Laminate, method for producing laminate, and method for deinking laminate

The laminate structure with a water-based resin anchor layer and active energy ray-curable ink layer addresses the deinking challenges in recycling, allowing for efficient ink removal and base material recovery, thus improving recycling efficiency and environmental sustainability.

WO2024214341A1PCT designated stage expired Publication Date: 2024-10-17TOYO INK MFG CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/044874
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2023-12-14
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Current methods for recycling active energy ray-curable inks and varnishes, particularly in non-absorbent materials like plastics, face challenges due to their difficulty in deinking and the resulting contamination during the recycling process, which limits the reuse of base materials and contributes to environmental issues like marine pollution.

Method used

A laminate structure comprising an anchor layer with a water-based resin and an ink layer of active energy ray-curable inks, which can be easily deinked using an alkaline aqueous solution, allowing for the recovery of non-absorbent base materials and facilitating recycling.

Benefits of technology

The method effectively removes active energy ray-curable inks from non-absorbent substrates, enhancing recycling efficiency, reducing waste, and minimizing environmental impact by enabling the reuse of base materials and reducing carbon footprint.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided is a laminate having an anchor layer and an ink layer in the stated order on a non-absorbent substrate, wherein the anchor layer includes an aqueous resin, the acid value of the aqueous resin is 25-300 mgKOH / g and the glass transition temperature thereof is 10-150°C, and the ink layer is a cured product of at least one ink selected from active energy ray-curable offset printing ink, active energy ray-curable flexographic printing ink, and active energy ray-curable resin letterpress printing ink.
Need to check novelty before this filing date? Find Prior Art

Description

Laminate, manufacturing method of laminate, and deinking method of laminate

[0001] Embodiments of the present invention relate to a laminate, a method for manufacturing a laminate, and a method for deinking a laminate.

[0002] Compared with oxidative polymerization, penetration drying, and hot air drying oil-based inks and varnishes, active energy ray-curable inks and varnishes have the convenience of instantaneous curing. They also have the property of being capable of forming a strong cured film and are VOC-free, meaning they do not contain petroleum-based volatile compounds. For these reasons, active energy ray-curable inks and varnishes are widely used in the package printing industry, including for beverage and food packaging, pharmaceutical packaging, cosmetic packaging, and even general paper containers.

[0003] In the food packaging field in particular, the ideal form of active energy ray-curable ink and varnish is an electron beam (hereinafter also referred to as "EB")-curable ink, which does not contain a photopolymerization initiator and takes into consideration safety and security for humans and the environment. However, EB-curable ink is not widely used due to the large initial capital investment required, and ultraviolet (hereinafter also referred to as "UV")-curable ink is more common on the market.

[0004] In recent years, it is known that there has been a gradual shift to new systems, such as LED curing systems that use UV-LED light sources that are energy-efficient and suppress the generation of ozone and heat, energy-saving UV systems that use a single metal halide lamp that eliminates the infrared region that generates heat and the ultraviolet region that generates ozone, and energy-saving UV systems that reduce the number of UV lamps from the usual three or four to just one.

[0005] Energy-saving UV-curable inks and varnishes designed to accommodate these new systems have seen a recent trend of replacing standard oil-based inks and varnishes, especially in commercial printing. Therefore, energy-saving UV-curable inks and varnishes are required to have the same performance as standard oil-based inks and varnishes, including printability and print quality. In particular, an increasing number of energy-saving UV-curable inks are being certified as "recyclable UV-curable inks" with a recyclability rating of A. However, not all UV systems on the market are being replaced by energy-saving UV systems, and many companies still use the established conventional UV systems (many of which are rated B for recyclability). UV-curable inks and varnishes are generally considered more difficult to recycle than standard oil-based inks and varnishes, with the exception of recyclable energy-saving UV-curable inks and some recyclable UV-curable inks. In order to simplify recycling when collecting printed materials, it is considered extremely difficult, and nearly impossible, to separate printed materials containing non-recyclable active energy ray-curable inks and varnishes, such as UV-curable inks.

[0006] Furthermore, even when the substrate is a non-absorbent substrate other than paper, there is an urgent need to develop a method for facilitating the recycling of the substrate, similar to that of paper substrates. This is because, in recent years, UV curing devices, UV-LED curing devices, and EB curing devices that are less susceptible to heat have been developed, making it possible to irradiate the substrate with active energy rays without causing thermal damage, even when the substrate is thin, and as a result, there has been an increase in the number of cases in which active energy ray-curable inks and varnishes are used.

[0007] In particular, for plastic substrates, marine pollution countermeasures are a key global environmental measure, and the development of a plastic recovery system that prevents the release of microplastics, which cause marine pollution, into the ocean is urgently needed. Compared to chemical recycling, which chemically decomposes and reuses materials such as plastics, material recycling, which pelletizes and reuses materials, is simpler. However, if active energy ray-curable inks and varnishes are not removed from the substrate during material recycling, the residual inks and varnishes will be trapped in the substrate melting process. This will likely make it difficult for the substrate to return to its original color, limiting the uses of the recycled substrate. Therefore, developing a simple method for removing additives such as active energy ray-curable inks and varnishes and adhesives from packaging materials such as plastics will increase the efficiency of material recycling.

[0008] Furthermore, a method is desired that can easily remove actinic ray-curable inks and varnishes from all kinds of non-absorbing substrates, including not only flexible packaging materials but also hard plastic substrates such as PET bottle caps, nonwoven fabrics, and metals. If the above method can easily reuse the substrate materials, it will be possible to improve recycling efficiency and reduce the use of fossil resources, which will in turn contribute to reducing carbon dioxide emissions.

[0009] For example, Patent Document 1 discloses an organic solvent-based ink for a release layer that can be removed by alkali treatment, a laminate such as a printed matter that includes a release layer using this ink, and a method for recycling this laminate. However, the inks that can be removed are limited to inks that use solvents, and there is no simple deinking method for actinic ray-curable inks, which are generally considered to be solvent-free. Therefore, there is a need to establish printed matters that are excellent in deinking suitability using general actinic ray-curable inks and varnishes, and a method for producing such printed matters.

[0010] Patent Document 2 describes an aqueous anchoring agent for a release layer that can be removed by alkali treatment, and a laminate such as a printed matter that includes a release layer using the same. However, the substrates that can be removed are limited to paper or synthetic paper, and no technology has been established for non-absorbent substrates such as plastics. In particular, for non-absorbent substrates such as plastics, adhesion between the substrate and the anchor layer and the blocking resistance of the anchor layer are major issues compared to paper substrates. Here, blocking resistance includes resistance to blocking in areas of the anchor layer where ink is not printed, and resistance to blocking when the ink is wound or stacked before printing. Among active energy ray-curable inks, active energy ray-curable offset printing inks, active energy ray-curable flexographic printing inks, and active energy ray-curable resin letterpress printing inks have high film strength and are difficult to deink. Therefore, there is a need for an anchoring agent that can be deinked even when using these inks.

[0011] JP 2020-090627 A Patent No. 7070772

[0012] One embodiment of the present invention provides a laminate that has excellent physical properties as a laminate, such as blocking resistance and scratch resistance, while also having excellent deinking properties for removing active energy ray-curable ink in the recycling process of non-absorbing substrates. Another embodiment of the present invention provides a method for producing the laminate of the above embodiment. Yet another embodiment of the present invention provides a method for deinking a laminate.

[0013] As a result of extensive research aimed at solving the above-mentioned problems, the inventors have found that the above-mentioned problems can be solved by the laminate and the method for manufacturing the laminate described below, and have thus completed the present invention. That is, embodiments of the present invention are exemplified below. However, the present invention is not limited to the following description and includes various embodiments.

[0014] One embodiment of the present invention relates to a laminate having an anchor layer and an ink layer in this order on a non-absorbing substrate, wherein the anchor layer contains an aqueous resin, the aqueous resin has an acid value of 25 to 300 mgKOH / g, and the aqueous resin has a glass transition temperature of 10 to 150°C, and the ink layer is a cured product of at least one ink selected from an active energy ray-curable offset printing ink, an active energy ray-curable flexographic printing ink, and an active energy ray-curable resin letterpress printing ink.

[0015] In the laminate of the above embodiment, the aqueous resin preferably includes at least one selected from the group consisting of aqueous acrylic resins and aqueous urethane resins.

[0016] Another embodiment of the present invention relates to a method for producing a laminate, comprising: Step 1 of applying an anchor agent containing water and an aqueous resin to a non-absorbing substrate, and drying the applied agent in an oven to form an anchor layer, thereby obtaining a laminate having an anchor layer on the non-absorbing substrate; and Step 2 of printing at least one ink selected from an active energy ray-curable offset printing ink, an active energy ray-curable flexographic printing ink, and an active energy ray-curable resin letterpress printing ink onto the anchor layer of the laminate having an anchor layer on the non-absorbing substrate, and curing the ink with active energy rays to form an ink layer, thereby obtaining a laminate having an ink layer on the anchor layer, wherein the aqueous resin has an acid value of 25 to 300 mgKOH / g, and a glass transition temperature of 10 to 150°C.

[0017] In the manufacturing method of the above embodiment, the aqueous resin preferably includes at least one selected from the group consisting of an aqueous acrylic resin and an aqueous urethane resin.

