Composite resin composition and molded article thereof
The composite resin composition, with biodegradable resin, fibers, and a controlled lubricant, enhances mechanical strength and biodegradability, enabling effective decomposition in industrial compost environments and reducing petroleum-derived resin use, addressing the limitations of conventional biodegradable plastics.
Patent Information
- Application Number
- PCT/JP2024/012959
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-17
AI Technical Summary
Conventional biodegradable plastics lack sufficient mechanical strength and durability for industrial applications and have limited biodegradability, especially in environments with few microorganisms, leading to accumulation of plastic waste and environmental pollution.
A composite resin composition combining biodegradable resin, biodegradable fibers, and a lubricant, where the fiber content is 30% to 99% by mass and the lubricant content is 0.5% to 10% by mass, with the fibers having a fibrillated portion to enhance water absorption and microorganism contact, and the lubricant controlling hydrophobicity at room temperature and hydrophilicity at high temperatures to promote biodegradation.
The composite resin composition achieves improved mechanical properties and biodegradability, allowing for effective decomposition in industrial compost environments while reducing petroleum-derived resin usage, thus addressing the limitations of conventional biodegradable plastics.
Smart Images

Figure JP2024012959_17102024_PF_FP_ABST
Abstract
Description
Composite resin composition and molded article thereof
[0001] The present disclosure relates to a composite resin composition that is excellent in mechanical properties and durability and exhibits excellent biodegradability, and to a molded article thereof.
[0002] So-called "general-purpose plastics," such as polyethylene (PE), polypropylene (PP), polystyrene (PS), and polyvinyl chloride (PVC), are not only very inexpensive, but also easy to mold and are a fraction of the weight of metals or ceramics. For this reason, general-purpose plastics are often used as materials for a variety of everyday items, such as bags, various types of packaging, various containers, and sheets, as well as industrial parts, such as automobile parts and electrical parts, and as materials for daily necessities and miscellaneous goods.
[0003] Under these circumstances, the amount of post-use plastic waste is increasing year by year, and because plastic waste is a substance that is difficult to decompose, it accumulates in the natural environment, causing pollution problems such as environmental destruction and contamination. In recent years, biodegradable plastics that decompose into water and carbon dioxide in the natural environment have been proposed as one of the measures to solve these problems, and it is expected that their use will expand, replacing general-purpose plastics made from petroleum-based raw materials.
[0004] However, biodegradable plastics have drawbacks compared to general-purpose plastics, such as insufficient mechanical strength and durability, and therefore do not have the sufficient properties required for materials used in various industrial products, including mechanical products such as automobiles and electrical, electronic, and information products, and the range of their application is currently limited.
[0005] Furthermore, the speed at which biodegradable plastics decompose is greatly affected by the environment. In environments with few microorganisms, it takes a significantly longer time for them to decompose completely, and their biodegradability is not fully utilized.
[0006] To solve these problems, methods have been disclosed in which a hydrolysis inhibitor is compounded with a biodegradable resin to impart durability (see, for example, Patent Document 1), and products have been disclosed in which microorganisms capable of decomposing biodegradable resins are incorporated to accelerate the decomposition rate (see, for example, Patent Document 2).
[0007] JP 2006-291091 A JP 2013-209587 A
[0008] In Patent Document 1, the addition of a hydrolysis inhibitor may decrease the decomposition rate in a natural environment, and Patent Document 2 does not mention a method for improving the mechanical properties or suppressing decomposition while increasing the decomposition rate.
[0009] One aspect of the present disclosure is intended to solve the above-described conventional problems, and aims to provide a composite resin composition that promotes biodegradation in the ocean or soil while reducing the amount of petroleum-derived resin used.
[0010] A composite resin composition according to one embodiment of the present disclosure is a composite resin composition containing a biodegradable resin, biodegradable fibers dispersed in the resin, and a lubricant, wherein, when the composite resin composition is taken as 100% by mass, the fiber content is 30% by mass or more and 99% by mass or less, and the lubricant content is 0.5% by mass or more and 10% by mass or less.
[0011] A composite resin molded article according to one embodiment of the present disclosure is a composite resin molded article obtained by molding the composite resin composition.
