Method for joining members made of material containing thermoplastic resin
The method addresses deformation issues in thermoplastic resin bonding by heating only the joining area to the melting point, using controlled temperatures and cooling, resulting in strong and accurate bonding without equipment or storage complexities.
Patent Information
- Application Number
- PCT/JP2023/015188
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-17
AI Technical Summary
Existing methods for joining members made of thermoplastic resin, such as mechanical bonding and adhesive bonding, face issues like reduced strength due to openings for fasteners and the need for specialized equipment and storage for adhesives, while fusion bonding can cause deformation due to thermoplastic resin flow.
A method where two members made of thermoplastic resin are joined by heating only the joining area to the melting point of the thermoplastic resin, using a first heat source at a temperature lower than the melting point and a second heat source at a temperature higher than the melting point, with controlled cooling to prevent deformation.
This method effectively prevents deformation of both members by limiting thermoplastic resin flow to the joining area, ensuring strong and accurate bonding without the need for additional equipment or complex temperature management.
Smart Images

Figure JP2023015188_17102024_PF_FP_ABST
Abstract
Description
Method for joining components made of a material containing a thermoplastic resin
[0001] FIELD OF THE DISCLOSURE The present disclosure relates to methods for joining components made of thermoplastic-containing materials, such as thermoplastic composite materials.
[0002] Known methods for joining members made of materials containing thermoplastic resins include mechanical bonding using fasteners and adhesive bonding using thermosetting resins (adhesives).
[0003] However, in the former mechanical connection, it is necessary to provide an opening in the member for passing the fastener, and the opening may reduce the strength of the member.
[0004] Furthermore, in the latter adhesive bonding, it is necessary to evaluate the compatibility between the adhesive and the members to be bonded in advance, and furthermore, it is necessary to have equipment such as a freezer for storing the adhesive and an autoclave for hardening the adhesive during the bonding process, as well as to manage the expiration date of the adhesive, which inevitably increases costs.
[0005] For this reason, a method known as fusion bonding has been proposed in which two members to be joined are heated to melt the thermoplastic resin contained in both members, and the two members are joined via the molten thermoplastic resin.
[0006] However, in normal fusion, the two workpieces to be joined must be heated to a temperature equal to or higher than the melting point of the thermoplastic resin, and deformation due to the flow of the liquid thermoplastic resin may occur throughout both workpieces. In particular, when two workpieces of significantly different sizes are fused together, even if the deformation of the smaller workpiece is tolerable or correctable, unacceptable or irreversible deformation may occur in the larger workpiece, which is not desirable.
[0007] The present disclosure has been made in consideration of the above-mentioned problems, and aims to provide a method for joining two members made of a material containing a thermoplastic resin by fusion, which is capable of preventing deformation of both members due to flow of the thermoplastic resin in a liquid phase.
[0008] In order to solve the above problem, a bonding method of the present invention is a method for bonding a first member and a second member, both of which are made of materials containing a thermoplastic resin, and includes the steps of placing the first member on an upper surface of a first heat source, placing the second member on the upper surface of the first member with or without a bonding film made of a thermoplastic resin therebetween, positioning a second heat source above the second member, heating the first heat source to a predetermined first temperature and the second heat source to a predetermined second temperature, while lowering the second heat source and pressing its lower surface against the upper surface of the second member with a predetermined downward load applied, and cooling the first member and the second member after a predetermined holding time has elapsed since the temperature of the first heat source reached the first temperature and the temperature of the second heat source reached the second temperature, wherein the second temperature is higher than the melting point of the thermoplastic resin and lower than the thermal decomposition temperature of the thermoplastic resin, and the first temperature is lower than the melting point of the thermoplastic resin.
[0009] According to the present disclosure, when two components made of a material containing a thermoplastic resin are joined by fusion, the heating for melting the thermoplastic resin is limited to the joining area of both components, thereby achieving the excellent effect of preventing deformation caused by the flow of the thermoplastic resin in its liquid phase from occurring throughout both components.
[0010] 1 is a schematic perspective view showing the arrangement of two members made of a material containing a thermoplastic resin and equipment for joining them just before the start of a joining process by a method of an embodiment of the present disclosure; FIG. 2 is a schematic cross-sectional view at the center in the width direction (direction w in FIG. 1 ) showing a main part of the arrangement of two members made of a material containing a thermoplastic resin and equipment for joining them just before the start of a joining process by a method of an embodiment of the present disclosure; FIG. 3 is a schematic perspective view of a second heat source used in a joining process by a method of an embodiment of the present disclosure, seen from below; FIG. 4 is a schematic cross-sectional view at the center in the width direction (direction w in FIG. 4 ) showing a main part of the arrangement of two members made of a material containing a thermoplastic resin and equipment for joining them just before the start of a joining process by a method of another embodiment of the present disclosure;
[0011] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings.
