Modified aromatic hydrocarbon formaldehyde resin, adhesive including same, and method for producing modified aromatic hydrocarbon formaldehyde resin

The modified aromatic hydrocarbon formaldehyde resin, produced by reacting an aromatic hydrocarbon formaldehyde resin with an aromatic monocarboxylic acid, addresses the insufficiencies in adhesive strength and tack strength by enhancing ester and acid values, resulting in improved adhesive performance and compatibility.

WO2024214592A1PCT designated stage expired Publication Date: 2024-10-17MITSUBISHI GAS CHEM CO INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013592
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2024-04-02
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing aromatic hydrocarbon formaldehyde resins are insufficient in improving adhesive strength, tack strength, and holding power, particularly in pressure-sensitive adhesives, which require balanced performance enhancements.

Method used

A modified aromatic hydrocarbon formaldehyde resin is produced by reacting an aromatic hydrocarbon formaldehyde resin with an aromatic monocarboxylic acid, resulting in a resin with specific ester, saponification, acid, and molecular weight values, enhancing compatibility and adhesive properties.

Benefits of technology

The modified resin significantly improves adhesive strength, tack strength, and holding power when used in adhesives, offering improved compatibility and plasticizing effects while maintaining flexibility and suppressing adverse effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided are: a modified aromatic hydrocarbon formaldehyde resin capable of improving the adhesive force, tack force, and holding force of an adhesive; an adhesive including the modified aromatic hydrocarbon formaldehyde resin; and a method for producing the modified aromatic hydrocarbon formaldehyde resin. The modified aromatic hydrocarbon formaldehyde resin is obtained by a reaction between an aromatic hydrocarbon formaldehyde resin and an aromatic monocarboxylic acid, and has an ester value of 50 mgKOH / g to 250 mgKOH / g.
Need to check novelty before this filing date? Find Prior Art

Description

Modified aromatic hydrocarbon formaldehyde resin, adhesive containing same, and method for producing modified aromatic hydrocarbon formaldehyde resin

[0001] The present invention relates to a modified aromatic hydrocarbon-formaldehyde resin, a pressure-sensitive adhesive containing the same, and a method for producing the modified aromatic hydrocarbon-formaldehyde resin.

[0002] Aromatic hydrocarbon-formaldehyde resins are widely used, for example, to modify adhesives, pressure-sensitive adhesives, paints, etc., and to modify coating materials and sealing materials used in electronic components, etc. For example, Patent Document 1 discloses a method for producing a light-colored, heat-resistant solid rosin-modified aromatic hydrocarbon-formaldehyde resin, which is intended for application in fields such as hot-melt adhesives and traffic paints that require high-temperature properties, and which comprises the steps of reacting rosin with an α,β-unsaturated polybasic acid, adding an oxygen-containing aromatic hydrocarbon-formaldehyde resin, carrying out an esterification reaction at 200 to 300°C in the absence of a catalyst, and then distilling off low-molecular-weight volatile components under reduced pressure.

[0003] Japanese Unexamined Patent Publication No. 48-67385

[0004] A pressure-sensitive adhesive modifier is required to improve various performances of the pressure-sensitive adhesive in a balanced manner, such as adhesive strength, tack strength, holding power, etc. Although Cited Document 1 is excellent in modifying adhesives that require high-temperature properties, it is not sufficient in modifying the adhesive strength, tack strength, and holding power of the pressure-sensitive adhesive.

[0005] The present invention aims to provide a modified aromatic hydrocarbon-formaldehyde resin that, when used in a pressure-sensitive adhesive or the like, can improve the adhesive strength, tackiness, and holding power of the pressure-sensitive adhesive; a pressure-sensitive adhesive containing the modified aromatic hydrocarbon-formaldehyde resin; and a method for producing the modified aromatic hydrocarbon-formaldehyde resin.

[0006] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by a modified aromatic hydrocarbon-formaldehyde resin obtained by reacting an aromatic hydrocarbon-formaldehyde resin with an aromatic monocarboxylic acid, the modified aromatic hydrocarbon-formaldehyde resin having an ester value of 50 mgKOH / g or more and 250 mgKOH / g or less.

[0007] That is, the present invention is as follows. The present invention relates to the following [1] to

[14] . [1] A modified aromatic hydrocarbon-formaldehyde resin obtained by reacting an aromatic hydrocarbon-formaldehyde resin with an aromatic monocarboxylic acid, the modified aromatic hydrocarbon-formaldehyde resin having an ester value of 50 mgKOH / g or more and 250 mgKOH / g or less. [2] The modified aromatic hydrocarbon-formaldehyde resin according to [1], wherein the aromatic hydrocarbon of the aromatic hydrocarbon-formaldehyde resin is at least one selected from xylene, toluene, mesitylene, and pseudocumene. [3] The modified aromatic hydrocarbon-formaldehyde resin according to [1] or [2], wherein the aromatic monocarboxylic acid is at least one selected from benzoic acid, toluic acid, dimethylbenzoic acid, trimethylbenzoic acid, ethylbenzoic acid, biphenylcarboxylic acid, and anthracenecarboxylic acid. [4] The modified aromatic hydrocarbon-formaldehyde resin according to any one of [1] to [3], having a saponification value of 60 mgKOH / g or more and 300 mgKOH / g or less. [5] The modified aromatic hydrocarbon-formaldehyde resin according to any one of [1] to [4], having an acid value of 1 mgKOH / g or more and 50 mgKOH / g or less. [6] The modified aromatic hydrocarbon-formaldehyde resin according to any one of [1] to [5], having a weight-average molecular weight of 300 or more and 3,000 or less. [7] The modified aromatic hydrocarbon-formaldehyde resin according to any one of [1] to [6], having a glass transition temperature of -20°C or more and 15°C or less. [8] The modified aromatic hydrocarbon-formaldehyde resin according to any one of [1] to [7], having a viscosity at 75°C of 500 mPa·s or more and 35,000 mPa·s or less. [9] The modified aromatic hydrocarbon-formaldehyde resin according to any one of [1] to [8], wherein the mass ratio of the aromatic monocarboxylic acid to the aromatic hydrocarbon-formaldehyde resin (aromatic monocarboxylic acid / aromatic hydrocarbon-formaldehyde resin) is 0.10 or more and 1.00 or less.

