Flame-retardant adhesive composition and flame-retardant adhesive tape

The use of an acidic phosphorus-based flame retardant and alkylated melamine curing agent in adhesive tapes addresses toxicity and corrosion issues, enhancing flame retardancy and adhesion, ensuring reliable electrical insulation and preventing peeling when wrapped around wires.

WO2024214476A1PCT designated stage expired Publication Date: 2024-10-17TERAOKA SEISAKUSHO CO LTD

Patent Information

Application Number
PCT/JP2024/010051
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2024-03-14
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Conventional flame-retardant adhesive tapes in the electronics and electrical fields face issues with toxicity from halogen-based flame retardants and antimony compounds, corrosion from acidic flame retardants, and peeling problems when wrapped around electrical wires, leading to deterioration of electrical properties and insulation failures.

Method used

A flame-retardant adhesive composition using an acidic phosphorus-based flame retardant with a pH between 2 and 6, combined with an alkylated melamine curing agent, which suppresses corrosion and improves adhesion, and a pressure-sensitive adhesive tape with a specific adhesive layer structure to prevent peeling.

Benefits of technology

The solution provides high flame retardancy, resistance to electrical property deterioration, and prevents peeling when wrapped around thin wires, ensuring reliable insulation and adhesion while avoiding toxic substances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure 00000029_0000
    Figure 00000029_0000
  • Figure 00000029_0001
    Figure 00000029_0001
Patent Text Reader

Abstract

Provided is an adhesive composition which enables the achievement of an adhesive tape that has high flame retardancy and is not likely to cause deterioration in the electrical characteristics of a member such as an electric wire due to corrosion or the like. This flame-retardant adhesive composition contains an adhesive polymer, a curing agent, and a flame retardant, the flame-retardant adhesive composition being characterized in that the curing agent contains an alkylated melamine curing agent and the flame retardant contains an acidic phosphorus-based flame retardant.
Need to check novelty before this filing date? Find Prior Art

Description

Flame-retardant adhesive composition and flame-retardant adhesive tape

[0001] The present invention relates to a flame-retardant pressure-sensitive adhesive composition and a flame-retardant pressure-sensitive adhesive tape.

[0002] In the electronics and electrical fields, high flame retardancy and insulation are required for the adhesive tapes that make up these products to ensure product safety. A common method of imparting flame retardancy to adhesive tapes has been to blend a halogen-based flame retardant with an antimony compound as a flame retardant aid into the adhesive. However, halogen-based flame retardants generate toxic gases when burned, and antimony compounds themselves are toxic, leading experts to point out their potential adverse effects on the human body.

[0003] In order to solve these problems, Patent Document 1 discloses an adhesive tape that does not use a halogen-based flame retardant or an antimony compound, but has an adhesive layer made of a composition in which an aromatic phosphate ester-based flame retardant (monomer-type aromatic phosphate ester, aromatic condensed phosphate ester) and a nitrogen-containing phosphate compound-based flame retardant (melamine polyphosphate, etc.) are added to a base polymer at a specific ratio, and it is described that this adhesive tape has excellent flame retardancy, adhesiveness, etc., and can effectively prevent deposition of the aromatic phosphate ester-based flame retardant on the surface of the adhesive layer.

[0004] Patent Document 2 discloses an adhesive containing an acrylic polymer obtained by using a specific amount of a carboxyl group-containing monomer, an isocyanate-based curing agent, and a phosphinate salt having a specific average particle size in specific ratios, and an adhesive tape having an adhesive layer made of this adhesive, and describes that this adhesive has flame retardancy, excellent adhesiveness, and also excellent adhesive retention.

[0005] JP 2006-219564 A JP 2012-149183 A

[0006] However, in order to obtain an adhesive with sufficient flame retardancy using the method described in Patent Document 1, it is necessary to use a combination of multiple specific flame retardants, and in reality, it takes a long time to disperse these uniformly.

[0007] On the other hand, many highly flame-retardant flame retardants are acidic, and when used in the electronics and electrical fields, they are prone to corrosion problems such as dissolution and deterioration of metals, and have the problem of deteriorating the electrical properties of components such as electric wires. The pressure-sensitive adhesive tape described in Patent Document 2 contains a phosphinate in the pressure-sensitive adhesive layer, which may cause corrosion.

[0008] Generally, rust inhibitors such as benzotriazole are used to prevent corrosion of electric wires. However, the inventors' research has revealed that the use of benzotriazole in adhesives containing acidic flame retardants actually causes severe corrosion of electric wires. Another corrosion prevention method is to add a free base to the adhesive to reduce the acidity, but this has the problem of reducing the cohesive strength of the adhesive after accelerated heat and humidity testing. In particular, adhesives containing materials containing ester bonds, such as (meth)acrylic polymers, are likely to experience a reduction in cohesive strength due to the cleavage of the ester bonds.

[0009] As described above, it has been difficult to solve the problems that arise when an acidic flame retardant is used in an adhesive by conventional methods.

[0010] Furthermore, when adhesive tapes are used for insulation purposes, for example, when they are wrapped around a coil around which an electric wire is wound, there is a problem that the adhesive tape may peel off depending on the structure of the adhesive.

[0011] Therefore, an object of the present invention is to solve the above problems and to provide a pressure-sensitive adhesive composition that can provide a pressure-sensitive adhesive tape that is highly flame-retardant and resistant to deterioration of electrical properties due to corrosion of members such as electric wires, etc., and a flame-retardant pressure-sensitive adhesive tape using the same. Another object of the present invention is to provide a pressure-sensitive adhesive composition that can provide a pressure-sensitive adhesive tape that is highly flame-retardant and resistant to deterioration of electrical properties due to corrosion of members such as electric wires, etc., and that is resistant to peeling even when wound, and a flame-retardant pressure-sensitive adhesive tape using the same.