[0012] Fig. 1 is a schematic cross-sectional view showing the cross-sectional structure of a composite resin composition according to embodiment 1. Fig. 2 is a schematic cross-sectional view showing the cross-sectional structure of a composite resin composition according to embodiment 1 after immersion in water at 60°C for 24 hours. Fig. 3 is a schematic cross-sectional view showing the cross-sectional structure of a composite resin composition containing fibers with defibrated regions according to embodiment 1. Fig. 4 is a flow diagram of a method for producing a composite resin composition according to embodiment 1 and a method for producing a composite resin molded body using the composite resin composition. Fig. 5 is a diagram showing the configuration and measurement results of composite resin molded bodies in examples and comparative examples in the embodiments.
[0013] The composite resin composition according to the first aspect is a composite resin composition containing a biodegradable resin, biodegradable fibers dispersed in the resin, and a lubricant, and when the composite resin composition is taken as 100% by mass, the fiber content is 30% by mass or more and 99% by mass or less, and the lubricant content is 0.5% by mass or more and 10% by mass or less.
[0014] In the composite resin composition according to a second aspect, in the first aspect, the fibers may include fibers having defibrated portions formed at ends in the fiber length direction.
[0015] In the composite resin composition according to the third aspect, in the first or second aspect, the moisture content of the biodegradable fiber may be 5% or more as measured by the method specified in JIS L0105:2020.
[0016] A composite resin composition according to a fourth aspect is the composite resin composition of any one of the first to third aspects, wherein the resin may include at least one of polyhydroxyalkanoic acid, polybutylene succinate, polylactic acid, polybutylene adipate-co-terephthalate, polycaprolactone, polyamide, modified starch, and derivatives thereof.
[0017] A composite resin composition according to a fifth aspect is any one of the first to fourth aspects, wherein the resin is a thermoplastic biodegradable resin having a flexural modulus of 100 MPa or more.
[0018] A composite resin composition according to a sixth aspect is the composite resin composition according to any one of the first to fifth aspects, wherein the lubricant contains 50 mol % or more of long-chain aliphatic carboxylic acids having 15 or more carbon atoms, long-chain aliphatic primary alcohols, or long-chain aliphatic esters.
[0019] A composite resin composition according to a seventh aspect is any one of the first to sixth aspects, wherein the lubricant has a melting point of 25° C. or higher and 70° C. or lower.
[0020] The composite resin composition according to an eighth aspect is the composite resin composition according to any one of the first to seventh aspects, wherein the fibers are cellulose fibers.
[0021] A composite resin molding according to a ninth aspect is obtained by molding the composite resin composition according to any one of the first to eighth aspects.
[0022] A composite resin molded product according to a tenth aspect may be the composite resin molded product of the ninth aspect, wherein the contact angle with water at 25° C. or less is 80° or more.
[0023] The composite resin molding according to the eleventh aspect may be the composite resin molding according to the ninth or tenth aspect, wherein the contact angle with water is less than 80° after the composite resin molding is immersed in water at 60°C for 24 hours.
[0024] The composite resin composition according to one embodiment of the present disclosure can realize a composite resin molded product that has a higher elastic modulus than a resin alone, as well as improved durability in a room temperature environment and high biodegradability in a high-temperature environment such as industrial composting.
[0025] Hereinafter, a composite resin composition and a method for manufacturing a molded article thereof according to an embodiment will be described with reference to the accompanying drawings. In the following description, the same components are denoted by the same reference numerals and the description will be omitted as appropriate.
[0026] First Embodiment FIG. 1 is a schematic cross-sectional view showing the cross-sectional structure of a composite resin composition 10 according to a first embodiment.
[0027] Composite resin composition 10 according to the first embodiment is made of a melt-kneaded mixture containing resin 1, fiber 2, lubricant 3, and, as necessary, additives. As shown in the schematic cross-sectional view of Fig. 1, composite resin composition 10 has fiber 2 and lubricant 3 dispersed in resin 1. In a room temperature environment of 25°C or less, the surface of composite resin composition 10 is made hydrophobic due to the effect of lubricant 3 contained in composite resin composition 10, thereby suppressing water absorption by fiber 2 and decomposition by microorganisms.
