Thermosetting resin composition, resin sheet, heat dissipation plate, method for manufacturing resin sheet, and method for manufacturing heat dissipation plate
The thermosetting resin composition with specific components addresses the poor heat cycle characteristics of metal-based substrates by enhancing thermal conductivity and stress relief, ensuring reliable electronic component performance.
Patent Information
- Application Number
- PCT/JP2024/010424
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-17
AI Technical Summary
Metal-based substrates used in electronic devices suffer from poor heat cycle characteristics due to stress generated by thermal expansion and contraction, leading to potential solder cracking and low thermal conductivity in insulating adhesive layers.
A thermosetting resin composition comprising epoxy resin, an ethylene acrylic copolymer, and spherical fillers with specific thermal conductivity and particle size ratios, along with an ion scavenger, is used to create a resin sheet and heat sink with improved thermal conductivity and stress relief, enhancing heat cycle characteristics.
The solution achieves excellent thermal conductivity and heat cycle characteristics, reducing stress and maintaining insulation, thereby preventing solder cracking and improving the reliability of electronic components.
Smart Images

Figure JP2024010424_17102024_PF_FP_ABST
Abstract
Description
Thermosetting resin composition, resin sheet, heat sink, method for manufacturing resin sheet, and method for manufacturing heat sink
[0001] The present invention relates to a thermosetting resin composition, a resin sheet, a heat sink, a method for producing a resin sheet, and a method for producing a heat sink.
[0002] When a device equipped with many electronic components such as IC chips and transistors is operated, the electronic components generate a large amount of heat. If this generated heat cannot be efficiently dissipated, the function of the electronic components will be impaired due to the heat, causing the device to malfunction. To prevent this malfunction, the substrate on which the electronic components are mounted is provided with a metal plate with high thermal conductivity, sandwiched between an insulating and thermally conductive resin sheet, on the side opposite the side on which the electronic components are mounted. This metal plate allows the heat generated by the electronic components to be efficiently dissipated through the resin sheet.
[0003] For example, Patent Document 1 discloses a metal base substrate comprising a metal plate, an insulating adhesive layer laminated thereon, and a copper foil laminated on the insulating adhesive layer. Patent Document 1 also discloses an adhesive composition that can be used as the insulating adhesive layer, the adhesive composition comprising an epoxy resin, a curing agent, a high-molecular-weight resin that is compatible with the epoxy resin and has a weight-average molecular weight of 30,000 or more, a high-molecular-weight resin that has a glass transition temperature of 0°C or less, has a reactive functional group, and has a weight-average molecular weight of 100,000 or more, a curing accelerator, and an inorganic filler with a small particle size.
[0004] Japanese Patent Application Publication No. 10-242606
[0005] Such metal base substrates may have poor heat cycle characteristics. Specifically, when a heat cycle test is performed on a metal base substrate with electronic components mounted on a circuit formed by etching copper foil, the metal plate constituting the metal base substrate repeatedly expands and contracts due to temperature changes. This repeated expansion and contraction generates stress within the insulating adhesive layer laminated on the metal plate. However, because the insulating adhesive layer cannot relieve this stress, the circuit moves in accordance with the expansion and contraction of the metal plate. The movement of the circuit concentrates stress on the solder connecting the electronic components and the circuit, making it prone to cracking in the solder. For this reason, the heat cycle characteristics of the above-mentioned metal base substrate may be poor. Furthermore, because the particle size of the inorganic filler contained in the insulating adhesive layer is small, resin is likely to be interposed between the fillers, resulting in low thermal conductivity of the insulating adhesive layer.
[0006] The present invention has been made in consideration of the above circumstances, and aims to provide a heat sink plate having excellent heat cycle characteristics, a resin sheet having excellent thermal conductivity, a thermosetting resin composition constituting the resin layer and resin sheet of the heat sink plate, a method for manufacturing a resin sheet, and a method for manufacturing a heat sink plate.
[0007] The present invention is as follows. [1] A thermosetting resin composition according to the present invention comprises: an epoxy resin; a curing agent for curing the epoxy resin; an ethylene-acrylic copolymer having a glass transition temperature of -30°C or lower and having a carboxy group in a side chain; first spherical fillers having a thermal conductivity of 20 W / m K or higher and an average particle size (D50) of 30 μm or higher and 60 μm or lower; and second spherical fillers having a thermal conductivity of 20 W / m K or higher and an average particle size (D50) of 1 μm or higher and 10 μm or lower, wherein the total weight ratio of the first spherical fillers and the second spherical fillers is 84 wt% or higher and 90 wt% or lower with respect to 100 wt% of the total solid content; the ratio of the first spherical fillers to the second spherical fillers is 55:45 to 85:15; and the content of the ethylene-acrylic copolymer is 700 parts by weight or higher and 1000 parts by weight or lower with respect to 100 parts by weight of the epoxy resin.
[0008] [2] The first spherical filler may be composed of at least one selected from the group consisting of alumina, boron nitride, aluminum nitride, magnesium oxide, zinc oxide, and silicon nitride.
[0009] [3] The second spherical filler may be composed of at least one selected from the group consisting of alumina, boron nitride, aluminum nitride, magnesium oxide, zinc oxide, and silicon nitride.
[0010] [4] The thermosetting resin composition may contain an ion scavenger that captures ions, and the content of the ion scavenger may be 40 parts by weight or more and 60 parts by weight or less relative to 100 parts by weight of the epoxy resin.
[0011] [5] The thermosetting resin composition may have a thermal conductivity of 2 W / m K or more after curing, a storage modulus of 7000 MPa or less at −30° C. after curing, a storage modulus of 10 MPa or more and 100 MPa or less at 25° C. after curing, and a storage modulus of 1 MPa or more and 100 MPa or less at 125° C. after curing.
[0012] [6] A resin sheet according to the present invention is composed of the thermosetting resin composition according to any one of [1] to [5].
[0013] [7] The resin sheet may be in a semi-cured state.
[0014] [8] A heat sink according to the present invention comprises a metal plate and a resin layer made of the thermosetting resin composition according to any one of [1] to [5], wherein the resin layer is formed on at least one surface of the metal plate.
[0015] [9] The cured state of the resin layer may be semi-cured.
[0016]
[10] A method for producing a resin sheet according to the present invention includes: a preparation step of preparing the thermosetting resin composition according to any one of [1] to [5]; a formation step of forming a resin layer composed of the thermosetting resin composition into a film; and a heating step of heating the film on which the resin layer has been formed.
[0017]
[11] A method for manufacturing a heat sink according to the present invention includes a lamination step of laminating a resin layer of the resin sheet obtained by the method for manufacturing a resin sheet according to
[10] onto a metal plate, and a heating and pressurizing step of heating and pressurizing the metal plate on which the resin layer is laminated.