[0012] The present invention includes the following aspects [1] to

[19] . [1] A flame-retardant pressure-sensitive adhesive composition comprising a pressure-sensitive adhesive polymer, a curing agent, and a flame retardant, wherein the curing agent comprises an alkylated melamine curing agent, and the flame retardant comprises an acidic phosphorus-based flame retardant. [2] The flame-retardant pressure-sensitive adhesive composition according to [1], wherein the acidic phosphorus-based flame retardant has a pH of 2 or more and 6 or less, as measured by the following pH measurement method. (pH Measurement Method) 1 g of the flame retardant and 50 g of ion-exchanged water are mixed at room temperature (23±2°C) and stirred for 1 minute. After 10 minutes, the pH of the resulting mixture is measured using a glass electrode pH meter. [3] The flame-retardant pressure-sensitive adhesive composition according to [1] or [2], wherein the acidic phosphorus-based flame retardant is a phosphinic acid-based flame retardant and / or a polyphosphoric acid-based flame retardant. [4] The flame-retardant pressure-sensitive adhesive composition according to [1] or [2], wherein the acidic phosphorus-based flame retardant is at least one selected from the group consisting of phosphinates, alkylphosphinates, and melamine polyphosphates. [5] The flame-retardant pressure-sensitive adhesive composition according to any one of [1] to [4], wherein the flame retardant is a flame retardant that is not liquid at 23°C. [6] The flame-retardant pressure-sensitive adhesive composition according to any one of [1] to [5], wherein the content of the acidic phosphorus-based flame retardant is 20 to 60 parts by mass per 100 parts by mass of the pressure-sensitive adhesive polymer, and the content of the alkylated melamine curing agent is 0.03 to 0.5 parts by mass per 100 parts by mass of the pressure-sensitive adhesive polymer. [7] The flame-retardant pressure-sensitive adhesive composition according to any one of [1] to [6], further comprising a curing agent other than an alkylated melamine curing agent. [8] The flame-retardant pressure-sensitive adhesive composition according to [7], wherein the curing agent other than the alkylated melamine curing agent is at least one selected from the group consisting of an epoxy-based curing agent, a metal chelate-based curing agent, an isocyanate-based curing agent, an acid anhydride-based curing agent, an amine-based curing agent, and an aziridine-based curing agent. [9] The flame-retardant pressure-sensitive adhesive composition according to [7], wherein the curing agent other than the alkylated melamine curing agent is an epoxy-based curing agent.

[10] The flame-retardant pressure-sensitive adhesive composition according to any one of [7] to [9], wherein the content of the curing agent other than the alkylated melamine curing agent is 0.002 parts by mass or more and 0.5 parts by mass or less per 100 parts by mass of the pressure-sensitive adhesive polymer.

[11] The flame-retardant pressure-sensitive adhesive composition according to any one of [1] to

[10] , wherein the pressure-sensitive adhesive polymer is a (meth)acrylic polymer.

[12] The flame-retardant pressure-sensitive adhesive composition according to any one of [1] to

[11] , wherein the peel distance measured in the following wrapping test is 7 mm or less. (Wrapping test) A release agent (long-chain alkyl pendant polymer) was applied to one side of a 50 μm-thick PET film using a Mayer bar at 0.15 g / m. 2After coating, the film was dried at 80°C for 1 minute. A flame-retardant adhesive composition was then coated on the other side of the PET film, dried at 100°C for 1 minute, and processed to a width of 10 mm to prepare a test adhesive tape. The test adhesive tape (10 mm wide) was wrapped around a round iron nail having a diameter of 5.20 mm ± 0.10 mm, with both longitudinal end portions of the test adhesive tape aligned, and the test adhesive tape was overlapped and wound two and a half times while applying a load of 100 gf (9.8 mN). The end was cut off to prepare a test sample without peeling. The test sample was left to stand for 20 minutes in an environment at a temperature of 23 ± 1°C and a relative humidity of 50 ± 5%, and then heated for 1 hour in a dryer set at 120°C. The length of the peeled portion (peel distance) at the end of the adhesive tape of the obtained test sample was measured with a ruler.

[13] A flame-retardant pressure-sensitive adhesive tape having a substrate and a pressure-sensitive adhesive layer provided on at least one surface of the substrate, wherein the pressure-sensitive adhesive layer comprises the flame-retardant pressure-sensitive adhesive composition according to any one of [1] to

[12] .

[14] The flame-retardant pressure-sensitive adhesive tape according to

[13] , wherein the substrate comprises at least one layer made of an electrically insulating material.

[15] The flame-retardant pressure-sensitive adhesive tape according to

[13] or

[14] , wherein the pressure-sensitive adhesive layer is provided on one surface of the substrate, and at least the outermost layer on the side of the substrate opposite to the side on which the pressure-sensitive adhesive layer is provided comprises a resin material.

[16] The flame-retardant pressure-sensitive adhesive tape according to

[15] , wherein the resin material is polyester.

[17] The flame-retardant pressure-sensitive adhesive tape according to any one of

[13] to

[16] , which passes the UL510 (standard for electrical insulating tapes) flammability test.

[18] The flame-retardant pressure-sensitive adhesive tape according to any one of

[13] to

[17] , which has an electrolytic corrosion coefficient of 0.98 or more as measured in accordance with JIS C 2107:2011 (7.8.2 Method B).

[19] The flame-retardant pressure-sensitive adhesive tape according to any one of

[13] to

[18] , which is used for electrical insulation.

[0013] According to one embodiment of the present invention, it is possible to provide a pressure-sensitive adhesive composition from which a pressure-sensitive adhesive tape having high flame retardancy and being resistant to deterioration in electrical properties due to corrosion of members such as electric wires, etc. can be obtained, and a flame-retardant pressure-sensitive adhesive tape using the same. According to another embodiment of the present invention, it is possible to provide a pressure-sensitive adhesive composition from which a pressure-sensitive adhesive tape having high flame retardancy and being resistant to deterioration in electrical properties due to corrosion of members such as electric wires, etc., and which is resistant to peeling even when wound, and a flame-retardant pressure-sensitive adhesive tape using the same.

[0014] 1 is a schematic cross-sectional view showing an example of the layer structure of the flame-retardant pressure-sensitive adhesive tape according to the present invention. 2 is a schematic cross-sectional view showing another example of the layer structure of the flame-retardant pressure-sensitive adhesive tape according to the present invention. 3 is an explanatory diagram of a method for measuring the adhesion (peel distance) of the flame-retardant pressure-sensitive adhesive tape when it is wound (winding test).

[0015] Preferred embodiments of the present invention will now be described.

[0016] A flame-retardant adhesive composition according to one embodiment of the present invention comprises an adhesive polymer, a curing agent (crosslinking agent) for the adhesive polymer, and a flame retardant, the curing agent comprising an alkylated melamine curing agent and the flame retardant comprising an acidic phosphorus-based flame retardant.A flame-retardant adhesive tape according to another embodiment of the present invention comprises a substrate and an adhesive layer provided on at least one surface of the substrate, the adhesive layer comprising the flame-retardant adhesive composition.

[0017] The present inventors focused on the problem of deterioration of electrical properties due to corrosion when an acidic flame retardant is used in the adhesive layer of a flame-retardant adhesive tape applied to the electronics and electrical fields. As a result of extensive research, they discovered that the deterioration of electrical properties can be suppressed by using an alkylated melamine curing agent as a curing agent (crosslinking agent) for the adhesive polymer, leading to the completion of the present invention. They also discovered that when the adhesive layer is formed from a specific adhesive composition, the adhesive tape is less likely to peel off even when wrapped around a thin electric wire. Hereinafter, embodiments of the present invention will be described in detail.

[0018] (Flame Retardant) The flame retardant contained in the flame retardant composition and the pressure-sensitive adhesive layer of the pressure-sensitive adhesive tape according to the present invention includes an acidic phosphorus-based flame retardant. The acidic phosphorus-based flame retardant is preferably a phosphorus-based flame retardant having a pH of 2 or more and 6 or less, as measured by the following pH measurement method. <pH Measurement Method> At room temperature (23±2°C), 1 g of the flame retardant and 50 g of ion-exchanged water are mixed and stirred for 1 minute using a glass rod. After 10 minutes have passed, the pH of the resulting mixture is measured using a glass electrode pH meter.