[0028] 2 is a schematic cross-sectional view showing the cross-sectional structure of the composite resin composition 10 according to embodiment 1 after immersion in water at 60° C. for 24 hours. As shown in FIG. 2, in a high-temperature environment of 60° C. or higher, such as industrial compost, a portion of the lubricant 3 on the surface of the composite resin composition 10 is eluted and desorbed, thereby making the surface of the composite resin composition 10 hydrophilic. This makes it possible to promote water absorption by the fibers 2 and decomposition by microorganisms.
[0029] 3 is a schematic cross-sectional view showing the cross-sectional structure of a composite resin composition 10 containing fibers 2 having defibrated portions according to embodiment 1. As shown in FIG. 3, having defibrated portions at the ends of fibers 2 increases the specific surface area of the defibrated portions and increases the number of contact points between fibers 2. This makes it possible for water to be absorbed into the interior of composite resin composition 10 through the contact points between fibers 2 in a high-temperature environment.
[0030] At least one of the fibers 2 is exposed on the surface of the composite resin molding. According to this composite resin composition 10, at least one of the fibers 2 is exposed on the surface of the composite resin molding, and in addition to having a high elastic modulus, it is possible to realize a composite resin molding that has durability in a room temperature environment, high water absorbency in a high temperature environment such as industrial compost, and excellent biodegradability.
[0031] Each of the components constituting the composite resin composition 10 will be described below.
[0032] <Resin> In this embodiment 1, resin 1 is preferably a biodegradable plastic containing any one of polyhydroxyalkanoic acid, polyhydroxyalkanoate, polyalkylene dicarboxylate, and modified starch. Furthermore, to ensure good moldability and mechanical properties, a thermoplastic resin with a flexural modulus of 100 MPa or more is preferred, and the above resins may be used alone or in combination of two or more. Note that resin 1 is not limited to the above materials as long as it is biodegradable.
[0033] In the present embodiment, "biodegradable plastic" refers to a resin that functions similarly to conventional petroleum-derived resins during use and is ultimately decomposed into water and carbon dioxide by microorganisms in the soil or oceans in nature after use. Specific examples include polyester-based resins such as polyhydroxyalkanoates (e.g., polyhydroxybutyrate, polyhydroxyvalerate), polyhydroxy acids (e.g., polylactic acid, polyglycolic acid, polycaprolactone), polyalkylene dicarboxylates (e.g., polybutylene adipate terephthalate, polyethylene succinate, polybutylene succinate), polyamides, modified starch, and derivatives thereof. Polyester-based resins include homopolymers of polyester monomers, copolymers of polyester monomers (e.g., poly(3-hydroxybutyrate-co-3-hydroxyvalerate)), and copolymers of polyester monomers with other copolymerizable monomers. These polyester-based resins may be used alone or in combination.
[0034] <Fibers> Next, the fibers 2 will be described. The first main purpose of adding the fibers 2 to the composite resin composition 10 in the present embodiment 1 is to promote decomposition of a molded body made of the composite resin composition 10 when the molded body is discarded after use. In other words, in a high-temperature environment of 60°C or higher, such as industrial compost, the fibers 2 absorb water into the interior of the molded body, promoting decomposition of the molded body. For this purpose, the fibers 2 are preferably biodegradable and highly water-absorbent, and the moisture content of the fibers 2 is preferably 5% or more as determined by the method specified in JIS L0105:2020. Specifically, pulp, cellulose, cellulose nanofibers, lignocellulose, lignocellulose nanofibers, cotton, silk, hemp, or the like is preferred.
[0035] The second purpose of adding fiber 2 is to improve mechanical properties and dimensional stability by reducing the linear expansion coefficient. For this purpose, fiber 2 preferably has a higher elastic modulus than resin 1. Specific examples include pulp, cellulose, cellulose nanofiber, lignocellulose, lignocellulose nanofiber, cotton, silk, wool, and hemp. Among these, celluloses are particularly preferred from the viewpoints of availability, high elastic modulus, and low linear expansion coefficient. However, fiber 2 is not limited to the above materials as long as it can improve mechanical properties and is biodegradable and water-absorbent.