[0018]
[12] A method for manufacturing a heat sink according to the present invention includes: a preparation step of preparing the thermosetting resin composition according to any one of [1] to [5]; a formation step of forming a resin layer composed of the thermosetting resin composition on a metal plate; and a heating step of heating the metal plate on which the resin layer has been formed.
[0019] According to the present invention, it is possible to provide a heat sink plate having excellent heat cycle characteristics, a resin sheet having excellent thermal conductivity, a thermosetting resin composition constituting the resin layer and resin sheet of the heat sink plate, a method for manufacturing a resin sheet, and a method for manufacturing a heat sink plate.
[0020] 1A and 1B are schematic cross-sectional views of a resin sheet according to an embodiment, a heat sink according to an embodiment, and a substrate on which electronic components are mounted and which includes a heat sink according to an embodiment.
[0021] Hereinafter, a thermosetting resin composition, a resin sheet, a heat sink, a method for manufacturing a resin sheet, and a method for manufacturing a heat sink, which are modes for carrying out the present invention (hereinafter referred to as embodiments), will be described in detail. The following embodiments are examples for explaining the present invention and are not intended to limit the present invention to the following content. The present invention can be practiced by appropriately modifying it within the scope of its gist. The parts by weight used in the embodiments refer to, for example, the weight of the resin alone excluding volatile components such as organic solvents contained in the resin, or the weight of the non-volatile components. The semi-cured state (B stage) refers to a state in which the curing reaction of the thermosetting resin composition has progressed halfway.
[0022] [Thermosetting Resin Composition] The thermosetting resin composition of the embodiment includes an epoxy resin, a curing agent, an ethylene-acrylic copolymer having a carboxy group in a side chain, a first spherical filler, and a second spherical filler. The thermosetting resin composition of the embodiment is also suitable for use as a resin composition constituting a resin sheet and a resin composition for a resin layer constituting a heat sink.
[0023] Components contained in the thermosetting resin composition of the embodiment will be described below.
[0024] (Epoxy Resin) The epoxy resin may be any resin capable of reacting with a curing agent to cure the thermosetting resin composition, and may, for example, have two or more epoxy groups in one molecule and an epoxy equivalent of 100 g / eq or more and 400 g / eq or less.
[0025] Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, novolac type epoxy resins, amine type epoxy resins, biphenyl type epoxy resins, alicyclic epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, naphthalene ring-containing epoxy resins, dicyclopentadiene type epoxy resins, etc. Among the above epoxy resins, novolac type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, and bisphenol A type epoxy resins are preferred from the viewpoint of improving the breakdown voltage characteristics.
[0026] The epoxy resin may be used alone or in combination of two or more kinds. The epoxy resin may be dissolved in an organic solvent in advance to facilitate mixing with other materials contained in the thermosetting resin composition.
[0027] (Curing Agent) The curing agent may be any agent capable of curing the epoxy resin, and examples thereof include diaminodiphenylmethane (DDM), diaminodiphenylsulfone (DDS), diaminodiphenylether (DDE), hexamethylenediamine, dicyandiamide, phenol novolac phenolic resin, and phenol novolac cyanate ester resin. From the viewpoint of ease of control of the curing reaction, dicyandiamide and diaminodiphenylsulfone are preferred as the curing agent. The curing agent may be used alone, or two or more types of curing agents may be used in combination.
[0028] The content of the curing agent may be any content that can cure the thermosetting resin composition, and is, for example, preferably 1 part by weight to 40 parts by weight, more preferably 5 parts by weight to 40 parts by weight, per 100 parts by weight of the epoxy resin. This can improve the breakdown voltage characteristics and heat resistance of the cured thermosetting resin composition. Furthermore, it can improve the heat cycle characteristics of resin sheets and heat sinks made from this resin composition.
[0029] The equivalent of the curing agent may be any amount sufficient to cure the thermosetting resin composition, and is preferably 0.1 to 0.8 equivalents relative to 1 equivalent of the epoxy group contained in the epoxy resin, more preferably 0.1 to 0.6 equivalents, and even more preferably 0.2 to 0.4 equivalents. This allows the thermosetting resin composition to have improved breakdown voltage characteristics and heat resistance after curing. Furthermore, the heat cycle characteristics of a heat sink using this resin composition can be improved.
[0030] (Ethylene-acrylic copolymer having a carboxy group in the side chain) Examples of the ethylene-acrylic copolymer having a carboxy group in the side chain include a (meth)acrylic acid ester copolymer having an ethylene structure in the main chain and a carboxy group in the side chain. From the viewpoint of alleviating stress generated during heat cycling, the glass transition temperature of the ethylene-acrylic copolymer having a carboxy group in the side chain is −30° C. or lower, preferably −35° C. or lower, and more preferably −40° C. or lower. Here, the (meth)acrylic acid ester copolymer refers to an acrylic acid ester copolymer or a methacrylic acid ester copolymer. The glass transition temperature can be measured by differential scanning calorimetry (DSC).
[0031] The (meth)acrylic acid ester copolymer having a carboxy group in the side chain is composed of, for example, two or more monomers. Examples of the monomers constituting this copolymer include a (meth)acrylic acid ester monomer, a carboxy group-containing monomer, and an anhydride of a carboxy group-containing monomer. Here, the (meth)acrylic acid ester monomer means an acrylic acid ester monomer or a methacrylic acid ester monomer.
[0032] An ethylene acrylic copolymer having a carboxy group in its side chain can have an ethylene structure introduced into the main chain of the copolymer by polymerizing the above-mentioned monomers. Examples of the introduction method include Ziegler-Natta catalyst polymerization, metallocene catalyst polymerization, Versipol catalyst polymerization, and free radical polymerization.
[0033] Examples of (meth)acrylic acid ester monomers include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; (meth)acrylic acid hydroxyalkyl esters such as hydroxyethyl (meth)acrylate; N,N-dimethylaminoalkyl (meth)acrylates such as N,N-dimethylaminomethyl (meth)acrylate; and epoxy group-containing (meth)acrylic acid esters such as glycidyl (meth)acrylate. Note that methyl (meth)acrylate means methyl acrylate or methyl methacrylate. Furthermore, (meth)acrylic acid means acrylic acid or methacrylic acid. The same applies hereinafter.
[0034] Examples of the carboxy group-containing monomer include (meth)acrylic acid, fumaric acid, and maleic acid.
[0035] Examples of the anhydrides of carboxyl group-containing monomers include anhydrides of (meth)acrylic acid, maleic acid, and the like.