[0018] Another embodiment of the present invention relates to a method for deinking a laminate having an anchor layer and an ink layer in this order on a non-absorbing substrate, wherein the anchor layer contains an aqueous resin, the acid value of the aqueous resin is 25 to 300 mgKOH / g, and the glass transition temperature of the aqueous resin is 10 to 150°C, and the ink layer is a cured product of at least one ink selected from an active energy ray-curable offset printing ink, an active energy ray-curable flexographic printing ink, and an active energy ray-curable resin letterpress printing ink, and the method comprises stirring the laminate in an alkaline aqueous solution to dissolve the anchor layer in the alkaline aqueous solution and deinking the ink layer from the non-absorbing substrate.

[0019] In the deinking method of the above embodiment, the aqueous resin preferably contains one or more types selected from the group consisting of aqueous acrylic resins and aqueous urethane resins.

[0020] Another embodiment of the present invention relates to a method for recovering ink, in which the ink layer deinked by the deinking method of the above embodiment is filtered and recovered. Another embodiment of the present invention relates to a method for producing a recycled substrate, in which the ink layer is removed by the deinking method of the above embodiment and a non-absorbing substrate is recovered. The disclosure of this application is related to the subject matter described in Japanese Patent Application No. 2023-066274, filed on April 14, 2023, the entire disclosure of which is incorporated herein by reference.

[0021] According to the present invention, it is possible to provide a laminate that has excellent physical properties as a laminate, such as blocking resistance and scratch resistance, while also having excellent deinking properties for removing active energy ray-curable ink in the recycling process of non-absorbent substrates. Also provided are a method for producing the laminate and a method for deinking the laminate.

[0022] The present invention will be described in detail below. Note that the present invention is not limited to the following embodiments and can be practiced with various modifications within the scope of the spirit thereof. Furthermore, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass."

[0023] <1> Laminate A laminate according to one embodiment of the present invention is a laminate having an anchor layer and an ink layer, in this order, on a non-absorbing substrate. The anchor layer is a layer in which an aqueous anchor agent containing an aqueous resin is dried in an oven, and the ink layer is a layer in which an active energy ray-curable ink is cured by active energy rays.

[0024] As will be described later, if the ink does not contain a colorant, it becomes a varnish (also called a clear ink). Therefore, the ink layer becomes a varnish layer (clear ink layer). The laminate will be described in more detail below.

[0025] <Ink Layer> The ink layer is composed of a cured product of an active energy ray-curable ink. Hereinafter, the active energy ray-curable ink (hereinafter also referred to as "ink") used to form the ink layer will be described.

[0026] <Actinic Energy Ray-Curable Ink> In one embodiment of the present invention, the active energy ray-curable ink may be at least one ink selected from the group consisting of active energy ray-curable offset printing ink, active energy ray-curable flexographic printing ink, and active energy ray-curable resin letterpress printing ink. These active energy ray-curable offset printing ink, active energy ray-curable flexographic printing ink, and active energy ray-curable resin letterpress printing ink are inks that have high film strength and are considered to be difficult to deink, even among active energy ray-curable inks.

[0027] [Colorant] In one embodiment of the present invention, the ink may contain a colorant. At least one of a pigment and a dye may be used as the colorant. From the viewpoint of lightfastness, a pigment is preferred. There are no particular restrictions on the pigment that can be used in the present invention, and any known pigment may be used. Both inorganic and organic pigments may be used. When the ink does not contain a colorant, it becomes a varnish (clear ink).

[0028] Examples of inorganic pigments include carbon blacks such as furnace black, lamp black, acetylene black, and channel black, iron oxide, and titanium oxide.

[0029] Examples of organic pigments include soluble azo pigments such as β-naphthol-based, β-oxynaphthoic acid-based, β-oxynaphthoic acid anilide-based, acetoacetic acid anilide-based, and pyrazolone-based pigments; Examples of suitable pigments include insoluble azo pigments such as β-naphthols, β-oxynaphthoic acid anilides, acetoacetate anilide monoazos, acetoacetate anilide disazos, and pyrazolone pigments; phthalocyanine pigments such as copper phthalocyanine blue, halogenated (for example, chlorinated or brominated) copper phthalocyanine blue, sulfonated copper phthalocyanine blue, and metal-free phthalocyanine; and polycyclic and heterocyclic pigments such as quinacridones, dioxazines, threnes (pyranthrones, anthranthrones, indanthrones, anthrapyrimidines, flavanthrones, thioindigo pigments, anthraquinones, perinones, and perylenes), isoindolinones, metal complexes, quinophthalones, and diketopyrrolopyrroles.

[0030] More specifically, in terms of the C.I. Color Index, examples of black pigments include C.I. Pigment Black 1, 6, 7, 9, 10, 11, 28, 26, and 31.

[0031] Examples of white pigments include C.I. Pigment White 5, 6, 7, 12, and 28.

[0032] Examples of yellow pigments include C.I. Pigment Yellow 1, 2, 3, 12, 13, 14, 16, 17, 18, 24, 73, 74, 75, 83, 93, 95, 97, 98, 100, 108, 109, 110, 114, 120, 128, 129, 138, 139, 174, 150, 151, 154, 155, 167, 174, 176, 180, 185, and 213.

[0033] Examples of blue or cyan pigments include C.I. Pigment Blue 1, 2, 14, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, and the like.

[0034] Red or crimson pigments include C.I. Pigment RED 1, 3, 5, 19, 21, 22, 31, 38, 42, 43, 48:1, 48:2, 48:3, 48:4, 48:5, 49:1, 50, 52, 53:1, 57:1, 57:2, 58:4, 63:1, 81, 81:1, 81:2, 81:3, 81:4, 83, 90, 104, 10 8, 112, 114, 122, 144, 146, 148, 149, 150, 166, 168, 169, 170, 172, 173, 176, 177, 178, 184, 185, 187, 193, 202, 209, 214, 242, 254, 255, 264, 266, 269, C.I. Pigment Violet 19, and the like.

[0035] Examples of green pigments include C.I. Pigment Green 1, 2, 3, 4, 7, 8, 10, 15, 17, 26, 36, 45, and 50.

[0036] Examples of purple pigments include C.I. Pigment Violet 1, 2, 3, 4, 5:1, 12, 13, 15, 16, 17, 19, 23, 25, 29, 31, 32, 36, 37, 39, and 42. Examples of orange pigments include C.I. Pigment Orange 13, 16, 20, 34, 36, 38, 39, 43, 51, 61, 63, 64, and 74.

[0037] In one embodiment of the present invention, the pigments may be used alone or in combination of two or more.

[0038] The pigment may be used in any amount as long as the desired density can be reproduced on the surface of the printing substrate. In one embodiment, the pigment content is preferably 5 to 30% by mass, more preferably 10 to 25% by mass, based on the total mass of the ink.

[0039] [(Meth)acrylate Compound] In this specification, unless otherwise specified, "(meth)acryloyl", "(meth)acrylic acid", "(meth)acrylate", and "(meth)acryloyloxy" mean "acryloyl and / or methacryloyl", "acrylic acid and / or methacrylic acid", "acrylate and / or methacrylate", and "acryloyloxy and / or methacryloyloxy", respectively. Furthermore, "PO" represents "propylene oxide", and "EO" represents "ethylene oxide". Furthermore, X in EO-modified (X) and PO-modified (X) represents the number of moles of EO or PO modified, and Y in polyethylene glycol (Y) di(meth)acrylate represents the approximate molecular weight of the polyethylene glycol portion.

[0040] In one embodiment of the present invention, the active energy ray-curable ink may contain a (meth)acrylate compound. The (meth)acrylate compound that can be used in the present invention is not particularly limited as long as it is a compound having one or more (meth)acryloyl groups, and includes any of the forms of a monomer, oligomer, and polymer. Here, "monomer" refers to a compound that is the smallest structural unit for constituting an oligomer or polymer, and "oligomer" refers to a polymer having structural units based on 2 to 100 monomers.

[0041] Specific examples of the (meth)acrylate compound used in the present invention include the compounds shown below.

[0042] [(Meth)acrylate compounds] (monomers) 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, β-carboxyethyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, tetrahydrofurfuryl acrylate, alkoxylated tetrahydrofurfuryl acrylate, caprolactone (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isoamyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, isodecyl (meth)acrylate, 3,3,5-trimethylcyclohexanol (meth)acrylate, ) acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, norbornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (oxyethyl) (meth)acrylate, 1,4-cyclohexanedimethanol (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, benzyl (meth)acrylate, EO-modified (2) nonylphenol acrylate, monofunctional (meth)acrylate monomers having one (meth)acryloyl group in the molecule, such as 2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl acrylate, 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 1,2-dodecanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol (200) di(meth)acrylate, polyethylene glycol (300) di(meth)acrylate, polyethylene glycol (400) di(meth)acrylate, polyethylene glycol (600) di(meth)acrylate, neopentyl glycol hydroxypivalate di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, EO-modified (2)1,6-hexanediol di(meth)acrylate, PO-modified (2) neopentyl glycol di(meth)acrylate, (neopentyl glycol-modified) trimethylolpropane di(meth)acrylate, dimethyloltricyclodecane di(meth)acrylate, EO-modified (4) bisphenol A di(meth)acrylate, PO-modified (4) bifunctional (meth)acrylate monomers having two (meth)acryloyl groups in the molecule, such as bisphenol A di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, and dicyclopentanyl di(meth)acrylate; Trimethylolpropane tri(meth)acrylate, EO-modified (3) trimethylolpropane tri(meth)acrylate, EO-modified (6) trimethylolpropane tri(meth)acrylate, PO-modified (3) trimethylolpropane tri(meth)acrylate, trifunctional (meth)acrylate monomers having three (meth)acryloyl groups in the molecule, such as pentaerythritol tri(meth)acrylate; pentaerythritol tetra(meth)acrylate, EO-modified (4) pentaerythritol tetra(meth)acrylate, tetrafunctional (meth)acrylate monomers having four acryloyl groups in the molecule, such as ditrimethylolpropane tetra(meth)acrylate; pentafunctional (meth)acrylate monomers having five (meth)acryloyl groups in the molecule, such as dipentaerythritol penta(meth)acrylate; and hexafunctional (meth)acrylate monomers having six (meth)acryloyl groups in the molecule, such as dipentaerythritol hexa(meth)acrylate.