[0036] The content of fiber 2 is preferably 30% by mass or more and 99% by mass or less, when the composite resin composition is taken as 100% by mass. If the content of fiber 2 is less than 30% by mass, the fibers 2 are unlikely to come into contact with each other within the composite resin composition, resulting in insufficient water absorption. On the other hand, if the content of fiber 2 is more than 99% by mass, the proportion of resin 1 becomes small, which eliminates the effect of bonding the fibers 2 together and deteriorates moldability. From the viewpoint of water absorption and moldability, the content of fiber 2 is more preferably 40% by mass or more and 70% by mass or less.
[0037] The morphology of the fiber 2 in the composite resin molded body will now be described. A larger bonding interface between the fiber 2 and the resin 1 increases the area of contact with microorganisms in the resin 1 when the fiber 2 absorbs and expands. Therefore, a high specific surface area of the fiber 2 is preferable. On the other hand, to improve the water absorption of the composite resin molded body, the fiber 2 is preferably exposed on the surface of the composite resin molded body. When the fiber 2 is exposed on the surface of the composite resin molded body, water is absorbed through the exposed portion of the fiber 2, and the water is absorbed into the interior of the composite resin molded body by capillary action of the fiber 2. The smaller the specific surface area of the fiber 2 exposed on the surface of the composite resin molded body, the higher the water absorption. This is because a large specific surface area of the fiber 2 exposed on the surface enhances water repellency due to the effect of fine irregularities. Furthermore, as shown in Figure 3, having defibrated portions at the ends of the fiber 2 increases the specific surface area of the defibrated portions and increases the number of contact points between the fibers 2. As a result, if the surface of the composite resin molded body becomes hydrophilic in a high-temperature environment of 60°C or higher, such as industrial compost, the water absorption rate can be increased through the contact points of the fibers 2.
[0038] The central portions of the undefibrated fibers 2, which have a small specific surface area, are less likely to be entangled with the resin 1 and, depending on the molding conditions, are more likely to be exposed on the surface of the composite resin molded product. Conversely, the tip portions of the defibrated fibers 2 are more likely to be entangled with the resin 1 and penetrate into the interior together with the resin 1. This allows for the production of a composite resin molded product in which the central portions of the fibers 2, not including both end portions, are exposed on the surface.
[0039] The tip defibrated region preferably occupies 5% or more and 50% or less of the entire fiber length of the fiber 2. If the defibrated region is less than 5% of the entire fiber length, the specific surface area is small and no improvement in elastic modulus is observed, and if the defibrated region is longer than 50% of the fiber length, the defibrated region with a large aspect ratio is exposed on the surface of the composite resin molding, resulting in a deterioration in water absorbency.
[0040] Next, the state of fiber 2 in a composite resin molded body will be described. A composite resin molded body includes a surface layer and an internal layer located deeper than the surface layer. By adjusting the molding conditions and increasing the shrinkage rate during molding of the composite resin composition, it is possible to segregate fiber 2 near the surface of the composite resin molded body. This results in more fiber 2 being present in the surface layer than in the internal layer of the composite resin molded body. Furthermore, when viewed as a molded body, having more fiber 2 present in the surface layer of the composite resin molded body increases the outer elastic modulus, thereby increasing the rigidity of the molded body as a whole. Therefore, a structure in which fiber 2 is segregated near the surface of the molded body also leads to improved rigidity. Segregation of fiber 2 near the surface can be evaluated by, for example, SEM observation of the cross section of the composite resin molded body.
[0041] Next, the characteristics of fiber 2 will be described. The types of resin 1 and fiber 2 are as described above. However, if fiber 2 is too soft relative to resin 1, i.e., if the fiber 2 has a low elastic modulus, the composite resin molding will have a low overall elastic modulus, resulting in reduced strength. On the other hand, if fiber 2 is too hard relative to resin 1, i.e., if the fiber 2 has a high elastic modulus, shock waves generated upon impact will not propagate, and the impact will be absorbed at the interface between resin 1 and fiber 2. This makes it more likely that cracks and crazes will occur near the interface, resulting in reduced impact resistance. Therefore, in the relationship between the elastic moduli of resin 1 and fiber 2, it is preferable that the elastic modulus of fiber 2 is higher, and that the difference between them is as small as possible. The optimal relationship is calculated from simulation results, and it is preferable that the difference in elastic modulus between resin 1 and fiber 2 is within 20 GPa.