[0036] From the viewpoint of preventing stress from being generated in the resin layer of the heat sink, the weight-average molecular weight of the ethylene-acrylic copolymer having a carboxy group in the side chain is, for example, from 100,000 to 400,000, and preferably from 150,000 to 300,000. Here, the weight-average molecular weight can be measured by gel permeation chromatography (GPC) using standard polystyrene having an average molecular weight of from about 500 to about 1,000,000.
[0037] The content of the ethylene-acrylic copolymer having a carboxy group in the side chain is 700 parts by weight or more and 1,000 parts by weight or less, and preferably 700 parts by weight or more and 900 parts by weight or less, relative to 100 parts by weight of the epoxy resin, from the viewpoint of preventing stress from occurring in the resin layer of the heat sink and from the viewpoint of thermal conductivity.
[0038] From the viewpoint of preventing stress from being generated in the resin layer of the heat sink, the content of the carboxyl group is, for example, preferably 3 mgKOH / g or more and 30 mgKOH / g or less, and more preferably 10 mgKOH / g or more and 30 mgKOH / g or less. The content of the carboxyl group can be measured by titration using a 0.1 N aqueous potassium hydroxide solution.
[0039] An example of a commercially available ethylene acrylic copolymer having a carboxy group in the side chain is VMX4017 manufactured by DuPont.
[0040] (First spherical filler) The average particle diameter (D50) of the first spherical filler is 30 μm or more and 60 μm or less. By having an average particle diameter (D50) of 30 μm or more and 60 μm or less, the first spherical filler is less likely to protrude from the surface of the resin layer. This improves the smoothness of the surface of the resin layer. Furthermore, by having the above particle size, a network between the first spherical filler particles is easily formed, improving the thermal conductivity of the resin layer.
[0041] The thermal conductivity of the first spherical filler is 20 W / m·K or more from the viewpoint of improving the thermal conductivity of the resin layer of the heat sink. The first spherical filler may be any filler having excellent insulating properties and thermal conductivity, and is composed of at least one material selected from the group consisting of alumina, boron nitride, aluminum nitride, magnesium oxide, zinc oxide, and silicon nitride, with alumina being more preferred. Here, the average particle size (D50) refers to the particle size when the particles are counted from the smallest particle size in a volume-based particle size distribution and their cumulative size reaches 50% of the total volume. The particle size can be measured by dynamic light scattering.
[0042] (Second spherical filler) The average particle diameter (D50) of the second spherical filler is 1 μm or more and 10 μm or less, more preferably 1 μm or more and 5 μm or less. The second spherical filler having such an average particle diameter (D50) is filled so as to fill the gap between one first spherical filler and another first spherical filler. This contributes to improving the thermal conductivity of the resin layer described below. The thermal conductivity of the second spherical filler is 20 W / m·K or more from the viewpoint of improving the thermal conductivity of the resin layer composed of the thermosetting resin composition. The second spherical filler may be any filler having excellent insulating properties and thermal conductivity, and is composed of at least one selected from the group consisting of alumina, boron nitride, aluminum nitride, magnesium oxide, zinc oxide, and silicon nitride, with alumina being more preferred.
[0043] The total weight ratio of the first spherical filler and the second spherical filler is 84% by weight or more and 90% by weight or less, preferably 85% by weight or more and 90% by weight or less, and more preferably 85% by weight or more and 89% by weight or less, based on 100% by weight of the total solid content contained in the thermosetting resin composition, from the viewpoint of improving thermal conductivity, heat cycle characteristics, and breakdown voltage characteristics. Furthermore, the ratio of the first spherical filler to the second spherical filler is 55:45 to 85:15, preferably 55:45 to 65:35, from the viewpoint of preventing stress from occurring in the resin layer of the heat sink.
[0044] A resin layer composed of a thermosetting resin composition containing the above-mentioned materials and having the above-mentioned proportions and other configurations has the following effects. A resin layer formed from a thermosetting resin composition in which the above-mentioned materials are uniformly mixed is composed by filling a second spherical filler so as to fill the gaps between one first spherical filler and another first spherical filler. By filling the spherical fillers without gaps, a dense network of spherical fillers is formed within the resin layer. As a result, a resin layer composed of the thermosetting resin composition of this embodiment has excellent thermal conductivity.
[0045] Furthermore, the thermosetting resin composition of this embodiment can reduce stress generation because it contains an ethylene-acrylic copolymer having a glass transition temperature of −30° C. or lower and the spherical filler described above. That is, a heat sink having a resin layer made of such a thermosetting resin composition can reduce stress generation in the resin layer even when temperature changes occur, and therefore has excellent heat cycle properties.
[0046] The first and second spherical fillers do not need to be perfectly spherical, but may be fillers having a shape with minimal surface irregularities that allow stress generated inside the resin layer to be released. Spherical fillers also include fillers composed of polyhedrons with 12 or more sides. The materials of the first and second spherical fillers may be the same or different.
[0047] (Other Components) The thermosetting resin composition of the embodiment may contain an ion scavenger that captures ions generated within the thermosetting resin composition. By including this ion scavenger, the number of ions present in the resin composition is reduced, improving the breakdown voltage characteristics. The content of the ion scavenger in the thermosetting resin composition is 40 parts by weight or more and 60 parts by weight or less per 100 parts by weight of the epoxy resin.
[0048] The thermosetting resin composition of the embodiment may further contain other additives. Examples of the other additives include imidazole-based curing accelerators such as 2-methylimidazole, 2-undecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, and N-benzyl-2-methylimidazole; Lewis acid complex-based curing accelerators such as boron trifluoride monoethylamine and boron trifluoride diethylamine; curing accelerators such as polyamines and melamine resins, dispersants, softeners, heat aging inhibitors, and silane coupling agents.
[0049] As described above, the thermosetting resin composition of the embodiment can be obtained by mixing the above-mentioned materials.
[0050] The thermosetting resin composition has a thermal conductivity of 2 W / m·K or more after curing, providing excellent thermal conductivity. Furthermore, this thermosetting resin composition has a storage modulus of 7000 MPa or less at −30°C after curing, a storage modulus of 10 MPa to 100 MPa at 25°C after curing, and a storage modulus of 1 MPa to 100 MPa at 125°C after curing. A heat sink comprising a resin layer made of such a thermosetting resin composition and a metal plate exhibits excellent heat cycle properties in a heat cycle test in which the heat sink is alternately and repeatedly exposed to two temperature atmospheres: a low-temperature atmosphere of −20°C to −40°C and a high-temperature atmosphere of 100°C to 175°C.
[0051] The thermosetting resin composition is cured, for example, at 160°C to 200°C for at least 1 hour. The thermal conductivity of the thermosetting resin composition can be measured by a laser flash method using an LFA (Laser Flash Analyzer). The storage modulus of the thermosetting resin composition can be measured by a dynamic viscoelasticity measurement method.