[0043] (Oligomer) Examples include urethane acrylate oligomers such as aliphatic urethane acrylate oligomers and aromatic urethane acrylate oligomers, acrylic ester oligomers, polyester acrylate oligomers, and epoxy acrylate oligomers, each having 1 to 6 (meth)acryloyl groups. [Other Components] In one embodiment of the present invention, the ink may contain, in addition to the above-mentioned components, a polymerization initiator, an amine compound, a resin, a polymerization inhibitor, a surface tension modifier, wax, an extender pigment, a pigment dispersant, an antifoaming agent, an ultraviolet absorber, an antioxidant, an antistatic agent, and the like, as needed.

[0044] (Polymerization initiator) In one embodiment of the present invention, the ink may contain a polymerization initiator. The polymerization initiator preferably contains a radical or cationic polymerization initiator, and more preferably contains a photopolymerization initiator. The polymerization initiator is a compound that undergoes a chemical change through the action of light or through interaction with the electronically excited state of the sensitizing dye, thereby generating radicals or cations. Among these, a photoradical polymerization initiator is preferred from the viewpoint that polymerization can be initiated by exposure to light.

[0045] In one embodiment of the present invention, the photoradical polymerization initiator is not particularly limited, and known ones can be used. Specific examples include benzophenone-based compounds, dialkoxyacetophenone-based compounds, α-hydroxyalkylphenone-based compounds, α-aminoalkylphenone-based compounds, acylphosphine oxide-based compounds, oxime ester-based compounds, and thioxanthone-based compounds. Furthermore, the photopolymerization initiators may be used alone or in combination of two or more.

[0046] Examples of the benzophenone compounds include benzophenone, 2-methylbenzophenone, 3-methylbenzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-phenylbenzophenone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(dimethylamino)benzophenone, [4-(methylphenylthio)phenyl]-phenylmethanone, 2-chloro-4phenyl-benzophenone, 1-{4-[(4-benzoylphenylsulfanyl)phenyl]-2-methyl-2-(4-methylbenzenesulfonyl)propan-1-one, and polybutylene glycol bis(4-benzoylphenoxy)acetate.

[0047] Examples of the dialkoxyacetophenone compounds include 2,2-dimethoxy-2-phenylacetophenone, dimethoxyacetophenone, and diethoxyacetophenone.

[0048] Examples of α-hydroxyalkylphenone compounds include 1-hydroxy-cyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxymethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, oligo[2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone], 2,3-dihydro-6-(2-hydroxy-2-methyl-1-oxopropyl)-1,1,3-trimethyl-3-[4-(2-hydroxy-2-methyl- a mixture of 2,3-dihydro-5-(2-hydroxy-2-methyl-1-oxopropyl)phenyl]-1H-indene and 2,3-dihydro-5-(2-hydroxy-2-methyl-1-oxopropyl)-1,1,3-trimethyl-3-[4-(2-hydroxy-2-methyl-1-oxopropyl)phenyl]-1H-indene, 2-hydroxy-1-[4-[4-(2-hydroxy-2-methylpropynyl)benzyl]phenyl]-2-methylpropan-1-one, 2-hydroxy-1-[4-[4-(2-hydroxy-2-methylpropanoyl)phenoxy]phenyl]-2-methylpropan-1-one, and 1-[4-(1,1-dimethylethyl)phenyl]-2-hydroxy-2-methylpropan-1-one.

[0049] Examples of α-aminoalkylphenone compounds include 2-methyl-1-[4-(methoxythio)-phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone, 1,2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 1-(9,9-dibutyl-9H-fluoren-2-yl)-2-methyl-2-morpholinopropan-1-one, 1-(4-methylphenyl ... phosphon-4-yl-propan-1-one, polyethylene glycol di(β-4-[4-(2-dimethylamino-2-benzyl)butanonylphenyl]piperazine)propinate, 2-benzyl-2-dimethylamino-1-(4-piperidinylphenyl)-1-butanone, 1-(biphenyl-4-yl)-2-methyl-2-morpholinopropan-1-one, 1-(biphenyl-4-yl)-2-methoxy-2-morpholinopropan-1-one, and the like.

[0050] Examples of the acylphosphine oxide compound include diphenylacylphenylphosphine oxide, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, tris(phenyl(2,4,6-trimethylbenzoyl)phosphinic acid) polyethylene glycol ester, ethyl(2,4,6-trimethylbenzoyl)phenylphosphinenate, and bis(2,4,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide.

[0051] Examples of oxime ester compounds include 1-[4-(phenylthio)phenyl]octane-1,2-dione, 2-benzoyl oxime, ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(o-acetyl oxime), 3-cyclopentyl-1-(4-(phenylthio)phenyl)propane-1,2-dione-2-(o-benzoyl oxime), ...3-cyclopentyl-1-(4-(phenylthio)phenyl)propane-1,2-dione-2-(o-benzoyl oxime), 3-cyclopentyl-1-(4-(phenylthio)phenyl)propane-1,2-dione-2-(o-acetyl oxime), 3-cyclopentyl-1-(4-(phenylthio)phenyl)propane-1,2-dione-2-(o-acetyl oxime), 3-cyclopentyl-1-(4-(phenylthio)phenyl)propane-1,2-dione -carbazol-3-yl]-3-cyclopentylpropane-1-(o-acetyloxime), methanone, [8-[[(acetyloxy)imino][2-(2,2,3,3-tetrafluoropropoxy)phenyl]methyl]-11-(2-ethylhexyl)-11H-benzo[a]carbazol-5-yl]-,(2,4,6-trimethylphenyl), 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime, and the like.

[0052] Examples of thioxanthone compounds include 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2,4-dichlorothioxanthone, 1-chloro-4-propylthioxanthone, 2-chlorothioxanthone, poly(oxy-1,4-butanediyl), α-[2-[(9-oxo-9H-thioxanthenyl)oxy]acetyl]-ω-[[2-[(9-oxo-9H-thioxanthenyl)oxy]acetyl]oxy]-, 1,3-di({α-[1-chloro-9-oxo-9H-thioxanthen-4-yl]oxy}acetylpoly[oxy(1-methylethylene)])oxy]-2,2-bis({α-[1-chloro-9-oxo-9H-thioxanthen-4-yl]oxy}acetylpoly[oxy(1-methylethylene)])oxymethyl)propane.

[0053] The content of the photopolymerization initiator is preferably 1 to 20% by mass, and more preferably 5 to 15% by mass, based on the total mass of the ink.

[0054] (Amine Compound) In one embodiment of the present invention, the ink may contain an amine compound. There are no particular limitations on the amine compound, and known amine compounds can be used. By using an amine compound as a component of the active energy ray-curable ink, it is expected that the effect of the hydrogen abstraction photopolymerization initiator will be enhanced. Specific examples include N,N-dimethylaniline, N,N-diethylaniline, N,N-dimethyl-p-toluidine, ethyl 4-(dimethylamino)benzoate, N,N-dihydroxyethylaniline, triethylamine, and N,N-dimethylhexylamine, poly(oxy-1,2-ethanediyl,α-[4-(dimethylamino)benzoyl]-ω-[[4-(dimethylamino)benzoyl]oxy]-, bis-N,N-[2-(4-dimethylaminobenzoyl)oxyethylene-1-yl ]methylamine, poly(oxy-1,2-ethanediyl), α-[4-(dimethylamino)benzoyl]-ω-[[4-(dimethylamino)benzoyl]oxy]-, poly[oxy(methyl-1,2-ethanediyl), α-[4-(dimethylamino)benzoyl-ω-butoxy-, 2-butoxyethyl-4-(dimethylamino)benzoate, 2-(dimethylamino)ethyl benzoate, and the like. The amine compounds may be used alone or in combination of two or more.

[0055] (Resin) In one embodiment of the present invention, the ink may contain a resin. By containing a resin, cure shrinkage of the coating film that occurs during curing is alleviated, curling of the substrate is suppressed, and adhesion to the anchoring agent is improved.

[0056] The resin may be used alone or in combination of two or more. The content of the resin is preferably 1 to 20% by mass based on the total mass of the ink.

[0057] Specific examples of the resin include polyvinyl chloride, (meth)acrylic resin, styrene (meth)acrylic resin, epoxy resin, polyester resin, polyurethane resin, cellulose derivatives (e.g., ethyl cellulose, cellulose acetate, nitrocellulose), vinyl chloride-vinyl acetate copolymer, polyamide resin, polyvinyl acetal resin, diallyl phthalate resin, allyl resin, alkyd resin, rosin-modified alkyd resin, petroleum resin, urea resin, synthetic rubber such as butadiene-acrylonitrile copolymer, etc. Of these, diallyl phthalate resin and polyester resin are more preferred from the viewpoint of dispersibility.