[0012] FIG. 1 is a schematic perspective view showing the arrangement of two members made of a material containing a thermoplastic resin and the equipment for joining them just before the start of a joining process according to a method of an embodiment of the present disclosure, and FIG. 2 is a schematic cross-sectional view at the center in the width direction (the w direction in FIG. 1 ) showing the main parts of the arrangement.
[0013] Both figures show the state when a second member M2, also made of a material containing thermoplastic resin, is joined to the upper surface M1U of a first member M1, also made of a material containing thermoplastic resin, at the joining portion M2W.
[0014] The material containing a thermoplastic resin may be, for example, a carbon fiber reinforced plastic (CFRP) made of a thermoplastic resin (e.g., polyether ether ketone (PEEK)) as a base material and carbon fiber as a reinforcing material, but any material containing a thermoplastic resin may be used. However, it is preferable that the thermoplastic resins contained in the first member M1 and the second member M2 are the same.
[0015] In the embodiment shown in FIGS. 1 and 2 , the first member M1 is a relatively large, substantially flat, plate-like member (e.g., 2 to 3 mm thick), and the second member M2 is a relatively small, substantially L-shaped, plate-like member (e.g., 2 to 3 mm thick). The second member M2 has a region M2W to be joined to the upper surface M1U of the first member M1, which is a substantially flat, plate-like region corresponding to one side of the L (the short side in the illustrated embodiment). This region is indicated by dense hatching in FIG. 2 . More precisely, the region M2W to be joined is a region between the lower surface M2L, which contacts the upper surface M1U of the first member M1 via the bonding film F (described later), and the upper surface M2U, which is located on the opposite side of the lower surface M2L in the plate thickness direction. The region M2W has side surfaces (M2S1, M2S2, and M2S3 in the embodiment shown in FIG. 1 ) that connect the lower surface M2L and the upper surface M2U. Here, the side surface means a surface that is open to the space surrounding the welded portion M2W.
[0016] The first member M1 and the second member M2 are each molded in advance using a molding die. Immediately after molding, a release agent remains on the surfaces of both members to facilitate removal from the molding die. However, this release agent interferes with the bonding process described below. Therefore, the release agent remaining on at least the portion of the upper surface M1U of the first member M1 that contacts the bonded portion M2W of the second member M2 via the bonding film F (described later) (first bonding surface) and the lower surface M2L of the bonded portion M2W of the second member M2 (second bonding surface) is removed in advance by appropriate methods such as sanding with sandpaper or sandblasting. With this removal of the release agent, a portion of the thermoplastic resin is also removed from the region of the first member M1 near the first bonding surface and the region of the second member M2 near the second bonding surface, leaving less thermoplastic resin available for fusion bonding (described later). If it is deemed necessary to compensate for this lack of thermoplastic resin, a bonding film F, also made of a thermoplastic resin, is sandwiched between the first and second bonding surfaces. If it is determined that a sufficient amount of thermoplastic resin capable of contributing to bonding by fusion, which will be described later, remains in the region of the first member M1 near the first bonding surface and the region of the second member M2 near the second bonding surface, it is not necessary to sandwich the bonding film F between the first bonding surface and the second bonding surface. In this case, the first bonding surface comes into direct contact with the to-be-bonded portion M2W of the second member M2 without the bonding film F therebetween, and the second bonding surface comes into direct contact with the upper surface M1U of the first member M1 without the bonding film F therebetween.
[0017] 1 and 2, immediately before the start of the bonding process, the first member M1 is placed on the upper surface H1U of the first heat source H1. The second member M2 is placed on the first member M1 with a bonding film F interposed therebetween. That is, the above-mentioned bonding film F is sandwiched between the lower surface M2L of the to-be-bonded portion M2W of the second member M2 and the upper surface M1U of the first member M1. Furthermore, the second heat source H2 is positioned above the to-be-bonded portion M2W of the second member M2.
[0018] The bonding film F has substantially the same shape and size as the lower surface M2L of the to-be-bonded portion M2W of the second member M2 in plan view. The bonding film F may be made of the same thermoplastic resin as that contained in the first member M1 and the second member M2, or may be made of a different thermoplastic resin.