[0052] Next, a resin sheet according to an embodiment will be described. [Resin Sheet] As shown in Fig. 1, a resin sheet 10 according to an embodiment is made of a thermosetting resin composition according to an embodiment and has a sheet-like shape. The cured state of the resin sheet 10 is a semi-cured state.
[0053] The thickness of the resin sheet 10 is sufficient if it has adhesiveness and exhibits excellent thermal conductivity and heat cycle characteristics when used as a resin layer of a heat sink, and is, for example, 80 μm or more and 500 μm or less.
[0054] The resin sheet 10 is produced, for example, by the following procedure. A thermosetting resin composition is prepared by adding predetermined amounts of an epoxy resin, a curing agent, an ethylene-acrylic copolymer, a first spherical filler, and a second spherical filler to a container and mixing them. The thermosetting resin composition is applied to a separate film using, for example, an application device, and heated. After cooling, a separate film is obtained, i.e., the resin sheet 10, on which a resin layer composed of the thermosetting resin composition is formed. The obtained resin sheet 10 is used by peeling off the separate film. The cured state of the resin sheet 10 is a semi-cured state. The curing conditions are, for example, 100°C or higher and 250°C or lower, and 5 seconds or higher and 30 minutes or lower, and can be adjusted depending on the thickness of the resin sheet 10.
[0055] The thickness of the separation film used when producing the resin sheet 10 may be any thickness that is easy to handle, for example, 25 μm or more and 100 μm or less. The thickness of the separation film is determined depending on the thickness of the resin layer. Examples of materials for the separation film include polyethylene, polypropylene, polyimide, polyamide, polyethylene naphthalate, and polyethylene terephthalate. To facilitate peeling of the separation film from the resin sheet 10, the surface of the separation film may be subjected to a release treatment. Examples of treatment agents for the release treatment include silicone-based treatment agents and fluorine-based treatment agents.
[0056] The resin sheet 10 may have a different configuration. An example of a resin sheet 10 having a different configuration is a double-sided resin sheet in which resin layers are formed on both sides of a film in order to improve rigidity and electrical insulation reliability. Examples of materials for this film include polyimide, polyamide, and polyethylene naphthalate in order to improve heat resistance and the rigidity of the resin sheet. The resin sheet of the embodiment has been described above.
[0057] Next, a heat sink according to an embodiment will be described. [Heat sink] As shown in Fig. 2, a heat sink 20 according to an embodiment includes a metal plate 21 and a resin layer 23 made of the thermosetting resin composition according to an embodiment. The resin layer 23 is formed on at least one surface of the metal plate 21. The resin layer 23 is in a semi-cured state. As shown in Fig. 3, an electronic component 40 is mounted on the substrate 30 via a circuit 31 formed on the substrate 30. The substrate 30 is provided on the surface of the resin layer 23 opposite to the surface on which the metal plate 21 is formed.
[0058] The thickness of the resin layer 23 may be any thickness that can maintain insulation between the substrate 30 and the metal plate 21, and is, for example, 80 μm to 500 μm, preferably 100 μm to 200 μm.
[0059] The metal plate 21 is preferably made of a metal having high thermal conductivity as long as it can efficiently dissipate heat generated from the electronic components 40 mounted on the substrate 30. Examples of metals having high thermal conductivity include copper, aluminum, and stainless steel. Among these, copper and aluminum are preferred because they are easy to process and have high thermal conductivity.
[0060] The thickness of the metal plate 21 may be any thickness that allows easy processing, and is, for example, 9 μm to 10 mm, and preferably 500 μm to 2 mm. The metal plate 21 also includes metal foil.
[0061] 3, the metal plate 21 may be provided with a plurality of fins 22 on the surface opposite to the surface on which the resin layer 23 is formed. The metal plate 21 provided with a plurality of fins 22 is also called a heat sink.
[0062] The thickness of the metal plate 21 on which the multiple fins 22 are provided is, for example, 0.3 mm or more and 50 mm or less. The fins 22 are formed, for example, from plates or rods. The height of the fins 22 is, for example, 1 mm or more and 100 mm or less. The thickness of the plate-shaped fins is, for example, 0.2 mm or more and 9 mm or less, and is preferably thinner than the thickness of the metal plate 21. Furthermore, the plate-shaped fins are preferably smaller than the metal plate 21. The cross-sectional shape of the rod-shaped fins in a direction perpendicular to the longitudinal direction of the fins is, for example, square or circular.
[0063] The entire surface of the fin 22 may be covered with the thermosetting resin composition of the embodiment, or only a part of the surface of the fin 22 may be covered with the thermosetting resin composition of the embodiment.
[0064] The heat sink 20 is produced, for example, by the following procedure. A metal plate 21 and a resin sheet 10 serving as the resin layer 23 are prepared. Before laminating the resin sheet 10 on the metal plate 21, the separate film is peeled off from the resin surface of the resin sheet 10. Next, the resin sheet 10 is laminated on the metal plate 21 so that the resin sheet 10 and the metal plate 21 are in contact with each other. Thereafter, the metal plate 21 on which the resin sheet 10 is laminated is heated and pressurized under conditions of, for example, 0.3 MPa to 10 MPa, 100°C to 250°C, and 5 seconds to 30 minutes. After cooling, the heat sink 20 is obtained. The heating and pressurizing conditions can be adjusted depending on the thickness of the resin layer 23.
[0065] Another method for manufacturing the heat sink 20 includes, for example, the following method. A thermosetting resin composition is prepared by adding predetermined amounts of epoxy resin, a curing agent, an ethylene-acrylic copolymer, first spherical fillers, and second spherical fillers to a container and mixing them. A metal plate 21 is also prepared. The thermosetting resin composition is then applied to the metal plate 21 using, for example, an application device, and heated. After cooling, the metal plate 21 with the resin layer 23 formed thereon, i.e., the heat sink 20, is obtained. The heating conditions are, for example, 100°C or higher and 250°C or lower, and 5 seconds or longer and 30 minutes or shorter. The heating conditions can be adjusted depending on the thickness of the resin layer 23. The heat sink of the embodiment has been described above.
[0066] An organic solvent may be used when preparing the thermosetting resin composition of the embodiment. Examples of the organic solvent include alcohols such as methanol and ethanol; glycols such as ethylene glycol and propylene glycol; glycol monoalkyl ethers such as ethylene glycol monomethyl ether and ethylene glycol monoethyl ether; glycol dialkyl ethers such as ethylene glycol dimethyl ether and ethylene glycol diethyl ether; alkyl esters such as methyl acetate, ethyl acetate, propyl acetate, and methyl acetoacetate; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene; aliphatic hydrocarbons such as hexane, cyclohexane, and octane; amides such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; and cyclic ethers such as tetrahydrofuran and dioxane.