[10] The modified aromatic hydrocarbon-formaldehyde resin according to any one of [1] to [9], wherein the molar ratio of the number of moles of the aromatic monocarboxylic acid to the number of moles of oxygen atoms contained in the aromatic hydrocarbon-formaldehyde resin (number of moles of aromatic monocarboxylic acid / number of moles of oxygen atoms contained in aromatic hydrocarbon-formaldehyde resin) is 0.05 or more and 1.00 or less.

[11] A pressure-sensitive adhesive containing the modified aromatic hydrocarbon-formaldehyde resin according to any one of [1] to

[10] .

[12] A method for producing a modified aromatic hydrocarbon-formaldehyde resin, comprising reacting an aromatic hydrocarbon-formaldehyde resin with an aromatic monocarboxylic acid to obtain a modified aromatic hydrocarbon-formaldehyde resin having an ester value of 50 mgKOH / g or more and 250 mgKOH / g or less.

[13] The method for producing a modified aromatic hydrocarbon-formaldehyde resin according to

[12] , wherein the mass ratio of the aromatic monocarboxylic acid to the aromatic hydrocarbon-formaldehyde resin (aromatic monocarboxylic acid / aromatic hydrocarbon-formaldehyde resin) is 0.1 or more and 1.0 or less.

[14] The method for producing a modified aromatic hydrocarbon-formaldehyde resin according to

[12] or

[13] , wherein the molar ratio of the number of moles of the aromatic monocarboxylic acid to the number of moles of oxygen atoms contained in the aromatic hydrocarbon-formaldehyde resin (number of moles of aromatic monocarboxylic acid / number of moles of oxygen atoms contained in the aromatic hydrocarbon-formaldehyde resin) is 0.05 or more and 1.0 or less.

[0008] According to the present invention, it is possible to provide a modified aromatic hydrocarbon-formaldehyde resin that, when used in a pressure-sensitive adhesive or the like, can improve the adhesive strength, tackiness, and holding power of the pressure-sensitive adhesive or the like; a pressure-sensitive adhesive containing the modified aromatic hydrocarbon-formaldehyde resin; and a method for producing the modified aromatic hydrocarbon-formaldehyde resin.

[0009] Hereinafter, a mode for carrying out the present invention (hereinafter also simply referred to as "the present embodiment") will be described in detail. The following present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to this embodiment. The present invention can be practiced by appropriately modifying it within the scope of its gist. In this specification, definitions that are considered preferable can be adopted arbitrarily, and it can be said that combinations of preferable definitions are more preferable. In this specification, the expression "XX to YY" means "XX or more and YY or less."

[0010] In this specification, "(meth)acrylic acid" means both "acrylic acid" and "methacrylic acid." The same applies to other similar terms (such as "(meth)acrylate" and "(meth)acryloyl group").

[0011] [Modified Aromatic Hydrocarbon Formaldehyde Resin] The modified aromatic hydrocarbon formaldehyde resin of this embodiment is a modified aromatic hydrocarbon formaldehyde resin obtained by reacting an aromatic hydrocarbon formaldehyde resin with an aromatic monocarboxylic acid, and has an ester value of 50 mgKOH / g or more and 250 mgKOH / g or less. In this embodiment, the aromatic hydrocarbon formaldehyde resin is a resin that serves as a raw material for the modified aromatic hydrocarbon formaldehyde resin. That is, the modified aromatic hydrocarbon formaldehyde resin of this embodiment is a resin obtained by modifying the raw material aromatic hydrocarbon formaldehyde resin with an aromatic monocarboxylic acid. The modified aromatic hydrocarbon formaldehyde resin of this embodiment uses as a raw material an aromatic hydrocarbon formaldehyde resin whose structure is difficult to identify by analysis, and therefore the structure of the modified aromatic hydrocarbon formaldehyde resin modified with an aromatic monocarboxylic acid is also difficult to identify by analysis.

[0012] The ester value of the modified aromatic hydrocarbon-formaldehyde resin of this embodiment is 50 mgKOH / g or more and 250 mgKOH / g or less, preferably 65 mgKOH / g or more and 230 mgKOH / g or less, more preferably 80 mgKOH / g or more and 210 mgKOH / g or less, and even more preferably 95 mgKOH / g or more and 190 mgKOH / g or less. When the ester value of the modified aromatic hydrocarbon-formaldehyde resin is within the above range, the proportion of ester groups in the molecular structure of the modified aromatic hydrocarbon-formaldehyde resin can be increased, thereby increasing polarity. Therefore, when used in adhesives, etc., compatibility with other resins contained in the adhesives, etc. can be improved, an efficient plasticizing effect can be obtained, and the adhesive strength, tackiness, and holding power of the adhesives, etc. can be improved. The ester value can be measured in accordance with JIS K0070:1992 by the method described in the examples.

[0013] The saponification value of the modified aromatic hydrocarbon formaldehyde resin of this embodiment is preferably 60 mgKOH / g or more and 300 mgKOH / g or less, more preferably 80 mgKOH / g or more and 260 mgKOH / g or less, and even more preferably 100 mgKOH / g or more and 220 mgKOH / g or less. When the saponification value of the modified aromatic hydrocarbon formaldehyde resin is within the above range, when used in a pressure-sensitive adhesive or the like, compatibility with other resins contained in the pressure-sensitive adhesive or the like can be easily improved, and an efficient plasticizing effect can be obtained, thereby improving the adhesive strength, tackiness, and holding power of the pressure-sensitive adhesive or the like. The saponification value can be measured in accordance with JIS K0070:1992 by the method described in the Examples.