[0019] The first heat source H1 is a generally flat, panel-like piece of equipment made of metal, and its upper surface H1U is formed to have a shape and size that allows the entire lower surface M1L of the first member M1 to come into close contact with it. For example, if the lower surface M1L of the first member M1 is a curved surface (e.g., a convex cylindrical surface), the upper surface H1U of the first heat source H1 is formed as a curved surface (e.g., a concave cylindrical surface) having a shape complementary to the shape of the curved surface.
[0020] Furthermore, heaters are embedded inside the first heat source H1. In the embodiment shown in Fig. 1, four cartridge heaters CH are embedded substantially parallel to the upper surface H1U of the first heat source H1 and parallel to each other. Note that Fig. 1 only shows the embedding state of one cartridge heater CH in a simplified manner to avoid cluttering the illustration.
[0021] Furthermore, a temperature sensor is embedded inside the first heat source H1. In the embodiment shown in Fig. 1, one thermocouple TC is embedded so that its temperature measuring junction (not shown) is located immediately below and in the vicinity of the upper surface H1U that contacts the lower surface M2L of the joining portion M2W of the second member M2.
[0022] On the other hand, the second heat source H2 is a substantially rectangular parallelepiped component, and has a recess H2R formed in its bottom surface H2L. Although not shown, a mechanism is attached to the second heat source H2 for pressing it downward and applying a downward load L (see arrow L in FIG. 2) when its bottom surface (the upper surface H2RU of the recess H2R) is in contact with the upper surface of the second member M2 (the upper surface M2U of the welded portion M2W). The mechanism is configured to be able to change the magnitude of the load L.
[0023] In the illustrated embodiment, as shown in FIG. 3, which is a schematic perspective view of the second heat source H2 as viewed from below, the recess H2R is a depression that is open in the bottom surface H2L and front surface H2F of the second heat source H2 (the surface facing a portion other than the joining portion M2W of the second member M2 (in the illustrated embodiment, a substantially flat plate-shaped portion corresponding to the long side of the L)), and is defined by an upper surface H2RU and three side surfaces H2RS1, H2RS2, and H2RS3 that connect the upper surface H2RU and the bottom surface H2L. As described below, when the second heat source H2 is pressed down, the upper surface H2RU of the recess H2R contacts the upper surface M2U of the joint portion M2W of the second member M2, and the side surfaces H2RS1, H2RS2, and H2RS3 of the recess H2R face the side surfaces M2S1, M2S2, and M2S3 (see FIG. 1 ) of the joint portion M2W of the second member M2, respectively, with a small gap therebetween. That is, the recess H2R of the second heat source H2 is formed so as to accommodate the joint portion M2W of the second member M2 in the above-described state. The gap between the side surface of the recess H2R and the side surface of the joint portion M2W of the second member M2 can be determined appropriately, taking into consideration factors such as the horizontal positioning accuracy when the second heat source H2 is pressed down and the predicted maximum deformation of the joint portion M2W of the heated second member M2 (due to thermal expansion and / or flow of the thermoplastic resin).
[0024] A heater is embedded inside the second heat source H2. In the embodiment shown in Fig. 1, one cartridge heater CH is embedded directly above the recess H2R of the second heat source H2, approximately parallel to the upper surface H2RU of the recess H2R. Furthermore, a temperature sensor is embedded inside the second heat source H2. In the embodiment shown in Fig. 1, one thermocouple TC is embedded so that its temperature measuring junction (not shown) is located near the upper surface H2RU of the recess H2R.
[0025] In the above description, cartridge heaters have been used as examples of heaters embedded inside the first heat source H1 and the second heat source H2, but any self-heating heaters can be used. Furthermore, the number of heaters and their arrangement inside each heat source are not limited to those shown in the drawings and can be set as desired.
[0026] The lead wires of the cartridge heaters CH and the conductor wires of the thermocouples TC embedded inside the first heat source H1 and the second heat source H2, respectively, are connected to a general-purpose temperature controller (not shown), and the temperatures of the first heat source H1 and the second heat source H2 are controlled by the temperature controller as described below during the bonding process.
[0027] Although not shown, a blower is provided to blow air over the first member M1 and the second member M2 to cool them after the joining process is completed.
[0028] With the first member M1 and second member M2 to be joined, the bonding film F, and the first heat source H1 and second heat source H2 arranged as described above, a bonding process is carried out using the method of an embodiment of the present disclosure, the details of which are described below.