[0042] Furthermore, these fibers 2 may be surface-treated for the purpose of improving adhesion to the resin 1 or dispersibility in the composite resin composition, but if the surface treatment impairs the water absorption properties of the fibers 2, it is preferable not to perform the surface treatment in advance.
[0043] <Lubricant> Next, the lubricant 3 will be described. In the present embodiment 1, the lubricant 3 is used in a room temperature environment to make the surface of the composite resin molding hydrophobic, thereby inhibiting the water absorption and expansion of the fibers 2 and the adsorption of decomposing microorganisms and / or enzymes, thereby suppressing decomposition. On the other hand, in a high-temperature environment such as industrial compost, the lubricant 3 is eluted and is used in a high-temperature environment such as industrial compost, thereby making the surface of the composite resin molding hydrophilic, thereby promoting the water absorption and expansion of the fibers 2 and the adsorption of decomposing microorganisms and / or enzymes. Therefore, the melting point of the lubricant 3 is preferably 25°C or higher and 70°C or lower.
[0044] The content of lubricant 3 is preferably 0.5% by mass or more and 10% by mass or less, when the composite resin composition is taken as 100% by mass. If the content of lubricant 3 is less than 0.5% by mass, it is difficult to obtain the effect of hydrophobizing the surface of the composite resin molding in a room temperature environment. On the other hand, if the content of lubricant 3 is more than 10% by mass, the mechanical properties of the composite resin molding may be reduced. From the viewpoint of hydrophobicity and mechanical properties, the content of lubricant 3 is more preferably 1% by mass or more and 5% by mass or less.
[0045] Furthermore, the composite resin molding containing lubricant 3 preferably has a contact angle with water of 80 degrees or more at 25°C or below. Furthermore, after immersing the composite resin molding containing lubricant 3 in water at 60°C for 24 hours, the contact angle with water is preferably less than 80 degrees. In order to control the hydrophilicity of the composite resin molding depending on the temperature, lubricant 3 preferably contains 50 mol% or more of long-chain aliphatic carboxylic acids, long-chain aliphatic primary alcohols, or long-chain aliphatic esters having 15 or more carbon atoms. If the carbon number is less than 15, the hydrophobicity decreases under room temperature conditions when lubricant 3 is compounded. If the content of long-chain aliphatic carboxylic acids, long-chain aliphatic primary alcohols, or long-chain aliphatic esters having 15 or more carbon atoms is less than 50 mol%, the intended functions, such as controlling the melting point and hydrophilicity / hydrophobicity, are not exhibited.
[0046] <Additives> The additives may be used as needed for the purpose of improving the affinity between the resin 1 and the fibers 2, etc.
[0047] <Method for producing composite resin composition> Next, a method for producing a composite resin composition will be described. Fig. 4 is a flow diagram illustrating a method for producing a composite resin composition according to the first embodiment and a method for producing a composite resin molded product using the composite resin composition.
[0048] (1) Resin 1, fibers 2, lubricant 3, and additives are charged into a melt-kneading processing device and melt-kneaded within the device. This melts the resin 1, and the fibers 2, lubricant 3, and additives are dispersed in the molten resin 1. At the same time, the shearing action of the device promotes defibration of agglomerates of fiber 2, allowing the fibers 2 to be finely dispersed in the resin 1.
[0049] Conventionally, when fibers are compounded with resin, fibers have been defibrated in advance through pretreatment such as wet dispersion. However, because defibration by wet dispersion is easier than defibration in molten resin, it is difficult to defibrate only the ends, and the entire fiber ends up defibrated. In addition, adding pretreatment increases the number of processes, which reduces productivity.