[0014] The acid value of the modified aromatic hydrocarbon-formaldehyde resin of this embodiment is preferably 1 mgKOH / g or more and 50 mgKOH / g or less, more preferably 2 mgKOH / g or more and 40 mgKOH / g or less, and even more preferably 3 mgKOH / g or more and 35 mgKOH / g or less. When the acid value of the modified aromatic hydrocarbon-formaldehyde resin is within the above range, when used in a pressure-sensitive adhesive or the like, the adverse effect of residual aromatic monocarboxylic acid on the adhesive properties can be suppressed, thereby improving the adhesive strength, tackiness, and holding power of the pressure-sensitive adhesive or the like. The acid value can be measured in accordance with JIS K0070:1992 by the method described in the Examples.

[0015] The weight-average molecular weight of the modified aromatic hydrocarbon-formaldehyde resin of this embodiment is preferably 300 to 3,000, more preferably 400 to 2,500, even more preferably 500 to 2,000, and even more preferably 600 to 1,400. When the weight-average molecular weight of the modified aromatic hydrocarbon-formaldehyde resin is within the above range, when used in a pressure-sensitive adhesive or the like, compatibility with other resins contained in the pressure-sensitive adhesive or the like can be easily improved, and an efficient plasticizing effect can be obtained, thereby improving the adhesive strength, tackiness, and holding power of the pressure-sensitive adhesive or the like. The weight-average molecular weight can be measured by gel permeation chromatography (GPC) using the method described in the Examples.

[0016] The glass transition temperature of the modified aromatic hydrocarbon-formaldehyde resin of this embodiment is preferably −20° C. or higher and 15° C. or lower, more preferably −16° C. or higher and 8° C. or lower, and even more preferably −12° C. or higher and 6° C. or lower. When the glass transition temperature of the modified aromatic hydrocarbon-formaldehyde resin is within the above range, when used in a pressure-sensitive adhesive or the like, it is easy to prevent the softening temperature of the pressure-sensitive adhesive or the like from being excessively lowered, and an efficient plasticizing effect on the pressure-sensitive adhesive or the like can be obtained, thereby improving the adhesive strength, tack strength, and holding power of the pressure-sensitive adhesive or the like. The glass transition temperature can be measured by the method described in the examples.

[0017] The viscosity of the modified aromatic hydrocarbon formaldehyde resin of this embodiment at 75°C is preferably 500 mPa·s or more and 35,000 mPa·s or less, more preferably 600 mPa·s or more and 30,000 mPa·s or less, even more preferably 800 mPa·s or more and 15,000 mPa·s or less, and even more preferably 1,000 mPa·s or more and 3,000 mPa·s or less. When the modified aromatic hydrocarbon formaldehyde resin has a viscosity of 500 mPa·s or more at 75°C, excessive plasticization of the adhesive or the like can be easily suppressed when used in an adhesive, etc., thereby making it easier to suppress a decrease in the adhesive's holding power. Furthermore, when the viscosity at 75°C is 35,000 mPa·s or less, the flexibility of the adhesive layer can be easily maintained and the tackiness can be easily improved. The viscosity at 75°C can be measured using an E-type viscometer by the method described in the examples.

[0018] (Aromatic Hydrocarbon Formaldehyde Resin) In this embodiment, the aromatic hydrocarbon formaldehyde resin is a resin that serves as a raw material for a modified aromatic hydrocarbon formaldehyde resin. The aromatic hydrocarbon formaldehyde resin is obtained by reacting an aromatic hydrocarbon with formaldehyde. Examples of the aromatic hydrocarbon include at least one selected from benzene, toluene, xylene, mesitylene, pseudocumene, ethylbenzene, propylbenzene, decylbenzene, cyclohexylbenzene, biphenyl, methylbiphenyl, naphthalene, methylnaphthalene, dimethylnaphthalene, ethylnaphthalene, anthracene, methylanthracene, dimethylanthracene, ethylanthracene, and binaphthyl. When used in a pressure-sensitive adhesive or the like, from the viewpoint of improving the adhesive strength, tackiness, and holding power of the pressure-sensitive adhesive or the like, at least one selected from xylene, toluene, mesitylene, and pseudocumene is preferred, xylene is more preferred, and meta-xylene is even more preferred. From the same viewpoint as above, the aromatic hydrocarbon formaldehyde resin preferably contains at least one selected from a xylene formaldehyde resin obtained by reacting xylene with formaldehyde, a toluene formaldehyde resin obtained by reacting toluene with formaldehyde, and a mesitylene formaldehyde resin obtained by reacting mesitylene with formaldehyde, and more preferably contains a xylene formaldehyde resin.

[0019] The aromatic hydrocarbon-formaldehyde resin may be a commercially available product or may be prepared by a known method. An example of a commercially available product is "NIKANOL G," a xylene resin manufactured by Fudow Co., Ltd. An example of a known method is the method described in Japanese Patent Publication No. 37-5747, in which an aromatic hydrocarbon and formaldehyde are subjected to a condensation reaction in the presence of a catalyst.

[0020] The weight-average molecular weight (Mw) of the aromatic hydrocarbon-formaldehyde resin, calculated as polystyrene, is preferably 200 to 10,000, more preferably 300 to 5,000, even more preferably 350 to 2,000, and even more preferably 500 to 1,500. Having the Mw of the aromatic hydrocarbon-formaldehyde resin within the above range is preferred because it allows for sufficient compatibility with other resin components when used in adhesives and the like. The weight-average molecular weight (Mw) can be measured by gel permeation chromatography (GPC) using the method described in the Examples.

[0021] (Aromatic Monocarboxylic Acid) The modified aromatic hydrocarbon-formaldehyde resin of this embodiment is obtained by reacting an aromatic hydrocarbon-formaldehyde resin with an aromatic monocarboxylic acid. That is, the modified aromatic hydrocarbon-formaldehyde resin of this embodiment is obtained by modifying an aromatic hydrocarbon-formaldehyde resin with an aromatic monocarboxylic acid. By using an aromatic monocarboxylic acid, the molecular weight of the modified aromatic hydrocarbon-formaldehyde resin can be reduced, and an ester group can be introduced, which improves compatibility with other resin components when used in adhesives and the like, and provides an efficient plasticizing effect, thereby improving the adhesive strength, tackiness, and holding power of the adhesive and the like.