[0029] Here, the first member M1 and the second member M2 are assumed to contain the same thermoplastic resin, and the following three temperatures are considered to characterize the thermal properties of the thermoplastic resin: Thermal decomposition temperature (Th): The highest temperature at which the thermoplastic resin can be used without thermal decomposition; Melting point (Tm): The temperature at which the thermoplastic resin changes from a solid phase to a liquid phase; Softening point (Ts): The temperature at which the thermoplastic resin softens and becomes deformable. Note that the relationship Th > Tm > Ts usually holds. As an example, Th = approximately 400°C, Tm = approximately 305°C, and Ts = approximately 280°C.
[0030] The bonding process according to the embodiment of the present disclosure is intended to make the temperature of the bonding region between the first member M1 and the second member M2, located between the first heat source H1 (first temperature) lower than the melting point Tm of the thermoplastic resin and simultaneously make the temperature of the second heat source H2 (second temperature) higher than the melting point Tm of the thermoplastic resin, so that the temperature of the bonding region between the first member M1 and the second member M2, located between the two heat sources, reaches the melting point Tm of the thermoplastic resin. As a result, the thermoplastic resin (including the bonding film F) melts in the bonding region, i.e., in the region between the first bonding surface (the portion of the upper surface M1U of the first member M1 facing the lower surface M2L of the bonded portion M2W of the second member M2) and the second bonding surface (the lower surface M2L of the bonded portion M2W of the second member M2), thereby fusing (bonding) the two members.
[0031] The above-described fusion bonding can also be achieved by setting the temperature of the first heat source H1 higher than the melting point Tm of the thermoplastic resin and simultaneously setting the temperature of the second heat source H2 lower than the melting point Tm of the thermoplastic resin. However, because the first member M1 is a relatively large member as described above, in order to avoid thermal effects on the already molded first member M1 (particularly deformation due to the flow of the thermoplastic resin in liquid phase), it is preferable to set the temperature of the first heat source H1 lower than the melting point Tm of the thermoplastic resin and the temperature of the second heat source H2 higher than the melting point Tm of the thermoplastic resin, as described above.
[0032] In the bonding process according to the method of the embodiment of the present disclosure, the temperatures measured by the thermocouples TC embedded in the first heat source H1 and the second heat source H2 are controlled by the temperature controller described above to be the first temperature T1 and the second temperature T2, respectively.
[0033] The first temperature T1 and the second temperature T2, which are the target values for control, are ultimately determined through a preliminary experiment as described below. However, the set temperatures T1e and T2e in the preliminary experiment must satisfy the following formula 1 as a basic premise: T1e<Tm<T2e<Th (Formula 1) In the above formula, T1e<Tm is intended to prevent melting of the thermoplastic resin contained in the first member M1, and T2e<Th is intended to prevent thermal decomposition of the thermoplastic resin contained in the second member M2. Note that in order to prevent deformation due to softening of the thermoplastic resin contained in the first member M1, it is preferable that the set temperatures T1e and T2e satisfy the following formula 2. T1e<Ts<Tm<T2e<Th (Equation 2) This condition can be realized when the heat radiation from the first member M1 is small and the heat input from the first heat source H1 can efficiently raise the temperature of the joining area to the melting point Tm of the thermoplastic resin (i.e., without excessively raising the temperature of the first member M1).
[0034] For example, assuming a simple case in which the heat transfer resistances of the first member M1 and the second member M2 directly below and directly above the joining region are equal, the initial values of the set temperatures T1e and T2e can be set as follows: T1e = Tm - ΔT T2e = Tm + ΔT where 0 < ΔT < Th - Tm (preferably, Tm - Ts < ΔT < Th - Tm).
[0035] In the preliminary experiment, experimental thermocouples were embedded in advance in the joining regions (preferably, a region inside the first member M1 near the first joining surface and a region inside the to-be-joined portion M2W of the second member M2 near the second joining surface). Then, while monitoring the temperature of the joining regions using the thermocouples, a temperature controller controls the on / off of cartridge heaters CH embedded in the first heat source H1 and the second heat source H2 so that the temperatures measured by the thermocouples TC embedded in the first heat source H1 and the second heat source H2 reach the set temperatures T1e and T2e, respectively. At this time, the second heat source H2 was pressed downward from the position shown in FIG. 2 until its lower surface (the upper surface H2RU of the recess H2R) came into contact with the upper surface of the second member M2 (the upper surface M2U of the to-be-joined portion M2W), and a downward load L was applied and maintained in this state.