[0019] Examples of the acidic phosphorus-based flame retardant include phosphinic acid flame retardants such as phosphinate salts or alkylphosphinate salts, such as aluminum phosphinate, aluminum dimethylphosphinate, aluminum ethylmethylphosphinate, aluminum diethylphosphinate, aluminum methyl-n-propylphosphinate, methane di(aluminum methylphosphinate), benzene-1,4-(dimethylphosphinate), aluminum methylphenylphosphinate, and aluminum diphenylphosphinate; melamine / melam / melem salts of phosphoric acid or polyphosphoric acid, such as melamine phosphate, dimelamine phosphate, melamine pyrophosphate, melamine polyphosphate, melam polyphosphate, and melem polyphosphate; and acidic phosphate esters such as methyl acid phosphate, ethyl acid phosphate, isopropyl acid phosphate, butyl acid phosphate, butoxyethyl acid phosphate, and 2-ethylhexyl acid phosphate. Among these, preferred acidic phosphorus-based flame retardants include phosphinic acid flame retardants and polyphosphate flame retardants, and more preferably at least one selected from phosphinates, alkylphosphinates, and melamine polyphosphates. Examples of phosphinates include a flame retardant manufactured by Universal Chemtech Co., Ltd. under the product name PNF100R. Examples of alkylphosphinates include a flame retardant manufactured by Universal Chemtech Co., Ltd. under the product name OMP-800. Examples of melamine polyphosphates include a flame retardant manufactured by Sanwa Chemical Co., Ltd. under the product name (grade name): MPP-A.

[0020] Furthermore, the flame retardant contained in the flame-retardant pressure-sensitive adhesive composition and the pressure-sensitive adhesive layer is preferably a flame retardant that is not liquid at 23° C. under atmospheric pressure (non-fluid flame retardant) in order to prevent the flame retardant from seeping out. Here, a flame retardant that is not liquid at 23° C. refers to a flame retardant that is semi-solid, gel-like, or solid at 23° C. A flame retardant that is solid at 23° C. is more preferred.

[0021] The content of the acidic phosphorus-based flame retardant in the flame-retardant adhesive composition and the adhesive layer is preferably 20 to 60 parts by mass, more preferably 30 to 50 parts by mass, per 100 parts by mass of the adhesive polymer. When the content of the acidic phosphorus-based flame retardant is 20 parts by mass or more per 100 parts by mass of the adhesive polymer, a sufficient flame-retardant effect can be obtained. Furthermore, when the content of the acidic phosphorus-based flame retardant is 60 parts by mass or less per 100 parts by mass of the adhesive polymer, deterioration in insulating properties, precipitation of the acidic phosphorus-based flame retardant on the surface of the adhesive layer, deterioration in the cohesive strength of the adhesive layer, deterioration in adhesive strength as an adhesive tape, etc. can be suppressed, and the corrosion prevention effect of the alkylated melamine curing agent can be more easily obtained.

[0022] From the viewpoint of further improving flame retardancy, the flame-retardant pressure-sensitive adhesive composition and the pressure-sensitive adhesive layer may contain a flame retardant (co-component) other than the acidic phosphorus-based flame retardant, as long as the desired effects of the present invention are not impaired. Examples of the co-component include metal hydroxides, melamine compounds, triazine compounds, guanidine compounds, guanylurea compounds, dicyandiamide, and boric acid compounds. Examples of the metal hydroxides include aluminum hydroxide, magnesium hydroxide, and calcium hydroxide. Examples of the melamine compounds include melamine sulfate, melamine nitrate, melamine borate, melamine phthalate, melamine sulfamate, and melamine cyanurate. These co-components may be used alone or in combination of two or more.

[0023] When the flame-retardant pressure-sensitive adhesive composition and the pressure-sensitive adhesive layer contain the co-component of a flame retardant, the content of the co-component in the flame-retardant pressure-sensitive adhesive composition and the pressure-sensitive adhesive layer can be set to 0.1 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the pressure-sensitive adhesive polymer, and it is preferable that the total amount of the co-component, the acidic phosphorus-based flame retardant, and the flame-retardant auxiliary described below is 60 parts by mass or less.

[0024] The flame-retardant pressure-sensitive adhesive composition and the pressure-sensitive adhesive layer may also contain a flame-retardant aid. Specific examples of the flame-retardant aid include zinc oxide, lead sulfide, tin oxide, zinc stannate, and zinc borate. These may be used alone or in combination. When the flame-retardant pressure-sensitive adhesive composition and the pressure-sensitive adhesive layer contain the flame-retardant aid, the content of the flame-retardant aid in the flame-retardant pressure-sensitive adhesive composition and the pressure-sensitive adhesive layer may be set to 0.1 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the pressure-sensitive adhesive polymer, and it is preferable that the total amount of the flame-retardant aid, the acidic phosphorus-based flame retardant, and the combined components is 60 parts by mass or less.

[0025] The average particle size of the flame retardant and the flame retardant auxiliary is preferably 0.5 μm or more and 25 μm or less, more preferably 1 μm or more and 10 μm or less. When the average particle size is 0.5 μm or more, they are easily handled as powder. Furthermore, when the average particle size is 25 μm or less, they are highly stable after being dispersed in the flame-retardant pressure-sensitive adhesive composition and the pressure-sensitive adhesive layer, and are less likely to cause surface roughness due to exposure to the pressure-sensitive adhesive layer, so that the adhesive strength is less likely to decrease.

[0026] (Adhesive Polymer) It is preferable to use an acrylic adhesive ((meth)acrylic polymer) as the adhesive polymer. Examples of the acrylic adhesive include acrylic adhesives obtained by copolymerizing a (meth)acrylic acid ester monomer such as methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, or isononyl (meth)acrylate as the main component with a monomer containing a functional group such as unsaturated carboxylic acid or anhydride thereof, such as (meth)acrylic acid, crotonic acid, fumaric acid, itaconic acid, or maleic acid (anhydride), a vinyl monomer such as vinyl acetate, acrylonitrile, or styrene, or a (meth)acrylic monomer such as 2-hydroxyethyl (meth)acrylate or 2-methylolethylacrylamide, as needed. In this specification, "(meth)acrylic" means "acrylic" and / or "methacrylic". In the case of a (meth)acrylic polymer, it means an "acrylic polymer" or / and a "methacrylic polymer".

[0027] The flame-retardant pressure-sensitive adhesive composition and the pressure-sensitive adhesive layer may contain, as necessary, one or a combination of two or more of various additives such as a tackifier resin, a colorant, an antioxidant, a weathering agent, a softener, a stabilizer, a filler, an extender, and a reinforcing agent, within a range that does not impair the effects of the present invention.