[0022] As the aromatic monocarboxylic acid, from the viewpoint of improving the adhesive strength, tackiness and holding power of the adhesive or the like when used in an adhesive or the like, at least one selected from benzoic acid, toluic acid, dimethylbenzoic acid, trimethylbenzoic acid, ethylbenzoic acid, biphenylcarboxylic acid and anthracenecarboxylic acid is preferred, at least one selected from benzoic acid and toluic acid is more preferred, and benzoic acid is even more preferred.

[0023] [Method for Producing Modified Aromatic Hydrocarbon-Formaldehyde Resin] The method for producing a modified aromatic hydrocarbon-formaldehyde resin of this embodiment is a production method in which an aromatic hydrocarbon-formaldehyde resin is reacted with an aromatic monocarboxylic acid to obtain a modified aromatic hydrocarbon-formaldehyde resin having an ester value of 50 mgKOH / g or more and 250 mgKOH / g or less. That is, the modified aromatic hydrocarbon-formaldehyde resin of this embodiment can be produced by reacting an aromatic hydrocarbon-formaldehyde resin with an aromatic monocarboxylic acid. Specifically, the method for producing a modified aromatic hydrocarbon-formaldehyde resin of this embodiment is preferably a production method including a step of reacting an aromatic hydrocarbon-formaldehyde resin with an aromatic monocarboxylic acid in the presence of an acidic catalyst to obtain the modified aromatic hydrocarbon-formaldehyde resin.

[0024] When an acidic catalyst is used in the method for producing a modified aromatic hydrocarbon-formaldehyde resin of this embodiment, the acidic catalyst is not particularly limited, but examples thereof include paratoluenesulfonic acid, metaxylenesulfonic acid, and paratoluenesulfonic acid chloride. Furthermore, in the method for producing a modified aromatic hydrocarbon-formaldehyde resin of this embodiment, the reaction temperature for the reaction between the aromatic hydrocarbon-formaldehyde resin and the aromatic monocarboxylic acid is preferably 70 to 130°C, more preferably 90 to 110°C. Furthermore, the reaction time is not particularly limited, but is preferably 0.5 to 30 hours, more preferably 0.5 to 15 hours. Furthermore, in the method for producing a modified aromatic hydrocarbon-formaldehyde resin of this embodiment, the reaction between the aromatic hydrocarbon-formaldehyde resin and the aromatic monocarboxylic acid is preferably carried out under a nitrogen atmosphere in order to improve reaction efficiency.

[0025] In the method for producing a modified aromatic hydrocarbon-formaldehyde resin of this embodiment, the mass ratio of the aromatic monocarboxylic acid to the aromatic hydrocarbon-formaldehyde resin (aromatic monocarboxylic acid / aromatic hydrocarbon-formaldehyde resin) is preferably 0.10 to 1.00, more preferably 0.15 to 0.95, even more preferably 0.20 to 0.85, and still more preferably 0.25 to 0.75. When the mass ratio of the aromatic monocarboxylic acid to the aromatic hydrocarbon-formaldehyde resin is within the above range, the ester value, saponification value, and acid value can be easily adjusted to fall within the above ranges, and when used in a pressure-sensitive adhesive or the like, the adhesive strength, tackiness, and holding power of the pressure-sensitive adhesive or the like can be improved.

[0026] In the method for producing a modified aromatic hydrocarbon-formaldehyde resin of this embodiment, the molar ratio of the number of moles of aromatic monocarboxylic acid to the number of moles of oxygen atoms contained in the aromatic hydrocarbon-formaldehyde resin (number of moles of aromatic monocarboxylic acid / number of moles of oxygen atoms contained in aromatic hydrocarbon-formaldehyde resin) is preferably 0.05 to 1.00, more preferably 0.15 to 0.95, even more preferably 0.20 to 0.90, and even more preferably 0.25 to 0.85. When the molar ratio of the number of moles of aromatic monocarboxylic acid to the number of moles of oxygen atoms contained in the aromatic hydrocarbon-formaldehyde resin is within the above range, the ester value, saponification value, and acid value can be easily adjusted within the above ranges, and when used in a pressure-sensitive adhesive or the like, the adhesive strength, tackiness, and holding power of the pressure-sensitive adhesive or the like can be improved.

[0027] Furthermore, from the viewpoint of obtaining a highly pure modified aromatic hydrocarbon-formaldehyde resin, it is preferable to carry out vacuum purification after completion of the reaction. The pressure during vacuum purification can be typically 100 hPa or less, preferably 50 hPa or less, from the viewpoint of obtaining a highly pure modified aromatic hydrocarbon-formaldehyde resin. The temperature during vacuum distillation can be typically 120 to 160°C, preferably 130 to 150°C, from the viewpoint of obtaining a highly pure modified aromatic hydrocarbon-formaldehyde resin.

[0028] Furthermore, in the method for producing a modified aromatic hydrocarbon-formaldehyde resin according to this embodiment, from the viewpoint of obtaining a highly pure modified aromatic hydrocarbon-formaldehyde resin, it is preferable to include a step of removing impurities such as formaldehyde from the raw aromatic hydrocarbon-formaldehyde resin before reacting the aromatic hydrocarbon-formaldehyde resin with an aromatic monocarboxylic acid. Specifically, the impurity-removing step preferably includes a step of adding an acidic catalyst to the aromatic hydrocarbon-formaldehyde resin and stirring the mixture while blowing in steam before reacting the aromatic hydrocarbon-formaldehyde resin with an aromatic monocarboxylic acid. This step allows for efficient removal of formaldehyde, particularly from the raw aromatic hydrocarbon-formaldehyde resin, making it easier to obtain a highly pure modified aromatic hydrocarbon-formaldehyde resin. When an acidic catalyst is used in the impurity-removing step, the acidic catalyst is not particularly limited, but examples include paratoluenesulfonic acid, metaxylenesulfonic acid, and paratoluenesulfonic acid chloride. In the step of removing impurities, the stirring temperature is preferably 100 to 190° C., more preferably 120 to 150° C. The stirring time is not particularly limited, but is preferably 0.5 to 30 hours, more preferably 0.5 to 15 hours.

