Resin composition, cured resin product, method for producing cured resin product, electronic device, method for producing electronic device, and resin sheet

The resin composition, featuring a urethane-acryloyl and epoxy-oxetanyl compound combination with specific initiators, achieves enhanced elasticity and low tackiness through phase separation, overcoming the balance challenges in conventional resin compositions for stretchable devices.

WO2024214490A1PCT designated stage expired Publication Date: 2024-10-17MITSUI CHEMICALS INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010456
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-10
Filing Date
2024-03-18
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Conventional resin compositions for stretchable devices often fail to achieve a balance between excellent elasticity and low tackiness, which is crucial for their performance as substrates or cover materials.

Method used

A resin composition comprising a compound with a urethane group and a (meth)acryloyl group, an epoxy group- or oxetanyl group-containing compound, a radical polymerization initiator, and a cationic polymerization initiator, where the surface tension of the latter is less than that of the former, allowing for phase separation and forming a cured product with distinct soft and hard segments, enhancing both elasticity and low tackiness.

Benefits of technology

The resin composition effectively produces a cured product with improved elasticity and low tackiness, as demonstrated by specific tan δ peak temperatures and phase-separated structures, addressing the limitations of existing compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010456_17102024_PF_FP_ABST
    Figure JP2024010456_17102024_PF_FP_ABST
Patent Text Reader

Abstract

This resin composition contains: a compound (A) having a urethane group and a (meth)acryloyl group; a compound (B) having an epoxy group and / or an oxetanyl group; a radical polymerization initiator (C); and a cationic polymerization initiator (D). The surface tension γB of the compound (B) is 80% or less with respect to the surface tension γA of the compound (A). The tanδ peaks of a cured product of the resin composition include a first peak having a peak temperature of lower than 100ºC and a second peak having a peak temperature of 100ºC or higher. The difference between the peak temperature T1 of the first peak and the peak temperature T2 of the second peak is at least 30ºC.
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition, cured resin product, method for manufacturing cured resin product, electronic device, method for manufacturing electronic device, and resin sheet

[0001] The present invention relates to a resin composition, a cured resin, a method for producing a cured resin, an electronic device, a method for producing an electronic device, and a resin sheet.

[0002] Conventionally, cured resins have been used as substrates for stretchable devices. Such cured resins are required to have excellent stretchability and low tackiness. Therefore, various resin compositions have been proposed to obtain cured resins having excellent stretchability and low tackiness.

[0003] More specifically, the following addition-curable silicone coating composition has been proposed as a resin composition: The addition-curable silicone coating composition contains (A) an alkenyl-containing organopolysiloxane, (B) an organohydrogenpolysiloxane, (C) a platinum group metal catalyst, and (D) a solvent in specific proportions. This addition-curable silicone coating composition cures upon heating to form a cured silicone product (see, for example, Patent Document 1).

[0004] Furthermore, for example, the following resin composition has been proposed as a resin composition. This resin composition contains (A) a rubber component, (B) a crosslinking component, and (C) a silicone oil having a reactive terminal group. The resin composition cures upon heating or light irradiation to form an elastic resin layer (see, for example, Patent Document 2).

[0005] JP 2020-203985 A JP 2019-195978 A

[0006] However, the cured product of the above-mentioned resin composition may not have sufficient stretchability and low tackiness.

[0007] Furthermore, in recent years, the use of cured resins as substrates and / or cover members for stretchable devices has been considered, and in such applications, particularly excellent stretchability and low tackiness are required.

[0008] The present invention relates to a resin composition that can give a cured resin product having both excellent stretchability and excellent low tackiness, a cured resin product that is a cured product of the resin composition, a method for manufacturing the cured resin product, an electronic device including the cured resin product, a method for manufacturing the electronic device, and a resin sheet.

[0009] The present invention [1] is a resin composition comprising a compound (A) having a urethane group and a (meth)acryloyl group, an epoxy group- and / or oxetanyl group-containing compound (B), a radical polymerization initiator (C), and a cationic polymerization initiator (D), wherein the surface tension γB of the compound (B) is 80% or less of the surface tension γA of the compound (A), and the peaks of tanδ of a cured product of the resin composition have a first peak having a peak temperature of less than 100°C and a second peak having a peak temperature of 100°C or higher, and the difference between the peak temperature T1 of the first peak and the peak temperature T2 of the second peak is 30°C or higher.

[0010] The present invention [2] includes the resin composition according to the above [1], in which the radical polymerization initiator (C) is a photopolymerization initiator, and the cationic polymerization initiator (D) is a thermal polymerization initiator.

[0011] The present invention [3] includes the resin composition according to the above [1], wherein the radical polymerization initiator (C) is a photopolymerization initiator, the cationic polymerization initiator (D) is a photopolymerization initiator, and the difference between the peak wavelength on the long wavelength side of the light absorption wavelength of the radical polymerization initiator (C) and the peak wavelength on the long wavelength side of the light absorption wavelength of the cationic polymerization initiator (D) is 30 nm or more.

[0012] The present invention [4] includes the resin composition according to any one of the above [1] to [3], in which the compound (A) contains a reaction product of an isocyanate compound (a1) and an active hydrogen group-containing (meth)acrylate (a2), the isocyanate compound (a1) has an alicyclic structure, and the alicyclic structure has a chair conformation.

[0013] The present invention [5] includes the resin composition according to any one of the above [1] to [4], wherein the compound (B) includes a bisphenol A epoxy compound and / or a hydrogenated bisphenol A epoxy compound or a bisphenol epoxy compound, and the hydrogen-bonding substituent value of the compound (B) is less than 0.0005 mol / g.

[0014] The present invention [6] includes a cured resin product comprising a cured resin composition according to any one of the above [1] to [5].

[0015] The present invention [7] includes a method for producing a cured resin product, which includes a preparation step of preparing the resin composition described in the above [2], and a curing step of curing the resin composition, the curing step including an irradiation step and a heating step, in which the resin composition is irradiated with active energy rays in the irradiation step, and the resin composition is heated in the heating step after the irradiation step.

[0016] The present invention [8] includes a method for producing a cured resin product, comprising: a preparation step of preparing the resin composition described in the above [3]; and a curing step of curing the resin composition, wherein the curing step comprises a first irradiation step and a second irradiation step, in which the resin composition is irradiated with active energy rays having a wavelength corresponding to a peak wavelength on the long wavelength side of the light absorption wavelengths of the radical polymerization initiator (C) in the first irradiation step; and in the second irradiation step, the resin composition is irradiated with active energy rays having a wavelength corresponding to a peak wavelength on the long wavelength side of the light absorption wavelengths of the cationic polymerization initiator (D) after the first irradiation step.

[0017] The present invention [9] includes an electronic device comprising the cured resin material described in the above [6].

[0018] The present invention

[10] is a method for producing an electronic device including a cured resin product, and includes a method for producing an electronic device, in which the cured resin product is produced by the method for producing a cured resin product described in [7] above.

[0019] The present invention

[11] is a method for producing an electronic device including a cured resin product, and includes a method for producing an electronic device, in which the cured resin product is produced by the method for producing a cured resin product described in [8] above.

[0020] The present invention

[12] includes a resin sheet having a phase-separated composite and a skin layer disposed on the surface of the phase-separated composite, wherein the skin layer is made of a cured product of an epoxy group- and / or oxetanyl group-containing compound (B), and the phase-separated composite contains a cured product of a compound (A) having a urethane group and a (meth)acryloyl group, and the cured product of the compound (B), wherein the cured product of the compound (A) and the cured product of the compound (B) are phase-separated.

[0021] The present invention

[13] includes the resin sheet according to the above

[12] , wherein the tan δ peak of the resin sheet has a first peak having a peak temperature of less than 100°C and a second peak having a peak temperature of 100°C or higher, and the difference between the peak temperature T1 of the first peak and the peak temperature T2 of the second peak is 30°C or higher.

[0022] The resin composition of the present invention includes a compound (A) having a urethane group and a (meth)acryloyl group, an epoxy group- and / or oxetanyl group-containing compound (B), a radical polymerization initiator (C), and a cationic polymerization initiator (D). The surface tension γB of the compound (B) is a predetermined value or less relative to the surface tension γA of the compound (A). Furthermore, the tan δ peak of a cured product of the resin composition has a first peak having a peak temperature of less than 100°C and a second peak having a peak temperature of 100°C or higher, and the difference between the peak temperature T1 of the first peak and the peak temperature T2 of the second peak is a predetermined value or more. Therefore, the resin composition can produce a cured resin product having both excellent elasticity and excellent low tackiness.

[0023] More specifically, the resin composition contains a compound (A) having a urethane group and a (meth)acryloyl group. The compound (A) having a urethane group and a (meth)acryloyl group is cured by a radical polymerization initiator (C). The cured product (α) of the compound (A) having a urethane group and a (meth)acryloyl group has excellent elasticity. Therefore, the cured product (cured resin product) of the resin composition has excellent elasticity derived from the cured product (α).

[0024] The resin composition also contains an epoxy group- and / or oxetanyl group-containing compound (B). The epoxy group- and / or oxetanyl group-containing compound (B) is cured by a cationic polymerization initiator (D). The cured product (β) of the epoxy group- and / or oxetanyl group-containing compound (B) has excellent low tackiness. Therefore, the cured product (resin cured product) of the resin composition has excellent low tackiness derived from the cured product (β).

[0025] Furthermore, in the above resin composition, the surface tension γB of compound (B) is equal to or less than a predetermined ratio of the surface tension γA of compound (A). Therefore, compound (A) and compound (B) undergo phase separation in the resin composition. As a result, a phase-separated composite of cured products (α) and (β) is obtained by curing the resin composition. In the phase-separated composite, cured product (α) forms soft segments, and cured product (β) forms hard segments. Therefore, the cured product of the above resin composition has both excellent stretchability and excellent low tackiness.

[0026] In particular, in the above-mentioned resin composition, the tan δ peaks of the cured product have a first peak having a peak temperature of less than 100°C and a second peak having a peak temperature of 100°C or higher. In addition, the difference between the peak temperature T1 of the first peak and the peak temperature T2 of the second peak is equal to or greater than a predetermined value. Therefore, the above-mentioned resin composition can satisfactorily exhibit the stretchability derived from the cured product (α) of compound (A) and the low tackiness derived from the cured product (β) of compound (B).

[0027] The cured resin includes a cured product of the resin composition, and therefore has both the stretchability derived from the cured product (α) of compound (A) and the low tackiness derived from the cured product (β) of compound (B).

[0028] Furthermore, according to the above-described method for producing a cured resin, a cured resin having both excellent stretchability and excellent low tackiness can be efficiently obtained.

[0029] The resin sheet has a surface layer and a phase-separated composite, and the phase-separated composite contains a cured product of compound (A) and the cured product of compound (B). The cured product (α) of compound (A) and the cured product (β) of compound (B) are phase-separated. Therefore, the resin sheet has both the stretchability derived from the cured product (α) of compound (A) and the low tackiness derived from the cured product (β) of compound (B).

[0030] FIG. 1 is a transmission electron microscope image (TEM image) of a cross section of the cured resin product of Example 5.

[0031] 1. Resin Composition The resin composition contains, as essential components, a compound (A) having a urethane group and a (meth)acryloyl group, an epoxy group- and / or oxetanyl group-containing compound (B), a radical polymerization initiator (C), and a cationic polymerization initiator (D).

[0032] Each of the above components will be described in detail below. Note that the following components are described as examples. That is, the components are not limited to the following examples. Any substance that exhibits the functions and effects of the present invention can be used as a raw material for the resin composition.

[0033] [1] Compound (A) Having a Urethane Group and a (Meth)acryloyl Group The compound (A) having a urethane group and a (meth)acryloyl group has one or more urethane groups and one or more (meth)acryloyl groups in the molecule. Note that (meth)acryloyl refers to acryloyl and / or methacryloyl. Furthermore, (meth)acrylic refers to acrylic and / or methacrylic. Furthermore, (meth)acrylate refers to acrylate and / or methacrylate. Hereinafter, the compound (A) having a urethane group and a (meth)acryloyl group may be simply referred to as compound (A).

[0034] The compound (A) is not particularly limited. The compound (A) can be produced, for example, by any method. For example, the compound (A) can be produced by a urethane reaction between an isocyanate compound (a1) and an active hydrogen group-containing (meth)acrylate (a2). That is, the compound (A) preferably contains a reaction product of the isocyanate compound (a1) and the active hydrogen group-containing (meth)acrylate (a2), and more preferably is a reaction product of the isocyanate compound (a1) and the active hydrogen group-containing (meth)acrylate (a2).

[0035] (1) Isocyanate Compound (a1) The isocyanate compound (a1) is an organic compound having one or more isocyanate groups in the molecule. The isocyanate compound (a1) is preferably an organic compound (polyisocyanate) having two or more isocyanate groups in the molecule. Examples of the isocyanate compound (a1) include polyisocyanate monomers, polyisocyanate derivatives, and isocyanate-terminated prepolymers. These can be used alone or in combination of two or more types.

[0036] Examples of polyisocyanate monomers include linear aliphatic polyisocyanate monomers, alicyclic polyisocyanate monomers, aromatic polyisocyanate monomers, and araliphatic polyisocyanate monomers. Examples of linear aliphatic polyisocyanate monomers include linear aliphatic diisocyanates. Examples of linear aliphatic diisocyanates include ethylene diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate (PDI), and hexamethylene diisocyanate (HDI). Examples of alicyclic polyisocyanate monomers include alicyclic diisocyanates. Examples of alicyclic diisocyanates include cyclohexane diisocyanate, bis(isocyanatomethyl)cyclohexane (HDI), and bis(isocyanatomethyl)cyclohexane (HDI). 6 XDI), isophorone diisocyanate (IPDI), norbornene diisocyanate (NBDI), and methylenebis(cyclohexyl isocyanate) (H 12 Examples of aromatic polyisocyanate monomers include aromatic diisocyanates. Examples of aromatic diisocyanates include diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), toluidine diisocyanate (TODI), paraphenylene diisocyanate, and naphthalene diisocyanate (NDI). Examples of araliphatic polyisocyanate monomers include araliphatic diisocyanates. Examples of araliphatic diisocyanates include xylylene diisocyanate (XDI) and tetramethylxylylene diisocyanate (TMXDI). These can be used alone or in combination of two or more types.

[0037] Examples of polyisocyanate derivatives include modified products obtained by modifying the above polyisocyanate monomers using known methods. More specifically, examples of polyisocyanate derivatives include polymers, isocyanurate modified products, allophanate modified products, polyol modified products, biuret modified products, urea modified products, oxadiazinetrione modified products, and carbodiimide modified products. Polyisocyanate derivatives also include polymethylene polyphenylene polyisocyanate. These can be used alone or in combination of two or more types.

[0038] The isocyanate group-terminated prepolymer is synthesized, for example, by reacting a known polyisocyanate component with a known active hydrogen group-containing component in a predetermined ratio.

[0039] Examples of the polyisocyanate component include the above-mentioned polyisocyanate monomers and / or polyisocyanate derivatives. The polyisocyanate component is preferably a polyisocyanate monomer.

[0040] The active hydrogen group-containing component is an organic compound having one or more active hydrogen groups in its molecule. Examples of the active hydrogen group include a hydroxyl group, a mercapto group, and an amino group. More specifically, the active hydrogen group-containing component includes a hydroxyl group-containing compound, a mercapto group-containing compound, and an amino group-containing compound. From the viewpoint of improving the mechanical strength of the cured resin (described below), an organic compound having two or more active hydrogen groups in its molecule is preferably used as the active hydrogen group-containing component. Furthermore, from the viewpoint of adjusting the hardness of the cured resin (described below), an organic compound having one active hydrogen group in its molecule may be used as the active hydrogen group-containing component.