[0036] In this state, if the temperatures measured by the thermocouples TC embedded in the first and second heat sources H1 and H2 reach the set temperatures T1e and T2e, respectively, and the temperature measured by the experimental thermocouple embedded in the joining area reaches or exceeds the melting point Tm of the thermoplastic resin after the holding time t has elapsed, it can be determined that the two members are fused. In this case, both the first and second heat sources H1 and H2 are turned off, and the first and second members M1 and M2 are cooled to below the melting point Tm by blowing air over them using the blower described above (see arrow A in Figure 1). After cooling is complete, it is confirmed whether the fusion is truly complete. This confirmation is performed by observing the condition of the joining area using non-destructive testing techniques such as ultrasonic flaw detection and X-ray CT scanning.
[0037] If it is confirmed that the fusion of the first member M1 and the second member M2 is truly complete, the set temperatures T1e and T2e at that time, the holding time t after the set temperatures are reached, and the load L applied to the second heat source H2 are set as the working conditions for the actual joining process. That is, the set temperatures T1e and T2e at that time are set as the temperature (first temperature) T1 of the first heat source H1 and the temperature (second temperature) T2 of the second heat source H2 in the actual joining process, respectively.
[0038] On the other hand, if it is confirmed that the fusion of the first member M1 and the second member M2 has not actually been completed, the preliminary experiment is repeated after changing at least one of the set temperatures T1e and T2e, the holding time t after the set temperature is reached, and the load L applied to the second heat source H2.
[0039] The above description has been made on the implicit assumption that the temperature (first temperature) T1 of the first heat source H1 is higher than room temperature. This is because, if the temperature T1 of the first heat source H1 is room temperature, the temperature (second temperature) T2 of the second heat source H2 required to raise the temperature of the joining region to or above the melting point Tm of a commonly used thermoplastic resin exceeds the thermal decomposition temperature Th, making it practically impossible to carry out the joining process. Thus, the first heat source H1 can literally be said to be a "heat source" because its T1 is higher than room temperature. However, in the joining process according to the embodiment of the present disclosure, the first heat source H1 can also be said to act as a heat sink for the second heat source H2, which acts as a heat source.
[0040] Based on the working conditions determined through the above-mentioned preliminary experiment (target values of the temperatures measured by the thermocouples TC embedded in the first heat source H1 and the second heat source H2 (first temperature T1 and second temperature T2), the holding time t after the measured temperatures reach the target values, and the load L applied to the second heat source H2), the actual bonding process is carried out by carrying out the following steps in this order: (1) a step of placing the first member M1 on the upper surface H1U of the first heat source H1; (2) a step of placing the second member M2 (the portion to be bonded M2W of the second member M2) on the upper surface M1U of the first member M1 with or without a bonding film F made of thermoplastic resin therebetween; and (3) a step of positioning the second heat source H2 above the second member M2. (4) a step of heating the first heat source H1 to a first temperature T1 (controlling the on / off of the cartridge heater CH embedded in the first heat source H1 by a temperature controller so that the temperature measured by the thermocouple TC embedded in the first heat source H1 becomes the first temperature T1); and (5) a step of heating the second heat source H2 to a second temperature T2 (controlling the on / off of the cartridge heater CH embedded in the second heat source H2 by a temperature controller so that the temperature measured by the thermocouple TC embedded in the second heat source H2 becomes the second temperature T2), and at the same time, lowering the second heat source H2 and pressing its lower surface (the upper surface H2RU (see FIG. 3) or the bottom surface H2L′ (see FIG. 5) of the recess H2R) against the upper surface M2U of the joining portion M2W while a downward load L is applied. (6) A step of cooling the first member M1 and the second member M2 (by blowing air onto them using a blower) after a predetermined holding time t has elapsed since the temperature measured by the thermocouple TC embedded in the first heat source H1 reaches the first temperature T1 and the temperature measured by the thermocouple TC embedded in the second heat source H2 reaches the second temperature T2.
[0041] In the above-mentioned step (5), after heating the second heat source H2 to the second temperature T2, the second heat source H2 may be lowered and its lower surface may be pressed against the upper surface of the second member M2 while a downward load L is applied, or the second heat source H2 may be lowered in advance and heated to the second temperature T2 while its lower surface is pressed against the upper surface of the second member M2 while a downward load L is applied.