[0058] (Polymerization inhibitor) In one embodiment of the present invention, the ink may contain a polymerization inhibitor. Specific examples of the polymerization inhibitor include 4-methoxyphenol, hydroquinone, methylhydroquinone, t-butylhydroquinone, 2,6-di-t-butyl-4-methylphenol, phenothiazine, and aluminum salt of N-nitrosophenylhydroxylamine.

[0059] The content of the polymerization inhibitor is preferably 0.01 to 2% by mass relative to the total mass of the ink, from the viewpoint of maintaining curability and enhancing the stability of the ink.

[0060] (Wax) In one embodiment of the present invention, the ink may contain a wax. By including a wax, it is possible to easily improve rub resistance, scratch resistance, anti-blocking properties, smoothness, and abrasion resistance. There are no particular limitations on the wax, and known waxes can be used. For example, natural waxes and synthetic waxes can be used. Examples of natural waxes include carnauba wax, Japan wax, lanolin, montan wax, paraffin wax, and microcrystalline wax. Examples of synthetic waxes include Fischer-Tropsch wax, polyethylene wax, polypropylene wax, and polytetrafluoroethylene wax.

[0061] The content of the wax is preferably 0.1 to 5% by mass relative to the total mass of the ink.

[0062] (Extender Pigment) In one embodiment of the present invention, the ink may contain a body pigment. Examples of the body pigment include clay, talc, barium sulfate, calcium carbonate, ground calcium carbonate, barium carbonate, magnesium carbonate, silica, and bentonite. Although not particularly limited, talc can be preferably used in one embodiment.

[0063] (Pigment Dispersant) In one embodiment of the present invention, the ink preferably contains a pigment dispersant to further improve pigment dispersibility. There are no particular limitations on the pigment dispersant, and known pigment dispersants can be used. Among these, resin-type pigment dispersants having a basic functional group are preferred, and examples of the basic functional group include primary, secondary, or tertiary amino groups, and nitrogen-containing heterocycles such as pyridine, pyrimidine, and pyrazine. Furthermore, as the skeleton constituting the resin-type pigment dispersant, a fatty acid amine skeleton and / or a urethane skeleton are more preferred, as these easily provide good pigment dispersibility.

[0064] The pigment dispersant is commercially available, and examples thereof include the Ajisper series (Ajisper PB821, PB822, PB824, etc.) manufactured by Ajinomoto Fine-Techno Co., Ltd., the Solsperse series (Solsperse 00, Solsperse 32000, Solsperse 38500, etc.) manufactured by Lubrizol, and the Disperbyk series (BYK-162, BYK-168, BYK-183, etc.) manufactured by BYK-Chemie.

[0065] The content of the pigment dispersant is preferably 0.1 to 10% by mass, and more preferably 0.2 to 5% by mass, based on the total mass of the ink.

[0066] In one embodiment of the present invention, the active energy ray-curable ink used to form the ink layer is preferably at least one ink selected from the group consisting of an active energy ray-curable offset printing ink, an active energy ray-curable flexographic printing ink, and an active energy ray-curable resin letterpress printing ink. These inks have high film strength among active energy ray-curable inks and are difficult to deink. Therefore, the effects of the present invention are particularly pronounced in laminates formed using these inks.

[0067] <Anchor Layer> In one embodiment of the present invention, the anchor layer of the laminate contains an aqueous resin. Such an anchor layer can be obtained by coating an aqueous anchor agent containing the aqueous resin and drying it.

[0068] [Aqueous Anchoring Agent] In one embodiment of the present invention, the aqueous anchoring agent contains water and an aqueous resin.

[0069] [Aqueous Resin] Examples of the aqueous resin include aqueous acrylic resin, aqueous urethane resin, and aqueous polyester resin. These resins may be used alone or in combination of two or more. Among them, aqueous acrylic resin and aqueous urethane resin are preferred, and aqueous acrylic resin is particularly preferred.

[0070] [Acid value of aqueous resin] The acid value of the aqueous resin is preferably 25 to 300 mgKOH / g. When the acid value of the aqueous resin is within the above range, a resin with good alkali solubility is obtained, and the deinking properties of active energy ray-curable inks such as UV inks are improved. The acid value of the aqueous resin is preferably 30 to 275 mgKOH / g, and more preferably 30 to 250 mgKOH / g.

[0071] [Glass transition temperature of aqueous resin] The glass transition temperature (Tg) of the aqueous resin is preferably 10 to 150°C. When the glass transition temperature is in the above range, good blocking resistance and good substrate adhesion can be easily obtained. The glass transition temperature (Tg) of the aqueous resin is preferably 10 to 120°C, and more preferably 10 to 100°C.

[0072] [Water-based acrylic resin] The water-based acrylic resin is preferably a resin obtained by making an acrylic resin having a carboxyl group aqueous (water-soluble) in the presence of an emulsifier and / or a basic compound. The acrylic resin may be a resin having an acrylic monomer unit. It may also be an acrylic resin obtained by copolymerizing a styrene-based monomer, a maleic acid-based monomer, or the like.

[0073] Suitable examples of the acrylic monomer include alkyl esters of (meth)acrylic acid, alkylamides of (meth)acrylic acid, hydroxyalkyl esters of (meth)acrylic acid, etc. The alkyl groups constituting the alkyl esters, etc., preferably have 1 to 18 carbon atoms.

[0074] Suitable examples of the styrene-based monomer include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, and m-methylstyrene. Suitable maleic acid-based monomers include maleic anhydride and maleic acid, and may be in the form of alkyl esters having 1 to 18 carbon atoms, alkylamides having 1 to 18 carbon atoms, or hydroxyalkyl esters having 2 to 4 carbon atoms. In yet another embodiment, the aqueous acrylic resin may use components other than those described above as reaction components for producing the resin. For example, known monomers generally used as reaction components for aqueous acrylic resins may also be used.

[0075] Using these reaction components, acrylic resins can be produced by known production methods. Furthermore, methods using known emulsifiers or polymeric protective colloids can be applied as methods for water-solubilizing resins. Alternatively, a method can be provided in which a carboxyl group is introduced into the molecule and then neutralized with a basic compound. As the basic compound, an amine compound is preferred, and ammonia is preferably used. Furthermore, the aqueous acrylic resin is preferably an aqueous emulsion, more preferably a core-shell type acrylic emulsion, and the core / shell ratio (core:shell) of the acrylic emulsion is preferably 10:90 to 70:30.

[0076] [Aqueous Urethane Resin] The aqueous urethane resin is preferably a polyurethane resin synthesized from a polyol, a hydroxy acid, and a polyisocyanate, or alternatively, a polyurethane urea resin containing a urethane prepolymer having an isocyanate group at its terminal, synthesized from a polyol, a hydroxy acid, and a polyisocyanate, and a polyurethane urea chain-extended with a polyamine.

[0077] Water-based urethane resins and polyurethane urea resins are made water-soluble by introducing ionic groups such as carboxyl groups and sulfonic groups into the resin during the reaction of polyol with polyisocyanate and then neutralizing the resulting resin with a basic compound. From the viewpoint of water resistance, carboxyl groups are preferred as the ionic groups.

[0078] <2> Manufacturing Method of Laminate One embodiment of the present invention relates to a manufacturing method of the laminate of the above embodiment. The laminate is obtained by printing an active energy ray-curable ink on an anchor layer formed from an anchor agent applied to a non-absorbent substrate, and curing the ink with active energy rays to form an ink layer.

[0079] More specifically, in one embodiment, the method for producing a laminate includes: step 1 of applying an aqueous anchor agent containing an aqueous resin to a non-absorbing substrate and drying it in an oven to form an anchor layer, thereby obtaining a laminate having an anchor layer on a non-absorbing substrate; and step 2 of printing an active energy ray-curable ink on the anchor layer of the laminate having an anchor layer on a non-absorbing substrate, and curing it with active energy rays to form an ink layer, thereby obtaining a laminate having an ink layer on the anchor layer.

[0080] As described above, by using an ink that does not contain a colorant (varnish or clear ink), a laminate having a varnish layer on an anchor layer can be obtained.

[0081] It is also possible to print an active energy ray-curable varnish on the ink and then cure it with active energy rays to form a laminate having a varnish layer on an ink layer.

[0082] The non-absorbing substrate (hereinafter also referred to as substrate) is not particularly limited, and known substrates can be used. The substrate may have a single-layer or multi-layer structure. The shape of the substrate is not particularly limited. For example, it may have various shapes such as a sheet, a film, a bottle cap, or a cup. The material constituting the substrate may be at least one selected from the group consisting of plastic, resin, and metal. Specific examples include plastic substrates such as polypropylene (PP), polyethylene (PE), polyethylene terephthalate (PET), and aluminum; plastic substrates having inorganic vapor-deposited layers such as silica and alumina; substrates made of resins such as polyvinyl chloride (PVC), polystyrene (PS), nylon, and cellophane; and metal foils or metal sheets such as aluminum foil. Substrates may also be made of resins such as ABS resin (a copolymer resin of acrylonitrile, butadiene, and styrene) and PC resin (polycarbonate resin). Various additives such as antistatic agents, antifogging agents, and ultraviolet protection agents may be used in the substrate. For example, various additives may be applied to the surface of the substrate. In one embodiment, as will be described later, plastic substrates made of PP, PE, PET, etc. are preferred from the viewpoint of recovering and reusing non-absorbent substrates.