[0041] The hydroxyl group-containing compound is an organic compound having one or more hydroxyl groups in the molecule. Examples of the hydroxyl group-containing compound include polyol compounds. Examples of the polyol compound include low-molecular-weight polyols and high-molecular-weight polyols. Examples of the low-molecular-weight polyols include ethylene glycol and trimethylolpropane. Examples of the high-molecular-weight polyols include polyether polyols (e.g., polyoxyethylene polyols, polyoxypropylene polyols, and polytetramethylene ether polyols), polyester polyols, polycarbonate polyols, polyurethane polyols, epoxy polyols, vegetable oil polyols, polyolefin polyols, acrylic polyols, and vinyl monomer-modified polyols. These compounds can be used alone or in combination of two or more.

[0042] The mercapto group-containing compound is an organic compound having one or more mercapto groups in the molecule. Examples of the mercapto group-containing compound include aliphatic mercaptan compounds, aromatic mercaptan compounds, aliphatic polythiol compounds, aromatic polythiol compounds, aliphatic polythiol compounds containing sulfur atoms other than mercapto groups, aromatic polythiol compounds containing sulfur atoms other than mercapto groups, aliphatic polythiol compounds containing sulfur atoms and ester bonds other than mercapto groups, heterocyclic compounds containing sulfur atoms other than mercapto groups, mercapto group-containing compounds containing hydroxyl groups, compounds having a dithioacetal or dithioketal skeleton, compounds having an orthocarboxylic acid trithioester skeleton, and compounds having an orthocarbonic acid tetrathioester skeleton. These compounds can be used alone or in combination of two or more.

[0043] Examples of aliphatic mercaptan compounds include 1,2,6,10,11-pentamercapto-4,8-dithiaundecane and 1,2,9,10-tetramercapto-6-mercaptomethyl-4,7-dithiadecane. Examples of aromatic mercaptan compounds include thiophenol and mercaptotoluene. Examples of aliphatic polythiol compounds include 1,1-methanedithiol, 1,2-ethanedithiol, 1,1-propanedithiol, and 1,2-propanedithiol. Examples of aromatic polythiol compounds include 1,2-dimercaptobenzene, 1,3-dimercaptobenzene, 1,4-dimercaptobenzene, 1,2-bis(mercaptomethyl)benzene, and 1,3-bis(mercaptomethyl)benzene. Aliphatic polythiol compounds containing sulfur atoms in addition to mercapto groups include, for example, bis(mercaptomethyl)sulfide, bis(mercaptoethyl)sulfide, bis(mercaptopropyl)sulfide, and bis(mercaptomethylthio)methane. Aromatic polythiol compounds containing sulfur atoms in addition to mercapto groups include, for example, 1,2-bis(mercaptoethylthio)benzene, 1,3-bis(mercaptoethylthio)benzene, 1,4-bis(mercaptoethylthio)benzene, and their nuclear alkylated derivatives. Examples of aliphatic polythiol compounds containing sulfur atoms and ester bonds in addition to mercapto groups include thioglycolic acid esters of aliphatic polythiol compounds containing sulfur atoms in addition to mercapto groups, mercaptopropionic acid esters of aliphatic polythiol compounds containing sulfur atoms in addition to mercapto groups, hydroxymethyl sulfide bis(2-mercaptoacetate), hydroxymethyl sulfide bis(3-mercaptopropionate), hydroxyethyl sulfide bis(2-mercaptoacetate), and hydroxyethyl sulfide bis(3-mercaptopropionate). Examples of heterocyclic compounds containing sulfur atoms in addition to mercapto groups include 3,4-thiophenedithiol and 2,5-dimercapto-1,3,4-thiadiazole.Examples of mercapto group-containing compounds containing hydroxyl groups include 2-mercaptoethanol, 3-mercapto-1,2-propanediol, glycerin di(mercaptoacetate), 1-hydroxy-4-mercaptocyclohexane, and 2,4-dimercaptophenol. Examples of compounds having a dithioacetal or dithioketal skeleton include 1,1,3,3-tetrakis(mercaptomethylthio)propane, 1,1,2,2-tetrakis(mercaptomethylthio)ethane, 4,6-bis(mercaptomethylthio)-1,3-dithiacyclohexane, and oligomers thereof. Examples of compounds having an orthocarboxylic acid trithioester skeleton include tris(mercaptomethylthio)methane, tris(mercaptoethylthio)methane, 1,1,5,5-tetrakis(mercaptomethylthio)-2,4-dithiapentane, and oligomers thereof. Examples of compounds having an orthocarbonate tetrathioester skeleton include 3,3'-di(mercaptomethylthio)-1,5-dimercapto-2,4-dithiapentane, 2,2'-di(mercaptomethylthio)-1,3-dithiacyclopentane, and oligomers thereof. These can be used alone or in combination of two or more types.

[0044] An amino group-containing compound is an organic compound having one or more amino groups in its molecule. Examples of amino group-containing compounds include polyamine compounds. Examples of polyamine compounds include ethylenediamine, 1,3-propanediamine, 1,3-butanediamine, 1,4-butanediamine, 1,6-hexamethylenediamine, 1,4-cyclohexanediamine, 3-aminomethyl-3,5,5-trimethylcyclohexylamine (isophoronediamine), 4,4'-dicyclohexylmethanediamine, 2,5-bis(aminomethyl)bicyclo[2.2.1]heptane, 2,6-bis(aminomethyl)bicyclo[2.2.1]heptane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, hydrazine, tolylenediamine, triethylenetetramine, and tetraethylenepentamine. These compounds can be used alone or in combination.

[0045] These may be used alone or in combination of two or more. As the active hydrogen group-containing component, preferably, a hydroxyl group-containing compound is used, more preferably, a polyol compound is used, still more preferably, a high molecular weight polyol is used, still more preferably, a polyether polyol is used, and particularly preferably, a polyoxypropylene polyol is used.

[0046] In the synthesis of the isocyanate group-terminated prepolymer, the polyisocyanate component and the active hydrogen group-containing component are blended in a predetermined ratio. More specifically, the equivalent ratio of the isocyanate groups in the polyisocyanate component to the active hydrogen groups of the active hydrogen group-containing component (isocyanate group / active hydrogen group) is, for example, more than 1, preferably 1.1 or more, more preferably 3 or more, and even more preferably 6 or more. Furthermore, the equivalent ratio of the isocyanate groups in the polyisocyanate component to the active hydrogen groups of the active hydrogen group-containing component (isocyanate group / active hydrogen group) is, for example, 20 or less, preferably 15 or less, and more preferably 10 or less.

[0047] A known polymerization method is used for the urethane reaction between the polyisocyanate component and the active hydrogen group-containing component. Examples of the polymerization method include bulk polymerization and solution polymerization. In bulk polymerization, for example, the above components are blended under a nitrogen atmosphere and reacted at a reaction temperature of 75 to 85°C for about 1 to 20 hours. In solution polymerization, for example, the above components are added to a known organic solvent under a nitrogen atmosphere and reacted at a reaction temperature of 20 to 80°C for about 1 to 20 hours.

[0048] In addition, a known urethane catalyst is added to the polymerization reaction as needed. After the reaction is completed, unreacted polyisocyanate components are removed by a known method as needed. This results in an isocyanate-terminated prepolymer.

[0049] The average functionality of the isocyanate groups in the isocyanate group-terminated prepolymer is, for example, 1.5 or more, or preferably 2.0 or more. The average functionality of the isocyanate groups in the isocyanate group-terminated prepolymer is, for example, 3.0 or less, or preferably 2.5 or less.

[0050] Furthermore, the above reaction produces a composition containing an isocyanate-terminated prepolymer and an unreacted polyisocyanate component (hereinafter referred to as a crude prepolymer product).

[0051] The isocyanate group concentration of the crude prepolymer product is, relative to the total amount (solid content) of the crude prepolymer product, for example, 0.3 mass% or more, preferably 0.5 mass% or more, more preferably 1.0 mass% or more, and for example, 15 mass% or less, preferably 12 mass% or less, more preferably 10 mass% or less.

[0052] The crude prepolymer product is preferably purified by distillation, which removes low molecular weight impurities and improves the heat resistance of the cured resin (described below).

[0053] The distillation method is not particularly limited, and examples thereof include batch distillation and continuous distillation. Examples of continuous distillation include thin film distillation (Smith thin film distillation). A preferred distillation method is thin film distillation (Smith thin film distillation).

[0054] The distillation conditions are set depending on the purpose and application. The distillation temperature is, for example, 120°C or higher, preferably 150°C or higher. The distillation temperature is, for example, 250°C or lower, preferably 200°C or lower. The distillation pressure (absolute pressure) is, for example, 1 Pa or higher, preferably 10 Pa or higher, more preferably 50 Pa or higher. The distillation pressure is, for example, 300 Pa or lower, preferably 200 Pa or lower, more preferably 100 Pa or lower.

[0055] The feed rate of the crude prepolymer product is, for example, 0.1 g / min or more, preferably 1.0 g / min or more, more preferably 2.0 g / min or more, and for example, 100 g / min or less, preferably 50 g / min or less, more preferably 10 g / min or less.

[0056] This removes the unreacted polyisocyanate component from the crude prepolymer product, yielding a purified isocyanate-terminated prepolymer (hereinafter referred to as "purified prepolymer"). The purified prepolymer consists of an isocyanate-terminated prepolymer or an isocyanate-terminated prepolymer and a trace amount (10,000 ppm or less) of unreacted polyisocyanate component.

[0057] In the purified prepolymer, the content of the isocyanate group-terminated prepolymer relative to the total amount of the purified prepolymer is, for example, 99.5 mass % or more, preferably 99.9 mass % or more, and for example, 100 mass % or less.

[0058] When an unreacted polyisocyanate component is contained, the content thereof is, for example, 0.0001% by mass or more, preferably 0.0005% by mass or more, based on the total amount (solid content) of the purified prepolymer product, and for example, 0.020% by mass or less, preferably 0.013% by mass or less, more preferably 0.010% by mass or less, based on the total amount (solid content) of the purified prepolymer product.

[0059] The isocyanate compound (a1) can be used alone or in combination of two or more kinds. As the isocyanate compound (a1), preferably, an isocyanate group-terminated prepolymer is used.

[0060] Furthermore, in order to facilitate phase separation in the cured resin product described below, the isocyanate compound (a1) preferably has an alicyclic structure. The alicyclic structure preferably has a chair conformation. That is, the isocyanate compound (a1) preferably has a chair alicyclic structure (hereinafter referred to as a chair alicyclic structure). The chair alicyclic structure is an alicyclic structure in which all bond angles constituting the alicyclic structure are in the range of 107 to 111°.

[0061] Examples of the isocyanate compound (a1) having a chair alicyclic structure include a polyisocyanate monomer having a chair alicyclic structure, a polyisocyanate derivative having a chair alicyclic structure, and an isocyanate group-terminated prepolymer having a chair alicyclic structure.

[0062] Examples of polyisocyanate monomers having a chair-type alicyclic structure include cyclohexane diisocyanate and bis(isocyanatomethyl)cyclohexane (H 6 XDI), and isophorone diisocyanate (IPDI), and preferably bis(isocyanatomethyl)cyclohexane (H 6 XDI). Examples of the polyisocyanate derivative having a chair alicyclic structure include derivatives of the polyisocyanate monomer having the chair alicyclic structure. Examples of the isocyanate group-terminated prepolymer having a chair alicyclic structure include isocyanate group-terminated prepolymers obtained using the polyisocyanate monomer having a chair alicyclic structure and / or the polyisocyanate derivative having a chair alicyclic structure. Particularly preferred examples of the isocyanate compound (a1) include isocyanate group-terminated prepolymers having a chair alicyclic structure.

[0063] (2) Active hydrogen group-containing (meth)acrylate (a2) The active hydrogen group-containing (meth)acrylate (a2) is an organic compound having one or more (meth)acroyl groups and one or more active hydrogen groups in the molecule. Examples of the active hydrogen group-containing (meth)acrylate (a2) include hydroxyl group-containing (meth)acrylate, mercapto group-containing (meth)acrylate, and amino group-containing (meth)acrylate. These can be used alone or in combination of two or more. The active hydrogen group-containing (meth)acrylate (a2) is preferably a hydroxyl group-containing (meth)acrylate.

[0064] Examples of hydroxyl group-containing (meth)acrylates include monohydroxyl mono(meth)acrylate, polyhydroxyl mono(meth)acrylate, monohydroxyl poly(meth)acrylate, and polyhydroxyl poly(meth)acrylate. These can be used alone or in combination of two or more.

[0065] Monohydroxyl mono(meth)acrylate is a compound having one hydroxyl group and one (meth)acryloyl group per molecule. Examples of monohydroxyl mono(meth)acrylates include 2-hydroxyethyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, 4-hydroxybutyl(meth)acrylate, 2-hydroxybutyl(meth)acrylate, 2-phenoxypropyl(meth)acrylate, 4-hydroxycyclohexyl(meth)acrylate, 3-chloro-2-hydroxypropyl(meth)acrylate, 2-hydroxy-3-phenyloxypropyl(meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethylphthalate, 2-hydroxyalkyl(meth)acryloylphosphate, pentanediol mono(meth)acrylate, neopentyl glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate. These can be used alone or in combination of two or more.

[0066] Polyhydroxyl mono(meth)acrylate is a compound having multiple hydroxyl groups and one (meth)acryloyl group in one molecule. Examples of polyhydroxyl mono(meth)acrylate include trimethylolpropane mono(meth)acrylate, glycerin mono(meth)acrylate, and pentaerythritol mono(meth)acrylate. These can be used alone or in combination of two or more.

[0067] Monohydroxyl poly(meth)acrylate is a compound having one hydroxyl group and multiple (meth)acryloyl groups in one molecule. Examples of monohydroxyl poly(meth)acrylates include trimethylolpropane di(meth)acrylate, glycerin di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, and 2-hydroxy-3-(meth)acryloyloxypropyl (meth)acrylate. These can be used alone or in combination of two or more.

[0068] Polyhydroxyl poly(meth)acrylate is a compound having multiple hydroxyl groups and multiple (meth)acryloyl groups in one molecule. Examples of polyhydroxyl poly(meth)acrylate include pentaerythritol di(meth)acrylate, dipentaerythritol tri(meth)acrylate, and dipentaerythritol tetra(meth)acrylate. These can be used alone or in combination of two or more.

[0069] The active hydrogen group-containing (meth)acrylate (a2) can be used alone or in combination of two or more. As the active hydrogen group-containing (meth)acrylate (a2), preferably, a hydroxyl group-containing (meth)acrylate is used, more preferably, a monohydroxyl mono(meth)acrylate is used, still more preferably, a hydroxyalkyl (meth)acrylate is used, and particularly preferably, 2-hydroxyethyl (meth)acrylate is used.

[0070] (3) Synthesis of Compound (A) In the synthesis of compound (A), the isocyanate compound (a1) (preferably a purified prepolymer) and the active hydrogen group-containing (meth)acrylate (a2) (preferably a hydroxyl group-containing (meth)acrylate) are blended in a predetermined ratio. More specifically, the equivalent ratio of the isocyanate groups in the isocyanate compound (a1) to the active hydrogen groups in the active hydrogen group-containing (meth)acrylate (a2) (isocyanate group / active hydrogen group) is, for example, 0.7 or more, preferably 0.9 or more. Furthermore, the equivalent ratio of the isocyanate groups in the isocyanate compound (a1) to the active hydrogen groups in the active hydrogen group-containing (meth)acrylate (a2) (isocyanate group / active hydrogen group) is, for example, 1.5 or less, preferably 1.2 or less.

[0071] The reaction conditions for the urethane-forming reaction between the isocyanate compound (a1) (preferably a purified prepolymer) and the active hydrogen group-containing (meth)acrylate (a2) (preferably a hydroxyl group-containing (meth)acrylate) are not particularly limited. For example, the environmental conditions are, for example, an inert gas atmosphere. The reaction temperature is, for example, 40°C or higher, preferably 50°C or higher, and more preferably 60°C or higher. The reaction temperature is, for example, 120°C or lower, preferably 100°C or lower, and more preferably 80°C or lower. The reaction time is, for example, 0.5 hours or longer, preferably 1.0 hour or longer. The reaction time is, for example, 24 hours or shorter, preferably 10 hours or shorter.