[0050] In contrast, in the manufacturing process of the composite resin composition in this embodiment, the fibers 2 are melt-kneaded together with the resin 1, the lubricant 3, and additives (all-dry method) without being subjected to a pretreatment by wet dispersion for the purpose of defibrating the fibers 2. In this method, by not performing a wet dispersion treatment of the fibers, it is possible to suppress swelling of the fibers 2 during the manufacturing process and improve the coefficient of expansion of the fibers 2 in the resin 1 of the composite resin composition by absorbing water. In addition, by drying the fibers 2 beforehand or during kneading and adjusting the moisture content to 5% or less, it is possible to further improve the coefficient of expansion of the fibers 2 upon absorption of water in the resin 1.
[0051] To produce the fiber 2 of this embodiment using an all-dry method, it is preferable to apply high shear stress during kneading, and specific kneading methods include a single-screw kneader, a twin-screw kneader, a roll kneader, a Banbury mixer, and combinations thereof. From the viewpoint of ease of applying high shear and high mass productivity, a continuous twin-screw kneader and a continuous roll kneader are particularly preferable. Kneading methods other than those mentioned above may also be used as long as they are capable of applying high shear stress.
[0052] A composite resin composition can be obtained by the above kneading step.
[0053] <Method for manufacturing a composite resin molded body> (2) The composite resin composition extruded from the melt kneader is cut into pellets using a pelletizer or the like. Pelletization methods include in-air hot cutting, underwater hot cutting, and strand cutting, which are carried out immediately after the resin is melted. Alternatively, a crushing method may be used in which a molded body or sheet is molded and then crushed and cut.
[0054] (3) By injection molding the pellets, an injection-molded article can be produced as a composite resin molding. As described above, the fiber 2 in the pellets is mixed with the resin 1, and therefore an injection-molded article having excellent elastic modulus, impact resistance, and appearance can be obtained.
[0055] Hereinafter, examples and comparative examples of the experiments conducted by the inventors will be described.
[0056] Example 1 In Example 1, a cellulose-composite polylactic acid resin molded article was produced by the following production method.
[0057] The starting material for the fibers was softwood pulp (manufactured by Mitsubishi Paper Mills, product name: NBKP Celgar). The resin was polylactic acid (manufactured by Unitika Ltd., product name: TE-2000). The lubricant was rice wax with a melting point of 70°C (manufactured by Nippon Seiro Co., Ltd., product name: ECOSOLE-1500). The softwood pulp, polylactic acid, and rice wax, which had been dried in advance and adjusted to a moisture content of 5% or less, were weighed out in a weight ratio of 55:44:1 and dry-blended.
[0058] Thereafter, the mixture was melt-kneaded in a twin-screw kneader (KRC Kneader manufactured by Kurimoto Iron Works Co., Ltd.). The screw was a medium shear type. The melt-kneading conditions were a resin temperature of 200°C and a rotation speed of 50 min. -1 The composite resin composition discharged from the twin-screw kneader was hot-cut to prepare cellulose-composite polylactic acid resin pellets.
[0059] Using the prepared cellulose-composite polylactic acid pellets, test pieces of cellulose-composite polylactic acid resin molded bodies were prepared using an injection molding machine (180AD manufactured by Japan Steel Works, Ltd.). The test piece preparation conditions were a resin temperature of 200°C, a mold temperature of 30°C, an injection speed of 100 mm / s, and a holding pressure of 100 Pa. The shape of the test piece was changed depending on the evaluation items described below, and a size 1 dumbbell was prepared for measuring the elastic modulus. The obtained test pieces of cellulose-composite polylactic acid resin molded bodies were evaluated using the following methods.
[0060] (Evaluation of fiber water absorbency) The water absorbency of the fibers was evaluated by measuring the moisture content of the fibers according to the method specified in JIS L0105:2020. Specifically, the weight of the fibers dried at 80°C for 24 hours was measured, and this was used as the reference weight. Then, the weight of the fibers maintained at a temperature of 20°C and a humidity of 65% for 24 hours was measured. The weight increase from the reference weight was taken as the moisture, and the moisture content was calculated. A moisture content of less than 5% was rated C, and a moisture content of 5% or more was rated A. The moisture content of the softwood pulp was 6.5%, and its rating was A (fiber end defibration ability).