[0083] In the above-mentioned production method, the method for printing the active energy ray-curable ink is not particularly limited as long as it is possible to print an active energy ray-curable offset printing ink, an active energy ray-curable flexographic printing ink, or an active energy ray-curable resin letterpress printing ink. For example, it is preferably any one of offset printing using an active energy ray-curable offset printing ink, resin letterpress printing using an active energy ray-curable resin letterpress printing ink, and flexographic printing using an active energy ray-curable flexographic printing ink.

[0084] In the above-mentioned production method, the method for applying the aqueous anchor agent is not particularly limited, and any known method can be used, such as a roll coater, gravure coater, flexo coater, air doctor coater, blade coater, air knife coater, squeeze coater, impregnation coater, transfer roll coater, kiss coater, curtain coater, cast coater, spray coater, die coater, offset printing, gravure printing, resin letterpress printing, and flexo printing.

[0085] In the above-described production method, the actinic energy ray source used when curing the ink is not particularly limited, and known sources can be used, such as mercury lamps, xenon lamps, metal hydride lamps, excimer lamps, LEDs (light-emitting diodes) such as ultraviolet light-emitting diodes (UV-LEDs) and ultraviolet laser diodes (UV-LDs), electron beam (EB) irradiation devices, and gas or solid-state lasers.

[0086] <3> Deinking method for laminate One embodiment of the present invention relates to a deinking method for laminate. Deinking means removing ink components from a printed non-absorbent substrate (a non-absorbent substrate having an ink layer). Therefore, the deinking method includes a step for removing ink components from the non-absorbent substrate.

[0087] (Step of Removing Ink Component with Alkaline Aqueous Solution) In one embodiment of the present invention, for example, when the laminate of the above embodiment is brought into contact with an alkaline aqueous solution in a treatment tank containing the alkaline aqueous solution, the ink layer can be easily removed. Therefore, the deinking method includes a step of bringing the laminate into contact with an alkaline aqueous solution to remove the ink layer.

[0088] (Alkaline aqueous solution) In one embodiment, the alkaline aqueous solution used in the deinking method may be an aqueous solution containing an alkaline compound. For example, based on the total mass of the aqueous solution, the content of the alkaline compound is preferably 0.5 to 10 mass%, more preferably 1 to 5 mass%. The alkaline compound is not particularly limited. For example, sodium hydroxide (NaOH), potassium hydroxide (KOH), calcium hydroxide (Ca(OH)2 ), ammonia, barium hydroxide (Ba(OH) 2 ), sodium carbonate (Na 2 CO 3 Preferred are NaOH and / or KOH.

[0089] (Ink Component Removal Process) The mechanism by which the ink layer becomes detachable from the laminate upon contact of the alkaline aqueous solution with the laminate is presumably that, because the anchor layer contains the aqueous resin, the alkaline aqueous solution penetrates through the surface of the anchor layer and / or the cross section of the laminate, causing the anchor layer to dissolve. The laminate may be a laminate in which an anchor layer is formed on a non-absorbing substrate, an ink layer is further formed, and then the laminate is shaped into a packaging container through a bag-making process or the like. A laminate in such a shape is preferably cut or crushed in the recycling process or before, and the laminate is brought into contact with the alkaline aqueous solution in a state where the cross section of the laminate is exposed.

[0090] The contact of the laminate with the alkaline aqueous solution is preferably carried out with stirring. The stirring means is not particularly limited, and examples include known stirring equipment such as a general disperser, radial flow turbine blade, axial flow turbine blade, paddle blade, propeller blade, anchor blade, and high shear mixer. Conditions such as the stirring speed are not particularly limited. For example, in the case of a 2-L flask scale, the speed is preferably 100 to 350 rpm, although this depends on the shape and size of the stirring blade. The stirring time is preferably 15 minutes or more and 24 hours or less.

[0091] <4> Method for manufacturing recycled substrate One embodiment of the present invention relates to a method for manufacturing recycled substrates, in which a non-absorbent substrate is recovered from a laminate. A recycled substrate refers to a substrate recovered from a printed non-absorbent substrate (a non-absorbent substrate having an ink layer) in a state in which the ink components have been removed. Therefore, the method for manufacturing recycled substrates includes a step of deinking the laminate and a step of recovering the non-absorbent substrate.

[0092] Therefore, one embodiment of the present invention may be a method for producing a recycled substrate, comprising deinking the ink layer from a laminate having an anchor layer and an ink layer in this order on a non-absorbent substrate, and recovering the non-absorbent substrate, wherein the anchor layer comprises an aqueous resin, the acid value of the aqueous resin being 25 to 300 mgKOH / g, and the glass transition temperature of the aqueous resin being 10 to 150°C, and the ink layer being a cured product of at least one ink selected from an actinic ray-curable offset printing ink, an actinic ray-curable flexographic printing ink, and an actinic ray-curable resin letterpress printing ink, bringing the laminate into contact with an alkaline aqueous solution to dissolve the anchor layer in the alkaline aqueous solution and deinking the ink layer from the non-absorbent substrate, separating and recovering the non-absorbent substrate from the alkaline aqueous solution, and washing and drying the recovered non-absorbent substrate to obtain the recycled substrate.

[0093] In the above embodiment, the aqueous resin preferably includes at least one selected from the group consisting of an aqueous acrylic resin and an aqueous urethane resin, and the non-absorbent substrate preferably includes PP, PE, or PET.

[0094] (Substrate Recovery Step) In one embodiment, the method for producing a recycled substrate includes a step of recovering a non-absorbent substrate after the ink layer has been removed from the laminate. The step of recovering a non-absorbent substrate refers to a step of separating and recovering the non-absorbent substrate from a treatment tank containing a mixture of the alkaline aqueous solution, the peeled ink layer fragments, and the non-absorbent substrate after treating the laminate with an alkaline aqueous solution. The recovered non-absorbent substrate is preferably obtained with high purity. The method for recovering the non-absorbent substrate is not particularly limited. For example, separation and recovery based on the size difference between the non-absorbent substrate and the ink layer fragments is preferred. As another example, separation and recovery based on the difference in specific gravity is also preferred. These methods may be combined appropriately for separation and recovery. In particular, in one embodiment of the method for producing a recycled substrate, a separation and recovery step based on the difference in specific gravity is preferably included, and more preferably, a separation and recovery step based on the difference in specific gravity and a separation and recovery step based on the difference in size may be performed in combination. Note that in the separation and recovery step based on the difference in specific gravity, it is preferred to recover only the substrate that floats in the alkaline aqueous solution in the treatment tank. If impurity components and ink layer fragments in the alkaline aqueous solution settle, they can be easily separated from the non-absorbent substrate, and only the non-absorbent substrate can be recovered more accurately, which is preferable. In this case, the physical properties and transparency of the non-absorbent substrate recycled after recovery can be easily improved. The method for separation based on the difference in specific gravity may be a conventionally known method, such as a method using a fluidized bed or a method using a centrifuge.

[0095] After the ink layer is removed from the laminate, the non-absorbent substrate is recovered. After recovery, the non-absorbent substrate is washed with water and dried to obtain a recycled non-absorbent substrate. In this case, it is preferable that the recycled non-absorbent substrate is as free as possible of any contaminants, including fragments of the removed ink layer. The non-absorbent substrate recycled as described above can be processed into pellets using an extruder or the like and reused as recycled resin. The use of the recycled resin is not limited, and it may be processed into a colorless, transparent film or a molded product to which a colorant is added.

[0096] In one embodiment, various additives may be added as needed when the laminate is brought into contact with the alkaline aqueous solution and stirred. For example, a surfactant may be suitably used, and a nonionic surfactant is particularly preferred. The nonionic surfactant may be a compound known in the art as a deinking agent.

[0097] For example, commercially available deinking agents include deinking agents DI-7020, DI-7027, DI-7250, and DI-767 manufactured by Kao Corporation, the DIA-Z series and DIA-Y series manufactured by Nissin Chemical Industry Co., Ltd., and the Riptor series manufactured by Lion Specialty Chemicals.

[0098] (Ink recovery step) In the above-mentioned substrate recovery step, the ink can be recovered by filtering the alkaline aqueous solution after substrate recovery. At this time, since the material of the anchor layer is soluble in the alkaline aqueous solution, it is possible to extract the ink components with high purity. Therefore, in one embodiment of the present invention, there is provided a method for recovering ink, which includes filtering and recovering the ink layer deinked in the method for producing a recycled substrate of the above-mentioned embodiment.

[0099] The present invention will be specifically described below with reference to examples and comparative examples. However, the present invention is not limited to the following examples. In the examples and comparative examples, "parts" and "%" represent "parts by mass" and "% by mass", respectively.

[0100] 1. Materials for Laminate <1-1> Preparation Example of Anchoring Agent (Anchor Agent 1) 99.0 parts of resin 1 (Hiros X X436 manufactured by Seiko PMC Corporation) and 1.0 part of polyethylene wax (Chemipearl W500 manufactured by Mitsui Chemicals, Inc.) were added and stirred with a disper for 10 minutes to prepare an aqueous anchoring agent (AC1).

[0101] (Anchoring agents 2 to 13) Aqueous anchoring agents (AC2) to (AC13) were prepared using the same formulation as anchoring agent 1, except that resin 1 was changed to resins 2 to 13 as shown in Table 1.

[0102] (Anchoring agent 14) 79.0 parts of resin 14 (Megarpur IM30AL manufactured by MEGARA Corporation), 10.0 parts of ethyl acetate, 10.0 parts of isopropyl alcohol, and 1.0 part of polyethylene wax (Chemipearl W500 manufactured by Mitsui Chemicals, Inc.) were added and stirred with a disper for 10 minutes to prepare an oil-based anchoring agent (AC14).