[0072] In the polymerization reaction, a known urethane catalyst is added as needed. After the reaction is completed, the unreacted isocyanate compound (a1) and / or the active hydrogen group-containing (meth)acrylate (a2) are removed as needed by a known method.

[0073] As a result, the isocyanate group of the isocyanate compound (a1) and the active hydrogen group-containing (meth)acrylate (a2) undergo a urethane reaction to form a urethane group. The reaction product also has a (meth)acryloyl group derived from the active hydrogen group-containing (meth)acrylate (a2). That is, the above reaction produces a compound (A) having a urethane group and a (meth)acryloyl group.

[0074] (4) Commercially Available Products Compound (A) may be a commercially available product. Examples of commercially available products include urethane prepolymer manufactured by Kyoeisha Chemical Co., Ltd. and UV-curable urethane acrylate manufactured by Mitsubishi Chemical Corporation. Examples of urethane prepolymers manufactured by Kyoeisha Chemical Co., Ltd. include AH-600 (phenyl glycidyl ether acrylate hexamethylene diisocyanate urethane prepolymer), UA-306H (pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer), UA-306T (pentaerythritol triacrylate toluene diisocyanate urethane prepolymer), UA-306I (pentaerythritol triacrylate isophorone diisocyanate urethane prepolymer), UA-510H (dipentaerythritol pentaacrylate hexamethylene diisocyanate urethane prepolymer), UF-8001G (non-yellowing type oligourethane acrylate (high hardness, medium elongation)), and DAUA-167 (carboxylic acid-containing urethane acrylate oligomer). Examples of UV-curable urethane acrylates manufactured by Mitsubishi Chemical Corporation include UV-1700B, UV-6300B, UV-7550B, UV-7600B, UV-7605B, UV-7610B, UV-7620EA, UV-7630B, UV-7640B, and UV-7650B. These can be used alone or in combination of two or more types.

[0075] The compound (A) may be used alone or in combination of two or more. The content of the compound (A) in the resin composition will be described later.

[0076] [2] Epoxy group- and / or oxetanyl group-containing compound (B) The epoxy group- and / or oxetanyl group-containing compound (B) has one or more epoxy groups and / or oxetanyl groups in the molecule. Hereinafter, the epoxy group- and / or oxetanyl group-containing compound (B) may be simply referred to as compound (B).

[0077] Examples of compound (B) include epoxy group-containing compounds, oxetanyl group-containing compounds, and compounds containing both epoxy and oxetanyl groups. These can be used alone or in combination of two or more. Preferred examples of compound (B) include epoxy group-containing compounds and oxetanyl group-containing compounds.

[0078] (1) Epoxy Group-Containing Compound An epoxy group-containing compound (hereinafter referred to as an epoxy compound) is an organic compound that has one or more epoxy groups in the molecule and does not have an oxetanyl group. Examples of epoxy compounds include aromatic epoxy compounds, aliphatic epoxy compounds, and alicyclic epoxy compounds. These can be used alone or in combination of two or more types.

[0079] Examples of aromatic epoxy compounds include bisphenol-type epoxy compounds, naphthalene-type epoxy compounds, novolac-type epoxy compounds, halogenated epoxy compounds, and other polyfunctional aromatic epoxy compounds. Examples of bisphenol-type epoxy compounds include butyl glycidyl ether, phenyl glycidyl ether, bisphenol A-type epoxy compounds, bisphenol F-type epoxy compounds, bisphenol AD-type epoxy compounds, and bisphenol S-type epoxy compounds. Examples of naphthalene-type epoxy compounds include 1,1-bis(2,7-diglycidyloxy-1-naphthyl)alkane. Examples of novolac-type epoxy compounds include phenol novolac-type epoxy compounds and cresol novolac-type epoxy compounds. Examples of halogenated epoxy compounds include brominated epoxy compounds (tetrabromobisphenol A diglycidyl ether and brominated bisphenol). Examples of other polyfunctional epoxy compounds include glycidyl ethers of tetra(hydroxyphenyl)alkanes, glycidyl ethers of tetrahydroxybenzophenone, and epoxidized polyvinylphenol. These can be used alone or in combination of two or more.

[0080] Furthermore, examples of aromatic epoxy compounds include commercially available aromatic epoxy compounds. Examples of commercially available aromatic epoxy compounds include the EPICLON series manufactured by DIC Corporation and the OGSOL series manufactured by Osaka Gas Chemicals Co., Ltd. Examples of the EPICLON series manufactured by DIC Corporation include EPICLON 850 (bisphenol A type epoxy compound), EPICLON 850-S (bisphenol A type epoxy compound), EXA-850CPR (bisphenol A type epoxy compound), EPICLON 830-S (bisphenol F type epoxy compound), EXA-830LVP (bisphenol F type epoxy compound), HP-4032D (naphthalene type epoxy compound), and HP-7200 (aromatic ring-containing dicyclopentasiloxane). Examples of epoxy resins that can be used include N-740 (phenol novolac epoxy compound), N-770 (phenol novolac epoxy compound), N-660 (cresol novolac epoxy compound), N-670 (cresol novolac epoxy compound), N-655-EXP-S (cresol novolac epoxy compound), and EXA-4850 (flexible and tough epoxy resin). Examples of the OGSOL series manufactured by Osaka Gas Chemicals Co., Ltd. include PG-100 (fluorene epoxy compound) and CG-500 (fluorene epoxy compound). These can be used alone or in combination of two or more types.

[0081] Examples of aliphatic epoxy compounds include polyglycidyl ethers of polyhydric alcohols or alkylene oxide adducts thereof. Examples of polyglycidyl ethers of polyhydric alcohols or alkylene oxide adducts thereof include ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, 1,9-nonanediol diglycidyl ether, 1,12-dodecanediol diglycidyl ether, glycerin triglycidyl ether, trimethylolpropane triglycidyl ether, and polyethylene glycol diglycidyl ether.

[0082] Examples of the aliphatic epoxy compound include commercially available aliphatic epoxy compounds, such as Epolite 100MF (trimethylolpropane triglycidyl ether) manufactured by Kyoeisha Chemical Co., Ltd. These compounds can be used alone or in combination of two or more.

[0083] Examples of alicyclic epoxy compounds include hydrogenated products of the above-mentioned aromatic epoxy compounds (e.g., hydrogenated bisphenol A-type epoxy compounds). Examples of alicyclic epoxy compounds include cyclohexane-type epoxy compounds, cyclohexyl methyl ester-type epoxy compounds, cyclohexyl methyl ether-type epoxy compounds, spiro-type epoxy compounds, and tricyclodecane-type epoxy compounds. More specific examples of alicyclic epoxy compounds include 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate, 1,2:8,9-diepoxylimonene, 1,2-epoxy-4-vinylcyclohexane, and 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol. These compounds can be used alone or in combination of two or more.

[0084] Examples of the alicyclic epoxy compound include commercially available alicyclic epoxy compounds. Examples of commercially available alicyclic epoxy compounds include KRM-2408 (hydrogenated bisphenol A epoxy compound) manufactured by ADEKA Corporation, YX-8034 (hydrogenated bisphenol A epoxy compound) manufactured by JER Corporation, and EHPE3150 (1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol) manufactured by Daicel Corporation. These can be used alone or in combination of two or more types.

[0085] In addition to the above, examples of epoxy compounds include heterocyclic epoxy compounds, glycidyl ether epoxy compounds, glycidyl ester epoxy compounds, glycidylamine epoxy compounds, rubber-modified epoxy compounds, urethane-modified epoxy compounds, epoxidized polybutadiene, epoxidized styrene-butadiene-styrene block copolymers, epoxy group-containing polyester compounds, epoxy group-containing polyurethane compounds, epoxy group-containing acrylic compounds, partially acrylated epoxy compounds, and epoxy-modified silicones. Commercially available epoxy compounds include the KF series manufactured by Shin-Etsu Chemical Co., Ltd. Examples of the KF series manufactured by Shin-Etsu Chemical Co., Ltd. include KF-101 (epoxy-modified silicone), KF-102 (epoxy-modified silicone), KF-1002 (epoxy-modified silicone), and KF-1005 (epoxy-modified silicone). These compounds can be used alone or in combination of two or more.

[0086] (2) Oxetanyl Group-Containing Compounds An oxetanyl group-containing compound (hereinafter referred to as an oxetanyl compound) is an organic compound that has one or more oxetanyl groups in the molecule and does not have an epoxy group. Examples of oxetanyl compounds include 3-ethyl-3-hydroxymethyloxetane (oxetane alcohol, 2-ethylhexyloxetane, xylylene bisoxetane, 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane, oxetanyl silsesquioxane, silsesquioxane, phenol novolac oxetane, 3-ethyl-3-phenoxymethyloxetane, and 3-ethyl-3-allyloxymethyloxetane. These compounds can be used alone or in combination of two or more.

[0087] Examples of the oxetanyl compound include commercially available oxetanyl compounds, such as those manufactured by Toagosei Co., Ltd. Examples of oxetanyl compounds available from Toagosei Co., Ltd. include OXT-101 (3-ethyl-3-hydroxymethyloxetane (oxetane alcohol)), OXT-212 (2-ethylhexyloxetane), OXT-121 (xylylene bisoxetane), OXT-221 (3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane), OXT-191 (oxetanyl silsesquioxetane), OX-SQ SI20 (silsesquioxane), PHOX (phenol novolac oxetane), OXT-211 (3-ethyl-3-phenoxymethyloxetane), and OXT-212 (2-ethylhexyloxetane). Furthermore, commercially available oxetanyl compounds include, for example, AL-EOX (3-ethyl-3-allyloxymethyloxetane) manufactured by Yokkaichi Synthetic Co., Ltd. These can be used alone or in combination of two or more kinds.

[0088] The compound (B) may be used alone or in combination of two or more. The compound (B) is preferably an epoxy group-containing compound, more preferably an aromatic epoxy compound or an alicyclic epoxy compound, and even more preferably a bisphenol A epoxy compound or a hydrogenated bisphenol A epoxy compound. That is, the compound (B) preferably contains an epoxy group-containing compound, more preferably an aromatic epoxy compound and / or an alicyclic epoxy compound, and even more preferably a bisphenol A epoxy compound and / or a hydrogenated bisphenol A epoxy compound. The content of the compound (B) in the resin composition will be described later.

[0089] [3] Radical Polymerization Initiator (C) The radical polymerization initiator (C) radically polymerizes, for example, the compound (A). Examples of the radical polymerization initiator (C) include a photopolymerization initiator and a thermal polymerization initiator. Hereinafter, the radical polymerization initiator (C) that is a photopolymerization initiator will be referred to as a photoradical polymerization initiator (C1). Furthermore, the radical polymerization initiator (C) that is a thermal polymerization initiator will be referred to as a thermal radical polymerization initiator (C2).

[0090] (1) Photoradical Polymerization Initiator (C1) Examples of the photoradical polymerization initiator (C1) include known photoradical polymerization initiators. More specifically, examples of the photoradical polymerization initiator (C1) include 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 1-hydroxycyclohexylphenyl-ketone, benzophenone, 2,2-dimethoxy-1,2-diphenylethan-1-one, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylethoxyphosphine oxide, 2-benzyl-2-dimethylamino-1-(4-methylbenzoyl)phenyl-2 ...-benzyl-2-dimethylamino-1-(4-methylbenzoyl)phenyl-2-propan-1-one, 1-hydroxycyclohexylphenyl-2-propan-1-one, 1-hydroxycyclohexylphenyl-2-propan-1-one, 1-hydroxycyclohexylphenyl-2-propan-1-one, 1-hydroxycyclohexylphenyl-2-propan-1-one, 1-hydroxycyclohexylphenyl-2-propan-1-one, 1-hydroxycyclohexylphenyl-2-propan-1-one, 1-hydroxycyclohexylphenyl-2-propan-1- 2-Methyl-1-[4-methylthio]phenyl]-2-morpholinophenyl)butanone-1,2-hydroxy-2-methyl-1-phenyl-propan-1-one, 2-methyl-1-[4-methylthio]phenyl]-2-morpholinopropan-1-one, benzoin methyl ether, benzoin ethyl ether, benzoin isobutyl ether, benzoin isopropyl ether, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2-hydroxy-2-methyl-[4-(1-methylvinyl)phenyl]propanol oligomer, 2-hydroxy- 2-methyl-[4-(1-methylvinyl)phenyl]propanol oligomer, 2-hydroxy-2-methyl-1-phenyl-1-propanone, isopropyl thioxanthone, methyl o-benzoylbenzoate, [4-(methylphenylthio)phenyl]phenylmethane, 2,4-diethyl thioxanthone, 2-chlorothioxanthone, benzophenone, ethyl anthraquinone, benzophenone ammonium salt, thioxanthone ammonium salt, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentane ethylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, 2,4,6-trimethylbenzophenone, 4-methylbenzophenone, 4,4'-bisdiethylaminobenzophenone, 1,4 dibenzoylbenzene, 10-butyl-2-chloroacridone, 2,2'-bis(o-chlorophenyl)4,5,4',5'-tetrakis(3,4,5-trimethoxyphenyl)1,2'-biimidazole, 2,2'-bis(o-chlorophenyl)4,5,4',Examples of the photopolymerization initiator (C1) include 5'-tetraphenyl-1,2'-biimidazole, 2-benzoylnaphthalene, 4-benzoylbiphenyl, 4-benzoyldiphenyl ether, acrylated benzophenone, bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, o-methylbenzoylbenzoate, p-dimethylaminobenzoic acid ethyl ester, p-dimethylaminobenzoic acid isoamyl ethyl ester, active tertiary amine, carbazole-phenone-based photopolymerization initiator, acridine-based photopolymerization initiator, triazine-based photopolymerization initiator, and benzoyl-based photopolymerization initiator. Examples of the photoradical polymerization initiator (C1) include commercially available photoradical polymerization initiators. Examples of commercially available photoradical polymerization initiators include those available from IGM Resins B.V. and Omnirad 819 (bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide) manufactured by Omnirad Chemical Industries, Ltd. These can be used alone or in combination of two or more types.

[0091] (2) Thermal Radical Polymerization Initiator (C2) Examples of the thermal radical polymerization initiator (C2) include known thermal radical polymerization initiators. More specifically, examples of the thermal radical polymerization initiator (C2) include organic peroxides. Examples of organic peroxides include benzoyl peroxide, ketone peroxide, peroxyketal, hydroperoxide, dialkyl peroxide, diacyl peroxide, peroxyester, t-butylperoxy-2-ethylhexanoate, and peroxydicarbonate. These can be used alone or in combination of two or more. In addition, a curing accelerator can be used together with the organic peroxide. Examples of the curing accelerator include naphthenic acid metal complex, dimethylaniline, quaternary ammonium salt, and phosphate ester. In addition, examples of the thermal radical polymerization initiator (C2) include commercially available thermal radical polymerization initiators. Examples of commercially available thermal radical polymerization initiators include the Percure series manufactured by NOF Corporation. An example of the Percure series manufactured by NOF Corp. is Percure O (t-butylperoxy-2-ethylhexanoate). These can be used alone or in combination of two or more types.

[0092] The radical polymerization initiator (C) may be used alone or in combination of two or more. The content of the radical polymerization initiator (C) in the resin composition will be described later.

[0093] The radical polymerization initiator (C) is used in combination with a radical source (e.g., benzopinacol) as needed. The mixing ratio of the radical polymerization initiator (C) and the radical source is appropriately set depending on the purpose and application.

[0094] [4] Cationic Polymerization Initiator (D) The cationic polymerization initiator (D) cationic polymerizes, for example, the compound (B). Examples of the cationic polymerization initiator (D) include a photopolymerization initiator and a thermal polymerization initiator. Hereinafter, the cationic polymerization initiator (D) that is a photopolymerization initiator will be referred to as a photocationic polymerization initiator (D1). Furthermore, the cationic polymerization initiator (D) that is a thermal polymerization initiator will be referred to as a thermal cationic polymerization initiator (D2).