[0029] As described above, when used in a pressure-sensitive adhesive, the modified aromatic hydrocarbon formaldehyde resin of the present embodiment can improve the adhesive strength, tackiness, and holding power of the pressure-sensitive adhesive, etc. Therefore, the modified aromatic hydrocarbon formaldehyde resin of the present embodiment can be suitably used as a tackifier for pressure-sensitive adhesives, an additive for adhesives, paints, rubbers, etc.

[0030] [Adhesive] The adhesive of this embodiment contains the modified aromatic hydrocarbon formaldehyde resin of this embodiment. The adhesive of this embodiment preferably contains the modified aromatic hydrocarbon formaldehyde resin as a tackifier. Because the adhesive of this embodiment contains the modified aromatic hydrocarbon formaldehyde resin, a high plasticizing effect can be obtained, resulting in excellent adhesive strength, tackiness, and holding power. The adhesive of this embodiment preferably contains the modified aromatic hydrocarbon formaldehyde resin of this embodiment, an acrylic resin, and a solvent.

[0031] (Acrylic Resin) In the pressure-sensitive adhesive of the present embodiment, the acrylic resin is not particularly limited, but is preferably an acrylic copolymer. Examples of the acrylic polymer include an acrylic copolymer having at least one component selected from a component derived from an acrylic acid alkyl ester having an alkyl group with 4 to 10 carbon atoms, a component derived from a compound having an olefinically unsaturated double bond, and a component derived from a (meth)acrylic acid ester containing a hydroxyl group.

[0032] The alkyl acrylate is preferably at least one selected from n-butyl acrylate, sec-butyl acrylate, isobutyl acrylate, n-amyl acrylate, isoamyl acrylate, n-hexyl acrylate, heptyl acrylate, n-octyl acrylate, capryl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, isononyl acrylate, and decyl acrylate, and more preferably at least one selected from n-butyl acrylate and 2-ethylhexyl acrylate.

[0033] The compound having an olefinically unsaturated double bond is preferably at least one selected from methacrylic acid, acrylic acid, itaconic acid, maleic acid, vinyl acetate, methyl acrylate, methyl methacrylate, vinylidene chloride, styrene, and acrylonitrile, and more preferably at least one selected from acrylic acid and vinyl acetate.

[0034] The hydroxyl group-containing (meth)acrylic acid ester is preferably at least one selected from 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 4-hydroxycyclohexyl (meth)acrylate, 5-hydroxycyclooctyl (meth)acrylate, 2-hydroxy-3-phenyloxypropyl (meth)acrylate, pentaerythritol tri(meth)acrylate, hydroxyalkyl (meth)acrylate; polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate; hydroxy group-containing (meth)acrylamides such as N-methylol (meth)acrylamide; and reaction products obtained by reacting a diglycidyl ester of vinyl alcohol, vinylphenol, or bisphenol A with (meth)acrylic acid; more preferably a hydroxyalkyl (meth)acrylate, and more preferably 2-hydroxyethyl acrylate.

[0035] The acrylic copolymer may be produced by a known polymerization method. It is preferable to use a polymerization initiator when polymerizing the acrylic copolymer. The polymerization initiator is not particularly limited, and examples thereof include organic peroxides such as benzoyl peroxide, cumene hydroperoxide, and tert-butyl hydroperoxide, and azo-based initiators such as azobisisobutyronitrile. These initiators may be used alone or in appropriate combinations of two or more. The solvent used when polymerizing the acrylic copolymer is not particularly limited, but examples of the solvent used in the pressure-sensitive adhesive of the present embodiment include, but are not limited to, aromatic hydrocarbons such as toluene, aliphatic hydrocarbons such as hexane, esters such as ethyl acetate, ketones such as methyl ethyl ketone, and alcohols such as ethanol. Among these, esters are preferred, and ethyl acetate is more preferred, from the viewpoint of workability.

[0036] (Solvent) In the pressure-sensitive adhesive of the present embodiment, the solvent is not particularly limited, and examples thereof include aromatic hydrocarbons such as toluene, aliphatic hydrocarbons such as hexane, esters such as ethyl acetate, ketones such as methyl ethyl ketone, and alcohols such as ethanol. Among these, from the viewpoint of workability, esters are preferred, and ethyl acetate is more preferred.

[0037] (Crosslinking Agent) The pressure-sensitive adhesive of the present embodiment preferably further contains a crosslinking agent as needed. The crosslinking agent is not particularly limited, but isocyanate-based crosslinking agents are preferred from the viewpoint of improving adhesive strength, tackiness, and holding power. Examples of isocyanate-based crosslinking agents include tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPID), xylylene diisocyanate (XDI), and derivatives thereof.

[0038] (Other Components) The pressure-sensitive adhesive of the present embodiment may contain other components such as fillers, flame retardants, silane coupling agents, wetting and dispersing agents, photopolymerization initiators, photocuring initiators, heat curing accelerators, and various additives, within the scope of not impairing the properties of the present embodiment.

[0039] The present invention will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way.

