium was sampled at hourly intervals (for the first 6 hours, including time zero) and the absorbance at 640 nm was measured using a spectrophotometer. If the medium was turbid, the sampled culture medium was diluted with PBS.

[0053] The measurement results are shown in Figure 2. As a result, it was confirmed that both chitosan (CH) and modified chitosan (LACH) have inhibitory activity against the growth of E. coli. Furthermore, the higher the concentration of these polysaccharides, the stronger the antibacterial effect.

[0054] Next, we evaluated the bactericidal effects of CH, LACH, DEXMA, and the LACH / DEXMA composite (0.5% wt / v) against Gram-negative bacteria (Escherichia coli) and Gram-positive bacteria (Staphylococcus aureus). Bacteria were incubated in the presence of polysaccharides, and optical density was measured after 24 hours (Figure 3A). Measurement results were normalized to the optical density measured at time zero (100% cultured bacteria). 100 μl of each culture broth was diluted (1:100,000) and plated on nutrient agar. Images of bacterial colony-forming units (CFUs) were taken after 24 hours of incubation (Figure 3B).

[0055] As shown in Figure 3, CH, LACH, and the LACH / DEXMA composite were found to exhibit antibacterial activity against both E. coli and Staphylococcus aureus. In contrast, the control sample (containing no polysaccharides) and DEXMA exhibited high bacterial growth rates and no antibacterial activity. These results demonstrate that both LACH and the LACH / DEXMA composite possess antibacterial activity against two of the most common bacteria found in clinical settings.

[0056] 4. In Vitro Degradation Test Hydrogels used in vivo must be degraded in a controlled manner to allow the target tissue to regenerate to its natural structure, morphology, and function. Chitosan is easily degraded by enzymes, particularly lysozyme, which is naturally present in various parts of the human body, through the cleavage of glycosidic bonds. Furthermore, dextran is known to be susceptible to enzymatic degradation by lysozyme. Therefore, the degradability of the LACH / DEXMA gel of the present invention was examined in the presence of lysozyme.

[0057] A gel precursor solution containing LACH / DEXMA was illuminated with 5 mW / cm at a distance of 5 cm from the light source. 2 Hydrogels were formed by irradiating the gel with UV light (365 nm) for 2 minutes. Low and medium molecular weight LACH were used. The composition of the gel precursor solution is shown in Table 1 above. VA-086 (2 mg / ml) was added to the gel precursor solution (PBS solution) before UV crosslinking. As a comparative example, a hydrogel consisting of DEXMA alone, without LACH, was prepared.

[0058] For degradation experiments, 100 μL droplets were crosslinked in a 24-well plate. After gelation, 500 μL of 4 mg / mL lysozyme in PBS was added to each well and incubated at 37°C with gentle agitation. At designated time intervals, the lysozyme solution was removed, and excess surface liquid from the gel samples was dried with filter paper. The weight of the gel samples was recorded, and then the gel samples were returned to the wells with freshly prepared lysozyme solution.

[0059] The degree of decomposition of the gel (% DD) was calculated using the measured weight change of the gel sample according to the following formula.

[0060] In this formula, "% DD" is the degree of decomposition of the gel, "W0" is the initial weight of the gel, and "W(t)" is the weight of the gel at the time of measurement.

[0061] The results of the degradation behavior of hydrogels affected by lysozyme activity are shown in Figure 4. It was found that hydrogels containing LACH degraded more readily over time than gels containing DEXMA alone. Furthermore, after 48 hours, different degradation behaviors were observed between gels containing low-molecular-weight LACH and gels containing medium-molecular-weight LACH. That is, hydrogels derived from low-molecular-weight chitosan exhibited accelerated degradation behavior compared to those derived from medium-molecular-weight chitosan. However, after 144 hours of incubation, both gels were approximately 50% degraded. These results confirmed that the hydrogels of the present invention have a degradation profile suitable for tissue engineering and that the degradation characteristics can be adjusted by the molecular weight of LACH.

[0062] 5. Evaluation of Printing Characteristics Next, a 3D bioprinting test was carried out using the LACH / DEXMA composite material of the present invention.