[0028] (Alkylated melamine curing agent) The curing agent acts as a crosslinking agent for the adhesive polymer, crosslinking the adhesive polymer and improving the performance of the adhesive layer. The flame-retardant adhesive composition and the adhesive layer contain an alkylated melamine curing agent as such a curing agent. Furthermore, by using an alkylated melamine curing agent, corrosion caused by the acidity of the flame retardant can be suppressed by the basicity of the alkylated melamine curing agent. In this case, the alkylated melamine curing agent binds to the adhesive polymer as a crosslinking agent, thereby preventing problems that occur when a free base is added.

[0029] Examples of alkylated melamine curing agents include methylated melamine resin, ethylated melamine resin, propylated melamine resin, butylated melamine resin, hexylated melamine resin, octylated melamine resin, methyl-butyl mixed alkylated melamine resin, etc. Specific examples of alkylated melamine curing agents include the following products: Examples of methylated melamine resins include methylated melamine resins manufactured by Sanwa Chemical Co., Ltd.: Nikalac MW-30 (product name), Nikalac MW-22 (product name), and Nikalac MS-11 (product name). Examples of n-butylated melamine resins include the melamine resin Amidia J-820-60 (product name) manufactured by DIC Corporation, and the amino resins U-VAN 20SB (product name), U-VAN 20SE60 (product name), U-VAN 21R (product name), U-VAN 22R (product name), U-VAN 122 (product name), U-VAN 125 (product name), U-VAN 128 (product name), and U-VAN 228 (product name) manufactured by Mitsui Chemicals, Inc. Examples of iso-butylated melamine resins include the amino resins U-VAN 60R (product name), U-VAN 62 (product name), U-VAN 62E (product name), U-VAN 360 (product name), U-VAN 165 (product name), and U-VAN 166-60 (product name) manufactured by Mitsui Chemicals, Inc. Examples of mixed alkylated melamine resins include mixed etherified melamine resins (alkyl group: methyl / n-butyl) manufactured by Sanwa Chemical Co., Ltd.: Nikalac MX-45 (product name) and Nikalac MX-410 (product name).

[0030] The content of the alkylated melamine curing agent in the flame-retardant adhesive composition and the adhesive layer is preferably 0.03 to 0.5 parts by mass, more preferably 0.05 to 0.4 parts by mass, and even more preferably 0.1 to 0.3 parts by mass, relative to 100 parts by mass of the adhesive polymer. When the content of the alkylated melamine curing agent is 0.03 parts by mass or more, the corrosion prevention effect can be more sufficiently obtained while the effect as a curing agent can be obtained, and when it is 0.5 parts by mass or less, the amount is not excessive for the desired effect, and material costs can be reduced.

[0031] (Other Curing Agents (Combined Curing Agent Components)) The curing agent contained in the flame-retardant adhesive composition and the adhesive layer preferably uses the alkylated melamine curing agent in combination with another curing agent (combined curing agent component). The component (combined curing agent component) used in combination with the alkylated melamine curing agent is not particularly limited as long as it can crosslink the adhesive polymer used, but examples include epoxy-based curing agents, metal chelate-based curing agents, isocyanate-based curing agents, acid anhydride-based curing agents, amine-based curing agents, and aziridine-based curing agents. Epoxy-based curing agents and chelate-based curing agents are preferred, and epoxy-based curing agents are more preferred. The combined use of the alkylated melamine curing agent and another curing agent (combined curing agent component) not only provides corrosion prevention effects but also improves adhesive strength, thereby enhancing the effect of preventing peeling after winding of the flame-retardant adhesive tape.

[0032] Specific examples of the curing agent combination component include the following products. Chelate-based curing agents include an organic titanium compound, Orgatix TC-100 (product name) (titanium acetylacetonate), manufactured by Matsumoto Fine Chemical Co., Ltd., and an aluminum organic compound, Aluminum Chelate A (product name) (aluminum tris(acetylacetonate)), manufactured by Kawaken Fine Chemical Co., Ltd. Epoxy-based curing agents include an epoxy-based curing agent, E-AX (product name), manufactured by Soken Chemical & Engineering Co., Ltd., and a multifunctional epoxy-based curing agent, TETRAD-C (product name), manufactured by Mitsubishi Gas Chemical Company, Inc. Isocyanate-based curing agents include a curing agent, Coronate L-45E (product name), manufactured by Nippon Polyurethane Industry Co., Ltd.

[0033] The content of the curing agent combination component in the flame-retardant adhesive composition and the adhesive layer is preferably 0.002 to 0.5 parts by mass, more preferably 0.005 to 0.4 parts by mass, and even more preferably 0.01 to 0.3 parts by mass, per 100 parts by mass of the adhesive polymer. In particular, when an epoxy-based curing agent is used as the curing agent combination component, the content of this epoxy-based curing agent is preferably 0.002 to 0.3 parts by mass, more preferably 0.005 to 0.1 parts by mass, and even more preferably 0.01 to 0.1 parts by mass, per 100 parts by mass of the adhesive polymer. When the content of the curing agent combination component is 0.002 parts by mass or more, higher adhesive strength can be obtained (peel-off after winding can also be suppressed), and when it is 0.5 parts by mass or less, moderate adhesive strength can be obtained, peel-off after winding can be suppressed, and the amount is not excessive for the desired effect, thereby reducing material costs.

[0034] The total content of the curing agent combination component and the alkylated melamine curing agent is preferably 0.05 parts by mass or more, and more preferably 0.07 parts by mass or more, relative to 100 parts by mass of the adhesive polymer in order to obtain sufficient adhesive strength (and further in order to prevent peeling after winding); and from the viewpoint of preventing an excessive amount for the desired effect and in order to prevent peeling after winding, the total content is preferably 0.7 parts by mass or less, and more preferably 0.5 parts by mass or less, and even more preferably 0.4 parts by mass, relative to 100 parts by mass of the adhesive polymer.

[0035] (Peel Distance After Winding) The flame-retardant adhesive composition preferably exhibits a peel distance of 12 mm or less, more preferably 7 mm or less, and even more preferably 3 mm or less, as measured in the following winding test. FIG. 3 shows an explanatory diagram of the winding test. FIG. 3(a) shows the state in which the test adhesive tape is wound around a round iron nail, and FIGS. 3(b) and 3(c) show the locations where the peel distance was measured. The peel distance refers to the measured value of the length of the peeled adhesive tape portion at the end of the wound test adhesive tape (as shown in FIG. 3(c), the length of the adhesive tape from the point where the adhesive tape starts to peel to the end of the adhesive tape). Note that FIG. 3(c) is a schematic diagram of a round iron nail 31 viewed from the longitudinal direction. In this figure, the peeled portion of the test adhesive tape 32 and the outer portion wrapped around the round iron nail 31 are shown, with the inner portion omitted, and the head (outer edge) of the round iron nail 31 omitted.