[0103] (Anchoring Agent 15) 20.0 parts of TMPTA (EO), 60.0 parts of DiTMPTA, 10.0 parts of DPHA, 6.0 parts of 4MBP, 3.0 parts of TPO, and 1.0 part of EDB were mixed and stirred using a butterfly mixer to prepare a UV flexographic acrylic anchoring agent (AC15).

[0104] (Anchoring Agent 16) 10.0 parts of TMPTA (EO), 18.0 parts of DiTMPTA, 7.0 parts of DPHA, 5.0 parts of 4MBP, 2.0 parts of TPO, 1.0 part of EDB, and 57.0 parts of a diallyl phthalate resin varnish prepared as described below were mixed and stirred using a butterfly mixer to produce a UV offset acrylic anchoring agent (AC16).

[0105] The diallyl phthalate resin varnish (active energy ray-curable resin varnish) used in the anchor agent 16 and in Ink Production Example 2 described later was prepared as follows: (Preparation Example of Diallyl Phthalate Resin Varnish) 65.0 parts of DPHA, 6.5 parts of TMPTA (EO), and 3.5 parts of DiTMPTA were mixed and heated to 100° C. with stirring. Next, 25.0 parts of diallyl phthalate resin was mixed and dissolved while maintaining the temperature at 100° C. to prepare a diallyl phthalate resin varnish.

[0106] <1-2> Ink Production Example The rosin-modified phenolic resin varnish (oil-based resin varnish) used in Ink Production Example 1 described below was prepared as follows. (Preparation Example of Rosin-Modified Phenolic Resin) In a reaction vessel, 54.3 parts of gum rosin were reacted in advance with 30.8 parts of tertiary butylphenol and 9.4 parts of 92% by weight paraformaldehyde in a xylene solvent at 100°C for 4 hours under sodium hydroxide catalyst, and the phenolic resin from which moisture had been removed was added dropwise at 150°C and reacted for 2 hours. 5.4 parts of glycerin were then added, and the mixture was reacted for 15 hours at 250°C using 0.1 part of calcium oxide as a catalyst to produce a rosin phenolic resin. (Example of Preparation of Rosin-Modified Phenolic Resin Varnish) Next, 45.0 parts of the rosin-modified phenolic resin as a binder resin, 44.0 parts of soybean oil, 10.0 parts of soybean oil fatty acid normal butyl ester, and 1.0 part of ALCH were placed in a four-neck flask equipped with a stirrer, a reflux condenser with a water separator, and a thermometer, and heated and stirred at 190°C for 1 hour to prepare a rosin-modified phenolic resin varnish.

[0107] (Ink Production Example 1 (Oil-based Ink)) 17.0 parts of RAVEN 1080 Ultra, 3.0 parts of BA-2550, 59.0 parts of the rosin-modified phenolic resin varnish obtained in the above-described Production Example, 20.0 parts of soybean oil, 0.5 parts of MK Dryer, and 0.5 parts of a drying inhibitor CP were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size would be 7.5 μm or less to prepare an ink.

[0108] (Ink Production Example 2 (UV Ink 1)) (Active energy ray-curable offset printing ink, active energy ray-curable resin letterpress printing ink) 17.0 parts of RAVEN 1080 Ultra, 3.0 parts of BA-2550, 6.0 parts of TMPTA (EO), 13.0 parts of DiTMPTA, 7.0 parts of DPHA, 3.0 parts of 379, 1.5 parts of DEABP, 1.5 parts of DETX, 1.0 part of EDB, and 47.0 parts of the diallyl phthalate resin varnish obtained in the above-described Production Example were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less, to prepare an ink.

[0109] (Ink Production Example 3 (UV Ink 2)) (Active energy ray-curable offset printing ink, active energy ray-curable resin letterpress printing ink) 17.0 parts of RAVEN 1080 Ultra, 3.0 parts of BA-2550, 6.0 parts of TMPTA (EO), 13.0 parts of DiTMPTA, 7.0 parts of DPHA, 3.0 parts of 379, 1.5 parts of DEABP, 1.5 parts of DETX, 1.0 part of EDB, and 47.0 parts of MIRAMER PS-4500 were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less, to prepare an ink.

[0110] (Ink Production Example 4 (LED Ink)) (Active energy ray-curable offset printing ink, active energy ray-curable resin letterpress printing ink) 17.0 parts of RAVEN 1080 Ultra, 3.0 parts of BA-2550, 6.0 parts of TMPTA (EO), 10.0 parts of DiTMPTA, 7.0 parts of DPHA, 3.0 parts of 379, 2.0 parts of TPO, 2.0 parts of DEABP, 2.5 parts of 4MBP, 2.5 parts of DETX, 1.0 part of EDB, and 44.0 parts of diallyl phthalate resin varnish were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less, to prepare an ink.

[0111] (Ink Production Example 5 (UV Flexographic Ink) (Active Energy Ray Curable Flexographic Printing Ink)) 15.0 parts of RAVEN 1080 Ultra, 1.0 part of BA-2550, 16.0 parts of TMPTA (EO), 5.0 parts of DiTMPTA, 7.0 parts of DPHA, 3.0 parts of 379, 2.0 parts of DEABP, 2.5 parts of 4MBP, 2.5 parts of DETX, 1.0 part of EDB, and 6.0 parts of Solsperse 24000 were stirred and mixed using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less to prepare an ink. Thereafter, 39.0 parts of TMPTA (EO) was added, and the mixture was stirred and mixed using a butterfly mixer to prepare an ink.

[0112] (Ink Production Example 6 (UV Ink Yellow) (Active Energy Ray-Curable Offset Printing Ink, Active Energy Ray-Curable Resin Letterpress Printing Ink)) 15.0 parts of Permanent Yellow BHS, 6.0 parts of TMPTA(EO), 18.0 parts of DiTMPTA, 7.0 parts of DPHA, 3.0 parts of 379, 1.5 parts of DEABP, 1.5 parts of DETX, 1.0 part of EDB, and 47.0 parts of diallyl phthalate resin varnish were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less, to prepare an ink.

[0113] (Ink Production Example 7 (UV Ink Crimson) (Active Energy Ray-Curable Offset Printing Ink, Active Energy Ray-Curable Resin Letterpress Printing Ink)) 20.0 parts of Permanent Rubine L5B-01, 6.0 parts of TMPTA (EO), 13.0 parts of DiTMPTA, 7.0 parts of DPHA, 3.0 parts of 379, 1.5 parts of DEABP, 1.5 parts of DETX, 1.0 part of EDB, and 47.0 parts of diallyl phthalate resin varnish were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less, to prepare an ink.

[0114] Ink Production Example 8 (UV Ink Blue) (Active Energy Ray-Curable Offset Printing Ink, Active Energy Ray-Curable Resin Letterpress Printing Ink) 20.0 parts of Heliogen Blue D7088, 6.0 parts of TMPTA(EO), 13.0 parts of DiTMPTA, 7.0 parts of DPHA, 3.0 parts of 379, 1.5 parts of DEABP, 1.5 parts of DETX, 1.0 part of EDB, and 47.0 parts of diallyl phthalate resin varnish were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size would be 7.5 μm or less, to prepare an ink.

[0115] (Ink Production Example 9 (EB Ink) (Active Energy Ray-Curable Offset Printing Ink, Active Energy Ray-Curable Resin Letterpress Printing Ink)) 17.0 parts of RAVEN 1080 Ultra, 3.0 parts of BA-2550, 6.0 parts of TMPTA(EO), 13.0 parts of DiTMPTA, 7.0 parts of DPHA, and 54.0 parts of diallyl phthalate resin varnish were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less, to prepare an ink.

[0116] (Varnish Production Example 1 (UV Varnish) (Active Energy Ray-Curable Varnish for Offset Printing, Active Energy Ray-Curable Resin Letterpress Printing Varnish)) 6.0 parts of TMPTA (EO), 13.0 parts of DiTMPTA, 7.0 parts of DPHA, 6.0 parts of 184, 2.0 parts of TPO, 1.0 part of EDB, 3.0 parts of filler, and 62.0 parts of diallyl phthalate resin varnish were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less to produce a varnish.