[0067] An example of an apparatus used to form the resin sheet 10 and the resin layer 23 of the heat sink 20 according to the embodiment is a coating apparatus. Examples of the coating apparatus include known coaters, such as a die coater and a comma coater.
[0068] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to these examples in any way.
[0069] The following were used as components contained in the thermosetting resin compositions in the examples and comparative examples: (Epoxy Resin) (1) jER (registered trademark) 828: bisphenol A type epoxy resin, epoxy equivalent 190 g / eq, manufactured by Mitsubishi Chemical Corporation.
[0070] (Curing agent) Seikacure-S: 4,4'-DDS (4,4'-diaminodiphenylsulfone), amine value 62 g / eq, manufactured by Wakayama Seika Kogyo Co., Ltd.
[0071] (Acrylic copolymers) (1) VMX4017: ethylene acrylic copolymer having carboxy groups on the side chains, glass transition temperature -41°C, manufactured by DuPont; (2) GLS: ethylene acrylic copolymer having carboxy groups on the side chains, glass transition temperature -24°C, manufactured by DuPont; (3) 1HY-3006Y: acrylic copolymer having carboxy groups on the side chains (not containing ethylene in the main chain), weight average molecular weight of about 280,000, glass transition temperature -53°C, manufactured by Taisei Fine Chemical Co., Ltd.; (4) 1HY-2002M: acrylic copolymer having carboxy groups on the side chains (not containing ethylene in the main chain), weight average molecular weight of about 280,000, glass transition temperature -3°C, manufactured by Taisei Fine Chemical Co., Ltd.
[0072] (Ion scavenger) KW-2200: magnesium oxide / aluminum oxide solid solution, manufactured by Kyowa Chemical Industry Co., Ltd.
[0073] (Filler) (1) DAM-45: spherical alumina, average particle size (D50) 45 μm, thermal conductivity 36 W / m·K, manufactured by Denka Company, Limited; (2) DAM-20: spherical alumina, average particle size (D50) 20 μm, thermal conductivity 36 W / m·K, manufactured by Denka Company, Limited; (3) DAM-10: spherical alumina, average particle size (D50) 10 μm, thermal conductivity 36 W / m·K, manufactured by Denka Company, Limited; (4) DAM-03: spherical alumina, average particle size (D50) 3 μm, thermal conductivity 36 W / m·K, manufactured by Denka Company, Limited; (5) AA18: non-spherical alumina, average particle size (D50) 20 μm, thermal conductivity 36 W / m·K, manufactured by Sumitomo Chemical Company, Limited; (6) AS-50: non-spherical alumina, average particle size (D50) 10 μm, thermal conductivity 36 W / m·K, manufactured by Showa Denko K.K. (7) LS-210: non-spherical alumina, average particle size (D50) 2 μm, thermal conductivity 36 W / m·K, manufactured by Nippon Light Metal Co., Ltd. (8) AO-502: spherical alumina, average particle size (D50) 0.25 μm, thermal conductivity 36 W / m·K, manufactured by Admatechs Co., Ltd. (9) FAN-f50-A1: spherical aluminum nitride, average particle size (D50) 50 μm, thermal conductivity 170 W / m·K, manufactured by Furukawa Denshi Co., Ltd. (10) FAN-f05: polyhedral shape, aluminum nitride, average particle size (D50) 5.0 μm, thermal conductivity 170 W / m·K, manufactured by Furukawa Denshi Co., Ltd. (11) FB-40R: spherical silica, average particle size (D50) 40 μm, thermal conductivity 1 W / m·K, manufactured by Denka Co., Ltd. (12) FB-5SDC: spherical silica, average particle size (D50) 3.0 μm, thermal conductivity 1 W / m·K, manufactured by Denka Co., Ltd.
[0074] Example 1 First, a thermosetting resin composition was prepared. A resin sheet 10 composed of the thermosetting resin composition was fabricated. Next, the storage modulus of the thermosetting resin composition after curing was measured using the resin sheet 10. The thermal conductivity of the resin sheet 10 was also measured. Furthermore, a heat cycle test was performed on a heat sink 20 using the resin sheet 10.
[0075] (Preparation of Thermosetting Resin Composition) A vessel was charged with 100 parts by weight of jER (registered trademark) 828, 10 parts by weight of Seikacure-S, 800 parts by weight of VMX4017, 4006 parts by weight of DAM-45, 2670 parts by weight of DAM-03, and 500 parts by weight of methyl ethyl ketone as an organic solvent. These were then stirred at room temperature to obtain a thermosetting resin composition.
[0076] (Measurement of storage modulus) To measure the storage modulus of the obtained thermosetting resin composition, a measurement sample was prepared. First, the thermosetting resin composition was applied to the release-treated surface of a 50 μm thick release PET (polyethylene terephthalate) film (PET5011 manufactured by Lintec Corporation) so that the thickness after pressing was 100 μm, and then covered with another release PET film. Then, a laminate formed by laminating the release PET film, the thermosetting resin composition, and the release PET film in this order was heated and pressurized under conditions of 180 ° C, 3 MPa, and 60 minutes. After cooling, a cured resin sheet 10 having a thickness of 100 μm was obtained. The obtained cured resin sheet 10 was cut into a rectangle with a length of 30 mm and a width of 4 mm to obtain a sample for measuring the storage modulus.
[0077] The storage modulus was measured by dynamic viscoelasticity measurement using an RSA-G2 (manufactured by TA Instruments). The measurement conditions were a temperature range of -50°C to 200°C, a heating rate of 10°C / min, a frequency of 1 Hz, a chuck distance of 20 mm, and tension mode. The storage modulus of the cured thermosetting resin composition of Example 1 was 325 MPa at -30°C, 15 MPa at 25°C, and 8 MPa at 125°C.
[0078] (Preparation of Resin Sheet 10) A thermosetting resin composition was applied to the release-treated surface of a 50 μm-thick release PET film (PET5011 manufactured by Lintec Corporation) so that the thickness after heating would be 100 μm. The composition was then heated at 120° C. for 10 minutes and cooled to obtain a resin sheet 10 with a release PET film attached to one side. The cured state of the resin sheet 10 was a semi-cured state (B stage).