[0095] (1) Photocationic Polymerization Initiator (D1) Examples of the photocationic polymerization initiator (D1) include known photocationic polymerization initiators. More specifically, examples of the photocationic polymerization initiator (D1) include iodonium salts. Examples of iodonium salts include diphenyliodonium hexafluoroarsenate, di(4-chlorophenyl)iodonium hexafluoroarsenate, di(4-bromophenyl)iodonium hexafluoroarsenate, phenyl(4-methoxyphenyl)iodonium hexafluoroarsenate, 4-methylphenyl-4-(1-methylethyl)phenyliodonium hexafluorophosphate, and 4-methylphenyl-4-(1-methylethyl)phenyliodonium trifluorophosphate. (pentafluoroethyl)trifluorophosphate, 4-methylphenyl-4-(1-methylethyl)phenyliodonium tetrakis(pentafluorophenyl)borate, 4-methylphenyl-4-(2-methylpropyl)phenyliodonium hexafluorophosphate, bis(C10-14-alkylphenyl)iodonium hexafluorophosphate, and 4-methylphenyl-4-(1-methylethyl)phenyliodonium hexafluoroantimonate. Examples of the photocationic polymerization initiator (D1) include commercially available iodonium salts. Examples of commercially available iodonium salts include IK-1 (4-methylphenyl-4-(1-methylethyl)phenyliodonium tri(pentafluoroethyl)trifluorophosphate) manufactured by San-Apro Co., Ltd., PI-2074 (4-methylphenyl-4-(1-methylethyl)phenyliodonium tetrakis(pentafluorophenyl)borate) manufactured by Rhodia, IRGACURE® 250 (4-methylphenyl-4-(2-methylpropyl)phenyliodonium hexafluorophosphate) manufactured by BASF, WPI-113 (bis(C10-14-alkylphenyl)iodonium hexafluorophosphate) manufactured by Wako Pure Chemical Industries, Ltd., and WPI-116 (4-methylphenyl-4-(1-methylethyl)phenyliodonium hexafluoroantimonate) manufactured by Wako Pure Chemical Industries, Ltd. These can be used alone or in combination of two or more types.These can be used alone or in combination of two or more.

[0096] (2) Thermal Cationic Polymerization Initiator (D2) Examples of the thermal cationic polymerization initiator (D2) include known thermal cationic polymerization initiators. More specifically, examples of the thermal cationic polymerization initiator (D2) include the TA series manufactured by San-Apro, the Adeka Opton series manufactured by ADEKA, the CI series manufactured by Nippon Soda, the CXC series manufactured by King Industries, and the San-Aid series manufactured by Sanshin Chemical Industry Co., Ltd. Examples of the TA series manufactured by San-Apro include TA-60, TA-60B, TA-100, and TA-120. Examples of the Adeka Opton series manufactured by ADEKA include Adeka Opton CP-77 and Adeka Opton CP-66. Examples of the CI series manufactured by Nippon Soda include CI-2639 and CI-2624. Examples of the CXC series manufactured by King Industries include CXC-1612 and CXC-1738. Examples of the San-Aid series manufactured by Sanshin Chemical Industry Co., Ltd. include San-Aid SI-45, San-Aid SI-60, San-Aid SI-80, San-Aid SI-100, San-Aid SI-110, San-Aid SI-110L, San-Aid SI-B3, San-Aid SI-B3A, and San-Aid SI-B4. These can be used alone or in combination of two or more types.

[0097] The cationic polymerization initiator (D) may be used alone or in combination of two or more. The content of the cationic polymerization initiator (D) in the resin composition will be described later.

[0098] [5] Additive (E) The resin composition may contain an additive (E) as an optional component within a range that does not impair the excellent effects of the present invention. Examples of the additive (E) include a photosensitizer, a filler, an antistatic agent, a coupling agent, a stabilizer, a surfactant, and a solvent.

[0099] (1) Photosensitizer Examples of photosensitizers include thioxanthone derivatives, carbonyl compounds, organic sulfur compounds, persulfides, redox compounds, azo compounds, diazo compounds, halogen compounds, and photoreducible dyes. These can be used alone or in combination of two or more. Preferably, thioxanthone derivatives are used. Examples of thioxanthone derivatives include isopropylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and thioxanthone ammonium. Preferably, 2,4-diethylthioxanthone is used. These can be used alone or in combination of two or more.

[0100] (2) Filler Examples of fillers include inorganic fillers and organic fillers. Inorganic fillers include carbon, metal oxides, sols, clay minerals, carbides, nitrides, borides, complex oxides, hydroxides, and salts. Examples of carbon include graphite, graphene, fullerene, acetylene black, and carbon nanotubes. Examples of metal oxides include silica, zirconia, beryllia, magnesium oxide, titania, and iron oxide. Examples of sols include colloidal silica, titania sol, and alumina sol. Examples of clay minerals include talc, kaolinite, and smectite. Examples of carbides include silicon carbide and titanium carbide. Examples of nitrides include silicon nitride, aluminum nitride, and titanium nitride. Examples of borides include boron nitride, titanium boride, and boron oxide. Examples of complex oxides include mullite. Examples of hydroxides include aluminum hydroxide, magnesium hydroxide, and iron hydroxide. Examples of salts include barium titanate, strontium carbonate, magnesium silicate, lithium silicate, sodium silicate, potassium silicate, lithium cobaltate, and olivine-type lithium iron phosphate. In addition to the above, inorganic fillers include glass. These can be used alone or in combination of two or more. Examples of organic fillers include acrylic resin, polyimide, and cellulose. These can be used alone or in combination of two or more.

[0101] The shape of the filler is not particularly limited, and examples thereof include powder, particles, fibers, and flakes. The filler may be used as a solid, a colloid, or a dispersion.

[0102] The average particle size of the filler is, for example, 0.005 μm or more, preferably 0.01 μm or more. The average particle size of the filler is, for example, 500 μm or less, preferably 100 μm or less. The average particle size is measured, for example, by a laser diffraction / scattering particle size distribution analyzer.

[0103] (3) Antistatic Agents Examples of antistatic agents include imidazolium salt derivatives, pyridinium salt derivatives, alkylammonium derivatives, phosphonium salt derivatives, and composite conductivity-imparting agents. Examples of imidazolium salt derivatives include 1,3-dimethylimidazolium methyl sulfate, 1-ethyl-3-methylimidazolium bis(pentafluoroethylsulfonyl)imide, and 1-ethyl-3-methylimidazolium bromide. Examples of pyridinium salt derivatives include 3-methyl-1-propylpyridinium bis(trifluoromethylsulfonyl)imide and 1-butyl-3-methylpyridinium bis(trifluoromethylsulfonyl)imide. Examples of alkylammonium derivatives include tetrabutylammonium heptadecafluorooctanesulfonate and tetraphenylammonium methanesulfonate. Examples of phosphonium salt derivatives include tetrabutylphosphonium methanesulfonate. An example of the composite conductivity-imparting agent is a composite of polyalkylene glycol and lithium perchlorate. These can be used alone or in combination of two or more kinds.

[0104] (4) Coupling Agent Examples of the coupling agent include silane coupling agents and titanium coupling agents. Examples of the silane coupling agent include vinyltrimethoxysilane, vinyltriethoxysilane, γ-chloropropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, γ-glycidoxypropyltrimethoxysilane, β-glycidoxypropylmethyldimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-mercaptopropyltrimethoxysilane, cyanohydrin silyl ether, and tridecafluoro-1,1,2,2-tetrahydrooctyl)triethoxysilane.Examples of titanium coupling agents include triethanolamine titanate, titanium acetylacetonate, titanium ethylacetoacetate, titanium lactate, titanium lactate ammonium salt, tetrastearyl titanate, isopropyl tricumylphenyl titanate, isopropyl tri(N-aminoethyl-aminoethyl) titanate, dicumylphenyloxyacetate titanate, isopropyl trioctanol titanate, isopropyl dimethacryisostearoyl titanate, titanium lactate ethyl ester, octylene glycol titanate, isopropyl triisostearoyl titanate, triisostearyl isopropyl titanate, isopropyl tridodecylbenzenesulfonyl titanate, tetra(2 bis(dioctylpyrophosphate)titanate, tetraisopropylbis(dioctylphosphate)titanate, tetraoctylbis(ditridecylphosphite)titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(di-tridecyl)phosphite titanate, bis(dioctylpyrophosphate)oxyacetate titanate, bis(dioctylpyrophosphate)ethylene titanate, tetra-i-propyl titanate, tetra-n-butyl titanate, and diisostearoylethylene titanate. These may be used alone or in combination of two or more.

[0105] (5) Stabilizers Examples of stabilizers include antioxidants, decomposers, and light stabilizers. Examples of antioxidants include phenolic antioxidants and aromatic amine antioxidants. Examples of phenolic antioxidants include 2,6-di-t-butylphenol, 2,4-di-t-butylphenol, 2,6-di-t-butyl-4-ethylphenol, and 2,4-bis-(N-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine. Examples of aromatic amine antioxidants include alkyldiphenylamines, N,N'-diphenyl-p-phenylenediamine, 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline, and N-phenyl-N'-isopropyl-p-phenylenediamine. Examples of decomposers include sulfide-based hydroperoxide decomposers and phosphorus-based hydroperoxide decomposers. Examples of sulfide-based hydroperoxide decomposers include dilauryl-3,3'-thiodipropionate, ditridecyl-3,3'-thiodipropionate, bis[2-methyl-4-{3-N-alkylthiopropionyloxy}-5-t-butylphenyl]sulfide, and 2-mercapto-5-methylbenzimidazole. Examples of phosphorus-based hydroperoxide decomposers include tris(isodecyl)phosphite, phenyldiisooctylphosphite, diphenylisooctylphosphite, di(nonylphenyl)pentaerythritol diphosphite, 3,5-di-t-butyl-4-hydroxybenzylphosphate diethyl ester, and sodium bis(4-t-butylphenyl)phosphate. Examples of light stabilizers include salicylate-based light stabilizers, benzophenone-based light stabilizers, benzotriazole-based light stabilizers, hindered amine-based light stabilizers, and nickel-based light stabilizers. Examples of salicylate-based light stabilizers include phenyl salicylate and 4-t-octylphenyl salicylate. Examples of benzophenone-based light stabilizers include 2,4-dihydroxybenzophenone and 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid.Examples of benzotriazole-based light stabilizers include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole and 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2N-benzotriazol-2-yl)phenol]. Examples of hindered amine-based light stabilizers include phenyl-4-piperidinyl carbonate and bis-[2,2,6,6-tetramethyl-4-piperidinyl] sebacate. Examples of nickel-based light stabilizers include [2,2'-thio-bis(4-t-octylphenolate)]-2-ethylhexylamine-nickel(II). Further examples of light stabilizers include cyanoacrylate-based light stabilizers, oxalic acid anilide-based light stabilizers, and fullerene-based light stabilizers. These can be used alone or in combination of two or more.

[0106] (6) Surfactants Examples of surfactants include anionic surfactants, amphoteric surfactants, and nonionic surfactants. Examples of anionic surfactants include soap, lauryl sulfate, polyoxyethylene alkyl ether sulfate, alkylbenzene sulfonate (e.g., dodecylbenzene sulfonate), polyoxyethylene alkyl ether phosphate, polyoxyethylene alkyl phenyl ether phosphate, N-acylamino acid salt, α-olefin sulfonate, alkyl sulfate ester salt, alkyl phenyl ether sulfate ester salt, methyl taurate, trifluoromethanesulfonate, pentafluoroethanesulfonate, heptafluoropropanesulfonate, and nonafluorobutanesulfonate. Examples of counter cations include sodium ions and lithium ions. Examples of amphoteric surfactants include alkyldiaminoethylglycine hydrochloride, 2-alkyl-N-carboxymethyl-N-hydroxyethylimidazolinium betaine, lauryldimethylaminoacetic acid betaine, coconut oil fatty acid amidopropyl betaine, fatty acid alkyl betaine, sulfobetaine, and amine oxide. Examples of nonionic surfactants include polyethylene glycol alkyl ester compounds, alkyl ether compounds, ester compounds, alkylphenol compounds, fluorine compounds, and silicone compounds. These can be used alone or in combination of two or more types.

[0107] (7) Solvents Examples of solvents include water, organic solvents, and inorganic solvents. Examples of organic solvents include hydrocarbons, halogenated hydrocarbons, alcohols, ethers, esters, polyhydric alcohols, fatty acids, phenols, and nitrogen compounds. Examples of hydrocarbons include propane, n-butane, n-pentane, isohexane, cyclohexane, n-octane, isooctane, benzene, toluene, xylene, ethylbenzene, amylbenzene, turpentine, and pinene. Examples of halogenated hydrocarbons include methyl chloride, chloroform, carbon tetrachloride, ethylene chloride, methyl bromide, ethyl bromide, chlorobenzene, chlorobromomethane, bromobenzene, fluorodichloromethane, dichlorodifluoromethane, and difluorochloroethane. Examples of alcohols (monohydric alcohols) include methanol, ethanol, 1-propanol, isopropanol, 1-butanol, 1-pentanol, isoamyl alcohol, 1-hexanol, 1-heptanol, 1-octanol, 2-octanol, 1-dodecanol, nonanol, cyclohexanol, and glycidol. Examples of ethers include diethyl ether, dichlorodiethyl ether, diisopropyl ether, dibutyl ether, diisoamyl ether, methyl phenyl ether, ethyl benzyl ether), furans (tetrahydrofuran, furfural, 2-methylfuran, cineole, methylal), ketones (acetone, methyl ethyl ketone, methyl-N-propyl ketone, methyl-N-amyl ketone, diisobutyl ketone, phorone, isophorone, cyclohexanone, and acetophenone. Examples of esters include methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, n-amyl acetate, cyclohexanemethyl acetate, methyl butyrate, ethyl butyrate, propyl butyrate, butyl stearate, propylene carbonate, diethyl carbonate, ethylene carbonate, and vinylene carbonate.Examples of polyhydric alcohols include ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether, methoxymethoxyethanol, ethylene glycol monoacetate, diethylene glycol, diethylene glycol monomethyl ether, propylene glycol, propylene glycol monoethyl ether, and 2-(2-butoxyethoxy)ethanol. Examples of fatty acids include formic acid, acetic acid, acetic anhydride, propionic acid, propionic anhydride, butyric acid, and isovaleric acid. Examples of phenols include phenol, cresol, o-cresol, and xylenol. Examples of nitrogen compounds include nitromethane, nitroethane, 1-nitropropane, nitrobenzene, monomethylamine, dimethylamine, trimethylamine, monoethylamine, diamylamine, aniline, monomethylaniline, o-toluidine, o-chloroaniline, dicyclohexylamine, dicyclohexylamine, monoethanolamine, formamide, N,N-dimethylformamide, acetamide, acetonitrile, pyridine, α-picoline, 2,4-lutidine, quinoline, and morpholine. In addition to the above, examples of organic solvents include carbon disulfide, dimethyl sulfoxide, 4,4-diethyl-1,2-dithiolane, dimethyl sulfide, dimethyl disulfide, methanethiol, propane sultone, triethyl phosphate, triphenyl phosphate, diethyl carbonate, ethylene carbonate, silicone oil, and amyl borate. Examples of inorganic solvents include liquid ammonia, sulfur, and phosphorus. These can be used alone or in combination.

[0108] The additive (E) can be used alone or in combination of two or more kinds. The blending ratio and blending timing of the additive (E) are appropriately set depending on the purpose and application.

[0109] [6] Method for Producing Resin Composition To produce a resin composition, first, the compound (A), the compound (B), the radical polymerization initiator (C), and the cationic polymerization initiator (D) are selected, and then these are blended together.

[0110] (1) Selection of Compound (A) and Compound (B) Compound (A) and compound (B) are selected so that they are phase-separated from each other in the resin composition. More specifically, compound (A) and compound (B) are selected based on the surface tension γ.

[0111] The surface tension γA of the compound (A) is, for example, 20 mN / m or more, preferably 25 mN / m or more, more preferably 40 mN / m or more, even more preferably 45 mN / m or more, and particularly preferably 50 mN / m or more. Furthermore, the surface tension γA of the compound (A) is, for example, 70 mN / m or less, preferably 65 mN / m or less. From these viewpoints, the surface tension γA of the compound (A) is, for example, 20 mN / m or more and 70 mN / m or less, preferably 40 mN / m or more and 70 mN / m or less, more preferably 45 mN / m or more and 70 mN / m or less, and even more preferably 50 mN / m or more and 65 mN / m or less.