[0063] Typically, hydrogel-based inks with shear-thinning properties are used to prevent excessive shear stress during the bioprinting process, which can affect cell viability. In this regard, the LACH / DEXMA composite solution (gel precursor) of the present invention has a lower viscosity than the final hydrogel after gelation, as shown in Figure 5A, and exhibits shear-thinning behavior at an optimal composition.

[0064] The bioprinting test was performed as follows. Bioprinting was performed using a 3D Cultures Tissue Scribe bioprinter. A polymer solution containing modified chitosan (LACH), modified dextran (DEXMA), and VA-086 (composition 7 in Table 1) was loaded into a 3 ml syringe (BD Luer-Lok™) equipped with a nozzle (inner diameter 0.8 mm). A 30 x 30 mm square object with a height of 5 mm was designed and loaded into the Repetier Host program (Figure 5B). The height was adjusted by scaling the Z axis to 0.1. The nozzle was 0.8 mm, the layer thickness was 0.8 mm, the initial layer and fill layer were 0.5 mm, the fill speed was 2 mm / s, and the fill rate was 60%. A printing temperature of 25°C was used. A representative photograph of the printing process is shown in Figure 5C.

[0065] After the printing process is completed, the resulting grid area is exposed to 5 mW / cm at a distance of 5 cm from the light source. 2 The printed structure was then exposed to UV light (365 nm) for 2 minutes to form a gel through photocrosslinking (Figure 5D). The printed structure was photographed with a digital camera, and the printing properties were evaluated using the following equation:

[0066] In this equation, "A'" is the measured area of ​​the square-like region in the printed structure, and "A" is the theoretical area of ​​the originally designed square. When the bioink (LACH / DEXMA solution) is in an ideal gelation state, the extruded filaments exhibit a well-defined morphology with a three-dimensionally smooth surface and consistent width, and the printed structure forms a regular grid with square holes. A structure printed using the LACH / DEXMA gel of the present invention is shown in Figure 9E. The printing characteristic in this case was Pr = 0.93 ± 0.05.

[0067] In an ideal printing process, the structure exhibits a perfect square shape, and the printing property Pr has a value of 1. The higher the Pr value, the greater the degree of gelation of the bioink, while the lower the Pr value, the less the degree of gelation of the bioink. Generally, a printing property Pr in the range of 0.9 to 1.1 indicates that the bioink is suitable for bioprinting applications. Therefore, the polymer material of the present invention has been demonstrated to be suitable as a bioink for 3D bioprinting applications.

[0068] 6. Evaluation of Cytotoxicity in Cell Culture Next, the cytotoxicity of the polymeric materials of the present invention was evaluated. Specifically, modified chitosan (LACH) and modified dextran (DEXMA) polysaccharides were tested individually or in combination against human dermal fibroblasts (HDFa, ATCC). Cell viability, proliferation, and cytotoxicity were evaluated using the standard colorimetric XTT assay.

[0069] Cells were plated in 96-well plates at 5 × 10 cells per well in 100 μL of DMEM containing 10% FBS. 3 The cells were plated at the final density and allowed to adhere to the bottom of the well overnight. Then, under serum-free conditions, the medium was replaced with DMEM containing 0.5% w / v of the polymer sample (the same concentration as in Example 3). The cells were incubated in a 5% CO atmosphere. 2 The cells were incubated for 48 hours at 37°C in 100% CO₂Cl. After the incubation period, XTT reagent (BIOTIUM, Cat: 10060y, Lot: 17X0824) was added, and the cells were incubated for an additional 2 hours. This allowed only metabolically active cells to reduce the yellow tetrazolium salt (XTT: sodium 3'-[1-(phenylaminocarbonyl)-3,4-tetrazolium]-bis(4-methoxy-6-nitro)benzenesulfonic acid hydrate) to an orange formazan dye. The resulting color change was measured at 460 nm (reference wavelength 650 nm) using a plate reader. Data were normalized to untreated wells (100% viability).