[0040] (1) Ester Value, Acid Value, and Saponification Value The acid value and saponification value of the modified aromatic hydrocarbon formaldehyde resins obtained in the Examples and Comparative Examples were measured by neutralization titration in accordance with JIS K0070:1992. The ester value was calculated from the acid value and saponification value measured above using the following formula: Ester value (mg KOH / g) = Saponification value (mg KOH / g) - Acid value (mg KOH / g)

[0041] (2) Weight-average molecular weight (Mw) The weight-average molecular weight (Mw) of the modified aromatic hydrocarbon-formaldehyde resins obtained in the Examples and Comparative Examples was determined by GPC analysis in terms of polystyrene. The apparatus and conditions used for the analysis are as follows: Apparatus: Shodex GPC-101 (manufactured by Resonac Co., Ltd.) Column: Shodex LF-804 x 3 (manufactured by Resonac Co., Ltd.) Eluent: tetrahydrofuran Flow rate: 1.0 mL / min Column temperature: 40°C Detector: RI (differential refractometer)

[0042] (3) Glass Transition Temperature The glass transition temperature (Tg) of the modified aromatic hydrocarbon formaldehyde resins obtained in the Examples and Comparative Examples was determined by differential scanning calorimetry. The apparatus and conditions used for the analysis are as follows: (Apparatus) DSC25 (manufactured by TA Instruments) (Analysis Conditions) Measurement was performed in a nitrogen atmosphere at a temperature rise rate of 10°C / min in the temperature range of -40°C to 100°C, and a DSC curve was obtained.

[0043] (4) Viscosity at 75°C The viscosity at 75°C of the modified aromatic hydrocarbon-formaldehyde resins obtained in the Examples and Comparative Examples was measured using an E-type viscometer "TVE-22H Cone-Plate Type Viscometer" (manufactured by Toki Sangyo Co., Ltd.).

[0044] (5) Molar Number of Oxygen Atoms The mole number of oxygen atoms in the aromatic hydrocarbon formaldehyde resins used in the examples and comparative examples was measured using an elemental analyzer "JM11" (manufactured by J Science Lab Co., Ltd.).

[0045] (6) Evaluation of adhesives Using the adhesives of the examples and comparative examples, double-sided adhesive tapes were prepared as evaluation samples, and the adhesive strength, tackiness, and holding power of each tape were measured and evaluated. Permeability was also measured. The evaluation results are shown in Tables 4 and 5.

[0046] (6-1) Preparation of double-sided adhesive tape The adhesives obtained in the examples and comparative examples were applied to a release film (NP50B, manufactured by Panac Corporation) using a bar coater (No. 24) and dried in a hot air dryer at 100°C for 2 minutes. Then, a PET film (E5100, manufactured by Toyobo Co., Ltd., thickness 12 μm) was attached using a laminator. The other side of the PET film was laminated in the same configuration, and then aged at 40°C for 2 days to obtain a double-sided adhesive tape.

[0047] (6-2) Adhesion (SUS Resistance) Peel strength was measured and evaluated in accordance with JIS Z 0237:2022. The obtained double-sided adhesive tape was cut into strips measuring 24±0.5 mm in width and approximately 300 mm in length, the release film on one side was peeled off, and the strips were attached to SUS plates (manufactured by Partec Co., Ltd.). The strips were then pressed using a 2 kg pressure roller to prepare measurement samples. A peel test was performed using the measurement samples to measure the peel strength and evaluate the adhesive strength. The peel test conditions were 23°C / 50% relative humidity, 180° peeling, and a test speed of 300 mm / min. The peel strength was measured within 1 minute after the evaluation sample was prepared. Regarding adhesive strength, the Examples and Comparative Examples using acrylic resin base A were evaluated based on the measured value of Comparative Example 2-8 as the blank, and the Examples and Comparative Examples using acrylic resin base B were evaluated based on the measured value of Comparative Example 2-9 as the blank. (Evaluation criteria) A: Peel strength is 2.0 N / 24 mm or more higher than the blank. B: Peel strength is 1.0 N / 24 mm or more but less than 2.0 N / 24 mm higher than the blank. C: Peel strength is less than 1.0 N / 24 mm higher than the blank, or lower than the blank.

[0048] (6-3) Adhesion (Polypropylene Resistance) Peel strength was measured and evaluated in accordance with JIS Z 0237:2022. The obtained double-sided adhesive tape was cut into strips measuring 24±0.5 mm in width and approximately 300 mm in length, the release film on one side was peeled off, and the strips were attached to a PP (polypropylene) plate (manufactured by Partec Co., Ltd.). The strips were then pressed using a 2 kg pressure roller to prepare measurement samples. A peel test was conducted using the measurement samples to measure the peel strength and evaluate the adhesive strength. The peel test conditions were 23°C / 50% relative humidity, 180° peeling, and a test speed of 300 mm / min. The peel strength was measured within 1 minute after the evaluation sample was prepared. Regarding adhesive strength, the Examples and Comparative Examples using acrylic resin base A were evaluated based on the measurement value of Comparative Example 2-8 as the blank, and the Examples and Comparative Examples using acrylic resin base B were evaluated based on the measurement value of Comparative Example 2-9 as the blank. Evaluation was performed based on the following evaluation criteria. When the peel strength observed during one test was calculated by dividing the maximum peel strength by the minimum peel strength, if the calculated value was 2.0 or more, it was determined that zipping had occurred. (Evaluation criteria) A: The peel strength was 2.0 N / 24 mm or more higher than that of the blank. B: The peel strength was 1.0 N / 24 mm or more but less than 2.0 N / 24 mm higher than that of the blank. C: The peel strength was less than 1.0 N / 24 mm higher than that of the blank, or was lower than that of the blank, or zipping had occurred.

[0049] (6-4) Tack Strength Evaluation was performed using the inclined ball tack method in accordance with JIS Z 0237:2022. Double-sided adhesive tape was cut into strips approximately 15 mm wide and 100 mm long, the release film on one side was peeled off, and the strip was attached to a 30° inclined plate. After peeling off the release film on the other side, the ball was quickly rolled and tested. The test conditions were 23°C / 50% relative humidity, a 100 mm runway, and the test ball was made of SUJ2 high-carbon chromium bearing steel. Regarding tack strength, the Examples and Comparative Examples using acrylic resin base A were evaluated based on the measurement results of Comparative Example 2-8 as the blank, while the Examples and Comparative Examples using acrylic resin base B were evaluated based on the measurement results of Comparative Example 2-9 as the blank. Evaluation criteria were as follows: (Evaluation Criteria) A: The ball number was at least three levels higher than the blank. B: The ball number was two levels higher than the blank. C: The ball number is one size larger or smaller than the blank.