[0112] When two or more types of compounds (A) are used in combination, the surface tension γA of the compounds (A) indicates the surface tension γ of the mixture of the compounds (A).

[0113] The surface tension γ of compound (B) is smaller than the surface tension γ of compound (A). The surface tension γ of compound (B) is, for example, 10 mN / m or more, preferably 15 mN / m or more. The surface tension γ of compound (B) is, for example, 60 mN / m or less, preferably 55 mN / m or less.

[0114] When two or more types of compounds (B) are used in combination, the surface tension γ B of the compounds (B) indicates the surface tension γ of the mixture of the compounds (B).

[0115] The surface tension γ of compound (B) is 80% or less (4 / 5 or less), preferably 75% or less, more preferably 70% or less of the surface tension γ of compound (A). The surface tension γ of compound (B) is, for example, 50% or more, preferably 60% or more of the surface tension γ of compound (A).

[0116] The surface tension γ can be measured using a commercially available surface tension measuring device. Measurement methods include, for example, the Wilhelmy method, the ring method, the hanging drop method, and the maximum bubble pressure method. The hanging drop method is preferred.

[0117] By selecting the compound (A) and the compound (B) based on the surface tension γ, it is possible to cause phase separation between the compound (A) and the compound (B) in the resin composition, and as a result, it is possible to cause phase separation into a cured product (α) of the compound (A) and a cured product (β) of the compound (B) in the cured resin.

[0118] The surface tension γ can be adjusted by introducing any substituent into compound (A) and / or compound (B). Examples of the substituent include hydrogen-bonding substituents. Examples of the hydrogen-bonding substituent include hydroxyl groups, mercapto groups, and amino groups. For example, when the hydrogen-bonding substituent of compound (A) and the hydrogen-bonding substituent of compound (B) are relatively close in value, the difference between the surface tension γA of compound (A) and the surface tension γB of compound (B) may be insufficient. In such cases, compound (A) and compound (B) may not be sufficiently phase-separated in the resin composition. As a result, the cured product (α) of compound (A) and the cured product (β) of compound (B) may not be sufficiently phase-separated in the cured resin. In such cases, hydrogen-bonding substituents can be introduced into compound (A) and / or compound (B) by known methods. In other words, the hydrogen-bonding substituent valence of compound (A) and the hydrogen-bonding substituent valence of compound (B) can be adjusted to be relatively far apart. This allows sufficient phase separation between the compound (A) and the compound (B) in the resin composition, and as a result, allows sufficient phase separation into a cured product (α) of the compound (A) and a cured product (β) of the compound (B) in the cured resin.

[0119] Specifically, the ratio of one hydrogen-bonding substituent valence to the other hydrogen-bonding substituent valence is, for example, 2 / 3 or less, preferably 1 / 2 or less. Furthermore, the ratio of one hydrogen-bonding substituent valence to the other hydrogen-bonding substituent valence is, for example, 1 / 100 or more, preferably 1 / 20 or more. That is, the ratio of one hydrogen-bonding substituent valence to the other hydrogen-bonding substituent valence is, for example, 1 / 100 or more to 2 / 3 or less, preferably 1 / 20 or more to 1 / 2 or less. The one hydrogen-bonding substituent valence indicates the higher hydrogen-bonding substituent valence of the hydrogen-bonding substituent of compound (A) and the hydrogen-bonding substituent valence of compound (B). The other hydrogen-bonding substituent valence indicates the lower hydrogen-bonding substituent valence of the hydrogen-bonding substituent of compound (A) and the hydrogen-bonding substituent valence of compound (B). That is, for example, when the hydrogen-bonding substituent valence of compound (A) is higher than the hydrogen-bonding substituent valence of compound (B), the ratio of one hydrogen-bonding substituent valence to the other hydrogen-bonding substituent valence indicates the hydrogen-bonding substituent valence of compound (B) relative to the hydrogen-bonding substituent valence of compound (A).

[0120] More specifically, the ratio of the hydrogen-bonding substituent valence of compound (B) to the hydrogen-bonding substituent valence of compound (A) is, for example, 2 / 3 or less, preferably 1 / 2 or less. Furthermore, the ratio of the hydrogen-bonding substituent valence of compound (B) to the hydrogen-bonding substituent valence of compound (A) is, for example, 1 / 100 or more, preferably 1 / 20 or more. That is, the ratio of the hydrogen-bonding substituent valence of compound (B) to the hydrogen-bonding substituent valence of compound (A) is, for example, 1 / 100 or more and 2 / 3 or less, preferably 1 / 20 or more and 1 / 2 or less.

[0121] More specifically, the hydrogen-bonding substituent valence of compound (A) is, for example, 0.000001 mol / g or more, preferably 0.000005 mol / g or more. Furthermore, the hydrogen-bonding substituent valence of compound (A) is, for example, 0.0741 mol / g or less, preferably 0.0667 mol / g or less. That is, the hydrogen-bonding substituent valence of compound (A) is, for example, 0.000001 mol / g or more and 0.0741 mol / g or less, preferably 0.000005 mol / g or more and 0.0667 mol / g or less.

[0122] The hydrogen-bonding substituent valence of compound (B) is, for example, 0.000001 mol / g or more, preferably 0.00005 mol / g or more. The hydrogen-bonding substituent valence of compound (B) is, for example, 0.1111 mol / g or less, preferably 0.1000 mol / g or less, more preferably 0.0011 mol / g or less, and even more preferably less than 0.0005 mol / g. That is, the hydrogen-bonding substituent valence of compound (B) is, for example, 0.000001 mol / g or more and 0.1111 mol / g or less, preferably 0.000001 mol / g or more and 0.0005 mol / g or less.

[0123] The hydrogen-bonding substituent value of a compound is the number of moles (mol) of hydrogen-bonding substituents in 1 g of the compound. The hydrogen-bonding substituent value is calculated, for example, from the amount of raw material and molecular structure of the compound.

[0124] For example, the hydrogen-bonding substituent value of a urethane acrylate is calculated from the amounts and molecular structures of polyisocyanate and polyol, which are raw materials for the urethane acrylate.

[0125] More specifically, the urethane acrylate is prepared by, for example, mixing a polyol having an average functionality of 2 with 1,3-bis(isocyanatomethyl)cyclohexane (hereinafter referred to as 1,3-H 6 In some cases, the polyol may be 10,000 g, the 1,3-bis(isocyanatomethyl)cyclohexane may be 388.46 g (2 mol), and the hydroxyethyl acrylate may be 232.24 g (2 mol).

[0126] In the above reaction, the mass of the resulting urethane acrylate is 10620.7 g (= 10000 g + 388.46 g + 232.24 g).

[0127] In addition, in the above reaction, one molecule of 1,3-H 6 HDI (i.e., two molecules of isocyanate group) undergoes urethane conversion, and two molecules of amino group (NH group) are generated as hydrogen-bonding functional groups. 6When HDI is urethane-converted, 4 mol of amino groups (NH groups) are generated as hydrogen-bonding functional groups.

[0128] That is, the hydrogen-bonding functional group value of the urethane acrylate is 0.000377 mol / g (=4 mol / 10620.7 g).

[0129] The hydrogen-bonding substituent value can also be calculated by gas chromatography.

[0130] That is, the object to be measured is hydrolyzed and subjected to gas chromatography to detect fragments corresponding to the hydrogen-bonding substituents. From the detection results, the hydrogen-bonding substituent value can be calculated.

[0131] More specifically, when the object to be measured is, for example, a urethane acrylate, the urethane acrylate is hydrolyzed using an aqueous sodium hydroxide solution, and then the decomposition product is extracted using dicyclomethane and subjected to gas chromatography. Then, the hydrogen-bonding substituent value can be calculated by detecting fragments corresponding to the hydrogen-bonding substituent. Examples of objects to be measured that can be hydrolyzed using an aqueous sodium hydroxide solution include partial acrylate esters of epoxy resins in addition to urethane acrylates.

[0132] The compound (A) and the compound (B) are selected based on the peak temperature of tan δ of the cured product. Tan δ is the loss factor. The peak temperature of tan δ is the temperature corresponding to the peak top position of tan δ. Tan δ is measured by the following method.

[0133] That is, first, the dynamic viscoelasticity of the sample for measuring tan δ is measured to obtain a viscoelasticity spectrum. Then, the storage tensile modulus E' and loss tensile modulus E'' are determined from the viscoelasticity spectrum. The ratio of the loss tensile modulus E'' to the storage tensile modulus E' (E'' / E') is defined as tan δ. In a graph showing the relationship between temperature and tan δ, the point at which tan δ is highest is defined as the peak of tan δ, and the temperature corresponding to the top of this peak is defined as the peak temperature.

[0134] The measurement method complies with JIS K7244 (1998). A dumbbell test piece type A is used as the measurement sample. The measurement mode is tension mode. The measurement frequency is 10 Hz. The measurement temperature range is -100 to 250°C. The temperature rise rate is 5°C / min.

[0135] The compound (A) is cured (polymerized) by the radical polymerization initiator (C) to form a cured product (α) as a sole cured product. The cured product (α) forms a soft segment in the cured resin product.

[0136] The tan δ of the cured product (α) (hereinafter referred to as tan δ a The peak temperature Ta of the cured product (β) of the compound (B) can be calculated by, for example, the tan δ (hereinafter, tan δ b ) is lower than the peak temperature Tb.

[0137] More specifically, the tan δ of the cured product (α) of the compound (A) a The peak temperature Ta (peak temperature of tan δ of the single cured product) is, for example, less than 100°C, preferably 50°C or less, more preferably 30°C or less, even more preferably 0°C or less, and particularly preferably -10°C or less. a The peak temperature Ta (peak temperature of tan δ of the single cured product) is preferably relatively low. More specifically, the peak temperature Ta of tan δ of the cured product (α) of the compound (A) is preferably relatively low. a The peak temperature Ta (peak temperature of tan δ of the single cured product) is, for example, −50° C. or higher. When the peak temperature Ta is lower, the peak temperature Ta is −80° C. or higher. When the peak temperature Ta is even lower, the peak temperature Ta is −100° C. or higher. When the peak temperature Ta is even lower, the peak temperature Ta is −200° C. or higher. When the peak temperature Ta is especially low, the peak temperature Ta is −250° C. or higher.

[0138] On the other hand, the compound (B) is cured (polymerized) by the cationic polymerization initiator (D) to form a cured product (β) as a sole cured product, which forms hard segments in the cured resin product.

[0139] Tan δ of the cured product (β) b The peak temperature is the tan δ of the cured product (α) of the compound (A). a Higher than the peak temperature.

[0140] More specifically, the tan δ of the cured product (β) of the compound (B) b The peak temperature Tb (peak temperature of tan δ of the cured product (β) of the compound (B)) is, for example, 100° C. or higher, preferably 105° C. or higher, and more preferably 110° C. or higher. b The peak temperature Tb (peak temperature of tan δ of the single cured product) is preferably relatively high. More specifically, the peak temperature Tb of tan δ of the cured product (β) of the compound (B) is b The peak temperature Tb (peak temperature of tan δ of the single cured product) is, for example, 350°C or lower. If the peak temperature Tb is higher, the peak temperature Tb is 400°C or lower. If the peak temperature Tb is even higher, the peak temperature Tb is 450°C or lower.

[0141] In addition, the tan δ of the cured product (α) a and the peak temperature Ta of the cured product (β). b The difference between the peak temperature Tb and the cured product (α) of the compound (A) is, for example, 30° C. or more, preferably 50° C. or more, more preferably 80° C. or more, even more preferably 100° C. or more, and particularly preferably 120° C. or more. a and the peak temperature Ta of the cured product (β) of the compound (B). b The difference between the peak temperature Tb and the peak temperature Tc is, for example, 200° C. or less.

[0142] (2) Selection of Radical Polymerization Initiator (C) and Cationic Polymerization Initiator (D) The radical polymerization initiator (C) and the cationic polymerization initiator (D) are selected depending on the type of compound (A) and the type of compound (B), and the method for curing the resin composition (method for producing a cured resin product) described below.

[0143] For example, as will be described in detail later, when the resin composition is cured only by active energy rays, a photoradical polymerization initiator (C1) is selected as the radical polymerization initiator (C), and a photocationic polymerization initiator (D1) is selected as the cationic polymerization initiator (D).

[0144] Furthermore, although this will be described in detail later, for example, when the resin composition is cured only by heat, a thermal radical polymerization initiator (C2) is selected as the radical polymerization initiator (C), and a thermal cationic polymerization initiator (D2) is selected as the cationic polymerization initiator (D).

[0145] In addition, as will be described in detail later, for example, when the resin composition is cured by heat and active energy rays, a thermal radical polymerization initiator (C2) is selected as the radical polymerization initiator (C) and a photocationic polymerization initiator (D1) is selected as the cationic polymerization initiator (D). In addition, when the resin composition is cured by heat and active energy rays, for example, a photoradical polymerization initiator (C1) can be selected as the radical polymerization initiator (C) and a thermal cationic polymerization initiator (D2) can be selected as the cationic polymerization initiator (D).

[0146] (3) Mixing of Components The compound (A) and the compound (B) are mixed with the radical polymerization initiator (C) and the cationic polymerization initiator (D) by a known method, thereby obtaining a resin composition.

[0147] In the resin composition, the content ratio of the compound (A), the content ratio of the compound (B), the content ratio of the radical polymerization initiator (C), and the content ratio of the cationic polymerization initiator (D) are adjusted, for example, so that the tan δ of a cured product of the resin composition has the properties described below.

[0148] For example, the content of compound (A) is, for example, 1% by mass or more, preferably 5% by mass or more, based on the total amount of compound (A), compound (B), radical polymerization initiator (C), and cationic polymerization initiator (D). The content of compound (A) is, for example, 99% by mass or less, preferably 95% by mass or less, based on the total amount of compound (A), compound (B), radical polymerization initiator (C), and cationic polymerization initiator (D).

[0149] The content of compound (B) is, for example, 0.1% by mass or more, preferably 1% by mass or more, more preferably 10% by mass or more, and even more preferably 30% by mass or more, based on the total amount of compound (A), compound (B), radical polymerization initiator (C), and cationic polymerization initiator (D). The content of compound (B) is, for example, 99% by mass or less, preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less, based on the total amount of compound (A), compound (B), radical polymerization initiator (C), and cationic polymerization initiator (D).

[0150] The content of compound (B) is, for example, 0.1 parts by mass or more, preferably 1 part by mass or more, more preferably 10 parts by mass or more, and even more preferably 70 parts by mass or more, relative to 100 parts by mass of compound (A). The content of compound (B) is, for example, 99,900 parts by mass or less, preferably 9,900 parts by mass or less, more preferably 990 parts by mass or less, and even more preferably 400 parts by mass or less, relative to 100 parts by mass of compound (A).

[0151] The content of the radical polymerization initiator (C) is, for example, 0.01% by mass or more, preferably 0.5% by mass or more, based on the total amount of the compound (A), the compound (B), the radical polymerization initiator (C), and the cationic polymerization initiator (D). The content of the radical polymerization initiator (C) is, for example, 60% by mass or less, preferably 30% by mass or less, based on the total amount of the compound (A), the compound (B), the radical polymerization initiator (C), and the cationic polymerization initiator (D).

[0152] The content of the radical polymerization initiator (C) relative to 100 parts by mass of the compound (A) is, for example, 0.01 parts by mass or more, or preferably 0.5 parts by mass or more, and for example, 60 parts by mass or less, or preferably 30 parts by mass or less.

[0153] The content of the cationic polymerization initiator (D) is, for example, 0.01% by mass or more, preferably 0.05% by mass or more, based on the total amount of the compound (A), the compound (B), the radical polymerization initiator (C), and the cationic polymerization initiator (D). The content of the cationic polymerization initiator (D) is, for example, 60% by mass or less, preferably 30% by mass or less, based on the total amount of the compound (A), the compound (B), the radical polymerization initiator (C), and the cationic polymerization initiator (D).