[0070] As shown in Figure 6, cells treated with the polymeric materials of the present invention showed nearly 100% viability after the incubation period, with no significant difference observed between the groups, demonstrating that the polymeric materials (gel precursor polymers) of the present invention, either individually or in combination, are not cytotoxic.

[0071] Next, we investigated whether the encapsulated cells could survive and proliferate within the photocrosslinked hydrogel. A polymer material (precursor solution) containing LACH and DEXMA was prepared according to the composition shown in Table 1, and mesenchymal stem cells (1 × 10 6 30 μl droplets were then dispensed into wells of a 96-well plate. As a comparative example, the same cell density was resuspended in methacrylated gelatin (Gelma), the most common photocrosslinkable polymer used as a bioink. Finally, the plate was illuminated with 5 mW / cm at a distance of 5 cm from the light source. 2 The cells were then irradiated with UV light (365 nm) for 2 minutes. Cell viability was assessed using the XXT assay described above.

[0072] As shown in Figure 7, no significant differences were observed in cells resuspended in hydrogels crosslinked with the polymeric material of the present invention compared to the comparative methacrylated gelatin (Gelma). Both samples showed nearly 100% viability after the incubation period. This result indicates that the LACH / DEXMA hydrogel of the present invention is non-cytotoxic and suitable for bioprinting live cells.

[0073] 7. Evaluation of protein release capacity A protein release assay was performed using bovine serum albumin (BSA). The procedure is shown in Figure 8. After a predetermined time, all collected samples were treated with known concentrations of BSA in PBS, and the protein concentration was determined using a standard curve.

[0074] The dynamic release profile obtained is shown in Figure 9. A strong release of protein, known as the burst effect, occurred during the first 24 hours. Subsequently, sustained protein release was observed from 24 to 168 hours. In particular, the release of BSA stabilized after 48 hours. The burst effect of approximately 30% suggests that the hydrogel of the present invention can provide both the targeted initial delivery of a drug at the required dose and the subsequent long-term maintenance of a constant therapeutic concentration in the internal environment.

[0075] 8. Formation of Photocrosslinked Gels Using Other Polysaccharide Combinations To demonstrate the applicability of this system to other methacrylated derivatives, the second polysaccharide was replaced with methacrylated chitosan (MACH), which was used to form hydrogels and evaluate their gelation properties and cell viability. MACH was synthesized by reacting medium molecular weight chitosan with methacrylic anhydride.

[0076] MACH was synthesized by reacting medium molecular weight chitosan with methacrylic anhydride. 1 The peaks in the H-NMR spectrum were analyzed to confirm the generation of MACH. The characteristic peak of chitosan was found at δ 2.0 ppm (-CH of the acetylated portion of chitosan). 3 ) and δ3.1-4 ppm, which represent protons from the glucosamine ring. The acrylic group (-CH=CH 2 ) peak was observed at δ 5.6-6.3 ppm, confirming the production of methacrylated chitosan MACH.

[0077] LACH (medium molecular weight) and MACH were dissolved in PBS and photocrosslinked in the presence of the crosslinker VA-086. Photocrosslinking was performed by applying 365 nm light at 5 mW / cm to a 30 μl drop of the polymer mixture. 2 The light source was irradiated at an intensity of 1000 kJ / cm from a distance of 5 cm. The results obtained using various polymer ratios are shown in Table 2.

[0078] As shown in Table 2, MACH as the second polysaccharide was also demonstrated to form hydrogels within minutes of UV light exposure over a wide range of concentration ratios in combination with LACH as the first polysaccharide. Furthermore, the resulting gels were transparent and may be suitable for several biomedical applications, such as vitreous substitutes.

Claims

1. A polymer material comprising: a) a first polysaccharide having repeating units containing two types of sugar units, d-glucosamine and N-acetyl-d-glucosamine, the first polysaccharide having a structure in which at least a portion of the amino groups in the d-glucosamine are substituted with sites having carboxyl groups to form amide bonds; and b) a second polysaccharide having a structure in which at least a portion of the hydroxyl groups in the repeating units are substituted with functional groups selected from the group consisting of acrylic groups and methacrylic groups, wherein both the first polysaccharide and the second polysaccharide are water-soluble, and the first polysaccharide and the second polysaccharide are capable of forming a hydrogel by crosslinking with each other.