[0079] <Thermal Conductivity> The thermal diffusion coefficient (α), specific heat (Cp), and density (ρ) of a sample for measuring thermal conductivity were measured, and the thermal conductivity was calculated using the following formula: Thermal conductivity [W / (m·K)]=α[mm 2 / s]×Cp[J / g・K]×ρ[g / cm 3 ] α[mm 2 / s]: thermal diffusion coefficient, Cp [J / g K]: specific heat, ρ [g / cm 3 ]: density. The evaluation criteria were as follows: Good: 2 W / (m·K) or more, Poor: less than 2 W / (m·K). Note that a sample for measuring thermal conductivity that received a Good evaluation result has excellent thermal conductivity.
[0080] (Preparation of sample for thermal conductivity measurement) Two resin sheets 10 with a release PET film on one side were prepared and laminated so that the resin surfaces of the two sheets were in contact with each other to obtain a laminate. The laminate was heated and pressurized at 185°C, 5 MPa, and 180 minutes. The release PET film was then peeled off from the laminate to obtain a sample for thermal conductivity measurement.
[0081] (Measurement of thermal diffusion coefficient (α)) A laser flash method was used to measure the temperature change on one side of a sample for thermal conductivity measurement when pulsed light was irradiated on the other side. The obtained measurement data was analyzed using the half-time method to determine the thermal diffusion coefficient (α). A NETZSCH LFA447 was used as the measuring instrument, and measurements were taken at 25°C.
[0082] (Measurement of specific heat (Cp)) The specific heat Cp (J / g·K) of the sample for measuring thermal conductivity was determined by differential scanning calorimetry (DSC) in accordance with JIS K 7123. The measurement was performed using a Q200 made by TA Instruments under conditions of a temperature rise rate of 10°C / min and a temperature range of −30°C to 50°C.
[0083] (Measurement of density (ρ)) The density (ρ) was measured using an immersion method. Shimadzu Corporation's AUX220 and SMK-401 were used as measuring instruments. The thermal conductivity was calculated by substituting the values of the thermal diffusion coefficient (α), specific heat (Cp), and density (ρ) obtained above into the thermal conductivity formula. The thermal conductivity of the resin sheet 10 of Example 1 was 2.9 W / (m·K), and was evaluated as Good. It was found that the resin sheet 10 of Example 1 had excellent thermal conductivity.
[0084] <Heat Cycle Test> Next, a heat cycle test was performed on the resin sheet 10 of Example 1. A sample for measurement in the heat cycle test was prepared as follows.
[0085] (Preparation of Samples for Heat Cycle Test Measurement) A 35 μm-thick rolled copper foil (BHY manufactured by JX Nippon Mining & Metals Corporation) was prepared to represent the substrate 30 and circuit 31. The rolled copper foil and resin sheet 10 were laminated together so that the rough surface of the rolled copper foil contacted the resin surface of the resin sheet 10. Next, a 50 μm-thick aluminum foil (soft single-sided aluminum foil manufactured by Toyo Aluminum Co., Ltd.), corresponding to the metal plate 21, was laminated on the resin sheet 10 so that the rough surface of the aluminum foil contacted the resin surface opposite the resin surface on which the rolled copper foil was laminated, thereby obtaining a laminate. The obtained laminate had a configuration in which the rolled copper foil, the resin sheet 10, and the aluminum foil were laminated in this order. Next, the laminate was heated and pressurized at 180° C., 5 MPa, and for 60 minutes. After cooling, the laminate was cut into a 10 mm x 50 mm rectangle. The release PET film on the resin sheet 10 was removed before use.
[0086] Next, to form a resin layer to protect the surface of the laminate, the laminate was placed in a container, and resin was poured in so that the entire surface of the laminate was covered with resin. The resin was then heated at 100°C for 24 hours to solidify. After cooling, the resin-covered laminate was removed from the container and polished until the end face (cross section) of the laminate was exposed. The polished end face (cross section) of the laminate confirmed a structure in which the rolled copper foil, resin sheet, and aluminum foil were laminated in this order. This was used as a sample for heat cycle test measurement. The resin used was a two-component epoxy adhesive (Denatite, manufactured by Nagase ChemteX Corporation). Specifically, a resin obtained by mixing the base agent (XNR5021) and the curing agent (XNH5021) was poured into the container containing the laminate.
[0087] The sample for heat cycle test measurement was placed in a thermal shock tester (TSA-72EL-A manufactured by Espec Corporation). After placement, the temperature inside the tester was cooled to -40°C and maintained at that temperature for 30 minutes, and then the temperature was raised to 150°C and maintained at that temperature for 30 minutes. This constitutes one cycle, and 3000 cycles were performed. (Evaluation) After 3000 cycles, the polished end surface (cross section) of the laminate was observed with an optical microscope (VHX-8000 manufactured by Keyence Corporation) and evaluated according to the following criteria. Good: When the end surface (cross section) of the laminate was inspected, no cracks were observed in the copper foil layer. Poor: When the end surface (cross section) of the laminate was inspected, cracks were observed in the copper foil layer. After the heat cycle test, the sample for heat cycle test measurement of Example 1 had no cracks and was evaluated as Good.
[0088] As described above, it was found that the resin sheet 10 of Example 1 had excellent thermal conductivity. Also, the heat sink using the resin sheet 10 of Example 1 had excellent thermal conductivity. Furthermore, it was found that the heat sink of Example 1 had excellent heat cycle characteristics.
[0089] (Examples 2) to 15) and (Comparative Examples 1) to 15) As shown in Tables 1 and 2, thermosetting resin compositions were prepared in the same manner as in Example 1, except that the type and content of each component contained in the thermosetting resin composition was changed, and resin sheets 10 were produced. For the fillers contained in the thermosetting resin compositions of Comparative Examples 1 to 7 shown in Table 2, the ratio of the first spherical filler to the second spherical filler could not be calculated, so the "First spherical filler: Second spherical filler" column was entered as "-". The storage modulus of the cured thermosetting resin compositions prepared in each Example and Comparative Example was measured using the same method as in Example 1. The thermal conductivity of the resin sheets prepared in each Example and Comparative Example and the heat cycle test were performed using the same method as in Example 1. The unit of content in the table is "parts by weight" unless otherwise specified.
[0090]
[0091]
[0092] As shown in Table 1, it was found that the resin sheets 10 of Examples 2 to 15 had excellent thermal conductivity. In addition, the heat sinks using the resin sheets 10 of Examples 2 to 15 had excellent thermal conductivity. Furthermore, it was found that the heat sinks of Examples 2 to 15 had excellent heat cycle characteristics.
[0093] Furthermore, the peel strength, the breakdown voltage, and the breakdown voltage after a long-term wet heat test were measured for the resin sheets 10 of Examples 1 to 15, and the adhesiveness and the breakdown voltage characteristics were evaluated. Example 1 will be described below as an example.