[0036] <Wrapping test> A release agent (long-chain alkyl pendant polymer) was applied to one side of a 50 μm thick PET film using a Mayer bar at a rate of approximately 0.15 g / m 2 After coating, the film was dried at 80°C for 1 minute. A flame-retardant adhesive composition was then coated on the other side of the PET film, dried at 100°C for 1 minute, and processed to a width of 10 mm to produce a test adhesive tape 32. The test adhesive tape (10 mm wide) 32 was then attached to a round iron nail 31 having a diameter of 5.20 mm ± 0.10 mm, with both longitudinal end portions of the test adhesive tape aligned. The test adhesive tape was then wrapped two and a half times while applying a load (100 gf (9.8 mN)) to a 100 g weight 33, and the end was cut off to produce a test sample without peeling. The test sample was left to stand for 20 minutes in an environment at a temperature of 23 ± 1°C and a relative humidity of 50 ± 5%, and then heated for 1 hour in a dryer set at 120°C. The length of the peeled portion (peel distance) at the end of the adhesive tape of the obtained test sample was measured with a ruler.

[0037] (Flame-retardant pressure-sensitive adhesive tape) The flame-retardant pressure-sensitive adhesive tape according to the present invention has a pressure-sensitive adhesive layer provided on at least one surface of a substrate. This pressure-sensitive adhesive layer is formed from the flame-retardant pressure-sensitive adhesive composition according to the present invention. The pressure-sensitive adhesive layer may be formed on only one surface of the substrate, or on both surfaces. The pressure-sensitive adhesive layer may be formed in direct contact with the substrate, or an adhesion-enhancing treatment layer may be provided between the substrate and the pressure-sensitive adhesive layer. The thickness of the pressure-sensitive adhesive layer is not particularly limited, but can be set to, for example, 5 μm to 100 μm, preferably 10 μm to 60 μm.

[0038] FIG. 1 shows a schematic cross-sectional view of an example of the layer structure of a flame-retardant pressure-sensitive adhesive tape according to the present invention. FIG. 1 shows a single-sided pressure-sensitive adhesive tape in which a pressure-sensitive adhesive layer 12 is provided on one side of a substrate 11. FIG. 2 shows a double-sided pressure-sensitive adhesive tape in which pressure-sensitive adhesive layers 22, 23 are provided on both sides of a substrate 21. In the single-sided pressure-sensitive adhesive tape, the substrate 11 may have a laminate structure, and the layer on the surface 11B side (the outermost layer) is preferably a resin layer, more preferably a polyester resin layer. Surface 11A of the substrate 11 may be optionally subjected to an adhesion-facilitating treatment, such as a surface treatment such as a corona discharge treatment, or may be provided with an undercoat layer such as an adhesion-facilitating treatment layer. By performing the adhesion-facilitating treatment, the adhesion of the pressure-sensitive adhesive layer 12 to the substrate 11 can be improved. By optionally providing surface 11B of the substrate 11 with a release agent treatment, such as a release layer, when the single-sided pressure-sensitive adhesive tape is wound into a roll, the pressure-sensitive adhesive composition of the pressure-sensitive adhesive layer 12 can be prevented from adhering to surface 11B of the substrate 11, while maintaining ease of unwinding (pulling out). A separator (release liner) described below can be provided on the surface of the pressure-sensitive adhesive layer 12 (the surface opposite to the substrate 11 side).

[0039] In the double-sided pressure-sensitive adhesive tape shown in Fig. 2, both surfaces (21A and 21B) or either one of the surfaces of the substrate 21 may be subjected to an adhesion-facilitating treatment, for example, a surface treatment such as corona discharge treatment, or an undercoat layer such as an adhesion-facilitating treatment layer may be provided. By performing the adhesion-facilitating treatment, it is possible to improve the adhesion between the pressure-sensitive adhesive layer 22 or the pressure-sensitive adhesive layer 23 and the substrate 21. A separator (release liner) as described below may be provided on the surface (the surface opposite the substrate 21 side) of the pressure-sensitive adhesive layer 22 and / or the pressure-sensitive adhesive layer 23.

[0040] (Substrate) The flame-retardant adhesive tape according to the present invention has a substrate as a support for supporting the adhesive layer. The substrate is not particularly limited, but examples include resin film substrates such as polyester, polypropylene, polyethylene, polyphenylene sulfide, polyimide, polyamide, polyphenylene sulfide, polyacetate, and polyether ether ketone; cloth substrates (woven fabric substrates) such as glass cloth, acetate cloth, and polyester cloth; nonwoven fabric substrates such as rayon nonwoven fabric, aromatic polyamide nonwoven fabric, and polyester nonwoven fabric; and paper substrates. The substrates may be used alone or in combination of two or more. The substrate preferably comprises at least one layer made of an electrically insulating material, and may also be a laminate containing a layer made of another material. Examples of the electrically insulating layer include the resin film substrate, the cloth substrate, the nonwoven fabric substrate, and the paper substrate. If necessary, a substrate may be used in which paper, woven fabric, or nonwoven fabric is laminated to the substrate using an adhesive or bonding agent. The surface of the substrate on which the adhesive layer is to be formed may be subjected to the aforementioned adhesion-enhancing treatment. As an adhesion-facilitating treatment, a synthetic resin may be coated. The adhesion-facilitating treatment can increase the adhesion between the substrate and the pressure-sensitive adhesive layer. The thickness of the substrate is not particularly limited, but a substrate having a thickness of, for example, 5 μm or more and 100 μm or less can be used.

[0041] When the pressure-sensitive adhesive layer is formed on only one surface of the substrate, at least the outermost layer on the side of the substrate opposite the pressure-sensitive adhesive layer is preferably made of a resin material, more preferably a polyester such as polyethylene terephthalate (PET). Furthermore, the surface of the substrate or the surface of the outermost layer (the side without the pressure-sensitive adhesive layer) is preferably treated with a release agent. The release agent treatment allows the insulating pressure-sensitive adhesive tape wound into a roll to be easily peeled and used. During production, the flame-retardant pressure-sensitive adhesive tape formed by applying a flame-retardant pressure-sensitive adhesive composition to a substrate is wound into a roll, and then the flame-retardant pressure-sensitive adhesive tape can be peeled (rewound), processed, and rewound again. As the release agent, non-silicone release agents such as acrylic resins, fluorine-based resins, alkyd resins, mixtures of alkyl resins and amino resins, polyvinyl carbamate resins, and long-chain alkyl-modified resins are preferred.

[0042] (Separator) The flame-retardant pressure-sensitive adhesive tape according to the present invention may further have a separator (release liner) on the pressure-sensitive adhesive layer, if necessary. The separator is treated with a release agent, and is peeled off from the pressure-sensitive adhesive layer during use. As the separator, a film, paper, cloth, or the like that can be used as the substrate and that has been treated with a release agent can be used.