[0117] Details of the materials used in the above-mentioned anchor agent production examples and ink production examples are as follows. [Colorants] Permanent Yellow BHS: Permanent Yellow BHS (C.I. Pigment Yellow 174) manufactured by Clariant Permanent Rubine L5B-01: Permanent Rubine L5B-01 (C.I. Pigment Red 57:1) manufactured by Clariant HELIOGEN BLUE D7088: HELIOGEN BLUE D7088 (C.I. Pigment Blue 15:3) manufactured by BASF Raven 1080 Ultra: Raven manufactured by Bilra Carbon 1080 Ultra Powder (C.I. Pigment Black 7) BA-2550: Morimura Shoji Co., Ltd., Alkaline Blue Toner BA-2550 (C.I. Pigment Blue 61)

[0118] [Extender pigment] Filler: Matsumura Sangyo Co., Ltd., High Filler #5000PJ, talc

[0119] [(Meth)acrylate compounds] TMPTA (EO): LAROMER LR8863, manufactured by BASF, trimethylolpropane ethylene oxide modified triacrylate DiTMPTA: EBECRYL1142, manufactured by Daicel Allnex Corporation, ditrimethylolpropane tetraacrylate DPHA: MIRAMER M600, manufactured by MIWON Corporation, dipentaerythritol hexaacrylate PS-4500: MIRAMER PS-4500, manufactured by MIWON Corporation, polyester acrylate oligomer

[0120] [Resins] Resin 1: Seiko PMC Corporation's Hi-Loss X436 (acid value 33 mg KOH / g, glass transition temperature 21°C) Resin 2: BASF Corporation's JONCRYL PDX-7615 (acid value 51 mg KOH / g, glass transition temperature 33°C) Resin 3: BASF Corporation's JONCRYL 63D (acid value 213 mg KOH / g, glass transition temperature 73°C) Resin 4: Covestro Corporation's Neocryl A-2091 (acid value 62 mg KOH / g, glass transition temperature 98°C) Resin 5: BASF Corporation's JONCRYL PDX-7732 (acid value 87 mg KOH / g, glass transition temperature 12°C) Resin 6: Gifu Ceramics Manufacturing Co., Ltd.'s Emapoly Resin 7: Gifu Ceramics Manufacturing Co., Ltd. Acris TGV40 (acid value 54 mg KOH / g, glass transition temperature 109 ° C.) Resin 8: Mitsui Chemicals, Inc. Takelac W605 (acid value 25 mg KOH / g, glass transition temperature 100 ° C.) Resin 9: Seiko PMC Corporation Hi-Loss X J-140A (acid value 33 mg KOH / g, glass transition temperature 6 ° C.) Resin 10: Covestro Corporation Neocryl A-1127 (acid value 18 mg KOH / g, glass transition temperature 5 ° C.) Resin 11: Toyochem Co., Ltd. LIOCRYL PFX0302 (acid value 150 mg KOH / g, glass transition temperature 4 ° C.) Resin 12: Taisei Fine Chemical Co., Ltd. Resin 13: JP-W2 manufactured by BASF (acid value 312 mg KOH / g, glass transition temperature 102°C) Resin 14: Megarpur IM30AL manufactured by MEGARA (acid value 0 mg KOH / g, glass transition temperature -10°C) Resin 15: Daisodap A manufactured by Osaka Soda (acid value 2 mg KOH / g, glass transition temperature 150°C)

[0121] [Photopolymerization initiator] 379: Omnirad 379, manufactured by IGM RESINS, 1,2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone TPO: CHEMARK TPO, manufactured by Chemark Chemical Co., 2,4,6-trimethylbenzoyl-diphenylphosphine oxide DEABP: CHEMARK DEABP, manufactured by Chemark Chemical Co., 4,4'-bis(dimethylamino)benzophenone 4MBP: SB-PI 712, manufactured by Sohbo Industrial Co., Ltd. DETX: CHEMARK DETX, manufactured by Chemark Chemical Co., 2,4-diethylthioxanthone 184: IGM RESINS, Omnirad 184, 1-hydroxy-cyclohexyl phenyl ketone

[0122] [Amine Compounds] EDB: CHEMARK EDB, ethyl 4-(dimethylamino)benzoate, manufactured by Chemark Chemical Co.

[0123] [Pigment dispersant] Solsperse 24000: Solsperse 24000 manufactured by Lubrizol

[0124] [Metal Dryer] MK Dryer: MK Dryer manufactured by Toyo Ink Co., Ltd.

[0125] [Drying Retardant] Drying Retardant CP: Drying Retardant CP manufactured by Toyo Ink Co., Ltd.

[0126] [Aluminum gelling agent] ALCH: ALCH, aluminum ethyl acetate diisopropylate, manufactured by Kawaken Fine Chemicals Co., Ltd.

[0127] [Others] Soybean oil fatty acid normal butyl ester: SFB2, manufactured by Toshin Yushi Co., Ltd.

[0128] <2> Production and Evaluation of Laminates (Examples 1 to 29, Comparative Examples 1 to 11) Using the anchoring agents prepared previously, laminates having an anchor layer on a non-absorbing substrate were prepared as follows, and their physical properties were evaluated. In the following description, the non-absorbing substrate will be abbreviated as "substrate." <Printing (Coating) of Anchor Agent on Substrate> In Examples 1 to 29 and Comparative Examples 1, 4 to 8, and 11, an anchoring agent shown in Table 1 was applied to the substrate using a bar coater (No. 4, manufactured by Yasuda Seiki Co., Ltd.). The substrate was then dried in an oven at 60°C for 10 minutes to produce an anchor layer. In this manner, laminates having an anchor layer on a substrate were obtained. In Comparative Examples 9 and 10, an anchoring agent shown in Table 1 was applied to the substrate using a bar coater (No. 4, manufactured by Yasuda Seiki Co., Ltd.). The coating was then cured using an ultraviolet curing device (160 W / cm metal halide lamp) manufactured by iGraphics Co., Ltd. at a conveyor speed of 30 m / min to produce an anchor layer. In this way, a laminate having an anchor layer on a substrate was obtained.

[0129] The substrates listed in Table 1 are as follows: PP1: Polypropylene sheet manufactured by Okamoto Corporation PP2: Novatec PP manufactured by Japan Polypropylene Corporation PE1: Taiko FC manufactured by Futamura Chemical Co., Ltd. PE2: Novatec HD manufactured by Japan Polyethylene Corporation PET: Reshine manufactured by Toyobo Co., Ltd. Aluminum vapor deposition: SPECIALITIES manufactured by Gojo Paper Co., Ltd. Aluminum foil: Leadmax manufactured by Toyo Aluminum K.K. Synthetic paper: New Yupo FGS manufactured by Yupo Corporation PVC: PVC80C P manufactured by Lintec Corporation PS: Styrophane manufactured by Oishi Sangyo Co., Ltd. Nylon: Emblem manufactured by Unitika Ltd. Cellophane: PL manufactured by Futamura Chemical Co., Ltd. Metal: ET2.8 / 2.8T2.5B manufactured by Nippon Steel Corporation

[0130] <Evaluation of Laminates Having an Anchor Layer on a Substrate> The properties of the laminates (anchor agent coated products) having an anchor layer on a substrate obtained in Examples 1 to 29 and Comparative Examples 1, 4 to 8, and 11 were evaluated as follows. (Blocking Resistance) The anchor agent coated products obtained in Examples 1 to 29 and Comparative Examples 1, 4 to 8, and 11 were cut into pieces measuring 4 cm wide and 4 cm long. The coated and uncoated surfaces of the two cut-out coated products were brought into close contact with each other, and a load of 10 N / cm was applied. 2 The coated sheets were then heated in an oven at 60°C for 24 hours. The coated sheets were then peeled off and evaluated. The results are shown in Table 1. (Evaluation criteria) Good (G): No noise or resistance was heard when peeled off. Poor (F): A crackling sound was heard when peeled off. There was significant resistance. Note that a good rating in the above evaluations is preferred in practice.

[0131] (Adhesion) An adhesive tape (Cellotape (registered trademark) manufactured by Nichiban Co., Ltd., 18 mm wide) was attached to the surface of the anchor layer of the prepared laminate. The adhesive tape attached to the surface of the anchor layer was peeled off in a direction perpendicular to the substrate at an angle of 90 degrees, and the adhesion to the substrate was evaluated based on the proportion of the coating area of ​​the anchor layer that peeled off from the substrate. The results are shown in Table 1. (Evaluation criteria) A: No peeling of the coating of the anchor layer B: No peeling of the coating of the anchor layer + B: Peeling of the anchor layer coating is less than 10%. C: Peeling of the anchor layer coating is 10% or more but less than 30%. + C: Peeling of the anchor layer coating is 30% or more but less than 70%. C: Peeling of 70% or more of the anchor layer coating is

[0132] <Printing (Coating) of Ink and Varnish> In Examples 1 to 21, 24 to 27 and Comparative Examples 1, 4 to 10, the inks shown in Table 1 were printed on half the area of ​​the substrate using an RI tester (a simple printing machine (capable of printing offset printing inks, flexographic printing inks, and resin letterpress printing inks) manufactured by Akebono Seisakusho Co., Ltd.) with an ink gauge of 0.25 mL. The ink coating on this printed material was then cured using an ultraviolet curing device (160 W / cm metal halide lamp) manufactured by iGraphics Co., Ltd. at a conveyor speed of 30 m / min, thereby producing an ink layer. In this manner, a laminate (non-absorbing substrate / anchor layer / ink layer) was obtained.

[0133] In Example 22, the sample ink shown in Table 1 was printed on the anchor layer of the previously prepared laminate (substrate / anchor layer) using an RI tester with an ink gauge of 0.25 mL, covering only half the area of ​​the substrate. The printed matter was then cured using an ultraviolet curing device (160 W / cm metal halide lamp) manufactured by iGraphics Co., Ltd. at a conveyor speed of 100 m / min to form an ink layer. In this way, a laminate (substrate / anchor layer / ink layer) was obtained.

[0134] In Example 23, the sample ink shown in Table 1 was printed on the anchor layer of the previously prepared laminate (substrate / anchor layer) using an RI tester with an ink gauge of 0.25 mL, covering only half the area of ​​the substrate, and the printed matter was then irradiated with 30 kGy of electron beams using a low-energy electron beam irradiation device manufactured by ESI Corporation (applied voltage 175 kV, nitrogen-substituted atmosphere with an oxygen concentration of 50 ppm) to cure the ink, thereby preparing an ink layer. In this way, a laminate (substrate / anchor layer / ink layer) was obtained.