[0094] <Breakdown Voltage> (Sample for Measuring Breakdown Voltage) A sample for measuring the breakdown voltage of Example 1 was prepared as follows. First, the resin sheet 10 prepared in Example 1, a 35 μm-thick rolled copper foil (BHY manufactured by JX Nippon Mining & Metals Corporation) representing the substrate 30 and circuit 31, and a 1 mm-thick aluminum plate (A1100 manufactured by Showa Denko K.K.) corresponding to the metal plate 21 were prepared. Next, the rolled copper foil and the resin sheet 10 were laminated so that the rough surface of the rolled copper foil was in contact with the resin surface of the resin sheet 10. Next, the aluminum plate and the resin sheet 10 were laminated so that one side of the aluminum plate was in contact with the resin surface opposite the resin surface on which the rolled copper foil was laminated, thereby obtaining a laminate. The obtained laminate had a configuration in which the rolled copper foil, the resin sheet 10, and the aluminum plate were laminated in this order. Next, this laminate was heated and pressurized at 185° C., 5 MPa, and for 180 minutes. The laminate was then heated in an oven at 160°C for another 5 hours and then cooled. The rolled copper foil of the resulting laminate was etched to form a circular shape with a diameter of 20 mm. The laminate was then washed with water and dried to obtain a sample for measuring the breakdown voltage. The resin sheet 10 was used after removing the release PET film.
[0095] (Measurement and Evaluation of Breakdown Voltage) A B-5120AT-2 manufactured by Nippon Technate Co., Ltd. was used as the breakdown tester. A sample for measuring breakdown voltage was immersed in oil at 25°C, and a voltage was applied between a circularly etched rolled copper foil and an aluminum plate. The voltage was increased at a rate of 1 kV / 0.5 sec, and the voltage at which breakdown occurred was measured. This test was performed five times, and the average value was calculated and evaluated according to the following criteria. This breakdown voltage is also referred to as the breakdown voltage before the long-term wet heat test. Good: Voltage is 2 kV or more; Poor: Voltage is less than 2 kV. The breakdown voltage of Example 1 was 3.5 kV, and the evaluation was Good. It was found that the resin sheet 10 of Example 1 had excellent insulation properties.
[0096] <Peel Strength> (Sample for Peel Strength Measurement) A laminate obtained during the process of producing a sample for measuring dielectric breakdown voltage was prepared separately. The rolled copper foil of this laminate was etched to a width of 10 mm and a length of 100 mm. The etched laminate was washed with water and dried to obtain a sample for peel strength measurement of Example 1.
[0097] (Measurement and Evaluation of Peel Strength) An Autograph AGS-500 manufactured by Shimadzu Corporation was used as the measuring instrument. The rolled copper foil was peeled off in a 90° direction (a direction perpendicular to the main surface of the sample), and the peel strength at the interface between the rolled copper foil and the resin sheet 10 was measured. The test speed was 50 mm / min. The test was performed twice, and the average value was calculated. The evaluation criteria were as follows: Good: Peel strength is 2 N / cm or more, Poor: Peel strength is less than 2 N / cm. The peel strength of Example 1 was 10 N / cm, and the evaluation was Good.
[0098] <Breakdown voltage after long-term damp heat test> The insulating properties of the resin sheet 10 after the long-term damp heat test were evaluated by measuring the breakdown voltage of the resin sheet 10. (Sample for measuring breakdown voltage after long-term damp heat test) The sample used in this evaluation was prepared using the same method as the preparation method for the sample for measuring breakdown voltage described above. (Measurement and evaluation of breakdown voltage after long-term damp heat test) The sample for measuring breakdown voltage after the long-term damp heat test was stored in an atmosphere of 85°C x 85% RH x 1000 hours, and then moisture adhering to the surface of the sample was wiped off and the breakdown voltage was measured under the same measurement conditions as the breakdown voltage described above. The evaluation criteria were as follows: Good: Voltage 1 kV or more; Poor: Voltage less than 1 kV. The breakdown voltage of Example 1 after the long-term damp heat test was 0.5 kV, and the evaluation was Poor.
[0099] As described above, the resin sheet 10 made from the thermosetting resin composition of Example 1 had a low breakdown voltage after the long-term damp heat test, but a high breakdown voltage before the long-term damp heat test, demonstrating excellent adhesion to metal. Furthermore, the resin sheets 10 made from the thermosetting resin compositions of Examples 2 to 15 were also measured for breakdown voltage, peel strength, and breakdown voltage after the long-term damp heat test in the same manner as in Example 1, and the breakdown voltage characteristics and adhesion were evaluated. The results are shown in Table 3.
[0100]
[0101] From Table 3, for example, the resin sheet 10 of Example 2, which was made of a thermosetting resin composition containing an ion scavenger, had high breakdown voltages before and after the long-term damp heat test, and high peel strength. This indicates that the resin sheet 10 of Example 2 has excellent breakdown voltage characteristics and adhesiveness.
[0102] It was also found that the resin sheets 10 of Examples 3 to 6, Examples 8 to 11, Example 13, and Example 14 were also excellent in breakdown voltage characteristics and adhesiveness.
[0103] From the above results, it was found that the resin sheets 10 of Examples 1 to 15 have excellent thermal conductivity and adhesiveness. In addition, the heat sinks using the resin sheets 10 of Examples 1 to 15 have excellent thermal conductivity. It was also found that the heat sinks 20 of Examples 1 to 15 have excellent heat cycle characteristics. Furthermore, it was found that the resin sheets 10 of Examples 2 to 6, Examples 8 to 11, Example 13, and Example 14 have excellent breakdown voltage characteristics.
[0104] The present invention allows various embodiments and modifications without departing from the broad spirit and scope of the present invention. Furthermore, the above-described embodiments are intended to illustrate the present invention and do not limit the scope of the present invention. That is, the scope of the present invention is defined by the claims, not the embodiments. Various modifications made within the scope of the claims and within the scope of the meaning of the invention equivalent thereto are considered to be within the scope of the present invention.
[0105] This application is based on Japanese Patent Application No. 2023-066101, filed on April 14, 2023. The specification and claims of Japanese Patent Application No. 2023-066101 are incorporated herein by reference.
[0106] (Notes) (Note 1) An epoxy resin; a curing agent for curing the epoxy resin; an ethylene acrylic copolymer having a glass transition temperature of -30°C or lower and having a carboxy group in a side chain; first spherical fillers having a thermal conductivity of 20 W / m·K or higher and an average particle size (D50) of 30 μm or more and 60 μm or less; and second spherical fillers having a thermal conductivity of 20 W / m·K or higher and an average particle size (D50) of 1 μm or more and 10 μm or less, wherein the total weight ratio of the first spherical fillers and the second spherical fillers is 84 wt% or more and 90 wt% or less with respect to 100 wt% of the total solid content, and the ratio of the first spherical fillers to the second spherical fillers is 55:45 to 85:15, The thermosetting resin composition has an ethylene-acrylic copolymer content of 700 parts by weight or more and 1,000 parts by weight or less relative to 100 parts by weight of the epoxy resin.