[0043] (Method for Producing Flame-Retardant Pressure-Sensitive Adhesive Tape) The method for producing the flame-retardant pressure-sensitive adhesive tape according to the present invention is not particularly limited, and examples include a method of coating a substrate with a flame-retardant pressure-sensitive adhesive composition in which additive components such as an acidic phosphorus-based flame retardant and a curing agent are dispersed in a pressure-sensitive adhesive polymer. A solvent may be added to adjust the viscosity of the pressure-sensitive adhesive composition during coating. Specific examples of solvents include aromatic solvents such as toluene and xylene; aliphatic solvents such as hexane, octane, and isoparaffin; ketone solvents such as methyl ethyl ketone and methyl isobutyl ketone; ester solvents such as ethyl acetate and isobutyl acetate; and ether solvents such as diisopropyl ether and 1,4-dioxane. Methods for dispersing additive components such as an acidic phosphorus-based flame retardant and a curing agent into a pressure-sensitive adhesive base polymer include mechanical kneading dispersion and solvent dispersion. Examples of equipment that can be used for this dispersion include a mixer / kneader, a ball mill, a planetary mixer, a paint conditioner, and a three-roll mill. Two or more of these devices may be used in combination. The flame-retardant pressure-sensitive adhesive composition can be applied to a substrate by, for example, a method using a roll coater or a reverse coater. By using the above-mentioned coating method, the flame-retardant pressure-sensitive adhesive composition can be applied to at least one surface of the substrate in one or more layers, and the applied layer can be heated as needed to obtain the flame-retardant pressure-sensitive adhesive tape according to the present invention.

[0044] (Characteristics and Uses of Flame-Retardant Pressure-Sensitive Adhesive Tape) The flame-retardant pressure-sensitive adhesive tape according to the present invention preferably has an electrolytic corrosion coefficient of 0.98 or more, measured in accordance with JIS C 2107:2011 (7.8.2 Method B). When the electrolytic corrosion coefficient is 0.98 or more, deterioration of electrical properties is less likely to occur.

[0045] The flame-retardant adhesive tape according to the present invention preferably has an adhesive strength (N / 10 mm) of 3.0 or more, more preferably 3.5 or more, and even more preferably 4.0 or more, as measured by the following method. <Method for measuring adhesive strength> The adhesive strength is measured in accordance with JIS Z0237:2000. However, the width of the test piece is 10 mm, and the test plate is a SUS304 steel plate polished with 280-grit waterproof abrasive paper, and the surface roughness is measured as the centerline average roughness R a: 0.05 μm < R a <0.40 μm, maximum height R max :R max The thickness is set to <3 μm, the pressing is performed at a speed of about 5 mm / s with one reciprocating motion, and the peeling is performed at a peeling angle of 180°.

[0046] Furthermore, the flame-retardant pressure-sensitive adhesive tape according to the present invention preferably has a pressure-sensitive adhesive layer made of a flame-retardant pressure-sensitive adhesive composition that results in a peel distance of 12 mm or less, more preferably 7 mm or less, and even more preferably 3 mm or less, as measured in the aforementioned winding test. A flame-retardant pressure-sensitive adhesive tape having a pressure-sensitive adhesive layer made of a flame-retardant pressure-sensitive adhesive composition that results in a peel distance of 7 mm or less is unlikely to peel off even when wrapped around a thin linear adherend such as an electric wire.

[0047] The flame-retardant pressure-sensitive adhesive tape according to the present invention preferably passes the UL510 (electrical insulating tape standard) combustion test. Passing the UL510 combustion test allows the tape to have high flame retardancy, which is preferable in practical use.

[0048] The flame-retardant pressure-sensitive adhesive tape according to the present invention preferably has a comparative tracking index (CTI value) measured in accordance with JIS C 2134 (IEC 112) of 600 V or more. When the comparative tracking index is 600 V or more, the tape can have high insulating properties, which is preferable in practical use.

[0049] The flame-retardant adhesive tape according to the present invention can be used in various fields such as electrical and electronic equipment, office automation equipment, home appliances, aircraft, ships, and vehicles. According to an embodiment of the present invention, a flame-retardant adhesive tape can be provided which suppresses fire even when high temperatures or heat accumulation occurs inside various devices, has the function of quickly extinguishing a fire even if it does break out, and changes little over time, and has sufficient adhesive strength to withstand heat.

[0050] When various equipment parts using the flame-retardant adhesive tape according to the present invention are recycled after their useful life has ended, even if they are incinerated as waste, the thermal decomposition of the flame-retardant adhesive tape does not generate halogen-containing gases containing chlorine, bromine, etc., which are undesirable for the environment and human body.

[0051] The flame-retardant pressure-sensitive adhesive tape according to the present invention has high flame retardancy, insulating properties, and excellent adhesive properties, and also has the effect of suppressing deterioration of electrical properties, and is therefore suitable for use in insulating electrical and electronic components such as electric wires and transformers, electrical and electronic devices in automobiles, and portable electronic devices such as audiovisual devices, game consoles, and information devices.

[0052] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples and comparative examples, "parts" means "parts by mass" and "%" means "% by mass".

[0053] (pH of Flame Retardant) The pH of the flame retardants used in the following Examples and Comparative Examples was measured by the following method. <Method for Measuring pH of Flame Retardant> 1 g of flame retardant was added to 50 g of ion-exchanged water at room temperature (23±2°C), and the mixture was stirred for 1 minute using a glass rod. After 10 minutes had passed, the pH of the resulting mixture was measured using a glass electrode pH meter (product name: Portable pH / Ion / ORP Meter HM-40P (pH Combined Electrode Set), manufactured by DKK-TOA Corporation).

[0054] (Adhesive Strength) The adhesive strength of the flame-retardant adhesive compositions obtained in the following Examples and Comparative Examples was measured by the following method. <Method for Measuring Adhesive Strength> The adhesive strength was measured in accordance with JIS Z0237:2000. However, the width of the test piece was 10 mm, and the test plate was a SUS304 steel plate polished with 280-grit waterproof abrasive paper, and the surface roughness was measured as the centerline average roughness R a : 0.05 μm < R a <0.40 μm, maximum height R max :R max The pressure bonding was performed at a speed of about 5 mm / s with one reciprocating motion, and the peeling was performed at a peeling angle of 180°.