[0135] In Example 28, a UV varnish prepared by mixing two parts of UV ink 1 with 0.25 mL of ink was printed onto half of the surface area of ​​the substrate on the anchor layer of the previously prepared laminate (substrate / anchor layer) using an RI tester. The ink coating was then cured using an ultraviolet curing device (160 W / cm metal halide lamp) manufactured by iGraphics Co., Ltd. at a conveyor speed of 30 m / min to produce an ink layer. In this way, a laminate (substrate / anchor layer / ink layer) was obtained.

[0136] In Example 29, UV ink 1 was printed on the anchor layer of the previously prepared laminate (substrate / anchor layer) using an RI tester with an ink gauge of 0.25 mL, covering only half of the substrate's area. The printed matter was then cured using an iGraphics UV curing device (160 W / cm metal halide lamp) at a conveyor speed of 30 m / min to form an ink layer. Furthermore, using an RI tester, UV varnish was printed on the ink layer with an ink gauge of 0.25 mL, and then the printed matter was cured using an iGraphics UV curing device (160 W / cm metal halide lamp) at a conveyor speed of 30 m / min to form a varnish layer. In this way, a laminate (substrate / anchor layer / ink layer / varnish layer) was obtained.

[0137] In Comparative Example 11, the sample ink shown in Table 1 was printed on the anchor layer of the previously prepared laminate (non-absorbent substrate / anchor layer) using an RI tester with 0.25 mL of ink gauge, covering only half of the substrate area. The ink was then left at room temperature for 24 hours to cure, producing an ink layer. In this manner, a laminate (non-absorbent substrate / anchor layer / ink layer) was obtained. In Comparative Examples 2 and 3, the ink shown in Table 1 was printed directly onto the non-absorbent substrate using an RI tester with 0.25 mL of ink gauge, covering only half of the substrate area. The ink was then cured using an ultraviolet curing device (160 W / cm metal halide lamp) manufactured by iGraphics Co., Ltd. at a conveyor speed of 30 m / min, producing an ink layer. In this manner, a laminate (non-absorbent substrate / ink layer) was obtained.

[0138] <Evaluation of Laminates Having an Ink Layer on an Anchor Layer> The laminates obtained as described above were subjected to performance evaluation according to the following method. The results are shown in Table 1. (Residual Solvent) The residual solvent in the obtained laminates was evaluated. The laminates of Examples 1 to 29 and Comparative Examples 1 to 11 were cut into pieces measuring 10 cm wide and 10 cm long, and 100 of the cut laminates were placed in an eggplant flask, sealed, and then heated (temperature: 80°C, 30 minutes). Thereafter, 0.4 ml of air was removed from the flask and analyzed by gas chromatography (GC) to confirm the amount of solvent component. (Evaluation Criteria) A: The total amount of residual solvent was 0.5 mg / cm 2 It was less than. B + : The total amount of residual solvent is 0.5 mg / cm 2 1mg / cm or more 2 B: The total amount of residual solvent was less than 1 mg / cm 2 2mg / cm or more 2 It was less than. + : The total amount of residual solvent is 2 mg / cm 2 3mg / cm or more 2 C: The total amount of residual solvent was less than 3 mg / cm 2 That was all. + " and "B" are practically preferred.

[0139] (Evaluation of Scratch Resistance) The prepared laminate was evaluated by rubbing the ink surface with a cotton cloth. The less rubbing, the better the scratch resistance. The evaluation criteria are as follows: "A", "B", "C", "D", "E", "F", "G", "H", "I", "I", "J", "J", "J", "J", "K", "K" and "K" are as follows: + "A" and "B" are practically preferable. (Evaluation criteria) A: No rubbing on the printed surface where the ink is applied. B + A: The ink is rubbed down to the surface of the printed surface where it has been spread. B: The ink is rubbed down to the middle part of the printed surface where it has been spread. C + : The ink is rubbed off to the bottom of the printed surface. C: The coating on the printed surface where the ink is spread is gone.

[0140] (Evaluation of deinking properties) The laminates prepared in Examples 1 to 29 and Comparative Examples 1 to 11 were aged at 60°C for one week, and then stored for a further 10 days in an environment of room temperature 23±1°C and humidity 50±2%. After that, the laminates were cut into 30 x 30 mm pieces, and 90 g of each piece was used as a sample for testing.

[0141] <Deinking test> A 2L flask was charged with 1.5L of 30°C warm water, 11mL of 3.75% aqueous sodium hydroxide solution, and 11mL of a deinking agent diluted to 1.5% (DI-7027 manufactured by Kao Corporation), followed by the addition of the sample and stirring at 300 rpm for 20 minutes. Two minutes after stirring began, any sample adhering to the lid was washed away into the tank with a small amount of water. After the deinking was complete, the substrate was removed and the area of ​​the 30 x 30mm sample that was covered with ink (the proportion of ink that had been removed from the substrate) was visually evaluated. (Evaluation criteria) A: Ink was removed from 99% or more of the substrate B: Ink was removed from 99% or more of the substrate + B: Ink has come off from 95% or more but less than 99% of the substrate. B: Ink has come off from 90% or more but less than 95% of the substrate. C: Ink has come off from less than 90% of the substrate.

[0142] (Blocking Resistance) The prepared laminate was cut into a size of 4 cm wide and 4 cm long so that half of the laminate was the portion printed with ink (coated surface) and half was the portion not printed with ink (uncoated surface). The coated surface and the uncoated surface of the cut laminate were brought into close contact with each other, and a load of 10 N / cm was applied to the laminate thus brought into close contact. 2 The laminate was heated in an oven at 60°C for 24 hours. After that, the adhered laminate was peeled from the other laminate and evaluated. (Evaluation criteria) Good (G): No noise or resistance was heard when peeled. Poor (F): A crackling sound was heard when peeled. There was a large resistance. Note that a good rating in the above evaluations is practically preferable.

[0143] In the laminate having an anchor layer on a substrate, both the blocking resistance and adhesion were evaluated as "A" and "B". + In the case of a laminate having an ink layer on an anchor layer, the three evaluations of residual solvent, scratch resistance, and deinking ability are all rated as "A" or "B".+ " or "B" can be considered to be practical.

[0144] From the above, it has been found that according to the present invention, even when a laminate is formed using at least one ink selected from the group consisting of an active energy ray-curable offset printing ink, an active energy ray-curable flexographic printing ink, and an active energy ray-curable resin letterpress printing ink, it is possible to obtain excellent deinking properties while maintaining print quality such as scratch resistance and adhesion required in the market. Therefore, according to the present invention, it is also possible to provide a method for producing a recycled substrate from a laminate, and a method for recovering ink from a laminate.

[0145]

[0146]

[0147]

[0148]

Claims

1. A laminate having an anchor layer and an ink layer in this order on a non-absorbing substrate, wherein the anchor layer contains an aqueous resin, the aqueous resin has an acid value of 25 to 300 mgKOH / g, and the aqueous resin has a glass transition temperature of 10 to 150°C, and the ink layer is a cured product of at least one ink selected from an active energy ray-curable offset printing ink, an active energy ray-curable flexographic printing ink, and an active energy ray-curable resin letterpress printing ink.

2. The laminate according to claim 1, wherein the aqueous resin comprises at least one resin selected from the group consisting of aqueous acrylic resins and aqueous urethane resins.

3. A method for producing a laminate, comprising: step 1 of applying an anchor agent containing water and an aqueous resin to a non-absorbing substrate, and drying in an oven to form an anchor layer, thereby obtaining a laminate having an anchor layer on a non-absorbing substrate; and step 2 of printing at least one ink selected from an active energy ray curable offset printing ink, an active energy ray curable flexographic printing ink, and an active energy ray curable resin letterpress printing ink on the anchor layer of the laminate having an anchor layer on a non-absorbing substrate, and curing the ink with active energy rays to form an ink layer, thereby obtaining a laminate having an ink layer on the anchor layer, wherein the acid value of the aqueous resin is 25 to 300 mgKOH / g, and the glass transition temperature of the aqueous resin is 10 to 150°C.

4. The method for producing a laminate according to claim 3, wherein the aqueous resin comprises at least one resin selected from the group consisting of an aqueous acrylic resin and an aqueous urethane resin.

5. A method for deinking a laminate having an anchor layer and an ink layer in this order on a non-absorbing substrate, wherein the anchor layer contains an aqueous resin, the aqueous resin has an acid value of 25 to 300 mg KOH / g, and the aqueous resin has a glass transition temperature of 10 to 150°C, and the ink layer is a cured product of at least one ink selected from an active energy ray curable offset printing ink, an active energy ray curable flexographic printing ink, and an active energy ray curable resin letterpress printing ink, and the method for deinking a laminate comprises stirring the laminate in an alkaline aqueous solution to dissolve the anchor layer in the alkaline aqueous solution, and deinking the ink layer from the non-absorbing substrate.

6. The method for deinking a laminate according to claim 5, wherein the aqueous resin comprises at least one selected from the group consisting of aqueous acrylic resins and aqueous urethane resins.

7. A method for recovering ink, comprising filtering and recovering the ink layer deinked by the method of claim 5 or 6.

Citation Information

Patent Citations

  • Organic solvent-based printing ink, printed material, and laminate

    JP2020090627A

  • Method for producing phosphate-containing composition

    JP2023066274A

  • Deinking method for laminate

    JP7070772B1

  • Ink jet recording ink, deinking pulp and manufacturing method of the same

    JP2015178633A

  • Packaging material, and recycled base material production method

    JP2021098295A