[0154] The content of the cationic polymerization initiator (D) relative to 100 parts by mass of the compound (A) is, for example, 0.01 parts by mass or more, or preferably 0.05 parts by mass or more, and for example, 60 parts by mass or less, or preferably 30 parts by mass or less.

[0155] The content of the cationic polymerization initiator (D) relative to 100 parts by mass of the compound (B) is, for example, 0.01 parts by mass or more, preferably 0.05 parts by mass or more, and for example, 60 parts by mass or less, preferably 30 parts by mass or less.

[0156] Furthermore, for example, by adjusting the volume ratio of compound (A) and compound (B), the ratio of the soft segment (cured product (α)) to the hard segment (cured product (β)) in the cured resin product can be adjusted.

[0157] More specifically, to improve the flexibility and stretchability of the cured resin product, for example, a relatively large amount of compound (A) is added to the resin composition, and a relatively large amount of soft segments (cured product (α)) are added to the cured resin product. To improve the rigidity and low tackiness of the cured resin product, for example, a relatively large amount of compound (B) is added to the resin composition, and a relatively large amount of hard segments (cured product (β)) are added to the cured resin product.

[0158] From the viewpoint of obtaining a cured resin having both excellent elasticity and excellent low tackiness, for example, the volume of compound (A) relative to the total volume of compound (A) and compound (B) is, for example, 0.1 vol% or more, preferably 1 vol% or more. Furthermore, the volume of compound (A) relative to the total volume of compound (A) and compound (B) is, for example, 99.9 vol% or less, preferably 99 vol% or less. Furthermore, the volume of compound (B) relative to the total volume of compound (A) and compound (B) is, for example, 0.1 vol% or more, preferably 1 vol% or more. Furthermore, the volume of compound (B) relative to the total volume of compound (A) and compound (B) is, for example, 99.9 vol% or less, preferably 99 vol% or less.

[0159] The mixing method is not particularly limited. For example, a known stirring device can be used. Examples of stirring devices include a propeller mixer, a planetary mixer, a hybrid mixer, a kneader, an emulsifying homogenizer, a three-roll mill, a bead mill, and an ultrasonic homogenizer. The mixing conditions are not particularly limited. For example, the mixture may be mixed under heating or under cooling.

[0160] This allows the compound (A), the compound (B), the radical polymerization initiator (C), and the cationic polymerization initiator (D) to be mixed together, thereby obtaining a resin composition.

[0161] 2. Cured Resin [1] Method for Producing Cured Resin (Method for Curing Resin Composition) The cured resin includes, and preferably consists of, a cured product of the above-described resin composition. The resin composition is cured by heating and / or irradiation with active energy rays.

[0162] For example, when the resin composition contains a photoradical polymerization initiator (C1) as the radical polymerization initiator (C) and a photocationic polymerization initiator (D1) as the cationic polymerization initiator (D), the resin composition is cured only by irradiation with active energy rays.

[0163] Furthermore, for example, when the resin composition contains a thermal radical polymerization initiator (C2) as the radical polymerization initiator (C) and a thermal cationic polymerization initiator (D2) as the cationic polymerization initiator (D), the resin composition is cured by heating alone.

[0164] Furthermore, for example, when the resin composition contains a thermal radical polymerization initiator (C2) as the radical polymerization initiator (C) and a photocationic polymerization initiator (D1) as the cationic polymerization initiator (D), the resin composition is cured by irradiation with active energy rays and heating.

[0165] Furthermore, for example, when the resin composition contains a photoradical polymerization initiator (C1) as the radical polymerization initiator (C) and a thermal cationic polymerization initiator (D2) as the cationic polymerization initiator (D), the resin composition is cured by irradiation with active energy rays and heating.

[0166] When the resin composition is cured by heating, the heating method is not particularly limited. For example, a known heating device can be used. Examples of the heating device include a hot air generator, a hot plate, an oven, infrared rays, and a microwave. The heating conditions are not particularly limited. For example, the heating temperature is, for example, 30°C or higher and, for example, 70°C or lower. The heating time is, for example, 10 minutes or longer and, for example, 120 minutes or shorter.

[0167] Furthermore, when the resin composition is cured by irradiation with active energy rays, the method of irradiating the active energy rays is not particularly limited. For example, a known active energy ray irradiation device is used. Examples of active energy rays include ultraviolet rays, visible light, electron beams, X-rays, and radioactive rays, and ultraviolet rays are preferred. Furthermore, the irradiation conditions are not particularly limited. For example, the irradiation dose (cumulative light amount) is, for example, 100 mJ / cm. 2 More than 300 mJ / cm 2 The irradiation amount (integrated light amount) is, for example, 60,000 J / cm 2 Preferably, 30,000 mJ / cm or less 2 The following is the result.

[0168] When the resin composition is heated and / or irradiated with active energy rays, the compound (A) is polymerized (cured) by the radical polymerization initiator (C) to form a cured product (α). When the resin composition is heated and / or irradiated with active energy rays, the compound (B) is polymerized (cured) by the cationic polymerization initiator (D) to form a cured product (β). This results in a cured resin product containing the cured product (α) and the cured product (β).

[0169] The cured resin product may have any shape. For example, the cured resin product may have a three-dimensional shape or a sheet shape. Preferably, the cured resin product has a sheet shape. In other words, a resin sheet is preferably used as the cured resin product.

[0170] [2] Physical Properties of Cured Resin The cured resin includes, and preferably consists of, the cured resin composition described above. The cured resin includes a cured product (α) of compound (A) and a cured product (β) of compound (B).

[0171] In addition, in the cured resin product, the cured product (α) and the cured product (β) are phase-separated from each other. That is, the cured resin product contains a phase-separated composite of the cured product (α) and the cured product (β). In the phase-separated composite, the cured product (α) forms a soft segment, and the cured product (β) forms a hard segment.

[0172] Such a cured resin contains a phase-separated complex of the cured product (α) and the cured product (β), and therefore has at least two (preferably two) tan δ peaks in its viscoelasticity spectrum. More specifically, the tan δ peaks of the cured resin include a first peak derived from the cured product (α) and a second peak derived from the cured product (β).

[0173] The peak temperature T1 of the first peak is lower than the peak temperature T2 of the second peak. More specifically, from the viewpoint of stretchability, the peak temperature T1 of the first peak is less than 100°C, preferably 50°C or less, more preferably 30°C or less, even more preferably 0°C or less, and particularly preferably -10°C or less. The peak temperature T1 of the first peak is preferably relatively low. More specifically, the peak temperature T1 of the first peak is, for example, -50°C or higher. When the peak temperature T1 is lower, the peak temperature T1 is -80°C or higher. When the peak temperature T1 is even lower, the peak temperature T1 is -100°C or higher. When the peak temperature T1 is even lower, the peak temperature T1 is -200°C or higher. When the peak temperature T1 is particularly low, the peak temperature T1 is -250°C or higher.

[0174] The peak temperature T1 of the first peak is higher than the peak temperature T2 of the second peak. More specifically, from the viewpoint of low tackiness, the peak temperature T2 of the second peak is 100°C or higher, preferably 105°C or higher, and more preferably 110°C or higher. The peak temperature T2 of the second peak is preferably relatively high. More specifically, the peak temperature T2 of the second peak is, for example, 350°C or lower. If the peak temperature T2 is higher, the peak temperature T2 is 400°C or lower. If the peak temperature T2 is even higher, the peak temperature T2 is 450°C or lower.

[0175] The difference between the peak temperature T1 of the first peak and the peak temperature T2 of the second peak is 30° C. or more, preferably 50° C. or more, more preferably 80° C. or more, even more preferably 100° C. or more, and particularly preferably 120° C. or more. The difference between the peak temperature T1 of the first peak and the peak temperature T2 of the second peak is, for example, 200° C. or less, preferably 160° C. or less.

[0176] When the tan δ of the cured resin has the first and second peaks, the cured resin has an excellent phase-separated composite, and therefore the cured resin has both the stretchability derived from the cured product (α) of compound (A) and the low tackiness derived from the cured product (β) of compound (B).

[0177] [3] Timing of Curing In the resin composition, the timing of curing the compound (A) and the timing of curing the compound (B) are not particularly limited.

[0178] For example, the compound (A) can be cured and the compound (B) can be initiated at the same time by heating the resin composition and / or irradiating the resin composition with active energy rays.

[0179] Furthermore, for example, when the resin composition is heated and / or the resin composition is irradiated with active energy rays, the timing of curing (polymerization) of the compound (A) and the timing of curing (polymerization) of the compound (B) can be made different by adjusting the operation method.

[0180] From the viewpoint of promoting phase separation between the cured product (α) of the compound (A) and the cured product (β) of the compound (B), the timing of curing (polymerization) of the compound (A) and the timing of curing (polymerization) of the compound (B) are preferably made to differ from each other.

[0181] In such a case, it is preferable to initiate the curing (polymerization) of the compound (A) first, and then initiate the curing (polymerization) of the compound (B).

[0182] That is, radical polymerization (polymerization of compound (A)) is inhibited by oxygen, but cationic polymerization (polymerization of compound (B)) is not inhibited by oxygen. Therefore, when compound (A) and compound (B) are cured in the above order, phase separation between a cured product (α) of compound (A) and a cured product (β) of compound (B) can be promoted, and a cured resin having both particularly excellent stretchability and particularly excellent low tackiness can be obtained.

[0183] An example of a method for differentiating the timing of curing (polymerization) of compound (A) from the timing of curing (polymerization) of compound (B) is a method in which heating and irradiation with active energy rays are performed sequentially.

[0184] In this method, for example, first, a resin composition that is cured by irradiation with active energy rays and heating is prepared (preparation step).

[0185] A resin composition that is cured by irradiation with active energy rays and heating contains, for example, a photopolymerization initiator (photoradical polymerization initiator (C1)) as the radical polymerization initiator (C), but does not contain a thermal polymerization initiator (thermal radical polymerization initiator (C2)). Also, a resin composition that is cured by irradiation with active energy rays and heating contains, for example, a thermal polymerization initiator (thermal cationic polymerization initiator (D2)) as the cationic polymerization initiator (D), but does not contain a photopolymerization initiator (photocationic polymerization initiator (D1)). That is, in the resin composition, the radical polymerization initiator (C) is the photopolymerization initiator, and the cationic polymerization initiator (D) is the thermal polymerization initiator.

[0186] In this method, the resin composition is cured by irradiation with active energy rays and heating (curing step).

[0187] More specifically, in this method, first, the resin composition is irradiated with active energy rays under the above-mentioned conditions (irradiation step), thereby activating the photoradical polymerization initiator (C1) and initiating the curing (polymerization) of the compound (A).

[0188] After the active energy ray irradiation, i.e., after the initiation of curing of the compound (A), the resin composition is heated under the above-mentioned conditions (heating step), thereby activating the thermal cationic polymerization initiator (D2) and initiating the curing (polymerization) of the compound (B).

[0189] That is, in the method for producing a cured resin, first, the resin composition is irradiated with active energy rays to initiate curing (polymerization) of the compound (A), and then, the resin composition is heated to initiate curing (polymerization) of the compound (B).

[0190] Thereafter, the curing (polymerization) of the compound (A) and the curing (polymerization) of the compound (B) are completed under appropriate conditions, thereby curing the compound (A) and the compound (B) sequentially, and curing the resin composition.

[0191] According to the above method, the cured product (α) of compound (A) and the cured product (β) of compound (B) are well phase-separated, resulting in an excellent phase-separated composite. Furthermore, in the above method, the cured product (α) is formed first, so a portion of the uncured compound (B) is extruded from the cured product (α) and disposed on the surface of the resin composition. In this state, when the uncured compound (B) is cured, the compound (A) and the compound (B) are cured in a phase-separated state to form a phase-separated composite, and the compound (B) is cured on the surface of the phase-separated composite to form a cured product (β) as a skin layer.

[0192] That is, according to the above method, a phase-separated composite of the cured product (α) and the cured product (β), and a cured product (β) serving as a skin layer covering the surface of the phase-separated composite are formed.

[0193] In other words, the cured resin (preferably a resin sheet) has a phase-separated composite and a skin layer disposed on the surface of the phase-separated composite. The skin layer is composed of a cured product of an epoxy group- and / or oxetanyl group-containing compound (B), and the phase-separated composite contains a cured product (α) of a compound (A) having a urethane group and a (meth)acryloyl group, and a cured product (β) of the compound (B). The cured product (α) of the compound (A) and the cured product (β) of the compound (B) are phase-separated. Such a cured resin (preferably a resin sheet) combines the stretchability derived from the cured product (α) of the compound (A) and the low tackiness derived from the cured product (β) of the compound (B), as described above. In particular, such a cured resin (preferably a resin sheet) has particularly excellent low tackiness due to the skin layer.

[0194] Furthermore, the timing of curing (polymerization) of the compound (A) and the timing of curing (polymerization) of the compound (B) can be made to differ only by irradiation with active energy rays.

[0195] More specifically, in this method, first, a resin composition that is cured only by irradiation with active energy rays is prepared (preparation step).

[0196] A resin composition that is cured only by irradiation with active energy rays contains, for example, a photopolymerization initiator (photoradical polymerization initiator (C1)) as the radical polymerization initiator (C) but does not contain a thermal polymerization initiator (thermal radical polymerization initiator (C2)). Also, a resin composition that is cured only by irradiation with active energy rays contains, for example, a photopolymerization initiator (photocationic polymerization initiator (D1)) as the cationic polymerization initiator (D) but does not contain a thermal polymerization initiator (thermal cationic polymerization initiator (D2)). That is, in the resin composition, the radical polymerization initiator (C) is the photopolymerization initiator, and the cationic polymerization initiator (D) is the photopolymerization initiator.

[0197] In the resin composition, the photoradical polymerization initiator (C1) and the photocationic polymerization initiator (D1) are selected so as to be activated by active energy rays having wavelengths different from each other.

[0198] That is, preferably, in the resin composition, the wavelength of the active energy ray that most activates the radical polymerization initiator (C) (photoradical polymerization initiator (C1)) and the wavelength of the active energy ray that most activates the cationic polymerization initiator (D) (photocationic polymerization initiator (D1)) are different from each other. More specifically, preferably, the absolute value of the difference between the peak wavelength on the long wavelength side of the light absorption wavelengths of the photoradical polymerization initiator (C1) and the peak wavelength on the long wavelength side of the light absorption wavelengths of the photocationic polymerization initiator (D1) is equal to or greater than a predetermined value.

[0199] The wavelength of the active energy ray that activates the radical polymerization initiator (C) and the cationic polymerization initiator (D) is the peak wavelength in the absorbance graph. More specifically, in a graph showing the relationship between the wavelength of the active energy ray and the absorbance of the active energy ray at that wavelength, the point at which the absorbance is highest is defined as the absorbance peak, and the wavelength corresponding to the top of that peak is defined as the peak wavelength. In this case, the peak wavelength on the long-wavelength side of the light absorption wavelengths of the photoradical polymerization initiator (C1) indicates the wavelength of the active energy ray that most activates the photoradical polymerization initiator (C1). Furthermore, the peak wavelength on the long-wavelength side of the light absorption wavelengths of the photocationic polymerization initiator (D1) indicates the wavelength of the active energy ray that most activates the photocationic polymerization initiator (D1).

[0200] The difference (absolute value) between the long-wavelength peak wavelength of the light absorption wavelengths of the photoradical polymerization initiator (C1) and the long-wavelength peak wavelength of the light absorption wavelengths of the photocationic polymerization initiator (D1) is, for example, 30 nm or more, preferably 50 nm or more. Also, the difference (absolute value) between the long-wavelength peak wavelength of the light absorption wavelengths of the photoradical polymerization initiator (C1) and the long-wavelength peak wavelength of the light absorption wavelengths of the photocationic polymerization initiator (D1) is, for example, 500 nm or less.

[0201] When the photoradical polymerization initiator (C1) and the photocationic polymerization initiator (D1) are selected as described above, the timing of curing (polymerization) of the compound (A) and the timing of curing (polymerization) of the compound (B) can be made different from each other by adjusting the wavelength of light.