[0061] The obtained cellulose composite polylactic acid resin composition was immersed in chloroform to dissolve the polylactic acid, and the shape of the remaining cellulose fibers was observed using a scanning electron microscope (SEM). The ends of the fibers were found to be defibrated.
[0062] (Elastic Modulus of Composite Resin Molded Product) A bending test was carried out using the obtained No. 1 dumbbell-shaped test piece. Here, the elastic modulus was evaluated as A when the value was 6.5 GPa or more, and C when it was less than 6.5 GPa.
[0063] The modulus of elasticity of the test piece was 6.9 GPa and the evaluation was A.
[0064] (Evaluation of hydrophilicity of composite resin molded article) The obtained No. 1 dumbbell-shaped test piece was used to measure the contact angle with water. To evaluate hydrophilicity in a room temperature environment, 3 μL of distilled water was dropped onto the test piece at room temperature of 23° C., and the contact angle was measured after 1 second. In the evaluation method for hydrophilicity in a room temperature environment, a contact angle with water of 80 degrees or more was rated as A, and a contact angle of less than 80 degrees was rated as C.
[0065] The contact angle of the test piece with water was 88.4 degrees, and the test piece was evaluated as A.
[0066] To evaluate hydrophilicity in a high-temperature environment, the test piece was immersed in distilled water at 60° C. for 24 hours, the moisture on the surface was wiped off, and 3 μL of distilled water was dropped onto the test piece at room temperature of 23° C. The contact angle was measured after 1 second. In the evaluation method for hydrophilicity in a high-temperature environment, a contact angle with water of less than 80 degrees was rated as A, and a contact angle of 80 degrees or more was rated as C.
[0067] The contact angle of the test piece with water was 72.3 degrees, and the test piece was evaluated as A.
[0068] (Biodegradability Evaluation of Composite Resin Molded Articles) A biodegradation test was conducted using bar-shaped test pieces made of the obtained composite resin molded articles according to JIS K 6953-1:2011. Specifically, 60 mL of compost inoculum (YK-12, manufactured by Yawata Bussan Co., Ltd.) was placed in a plastic container, and a pre-weighed bar-shaped test piece measuring 20 mm in height, 10 mm in width, and 4 mm in thickness was buried in the inoculum. The test piece was kept at a temperature of 58°C and a moisture content of 50%, and the weight loss after one month was evaluated. The biodegradability evaluation method rated a value of 8% or more as A, a value of 5% to less than 8% as B, and a value of less than 5% as C.
[0069] The biodegradation rate of the test specimen was 9.1%, and the evaluation was A.
[0070] In Comparative Example 1, a polylactic acid resin molded body was produced using polylactic acid as a raw material without compounding fibers and lubricants, with the other process conditions being the same as in Example 1. The same evaluation as in Example 1 was also carried out.
[0071] In Comparative Example 2, a cellulose-composite polylactic acid resin pellet and a composite resin molding were produced without compounding a lubricant, and the other material conditions and process conditions were the same as in Example 1. The evaluations were also the same as in Example 1.
[0072] In Comparative Example 3, cellulose-composite polylactic acid resin pellets and a composite resin molded product were produced using carnauba wax, which has a melting point of 82°C, instead of rice wax as a lubricant, with the other material conditions and process conditions being the same as in Example 1. Evaluations were also performed in the same manner as in Example 1.
[0073] In Comparative Example 4, PET fiber was used instead of softwood pulp as the fiber, and the other material conditions and process conditions were the same as in Example 1 to produce PET fiber-composite polylactic acid resin pellets and a composite resin molded product. Evaluations similar to those in Example 1 were also carried out.
[0074] FIG. 5 is a diagram showing the structure and measurement results of the composite resin moldings in Example 1 and Comparative Examples 1 to 4.