[0042] Furthermore, the cooling of the first member M1 and the second member M2 in the above-mentioned step (6) may be performed while the second heat source H2 remains lowered. However, the cooling of the first member M1 and the second member M2 can be promoted by raising the second heat source H2 when the temperatures measured by the thermocouples TC embedded in the first heat source H1 and the second heat source H2 both fall below the melting point Tm (preferably, the softening point Ts) of the thermoplastic resin contained in the first member H1 and the second member H2.
[0043] In step (5) described above, the joining portion M2W of the second member M2 is accommodated in a recess H2R provided in the bottom surface H2L of the second heat source H2. At this time, the thermoplastic resin in the joining portion M2W of the second member M2 is at least partially liquidized and becomes flowable due to heat transfer from the second heat source H2, which has a temperature T2 exceeding the melting point Tm of the thermoplastic resin. However, the top surface M2U of the joining portion M2W of the second member M2 is in contact with the top surface H2RU of the recess H2R of the second heat source H2, and only small gaps exist between the side surfaces M2S1, M2S2, and M2S3 of the joining portion M2W of the second member M2 and the side surfaces H2RS1, H2RS2, and H2RS3 of the recess H2R of the second heat source H2. Therefore, the thermoplastic resin in the liquid phase does not flow significantly, and the to-be-joined portion M2W of the second member M2 can substantially maintain its shape.
[0044] In the above description, the shape of the recess H2R provided on the bottom surface H2L of the second heat source H2 has been described as having an open portion on the front surface of the second heat source H2 corresponding to the L-shaped portion of the second member M2. However, this is not limited to this. That is, depending on the shape of the second member M2, the open portion may be absent or may be present in multiple portions. In short, the recess H2R provided on the bottom surface H2L of the second heat source H2 essentially includes an upper surface H2RU that contacts and heats the upper surface of the second member M2 (the portion M2W to be joined of the second member M2), and further includes side surfaces (H2RS1, H2RS2, and H2RS3 in the embodiment shown in FIG. 3) that face the side surfaces (M2S1, M2S2, and M2S3 in the embodiment shown in FIG. 1) of the second member M2 (the portion M2W to be joined of the second member M2) with a small gap therebetween.
[0045] The above describes an embodiment in which a recess H2R is provided in the bottom surface H2L of the second heat source H2 and the to-be-joined portion M2W of the second member M2 is housed in the recess H2R to prevent significant flow of the thermoplastic resin in the to-be-joined portion M2W of the second member M2 in steps (5) and (6). However, another embodiment can also be adopted to prevent significant flow of the thermoplastic resin in the to-be-joined portion M2W of the second member M2. This will be described below.
[0046] FIG. 4 is a schematic perspective view showing the arrangement of two components made of a material containing a thermoplastic resin and the equipment for joining them just before the start of a joining process by a method of another embodiment of the present disclosure, and FIG. 5 is a schematic cross-sectional view at the center in the width direction (the w direction in FIG. 4) showing the main parts of the arrangement.
[0047] As shown in both figures, in this embodiment, a resin flow prevention jig J is placed on the upper surface M1U of the first member M1, and is configured to accommodate (strictly speaking, surround on three sides) the joining portion M2W of the second member M2.
[0048] The resin flow prevention jig J is a member made of a thermal insulating material (or a thermal insulating material reinforced with metal) and has a U-shape (an angular U-shape) in a plan view. The inner side surfaces JS1, JS2, and JS3 of the resin flow prevention jig J face the side surfaces M2S1, M2S2, and M2S3 of the joining portion M2W of the second member M2, respectively, with a small gap therebetween. The height of the resin flow prevention jig J is sufficiently greater than the height from the upper surface M1U of the first member M1 to the upper surface M1U of the joining portion M2W of the second member M2, which is placed on the upper surface M1U of the first member M1 with or without the bonding film F interposed therebetween. Furthermore, in the illustrated example, the inner side surfaces JS1 and JS3 of the resin flow prevention jig J are configured to face, with a small gap therebetween, the side surfaces of the substantially flat, plate-shaped portion of the second member M2 corresponding to the long side of the L-shape. As a result, the space defined between the second member M2 and the resin flow prevention jig J is substantially open only upward (i.e., substantially closed in the horizontal direction).
[0049] On the other hand, the second heat source H2' is formed in a rectangular parallelepiped shape, and unlike the above-described embodiment, no recess is formed on its bottom surface H2L'. Furthermore, the bottom surface H2L' of the second heat source H2' has the same shape and dimensions as the top surface M2U of the joint portion M2W of the second member M2. Therefore, in the above-described step (5), when the second heat source H2' is lowered and its bottom surface H2L' comes into contact with the top surface M2U of the joint portion M2W of the second member M2, the three side surfaces of the second heat source H2' face the inner side surfaces JS1, JS2, and JS3 of the resin flow prevention jig J with a small gap therebetween.