2. The polymeric material of claim 1, wherein hydrogen bonds are formed between said first polysaccharide and said second polysaccharide.

3. The polymer material of claim 1, wherein the carboxyl-containing moieties in the first polysaccharide comprise sugar acids formed by oxidation of monosaccharides and / or disaccharides.

4. The polymeric material of claim 3, wherein the sugar acid comprises a galactosyl group.

5. The polymeric material of claim 3, wherein the sugar acid is selected from the group consisting of lactobionic acid, threonic acid, xylonic acid, and gluconic acid derivatives having one or more sugar structures.

6. The polymer material according to claim 1, wherein the introduction rate of the site having a carboxyl group in the first polysaccharide is 1 to 10%.

7. The polymeric material of claim 1, wherein the functional groups on the second polysaccharide are methacrylic groups.

8. The polymeric material of claim 1, wherein the first polysaccharide has a weight average molecular weight (Mw) in the range of 50 to 2000 kDa.

9. The polymeric material of claim 1, wherein the second polysaccharide has a weight average molecular weight (Mw) in the range of 4 to 2000 kDa.

10. The polymeric material of claim 1, wherein said first polysaccharide has antibacterial activity.

11. The polymeric material of claim 1, wherein the first polysaccharide is a modified polysaccharide of a cationic polysaccharide.

12. The polymeric material of claim 11, wherein the cationic polysaccharide is chitosan or a chitosan derivative.

13. The first polysaccharide comprises the following repeating units: The polymeric material of claim 1 , which is a galactosylated chitosan comprising at least in part:

14. The polymeric material of claim 1, wherein the second polysaccharide is a modified polysaccharide of a neutral water-soluble polysaccharide.

15. The polymeric material of claim 14, wherein said neutral water-soluble polysaccharide comprises repeating units selected from the group consisting of glucose, galactose, mannose, and combinations thereof.

16. The polymeric material of claim 1, wherein said second polysaccharide is selected from the group consisting of dextran, chitosan, locust bean gum, carrageenan, and derivatives thereof.

17. The second polysaccharide comprises the following repeating units:

2. The polymeric material of claim 1, which is a methacrylated dextran comprising at least in part:

18. The second polysaccharide comprises the following repeating units:

2. The polymeric material of claim 1, which is a methacrylated chitosan comprising at least in part:

19. The polymeric material of claim 1, wherein the molar ratio of said first polysaccharide to said second polysaccharide ranges from 1:0.1 to 1:

10.

20. The polymeric material of claim 1, wherein the first polysaccharide and the second polysaccharide have the same polymer backbone and optionally different chemical modifications from each other.

21. The polymeric material of claim 1, further comprising a crosslinking agent.

22. The polymeric material of claim 21, wherein the crosslinking agent is a water-soluble photocrosslinking agent.

23. The polymeric material of claim 1 for use as a matrix in bioprinting; for encapsulation of proteins, particles or exosomes; or for drug delivery.

24. A matrix for bioprinting comprising the polymeric material of any one of claims 1 to 23, wherein the first polysaccharide and the second polysaccharide are crosslinked to each other during bioprinting to form a hydrogel.

25. The bioprinting matrix of claim 24, having antibacterial activity and low toxicity.

26. Use of a polymeric material according to any one of claims 1 to 23 or a matrix according to claim 24 or 25 in bioprinting; encapsulation of proteins, particles or exosomes; or drug delivery.

Citation Information

Patent Citations

  • Preparation method of multiple cross-linked polysaccharide injectable hydrogel

    CN104479150A

  • Crosslinkable Polysaccharides, Polycations and Lipids Useful for Encapsulation and Drug Release

    JP1995503943A

  • Chitosan derivative and active energy ray-curable resin composition including the chitosan derivative as polymerization initiator

    JP2010144076A

  • Biocompatible compositions comprising biocompatible thickening polymers and chitosan derivatives

    JP2022538467A

  • Lubricious biopolymeric network compositions and methods of making same