[0050] (6-5) Holding Power The obtained double-sided adhesive tape was cut into strips measuring 12±0.5 mm in width and approximately 150 mm in length. The release film on one side was peeled off and the tape was attached to the edge of a stainless steel plate (manufactured by Partec Co., Ltd.) in an area measuring 12±0.5 mm in width and 12±0.5 mm in length. The tape was then pressed using a 2 kg pressure roller, and a 500 g weight was attached to the opposite end of the tape, and a holding power test was performed. The holding power test was performed at 40°C for 1 hour. After 1 hour of testing, the distance the double-sided adhesive tape had shifted from the initial bonding position was observed, and the holding power was evaluated based on the following evaluation criteria. (Evaluation Criteria) A: No deviation in the bonding position was observed. B: No deviation in the bonding position was observed, but when the double-sided adhesive tape was peeled off after the test, adhesive remained on the SUS plate. C: Deviation in the bonding position was observed, and when the double-sided adhesive tape was peeled off after the test, adhesive remained on the SUS plate.

[0051] (6-6) Transparency The obtained double-sided adhesive tape was cut into a 30 mm square, the release film on one side was peeled off, and the tape was attached to a 2 mm thick glass plate (manufactured by Partec Co., Ltd.). After peeling off the release film on the other side, the transmittance was immediately measured under the following test conditions. A higher transmittance indicates higher transparency. Test conditions: 23°C / 50% relative humidity. Measuring instrument: Haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., COH400).

[0052] <Preparation of Modified Aromatic Hydrocarbon Formaldehyde Resin> (Example 1-1) 400 parts by mass of NIKANOL G (manufactured by Fudow Co., Ltd., xylene resin, hydroxyl value: 32 mg KOH / g, weight average molecular weight: 1,170) and 1.2 parts by mass of p-toluenesulfonic acid (manufactured by Kanto Chemical Co., Ltd.) were charged into a flask equipped with a stirrer, a Snyder tube, a condenser, and a steam generator. The mixture was stirred for 2 hours while blowing in steam and controlling the internal temperature at 120°C. Thereafter, 220 parts by mass of benzoic acid (manufactured by Kanto Chemical Co., Ltd.) as an aromatic monocarboxylic acid, 1.2 parts by mass of p-toluenesulfonic acid, and 62 parts by mass of purified water were added, and the mixture was refluxed for 30 minutes under a nitrogen atmosphere. Thereafter, the temperature was raised to 140°C over 1 hour while slowly distilling off the purified water, while paying attention to sublimation of the aromatic monocarboxylic acid, and the mixture was stirred at 140°C for an additional 1 hour. Next, while maintaining the temperature at 140° C., the pressure was reduced to 50 hPa, and purification was carried out under reduced pressure for 1.5 hours to obtain a modified aromatic hydrocarbon-formaldehyde resin.

[0053] Examples 1-2 to 1-5 Modified aromatic hydrocarbon-formaldehyde resins were obtained in the same manner as in Example 1-1, except that the amounts of p-toluenesulfonic acid, benzoic acid, additional p-toluenesulfonic acid, and additional purified water were changed as shown in Table 1.

[0054] Example 1-6 A modified aromatic hydrocarbon-formaldehyde resin was obtained in the same manner as in Example 1-1, except that m-toluic acid (manufactured by Kanto Chemical Co., Inc.) was used as the aromatic monocarboxylic acid, and the amounts of p-toluenesulfonic acid, m-toluic acid, additional p-toluenesulfonic acid, and additional purified water were changed as shown in Table 1.

[0055] Comparative Example 1-1 A modified aromatic hydrocarbon-formaldehyde resin was obtained in the same manner as in Example 1-1, except that no aromatic monocarboxylic acid was used and the amounts of p-toluenesulfonic acid, additional p-toluenesulfonic acid, and additional purified water were changed as shown in Table 1.

[0056]

[0057] <Preparation of Pressure-Sensitive Adhesive> (Preparation of Acrylic Resin Base) [Synthesis Example 1] A flask equipped with a stirrer, a Snyder tube, and a condenser was charged with 200 parts by mass of n-butyl acrylate (manufactured by Kanto Chemical Co., Ltd.), 6 parts by mass of acrylic acid (manufactured by Kanto Chemical Co., Ltd.), 10 parts by mass of vinyl acrylate (manufactured by Kanto Chemical Co., Ltd.), 0.2 parts by mass of 2-hydroxyethyl acrylate (manufactured by Kanto Chemical Co., Ltd.), and 344 parts by mass of ethyl acetate (manufactured by Kanto Chemical Co., Ltd.), and refluxing was initiated under a nitrogen atmosphere. Thereafter, 0.2 parts by mass of azobisisobutyronitrile (manufactured by Kanto Chemical Co., Ltd.) was added, and the mixture was refluxed for 6 hours. Thereafter, an additional 95 parts by mass of ethyl acetate was added to obtain an acrylic resin base A having a solids concentration of 33% and a weight average molecular weight of 511,000.

[0058] Synthesis Example 2: A flask equipped with a stirrer, a Snyder tube, and a condenser was charged with 140 parts by mass of n-butyl acrylate (manufactured by Kanto Chemical Co., Ltd.), 6 parts by mass of acrylic acid (manufactured by Kanto Chemical Co., Ltd.), 54 parts by mass of 2-ethylhexyl acrylate (manufactured by Kanto Chemical Co., Ltd.), 0.4 parts by mass of 2-hydroxyethyl acrylate (manufactured by Kanto Chemical Co., Ltd.), and 160 parts by mass of ethyl acetate (manufactured by Kanto Chemical Co., Ltd.), and refluxing was initiated under a nitrogen atmosphere. Subsequently, 0.2 parts by mass of azobisisobutyronitrile (manufactured by Kanto Chemical Co., Ltd.) was added, and the mixture was refluxed for 6 hours. Subsequently, 247 parts by mass of ethyl acetate was added to obtain an acrylic adhesive base resin B having a solids concentration of 33% and a weight average molecular weight of 619,000.