[0202] In this method, the resin composition is cured only by irradiation with active energy rays (curing step).

[0203] More specifically, in this method, first, the resin composition is irradiated with active energy rays having a wavelength at which the photoradical polymerization initiator (C1) is most activated (first irradiation step).

[0204] That is, in the first irradiation step, for example, the resin composition is irradiated with active energy rays having a wavelength corresponding to the peak wavelength on the long wavelength side of the light absorption wavelength of the photoradical polymerization initiator (C1) (first active energy ray irradiation), thereby activating the photoradical polymerization initiator (C1) and initiating curing (polymerization) of the compound (A).

[0205] Then, after the above-mentioned first active energy ray irradiation, i.e., after the initiation of curing of the compound (A), the resin composition is irradiated with active energy rays having a wavelength that activates the photocationic polymerization initiator (D1) (second irradiation step).

[0206] That is, in the second irradiation step, for example, the resin composition is irradiated with active energy rays having a wavelength corresponding to the peak wavelength on the long wavelength side of the light absorption wavelength of the cationic photopolymerization initiator (D1) (second active energy ray irradiation), thereby activating the cationic photopolymerization initiator (D1) and initiating the curing (polymerization) of the compound (B).

[0207] That is, in the above-mentioned method for producing a cured resin, first, the resin composition is irradiated with active energy rays of a specific wavelength that activates the photoradical polymerization initiator (C1), thereby initiating curing (polymerization) of the compound (A). Next, in this method, the resin composition is irradiated with active energy rays of a specific wavelength that activates the photocationic polymerization initiator (D1), thereby initiating curing (polymerization) of the compound (B). In other words, the resin composition is sequentially irradiated with active energy rays of different wavelengths.

[0208] Thereafter, the curing (polymerization) of the compound (A) and the curing (polymerization) of the compound (B) are completed under appropriate conditions, thereby curing the compound (A) and the compound (B) sequentially, and curing the resin composition.

[0209] The above method also results in good phase separation between the cured product (α) of compound (A) and the cured product (β) of compound (B), resulting in an excellent phase-separated composite. Furthermore, in the above method, the cured product (α) is formed first, so a portion of the uncured compound (B) is extruded from the cured product (α) and disposed on the surface of the resin composition. When the uncured compound (B) is cured in this state, the compounds (A) and (B) are cured in a phase-separated state to form a phase-separated composite, and the compound (B) is cured on the surface of the phase-separated composite to form a cured product (β) as a skin layer.

[0210] That is, according to the above method, a phase-separated composite of cured products (α) and (β) and cured product (β) as a skin layer covering the surface of the phase-separated composite are formed. Such a cured resin has particularly excellent low tackiness.

[0211] 3. Effects The resin composition includes a compound (A) having a urethane group and a (meth)acryloyl group, an epoxy group- and / or oxetanyl group-containing compound (B), a radical polymerization initiator (C), and a cationic polymerization initiator (D). The surface tension γB of the compound (B) is a predetermined value or less relative to the surface tension γA of the compound (A). The cured product of the resin composition has a first peak having a peak temperature of less than 100°C and a second peak having a peak temperature of 100°C or higher, and the difference between the peak temperature T1 of the first peak and the peak temperature T2 of the second peak is a predetermined value or more. Therefore, the resin composition can produce a cured resin product having both excellent elasticity and low tackiness.

[0212] More specifically, the resin composition contains a compound (A) having a urethane group and a (meth)acryloyl group. The compound (A) having a urethane group and a (meth)acryloyl group is cured by a radical polymerization initiator (C). The cured product (α) of the compound (A) having a urethane group and a (meth)acryloyl group has excellent elasticity. Therefore, the cured product (cured resin product) of the resin composition has excellent elasticity derived from the cured product (α).

[0213] The resin composition also contains an epoxy group- and / or oxetanyl group-containing compound (B). The epoxy group- and / or oxetanyl group-containing compound (B) is cured by a cationic polymerization initiator (D). The cured product (β) of the epoxy group- and / or oxetanyl group-containing compound (B) has excellent low tackiness. Therefore, the cured product (resin cured product) of the resin composition has excellent low tackiness derived from the cured product (β). The cured product (β) of the epoxy group- and / or oxetanyl group-containing compound (B) also has excellent heat resistance due to its high Tg. Compounds that have a low coefficient of linear thermal expansion and no clear glass transition temperature, so-called Tgless compounds, can also be preferably used as the epoxy group- and / or oxetanyl group-containing compound (B).

[0214] Furthermore, in the above resin composition, the surface tension γB of compound (B) is equal to or less than a predetermined ratio of the surface tension γA of compound (A). Therefore, compound (A) and compound (B) undergo phase separation in the resin composition. As a result, a phase-separated composite of cured products (α) and (β) is obtained by curing the resin composition. In the phase-separated composite, cured product (α) forms soft segments, and cured product (β) forms hard segments. Therefore, the cured product of the above resin composition has excellent stretchability, excellent low tackiness, and also excellent heat resistance.

[0215] In particular, in the above-mentioned resin composition, the tan δ peaks of the cured product have a first peak having a peak temperature of less than 100°C and a second peak having a peak temperature of 100°C or higher. In addition, the difference between the peak temperature T1 of the first peak and the peak temperature T2 of the second peak is equal to or greater than a predetermined value. Therefore, the above-mentioned resin composition can satisfactorily exhibit the elasticity derived from the cured product (α) of compound (A) and the low tackiness and heat resistance derived from the cured product (β) of compound (B).

[0216] The cured resin includes a cured product of the resin composition, and therefore has both the stretchability derived from the cured product (α) of compound (A) and the low tackiness and heat resistance derived from the cured product (β) of compound (B).

[0217] Furthermore, the above-described method for producing a cured resin product can efficiently produce a cured resin product that has excellent stretchability, low tackiness, and also excellent heat resistance. Furthermore, the above-described method for producing a cured resin product can efficiently produce a cured resin product that has excellent flexural strength and excellent heat resistance.

[0218] The present invention also includes an electronic device including the cured resin, such as a display, a sensor, a smartphone, a personal computer, a digital camera, a refrigerator, a microwave oven, or a vacuum cleaner.

[0219] An electronic device can be manufactured by a known method using the cured resin obtained by the above manufacturing method. For example, printed wiring can be formed on the cured resin using a metal paste. Furthermore, for example, the cured resins can be assembled together or with other components by soldering.

[0220] 4. Applications The cured resin and electronic device described above have both excellent stretchability and low tack. Furthermore, the cured resin and electronic device have excellent flexural strength and heat resistance. Therefore, the cured resin and electronic device described above are suitable for use in the fields of stretchable devices, wearable devices, liquid crystal displays, and organic electroluminescent displays.

[0221] More specifically, the cured resin and the electronic device are suitable for use as a substrate for a touch panel, a cover member for a touch panel, a substrate for a wearable device, a cover member for a wearable device, a substrate for a stretchable device, and a cover member for a stretchable device. In particular, the cured resin has excellent low tackiness and is therefore suitable for use as a cover member for a touch panel, a substrate for a wearable device, and a substrate for a stretchable device.

[0222] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited to the following examples. Note that "parts" and "%" are by mass unless otherwise specified. Furthermore, specific numerical values ​​such as blending ratios (content ratios), physical property values, and parameters used in the following description can be substituted with the upper limit values ​​(numeric values ​​defined as "equal to or less than") or lower limit values ​​(numeric values ​​defined as "equal to or more than" or "exceeding") of the corresponding blending ratios (content ratios), physical property values, and parameters described in the above "Description of the Invention."

[0223] 1. Compound (A) Having a Urethane Group and a (Meth)acryloyl Group Production Example 1 (Compound A1) (1) Synthesis of Isocyanate Group-Terminated Prepolymer Under a nitrogen atmosphere, 100 parts by mass of polyoxypropylene polyol (manufactured by Mitsui Chemicals, Inc.; Actocol DL-10000, average functionality 2, number average molecular weight 10,000) as a polyol component was placed in a separable glass flask. Next, 1,3-bis(isocyanatomethyl)cyclohexane (manufactured by Mitsui Chemicals, Inc.; 1,3-H 6 XDI) was added at a ratio such that the equivalent ratio (NCO / OH) was 8.0. The mixture was then heated to 80°C. Stanoct (tin(II) ethylhexanoate) as a urethanization catalyst was then added at a ratio of 10 ppm relative to the mixture. The mixture was then reacted for 4 hours. This yielded a crude product containing an isocyanate-terminated prepolymer and unreacted polyisocyanate components.

[0224] (2) Purification of Isocyanate-Terminated Prepolymer The crude product containing the isocyanate-terminated prepolymer was placed in a Smith thin-film distillation apparatus, and the isocyanate-terminated prepolymer and unreacted polyisocyanate components were separated under the following conditions. In this way, the isocyanate-terminated prepolymer was purified. Temperature conditions: 160-170°C Pressure conditions: 70-100 Pa Supply flow rate: 3.5-4 g / min

[0225] (3) Synthesis of urethane acrylate resin (compound A) 100 parts by mass of purified isocyanate-terminated prepolymer (prepolymer purification product) was placed in a separable flask under atmospheric pressure (dry air). Next, 2-hydroxyethyl acrylate was placed in the separable flask as a hydroxyl-containing unsaturated compound in such a ratio that the equivalent ratio (NCO / OH) of the isocyanate groups of the isocyanate-terminated prepolymer to the hydroxyl groups of the hydroxyl-containing unsaturated compound was 1.0. The mixture was then heated to 70°C.

[0226] Subsequently, Stanoct (tin(II) ethylhexanoate) was added as a urethanization catalyst at a ratio of 200 ppm relative to the isocyanate-terminated prepolymer, and the reaction was carried out for 4 hours until the isocyanate group concentration reached 0.01% or less. This resulted in the synthesis of a radical-curing urethane acrylate resin. The urethane acrylate resin was used as a compound having a urethane group and a (meth)acryloyl group (hereinafter referred to as Compound A1).

[0227] From the viewpoint of molecular equivalent, it was estimated that the raw materials constituting Compound A1 were as follows: Polyoxypropylene polyol (average number of functional groups: 2) 1 mol 1,3-bis(isocyanatomethyl)cyclohexane 2 mol Hydroxyethyl acrylate 2 mol

[0228] Based on the amounts of the raw materials and the molecular structure, the hydrogen-bonding substituent value of Compound A1 was calculated by the following method.

[0229] That is, the amount of polyoxypropylene polyol was 10,000 g (1 mol), and 1,3-bis(isocyanatomethyl)cyclohexane (1,3-H 6 If the amount of hydroxyethyl acrylate is 388.46 g (2 mol) and the amount of hydroxyethyl acrylate is 232.24 g (2 mol), the mass of the urethane acrylate is 10620.7 g (= 10000 g + 388.46 g + 232.24 g).

[0230] In addition, in the above reaction, one molecule of 1,3-H 6HDI (i.e., two molecules of isocyanate group) undergoes urethane conversion, and two molecules of amino group (NH group) are generated as hydrogen-bonding functional groups. 6 When HDI is urethane-converted, 4 mol of amino groups (NH groups) are generated as hydrogen-bonding functional groups.

[0231] That is, the hydrogen-bonding functional group value of compound A1 was 0.000377 mol / g (=4 mol / 10620.7 g).

[0232] Production Example 2 (Compound A2) A radical-curable urethane acrylate resin was synthesized in the same manner as in Production Example 1, except that polyoxypropylene polyol (Actocol DL-2000, manufactured by Mitsui Chemicals, Inc., average functionality 2, number-average molecular weight 2000) was used as the polyol component instead of polyoxypropylene polyol (Actocol DL-10000, manufactured by Mitsui Chemicals, Inc., average functionality 2, number-average molecular weight 10000). The urethane acrylate resin was used as a compound having a urethane group and a (meth)acryloyl group (hereinafter, compound A2).

[0233] From the viewpoint of molecular equivalent, it was estimated that the raw materials constituting Compound A2 were as follows: Polyoxypropylene polyol (average number of functional groups: 2) 1 mol 1,3-bis(isocyanatomethyl)cyclohexane 2 mol Hydroxyethyl acrylate 2 mol

[0234] Based on the amounts of the above raw materials and the molecular structure, the hydrogen-bonding substituent value of Compound A2 was calculated by the following method.

[0235] That is, the amount of polyoxypropylene polyol was 2000 g (1 mol), and 1,3-bis(isocyanatomethyl)cyclohexane (1,3-H 6 XDI) is 388.46 g (2 mol) and the amount of hydroxyethyl acrylate is 232.24 g (2 mol), the mass of the urethane acrylate is 2620.7 g (= 2000 g + 388.46 g + 232.24 g).

[0236] In addition, in the above reaction, one molecule of 1,3-H 6HDI (i.e., two molecules of isocyanate group) undergoes urethane conversion, and two molecules of amino group (NH group) are generated as hydrogen-bonding functional groups. 6 When XDI is urethane-converted, 4 mol of amino groups (NH groups) are generated as hydrogen-bonding functional groups.

[0237] That is, the hydrogen-bonding functional group value of compound A2 was 0.00153 mol / g (=4 mol / 2620.7 g).

[0238] Production Example 3 (Compound A3) As the polyol component, polyoxypropylene polyol (manufactured by Mitsui Chemicals, Inc.; Actocol DL-10000, average functionality 2, number-average molecular weight 10,000) was replaced with polyoxypropylene polyol (manufactured by Mitsui Chemicals, Inc.; Actocol T-300, average functionality 3, number-average molecular weight 300). In addition, 1,3-bis(isocyanatomethyl)cyclohexane (manufactured by Mitsui Chemicals, Inc.; 1,3-H 6 In place of toluene diisocyanate (XDI), toluene diisocyanate (Cosmonate T-80, manufactured by Mitsui Chemicals, Inc.) was used. Except for these, a radical curing type urethane acrylate resin was synthesized in the same manner as in Production Example 1. The urethane acrylate resin was used as a compound having a urethane group and a (meth)acryloyl group (hereinafter, referred to as Compound A3).

[0239] From the viewpoint of molecular equivalent, it was estimated that the raw materials constituting Compound A3 were as follows: Polyoxypropylene polyol (average number of functional groups: 3) 1 mol Toluene diisocyanate 3 mol Hydroxyethyl acrylate 3 mol

[0240] Based on the amounts of the above raw materials and the molecular structure, the hydrogen-bonding substituent value of Compound A3 was calculated by the following method.

[0241] That is, when the amount of polyoxypropylene polyol is 300 g (1 mol), the amount of toluene diisocyanate (TDI) is 522.48 g (3 mol), and the amount of hydroxyethyl acrylate is 348.36 g (3 mol), the mass of the urethane acrylate is 1170.84 g (= 300 g + 522.48 g + 348.36 g).

[0242] In the above reaction, one molecule of TDI (i.e., two molecules of isocyanate groups) undergoes urethane conversion, generating two molecules of amino groups (NH groups) as hydrogen-bonding functional groups. In other words, when 3 mol of TDI undergoes urethane conversion, 6 mol of amino groups (NH groups) are generated as hydrogen-bonding functional groups.

[0243] That is, the hydrogen-bonding functional group value of compound A3 was 0.00512 mol / g (=6 mol / 1170.84 g).

[0244] 2. Epoxy Group- and / or Oxetanyl Group-Containing Compound (B) Preparation Example 1 (Compound B1) EXA-850CRP (a bisphenol A-type epoxy compound manufactured by DIC Corporation) was prepared as an epoxy group- and / or oxetanyl group-containing compound (hereinafter, compound B1).

[0245] Compound B1 did not have a hydrogen-bonding substituent, that is, the hydrogen-bonding substituent value of Compound B1 was 0 mol / g.

[0246] Preparation Example 2 (Compound B2) 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate was prepared as an epoxy group and / or oxetanyl group-containing compound (hereinafter, compound B2).

[0247] Compound B2 did not have a hydrogen-bonding substituent, that is, the hydrogen-bonding substituent value of Compound B2 was 0 mol / g.