[0050] With the above-described configuration, in this embodiment, in step (5) described above, the to-be-joined portion M2W of the second member M2 is accommodated in the space defined by the inner side surfaces JS1, JS2, and JS3 of the resin flow prevention jig J. Therefore, the thermoplastic resin in its liquid phase does not flow significantly, and the to-be-joined portion M2W of the second member M2 can substantially maintain its shape.
[0051] Although the above description has been given using an example in which the relatively large first member M1 is a substantially flat plate and the relatively small second member M2 is a substantially L-shaped plate, the embodiments of the present disclosure are not limited to this. For example, even if the relatively large first member M1 has a curved surface, such as a concave or convex cylindrical surface or a spherical surface, that is bonded to the second member M2, and the relatively small second member M2 is a U-shaped, T-shaped, or other member that has a substantially flat plate-like portion that is bonded to the first member M1, the two members can still be bonded together using the method of the embodiments of the present disclosure.
[0052] Although the above description has been given assuming that the first member M1 and the second member M2 are cooled after the joining process is completed by blowing air onto them using a blower, the present invention is not limited to this. For example, the first heat source H1 and the second heat source H2 may be cooled by circulating a cooling medium (e.g., air, water, oil, etc.) through passages provided inside the respective heat sources.
[0053] (Aspects of the Present Disclosure) A joining method of a first aspect of the present disclosure is a method for joining a first member and a second member, both of which are made of materials containing a thermoplastic resin, the method including, in this order: placing the first member on an upper surface of a first heat source; placing the second member on the upper surface of the first member with or without a bonding film made of a thermoplastic resin therebetween; positioning a second heat source above the second member; heating the first heat source to a predetermined first temperature and the second heat source to a predetermined second temperature, while lowering the second heat source and pressing its lower surface against the upper surface of the second member with a predetermined downward load being applied; and cooling the first member and the second member after a predetermined holding time has elapsed since the temperature of the first heat source reached the first temperature and the temperature of the second heat source reached the second temperature, wherein the second temperature is higher than the melting point of the thermoplastic resin and lower than the thermal decomposition temperature of the thermoplastic resin, and the first temperature is lower than the melting point of the thermoplastic resin.
[0054] In the joining method of the second aspect of the present disclosure, the first temperature, the second temperature, the load, and the holding time are set in advance through a preliminary experiment including each of the steps and a non-destructive inspection of the joining area of the first member and the second member performed after the preliminary experiment.
[0055] In the joining method of the third aspect of the present disclosure, the first member and the second member are each molded in advance using a molding die, and after the molding, any release agent remaining in the portion of the first member that will come into contact with the second member, either through the bonding film or not, and in the portion of the second member that will come into contact with the first member, either through the bonding film or not, has been removed in advance.
[0056] In the joining method of the fourth aspect of the present disclosure, the second member includes a plate-shaped joining portion having a lower surface that contacts the upper surface of the first member with or without the bonding film, the joining portion has an upper surface that is located opposite the lower surface in the plate thickness direction, and when the second heat source descends, the second heat source is pressed against the upper surface of the joining portion.
[0057] In the joining method of the fifth aspect of the present disclosure, a recess is formed in the bottom surface of the second heat source, and when the second heat source is lowered, the upper surface of the recess is pressed against the upper surface of the joining portion of the second member.
[0058] In the joining method according to the sixth aspect of the present disclosure, the recess is configured to accommodate the portion to be joined of the second member when the second heat source is lowered.
[0059] In the joining method of the seventh aspect of the present disclosure, the portion to be joined of the second member has a side surface connecting the upper surface and the lower surface, the recess of the second heat source has a side surface connecting the upper surface of the recess and the bottom surface of the second heat source, and when the second heat source is lowered, the side surface of the recess of the second heat source is configured to face the side surface of the portion to be joined of the second member via a gap.
[0060] In the joining method of the eighth aspect of the present disclosure, a resin flow prevention jig configured to accommodate the portion to be joined of the second member is placed on the upper surface of the first member, the bottom surface of the second heat source has the same shape and dimensions as the upper surface of the portion to be joined of the second member, and when the second heat source is lowered, the bottom surface of the second heat source is pressed against the upper surface of the portion to be joined of the second member.