[0059]

[0060] Example 2-1 To a 50 mL vial, 15.0 parts by mass of acrylic resin base A, 0.6 parts by mass of the modified aromatic hydrocarbon formaldehyde resin obtained in Example 1-1 as a tackifier, and 0.1 parts by mass of Coronate L (manufactured by Tosoh Corporation, isocyanate-based crosslinking agent) as a crosslinking agent were added, and the mixture was stirred with a wooden spatula to obtain a pressure-sensitive adhesive.

[0061] Examples 2-2 to 2-8, Comparative Examples 2-1 to 2-7 Except for changing the types of tackifier and acrylic resin base as shown in Table 3 and changing the amounts of the acrylic base resin, tackifier, and crosslinking agent charged as shown in Table 3, pressure-sensitive adhesives were obtained in the same manner as in Example 2-1.

[0062] (Comparative Examples 2-8 and 2-9) PSA was obtained in the same manner as in Example 2-1, except that no tackifier was used, the type of acrylic resin base was changed as shown in Table 3, and the amounts of the acrylic base resin and crosslinking agent charged were changed as shown in Table 3. Comparative Example 2-8 served as the basis for evaluation of the Examples and Comparative Examples using acrylic resin base A, and Comparative Example 2-9 served as the basis for evaluation of the Examples and Comparative Examples using acrylic resin base B.

[0063]

[0064]

[0065]

[0066] The results in Tables 4 and 5 confirm that the adhesives of Examples 2-1 to 2-8, including Examples 1-1 to 1-6, which are modified aromatic hydrocarbon formaldehyde resins of the present invention, have improved adhesive strength, tack strength, and holding power compared to the adhesives of Comparative Examples 2-1 to 2-9.

Claims

1. A modified aromatic hydrocarbon formaldehyde resin obtained by reacting an aromatic hydrocarbon formaldehyde resin with an aromatic monocarboxylic acid, the modified aromatic hydrocarbon formaldehyde resin having an ester value of 50 mg KOH / g or more and 250 mg KOH / g or less.

2. The modified aromatic hydrocarbon-formaldehyde resin according to claim 1, wherein the aromatic hydrocarbon of the aromatic hydrocarbon-formaldehyde resin is at least one selected from the group consisting of xylene, toluene, mesitylene and pseudocumene.

3. The modified aromatic hydrocarbon formaldehyde resin according to claim 1 or 2, wherein the aromatic monocarboxylic acid is at least one selected from the group consisting of benzoic acid, toluic acid, dimethylbenzoic acid, trimethylbenzoic acid, ethylbenzoic acid, biphenylcarboxylic acid and anthracenecarboxylic acid.

4. The modified aromatic hydrocarbon formaldehyde resin according to any one of claims 1 to 3, having a saponification value of 60 mg KOH / g or more and 300 mg KOH / g or less.

5. The modified aromatic hydrocarbon formaldehyde resin according to any one of claims 1 to 4, having an acid value of 1 mgKOH / g or more and 50 mgKOH / g or less.

6. The modified aromatic hydrocarbon formaldehyde resin according to any one of claims 1 to 5, having a weight average molecular weight of 300 or more and 3,000 or less.

7. The modified aromatic hydrocarbon formaldehyde resin according to any one of claims 1 to 6, having a glass transition temperature of -20°C or higher and 15°C or lower.

8. The modified aromatic hydrocarbon formaldehyde resin according to any one of claims 1 to 7, having a viscosity at 75°C of 500 mPa·s or more and 35,000 mPa·s or less.

9. The modified aromatic hydrocarbon formaldehyde resin according to any one of claims 1 to 8, wherein the mass ratio of the aromatic monocarboxylic acid to the aromatic hydrocarbon formaldehyde resin (aromatic monocarboxylic acid / aromatic hydrocarbon formaldehyde resin) is 0.10 or more and 1.00 or less.

10. The modified aromatic hydrocarbon formaldehyde resin according to any one of claims 1 to 9, wherein the molar ratio of the number of moles of the aromatic monocarboxylic acid to the number of moles of oxygen atoms contained in the aromatic hydrocarbon formaldehyde resin (number of moles of aromatic monocarboxylic acid / number of moles of oxygen atoms contained in the aromatic hydrocarbon formaldehyde resin) is 0.05 or more and 1.00 or less.

11. A pressure sensitive adhesive comprising the modified aromatic hydrocarbon formaldehyde resin according to any one of claims 1 to 10.

12. A method for producing a modified aromatic hydrocarbon formaldehyde resin, comprising reacting an aromatic hydrocarbon formaldehyde resin with an aromatic monocarboxylic acid to obtain a modified aromatic hydrocarbon formaldehyde resin having an ester value of 50 mg KOH / g or more and 250 mg KOH / g or less.

13. A method for producing a modified aromatic hydrocarbon formaldehyde resin according to claim 12, wherein the mass ratio of the aromatic monocarboxylic acid to the aromatic hydrocarbon formaldehyde resin (aromatic monocarboxylic acid / aromatic hydrocarbon formaldehyde resin) is 0.10 or more and 1.00 or less.

14. A method for producing a modified aromatic hydrocarbon formaldehyde resin according to claim 12 or 13, wherein the molar ratio of the number of moles of the aromatic monocarboxylic acid to the number of moles of oxygen atoms contained in the aromatic hydrocarbon formaldehyde resin (number of moles of aromatic monocarboxylic acid / number of moles of oxygen atoms contained in the aromatic hydrocarbon formaldehyde resin) is 0.05 or more and 1.00 or less.

Citation Information

Patent Citations

  • Method for producing low-viscosity phenol-modified aromatic hydrocarbon formaldehyde resin

    JP2007297610A

  • Ultraviolet-curable resin composition, cured product and article

    JP2014034605A

  • Epoxy resin, epoxy resin composition, and cured product thereof

    WO2020044787A1

  • Urethane resin

    WO2021039832A1

  • Resin, method for producing resin, curable resin composition, and cured object

    WO2023021813A1