[0055] (Peel Distance) The adhesive strength (peel distance) of the flame-retardant pressure-sensitive adhesive compositions obtained in the following Examples and Comparative Examples when wound as pressure-sensitive adhesive tapes was measured by the following method. FIG. 3 shows an explanatory diagram of the winding test. FIG. 3(a) shows the state in which the test pressure-sensitive adhesive tape was wound around a round iron nail, and FIGS. 3(b) and 3(c) show the measurement points for the peel distance. As mentioned above, the peel distance means the measured value of the length of the peeled adhesive tape portion at the end of the wound test pressure-sensitive adhesive tape (the length of the adhesive tape from the point where peeling of the adhesive tape begins to the end of the adhesive tape, as shown in FIG. 3(c)). <Wrapping Test> A release agent (manufactured by Lion Specialty Chemicals Co., Ltd., trade name: Piroil 1010) was applied to one side of a 50 μm-thick PET film (manufactured by Toray Industries, Inc., trade name: Lumirror, product number type: #50-S10) at a rate of 0.15 g / m using a Meyer bar. 2 After coating, the PET film was dried at 80°C for 1 minute, and then the other side of the PET film was coated with the flame-retardant adhesive composition of each Example and Comparative Example, dried at 100°C for 1 minute, and processed to a width of 10 mm to prepare a test adhesive tape 32. Next, the test adhesive tape (10 mm wide) was wrapped around a round iron nail 31 (manufactured by Amatei Co., Ltd., product name: N150, JIS A 5508 compliant) with a diameter of 5.20 mm ± 0.10 mm and a length of 150 mm, from which any foreign matter had been wiped off, with both longitudinal ends of the test adhesive tape aligned, and the test adhesive tape was wrapped two and a half times while applying a load (100 gf (9.8 mN)) to the test adhesive tape with a 100 g weight 33, and the end was cut off to prepare a test sample without peeling. Next, the test sample was left to stand for 20 minutes in an environment at a temperature of 23±1°C and a relative humidity of 50±5%, and then the test sample was heated in a dryer (manufactured by Espec Corporation, incubator (forced hot air circulation and ventilation type), model: PH-101, air speed 2) set to 120°C, and after 1 hour, it was taken out. The length of the peeled part (peeling distance) at the adhesive tape end of the taken-out test sample was measured with a ruler.

[0056] (Electrolytic corrosion coefficient) The electrolytic corrosion coefficient of the flame-retardant pressure-sensitive adhesive tapes obtained in the following examples and comparative examples was measured in accordance with JIS C 2107:2011 (7.8.2 Method B).

[0057] (Flame Retardancy) The flame retardancy of the flame retardant pressure-sensitive adhesive tapes obtained in the following Examples and Comparative Examples was evaluated by a UL510 (electrical insulating tape standard) combustion test.

[0058] (Preparation of Pressure-Sensitive Adhesive) 75 parts of butyl acrylate, 20 parts of 2-ethylhexyl acrylate, 4.5 parts of acrylic acid, 0.5 parts of 2-hydroxyethyl acrylate, and 1 part of benzoyl peroxide as a polymerization initiator were dissolved in ethyl acetate, and the mixture was reacted at 67°C for 5 hours under a nitrogen atmosphere, and the solid content was diluted to 40% to prepare a solution of an acrylic acid ester copolymer having a weight-average molecular weight of approximately 600,000 (hereinafter referred to as an acrylic pressure-sensitive adhesive). The weight-average molecular weight was measured by GPC (Gel Permeation Chromatography) (molecular weight standard: polystyrene).

[0059] Examples 1 to 9 An acidic phosphorus-based flame retardant was added to 100 parts of the solid content of the acrylic pressure-sensitive adhesive prepared above in the blending ratio shown in Table 1, and the mixture was thoroughly dispersed using a mixer / kneader (manufactured by Primix Corporation, product name: Hivis Dispermix 3D-5). Subsequently, an alkylated melamine curing agent, other curing agents (combined components of the curing agent), and an appropriate amount of organic solvent were added in the blending ratios shown in Table 1, and the mixture was thoroughly stirred until uniform, thereby obtaining a flame-retardant pressure-sensitive adhesive composition for application. The resulting flame-retardant pressure-sensitive adhesive composition was then applied to the adhesion-facilitated surface of a PET film (thickness: 25 μm) that had been treated with an adhesion-facilitating agent on one side and a release agent on the other side, so that the thickness of the pressure-sensitive adhesive layer after drying would be 25 μm to 35 μm, and the composition was dried to obtain a flame-retardant pressure-sensitive adhesive tape.

[0060] Comparative Example 1 A flame-retardant pressure-sensitive adhesive composition and a flame-retardant pressure-sensitive adhesive tape were obtained in the same manner as in Example 1, except that no alkylmelamine curing agent was added.

[0061] (Comparative Example 2) A flame-retardant pressure-sensitive adhesive composition and a flame-retardant pressure-sensitive adhesive tape were obtained in the same manner as in Example 7, except that no alkylmelamine curing agent was added, the curing agent was an isocyanate-based curing agent alone, and the blending ratios of each component were as shown in Table 1.

[0062] (Comparative Example 3) A flame-retardant pressure-sensitive adhesive composition and a flame-retardant pressure-sensitive adhesive tape were obtained in the same manner as in Example 7, except that no alkylmelamine curing agent was added, but benzotriazole was added, and the blending ratios of each component were as shown in Table 1.

[0063] The flame-retardant pressure-sensitive adhesive compositions and flame-retardant pressure-sensitive adhesive tapes obtained in Examples 1 to 9 and Comparative Examples 1 to 3 were evaluated by the methods described above. The results are shown in Table 1. The numerical values ​​(parts by mass) of each component, such as the curing agent, in Table 1 indicate the blended amount (parts by mass) of the active ingredient.

[0064] The symbols in the table indicating the judgment results of the overall evaluation have the following meanings: ⊚: The electrolytic corrosion coefficient is high (0.98 or more), and the adhesive strength is high, and peeling after winding is small (7 mm or less); ◯: The electrolytic corrosion coefficient is high (0.98 or more), and peeling after winding is somewhat large (more than 7 mm but 12 mm or less), but the adhesive strength is sufficiently high; ×: The electrolytic corrosion coefficient is low (less than 0.98).

[0065] The components in Table 1 are described as follows: Adhesive polymer: acrylic ester copolymer formed in the preparation of the adhesive Acidic phosphorus-based flame retardant A: metal alkylphosphinate (product name: OMP-800, manufactured by Universal Chemtech Co., Ltd.) Acidic phosphorus-based flame retardant B: metal phosphinate (product name: PNF100R, manufactured by Universal Chemtech Co., Ltd.) Acidic phosphorus-based flame retardant C: melamine polyphosphate (product name: MPP-A, manufactured by Sanwa Chemical Co., Ltd.) Butylated melamine curing agent: Amidia J-820-60 (product name), 60%, manufactured by DIC Corporation Methylated melamine curing agent: Nikalac MW-30 (product name), 100%, manufactured by Sanwa Chemical Co., Ltd. Chelate-based curing agent: Orgatix TC-100 (product name), 75%, manufactured by Matsumoto Fine Chemical Co., Ltd. Epoxy-based curing agent: E-AX (product name), 5%, manufactured by Soken Chemical & Engineering Co., Ltd. Isocyanate-based curing agent: Coronate L-45E (product name), 45%, manufactured by Nippon Polyurethane Industry Co., Ltd. PET: polyethylene terephthalate PEN: polyethylene naphthalate PI: polyimide

[0066]

[0067] As shown in Table 1, a comparison between Example 1 and Comparative Example 1, and a comparison between Example 7 and Comparative Examples 2 and 3, reveals that the pressure-sensitive adhesive tape containing an alkylated melamine curing agent in the pressure-sensitive adhesive layer has a higher electrolytic corrosion coefficient than the pressure-sensitive adhesive tape not containing an alkylated melamine curing agent in the pressure-sensitive adhesive layer. Furthermore, as shown by the evaluation results of Comparative Example 3, the pressure-sensitive adhesive tape containing benzotriazole in the pressure-sensitive adhesive layer exhibits a significantly lower electrolytic corrosion coefficient. These findings demonstrate that the pressure-sensitive adhesive tapes of the examples of the present invention are excellent as electrical insulating tapes.