[0061] In the joining method of the ninth aspect of the present disclosure, the portion to be joined of the second member has a side surface connecting the upper surface and the lower surface, the resin flow prevention jig has an inner side surface, and when the second heat source is lowered, the side surface of the second heat source is configured to face the inner side surface of the resin flow prevention jig through a gap.
[0062] F Bonding film H1 First heat source H1U Top surface of first heat source H2, H2' Second heat source H2L' Bottom surface of second heat source H2R Recessed portion of second heat source H2RU Top surface of recessed portion of second heat source H2RS1, H2RS2, H2RS3 Side surface of recessed portion of second heat source L Load J Resin flow prevention jig JS1, JS2, JS3 Inner side surface of resin flow prevention jig M1 First member M2 Second member M2L Bottom surface of the part to be joined of the second member M2S1, M2S2, M2S3 Side surface of the part to be joined of the second member M2U Top surface of the part to be joined of the second member M2W Part to be joined of the second member T1 First temperature T2 Second temperature Th Thermal decomposition temperature of thermoplastic resin Tm Melting point of thermoplastic resin Ts Softening point of thermoplastic resin t retention time
Claims
1. A method for bonding a first member and a second member, both of which are made of materials containing thermoplastic resin, comprising the steps of: placing the first member on an upper surface of a first heat source; placing the second member on the upper surface of the first member with or without a bonding film made of thermoplastic resin in between; positioning a second heat source above the second member; heating the first heat source to a predetermined first temperature and the second heat source to a predetermined second temperature, respectively, while lowering the second heat source and pressing its lower surface against the upper surface of the second member while a predetermined downward load is applied; and cooling the first member and the second member after a predetermined holding time has elapsed since the temperature of the first heat source reached the first temperature and the temperature of the second heat source reached the second temperature, wherein the second temperature is higher than the melting point of the thermoplastic resin and lower than the thermal decomposition temperature of the thermoplastic resin, and the first temperature is lower than the melting point of the thermoplastic resin.
2. The method according to claim 1, characterized in that the first temperature, the second temperature, the load and the holding time are preset through a preliminary experiment including each of the steps and a non-destructive inspection of the bonding area of the first member and the second member performed after the preliminary experiment.
3. The method according to claim 1 or 2, characterized in that the first member and the second member are each molded in advance using a molding die, and that after the molding, any release agent remaining in a portion of the first member that comes into contact with the second member through or without the bonding film, and in a portion of the second member that comes into contact with the first member through or without the bonding film, has been removed in advance.
4. A method according to any one of claims 1 to 3, characterized in that the second member includes a plate-shaped portion to be joined having a lower surface that contacts the upper surface of the first member with or without the bonding film, the portion to be joined has an upper surface located opposite the lower surface in the plate thickness direction, and when the second heat source is lowered, the second heat source is pressed against the upper surface of the portion to be joined.
5. The method according to claim 4, characterized in that a recess is formed in the bottom surface of the second heat source, and when the second heat source is lowered, the upper surface of the recess is pressed against the upper surface of the portion to be joined of the second member.
6. The method according to claim 5, wherein the recess is configured to accommodate the portion of the second member to be joined when the second heat source is in a lowered state.
7. The method according to claim 6, characterized in that the portion to be joined of the second member has a side surface connecting the upper surface and the lower surface, the recess of the second heat source has a side surface connecting the upper surface of the recess and the bottom surface of the second heat source, and when the second heat source is lowered, the side surface of the recess of the second heat source is configured to face the side surface of the portion to be joined of the second member across a gap.
8. The method according to claim 4, characterized in that a resin flow prevention jig configured to accommodate the joined portion of the second member is placed on the upper surface of the first member, the bottom surface of the second heat source has the same shape and dimensions as the upper surface of the joined portion of the second member, and when the second heat source is lowered, the bottom surface of the second heat source is pressed against the upper surface of the joined portion of the second member.
9. The method according to claim 8, characterized in that the portion to be joined of the second member has a side surface connecting the upper surface and the lower surface, the resin flow prevention jig has an inner side surface, and when the second heat source is lowered, the side surface of the second heat source is configured to face the inner side surface of the resin flow prevention jig across a gap.
Citation Information
Patent Citations
Forming method of porous PTFE layer, and porous PTFE layer and molded article prepared by this method
JP2008110562A
Molding device for fiber-reinforced composite member
JP2017128035A
Thermal welding device
JP2020124886A