[0075] As is clear from Figure 5, in Example 1, in which polylactic acid was compounded with cellulose and rice wax, the elastic modulus was high at 6.9 GPa, and the addition of a lubricant improved the hydrophobicity of the molded body surface at room temperature compared to the cellulose-composite polylactic acid resin molded body without a lubricant in Comparative Example 2. On the other hand, in a high-temperature environment, the molded body surface became hydrophilic, and the water absorption properties of the cellulose were exhibited, resulting in an improved biodegradability compared to the polylactic acid resin molded body in Comparative Example 1. It was confirmed that by compounding highly water-absorbent fibers and compounding a lubricant that hydrophobicizes the molded body surface at room temperature and hydrophilizes the molded body surface at high temperatures, a composite resin with a high elastic modulus, high durability, and high biodegradability can be obtained.
[0076] In Comparative Example 3, in which carnauba wax was combined as a lubricant, the melting point of the lubricant was higher than 70°C, so compared to Example 1, the contact angle with water after immersion in water at 60°C was higher and the biodegradation rate was lower, at 4.3%, resulting in a rating of C.
[0077] In Comparative Example 4, in which PET fiber was used as the fiber, the moisture content of the fiber was low, so the molded body did not absorb water even after being hydrophilized in a high-temperature environment, and the biodegradation rate was lower than in Example 1, at 4.6%, earning a rating of C.
[0078] From the above evaluations, it was confirmed that by combining highly absorbent fibers and a lubricant that makes the surface of the molded body hydrophobic in a room temperature environment and hydrophilic in a high temperature environment, a composite resin with a high elastic modulus, high durability, and high biodegradability can be obtained.
[0079] It should be noted that the present disclosure includes appropriate combinations of any of the various embodiments and / or examples described above, and can achieve the effects of each embodiment and / or example.
[0080] The composite resin composition according to the present disclosure can provide molded articles with superior mechanical strength and biodegradability compared to conventional biodegradable plastics. Because the present invention can improve the properties of the resin, it can be used as a substitute for petroleum-derived general-purpose plastics. Therefore, the environmental impact of various industrial products or household goods made from petroleum-derived general-purpose plastics can be significantly reduced. Furthermore, it can be used for packaging materials, daily necessities, home appliance housings, building materials, etc.
[0081] REFERENCE SIGNS LIST 1 resin 2 fiber 3 lubricant 10 composite resin composition
Claims
1. A composite resin composition containing a biodegradable resin, biodegradable fibers dispersed in the resin, and a lubricant, wherein, when the composite resin composition is 100% by mass, the fiber content is 30% by mass or more and 99% by mass or less, and the lubricant content is 0.5% by mass or more and 10% by mass or less.
2. The composite resin composition according to claim 1, wherein the fibers include fibers having defibrated portions formed at ends in the fiber length direction.
3. The composite resin composition according to claim 1, wherein the moisture content of the fiber is 5% or more as measured by the method specified in JIS L0105:2020.
4. The composite resin composition according to claim 1, wherein the resin comprises at least one of polyhydroxyalkanoic acid, polybutylene succinate, polylactic acid, polybutylene adipate-co-terephthalate, polycaprolactone, polyamide, modified starches, and derivatives thereof.
5. The composite resin composition according to claim 1, wherein the resin is a thermoplastic biodegradable resin having a flexural modulus of 100 MPa or more.
6. The composite resin composition according to claim 1, wherein the lubricant contains 50 mol % or more of long-chain aliphatic carboxylic acids having 15 or more carbon atoms, long-chain aliphatic primary alcohols, or long-chain aliphatic esters.
7. The composite resin composition according to claim 1, wherein the melting point of the lubricant is 25°C or higher and 70°C or lower.
8. The composite resin composition according to claim 1, wherein the fibers are cellulose fibers.
9. A composite resin molding obtained by molding the composite resin composition according to any one of claims 1 to 8.
10. The composite resin molding according to claim 9, which has a contact angle with water of 80° or more at a temperature of 25° C. or less.
11. The composite resin molding according to claim 9, wherein after immersing the composite resin molding in water at 60° C. for 24 hours, the contact angle with water is less than 80°.
Citation Information
Patent Citations
Fiber composite resin composition and manufacturing method therefor
JP2019157049A
Hydrophilic cellulose composite resin molding
JP2020143249A
Composition for molding and molding
JP2021095432A
Biodegradable biocomposite material and method for preparing same
JP2023503533A