[0107] (Appendix 2) The thermosetting resin composition according to Appendix 1, wherein the first spherical filler is composed of at least one selected from the group consisting of alumina, boron nitride, aluminum nitride, magnesium oxide, zinc oxide, and silicon nitride.
[0108] (Appendix 3) The thermosetting resin composition according to Appendix 1 or Appendix 2, wherein the second spherical filler is composed of at least one selected from the group consisting of alumina, boron nitride, aluminum nitride, magnesium oxide, zinc oxide, and silicon nitride.
[0109] (Appendix 4) The thermosetting resin composition according to any one of Appendices 1 to 3, further comprising an ion scavenger that captures ions, wherein the content of the ion scavenger is 40 parts by weight or more and 60 parts by weight or less relative to 100 parts by weight of the epoxy resin.
[0110] (Appendix 5) The thermosetting resin composition according to any one of Appendices 1 to 4, having a thermal conductivity after curing of 2 W / m K or more, a storage modulus after curing at −30° C. of 7000 MPa or less, a storage modulus after curing at 25° C. of 10 MPa or more and 100 MPa or less, and a storage modulus after curing at 125° C. of 1 MPa or more and 100 MPa or less.
[0111] (Appendix 6) A resin sheet comprising the thermosetting resin composition according to any one of Appendices 1 to 5.
[0112] (Supplementary Note 7) The resin sheet according to Supplementary Note 6, which is in a semi-cured state.
[0113] (Supplementary Note 8) A heat sink comprising: a metal plate; and a resin layer formed from the thermosetting resin composition according to any one of Supplementary Note 1 to Supplementary Note 5, wherein the resin layer is formed on at least one surface of the metal plate.
[0114] (Supplementary Note 9) The heat sink according to Supplementary Note 8, wherein the cured state of the resin layer is a semi-cured state.
[0115] (Appendix 10) A method for producing a resin sheet, comprising: a preparation step of preparing the thermosetting resin composition according to any one of Appendices 1 to 5; a formation step of forming a resin layer composed of the thermosetting resin composition into a film; and a heating step of heating the film on which the resin layer has been formed.
[0116] (Appendix 11) A method for manufacturing a heat sink, comprising: a lamination step of laminating a resin layer of a resin sheet obtained by the method for manufacturing a resin sheet according to Appendix 10 onto a metal plate; and a heating and pressurizing step of heating and pressurizing the metal plate on which the resin layer is laminated.
[0117] (Appendix 12) A method for manufacturing a heat sink, comprising: a preparation step of preparing the thermosetting resin composition according to any one of Appendices 1 to 5; a formation step of forming a resin layer composed of the thermosetting resin composition on a metal plate; and a heating step of heating the metal plate on which the resin layer has been formed.
[0118] 10 Resin sheet, 20 Heat sink, 21 Metal plate, 22 Fin, 23 Resin layer, 30 Substrate, 31 Circuit, 40 Electronic component
Claims
1. A thermosetting resin composition comprising: an epoxy resin; a curing agent for curing the epoxy resin; an ethylene-acrylic copolymer having a glass transition temperature of -30°C or lower and having a carboxy group in a side chain; first spherical fillers having a thermal conductivity of 20 W / m·K or higher and an average particle size (D50) of 30 μm to 60 μm; and second spherical fillers having a thermal conductivity of 20 W / m·K or higher and an average particle size (D50) of 1 μm to 10 μm, wherein the total weight ratio of the first spherical fillers and the second spherical fillers is 84% by weight to 90% by weight based on 100% by weight of total solids, the ratio of the first spherical fillers to the second spherical fillers is 55:45 to 85:15, and the content of the ethylene-acrylic copolymer is 700 parts by weight to 1000 parts by weight based on 100 parts by weight of the epoxy resin.
2. The thermosetting resin composition according to claim 1, wherein the first spherical filler is composed of at least one material selected from the group consisting of alumina, boron nitride, aluminum nitride, magnesium oxide, zinc oxide, and silicon nitride.
3. The thermosetting resin composition according to claim 1, wherein the second spherical filler is composed of at least one material selected from the group consisting of alumina, boron nitride, aluminum nitride, magnesium oxide, zinc oxide, and silicon nitride.
4. The thermosetting resin composition according to claim 1, comprising an ion scavenger that captures ions, the content of the ion scavenger being 40 parts by weight or more and 60 parts by weight or less per 100 parts by weight of the epoxy resin.
5. The thermosetting resin composition according to claim 1, having a thermal conductivity after curing of 2 W / m K or more, a storage modulus after curing at -30°C of 7,000 MPa or less, a storage modulus after curing at 25°C of 10 MPa or more and 100 MPa or less, and a storage modulus after curing at 125°C of 1 MPa or more and 100 MPa or less.
6. A resin sheet comprising the thermosetting resin composition according to any one of claims 1 to 5.
7. The resin sheet according to claim 6, which is in a semi-cured state.
8. A heat sink comprising: a metal plate; and a resin layer formed from the thermosetting resin composition according to any one of claims 1 to 5, said resin layer being formed on at least one surface of said metal plate.
9. The heat sink according to claim 8, wherein the cured state of the resin layer is a semi-cured state.
10. A method for producing a resin sheet, comprising: a preparation step of preparing a thermosetting resin composition according to any one of claims 1 to 5; a formation step of forming a resin layer composed of the thermosetting resin composition into a film; and a heating step of heating the film on which the resin layer has been formed.
11. A method for manufacturing a heat sink, comprising: a lamination step of laminating a resin layer of a resin sheet obtained by the method for manufacturing a resin sheet according to claim 10 onto a metal plate; and a heating and pressurizing step of heating and pressurizing the metal plate on which the resin layer is laminated.
12. A method for manufacturing a heat sink, comprising: a preparation step of preparing a thermosetting resin composition according to any one of claims 1 to 5; a formation step of forming a resin layer composed of the thermosetting resin composition on a metal plate; and a heating step of heating the metal plate on which the resin layer has been formed.
Citation Information
Patent Citations
Adhesive sheet for electronic equipment
JP2008106231A
Resin sheet for sealing
JP2016000784A
Thermosetting resin composition, heat dissipation sheet, heat dissipation plate, method for manufacturing heat dissipation sheet, and method for manufacturing heat dissipation plate
WO2023068024A1