[0068] Furthermore, the flame-retardant adhesive compositions of Examples 1 to 8, particularly Examples 1 to 4 and 6 to 8, exhibited a short peel distance after winding. This demonstrates that adhesive tapes having an adhesive layer made of the adhesive composition of the present invention are resistant to peeling even when wound around a narrow adherend with a diameter of approximately 5 mm. On the other hand, the flame-retardant adhesive compositions of Example 9 and Comparative Example 2, which contain a high content of curing agent (particularly curing agents other than alkylated melamine curing agents) in the adhesive layer, exhibited a long peel distance after winding. Conversely, as shown by the evaluation results of Example 5, the peel distance after winding was long even when the content of curing agent (particularly curing agents other than alkylated melamine curing agents) in the adhesive layer was low.

[0069] REFERENCE SIGNS LIST 11 Substrate 12 Adhesive layer 21 Substrate 22 Adhesive layer 23 Adhesive layer 31 Iron round nail 32 Test adhesive tape (10 mm width) 33 Weight

Claims

1. A flame-retardant adhesive composition comprising an adhesive polymer, a curing agent, and a flame retardant, wherein the curing agent comprises an alkylated melamine curing agent, and the flame retardant comprises an acidic phosphorus-based flame retardant.

2. The flame-retardant adhesive composition according to claim 1, wherein the acidic phosphorus-based flame retardant is a flame retardant having a pH of 2 or more and 6 or less, as measured by the following pH measurement method: (pH measurement method) 1 g of the flame retardant is mixed with 50 g of ion-exchanged water at room temperature (23±2°C) and stirred for 1 minute. After 10 minutes have passed, the pH of the resulting mixture is measured with a glass electrode pH meter.

3. The flame-retardant adhesive composition according to claim 1, wherein the acidic phosphorus-based flame retardant is a phosphinic acid-based flame retardant and / or a polyphosphoric acid-based flame retardant.

4. The flame-retardant adhesive composition according to claim 1, wherein the acidic phosphorus-based flame retardant is at least one selected from the group consisting of phosphinates, alkyl phosphinates, and melamine polyphosphates.

5. The flame-retardant pressure-sensitive adhesive composition according to claim 1, wherein the flame retardant is a flame retardant that is not liquid at 23°C.

6. The flame-retardant adhesive composition according to claim 1, wherein the content of the acidic phosphorus-based flame retardant is 20 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the adhesive polymer, and the content of the alkylated melamine curing agent is 0.03 parts by mass or more and 0.5 parts by mass or less per 100 parts by mass of the adhesive polymer.

7. The flame-retardant pressure-sensitive adhesive composition according to claim 1, further comprising a curing agent other than an alkylated melamine curing agent.

8. The flame-retardant adhesive composition according to claim 7, comprising at least one curing agent selected from the group consisting of epoxy-based curing agents, metal chelate-based curing agents, isocyanate-based curing agents, acid anhydride-based curing agents, amine-based curing agents, and aziridine-based curing agents, as the curing agent other than the alkylated melamine curing agent.

9. The flame-retardant pressure-sensitive adhesive composition according to claim 7, further comprising an epoxy-based curing agent as a curing agent other than the alkylated melamine curing agent.

10. The flame-retardant adhesive composition according to claim 7, wherein the content of the curing agent other than the alkylated melamine curing agent is 0.002 parts by mass or more and 0.5 parts by mass or less per 100 parts by mass of the adhesive polymer.

11. The flame-retardant adhesive composition according to claim 1, wherein the adhesive polymer is a (meth)acrylic polymer.

12. The flame-retardant pressure-sensitive adhesive composition according to claim 1, which has a peel distance of 7 mm or less as measured in the following wrapping test. (Wrapping test) A release agent (long-chain alkyl pendant polymer) was applied to one side of a 50 μm-thick PET film at a rate of 0.15 g / m2 using a Mayer bar. 2 After coating, the film is dried at 80°C for 1 minute, and then a flame-retardant adhesive composition is coated on the other side of the PET film, followed by drying at 100°C for 1 minute and processing to a width of 10 mm to prepare a test adhesive tape. The test adhesive tape (10 mm wide) is wrapped around a round iron nail having a diameter of 5.20 mm ± 0.10 mm, with both longitudinal ends of the test adhesive tape aligned, and the test adhesive tape is wrapped around the nail by two and a half turns while applying a load of 100 gf (9.8 mN), and the end is cut off to prepare a test sample without peeling. The test sample is left for 20 minutes in an environment of a temperature of 23 ± 1°C and a relative humidity of 50 ± 5%, and then heated in a dryer set at 120°C for 1 hour, and the length of the peeled part (peeling distance) of the adhesive tape end of the obtained test sample is measured with a ruler.

13. A flame-retardant adhesive tape having a substrate and an adhesive layer provided on at least one surface of the substrate, the adhesive layer being made of a flame-retardant adhesive composition according to any one of claims 1 to 12.

14. The flame-retardant adhesive tape according to claim 13, wherein the substrate comprises at least one layer made of an electrically insulating material.

15. The flame-retardant adhesive tape according to claim 13, having the adhesive layer on one surface of the substrate, and at least the outermost layer on the side of the substrate opposite to the adhesive layer is made of a resin material.

16. The flame-retardant adhesive tape according to claim 15, wherein the resin material is polyester.

17. The flame-retardant adhesive tape according to claim 13, which passes the UL510 (electrical insulating tape standard) flame test.

18. The flame-retardant adhesive tape according to claim 13, having an electrolytic corrosion coefficient of 0.98 or more as measured in accordance with JIS C 2107:2011 (7.8.2 Method B).

19. The flame-retardant adhesive tape according to claim 13, which is for electrical insulation.

Citation Information

Patent Citations

  • Cable combined type fireproof blocking module for nuclear power, and preparation method thereof

    CN103337263A

  • UV (Ultraviolet) photocuring adhesive and double-sided adhesive tape prepared by using same

    CN111004602A

  • Laminate for flame retardant label

    JP1995101021A

  • Heat-resisting adhesive tape

    JP2010076261A

  • Flame-retardant adhesive composition for flexible printed circuit board and flexible printed circuit board using the same

    JP2010184952A

Cited By

  • Preparation method of high-temperature-resistant flame-retardant BOPP insulating tape

    CN121518055A