[0248] Preparation Example 3 (Compound B3) Trade name jER-YX8000 (manufactured by Mitsubishi Chemical Corporation, hydrogenated bisphenol A type epoxy resin) was prepared as an epoxy group and / or oxetanyl group-containing compound (hereinafter, compound B3).

[0249] Compound B3 did not have a hydrogen-bonding substituent, i.e., the hydrogen-bonding substituent value of Compound B3 was 0 mol / g.

[0250] Preparation Example 4 (Compound B4) OXT-212 (trade name, manufactured by Toagosei Co., Ltd., oxetane resin) was prepared as an epoxy group and / or oxetanyl group-containing compound (hereinafter, compound B4).

[0251] Compound B4 did not have a hydrogen-bonding substituent, that is, the hydrogen-bonding substituent value of Compound B4 was 0 mol / g.

[0252] Preparative Example 5 (Compound B5) 100 g of bisphenol A epoxy resin (product name: Epicoat 1004, epoxy equivalent: 900, manufactured by Yuka Shell Epoxy Co., Ltd.), 0.07 g of triphenylphosphine, 0.03 g of hydroquinone, and 100 g of toluene were placed in a 500 mL three-neck flask. Next, under an argon atmosphere, 0.014412 g (0.0002 mol) of acrylic acid was added dropwise to the flask over 1 hour at 100°C. The contents of the flask were heated for an additional 4 hours. Next, 0.2 g of xylene sulfonic acid was added to the flask, and the contents of the flask were stirred at 40°C for 1 hour. The toluene was then removed from the flask using an evaporator. As a result, a partially acrylated epoxy resin was obtained as the reaction product. The partially acrylated epoxy resin was used as an epoxy group-containing compound (hereinafter referred to as Compound B5).

[0253] Compound B5 had a hydrogen-bonding substituent (OH) derived from acrylic acid. The amount of the hydrogen-bonding substituent (OH) was 0.0002 mol.

[0254] The amount of the partially acrylated epoxy resin was 100.014412 g, which was the total of the amount of the bisphenol A epoxy resin (100 g) and the amount of acrylic acid (0.014412 g).

[0255] That is, the hydrogen-bonding substituent valence of compound B5 is 2.0 × 10 -6 mol / g.

[0256] Preparation Example 6 (Photoradical polymerization initiator C1) Omnirad 819 (manufactured by IGM Resins B.V.) was prepared as a photoradical polymerization initiator (hereinafter referred to as photoinitiator C1). The peak wavelength on the long wavelength side of the light absorption wavelength of photoinitiator C1 was 380 nm.

[0257] Preparation Example 7 (Thermal Radical Polymerization Initiator C2) Percure O (manufactured by NOF Corp.) was prepared as a thermal radical polymerization initiator (hereinafter referred to as thermal initiator C2).

[0258] Preparation Example 8 (Photocationic Polymerization Initiator D1) PI2074 (manufactured by Rhodia) was prepared as a photocationic polymerization initiator (hereinafter referred to as photoinitiator D1). The peak wavelength on the long wavelength side of the light absorption wavelength of photoinitiator D1 was 240 nm.

[0259] Preparation Example 9 (Thermal Cationic Polymerization Initiator D2) SI-100L (product name, manufactured by Sanshin Chemical Industry Co., Ltd.) was prepared as a thermal cationic polymerization initiator (hereinafter, thermal initiator D2).

[0260] Preparation Example 10 (Additive) Irganox 1010 (trade name, antioxidant, manufactured by BASF Japan) was prepared as an antioxidant (hereinafter, antioxidant E).

[0261] 3. Resin Composition and Cured Resin Example 1 (1) Resin Composition A resin composition was obtained by mixing compound (A), compound (B), radical polymerization initiator (C), cationic polymerization initiator (D), and additive (E) according to the formulation shown in Table 1. One part of benzopinacol as a radical source was mixed into the resin composition together with the radical polymerization initiator (C).

[0262] (2) Cured Resin The resin composition was cured to obtain a cured resin by the following method. That is, the resin composition was formed into a film on a polyethylene terephthalate (PET) film using a doctor blade to obtain a coating film with a thickness of 100 μm. Next, the coating film was irradiated with active energy rays (ultraviolet rays) with a wavelength of 405 nm.

[0263] The output of the active energy ray (ultraviolet ray) with a wavelength of 405 nm was 100 mW / cm 2(Measured with an illuminance meter (Hioki 3664 optical power meter (measurement wavelength 405 nm)). The cumulative light intensity was 6000 mJ / cm 2 The resin composition was irradiated with the active energy rays so that the cured resin was cured. The cured resin was then aged at 120°C for 30 minutes.

[0264] Examples 2 to 4, Examples 8 to 9, Example 11 and Comparative Examples 1 to 6 Resin compositions and cured resins were obtained in the same manner as in Example 1, except that the compounding formulation was changed as shown in Table 1.

[0265] Example 5 A resin composition was irradiated with active energy rays (ultraviolet rays) having a wavelength of 405 nm at an accumulated light dose of 6000 mJ / cm 2 Instead of irradiating the resin composition with active energy rays (ultraviolet rays) having a wavelength of 405 nm until the cumulative amount of light reaches 1000 mJ / cm 2 After that, the active energy ray (ultraviolet ray) having a wavelength of 365 nm was irradiated until the cumulative light amount reached 6000 mJ / cm 2 The resin composition and the cured resin were obtained in the same manner as in Example 1 except for the above.

[0266] Example 6 Instead of the photocationic polymerization initiator (photoinitiator D1), a thermal cationic polymerization initiator (thermal initiator D2) was blended according to the formulation shown in Table 1. Otherwise, a resin composition and a cured resin were obtained in the same manner as in Example 1.

[0267] Example 7 Instead of the photocationic polymerization initiator (photoinitiator D1), a thermal cationic polymerization initiator (thermal initiator D2) was blended according to the formulation shown in Table 1. Also, instead of the photoradical polymerization initiator (C1), a thermal radical polymerization initiator (thermal initiator C2) was blended according to the formulation shown in Table 1.

[0268] In addition, instead of irradiating the resin composition with active energy rays, the resin composition was heated at 120° C. for 30 minutes. Otherwise, a resin composition and a cured resin were obtained in the same manner as in Example 1.

[0269] Example 10 Instead of the photoradical polymerization initiator (C1), a thermal radical polymerization initiator (thermal initiator C2) was blended in the formulation shown in Table 1.

[0270] In addition, the resin composition was irradiated with active energy rays (ultraviolet rays) having a wavelength of 405 nm at an integrated light dose of 6000 mJ / cm 2 Instead of irradiating the resin composition until the temperature reached 1000° C., the resin composition was first heated at 120° C. for 30 minutes. Thereafter, the resin composition was irradiated with active energy rays (ultraviolet rays) having a wavelength of 405 nm until the cumulative light amount reached 6000 mJ / cm. 2 The resin composition and the cured resin were obtained in the same manner as in Example 1 except for the above.

[0271] <Physical Properties> (1) Surface Tension γ The surface tension γA of the compound (A) and the surface tension γB of the compound (B) used in the production of the resin composition were measured by the hanging drop method.

[0272] More specifically, compound (A) and compound (B) were dropped from the tip of a 1 mm outer diameter stainless steel needle at 25°C and 50% humidity until they were almost dropped to form droplets. The Young-Laplace equation was then fitted by image processing based on the contour shape and density difference of the droplets to calculate the surface tension.

[0273] (2) Dynamic Viscoelasticity (tan δ) The dynamic viscoelasticity of the cured resin was measured in accordance with JIS K7244 (1998) under the following conditions. Specifically, a type A dumbbell test piece was used as the measurement sample. The measurement mode was a tension mode. The measurement frequency was 10 Hz. The measurement temperature range was -100 to 250°C. The temperature rise rate was 5°C / min.

[0274] The storage modulus and loss factor (tan δ) of the cured resin were then measured. When two tan δ peaks were observed, the tan δ corresponding to the lower temperature peak was designated as tan δ1 (peak temperature T1), and the tan δ corresponding to the higher temperature peak was designated as tan δ2 (peak temperature T2).

[0275] <Evaluation> (1) Stretchability (Number of Stretching and Retraction) Using a 201X universal testing machine (manufactured by Intesco Co., Ltd.), the cured resin was stretched and retracted by 5% at a rate of 1 Hz. The number of stretching and retraction cycles until the cured resin broke was measured.

[0276] In addition, as a heat resistance test, the cured resin was heated in an oven at 260°C for 1 minute. After the heat resistance test, the cured resin was stretched and contracted in the same manner as above. The number of stretches was measured until the cured resin broke.

[0277] If the number of stretches at which the cured resin broke was 50,000 or more both before and after the heat resistance test, the cured resin was determined to have excellent stretchability.

[0278] (2) Tackiness The surface of the cured resin was touched with a finger to check for the presence or absence of surface tackiness. Cured resins for which no surface tackiness was observed were rated as ◯, and cured resins for which surface tackiness was observed were rated as ×.

[0279] (3) Number of stretches until tack appears The cured resin was stretched by 5% using the method described above. The stretching was repeated, and every 100 stretches, the surface of the cured resin was touched with a finger to check for the presence or absence of surface tack. The number of stretches until surface tack appeared was also measured.

[0280] When the number of stretches when surface tack was confirmed was 10,000 or more, the cured resin was judged to have excellent stretchability and excellent low tackiness.

[0281] If the number of stretches when surface tack was confirmed was less than 10,000, the cured resin was judged to have poor low tack properties. If the cured resin broke before surface tack was confirmed (break before tack), the cured resin was judged to have poor stretchability.

[0282] (4) Metal Paste Wiring Test Using a screen printer (LS-150 type screen printer manufactured by Newlong Precision Industry Co., Ltd.) and a screen plate (L-screen 180-027 / 460PW manufactured by Mesh Co., Ltd., line and space 100 μm × 100 mm pattern), silver paste (Dotite XA-5617 silver paste manufactured by Fujikura Chemical Industries Co., Ltd.) was printed on the cured resin. The cured resin and silver paste were then heated at 200 ° C for 15 minutes.

[0283] The shrinkage rate of the cured resin before and after heating (= 100 × [volume before heating − volume after heating] / volume before heating (volume %)) was measured. Cured resins with a shrinkage rate of less than 10% by volume were evaluated as good. Cured resins with a shrinkage rate of 10% by volume or more were evaluated as bad.

[0284] (5) Solder heat resistance test: Solder bath (Sn 60 Pb 40 The cured resin was immersed in the solution for 30 seconds and then removed.

[0285] The shrinkage rate of the cured resin before and after immersion was measured (= 100 × [volume before immersion − volume after immersion] / volume before immersion (volume %)). Cured resins with a shrinkage rate of less than 10% by volume were evaluated as good. Cured resins with a shrinkage rate of 10% by volume or more were evaluated as bad.

[0286] (6) Cross-Section Photography A cross-section of the cured resin of Example 5 was photographed using a transmission electron microscope (TEM). The photograph is shown in FIG. 1. FIG. 1 shows a phase-separated composite having a cured product (α) of a compound (A) having a urethane group and a (meth)acryloyl group, and a cured product (β) of a compound (B) containing an epoxy group and / or an oxetanyl group (i.e., a phase-separated composite of the cured product (α) and the cured product (β)). FIG. 1 also shows a surface layer made of the cured product (β).

[0287] Furthermore, similarly to the above, the cross sections of the cured resin products of Examples 1 to 4 and Examples 6 to 11 were photographed using a transmission electron microscope (TEM). As a result, a surface layer of cured product (β) and a phase-separated composite of cured product (α) and cured product (β) were confirmed.

[0288]

[0289]

[0290] The above invention is provided as an exemplary embodiment of the present invention, but it is merely an example and should not be interpreted as being limiting. Modifications of the present invention that are obvious to those skilled in the art are intended to be included in the scope of the following claims.

[0291] The resin composition, cured resin product, method for producing a cured resin product, electronic device, method for producing an electronic device, and resin sheet of the present invention are suitably used in the fields of stretchable devices, wearable devices, liquid crystal displays, and organic EL displays.

Claims

1. A resin composition comprising a compound (A) having a urethane group and a (meth)acryloyl group, an epoxy group- and / or oxetanyl group-containing compound (B), a radical polymerization initiator (C), and a cationic polymerization initiator (D), wherein the surface tension γB of the compound (B) is 80% or less of the surface tension γA of the compound (A), and the peaks of tan δ of a cured product of the resin composition have a first peak having a peak temperature of less than 100°C and a second peak having a peak temperature of 100°C or higher, and the difference between the peak temperature T1 of the first peak and the peak temperature T2 of the second peak is 30°C or higher.

2. The resin composition according to claim 1, wherein the radical polymerization initiator (C) is a photopolymerization initiator, and the cationic polymerization initiator (D) is a thermal polymerization initiator.

3. The resin composition according to claim 1, wherein the radical polymerization initiator (C) is a photopolymerization initiator, the cationic polymerization initiator (D) is a photopolymerization initiator, and the difference between the peak wavelength on the long wavelength side of the light absorption wavelength of the radical polymerization initiator (C) and the peak wavelength on the long wavelength side of the light absorption wavelength of the cationic polymerization initiator (D) is 30 nm or more.

4. The resin composition according to claim 1, wherein the compound (A) contains a reaction product of an isocyanate compound (a1) and an active hydrogen group-containing (meth)acrylate (a2), the isocyanate compound (a1) has an alicyclic structure, and the alicyclic structure has a chair conformation.

5. The resin composition according to claim 1, wherein the compound (B) comprises a bisphenol A type epoxy compound and / or a hydrogenated bisphenol A type epoxy compound, and the hydrogen-bonding substituent value of the compound (B) is less than 0.0005 mol / g.

6. A cured resin comprising a cured resin composition according to any one of claims 1 to 5.

7. A method for producing a cured resin product, comprising: a preparation step of preparing the resin composition according to claim 2; and a curing step of curing the resin composition, the curing step comprising an irradiation step and a heating step, in which the resin composition is irradiated with active energy rays in the irradiation step, and the resin composition is heated in the heating step after the irradiation step.

8. A method for producing a cured resin product, comprising: a preparation step of preparing the resin composition according to claim 3; and a curing step of curing the resin composition, the curing step comprising a first irradiation step and a second irradiation step, in which in the first irradiation step, the resin composition is irradiated with active energy rays having a wavelength corresponding to a peak wavelength on the long wavelength side of the light absorption wavelengths of the radical polymerization initiator (C), and in the second irradiation step, after the first irradiation step, the resin composition is irradiated with active energy rays having a wavelength corresponding to a peak wavelength on the long wavelength side of the light absorption wavelengths of the cationic polymerization initiator (D).

9. An electronic device comprising the cured resin according to claim 6.

10. A method for producing an electronic device including a cured resin, the cured resin being produced by the method for producing a cured resin according to claim 7.

11. A method for producing an electronic device comprising a cured resin material, the cured resin material being produced by the method for producing a cured resin material described in claim 8.

12. A resin sheet comprising a phase-separated composite and a skin layer disposed on a surface of the phase-separated composite, wherein the skin layer is made of a cured product of an epoxy group- and / or oxetanyl group-containing compound (B), and the phase-separated composite contains a cured product of a compound (A) having a urethane group and a (meth)acryloyl group, and the cured product of the compound (B), and the cured product of the compound (A) and the cured product of the compound (B) are phase-separated.

13. The resin sheet according to claim 12, wherein the peaks of tan δ of the resin sheet have a first peak having a peak temperature of less than 100°C and a second peak having a peak temperature of 100°C or higher, and the difference between a peak temperature T1 of the first peak and a peak temperature T2 of the second peak is 30°C or higher.

Citation Information

Patent Citations

  • High-toughness photosensitive resin for 3D printing and preparation method thereof.

    CN104765251A

  • Bio-based odorless water-based UV-cured urethane acrylate aqueous dispersion as well as preparation method and application thereof

    CN112409565A

  • Urethane acrylate resin and epoxy paint composition having the same

    CN1990518A

  • Curable composition

    KR1020150143045A

  • Polyurethane-acrylate epoxy adhesive

    US20170029673A1